Bipolar triode device and preparation method thereof

By using a P-type single-crystal silicon-germanium alloy base region doped with carbon atoms and a heavily doped N+-type single-crystal silicon emitter region in a bipolar transistor, combined with a reverse PN junction and an edge isolation region, the existing dual The problem of poor current gain and isolation effect of polar transistors has been achieved, and the performance of high frequency and low noise has been improved.

CN111354776BActive Publication Date: 2024-10-29WEEN SEMICON TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN201811573593.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-12-21
Publication Date
2024-10-29
Estimated Expiration
2038-12-21

AI Technical Summary

Technical Problem

The current gain of existing bipolar transistors is not large enough and the isolation effect from other devices is not good, making it difficult to meet the needs of semiconductor devices in high-frequency and low-noise environments.

Method used

It adopts a bipolar transistor structure composed of a lightly doped N-type single crystal silicon epitaxial layer, a carbon atom-doped P-type single crystal silicon germanium alloy base region, and a heavily doped N+ type single crystal silicon emitter region, and By forming a reverse PN junction and edge isolation area on the substrate, the current gain and isolation effect are improved.

Benefits of technology

It achieves the high current gain and good isolation effect of bipolar transistors, improves the frequency characteristics and reliability of the device, and reduces noise and leakage current.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111354776B_ABST
    Figure CN111354776B_ABST
Patent Text Reader

Abstract

The invention discloses a bipolar triode device and a preparation method thereof, wherein the bipolar triode device comprises a substrate, an epitaxial layer and a bipolar triode; the bipolar triode comprises: a collector region composed of a lightly doped N-type single crystal silicon epitaxial layer; a base region composed of a P-type single crystal silicon germanium alloy doped with carbon atoms, wherein the content of germanium in the P-type single crystal silicon germanium alloy increases from zero to a first threshold along a first direction and then decreases to zero; an emitter region composed of heavily doped N+ type single crystal silicon; a metal electrode, comprising a collector, a base and an emitter; the substrate is a heavily doped P+ type single crystal silicon substrate; the epitaxial layer comprises a lightly doped P-type single crystal silicon epitaxial layer and a heavily doped N+ type single crystal silicon epitaxial layer stacked along a first direction, and the collector region is located on the N+ type single crystal silicon epitaxial layer, so that a reverse PN junction isolation is formed between the P+ type single crystal silicon substrate and the collector region. The bipolar triode device of this embodiment has a higher current gain and a better isolation effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor technology, and in particular relates to a bipolar triode device and a preparation method thereof. Background Art

[0002] With the rapid development of semiconductor manufacturing, the number of transistors integrated on the chip is increasing, and the speed of the circuit is getting faster and faster. Bipolar transistors have become a commonly used electronic device in the semiconductor industry because they have the advantages of CMOS technology, good high-frequency performance, low preparation cost and excellent noise performance.

[0003] Existing bipolar transistors generally use a pure silicon base region, or a base region of a silicon-germanium alloy uniformly doped in a certain proportion, the current gain is not large enough, and the isolation effect of the existing bipolar transistors and other devices is not good.

[0004] Therefore, there is an urgent need for a bipolar transistor that can improve current gain and has a better isolation effect. Summary of the invention

[0005] The embodiment of the present invention provides a bipolar triode device and a preparation method thereof, which can achieve a higher current gain and a better isolation effect of the bipolar triode device.

[0006] On the one hand, the present invention provides a bipolar triode device, comprising a substrate, an epitaxial layer stacked in sequence on the substrate along a first direction, and a bipolar triode; the bipolar triode comprises: a collector region, composed of a lightly doped N-type single crystal silicon epitaxial layer; a base region, stacked in the first direction on a side of the collector region away from the substrate, the base region being composed of a P-type single crystal silicon germanium alloy doped with carbon atoms, the germanium content in the P-type single crystal silicon germanium alloy increasing from zero to a first threshold value along the first direction and then decreasing to zero; an emitter region , stacked along a first direction on a side of the base region away from the substrate, and composed of heavily doped N+ type single crystal silicon; a metal electrode, including a collector, a base and an emitter, the collector is electrically connected to the collector region, the base is electrically connected to the base region, and the emitter is electrically connected to the emitter region; a first edge isolation region is arranged on the peripheral side of the bipolar triode, the first edge isolation region includes a first groove arranged along a first direction, the first groove extends from the N-type single crystal silicon epitaxial layer to the substrate, the first groove is filled with polysilicon, and the inner surface of the first groove The substrate is a heavily doped P+ type single crystal silicon substrate, the epitaxial layer includes a lightly doped P- type single crystal silicon epitaxial layer and a heavily doped N+ type single crystal silicon epitaxial layer, and the collector region is located on the N+ type single crystal silicon epitaxial layer, so that a reverse PN junction isolation is formed between the P+ type single crystal silicon substrate and the collector region; the thickness of the P+ type single crystal silicon substrate is 600 microns to 800 microns, the thickness of the P- type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the P- type single crystal silicon epitaxial layer is 1E16cm -3 The thickness of the N+ type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the N+ type single crystal silicon epitaxial layer is 1E19cm -3 The thickness of the N-type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the N-type single crystal silicon epitaxial layer is 1E16cm -3 According to one aspect of the present invention, the depth of the first groove is 6 microns to 10 microns, the depth of the second groove is 0.4 microns to 0.6 microns, the thickness of the oxide layer in the first groove is 800 angstroms to 1200 angstroms, the thickness of the oxide layer in the second groove is 100 angstroms to 300 angstroms, the thickness of the polysilicon is greater than half the width of the first groove, and the thickness of the high-density plasma oxide layer is greater than half the width of the second groove.

[0007] According to one aspect of the present invention, the first threshold is the number ratio of germanium atoms to silicon atoms in the P-type single crystal silicon-germanium alloy, and the value range of the first threshold is 30% to 50%.

[0008] According to one aspect of the present invention, the doping content of carbon atoms in the P-type single crystal silicon-germanium alloy is 0.1% to 0.2%, and the doping amount is the ratio of the number of carbon atoms to silicon atoms.

[0009] According to one aspect of the present invention, the thickness of the P-type single crystal silicon germanium alloy in the base region is 100 angstroms to 300 angstroms, and the doping concentration of the P-type single crystal silicon germanium alloy is 1E18 cm -3 Magnitude.

[0010] According to one aspect of the present invention, the bipolar transistor further comprises: a base lead-out region, which is arranged on the peripheral side of the base region and the emitter region and is in electrical contact with the base region, the emitter region and the collector region; the base is arranged on the base lead-out region and is electrically connected to the base region through the base lead-out region; the base lead-out region is composed of P+ type single crystal silicon with a doping concentration gradient; the thickness of the base lead-out region is 1 micron to 2 microns; an emitter lead-out region, which is stacked along a first direction on a side of the emitter region away from the substrate and is in electrical contact with the emitter; the emitter is arranged It is placed on the emitter lead-out region and is electrically connected to the emitter region through the emitter lead-out region. The emitter lead-out region is composed of N+ type polycrystalline silicon, and the thickness of the emitter lead-out region is 1000 angstroms to 3000 angstroms; the collector lead-out region is arranged on one side of the collector region, and one side of the collector region is electrically contacted. The collector is arranged on the collector lead-out region and is electrically connected to the collector region through the collector lead-out region. The collector lead-out region is composed of N+ type single crystal silicon with a doping concentration gradient, and the thickness of the collector lead-out region is 2 microns to 4 microns.

[0011] According to one aspect of the present invention, the material of the metal electrode includes at least one of titanium and copper.

