Device and method for eliminating internal stress of spandex

By designing thermal setting and quenching treatment equipment for spandex fibers, the molding processing instability and dimensional shrinkage caused by internal stress of spandex fibers is solved, and the dimensional stability and mechanical properties of spandex fibers are improved.

CN111350002BActive Publication Date: 2024-11-26ZHONGYUAN ENGINEERING COLLEGE
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202010377429.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-07
Publication Date
2024-11-26
Estimated Expiration
2040-05-07

AI Technical Summary

Technical Problem

It is difficult to completely eliminate internal stress during the molding process, resulting in unstable molding processing and easy shrinkage of product size, affecting the quality of textiles.

Method used

A device including a wire releaser, a heating box, a cold bellows, a tension roller and a wire collector is designed to eliminate residual internal stress of spandex fibers or yarns through thermal setting and rapid quenching treatment. The specific steps are: After the spandex tow is plasticized in the heating bath, it is shaped by the first tension roller and the second tension roller, and then enters the cold bellows for quenching and stencil, and finally winds up by the wire collector, controlling the temperature and Tension sensor ensures the elimination of internal stress.

Benefits of technology

It effectively eliminates the internal stress of spandex fibers, improves the dimensional stability of the fibers, and improves the orientation of the hard segment of the macromolecule and the degree of microphase separation, enhances the elasticity and mechanical strength of spandex, and the shrinkage rate of boiling water is less than 10%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111350002B_ABST
    Figure CN111350002B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of spandex preparation, and particularly refers to a device and method for eliminating spandex internal stress. The problem of unstable subsequent molding process and easy shrinkage of products caused by the residual internal stress of spandex fiber / yarn is solved. It includes a wire releaser, a first wire guide is arranged on the right side of the wire releaser, a heating box is arranged on the right side of the first wire guider, a cold air box is arranged adjacent to the right side of the heating box, and a fourth wire guider and a wire collector are arranged on the right side of the cold air box in sequence. After the spandex bundle is led out by the wire releaser, it enters the heating bath through the first wire guide, and then is heat-set under tension by the first and second tension rollers. After being quenched in the cold air chamber, it is reeled by the wire collector, and the internal stress can be eliminated. The spandex fiber / yarn passes through the heating bath, the segment temperature is above Tg, and the molecular segment is in a plasticized motion state, which is conducive to the subsequent elimination of internal stress through tension setting, and ensures the dimensional stability of the spandex during subsequent use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of spandex preparation, and in particular relates to a device and a method for eliminating the internal stress of spandex. Background Art

[0002] Spandex is the abbreviation of a fiber with polyurethane (polyurethane) as the main component. Its English name is Polyurethane fiber, and its international name is Spandex. Spandex has excellent elastic properties that other fibers do not have. Its elongation at break is generally 400%-700%; the elastic recovery rate after 300% elongation can reach more than 95%. Since adding 6%-8% of spandex to the fabric will make the fabric have good elasticity, it can give textiles comfort that other fibers do not have, and greatly improve the grade of clothing. Therefore, spandex is often praised as the "MSG in textile fibers" and is an indispensable special fiber for the development of high-end elastic textiles. Due to the long soft segment chain of spandex fiber molecules, the force it is subjected to during the molding process cannot be completely eliminated, and it is very easy to store internal stress, which is not conducive to the implementation of its subsequent weaving molding and dyeing and finishing processes, and the product quality cannot be guaranteed. In the prior art, spandex is mostly mixed with natural fibers and chemical fibers in different proportions, knitted or woven into various forms of elastic fabrics, and then the fabrics are heat-set to eliminate internal stress to achieve the purpose of stabilizing the size of the product. With the improvement of textile technology and consumers' requirements for clothing comfort, the proportion of spandex added to textile fabrics is increasing, and it is necessary to develop relevant technologies and equipment to solve the adverse effects of spandex fiber and yarn internal stress on molding and product quality. Summary of the invention

[0003] The invention provides a device and method for eliminating spandex internal stress, which eliminates the residual internal stress in spandex fibers or yarns by designing heat setting equipment and processing methods, thereby solving the problems of unstable molding process and easy shrinkage of product size caused by residual internal stress.

