Adhesive kneading device and adhesive kneading treatment process

Through the rubbing and treatment technology, the particle size of the adhesive is reduced to 200 mesh-600 mesh, solving the problem of poor isolation performance of environmentally friendly, green, ecologically energy-saving integrated house floor wall panels, and achieving effective isolation of carbon dioxide and water vapor , prevent problems such as brine and frost.

CN111151343BActive Publication Date: 2024-11-08叶绍彬
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010060119.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-01-19
Publication Date
2024-11-08
Estimated Expiration
2040-01-19

AI Technical Summary

Technical Problem

The adhesive particle size of the environmentally friendly, green, ecologically energy-saving integrated house floor wall panels is large, causing carbon dioxide and water vapor in the air to enter the interior of the floor wall panels, resulting in poor isolation performance and easy to cause halogen reflux, frost, warping and Cracking and other problems.

Method used

Using a kneading device and kneading process of adhesive, the bonding particles are rubbed through the kneading device to reduce the particle size to 200 mesh-600 mesh, remove the passivation on the surface, and improve the stickiness. The reactivity of the injector enhances the isolation performance of carbon dioxide and water vapor.

Benefits of technology

It effectively reduces the gap inside the floor wall panel, improves the isolation performance of carbon dioxide and water vapor, prevents problems such as halogenation, frost, warping and cracks, and enhances the reaction effect of the adhesive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111151343B_ABST
    Figure CN111151343B_ABST
Patent Text Reader

Abstract

The invention discloses a kneading device for an adhesive, comprising an outer cylinder and an inner cylinder, wherein a spiral baffle is spirally arranged on the outer wall of the inner cylinder along its length direction, a gap is provided between the side of the spiral baffle away from the inner cylinder and the inner wall of the outer cylinder, and a spiral channel is formed between the spiral baffle and the outer wall of the inner cylinder; a hollow shaft torque motor is arranged on the top of the outer cylinder, the stator of the hollow shaft torque motor is arranged on the top of the outer cylinder, the rotor of the hollow shaft torque motor is connected to the top of the inner cylinder, a stirring motor is also arranged on the top of the outer cylinder through a support seat, the output shaft of the stirring motor is connected with a stirring shaft that passes through a middle through hole of the hollow shaft torque motor and is arranged in the inner cylinder; a plurality of feeding holes are arranged at the top of the inner cylinder corresponding to the output end of the spiral channel, a plurality of discharging holes are arranged at the bottom of the inner cylinder, a discharge pipe is arranged at the bottom of the outer cylinder, and a plurality of feeding ports corresponding to the feeding holes on the inner cylinder are arranged at the top of the outer cylinder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of integrated house adhesive processing, in particular to an adhesive used for environmentally friendly, green, ecological and energy-saving integrated house wall and floor slabs, an adhesive kneading device used in production and an adhesive kneading processing process. Background Art

[0002] At present, the particle size of the adhesive used in the floor and wall panels of environmentally friendly, green ecological and energy-saving integrated houses is relatively large. After the floor and wall panels are made, there will be large gaps between the adhesive particles, which will provide a channel for carbon dioxide and water vapor in the air to enter the interior of the floor and wall panels, making the floor and wall panels' performance in isolating carbon dioxide and water vapor poor. The carbon dioxide and water vapor in the air will react with the magnesium material inside the floor and wall panels, breaking the balance of the internal system of the floor and wall panels, and easily causing seven harmful phenomena such as halogen backflow, frost, warping and cracks. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the present invention provides an adhesive kneading device and an adhesive kneading treatment process. The adhesive is kneaded by the kneading device, and the mesh number of the adhesive particles after the treatment is less than 200 meshes, so that after the integrated house floor wall panels are formed, the gap inside the floor wall panels becomes smaller, thereby improving the performance of the floor wall panels in isolating carbon dioxide and water vapor in the air.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] A kneading device for adhesive comprises an outer cylinder and an inner cylinder, wherein the inner cylinder is arranged inside the outer cylinder, a spiral baffle is spirally arranged on the outer wall of the inner cylinder along its length direction, a gap is formed between the side of the spiral baffle away from the inner cylinder and the inner wall of the outer cylinder, and a spiral channel for adhesive particles and auxiliary fillers to pass through is formed between the spiral baffle and the outer wall of the inner cylinder; a hollow shaft torque motor is arranged on the top of the outer cylinder, the stator of the hollow shaft torque motor is arranged on the top of the outer cylinder, the rotor of the hollow shaft torque motor is connected to the top of the inner cylinder, and the outer cylinder A stirring motor is also provided at the top through a support seat, and the output shaft of the stirring motor is connected to a stirring shaft that passes through the middle through hole of the hollow shaft torque motor and is arranged in the inner cylinder; a plurality of feed holes are provided at the top of the inner cylinder corresponding to the output end of the spiral channel, and the feed holes are preferably 8 holes evenly distributed circumferentially; a plurality of discharge holes are provided at the bottom of the inner cylinder, and the discharge holes are preferably 8 holes evenly distributed circumferentially; a discharge pipe is provided at the bottom of the outer cylinder, and a sealing device is provided at the connection between the discharge pipe and the outer cylinder; a plurality of feeding ports corresponding to the feed holes on the inner cylinder are provided at the top of the outer cylinder.