[0012] On the other hand, an embodiment of the present invention provides a method for preparing a bipolar triode device, comprising: providing a P+ type single crystal silicon substrate, and doping to sequentially form a P- type single crystal silicon epitaxial layer, an N+ type single crystal silicon epitaxial layer and an N- type single crystal silicon epitaxial layer on the P+ type single crystal silicon substrate along a first direction, wherein the collector region is located in the N- type single crystal silicon epitaxial layer; forming a first edge isolation region on the peripheral side of the collector region, wherein the first edge isolation region comprises a first groove arranged along a first direction, the first groove extends from the N- type single crystal silicon epitaxial layer to the P+ type single crystal silicon substrate, and the first groove is filled with The invention relates to polycrystalline silicon, wherein an oxide layer is arranged on the inner surface of the first groove to surround the polycrystalline silicon; a second edge isolation region is formed on the side of the first edge isolation region away from the P+ type single crystal silicon substrate, wherein a part of the second edge isolation region corresponds to the first edge isolation region, and the other part is arranged between the base region and the collector region; the second edge isolation region comprises a second groove arranged along the first direction, the second groove is filled with a high-density plasma oxide layer, an oxide layer is arranged on the inner surface of the second groove to surround the high-density plasma oxide layer, and a surface of the second edge isolation region away from the substrate is flush with the collector region; through the first A photolithography process and a first doping process are performed on one side of the collector region to form a collector lead-out region, wherein the collector lead-out region is composed of N+ type single crystal silicon with a doping concentration gradient to lead the N+ epitaxial layer to the surface of the N- type single crystal silicon epitaxial layer; in the corresponding area of ​​the base region, a P-type single crystal silicon germanium alloy is epitaxially grown, and carbon atoms are introduced during the growth process to fill the gaps between atoms, wherein the germanium content in the P-type single crystal silicon germanium alloy increases from zero to a first threshold along a first direction and then decreases to zero; in the corresponding area of ​​the emitter region, an N+ type single crystal silicon layer is epitaxially grown; by The second photolithography process and the second doping process form a base lead-out region with part of the N-type single crystal silicon epitaxial layer, part of the P-type single crystal silicon germanium alloy epitaxial layer and part of the N+ type single crystal silicon layer, wherein the base lead-out region is composed of P+ type single crystal silicon with a doping concentration gradient; through the third photolithography process, a base region and an emitter region are formed; through the fourth photolithography process and the deposition process, N+ type polysilicon is deposited on the N+ type single crystal silicon epitaxial layer in the area corresponding to the emitter lead-out region to form an emitter lead-out region; a preparation process for forming a metal electrode, the metal electrode includes a collector, a base and an emitter.

[0013] According to one aspect of the present invention, in a region corresponding to the base region, epitaxial growth of a P-type single crystal silicon-germanium alloy is performed, and carbon atoms are introduced during the growth process to fill the gaps between atoms, including the steps of: in a silicon-germanium alloy high-vacuum UHV-CVD furnace, after surface hydrogen passivation, by adjusting the flow rates of silicon atoms and germanium atoms, a P-type single crystal silicon-germanium alloy epitaxy is formed in a region corresponding to the base region, in which the germanium content increases from zero to a first threshold along a first direction and then decreases to zero, and carbon atoms are introduced during the formation of the P-type single crystal silicon-germanium alloy epitaxy, and the temperature of the silicon-germanium alloy high-vacuum UHV-CVD furnace is 500°C to 800°C.

[0014] According to one aspect of the present invention, the step of forming a collector lead-out region on the peripheral side of the collector region by a first photolithography process and a first doping process specifically includes: defining a region corresponding to the collector lead-out region by a first photolithography process; performing a photolithography on an N-type single crystal silicon epitaxial layer in a region corresponding to the collector lead-out region at an energy of 30KeV to 70KeV and a doping temperature of 1E14cm -2 ~1E15cm -2 Shallow arsenic ion bombardment was carried out at the level of 200KeV to 600KeV and 1E14cm -2 ~1E15cm -2 Deep phosphorus ion bombardment is carried out under high-level measurement, and arsenic ions and phosphorus ions are injected into the silicon wafer to form a collector lead-out area with an N+ type doping concentration gradient. The photoresist formed in the collector lead-out area in the first photolithography process is then removed, and the silicon wafer is subjected to rapid annealing at 900°C to 1000°C for about 20 seconds to 40 seconds to activate the arsenic ions and phosphorus ions.

[0015] According to one aspect of the present invention, the step of forming a base lead-out region from a portion of an N-type single crystal silicon epitaxial layer, a portion of a P-type single crystal silicon germanium alloy epitaxial layer, and a portion of an N+ type single crystal silicon layer through a second photolithography process and a second doping process comprises: defining a region corresponding to the base lead-out region through a second photolithography process; performing photolithography on the N-type single crystal silicon epitaxial layer, the P-type single crystal silicon germanium alloy, and a portion of the N+ type single crystal silicon layer in the region corresponding to the base lead-out region at an energy of 10KeV to 20KeV and a doping rate of 1E15cm -2 Shallow boron ion bombardment was performed at the level of 100KeV to 200KeV and 1E14cm -2 Deep boron ion bombardment is carried out under high-level measurement, and boron ions are injected into the silicon wafer to form a base lead-out area with a P+ type doping concentration gradient. The photoresist formed in the base lead-out area in the second photolithography process is then removed, and the silicon wafer is subjected to rapid annealing at 900°C to 1000°C for about 20 seconds to 40 seconds to activate the boron ions.

[0016] The bipolar triode device of the embodiment of the present invention is stacked on a substrate, and a reverse PN junction is formed between the collector region and the P+ type single crystal silicon substrate. The current from the emitter through the emitter region and the base region to the collector region will not flow downward to the bottom of the substrate due to the presence of the reverse PN junction, but will directly flow from the collector region to the collector. In addition, the base region is composed of a P-type single crystal silicon germanium alloy doped with carbon atoms, and the germanium content in the P-type single crystal silicon germanium alloy increases from zero to the first threshold along the first direction and then decreases to zero, which has achieved the release of lattice mismatch and adjusted the energy band width of different layers to achieve energy band cutting, so that electrons produce an acceleration effect when moving in the base region, improve current gain, and doping carbon atoms in the P-type single crystal silicon germanium alloy can fill the gaps between atoms, thereby effectively preventing the movement of germanium and impurity atoms in the base region during subsequent thermal processes. The triode device of this embodiment has a higher current gain, and is isolated from other devices by the reverse PN junction, so the isolation effect is good and the reliability is strong. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments of the present invention are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0018] Figure 1 It is a structural schematic diagram of a bipolar triode device provided by an embodiment of the present invention;

[0019] Figure 2 It is a flow chart of a method for preparing a bipolar triode device provided by an embodiment of the present invention;

[0020] Figure 3 It is a flow chart of another method for preparing a bipolar triode device provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0021] The features and exemplary embodiments of various aspects of the present invention will be described in detail below. In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only configured to explain the present invention and are not configured to limit the present invention. For those skilled in the art, the present invention can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present invention by illustrating examples of the present invention.

[0022] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0023] In order to better understand the present invention, Figure 1 and Figure 2 The bipolar transistor device and the preparation method thereof according to the present invention are described in detail.

[0024] It should be noted that in this application, the P+ type single crystal silicon mentioned refers to single crystal silicon formed by heavily doping with boron on single crystal silicon, P- type single crystal silicon refers to single crystal silicon formed by lightly doping with boron on single crystal silicon, N+ type single crystal silicon refers to single crystal silicon formed by heavily doping with phosphorus and / or arsenic on single crystal silicon, and N- type single crystal silicon refers to single crystal silicon formed by lightly doping with phosphorus and / or arsenic on single crystal silicon. The doping concentration mentioned, unless otherwise specified, refers to the concentration of doping with phosphorus and / or arsenic in N-type single crystal silicon, and refers to the concentration of doping with boron in P-type single crystal silicon.

[0025] See also Figure 1 , Figure 1 A schematic structural diagram of a bipolar triode device provided by an embodiment of the present invention comprises a substrate and an epitaxial layer and a bipolar triode sequentially stacked on the substrate along a first direction (Y direction).

