Catalyst composite for fuel cell, method for producing the same, and electrode

By using a catalyst composite of iridium compounds and platinum supported on a carbon support in fuel cells, the problems of water overflow and voltage reversal under high current density were solved, improving the battery's tolerance and lifespan and reducing replacement costs.

CN112151811BActive Publication Date: 2024-11-01HYUNDAI MOTOR CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010306335.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-27
Filing Date
2020-04-17
Publication Date
2024-11-01
Estimated Expiration
2040-04-17

AI Technical Summary

Technical Problem

Existing polymer electrolyte membrane fuel cells are prone to water overflow and voltage reversal at high current densities, which can obstruct the supply of reactant gases and affect battery performance and lifespan.

Method used

A catalyst complex in which iridium compounds and platinum are supported on a carbon support to form a highly dispersed structure is used to prepare the catalyst by adjusting the pH and heat treatment, thereby improving the electroconnectivity and water splitting activity.

Benefits of technology

It enhances the voltage reversal tolerance of fuel cells, stabilizes voltage reversal control, extends the life of fuel cell stacks, and reduces replacement costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112151811B_ABST
    Figure CN112151811B_ABST
Patent Text Reader

Abstract

Disclosed are a catalyst composite for a fuel cell, a method for manufacturing the same, and an electrode. A catalyst composite for a fuel cell. The catalyst composite includes a carrier, the carrier includes carbon (C), platinum (Pt) supported on the carrier, and an iridium (Ir) compound supported on the carrier, and the iridium compound includes a chemical formula of 1IrO x Iridium oxide represented by the chemical formula 2IrMO x At least one of the iridium transition metal oxides represented by, wherein M is a transition metal selected from the group consisting of Fe, Co, Cu, Ni and a combination thereof, and x is 1 to 2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalyst composite for a fuel cell and a method for producing the same. Background Art

[0002] Generally, polymer electrolyte membrane fuel cells (PEMFCs) have been applied in fuel cells for vehicles. The PEMFCs must stably operate in a wide current density range in order to exhibit normal high power output performance of at least several tens of kW under various operating conditions encountered in vehicles.

[0003] Typically, polymer electrolyte membrane fuel cells have been used in the form of a stack assembled by stacking unit cells to meet the required power output level. In addition, a membrane electrode assembly (MEA) is located at the innermost position of the unit cell structure of the fuel cell stack, and the membrane electrode assembly (MEA) may include an electrolyte membrane capable of moving protons, and an anode and a cathode applied to the respective sides of the electrolyte membrane. Hereinafter, the term "fuel cell" may refer to a polymer electrolyte membrane fuel cell.

[0004] In addition, a gas diffusion layer (GDL) and a gasket are stacked outside the MEA, that is, at the outer portion where the anode and cathode are located, and a separator or bipolar plate providing a flow field can be joined to the outside of the gas diffusion layer (GDL), and the reaction gas, cooling water and water generated by the reaction flow can flow through the flow field. In the electrochemical reaction of power generation by the polymer electrolyte membrane fuel cell, hydrogen supplied to the anode as the oxidation electrode of the fuel cell is separated into protons and electrons, after which the protons move to the cathode as the reduction electrode through the polymer electrolyte membrane, and the electrons move to the cathode through the external circuit, and at the cathode, oxygen molecules, protons and electrons react together to generate electricity and heat and water as a reaction byproduct. Although the appropriate amount of water generated during the electrochemical reaction in the fuel cell plays a desired role in maintaining the humidity of the membrane electrode assembly (MEA), if excessive water is generated and not properly removed, "overflow" or "flooding" of water occurs at high current density, and this overflowing water prevents the reaction gas from being effectively supplied to the fuel cell, undesirably further increasing the voltage loss. Summary of the invention

[0005] In a preferred aspect, a catalyst composite included in a membrane electrode assembly (MEA) is provided, which may be a highly dispersed high-activity voltage reversal catalyst, thereby improving an irreversible voltage reversal phenomenon.

[0006] In a preferred aspect, a catalyst composite is provided, wherein IrO xand Pt can be loaded together on a carbon support, and a highly dispersed structure can be formed, which is different from the conventional electrode structure. x The distribution is restricted.

[0007] The purpose of the present invention is not limited to the above contents, and other specific contents of the present invention are incorporated in the following description and drawings.

[0008] In one aspect, a catalyst composite that can be included in an electrode for a fuel cell is provided. The catalyst composite may include: a carrier including carbon (C); platinum (Pt) supported on the carrier; and an iridium (Ir) compound supported on the carrier. The iridium compound may include at least one of iridium oxide represented by the following chemical formula 1 and transition metal iridium oxide represented by the following chemical formula 2.

[0009] [Chemical formula 1]

[0010] Ir x

[0011] [Chemical formula 2]

[0012] IrMO x

[0013] Here, M is a transition metal selected from the group consisting of Fe, Co, Cu, Ni, and a combination thereof, and x is 1 to 2.

[0014] The weight ratio of platinum (Pt) and iridium (Ir) in iridium oxide may be appropriately about 1:0.5 to 1:1.

[0015] The weight ratio of platinum (Pt) and iridium (Ir) in the iridium transition metal oxide may be appropriately about 1:0.5 to 1:1, and the atomic ratio of platinum (Pt) and transition metal (M) in the iridium transition metal oxide may be appropriately about 1:1 to 1:5.

[0016] In one aspect, a method for manufacturing a catalyst composite included in an electrode for a fuel cell is provided. The method may include: preparing a starting solution including a platinum-loaded carrier and an iridium precursor added to a solvent; obtaining an intermediate product including the platinum-loaded carrier and iridium particles by heat treating the starting solution; loading the iridium particles on the platinum-loaded carrier by adjusting the pH of the intermediate product; drying the obtained product; and iridium oxide particles.

[0017] When preparing the starting solution, the solvent may be adjusted to a basic pH.

[0018] The intermediate product can be suitably obtained by heat-treating the starting solution at a temperature of about 100° C. to 200° C. for about 1 hour to 5 hours in an inert atmosphere.

[0019] The intermediate product may be acidic in the pH range of about 0.5 to 3.0, and thus the iridium particles may be supported on the platinum-supported support.