[0006] After mixing the adhesive particles to be treated, auxiliary fillers and kneading media (steel balls), insert the feeding tube from the feeding port on the outer tube to the top of the feeding hole on the inner tube, and pour the material into the inner tube of the device through the feeding tube. The inner tube is driven to rotate (counterclockwise) by a hollow shaft torque motor, and the stirring shaft inside the inner tube is driven to rotate (clockwise) by a stirring motor. The stirring shaft is provided with blades with a spiral curved surface, and the blades form an angle of 45 degrees with the horizontal direction. When the stirring shaft is stirring, it shovels and throws the material in the inner cylinder upward. The diameter of the auxiliary filler and the kneading medium (steel ball) is larger than that of the powder material, and its weight is also heavier than that of the powder material. When these large-particle media are first rolled down at the bottom of the inner cylinder, the large particles of the adhesive are smashed into small particles and kneaded. At the same time, when the stirring shaft is rotating, it gives the kneading medium (steel ball) a movement along the rotation direction of the stirring shaft. These particles of different sizes have different movement speeds, different friction forces, and different movement directions, resulting in mutual extrusion and shearing, and the adhesive material particles can be continuously refined. This process is part of the kneading process. The kneaded fine particles are discharged from the discharge hole on the inner cylinder into the outer cylinder. When the inner cylinder rotates, the fine material in the outer cylinder is stirred into the spiral The magnesium particles are transported into the channel and lifted by the spiral channel, and re-enter the inner cylinder from the feed hole at the top of the inner cylinder for repeated kneading treatment. The present invention realizes rolling kneading of the adhesive particles on the x, y and z axes of the space through multiple cycles of kneading treatment, breaks up large particles of adhesive, and kneads the particle size of the adhesive particles to 200 mesh-600 mesh. The gap after the adhesive is formed is smaller, and the passivation on the surface of the adhesive is removed at the same time. The magnesium particles form a gel layer with the water vapor in the air during transportation. If the kneading treatment is not performed, the gel layer will not react with the curing agent, which will affect the quality of the product. In addition, due to a series of defects of the magnesium material itself, the reaction activity of the adhesive will not be improved, and the reaction effect of the adhesive will not be improved. Only by kneading can the surface of the magnesium material particles be forced to remove the gel layer through kneading so that the fresh surface can be exposed to react with the curing agent. In addition, the fine particles will block the gap channel after the intermolecular reaction, improve the waterproof performance of the magnesium product, further reduce the gap after the filling adhesive is formed, and improve the performance of isolating carbon dioxide and water vapor in the air from entering the system. In addition, the present invention adopts the method of lifting and kneading. When the adhesive particles and auxiliary fillers flow out and fall from the top port of the spiral channel, under the action of gravity, the adhesive particles at the bottom of the inner cylinder will be hit by the kneading medium (steel ball), which further improves the kneading effect on the adhesive and makes the particles continuously refined.

[0007] Preferably, a cooling water jacket is provided on the outside of the outer cylinder, and a water inlet and a water outlet are respectively provided at the bottom and the top of the cooling water jacket. The setting of the cooling water jacket can provide a water cooling system for the kneading process of the adhesive, thereby ensuring the stability of the kneading process and preventing the equipment from being deformed due to the increase in temperature. The heat generated during the kneading process is taken away by the circulation of cooling water, making the kneading system more stable.

