Photosensitive resin composition for partition wall, cured product, and method for producing partition wall

By adding unsaturated groups, dendritic polymers and photopolymerization initiators to the resin composition, and adopting specific manufacturing methods, the problems of optical density, shape and ink repellency of the partition walls in the prior art are solved, and efficient Barrier fabrication for a variety of electronic component applications.

CN111103760BActive Publication Date: 2024-10-18NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN201911021895.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-25
Publication Date
2024-10-18
Estimated Expiration
2039-10-25

AI Technical Summary

Technical Problem

When using a resin composition to form a partition wall in the prior art, it is difficult to meet the conditions of optical density, cross-sectional shape, and no shrinkage difference during hardening, and the resin composition has poor ink repellency and pattern shape.

Method used

A manufacturing method using a photosensitive resin composition for partition walls containing a photosensitive resin containing an unsaturated group, a dendritic polymer and a photopolymerization initiator, and controlling the ratio and processing conditions of the resin composition through ultraviolet exposure and alkaline development , to achieve excellent light shielding, surface appearance and pattern shape.

Benefits of technology

A partition wall with excellent light-shielding properties, good surface appearance, fine pattern shape and good surface ink repellency is realized, which is suitable for the manufacture of color filters and other electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002247484290000031
    Figure BDA0002247484290000031
  • Figure BDA0002247484290000041
    Figure BDA0002247484290000041
  • Figure BDA0002247484290000071
    Figure BDA0002247484290000071
Patent Text Reader

Abstract

The present invention provides a photosensitive resin composition for partition walls having a desired optical density, a desired cross-sectional shape, and no shrinkage difference during curing, a cured product, and a method for producing the partition walls. The photosensitive resin composition for partition walls of the present invention is a photosensitive resin composition for partition walls comprising a photosensitive resin containing an unsaturated group, a dendritic polymer having two or more ethylene polymerizable groups at the end, and a photopolymerization initiator. The partition walls of the present invention are cured products obtained by curing the photosensitive resin composition for partition walls.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photosensitive resin composition for a partition wall, a cured product obtained by curing the resin composition, and a method for producing a partition wall. Background Art

[0002] In recent years, in the manufacture of organic electroluminescence (EL) elements, quantum dot displays, thin film transistor (TFT) arrays, and color filters including wavelength conversion elements, an inkjet method is used, which does not require exposure and can pattern print organic layers such as pixels by inkjet methods that can apply coloring materials only to the required parts. Here, the inkjet method is a method in which a predetermined amount of ink containing a material of an organic layer is injected into an area surrounded by a partition wall formed on a transparent substrate such as a glass or plastic sheet.

[0003] In the case of inkjet method, when injecting ink into the area surrounded by the partition wall, in order to suppress the ink from flowing into the adjacent area and the ink from adhering to the partition wall, it is necessary to give the partition wall ink-repellent properties. In addition, in order to keep the ink in the partition wall, the partition wall is required to be a thick film. However, as the partition wall thickens, the difference in the cross-linking density relative to the film thickness direction in the exposed part expands, and therefore, it is difficult to obtain a partition wall without wrinkles and in a good shape.

[0004] Patent Document 1 discloses that a black resist to which an acrylic copolymer is added as an alkali-soluble resin can suppress the occurrence of wrinkles in a thick film having a thickness of 1 μm or more.

[0005] Patent Document 2 discloses a dendritic polymer, which is obtained by Michael addition of a small amount of a polyvalent mercapto compound to the ethylenic double bonds of a multifunctional acrylate. Thus, a resin composition containing a multi-branched polymer having flexibility in bending and scratch resistance can be provided. Here, the dendritic polymer is also called a dendrimer or a multi-branched polymer.

[0006] [Prior art literature]

[0007] [Patent Document]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 2007-286478

[0009] [Patent Document 2] International Publication No. 2008 / 47620 Summary of the invention

[0010] [Problems to be solved by the invention]

[0011] Patent Document 1 provides a resin composition that can suppress wrinkles even in a thick film, and Patent Document 2 provides a resin composition that is excellent in flexibility and scratch resistance. However, according to the research of the present inventors, when the partition walls are formed using the resin compositions described in Patent Documents 1 and 2, a partition wall that satisfies all the conditions of a desired optical density, a desired cross-sectional shape, and no shrinkage difference during curing is not obtained.

[0012] The object of the present invention is to provide a partition wall resin composition and a cured product thereof which have a desired optical density, a desired cross-sectional shape and do not produce a shrinkage difference during curing. In addition, the object of the present invention is to provide a method for producing a partition wall using the resin composition.

[0013] [Technical means to solve the problem]

[0014] The photosensitive resin composition for partition walls of the present invention comprises (A) a photosensitive resin containing an unsaturated group, (B) a dendrimer having two or more ethylenically polymerizable groups at the terminals, and (C) a photopolymerization initiator.

[0015] The cured product of the present invention is a cured product obtained by curing the photosensitive resin composition for partition walls.

[0016] The method for manufacturing a partition wall of the present invention comprises: applying the photosensitive resin composition for partition walls, wherein the component (E) is a black pigment or a mixed color organic pigment, on a substrate to form a coating film and drying the coating film; exposing the coating film using an ultraviolet exposure device; and developing the coating film using an alkaline aqueous solution and thermally calcining the coating film. The optical density (OD) of the partition wall is 0.2 / μm to 4.0 / μm.

[0017] In addition, the method for manufacturing the partition wall of the present invention comprises: applying the photosensitive resin composition for the partition wall, wherein the component (E) is a white pigment, on a substrate to form a coating film and drying the coating film; exposing the coating film using an ultraviolet exposure device; and developing the coating film using an alkaline aqueous solution and thermally calcining the coating film. The optical density (OD) of the partition wall is 0.1 / μm to 0.3 / μm.

[0018] [Effects of the Invention]

[0019] According to the present invention, a resin composition for partition walls having excellent light-shielding properties, good surface appearance and pattern shape, and excellent surface ink repellency and a cured product thereof can be provided. In addition, an object of the present invention is to provide a method for producing a partition wall using the resin composition. DETAILED DESCRIPTION

[0020] The present invention will be described in detail below. The photosensitive resin composition for partition walls of the present invention (hereinafter, sometimes simply referred to as a photosensitive resin composition) contains components (A) to (E). Components (A) to (E) will be described below.

[0021] ((A) ingredient)

[0022] The unsaturated group-containing photosensitive resin as the component (A) preferably has a polymerizable unsaturated group and an acidic group for developing alkali solubility in one molecule, and more preferably contains both a polymerizable unsaturated group and a carboxyl group.

[0023] Examples of the photosensitive resin containing unsaturated groups include epoxy (meth) acrylate acid adducts obtained by reacting (meth) acrylic acid with an epoxy compound having two glycidyl ether groups derived from bisphenols (hereinafter referred to as "bisphenol-type epoxy compound") to obtain a compound having a hydroxyl group, and reacting a polycarboxylic acid or its anhydride with the obtained compound having a hydroxyl group. The epoxy compound derived from bisphenols refers to an epoxy compound or its equivalent obtained by reacting bisphenols with epihalohydrins. The photosensitive resin containing unsaturated groups as component (A) has both ethylenic unsaturated double bonds and carboxyl groups, so as a photosensitive resin composition, it can be given excellent photohardening, good developability, patterning characteristics and can bring about the improvement of the physical properties of the light-shielding film. In particular, regarding the patternability of the resin, for example, not only the pixel pattern of thick lines formed when using a negative photomask with a 20μm opening can have good patternability, but also the pixel pattern of thin lines formed when using a negative photomask with a 5μm opening can also have good patternability. In addition, "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid, and means one or both of these.

