Additive for oil well cement and cement slurry using the same
By copolymerizing vinyl ester monomers and multifunctional monomers of vinyl alcohol polymers, a polymer with excellent fluid loss performance is formed, which solves the problem of insufficient fluid loss performance of existing PVA at high temperatures and high pressures, and realizes oil well Efficient bonding of cement slurries and cost reduction.
Patent Information
- Application Number
- CN201980005732.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-02-22
- Filing Date
- 2019-02-04
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-02-04
AI Technical Summary
Existing polyvinyl alcohol (PVA) fluid loss additives are difficult to effectively reduce the fluid loss of oil well cement slurry under high temperature and high pressure conditions, resulting in reduced fluidity and increased costs.
Vinyl alcohol polymers are used as additives for oil well cement. By copolymerizing vinyl ester monomers and multifunctional monomers, the degree of saponification and the average degree of viscosity polymerization are controlled to form a polymer with excellent fluid loss reduction performance and added to the cement. Added to slurry to reduce moisture loss.
Under high temperature and high pressure conditions, it can significantly reduce the fluid loss of oil well cement, maintain the fluidity of cement slurry, improve the cementing effect, and reduce costs.
Smart Images

Figure BDA0002492124310000111
Abstract
Description
Technical Field
[0001] The present invention relates to an oil well cement additive containing a vinyl alcohol polymer and a cement slurry using the oil well cement additive. Background Art
[0002] Oil well cement used to cement oil wells, gas wells, steam wells for geothermal power generation, etc., is filled in the gap between the steel pipe and the pit in order to protect the steel pipe (shell). Generally, the loss of water contained in the cement slurry due to high pressure and geothermal heat during injection is called "filtration loss". Since the fluidity of cement slurry and the strength after curing will be damaged by filtration loss, filtration reducers are usually added to cement slurry.
[0003] As an example of a fluid loss reducer, polyvinyl alcohol (hereinafter also referred to as PVA) is known. In recent years, as shale gas wells are being dug deeper, pressure and temperature conditions have become more severe, and the amount of fluid loss reducer added has increased accordingly.
[0004] However, since the viscosity increase of cement slurry leads to a decrease in fluidity and an increase in cost, there is a demand for improved fluid loss control performance of fluid loss control agents.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2007 / 146348
[0008] Patent Document 2: Japanese Patent Application Publication No. 2015-196733 Summary of the invention
[0009] Problems to be solved by the invention
[0010] Patent Documents 1 and 2 describe PVA used as a fluid loss reducer. However, these fluid loss reducers containing PVA have not yet achieved the fluid loss reduction performance required for cement slurry injected under high temperature and high pressure.
[0011] Therefore, a main object of the present invention is to provide an oil well cement additive containing a vinyl alcohol polymer having excellent fluid loss reduction performance.
[0012] Means for solving problems
[0013] That is, the present invention provides an additive for oil well cement, which contains a vinyl alcohol polymer, wherein the vinyl alcohol polymer is a saponified product of a copolymer of a vinyl ester monomer and a multifunctional monomer, has a saponification degree of 70 to 95 mol %, and has a viscosity average polymerization degree of 1000 to 10000.
[0014] The above-mentioned multifunctional monomer may have a carbonyl group or an amide group.
[0015] The multifunctional monomer may be triallyl isocyanurate.
[0016] The content of the structural unit derived from the polyfunctional monomer in the vinyl alcohol polymer may be 0.001 to 1.0 mol % based on 100 mol % of the structural unit derived from the vinyl ester monomer.
[0017] The particle size of the vinyl alcohol polymer may be 75 μm or less, accounting for 30% by mass or less, and 500 μm or more, accounting for 10% by mass or less.
[0018] The present invention also provides a cement slurry containing 0.01 to 30% bwoc of the above-mentioned additive for oil well cement.
[0019] Effects of the Invention
[0020] According to the present invention, an oil well cement additive containing a vinyl alcohol polymer having excellent fluid loss reduction performance can be provided. DETAILED DESCRIPTION
[0021] Hereinafter, the mode for implementing the present invention will be described in detail. It should be noted that the present invention is not limited to the embodiment described below.