[0008] Preferably, the discharge pipe is connected to a circulation pipe, the end of the circulation pipe away from the discharge pipe extends to the inner top of the outer cylinder, and the port of the circulation pipe is located at the output end of the spiral channel. The setting of the circulation pipe facilitates the re-transfer of materials that do not meet the fineness standards to the inner cylinder for repeated kneading. The circulation pipe is provided with a gear pump to provide power for the circulation of the material.

[0009] Preferably, a filter screen is provided on the discharge hole, and material particles that meet the fineness requirements can enter the outer cylinder through the discharge hole and are finally discharged from the discharge pipe, while those that do not meet the fineness requirements are intercepted by the filter screen and continue to be kneaded in the inner cylinder.

[0010] Preferably, the hollow shaft torque motor and the stirring motor rotate in opposite directions, which can achieve a more sufficient stirring and kneading effect.

[0011] Preferably, overflow ports are provided at each quarter of the circumference of the spiral baffle, so that the material can flow downward in each section under the action of centrifugal force, thereby improving the mixing effect between the materials.

[0012] Preferably, the surface of the spiral baffle, the outer wall of the inner cylinder and the inner wall of the outer cylinder are respectively provided with a wear-resistant coating (the wear-resistant coating can be made of high manganese steel, wear-resistant chromium cast iron material or wear-resistant ceramic lining) to improve wear resistance and extend the service life of the device.

[0013] The present invention also provides a kneading treatment process of an adhesive using the kneading device, and the technical scheme thereof is as follows:

[0014] A kneading process of an adhesive comprises the following steps:

[0015] S1. Take adhesive particles, auxiliary fillers and kneading medium and mix them evenly;

[0016] S2, adding the uniformly mixed adhesive particles, auxiliary fillers and kneading medium into the inner cylinder;

[0017] S3, start the motor, adjust the motor speed to 300r / min-500r / min, knead the adhesive particles, and filter while kneading.

[0018] Preferably, the auxiliary filler includes liquid filler and activated filler, the liquid filler includes acrylic emulsion, chloroprene latex, terpene resin, coupling agent, thickener and emulsifier; the activated filler includes lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate.

[0019] Preferably, the weight ratios of lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate to the adhesive particles are 2%-2.5%, 5%-8%, 10%-20%, 10%-15%, 10%-15% and 5%-8%, respectively.

[0020] The activated filler is prepared from lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate. After rubbing the adhesive particles, the passivation on the surface of the adhesive particles can be removed, the surface activity of the adhesive particles can be improved, and the adhesive particles can be activated so that the effective ingredients of the adhesive particles can reach more than 85%, so that the gaps existing after the adhesive is cured and formed are larger, thereby improving the performance of the integrated house wall panels in isolating carbon dioxide and water vapor in the air from entering the magnesium system.

[0021] Preferably, the emulsifier is one or more of JFC-165, TX-10 and AEO-9.

[0022] The beneficial effects of the present invention are:

[0023] 1. The present invention realizes rolling and kneading of adhesive particles on the x, y, and z axes of space, breaks up large particles of adhesive, and kneads the particle size of adhesive particles to 200-600 meshes, so that the gap after the adhesive is formed is smaller, and the passivation on the adhesive surface is removed at the same time, thereby improving the reactivity of the adhesive, improving the reaction effect of the adhesive, further reducing the gap existing after the adhesive is formed, and improving the performance of isolating carbon dioxide and water vapor in the air from entering and exiting the magnesium oxide system. In addition, the present invention adopts the method of lifting and kneading, and when the adhesive particles and auxiliary fillers flow out and fall from the top port of the spiral channel, under the action of gravity, the adhesive particles at the bottom of the inner cylinder will be hit by the kneading medium (steel ball), further improving the kneading effect of the adhesive.

[0024] 2. The setting of the cooling water jacket can provide a water cooling system for the kneading process of the adhesive to ensure the stability of the kneading process.

[0025] 3. The setting of the circulation pipe makes it convenient to transfer the materials that do not meet the fineness standards back to the inner cylinder for repeated kneading.

[0026] 4. A filter screen is provided on the discharge hole. The material particles that meet the fineness requirements can enter the outer cylinder through the discharge hole and are finally discharged from the discharge pipe. The particles that do not meet the fineness requirements are intercepted by the filter screen and continue to be kneaded in the inner cylinder.

[0027] 5. The rotation directions of the hollow shaft torque motor and the stirring motor are opposite, which can achieve a more complete stirring and kneading effect.