[0024] The unsaturated group-containing photosensitive resin as the component (A) is preferably a bisphenol-type epoxy compound represented by the general formula (1).

[0025] [Chemistry 1]

[0026]

[0027] In the general formula (1), R 1 , R 2 , R3 and R 4 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a halogen atom; X represents -CO-, -SO 2 -、-C(CF 3 ) 2 -、-Si(CH 3 ) 2 -、-CH 2 -、-C(CH 3 ) 2 -, -O-, a fluorene-9,9-diyl radical represented by the general formula (2) or a single bond; and l is an integer of 0 to 10.

[0028] [Chemistry 2]

[0029]

[0030] The bisphenol type epoxy compound represented by the general formula (1) is an epoxy compound having two glycidyl ether groups obtained by reacting bisphenols with epichlorohydrin. The above reaction is usually accompanied by oligomerization of the diglycidyl ether compound, and therefore includes epoxy compounds having two or more bisphenol skeletons.

[0031] Examples of the bisphenols used in the reaction include bis(4-hydroxyphenyl)ketone, bis(4-hydroxy-3,5-dimethylphenyl)ketone, bis(4-hydroxy-3,5-dichlorophenyl)ketone, bis(4-hydroxyphenyl)sulfone, bis(4-hydroxy-3,5-dimethylphenyl)sulfone, bis(4-hydroxy-3,5-dichlorophenyl)sulfone, bis(4-hydroxyphenyl)hexafluoropropane, bis(4-hydroxy-3,5-dimethylphenyl)hexafluoropropane, bis(4-hydroxy-3 ,5-dichlorophenyl)hexafluoropropane, bis(4-hydroxyphenyl)dimethylsilane, bis(4-hydroxy-3,5-dimethylphenyl)dimethylsilane, bis(4-hydroxy-3,5-dichlorophenyl)dimethylsilane, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3,5-dichlorophenyl)methane, bis(4-hydroxy-3,5-dibromophenyl)methane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl) 2,2-bis(4-hydroxy-3,5-dichlorophenyl)propane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxy-3-chlorophenyl)propane, bis(4-hydroxyphenyl)ether, bis(4-hydroxy-3,5-dimethylphenyl)ether, bis(4-hydroxy-3,5-dichlorophenyl)ether, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9-bis( 9,9-bis(4-hydroxy-3-chlorophenyl)fluorene, 9,9-bis(4-hydroxy-3-bromophenyl)fluorene, 9,9-bis(4-hydroxy-3-fluorophenyl)fluorene, 9,9-bis(4-hydroxy-3-methoxyphenyl)fluorene, 9,9-bis(4-hydroxy-3,5-dimethylphenyl)fluorene, 9,9-bis(4-hydroxy-3,5-dichlorophenyl)fluorene, 9,9-bis(4-hydroxy-3,5-dibromophenyl)fluorene, 4,4'-biphenol, 3,3'-biphenol, etc. Among them, bisphenols having a fluorene-9,9-diyl group are preferred.

[0032] In addition, examples of the (a) acid monoanhydride of a dicarboxylic acid or tricarboxylic acid that reacts with a hydroxyl group in an epoxy (meth)acrylate molecule obtained by reacting such an epoxy compound with (meth)acrylic acid include acid monoanhydrides of chain hydrocarbon dicarboxylic acids or tricarboxylic acids, acid monoanhydrides of alicyclic dicarboxylic acids or tricarboxylic acids, and acid monoanhydrides of aromatic dicarboxylic acids or tricarboxylic acids. Here, examples of acid monoanhydrides of chain hydrocarbon dicarboxylic acids or tricarboxylic acids include acid monoanhydrides of succinic acid, acetylsuccinic acid, maleic acid, adipic acid, itaconic acid, azelaic acid, citramalic acid, malonic acid, glutaric acid, citric acid, tartaric acid, oxoglutaric acid, pimelic acid, sebacic acid, suberic acid, diglycolic acid, and the like. Furthermore, acid monoanhydrides of dicarboxylic acids or tricarboxylic acids into which any substituent is introduced are included. In addition, examples of the acid monoanhydride of alicyclic dicarboxylic acids or tricarboxylic acids include acid monoanhydrides of cyclobutane dicarboxylic acid, cyclopentane dicarboxylic acid, hexahydrophthalic acid, tetrahydrophthalic acid, norbornane dicarboxylic acid, etc. Further, acid monoanhydrides of dicarboxylic acids or tricarboxylic acids introduced with arbitrary substituents are also included. In addition, examples of the acid monoanhydrides of aromatic dicarboxylic acids or tricarboxylic acids include acid monoanhydrides of phthalic acid, isophthalic acid, trimellitic acid, etc. Further, acid monoanhydrides of dicarboxylic acids or tricarboxylic acids introduced with arbitrary substituents are also included.

[0033] In addition, examples of the (b) tetracarboxylic acid dianhydride that reacts with the hydroxyl group in the epoxy (meth)acrylate molecule obtained by reacting such an epoxy compound with (meth) acrylic acid include: dianhydrides of chain hydrocarbon tetracarboxylic acids, dianhydrides of alicyclic tetracarboxylic acids, or dianhydrides of aromatic tetracarboxylic acids. Here, examples of the dianhydrides of chain hydrocarbon tetracarboxylic acids include: dianhydrides of butane tetracarboxylic acids, pentane tetracarboxylic acids, hexane tetracarboxylic acids, etc., and further include dianhydrides of tetracarboxylic acids introduced with arbitrary substituents. In addition, examples of the dianhydrides of alicyclic tetracarboxylic acids include: dianhydrides of cyclobutane tetracarboxylic acids, cyclopentane tetracarboxylic acids, cyclohexane tetracarboxylic acids, cycloheptane tetracarboxylic acids, norbornane tetracarboxylic acids, etc., and further include dianhydrides of tetracarboxylic acids introduced with arbitrary substituents. Furthermore, examples of the acid dianhydride of the aromatic tetracarboxylic acid include acid dianhydrides of pyromellitic acid, benzophenonetetracarboxylic acid, biphenyltetracarboxylic acid, biphenyl ether tetracarboxylic acid, and the like, and further include acid dianhydrides of tetracarboxylic acids into which an arbitrary substituent is introduced.

[0034] The molar ratio (a) / (b) of the anhydride of (a) dicarboxylic acid or tricarboxylic acid and (b) tetracarboxylic acid dianhydride reacting with epoxy (meth) acrylate is preferably 0.01 to 10.0, more preferably 0.02 or more and less than 3.0. If the molar ratio (a) / (b) deviates from the range, the optimal molecular weight for preparing a photosensitive resin composition having good light patterning properties cannot be obtained, so it is not preferred. Furthermore, there is a tendency that the smaller the molar ratio (a) / (b), the larger the molecular weight, and the lower the alkali solubility.

[0035] In addition, the reaction of the epoxy compound with (meth) acrylic acid, and the reaction of the epoxy (meth) acrylate obtained by the reaction with a polycarboxylic acid or anhydride thereof are not particularly limited, and a known method can be used. In addition, the weight average molecular weight (Mw) of the photosensitive resin containing an unsaturated group synthesized by the reaction is preferably 2000 to 10000, and the acid value is preferably 30 mgKOH / g to 200 mgKOH / g.