[0020] The iridium particles may be oxidized by heat-treating the dried product at a temperature of about 200° C. to 400° C. for about 1 hour to 5 hours in air.

[0021] The starting solution may further include a transition metal precursor, and thus the intermediate product may include a platinum-loaded support, iridium particles, and transition metal particles.

[0022] The pH of the intermediate product may be adjusted so that the iridium particles and the transition metal particles are supported on the platinum-supported carrier, the resulting product may be dried, and the iridium particles and the transition metal particles may be oxidized.

[0023] In one aspect, a method for manufacturing a catalyst composite included in an electrode for a fuel cell is provided. The method may include: preparing a starting solution including an iridium precursor added to a solvent; obtaining an intermediate product including iridium particles by heat treating the starting solution; adding a platinum-loaded carrier to the intermediate product, and loading the iridium particles on the platinum-loaded carrier by adjusting the pH of the intermediate product; drying the obtained product; and iridium oxide particles.

[0024] When preparing the starting solution, the solvent may be adjusted to a basic pH.

[0025] The intermediate product can be obtained by heat-treating the starting solution at a temperature of about 100° C. to 200° C. for about 1 hour to 5 hours in an inert atmosphere.

[0026] The intermediate product may include a platinum-loaded support, and then the intermediate product may be made acidic within a pH range of about 0.5 to 3.0, and thus iridium particles may be loaded on the platinum-loaded support.

[0027] The iridium particles may be oxidized by heat-treating the dried product at a temperature of about 200° C. to 400° C. in air for about 1 hour to 5 hours.

[0028] The starting solution may further include a transition metal precursor, so the intermediate product may include iridium particles, transition metal particles and a carrier loaded with platinum. For example, the intermediate product including iridium particles and transition metal particles may be added with a carrier loaded with platinum. The pH of the intermediate product may be adjusted so that the iridium particles and transition metal particles are loaded on a carrier loaded with platinum, the resulting product may be dried, and the iridium particles and transition metal particles may be oxidized.

[0029] Further provided are electrodes comprising the catalyst composites described herein.For example, the catalyst composites can be made by the methods described herein.

[0030] In the catalyst composite for a fuel cell and the method for manufacturing the same according to various exemplary embodiments of the present invention, the iridium compound may be supported on the platinum-supported carbon support, thereby exhibiting excellent electrical connectivity and improving catalytic activity due to its uniform distribution on the carbon support.

[0031] In addition, voltage reversal tolerance can be enhanced by increasing electrical connectivity and water splitting activity upon voltage reversal in a fuel cell.

[0032] Therefore, when voltage reversal occurs in the fuel cell, the voltage reversal can be stably controlled compared to conventional cases, so that the life of the fuel cell stack can be increased, and cost reduction can also be achieved by reducing replacement cost.

[0033] The effects of the present invention are not limited to the foregoing, and should be understood to include all effects that can be reasonably expected from the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 shows a control logic when a voltage drop occurs during operation of a fuel cell according to conventional technology;

[0035] Figure 2 A conventional catalyst for a fuel cell is schematically shown;

[0036] Figure 3 schematically illustrates an exemplary catalyst composite for an exemplary fuel cell according to an exemplary embodiment of the present invention;

[0037] Figure 4 is a flow chart showing an exemplary manufacturing process of an exemplary catalyst composite for an exemplary fuel cell according to an exemplary embodiment of the present invention;

[0038] Figure 5 schematically illustrates an exemplary manufacturing process of an exemplary catalyst composite for an exemplary fuel cell according to an exemplary embodiment of the present invention;

[0039] Figure 6 is a graph showing the results of voltage reversal time of Example 1, Comparative Example 1, and Comparative Example 2;

[0040] Figure 7 is a graph showing the results of voltage reversal time of Example 1 and Example 2;

[0041] Figure 8 is a graph showing the results of voltage reversal time of Examples 1 to 4;

[0042] Fig. 9 is a graph showing the results of voltage reversal time of Examples 4 to 7;

[0043] Fig.10 and Fig.11 shows the distribution of iridium compounds in catalyst composites used in fuel cells of comparative examples and examples;

[0044] Fig.12 is a graph showing the results of voltage reversal time of Example 1 and Comparative Example 6;

[0045] Fig.13 is a graph showing the results of voltage reversal time of Example 1 and Comparative Examples 3 to 5; and

[0046] Fig.14 Results of measuring the water-splitting activity of the catalyst composite of each of Comparative Example 2 and Examples 8 to 13 by a half-electrode test are shown. DETAILED DESCRIPTION

[0047] From the following preferred embodiments in conjunction with the accompanying drawings, the above and other purposes, features and advantages of the present invention will be more clearly understood. However, the present invention is not limited to the embodiments disclosed herein and can be modified into different forms. These embodiments are provided to thoroughly explain the present invention and fully convey the spirit of the present invention to those skilled in the art.

[0048] Throughout the accompanying drawings, the same reference numerals will refer to the same or similar elements. For clarity of the present invention, the size of the structure is described as being larger than its actual size. It should be understood that although various elements can be described herein using terms such as "first", "second", etc., these elements are not limited by these terms. These terms are only used to distinguish one element from another element. For example, without departing from the scope of the present invention, the "first" element discussed below may be referred to as the "second" element. Similarly, the "second" element may also be referred to as the "first" element. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form.

[0049] It will be further understood that when used in this specification, the terms "comprise", "include", "having", etc. specify the presence of the features, integers, steps, operations, elements, components, or combinations thereof, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, or combinations thereof. In addition, it should be understood that when an element such as a layer, film, region, or sheet is referred to as being "on" another element, it can be directly on the other element, or there can be intervening elements between them. Similarly, when an element such as a layer, film, region, or sheet is referred to as being "under" another element, it can be directly under the other element, or there can be intervening elements between them.