[0026] The substrate includes a heavily doped P+ type single crystal silicon substrate 11 , and the epitaxial layer includes a lightly doped P- type single crystal silicon epitaxial layer 12 and a heavily doped N+ type single crystal silicon epitaxial layer 13 .

[0027] The above-mentioned bipolar transistor includes a collector region 21, a base region 22, an emitter region 23 and a metal electrode. The metal electrode includes a collector 211 electrically connected to the collector region 21, a base 221 electrically connected to the base region 22 and an emitter 231 electrically connected to the emitter region 23. The collector region 21 is composed of a lightly doped N-type single crystal silicon epitaxial layer, formed on an N+ type single crystal silicon epitaxial layer 13; the base region 22 is stacked along a first direction on the side of the collector region 21 away from the substrate, and the base region 22 is composed of a P-type single crystal silicon germanium alloy doped with carbon atoms, and the germanium content in the P-type single crystal silicon germanium alloy increases from zero to a first threshold along the first direction and then decreases to zero. The increase or decrease mentioned here can be a step-by-step increase or decrease, or a continuous increase or decrease. Continuous increase or decrease is preferred. The emitter region 23 is stacked along the first direction on the side of the base region 22 away from the substrate, and is composed of heavily doped N+ type single crystal silicon. In this way, a reverse PN junction isolation is formed between the P+ type single crystal silicon substrate 11 and the collector region 21, that is, the bipolar transistor can be isolated from the substrate to prevent the device located on the side of the substrate away from the transistor from affecting the bipolar transistor.

[0028] In an embodiment of the present invention, a bipolar transistor is stacked on a P+ type single crystal silicon substrate, and a collector region 21 of the bipolar transistor is formed by an N- type single crystal silicon epitaxial layer, which is formed on an N+ type single crystal silicon epitaxial layer 13 of the substrate, and a P- type single crystal silicon epitaxial layer 12 and a P+ type single crystal silicon substrate 11 are formed on the side of the N+ type single crystal silicon epitaxial layer 13 away from the collector region 21. In this way, a reverse PN junction is formed between the collector region 21 and the P+ type single crystal silicon substrate 11. The current flowing from the emitter 231 through the emitter region 23 and the base region 22 to the collector region 21 will not flow downward to the bottom of the substrate due to the existence of the reverse PN junction, but will directly flow from the collector region 21 to the collector electrode 211. In addition, the base region 22 is composed of a P-type single crystal silicon-germanium alloy doped with carbon atoms, and the germanium content in the P-type single crystal silicon-germanium alloy increases from zero to a first threshold along the first direction and then decreases to zero, so as to release the lattice mismatch and adjust the energy band width of different layers to achieve energy band tailoring, thereby causing an acceleration effect when electrons move in the base region 22, thereby improving the current gain, and doping carbon atoms in the P-type single crystal silicon-germanium alloy can fill the gaps between atoms, thereby effectively preventing the movement of germanium and impurity atoms in the base region 22 during subsequent thermal processes.

[0029] In some optional embodiments, the germanium content in the P-type single crystal silicon germanium alloy in the base region 22 increases from zero to a first threshold along the first direction and then decreases to zero. The first threshold refers to the ratio of the number of germanium atoms to silicon atoms in the P-type single crystal silicon germanium alloy. The value range of the first threshold is 30% to 50%, preferably 40%. The thickness of the P-type single crystal silicon germanium alloy in the base region is 100 angstroms to 300 angstroms, preferably 200 angstroms, and the doping concentration of the P-type single crystal silicon germanium alloy is 1E18cm -3 Magnitude.

[0030] Furthermore, the doping content of carbon atoms in the P-type single crystal silicon germanium alloy is 0.1% to 0.2%, where the doping content of carbon atoms refers to the ratio of the number of carbon atoms to silicon atoms in the P-type single crystal silicon germanium alloy. Preferably, the doping content of carbon atoms is 0.1%.

[0031] The thickness of the P+ type single crystal silicon substrate 11 is 600 microns to 800 microns, preferably 700 microns. The thickness of the P- type single crystal silicon epitaxial layer 12 is 2 microns to 4 microns, and the doping concentration of the P- type single crystal silicon epitaxial layer 12 is 1E16 cm -3 The thickness of the N+ type single crystal silicon epitaxial layer 13 is 2 microns to 4 microns, and the doping concentration of the N+ type single crystal silicon epitaxial layer 13 is 1E19 cm -3 The order of magnitude can provide a low resistance region to guide the current of the collector region 21 to the collector 211. The thickness of the N-type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the N-type single crystal silicon epitaxial layer is 1E16cm -3 Magnitude.

[0032] In some optional embodiments, the bipolar triode device further includes a first edge isolation region 3, which is arranged on the periphery of the bipolar triode. The first edge isolation region 3 includes a first groove arranged along a first direction, the first groove extends from the N-type single crystal silicon epitaxial layer to the substrate, the first groove is filled with polysilicon, and the inner surface of the first groove is provided with an oxide layer to surround the polysilicon. In this way, by providing the first edge isolation region on the periphery of the bipolar triode, the bipolar triode can be effectively isolated from other surrounding devices, effectively avoiding mutual signal interference and reducing parasitic effects. The depth of the first groove is 6 microns to 10 microns, preferably 8 microns and 9 microns. The thickness of the oxide layer on the inner surface of the first groove is 800 angstroms to 1200 angstroms, preferably 1000 angstroms. The thickness of the polysilicon in the first groove is greater than half of the width of the first groove, so that the first groove can be fully filled without leaving any gaps.

[0033] Further, the bipolar transistor device also includes a second edge isolation region 4, which is located on the side of the first edge isolation region 3 away from the substrate in the first direction, and a part of the second edge isolation region 4 corresponds to the first edge isolation region 3, and the other part is located between the base region 22 and the collector region 21. The second edge isolation region 4 includes a second groove arranged along the first direction, the second groove is filled with a high-density plasma oxide layer, the inner surface of the second groove is provided with an oxide layer to surround the high-density plasma oxide layer, and the surface of the second edge isolation region 4 away from the substrate is flush with the collector region. In this way, the second edge isolation region 4 located directly above the first edge isolation region 3 and the first edge isolation region 3 together form the isolation of the bipolar transistor from other devices located at its edge, avoiding signal interference between other devices and the bipolar transistor, and reducing parasitic effects. The depth of the second groove is 0.4 microns to 0.6 microns, preferably 0.5 microns. The thickness of the oxide layer on the inner surface of the second groove is 100 angstroms to 300 angstroms, preferably 200 angstroms. The thickness of the high-density plasma oxidation layer of the second groove is greater than half of the width of the second groove, so that the second groove can be fully filled without leaving any gaps.

[0034] In order to facilitate the electrical connection of the collector 211 , the base 221 , and the emitter 231 to the collector region 21 , the base region 22 , and the emitter region 23 , respectively, the bipolar transistor further includes a collector lead-out region 212 , a base lead-out region 222 , and an emitter lead-out region 232 .

[0035] The base lead-out region 222 is arranged on the peripheral side of the base region 22 and the emitter region 23, and is in electrical contact with the base region 22 and the collector region 21. The base 221 is arranged on the base lead-out region 222, and is electrically connected to the base region 22 through the base lead-out region 222. The base lead-out region 222 is composed of P+ type single crystal silicon with a doping concentration gradient, which is convenient for leading the base region 22 to the base 221 and reducing the electric field strength. The thickness of the base lead-out region 222 is 1 micron to 2 microns, preferably 1 micron.

[0036] The emitter lead-out region 232 is stacked along the first direction on the side of the emitter region 23 away from the substrate and is in electrical contact with the emitter 231. The emitter 231 is arranged on the emitter lead-out region 232 and is electrically connected to the emitter region 23 through the emitter lead-out region 232. The emitter lead-out region 232 is composed of N+ type polysilicon, and the thickness of the emitter lead-out region 232 is 1000 angstroms to 3000 angstroms, preferably 2000 angstroms.