[0028] 6. Overflow ports are provided at every quarter of the circumference of the spiral baffle, which allows the material to flow downward in each section under the action of centrifugal force, thereby improving the mixing effect between materials.

[0029] 7. The inner wall of the spiral channel is provided with a wear-resistant coating to improve wear resistance and extend the service life of the device.

[0030] 8. The activated filler is prepared from lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate. After rubbing the adhesive particles, the passivation on the surface of the adhesive particles can be removed, the surface activity of the adhesive particles can be improved, and the adhesive particles can be activated so that the effective ingredients of the adhesive particles can reach more than 85%, making the gaps smaller after the adhesive is cured and formed, thereby improving the performance of the integrated house wall panels in isolating carbon dioxide and water vapor in the air from entering the magnesium system. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic diagram of the internal structure of the kneading device of the adhesive according to the embodiment of the present invention Figure 1 ;

[0032] Figure 2 Schematic diagram of the internal structure of the kneading device of the adhesive according to the embodiment of the present invention Figure 2 ;

[0033] Figure 3 The present invention is a ternary phase diagram of the MgO-MgCl2-H2O system at 22-28°C inside the integrated house wall panels bonded by the adhesive prepared by the embodiment of the present invention.

[0034] Description of reference numerals:

[0035] 1. Inner cylinder; 101. Feed hole; 102. Discharge hole; 201. Feed port; 2. Outer cylinder; 3. Hollow shaft torque motor; 4. Stirring motor; 5. Spiral baffle; 6. Discharge pipe; 7. Cooling water jacket; 8. Water inlet; 9. Water outlet; 10. Circulation pipe; 11. Stirring shaft; 12. Gear pump. DETAILED DESCRIPTION

[0036] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0037] Example:

[0038] like Figure 1 and Figure 2As shown, a kneading device for adhesive comprises an outer cylinder 2 and an inner cylinder 1, wherein the inner cylinder 1 is arranged inside the outer cylinder 2, and a spiral baffle 5 is spirally arranged on the outer wall of the inner cylinder 1 along its length direction, and a gap is formed between the side of the spiral baffle 5 away from the inner cylinder 1 and the inner wall of the outer cylinder 2, and a spiral channel for adhesive particles and auxiliary fillers to pass through is formed between the spiral baffle 5 and the outer wall of the inner cylinder 1; a hollow shaft torque motor 3 is arranged on the top of the outer cylinder 2, and the stator of the hollow shaft torque motor 3 is arranged on the top of the outer cylinder 2, and the rotor of the hollow shaft torque motor 3 is connected to the top of the inner cylinder 1, and the outer cylinder 2 A stirring motor 4 is also provided at the top through a support seat, and the output shaft of the stirring motor 4 is connected to a stirring shaft 11 that passes through the middle through hole of the hollow shaft torque motor 3 and is arranged in the inner cylinder 1; a plurality of feed holes 101 are provided at the top of the inner cylinder 1 corresponding to the output end of the spiral channel, and the feed holes 101 are preferably 8 holes evenly distributed circumferentially, and a plurality of discharge holes 102 are provided at the bottom of the inner cylinder 1, and the discharge holes 102 are preferably 8 holes evenly distributed circumferentially, a discharge pipe 6 is provided at the bottom of the outer cylinder 2, and a plurality of feeding ports 201 corresponding to the feed holes 101 on the inner cylinder 1 are provided at the top of the outer cylinder 2.

[0039] After the adhesive particles to be processed, the auxiliary filler and the kneading medium (steel balls) are mixed, the feeding tube is inserted from the feeding port 201 on the outer cylinder 2 above the feeding hole 101 on the inner cylinder 1, and the material is poured into the inner cylinder 1 of the device through the feeding tube. The inner cylinder 1 is driven to rotate by the hollow shaft torque motor 3, and the stirring shaft 11 inside the inner cylinder 1 is driven to rotate by the stirring motor 4. The stirring shaft 11 stirs the material in the inner cylinder 1 to knead the material, and the kneaded fine particles are discharged from the discharge hole 102 on the inner cylinder 1 into the outer cylinder 2. When the inner cylinder 1 rotates, the fine material in the outer cylinder 2 is stirred into the spiral channel and is stirred by the spiral channel. The material is lifted and re-entered into the inner cylinder 1 from the feed hole 101 at the top of the inner cylinder 1 to perform repeated kneading treatment. The present invention realizes rolling kneading of adhesive particles on the x, y, and z axes of space through multiple cycles of kneading treatment, breaks up large particles of adhesive, and rubs the particle size of adhesive particles to 200 mesh-600 mesh. The gap after the adhesive is formed is smaller, and the passivation on the surface of the adhesive is removed at the same time, thereby improving the reaction activity of the adhesive, improving the reaction effect of the adhesive, further reducing the gap existing after the adhesive is formed, and improving the effect of isolating carbon dioxide and water vapor in the air. In addition, the present invention adopts the method of lifting and kneading. When the adhesive particles and auxiliary fillers flow out and fall from the top port of the spiral channel, under the action of gravity, the adhesive particles at the bottom of the inner cylinder will be hit by the kneading medium (steel ball), which further improves the kneading effect of the adhesive.