[0050] Unless otherwise indicated, all numbers, values ​​and / or representations representing the amounts of components, reaction conditions, polymer compositions and mixtures used herein should be considered approximate, including various uncertainties affecting the measurements that occur substantially when obtaining these values, and therefore should be understood to be modified by the term "about" in all cases. In addition, when a numerical range is disclosed in this specification, unless otherwise indicated, the range is continuous and includes all values ​​from the minimum value of the range to its maximum value. In addition, when such a range involves integer values, unless otherwise indicated, all integers including the minimum value to the maximum value are included.

[0051] Unless specifically stated or obvious from the context, as used herein, the term "about" should be understood to be within the normal tolerance range in the art, such as within 2 standard deviations of the mean. "About" can be understood to be within 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, 0.1%, 0.05% or 0.01% of the specified value. Unless otherwise clearly indicated from the context, all numerical values ​​provided herein are modified by the term "about".

[0052] Hereinafter, a detailed description of the present invention will be given with reference to the accompanying drawings.

[0053] Figure 1 A control logic when a voltage drop occurs during operation of a fuel cell according to conventional technology is shown.

[0054] like Figure 1 As shown, control logic can be applied when the battery performance is reversibly restored, such as the water-flooding phenomenon, in which the battery performance is degraded due to the accumulation or accumulation of water in the fuel cell stack hindering the flow of the reactant gases (hydrogen and oxygen in the air). However, its application may be limited to irreversible degradation modes. For example, the cell voltage reversal may be caused by hydrogen fuel starvation, in which the anode for the fuel cell lacks hydrogen fuel due to various reasons such as water flooding in the fuel cell, ice formation in winter, and abnormalities of the hydrogen fuel supply device.

[0055] As reported in the prior art, the occurrence of voltage reversal is known to significantly reduce the cell voltage by adversely affecting the performance of the fuel cell.

[0056] Generally, hydrogen fuel starvation can be broadly classified into overall hydrogen starvation, in which the hydrogen supply in the entire fuel cell becomes insufficient, and local hydrogen starvation, in which the overall hydrogen supply of the cell is sufficient, but a partial hydrogen supply shortage occurs due to an uneven distribution of the hydrogen supply. Hydrogen fuel starvation may occur frequently under operating conditions such as uneven supply and distribution of hydrogen, sudden increase in fuel cell load requirements, and fuel cell startup. For example, when the anode lacks hydrogen, the anode voltage (V anode ) increases. However, when the anode voltage continues to increase, the anode voltage is greater than the cathode voltage (V cathode ) increases more, resulting in the battery voltage (V cell ) becomes less than zero voltage reversal state (V cell =V cathode -V anode <0). Under the voltage reversal state, due to the increase of anode voltage, water electrolysis reaction occurs first, as shown in the following Scheme 1.

[0057] [Solution 1]

[0058] H 2 O→1 / 2O 2 +2H + +2e - ,E o =1.229V(vs.SHE)

[0059] (Among them, E o is the standard electrode potential, and SHE is the standard hydrogen electrode)

[0060] However, as the anode voltage continues to increase, the carbon corrosion reaction at the anode accelerates, as shown in Schemes 2 and 3 below.

[0061] [Solution 2]

[0062] C+2H 2 O→CO 2 +4H + +4e - ,E o =0.207V(vs.SHE)

[0063] [Solution 3]

[0064] C+H 2 O→CO+2H + +2e - ,E o =0.518V(vs.SHE)

[0065] When the cell voltage reversal continues and thus reaches an overvoltage reversal state in which the cell voltage is less than about -2V, the heat generation in the fuel cell becomes excessive, so that the membrane electrode assembly (MEA) and the gas diffusion layer (GDL) may be damaged. Specifically, pinholes are formed in the membrane electrode assembly (MEA). In addition, there may be a problem of the cell being electrically short-circuited. In this case, a cell failure may result in the fuel cell not being able to operate normally. Therefore, by monitoring the hydrogen supply status using sensors in the fuel cell operating system ("Balance of Plant"), overall hydrogen deficiency can be detected relatively easily, but local hydrogen deficiency in some cells can only be detected by closely monitoring each cell of the fuel cell stack using a stack voltage monitoring device, so additional measures, such as a complex control system, are required. Therefore, it is necessary to fundamentally solve the above phenomenon. Conventionally, RuO has been used. 2 、IrO 2 、TiO 2 etc. are added to the anode to induce water decomposition reaction instead of carbon corrosion reaction. From the aspect of alleviating voltage reversal, RuO 2 、IrO 2 and TiO 2 However, considering the performance and durability of the catalyst, it is preferred to mainly use IrO 2 .

[0066] In order to realize a more stable hydrogen electric vehicle, it is necessary to simply replace IrO 2 The catalyst composite according to an exemplary embodiment of the present invention may exhibit high activity of a voltage reversal catalyst and excellent resistance to voltage reversal when added to an electrode.

[0067] The following is a description of the catalyst composite for a fuel cell according to the present invention compared with conventional catalysts.

[0068] Figure 2 A schematic diagram of a conventional catalyst used in a fuel cell. Figure 3 An exemplary catalyst composite for an exemplary fuel cell according to an exemplary embodiment of the present invention is schematically illustrated.

[0069] like Figure 2 As shown, in conventional technology, an electrode (such as an anode) can be formed by adding iridium oxide (IrO 2) 5 is mixed with a catalyst (i.e., Pt / C) configured such that platinum 20 is supported on a carbon support 30. Therefore, iridium oxide 5 aggregates or exists in a form separated from the carbon support (Pt / C) supporting platinum, thereby limiting the electrochemical water decomposition activity of iridium oxide 5. Therefore, a fuel cell including the above catalyst may cause degradation due to voltage reversal during its operation.

[0070] According to an exemplary embodiment of the present invention, Figure 3 As shown, the catalyst composite may be configured such that platinum 20 and an iridium compound 100 (e.g., iridium oxide (IrO x )) can be supported together on the carbon support 30. In addition to iridium oxide (IrO x ) In addition, iridium transition metal oxide can also be supported on the carbon support 30 together with platinum 20.

[0071] The catalyst composite included in the electrode for a fuel cell according to an exemplary embodiment of the present invention may include: a carrier 30 including carbon (C); platinum 20 supported on the carrier 30 ; and an iridium (Ir) compound 100 supported on the carrier 30 .

