A liquid crystal panel copper-containing laminated film etching solution and its application

By using etching solutions composed of aminocarbazole metal corrosion inhibitors and other formulas, the problem of high cost of IGZO non-destructive copper-molybdenum film etching solutions has been solved, and low-cost, efficient etching effects and good electrical properties have been achieved to meet the needs of liquid crystal displays. production needs.

CN111663138BActive Publication Date: 2024-10-11JIANGSU HEDA ELECTRONIC TECH CO LTD +1
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202010651700.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-08
Publication Date
2024-10-11
Estimated Expiration
2040-07-08

AI Technical Summary

Technical Problem

The existing IGZO lossless copper-molybdenum film etching solution is costly, which affects the production efficiency and profits of LCD displays.

Method used

Using aminocarbazole metal corrosion inhibitors as the main agent and auxiliary agent, combined with hydrogen peroxide, nitric acid, organic acids and organic bases, a low-cost etching solution was designed. By optimizing the formula composition, the cost was reduced and the performance of the etching solution was improved. longevity and stability.

Benefits of technology

A low-cost etching solution is realized, which ensures the electrical performance and etching morphology of the IGZO semiconductor layer, reduces CD-loss and taper angle, meets production needs, and reduces wastewater treatment pressure, meeting green production requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111663138B_ABST
    Figure CN111663138B_ABST
Patent Text Reader

Abstract

The present invention provides a liquid crystal panel copper-containing laminated thin film etching solution and application thereof, wherein the etching solution comprises a main agent and an auxiliary agent, wherein the metal copper corrosion inhibitors in the main agent and the auxiliary agent are aminocarbazole metal corrosion inhibitors. In the present invention, aminocarbazole metal corrosion inhibitors are selected as the metal corrosion inhibitors in the main agent and the auxiliary agent, thereby reducing the product cost, and the etching solution has no effect on the electrical properties of IGZO due to the corrosion inhibitors, and the etching effect is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal surface chemical treatment and relates to a liquid crystal panel copper-containing laminated film etching solution and application thereof. Background Art

[0002] With the development of display technology, flat display devices such as liquid crystal displays (LCD) have been widely used in various consumer electronic products such as mobile phones, televisions, personal digital assistants, digital cameras, laptops, desktop computers, etc. due to their advantages of high image quality, power saving, thin body and wide application range, becoming the mainstream of display devices.

[0003] The working principle of the liquid crystal display panel is to fill liquid crystal molecules between the parallel array (TFT) substrate and the color film (CF) substrate, and adjust the rotation direction of the liquid crystal molecules by adjusting the voltage between the upper and lower substrates, thereby changing the amount of light output of different color resists on the CF and presenting different colors, displaying a colorful picture.

[0004] Existing TFT array substrates usually use amorphous silicon (a-Si) materials to make semiconductor layers. However, as liquid crystal display devices develop towards larger size and higher resolution, the mobility of traditional a-Si can no longer meet the requirements. Metal oxide materials represented by indium gallium zinc oxide (IGZO) have high mobility, and the preparation of corresponding thin film transistors is compatible with existing a-Si semiconductor-driven production lines. In recent years, they have rapidly become the focus of research and development in the display field.

[0005] Commonly used oxide TFT structures include back channel etching (BCE) and etch-stop layer (ESL). In order to prevent the etching solution from damaging the semiconductor layer, the etch-stop layer technology (ESL) needs to construct an etch-stop layer pattern above the semiconductor layer. The back channel etching technology (BCE) uses an etching solution that does not damage the semiconductor and does not require an etch-stop layer pattern. Therefore, BCE has one less mask process than ESL. Therefore, from the perspective of production efficiency and cost, the flat panel display industry prefers to use BCE structure thin film transistors to produce array substrates.

[0006] When IGZO is used as a semiconductor layer of a thin-film transistor, it is formed on a glass substrate using a film forming process such as sputtering, and the IGZO active layer pattern is constructed using a dry etching process. Then, copper (Cu), molybdenum (Mo), etc. are formed on it using a PVD film forming process, and then the electrode pattern that needs to be retained is formed through processes such as applying photoresist, exposure, and development, thereby forming the source / drain wiring.