[0037] The collector lead-out region 212 is arranged at one side of the collector region 21 and is in electrical contact with one side of the collector region 21. The collector 211 is arranged on the collector lead-out region 212 and is electrically connected to the collector region 21 through the collector lead-out region 212. The collector lead-out region 212 is composed of N+ type single crystal silicon with a doping concentration gradient, and the N+ single crystal silicon epitaxial layer 13 can be led to the collector 211 and the electric field strength can be reduced. The thickness of the collector lead-out region 212 is 2 microns to 4 microns, preferably 2 microns.

[0038] It is understandable that an insulating layer 24 is also provided on the side of the bipolar transistor away from the substrate, and the insulating layer 24 may include an oxide layer and a dielectric layer. The insulating layer 24 is provided with vias, and the collector 211, the base 221 and the emitter 231 are electrically connected to the collector lead-out region 212, the base lead-out region 222 and the emitter lead-out region 232 through the vias. The material of the metal electrode includes at least one of titanium and copper, so that the bipolar transistor device has better conductivity, high reliability and low energy consumption.

[0039] The bipolar transistor device of the above embodiment has the advantages of high gain, high frequency, low noise, high reliability, small leakage current and low switching loss. The parameters of the device are as follows:

[0040] Emitter collector breakdown voltage BVCEO ≥ 10V;

[0041] Current gain Beta ≥ 200;

[0042] Cut-off frequency fT ≥ 100 GHz;

[0043] The highest characteristic frequency fmax ≥ 100GHz;

[0044] Noise factor NFmin≤1dB;

[0045] The electrical properties are as follows: BVCEO=12V, Beta=230, fT=150GHz, NFmin=0.6.

[0046] The present invention also provides an embodiment of a method for preparing a bipolar triode device, please refer to Figure 2 , is a flow chart of a method for preparing a bipolar triode device provided by an embodiment of the present invention. The method for preparing a bipolar triode device comprises the following steps:

[0047] Step 100, providing a P+ type single crystal silicon substrate, and doping to sequentially form a P- type single crystal silicon epitaxial layer, an N+ type single crystal silicon epitaxial layer and an N- type single crystal silicon epitaxial layer on the P+ type single crystal silicon substrate along a first direction, wherein the collector region is located in the N- type single crystal silicon epitaxial layer.

[0048] Step 200: forming a collector lead-out region on one side of the collector region by a first photolithography process and a first doping process.

[0049] In step 200, the collector lead-out region is composed of N+ type single crystal silicon with a doping concentration gradient, so as to lead the N+ epitaxial layer to the surface of the N- type single crystal silicon epitaxial layer.

[0050] Step 300, epitaxial growth of a P-type single crystal silicon-germanium alloy is performed in a region corresponding to the base region, and carbon atoms are introduced during the growth process to fill the gaps between atoms.

[0051] In step 300, the germanium content in the P-type single crystal silicon-germanium alloy increases from zero to a first threshold along the first direction and then decreases to zero.

[0052] Step 400, growing an N+ type single crystal silicon layer in a region corresponding to the emitter region.

[0053] Step 500, through a second photolithography process and a second doping process, a portion of the N-type single crystal silicon epitaxial layer, a portion of the P-type single crystal silicon germanium alloy epitaxial layer and a portion of the N+ type single crystal silicon layer are formed into a base lead-out region.

[0054] In step 500, the base lead-out region is composed of P+ type single crystal silicon with a doping concentration gradient.

[0055] Step 600: forming a base region and an emitter region through a third photolithography process.

[0056] Step 700 , depositing N+ type polysilicon on the N+ type single crystal silicon epitaxial layer in a region corresponding to the emitter lead-out region through a fourth photolithography process and a deposition process to form an emitter lead-out region.

[0057] Step 800, forming a preparation process of a metal electrode.

[0058] The metal electrode comprises a collector, a base and an emitter. The collector is electrically connected to the collector region through a collector lead-out region, the base is electrically connected to the base region through a base lead-out region, and the emitter is electrically connected to the emitter region through an emitter lead-out region.

[0059] Through the above steps, the preparation of the bipolar triode device is completed.

[0060] In this embodiment, in the bipolar triode device prepared by the preparation method, a P-type single crystal silicon-germanium alloy is formed in the area corresponding to the base region, and the germanium content in the P-type single crystal silicon-germanium alloy increases from zero to the first threshold along the first direction and then decreases to zero, which can release the lattice mismatch and adjust the band width of different layers to achieve band cutting, so that the electrons produce an acceleration effect when moving in the base region, and improve the current gain of the prepared bipolar triode device, and doping carbon atoms in the P-type single crystal silicon-germanium alloy can fill the gaps between atoms, thereby effectively preventing the movement of germanium and impurity atoms caused by subsequent thermal processes. In addition, a collector lead-out region composed of N+ type single crystal silicon with a doping concentration gradient is formed, which can lead the N+ single crystal silicon epitaxial layer to the collector and reduce the electric field strength, and a reverse PN junction is formed between the P+ type single crystal silicon substrate and the collector region, and the current flowing through the collector region will be directly led to the collector through the collector lead-out region, and will not flow to one side of the P+ type single crystal silicon substrate. In addition, a base lead-out region composed of P+ type single crystal silicon with a doping concentration gradient is formed to facilitate the current in the base region to be led to the base and reduce the electric field strength.

[0061] In some optional embodiments, before the above step 200, the steps of forming a first edge isolation region on the peripheral side of the collector region and forming a second edge isolation region on the side of the first edge isolation region away from the P+ type single crystal silicon substrate are also included. The first edge isolation region includes a first groove arranged along the first direction, the first groove extends from the N-type single crystal silicon epitaxial layer to the P+ type single crystal silicon substrate, the first groove is filled with polysilicon, and the inner surface of the first groove is provided with an oxide layer to surround the polysilicon. A part of the second edge isolation region corresponds to the first edge isolation region, and the other part is arranged between the base region and the collector region; the second edge isolation region includes a second groove arranged along the first direction, the second groove is filled with a high-density plasma oxide layer, the inner surface of the second groove is provided with an oxide layer to surround the high-density plasma oxide layer, and the surface of the second edge isolation region away from the substrate is flush with the collector region.

[0062] In some optional embodiments, in the above step 100, the thickness of the provided P+ type single crystal silicon substrate is 600 microns to 800 microns, preferably 700 microns, and the P-type single crystal silicon epitaxial layer, the N+ type single crystal silicon epitaxial layer and the N-type single crystal silicon epitaxial layer are formed by epitaxy from the inside to the surface (i.e., along the first direction), the thickness of the P-type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the P-type single crystal silicon epitaxial layer is 1E16cm -3 The thickness of the N+ type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the N+ type single crystal silicon epitaxial layer is 1E19cm -3The thickness of the N-type single crystal silicon epitaxial layer is 2 microns to 4 microns, preferably 3 microns or 4 microns, and the doping concentration of the N-type single crystal silicon epitaxial layer is 1E16cm -3 Magnitude.

[0063] Combine the following Figure 3 The above steps are explained in detail.

[0064] After step 100, the step of forming a first edge isolation region on the peripheral side of the collector region specifically includes the following steps:

[0065] (1) Growth of an initial oxide layer: The silicon wafer formed in step 100 is surface cleaned and then placed in an oxidation furnace to form an initial oxide layer with a thickness of about 100 angstroms. The temperature of the oxidation furnace is 800°C to 1000°C. In some optional embodiments, the temperature of the oxidation furnace is 1000°C. In other optional embodiments, the temperature of the oxidation furnace is 900°C.

[0066] (2) Deposition of silicon nitride layer: Place the silicon wafer processed in step (1) in a silicon nitride LPCVD furnace to deposit a silicon nitride layer with a thickness of about 1600 angstroms. The temperature of the CVD furnace is 600°C to 900°C. In some optional embodiments, the temperature of the CVD furnace is 800°C. In other optional embodiments, the temperature of the CVD furnace is 700°C.

