R-T-B series sintered magnet and preparation method thereof
Through the spherical transformation of R-T-B alloy powder and the introduction of heavy rare earth elements, the 'core-shell structure' is constructed, which solves the problems of low coercivity and poor temperature resistance of R-T-B sintered magnets, and the preparation of large-size high-performance magnets is realized. Reduced heavy rare earth usage and production costs.
Patent Information
- Application Number
- CN202411130018.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing R-T-B system sintered magnets have low coercivity and poor temperature resistance, which leads to limited expansion of their application areas. The existing powder mixing and powder surface deposition technologies are low in production efficiency and high in large-size magnets.
By spherical transformation of R-T-B alloy powder and introducing heavy rare earth elements, a ‘core-shell structure’ is constructed to improve the intrinsic coercive force and magnetic properties of the magnet, it is suitable for large-sized sintered magnets.
It significantly improves the intrinsic coercive force and maximum magnetic energy product of the R-T-B system sintered magnet, reduces the use of heavy rare earth elements, and is suitable for the preparation of large-size high-performance magnets, reducing production costs.
Smart Images

Figure BDA0004997545640000151
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of rare earth permanent magnet materials, and in particular relates to a method for preparing an RTB-based sintered magnet, and a high-performance RTB-based sintered magnet prepared by the preparation method. Background Art
[0002] RTB-based sintered magnets are a high-performance type of permanent magnet. R represents at least one rare earth element, which must include Nd; T represents at least one transition metal element, which must include Fe; and B represents boron. RTB-based sintered magnets are widely used in various generators and motors in automotive, household appliances, and other fields.
[0003] As the core component of permanent magnet motors, the performance of RTB-based sintered magnets directly impacts the motor's performance. The physical quantities that characterize the magnetic properties of permanent magnets in the industry primarily include remanence, intrinsic coercivity, and maximum magnetic energy product. Remanence and maximum magnetic energy product reflect the strength of the magnetic field provided by the magnet in space, while intrinsic coercivity reflects the magnet's resistance to demagnetization. Therefore, to ensure efficient, safe, and stable operation of permanent magnet motors, high standards must be met for the intrinsic coercivity, remanence, and maximum magnetic energy product of RTB-based sintered magnets.
[0004] However, the low coercivity and poor temperature resistance of conventional RTB-based sintered magnets have, to a certain extent, restricted the expansion of their application areas. For a long time, a widely used method to improve the coercivity of magnets has been to add heavy rare earth elements (such as dysprosium or terbium) to RTB-based alloys to replace (or partially replace) neodymium to form dysprosium iron boron (or dysprosium neodymium iron boron) or terbium iron boron (or terbium neodymium iron boron) with higher anisotropy fields. This method not only increases the coercivity of the magnets, but also significantly improves the temperature resistance of the magnets. However, this method has two obvious disadvantages: (1) In dysprosium iron boron (or dysprosium neodymium iron boron) or terbium iron boron (or terbium neodymium iron boron), dysprosium (or terbium) and iron are antiferromagnetic, while neodymium and iron in neodymium iron boron are ferromagnetic. After dysprosium or terbium replaces (or partially replaces) neodymium, the magnetization intensity of the magnet will be reduced (reducing the remanence and maximum magnetic energy product), thereby reducing the magnitude of the magnetic field intensity provided by the magnet in space; (2) Dysprosium and terbium are heavy rare earth resources with small reserves and high prices. Using dysprosium or terbium to replace (or partially replace) neodymium will consume a large amount of heavy rare earth resources and greatly increase the manufacturing cost of the magnet. The manufacturing cost will be passed on to downstream users, which also restricts the expansion of the application field of RTB series sintered magnets to a certain extent. How to achieve low heavy rare earth and high coercivity at the same time has become a common and key technical problem in the rare earth permanent magnet industry.
[0005] Previous studies have shown that the coercivity mechanism of RTB-based sintered magnets is the nucleation of reversed magnetization domains. Defective layers exist on the surface of the primary phase grains, where their coercivity is significantly lower than that of the grain interior. Under the influence of a reverse magnetic field, these defective layers first reverse nucleate and then extend throughout the primary phase's "core-shell structure" (heavy rare earth-rich shell, light rare earth-rich core). This significantly increases the coercivity of the primary phase's surface grains, and thus the entire primary phase grain. Because heavy rare earth elements are confined to the surface of the primary phase grains, these processes require significantly less heavy rare earth elements than direct addition prior to alloy smelting. The resulting magnets exhibit low levels of heavy rare earth elements and high coercivity.
[0006] At present, there are mainly the following schemes to construct the main phase grain structure of "core-shell structure" for the preparation of low heavy rare earth and high coercivity RTB system sintered magnets:
[0007] (1) Powder mixing and adding technology
[0008] This technology mainly mixes heavy rare earth-rich modified powder into RTB alloy powder, then makes the modified RTB alloy powder into a magnet, and uses the material migration in the liquid phase sintering process to regulate the surface composition and structure of the main phase grains with the mixed modified powder to construct a "core-shell structure". For example, Chinese patent applications with publication numbers CN1905088A, CN101521069A, CN103106991A, etc. all adopt a similar powder mixing and addition method.
[0009] (2) Powder surface deposition technology
[0010] This technology mainly deposits a heavy rare earth metal-rich film layer on the surface of RTB alloy powder through magnetron sputtering, thermal evaporation, etc., and then makes the RTB alloy powder covered with the heavy rare earth metal film layer into a magnet. The material migration in the liquid phase sintering process is used to realize the regulation of the surface composition and structure of the main phase grains by the heavy rare earth metal film layer to construct a "core-shell structure". For example, Chinese patent applications with publication numbers CN103456452A, CN102280240A, CN103956244A, etc. all adopt similar powder surface deposition methods.
[0011] (3) Grain boundary diffusion technology
[0012] This technology mainly covers the surface of the sintered RTB magnet with a rich heavy rare earth diffusion source and then heats it, using the grain boundary phase as a diffusion channel to introduce the heavy rare earth elements in the rich heavy rare earth diffusion source into the surface layer of the main phase grains to construct a "core-shell structure". For example, Chinese patent applications with publication numbers CN101331566A, CN102682987A, CN102693828A, etc. all use similar grain boundary diffusion methods.