[0036] Regarding the photosensitive resin containing an unsaturated group as the component (A), other preferred examples of the resin include: a resin which is a copolymer of (meth)acrylic acid, (meth)acrylic acid ester, etc., and has a (meth)acrylic acid group and a carboxyl group. Examples of the resin include an alkali-soluble resin containing a polymerizable unsaturated group obtained by copolymerizing (meth)acrylic acid esters including glycidyl (meth)acrylate in a solvent to obtain a copolymer, reacting (meth)acrylic acid with the obtained copolymer, and finally reacting an anhydride of a dicarboxylic acid or a tricarboxylic acid. The copolymer can refer to: a copolymer represented by Japanese Patent Laid-Open No. 2014-111722, comprising 20 mol% to 90 mol% of repeating units derived from diester glycerol obtained by esterifying hydroxyl groups at both ends with (meth) acrylic acid, and 10 mol% to 80 mol% of repeating units derived from one or more polymerizable unsaturated compounds copolymerizable therewith, and having a number average molecular weight of 2,000 to 20,000 and an acid value of 35 mgKOH / g to 120 mgKOH / g; and a polymer represented by Japanese Patent Laid-Open No. 2018-141968, comprising units derived from a (meth)acrylate compound, and units having a (meth)acryloyl group and a dicarboxylic acid residue or a tricarboxylic acid residue, having a weight average molecular weight (Mw) of 3,000 to 50,000, and an acid value of 30 mgKOH / g to 200 mgKOH / g, i.e., an alkali-soluble resin containing a polymerizable unsaturated group.

[0037] (A) The unsaturated group-containing photosensitive resin of the component may be used alone or in combination of two or more.

[0038] ((B) ingredient)

[0039] The dendritic polymer as component (B) is a multi-branched polymer having two or more ethylene polymerizable groups at the end. The ethylene polymerizable group is preferably derived from (meth)acrylate. Here, the ethylene polymerizable group is a group having a carbon-carbon double bond, and it is known that in a conjugated compound such as an α,β-unsaturated carbonyl compound in which a carbonyl group is bonded to the carbon-carbon double bond, a Michael addition reaction is caused by the vinyl group that has the strongest interaction with a nucleophilic agent such as a mercapto compound. Therefore, by reacting a compound having multiple ethylene polymerizable groups such as an α,β-unsaturated carbonyl compound with a compound having multiple nucleophilic groups such as a polythiol compound, an addition reaction is generated in the carbon at the β position relative to the carbonyl group. Here, when there are multiple groups that produce an addition reaction, a large number of branches are generated to form a dendritic polymer. This type of dendritic polymer is known through Patent Document 2 and the like, and can be obtained using the method described in the document.

[0040] Examples of the dendrimer as the component (B) include polymers obtained by Michael addition polymerization (addition of carbon-carbon double bonds at the β-position with respect to carbonyl groups) of a polyfunctional (meth)acrylate represented by the general formula (3) and a polyvalent mercapto compound represented by the general formula (4).

[0041] [Chemistry 3]

[0042]

[0043] [Chemistry 4]

[0044]

[0045] Here, the Michael addition of the polyfunctional (meth)acrylate represented by the general formula (3) and the polythiol compound represented by the general formula (4) is preferably carried out in the following manner: the obtained dendritic polymer can still be subjected to radiation polymerization based on carbon-carbon double bonds, and when the total amount of carbon-carbon double bonds possessed by the compound represented by the general formula (3) is set to 100 mol%, the carbon-carbon double bonds remain in the range of 0.1 mol% to 50 mol%.

[0046] For example, the mercapto group of the polyvalent mercapto compound represented by the general formula (4) and the carbon-carbon double bond (referring to the CH in the general formula (3)) of the polyfunctional (meth)acrylate represented by the general formula (3) 2 =C(R 5 The double bond represented by )- refers to the double bond when calculating the molar ratio. The addition ratio of the mercapto group / double bond is preferably 1 / 100 to 1 / 3, more preferably 1 / 50 to 1 / 5, and particularly preferably 1 / 20 to 1 / 8.

[0047] In addition, the dendritic polymer preferably has a sufficient amount of functional groups for radiation polymerization. Therefore, in the molecular weight of the dendritic polymer, the molecular weight per 1 mol of carbon-carbon double bonds is preferably in the range of 100 to 10,000. In addition, the weight average molecular weight (Mw) of the dendritic polymer is preferably in the range of 1,000 to 20,000, and more preferably in the range of 8,000 to 15,000.

[0048] In the general formula (3), R 5 is hydrogen or an alkyl group having 1 to 4 carbon atoms, R 6 To convert polyol R 7 (OH) m Of the m hydroxyl groups, n hydroxyl groups are provided to the remaining portion after the ester bond in the general formula (3). 7 (OH) m It is a polyol based on a non-aromatic straight-chain or branched hydrocarbon skeleton having 2 to 8 carbon atoms, or a polyol ether formed by dehydration condensation of a plurality of polyol molecules and linking them via an ether bond, or an ester of these polyols or polyol ethers with a hydroxy acid. In the general formula (3), m represents an integer of 2 to 20, n represents an integer of 2 to 20, and m≧n.

[0049] Examples of the polyfunctional (meth)acrylate represented by the general formula (3) include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, caprolactone (Meth)acrylates such as modified pentaerythritol tetra(meth)acrylate, caprolactone-modified dipentaerythritol hexa(meth)acrylate, epichlorohydrin-modified hexahydrophthalic acid di(meth)acrylate, hydroxypivalate neopentyl glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethylene oxide-modified neopentyl glycol di(meth)acrylate, propylene oxide-modified neopentyl glycol di(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, trimethylolpropane benzoate (meth)acrylate, tris((meth)acryloyloxyethyl) isocyanurate, alkoxy-modified trimethylolpropane tri(meth)acrylate, dipentaerythritol poly(meth)acrylate, alkyl-modified dipentaerythritol tri(meth)acrylate, and di-trimethylolpropane tetra(meth)acrylate. These compounds may be used alone or in combination of two or more.

[0050] In the general formula (4), R 8 is a single bond or a divalent to hexavalent hydrocarbon group having 1 to 6 carbon atoms, and p is 8 When it is a single bond, it is 2. 8 When it is a divalent to hexavalent group, it represents an integer of 2 to 6. Here, R 8 It may have a single bond or a substituent, and may further contain an oxygen atom in a hydrocarbon group having 1 to 6 carbon atoms or in the skeleton of the hydrocarbon group. These hydrocarbon groups may be straight chain or branched. In addition, these hydrocarbon group-containing groups may further have a thiomethyl group (HSCH 2 -). In addition, when the hydrocarbon group contains an oxygen atom in the skeleton, both ends are preferably hydrocarbon groups. Here, p represents an integer of 2 to 6, and R 8 Therefore, in R 8 When it is a single bond, p is 2. 8 When the carbon number of is 1, p is 2 to 4.8 When the carbon number of is 2-6, p is 2-6.

[0051] Examples of the polythiol compounds represented by the general formula (4) include: 1,2-dimercaptoethane, 1,3-dimercaptopropane, 1,4-dimercaptobutane, bis(dimercaptoethanethiol), trimethylolpropane tris(thioglycolate), trimethylolpropane tris(thiopropionate), pentaerythritol tetra(thioglycolate), pentaerythritol tris(thioglycolate), pentaerythritol tetra(thiopropionate), dipentaerythritol hexa(thioglycolate), dipentaerythritol hexa(thiopropionate), etc.

[0052] When synthesizing the dendritic polymer as the component (B), a polymerization inhibitor may be added as needed. Examples of polymerization inhibitors include hydroquinone compounds and phenol compounds. Specific examples thereof include hydroquinone, methoxyhydroquinone, catechol, p-tert-butylcatechol, cresol, butylated hydroxytoluene, 2,4,6-tri-tert-butylphenol (2,4,6-tri-tert-butylphenol, BHT), etc.

[0053] The completion of the synthesis of the dendrimer as the component (B) can be confirmed by liquid chromatography, gel filtration chromatography or other common analytical equipment.