[0067] (3) First groove photolithography: Photolithography is performed on the silicon wafer processed in step (2) to form a region for isolating the bipolar transistor and other devices to reduce parasitic effects.

[0068] (4) Dry etching of the silicon nitride layer and the oxide layer: Dry etching is performed on the silicon wafer processed in step (3) to remove the silicon nitride layer deposited in step (2) and the initial oxide layer grown in step (1) in the area exposed by the first groove lithography.

[0069] (5) Dry etching the first groove: dry etching the silicon wafer processed in step (4), dry etching a first groove for isolating the bipolar transistor and other devices in the area exposed by photolithography of the first groove, the depth of the first groove being 6 microns to 10 microns; remove the photoresist of the photolithography of the first groove. In some optional embodiments, the depth of the first groove is 8 microns, and in other optional embodiments, the depth of the first groove is 10 microns.

[0070] (6) Growth of oxide layer in the first groove: The silicon wafer in step (5) is surface cleaned, and after completion, the silicon wafer is placed in an oxidation furnace to form an oxide layer in the first groove, the oxide layer thickness is 800 angstroms to 1200 angstroms, the oxidation furnace temperature is 1000°C, and the area outside the first groove is protected by the silicon nitride layer deposited in step (2), and no oxide layer grows except in the edge area; after the oxide layer growth in the first groove is completed, the silicon wafer is placed in nitrogen at 1100°C for annealing. In some optional embodiments, the thickness of the oxide layer in the first groove is 1000 angstroms, and in other optional embodiments, the thickness of the oxide layer in the first groove is 1200 angstroms.

[0071] (7) Deposition of polysilicon in the first groove: Place the silicon wafer in step (6) in a polysilicon LPCVD furnace, and deposit a layer of polysilicon in the first groove and on the surface of the silicon wafer. The thickness of the polysilicon is required to be greater than half of the width of the first groove so as to fully fill the first groove without leaving any gaps. The deposition temperature is 500° C. to 800° C. In some optional embodiments, the deposition temperature is 700° C., and in other optional embodiments, the deposition temperature is 600° C.

[0072] (8) Grinding the front side of the silicon wafer: Grinding the front side of the silicon wafer after the processing in step (7) is performed to remove the polysilicon deposited in step (7), the silicon nitride layer deposited in step (2) and the initial oxide layer grown in step (1) on the surface of the silicon wafer, so that the surface of the silicon wafer is smooth for subsequent process operations. According to different process requirements, a certain thickness of polysilicon can be deposited in different areas before front side grinding to reduce the load effect of the front side grinding process.

[0073] The above steps form a first edge isolation region. Then, a second edge isolation region is formed on the side of the first edge isolation region away from the P+ type single crystal silicon substrate. Specifically, the following steps are included:

[0074] (9) Growth of oxide layer: The silicon wafer in step (8) is surface cleaned, and after completion, the silicon wafer is placed in an oxidation furnace to form an oxide layer with a thickness of about 100 Å, and the temperature of the oxidation furnace is 900° C. to 1000° C. In some optional embodiments, the temperature of the oxidation furnace is 900° C., and in other optional embodiments, the temperature of the oxidation furnace is 1000° C.

[0075] (10) Deposition of silicon nitride layer: Place the silicon wafer processed in step (9) in a silicon nitride LPCVD furnace to deposit a silicon nitride layer with a thickness of about 1600 Å. The temperature of the CVD furnace is 600° C. to 1000° C. In some optional embodiments, the temperature of the CVD furnace is 800° C., and in other optional embodiments, the temperature of the CVD furnace is 700° C.

[0076] (11) Second groove photolithography: The silicon wafer processed in step (10) is subjected to photolithography to form an oxide layer on the top of the first groove and to form isolation between the base region and the collector region.

[0077] (12) Dry etching of the silicon nitride layer and the oxide layer: Dry etching is performed on the silicon wafer processed in step (11) to remove the silicon nitride layer deposited in step (12) and the oxide layer grown in step (9) in the area exposed by the second groove lithography.

[0078] (13) Dry etching the second groove: Dry etching the silicon wafer processed in step (12) to form a second groove in the area exposed by the second groove, with the depth of the second groove being 0.4 micrometers to 0.6 micrometers; and removing the photoresist of the second groove. In some optional embodiments, the depth of the second groove is 0.5 micrometers.

[0079] (14) Growth of oxide layer in the second groove: After cleaning the surface of the silicon wafer in step (13), the silicon wafer is placed in an oxidation furnace to form an oxide layer in the second groove. The oxide layer thickness is between 100 angstroms and 300 angstroms. The temperature of the oxidation furnace is 1000° C. Since the area outside the second groove is protected by the silicon nitride layer deposited in step (10), no oxide layer grows except in the edge area. After the oxide layer growth in the second groove is completed, the silicon wafer is placed in nitrogen at 1100° C. for annealing. In some optional embodiments, the oxide layer thickness can be 200 angstroms.

[0080] (15) Deposition of a high-density plasma oxide layer in the second groove: The silicon wafer in step (14) is placed in a plasma PE-CVD chamber, and a high-density plasma oxide layer is deposited in the second groove and other areas of the silicon wafer. The thickness of the high-density plasma oxide layer is required to be greater than half of the width of the second groove so as to fully fill the second groove without leaving any gaps. After the high-density plasma oxide layer is grown, the silicon wafer is placed at 1000° C. to 1100° C. for rapid annealing for about 30 seconds. In some optional embodiments, the silicon wafer is placed at 1100° C. for rapid annealing for about 30 seconds. In other optional embodiments, the silicon wafer is placed at 1050° C. for rapid annealing for about 30 seconds.

[0081] (16) Front side grinding of silicon wafer: The front side of the silicon wafer processed in step (15) is grinded to remove the high-density plasma oxide layer deposited in step (15), the silicon nitride layer deposited in step (10) and the oxide layer grown in step (9) on the surface of the silicon wafer, so that the surface of the silicon wafer is smooth for subsequent process operations. According to different process requirements, a high-density plasma oxide layer of a certain thickness can be deposited in different areas before front side grinding to reduce the load effect of the front side grinding process.

[0082] The above steps form a second edge isolation region. Then, a step of forming a collector lead-out region on one side of the collector region is performed by a first photolithography process and a first doping process. Specifically, the step of defining the region corresponding to the collector lead-out region by a first photolithography process and the step of forming the collector are as follows:

[0083] (17) Photolithography of the collector lead-out region: The silicon wafer processed in step (16) is photolithographically processed by the first photolithography process so as to lead the current serving as the collector region to the collector through the heavily doped N+ type single crystal silicon epitaxial layer and the collector lead-out region. After the first photolithography process, the region corresponding to the collector lead-out region can be defined.

[0084] (18) Collector lead region doping: The silicon wafer processed in step (17) is doped at an energy of 30 KeV to 70 KeV and 1E14 cm -2 ~1E15cm -2 Shallow arsenic ion bombardment was carried out at the level of 200KeV to 600KeV and 1E14cm -2 ~1E15cm -2 Deep phosphorus ion bombardment is carried out under mass metering, and arsenic ions and phosphorus ions are injected into the silicon wafer to form an N+ type doping concentration gradient, which leads the heavily doped N+ type single crystal silicon epitaxial layer to the surface of the silicon wafer and reduces the electric field strength; the photoresist of the collector lead-out area is removed; the silicon wafer is placed at 900℃~1000℃ for rapid annealing for about 30 seconds to activate the arsenic ions and phosphorus ions.