[0007] The metal layer of the copper and molybdenum multilayer metal film, which is more common recently, is generally wet-etched to produce a predetermined pattern on the metal layer. If there is an undercut between the end of the metal layer and the substrate of the pattern, it will make the coverage uneven in the subsequent process, and then cause unexpected short circuit. Therefore, the etching shape between the end of the metal layer and the substrate is very important for the yield of the liquid crystal display, and the composition of the etching solution used in wet etching is one of the key factors to control the etching shape.

[0008] In order to obtain a better wiring shape, azole corrosion inhibitors such as 5-aminotetrazolyl and 3-aminotriazole are often added to the hydrogen peroxide etching solution used in the past. However, these azole corrosion inhibitors are quite expensive (up to 800 to 900 yuan per kilogram), which affects the profit level of the enterprise.

[0009] Therefore, how to reduce the production cost of the chemical solution while ensuring the chemical solution etching characteristics and the product electrical characteristics (especially achieving better electrical characteristics) is a problem that each chemical solution manufacturer needs to solve. Summary of the invention

[0010] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a liquid crystal panel copper-containing laminated thin film etching solution and its application, which overcomes the high cost problem of the existing IGZO non-destructive copper-molybdenum film etching solution and provides an etching solution with low cost, no effect on the electrical properties of IGZO and good etching effect.

[0011] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0012] On the one hand, the present invention provides a liquid crystal panel copper-containing laminated thin film etching solution, the etching solution comprises a main agent and an auxiliary agent, and the metal corrosion inhibitors in the main agent and the auxiliary agent are aminocarbazole metal corrosion inhibitors.

[0013] In the present invention, aminocarbazole metal corrosion inhibitors are selected as the metal corrosion inhibitors in the main agent and the auxiliary agent, which reduces the product cost on the one hand, and on the other hand, the addition of such corrosion inhibitors can obtain good etching morphology and has no effect on the electrical properties of the product.

[0014] Preferably, the main agent, with its total mass being 100%, comprises the following components:

[0015]

[0016] In the present invention, the formula composition of the main agent is screened. By using such a combination of components, the cost can be reduced on the one hand, and the service life and etching stability of the etching solution can be improved on the other hand.

[0017] In the main agent of the present invention, the mass percentage of the hydrogen peroxide can be 5%, 5.5%, 5.8%, 6%, 6.3%, 6.5%, 6.8%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 11%, 12%, 13%, 14% or 15%.

[0018] In the main agent of the present invention, the mass percentage of the nitric acid (calculated as its solute HNO3) can be 0.01%, 0.05%, 0.08%, 1%, 1.3%, 1.5%, 1.8% or 2%.

[0019] In the main agent of the present invention, the mass percentage of the organic acid can be 0.01%, 0.05%, 0.08%, 1%, 1.3%, 1.5%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9% or 10%.

[0020] In the main agent of the present invention, the mass percentage of the organic base can be 0.01%, 0.05%, 0.08%, 1%, 1.3%, 1.5%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9% or 10%.

[0021] In the main agent of the present invention, the mass percentage of the hydrogen peroxide stabilizer can be 0.01%, 0.03%, 0.05%, 0.08%, 0.1%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8% or 2%.

[0022] In the main agent of the present invention, the mass percentage of the aminocarbazole metal corrosion inhibitor can be 0.01%, 0.03%, 0.05%, 0.08%, 0.1%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8% or 2%, preferably 0.05-1.5%. In order to obtain lower CD-loss and avoid tailing, the mass percentage of the aminocarbazole metal corrosion inhibitor is preferably 0.05% or more. In order to shorten the etching time or to avoid the occurrence of chamfering, the mass percentage of the aminocarbazole metal corrosion inhibitor is preferably 1.5% or less.

[0023] As a preferred technical solution, the main agent, with its total mass as 100%, includes the following components:

[0024]

[0025] Preferably, the auxiliary agent, with its total mass as 100%, comprises the following components:

[0026]

[0027] In the present invention, the components of the auxiliary agent cooperate with each other and can cooperate well with the main agent, thereby improving the copper loading capacity of the etching solution and enhancing the etching effect.

