A multi-layer bionic joint based on curved surface 3D printing and preparation method thereof

Through the design of multi-layer bionic joints and combined with 3D printing technology, the multi-layer structure of human cartilage and bone tissue is simulated, the problem of repairing large-area osteocartilage joint defects is solved, and efficient bone tissue healing and implant stability is achieved. Improve the feasibility of clinical applications.

CN112076009BActive Publication Date: 2024-11-12AFFILIATED ZHONGSHAN HOSPITAL OF DALIAN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011080543.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-10
Publication Date
2024-11-12
Estimated Expiration
2040-10-10

AI Technical Summary

Technical Problem

The prior art is difficult to effectively repair large-area osteocartilage joint defects, especially in terms of the complex structure and mechanical needs of cartilage tissues. It is difficult for existing materials to simulate the multi-layer structure of human cartilage and bone tissue, resulting in poor repair results.

Method used

Multi-layer bionic joints are adopted, including the inner layer as a porous tantalum metal bracket, the middle layer as a solid bioceramic bracket and the outer layer as a solid gelatin/sodium alginate composite hydrogel bracket, which is prepared by 3D printing technology to form an arc-shaped shell structure , and a cell loading cavity is formed on the outer surface to simulate the structural and mechanical properties of the human cartilage and bone tissue.

Benefits of technology

It has achieved personalized repair of large-area osteocartilage joint defects, improved the healing ability of bone tissue and the stability of implants, avoided stress occlusion, enhanced bone integration performance, reduced the number of surgeries, and improved clinical application feasibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112076009B_ABST
    Figure CN112076009B_ABST
Patent Text Reader

Abstract

The present invention discloses a bionic bone joint based on curved surface 3D printing and a preparation method thereof. The multilayer bionic joint is formed by closely contacting the inner layer, the middle layer and the outer layer in the order of the inner layer, the porous tantalum metal scaffold, the middle layer is a solid bioceramic scaffold, and the outer layer is a solid gelatin / sodium alginate composite hydrogel scaffold. The inner layer, the middle layer and the outer layer are all in an arc-shaped shell structure, and the curvature of the shell is 120-240°. A cell loading cavity consisting of continuous or discontinuous edges protruding outward from the outer surface and grooves formed between the edges is formed on the outer surface. The multilayer bionic joint of the present invention has a large arc surface curvature and is suitable for repairing large-area osteochondral joint defects, and the repair area can be greater than 1 / 2 of the entire joint area. Cells are accessed in the cell loading cavity to increase the cell attachment rate, overcoming the problem that the outer surface of the bionic joint is smooth and the accessed cells are not easy to attach.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical bone cartilage repair, and in particular to a bionic bone joint based on curved surface 3D printing and a preparation method thereof. Background Art

[0002] Osteochondral lesions are common orthopedic diseases, and there is a lack of effective treatment methods. The main methods used for the clinical repair of osteochondral defects include debridement, bone marrow stimulation, osteochondral transplantation, and joint replacement. For small-area injuries, osteochondral transplantation is currently the main clinical treatment method, but there are problems such as limited material intake, donor site damage, and difficulty in matching the graft with the joint surface; for large-area osteochondral synostosis defects, the most commonly used method in clinical practice is joint replacement. However, artificial joint prostheses have complications such as infection, loosening, and sinking. In clinical practice, joint lesions can often only be treated by simply repairing the defective bone, while defects of cartilage, etc., especially when the defects are large and deep, are almost impossible to repair.

[0003] From the surface of the joint to the deep part of the bone, the autologous joint is divided into three layers, namely the hyaline cartilage layer, the dense calcification layer and the subchondral bone layer. Each layer has different complex structures and properties. The subchondral bone tissue supplies nutrients and oxygen through its blood circulation to provide the needs of tissue metabolism; the rich blood supply and oxygen supply enable the bone tissue to have a certain self-repair ability. However, the microenvironment of the cartilage tissue lacks oxygen and blood supply, and nutrients are mainly supplied by the synovial fluid in the joint cavity. Therefore, the repair and regeneration ability of the cartilage tissue is weaker than that of the bone tissue. Between the subchondral bone tissue and the cartilage tissue, there is a dense calcification layer structure that connects the two and forms a barrier to prevent the fluid in the medullary cavity from entering the joint cavity, thereby keeping the microenvironment of the cartilage and subchondral bone stable. The ideal tissue engineering scaffold should highly simulate the in vivo structure of these three layers at the same time, and take into account the strength of the bonding between the layers, the matching of the material degradation time with the speed of tissue regeneration in the body, and the biocompatibility of the material. To this end, CN108201634A researchers tried to prepare a three-layer composite material using porous tantalum, porous salt and porous polymer prepared by foam slurry method. However, it is difficult to accurately control the uniformity of the pore size of the prepared porous metal by foam slurry method; and the different layers of porous tantalum metal need to be connected again by resistance welding; at the same time, the slurry method is difficult to meet the high opening rate; the porous salt and polymer on it cannot evenly prepare the curved surface effect required for the joint part. As we all know, the larger the curved surface, the larger the joint part that can be repaired. CN107485731A uses 3D integrated printing technology to prepare an integrated three-layer composite scaffold for articular cartilage repair, and its calcified subchondral bone plate layer and cancellous bone layer are both porous layers of bioceramic particles and sodium alginate composite hydrogel. However, the product is highly brittle and it is difficult to meet the clinical mechanical requirements for the bone layer. CN105287057A uses materials such as polyvinyl alcohol hydrogel doped with carbon nanotubes and bacterial cellulose impregnated with polyvinyl alcohol hydrogel to prepare an artificial femoral head. It is difficult for the above-mentioned components to enter clinical trials and obtain clinical approval, and there is no report on the efficacy of long-term follow-up. CN105105875A designed a bionic artificial hip joint with ingrowth function, but its joint surface wrap angle is only 60-120°, which cannot meet the repair of joints in large-area bone and cartilage joint injuries. At the same time, the middle layer of the bionic joint is made of fibrin glue or biological glue. This product is mainly used for soft tissue bonding. The bonding strength that can be provided by integrating the lower metal and the upper polymer material is insufficient, and it is easy to produce interlayer separation. Moreover, due to the limitation of the ingredients, the biological glue cannot simulate the calcification layer in the body well, and it is difficult to achieve effective isolation of the cartilage microenvironment and the osteogenic microenvironment. Summary of the invention

[0004] In view of the deficiencies in the repair process of large-area osteochondral defects, the present invention provides a bionic joint that can be customized individually. The bionic joint is made by 3D printing and has a multi-layer structure, and can be used as a repair implant for large-area osteochondral defects.

[0005] The technical solution of the present invention is as follows:

[0006] According to a first aspect of the present invention, a multi-layer bionic joint is provided, wherein the multi-layer bionic joint is formed by closely contacting an inner layer, a middle layer and an outer layer in order, wherein the inner layer is a porous tantalum metal scaffold, the middle layer is a solid bioceramic scaffold, and the outer layer is a solid gelatin / sodium alginate composite hydrogel scaffold. The inner layer, the middle layer and the outer layer are all in an arc-shaped shell structure, and the arc of the arc shell has an arc angle of 120-240°. A cell loading cavity is formed on the surface of the outer layer, and the cell loading cavity is composed of continuous or discontinuous edges protruding outward from the surface of the outer layer and grooves formed between the edges.

[0007] In the above technical solution, the inner layer is made of tantalum metal powder as the base material and is produced by metal 3D printing processing, the middle layer is made by depositing the bioceramic slurry as the base material on the outer surface of the inner layer through biological 3D printing, and the outer layer is made by depositing the gelatin / sodium alginate composite hydrogel liquid as the base material on the outer surface of the middle layer through biological 3D printing.