[0040] In one embodiment, if Figure 1 and Figure 2As shown, a cooling water jacket 7 is provided on the outside of the outer cylinder 2, and a water inlet 8 and a water outlet 9 are provided at the bottom and the top of the cooling water jacket 7 respectively. The setting of the cooling water jacket 7 can provide a water cooling system for the kneading process of the adhesive to ensure the stable progress of the kneading process.

[0041] In one embodiment, if Figure 1 and Figure 2 As shown, the discharge pipe 6 is connected to a circulation pipe 10, and one end of the circulation pipe 10 away from the discharge pipe 6 extends to the inner top of the outer cylinder 2, and the port of the circulation pipe 10 is located at the output end of the spiral channel. The setting of the circulation pipe 10 facilitates the re-transfer of materials that do not meet the fineness standards to the inner cylinder 1 for repeated kneading. The circulation pipe 10 is provided with a gear pump 12 to provide power for the circulation of the material.

[0042] In one embodiment, a filter screen is provided on the discharge hole 102, and material particles that meet the fineness requirements can enter the outer cylinder 2 through the discharge hole 102 and are finally discharged from the discharge pipe 6. Those that do not meet the fineness requirements are intercepted by the filter screen and continue to be kneaded in the inner cylinder 1.

[0043] In one embodiment, the hollow shaft torque motor 3 and the stirring motor 4 rotate in opposite directions, which can achieve a more sufficient stirring and kneading effect.

[0044] In one embodiment, overflow ports are provided at each quarter of the circumference of the spiral baffle 5, so that the material can flow downward in each section under the action of centrifugal force, thereby improving the mixing effect between the materials.

[0045] In one of the embodiments, the surface of the spiral baffle 5, the outer wall of the inner cylinder 1 and the inner wall of the outer cylinder 2 are respectively provided with a wear-resistant coating (the wear-resistant coating can be made of high manganese steel, wear-resistant chromium cast iron material or wear-resistant ceramic lining) to improve wear resistance and extend the service life of the device.

[0046] A kneading process of an adhesive comprises the following steps:

[0047] S1. Take adhesive particles, auxiliary fillers and kneading medium (steel balls) and mix them evenly;

[0048] S2, adding the uniformly mixed adhesive particles, auxiliary fillers and kneading medium (steel balls) into the inner cylinder;

[0049] S3. Start the motor and adjust the motor speed to 300r / min-500r / min, knead the adhesive particles and filter them while kneading. The adhesive particles with auxiliary fillers are in a viscous liquid state. The motor speed needs to be controlled at more than 300r / min to achieve the effect of pushing the material into the spiral channel and flowing upward along the spiral channel. At the same time, if the motor speed is too fast, it will affect the kneading effect of the adhesive.

[0050] In one embodiment, the auxiliary filler includes a liquid filler and an activated filler, the liquid filler includes acrylic emulsion, chloroprene latex, terpene resin, coupling agent, thickener and emulsifier; the activated filler includes lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate.

[0051] In one embodiment, the weight ratios of lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate to the adhesive particles are 2%-2.5%, 5%-8%, 10%-20%, 10%-15%, 10%-15% and 5%-8% respectively.

[0052] The activated filler is prepared from lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate. After the adhesive particles are rubbed, the passivation on the surface of the adhesive particles can be removed, the surface activity of the adhesive particles can be improved, and the adhesive particles can be activated so that the effective ingredients of the adhesive particles can reach more than 85%, so that the gaps existing after the adhesive is cured and formed are smaller, and the performance of the integrated house wall panels in isolating carbon dioxide and water vapor in the air from entering the magnesium system is improved.