[0013] All three of the aforementioned process technologies can construct a "core-shell structure" to achieve low heavy rare earth elements and high coercivity. However, for grain boundary diffusion techniques, the driving force behind the grain boundary diffusion of the diffusion source material is primarily the concentration gradient of the element. As the diffusion depth increases, the concentration gradient gradually decreases, and the diffusion difficulty gradually increases. Grain boundary diffusion for thicker magnets requires long diffusion heat treatment, resulting in low production efficiency and poor technical versatility, making it unsuitable for industrial application. Therefore, for large-scale RTB-based sintered magnets (thickness greater than 15mm), powder mixing and addition techniques and powder surface deposition techniques are preferred.
[0014] However, the existing powder mixing and addition technology and powder surface deposition technology have many sharp corners in the powder particles. During the liquid phase sintering process, the sharp corners of the powder particles melt and produce a large amount of liquid phase. The heavy rare earth elements in the mixed added heavy rare earth-rich powder or the plated heavy rare earth-rich film layer will melt into the liquid phase. In the subsequent precipitation process, more heavy rare earth elements will be directly precipitated in the low-lying areas on the surface of the powder particles, resulting in a reduction in the amount of heavy rare earth that can be used to diffuse into the surface of the main phase grains, and the performance improvement is not significant. If a higher coercive force improvement is to be achieved, a relatively large amount of heavy rare earth needs to be added, which increases the manufacturing cost. Summary of the Invention
[0015] Based on the shortcomings of the existing powder mixing and addition technology and powder surface deposition technology for preparing RTB-based sintered magnets, the primary purpose of the present invention is to provide a method for preparing RTB-based sintered magnets. By sphericalizing the RTB alloy powder and introducing heavy rare earth elements, a "core-shell structure" is constructed inside the RTB-based sintered magnet. Under the condition of adding a small amount of heavy rare earth elements, the intrinsic coercive force of the RTB-based sintered magnet is significantly improved, and high remanence and maximum magnetic energy product are obtained. In addition, this preparation method can be used for large-sized RTB-based sintered magnets.
[0016] In order to achieve the above object, the present invention adopts the following technical solutions:
[0017] The present invention first provides a method for preparing an RTB-based sintered magnet, comprising the following steps:
[0018] S1. preparing RTB alloy powder;
[0019] S2. Spheroidizing the RTB alloy powder to obtain an alloy powder having a sphericity of not less than 0.8;
[0020] S3, introducing heavy rare earth metal elements into the spherical alloy powder to obtain modified powder;
[0021] S4. preparing the modified powder into an RTB-based sintered magnet.
[0022] In a further embodiment, the composition of the RTB alloy is R x T y B z M a , wherein, 29wt.%≤x≤30.5wt.%, z=1.51-0.02x, 0.4wt.%≤a≤0.7wt.%, y=100-xza;
[0023] R is a rare earth element and must include Nd, with Nd accounting for more than 65% of the total mass of R; T is a transition metal element and must include Fe, with Fe accounting for 98% or more of the total mass of T; B is boron; M is an auxiliary metal element, consisting of any one of Cu, Al, Ga, Zn, Zr, Nb, and Ti, or a mixture of two or more thereof.
[0024] In a further embodiment, the R further comprises Pr and / or Dy, wherein Pr accounts for less than 25% of the total mass of R, and Pr and Nd account for 90% or more of the total mass of R; and Dy accounts for less than 10% of the total mass of R.
[0025] In a further embodiment, the T further comprises Co and / or Ni, wherein Co accounts for less than 2% of the total mass of T and Ni accounts for less than 1% of the total mass of T.
[0026] In a further embodiment, the average particle size of the RTB alloy powder is 2.0 to 2.8 μm.
[0027] In a further embodiment, the RTB alloy powder is made of R2T 14 It is composed of B phase and rare earth-rich phase.
[0028] In a further embodiment, the spheroidization transformation is carried out by mechanical grinding or high-temperature melting.
[0029] In a further embodiment, the mechanical grinding method includes stirring, rolling, collision or friction to grind away sharp edges and corners on the surface of the powder particles and achieve sphericalization of the powder.
[0030] In a further embodiment, after the mechanical grinding step, a powder screening step is also included.
[0031] In a further embodiment, the high temperature melting is to melt the sharp edges and corners on the surface of the powder by heating, thereby achieving sphericalization of the powder.
[0032] In a further embodiment, the heating temperature is 1000-1050°C.
[0033] In a further embodiment, the heating method is resistance heating, induction heating, radio frequency induction plasma heating or laser heating.
[0034] In a further embodiment, after the high-temperature melting step, a crushing and powdering step is also included.
[0035] In a further embodiment, in step S3, the heavy rare earth metal element is introduced by depositing the heavy rare earth metal element on the surface of the spherical alloy powder or mixing the spherical alloy powder with the heavy rare earth metal element powder.
[0036] In a further embodiment, the deposition method is physical vapor deposition or chemical vapor deposition.
[0037] In a further embodiment, the heavy rare earth metal element powder is dysprosium or terbium powder, or dysprosium hydride or terbium hydride powder.
[0038] In a further embodiment, the difference between the average particle size of the heavy rare earth metal element powder and the average particle size of the RTB alloy powder is ≤0.2 μm.
[0039] In a further embodiment, the introduction ratio of the heavy rare earth metal element is 0.5-1.0 wt % of the mass of the alloy powder after spheroidization in step S2.
[0040] In a further embodiment, step S4 includes the steps of oriented pressing, sintering and heat treating the modified powder.
[0041] In a further embodiment, the oriented pressing molding is to mold the modified powder in an oriented magnetic field with an intensity of 1.2T to 1.5T in a protective atmosphere isolated from water and oxygen;
[0042] And / or, the sintering temperature is 1030° C. to 1080° C., and the sintering time is 3 to 5 hours;
[0043] And / or, the heat treatment includes primary heat treatment and secondary heat treatment, the primary heat treatment temperature is 880°C to 920°C, the heat treatment time is 2 to 5 hours, and the secondary heat treatment temperature is 480°C to 560°C, and the heat treatment time is 2 to 5 hours.