[0072] The iridium compound 100 may appropriately include at least one of iridium oxide represented by the following Chemical Formula 1 and iridium transition metal oxide represented by the following Chemical Formula 2.

[0073] [Chemical formula 1]

[0074] Ir x

[0075] [Chemical formula 2]

[0076] IrMO x

[0077] Here, M is a transition metal selected from the group consisting of Fe, Co, Cu, Ni, and a combination thereof, and x is 1 to 2.

[0078] Therefore, the carbon support 30 (for example, a carbon support supporting iridium oxide and platinum (Pt—IrO x / C)), the iridium compound 100 (for example, iridium oxide (IrO x )) can be loaded on the carbon support 30, thereby exhibiting excellent electrical connectivity, and can also be uniformly distributed on the carbon support 30, thereby increasing the catalytic activity compared to conventional cases.

[0079] For example, when the iridium compound 100 includes iridium oxide (IrO x), the weight ratio of platinum (Pt) to iridium (Ir) may appropriately fall within the range of, for example, about 1:0.5 to 1:1.

[0080] In addition, for example, when the iridium compound 100 includes an iridium transition metal oxide (IrMO x ), the weight ratio of platinum (Pt) and iridium (Ir) may appropriately fall within the range of, for example, about 1:0.5 to 1:1. In addition, the atomic ratio of platinum (Pt) and transition metal (M) may appropriately fall within the range of, for example, about 1:1 to 1:5.

[0081] Figure 4 A manufacturing process of a catalyst composite for a fuel cell according to an exemplary embodiment of the present invention is shown.

[0082] like Figure 4 As shown, the method for manufacturing a catalyst composite according to an exemplary embodiment of the present invention may include: preparing a starting solution by adding a platinum-loaded carbon support (Pt / C) and an iridium precursor to a solvent (S10); obtaining an intermediate product including Pt / C and iridium particles by heat-treating the starting solution (S20); loading the iridium particles on the Pt / C by adjusting the pH of the intermediate product (S30); drying the obtained product (S40); and iridium oxide particles (S50).

[0083] When preparing the starting solution ( S10 ), the solvent is not particularly limited, and may appropriately include, for example, ethylene glycol (EG).

[0084] When preparing the starting solution ( S10 ), Pt / C may be placed in a container having a predetermined shape and volume, and then a small amount of solvent may be added thereto, which may prevent Pt oxidation of the Pt / C.

[0085] The iridium precursor is not particularly limited and may suitably include, for example, iridium (III) chloride hydrate (IrCl 3 ·xH 2 O).

[0086] When preparing the starting solution (S10), the solvent may be adjusted to an alkaline pH. For example, the pH of the solvent may be about 10 or more, and preferably about 12.

[0087] The preparation of the starting solution (S10) may be performed in the following manner: a solvent is placed in a container containing Pt / C, and then sodium hydroxide (NaOH) used as a pH adjuster is added thereto so that the solvent is alkaline, after which an iridium precursor may be added thereto. For example, the iridium precursor may be mixed with sodium acetate (CH 3 COONa) was added together.

[0088] When the intermediate product ( S20 ) is obtained, the starting solution may be heat-treated in an inert atmosphere, and thus the iridium precursor may form iridium particles.

[0089] The inert gas is not particularly limited and may include, for example, nitrogen (N 2 ).

[0090] The intermediate product may suitably include Pt / C and iridium particles. Here, the iridium particles may not be supported on Pt / C. As used herein, the term "supported" refers to that the catalyst metal is firmly fixed on a carrier. In the intermediate product, the iridium particles may not be supported on Pt / C, and some iridium particles may be in physical contact with Pt / C.

[0091] When obtaining the intermediate product ( S20 ), the starting solution may be heat-treated at a temperature of about 100° C. to 200° C. for about 1 to 5 hours in an atmosphere purged with an inert gas.

[0092] Here, the heat treatment can be performed in the following manner: the starting solution is gradually heated from room temperature to the desired temperature, or the starting solution is placed in a constant temperature bath preset to the desired temperature. Preferably, the heat treatment can be performed by the previous process. In the previous process, the voltage reversal time can be about 80 minutes longer than the latter process.

[0093] When the iridium particles are loaded (S30), the pH of the intermediate product may be adjusted, and thus the iridium particles may be loaded on Pt / C. For example, the intermediate product may be adjusted to an acidic pH of about 0.5 to 3.0, and thus the iridium particles may be loaded on Pt / C.

[0094] The process of adjusting the pH of the intermediate product is not particularly limited, and may include, for example, adding a hydrochloric acid (HCl) solution and an acetic acid (CH 3 COOH) solution.

[0095] The product obtained by loading the iridium particles on Pt / C can be dried, and thus the solvent can be removed (S40). For example, the obtained product can be stirred at room temperature for 10 hours or longer, filtered, and then dried in a vacuum oven at a temperature of about 50°C for about 2 hours.

[0096] When the solvent is removed in this manner, a catalyst composite precursor in which iridium particles may be supported on Pt / C may be obtained.

[0097] Thereafter, oxidation of the iridium particles contained in the catalyst composite precursor may be performed (S50). Thus, the above-mentioned catalyst composite may be obtained.

[0098] When oxidizing the iridium particles ( S50 ), the iridium particles supported on Pt / C may be oxidized, thereby providing an iridium compound represented by Chemical Formula 1.

[0099] The process of oxidizing the iridium particles is not particularly limited, and may include, for example, heat-treating the catalyst composite precursor in air at a temperature of about 200 to 400° C., or specifically about 200 to 300° C., for about 1 to 5 hours.

[0100] The method of manufacturing the catalyst composite according to the exemplary embodiment of the present invention may further include the following modifications.

[0101] Here, the starting solution may further include a transition metal precursor, thereby obtaining an intermediate product including Pt / C, iridium particles, and transition metal particles.

[0102] The transition metal precursor is not particularly limited and can be selected from, for example, iron (II) chloride (FeCl 2 ), cobalt(II) chloride hexahydrate (CoCl 2 6H 2 O), copper(II) chloride dihydrate (CuCl 2 ·2H 2 O) and a group consisting of a combination thereof.