[0008] In the above technical solution, in the structure of the cell loading chamber, the thickness of the rib is 0.2-0.4 mm, the height of the rib is 0.8-1.2 mm, and the width of the groove is 0.7-1 mm. Preferably, the thickness of the rib is 0.3 mm, the height of the rib is 1.0 mm, and the width of the groove is 0.8 mm. The thickness and height of the rib and the width of the groove affect the attachment and growth of the loaded cells.

[0009] In the above technical solution, the bioceramic is composed of hydroxyapatite, calcium sulfate or a mixture of the two.

[0010] In the above technical solution, the inner surface of the middle layer is in close contact with the outer surface of the inner layer by covering the outer surface of the inner layer, and the inner surface of the outer layer is in close contact with the outer surface of the middle layer by covering the outer surface of the middle layer.

[0011] In the above technical solution, the inner diameter of the arc-shaped shell is 20-40 mm, the thickness of the porous tantalum metal stent is 1-3 mm, the thickness of the solid hydroxyapatite stent is 0.3-0.5 mm, and the thickness of the solid gelatin / sodium alginate composite hydrogel stent is 2-3 mm. The inner diameters of the inner layer, the middle layer and the outer layer of the multi-layer bionic joint are all 20-40 mm, the shape of the arc-shaped shell is preferably a hemispherical shell, and the curvature of the arc-shaped shell is 120-240°, preferably 150°, and more preferably 180°. Appropriate inner diameter, outer diameter and curvature can be used according to the characteristics of different joint parts implanted.

[0012] In the above technical solution, the pore size of the porous tantalum metal stent is 200-800 μm, preferably 400-600 μm, and the porosity is 50-90%, preferably 70-90%. The porous structure is an interconnected pore structure, and the shape of the porous structure can adopt a variety of shapes, which can be a regular pore structure or a trabecular pore structure.

[0013] In the above technical solution, the porous tantalum metal stent has at least one fixing hole, preferably 2 to 4 fixing holes, and when there are more than one fixing hole, the adjacent fixing holes are 90° apart; the diameter of the fixing hole is 2-8 mm, and the fixing holes can be symmetrically or asymmetrically distributed in the arc-shaped porous tantalum metal stent, and their positions are appropriately adjusted according to the diameter of the arc-shaped porous tantalum metal stent. The fixing hole is a screw hole, and the screw hole can be a profile countersunk hole. Such a structure facilitates the screw to sink into the screw hole, avoiding the stimulation of the protruding part to the surrounding tissue.

[0014] In the above technical solution, the porous tantalum metal scaffold layer (inner layer) used to simulate subchondral bone is loaded with bone marrow mesenchymal stem cells. The solid gelatin / sodium alginate composite hydrogel scaffold (outer layer) used to simulate the cartilage layer is loaded with chondrocytes. The solid bioceramic scaffold in the middle layer is a simulated calcified layer. After the three-layer composite scaffold of the present invention is implanted in the body, it forms a subchondral bone layer, a calcified layer and a cartilage layer respectively.

[0015] In the present invention, a 3D geometric image of the patient's lesion (such as a cartilage defect lesion) can be obtained through CT scanning data and three-dimensional image software, and based on the 3D geometric image, a three-dimensional geometric model of the inner layer, middle layer and outer layer of the multi-layer bionic joint described in the present invention can be designed, and a personalized multi-layer bionic joint for the patient can be obtained through 3D printing.

[0016] In the present invention, the solid bioceramic scaffold serves as the middle layer of the multi-layer bionic joint and is closely attached to the outer surface of the porous tantalum metal scaffold. Since 3D printing is performed using hydroxyapatite or calcium sulfate slurry with suitable viscosity, part of the slurry penetrates into the porous tantalum metal scaffold through the pores, thereby achieving an integrated combination effect between the porous tantalum metal and the bioceramic.

[0017] In the present invention, the gelatin / sodium alginate composite hydrogel solution is composed of a gelatin solution and a sodium alginate solution, wherein the mass content of gelatin in the gelatin solution is 2-20%, and the mass content of sodium alginate in the sodium alginate solution is 0.5-10%. Growth factors may also be added to the gelatin / sodium alginate composite hydrogel solution, such as vascular endothelial growth factor protein or / and fibroblast growth factor protein components that promote chondrocyte proliferation and differentiation. The amount of growth factor protein added accounts for 0.1-1% of the mass of the gelatin / sodium alginate composite hydrogel solution.

[0018] A second aspect of the present invention provides a method for preparing the above-mentioned multi-layer bionic joint, comprising the following steps:

[0019] (1) Using 3D design software, the 3D geometric models of the inner layer, middle layer, and outer layer of the multi-layer bionic joint are designed respectively;

[0020] (2) According to the three-dimensional geometric model of the multilayer bionic joint inner layer obtained in step (1), tantalum metal powder is used as the substrate, and metal 3D printing is performed under argon environment protection to obtain a porous tantalum metal stent print; wherein the process parameters of the 3D printing are: powder thickness of 30-50 μm, laser power of 100-200 W, exposure time of 40-70 μs, laser scanning point spacing of 30-60 μm, and line spacing of 30-60 μm;

[0021] (3) heat treating the porous tantalum metal bracket printout obtained in step (2), and then sandblasting, cleaning, and drying to obtain a multi-layer bionic joint inner layer, wherein the heat treatment conditions are: heating rate of 5°C / min, heating to 1200-2000°C, and keeping warm for 1 hour; the sandblasting conditions are: force of 0.1-1MPa, and treatment time of 30-120s;

[0022] (4) According to the three-dimensional geometric model of the multi-layer bionic joint middle layer obtained in step (1), the bioceramic slurry is printed onto the outer surface of the multi-layer bionic joint inner layer obtained in step (3) by bio-3D printing according to the printing path, so as to generate a multi-layer bionic joint middle layer and obtain a printed part I, wherein the 3D printing conditions are as follows: the printing temperature is 15-20° C., the printing pressure is 0.18-0.22 MPa, the printing speed is 3-7 mm / s, the printing spacing is 0.5-1 mm, the needle tip compensation parameter is 1-2 mm, the printing layer thickness is 0.3-0.5 mm, and the printing nozzle is moved during printing to pull the extruded bioceramic slurry into a filament shape and deposit it onto the outer surface of the multi-layer bionic joint inner layer, and the printing is completed according to the printing path;

[0023] (5) According to the three-dimensional geometric model of the multi-layer bionic joint outer layer obtained in step (1), the gelatin / sodium alginate composite hydrogel liquid is printed on the outer surface of the multi-layer bionic joint middle layer in the printed part I obtained in step (4) according to the printing path by biological 3D printing, so as to generate a multi-layer bionic joint outer layer and obtain a printed part II, wherein the 3D printing conditions are: printing temperature of 25-40° C., printing pressure of 0.1-0.4 MPa, printing speed of 5-20 mm / s, needle tip compensation parameter of 1-2 mm, and the printing nozzle moves during printing to draw the ejected gelatin / sodium alginate composite hydrogel liquid into a filament, and deposit it on the outer surface of the multi-layer bionic joint middle layer to complete the printing;

[0024] (6) placing the printed part II obtained in step (5) in a divalent ion solution for cross-linking;

[0025] (7) The cross-linked printed part II is placed into a molding mold to form a cell loading cavity on the outer surface of the printed part II.

[0026] In the above technical solution, the shaping mold has a groove structure, and the outer layer of the printed part II contacts the surface of the shaping mold having the groove, thereby forming a cell loading cavity on the surface of the outer layer.

