Crystalline silicon wafer corrosion rate test method
By using a combination of rolling conveyor device and electronic balance in the silicon wafer corrosion rate test, the corrosion depth and rate of the silicon wafer are calculated, and the problems of large operating errors and poor accuracy in the prior art are solved, achieving more efficient and accurate Test results.
Patent Information
- Application Number
- CN202010744349.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-07-29
AI Technical Summary
The existing silicon wafer corrosion rate testing methods have problems such as large operating errors, poor calculation accuracy, cumbersome operation and silicon wafer damage.
The rolling conveyor device is used to transfer silicon wafers in the cleaning tank, and combined with the weighing method of electronic balances, the corrosion depth and corrosion rate of the silicon wafer are calculated through formulas, reducing the complexity of human operations and improving the accuracy of the test data.
Simplifies the operation process, reduces errors, improves the accuracy and working efficiency of test data, and avoids silicon wafer damage.
Smart Images

Figure CN112038247B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon wafers, and more specifically, relates to a method for testing the corrosion rate of a crystal silicon wafer. Background Art
[0002] At present, there are more than 500 domestic companies engaged in the photovoltaic industry, with about 300,000 employees, and the production capacity of solar cells accounts for 51% of the world's total production capacity. Whether it is production or scientific research on high-efficiency batteries, the etching and corrosion depth of solar cells must be tested to observe the stability of product quality. The photovoltaic industry uses solar energy as an emerging energy source for clean production, which has attracted global attention. Improving battery conversion efficiency has become the focus of scientific research; the optimal corrosion depth of solar cells directly affects the efficiency of the battery.
[0003] The current silicon wafer rate test method is to use a fixed small water tank without a conveying device. After the chemical solvent is placed in the water tank and the ratio is good, the operator uses a clamp to put the silicon wafer to be tested into the water tank, and uses a stopwatch to record the time. After the time is up, the silicon wafer is clamped out and weighed to calculate the weight difference before and after. This operation is repeated after the chemical reagent is replaced in the water tank. There is no standardized corrosion rate test method.
[0004] According to the current silicon wafer corrosion rate test method, there are disadvantages in the process of manually taking and placing silicon wafers multiple times: 1. It requires special personnel to operate, and the operation time is long. 2. The operation error is large, which is easy to cause damage to the test sample. 3. The operation is cumbersome and the calculation accuracy is poor. Summary of the invention
[0005] The purpose of the present invention is to provide a method for testing the corrosion rate of a crystalline silicon wafer, aiming to solve the problems of large operation errors and poor calculation accuracy in the existing corrosion rate test.
[0006] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for testing the corrosion rate of a crystalline silicon wafer, comprising:
[0007] Weigh the silicon wafer to be corroded, and record the weight W1 of the silicon wafer before corrosion;
[0008] Put the silicon wafer on the rolling conveyor in the cleaning tank and immerse the silicon wafer completely in the chemical solution in the cleaning tank, set the conveying time and conveying speed of the rolling conveyor in the cleaning tank, and clean and corrode the silicon wafer;
[0009] Take out the corroded silicon wafer and weigh it, and record the weight of the corroded silicon wafer W2;
[0010] The corrosion depth Δh of the silicon wafer is calculated by the corrosion depth formula (1):
[0011]
[0012] According to formula (2) and formula (1), formula (3) is obtained, and the silicon wafer corrosion rate ν is calculated by formula (3):
[0013] Δh=ν×T (2)
[0014]
[0015] Where:
[0016] Δh—Corrosion depth of silicon wafer after etching, unit: μm
[0017] ν—Corrosion rate, unit: μm / s
[0018] W1—weight of sample silicon wafer before corrosion, unit: g
[0019] W2—The weight of the impurities removed after silicon wafer etching, in g
[0020] S—area of the two etched surfaces of the silicon wafer, in cm 2
[0021] T—corrosion time, unit: s
[0022] ρ—Silicon density, unit: g / cm 3
[0023] Repeat the above steps and calculate the average silicon wafer corrosion rate according to formula (4):
[0024]
[0025] (4) Where:
[0026] ν—average value of corrosion rate, μm / s;
[0027] ν n —Corrosion rate of a single sample, μm / s;
[0028] n—positive integer.