[0103] Thereafter, the pH of the intermediate product may be adjusted to load the iridium particles and the transition metal particles on Pt / C, the resultant product may be dried, and the iridium particles and the transition metal particles may be oxidized to obtain the iridium compound represented by Chemical Formula 2.

[0104] Specific conditions of each step of the above manufacturing method are omitted because they are approximately the same as or similar to those of the above-mentioned method.

[0105] Figure 5 An exemplary manufacturing process of an exemplary catalyst composite for an exemplary fuel cell according to an exemplary embodiment of the present invention is shown.

[0106] like Figure 5 As shown, the method for manufacturing a catalyst composite according to an exemplary embodiment of the present invention may include: preparing a starting solution by adding an iridium precursor to a solvent (S10'); obtaining an intermediate product including iridium particles by heat treating the starting solution (S20'); adding a platinum-loaded carbon support (Pt / C) to the intermediate product, and loading the iridium particles on the Pt / C by adjusting the pH of the intermediate product (S30'); drying the obtained product (S40'); and iridium oxide particles (S50').

[0107] When preparing the starting solution ( S10 ′), the solvent is not particularly limited, and may appropriately include, for example, ethylene glycol (EG).

[0108] The iridium precursor is not particularly limited and may suitably include, for example, iridium (III) chloride hydrate (IrCl 3 ·xH 2 O).

[0109] When preparing the starting solution (S10'), the solvent may be adjusted to a basic pH. For example, the pH of the solvent may be about 10 or greater, and or particularly about 12.

[0110] The preparation of the starting solution (S10′) may be performed in the following manner: sodium hydroxide (NaOH) used as a pH adjuster may be added to the solvent so that the solvent may be alkaline, and then the iridium precursor may be added thereto. For example, the iridium precursor may be mixed with sodium acetate (CH 3 COONa) was added together.

[0111] When the intermediate product (S20') is obtained, the starting solution may be heat-treated in an inert atmosphere, whereby the iridium precursor forms iridium particles.

[0112] The inert gas is not particularly limited and may include, for example, nitrogen (N 2 ).

[0113] When obtaining the intermediate product ( S20 ′), the starting solution may be heat-treated at a temperature of about 100° C. to 200° C. for about 1 to 5 hours in an atmosphere purged with an inert gas.

[0114] The heat treatment can be performed in the following manner: the starting solution is gradually heated from room temperature to the desired temperature, or the starting solution is placed in a constant temperature bath preset to the desired temperature. Preferably, the heat treatment can be performed by the previous process. In the previous process, the voltage reversal time can be about 80 minutes longer than the latter process.

[0115] The above manufacturing method may further include cooling the intermediate product to room temperature.

[0116] When loading iridium particles (S30'), the intermediate product may be added with Pt / C, after which the pH of the intermediate product may be adjusted, and thus the iridium particles are loaded on Pt / C. For example, the intermediate product may be appropriately adjusted to an acidic pH of about 0.5 to 3.0, whereby the iridium particles are loaded on Pt / C.

[0117] The process of adding Pt / C is not particularly limited, and may include, for example, preparing an acidic solution including Pt / C, such as a hydrochloric acid solution or an acetic acid solution, and then adding the acidic solution to the intermediate product.

[0118] The process of adjusting the pH of the intermediate product is not particularly limited, and may appropriately include, for example, adding a hydrochloric acid (HCl) solution and an acetic acid (CH 3 at least one of COOH) solutions.

[0119] The product obtained by loading iridium particles on Pt / C is dried, and thus the solvent can be removed (S40′). For example, the obtained product can be stirred at room temperature for about 10 hours or longer, filtered, and then dried in a vacuum oven at a temperature of about 50° C. for about 2 hours.

[0120] When the solvent is removed in this way, a catalyst composite precursor in which iridium particles are supported on Pt / C can be obtained.

[0121] Thereafter, oxidation of the iridium particles contained in the catalyst composite precursor may be performed (S50'). Thus, the above-mentioned catalyst composite may be obtained.

[0122] When oxidizing the iridium particles ( S50 ′), the iridium particles supported on Pt / C may be oxidized, thereby providing the iridium compound represented by Chemical Formula 1.

[0123] The process of oxidizing the iridium particles is not particularly limited, and may include, for example, heat-treating the catalyst composite precursor in air at a temperature of about 200 to 400° C., or specifically about 200 to 300° C., for about 1 to 5 hours.

[0124] The method of manufacturing the catalyst composite according to the exemplary embodiment of the present invention may further include the following modifications.

[0125] The starting solution may be further added with a transition metal precursor to obtain an intermediate product including iridium particles and transition metal particles.

[0126] The transition metal precursor is not particularly limited and can be selected from, for example, iron (II) chloride (FeCl 2 ), cobalt(II) chloride hexahydrate (CoCl 2 6H 2 O), copper(II) chloride dihydrate (CuCl 2 ·2H 2 O) and a group consisting of a combination thereof.

[0127] Thereafter, the intermediate product is added with Pt / C, and the pH of the intermediate product may be adjusted so that iridium particles and transition metal particles are loaded on Pt / C, the resulting product may be dried, and the iridium particles and transition metal particles may be oxidized to obtain the iridium compound represented by Chemical Formula 2.

[0128] Specific conditions of each step of the above manufacturing method are omitted because they are approximately the same as or similar to those of the above-mentioned method.

[0129] Example

[0130] A better understanding of the present invention will be provided by the following examples and test examples, which are only set forth for the purpose of illustrating the present invention but should not be construed as limiting the present invention. Examples 1 to 5 of the present invention can be prepared with Pt-IrO x In Comparative Example 1, an anode catalyst not including a voltage reversal catalyst is described as an example, and in Comparative Example 2, an anode catalyst in which Pt / C and IrO are combined as in the conventional art is described as an example. x In Comparative Example 2, the ratio of Pt to Ir was 2:1, and IrO was synthesized by the Adams Fusion method. x .

[0131] The processing conditions are schematically shown in Table 1 below.

