Method for preparing a catalyst having a conductive oxide protective layer and a catalyst prepared by the method
By using atomic layer deposition technology to form a conductive oxide protective layer on the fuel cell catalyst, the problem of catalyst particle agglomeration is solved and the durability and battery performance of the fuel cell are improved.
Patent Information
- Application Number
- CN202010120226.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-02-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-02-26
AI Technical Summary
Existing fuel cell catalysts are prone to catalyst particle agglomeration during long-term use, resulting in reduced battery performance and durability.
Atomic layer deposition (ALD) technology is used to form a conductive oxide protective layer on the carbon support, forming a network structure to prevent the agglomeration of catalyst particles.
It can effectively prevent the agglomeration of catalyst particles, improve the durability of the catalyst, maintain or improve the catalytic activity, and extend the service life of the fuel cell.
Smart Images

Figure CN111725522B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a catalyst having a conductive oxide protective layer and a catalyst prepared by the method. Background Art
[0002] Polymer electrolyte membrane fuel cell (PEMFC) is a high current density, high power fuel cell that can provide at least tens of kilowatts or more of high power under various operating conditions for application in vehicles. For example, PEMFC needs to operate stably in a wide current density range, have no water leakage problems, and be driven quickly.
[0003] The reaction of the fuel cell to generate electricity occurs in a membrane electrode assembly (MEA), which includes an ionomer-based membrane and a pair of electrodes (i.e., an anode and a cathode). Meanwhile, in order to improve the performance of electrodes used in PEMFC, a catalyst is usually added to the electrodes.
[0004] For example, the catalyst of platinum (Pt) nanoparticles dispersed on the carrier made of carbon (C) material can be mainly used as the catalyst of fuel cell electrochemical reaction. In particular, it is necessary to develop a method that can improve the efficiency of catalyst use while reducing the amount of precious metal catalyst (e.g., platinum (Pt)). For this purpose, research is being conducted to improve the activity of catalyst by adjusting the size of platinum (Pt) particles to a small level of several nanometers (nm). On the other hand, conventional fuel cells will undergo coarsening (e.g., Ostwald ripening) during long-term use, and the metal catalyst contained in the carbon carrier will agglomerate together.
[0005] For example, in related fields, Figure 1A and Figure 1B The changes in catalyst distribution in a conventional fuel cell during initial use and after long-term use are shown respectively.
[0006] like Figure 1A As shown in Figure 1, at the initial stage, the catalyst present in the fuel cell is uniformly distributed with a relatively uniform size (mainly 3 to 5 nm). Figure 1B As shown, after using the fuel cell for a long time, the nano-sized catalyst particles may be observed to aggregate (ie, coarsen). In particular, the catalyst particles may aggregate into particles of 6 nm or larger, and a large number of the catalyst particles may aggregate into particles of 10 nm or larger.
[0007] The agglomeration of the catalyst particles can reduce the cell performance and the overall durability of the fuel cell. Therefore, it is necessary to develop a technology to prevent the agglomeration of fuel cell catalyst particles.
[0008] The above information disclosed in this Background Art is provided only for enhancement of understanding of the background of the invention and therefore it may contain information that does not form the prior art that is already known in his country to a person skilled in the art. Summary of the invention
[0009] In a preferred aspect, provided is a method of forming a catalyst provided with a conductive oxide protective layer by using atomic layer deposition (ALD) so that agglomeration of catalyst particles included in a fuel cell can be prevented and durability of the catalyst can be improved.
[0010] In one aspect, provided is a conductive oxide protective layer uniformly formed on a catalyst and a support having a large surface area by performing atomic layer deposition (ALD).
[0011] In one aspect, provided is a method for preventing agglomeration of catalyst particles by forming a conductive oxide having a controlled network structure on an atomic basis using atomic layer deposition (ALD).
[0012] The purpose of the present invention is not limited to the above-mentioned purpose. Other details of the present invention will be incorporated into the specific implementation manner and the drawings of the present invention.
[0013] In a preferred aspect, a method for preparing a catalyst including a conductive oxide protective layer is provided. The method may include providing (e.g., supplying) a carbon support loaded with a metal catalyst to a fluidized bed reactor; and forming the conductive oxide protective layer using atomic layer deposition (ALD). The conductive oxide protective layer may be suitably formed on or around the carbon support and the metal catalyst disposed in the fluidized bed reactor.
[0014] As used herein, the term "atomic layer deposition" or "ALD" refers to a deposition technique that forms a surface structure (e.g., a thin film or a mesh surface) having, for example, atomic-level thickness. For example, ALD can include the sequential use of a vapor phase chemistry, for example, using two chemicals or precursors. In certain embodiments, these precursors can be reacted one at a time in a sequential manner on the surface of a substrate (e.g., a carbon support). In certain embodiments, separate and / or different precursors can be sequentially and / or alternately exposed to the surface to react, thereby forming a mesh surface.
[0015] Atomic layer deposition may suitably include: supplying a conductive oxide precursor to a fluidized bed reactor; performing a first purge by supplying an inert gas to the fluidized bed reactor; converting the conductive oxide precursor into a conductive oxide by supplying a reactive gas to the fluidized bed reactor; and performing a second purge by supplying an inert gas to the fluidized bed reactor.