[0044] The present invention further provides an RTB-based sintered magnet, which is prepared using the preparation method described above.
[0045] Beneficial effects of the present invention:
[0046] The present invention spheroidizes RTB alloy powder and introduces heavy rare earth metal elements. On the one hand, this reduces the dissolution and precipitation of corners during high-temperature liquid phase sintering, reduces the liquid phase content, increases the concentration of heavy rare earth elements in the liquid phase, and promotes more heavy rare earth elements to form a "shell" with a high anisotropy field on the surface of the main phase grains, thereby improving the intrinsic coercive force of the magnet. On the other hand, it reduces the rotational resistance of the powder particles during the orientation molding process, thereby improving the remanence and maximum magnetic energy product of the magnet.
[0047] The method for preparing the RTB system sintered magnet of the present invention does not involve the grain boundary diffusion of heavy rare earth elements and is not limited by the size of the magnet, and is very suitable for preparing large-sized high-performance RTB system sintered magnets. DETAILED DESCRIPTION
[0048] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and are not to be construed as limiting the present invention.
[0049] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0050] A first aspect of the present invention provides a method for preparing an RTB-based sintered magnet, comprising the following steps:
[0051] S1. preparing RTB alloy powder;
[0052] S2. Spheroidizing the RTB alloy powder to obtain an alloy powder having a sphericity of not less than 0.8;
[0053] S3, introducing heavy rare earth metal elements into the spherical alloy powder to obtain modified powder;
[0054] S4. preparing the modified powder into an RTB-based sintered magnet.
[0055] In the present invention, by optimizing the composition and content of R, T, and M in the RTB alloy powder, the relationship between the R content and the B content, and the structure of the RTB alloy, it is possible to ensure that the RTB alloy has sufficient R2T 14 B phase, an appropriate amount of rare earth-rich phase and a trace amount of modifying element M. These phases and elements can ensure the high performance of the final RTB magnet.
[0056] Preferably, in some specific implementation cases of the present invention, the composition of the RTB alloy powder is R x T y B z M a , wherein x, y, z and a represent the mass percentages of elements R, T, B and M, respectively. In an embodiment of the present invention, 29wt.%≤x≤30.5wt.%, z=1.51-0.02x, 0.4wt.%≤a≤0.7wt.%, y=100-xza.
[0057] In the present invention, R is a rare earth element and must contain Nd, with Nd accounting for more than 65% of the total mass of R. In some embodiments of the present invention, R further contains Pr and / or Dy, wherein Pr accounts for less than 25% of the total mass of R, Pr and Nd account for more than 90% of the mass of R, and Dy accounts for less than 10% of the total mass of R.
[0058] In the present invention, T is a transition metal element and must contain Fe, with Fe accounting for more than 98% of the total mass of T. In some embodiments of the present invention, T further contains Co and / or Ni, wherein Co accounts for less than 2% of the total mass of T and Ni accounts for 1% or less of the total mass of T.
[0059] In the present invention, B is boron element.
[0060] In the present invention, M is an auxiliary metal element, which is composed of any one of Cu, Al, Ga, Zn, Zr, Nb, and Ti, or a mixture of two or more thereof, wherein Cu accounts for R x T y B z M a Less than 0.2% of the total mass of the alloy, Al accounts for R x T y B z M a Less than 0.1% of the total mass of the alloy, Ga accounts for R x T y B z M a Less than 0.2% of the total mass of the alloy, Zn accounts for R x T y B z M a Less than 0.1% of the total mass of the alloy, Zr, Nb and Ti account for R x T y B z M a Less than 0.2% of the total mass of the alloy.
[0061] In one embodiment of the present invention, the average particle size of the RTB-based alloy powder is 2.0 to 2.8 μm.
[0062] Furthermore, the RTB alloy powder of the present invention is composed of R2T 14 B phase and rare earth-rich phase, and can be prepared by methods known in the art. In one embodiment of the present invention, the RTB alloy powder is prepared by crushing and powdering RTB alloy strips or alloy blocks, wherein the RTB alloy strips or alloy blocks are composed of R2T 14The RTB alloy is composed of a main phase of columnar crystals and a rare earth-rich phase located between the main phases. The preparation method of the RTB alloy ribbon or ingot herein is not particularly limited and can be carried out using processes well known in the art, such as a melting-rapid solidification process, in which the prepared raw materials are mixed according to their composition, fully melted, and then rapidly solidified into an alloy ribbon or ingot. Specific process conditions and parameters can be adjusted and confirmed based on methods known in the art and will not be elaborated here.
[0063] The spheroidization mentioned herein refers to removing sharp edges and corners on the surface of the RTB alloy powder by a certain method, thereby obtaining a powder with high sphericity (sphericity not less than 0.8). In the present invention, the specific transformation method can be mechanical grinding or high-temperature melting.
[0064] In some embodiments of the present invention, the transformation method is mechanical grinding. Specifically, the sharp edges and corners on the surface of the powder particles are ground off by stirring, rolling, collision, friction, etc. to achieve the sphericalization of the powder. Among them, the stirring refers to a high-speed rotating metal blade that stirs and cuts off the sharp corners on the surface of the powder, such as a wall breaker, and the preferred rotation speed is above 1000rpm; the rolling refers to placing the powder between two relatively moving and rough hard surfaces, and applying a force that brings the two surfaces closer to each other while the two surfaces move relative to each other, thereby crushing the powder particles, such as a stone mill or mortar; the collision refers to accelerating the powder to a certain speed, and then colliding it vertically or nearly vertically against the surface of a fixed and hard object, using the impact force to make the sharp corners fall off; the friction is to accelerate the powder and collide it with a fixed, hard and rough surface at a certain angle (generally less than 45°), skimming the surface at a certain angle to form friction, thereby grinding off the sharp edges and corners.
[0065] It should be noted that, in order to remove the ultrafine powder generated by grinding during the mechanical grinding process, the mechanical grinding step also includes a powder screening step.
[0066] In other embodiments of the present invention, the transformation method involves high-temperature melting, which involves melting the sharp edges on the powder surface through heating, thereby achieving powder sphericity. The process then utilizes a melting-flow-precipitation process to melt the sharp edges on the powder surface, allowing the powder to flow under the action of surface tension and reprecipitate in depressions on the powder surface. It should be noted that the heating temperature must be strictly controlled to melt only the sharp edges on the powder particle surface and not completely melt the entire powder particle.