[0132] Table 1

[0133]

[0134]

[0135] In Table 1,

[0136] 1) refers to the carbon carrier loaded with platinum

[0137] 2) refers to the carbon support loaded with platinum and IrO x A simple mixture of

[0138] 3) refers to platinum and IrO x Loaded on carbon support

[0139] 4) refers to platinum and Ir loaded on carbon carrier

[0140] Example 1

[0141] The catalyst complex was synthesized by performing the following steps in sequence:

[0142] (S10) A small amount of EG solvent was added to the flask containing Pt / C to prevent Pt oxidation, NaOH and EG were added to adjust the pH of the solution to 12, and iridium (III) chloride hydrate (IrCl 3 ·xH 2 O) and sodium acetate (CH 3 COONa), thereby preparing a starting solution;

[0143] (S20) treating the starting solution at a temperature of 160° C. for 3 hours in a nitrogen-purged atmosphere to produce an intermediate product including Pt / C and iridium particles, and cooling the intermediate product to room temperature;

[0144] (S30) the intermediate product is added with 10% hydrochloric acid (HCl) solution to adjust its pH to 0.5, thereby loading iridium particles on Pt / C;

[0145] (S40) stirring the intermediate product at room temperature for 10 hours or longer, then filtering and drying in a vacuum oven at a temperature of 50° C. for 2 hours; and

[0146] (S50) The dried product is heat-treated in an electric furnace at 200°C in air for 2 hours to oxidize the surface of the iridium particles, ultimately producing a catalyst composite configured such that platinum and iridium oxide are supported on a carbon support.

[0147] Example 2

[0148] The catalyst composite was manufactured in the same manner as in Example 1, except that Pt / C was not added when preparing the starting solution (S10), and Pt / C was added to the intermediate product cooled to room temperature, and specifically a 3% hydrochloric acid solution including Pt / C was added to the intermediate product.

[0149] Example 3

[0150] A catalyst composite was manufactured in the same manner as in Example 2, except that a 14% acetic acid solution including Pt / C was added to the intermediate product.

[0151] Example 4

[0152] A catalyst composite was manufactured in the same manner as in Example 2, except that a 0.3% hydrochloric acid solution including Pt / C was added to the intermediate product.

[0153] Example 5

[0154] A catalyst composite was manufactured in the same manner as in Example 4, except that the heat treatment temperature was adjusted to 100° C. when oxidizing the iridium particles ( S50 ).

[0155] Example 6

[0156] A catalyst composite was manufactured in the same manner as in Example 4, except that the heat treatment temperature was adjusted to 300° C. when oxidizing the iridium particles ( S50 ).

[0157] Example 7

[0158] A catalyst composite was manufactured in the same manner as in Example 4, except that the heat treatment temperature was adjusted to 400° C. when oxidizing the iridium particles ( S50 ).

[0159] Example 8

[0160] The catalyst complex was synthesized by performing the following steps in sequence:

[0161] (S10) NaOH was added to the EG (ethylene glycol) solvent to adjust the pH of the solution to 12, and then iridium (III) chloride hydrate (IrCl 3 ·xH 2 O), sodium acetate (CH 3 COONa) and iron(II) chloride (FeCl 2 ) is added thereto, thereby preparing a starting solution having Ir and Fe nanoparticles;

[0162] (S20) slowly heating the starting solution from room temperature to 160° C. in a nitrogen-purged atmosphere, then maintaining the temperature for 3 hours and cooling to room temperature;

[0163] (S30) the resulting product is added with a 3% hydrochloric acid (HCl) solution including Pt / C, and then with a 10% HCl solution to obtain a pH of 0.5;

[0164] (S40) stirring the obtained product at room temperature for 10 hours or longer, then filtering and drying in a vacuum oven at 50° C. for 2 hours; and

[0165] (S50) The dried product is heat-treated in an electric furnace at 200°C in air for 2 hours.

[0166] Example 9

[0167] A catalyst composite was manufactured in the same manner as in Example 8, except that rapid heating was performed in such a manner that the starting solution was placed in a constant temperature bath preset at a temperature of 160° C. and treated in a nitrogen atmosphere for 3 hours in ( S20 ).

[0168] Example 10

[0169] In addition to using cobalt(II) chloride hexahydrate (CoCl 2 6H 2 A catalyst composite was prepared in the same manner as in Example 8 except that ferric chloride was replaced with 2-(4-(2-nitrogen)-2-ol).

[0170] Example 11

[0171] In addition to using cobalt(II) chloride hexahydrate (CoCl 2 6H 2 A catalyst composite was prepared in the same manner as in Example 9 except that ferric chloride was replaced with 2-(4-(2-nitrogen)-2-ol).

[0172] Example 12

[0173] In addition to using copper(II) chloride dihydrate (CuCl 2 ·2H 2 A catalyst composite was prepared in the same manner as in Example 8 except that ferric chloride was replaced with 2-(4-(2-nitrogen)-2-ol).

[0174] Example 13

[0175] In addition to using copper(II) chloride dihydrate (CuCl 2 ·2H 2 A catalyst composite was prepared in the same manner as in Example 9 except that ferric chloride was replaced with 2-(4-(2-nitrogen)-2-ol).

[0176] Comparative Example 1

[0177] An anode catalyst is used that does not include a voltage reversal catalyst.

[0178] Comparative Example 2

[0179] As with conventional technology, Pt / C and IrO x Here, the ratio of Pt and Ir is 2:1, and IrO is synthesized by the Adams melt method. x .

[0180] Comparative Examples 3 to 5

[0181] The same steps as in Example 1 were performed, but the Pt / C and iridium (III) chloride hydrate (IrCl 3 ·xH 2 In Comparative Example 3, Pt:Ir=1:0.125, in Comparative Example 4, Pt:Ir=1:0.25, and in Comparative Example 5, Pt:Ir=1:0.4.

[0182] Comparative Example 6

[0183] Except for 25% H 2 / 75%N 2 A catalyst composite was manufactured in the same manner as in Example 1, except that the reduction treatment was performed under conditions of 400° C. and 200° C. instead of the iridium oxide particles ( S50 ).

[0184] Evaluation Methodology

[0185] Manufacturing fuel cells

[0186] In order to evaluate the voltage reversal tolerance of each example and comparative example, a fuel cell was manufactured using the catalyst composite of each example and comparative example, and a voltage reversal tolerance test was performed by the following steps.