[0016] Preferably, the metal catalyst may include platinum (Pt).
[0017] The method may further include adjusting an internal pressure of the fluidized bed reactor to about 0.1 Torr to 0.5 Torr by pumping after providing the carbon support to the fluidized bed reactor and before forming the conductive oxide protective layer.
[0018] In the step of supplying the conductive oxide precursor to the fluidized bed reactor, the conductive oxide precursor may include tetraisopropoxytitanium (Ti[OCH(CH 3 ) 2 ] 4 ), tin tetrachloride (SnCl 4 ) and their combinations.
[0019] In the step of supplying the conductive oxide precursor to the fluidized bed reactor, the deposition operation pressure of the conductive oxide precursor may be appropriately about 1 Torr to 5 Torr.
[0020] In the step of supplying the conductive oxide precursor to the fluidized bed reactor, the conductive oxide precursor may be appropriately supplied to the fluidized bed reactor for about 20 seconds to 100 seconds.
[0021] In the step of converting the conductive oxide precursor into the conductive oxide, the reactive gas may include water vapor (H 2 O).
[0022] In the step of converting the conductive oxide precursor into the conductive oxide, the reactive gas may be supplied to the fluidized bed reactor at a flow rate of about 10 sccm to about 200 sccm.
[0023] In the step of converting the conductive oxide precursor into a conductive oxide, the conductive oxide may include titanium dioxide (TiO 2 ), tin dioxide (SnO 2 ) and their combinations.
[0024] In the purging step, the inert gas may be purged appropriately at a flow rate of about 50 sccm to about 200 sccm.
[0025] In the purging step, the inert gas may be purged for about 60 seconds to 120 seconds.
[0026] Preferably, the atomic layer deposition described herein may be set up as a cycle and repeated.
[0027] The cycle of atomic layer deposition may suitably be repeated about 1 to 20 times.
[0028] In another aspect, a catalyst comprising a conductive oxide protective layer prepared by the above method is provided. The catalyst may include a carbon support, metal catalyst particles and a conductive oxide protective layer, wherein the metal catalyst particles are supported on the carbon support, and the conductive oxide protective layer is formed on the surface of the metal catalyst particles and has a mesh structure.
[0029] The term "net-like structure" used herein refers to a structure having geometric connection points (eg, dots) which do not substantially cover or do not completely cover the structure. Preferably, the dots and the connection parts between the connection points can form a net-like structure.
[0030] The conductive oxide protective layer may suitably have a thickness of about 0.05 nm to 10 nm.
[0031] The metal catalyst particles may suitably include platinum (Pt).
[0032] The conductive oxide protective layer may include a conductive oxide, wherein the conductive oxide includes titanium dioxide (TiO 2 ), tin dioxide (SnO 2 ) and their combinations.
[0033] Also provided is a polymer electrolyte membrane for a fuel cell, which may include the catalyst described herein.
[0034] Further provided is a fuel cell comprising the polymer electrolyte membrane described herein.
[0035] Other aspects and preferred embodiments of the invention are discussed infra. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The above-mentioned and other characteristics of the present invention will be described in detail with reference to certain exemplary embodiments shown in the accompanying drawings, which are given hereinafter only by way of illustration and therefore do not limit the present invention, wherein:
[0037] Figure 1A and Figure 1B The changes in catalyst distribution in a conventional fuel cell during initial use and after long-term use are shown respectively.
[0038] Figure 2 A flow chart is provided to illustrate an exemplary method of preparing an exemplary catalyst provided with an exemplary conductive oxide protection layer according to an exemplary embodiment of the present invention.
[0039] Figure 3 A flow chart is provided to illustrate an exemplary method of preparing an exemplary catalyst provided with an exemplary conductive oxide protection layer according to an exemplary embodiment of the present invention.
[0040] Figure 4 A schematic diagram of an exemplary apparatus for illustrating an exemplary method for preparing a catalyst provided with an exemplary conductive oxide protective layer according to an exemplary embodiment of the present invention.
[0041] Figure 5A and Figure 5B 2 are conceptual diagrams showing changes in a conventional fuel cell and a catalyst composite material according to an exemplary embodiment of the present invention with increase in fuel cell operation time, respectively.
[0042] Figure 6 The transmission electron microscope (TEM) image and energy dispersive X-ray spectroscopy (EDS) image of Example 1 are shown.
[0043] Figure 7 The TEM image and EDS image of Example 2 are shown.
[0044] Figure 8 TEM images and EDS images depending on the change in the cycle number in Example 1 are shown.
[0045] Fig. 9 TEM images and EDS images depending on the change in the cycle number in Example 2 are shown.
[0046] Fig.10 The evaluation results of the catalyst durability depending on the change in the cycle number in Example 1 are shown.
[0047] Fig.11 The evaluation results of the catalyst durability depending on the change in the cycle number in Example 2 are shown. DETAILED DESCRIPTION
[0048] The various exemplary embodiments of the present invention will be described in detail below with reference to the accompanying drawings. The advantages and features of the present invention and the methods for achieving the advantages and features of the present invention will be clearly understood from the preferred embodiments below with reference to the accompanying drawings. However, the present invention is not limited to these embodiments and will be implemented in different forms. The embodiments are only to provide a thorough and complete understanding of the disclosed content and are sufficient to inform those skilled in the art of the technical concept of the present invention. The scope of the present invention is limited only by the claims. In the description of the drawings, the same reference numerals represent the same elements.