[0054] When synthesizing the dendritic polymer as the component (B), a Michael addition reaction occurs in which the polyvalent mercapto compound represented by the general formula (4) is added to the double bond of the polyfunctional (meth)acrylate represented by the general formula (3). The reaction can be carried out by mixing the polyfunctional (meth)acrylate and the polyvalent mercapto compound and adding a basic catalyst at room temperature to 100° C. The reaction time is usually preferably 30 minutes to 20 hours, and more preferably 6 hours to 12 hours.

[0055] The detailed mechanism by which the dendritic polymer as the component (B) has excellent properties as a photosensitive resin composition is not clear. However, it is believed that the dendritic polymer generally using thiol and acrylate is not easily inhibited by reaction due to oxygen or solvent in free radical polymerization due to its unique structure, and cures with low energy, has little shrinkage during curing, and suppresses deterioration of the surface roughness of the coating film. Therefore, for example, when it is made into a light-shielding film, it has particularly excellent properties.

[0056] In addition, the ratio of the content of component (A) and component (B) is preferably 95 / 5 to 40 / 60, and more preferably 60 / 40 to 50 / 50. By setting the ratio of the content of component (A) and component (B) within a preferred range, appropriate patterning that can suppress peeling and surface wrinkles can be performed. In addition, by setting it within a more preferred range, patterning of a thick film of 5 μm to 25 μm required for the partition wall can be performed at an appropriate development time, and a cured film pattern with excellent pattern shape and pattern surface properties can be obtained.

[0057] When the proportion of component (A) is less than the range, the cured product after the photocuring reaction tends to become brittle. On the contrary, when the proportion of component (A) is more than the range, it is difficult to increase the dissolution rate of the unexposed portion relative to the alkaline developer. Therefore, when the proportion of component (A) is more than the range, when the patterning of a film thickness of less than 2 μm is performed as a color filter, it can be controlled to an appropriate development speed, but when the patterning of a film thickness of more than 5 μm is performed, it is difficult to control to an appropriate development speed and pattern shape.

[0058] (Other photopolymerizable monomers)

[0059] In order to control the photocurability, in addition to the combination of the components (A) and (B), a photopolymerizable monomer (component B′) having at least two ethylenically unsaturated bonds may be used in combination. Examples of the photopolymerizable monomer include (meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, tetramethylene glycol di(meth)acrylate, glycerol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, glycerol tri(meth)acrylate, sorbitol penta(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, sorbitol hexa(meth)acrylate, phosphazene alkylene oxide-modified hexa(meth)acrylate, and caprolactone-modified dipentaerythritol hexa(meth)acrylate. These photopolymerizable monomers may be used alone or in combination of two or more.

[0060] ((C) ingredient)

[0061] (C) Examples of photopolymerization initiators include: acetophenones such as acetophenone, 2,2-diethoxyacetophenone, p-dimethylacetophenone, p-dimethylaminoacetophenone, dichloroacetophenone, trichloroacetophenone, and p-tert-butylacetophenone; benzophenones such as benzophenone, 2-chlorobenzophenone, and p,p'-bisdimethylaminobenzophenone; benzoin ethers such as benzil, benzoin, benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; 2-(o-chlorophenyl)-4,5-phenylbiimidazole, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)biimidazole, 2-(o-fluorophenyl)-4,5-diphenylbiimidazole, 2-(o-methoxyphenyl)-4,5-diphenylbiimidazole, 2,4, 5-triarylbiimidazole and other biimidazole compounds; 2-trichloromethyl-5-phenylvinyl-1,3,4-oxadiazole, 2-trichloromethyl-5-(p-cyanophenylvinyl)-1,3,4-oxadiazole, 2-trichloromethyl-5-(p-methoxyphenylvinyl)-1,3,4-oxadiazole and other halogenated methyl thiazole compounds; 2,4,6-tris(trichloromethyl)-1,3,5-triazine, 2-methyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-phenyl-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-chlorophenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine 2-(4-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(3,4,5-trimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-(4-methylthiophenylvinyl)-4,6-bis(trichloromethyl)-1,3,5-triazine and other halogenated methyl-s-triazine compounds; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-,2-(O-benzoyl oxime), 1-(4-phenylthiophenyl)butane-1,2-dione-2-oxime-O-benzoate, O-acyl oxime compounds such as 1-(4-methylthiophenyl)butane-1,2-dione-2-oxime-O-acetate and 1-(4-methylthiophenyl)butane-1-one oxime-O-acetate; sulfur compounds such as benzyl dimethyl ketal, thioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthone, 2-methylthioxanthone, and 2-isopropylthioxanthone; anthraquinones such as 2-ethylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, and 2,3-diphenylanthraquinone; organic peroxides such as azobisisobutyronitrile, benzoyl peroxide, and cumene peroxide; thiol compounds such as 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, and 2-mercaptobenzothiazole; tertiary amines such as triethanolamine and triethylamine, etc. These photopolymerization initiators may be used alone or in combination of two or more.

[0062] In particular, in the case of a photosensitive resin composition containing a colorant, it is preferred to use an O-acyl oxime compound (including ketoxime). In addition, in the case of using a colorant at a high pigment concentration and forming a light-shielding film pattern, it is preferred to use an O-acyl oxime photopolymerization initiator having a molar absorption coefficient of 10,000 or more at 365 nm. As a specific compound group, there is an O-acyl oxime photopolymerization initiator represented by general formula (5). Furthermore, the "photopolymerization initiator" described in the present invention is used in the sense of including a sensitizer.

[0063] [Chemistry 5]

[0064]

[0065] In formula (5), R 9 , R 10 Each independently represents a C1-C15 alkyl group, a C6-C18 aryl group, a C7-C20 arylalkyl group or a C4-C12 heterocyclic group, and R 11 represents a C1-C15 alkyl group, a C6-C18 aryl group, or a C7-C20 arylalkyl group. Here, the alkyl group and the aryl group may be substituted by a C1-C10 alkyl group, a C1-C10 alkoxy group, a C1-C10 alkanoyl group, or a halogen, and the alkylene moiety may contain an unsaturated bond, an ether bond, a thioether bond, or an ester bond. In addition, the alkyl group may be any of a linear, branched, or cyclic alkyl group.

[0066] The amount of the photopolymerization initiator of the component (C) is preferably 3 to 30 parts by weight, more preferably 5 to 20 parts by weight, based on 100 parts by weight of the total of the components (A) and (B). When the proportion of the component (C) is less than 3 parts by weight, the sensitivity is reduced, thereby slowing down the speed of photopolymerization. In contrast, when the proportion of the component (C) exceeds 30 parts by weight, the sensitivity is too strong, thereby causing concerns that the desired pattern line width and the desired pattern edge cannot be obtained.

[0067] ((D) ingredient)

[0068] The ink repellent of component (D) is a component that imparts ink repellency to the partition wall relative to the ink. When a predetermined amount of ink containing a material of an organic layer is injected into an area surrounded by the partition wall, it is preferred to contain the ink repellent. The reason for this is that it can suppress the ink from flowing into the adjacent partition wall and the ink from adhering to the partition wall.

[0069] (D) The example of the ink-repellent of component includes a compound containing silicone or a fluorine compound. In the present invention, the ink-repellent of component (D) is preferably a fluorine compound, more preferably a fluorine compound containing a crosslinking group. The reason is that: when using a fluorine compound as an ink-repellent, the base with a fluorine atom is oriented on the surface of the partition wall, thereby suppressing the oozing or color mixing of ink. In addition, the reason is that: the base repels ink, thereby suppressing the entry into the region of the adjacent partition wall. In addition, by using a fluorine compound containing a crosslinking group, the crosslinking reaction in its surface can be accelerated when the formed coating film is exposed. Thus, in the development process, the ink-repellent is not easy to flow out from the coating film, so the partition wall with high ink-repellent can be obtained.

