Method for manufacturing zero-plane anchoring film and liquid crystal display element
By forming a patterned free radical generation film in the liquid crystal display element and carrying out a polymerization reaction, the problems of response speed delay and coating were solved, realizing a low-cost, high-efficiency zero-surface anchored IPS mode and improving the performance of the liquid crystal display element.
Patent Information
- Application Number
- CN201980041213.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-18
- Filing Date
- 2019-06-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-06-17
AI Technical Summary
Existing technologies for manufacturing zero-surface anchored IPS mode liquid crystal display elements suffer from problems such as delayed response speed and difficulty in coating different materials in small areas, resulting in high costs and increased battery consumption.
A patterned free radical generating film is formed by irradiating a specific area with radiation, and a liquid crystal composition containing liquid crystal and free radical polymerizable compounds is brought into contact with the film to carry out a polymerization reaction, forming a zero-plane anchoring film. The anchoring energy is controlled to achieve low driving voltage and fast response speed.
It achieves low-cost, high-yield zero-surface anchoring film manufacturing, improves the response speed and contrast of liquid crystal display elements, reduces driving voltage, suppresses Vcom offset, and is suitable for high-precision rendering in FFS mode.
Smart Images

Figure BDA0002844704230000041 
Figure BDA0002844704230000042 
Figure BDA0002844704230000051
Abstract
Description
Technical Field
[0001] The present invention relates to a manufacturing method using a polymer stabilization technology capable of manufacturing a zero-azimuthal surface anchoring film inexpensively and without involving complicated processes, and a liquid crystal display element and a manufacturing method thereof for realizing further low-voltage driving using the manufacturing method. Background Art
[0002] In recent years, liquid crystal display elements have been widely used in mobile phones, computers, and television displays. Liquid crystal display elements have the characteristics of being thin, lightweight, and low in power consumption, and are expected to be further applied in VR, ultra-high-definition displays, and the like in the future. Various display modes such as TN (Twisted Nematic), IPS (In-Plane Switching), and VA (Vertical Alignment) have been proposed for the display of liquid crystal displays, but all modes use a film (liquid crystal alignment film) that induces the liquid crystal to the desired orientation state.
[0003] In particular, in products with touch panels such as tablet PCs, smartphones, and smart TVs, the IPS mode in which the display is not easily disturbed even when touched is preferred. In recent years, liquid crystal display elements using FFS (Frindge Field Switching) and non-contact technologies using light orientation have been gradually adopted to improve contrast and viewing angle characteristics.
[0004] However, compared with IPS, FFS has the problem of high manufacturing cost of substrates and poor display unique to the FFS mode, which is called Vcom offset. In addition, compared with the friction method, photo-orientation has the advantages of increasing the size of the element that can be manufactured and greatly improving the display characteristics, but the problems in the principle of photo-orientation can be cited (if it is a decomposition type, there is poor display from the decomposition product, if it is an isomerization type, there is burning caused by insufficient orientation force, etc.). In order to solve these problems, liquid crystal display element manufacturers and liquid crystal alignment film manufacturers are currently conducting various studies.
[0005] On the other hand, in recent years, an IPS mode using a zero-plane anchoring technique has been proposed, and it has been reported that this technique can improve contrast and achieve significantly lower voltage driving compared to the conventional IPS mode (see Patent Document 1).
[0006] Specifically, it is a method in which a liquid crystal orientation film having strong anchoring energy is used on a single-sided substrate, a substrate side having an electrode generating a lateral electric field is treated to have no orientation restriction force on the liquid crystal, and an IPS mode liquid crystal display element is produced using these processes.
[0007] In recent years, a zero-plane state has been created using a thick polymer brush, and a zero-plane anchor IPS mode technology proposal has been completed (Reference 2). This technology has achieved a significant increase in contrast ratio and a significant reduction in driving voltage.
[0008] On the other hand, there is a problem that the response speed, especially the response speed when the voltage is turned off (OFF), is significantly reduced. The reason is that the driving voltage becomes lower, so the liquid crystal takes time to recover due to the influence caused by responding in an electric field weaker than the usual driving method, and the anchoring force of the alignment film is very small. As a solution to this, a means of making zero anchoring only on the pixel electrode is proposed (Patent Document 3). Thus, it is reported that both the increase in brightness and the response speed can be taken into account.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent No. 4053530
[0012] Patent Document 2: Japanese Patent Application Publication No. 2013-231757
[0013] Patent Document 3: Japanese Patent Application Publication No. 2017-211566 Summary of the invention
[0014] Problems to be solved by the invention
[0015] By making zero-surface anchoring only on the electrodes of the IPS comb-tooth electrodes, the response speed delay during driving can be suppressed. On the other hand, in order to make the zero-surface anchoring state only on the electrodes, it is necessary to prepare difficult technologies such as coating different materials on very small areas separately. It is believed that actual industrialization will become a major issue.
[0016] If the above-mentioned technical problems can be solved, it will be a great cost advantage for panel manufacturers, and it will also be an advantage to suppress battery consumption and improve image quality.