[0049] Unless otherwise defined, all terms (including technical or scientific terms) used herein have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. In addition, terms that are the same as those defined in commonly used dictionaries should be interpreted as having the same meaning as the contextual meaning of the prior art, and unless otherwise clearly defined in this specification, should not be interpreted as having an ideal or overly formal meaning.
[0050] In addition, the terms used herein are only used to illustrate the embodiments, and should not be construed as limiting the scope of the present invention. Unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. It should be further understood that when used in this specification, the terms "include", "comprising" etc. represent the presence of the elements, features, numerical values, steps and / or operations, but do not exclude the presence or addition of more than one other elements, features, numerical values, steps and / or operations. In addition, "and / or" includes each of the items mentioned and more than one combination thereof.
[0051] In addition, it should be understood that when an element (e.g., a layer, film, region, or substrate) is referred to as being "on" another element, it can be directly on the other element or intervening elements may also be present. It should also be understood that when an element (e.g., a layer, film, region, or substrate) is referred to as being "under" another element, it can be directly under the other element or intervening elements may also be present.
[0052] Unless otherwise clearly stated in the context, all numbers, values and / or expressions representing the amount of ingredients, reaction conditions, polymer compositions and mixtures used in this specification are approximate values, which reflect the various measurement uncertainties inherent in obtaining these values. For this reason, it should be understood that in all cases, the term "about" should be understood to modify all numbers, values and / or expressions. Unless otherwise stated or obvious from the context, the term "about" used herein is understood to be within the normal tolerance range of this field, such as within an average of 2 standard deviations. "About" can be understood to be within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05% or 0.01% of the value. In addition, unless obvious from the context, all numerical values provided herein should be modified by the term "about".
[0053] In addition, when numerical ranges are disclosed in this specification, unless otherwise defined, these ranges are continuous and include all values from a minimum value to a maximum value, and include the maximum value in each range. In addition, when a range represents an integer, unless otherwise defined, it includes all integers from a minimum value to a maximum value, and includes the maximum value in the range.
[0054] Hereinafter, the present invention will be described in more detail with reference to the accompanying drawings.
[0055] Figure 2 and Figure 3 A flow chart is provided to illustrate an exemplary method of preparing an exemplary catalyst provided with an exemplary conductive oxide protection layer according to an exemplary embodiment of the present invention.
[0056] like Figure 2 As shown, a method for preparing a catalyst provided with a conductive oxide protective layer according to an exemplary embodiment of the present invention may include: preparing a carbon support loaded with a metal catalyst (step S10), and forming a conductive oxide protective layer using atomic layer deposition (ALD) (step S30).
[0057] In addition, reference will be made to Figure 3 Methods of preparing a catalyst provided with a conductive oxide protective layer (particularly including an exemplary atomic layer deposition (ALD) step) are described.
[0058] like Figure 3 As shown, a method for preparing an exemplary catalyst provided with a conductive oxide protective layer according to an exemplary embodiment of the present invention may include: providing (e.g., supplying) a carbon carrier loaded with a metal catalyst to a fluidized bed reactor (step S11) and forming a conductive oxide protective layer using atomic layer deposition (ALD) (steps S31 to S37).
[0059] In particular, atomic layer deposition may include: supplying a conductive oxide precursor to a fluidized bed reactor (step S31), performing a first purge by supplying an inert gas to the fluidized bed reactor (step S33), converting the conductive oxide precursor into a conductive oxide by supplying a reactive gas to the fluidized bed reactor (step S35), and performing a second purge by supplying an inert gas to the fluidized bed reactor (step S37).
[0060] In the step S11 of supplying the carbon support loaded with the metal catalyst to the fluidized bed reactor, the metal catalyst may include platinum (Pt), but the present invention is not limited thereto.
[0061] In particular, in the step S31 of supplying the conductive oxide precursor to the fluidized bed reactor, the conductive oxide precursor can be selected from, for example, tetraisopropoxytitanium (Ti[OCH(CH 3 ) 2 ] 4 , refer to the following formula 1), tin tetrachloride (SnCl 4 , refer to the following formula 2) and combinations thereof.
[0062] Formula 1
[0063]
[0064] Formula 2
[0065]
[0066] In addition, the deposition operation pressure of the conductive oxide precursor may preferably be about 1 Torr to 5 Torr. That is, the deposition pressure may be maintained at about 1 Torr to 5 Torr.
[0067] In addition, the conductive oxide precursor may be supplied to the fluidized bed reactor for about 20 seconds to 100 seconds.
[0068] A first purging step S33 may be performed after the step S31 of supplying the conductive oxide precursor and before the step S35 of supplying the reactive gas. The purging step S33 may include purging an inert gas at a flow rate of about 50 sccm to about 200 sccm. In addition, the inert gas is preferably purged for about 60 seconds to 120 seconds. The purging step S33 may remove unreacted residual free radicals.