[0027] In the above technical solution, in step (4) and step (5), the method for generating the printing path of the biological 3D printing is as follows: using layering software to slice the three-dimensional geometric model (i.e., the three-dimensional geometric model of the middle layer or the outer layer of the multi-layer bionic joint), and cutting the model into multiple surfaces, wherein the surface can be a closed surface composed of closely arranged curves (such as Figure 2 A) or a porous surface with a grid composed of spaced curves (such as Figure 2 B); During printing, the printer's nozzle will print the material into a specific surface along the path of the generated curve, and the final 3D model is composed of stacked surfaces ( Figure 2). The layering software is the existing layering software that comes with the device. In step (4) and step (5), printing is performed based on the printing path of the curved surface slice, and specific needle tip compensation parameters are set during printing, that is, the needle tip compensation parameter is 1-2mm, so that the material can be better printed on the curved surface, thereby obtaining a multi-layer bionic joint with a large curvature.

[0028] In the above technical solution, in step (2), the tantalum metal powder is medical grade spherical tantalum metal powder with a particle size of 15-45 μm.

[0029] In the above technical solution, in step (3), the abrasive used in the sandblasting process is white corundum, and the particle size of the white corundum is 50-150 μm.

[0030] In the above technical solution, in step (3), the cleaning conditions are: ultrasonic cleaning is performed using acetone, alcohol and distilled water in sequence for 15-30 minutes respectively; and the drying temperature is 40-60°C.

[0031] In the above technical scheme, in step (4), the bioceramic slurry is mixed with ultrapure water, glycerol, hydroxyapatite powder or / and calcium sulfate powder, sodium alginate, wherein the particle size of the powder is ≤20nm. Hydroxyapatite powder and calcium sulfate powder can be used alone as bioceramic components, or can be mixed in a certain proportion. When used alone, the content of hydroxyapatite in the bioceramic slurry is 10-40wt%, and the content of calcium sulfate in the bioceramic slurry is 30-50wt%; when mixed, hydroxyapatite powder and calcium sulfate powder are mixed in a mass ratio of 1-2:1-2, and the content of the mixture in the bioceramic slurry is 10-50wt%.

[0032] In the above technical solution, in step (5), the gelatin / sodium alginate composite hydrogel solution is composed of a gelatin solution and a sodium alginate solution, the mass content of gelatin in the gelatin solution is 2-20%, and the mass content of sodium alginate in the sodium alginate solution is 0.5-10%.

[0033] In the above technical solution, in step (5), growth factors, such as growth factor protein or fibroblast growth factor protein components that promote chondrocyte proliferation and differentiation, are added to the gelatin / sodium alginate composite hydrogel solution. The amount of the growth factor protein added accounts for 0.1-1% of the mass of the gelatin / sodium alginate composite hydrogel solution.

[0034] In the above technical solution, in step (6), the method for preparing the gelatin / sodium alginate composite hydrogel solution comprises the following steps:

[0035] (a) fully dissolving gelatin at a temperature of 40-80° C. and under magnetic stirring to prepare a gelatin solution;

[0036] (b) adding sodium alginate to the gelatin solution, fully dissolving it, and stirring and mixing it evenly to prepare a gelatin / sodium alginate composite hydrogel solution.

[0037] In the above technical solution, in step (6), the divalent ion is a divalent cation, such as Ca 2+ , Cu 2+ , Fe 2+ , Sr 2+ 、Zn 2+ Or Ba 2+ The concentration of the divalent ion solution is 2-5%, and the cross-linking time is 5 min-24 h, preferably 5 min-2 h, and more preferably 10 min-40 min.

[0038] In the above technical solution, the inner layer and outer layer of the multilayer bionic joint obtained in step (6) are inoculated with bone marrow mesenchymal stem cells and chondrocytes, respectively. The bone marrow mesenchymal stem cells are autologous bone marrow mesenchymal stem cells, and the chondrocytes are autologous chondrocytes. The cell density during inoculation is preferably 10 7 -10 8 Pieces / mL.

[0039] The multilayer bionic joint of the present invention is a bracket with a curved surface with a large curvature, and its outermost layer is a gelatin / sodium alginate composite hydrogel, which is relatively soft and has good fluidity. The surface of the finished product after 3D printing is relatively smooth, which is not conducive to the attachment of cells. The multilayer bionic joint of the present invention has a cell loading cavity on its outer surface for cell access and culture. The cell loading cavity is composed of continuous or discontinuous edges protruding outward from the outer surface and grooves formed between the edges. The cell loading cavity can be formed by continuous or discontinuous threads evenly distributed on the outer surface, and the cell loading cavity can also be irregular in shape. For the shape of the cell loading cavity, at least a groove structure that can allow cells and culture medium to stay is included. In the present invention, it is preferred to use a stereotyped mold with a groove to form a cell loading cavity on the outer surface of the multilayer bionic joint. As in step (6) of the above-mentioned preparation method of the present invention, the printed part II is placed in a divalent ion solution for cross-linking to solidify the outer hydrogel layer. The cross-linking time varies according to the size and thickness of the printed part. Generally, the cross-linking is performed until the outer surface does not flow but has a certain degree of softness and plasticity. The cross-linking time is generally 5min-1h. The printed part after a certain period of cross-linking is taken out of the cross-linking liquid and placed in a stereotyped mold to form a cell loading cavity on the outside of the printed part. The printed part with the cell loading cavity is then placed in the cross-linking liquid to completely solidify the outside to obtain a multi-layer bionic joint for implants to repair osteochondral defects.

[0040] The third aspect of the present invention provides the use of the above-mentioned multi-layer bionic joint as a repair implant for repairing osteochondral syndesmosis defects. The multi-layer bionic joint of the present invention can preferably be used as a repair implant for large-area osteochondral syndesmosis defects.

[0041] Beneficial effects of the present invention:

[0042] 1. In the multi-layer bionic joint of the present invention, the porous tantalum metal stent as the inner layer can be customized according to the mechanical properties of the bone tissue in the implanted joint, avoiding stress shielding and facilitating bone tissue healing. The porous tantalum bionic trabecular hemisphere has a pore structure suitable for bone tissue growth, which helps to improve the bone integration performance of the hemisphere and surrounding bone tissue, and has excellent bone integration, achieving permanent biological internal fixation without the need for secondary surgery to remove it.

[0043] 2. In the multi-layer bionic joint of the present invention, the connection between the porous tantalum bionic bone trabeculae (inner layer) and the degradable hydrogel bionic cartilage (outer layer) uses bioceramic slurry as the base material, and the calcified layer (middle layer) is prepared by 3D printing processing technology, which effectively realizes the construction of integrated bone cartilage tissue engineering, so that the connection part has sufficient interface adhesion and shear strength. The 3D printed calcified layer can partially degrade the main inorganic components of natural bone such as calcium phosphate.

[0044] 3. The multi-layer bionic joint of the present invention is an arc-shaped shell structure, and the arc surface curvature of the arc-shaped shell is 120-240°, which can completely cover the maximum torsion curvature of the prosthesis required for large-area joint injuries in clinical practice. Although metal 3D printing can achieve such large-curvature metal printing by designing support beams, there is currently no bionic cartilage layer and calcification layer with such a large curvature prepared by biological 3D printing technology. The present invention realizes the 4-axis linkage of the X-axis, Y-axis, Z-axis and U-axis by designing a specific "printing path", adopts curved surface slicing instead of traditional plane slicing, and fully considers the collision between the needle tip and the printing model to introduce the parameters of needle tip compensation, so that the material can be better printed on the curved surface, breaking through the current international technical bottleneck of large-curvature curved surface printing, thereby obtaining a large-curvature multi-layer bionic joint.