[0022] An oil well cement additive according to one embodiment of the present invention is suitable as an additive for oil well cement used when cementing oil wells, gas wells, steam wells for geothermal power generation, etc. The oil well cement additive of this embodiment contains a vinyl alcohol polymer obtained by copolymerizing a vinyl ester monomer and a multifunctional monomer, and controlling the saponification degree and viscosity average polymerization degree.
[0023] Cementing during pit excavation is the process of injecting cement into the gap between the excavated pit and the steel pipe inserted into the pit. As a cementing method, the following method is widely used: cement and various additives are mixed in a dry state, and then pumped into the mixture while being made into a slurry using high-pressure water. Among the additives, if vinyl alcohol polymer is used as a fluid loss reducer, it is possible to reduce the loss of water contained in the cement slurry during cementing (i.e., reduce fluid loss) and maintain the fluidity of the cement slurry. In the case of large fluid loss, the cement slurry will lose fluidity and it will be difficult to fully cement.
[0024] It should be noted that fluid loss is a physical property of oil well cement defined by the American Petroleum Institute (API). The test method for fluid loss is described in the Recommended Practice for Testing Well Cements, API Recommended Practice 10B-2, April 2013.
[0025] The vinyl alcohol polymer used in the oil well cement additive of this embodiment is a polymer obtained by saponifying a copolymer of a vinyl ester monomer and a multifunctional monomer, has a saponification degree of 70 to 95 mol % and a viscosity average polymerization degree of 1000 to 10000. The particle size of the vinyl alcohol polymer is preferably controlled.
[0026] The copolymer of the vinyl ester monomer and the polyfunctional monomer may further contain a monomer other than the vinyl ester monomer that is copolymerizable with the vinyl ester monomer and the polyfunctional monomer, within a range not impairing the effects of the present invention.
[0027] As the vinyl ester monomer, for example, vinyl acetate, vinyl propionate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl pivalate, etc. may be used, and a mixture thereof may also be used. From the viewpoint of ease of polymerization, vinyl acetate is preferred as the vinyl ester monomer.
[0028] Examples of monomers other than vinyl ester monomers copolymerizable with vinyl ester monomers include α-olefin monomers such as ethylene and propylene; alkyl (meth)acrylate monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; unsaturated amide monomers such as (meth)acrylamide and N-hydroxymethyl acrylamide; unsaturated carboxylic acid monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, and fumaric acid; alkyl (methyl, ethyl, propyl, etc.) ester monomers of unsaturated carboxylic acids; anhydrides of unsaturated carboxylic acids such as maleic anhydride; salts of unsaturated carboxylic acids with sodium, potassium, ammonium, and the like; monomers containing a glycidyl group such as allyl glycidyl ether and glycidyl (meth)acrylate; monomers containing a sulfonic acid group such as 2-acrylamido-2-methylpropanesulfonic acid or their salts; monomers containing a phosphoric acid group such as (acid phosphoryloxy)ethyl methacrylate and (acid phosphoryloxy)propyl methacrylate; alkyl vinyl ether monomers; and the like.
[0029] The multifunctional monomer copolymerizable with the vinyl ester monomer is not particularly limited, and compounds having two or more polymerizable unsaturated bonds in the molecule can be used, for example, divinyl ethers such as propylene glycol divinyl ether, butanediol divinyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, and polypropylene glycol divinyl ether; divinyl sulfonic acid compounds; and the like.