[0085] In some optional embodiments, the silicon wafer processed in step (17) can be heated at 50 KeV energy and 1E15 cm -2 Shallow arsenic ion bombardment was performed at the energy of 400 KeV and 1E14 cm -2 Deep phosphorus ion bombardment is carried out under mass metering, and arsenic ions and phosphorus ions are injected into the silicon wafer to form an N+ type doping concentration gradient, which leads the heavily doped N+ type single crystal silicon epitaxial layer to the surface of the silicon wafer and reduces the electric field strength; the photoresist of the collector lead-out area is removed; the silicon wafer is placed at 1000℃ for rapid annealing for about 30 seconds to activate the arsenic ions and phosphorus ions.

[0086] In some other optional embodiments, the silicon wafer processed in step (17) can be heated at 30 KeV energy and 1E15 cm -2 Shallow arsenic ion bombardment was performed at the energy of 300 KeV and 1E14 cm -2Deep phosphorus ion bombardment is carried out under mass metering, and arsenic ions and phosphorus ions are injected into the silicon wafer to form an N+ type doping concentration gradient, which leads the heavily doped N+ type single crystal silicon epitaxial layer to the surface of the silicon wafer and reduces the electric field strength; the photoresist of the collector lead-out area is removed; the silicon wafer is placed at 900°C for rapid annealing for about 30 seconds to activate the arsenic ions and phosphorus ions.

[0087] The above steps form the collector lead-out region. Then, a step of growing a P-type single crystal silicon-germanium alloy epitaxial layer in the corresponding region of the base region is performed, which specifically includes the following steps:

[0088] (19) Growth of sacrificial oxide layer: The silicon wafer in step (18) is surface cleaned and then placed in an oxidation furnace to form a sacrificial oxide layer with a thickness of about 100 Å. The temperature of the oxidation furnace is 1000°C.

[0089] (20) Wet etching of the sacrificial oxide layer: The sacrificial oxide layer of the silicon wafer processed in step (19) is removed using an ammonium fluoride and hydrofluoric acid solution with a volume ratio of 6:1.

[0090] (21) Epitaxial growth of P-type single crystal silicon-germanium alloy: The silicon wafer processed in step (20) is placed in a silicon-germanium alloy ultra-high vacuum UHV-CVD furnace. After surface hydrogen passivation, a layer of P-type single crystal silicon-germanium alloy is deposited on the exposed silicon surface of the silicon wafer by adjusting the flow rate of silicon atoms and germanium atoms. The thickness of the single crystal silicon-germanium alloy is 100 angstroms to 300 angstroms, and the doping concentration is 1E18 cm -3 The temperature of the UHV-CVD furnace of the silicon-germanium alloy is 500℃~800℃. In order to produce the base band shearing effect, the proportion of germanium in the silicon-germanium alloy in the single-crystal silicon-germanium alloy layer is not uniform, but an optimized design is adopted. After changing layer by layer to the first threshold, it is reduced to zero to release the lattice mismatch and adjust the band width of different layers, so that the electrons move in the base region. Acceleration effect; in order to effectively prevent the movement of germanium and impurity atoms caused by subsequent thermal processes, carbon atoms are introduced during the growth of the P-type single-crystal silicon-germanium alloy layer to fill the gaps between atoms. The above-mentioned first threshold is the ratio of the number of germanium atoms to silicon atoms in the P-type single-crystal silicon-germanium alloy, and the value range of the first threshold is 30%~50%. The content of carbon atoms doped in the silicon-germanium alloy is 0.1%~0.2%, and the doping amount is the ratio of the number of carbon atoms to the number of silicon atoms. Preferably, the first threshold can be 40%, and the doping content of carbon atoms is 0.1%. In some optional embodiments, the temperature of the silicon-germanium alloy high vacuum UHV-CVD furnace is 600°C. In other optional embodiments, the temperature of the silicon-germanium alloy high vacuum UHV-CVD furnace is 550°C.

[0091] The above steps form the growth of a P-type single crystal silicon-germanium alloy epitaxial layer. Then, a step of growing an N+ type single crystal silicon layer is performed in the corresponding area of ​​the emitter region. Specifically, the steps include:

[0092] (22) Epitaxial growth of N+ type single crystal silicon layer: The silicon wafer processed in step (21) is placed in an LP-CVD furnace. After surface hydrogen passivation, a layer of N+ type single crystal silicon layer is deposited on the exposed silicon surface of the silicon wafer. The thickness of the single crystal silicon layer is about 1000 angstroms and the doping concentration is 1E19 cm -3 In some optional embodiments, the LP-CVD furnace temperature is 550°C, and in other optional embodiments, the LP-CVD furnace temperature is 600°C.

[0093] After the above steps, a second photolithography process and a second doping process are performed to form the base lead-out region from part of the N-type single crystal silicon epitaxial layer, part of the P-type single crystal silicon germanium alloy epitaxial layer and part of the N+ type single crystal silicon layer, which specifically includes the following steps:

[0094] (23) Photolithography of the base lead-out region: The silicon wafer processed in step (22) is photolithographically processed by a second photolithography process so as to lead the P-type single crystal silicon-germanium alloy epitaxy serving as the base region to the base through heavily doped P+ single crystal silicon. After the second photolithography process, the area corresponding to the base lead-out region can be defined.

[0095] (24) Base lead region doping: The silicon wafer processed in step (23) is doped at an energy of 10 KeV to 20 KeV and 1E15 cm -2 Shallow boron ion bombardment was performed at the level of 100KeV to 200KeV and 1E14cm -2 The boron ion bombardment is carried out at a deep level under the metering level. The boron ion implantation into the silicon wafer will compensate for the N-type impurities of the N+ type single crystal silicon epitaxial layer and the N- single crystal silicon epitaxial layer in step (22) and form a P+ type doping concentration gradient to lead the P-type base region to the surface of the silicon wafer and reduce the electric field strength; remove the photoresist of the base lead-out region; and place the silicon wafer at 1000° C. for rapid annealing for about 30 seconds to activate the boron ions. In some optional embodiments, the energy of the shallow boron ion bombardment is 10 KeV, and the energy of the deep boron ion bombardment is 100 KeV. In other optional embodiments, the energy of the shallow boron ion bombardment is 20 KeV, and the energy of the deep boron ion bombardment is 200 KeV.

[0096] The above steps form a base lead-out region, and then a third photolithography process is performed to form a base region and an emitter region, which specifically includes:

[0097] (25) Photolithography of the base region and emitter region: Photolithography is performed on the silicon wafer processed in step (24) to remove the N+ type single crystal silicon layer epitaxially grown in step (22) and the P type single crystal silicon germanium alloy epitaxially grown in step (21) outside the base region and the emitter region.

[0098] (26) Dry etching the epitaxially grown layer: dry etching the silicon wafer processed in step (25) to remove the N+ type single crystal silicon layer epitaxially grown in step (22) and the P type single crystal silicon germanium alloy epitaxially grown in step (21) outside the base region and the emitter region; and remove the photoresist used for the photolithography of the base region and the emitter region.

[0099] The above steps form a base region and an emitter region, and then a fourth photolithography process and a deposition process are performed to deposit N+ type polysilicon on the N+ type single crystal silicon epitaxial layer in a region corresponding to the emitter lead-out region to form an emitter lead-out region, which specifically includes the following steps:

[0100] (27) Deposition of TEOS layer: Place the silicon wafer processed in step (26) in a TEOS LPCVD furnace to deposit a TEOS layer with a thickness of about 1000 Å. The temperature of the CVD furnace is 600°C.

[0101] (28) Photolithography of the emitter lead-out region: The silicon wafer processed in step (27) is subjected to photolithography through a fourth photolithography process to define the region where the emitter contacts the polysilicon, that is, to define the region corresponding to the emitter lead-out region.

[0102] (29) Dry etching of the TEOS layer: Dry etching is performed on the silicon wafer processed in step (28) to remove the TEOS layer deposited in step (27) in the area exposed by the photolithography of the emitter lead-out region; and the photoresist of the photolithography of the emitter lead-out region is removed.