[0045] 4. The multilayer bionic joint of the present invention has a cell loading cavity for loading cells formed on its outer surface, and chondrocytes are loaded (accessed) in the cell loading cavity for cultivation, which is conducive to the attachment of chondrocytes in gelatin / sodium alginate hydrogel and deep penetration into the hydrogel, and can well overcome the problem that the accessed cells are not easy to attach due to the smooth surface of the hydrogel. This cell access method has almost no harm to the cells, and can solve the damage to the cells caused by placing the cells in the 3D printing slurry for printing in the prior art.

[0046] 5. The bionic joint of the present invention is processed and manufactured by 3D printing technology. The biomechanical properties of the bionic joint can be optimized by adjusting the porosity and pore size of the porous tantalum base. The porous tantalum hemispherical shell provides biomechanical internal fixation for the bone tissue at the implantation site, and can also ensure that the bone tissue is subjected to sufficient stress stimulation to stimulate the self-repair function of the bone tissue; through the osteoinduction effect of the porous hemisphere, the bone tissue and the bionic joint can achieve good bone integration, avoid loosening in the body, and need secondary surgery to remove the problem, thereby alleviating the pain of the patient. The bionic calcification layer made of bioceramic slurry plays a transitional role between bone and cartilage tissue, effectively preventing the flow of cells and blood to the cartilage layer, and plays a mechanical support and barrier effect. Gelatin / sodium alginate hydrogel has good biocompatibility and degradability, and is an ideal biological scaffold that can carry chondrocytes. 3D printed gelatin / sodium alginate hydrogel can simulate the special three-dimensional microenvironment required for the growth of chondrocytes, maintain their phenotypes, promote the expression of related proteins, and easily construct a mechanical environment similar to natural articular cartilage.

[0047] 6. The bionic joint prepared by the present invention is suitable for repairing large-area osteochondral joint defects, and the repair area can be greater than 1 / 2 of the entire joint area. The cells used in the integrated repair material are all autologous cells, and the components of the three-layer scaffold material are all clinically approved access materials. The product can be quickly connected to clinical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 A schematic diagram of the three-dimensional geometric model of the porous hemispherical shell designed using mapping software, wherein A is a top view of the three-dimensional geometric model; B is a side view of the three-dimensional geometric model; C is a bottom view of the three-dimensional geometric model; and D is a top view of the actual 3D printed porous tantalum metal hemispherical shell obtained by 3D printing based on the three-dimensional model.

[0049] Figure 2 Schematic diagram of the printing path designed and generated by computer layering software for printing bioceramic scaffolds and gelatin / sodium alginate composite hydrogel scaffolds.

[0050] Figure 3 Indicates based on Figure 2 The printing path is a physical picture of the 3D printed part after 3D printing the hydroxyapatite calcification layer and the gelatin / sodium alginate composite hydrogel layer in sequence on the porous tantalum metal hemispherical shell 3D printed part, wherein A is a top view of the double-layer 3D printed part after printing the hydroxyapatite calcification layer, B is a top view of the three-layer 3D printed part after printing the gelatin / sodium alginate composite hydrogel layer (outer layer), and C is a bottom view of the three-layer 3D printed part.

[0051] Figure 4 express Figure 3A physical picture of the multi-layer bionic joint of the present invention having a cell-loading cavity formed on the outer surface of a three-layer 3D printed part.

[0052] Figure 5 A shaping mold for forming a cell-loading cavity on the outer surface of the multi-layer bionic joint of the present invention, wherein A is a schematic diagram of a three-dimensional geometric model designed using mapping software; B is a top view of the three-dimensional geometric model; C is a side view of the three-dimensional geometric model; and D is a physical picture of the titanium alloy shaping mold after 3D printing based on the three-dimensional geometric model.

[0053] Figure 6 The figure shows the treatment process of implanting the multi-layer bionic joint of the present invention to repair a large area of ​​femoral head defect, wherein A is a surgical diagram of preparing a half femoral head defect model of a goat; B and C are surgical diagrams of implanting a bionic joint in the hind leg of a goat and fixing it with screws; and D is an X-ray photograph taken 6 weeks after implantation of the bionic joint.

[0054] Figure 7 yes Figure 6 The stained images of histological specimens at the femoral head defect site 6 weeks after the implantation of the bionic joint, among which A is the VG staining result after the hard tissue section of the osteochondral repair area; B is the VG staining result after the hard tissue section of the bone repair area; C is the immunohistochemical staining result of the chondrogenic specific molecule-type II collagen; D is the immunohistochemical staining result of the osteogenic specific molecule-type I collagen.

[0055] Explanation of symbols: 1. inner layer, 2. middle layer, 3. outer layer, 4. fixing hole, 5. cell loading cavity, 51. edge, 52. groove, 7. shaping mold, 71. support part, 72. forming part. DETAILED DESCRIPTION

[0056] The following non-limiting examples are provided to enable those skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way. In the following examples, unless otherwise specified, the experimental methods used are all conventional methods, and the materials and reagents used can be purchased from biological or chemical companies.

[0057] Example 1

[0058] A multi-layer bionic joint, wherein the multi-layer bionic joint is formed by closely contacting an inner layer, a middle layer and an outer layer in order, wherein the inner layer is a porous tantalum metal bracket, the middle layer is a solid bracket, and the outer layer is a solid gelatin / sodium alginate composite hydrogel bracket, and the inner layer, the middle layer and the outer layer are all in an arc-shaped shell structure, and the arc-shaped shell is a hemispherical shell.

[0059] The inner layer is made of tantalum metal powder as a base material and is made by metal 3D printing. The middle layer is made by depositing hydroxyapatite slurry as a base material on the outer surface of the inner layer by biological 3D printing. The outer layer is made by depositing gelatin / sodium alginate composite hydrogel liquid as a base material on the outer surface of the middle layer by biological 3D printing. The inner surface of the middle layer is in close contact with the outer surface of the inner layer in a manner of covering the outer surface of the inner layer, and the inner surface of the outer layer is in close contact with the outer surface of the middle layer in a manner of covering the outer surface of the middle layer.

[0060] A method for preparing a multi-layer bionic joint based on 3D printing comprises the following steps:

[0061] 1) Use Creo graphics software to design and obtain the three-dimensional geometric model of the porous hemispherical shell (the inner layer of the multi-layer bionic joint) (such as Figure 1 As shown), output .stl format file;

[0062] 2) Import the .stl format file into the 3D printing software, use the porous tantalum metal powder as the substrate for 3D printing, and obtain a porous tantalum metal hemispherical shell (such as Figure 1 D);

[0063] The 3D printing steps of the porous tantalum metal hemispherical shell are as follows: in the 3D printing software, in the Building Processing interface, the tantalum metal parameter package is merged with the .stl file to obtain the .mtt format file of the three-dimensional geometric model of the porous tantalum metal hemispherical shell that can be recognized in the 3D printer device, and the .mtt format file is input into the 3D printing device, and 3D printing is performed under the protection of a protective gas atmosphere; the 3D printing conditions are: the powder thickness is 30 μm, the laser power is 180 W, the exposure time is 70 μs, the laser scanning point spacing is 30 μm, and the line spacing is 40 μm; wherein the porous tantalum metal powder is a medical-grade spherical powder with a purity of ≥99.99wt% and a particle size of 30 μm, the protective gas is high-purity argon (purity ≥99.99%), and during the printing process, the oxygen content in the working cavity is less than 1000 ppm;

[0064] 3) The printed parts are subjected to high-temperature heat treatment to eliminate the residual stress generated during the processing and to make the surface of the hemispherical shell smooth. The heat treatment temperature is 1250°C, the heating rate is 5°C / min, the temperature is kept for 1 hour, and the furnace is cooled;

[0065] 4) The heat-treated printed part is placed in a sandblasting machine for sandblasting to remove excess metal powder adhering to the surface; the abrasive used for sandblasting is white corundum, the particle size of white corundum is 50μm-150μm, the sandblasting force is 0.3MPa, and the sandblasting time is 40s;