[0030] In addition, as the multifunctional monomers copolymerizable with the vinyl ester monomers, there are diene compounds such as pentadiene, hexadiene, heptadiene, octadiene, nonadiene, and decadiene; diallyl ether compounds such as glycerol diallyl ether, diethylene glycol diallyl ether, ethylene glycol diallyl ether, triethylene glycol diallyl ether, polyethylene glycol diallyl ether, trimethylolpropane diallyl ether, and pentaerythritol diallyl ether; triallyl ether compounds such as allyl methacrylate, glycerol triallyl ether, trimethylolpropane triallyl ether, and pentaerythritol triallyl ether; pentaerythritol triallyl ether; Tetraallyl ether compounds such as alcohol tetraallyl ether; monomers containing allyl ester groups such as diallyl phthalate, diallyl maleate, diallyl itaconate, diallyl terephthalate, and diallyl adipate; monomers containing allyl amino groups such as diallylamine and diallylmethylamine, diallylamine compounds, and triallylamine; monomers containing allyl ammonium groups such as diallyl ammonium salts such as diallyldimethylammonium chloride; monomers containing two or more allyl groups such as triallyl isocyanurate, 1,3-diallyl urea, triallyl phosphate, and diallyl disulfide; and the like.
[0031] In addition, examples of the multifunctional monomer copolymerizable with the vinyl ester monomer include: monomers having (meth)acrylic acid such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, glycerol di(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and isocyanuric acid tri(meth)acrylate; monomers having (meth)acrylamide such as N,N'-methylenebis(meth)acrylamide and N,N'-ethylenebis(meth)acrylamide; divinylbenzene and trivinylbenzene; and the like.
[0032] Among these polyfunctional monomers, triallyl isocyanurate or allyl methacrylate having a carbonyl group or an amide group in the molecule is preferably used from the viewpoint of reactivity with the vinyl ester monomer, and triallyl isocyanurate is particularly preferably used from the viewpoint of being less likely to decompose in a saponification reaction.
[0033] The copolymerization amount of the multifunctional monomer in the vinyl alcohol polymer, that is, the structural unit derived from the multifunctional monomer in the vinyl alcohol polymer is preferably 0.001 to 1.0 mol% relative to 100 mol% of the structural unit derived from the vinyl ester monomer in the vinyl alcohol polymer. The structural unit derived from the multifunctional monomer is more preferably 0.005 to 0.5 mol%, and further preferably 0.01 to 0.2 mol%. When the copolymerization amount of the multifunctional monomer is 0.001 mol% or more, the fluid loss reduction effect can be more fully exerted. When it is 1.0 mol% or less, the vinyl alcohol polymer is not easy to form an excessive cross-linked structure, and in addition to the fluid loss reduction effect, the operability also becomes better.
[0034] The copolymerization amount of the multifunctional monomer can be 13 C-NMR calculation: As an example, the calculation procedure of the copolymerization amount when the polyfunctional monomer is triallyl isocyanurate will be described.
[0035] The vinyl alcohol polymer obtained by copolymerization with triallyl isocyanurate was thoroughly washed with methanol, air-dried at 90° C. for 1 hour, and then dissolved in heavy water to prepare a solution having a concentration of 10% by mass.
[0036] The obtained solution was subjected to a 500 MHz 13 C-NMR (Bruker AV-III HD 500) was used at a measurement temperature of 80°C, an accumulation time of 20,000, and a DCH cryoprobe to obtain 13 C-NMR spectroscopy.
[0037] Based on the obtained spectrum, the integrated value of the peak (30 to 50 ppm) of the methylene group not adjacent to the hydroxyl group in the main chain of the vinyl alcohol polymer obtained by copolymerization with triallyl isocyanurate is set as b, and the integrated value of the peak (150 to 155 ppm) derived from the carbonyl group of triallyl isocyanurate is set as a, and the copolymerization amount X (mol %) of triallyl isocyanurate in the vinyl alcohol polymer obtained by copolymerization with triallyl isocyanurate is calculated according to the following formula (1).
[0038] X=((1 / 3)a / b)×100···(1)
[0039] The polymerization method of the vinyl ester monomer and the multifunctional monomer is not particularly limited, and known polymerization methods such as solution polymerization, suspension polymerization, and bulk polymerization can be used. From the perspective of easy operation and the use of a common solvent with the saponification reaction as a subsequent step, a solution polymerization method in alcohol is preferably used. As the alcohol, methanol is particularly preferably used.