[0069] In the step S35 of converting the conductive oxide precursor into the conductive oxide by supplying the reactive gas to the fluidized bed reactor, the reactive gas may include, for example, water (H 2 O), in particular water vapor. In addition, the reactive gas may be supplied to the fluidized bed reactor at a flow rate of about 10 sccm to about 200 sccm.
[0070] The conductive oxide precursor may be converted into a conductive oxide by reaction with a reactive gas, and the conductive oxide may suitably include, for example, titanium dioxide (TiO 2 ), tin dioxide (SnO 2 ) and their combinations.
[0071] On the other hand, after the reactive gas is supplied (step S35), a second purge (step S37) may be performed. The purge step S37 may include purging the inert gas at a flow rate of about 50 sccm to about 200 sccm. In addition, the inert gas may preferably be purged for about 60 seconds to 120 seconds. The purge step S37 can remove unreacted residual free radicals.
[0072] Meanwhile, in the method of manufacturing a catalyst provided with a conductive oxide protective layer according to an exemplary embodiment of the present invention, a series of the above-described atomic layer deposition steps (eg, S31 to S37 ) sequentially performed may be set as one cycle and repeated.
[0073] The cycle may be preferably repeated about 1 to 20 times. At the same time, as the number of cycles increases, the thickness of the formed conductive oxide protective layer increases. For example, when the conductive oxide protective layer comprises titanium dioxide (TiO 2 ), when the above cycle is repeated (preferably about 10 times or more), the improvement effect of catalyst durability is most excellent. In addition, when the conductive oxide protective layer comprises tin dioxide (SnO 2 ), when the above cycle is repeated (preferably about 5 times or more), the effect of improving the catalyst durability is excellent.
[0074] As described above, by using the preparation method of the atomic layer deposition process (ALD-FBR) using a fluidized bed reactor, a conductive oxide protective layer having a structure (e.g., a mesh structure) that does not cover the entire surface of the metal oxide supported on the carbon support can be formed. In addition, the conductive oxide protective layer thus formed can prevent the catalyst particles (e.g., noble metal nanoparticles) from being eluted or agglomerated (coarsened).
[0075] In particular, when a conventional wet method or other vapor deposition method (e.g., PVD or CVD) is used, the desired conductive oxide protective layer may form a layer applied to the entire surface of the catalyst particles, and thus there is a risk of reduced catalyst activity. However, in the preparation method according to an exemplary embodiment of the present invention, the conductive oxide protective layer may be uniformly formed on the catalyst particles, so that the conductive oxide protective layer may have a property of not interfering with the interaction between the catalyst particles and oxygen (O 2 ) or hydrogen (H 2 ) contact structure. Therefore, a fuel cell catalyst that can prevent coarsening while maintaining or improving catalytic activity can be prepared. Therefore, the durability of the fuel cell catalyst can be greatly improved.
[0076] The following will refer to Figure 4 The apparatus shown in the figure describes in detail the method for preparing a catalyst provided with a conductive oxide protective layer. For ease of explanation, the following description will focus on Figures 2 to 3 The difference.
[0077] Figure 4 A schematic diagram illustrating an exemplary apparatus for a method of preparing an exemplary catalyst provided with an exemplary conductive oxide protective layer according to an exemplary embodiment of the present invention.
[0078] like Figure 4 As shown, a fluidized bed reactor for atomic layer deposition (ALD-FBR) used in some embodiments of the present invention may include a fluidized bed reactor 100, a rotary pump (or vacuum pump) 200, a container 300, an inert gas tank 400, and a reactive gas tank 500. The rotary pump 200 is used to control the internal pressure of the fluidized bed reactor 100. The container 300 contains a conductive oxide precursor for introducing the conductive oxide precursor into the fluidized bed reactor 100. The inert gas tank 400 is used to introduce a purge gas into the fluidized bed reactor 100. The reactive gas tank 500 is used to introduce a reactive gas into the fluidized bed reactor 100. Meanwhile, each of the gas tanks 400 and 500 may include a mass flow controller (MFC).
[0079] The fluidized bed reactor 100 can also be used as a chamber for atomic layer deposition (ALD), so vacuum treatment can be first performed using the rotary pump 200, and even in the process, the vacuum strength (e.g., operating pressure) can be kept constant. Therefore, the carbon carrier (which can be loaded with a metal catalyst (e.g., platinum (Pt)) can be introduced into the fluidized bed reactor 100 (see Figure 3 in S11).
[0080] At the same time, the conductive oxide protective layer (e.g., titanium dioxide (TiO 2 ) or tin dioxide (SnO 2 )) of a conductive oxide precursor (e.g., titanium tetraisopropoxide (Ti[OCH(CH 3 ) 2 ] 4 ) or tin tetrachloride (SnCl 4 )) is introduced into the container 300 and connected to the fluidized bed reactor 100 through a pipeline.
[0081] Inert gas (e.g., argon (Ar)) as a purge gas required for atomic layer deposition (ALD) may be prepared in the inert gas tank 400, and reactive gas (e.g., water vapor (H2O)) may be prepared in the reactive gas tank 500. 2 O)), which can be connected to the fluidized bed reactor 100 through each mass flow controller (MFC).