[0067] In some specific embodiments of the present invention, the heating temperature is 1000-1050° C.; the heating method can be performed in a manner known in the art, such as resistance heating, induction heating, radio frequency induction plasma heating or laser heating.
[0068] It should be noted that, in order to prevent the adhesion between powder particles during the high-temperature melting and spheroidization process, the high-temperature melting step also includes a crushing and powdering step.
[0069] The heavy rare earth metal elements described herein refer to heavy rare earth metals commonly used in the art, such as at least one of dysprosium (Dy) and terbium (Tb).
[0070] The method of introducing the heavy rare earth metal element described herein may be to deposit the heavy rare earth metal element on the surface of the alloy powder in step S2, or to mix the alloy powder after spherical transformation in step S2 with the heavy rare earth metal element powder;
[0071] The surface deposition method is physical vapor deposition or chemical vapor deposition well known in the art, and specific examples include evaporation, sputtering, ion beam deposition, thermal CVD, plasma enhanced CVD, and the like.
[0072] Furthermore, the heavy rare earth metal element powder used in the powder mixing may be not only dysprosium or terbium powder, but also dysprosium hydride or terbium hydride powder.
[0073] In the present invention, the introduction ratio of the heavy rare earth metal element is 0.5-1.0wt% of the mass of the alloy powder in step S2. The preparation method of the present invention has significant advantages in that the coercive force of the magnet is improved by introducing a small amount of heavy rare earth metal elements.
[0074] Furthermore, the process of preparing the mixed powder into an RTB-based sintered magnet in step S4 described herein is a process well known in the art, specifically comprising the steps of oriented pressing, sintering, and heat treating the mixed powder.
[0075] In some specific embodiments of the present invention, the oriented pressing molding is to mold the mixed powder in an oriented magnetic field with an intensity of 1.2T to 1.5T in a protective atmosphere that isolates water and oxygen, wherein the protective atmosphere described in this article refers to an inert or inactive gas commonly used in the art, such as nitrogen, rare gas (helium, argon, etc.); the condition for isolating water and oxygen is preferably an oxygen content less than 100ppm and a water content less than 10ppm.
[0076] The sintering temperature is 1030° C. to 1080° C., and the sintering time is 3 to 5 hours.
[0077] The purpose of the heat treatment is to improve the magnetic properties of the sintered magnet through heat treatment. The heat treatment temperature, time, etc. can adopt known conditions. In some specific embodiments of the present invention, it includes primary heat treatment and secondary heat treatment. The primary heat treatment temperature is 880℃~920℃, and the heat treatment time is 2~5 hours. The secondary heat treatment temperature is 480℃~560℃, and the heat treatment time is 2~5 hours.
[0078] A second aspect of the present invention provides an RTB-based sintered magnet produced using the preparation method described above. This method can produce a large-sized RTB-based sintered magnet with dimensions exceeding 15 mm in all three dimensions. This large-sized RTB-based sintered magnet exhibits high magnetic properties, with an intrinsic coercivity exceeding 18 kOe, a maximum magnetic energy product exceeding 45 MGOe, and a sum of the intrinsic coercivity (in kOe) and the maximum magnetic energy product (in MGOe) exceeding 67.
[0079] The present invention is described below by means of specific examples. It should be noted that the following specific examples are for illustrative purposes only and do not limit the scope of the present invention in any way. In addition, unless otherwise specified, methods without specific conditions or steps are conventional methods, and the reagents and materials used are all commercially available.
[0080] Example 1
[0081] This embodiment provides a method for preparing an RTB-based sintered magnet, and the specific steps are as follows:
[0082] (1) Preparation of RTB alloy powder
[0083] The RTB alloy ribbon was prepared by melting-rapid solidification process. The RTB alloy ribbon was composed of R2T with an average width of 2.6 μm. 14 B columnar crystal main phase and rare earth-rich phase located between the columnar crystal main phase, the composition is Pr 7.5 Nd 21.5 Dy1Fe 68.49 Cu 0.15 Al 0.1 Ga 0.2 Ti 0.15 B 0.91 (wt.%);
[0084] The RTB alloy ribbon is crushed into RTB alloy powder F with an average particle size of 2.5 μm by hydrogen crushing + air flow grinding process. 10 .
[0085] (2) Spheroidization of alloy powder
[0086] The RTB alloy powder was sphericalized by high-speed rolling and mixing, and the sharp edges and corners on the surface of the powder particles were ground off. The powder after high-speed rolling and mixing was sieved to remove the ultrafine powder (i.e., the sharp corners ground off) produced during the high-speed rolling and mixing process, and a powder F with a sphericity of 0.81 was obtained. 11 .
[0087] (3) Introduction of heavy rare earth elements
[0088] Alloy powder F after spherical transformation 11 0.8 wt.% metal Dy film was deposited on the surface to obtain modified powder F 12 .
[0089] (4) Preparation of sintered magnets
[0090] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the modified powder F was quenched in a 1.4T orientation magnetic field. 12 The mold is pressed to produce a green compact with dimensions greater than 21 mm in length, width and height. The green compact is then sintered at 1050°C for 4 hours, subjected to a primary heat treatment at 880°C for 3 hours, and a secondary heat treatment at 500°C for 4 hours to produce an RTB sintered magnet with dimensions greater than 15 mm in length, width and height.
[0091] Comparative Example 1
[0092] This comparative example discloses a method for preparing a RTB-based sintered magnet, which adopts the same method as Example 1, except that the RTB-based alloy powder F is not subjected to the sintering. 10 The spheroidization treatment was performed, and no metal Dy film was deposited on the surface of the alloy powder. Other steps and process conditions were the same as those in Example 1.
[0093] The preparation method of the RTB-based sintered magnet in this comparative example comprises the following specific steps:
[0094] (1) Preparation of RTB alloy powder
[0095] The RTB alloy ribbon was prepared by melting-rapid solidification process. The RTB alloy ribbon was composed of R2T with an average width of 2.6 μm. 14 B columnar crystal main phase and rare earth-rich phase located between the columnar crystal main phase, the composition is Pr 7.5 Nd 21.5 Dy1Fe 68.49 Cu 0.15 Al 0.1 Ga 0.2 Ti 0.15 B 0.91 (wt.%);
[0096] The RTB alloy ribbon is crushed into RTB alloy powder F with an average particle size of 2.5 μm by hydrogen crushing + air flow grinding process. 10 .