[0028] In the adjuvant of the present invention, the mass percentage of the nitric acid (calculated as its solute HNO3) can be 0.1%, 0.5%, 1%, 3%, 5%, 7%, 9%, 10%, 13%, 15%, 18%, 20%.

[0029] In the adjuvant of the present invention, the mass percentage of the organic acid can be 1%, 3%, 5%, 7%, 9%, 10%, 13%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, or 50%.

[0030] In the adjuvant of the present invention, the mass percentage of the organic base can be 1%, 3%, 5%, 7%, 9%, 10%, 13%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%.

[0031] In the adjuvant of the present invention, the mass percentage of the aminocarbazole metal corrosion inhibitor can be 0.01%, 0.03%, 0.05%, 0.08%, 0.1%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8% or 2%.

[0032] As a preferred technical solution, the auxiliary agent, with its total mass as 100%, includes the following components:

[0033]

[0034] In the present invention, the hydrogen peroxide is provided by hydrogen peroxide. Preferably, the hydrogen peroxide of the present invention is electronic grade hydrogen peroxide, which can oxidize metal elements into metal oxides.

[0035] In order to improve the copper loading capacity of the etching solution, the present invention adopts a main agent and an auxiliary agent. In order to reduce the cost of the etching solution, the present invention adds a small amount of inorganic acid to the system, which can reduce the use of organic acid.

[0036] In the present invention, the mass percentage of the nitric acid is calculated based on the solute HNO3. In actual operation, electronic grade nitric acid of different concentrations can be selected according to actual conditions. The reagent is used to dissolve the metal oxide after metal oxidation, so that it is converted into a free state.

[0037] Preferably, the organic acid of the present invention is any one of polybasic organic acids and amino acids or a combination of at least two thereof. These reagents can provide hydrogen ions to the system, so that the metal oxide is continuously dissolved. At the same time, the carbonyl group in the organic acid can form a coordination bond with the copper ion to form a complex, thereby reducing the concentration of free copper ions in the etching solution, inhibiting the active decomposition rate of hydrogen peroxide, and improving the service life and etching stability of the etching solution.

[0038] Preferably, the organic acid is a polycarboxylic acid having 2 to 6 (eg, 2, 3, 4, 5 or 6) carbon atoms.

[0039] Preferably, the organic acid of the present invention is selected from but not limited to any one of oxalic acid, succinic acid, malic acid, citric acid, isocitric acid, maleic acid, glutamic acid, alanine, glycine, alanine, aminosuccinic acid or tartaric acid, or a combination of at least two thereof.

[0040] Preferably, the organic base of the present invention is any one or a combination of at least two of alcohol amines or polyamine compounds. These reagents can adjust the pH of the solution to prevent large fluctuations in the pH of the solution, dissolve metal oxides such as molybdenum oxide, and complex with metal copper ions to inhibit the catalytic decomposition of hydrogen peroxide by metal ions, which is beneficial to improving etching stability.

[0041] Preferably, the organic base is any one or a combination of at least two of an alcohol amine compound or a polyamine compound containing 2-6 (eg, 2, 3, 4, 5 or 6) carbon atoms.

[0042] Preferably, the organic base of the present invention is selected from but not limited to isopropanolamine, dimethylethanolamine, triethanolamine, diisopropanolamine, tetramethylammonium hydroxide, diethylaminopropylamine, ethylenediamine, diethylamine, propylenediamine, butylenediamine, 2-hydroxybutylenediamine, N,N-dihydroxyethylbutylenediamine, N,N-diaminomethylethylenediamine, N,N-diaminomethylpropylenediamine or any one of N,N-diaminoethylpropylenediamine or a combination of at least two thereof.

[0043] Preferably, the hydrogen peroxide stabilizer of the present invention is any one of urea or sulfonic acid compounds or a combination of at least two of them. These compounds can form complexes with metal impurity ions such as calcium, iron, and magnesium in the etching solution, reduce the catalytic decomposition rate of metal ions on hydrogen peroxide, increase the storage life of the etching solution, and extend the storage period of the etching solution.