[0029] As another embodiment of the present application, when cleaning in the cleaning tank, the silicon wafer passes through the alkaline cleaning tank, the rinsing tank, the pickling tank and the rinsing tank in sequence along with the rolling conveyor device, the concentration of NaOH in the alkaline cleaning tank is 3-10g / L; the concentration of HF acid in the pickling tank is 3-10g / L; the conveying speed of the rolling conveyor device is greater than or equal to 1.0m / min.
[0030] As another embodiment of the present application, the weighing is performed using an electronic balance, and the electronic balance is provided with a bracket for fixing the silicon wafer.
[0031] As another embodiment of the present application, the bracket includes a chassis placed on the electronic balance and a backing plate arranged on the chassis, and a slot for positioning the silicon wafer is provided at the intersection of the backing plate and the chassis.
[0032] As another embodiment of the present application, the backing plate is an arc-shaped plate, and two vertical edges of the arc-shaped plate have an inclination for the silicon wafer to lean against.
[0033] As another embodiment of the present application, the area of the orthographic projection of the arc plate on the chassis is greater than half of the area of the chassis.
[0034] As another embodiment of the present application, the lower surface of the chassis is provided with an annular groove for clamping with the tray of the electronic balance.
[0035] As another embodiment of the present application, the chassis has support edges extending upward on all sides, and the card slot is arranged at the intersection of the back plate and the support edge.
[0036] As another embodiment of the present application, the card slot is a V-shaped groove.
[0037] As another embodiment of the present application, the bracket is a plastic product or a rubber product.
[0038] The beneficial effect of the crystalline silicon wafer corrosion rate testing method provided by the present invention is that: compared with the prior art, the crystalline silicon wafer corrosion rate testing method of the present invention uses a rolling conveyor device to convey silicon wafers in a cleaning tank, which reduces the complexity of manual operation, avoids the possibility of damage to the silicon wafer, reduces the error caused by manual operation, and improves the accuracy of test data. The test method is simple to operate, convenient and reliable, which not only improves the accuracy of test data, but also improves the work efficiency of the test. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 A process flow chart of a method for testing the corrosion rate of a crystalline silicon wafer provided in an embodiment of the present invention;
[0041] Figure 2 A schematic diagram of the structure of a crystalline silicon wafer rolling conveyor provided in an embodiment of the present invention;
[0042] Figure 3 A schematic diagram of the three-dimensional structure of a crystalline silicon wafer weighing bracket provided in an embodiment of the present invention;
[0043] Figure 4 for Figure 3 The cross-sectional structure of the crystalline silicon weighing bracket shown Figure 1 ;
[0044] Figure 5 for Figure 4 A schematic diagram of the local enlarged structure at point A in the middle;
[0045] Figure 6 for Figure 3 The cross-sectional structure of the crystalline silicon weighing bracket shown Figure 2 .
[0046] In the figure: 1. back plate; 2. card slot; 3. support edge; 4. chassis; 5. silicon wafer; 6. rolling conveyor; 7. annular groove. DETAILED DESCRIPTION
[0047] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0048] Please also read Figure 1 and Figure 2 The crystalline silicon wafer corrosion rate testing method provided by the present invention is now described. The crystalline silicon wafer corrosion rate testing method comprises:
[0049] Step 1, weigh the silicon wafer before corrosion, and record the weight W1 of the silicon wafer before corrosion;
[0050] Step 2: Place the silicon wafer on the rolling conveyor 6 in the cleaning tank and completely immerse the silicon wafer in the chemical solution in the cleaning tank, set the conveying time and conveying speed of the rolling conveyor in the cleaning tank, and clean and corrode the silicon wafer;
[0051] Step 3, taking out the corroded silicon wafer and weighing it, and recording the weight W2 of the corroded silicon wafer;
[0052] Step 4: Calculate the silicon wafer corrosion depth Δh using the corrosion depth formula (1):
[0053]
[0054] According to formula (2) and formula (1), formula (3) is obtained, and the silicon wafer corrosion rate ν is calculated by formula (3):
[0055] Δh=ν×T (2)
[0056]
[0057] Where:
[0058] Δh—Corrosion depth of silicon wafer after etching, unit: μm
[0059] ν—Corrosion rate, unit: μm / s
[0060] W1—weight of sample silicon wafer before corrosion, unit: g
[0061] W2—The weight of the impurities removed after silicon wafer etching, in g
[0062] S—area of the two etched surfaces of the silicon wafer, in cm 2
[0063] T—corrosion time, unit: s
[0064] ρ—Silicon density, unit: g / cm 3
[0065] Step 5: Repeat steps 1 to 4 and calculate the average silicon wafer corrosion rate according to formula (4):
[0066]
[0067] (4) Where:
[0068] ν—average value of corrosion rate, μm / s;
[0069] ν n —Corrosion rate of a single sample, μm / s;
[0070] n—positive integer.