[0070] As the cross-linking group, preferably an epoxy group or an ethylenic unsaturated group, preferably an ethylenic unsaturated group in terms of the viewpoint of suppressing the outflow of the ink-repellent agent from the partition wall. Here, the example of the fluorine-based compound with an ethylenic unsaturated group includes: perfluoroalkyl sulfonic acid, perfluoroalkyl carboxylic acid, perfluoroalkyl alkylene oxide adduct, perfluoroalkyl trialkyl ammonium salt, oligomers including perfluoroalkyl and hydrophilic groups, oligomers including perfluoroalkyl and lipophilic groups, oligomers including perfluoroalkyl and hydrophilic groups and lipophilic groups, carbamates including perfluoroalkyl and hydrophilic groups, perfluoroalkyl esters, perfluoroalkyl phosphates, etc. containing fluorine organic compounds, etc.

[0071] The molecular weight of the ink repellent of the component (D) used in the present invention is not particularly limited and may be small or large. Here, by using an ink repellent with a large molecular weight, the fluidity of the ink repellent caused by calcination can be suppressed, and the outflow of the ink repellent from the partition wall can be suppressed, so it is preferred. In addition, the weight average molecular weight (Mw) of the ink repellent is preferably in the range of 100 to 200,000, more preferably in the range of 1,000 to 150,000, and particularly preferably in the range of 10,000 to 130,000. If the weight average molecular weight (Mw) is above the lower limit (Mw: 100), the ink repellent is easy to migrate on the upper surface when a cured film is formed using a negative photosensitive resin composition. In addition, if it is below the upper limit (Mw: 200,000), the residue in the opening becomes less, so it is preferred.

[0072] The content of the ink-repellent agent of the component (D) in the photosensitive resin composition of the present invention is preferably 0.01% by mass or more and 10% by mass or less relative to all solid components, more preferably 0.05% by mass or more and 8% by mass or less, and particularly preferably 0.1% by mass or more and 6% by mass or less. Here, by setting the content of the ink-repellent agent to 0.01% by mass or more, it has high ink-repellent properties, and by setting it to 10% by mass or less, it is possible to suppress outflow to the pixel portion.

[0073] Examples of ink repellents include: ink repellents including compounds having a hydrocarbon chain as the main chain and containing fluorine atoms in the side chains. In addition, ink repellents may also include ink repellents containing partially hydrolyzed condensates of hydrolyzable silane compounds, wherein the hydrolyzable silane compounds contain hydrolyzable silane compounds having fluorine atoms. The ink repellents may be used alone or in combination of two or more.

[0074] ((E) ingredient)

[0075] The colorant of the black pigment, mixed color organic pigment and white pigment of the component (E) that can be used in the present invention can be any known colorant without particular limitation as long as it is a colorant dispersed with an average particle size of 1 nm to 1000 nm (average particle size measured by a laser diffraction / scattering particle size distribution meter or a dynamic light scattering particle size distribution meter).

[0076] Here, examples of black pigments include: perylene black, cyanine black, aniline black, carbon black, titanium black, etc. Examples of mixed color organic pigments include: pigments obtained by mixing at least two colors selected from organic pigments such as azo pigments, condensed azo pigments, azomethine pigments, phthalocyanine pigments, quinacridone pigments, isoindolinone pigments, isoindolinoline pigments, dioxazine pigments, threne pigments, perylene pigments, perinone pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, and thioindigo pigments. Examples of white pigments include: titanium oxide pigments, composite oxide pigments; inorganic fillers such as calcium silicate, magnesium carbonate, calcium carbonate, calcium sulfate, and barium sulfate. Depending on the function of the target photosensitive resin composition, these (E) components may be used alone or in combination of two or more.

[0077] In addition, examples of the organic pigment which can be used as the (E) component include the pigments with the following numbers in the name of the Color Index, but are not limited to these.

[0078] Pigment red 2, 3, 4, 5, 9, 12, 14, 22, 23, 31, 38, 112, 122, 144, 146, 147, 149, 166, 168, 170, 175, 176, 177, 178, 179, 184, 185, 187, 188, 202, 207, 208, 209, 210, 213, 214, 220, 221, 242, 247, 253, 254, 255, 256, 257, 262, 264, 266, 272, 279, etc.

[0079] Pigment orange: 5, 13, 16, 34, 36, 38, 43, 61, 62, 64, 67, 68, 71, 72, 73, 74, 81, etc.

[0080] Pigment yellow: 1, 3, 12, 13, 14, 16, 17, 55, 73, 74, 81, 83, 93, 95, 97, 109, 110, 111, 117, 120, 126, 127, 128, 129, 130, 136, 138, 139, 150, 151, 153, 154, 155, 173, 174, 175, 176, 180, 181, 183, 185, 191, 194, 199, 213, 214, etc.

[0081] Pigment green: 7, 36, 58, etc.

[0082] Pigment blue 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 60, 80, etc.

[0083] Pigment violet 19, 23, 37, etc.

[0084] The mixing ratio of the colorant of the component (E) can be arbitrarily determined according to the desired light shielding degree, and is preferably 1% to 80% by mass relative to the solid content in the photosensitive resin composition. Here, in the case of forming a black partition wall, it is more preferably 3% to 50% by mass, and in the case of forming a white partition wall, it is more preferably 10% to 80% by mass.

[0085] The (E) component is usually mixed with other formulation components in the form of a colorant dispersion dispersed in a solvent, and a dispersant (E' component) may be added at this time. The dispersant may be a known compound used in the dispersion of the pigment (colorant) without particular limitation (a compound commercially available under the name of a dispersant, a dispersing wetting agent, a dispersion accelerator, etc.). Examples of dispersants include: cationic polymer dispersants, anionic polymer dispersants, nonionic polymer dispersants, and pigment derivative dispersants (dispersing aids). In particular, in terms of adsorption of the colorant, the dispersant is preferably a cationic polymer dispersant having a cationic functional group such as an imidazole group, a pyrrolyl group, a pyridine group, a primary amino group, a secondary amino group, or a tertiary amino group, and an amine value of 1 mgKOH / g to 100 mgKOH / g, and a number average molecular weight in the range of 1,000 to 100,000. The amount of the dispersant is preferably 1% to 35% by mass relative to the colorant, and more preferably 2% to 25% by mass. Furthermore, a high-viscosity substance such as a resin generally has a function of stabilizing dispersion, but a substance that does not have the ability to promote dispersion is not treated as a dispersant. However, the use for the purpose of stabilizing dispersion is not limited.

[0086] The photosensitive resin composition of the present invention can be prepared by mixing and dispersing the components (A) to (E) by an appropriate method.

[0087] (Solvent)

[0088] In the photosensitive resin composition of the present invention, it is preferred to use a solvent as the component (F) in addition to the components (A) to (E). Examples of the solvent include alcohols such as methanol, ethanol, n-propanol, isopropanol, ethylene glycol, and propylene glycol; terpenes such as α-terpineol and β-terpineol; ketones such as acetone, methyl ethyl ketone, cyclohexanone, and N-methyl-2-pyrrolidone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, ethyl cellosolve, carbitol, methyl carbitol, ethyl carbitol, butyl carbitol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, triethylene glycol monomethyl ether, and triethylene glycol monoethyl ether; acetates such as ethyl acetate, butyl acetate, cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, carbitol acetate, ethyl carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; and the like. By using these alone or in combination of two or more kinds and dissolving and mixing them, a uniform solution-like composition can be prepared.