[0044] Preferably, the hydrogen peroxide stabilizer of the present invention is selected from but not limited to any one of phenylurea, p-hydroxyphenylurea, p-aminophenylurea, thiourea, urea, p-hydroxybenzenesulfonic acid or sodium p-hydroxybenzenesulfonate, or a combination of at least two thereof.

[0045] In order to obtain better copper loading capacity and improve the service life of the etching solution, the present invention selects aminocarbazole metal corrosion inhibitors. The molecules of this type of compound can generate certain van der Waals forces with copper atoms, which can inhibit the etching rate of the etching solution on the copper film.

[0046] Preferably, the aminocarbazole metal corrosion inhibitor of the present invention is selected from 9-aminocarbazole and / or 3,9-diaminocarbazole. If the metal corrosion inhibitor in the etching solution is two or more aminocarbazole compounds, the present invention does not particularly limit the ratio between the compounds.

[0047] Preferably, the pH value of the etching solution system of the present invention is 3-5, for example, 3, 3.3, 3.5, 3.8, 4, 4.3, 4.5, 4.8 or 5.

[0048] The etching solution of the present invention can be used for etching copper-containing laminated wires on an IGZO-TFT substrate, wherein the copper-containing laminated wires are copper / molybdenum, copper / molybdenum-niobium, copper / magnesium-aluminum, and the like.

[0049] IGZO is easily corroded under high concentrations of strong acid, strong alkali or hydrofluoric acid, so it is necessary to avoid the etching solution containing high concentrations of strong acid or hydrofluoric acid. In the etching solution of the present invention, in order to ensure the corrosion of the IGZO semiconductor film layer, ensure the electrical properties of the semiconductor, and stabilize the etching effect, a low mass percentage of nitric acid is used in combination with an organic acid.

[0050] On the other hand, the present invention provides the use of the above-mentioned copper-containing laminated thin film etching solution for liquid crystal panels in etching of liquid crystal panels.

[0051] In the present invention, when etching is performed using the etching solution, the weight of the main agent is 100%, and the added amount of the auxiliary agent is 0.3%-0.7%, for example, 0.3%, 0.35%, 0.38%, 0.4%, 0.45%, 0.48%, 0.5%, 0.55%, 0.58%, 0.6%, 0.65%, 0.68% or 0.7%.

[0052] Compared with the prior art, the present invention has the following beneficial effects:

[0053] 1. Using a small amount of nitric acid greatly reduces the amount of organic acid used, and can even completely replace the expensive malonic acid, greatly reducing the cost of etching solution.

[0054] 2. The combination of organic acid and organic base can have a great buffering effect on the pH of the system, preventing the pH of the etching solution system from fluctuating greatly. At the same time, organic acid and organic base can act as complexing agents for metal ions such as copper ions, which can capture free metal ions, weaken the catalytic decomposition of hydrogen peroxide by metal ions, and avoid the occurrence of phenomena such as boiling caused by the rapid decomposition of hydrogen peroxide, ultimately ensuring that the etching requirements are met under safe conditions.

[0055] 4. The aminocarbazole metal corrosion inhibitor described in the present invention perfectly ensures the integrity of the film layer of the IGZO semiconductor layer, obtains a good etching morphology, enables the CD-loss and taper angle of the etching solution to better meet production requirements (such as CD loss of one side is less than 1 μm and the slope angle is 35-55 degrees), and ensures the electrical properties of the semiconductor.