[0082] Meanwhile, as described above, the inert gas tank 400 may be used for purging at a flow rate of about 50 sccm to about 200 sccm (e.g., Figure 3 Preferably, argon (Ar) (inert gas) may be continuously introduced into the fluidized bed reactor 100 from the inert gas tank 400 through a mass flow controller (MFC) at a flow rate of about 80 sccm to about 120 sccm.
[0083] Meanwhile, the fluidized bed reactor 100 may be initially pumped to an internal pressure of about 0.1 Torr to 0.5 Torr (preferably 0.4 Torr). For example, platinum-loaded carbon support (Pt / C) particles may be fed into the fluidized bed reactor 100 and then pumped to the above basic pressure. Specifically, for example, after step S11 of supplying the carbon support loaded with the metal catalyst to the fluidized bed reactor 100 and after supplying the conductive oxide precursor (see Figure 3 Before S31), the method may further include: performing pumping to adjust the internal pressure of the fluidized bed reactor 100 to about 0.1 Torr to 0.5 Torr.
[0084] Meanwhile, the internal reaction temperature of the fluidized bed reactor 100 may be maintained at about 300° C., the temperature of each pipe may be maintained at about 100° C., and the internal temperature of the container 300 may be maintained at room temperature to about 50° C. For example, the internal temperature of the container having the conductive oxide precursor containing titanium (Ti) may be maintained at about 50° C., and the internal temperature of the container having the conductive oxide precursor containing tin (Sn) may be maintained at room temperature.
[0085] In an exemplary embodiment, in the process, an inert gas (e.g., argon (Ar)) contained in the inert gas tank 400 may be introduced into the fluidized bed reactor 100 through a mass flow controller (MFC) at a flow rate of about 100 sccm. Thus, in the furnace of the fluidized bed reactor 100, a carbon support loaded with a metal catalyst (e.g., a carbon support loaded with platinum (Pt / C)) may be fluidized and floated, and a conductive oxide precursor S31 may be fed therein.
[0086] The conductive oxide precursor may be contacted with the catalyst particles to be fixed in the form of dots on the catalyst composite material, which may include a metal catalyst and a carbon support. Argon (Ar) (as a purge gas) may be fed into the fluidized bed reactor 100, and water vapor (H 2 Argon (O) (as a reactive gas) is fed into the fluidized bed reactor 100 so that the conductive oxide adheres to the carbon black of the catalyst composite material in the form of dots, and argon (Ar) may be fed into the fluidized bed reactor 100 again and purged. As described above, purging with argon (Ar) can remove unreacted residual free radicals.
[0087] During the atomic layer deposition, the operating pressure may be maintained at about 1 Torr to 5 Torr, and the flow rate of the gas may be about 50 sccm to 200 sccm for argon (Ar) and about 10 sccm to 200 sccm for water vapor (H2O). 2 In addition, the time range of supplying the conductive oxide precursor (S31) to the fluidized bed reactor 100 may be about 40 seconds to about 100 seconds, the time range of purging argon (Ar) (S33) may be about 60 seconds to about 120 seconds, and the time range of purging water vapor (H2O) may be about 10 seconds to about 20 seconds. 2 O) (e.g. Figure 3 The time range of S35 in the step S31 can be about 40 seconds to about 100 seconds, and the time range of purging argon (Ar) (S37) can be about 60 seconds to about 120 seconds. A unit cycle including S31, S33, S35 and S37 can be repeated several times.
[0088] Figure 5A and Figure 5B2 are conceptual diagrams showing changes in a conventional fuel cell and a catalyst composite material according to an exemplary embodiment of the present invention with increase in fuel cell operation time, respectively.
[0089] like Figure 5A As shown, in a conventional fuel cell, the catalyst composite material may include a carbon support 10 and catalyst particles 20 supported on the carbon support 10. In the conventional catalyst composite material, as the operation time increases, adjacent metal catalyst particles 20 may agglomerate (in other words, coarsen). For example, as Ostwald ripening occurs between the metal catalyst particles 20, the size of the metal catalyst particles 20 increases. Therefore, unlike the initial operation stage, during the fuel cell reaction, the metal catalyst particles 20 and hydrogen (H 2 ) or oxygen (O 2 ) is reduced, so the catalytic activity decreases.
[0090] On the other hand, the above method (see Figure 2 or Figure 3 ) prepares the catalyst composite material according to an exemplary embodiment of the present invention, and thus the conductive oxide protective layer 30 may also be formed.
[0091] In addition, if Figure 5B As shown, the catalyst composite material may be formed on a carbon carrier 10, metal catalyst particles 20 supported on the carbon carrier 10, and the surface of the metal catalyst particles 20, and may include a conductive oxide protective layer 30 having a mesh structure. For example, the metal catalyst particles 20 may include platinum (Pt).
[0092] The mechanism of forming the conductive oxide protective layer 30 by atomic layer deposition (ALD) will be described. When the conductive oxide precursor is introduced onto the carbon support 10 loaded with the metal catalyst particles 20, the conductive oxide precursor may be adsorbed on the metal catalyst particles (particularly the noble metal particles) 20 having a higher surface energy than the surface energy of the carbon support 10. Therefore, the conductive oxide precursor may be more adsorbed on the surface of the metal catalyst particles 20 than on the surface of the carbon support 10 (see Figure 3 S31 in ).