[0004] The technical solution of the present invention is achieved in this way:

[0005] A device for eliminating internal stress of spandex comprises a wire unwinder, a first wire guide is arranged on the right side of the wire unwinder, a heating box is arranged on the right side of the first wire guide, a cold air box is arranged adjacent to the right side of the heating box, a fourth wire guide and a wire collector are arranged in sequence on the right side of the cold air box. In order to improve efficiency, a plurality of the above-mentioned devices for eliminating internal stress of spandex can be arranged perpendicular to the moving direction of the yarn bundle.

[0006] The heating box is also provided with a heating bath, a second wire guide, a first tension roller, a second tension roller and a third wire guide from left to right; the heating bath is located on the right side of the first wire guide, and the cold air box is located between the third wire guide and the fourth wire guide.

[0007] The motors on the wire unwinder, the first wire guide, the second wire guide, the third wire guide, the fourth wire guide and the wire collector are all provided with a torque display system, and the torque is 10-100Nm.

[0008] The first tension roller and the second tension roller are connected with a tension sensor, which is connected to a controller. The tension applied by the first tension roller is 10-100 grams-force, and the tension applied by the second tension roller is 50-200 grams-force.

[0009] The method for eliminating the internal stress of spandex by using the device comprises the following steps: the spandex tow is led out from the unwinding device and enters into the heating bath built in the heating box; after being plasticized in the heating bath, the spandex tow is introduced into the first tension roller through the second guide for primary shaping treatment; the spandex tow is then subjected to secondary shaping treatment by the second tension roller; the spandex tow is then sent into the cold air box through the third guide for rapid quenching and shaping; and finally is wound up by the winder.

[0010] The temperature of the heating bath is controlled at (Tg+30)-(Tg+80)°C (Tg is the glass transition temperature of the spandex fiber, measured by DSC or DMA), and the heating medium in the bath is a solvent containing hydroxyl groups, which is water, diethylene glycol, ethylene glycol or glycerol.

[0011] The heating box adopts multi-stage temperature control, the heating medium is moist hot air or dry hot gas, the temperature range is (Tg+20)-(Tm-50)℃ (Tm is the melting temperature of spandex, measured by DSC or melting point meter), and the temperature of the second tension roller is 10-60℃ higher than that of the first tension roller.

[0012] The temperature of the cold air box is 10-25°C, and the cooling time is 5-30s.

[0013] The time from the spandex tow entering the unwinder to being wound up by the winder is controlled at 20-300s. After heat treatment, the internal stress is eliminated and the fiber boiling water shrinkage is less than 10%.

[0014] The present invention has the following beneficial effects:

[0015] 1. After the spandex tow is led out by the unwinder, it enters the heating bath through the first yarn guide, and then is heat-set under tension by the first and second tension rollers. After being rapidly cooled in the cold air chamber, it is reeled up by the reel, thereby eliminating the internal stress. When the spandex fiber / yarn passes through the heating bath, the chain segment temperature is above Tg, and the molecular chain segment is in a plasticized motion state, which is conducive to the subsequent elimination of internal stress through tension setting, thereby ensuring the dimensional stability of the spandex during use.

[0016] 2. Through this technical solution, the degree of orientation of the hard segment and the degree of microphase separation in the spandex macromolecule can be improved at the same time, which is beneficial to the improvement of the elasticity and mechanical strength of the spandex (the increase is more than 5%). BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 This is a schematic diagram of the spandex internal stress elimination equipment for this application.

[0019] Figure 2 This is a schematic diagram of the spandex internal stress elimination process for this application.

[0020] Figure 3 This is an electron microscope comparison of spandex before and after the internal stress is eliminated in Example 1.

[0021] Figure 4 This is an electron microscope comparison of spandex before and after the internal stress is eliminated in Example 2. DETAILED DESCRIPTION

[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] like Figure 1 As shown, the present invention provides a device for eliminating the internal stress of spandex, including a wire release device 1, a first wire guide 2 is arranged on the right side of the wire release device 1, a heating box is arranged on the right side of the first wire guide 2 (the heating box is a steam heating box purchased from Jiangyin Shunfeng Chemical Fiber Equipment Co., Ltd.; or a dry hot gas heating box purchased from Jingjiang Yonghong Chemical Fiber Equipment Factory), a cold air box (chemical fiber side blowing cold air box purchased from Jingjiang Kaiyu Air Conditioning Equipment Factory) is arranged adjacent to the right side of the heating box, and a fourth wire guide 8 and a wire collector 9 are arranged on the right side of the cold air box in sequence. In order to improve efficiency, multiple devices for eliminating the internal stress of spandex can be arranged perpendicular to the direction of movement of the tow.