[0056] 5. The etching solution of the present invention does not contain fluorine ions and phosphorus ions, which reduces the pressure of wastewater treatment, reduces the cost of sewage treatment, and meets the requirements of green production. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1A This is a SEM photograph of the etched cross section of the etching solution of Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 130s, and the scale is 1μm;

[0058] Figure 1B This is a SEM photograph of the etched surface of the etching solution of Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 130s, and the scale is 3μm;

[0059] Figure 2A This is a SEM photograph of the etched cross section of the etching solution of Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 150s, and the scale is 1μm;

[0060] Figure 2B This is a SEM photograph of the etched surface of the etching solution of Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 150s, and the scale is 3μm;

[0061] Figure 3A This is a SEM photograph of the etching cross section of the etching solution of Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 170s, and the scale is 500nm;

[0062] Figure 3B This is a SEM photograph of the etched surface of the etching solution of Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 170s, and the scale is 3μm;

[0063] Figure 4A This is a SEM photograph of the etched cross section of the etching solution of Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 140s, and the scale is 1μm;

[0064] Figure 4B This is a SEM photograph of the etched surface of the etching solution of Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 140s, and the scale is 3μm;

[0065] Figure 5AThis is a SEM photograph of the etched cross section of the etching solution of Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 160s, and the scale is 1μm;

[0066] Figure 5B This is a SEM photograph of the etched surface of the etching solution of Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 160s, and the scale is 3μm;

[0067] Fig. 6A This is a SEM photograph of the etched cross section of the etching solution of Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 180s, and the scale is 1μm;

[0068] Figure 6B This is a SEM photograph of the etched surface of the etching solution of Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 180s, and the scale is 3μm;

[0069] Fig. 7A This is a SEM photograph of the etching cross section of the etching solution of Comparative Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 130s, and the scale is 1μm;

[0070] Figure 7B This is a SEM photograph of the etched surface of the etching solution of Comparative Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 130s, and the scale is 2μm;

[0071] Fig. 8A This is a SEM photograph of the etching cross section of the etching solution of Comparative Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 150s, and the scale is 500nm;

[0072] Figure 8B This is a SEM photograph of the etched surface of the etching solution of Comparative Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 150s, and the scale is 3μm;

[0073] Fig. 9A This is a SEM photograph of the etching cross section of the etching solution of Comparative Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 170s, and the scale is 1μm;

[0074] Fig. 9B This is a SEM photograph of the etched surface of the etching solution of Comparative Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 170s, and the scale is 3μm;

[0075] Fig. 10A This is a SEM photograph of the etching cross section of the etching solution of Comparative Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 190s, and the scale is 1μm;

[0076] Fig. 10BThis is a SEM photograph of the etched surface of the etching solution of Comparative Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 190s, and the scale is 3μm;

[0077] Fig.11A This is a SEM photograph of the etching cross section of the etching solution of Comparative Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 210s, and the scale is 1μm;

[0078] Fig. 11B This is a SEM photograph of the etched surface of the etching solution of Comparative Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 210s, and the scale is 2μm;

[0079] Fig. 12A This is a SEM photograph of the etching cross section of the etching solution of Comparative Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 230s, and the scale is 1μm;

[0080] Fig. 12B This is a SEM photograph of the etched surface of the etching solution of Comparative Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 230s, and the scale is 3μm;

[0081] Fig.13 This is a SEM photograph of the etched cross section of the etching solution of Example 1 of the present invention when the copper ion concentration is 500ppm and the etching time is 165s, and the scale is 1μm;

[0082] Fig.14 This is a SEM photograph of the etching cross section of the etching solution of Example 1 of the present invention when the copper ion concentration is 2500ppm and the etching time is 165s, and the scale is 1μm;

[0083] Fig.15 This is a SEM photograph of the etching cross section of the etching solution of Example 1 of the present invention when the copper ion concentration is 5000ppm and the etching time is 165s, and the scale is 1μm;

[0084] Fig.16 This is a SEM photograph of the etched cross section of the etching solution of Example 1 of the present invention when the copper ion concentration is 7500ppm and the etching time is 165s, and the scale is 1μm;

[0085] Fig.17 This is a SEM photograph of the etching cross section of the etching solution of Example 1 of the present invention when the copper ion concentration is 10000ppm and the etching time is 165s, and the scale is 1μm;

[0086] Fig.18 This is a SEM photograph of the etched cross section of the etching solution of Example 2 of the present invention when the copper ion concentration is 500ppm and the etching time is 170s, and the scale is 1μm;

[0087] Fig.19This is a SEM photograph of the etched cross section of the etching solution of Example 2 of the present invention when the copper ion concentration is 2500ppm and the etching time is 170s, and the scale is 1μm;