[0187] (1) Catalyst slurry was prepared using the catalyst of each example and comparative example, and then the catalyst slurry was sprayed onto GDL (39BC, SGL) to form an anode. The weight ratio of perfluorosulfonic acid ionomer dispersion (5wt% Nafion dispersion, DuPont Co., USA) to carbon was 0.8, and each loading amount was as follows.

[0188] - Comparative Example 1, Comparative Example 2, and Examples 1 to 7: 0.1 mg Pt / cm 2 +0.05mg Ir / cm 2

[0189] -Comparative Example 3: 0.1 mg Pt / cm 2 +0.0125mg Ir / cm 2

[0190] -Comparative Example 4: 0.1 mg Pt / cm 2 +0.025mg Ir / cm 2

[0191] -Comparative Example 5: 0.1 mg Pt / cm 2 +0.04mg Ir / cm 2

[0192] (2) A catalyst slurry was prepared by using the same Pt / C catalyst and the catalyst slurry was sprayed onto GDL (39BC, SGL) to form a cathode. The weight ratio of perfluorosulfonic acid ionomer dispersion (5 wt% Nafion dispersion, DuPont Co., USA) to carbon was 0.8, and the Pt loading was 0.4 mg. Pt / cm 2 .

[0193] (3) A membrane electrode assembly (MEA) was manufactured by arranging an anode and a cathode on both sides of an electrolyte membrane (NRE211, Dupont) and pressurizing at a pressure of 430 psi at a temperature of 135° C. for 135 seconds.

[0194] (4) A fuel cell is manufactured using a titanium (Ti) anode separator MEA and a graphite cathode separator.

[0195] Here, the torque applied to the eight bolts for battery fixing was 50 kgf·cm.

[0196] Activating the fuel cell

[0197] 200 ml / min of hydrogen and 600 ml / min of air were supplied to the anode and cathode respectively, and the battery voltage increased by 100 mA / cm2 in 1 second under the OCV (open circuit voltage) state. 2 , until it reaches 0.25 V. After the battery voltage reaches 0.25 V, repeat the above process until the OCV and performance are stable. The battery temperature is 65°C and the relative humidity is 100%.

[0198] Voltage reversal tolerance test method - after stopping the hydrogen supply, measure the battery voltage based on the voltage reversal time

[0199] The voltage reversal tolerance test was conducted by measuring the battery voltage at a battery temperature of 65° C. and a relative humidity of 100% by the following method.

[0200] (1) At 0.2A / cm 2 An electrical load was applied at a current density of 1.00 Å, and hydrogen and air were supplied at a stoichiometric ratio (SR) of 1.5:2.0.

[0201] (2) After 5 minutes of applying the electrical load, the supply of hydrogen to the anode side was stopped, and argon was supplied at the same flow rate.

[0202] (3) Measure the time and voltage until the battery voltage reaches -2.5V.

[0203] (4) The time required for the battery voltage to reach -2.5 V from 0 V is determined as the voltage reversal time.

[0204] Therefore, the measurement results of the voltage reversal time of the example and the comparative example are shown in Table 2 below.

[0205] Table 2

[0206]

[0207] Evaluation results

[0208] Evaluation Example 1: Evaluation of voltage reversal time

[0209] Figures 6 to 9 is a graph showing voltage reversal time results of the example and the comparative example.

[0210] like Figure 6 As shown, the voltage reversal time in Example 1 is significantly increased compared with Comparative Examples 1 and 2. Figures 7 to 9 In all examples (Example 1 to Example 7) according to the present invention, the voltage reversal time increased by at least about 25 times compared with Comparative Example 1, and the voltage reversal time increased by at least 2 times compared with Comparative Example 2.

[0211] refer to Figure 7, when the addition of Pt / C was performed in S30 during the synthesis process of Example 2, the voltage reversal time increased by about 86 minutes compared with Example 1. This is considered to be because the addition time of Pt / C was changed, thereby reducing the aggregation of platinum (Pt) particles, thereby maintaining the coverage of carbon.

[0212] refer to Figure 8 In Examples 3 and 4, 14% acetic acid and 0.3% hydrochloric acid were added in S30 during the synthesis process, whereby the voltage reversal time was increased by 10 to 40 minutes compared with Example 2. This is considered to be because damage to carbon was reduced in a weakly acidic environment.

[0213] like Fig. 9 As shown, in the voltage reversal time depending on the heat treatment temperature in Examples 4, 6, and 7, it can be seen that even when the heat treatment is performed at a relatively low temperature of 100°C or less to perform Ir surface oxidation at a similar level of about 10 minutes, the effect of reducing voltage reversal degradation can be ensured. In Example 6, the heat treatment was performed at 300°C, and the voltage reversal time increased by about 17 times compared with Comparative Example 2, showing the best effect. On the other hand, it is preferred to perform the heat treatment at a higher temperature to oxidize iridium, but when the heat treatment temperature exceeds 400°C, the carrier carbon may be oxidized. Therefore, it is preferred to perform the heat treatment in the range of 200°C to 400°C.

[0214] Evaluation Example 2: Evaluation of IrO of Load x distributed

[0215] Fig.10 and Fig.11 The distribution of the iridium compound in the catalyst composite for a fuel cell in the comparative example and the example is shown.

[0216] like Fig.10 As shown in the enlarged view on the right, IrOx synthesized by the Adams melt method (Comparative Example 2) has a random block structure with no formal size.

[0217] On the other hand, Fig.11 As shown, the size of IrO is about 2 nm. x Evenly distributed on the carbon support (Pt-IrO x Therefore, an increase in catalytic activity can be expected.