[0066] 5) The sandblasted printed part was ultrasonically cleaned with acetone, alcohol, and distilled water for 15 minutes respectively, and vacuum dried at 40° C. to obtain a 3D printed porous tantalum metal hemispherical shell (i.e., the inner layer of the multilayer bionic joint), as shown in FIG. Figure 1 As shown in D;

[0067] like Figure 1 The hemispherical shell shown is a porous structure, and four fixing holes are arranged on the top of the shell. The diameter of the screw holes is 3.5 mm. The screw holes are profile countersunk holes, so that after the screws are fixed, there will be no irritation to the surrounding tissues due to the protrusion of the screws. The inner diameter of the hemispherical shell is 21 mm, and the thickness of the hemispherical shell is 1 mm. The porous structure consists of an internally connected three-dimensional cross-cross (space diamond body-centered cubic) pore structure, with a porosity of 80% and a pore size of 800 μm. Figure 1 middle, Figure 1 A to C represent the top view, side view, and bottom view of the three-dimensional geometric model, respectively. Figure 1 D represents the top view of the porous tantalum metal hemispherical shell 3D printed based on the three-dimensional geometric model. Its actual size is Figure 1 The computer design models shown are basically the same.

[0068] The 3D printed porous tantalum metal hemispherical shell has a compressive strength of 54 MPa, a flexural strength of 77 MPa, and an elastic modulus of 3.3 GPa.

[0069] 6) Using Creo drawing software to design and obtain a three-dimensional geometric model of the hydroxyapatite scaffold (middle layer), importing the three-dimensional geometric model data file, generating a printing path, adjusting the printing parameters of the bioprinter: the temperature is 18° C., the printing pressure is 0.2 MPa, the printing speed is 3 mm / s, the printing spacing is 0.6 mm, the printing layer thickness is 0.35 mm, the needle tip compensation parameter is 1.2 mm, and 3D printing is performed according to the printing path, that is, the porous tantalum metal hemispherical shell obtained in step 5) is first placed on the printer platform, the printing program is started, the print head moves, and the extruded hydroxyapatite slurry is pulled into a filament and printed on the outer surface of the porous tantalum metal hemispherical shell according to the printing path, so that the calcified layer can be closely attached to the outer surface of the porous tantalum bionic trabecular bone hemisphere, generating a multi-layer bionic joint middle layer, and obtaining a printed part I;

[0070] Preparation of slurry: (HAP) powder with a particle size of 20 nm is placed in a mixed solvent of glycerol and ultrapure water (the volume ratio of glycerol to ultrapure water is 5:5), and stirred for about 0.5 h by a stirrer with a rotation speed of 1500 rpm to prepare a slurry with a solid content of 30%; then sodium alginate is added to the slurry as a bioadhesive, and the final concentration of sodium alginate in the slurry is 2%, and stirred for about 1.5 h by a stirrer with a rotation speed of 2000 rpm, and degassed by centrifugation (rotation speed is 5000 rpm) for about 0.5 h, and then degassed by low temperature to obtain a bioactive hydroxyapatite slurry; wherein the weight average molecular weight of sodium alginate is 12-190 KDa;

[0071] 7) Using Creo drawing software to design a three-dimensional geometric model of the gelatin / sodium alginate composite hydrogel scaffold (outer layer), importing the three-dimensional geometric model data file, generating a printing path, and adjusting the printing parameters of the bioprinter: the printing temperature is 35°C, the printing pressure is 0.3MPa, the printing speed is 8mm / s, and the needle tip compensation parameter is 1.2mm. 3D printing is performed according to the printing path, that is, the gelatin / sodium alginate composite hydrogel liquid is placed in the printing syringe, and the printing nozzle moves during printing to pull the ejected hydrogel liquid into a filament and deposit it on the outer surface of the porous hydroxyapatite calcification layer of the printed part I obtained in step 6), completing the printing, generating the outer layer of the bionic joint, and obtaining the printed part II;

[0072] Preparation of gelatin / sodium alginate composite hydrogel solution: fully dissolve gelatin (weight average molecular weight of 50-100KDa) at a temperature of 65°C and under magnetic stirring to prepare a gelatin solution with a mass concentration of 10%; add sodium alginate to the gelatin solution and fully dissolve it, wherein the mass concentration of sodium alginate is 2%, stir and mix evenly, and then remove bubbles by low-speed centrifugation to prepare a gelatin / sodium alginate composite hydrogel solution;

[0073] 8) The printed part II obtained in step 7) is placed in a pre-prepared 5% calcium chloride solution for cross-linking for 10 minutes to form a gelatin / sodium alginate composite hydrogel scaffold to obtain a 3D printed multi-layer bionic joint. The scaffold is sterilized by ethylene oxide fumigation and stored aseptically for later use.

[0074] In the above step 8), in order to stably form the gelatin / sodium alginate composite hydrogel scaffold layer, the cross-linking time of the printed part II in the cross-linking solution can be appropriately extended, such as cross-linking for 30 minutes to 2 hours, and then taken out, sterilized, and stored aseptically for later use.

[0075] In the above step 6) and step 7), the method of generating the printing path is the same, and the method of generating the printing path is as follows:

[0076] The 3D geometric models designed by the 3D design software are sliced ​​using the layering software provided by the device, and the models are cut into multiple curved surfaces, which are closed curved surfaces composed of closely arranged curves (such as Figure 2 A). When printing, the printer's nozzle will print the material into a specific surface along the path of the generated curve, and the final 3D model is composed of stacked surfaces ( Figure 2 ).

[0077] Figure 3 Indicates based on Figure 2 The actual picture of the 3D printed part after 3D printing the hydroxyapatite calcification layer and the gelatin / sodium alginate composite hydrogel layer on the porous tantalum metal hemispherical shell 3D printed part in sequence, where A is a top view of the double-layer 3D printed part after printing the hydroxyapatite calcification layer, B is a top view of the three-layer 3D printed part after printing the gelatin / sodium alginate composite hydrogel layer (outer layer), and C is a bottom view of the three-layer 3D printed part. Figure 3 It can be clearly seen in A to 3C that the multi-layer bionic joint obtained by the method of the present invention presents a complete hemispherical shell shape, and the thickness of each layer is uniform without falling off. Figure 3 In C, the outer layer is a solid gelatin / sodium alginate hydrogel scaffold hemispherical layer (gelatin / sodium alginate composite hydrogel scaffold), the middle layer is a solid hydroxyapatite calcification layer (hydroxyapatite scaffold), and the inner layer is a porous tantalum metal scaffold hemispherical layer (porous tantalum metal scaffold).

[0078] Example 2

[0079] The multilayer bionic joint with a cell loading cavity is prepared by the following method:

[0080] (1) preparing a three-layer 3D printed bionic joint having a three-layer structure through steps 1) to 8) described in Example 1;

[0081] (2) The three-layer 3D printed bionic joint, which had been cross-linked in a 5% calcium chloride solution for 10 min, was placed in a mold to form a cell loading cavity on its outer surface.

[0082] Figure 5 It is a schematic diagram of the structure of a molding die for forming a cell loading chamber, wherein: Figure 5 A to C are the schematic diagram, top view and side view of the three-dimensional geometric model designed by drawing software. Figure 5 D is a physical picture of the titanium alloy finalizing mold after 3D printing based on the three-dimensional geometric model. When the software designs the finalizing mold, its size and shape are consistent with the three-dimensional geometric model of the bionic joint of the present invention (such as Figure 1The size and shape are the same as the three-dimensional geometric model of the bionic joint of the present invention, or the shape is the same but the size can take into account the thickness of the middle layer and the outer layer. When designing, the size (such as the inner diameter of the hemisphere) is larger than the outer diameter of the bionic joint after the three-layer printing is completed (or the same is also acceptable), but controlled within 5%.