[0097] (2) Preparation of sintered magnets
[0098] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the alloy powder F was oriented in a 1.4T magnetic field. 10 The mold is pressed to produce a green compact with dimensions greater than 21 mm in length, width and height. The green compact is then sintered at 1050°C for 4 hours, subjected to a primary heat treatment at 880°C for 3 hours, and a secondary heat treatment at 500°C for 4 hours to produce an RTB sintered magnet with dimensions greater than 15 mm in length, width and height.
[0099] Comparative Example 2
[0100] This comparative example discloses a method for preparing a RTB-based sintered magnet, which adopts the same method as Example 1, except that the RTB-based alloy powder F is not subjected to the sintering. 10 The other steps and process conditions are the same as those in Example 1.
[0101] The preparation method of the RTB sintered magnet in this comparative example comprises the following specific steps:
[0102] (1) Preparation of RTB alloy powder
[0103] The RTB alloy ribbon was prepared by melting-rapid solidification process. The RTB alloy ribbon was composed of R2T with an average width of 2.6 μm. 14 B columnar crystal main phase and rare earth-rich phase located between the columnar crystal main phase, the composition is Pr 7.5 Nd 21.5 Dy1Fe 68.49 Cu 0.15 Al 0.1 Ga 0.2 Ti 0.15 B 0.91 (wt.%);
[0104] The RTB alloy ribbon is crushed into RTB alloy powder F with an average particle size of 2.5 μm by hydrogen crushing + air flow grinding process. 10 .
[0105] (2) Introduction of heavy rare earth elements
[0106] In RTB alloy powder F 10 0.8 wt.% metal Dy film was deposited on the surface to obtain modified powder F12 '.
[0107] (3) Preparation of sintered magnets
[0108] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the modified powder F was quenched in a 1.4T orientation magnetic field. 12 The green sheets were compression molded to produce green sheets with dimensions greater than 21 mm in length, width and height. The green sheets were then sintered at 1050°C for 4 hours, subjected to a primary heat treatment at 880°C for 3 hours, and a secondary heat treatment at 500°C for 4 hours to produce RTB sintered magnets with dimensions greater than 15 mm in length, width and height.
[0109] Example 2
[0110] This embodiment provides a method for preparing an RTB-based sintered magnet, and the specific steps are as follows:
[0111] (1) Preparation of RTB alloy powder:
[0112] The RTB alloy ribbon was prepared by melting-rapid solidification process. The RTB alloy ribbon was composed of R2T with an average width of 2.9 μm. 14 B is composed of a columnar crystal main phase and a rare earth-rich phase located between the columnar crystal main phases, and its composition is Pr6Nd 23 Dy 0.5 Fe 68.18 Co 0.5 Ni 0.5 Cu 0.05 Al 0.07 Ga 0.05 Zn 0.08 Nb 0.05 Zr 0.1 B 0.92 (wt.%);
[0113] The RTB alloy ribbon was crushed into RTB alloy powder F with an average particle size of 2.3 μm by hydrogen crushing + air flow grinding process. 20 .
[0114] (2) Spheroidization of alloy powder
[0115] The RTB alloy powder was spheroidized by radio frequency induction plasma heating at 1020℃ to melt the sharp edges on the surface of the powder particles. The spheroidized powder was then jet milled to prevent adhesion between the powder particles. The powder F with a sphericity of 0.85 was obtained. 21 .
[0116] (3) Introduction of heavy rare earth elements
[0117] Alloy powder F after spherical transformation 21 0.6 wt.% of terbium hydride powder was mixed into the modified powder F. 22 .
[0118] (4) Preparation of sintered magnets
[0119] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the modified powder F was oriented in a 1.5T magnetic field. 22 The mold is pressed to produce a green compact with dimensions greater than 25 mm in length, width and height. The green compact is then sintered at 1030°C for 5 hours, subjected to a primary heat treatment at 900°C for 5 hours, and a secondary heat treatment at 480°C for 2 hours to produce an RTB sintered magnet with dimensions greater than 17.5 mm in length, width and height.
[0120] Comparative Example 3
[0121] This comparative example discloses a method for preparing a RTB-based sintered magnet, which adopts the same method as Example 2, except that the RTB-based alloy powder F is not subjected to the sintering. 20 The spheroidization treatment was performed, and no terbium hydride powder was mixed into the alloy powder. Other steps and process conditions were the same as those in Example 2.
[0122] The preparation method of the RTB-based sintered magnet in this comparative example comprises the following specific steps:
[0123] (1) Preparation of RTB alloy powder:
[0124] The RTB alloy ribbon was prepared by melting-rapid solidification process. The RTB alloy ribbon was composed of R2T with an average width of 2.9 μm. 14 B is composed of a columnar crystal main phase and a rare earth-rich phase located between the columnar crystal main phases, and its composition is Pr6Nd 23 Dy 0.5 Fe 68.18 Co 0.5 Ni 0.5 Cu 0.05 Al 0.07 Ga 0.05 zn 0.08 Nb 0.05 Zr 0.1 B 0.92 (wt.%);
[0125] The RTB alloy ribbon was crushed into RTB alloy powder F with an average particle size of 2.3 μm by hydrogen crushing + air flow grinding process. 20 .
[0126] (2) Preparation of sintered magnets
[0127] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, RTB alloy powder F was oriented in a 1.5T magnetic field. 20 The mold is pressed to produce a green compact with dimensions greater than 25 mm in length, width and height. The green compact is then sintered at 1030°C for 5 hours, subjected to a primary heat treatment at 900°C for 5 hours, and a secondary heat treatment at 480°C for 2 hours to produce an RTB sintered magnet with dimensions greater than 17.5 mm in length, width and height.
[0128] Comparative Example 4
[0129] This comparative example discloses a method for preparing a RTB-based sintered magnet, which adopts the same method as Example 2, except that the RTB-based alloy powder F is not subjected to the sintering. 20 The other steps and process conditions are the same as those in Example 2.