[0218] Evaluation Example 3: Evaluation of voltage reversal time according to heat treatment conditions

[0219] like Fig.12 As shown, the results of the voltage reversal time of Comparative Example 6 (Pt-Ir / C) which was subjected to hydrogen reduction heat treatment at a temperature of 200°C and Example 1 which was subjected to heat treatment at a temperature of 200°C in air were compared. In Example 1, Pt-IrO was heat treated at a temperature of 200°C in air.x / C structure, the voltage reversal time is increased compared with Comparative Example 6 in which a Pt-Ir / C structure is given by hydrogen reduction heat treatment at a temperature of 200°C. It is confirmed that in the catalyst structure loaded in the same manner, the oxidized structure of Ir helps to mitigate the voltage reversal of the fuel cell. Considering the voltage reversal time (about 62 minutes) of Comparative Example 2 according to conventional technology, it can be assumed that the oxidized structure of Ir is a factor that promotes the voltage reversal tolerance of the fuel cell.

[0220] Evaluation Example 4: Evaluation of voltage reversal time based on the weight ratio of Pt and Ir

[0221] refer to Fig.13 , in Pt-IrO x In the / C catalyst, the voltage reversal time was evaluated according to the weight ratio of Pt and Ir. Fig.13 As shown, the results of the voltage reversal time in Comparative Example 1 (Pt:Ir=1:0.5), Comparative Example 3 (Pt:Ir=1:0.125), Comparative Example 4 (Pt:Ir=1:0.25) and Comparative Example 5 (Pt:Ir=1:0.4) are shown. Considering the voltage reversal time of 62 minutes in Comparative Example 2, it is concluded that the ratio of Pt to Ir (Ir / Pt) is preferably 0.5 or more.

[0222] Although according to conventional technology IrO x The distribution of mixed Pt / C and IrO x However, in the present invention, IrO x The Pt and the Pt can be loaded together on the carbon support, and in addition, a highly dispersed structure can be formed, thereby increasing the water decomposition activity and electrical connectivity during the voltage reversal of the fuel cell, and ultimately increasing the voltage reversal tolerance. Therefore, when the voltage reversal of the fuel cell occurs, the voltage reversal can be stably controlled compared to conventional cases, so that the life of the fuel cell stack can be increased, and cost reduction can also be achieved by reducing the replacement cost.

[0223] Evaluation Example 5

[0224] The water decomposition activity of the catalyst composite of each of Comparative Example 2 and Examples 8 to 13 was measured by a half-electrode test. Fig.14 The results are shown in . With reference to this, it was found that the activities of the catalyst composites of Examples 8 to 13 were superior to those of the comparative example.

[0225] Although various exemplary embodiments of the present invention have been disclosed for illustrative purposes, those skilled in the art will understand that various modifications are possible without departing from the scope and spirit of the present invention as disclosed in the appended claims, and such modifications should not be understood separately from the technical ideas or essential features of the present invention.

Claims

1. A catalyst composite for an electrode of a fuel cell, include: Carrier; Platinum supported on the carrier; as well as an iridium compound supported on the carrier, The iridium compound includes at least one of iridium oxide represented by the following chemical formula 1 and iridium transition metal oxide represented by the following chemical formula 2: [Chemical formula 1] dogs x [Chemical formula 2] IrMO x wherein M is a transition metal selected from the group consisting of Fe, Co, Cu, Ni and combinations thereof, and x is 1 to 2, Wherein, the weight ratio of platinum to iridium in the iridium oxide or the weight ratio of platinum to iridium in the iridium transition metal oxide is 1:0.5 to 1:

1.

2. The catalyst composite according to claim 1, in, The atomic ratio of platinum to transition metal in the iridium transition metal oxide is 1:1 to 1:

5.

3. A method for producing a catalyst composite, include: preparing a starting solution comprising a platinum-loaded support and an iridium precursor added to a solvent; obtaining an intermediate product including the platinum-loaded carrier and iridium particles by heat treating the starting solution; The iridium particles are loaded on the platinum-loaded carrier by adjusting the pH of the intermediate product; drying the resulting product; and oxidizing the iridium particles, Wherein, when preparing the starting solution, the solvent is adjusted to an alkaline pH.

4. The method according to claim 3, in, The intermediate product is obtained by heat-treating the starting solution at a temperature of 100° C. to 200° C. for 1 to 5 hours in an inert atmosphere.

5. The method according to claim 3, in, The intermediate product is made acidic within a pH range of 0.5 to 3.0, and thus the iridium particles are supported on the platinum-supported support.

6. The method according to claim 3, in, The iridium particles are oxidized by heat-treating the dried product at a temperature of 200° C. to 400° C. for 1 to 5 hours in air.

7. The method according to claim 3, in, The starting solution also includes a transition metal precursor, and the intermediate product includes the platinum-loaded support, the iridium particles, and transition metal particles.

8. The method according to claim 7, in, The pH of the intermediate product is adjusted so that the iridium particles and the transition metal particles are supported on the platinum-supported carrier.

9. The method according to claim 8, in, The resulting product is dried, and the iridium particles and the transition metal particles are oxidized.

10. A method for producing a catalyst composite, include: preparing a starting solution comprising an iridium precursor added to a solvent; obtaining an intermediate product including iridium particles by heat treating the starting solution; adding a platinum-loaded carrier to the intermediate product, and loading the iridium particles on the platinum-loaded carrier by adjusting the pH of the intermediate product; drying the resulting product; and oxidizing the iridium particles, Wherein, when preparing the starting solution, the solvent is adjusted to an alkaline pH.

11. The method according to claim 10, in, The intermediate product is obtained by heat-treating the starting solution at a temperature of 100° C. to 200° C. for 1 to 5 hours in an inert atmosphere.

12. The method according to claim 10, in, The intermediate product includes the platinum-loaded carrier, and then the intermediate product is made acidic within a pH range of 0.5 to 3.0, and thus the iridium particles are loaded on the platinum-loaded carrier.

13. The method according to claim 10, in, The iridium particles are oxidized by heat-treating the dried product at a temperature of 200° C. to 400° C. for 1 to 5 hours in air.

14. The method according to claim 10, in, The starting solution also includes a transition metal precursor, and the intermediate product includes the iridium particles, transition metal particles and the platinum-loaded carrier.

15. The method according to claim 14, in, The pH of the intermediate product is adjusted so that the iridium particles and the transition metal particles are supported on the platinum-supported carrier.

16. The method according to claim 15, in, The resulting product is dried, and the iridium particles and the transition metal particles are oxidized.

17. An electrode comprising the catalyst composite according to claim 1.