[0071] Compared with the prior art, the crystalline silicon wafer corrosion rate test method provided by the present invention uses a rolling conveyor 6 to convey silicon wafers in a cleaning tank, which reduces the complexity of manual operation, avoids the possibility of damage to the silicon wafer, reduces the error caused by manual operation, and improves the accuracy of test data. The test method is simple to operate, convenient and reliable, and not only improves the accuracy of test data, but also improves the work efficiency of the test.
[0072] The principle of the testing method provided by the present invention is to obtain the mass difference before and after corrosion of the solar cell by weighing, and calculate the corrosion depth by using the formula that density equals mass divided by volume and the relationship that volume equals length times width times height.
[0073] Among them, there are multiple cleaning tanks arranged in parallel, each of which is filled with different chemical solutions, which can clean and corrode the silicon wafers. The solutions are transmitted through the rolling conveyor 6, which greatly reduces the errors in test data caused by human factors and the problem of easy damage to silicon wafers, and at the same time reduces the tediousness and labor intensity of the operation.
[0074] Specifically, when cleaning in the cleaning tank, the silicon wafer passes through the alkaline cleaning tank, the rinsing tank, the acid cleaning tank and the rinsing tank in sequence along with the rolling conveyor device. The concentration of NaOH in the alkaline cleaning tank is 3-10g / L; the concentration of HF acid in the acid cleaning tank is 3-10g / L; the conveying speed of the rolling conveyor device is greater than or equal to 1.0m / min.
[0075] The rolling conveying device 6 can adopt the existing technology, and the improvement is that a plastic tube is sleeved on the roller to prevent the silicon wafer from being damaged.
[0076] The test environment temperature is 25℃±2℃; it is carried out in a Class 10,000 clean room to prevent the silicon wafer from being disturbed by the external environment and affecting the accuracy of the test data.
[0077] In this embodiment, 3 silicon wafers are selected as test samples, that is, n=3. Selecting 3 samples can achieve better results without wasting resources, based on the following demonstration data:
[0078] When the number of silicon wafers to be corroded is different, the corrosion values of different silicon wafers will have deviations. In order to observe the corrosion values of silicon wafers as a whole, the present invention adopts a three-sample corrosion method for testing. The upper deviation of the corrosion rate is 1.52m / min, and the lower deviation is 1.2m / min. Through the following time comparison, one sample corrosion method, three sample corrosion method and five sample corrosion method; one sample reflects a single value and cannot cover the entire batch; three samples and five samples are within the standard deviation of 0.32m / min, and can cover the entire batch. Because five samples require a long time, a large number, and a cumbersome process; so the three-sample solution is selected as the method included in the present invention. In this way, the sample test data is less than the allowable error range, which not only covers the corrosion depth and rate test data of the entire batch of silicon wafers, but also reduces the test time and the number of tests. The experimental data are shown in Table 1, Table 2, and Table 3:
[0079] Table 1 Corrosion test data of a sample
[0080]
[0081] Table 2 Corrosion test data of three samples
[0082]
[0083] Table 3 Corrosion test data of five samples
[0084]
[0085] From the above three tables, it can be seen that the three-piece sample and the five-piece sample are both within the standard deviation of 0.32m / min, and can cover the entire batch, while the five-piece sample requires a long time, a large number, and a cumbersome process; so the three-piece sample solution is selected as the method included in the present invention. In this way, the sample test data is less than the allowable error range, which not only covers the corrosion depth and rate test data of the entire batch of silicon wafers, but also reduces the test time and the number of tests, which is economical and applicable.