[0130] The preparation method of the RTB sintered magnet in this comparative example comprises the following specific steps:
[0131] (1) Preparation of RTB alloy powder:
[0132] The RTB alloy ribbon was prepared by melting-rapid solidification process. The RTB alloy ribbon was composed of R2T with an average width of 2.9 μm. 14 B is composed of a columnar crystal main phase and a rare earth-rich phase located between the columnar crystal main phases, and its composition is Pr6Nd 23 Dy 0.5 Fe 68.18 Co 0.5 Ni 0.5 Cu 0.05 Al 0.07 Ga 0.05 zn 0.08 Nb 0.05 Zr 0.1 B 0.92 (wt.%);
[0133] The RTB alloy ribbon was crushed into RTB alloy powder F with an average particle size of 2.3 μm by hydrogen crushing + air flow grinding process. 20 .
[0134] (2) Introduction of heavy rare earth elements
[0135] In alloy powder F 20 0.6 wt.% of terbium hydride powder was mixed into the modified powder F. 22 '.
[0136] (4) Preparation of sintered magnets
[0137] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the modified powder F was oriented in a 1.5T magnetic field. 22 The green sheet is compression molded to produce a green sheet with dimensions greater than 25 mm in length, width and height. The green sheet is then sintered at 1030°C for 5 hours, subjected to a primary heat treatment at 900°C for 5 hours, and a secondary heat treatment at 480°C for 2 hours to produce an RTB sintered magnet with dimensions greater than 17.5 mm in length, width and height.
[0138] Example 3
[0139] This embodiment provides a method for preparing an RTB-based sintered magnet, and the specific steps are as follows:
[0140] (1) Preparation of RTB alloy powder
[0141] The RTB alloy ribbon is designed and manufactured by the melting-rapid solidification process. The RTB alloy ribbon is composed of R2T with an average width of 3.1μm. 14 B columnar crystal main phase and rare earth rich phase located between the columnar crystal main phase, the composition of which is Pr5Nd 22 Dy2Fe 68.29 Co 1.3 Cu 0.2 Ga 0.1 Zr 0.08 Ti 0.1 B 0.93 (wt.%);
[0142] The RTB alloy ribbon was crushed into RTB alloy powder F with an average particle size of 2.8 μm by hydrogen crushing + air flow grinding process. 30 .
[0143] (2) Spheroidization of alloy powder
[0144] The RTB alloy powder F was subjected to high pressure air flow collision. 03 The powder was sphericalized and sharp corners on the surface of the powder particles were ground off. The powder was sieved after the high-pressure airflow collision to remove the sharp corners of the powder particles that fell off during the high-pressure airflow collision. The powder F with a sphericity of 0.82 was obtained. 31 .
[0145] (3) Introduction of heavy rare earth elements
[0146] Alloy powder F after spherical transformation 31 A 1.0 wt.% Dy layer was deposited on the surface to obtain modified powder F. 32 .
[0147] (4) Preparation of sintered magnets
[0148] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the modified powder F was quenched in a 1.2T orientation magnetic field. 32 The mold is pressed to produce a green compact with dimensions greater than 30 mm in length, width and height. The green compact is then sintered at 1080°C for 3 hours, subjected to primary heat treatment at 920°C for 2 hours, and secondary heat treatment at 530°C for 5 hours to produce an RTB sintered magnet with dimensions greater than 21 mm in length, width and height.
[0149] Comparative Example 5
[0150] This comparative example discloses a method for preparing a RTB-based sintered magnet, which adopts the same method as Example 3, except that the RTB-based alloy powder F is not subjected to the sintering. 30 The spheroidization treatment was performed, and no 1.0 wt.% Dy layer was deposited on the surface of the alloy powder. The other steps and process conditions were the same as those in Example 2.
[0151] The preparation method of the RTB-based sintered magnet in this comparative example comprises the following specific steps:
[0152] (1) Preparation of RTB alloy powder
[0153] The RTB alloy ribbon is designed and manufactured by the melting-rapid solidification process. The RTB alloy ribbon is composed of R2T with an average width of 3.1μm. 14 B columnar crystal main phase and rare earth rich phase located between the columnar crystal main phase, the composition of which is Pr5Nd 22 Dy2Fe 68.29 Co 1.3 Cu 0.2 Ga 0.1 Zr 0.08 Ti 0.1 B 0.93 (wt.%);
[0154] The RTB alloy ribbon was crushed into RTB alloy powder F with an average particle size of 2.8 μm by hydrogen crushing + air flow grinding process. 30 .
[0155] (2) Preparation of sintered magnets
[0156] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, RTB alloy powder F was oriented in a 1.2T magnetic field. 30The mold is pressed to produce a green compact with dimensions greater than 30 mm in length, width and height. The green compact is then sintered at 1080°C for 3 hours, subjected to primary heat treatment at 920°C for 2 hours, and secondary heat treatment at 530°C for 5 hours to produce an RTB sintered magnet with dimensions greater than 21 mm in length, width and height.
[0157] Comparative Example 6
[0158] This comparative example discloses a method for preparing a RTB-based sintered magnet, which adopts the same method as Example 3, except that the RTB-based alloy powder F is not subjected to the sintering. 30 The other steps and process conditions are the same as those in Example 3.
[0159] The preparation method of the RTB-based sintered magnet in this comparative example comprises the following specific steps:
[0160] (1) Preparation of RTB alloy powder
[0161] The RTB alloy ribbon is designed and manufactured by the melting-rapid solidification process. The RTB alloy ribbon is composed of R2T with an average width of 3.1μm. 14 B columnar crystal main phase and rare earth rich phase located between the columnar crystal main phase, the composition of which is Pr5Nd 22 Dy2Fe 68.29 Co 1.3 Cu 0.2 Ga 0.1 Zr 0.08 Ti 0.1 B 0.93 (wt.%);
[0162] The RTB alloy ribbon was crushed into RTB alloy powder F with an average particle size of 2.8 μm by hydrogen crushing + air flow grinding process. 30 .
[0163] (2) Introduction of heavy rare earth elements
[0164] In alloy powder F 30 A 1.0 wt.% Dy layer was deposited on the surface to obtain modified powder F. 32 '.