[0089] In addition, the photosensitive resin composition of the present invention may contain resins other than the epoxy resin (A) component, hardeners, hardening accelerators, thermal polymerization inhibitors and antioxidants, plasticizers, fillers, leveling agents, defoamers, surfactants, coupling agents and other additives as needed. Here, examples of thermal polymerization inhibitors and antioxidants include: hydroquinone, hydroquinone monomethyl ether, pyrogallol, tert-butylcatechol, phenothiazine, hindered phenol compounds, etc. Examples of plasticizers include: dibutyl phthalate, dioctyl phthalate, tricresyl phosphate, etc. Examples of fillers include: glass fiber, silica, mica, alumina, etc. Examples of defoamers or leveling agents include: silicone, fluorine, and acrylic compounds. Examples of surfactants include fluorine-based surfactants, silicone-based surfactants, etc. Examples of the coupling agent include 3-(glycidyloxy)propyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-ureidopropyltriethoxysilane and the like.

[0090] The photosensitive resin composition of the present invention preferably contains a photosensitive resin containing an unsaturated group as component (A), a dendritic polymer as component (B), a photopolymerization initiator as component (C), an ink-repellent as component (D), and a colorant as component (E) in a total of 80% by mass or more, preferably 90% by mass or more, in the solid component (the solid component contains a monomer that becomes a solid component after curing) excluding the solvent. The amount of the solvent varies according to the target viscosity, and is preferably 40% to 90% by mass relative to the total amount.

[0091] In addition, the cured product (partition wall) formed by curing the photosensitive resin composition of the present invention can be obtained, for example, by applying a solution of the photosensitive resin composition on a substrate, drying the solvent, and curing by irradiating light (including ultraviolet rays, radiation, etc.). If a portion irradiated with light and a portion not irradiated with light are provided using a photomask, and only the portion irradiated with light is cured, and the other portion is dissolved using an alkaline solution, a partition wall of a desired pattern can be obtained.

[0092] Each step of the film-forming method by coating and drying of the photosensitive resin composition will be specifically exemplified.

[0093] As a method for coating the photosensitive resin composition on the substrate, any method such as a known solution immersion method, a spray method, a method using a roll coater, a disc coater (Land coater machine), a slit coater or a rotary machine can also be used. After coating to the desired thickness using these methods, the solvent is removed (pre-baked) to form a film. Pre-baking is carried out by heating, vacuum drying or a combination of these using an oven, a hot plate, etc. The heating temperature and heating time in the pre-baking can be appropriately selected according to the solvent used, for example, preferably at 80°C to 120°C for 1 minute to 10 minutes.

[0094] As the radiation used in the exposure, for example, visible light, ultraviolet light, far ultraviolet light, electron beam, X-ray, etc. can be used, and the wavelength range of the radiation is preferably 250nm to 450nm. In addition, as a developer suitable for the alkali development, for example, an aqueous solution of sodium carbonate, potassium carbonate, potassium hydroxide, diethanolamine, tetramethylammonium hydroxide, etc. can be used. These developers can be appropriately selected according to the characteristics of the resin layer, but it is also effective to add a surfactant as needed. The development temperature is preferably 20°C to 35°C, and a commercially available developer or ultrasonic cleaning machine can be used to accurately form a fine image. Furthermore, after the alkali development, water washing is usually performed. As a development treatment method, a spray development method, a spray development method, an immersion (dip) development method, a puddle development method, etc. can be applied.

[0095] After developing in this way, heat treatment (post-baking) is performed at 180°C to 250°C for 20 minutes to 100 minutes. Among them, when the heat resistance of the substrate for film formation is low, the formulation of the composition can also be designed so that the post-baking conditions can be set at 80°C to 180°C for 30 minutes to 100 minutes. The post-baking is performed for the purpose of improving the adhesion between the patterned coating film and the substrate. Post-baking can be performed by heating using an oven, a hot plate, etc., similarly to pre-baking.

[0096] According to the above, in the present invention, a black partition wall having an optical density (OD) of 0.2 / μm to 4.0 / μm and a cone angle of 21° or more and a white partition wall having an optical density (OD) of 0.1 / μm to 0.3 / μm and a cone angle of 21° or more can be obtained. In addition, a black partition wall having an optical density (OD) of 0.2 / μm to 4.0 / μm and a cone angle of 51° or more and a white partition wall having an optical density (OD) of 0.1 / μm to 0.3 / μm and a cone angle of 51° or more can be obtained.

[0097] The photosensitive resin composition of the present invention can be used in the production of organic EL devices, quantum dot displays, TFT arrays, color filters including wavelength conversion elements, and the like.

[0098] [Example]

[0099] Hereinafter, the present invention will be described in detail based on examples and comparative examples, but the present invention is not limited thereto. In addition, synthesis examples of the photosensitive resin containing an unsaturated group as the component (A) and the dendritic polymer as the component (B) are shown. Furthermore, the scope of the present invention is not limited by these examples, etc.

[0100] The abbreviations used in Synthesis Examples 1 to 3 are as follows.

[0101] BPFE: Bisphenol fluorene epoxy compound (reaction product of 9,9-bis(4-hydroxyphenyl)fluorene and chloromethyloxirane (epoxide equivalent 250g / eq))

[0102] AA: Acrylic acid

[0103] PGMEA: Propylene glycol monomethyl ether acetate

[0104] TEAB: Tetraethylammonium bromide

[0105] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0106] THPA: Tetrahydrophthalic anhydride

[0107] MAA: Methacrylic acid

[0108] MMA: Methyl Methacrylate

[0109] CHMA: Cyclohexyl methacrylate

[0110] AIBN: Azobisisobutyronitrile

[0111] GMA: Glycidyl Methacrylate

[0112] TPP: triphenylphosphine

[0113] TBPC: 2,6-di-tert-butyl-p-cresol

[0114] PTMA: Pentaerythritol tetrakis(thioglycolate)

[0115] DPHA: A mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate

[0116] HQ: Hydroquinone

[0117] BzDMA: benzyl dimethylamine

[0118] [Synthesis example 1]

[0119] BPFE (114.4 g (0.23 mol)), AA (33.2 g (0.46 mol)), PGMEA (157 g) and TEAB (0.48 g) were placed in a 500 ml four-necked flask with a reflux cooler, and stirred at 100°C to 105°C for 20 hours to react. Subsequently, BPDA (35.3 g (0.12 mol)) and THPA (18.3 g (0.12 mol)) were placed in the flask, and stirred at 120°C to 125°C for 6 hours to obtain a photosensitive resin (A)-1 containing an unsaturated group. The solid content concentration of the obtained resin solution was 56.1% by mass, the acid value (solid content conversion) was 103 mgKOH / g, and the Mw was 3600 as analyzed by gel permeation chromatography (GPC).

[0120] [Synthesis example 2]

[0121] MAA (51.65 g (0.60 mol)), MMA (36.04 g (0.36 mol)), CHMA (40.38 g (0.24 mol)), AIBN (5.91 g), and PGMEA (360 g) were placed in a 1000 ml four-necked flask equipped with a nitrogen inlet tube and a reflux tube, and polymerization was carried out by stirring at 80° C. to 85° C. for 8 hours under a nitrogen flow. Furthermore, GMA (61.41 g (0.43 mol)), TPP (2.27 g), and TBPC (0.086 g) were placed in the flask, and stirred at 80° C. to 85° C. for 16 hours to obtain a photosensitive resin (A)-2 containing an unsaturated group. The solid content concentration of the obtained resin solution was 35.7% by mass, the acid value (solid content conversion) was 50 mgKOH / g, and the Mw obtained by GPC analysis was 19600.