[0040] The saponification degree of the vinyl alcohol polymer used in the present embodiment is 70 to 95 mol%. When the saponification degree is less than 70 mol%, the hydrophobicity of the residual acetyl group is strong, and when the saponification degree is greater than 95 mol%, the hydrogen bonds between the molecules of the vinyl alcohol polymer are too strong. Therefore, in either case, the affinity with water is reduced, resulting in an insufficient fluid loss reduction effect.
[0041] From the viewpoint of the fluid loss reduction effect, the saponification degree is preferably 75 to 90 mol %.
[0042] In addition, the "saponification degree" in this specification means the value calculated by measuring according to JIS K6726 "3.5 saponification degree" of Japanese Industrial Standards.
[0043] The saponification reaction is carried out by dissolving the copolymer of the vinyl ester monomer and the multifunctional monomer in alcohol and adding a base catalyst or an acid catalyst. Examples of the alcohol include methanol, ethanol, butanol, etc. As mentioned above, methanol is particularly preferably used.
[0044] The concentration of the vinyl ester polymer in the alcohol is preferably 5 to 80% in terms of solid content concentration. As an alkali catalyst, for example, alkali catalysts such as hydroxides and alkoxides of alkali metals such as sodium hydroxide, potassium hydroxide, sodium methoxide, sodium ethoxide, and potassium methoxide can be used. As an acid catalyst, for example, inorganic acid aqueous solutions such as hydrochloric acid and sulfuric acid, and organic acids such as p-toluenesulfonic acid can be used. With regard to the amount of these catalysts used, it is preferably 0.1 to 100 millimole equivalents relative to the structural unit from the vinyl ester monomer. The reaction temperature during saponification is preferably in the range of 10 to 70° C., more preferably in the range of 30 to 50° C. The reaction time is preferably 1 to 10 hours.
[0045] The viscosity average polymerization degree of the vinyl alcohol polymer is 1000 to 10000, preferably 1500 to 6000, more preferably 2000 to 5000. If the viscosity average polymerization degree is too low, the fluid loss reduction effect becomes insufficient, while if it is too high, the cement slurry becomes highly viscous and the fluidity decreases.
[0046] The "viscosity average polymerization degree" is a value calculated by the following formula (2) from the limiting viscosity [η] (g / dL) measured at 30°C using an Ostwald viscometer using ion-exchanged water as a solvent.
[0047] log(P)=1.613×log([η]×104 / 8.29)···(2)
[0048] Here, P represents the viscosity average degree of polymerization.
[0049] The particle size of the vinyl alcohol polymer is preferably 75 μm or less and 30% by mass or less, more preferably 25% by mass or less, and further preferably 15% by mass or less. By adjusting the particle size of the vinyl alcohol polymer to 75 μm or less and 30% by mass or less, the dissolution rate of the vinyl alcohol polymer in the cement slurry will not be too fast, and the deterioration of the fluid loss reduction performance can be suppressed.
[0050] In addition, the particle size of the vinyl alcohol polymer is preferably 500 μm or more and 10% by mass or less, more preferably 8% by mass or less, and further preferably 5% by mass or less. By adjusting the particle size of the vinyl alcohol polymer to 500 μm or more and 10% by mass or less, the problem of the vinyl alcohol polymer becoming a defective part and reducing the strength of the cement cured product is less likely to occur during cement curing.
[0051] A cement slurry according to one embodiment of the present invention is characterized by containing a specific amount of the above-mentioned additive for oil well cement.
[0052] The method for adding the vinyl alcohol polymer to the cement slurry is not particularly limited, and a common method such as a method of mixing with a dry cement composition in advance or a method of mixing when preparing the cement slurry can be used.
[0053] The content of the vinyl alcohol polymer in the cement slurry is 0.01 to 30% bwoc, preferably 0.05 to 10% bwoc, and more preferably 0.1 to 5% bwoc. It should be noted that the term "cement weight basis" (bwoc) refers to the weight of the dry additive added to the cement composition based only on the solid content of the cement.
[0054] Example
[0055] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited thereto. It should be noted that, unless otherwise specified, "parts" and "%" mean "parts by mass" and "mass %".