[0088] Fig. 20 This is a SEM photograph of the etched cross section of the etching solution of Example 2 of the present invention when the copper ion concentration is 5000ppm and the etching time is 170s, and the scale is 1μm;

[0089] Fig.21 This is a SEM photograph of the etched cross section of the etching solution of Example 2 of the present invention when the copper ion concentration is 7500ppm and the etching time is 170s, and the scale is 1μm;

[0090] Fig. 22 This is a SEM photograph of the etched cross section of the etching solution of Example 2 of the present invention when the copper ion concentration is 10000 ppm and the etching time is 170 s, and the scale is 1 μm. DETAILED DESCRIPTION

[0091] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only used to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0092] Examples 1-5 and Comparative Examples 1-4

[0093] The compositions of the etching solutions of the embodiments and comparative examples are shown in Table 1.

[0094] Table 1

[0095]

[0096]

[0097] The above etching solution main agent and auxiliary agent (see Table 1) are produced using a PP lined stirred kettle with a condenser tube. After being filtered and qualified (the number of particles with a particle size of 0.5 μm or more is less than 100), they can be used. The etching solution system is maintained below 45°C during the production process.

[0098] A hand-operated etcher was used to etch a TFT substrate with a copper / molybdenum-niobium / IGZO film thickness of 4000 / 200 / 800A, and different etching times were used to obtain the optimal etching time for the substrate.

[0099] Experimental steps: 1: Take a portion of the etching agent and inject it into the tank of the etching machine, 2: Add 0.5% of the etching auxiliary agent to the tank relative to the weight of the etching agent, 3: Increase the copper ion concentration in the etching solution to 500ppm by dissolving the copper foil, 4: While dissolving the copper foil, turn on the temperature control system of the etching machine to maintain the etching solution temperature at 30°C, 5: After the temperature is stable and the copper foil is dissolved, put the prepared substrate in and start etching. The etching conditions (i.e., etching time TET) and etching results are shown in Table 2.

[0100] Table 2

[0101]

[0102]

[0103] By comparing the above experimental results, it can be found that the etching solution containing aminonitrogen azole compounds of the present invention has good etching characteristics for laminated metal films, wherein the content of aminocarbazole compounds has a significant effect on the etching effect. When the content of aminocarbazole compounds in the etching solution is low, the etching rate of the etching solution on copper is high, so the CD-loss is large, and the molybdenum layer is prone to tailing. When the content of aminonitrogen azole compounds in the etching solution is high, the etching time is long, and chamfers will occur, and there is a risk of disconnection.

[0104] Comparing the above experimental results, it can be found that the effect of the addition of nitric acid on the product etching is very obvious: when the addition of nitric acid is 1% and 0.5%, the etching results meet the customer's requirements of single-side loss less than 1μm and taper angle between 35 and 55°. Figure 1A to Figure 6B (Measured by Hitachi's S-3400N scanning electron microscope); When the amount of nitric acid added is 3%, the copper layer etching rate is very fast, while the molybdenum-niobium layer etching rate is slow. When the CD-loss reaches 1μm, there is still a lot of molybdenum residue, and the SEM photos show that there are obvious cracks between the copper and molybdenum-niobium layers, which will cause short circuits during subsequent coating. Figures 7A to 9B When nitric acid is not added, the etching rate of the copper layer is very slow, and molybdenum residue or chamfers are likely to appear, causing the subsequent coating to collapse and resulting in product defects. Figures 10A to 12B .

[0105] Copper ion loading capacity test:

[0106] 0.5% auxiliary agent was added to the etching agent of Example 1 (based on the weight of the main agent as 100%, the same below), copper foil was added to increase the copper ion concentration to 500ppm, and etching was continued for 170s to obtain an etching sample 1 after etching with an etching solution at a copper ion concentration of 500ppm. The sample was split and a SEM photo was taken. Fig.13 .

[0107] 2% auxiliary agent was added to the etching agent of Example 1, copper foil was added to increase the copper ion concentration to 2500ppm, and etching was continued for 170s to obtain an etching sample 2 after etching with an etching solution at a copper ion concentration of 2500ppm. The sample was split and SEM photos were taken. Fig.14 .