[0086] The main tests or analyses of the present invention are as follows:
[0087] The average value of three samples was taken, and after multiple tests, the following test verification scheme was determined:
[0088] The repeatability of the test method of the present invention was verified: the same operator, under the same conditions, repeated the corrosion test three times on the same sample, each time performing the operation and calculation according to the steps of the present invention and recording the values; the standard deviation was 0.0653 m / min, and the relative standard deviation was 4.8%, which was less than the standard allowable error range of 0.32 m / min, meeting the requirements of the standard analysis. The test data are shown in Table 4:
[0089] Table 4 Repeatability test data
[0090]
[0091] Table 5. Data of joint comparative tests by multiple companies
[0092] The following data are experimental verification data of this method by different personnel and different factories. The feasibility and effectiveness of this method are illustrated through joint comparison.
[0093]
[0094] As a specific implementation method of the crystalline silicon wafer corrosion rate test method provided by the present invention, please refer to Figures 3 to 6 The weighing is done by using an electronic balance. The technical parameters of the selected electronic balance are: range 220 grams, readability 0.0001, repeatability 0.0001, and allowable error ±0.0002. The electronic balance has a metrological certificate from a third-party authority, and the balance is zeroed and calibrated before use.
[0095] As a specific implementation of the embodiment of the present invention, please refer to Figures 3 to 6 The electronic balance is provided with a bracket for fixing the silicon wafer. By placing the silicon wafer on the bracket, the silicon wafer is prevented from being damaged, and the surface of the silicon wafer is prevented from being directly in contact with the tray of the electronic balance and being contaminated, which affects the accuracy of weighing.
[0096] As a specific implementation of the embodiment of the present invention, refer to Figures 3 to 6The bracket includes a chassis 4 placed on the electronic balance and a backing plate 1 arranged on the chassis 4. A slot 2 for positioning the silicon wafer is arranged at the intersection of the backing plate 1 and the chassis 4. When weighing, the bottom of the silicon wafer is placed in the slot 2 and the silicon wafer is placed on the backing plate 1. The slot 2 can position the silicon wafer and prevent the sample battery from being damaged. A 1mm wide plane is made at the bottom of the slot 2 to improve the stability of the silicon wafer support.
[0097] The chassis 4 can be square or circular. When the chassis 4 is circular, the backing plate 1 is an arc-shaped plate. When the chassis 4 is square, the cross section of the backing plate 1 is a rectangular structure. The shape of the chassis 4 is consistent with the shape of the tray of the electronic balance.
[0098] As a specific implementation of the embodiment of the present invention, please refer to Figures 3 to 6 The support plate 1 is an arc-shaped plate, and the two vertical edges of the arc-shaped plate have an inclination for the silicon wafer to support. The two vertical edges for supporting the silicon wafer are inclined to improve the stability of the silicon wafer support.
[0099] As a specific implementation of the embodiment of the present invention, please refer to Figures 3 to 6 , the area of the positive projection of the arc plate on the chassis 4 is greater than half of the area of the chassis 4. The main thing here is that the surface area surrounded by the bottom of the arc plate is greater than half of the area of the chassis 4, which can provide a reliable support for the silicon wafer.
[0100] As a specific implementation of the embodiment of the present invention, please refer to Figure 6 The lower surface of the chassis 4 is provided with an annular groove 7 which is clamped with the tray of the electronic balance. When weighing, the annular groove 7 is clamped on the tray to fix the position of the bracket to avoid the problem of the silicon wafer slipping due to the instability of the bracket and inaccurate weighing.
[0101] As a specific implementation of the embodiment of the present invention, please refer to Figures 3 to 6 The chassis 4 has support edges 3 extending upwards around it, and the card slot 2 is arranged at the intersection of the support plate 1 and the support edge 3. The silicon wafer is supported by the support edge 3, the contact area between the silicon wafer and the chassis 4 is reduced, and interference with the silicon wafer is avoided.
[0102] As a specific implementation of the embodiment of the present invention, please refer to Figures 3 to 6 The card slot 2 is a V-shaped groove. A plane is provided at the bottom of the V-shaped groove, so that the silicon wafer can be placed stably in the card slot 2.
[0103] As a specific implementation of the embodiment of the present invention, the bracket is a plastic product or a rubber product.