[0083] like Figure 5 As shown, the shaping mold includes a support part and a shaping part that are integrally connected. The shaping part is a groove structure. The shape and size of the groove structure match the shape and size of the bionic joint. The inner side of the groove has a shaping structure formed by edges and recessed parts. When the three-layer printed bionic joint is placed in the groove of the shaping part, the shaping structure is imprinted on the outer surface of the three-layer printed bionic joint to form a cell loading cavity. The cell loading cavity formed is as shown in FIG. Figure 4 As shown, the cell loading cavity is formed by continuous ridges protruding outward from the outer surface of the bionic joint and grooves formed between the ridges. The thickness of the ridges is 0.3 mm, the height of the ridges is 1 mm, and the width of the grooves is 0.8 mm.

[0084] Example 3

[0085] A method for preparing a multi-layer bionic joint based on 3D printing comprises the following steps:

[0086] 1) According to the method described in steps 1) to 2) of Example 1, a porous tantalum metal powder is used as a matrix, and a porous tantalum metal hemispherical shell (such as Figure 1 );

[0087] The 3D printing conditions are as follows: the powder thickness is 30 μm, the laser power is 200 W, the exposure time is 70 μs, the laser scanning point spacing is 40 μm, and the line spacing is 40 μm; the porous tantalum metal powder is a medical-grade spherical powder with a purity of ≥99.99 wt% and a particle size of 30 μm; the protective gas is high-purity argon (purity ≥99.99%), and the oxygen content in the working chamber is less than 1000 ppm during the printing process;

[0088] 2) The printed parts are subjected to high-temperature heat treatment to eliminate the residual stress generated during the processing and to make the surface of the hemispherical shell smooth. The heat treatment temperature is 1250°C, the heating rate is 5°C / min, the temperature is kept for 1 hour, and the furnace is cooled;

[0089] 3) The heat-treated printed part is placed in a sandblasting machine for sandblasting to remove excess metal powder adhering to the surface; the abrasive used for sandblasting is white corundum, the particle size of white corundum is 50μm-150μm, the sandblasting force is 0.3MPa, and the sandblasting time is 40s;

[0090] 4) The printed part after sandblasting was ultrasonically cleaned with acetone, alcohol, and distilled water for 15 minutes respectively, and vacuum dried at 40° C. to obtain a 3D printed porous tantalum metal hemispherical shell (i.e., the inner layer of the bionic joint);

[0091] The 3D printed porous tantalum metal hemispherical shell is a porous structure, and the porous structure is provided with fixing holes, and the fixing holes are screw holes. There are 4 screw holes at the bottom of the hemispherical shell, and the screw hole diameter is 5mm. The screw hole is located at 0.5mm from the center plane of the hemisphere, and the direction is 30° with the center plane of the hemisphere. The screw hole on the hemispherical shell is a profile countersunk hole, which is convenient for screw fixation without irritating the surrounding tissues due to the protrusion of the screw (such as Figure 1 ). The hemispherical shell is an arc-shaped hemispherical shell with an outer diameter of 28 mm and a thickness of 1.5 mm. The porous structure is composed of an internally connected body-centered cubic pore structure with a porosity of 80% and a pore size of 600 μm. The actual size of the porous tantalum metal hemispherical shell produced by 3D printing is basically consistent with the computer design model;

[0092] The 3D printed porous tantalum metal hemispherical shell has a compressive strength of 50MPa, a flexural strength of 72MPa, and an elastic modulus of 3.1GPa;

[0093] 5) Using a drawing software to design a three-dimensional geometric model of a bioceramic scaffold, importing the three-dimensional geometric model, generating a printing path, and adjusting the bioprinter temperature to 20° C., the printing pressure to 0.22 MPa, the printing speed to 5 mm / s, the printing spacing to 0.7 mm, the printing layer thickness to 0.4 mm, and the needle tip compensation to 1.0 mm, the printing parameters are 3D printed according to the printing path, that is, the porous tantalum metal hemispherical shell obtained in step 4) is first placed on the printer platform, the printing program is started, and the bioceramic slurry is gradually printed onto the outer surface of the porous tantalum metal hemispherical shell, so that the bioceramic calcification layer can be closely attached to the outer side of the porous tantalum bionic trabecular bone hemisphere, generating a bionic joint intermediate layer, and obtaining a printed part I;

[0094] Preparation of bioceramic slurry: Hydroxyapatite (HAP) powder (particle size of 20 nm) and calcium sulfate powder are placed in a mixed solvent of glycerol and ultrapure water (the volume ratio of glycerol to ultrapure water is 5:5), and stirred for about 0.5 h by a stirrer with a rotation speed of 1500 rpm to prepare a slurry with a hydroxyapatite content of 20% and a calcium sulfate content of 20%; then sodium alginate is added to the slurry as a bioadhesive to prepare a slurry with a solid phase content of 1%, and stirred for about 1.5 h by a stirrer with a rotation speed of 2000 rpm, and degassed by centrifugation (rotation speed of 5000 rpm) for about 1 h, and then degassed by low-temperature degassing to obtain a bioactive bioceramic slurry; wherein the weight average molecular weight of sodium alginate is 12-190 KDa;

[0095] 6) Using mapping software to design a three-dimensional geometric model of the gelatin / sodium alginate composite hydrogel scaffold (outer layer), importing the three-dimensional geometric model data file, generating a printing path, and adjusting the printing parameters of the bioprinter: the printing temperature is 35° C., the printing pressure is 0.2 MPa, the printing speed is 10 mm / s, and the needle tip compensation parameter is 1 mm. 3D printing is performed according to the printing path, that is, the gelatin / sodium alginate composite hydrogel liquid is placed in the printing syringe, and the printing nozzle moves during printing to pull the ejected hydrogel liquid into a filament and deposit it on the outer surface of the porous bioceramic calcified layer of the print obtained in step 5), completing the printing, generating the outer layer of the bionic joint, and obtaining print part II;

[0096] Preparation of gelatin / sodium alginate composite hydrogel solution: fully dissolve gelatin (weight average molecular weight of 50-100KDa) at a temperature of 65°C and under magnetic stirring to prepare a gelatin solution with a mass concentration of 15%; add sodium alginate to the gelatin solution and fully dissolve it, wherein the mass concentration of sodium alginate is 5%, stir and mix evenly to prepare a gelatin / sodium alginate composite hydrogel solution; adjust the pH of the gelatin / sodium alginate composite hydrogel solution to 7.2-7.4;

[0097] 7) placing the printed part II obtained in step 6) in a pre-prepared 2% calcium chloride solution for cross-linking for 10 minutes, so that the gelatin / sodium alginate composite hydrogel scaffold is formed to obtain a 3D printed multi-layer bionic joint;

[0098] 8) Gently place the 3D printed multilayer bionic joint into a shaping mold, and form a cell loading cavity on the outer surface of the outermost gelatin / sodium alginate composite hydrogel layer (see Example 2 for the specific preparation method and shape), to obtain a 3D printed multilayer bionic joint with a cell loading cavity.

[0099] In the above step 5) and step 6), the method of generating the printing path is the same, and the method of generating the printing path is the same as that in embodiment 1.