[0056] <Preparation of Vinyl Alcohol Polymer>
[0057] Example 1
[0058] In a polymerization tank equipped with a reflux condenser, a dropping funnel, and a stirrer, 100 parts by mass of vinyl acetate, 0.01 parts by mass of triallyl isocyanurate, 17.0 parts by mass of methanol, and 0.07 parts by mass of Peroyl NPP (NOF Corporation) were charged, and polymerization was carried out at boiling point for 5 hours while stirring under a nitrogen stream. The polymerization was terminated when the conversion rate of vinyl acetate reached 50%, and unreacted vinyl acetate was removed from the polymerization system by a conventional method. A methanol solution of a vinyl acetate-based polymer having a viscosity average degree of polymerization of 5900 was obtained.
[0059] To the methanol solution of the vinyl acetate polymer obtained above, a methanol solution of sodium hydroxide (0.007 mol in terms of sodium hydroxide relative to the structural unit derived from vinyl acetate) was added, and a saponification reaction was carried out at 45° C. for 90 minutes. The obtained reaction solution was heated and dried to obtain a vinyl alcohol polymer according to Example 1 having a saponification degree of 80.0 mol%.
[0060] The dried vinyl alcohol polymer was crushed once with a crusher, and then sieved with a sieve with a mesh size of 500 μm. The sieved product was crushed again with a crusher and mixed thoroughly with the previous sieved product. The vinyl alcohol polymer was obtained with a particle size adjusted to 0% for particles above 500 μm and 12.0% for particles below 75 μm.
[0061] It should be noted that the time until the ratio of particles larger than 500 μm in the primary pulverization becomes 30% or less and the approximate time until the ratio of particles larger than 500 μm in the re-pulverization of the oversize product becomes 5% or less were confirmed in advance by preliminary tests. In the examples, pulverization was performed based on the times confirmed by the preliminary tests.
[0062] Example 2
[0063] A vinyl alcohol polymer was obtained in the same manner as in Example 1 except that the methanol solution of the vinyl acetate polymer obtained in Example 1 was used and the saponification degree of the vinyl alcohol polymer was changed to 88.2 mol %.
[0064] The dried vinyl alcohol polymer was pulverized in the same manner as in Example 1 to adjust the particle size to 0.2% for particles of 500 μm or more and 8.5% for particles of 75 μm or less.
[0065] Example 3
[0066] In a polymerization tank equipped with a reflux condenser, a dropping funnel, and a stirrer, 100 parts by mass of vinyl acetate, 0.036 parts by mass of triallyl isocyanurate, 22.1 parts by mass of methanol, and 0.06 parts by mass of Peroyl NPP (NOF Corporation) were charged, and polymerization was carried out at boiling point for 5 hours while stirring under a nitrogen stream. The polymerization was terminated when the conversion rate of vinyl acetate reached 50%, and unreacted vinyl acetate was removed from the polymerization system by a conventional method. A methanol solution of a vinyl acetate-based polymer having a viscosity average degree of polymerization of 4600 was obtained.
[0067] To the methanol solution of the vinyl acetate polymer obtained above, a methanol solution of sodium hydroxide (0.007 mol in terms of sodium hydroxide relative to the structural unit derived from vinyl acetate) was added, and a saponification reaction was carried out at 45° C. for 90 minutes. The obtained reaction solution was heated and dried to obtain a vinyl alcohol polymer according to Example 3 having a saponification degree of 79.7 mol%.
[0068] The dried vinyl alcohol polymer was pulverized to adjust the particle size in the same manner as in Example 1, thereby obtaining a vinyl alcohol polymer having a particle size of 0.1% or more of 500 μm and 9.8% or less of 75 μm.
[0069] Example 4
[0070] Using the methanol solution of the vinyl acetate polymer obtained in Example 3, the same operation as in Example 3 was carried out to obtain a vinyl alcohol polymer.
[0071] The dried vinyl alcohol polymer was crushed once with a crusher, and then sieved with a sieve with a mesh size of 500 μm. The over-sieve product was crushed again with a crusher and mixed thoroughly with the under-sieve product. The vinyl alcohol polymer was obtained with a particle size adjusted to 0.1% for particles above 500 μm and 32.2% for particles below 75 μm.