[0104] This embodiment takes three silicon wafers as an example, and the silicon wafer corrosion rate test steps are as follows:
[0105] Step 1: Select 3 samples from the same batch of silicon wafers and place them separately;
[0106] Step 2: Place a clean sample into the calibrated balance and weigh it, and record the data W1;
[0107] Step 3, dry the corroded sample, weigh it with an electronic balance, and record the number;
[0108] Step 4: Calculate the mass difference before and after corrosion using formula (5) and record the data ΔW;
[0109] ΔW=W1-W2 (5)
[0110] Where:
[0111] ΔW—Mass difference before and after corrosion, unit: g
[0112] W1—sample original weight, unit: g
[0113] W2—weight of sample corroded and surface debris removed, unit: g
[0114] Step 5: Calculate the corrosion depth of the sample using formula (1).
[0115] Step 6: Record the corrosion time during the corrosion process.
[0116] Step 7: Use formula (2) and formula (3) to calculate the corrosion rate of the sample and make a record.
[0117] Test the remaining two samples using the above steps and record the values. Take the average value of the three samples.
[0118] Step 8: The corrosion rate of the sample is calculated according to formula (4):
[0119]
[0120] Where:
[0121] ν—average value of corrosion rate, μm / s;
[0122] ν n —Corrosion rate of a single sample, μm / s;
[0123] n—3.
[0124] The silicon wafer corrosion rate test method provided by the present invention is carried out in the silicon wafer corrosion process. The silicon wafer corrosion method can be used in multiple processes in the battery manufacturing process, such as the texturing process and the wet etching process. Introduction The application of this method in the wet etching process, the rolling conveyor device of the present invention plays an indispensable role in the application.
[0125] The wet etching process flow is:
[0126] Loading - etching - rinsing - alkaline washing tank - rinsing tank - pickling tank - rinsing tank - air drying - unloading.
[0127] The role of etching: remove edge PN junction, remove edges, and prevent battery short circuit.
[0128] Each step in the process works by chemical reaction to etch silicon, and the reaction system is very complex. Here are some of the reaction equations:
[0129] (1)Si+2HNO3+6HF=H2SiF6+2HNO2+2H2O
[0130] (2)3Si+4HNO3+18HF=3H2SiF6+4NO+8H2O
[0131] (3)3Si+2HNO3+18HF=3H2SiF6+2NO+4H2O+3H2
[0132] (4)5Si+6HNO3+30HF=5H2SiF6+2NO2+4NO+10H2O+3H2
[0133] Although complex, the etching reaction can be divided into two steps:
[0134] The first step: nitric acid / nitrous acid (HNO2) oxidizes silicon into silicon dioxide (mainly nitrous acid oxidizes silicon).
[0135] Silicon dioxide reacts with hydrofluoric acid (fast reaction) to generate silicon tetrafluoride and water (fast reaction), and silicon tetrafluoride reacts with water to generate fluorosilicic acid and enters the solution.
[0136] Sulfuric acid does not participate in the reaction, but only increases the hydrogen ion concentration, accelerates the reaction, and increases the solution viscosity (increases the interfacial tension between the solution and the PSG thin layer) and the solution density.
[0137] Triggering of the chain: Nitric acid oxidizes silicon to silicon dioxide, which produces nitrogen dioxide or nitric oxide.
[0138] Si+4HNO3=SiO2+4NO2+2H2O (slow reaction)
[0139] Si+2HNO3=SiO2+2NO+2H2O (slow reaction)
[0140] Chain extension: Nitrogen dioxide and nitric oxide react with water to form nitrous acid, which quickly oxidizes silicon into silicon dioxide.
[0141] 2NO2+H2O=HNO2+HNO3(fast reaction)
[0142] Si+4HNO2=SiO2+4NO+2H2O (fast reaction) (main reaction of the first step)
[0143] 4HNO3+NO+H2O=6HNO2(fast reaction)
[0144] As long as a small amount of nitrogen dioxide is generated, it will react with water to become nitrous acid. As long as a small amount of nitric oxide is generated, it will quickly react with nitric acid and water to form nitrous acid. Nitrous acid will quickly oxidize silicon to form nitric oxide. Nitric oxide will react with nitric acid and water to cause rapid oxidation of silicon. Nitric acid will eventually be reduced to nitrogen oxides.
[0145] Eventually the back side of the silicon wafer (in contact with the etching solution) is oxidized.