[0024] The heating box is also provided with a heating bath 3, a second wire guide 4, a first tension roller 5, a second tension roller 6 and a third wire guide 7 from left to right; the heating bath 3 is located on the right side of the first wire guide 2, and the cold air box is located between the third wire guide 7 and the fourth wire guide 8.

[0025] The motors on the wire unwinder 1, the first wire guide 2, the second wire guide 4, the third wire guide 7, the fourth wire guide 8 and the wire collector 9 are all provided with a torque display system, and the torque is 10-100 Nm.

[0026] The first tension roller 5 and the second tension roller 6 are connected with tension sensors, which are connected to a controller. The first tension roller 5 applies a tension of 10-100 grams-force, and the second tension roller 6 applies a tension of 50-200 grams-force.

[0027] A method for eliminating internal stress of spandex using the device, such as Figure 2 As shown in the process, the specific method steps are as follows: the spandex tow is led out from the unwinder 1 and enters the heating bath 3 built into the heating box; after being plasticized in the heating bath 3, it is introduced into the first tension roller 5 through the second yarn guide 4 for a primary shaping treatment; then it is subjected to a secondary shaping treatment through the second tension roller 6; thereafter, it is sent into the cold air box through the third yarn guide 7 for rapid quenching and shaping; and finally it is wound up by the yarn collector 9.

[0028] The temperature of the heating bath 3 is controlled at (Tg+30)-(Tg+80)°C (Tg is the glass transition temperature of the spandex fiber, measured by DSC or DMA), and the heating medium in the bath is a solvent containing hydroxyl groups, and the solvent containing hydroxyl groups is water, diethylene glycol, ethylene glycol or glycerol.

[0029] The heating box adopts multi-stage temperature control, and the heating medium is moist hot air or dry hot gas, wherein the dry hot gas can be dry hot air, nitrogen, or argon. The temperature range is (Tg+20)-(Tm-50)°C (Tm is the melting temperature of spandex, measured by DSC or melting point meter), and the temperature of the second tension roller is 10-60°C higher than that of the first tension roller.

[0030] The temperature of the cold air box is 10-25°C, and the cooling time is 5-30s.

[0031] The time from the spandex tow entering the unwinding device 1 to being wound up by the winding device 9 is controlled within 20-300 seconds. After the heat treatment, the internal stress is eliminated and the fiber boiling water shrinkage rate is less than 10%.

[0032] Example 1

[0033] The method of eliminating the internal stress of spandex by using the equipment in this embodiment comprises the following steps:

[0034] The spandex tow is led out from the unwinder into the ethylene glycol bath (temperature set to Tg+30℃) built into the heating box. After plasticization in the bath, it is first shaped by the first tension roller (temperature set to Tg+30℃, tension 10gf), and then shaped by the second tension roller (temperature set to Tg+40℃, tension 50gf). It is then sent into the cold air box (temperature set to 20℃) through the third yarn guide for rapid quenching and shaping, and finally reeled by the collector.

[0035] The temperature control of the heating box is divided into three sections, with the box temperatures of Tg+20°C, Tg+30°C, and Tg+40°C. The heating medium is dry hot air. The motors on the wire unwinder 1, the first wire guide 2, the second wire guide 4, the third wire guide 7, the fourth wire guide 8, and the wire collector 9 are all equipped with a torque display system with a torque of 10 Nm. The heat setting time is 30 s, the cooling setting time is 5 s, and the boiling water shrinkage of the fiber after setting is 7.6%.

[0036] For specific electron micrographs, see Figure 3 , Figure 3 (a) and (b) are microscope photos (500X) of spandex fibers before and after internal stress elimination and boiling water shrinkage test. It can be seen that the diameter of the untreated fiber is significantly higher than that of the treated fiber, and the fiber surface of the former is rougher, indicating that the shrinkage of the fiber is significantly reduced after treatment.

[0037] Example 2

[0038] The method of eliminating the internal stress of spandex by using the equipment in this embodiment comprises the following steps:

[0039] The spandex tow is led out from the unwinder and enters the water bath built into the heating box (temperature set to Tg+80℃). After plasticization in the bath, it is first shaped by the first tension roller (temperature set to Tg+70℃, tension 100g-f), and then shaped by the second tension roller (temperature set to Tg+130℃, tension 80g-f). It is then sent into the cold air box (temperature set to 10℃) through the third yarn guide for rapid quenching and shaping, and finally reeled by the collector.