[0053] In one embodiment, the emulsifier is one or more of JFC-165, TX-10 and AEO-9.

[0054] The adhesive kneaded by the kneading device of the embodiment of the present invention is bonded to the integrated house wall panels. After curing and forming, the ternary phase diagram of the MgO-MgCl2-H2O system inside the integrated house wall panels at 22-28°C is as follows: Figure 3 As shown, where:

[0055] A-MgO-Mg(OH)2-5·1·8; B-MgO-5·1·8-3·1·8; C-MgO-3·1·8-MgCl2·6H2O; D-3·1·8-MgCl2·6H2O-GEL; E-3·1·8-5·1·8-GEL; F-5·1·8-Mg(OH)2-GEL; G-Mg(OH)2-GEL; H-MgCl2-GEL-5·1·8; I-3·1·8-GEL; J-MgCl2·6H2O-GEL; K-GEL; L-GEL-liquid phase.

[0056] The MgO-MgCl2-H2O system inside the integrated house wall panels bonded by the adhesive after rubbing by the rubbing device of the present invention is in area A in the above figure. The system has good stability and has good waterproof performance while ensuring the bonding strength. The balance of the system is not easy to break, which fundamentally plays an effect of preventing seven harmful phenomena such as halogen backflow, frost, warping and cracks.

[0057] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. An adhesive kneading device, comprising an outer cylinder and an inner cylinder, characterized in that: The inner cylinder is arranged inside the outer cylinder, and a spiral baffle is spirally arranged on the outer wall of the inner cylinder along its length direction, and a gap is provided between the side of the spiral baffle away from the inner cylinder and the inner wall of the outer cylinder, and a spiral channel is formed between the spiral baffle and the outer wall of the inner cylinder; a hollow shaft torque motor is arranged on the top of the outer cylinder, and the stator of the hollow shaft torque motor is arranged on the top of the outer cylinder, and the rotor of the hollow shaft torque motor is connected to the top of the inner cylinder, and a stirring motor is also arranged on the top of the outer cylinder through a support seat, and the output shaft of the stirring motor is connected to a stirring shaft that passes through the middle through hole of the hollow shaft torque motor and is arranged in the inner cylinder; the inner cylinder contains a kneading medium, and a top of the inner cylinder corresponding to the output end of the spiral channel is provided There are several feed holes, several discharge holes are arranged at the bottom of the inner cylinder, a discharge pipe is arranged at the bottom of the outer cylinder, and several feeding ports corresponding to the feed holes on the inner cylinder are arranged at the top of the outer cylinder; a cooling water jacket is arranged on the outside of the outer cylinder, and a water inlet and a water outlet are arranged at the bottom and the top of the cooling water jacket respectively; a circulation pipe is connected to the discharge pipe, and the end of the circulation pipe away from the discharge pipe extends to the inner top of the outer cylinder, and the port of the circulation pipe is located at the output end of the spiral channel, and a gear pump is arranged on the circulation pipe; a filter is arranged on the discharge hole; the hollow shaft torque motor and the stirring motor have opposite rotation directions; overflow ports are arranged at each quarter of the circumference of the spiral baffle.

2. A kneading treatment process using the adhesive of the kneading device of claim 1, characterized in that: The following steps are involved: S1. Take adhesive particles, auxiliary fillers and kneading medium and mix them evenly; S2, adding the uniformly mixed adhesive particles, auxiliary fillers and kneading medium into the inner cylinder; S3, start the motor, adjust the motor speed to 300r / min-500r / min, knead the adhesive particles, and filter while kneading.

3. The kneading process of the adhesive according to claim 2, characterized in that: The auxiliary filler includes liquid filler and activated filler. The liquid filler includes acrylic emulsion, chloroprene latex, terpene resin, coupling agent, thickener and emulsifier; the activated filler includes lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate.

4. The kneading process of the adhesive according to claim 3, characterized in that: The weight ratios of lithium silicate, zirconium carbonate, potassium silicate, aluminum oxide, iron oxide and sodium silicate to the adhesive particles are 2%-2.5%, 5%-8%, 10%-20%, 10%-15%, 10%-15% and 5%-8% respectively.

5. The kneading process of the adhesive according to claim 4, characterized in that: The emulsifier is one or more of JFC-165, TX-10 and AEO-9.