[0146] Step 2: Dissolution of Silica
[0147] After silicon dioxide is generated, it quickly reacts with hydrofluoric acid
[0148] SiO2+4HF=SiF4+2H2O (silicon tetrafluoride is a gas)
[0149] SiF4+2HF=H2SiF6.
[0150] Overall reaction: SiO2+6HF=H2SiF6+2H2O
[0151] The etched silicon eventually enters the solution as fluorosilicic acid.
[0152] Nitrous acid itself is not particularly stable and will slowly decompose. In small batch production with constant on-off operation, the equilibrium point of nitrous acid concentration in the solution will not exceed a certain limit, and the etching solution will remain colorless. In large batch production, the equilibrium point of nitrous acid concentration will rise. A slight increase in nitrous acid concentration will lead to an interesting phenomenon - the solution color will turn light green and green.
[0153] As long as the etching is normal, the solution color turning green will not have any impact on the efficiency of the wafer. When etching unqualified wafers, some impurities may be introduced into the etching solution, contaminating the etching solution, but this has nothing to do with the greening.
[0154] The role of the alkaline cleaning tank: The alkaline cleaning tank is located after the etching tank and the first water spray. Its role is to use potassium hydroxide or sodium hydroxide to neutralize and wash away the acid attached to the back side (the side in contact with the etching solution) and the edge of the silicon wafer.
[0155] Due to the low temperature, very low alkali concentration and short alkali washing time, the alkali solution will not have any effect on the silicon wafer. Acid-base neutralization is a fast reaction.
[0156] As NaOH absorbs carbon dioxide in the air, sodium carbonate is precipitated, causing crystallization and alkali blocking. When the temperature is low or it is not used for a long time, crystallization and alkali blocking will be very serious. Pay attention to flushing the crystals in the alkali tank. Among them, the initial concentration (%) of KOH or NaOH is 3-10 g / L.
[0157] The function of the pickling tank: The pickling tank is used after the alkaline cleaning tank. It uses hydrofluoric acid to neutralize and rinse away the alkali on the surface of the silicon wafer, remove the metal ions on the surface of the silicon wafer, clean the residual solution in the acid tank, and dry the silicon wafer. The initial concentration of acid HF (%) is 3-10 g / L.
[0158] In the process, the rolling conveyor device of the present invention plays a vital role, including loading - etching - rinsing - alkaline washing tank - rinsing tank - acid washing tank - rinsing tank - air drying - unloading. The rolling conveyor device of the present invention is used for transmission between each tank in the process, which solves the problems of long transmission cycle, easy damage to silicon wafers and difficult to control time.
[0159] The corrosion rate and corrosion depth are the key points to control during the process. Under the same time conditions, if the corrosion rate is too high, the corrosion depth will be too high, resulting in a reduction in the thickness of the silicon wafer. The current silicon wafer is 160um or 180um. It is easy to break due to its thin thickness. The thinner the silicon wafer, the easier it is to be damaged during the process, affecting the conformity rate of the finished product during the production process; and affecting the efficiency of the battery. Under the same time conditions, if the corrosion rate is too low and the corrosion depth is not enough, it is equivalent to not playing the role required by this process, affecting the efficiency of the battery.
[0160] The transmission speed of the corrosion process, the ratio of the corrosion solution, and the corrosion depth all complement each other and affect the following test processes:
[0161] The test found that as the number of etched wafers increases, the corrosion rate will continue to decrease, so in order to ensure the etching depth, the etching rate has to be gradually reduced. After the number exceeds 150,000 wafers, the efficiency is affected.
[0162] The above process problem is actually caused by the incorrect proportion of the etching solution, the proportion of hydrofluoric acid is too little. For the etching solution, if one of the hydrofluoric acid and nitric acid is less, the etching rate will still be very low no matter how much the other one is.
[0163] Through a large number of tests on SE cells, it was found that the etching advantage can be basically maintained when the corrosion rate is maintained at about 0.8m / min or more and the corresponding belt speed is above 1.0m / min to erode to a depth of about 1um. When the etching rate drops to a transmission speed of less than 0.7m / min to reach the etching depth, the efficiency is lower than the corrosion demand. At this time, the parallel resistance of the silicon wafer (semi-finished photovoltaic cell) still has an advantage, but the short-circuit current and open-circuit voltage are small. The test shows: "There must be a corrosion rate of more than 1.0m / min."