[0040] The temperature control of the heating box is divided into 5 sections, and the box temperature is Tg+30℃, Tg+40℃, Tg+50℃, Tg+60℃, Tg+70℃. The heating medium is dry hot nitrogen. The motors on the wire unwinder 1, the first wire guide 2, the second wire guide 4, the third wire guide 7, the fourth wire guide 8 and the wire collector 9 are all equipped with a torque display system with a torque of 60Nm. The heat setting time is 100s, the cooling setting time is 5s, and the boiling water shrinkage of the fiber after setting is 4.2%.

[0041] For specific electron micrographs, see Figure 4 , Figure 4 (a) and (b) are microscope photos (500x) of spandex fibers before and after internal stress elimination and boiling water shrinkage test. It can be seen that the diameter of the untreated fiber is significantly higher than that of the treated fiber, and the fiber surface of the former is rougher, indicating that the shrinkage of the fiber is significantly reduced after treatment.

[0042] Example 3

[0043] The method of eliminating the internal stress of spandex by using the equipment in this embodiment comprises the following steps:

[0044] The spandex tow is led out from the unwinder and enters the diethylene glycol bath (temperature set to Tg+30℃) built into the heating box. After plasticization in the bath, it is first shaped by the first tension roller (temperature set to Tg+30℃, tension 70gf), and then shaped by the second tension roller (temperature set to Tg+80℃, tension 100gf). It is then sent into the cold air box (temperature set to 25℃) through the third guide roller for rapid quenching and shaping, and finally reeled by the collector.

[0045] The temperature control of the heating box is divided into 4 sections, with the box temperatures of Tg+20°C, Tg+40°C, Tg+60°C, and Tm-50°C. The heating medium is dry hot argon gas. The motors on the wire unwinder 1, the first wire guide 2, the second wire guide 4, the third wire guide 7, the fourth wire guide 8, and the wire collector 9 are all equipped with a torque display system with a torque of 100Nm. The heat setting time is 300s, the cooling setting time is 10s, and the boiling water shrinkage of the fiber after setting is 6.8%.

[0046] Example 4

[0047] The method of eliminating the internal stress of spandex by using the equipment in this embodiment comprises the following steps:

[0048] The spandex tow is led out from the unwinder into the glycerin bath (temperature set to Tg+70℃) built into the heating box. After plasticization in the bath, it is first shaped by the first tension roller (temperature set to Tg+80℃, tension 20gf), then shaped by the second tension roller (temperature set to Tg+110℃, tension 100gf), and then sent into the cold air box (temperature set to 15℃) through the third yarn guide for rapid quenching and shaping, and finally reeled by the collector.

[0049] The temperature control of the heating box is divided into 6 sections, and the box temperature is Tg+50℃, Tg+60℃, Tg+70℃, Tg+80℃, Tg+90℃, Tg+110℃. The heating medium is hot and humid air. The motors on the wire unwinder 1, the first wire guide 2, the second wire guide 4, the third wire guide 7, the fourth wire guide 8 and the wire collector 9 are all equipped with a torque display system with a torque of 30Nm. The heat setting time is 60s, the cooling setting time is 15s, and the boiling water shrinkage of the fiber after setting is 8.1%.

[0050] Example 5

[0051] The method of eliminating the internal stress of spandex by using the equipment in this embodiment comprises the following steps:

[0052] The spandex tow is led out from the unwinder and enters the water bath built into the heating box (temperature set to Tg+30℃). After plasticization in the bath, it is first shaped by the first tension roller (temperature set to Tg+50℃, tension 80gf), and then shaped by the second tension roller (temperature set to Tg+70℃, tension 200gf). It is then sent into the cold air box (temperature set to 15℃) through the third yarn guide for rapid quenching and shaping, and finally reeled by the collector.

[0053] The temperature control of the heating box is divided into three sections, with the box temperatures of Tg+40°C, Tg+50°C, and Tg+70°C. The heating medium is dry hot air. The motors on the wire unwinder 1, the first wire guide 2, the second wire guide 4, the third wire guide 7, the fourth wire guide 8, and the wire collector 9 are all equipped with a torque display system with a torque of 30 Nm. The heat setting time is 60 s, the cooling setting time is 30 s, and the boiling water shrinkage of the fiber after setting is 5.7%.