[0165] (4) Preparation of sintered magnets
[0166] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the modified powder F was quenched in a 1.2T orientation magnetic field. 32The green sheets were compression molded to produce green sheets with dimensions greater than 30 mm in length, width and height. The green sheets were then sintered at 1080°C for 3 hours, subjected to a primary heat treatment at 920°C for 2 hours, and a secondary heat treatment at 530°C for 5 hours to produce RTB sintered magnets with dimensions greater than 21 mm in length, width and height.
[0167] Example 4
[0168] This embodiment provides a method for preparing an RTB-based sintered magnet, and the specific steps are as follows:
[0169] (1) Preparation of RTB alloy powder
[0170] The RTB alloy ribbon is designed and manufactured by the melting-rapid solidification process. The RTB alloy ribbon is composed of R2T with an average width of 3.4μm. 14 B columnar crystal main phase and rare earth rich phase located between the columnar crystal main phase, the composition of which is Pr4Nd 23.5 Dy3Fe 67.3 Ni 0.6 Cu 0.15 Al 0.1 Ga 0.15 Zn 0.1 Zr 0.05 Ti 0.1 Nb 0.05 B 0.9 (wt.%);
[0171] The RTB alloy ribbon is crushed into RTB alloy powder F with an average particle size of 2.0 μm by hydrogen crushing + air flow grinding process. 40 .
[0172] (2) Spheroidization of alloy powder
[0173] Laser heating of RTB alloy powder F 04 The spherical transformation was carried out at a heating temperature of 1040°C to melt the sharp edges on the surface of the powder particles. The powder after spherical transformation was subjected to air flow milling to prevent adhesion between the powder particles, and a powder F with a sphericity of 0.83 was obtained. 41 .
[0174] (3) Introduction of heavy rare earth elements
[0175] Alloy powder F after spherical transformation 41 0.5 wt.% of terbium hydride powder was mixed into the modified powder F. 42 .
[0176] (4) Preparation of sintered magnets
[0177] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the modified powder F was oriented in a 1.3T magnetic field. 42 The mold is pressed to produce a green compact with dimensions greater than 35 mm in length, width and height. The green compact is then sintered at 1060°C for 4 hours, subjected to a primary heat treatment at 900°C for 4 hours, and a secondary heat treatment at 560°C for 3 hours to produce an RTB sintered magnet with dimensions greater than 25 mm in length, width and height.
[0178] Comparative Example 7
[0179] This comparative example discloses a method for preparing a RTB-based sintered magnet, which adopts the same method as Example 4, except that the RTB-based alloy powder F is not subjected to the sintering. 40 The spheroidization treatment was performed, and the 0.5 wt.% terbium hydride powder was not mixed into the alloy powder. The other steps and process conditions were the same as those in Example 4.
[0180] The preparation method of the RTB-based sintered magnet in this comparative example comprises the following specific steps:
[0181] (1) Preparation of RTB alloy powder
[0182] The RTB alloy ribbon is designed and manufactured by the melting-rapid solidification process. The RTB alloy ribbon is composed of R2T with an average width of 3.4μm. 14 B columnar crystal main phase and rare earth rich phase located between the columnar crystal main phase, the composition of which is Pr4Nd 23.5 Dy3Fe 67.3 Ni 0.6 Cu 0.15 Al 0.1 Ga 0.15 Zn 0.1 Zr 0.05 Ti 0.1 Nb 0.05 B 0.9 (wt.%);
[0183] The RTB alloy ribbon is crushed into RTB alloy powder F with an average particle size of 2.0 μm by hydrogen crushing + air flow grinding process. 40 .
[0184] (2) Preparation of sintered magnets
[0185] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, RTB alloy powder F was oriented in a 1.3T magnetic field. 40The mold is pressed to produce a green compact with dimensions greater than 35 mm in length, width and height. The green compact is then sintered at 1060°C for 4 hours, subjected to a primary heat treatment at 900°C for 4 hours, and a secondary heat treatment at 560°C for 3 hours to produce an RTB sintered magnet with dimensions greater than 25 mm in length, width and height.
[0186] Comparative Example 8
[0187] This comparative example discloses a method for preparing a RTB-based sintered magnet, which adopts the same method as Example 4, except that the RTB-based alloy powder F is not subjected to the sintering. 40 The other steps and process conditions are the same as those in Example 4.
[0188] The preparation method of the RTB-based sintered magnet in this comparative example comprises the following specific steps:
[0189] (1) Preparation of RTB alloy powder
[0190] The RTB alloy ribbon is designed and manufactured by the melting-rapid solidification process. The RTB alloy ribbon is composed of R2T with an average width of 3.4μm. 14 B columnar crystal main phase and rare earth rich phase located between the columnar crystal main phase, the composition of which is Pr4Nd 23.5 Dy3Fe 67.3 Ni 0.6 Cu 0.15 Al 0.1 Ga 0.15 Zn 0.1 Zr 0.05 Ti 0.1 Nb 0.05 B 0.9 (wt.%);
[0191] The RTB alloy ribbon is crushed into RTB alloy powder F with an average particle size of 2.0 μm by hydrogen crushing + air flow grinding process. 40 .
[0192] (2) Introduction of heavy rare earth elements
[0193] In alloy powder F 40 0.5 wt.% of terbium hydride powder was mixed into the modified powder F. 42 '.
[0194] (3) Preparation of sintered magnets
[0195] In a nitrogen protection environment with an oxygen content of less than 100ppm and a water content of less than 10ppm, the modified powder F was oriented in a 1.3T magnetic field. 42The green sheets were compression molded to produce green sheets with dimensions greater than 35 mm in length, width and height. The green sheets were then sintered at 1060°C for 4 hours, subjected to a primary heat treatment at 900°C for 4 hours, and a secondary heat treatment at 560°C for 3 hours to produce RTB sintered magnets with dimensions greater than 25 mm in length, width and height.
[0196] Performance Testing
[0197] The main magnetic properties (remanence, intrinsic coercivity, and maximum energy product) of the RTB-based sintered magnets in Examples 1-4 and Comparative Examples 1-8 were tested in accordance with the "Magnetic Test Methods for Permanent Magnet (Hard Magnetic) Materials" (GB / T 3217-2013). The results are shown in Table 1.