[0108] 2.5% auxiliary agent was added to the etching agent of Example 1, copper foil was added to increase the copper ion concentration to 5000ppm, and etching was continued for 170s to obtain an etching sample 3 after etching with an etching solution at a copper ion concentration of 5000ppm. The sample was split and SEM photos were taken. Fig.15 .

[0109] 2.5% auxiliary agent was added to the etching agent of Example 1, copper foil was added to increase the copper ion concentration to 7500ppm, and etching was continued for 170s to obtain an etching sample 4 after etching with an etching solution at a copper ion concentration of 7500ppm. The sample was split and SEM photos were taken. Fig.16 .

[0110] 2.5% auxiliary agent was added to the etching agent of Example 1, and copper foil was added to increase the copper ion concentration to 10000ppm. Etching was continued for 170s to obtain an etched sample 5 after etching with an etching solution with a copper ion concentration of 10000ppm. The sample was split and SEM photos were taken. Fig.17 .

[0111] According to the copper ion loading capacity test process of the etching solution of Example 1, the copper ion loading capacity test was performed on Examples 2-3 and Comparative Examples 3-4, respectively. The SEM photos of the etching cross-section of the sample etched for 170s by the etching solution of Example 2 at different copper ion concentrations are shown in FIG. Figures 18 to 22 The SEM data of each group of experiments are shown in Tables 3 to 7 below.

[0112] Table 3

[0113]

[0114] Table 4

[0115]

[0116] Table 5

[0117]

[0118] Table 6

[0119]

[0120] Table 7

[0121]

[0122]

[0123] It can be seen from Tables 3 to 5 that Examples 1-3 all demonstrate a very high copper ion loading capacity of about 10,000 ppm, and within the etching life range, the CD-loss and taper angle change ranges are small, which can better meet the needs of large-size, high-precision products.

[0124] It can be seen from Table 6 and Table 7 that Comparative Examples 3 and Comparative Examples 4 can also show good etching characteristics when the copper ion content is below 7000ppm, but when the copper ion content is higher, all aspects of performance will be affected. It can be seen that from the perspective of copper ion loading capacity, Comparative Examples 3-4 are significantly lower than Examples 1-3.

[0125] In the above embodiment, from the perspective of material cost, the unit price of aminocarbazole chemicals (less than 100 yuan per kilogram) is one order of magnitude lower than that of 5-aminotetrazolyl and 3-aminotriazole, and the etching solution prepared with them has a higher copper loading capacity. Therefore, aminocarbazole corrosion inhibitors have obvious advantages over corrosion inhibitors such as 5-aminotetrazolyl and 3-aminotriazole. While reducing costs, they can also make the etching solution have a higher copper loading capacity and a longer service life.

[0126] Electrical performance test:

[0127] Take one substrate sample and divide it into four small pieces. Three of them are placed in the etching solution of Example 1 with a copper ion concentration of 5000ppm for 0, 30, and 60 minutes respectively, then taken out and cleaned. Then measure the CV curve of the TFT in the substrate and calculate the electron mobility of the active layer. The calculation results are shown in Table 8 below.

[0128] Table 8

[0129]

[0130]

[0131] It can be seen from Table 8 that the etching solution has limited impact on the performance of the IGZO-TFT device before and after etching, and does not affect the product quality, and can fully meet customer needs. The same investigation was carried out on the etching solution of Example 2-3, and the same conclusion was obtained, that is, the single-sided CD-loss and taper angle can perfectly meet the product requirements, there is no metal residue, no chamfers and cracks, and the electrical properties of the product are not damaged.

[0132] In summary, the etching solution containing aminocarbazole metal corrosion inhibitor of the present invention can reduce the cost while making the etching solution have a higher copper loading capacity, has no effect on the electrical properties of IGZO, has a good etching effect, and has a longer service life.