[0093] Furthermore, when contacted with a reactive gas, the conductive oxide precursor may be converted into a conductive oxide protective layer 30 (eg, Figure 3 S35 in, the conductive oxide is selected from titanium dioxide (TiO 2 ), tin dioxide (SnO 2 ) and combinations thereof. In particular, conductive oxides such as titanium dioxide (TiO 2 ) or tin dioxide (SnO2 ). In the initial stage, the conductive oxide may be deposited in the form of dots, which may gradually grow and contact with adjacent conductive oxide dots to form a mesh structure. Then, the mesh structure may gradually grow to form a layer, thereby producing a conductive oxide protective layer 30.
[0094] Since the surface energy of the metal catalyst particles 20 is greater than the surface energy of the carbon carrier 10, Figure 5B As shown, a conductive oxide network structure may be first formed on the surface of the metal catalyst particles 20, and then the conductive oxide may exist in the form of nano-sized dots on the carbon support 10. The conductive oxide protective layer 30 having a network structure thus formed may prevent the nano-sized metal catalyst particles 20 from agglomerating (coarsening).
[0095] According to various exemplary embodiments of the present invention, by using an atomic layer deposition process, a conductive oxide protective layer 30 having a mesh structure that does not completely cover the metal catalyst particles 20 can be uniformly formed. In this way, the conductive oxide protective layer 30 can be formed without interfering with the interaction between the catalyst particles and oxygen (O 2 ) or hydrogen (H 2 ) between the catalyst particles, thereby maintaining and improving the catalytic activity and improving the durability despite the use of the fuel cell.
[0096] Preferably, the thickness of the conductive oxide protective layer 30 may be about 0.05 nm to 10 nm. In particular, when the thickness of the conductive oxide protective layer 30 is about 10 nm or less, the durability is improved most effectively while maintaining the catalytic activity.
[0097] Example
[0098] The present invention will be described in more detail below with reference to specific examples and comparative examples. However, the following examples are provided only to illustrate the present invention and should not be construed as limiting the scope of the present invention.
[0099] Example 1: Titanium dioxide (TiO 2 ) conductive oxide protective layer
[0100] An atomic layer deposition process using a fluidized bed reactor (ALD-FBR) was performed as follows to prepare a catalyst composite material in which platinum (Pt) nanoparticles (as a metal catalyst) were supported on a carbon support: At this time, the operating pressure was maintained at 1 Torr to 5 Torr.
[0101] (1) Platinum-loaded carbon support (Pt / C) particles were fed into a fluidized bed reactor and pumped so that the base pressure of the fluidized bed reactor was 0.4 Torr. At this time, the internal temperature of the fluidized bed reactor was maintained at 300° C., and the temperature of the pipe was maintained at about 100° C.
[0102] (2) The internal temperature of the inert gas tank containing the Ti precursor was maintained at 50° C., and the Ti precursor was injected from the inert gas tank into the fluidized bed reactor for 40 to 100 seconds.
[0103] (3) Argon (Ar) was purged from the inert gas tank at a flow rate of 100 sccm for 60 to 120 seconds through a mass flow controller (MFC). At this time, the platinum-loaded carbon support (Pt / C) in the fluidized bed reactor was fluidized and floated.
[0104] (4) Water vapor (H) was added at flow rates of 10 sccm and 200 sccm. 2 O) is injected into the fluidized bed reactor for 40 to 100 seconds. 2 ) were fixed to a platinum-loaded carbon support (Pt / C) in the form of dots.
[0105] (5) Again, argon (Ar) gas is injected into the fluidized bed reactor at a flow rate of 50 to 200 sccm for 60 to 120 seconds for purging to remove unreacted residual radicals.
[0106] The series of processes from (2) to (5) above is set as one cycle, and the cycle is repeated once (TiO 2 1-Pt 1), tertiary (TiO 2 3-Pt 15), five times (TiO 2 5-Pt 15) and ten times (TiO 2 10-Pt 15).
[0107] Example 2: Containing tin dioxide (SnO 2 ) conductive oxide protective layer
[0108] An atomic layer deposition process using a fluidized bed reactor (ALD-FBR) was performed as follows to prepare a catalyst composite material in which platinum (Pt) nanoparticles (as a metal catalyst) were supported on a carbon support: At this time, the operating pressure was maintained at 1 Torr to 5 Torr.
[0109] (1) Platinum-loaded carbon support (Pt / C) particles were fed into a fluidized bed reactor and pumped so that the base pressure of the fluidized bed reactor was 0.4 Torr. At this time, the internal temperature of the fluidized bed reactor was maintained at 300° C., and the temperature of the pipe was maintained at 100° C.
[0110] (2) The internal temperature of the inert gas tank containing the Sn precursor is maintained at room temperature, and the Sn precursor is injected from the inert gas tank into the fluidized bed reactor for 20 seconds to 80 seconds.
[0111] (3) Argon (Ar) was purged from the inert gas tank at a flow rate of 100 sccm for 60 to 120 seconds through a mass flow controller (MFC). At this time, the platinum-loaded carbon support (Pt / C) in the fluidized bed reactor was fluidized and floated.