[0103] (30) Deposition of N+ type polysilicon in the emitter lead-out region: Place the silicon wafer in step (29) in a polysilicon LPCVD furnace, and deposit a layer of N+ type polysilicon on the surface of the silicon wafer. The thickness of the polysilicon is between 1000 angstroms and 3000 angstroms, and the deposition temperature is between 600°C and 700°C. After the deposition is completed, place the silicon wafer at 1000°C to 1100°C for rapid annealing for about 40 seconds. Preferably, the thickness of the polysilicon is 2000 angstroms. In some optional embodiments, the temperature of polysilicon deposition is 700°C, and the annealing temperature is 1100°C. In other optional embodiments, the temperature of polysilicon deposition is 600°C, and the annealing temperature is 1000°C.

[0104] (31) Photolithography of the polysilicon region in the emitter lead-out region: Photolithography is performed on the silicon wafer processed in step (30) to define the polysilicon region in the emitter lead-out region.

[0105] (32) Dry etching of polysilicon: Dry etching of the silicon wafer processed in step (31) is performed to remove the polysilicon deposited in step (30) except for the area exposed by photolithography in the polysilicon region of the emitter lead-out region; and the photoresist of the photolithography in the polysilicon region of the emitter lead-out region is removed.

[0106] The above steps form the emitter lead-out region, and then the preparation process of forming the metal electrode is carried out. It can be understood that the metal electrode includes the collector, the base and the emitter. Specifically, the following steps are included:

[0107] (33) Deposition of TEOS layer: Place the silicon wafer processed in step (32) in a TEOS LPCVD furnace to deposit a TEOS layer with a thickness of about 400 Å. The temperature of the CVD furnace is 600° C. to 700° C. In some optional embodiments, the temperature of the CVD furnace is 700° C., and in other optional embodiments, the temperature of the CVD furnace is 600° C.

[0108] (34) Deposition of silicon nitride layer: The silicon wafer processed in step (34) is placed in a silicon nitride plasma PE-CVD chamber to deposit a silicon nitride layer with a thickness of about 800 Å.

[0109] (35) Deposition of SAUSG layer and PETEOS layer: Place the silicon wafer in step (34) in a plasma PE-CVD chamber to deposit SAUSG layer and PETEOS layer. The thickness of the SAUSG layer is about 4000 Å, and the thickness of the PETEOS layer is about 7000 Å.

[0110] (36) Metal contact window photolithography: The silicon wafer processed in step (35) is subjected to photolithography to form metal contact window areas in the areas corresponding to the base, emitter and collector.

[0111] (37) dry etching the dielectric layer: dry etching the silicon wafer processed in step (36) to remove the SAUSG layer and the PETEOS layer deposited in step (35), the silicon nitride layer deposited in step (34) and the TEOS layer deposited in step (33) in the area exposed by the metal contact window photolithography; and remove the photoresist of the metal contact window photolithography;

[0112] (38) Sputtering front metal: performing metal sputtering on the silicon wafer processed in step (37) to deposit front metal on the silicon wafer.

[0113] (39) front metal photolithography: performing photolithography on the silicon wafer processed in step (38), defining the front metal area in the corresponding areas of the base, emitter and collector;

[0114] (40) Dry etching of the front metal: Dry etching of the silicon wafer processed in step (39) to remove the front metal layer deposited in step (38) in the area exposed by the front metal lithography; and removal of the photoresist of the front metal lithography.

[0115] (41) Front metal alloy: The silicon wafer processed in step (40) is placed in an alloy furnace tube, and the front metal portion forms a front metal alloy. The temperature of the alloy furnace tube is 400° C. to 450° C., and the alloying time is 20 minutes. In some optional embodiments, the temperature of the alloy furnace tube is 420° C., and in other optional embodiments, the temperature of the alloy furnace tube is 450° C.

[0116] After the above steps, a bipolar transistor device is formed. Its specific structure can be referred to Figure 1 After the bipolar transistor device is formed, the bipolar transistor device needs to be tested.

[0117] In some optional embodiments, the front thinning method in the above steps (8) and (16) can be replaced by wet etching.

[0118] In some other optional embodiments, the front thinning method described in the above steps (8) and (16) is atmospheric pressure plasma etching.

[0119] The bipolar triode device formed by the above preparation method adopts a new base region structure in which carbon atoms are added to the P-type single crystal silicon germanium alloy base region, and the proportion of germanium in the P-type single crystal silicon germanium alloy is not single and uniform, but adopts an optimized design, changes layer by layer to the first threshold and then decreases, so as to release the lattice mismatch and adjust the energy band width of different layers to achieve base region energy band cutting, so that the electrons move in the base region to produce an acceleration effect. The bipolar triode device made in this way has the advantages of high gain, high frequency, high reliability, small leakage current and low switching loss; the edge of the bipolar triode adopts a first edge isolation region and a second edge The device is isolated from surrounding devices by combining isolation zones, and the bottom of the device is isolated from the substrate by a reverse PN junction, which effectively avoids mutual signal interference and reduces parasitic effects; and a front thinning method is adopted in the first groove and the second groove process to make the surface of the silicon wafer flat for subsequent process operations, while improving the reliability of the bipolar triode device and reducing leakage current; the grown front surface metal uses at least one of titanium and copper, so that the bipolar triode device has better conductivity, high reliability and low energy consumption; and the preparation method has good compatibility with the existing CMOS platform process and can quickly achieve large-scale production.

[0120] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A bipolar transistor device, characterized in that: It comprises a substrate and an epitaxial layer and a bipolar transistor which are sequentially stacked on the substrate along a first direction; The bipolar transistor comprises: The collector region is composed of a lightly doped N-type single crystal silicon epitaxial layer; A base region, stacked along the first direction on a side of the collector region away from the substrate, the base region being composed of a P-type single crystal silicon-germanium alloy doped with carbon atoms, wherein a germanium content in the P-type single crystal silicon-germanium alloy increases from zero to a first threshold value and then decreases to zero along the first direction; an emitter region, stacked along the first direction on a side of the base region away from the substrate, and composed of heavily doped N+ type single crystal silicon; A metal electrode, comprising a collector, a base and an emitter, wherein the collector is electrically connected to the collector region, the base is electrically connected to the base region, and the emitter is electrically connected to the emitter region; A first edge isolation region is arranged on the peripheral side of the bipolar transistor, the first edge isolation region comprises a first groove arranged along the first direction, the first groove extends from the N-type single crystal silicon epitaxial layer to the substrate, the first groove is filled with polysilicon, and an oxide layer is arranged on the inner surface of the first groove to surround the polysilicon; a second edge isolation region, wherein the second edge isolation region is located on a side of the first edge isolation region away from the substrate in the first direction, a portion of the second edge isolation region corresponds to the first edge isolation region, and another portion of the second edge isolation region is located between the base region and the collector region, the second edge isolation region comprises a second groove arranged along the first direction, the second groove is filled with a high-density plasma oxide layer, an inner surface of the second groove is provided with an oxide layer to surround the high-density plasma oxide layer, and a surface of the second edge isolation region away from the substrate is flush with the collector region; The substrate is a heavily doped P+ type single crystal silicon substrate, the epitaxial layer comprises a lightly doped P- type single crystal silicon epitaxial layer and a heavily doped N+ type single crystal silicon epitaxial layer sequentially stacked along a first direction, and the collector region is located on the N+ type single crystal silicon epitaxial layer, so that a reverse PN junction isolation is formed between the P+ type single crystal silicon substrate and the collector region; The thickness of the P+ type single crystal silicon substrate is 600 microns to 800 microns, the thickness of the P- type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the P- type single crystal silicon epitaxial layer is 1E16 cm -3 The thickness of the N + type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the N + type single crystal silicon epitaxial layer is 1E19cm -3 The thickness of the N-type single crystal silicon epitaxial layer is 2 microns to 4 microns, and the doping concentration of the N-type single crystal silicon epitaxial layer is 1E16cm -3 Magnitude.