[0072] Example 5
[0073] A vinyl alcohol polymer was obtained in the same manner as in Example 3 except that the degree of saponification of the vinyl alcohol polymer was changed to 87.6% by using the methanol solution of the vinyl acetate polymer obtained in Example 3.
[0074] Example 6
[0075] In a polymerization tank equipped with a reflux condenser, a dropping funnel, and a stirrer, 100 parts by mass of vinyl acetate, 0.013 parts by mass of allyl methacrylate, 22.1 parts by mass of methanol, and 0.04 parts by mass of Peroyl NPP (NOF Corporation) were charged, and polymerization was carried out at boiling point for 5 hours while stirring under a nitrogen stream. The polymerization was terminated when the conversion rate of vinyl acetate reached 56%, and unreacted vinyl acetate was removed from the polymerization system by a conventional method. A methanol solution of a vinyl acetate-based polymer having a viscosity average degree of polymerization of 3900 was obtained.
[0076] To the methanol solution of the vinyl acetate polymer obtained above, a methanol solution of sodium hydroxide (0.007 mol in terms of sodium hydroxide relative to the structural unit derived from vinyl acetate) was added, and a saponification reaction was carried out at 45° C. for 90 minutes. The obtained reaction solution was heated and dried to obtain a vinyl alcohol polymer according to Example 6 having a saponification degree of 80.1 mol%.
[0077] The dried vinyl alcohol polymer was pulverized in the same manner as in Example 1 to adjust the particle size to 0% for particles of 500 μm or more and 9.9% for particles of 75 μm or less.
[0078] Comparative Examples 1 to 4
[0079] The case where PVA was not added was designated as Comparative Example 1. In addition, in Comparative Example 1, the filtration loss was measured.
[0080] A PVA according to Comparative Example 2 was obtained in the same manner as in Example 1 except that the polyfunctional monomer was removed.
[0081] A vinyl alcohol polymer according to Comparative Example 3 was obtained in the same manner as in Example 1 except that the methanol solution of the vinyl acetate polymer obtained in Example 1 was used and the saponification degree of the vinyl alcohol polymer was changed to 99 mol %.
[0082] PVA according to Comparative Example 4 was obtained in the same manner as in Example 1 except that the polyfunctional monomer was removed and the amount of methanol charged was reduced to 5.0 parts.
[0083] <Calculation of Viscosity Average Degree of Polymerization of Vinyl Alcohol Polymer>
[0084] The limiting viscosity [η] (g / dL) of the vinyl alcohol polymers of Examples 1 to 6 and Comparative Examples 2 to 4 obtained above was measured, and the viscosity average degree of polymerization was calculated using the above formula (2).
[0085] <Amount of Polyfunctional Monomer Copolymer in Vinyl Alcohol Polymer>
[0086] For the vinyl alcohol polymers according to Examples 1 to 5 obtained above, the copolymerization amount of the polyfunctional monomer was calculated by the following method.
[0087] The vinyl alcohol polymer obtained by copolymerization with triallyl isocyanurate was thoroughly washed with methanol, air-dried at 90° C. for 1 hour, and then dissolved in heavy water to prepare a solution having a concentration of 10% by mass.
[0088] The obtained solution was subjected to a 500 MHz 13 C-NMR (Bruker AV-III HD 500) was used at a measurement temperature of 80°C, an accumulation time of 20,000, and a DCH cryoprobe to obtain 13 C-NMR spectroscopy.
[0089] Based on the obtained spectrum, the integrated value of the peak of the methylene group not adjacent to the hydroxyl group in the main chain of the vinyl alcohol polymer (30 to 50 ppm) is set as b, and the integrated value of the peak of the carbonyl group from triallyl isocyanurate (150 to 155 ppm) is set as a, and the copolymerization amount X (mol %) of triallyl isocyanurate in the vinyl alcohol polymer obtained by copolymerization with triallyl isocyanurate is calculated according to the following formula (1).