[0100] The 3D printed multilayer bionic joint (such as Figure 4 ), placed in a cell culture medium, and autologous chondrocytes were added dropwise into the cell loading cavity on the outer surface; the density of the autologous chondrocytes was 8×10 7 The printed part was placed in a new culture well plate the next morning. The printed part was flipped 180° and autologous bone marrow mesenchymal stem cells were inoculated on the inner porous tantalum metal bionic trabeculae in the opposite direction. The cell inoculation concentration was 5×10 7 / ml; remove the culture medium in the morning of the next day. Replace the new culture medium and continue to culture. After 7 days of in vitro culture, the cells can completely penetrate into the printed material. When the cell-infiltrated print is implanted into the joint defect, the 3D-printed gelatin / sodium alginate hydrogel can simulate the special three-dimensional microenvironment required for chondrocyte growth and construct a mechanical environment similar to that of natural articular cartilage, which is conducive to repair. The internal pores of the 3D-printed porous tantalum metal have been filled with bone marrow mesenchymal stem cells. The interface of the solid bioceramic calcified layer in the middle of the print can effectively carry out the cell barrier effect between bone and cartilage and the interlayer connection effect of tissue.

[0101] Example 4

[0102] A method for preparing a multi-layer bionic joint based on 3D printing comprises the following steps:

[0103] 1) According to the method described in steps 1) to 2) of Example 1, a porous carbon metal powder is used as a matrix to obtain a porous tantalum metal hemispherical shell by 3D printing;

[0104] The 3D printing conditions are as follows: the powder thickness is 30 μm, the laser power is 200 W, the exposure time is 70 μs, the laser scanning point spacing is 35 μm, and the line spacing is 35 μm; the porous tantalum metal powder is a medical-grade spherical powder with a purity of ≥99.99 wt% and a particle size of 30 μm; the protective gas is high-purity argon (purity ≥99.99%), and the oxygen content in the working chamber is less than 1000 ppm during the printing process;

[0105] 2) The printed parts are subjected to high-temperature heat treatment to eliminate the residual stress generated during the processing and to make the surface of the hemispherical shell smooth. The heat treatment temperature is 1250°C, the heating rate is 5°C / min, the temperature is kept for 1 hour, and the furnace is cooled;

[0106] 3) The heat-treated printed part is placed in a sandblasting machine for sandblasting to remove excess metal powder adhering to the surface; the abrasive used for sandblasting is white corundum, the particle size of white corundum is 50μm-150μm, the sandblasting force is 0.3MPa, and the sandblasting time is 40s;

[0107] 4) The printed part after sandblasting was ultrasonically cleaned with acetone, alcohol, and distilled water for 15 minutes respectively, and vacuum dried at 40° C. to obtain a 3D printed porous tantalum metal hemispherical shell (i.e., the inner layer of the bionic joint);

[0108] The 3D printed porous tantalum metal hemispherical shell is a porous structure, and the porous structure is provided with fixing holes, which are screw holes. There are 2 screw holes at the bottom of the hemispherical shell, and the screw hole diameter is 5mm. The screw hole is located at 0.8mm from the center plane of the hemisphere, and the direction is 50° with the center plane of the hemisphere. The screw hole on the hemispherical shell is a profile countersunk hole, which is convenient for screw fixation without irritating the surrounding tissue due to the protrusion of the screw. The hemispherical shell is an arc-shaped hemispherical shell, with an inner diameter of 32mm and a thickness of 1.5mm. The porous structure is composed of an internally connected diamond-shaped pore structure, with a porosity of 85% and a pore size of 750μm; the actual size of the porous tantalum metal hemispherical shell produced by 3D printing is basically consistent with the computer design model;

[0109] The 3D printed porous tantalum metal hemispherical shell has a compressive strength of 58MPa, a flexural strength of 80MPa, and an elastic modulus of 3.3GPa;

[0110] 5) Using a drawing software to design a three-dimensional geometric model of a bioceramic scaffold, importing the three-dimensional geometric model, generating a printing path and adjusting the bioprinter temperature to 20° C., the printing pressure to 0.18 MPa, the printing speed to 3 mm / s, the printing spacing to 0.5 mm, the layer thickness to 0.32 mm, and the needle tip compensation to 1.5 mm, the printing parameters, and performing 3D printing according to the generated printing path, that is, placing the porous tantalum metal hemispherical shell obtained in step 4) on the printer platform, starting the printing program, and gradually printing the bioceramic slurry onto the outer surface of the porous tantalum metal hemispherical shell, so that the bioceramic calcification layer can be closely attached to the outer side of the porous tantalum bionic trabecular bone hemisphere, generating a bionic joint intermediate layer, and obtaining a printed part I;

[0111] The method for generating the printing path is: using the layering software provided by the device to slice the three-dimensional geometric model designed by the three-dimensional design software, and cutting the model into a plurality of curved surfaces, wherein the curved surface is a porous curved surface with a grid composed of curves arranged at intervals (such as Figure 2 B). When printing, the printer's nozzle will print the material into a specific surface along the path of the generated curve, and the final 3D model will be composed of stacked surfaces ( Figure 2 ).

[0112] Preparation of bioceramic slurry: Calcium sulfate powder is placed in a mixed solvent of glycerol and ultrapure water (the volume ratio of glycerol to ultrapure water is 5:5), and stirred for about 0.5 h by a stirrer with a rotation speed of 1000 rpm to prepare a slurry with a solid content of 50%; then sodium alginate is added to the slurry as a bioadhesive to prepare a slurry with a solid content of 3%, and stirred for about 2 h by a stirrer with a rotation speed of 2000 rpm, and degassed by centrifugation (rotation speed is 5000 rpm) for about 1 h, and then degassed by low temperature to obtain a bioactive bioceramic slurry; wherein the weight average molecular weight of sodium alginate is 12-190 KDa;

[0113] 6) Use Creo graphics software to design and obtain the 3D geometric model of the gelatin / sodium alginate composite hydrogel scaffold (outer layer), import the 3D geometric model data file, generate the printing path, and adjust the printing parameters of the bioprinter: the printing temperature is 40°C, the printing pressure is 0.4MPa, the printing speed is 8mm / s, the needle tip compensation parameter is 1.5mm, and 3D printing is performed according to the printing path, that is, the protein / gelatin / sodium alginate composite hydrogel liquid is placed in the printing syringe, and the printing nozzle moves during printing to pull the ejected hydrogel liquid into filaments and deposit them on the step 5) On the outer surface of the porous bioceramic calcified layer of the obtained print part I, complete printing to generate the outer layer of the bionic joint, and obtain print part II; wherein, the method for generating the printing path is the same as step 5); Preparation of protein / gelatin / sodium alginate composite hydrogel liquid: under sterile conditions, at a temperature of 65°C and magnetic stirring, fully dissolve gelatin (weight average molecular weight of 50-100KDa) to prepare a gelatin solution with a mass concentration of 10%; add sodium alginate to the gelatin solution and fully dissolve it, wherein the mass concentration of sodium alginate is 2%, and stir and mix evenly. It is composed of 10 parts of sodium alginate and 0.1 parts of growth factor protein (or fibroblast growth factor protein) by weight. The protein / gelatin / sodium alginate composite hydrogel liquid is prepared by low-speed centrifugation to remove bubbles;

[0114] 7) The printed part II obtained in step 6) is placed in a pre-prepared 5% calcium chloride solution for cross-linking for 10 minutes to form the gelatin / sodium alginate composite hydrogel scaffold and obtain a multi-layer bionic joint loaded with protein.

[0115] Example 5

[0116] The repairing effect of the multi-layer bionic joint of the present invention on large-area femoral head defects:

[0117] A 3D printed three-layer bionic joint (joint prosthesis) was prepared by the method of Example 1. The difference from Example 1 is that only one fixing hole is provided in the hemispherical shell.