[0133] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the copper-containing laminated thin film etching solution for liquid crystal panels and its application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A liquid crystal panel copper-containing laminated thin film etching solution, characterized in that: The etching solution comprises a main agent and an auxiliary agent, wherein the metal copper corrosion inhibitors in the main agent and the auxiliary agent are aminocarbazole metal corrosion inhibitors; The main agent, with its total mass as 100%, is composed of the following components: The balance is water; The auxiliary agent, with its total mass as 100%, is composed of the following components: The balance is water; The organic acid is succinic acid and / or glycine; the aminocarbazole metal corrosion inhibitor is 9-aminocarbazole; The hydrogen peroxide stabilizer is selected from any one or a combination of at least two of phenylurea, p-hydroxyphenylurea, p-aminophenylurea, thiourea, urea, p-hydroxybenzenesulfonic acid or sodium p-hydroxybenzenesulfonate; When etching is performed using the etching solution, the weight of the main agent is 100%, and the amount of the auxiliary agent added is 2.5%.

2. The etching solution for the copper-containing laminated thin film of a liquid crystal panel according to claim 1, characterized in that: In the main agent, the mass percentage content of aminocarbazole metal corrosion inhibitor is 0.05-1.5%.

3. The etching solution for the copper-containing laminated thin film of liquid crystal panel according to claim 1, characterized in that: The main agent, with its total mass as 100%, is composed of the following components composition: The balance is water.

4. The etching solution for the copper-containing laminated thin film of a liquid crystal panel according to claim 1, characterized in that: The auxiliary agent, with its total mass as 100%, is composed of the following components composition: The balance is water.

5. The etching solution for the copper-containing laminated thin film of liquid crystal panel according to claim 1, characterized in that: The hydrogen peroxide is provided by hydrogen peroxide.

6. The etching solution for the copper-containing laminated thin film of liquid crystal panel according to claim 5, characterized in that: The hydrogen peroxide is electronic grade hydrogen peroxide.

7. The etching solution for the copper-containing laminated thin film of a liquid crystal panel according to claim 1, characterized in that: The nitric acid is electronic grade nitric acid.

8. The etching solution for the copper-containing laminated thin film of a liquid crystal panel according to claim 1, characterized in that: The organic base is any one of alcohol amines or polyamine compounds or a combination of at least two of them.

9. The etching solution for the copper-containing laminated thin film of a liquid crystal panel according to claim 1, characterized in that: The organic base is any one of an alcohol amine compound or a polyamine compound containing 2 to 6 carbon atoms, or a combination of at least two of them.

10. The etching solution for the copper-containing laminated thin film of a liquid crystal panel according to claim 1, characterized in that: The organic base is selected from any one or a combination of at least two of isopropanolamine, dimethylethanolamine, triethanolamine, diisopropanolamine, tetramethylammonium hydroxide, diethylaminopropylamine, ethylenediamine, diethylamine, propylenediamine, butylenediamine, 2-hydroxybutylenediamine, N,N-dihydroxyethylbutylenediamine, N,N-diaminomethylethylenediamine, N,N-diaminomethylpropylenediamine or N,N-diaminoethylpropylenediamine.

11. The etching solution for the copper-containing laminated thin film of a liquid crystal panel according to claim 1, characterized in that: The hydrogen peroxide stabilizer is any one of urea or sulfonic acid compounds or a combination of at least two of them.

12. The etching solution for the copper-containing laminated thin film of a liquid crystal panel according to claim 1, characterized in that: The pH value of the etching solution system is 3-5.

13. Use of the etching solution for copper-containing laminated thin films of liquid crystal panels according to any one of claims 1 to 12 in etching of liquid crystal panels.

Citation Information

Patent Citations

  • Etchant for copper / molybdenum-based multilayer thin film

    CN103717787A

  • Etching solution for copper-molybdenum alloy film

    CN107151795A

  • Etching Liquid Composition Used For Copper-based Metal Film And Method Of Utilizing Same To Manufacture Array Substrate Used For Liquid Crystal Display

    CN107447215A

  • hydrogen peroxide stabilizer and etching composition containing the same

    CN107475715A

  • Etching solution for copper / molybdenum film layer and application thereof

    CN107858685A