[0090] X=((1 / 3)a / b)×100···(1)
[0091] <Determination of Filtrate Loss>
[0092] The filtration loss reduction effect of the vinyl alcohol polymers of each embodiment and comparative example 3 and the PVA of comparative examples 1, 2 and 4 was measured using a 7120 type filtration loss tester manufactured by Chandler Engineering in accordance with the filtration loss evaluation method of the American Petroleum Institute (API) standard 10B-2 (April 2013). The oil well cement used was type G, with a formulation without added coal fly ash and bentonite, and the cement slurry density was 1900 kg / m 3 , slurry output is 0.758m 3 The test was conducted under the condition of 1000 g / m2 of cement. The amount of vinyl alcohol polymer added was 0.25% bwoc at an evaluation temperature of 20°C, 0.4% bwoc at 40°C, 0.6% bwoc at 60°C, 0.8% bwoc at 80°C, and 0.8% bwoc at 100°C. In addition, 0.2% bwoc of lignin sulfonic acid was added as a cement setting retarder at 40°C, and 0.4% bwoc of lignin sulfonic acid was added as a cement setting retarder at 60°C or above.
[0093] The obtained results are shown in Table 1. In the table, "TAIC" of the polyfunctional monomer represents triallyl isocyanurate, and "AM" represents allyl methacrylate.
[0094] [Table 1]
[0095]
[0096] As can be seen from Table 1, the additive for oil well cement containing a vinyl alcohol polymer obtained by the present invention can significantly reduce the fluid loss of oil well cement even at high temperatures.
[0097] From the comparison between the examples and comparative examples 2 and 4, it can be seen that the fluid loss reduction effect at high temperature is insufficient when no multifunctional monomer is copolymerized. In addition, from the comparison between the examples and comparative example 3, it can be seen that if the saponification degree is too high, the fluid loss reduction effect is not exhibited even when a multifunctional monomer is copolymerized.
[0098] The present invention may also be implemented in the following aspects.
[0099] [1] An additive for oil well cement, comprising a vinyl alcohol polymer, wherein the vinyl alcohol polymer is a saponified product of a copolymer of a vinyl ester monomer and a multifunctional monomer, has a saponification degree of 70 to 95 mol % and a viscosity average degree of polymerization of 1,000 to 10,000.
[0100] [2] The oil well cement additive according to [1], wherein the polyfunctional monomer has a carbonyl group or an amide group.
[0101] [3] The oil well cement additive according to [1] or [2], wherein the polyfunctional monomer is triallyl isocyanurate.
[0102] [4] The oil well cement additive according to any one of [1] to [3], wherein the structural unit derived from the polyfunctional monomer in the vinyl alcohol polymer is 0.001 to 1.0 mol % based on 100 mol % of the structural unit derived from the vinyl ester monomer.
[0103] [5] The oil well cement additive according to any one of [1] to [4], wherein the particle size of the vinyl alcohol polymer is 30% by mass or less of 75 μm or less and 10% by mass or less of 500 μm or more.
[0104] [6] A cement slurry comprising 0.01 to 30% bwoc of the additive for oil well cement described in any one of [1] to [5].
Claims
1. An additive for oil well cement, comprising a vinyl alcohol polymer, wherein the vinyl alcohol polymer is a saponified product of a copolymer of a vinyl ester monomer and triallyl isocyanurate, the saponification degree is 70 to 95 mol %, and the viscosity average polymerization degree is 2000 to 10000, Regarding the particle size of the vinyl alcohol polymer, particles of 75 μm or less account for 30% by mass or less, and particles of 500 μm or more account for 10% by mass or less.
2. The oil well cement additive according to claim 1, wherein: The content of the structural unit derived from triallyl isocyanurate in the vinyl alcohol polymer is 0.001 to 1.0 mol % based on 100 mol % of the structural unit derived from the vinyl ester monomer.
3. The oil well cement additive according to claim 1 or 2, wherein: Regarding the particle size of the vinyl alcohol polymer, particles of 75 μm or less account for 25% by mass or less, and particles of 500 μm or more account for 8% by mass or less.
4. A cement slurry comprising 0.01 to 30% bwoc of the oil well cement additive according to any one of claims 1 to 3.