[0112] (4) Water vapor (H) was added at flow rates of 10 sccm and 200 sccm. 2 O) is injected into the fluidized bed reactor for 40 to 100 seconds. 2 ) were fixed to a platinum-loaded carbon support (Pt / C) in the form of dots.
[0113] (5) Again, argon (Ar) gas is injected into the fluidized bed reactor at a flow rate of 50 to 200 sccm for 60 to 120 seconds for purging to remove unreacted residual radicals.
[0114] The series of processes from (2) to (5) above is set as one cycle, and the cycle is repeated once (SnO 2 1-Pt 1), tertiary (SnO 2 3-Pt 15), five times (SnO 2 5-Pt 15) and ten times (SnO 2 10-Pt 15).
[0115] Evaluation Example 1: Deposition rate per cycle [ / cycle]
[0116] It was observed that titanium dioxide (TiO 2 The deposition rate per cycle of ) (used as the conductive oxide in Example 1) is / cycle. It was observed that tin dioxide (SnO 2 The deposition rate of ) (used as the conductive oxide in Example 2) is / cycle.
[0117] Evaluation Example 2: Transmission electron microscope (TEM) image analysis of a catalyst provided with a conductive oxide protective layer Analysis and Energy Dispersive X-ray Spectroscopy (EDS) Image Analysis
[0118] Figure 6 The TEM image and EDS image of Example 1 are shown. Figure 7 The TEM image and EDS image of Example 2 are shown.
[0119] like Figure 6 and Figure 7 As shown, due to the high surface energy of platinum (Pt), titanium dioxide (TiO 2 ) and tin dioxide (SnO 2 ) (respectively as conductive oxides) are deposited particularly uniformly on the platinum (Pt) catalyst.
[0120] Evaluation Example 3: Analysis of TEM images and energy dispersive X-ray spectroscopy (EDS) images depending on the number of cycles
[0121] The following will refer to Figure 8 and Fig. 9 TEM images and EDS images depending on the cycle number in Examples 1 and 2 are described.
[0122] like Figure 8 As shown, it can be seen that in Example 1, titanium dioxide (TiO 2 ) increases with the increase of the number of ALD cycles. In addition, it can be seen that with the increase of the number of ALD cycles, the loading rate of titanium dioxide (TiO 2 )The thickness of the protective layer increases.
[0123] like Fig. 9 As shown in Example 1, it can be seen that with the increase of the number of cycles, the SnO 2 ) loading rate increases, SnO 2 )The thickness of the protective layer increases.
[0124] Evaluation Example 4: Evaluation of catalyst durability depending on the number of cycles
[0125] Fig.10 and Fig.11 The evaluation results of the catalyst durability depending on the number of cycles in Examples 1 and 2 are shown, respectively.
[0126] like Fig.10 As shown, with the increase of titanium dioxide (TiO 2 ) of the atomic layer deposition (ALD) cycles, the Q H The titanium dioxide (TiO) that is most suitable for improving the durability of fuel cell catalysts (i.e., catalyst composites) is determined by the 2 ) deposition rate. It can be seen that with the increase of the number of atomic layer deposition (ALD) cycles, the TiO 2 The thickness of the protective layer increases. In particular, it is found that after 10 cycles (see TiO 2 10-Pt 15) has the best durability.
[0127] On the other hand, in the absence of titanium dioxide (TiO 2 ) protective layer catalyst (Pt 15), it can be seen that with the increase of CV cycles, Q H This proves that when the number of cycles is less than 10, titanium dioxide (TiO 2) protective layer, is not enough to form a mesh structure, and cannot effectively prevent the agglomeration of catalyst particles during fuel cell operation. However, when the cycle number is about 10, it can be seen that the titanium dioxide (TiO 2 )'s mesh structure is firmly formed into a network structure and improves the durability of the catalyst and the fuel cell.
[0128] In addition, if Fig.11 As shown, with the tin dioxide (SnO 2 ) of atomic layer deposition (ALD) cycles, the Q H Variations to determine the most suitable tin dioxide (SnO) for improving the durability of fuel cell catalysts (i.e., catalyst composites) 2 ) deposition rate. It can be seen that with the increase of the number of atomic layer deposition (ALD) cycles, SnO 2 The thickness of the protective layer increases. In particular, it is found that after 5 cycles (see SnO 2 5-Pt 15) has the best durability.
[0129] When the catalyst does not have tin dioxide (SnO 2 ) protection layer, it can be seen that with the increase of CV cycles, Q H This proves that when the number of cycles is less than 5, tin dioxide (SnO 2 ) protective layer, is not enough to form a mesh structure, and cannot effectively prevent the agglomeration of catalyst particles that occurs during fuel cell operation. However, when the cycle number is about 5, it can be seen that the tin dioxide (SnO 2 )'s mesh structure is firmly formed into a network structure and improves the durability of the catalyst and the fuel cell.