[0118] 12-month-old goats weighing 30-40kg were given a mixture of ketamine and lumianning (2:1) and injected intramuscularly at 0.5ml / kg. After successful anesthesia, the greater trochanter of the right hind limb of the goat was used as the center for local shaving, skin preparation, iodine disinfection, and sterile towels. A surgical incision of about 5 cm was made with the femoral head as the center. The anterolateral incision of the right hip joint was made, and the skin, subcutaneous tissue and fascia lata were cut layer by layer. Part of the gluteal muscle was cut, and blunt separation was performed after exposure to expose the joint capsule. The joint capsule was cut in a "cross" shape, the round ligament of the femoral head was cut, and the femoral head was dislocated to expose the femoral head. The femoral head defect model was made according to the size of the joint prosthesis ( Figure 6 A), after proper installation ( Figure 6 B) uses a tantalum metal screw to fix the joint prosthesis ( Figure 6 C). Then the joint capsule, gluteus medius, subcutaneous tissue and skin were sutured in sequence, the incision was closed, and the surgical area was disinfected again. 800,000 U / d of penicillin was injected intramuscularly 30 minutes before surgery and 3 days after surgery to prevent infection. The external fixator was removed 6 weeks later and X-rays were taken ( Figure 6 D), X-ray results showed that the porous tantalum metal was well integrated with the surrounding bone tissue without dislocation or collapse.

[0119] Six weeks after surgery, the goats were killed and the femoral head specimens were taken for gross observation. The results showed that the repair area was flat, uniform in color, well connected with the surrounding normal tissues, and without gaps. Next, a histological evaluation was performed: specimens of the defect repair area were cut out. Because the repair area contained tantalum metal, hard tissue sections and VG staining were performed to observe the repair of the articular osteochondral defect. The results showed that the interface between bone and cartilage was well integrated without faults, and the cartilage defect area and the internal area of ​​tantalum metal were filled with new tissue ( Figure 7 A), Figure 7 The upper area in A (marked by the letter i) is the new cartilage layer, and the lower black area (marked by the letter ii) is the tantalum metal. VG staining shows that 6 weeks after implantation, the internal tissue of the porous tantalum metal is new osteoid ( Figure 7 B), Figure 7 The area in B (marked with letter i) is new osteoid.

[0120] The specimens of the cartilage repair area were cut, fixed with 40g / L paraformaldehyde, embedded in wax blocks, and sliced ​​at 5μm. After dewaxing, immunohistochemical staining of type II collagen and type I collagen was performed to observe the repair of articular cartilage defects. The results showed that the cartilage surface was smooth, the chondrocytes were round or oval, encapsulated in the cartilage pits, and arranged in a columnar orientation, perpendicular to the cartilage surface, and showed obvious expression of type II collagen ( Figure 7 C) but not type I collagen expression ( Figure 7 D), indicating that the new tissue is cartilage tissue.

[0121] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A multi-layer bionic joint, characterized in that: The multi-layer bionic joint is formed by closely contacting an inner layer, a middle layer and an outer layer in the order of an inner layer, a porous tantalum metal scaffold, a solid bioceramic scaffold, and a solid gelatin / sodium alginate composite hydrogel scaffold. The inner layer, the middle layer and the outer layer are all in an arc-shaped shell structure, and the arc of the arc-shaped shell is 120-240°. A cell loading cavity is formed on the surface of the outer layer, and the cell loading cavity is composed of continuous or discontinuous edges protruding outward from the surface of the outer layer and grooves formed between the edges. The inner layer is made of tantalum metal powder as a base material through metal 3D printing, the middle layer is made of bioceramic slurry as a base material deposited on the outer surface of the inner layer through bio 3D printing, and the outer layer is made of gelatin / sodium alginate composite hydrogel liquid as a base material deposited on the outer surface of the middle layer through bio 3D printing. The thickness of the rib is 0.2-0.4 mm, the height of the rib is 0.8-1.2 mm, and the width of the groove is 0.7-1 mm. The inner diameter of the arc-shaped shell is 20-40 mm, the thickness of the porous tantalum metal stent is 1-3 mm, the thickness of the solid bioceramic stent is 0.3-0.5 mm, and the thickness of the solid gelatin / sodium alginate composite hydrogel stent is 2-3 mm.

2. The multi-layer bionic joint according to claim 1, characterized in that: The bioceramic is composed of hydroxyapatite, calcium sulfate or a mixture of the two.

3. The method for preparing the multi-layer bionic joint according to claim 1 or 2, comprising the following steps: (1) Using 3D design software, the 3D geometric models of the inner layer, middle layer, and outer layer of the multi-layer bionic joint are designed respectively; (2) According to the three-dimensional geometric model of the inner layer of the multilayer bionic joint obtained in step (1), tantalum metal powder is used as the substrate, and metal 3D printing is performed under argon environment protection to obtain a porous tantalum metal stent print; wherein the process parameters of the 3D printing are: powder thickness of 30-50 μm, laser power of 100-200 W, exposure time of 40-70 μs, laser scanning point spacing of 30-60 μm, and line spacing of 30-60 μm; (3) The porous tantalum metal bracket printed part obtained in step (2) is subjected to heat treatment, followed by sandblasting, cleaning, and drying to obtain a multi-layer bionic joint inner layer, wherein: The heat treatment conditions are: heating rate of 5°C / min, heating to 1200-2000°C, and keeping warm for 1 hour; the sandblasting conditions are: force of 0.1-1MPa, and treatment time of 30-120s; (4) According to the three-dimensional geometric model of the multi-layer bionic joint middle layer obtained in step (1), the bioceramic slurry is printed onto the outer surface of the multi-layer bionic joint inner layer obtained in step (3) by bio-3D printing according to the printing path, so as to generate a multi-layer bionic joint middle layer and obtain a printed part I, wherein the 3D printing conditions are: printing temperature of 15-20° C., printing pressure of 0.18-0.22 MPa, printing speed of 3-7 mm / s, printing spacing of 0.5-1 mm, needle tip compensation parameter of 1-2 mm, printing layer thickness of 0.3-0.5 mm, and the printing nozzle is moved during printing to pull the extruded bioceramic slurry into a filament shape and deposit it onto the outer surface of the multi-layer bionic joint inner layer, and the printing is completed according to the printing path; (5) According to the three-dimensional geometric model of the multi-layer bionic joint outer layer obtained in step (1), the gelatin / sodium alginate composite hydrogel liquid is printed on the outer surface of the multi-layer bionic joint middle layer in the printed part I obtained in step (4) according to the printing path by biological 3D printing, so as to generate a multi-layer bionic joint outer layer and obtain a printed part II, wherein the 3D printing conditions are: printing temperature of 25-40°C, printing pressure of 0.1-0.4MPa, printing speed of 5-20mm / s, needle tip compensation parameter of 1-2mm, and the printing nozzle moves during printing to draw the ejected composite hydrogel liquid into filaments and deposit them on the outer surface of the multi-layer bionic joint middle layer to complete the printing; (6) placing the printed part II obtained in step (5) in a divalent ion solution for cross-linking; (7) The cross-linked printed part II is placed into a molding mold to form a cell loading cavity on the outer surface of the printed part II.

4. The preparation method according to claim 3, characterized in that: The shaping mold has a groove structure, and the outer layer of the printed part II contacts the surface of the shaping mold having the groove, thereby forming a cell loading cavity on the surface of the outer layer.

5. The preparation method according to claim 3, characterized in that: In step (5), a chondrogenesis-promoting factor is added to the gelatin / sodium alginate composite hydrogel solution, and the added amount is 0.1-1% of the mass of the gelatin / sodium alginate composite hydrogel solution.

6. The preparation method according to claim 3, characterized in that: The inner layer and outer layer of the multilayer bionic joint obtained in step (7) are inoculated with bone marrow mesenchymal stem cells and chondrocytes respectively.

7. Use of the multi-layer bionic joint as claimed in claim 1 or 2 in preparing a repair implant for repairing large-area osteochondral syndesmotic defects.