[0122] [Synthesis example 3]

[0123] PTMA (20 g (mercapto group: 0.19 mol)), DPHA (212 g (acrylic acid group: 2.12 mol)), PGMEA (58 g), HQ (0.1 g), and BzDMA (0.01 g) were placed in a 1 L four-necked flask, and polymerization was carried out by stirring at 60° C. for 12 hours to obtain a dendritic polymer (B). The solid content concentration of the obtained dendritic polymer was 80% by mass, and the Mw obtained by GPC analysis was 10000. The disappearance of the mercapto group was confirmed by iodometry of the dendritic polymer.

[0124] The solid content concentration, acid value, and molecular weight of the unsaturated group-containing photosensitive resin and dendrimer obtained in Synthesis Examples 1 to 3 were determined by the following method.

[0125] [Solid content concentration]

[0126] 1 g of the resin solution obtained in the synthesis example was impregnated into a glass filter [weight: W0 (g)] and weighed [W1 (g)]. The weight after heating at 160° C. for 2 hours [W2 (g)] was determined using the following formula.

[0127] Solid content concentration (weight %) = 100 × (W2-W0) / (W1-W0)

[0128] [Acid value]

[0129] The resin solution was dissolved in dioxane and titrated with a 1 / 10 N-KOH aqueous solution using a potentiometric titrator (manufactured by Hiranuma Sangyo Co., Ltd., trade name COM-1600) to determine the concentration.

[0130] [Molecular weight]

[0131] The measurement was performed using a gel permeation chromatograph (GPC) [trade name: HLC-8220GPC manufactured by Tosoh Corporation, solvent: tetrahydrofuran, column: TSKgelSuperH-2000 (2 tubes) + TSKgelSuperH-3000 (1 tube) + TSKgelSuperH-4000 (1 tube) + TSKgelSuper-H5000 (1 tube) [manufactured by Tosoh Corporation], temperature: 40°C, flow rate: 0.6 ml / min], and the weight average molecular weight (Mw) was calculated using a standard polystyrene [PS-oligomer set manufactured by Tosoh Corporation] conversion value.

[0132] The components and their blending amounts of the photosensitive resin compositions for partition walls of Examples 1 to 17 and Comparative Example 1 are shown in Tables 1 and 2. In addition, the components (A) to (E) in Tables 1 and 2 are the amounts of solid components other than the solvent, and the amounts of the solvents in the resin solutions and coloring dispersions are expressed in total with the solvent (F). In addition, the components represented by (A) to (F) are described below.

[0133] The symbols used in the Examples and Comparative Examples shown in Tables 1 and 2 are as follows.

[0134] (A) Photosensitive resin containing unsaturated groups

[0135] (A)-1: Resin obtained in Synthesis Example 1

[0136] (A)-2: Resin obtained in Synthesis Example 2

[0137] (B) Dendritic polymer: Dendritic polymer obtained in Synthesis Example 3

[0138] (B') Photopolymerizable monomer: a mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (DPHA, manufactured by Nippon Kayaku Co., Ltd.)

[0139] (C) Photopolymerization initiator: oxime ester-based photopolymerization initiator (Adeka Arkls NCI-831, manufactured by Adeka Co., Ltd., "Adeka Arkls" is a registered trademark of the company)

[0140] (D) Ink repellent: (Megafac RS-72-K, DIC Corporation, "Megafac" is a registered trademark of the company)

[0141] (E) Colorant

[0142] (E)-1: Carbon black

[0143] (E)-2: Lactam Black

[0144] (E)-3: Titanium oxide

[0145] (E') Dispersant

[0146] (F) Solvent: PGMEA

[0147]

[0148]

[0149] [Example 1]

[0150] The respective components (A) to (F) were blended in the ratios described in Table 1 and uniformly mixed to obtain the photosensitive resin composition for partition walls of Example 1.

[0151] Using the photosensitive resin composition for partition walls obtained in Example 1, the following evaluations were performed.

[0152] [Optical density (OD)]

[0153] The photosensitive resin composition for partition walls was applied on a 125 mm×125 mm glass plate (EAGLE XG, manufactured by Corning, "EAGLE XG" is a registered trademark of the company) using a spin coater so that the film thickness after post-baking was 1 μm, and pre-baked at 90° C. for 1 minute. After post-baking at 230° C. for 30 minutes using a hot air dryer, the optical density (OD) was measured using a Macbeth transmission densitometer to evaluate the optical density.

[0154] The optical density (OD) was calculated using the following formula (1).

[0155] Optical density (OD) = -log 10 T (1)

[0156] (T represents transmittance)

[0157] [Development time (film thickness: 10 μm)]

[0158] The photosensitive resin composition for partition walls was applied to a 125 mm × 125 mm glass plate (EAGLE XG, manufactured by Corning) using a spin coater so that the film thickness after post-baking was 10 μm, and pre-baked at 90°C for 1 minute. A negative photomask with an opening of 20 μm was adjusted to an exposure gap of 100 μm and covered on the dried coating film, and an i-ray irradiance of 30 mW / cm 2 Ultra-high pressure mercury lamp irradiation 80mJ / cm 2 Then, the exposed coated plate was treated with a 0.05% potassium hydroxide aqueous solution at 25°C and 1 kgf / cm 2 The development time at which the pattern begins to appear is evaluated by the spray development pressure.

[0159] The development time when the film thickness was 10 μm was evaluated as follows.

[0160] (evaluate)

[0161] ○: The development time for the pattern to begin to appear is less than 2 minutes

[0162] △: The development time for the pattern to begin to appear is 2 minutes or more and less than 3 minutes

[0163] ×: The development time when the pattern begins to appear is more than 3 minutes

[0164] [Development time (film thickness: 2 μm)]

[0165] Evaluation was performed in the same manner as in the operation of the development time for the film thickness (10 μm), except that the film thickness after post-baking was 2 μm.

[0166] The development time when the film thickness was 2 μm was evaluated as follows.

[0167] (evaluate)

[0168] ○: The development time for the pattern to begin to appear is more than 20 seconds

[0169] △: The development time for the pattern to begin to appear is less than 20 seconds

[0170] ×: The development time from the beginning of the pattern to the beginning is less than 5 seconds

[0171] [Thin line patterning properties (film thickness: 5 μm)]

[0172] The photosensitive resin composition for partition walls was applied on a 125 mm × 125 mm glass plate (EAGLE XG, manufactured by Corning) using a spin coater so that the film thickness after post-baking was 10 μm, and pre-baked at 90°C for 1 minute. A negative photomask with an opening of 5 μm was adjusted to an exposure gap of 100 μm and covered on the dried coating film, and an i-ray irradiance of 30 mW / cm 2 Ultra-high pressure mercury lamp irradiation 80mJ / cm 2 Then, the exposed coated plate was treated with a 0.05% potassium hydroxide aqueous solution at 25°C and 1 kgf / cm 2 The spray development pressure was 5kgf / cm2 from the time when the pattern began to appear, and then 10 seconds later, the development was continued. 2 The unexposed portion of the coating film was removed by pressure spray water washing, and it was confirmed whether a pixel pattern was formed on the glass substrate.

[0173] [Patterning properties of thick lines (film thickness: 20 μm)]

[0174] Whether or not a pixel pattern was formed on the glass substrate was confirmed in the same manner as in the patterning of the thin lines, except that the opening of the negative photomask was changed from 5 μm to 20 μm.

[0175] The patterning characteristics of thin lines and thick lines were evaluated as follows.