2. The bipolar transistor device according to claim 1, characterized in that: The depth of the first groove is 6 microns to 10 microns, the depth of the second groove is 0.4 microns to 0.6 microns, the thickness of the oxide layer in the first groove is 800 angstroms to 1200 angstroms, the thickness of the oxide layer in the second groove is 100 angstroms to 300 angstroms, the thickness of the polysilicon is greater than half the width of the first groove, and the thickness of the high-density plasma oxide layer is greater than half the width of the second groove.

3. The bipolar transistor device according to claim 1, characterized in that: The first threshold is the ratio of the number of germanium atoms to the number of silicon atoms in the P-type single crystal silicon-germanium alloy, and the value range of the first threshold is 30% to 50%.

4. The bipolar transistor device according to claim 3, characterized in that: The doping content of carbon atoms in the P-type single crystal silicon-germanium alloy is 0.1% to 0.2%, and the doping content is the ratio of the number of carbon atoms to the number of silicon atoms.

5. The bipolar transistor device according to claim 1, characterized in that: The thickness of the P-type single crystal silicon germanium alloy in the base region is 100 angstroms to 300 angstroms, and the doping concentration of the P-type single crystal silicon germanium alloy is 1E18 cm -3 Magnitude.

6. The bipolar transistor device according to claim 1, characterized in that: The bipolar transistor also includes: A base lead-out region is arranged on the peripheral side of the base region and the emitter region and is in electrical contact with the base region, the emitter region and the collector region. The base is arranged on the base lead-out region and is electrically connected to the base region through the base lead-out region. The base lead-out region is composed of P+ type single crystal silicon with a doping concentration gradient, and the thickness of the base lead-out region is 1 micron to 2 microns; An emitter lead-out region is stacked along the first direction on a side of the emitter region away from the substrate and is in electrical contact with the emitter. The emitter is arranged on the emitter lead-out region and is electrically connected to the emitter region through the emitter lead-out region. The emitter lead-out region is composed of N+ type polysilicon and has a thickness of 1000 angstroms to 3000 angstroms. A collector lead-out region is arranged on one side of the collector region, and one side of the collector region is electrically contacted. The collector is arranged on the collector lead-out region and is electrically connected to the collector region through the collector lead-out region. The collector lead-out region is composed of N+ type single crystal silicon with a doping concentration gradient, and the thickness of the collector lead-out region is 2 microns to 4 microns.

7. The bipolar transistor device according to claim 1, characterized in that: The material of the metal electrode includes at least one of titanium and copper.

8. A method for preparing a bipolar transistor device according to any one of claims 1 to 7, characterized in that: include: Providing a P+ type single crystal silicon substrate, and doping to sequentially form a P- type single crystal silicon epitaxial layer, an N+ type single crystal silicon epitaxial layer and an N- type single crystal silicon epitaxial layer on the P+ type single crystal silicon substrate along a first direction, wherein the collector region is located in the N- type single crystal silicon epitaxial layer; A first edge isolation region is formed on the peripheral side of the collector region, wherein the first edge isolation region includes a first groove arranged along the first direction, the first groove extends from the N-type single crystal silicon epitaxial layer to the P+ type single crystal silicon substrate, the first groove is filled with polycrystalline silicon, and an oxide layer is arranged on the inner surface of the first groove to surround the polycrystalline silicon; A second edge isolation region is formed on a side of the first edge isolation region away from the P+ type single crystal silicon substrate, wherein a portion of the second edge isolation region corresponds to the first edge isolation region, and another portion of the second edge isolation region is arranged between the base region and the collector region; the second edge isolation region comprises a second groove arranged along the first direction, the second groove is filled with a high-density plasma oxidation layer, an oxide layer is arranged on the inner surface of the second groove to surround the high-density plasma oxidation layer, and a surface of the second edge isolation region away from the substrate is flush with the collector region; Forming a collector lead-out region on one side of the collector region by a first photolithography process and a first doping process, wherein the collector lead-out region is composed of N+ type single crystal silicon with a doping concentration gradient, so as to lead the N+ type single crystal silicon epitaxial layer to the surface of the N- type single crystal silicon epitaxial layer; In the area corresponding to the base region, epitaxial growth of a P-type single crystal silicon-germanium alloy is performed, and carbon atoms are introduced during the growth process to fill the gaps between atoms, wherein the germanium content in the P-type single crystal silicon-germanium alloy increases from zero to a first threshold along the first direction and then decreases to zero; In the area corresponding to the emitter region, epitaxial growth of an N+ type single crystal silicon layer is performed; Through a second photolithography process and a second doping process, part of the N-type single crystal silicon epitaxial layer, part of the P-type single crystal silicon germanium alloy epitaxial layer and part of the N+ type single crystal silicon layer are formed into the base lead-out region, wherein the base lead-out region is composed of P+ type single crystal silicon with a doping concentration gradient; Forming the base region and the emitter region through a third photolithography process; Depositing N+ type polysilicon on the N+ type single crystal silicon epitaxial layer in a region corresponding to the emitter lead-out region through a fourth photolithography process and a deposition process to form the emitter lead-out region; A preparation process for forming a metal electrode, wherein the metal electrode includes a collector, a base and an emitter.

9. The method for preparing a bipolar transistor device according to claim 8, characterized in that: The step of performing epitaxial growth of a P-type single crystal silicon-germanium alloy in a region corresponding to the base region and introducing carbon atoms to fill the gaps between atoms during the growth process comprises: In a silicon-germanium alloy high-vacuum UHV-CVD furnace, after surface hydrogen passivation, by adjusting the flow rates of silicon atoms and germanium atoms, a P-type single crystal silicon-germanium alloy epitaxy is formed in a corresponding area of ​​the base region, in which the germanium content increases from zero to a first threshold along the first direction and then decreases to zero, and carbon atoms are introduced during the formation of the P-type single crystal silicon-germanium alloy epitaxy. The temperature of the silicon-germanium alloy high-vacuum UHV-CVD furnace is 500°C to 800°C.

10. The method for preparing a bipolar transistor device according to claim 8, characterized in that: The step of forming a collector lead-out region on the peripheral side of the collector region by a first photolithography process and a first doping process specifically includes: Defining the collector lead-out region corresponding to the region by a first photolithography process; The N-type single crystal silicon epitaxial layer in the region corresponding to the collector lead-out region is heated at 30KeV to 70KeV and 1E14cm -2 ~1E15cm -2 Shallow arsenic ion bombardment was carried out at the level of 200KeV to 600KeV and 1E14cm -2 ~1E15cm -2 Deep phosphorus ion bombardment is performed under high-level measurement, and the arsenic ions and the phosphorus ions are implanted into the silicon wafer to form the collector lead-out region with an N+ type doping concentration gradient. Then, the photoresist formed in the collector lead-out region in the first photolithography process is removed, and the silicon wafer is subjected to rapid annealing at 900° C. to 1000° C. for 20 seconds to 40 seconds to activate the arsenic ions and the phosphorus ions.

11. The method for preparing a bipolar transistor device according to claim 9, characterized in that: The step of forming the base lead-out region from part of the N-type single crystal silicon epitaxial layer, part of the P-type single crystal silicon germanium alloy epitaxial layer and part of the N+ type single crystal silicon layer through a second photolithography process and a second doping process comprises: Defining the area corresponding to the base lead-out region by a second photolithography process; The N-type single crystal silicon epitaxial layer, the P-type single crystal silicon germanium alloy and part of the N+ type single crystal silicon layer in the area corresponding to the base lead-out region are heated at 10KeV to 20KeV and 1E15cm -2 Shallow boron ion bombardment was performed at the level of 100KeV to 200KeV and 1E14cm -2 Deep boron ion bombardment is performed under high-level measurement, and the boron ions are injected into the silicon wafer to form the base lead-out area with a P+ type doping concentration gradient. The photoresist formed in the base lead-out area in the second photolithography process is then removed, and the base is placed at 900° C. to 1000° C. for rapid annealing for 20 seconds to 40 seconds to activate the boron ions.