[0054] Example 6

[0055] The method of eliminating the internal stress of spandex by using the equipment in this embodiment comprises the following steps:

[0056] The spandex tow is led out from the unwinder into the glycerin bath (temperature set to Tg+40℃) built into the heating box. After plasticization in the bath, it is first shaped by the first tension roller (temperature set to Tg+40℃, tension 100 grams-force), and then shaped by the second tension roller (temperature set to Tg+70℃, tension 150 grams-force). It is then sent into the cold air box (temperature set to 10℃) through the third yarn guide for rapid quenching and shaping, and finally reeled by the collector.

[0057] The temperature control of the heating box is divided into 4 sections, and the box temperature is Tg+20℃, Tg+40℃, Tg+80℃, Tm-100℃. The heating medium is dry hot nitrogen. The motors on the wire unwinder 1, the first wire guide 2, the second wire guide 4, the third wire guide 7, the fourth wire guide 8 and the wire collector 9 are all equipped with a torque display system with a torque of 50Nm. The heat setting time is 90s, the cooling setting time is 10s, and the boiling water shrinkage of the fiber after setting is 6.3%.

[0058] Table 1 shows the physical properties of the spandex fibers in the examples.

[0059]

[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for eliminating internal stress of spandex, characterized in that: The method is implemented based on a device for eliminating the internal stress of spandex. The device comprises a wire unwinder (1), a first wire guide (2) is arranged on the right side of the wire unwinder (1), a heating box is arranged on the right side of the first wire guide (2), a cold air box is arranged adjacent to the right side of the heating box, and a fourth wire guide (8) and a wire collector (9) are arranged in sequence on the right side of the cold air box; The heating box is also provided with a heating bath (3), a second yarn guide (4), a first tension roller (5), a second tension roller (6) and a third yarn guide (7) from left to right; the heating bath (3) is located on the right side of the first yarn guide (2), and the cold air box is located between the third yarn guide (7) and the fourth yarn guide (8); The steps of eliminating the internal stress of spandex are as follows: the spandex tow is led out from the unwinding device (1) and enters the heating bath (3) built in the heating box, and after being plasticized in the heating bath (3), it is introduced into the first tension roller (5) through the second yarn guide (4) for primary shaping treatment, and then is subjected to secondary shaping treatment by the second tension roller (6), and then is sent into the cold air box through the third yarn guide (7) for rapid quenching and shaping, and finally is wound up by the yarn collector (9); The temperature of the heating bath (3) is controlled at (Tg+30)-(Tg+80)°C, and the heating medium in the bath is a solvent containing hydroxyl groups, and the solvent containing hydroxyl groups is water, diethylene glycol, ethylene glycol or glycerol.

2. The method for eliminating internal stress of spandex according to claim 1, characterized in that: The motors on the wire unwinder (1), the first wire guide (2), the second wire guide (4), the third wire guide (7), the fourth wire guide (8) and the wire collector (9) are all equipped with a torque display system, and the torque is 10-100 Nm.

3. The method for eliminating internal stress of spandex according to claim 2, characterized in that: The first tension roller (5) and the second tension roller (6) are connected to tension sensors, which are connected to a controller. The tension applied by the first tension roller (5) is 10-100 grams of force, and the tension applied by the second tension roller (6) is 50-200 grams of force.

4. The method for eliminating internal stress of spandex according to claim 1, characterized in that: The heating box adopts multi-stage temperature control, the heating medium is moist hot air or dry hot gas, the temperature range is (Tg+20)-(Tm-50)℃, and the temperature of the second tension roller is 10-60℃ higher than that of the first tension roller.

5. The method for eliminating internal stress of spandex according to claim 1, characterized in that: The temperature of the cold air box is 10-25°C, and the cooling time is 5-30s.

6. The method for eliminating internal stress of spandex according to claim 1, characterized in that: The time from the spandex tow entering the tow unwinder (1) to the tow being reeled up by the tow reel (9) is controlled within 20-300 seconds.

Citation Information

Patent Citations

  • Corterra fully-drafted filament drafting and winding device

    CN102586909A

  • Polyurethane elastic fiber with improved heat-setting performance, and preparation method thereof

    CN104726960A

  • Spandex fibers with good heat resistance and low-temperature setting property and preparation method

    CN109487361A

  • Spandex fiber with good heat stability and preparation method of spandex fiber

    CN110760945A

  • Equipment for eliminating internal stress of spandex

    CN212640744U