[0130] In conclusion, according to the preparation method using atomic layer deposition (ALD-FBR) using a fluidized bed reactor and the nanoparticle catalyst prepared thereby according to various exemplary embodiments of the present invention, a conductive oxide protective layer as a protective film having a mesh structure can be formed, thereby preventing the agglomeration of nano-sized catalyst particles without reducing the catalytic active surface area, thereby maintaining the performance of the fuel cell and improving the durability of the fuel cell. The reason for this is that, as described above, unlike the protective layer as a layer applied to the entire surface of the catalyst particles when a wet method or other vapor deposition method (such as PVD or CVD) is performed, a protective layer having a mesh structure (i.e., a conductive oxide protective layer) can be formed by deposition at the atomic level, thereby maintaining and improving the catalytic activity while preventing the coarsening of the catalyst particles.
[0131] According to the method of preparing a catalyst provided with a conductive oxide protective layer according to various exemplary embodiments of the present invention, a conductive oxide protective layer may be uniformly formed on a catalyst and a support having a large surface area using atomic layer deposition (ALD).
[0132] For example, by controlling the conductive oxide on an atomic basis, a conductive oxide protective layer having a mesh structure that does not cover the entire surface of the catalyst particles can be formed. Thus, the coarsening of the catalyst particles can be effectively prevented without interfering with the interaction of the catalyst particles with oxygen (O 2 ) or hydrogen (H 2 ) contact.
[0133] Furthermore, since coarsening of catalyst particles can be suppressed, catalytic activity can be maintained or improved, and thus the durability of the fuel cell can be greatly improved.
[0134] Other effects of the present invention are not limited to the above-mentioned effects. The present invention should be understood to include all the effects that can be inferred from the above description.
[0135] The present invention has been described in detail with reference to exemplary embodiments thereof. However, it will be appreciated by those skilled in the art that these embodiments may be modified without departing from the principles and spirit of the present invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a catalyst comprising a conductive oxide protective layer, the method comprising: include: providing a carbon support loaded with a metal catalyst to a fluidized bed reactor; as well as Atomic layer deposition is used to form a conductive oxide protective layer. Wherein, the atomic layer deposition comprises: supplying a conductive oxide precursor to a fluidized bed reactor; A first purge is performed by supplying an inert gas to the fluidized bed reactor; Converting a conductive oxide precursor into a conductive oxide by supplying a reactive gas to the fluidized bed reactor; and By supplying an inert gas to the fluidized bed reactor for a second purge, During the first purge, the carbon support including the metal catalyst floats up.
2. The method according to claim 1, in, The metal catalyst includes platinum. 3 . The method according to claim 1 , further comprising adjusting an internal pressure of the fluidized bed reactor to 0.1 Torr to 0.5 Torr after providing the carbon support to the fluidized bed reactor and before forming the conductive oxide protective layer.
4. The method according to claim 1, in, In supplying the conductive oxide precursor to the fluidized bed reactor, the conductive oxide precursor includes titanium tetraisopropoxide, tin tetrachloride, and a combination thereof.
5. The method according to claim 1, in, In supplying the conductive oxide precursor to the fluidized bed reactor, a deposition operation pressure of the conductive oxide precursor is 1 Torr to 5 Torr.
6. The method according to claim 1, in, In supplying the conductive oxide precursor to the fluidized bed reactor, the conductive oxide precursor is supplied to the fluidized bed reactor for 20 seconds to 100 seconds.
7. The method according to claim 1, in, In converting the conductive oxide precursor into the conductive oxide, the reactive gas includes water vapor.
8. The method according to claim 1, in, In converting the conductive oxide precursor into the conductive oxide, a reactive gas is supplied to the fluidized bed reactor at a flow rate of 10 to 200 sccm.
9. The method according to claim 1, in, In converting the conductive oxide precursor into the conductive oxide, the conductive oxide includes titanium dioxide, tin dioxide, and combinations thereof.
10. The method according to claim 1, in, During the purge, the inert gas is purged at a flow rate of 50 sccm to 200 sccm.
11. The method according to claim 1, in, During the purging, the inert gas is purged for 60 seconds to 120 seconds.
12. The method according to claim 1, in, The atomic layer deposition is repeated.
13. The method according to claim 12, in, The atomic layer deposition was repeated 1 to 20 times.
14. A catalyst comprising a conductive oxide protective layer prepared by the method according to claim 1, wherein the catalyst include: Carbon support; Metal catalyst particles supported on a carbon support; as well as a conductive oxide protective layer formed on the surface of the metal catalyst particles and having a mesh structure, Compared with the surface of the carbon carrier, the conductive oxide precursor is more adsorbed on the surface of the metal catalyst particles, so a network structure is formed on the surface of the metal catalyst particles, and the conductive oxide exists on the carbon carrier in the form of dots.
15. The catalyst according to claim 14, in, The thickness of the conductive oxide protective layer is 0.05 nm to 10 nm.
16. The catalyst according to claim 14, in, The metal catalyst particles include platinum.
17. The catalyst according to claim 14, in, The conductive oxide protection layer includes a conductive oxide, and the conductive oxide includes titanium dioxide, tin dioxide or a combination thereof.
18. A polymer electrolyte membrane for a fuel cell, comprising the catalyst according to claim 14.
19. A fuel cell comprising the polymer electrolyte membrane for a fuel cell according to claim 18.
Citation Information
Patent Citations
Fluidized bed atomic layer deposition device for manufacturing nanocoating particles
US20160258059A1