[0198] Table 1 Magnetic properties of R-TB sintered magnets
[0199]
[0200] The test results in Table 1 show that, compared with the comparative examples (Comparative Examples 1, 3, 5, and 7) in which no heavy rare earth powder was added / heavy rare earth film layers were deposited and no spherical transformation was performed, the RTB-based sintered magnets (Examples 1 to 4) prepared by the process of the present invention have slightly lower remanence and maximum energy product, and significantly improved intrinsic coercivity, with the intrinsic coercivity (kOe) + maximum energy product (MGOe) increasing by more than 3.50. Compared with the comparative examples (Comparative Examples 2, 4, 6, and 8) in which heavy rare earth powder was added / heavy rare earth film layers were deposited but no spherical transformation was performed, the RTB-based sintered magnets (Examples 1 to 4) prepared by the process of the present invention have slightly higher remanence and maximum energy product, and significantly improved intrinsic coercivity, with the intrinsic coercivity (kOe) + maximum energy product (MGOe) increasing by more than 1.79.
[0201] The above results show that the preparation method of the present invention can effectively achieve the significant improvement of the intrinsic coercivity of RTB sintered magnets under the condition of adding a small amount of heavy rare earth elements, while obtaining high remanence and maximum magnetic energy product, which is very suitable for large-sized RTB sintered magnets.
[0202] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0203] The above-described embodiments merely illustrate several implementations of the present invention, and while their descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art would be able to make numerous variations and improvements without departing from the spirit of the present invention, all of which fall within the scope of protection of the present invention. Therefore, the scope of protection of the patent for this invention shall be determined by the appended claims.
Claims
1. A method for preparing a RTB based sintered magnet, characterized in that: The following steps are involved: S1, preparing RTB alloy powder; S2, spheroidizing the RTB alloy powder to obtain an alloy powder having a sphericity of not less than 0.8; S3, introducing heavy rare earth metal elements into the alloy powder after spheroidization to obtain modified powder; S4. preparing the modified powder into an RTB-based sintered magnet.
2. The method for preparing a RTB based sintered magnet according to claim 1, wherein: The composition of the RTB alloy is R x T y B z M a , wherein 29wt.%≤x≤30.5wt.%, z=1.51-0.02x, 0.4wt.%≤a≤0.7wt.%, y=100-xza; R is a rare earth element and must contain Nd, which accounts for more than 65% of the total mass of R; T is a transition metal element and must contain Fe, which accounts for 98% or more of the total mass of T; B is boron; M is an auxiliary metal element, which is composed of any one of Cu, Al, Ga, Zn, Zr, Nb, and Ti, or a mixture of two or more thereof; Preferably, the R further comprises Pr and / or Dy, wherein Pr accounts for less than 25% of the total mass of R, and Pr and Nd account for 90% or more of the total mass of R; Dy accounts for less than 10% of the total mass of R; Preferably, the T further comprises Co and / or Ni, wherein Co accounts for less than 2% of the total mass of T, and Ni accounts for less than 1% of the total mass of T.
3. The method for preparing a RTB based sintered magnet according to claim 1, wherein: The average particle size of the RTB alloy powder is 2.0 to 2.8 μm.
4. The method for preparing a RTB based sintered magnet according to claim 1, wherein: The RTB alloy powder is composed of R2T 14 It is composed of phase B and rare earth-rich phase.
5. The method for preparing a RTB based sintered magnet according to claim 1, wherein: The spheroidization transformation method is mechanical grinding or high-temperature melting; Preferably, the mechanical grinding method includes stirring, rolling, collision or friction to grind away the sharp edges and corners on the surface of the powder particles to achieve sphericalization of the powder; Preferably, after the mechanical grinding step, a powder screening step is also included; Preferably, the high temperature melting is to melt the sharp edges and corners on the surface of the powder by heating, thereby achieving sphericalization of the powder; Preferably, the heating temperature is 1000-1050°C; Preferably, the heating method is resistance heating, induction heating, radio frequency induction plasma heating or laser heating; Preferably, after the high-temperature melting step, a crushing and powdering step is also included.
6. The method for preparing a RTB based sintered magnet according to claim 1, wherein: In step S3, the heavy rare earth metal element is introduced by depositing the heavy rare earth metal element on the surface of the alloy powder after spherical transformation or mixing the alloy powder after spherical transformation with heavy rare earth metal element powder; Preferably, the deposition method is physical vapor deposition or chemical vapor deposition; Preferably, the heavy rare earth metal element powder is dysprosium or terbium powder, or dysprosium hydride or terbium hydride powder; Preferably, the difference between the average particle size of the heavy rare earth metal element powder and the average particle size of the RTB series alloy powder is ≤0.2 μm.
7. The method for preparing a RTB based sintered magnet according to claim 1, wherein: The introduction ratio of the heavy rare earth metal element is 0.5-1.0wt% of the mass of the alloy powder after spheroidization in step S2.
8. The method for preparing a RTB based sintered magnet according to claim 1, wherein: Step S4 includes the steps of oriented pressing, sintering and heat treating the modified powder.
9. The method for preparing a RTB based sintered magnet according to claim 8, characterized in that: The oriented pressing molding is to mold the modified powder in an oriented magnetic field with a strength of 1.2T to 1.5T in a protective atmosphere isolated from water and oxygen; And / or, the sintering temperature is 1030°C to 1080°C, and the sintering time is 3 to 5 hours; And / or, the heat treatment includes primary heat treatment and secondary heat treatment, the primary heat treatment temperature is 880°C to 920°C, the heat treatment time is 2 to 5 hours, and the secondary heat treatment temperature is 480°C to 560°C, and the heat treatment time is 2 to 5 hours.
10. An RTB based sintered magnet, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method for improving coercive force of neodymium-iron-boron sintered permanent magnet
CN110911149A
Magnetic material and preparation method and application thereof
CN114284016A
Neodymium-iron-boron magnet and preparation method thereof
CN116844811A
Preparation method of radiation orientation magnetic ring and radiation orientation magnetic ring
CN117174475A
R-t-b based permanent magnet material, preparation method therefor and use thereof
US20240194379A1