[0176] (evaluate)

[0177] ○: Pattern formed

[0178] △: Although the pattern was formed, peeling was observed in part

[0179] ×: No pattern is formed

[0180] [Cone Angle]

[0181] The photosensitive resin composition for partition walls was applied to a 125 mm × 125 mm glass plate (EAGLE XG, manufactured by Corning) using a spin coater so that the film thickness after post-baking was 10 μm, and pre-baked at 90°C for 1 minute. A negative photomask with an opening of 20 μm was adjusted to an exposure gap of 100 μm and covered on the dried coating film, and an i-ray irradiance of 30 mW / cm 2 Ultra-high pressure mercury lamp irradiation 80mJ / cm 2 Then, the exposed coated plate was treated with a 0.05% potassium hydroxide aqueous solution at 25°C and 1 kgf / cm 2The spray development pressure was 5kgf / cm2 from the time when the pattern began to appear, and then 10 seconds later, the development was continued. 2 The unexposed portion of the coating film was removed by pressure spray water washing, thereby forming a pixel pattern on the glass substrate. The formed pixel pattern (grid-shaped partition wall) was cut to prepare a sample for cross-sectional observation, and the cross-sectional shape of the partition wall was observed using a scanning electron microscope (manufactured by Keyence Co., Ltd.) to measure its taper angle.

[0182] The taper angle was evaluated in the following manner.

[0183] (evaluate)

[0184] ◎: Cone angle is 51°~90°

[0185] ○: Cone angle is 21° to 50°

[0186] ×: Cone angle is 5°~20°

[0187] (Evaluation of surface wrinkles)

[0188] The surface of the formed pixel pattern of the sample for evaluating the taper angle was observed with an optical microscope to evaluate the presence or absence of wrinkles.

[0189] The evaluation of surface wrinkles was performed in the following manner.

[0190] (evaluate)

[0191] ○: No wrinkles on the surface

[0192] △: There are wrinkles to a degree that will not affect the next process

[0193] ×: There are wrinkles on the surface

[0194] [Example 2 to Example 17 and Comparative Example 1]

[0195] Regarding Examples 2 to 17 and Comparative Example 1, the components (A) to (F) were prepared in the ratios described in Table 1 and uniformly mixed in the same manner as in Example 1, thereby obtaining photosensitive resin compositions for partition walls of Examples 2 to 17 and Comparative Example 1. Each evaluation of the photosensitive resin compositions for partition walls of Examples 2 to 17 and Comparative Example 1 was performed in the same manner as in Example 1.

[0196] The evaluation results of Examples 1 to 17 and Comparative Example 1 are shown in Tables 3 and 4.

[0197]

[0198] The evaluation results shown in Tables 3 and 4 show that the combined use of the photosensitive resin (A) containing an unsaturated group and the dendritic polymer (B) prevents wrinkles from forming on the surface of the pixel pattern after curing. Therefore, the dendritic polymer (B) is effective in suppressing the difference in shrinkage during the curing of the photosensitive resin composition for partition walls.

[0199] Furthermore, by adjusting the blending amounts of the unsaturated group-containing photosensitive resin (A) and the dendritic polymer (B), a photosensitive resin composition for partition walls applicable to films ranging from thin films of 2 μm to thick films of 10 μm can be provided.

[0200] It was also found that by using an epoxy acrylate acid adduct derived from a bisphenol epoxy compound (eg, (A)-1) as the photosensitive resin containing an unsaturated group, good patterning properties can be obtained not only in thick lines but also in thin lines.

[0201] [Industrial Applicability]

[0202] The photosensitive resin composition of the present invention is extremely useful in the manufacture of organic EL elements, quantum dot displays, TFT arrays, and color filters including wavelength conversion elements, etc. In addition, there are also specialized compositions for thick film partition walls, so it is considered that it is also useful as an anti-color mixing material for strong light sources such as partition walls of mini light emitting diodes (LEDs) or micro LEDs.

Claims

1. A photosensitive resin composition for a partition wall, comprising: Component A: a photosensitive resin containing an unsaturated group; Component B: a dendritic polymer having two or more ethylenic polymerizable groups at the ends, wherein the weight average molecular weight of the dendritic polymer is in the range of 1,000 to 20,000; Component C: a photopolymerization initiator; and Component D, an ink repellent, wherein the ink repellent is a fluorine compound containing a cross-linking group, The content ratio of the A component and the B component is 60 / 40 to 50 / 50, The content of the ink repellent in D is 0.05% by mass or more and 8% by mass or less based on the total solid content.

2. The photosensitive resin composition for partition walls according to claim 1, wherein: The component A is a photosensitive resin containing an unsaturated group obtained by reacting a reaction product of an epoxy compound having two glycidyl ether groups derived from a bisphenol represented by the general formula (1) with (meth)acrylic acid and further with a polycarboxylic acid or anhydride thereof: In formula (1), R1, R2, R3 and R4 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms or a halogen atom, X represents -CO-, -SO2-, -C(CF3)2-, -Si(CH3)2-, -CH2-, -C(CH3)2-, -O-, a fluorene-9,9-diyl group represented by general formula (2) or a single bond, and l is an integer from 0 to 10; 3. The photosensitive resin composition for partition walls according to claim 1 or 2, characterized in that: The component B is a dendrimer obtained by adding a polyvalent mercapto compound represented by the general formula (4) to a part of the carbon-carbon double bonds in the (meth)acryloyl group of the polyfunctional (meth)acrylate represented by the general formula (3): In formula (3), R5 represents hydrogen or an alkyl group having 1 to 4 carbon atoms, and R6 represents a polyol R7 (OH) m n hydroxyl groups out of the m hydroxyl groups are supplied to the remaining portion after the ester bond in the general formula (3), m represents an integer of 2 to 20, n represents an integer of 2 to 20, and m≧n; In formula (4), R8 is a single bond or a divalent to hexavalent group containing a hydrocarbon group having 1 to 6 carbon atoms, and p is 2 when R8 is a single bond and represents an integer of 2 to 6 when R8 is a divalent to hexavalent group.

4. The photosensitive resin composition for partition walls according to claim 1 or 2, wherein: The photosensitive resin composition for partition walls contains, as component E, at least one colorant selected from the group consisting of a black pigment, a mixed color organic pigment, and a white pigment. 5 . A cured product obtained by curing the photosensitive resin composition for partition walls according to claim 1 .

6. A method for manufacturing a partition wall, comprising: The process of applying the photosensitive resin composition for partition walls according to claim 4, wherein the component E is a black pigment or a mixed color organic pigment, on a substrate to form a coating film and drying the coating film; A step of exposing the coating film to light using an ultraviolet light exposure device; and The coating film is developed with an alkaline aqueous solution and then thermally calcined. The method for producing the partition wall is characterized in that: The optical density of the partition wall is 0.2 / μm to 4.0 / μm.

7. A method for manufacturing a partition wall, comprising: The process of applying the photosensitive resin composition for partition walls according to claim 4, wherein the component E is a white pigment, on a substrate to form a coating film and drying the coating film; A step of exposing the coating film to light using an ultraviolet light exposure device; and The coating film is developed with an alkaline aqueous solution and then thermally calcined. The method for producing the partition wall is characterized in that: The optical density of the partition wall is 0.1 / μm to 0.3 / μm.

Citation Information

Patent Citations

  • Photosensitive composition and color filter formed from the same

    JP2007286478A

  • Light-shielding composition for touch panel and touch panel

    JP2014111722A

  • Photosensitive resin composition for light-shielding film, light-shielding film, liquid crystal display, method for manufacturing light-shielding film having spacer function, and method for manufacturing liquid crystal display

    JP2018141968A

  • Hyperbranched polymer, process for production thereof, and resin composition

    WO2008047620A1

  • Photosensitive resin composition for black resist, and light shielding film for color filter

    CN102314086A