[0164] Therefore, in order to achieve the service life of the etching solution, a certain corrosion rate must be maintained.
[0165] After batch process tests, the upper and lower limits of the corrosion rate are: upper limit 1.52m / min, lower limit 1.2m / min. This is the best range of corrosion rate obtained after the above process tests; before and after each batch of silicon wafers are corroded or etched, 3 silicon wafers representing the batch will be drawn according to the test method of the present invention, and the corrosion depth of the silicon wafers will be calculated, and the corrosion rate will be calculated continuously, so as to achieve the purpose of controlling the quality of the entire process.
[0166] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for testing the corrosion rate of a crystalline silicon wafer, characterized in that: include: Weigh the silicon wafer to be corroded, and record the weight W1 of the silicon wafer before corrosion; Put the silicon wafer on the rolling conveyor in the cleaning tank and immerse the silicon wafer completely in the chemical solution in the cleaning tank, set the conveying time and conveying speed of the rolling conveyor in the cleaning tank, and clean and corrode the silicon wafer; Take out the corroded silicon wafer and weigh it, and record the weight of the corroded silicon wafer W2; The corrosion depth Δh of the silicon wafer is calculated by the corrosion depth formula (1): According to formula (2) and formula (1), formula (3) is obtained, and the silicon wafer corrosion rate ν is calculated by formula (3): Δh=ν×T (2) Where: Δh—Corrosion depth of silicon wafer after etching, unit: μm ν—Corrosion rate, unit: μm / s W1—weight of sample silicon wafer before corrosion, unit: g W2—The weight of the impurities removed after silicon wafer etching, in g S—area of the two etched surfaces of the silicon wafer, in cm 2 T—corrosion time, unit: s ρ—Silicon density, unit: g / cm 3 Repeat the above test silicon wafer, calculate the silicon wafer corrosion rate of each test, and calculate the average silicon wafer corrosion rate according to formula (4): (4) Where: ν—average value of corrosion rate, μm / s; ν n —Corrosion rate of a single sample, μm / s; n—positive integer; When cleaning in the cleaning tank, the silicon wafer passes through the alkaline cleaning tank, the rinsing tank, the acid cleaning tank and the rinsing tank in sequence along with the rolling conveyor device. The concentration of the NaOH solution in the alkaline cleaning tank is 3-10g / L; the concentration of the HF acid solution in the acid cleaning tank is 3-10g / L; the conveying speed of the rolling conveyor device is greater than or equal to 1.0m / min; Three samples were selected for testing; the test environment temperature was 25℃±2℃; the upper deviation of the measured corrosion rate was 1.52m / min, and the lower deviation was 1.2m / min; each sample was within the standard deviation of 0.32m / min.
2. The method for testing the corrosion rate of a crystalline silicon wafer according to claim 1, wherein: The weighing is performed using an electronic balance; a bracket for supporting the silicon wafer is provided on the electronic balance.
3. The method for testing the corrosion rate of a crystalline silicon wafer according to claim 2, wherein: The bracket comprises a chassis placed on the electronic balance and a backing plate arranged on the chassis, and a slot for positioning the silicon wafer is arranged at the intersection of the backing plate and the chassis.
4. The method for testing the corrosion rate of a crystalline silicon wafer according to claim 3, wherein: The backing plate is an arc-shaped plate, and two vertical sides of the arc-shaped plate have an inclination for the silicon wafer to lean against.
5. The method for testing the corrosion rate of a crystalline silicon wafer according to claim 4, wherein: The area of the orthographic projection of the arc-shaped plate on the chassis is greater than half of the area of the chassis.
6. The method for testing the corrosion rate of a crystalline silicon wafer according to claim 3, wherein: The lower surface of the chassis is provided with an annular groove which is clamped with the tray of the electronic balance.
7. The method for testing the corrosion rate of a crystalline silicon wafer according to claim 3, wherein: The chassis is provided with support edges extending upwards on all sides, and the clamping slot is arranged at the intersection of the support plate and the support edge.
8. The method for testing the corrosion rate of a crystalline silicon wafer according to claim 3, wherein: The card slot is a V-shaped slot.
9. The method for testing the corrosion rate of a crystalline silicon wafer according to claim 2, wherein: The bracket is made of plastic or rubber.