[0017] The present invention has been carried out and completed in order to solve the above-mentioned problems, and its purpose is to provide a lateral electric field liquid crystal display element and its manufacturing method which can simultaneously achieve non-contact orientation, low driving voltage and faster response speed when turned off (Off) by a method that can produce a portion having an anchoring force with a zero-plane anchoring portion within the plane of a liquid crystal orientation film, a method that controls the anchoring energy to an arbitrary state, and a simple and inexpensive method at room temperature.
[0018] Means used to solve problems
[0019] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved, and have completed the present invention having the following gist.
[0020] That is, the present invention includes the following aspects.
[0021] [1] A method for manufacturing a patterned zero-plane anchoring film, comprising: a step of irradiating a radical generating film with radiation in a specific area to form a patterned radical generating film; and a step of bringing a liquid crystal composition containing a liquid crystal and a radical polymerizing compound into contact with the patterned radical generating film, and while maintaining the contact state, imparting energy sufficient to cause the radical polymerizing compound to undergo a polymerization reaction to the liquid crystal composition.
[0022] [2] The method according to [1], wherein the radical generating film is a radical generating film subjected to a uniaxial orientation treatment.
[0023] [3] The method according to [1] or [2], wherein the step of imparting energy is performed in the absence of an electric field.
[0024] [4] The method according to any one of [1] to [3], wherein the radical generating film is a film in which an organic group that induces radical polymerization is fixed.
[0025] [5] The method according to any one of [1] to [3], characterized in that the above-mentioned free radical generating film is obtained by applying a composition of a compound having a group generating free radicals and a polymer, curing it to form a film, and fixing it in the film.
[0026] [6] The method according to any one of [1] to [3], wherein the radical generating film comprises a polymer containing an organic group that induces radical polymerization.
[0027] [7] The method according to [6], characterized in that the polymer containing an organic group that induces free radical polymerization is at least one polymer selected from a polyimide precursor, polyimide, polyurea and polyamide obtained using a diamine component, and the diamine component contains a diamine containing an organic group that induces free radical polymerization.
[0028] [8] The method according to any one of [4], [6] and [7], wherein the organic group inducing free radical polymerization is an organic group represented by any one of the following structures [X-1] to [X-18], [W], [Y] and [Z],
[0029]
Compound 1
[0030]
[0031] (In formulas [X-1] to [X-18], * represents a site bonded to a portion other than a polymerizable unsaturated bond of a compound molecule, S1 and S2 each independently represent -O-, -NR-, or -S-, R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, and R1 and R2 each independently represent a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms)
[0032]
Compound 2
[0033]
[0034] (In the formulas [W], [Y], and [Z], * represents a site bonded to a portion other than the polymerizable unsaturated bond of the compound molecule, Ar represents an aromatic hydrocarbon group selected from phenylene, naphthylene, and biphenylene groups which may have an organic group and / or a halogen atom as a substituent, and R 9 and R 10 Each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and R 9 and R 10 In the case of an alkyl group, the terminals may be bonded to each other to form a ring structure or may not be bonded to each other to form a ring structure; Q represents the following structure;
[0035]
Compound 3
[0036]
[0037] (Where R 11 represents -CH2-, -NR-, -O- or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a site bonded to a portion other than Q of the compound molecule)
[0038] R 12represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms).
[0039] [9] The method according to claim 7, wherein the diamine containing an organic group that induces free radical polymerization is a diamine having a structure represented by the following general formula (6) or the following general formula (7),
[0040]
Compound 4
[0041]
[0042] (In formula (6), R 6 represents a single bond, -CH2-, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-,
[0043] R 7 represents a single bond, or an alkylene group having 1 to 20 carbon atoms which is unsubstituted or substituted with a fluorine atom, wherein at least one of any -CH2- or -CF2- of the alkylene group is independently substituted with or not substituted with a group selected from -CH=CH-, a divalent carbocyclic ring and a divalent heterocyclic ring, and is substituted with or not substituted with any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH- or -NH-, provided that they are not adjacent to each other;
[0044] R 8 represents a free radical polymerization reactive group selected from the following formulae;
[0045]
Compound 5
[0046]
[0047] (In formulas [X-1] to [X-18], * represents a site bonded to a portion other than the radical polymerizable group of the compound molecule, S1 and S2 each independently represent -O-, -NR-, or -S-, R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, and R 1 , R 2 Each independently represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms)
[0048]
Compound 6
[0049]
[0050] (In formula (7), T 1 and T 2are each independently a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-,
[0051] S 0 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, wherein at least one of any -CH2- or -CF2- of the alkylene group is independently substituted by or is not substituted by a group selected from -CH=CH-, a divalent carbocyclic ring and a divalent heterocyclic ring, and is substituted by or is not substituted by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH- or -NH-, provided that they are not adjacent to each other,
[0052] J is an organic group represented by any one of the following formulae,
[0053]
Compound 7
[0054]
[0055] (In the formulas [W], [Y], and [Z], * represents a site bonded to T2, Ar represents an aromatic hydrocarbon group selected from phenylene, naphthylene, and biphenylene groups which may have an organic group and / or a halogen atom as a substituent, and R 9 and R 10 Each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and Q represents any of the following structures;
[0056]
Compound 8
[0057]
[0058] (Where R 11 represents -CH2-, -NR-, -O- or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a site bonded to a part of the compound molecule other than Q)
[0059] R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms).
[0060]
[10] The method according to any one of [1] to [9], wherein at least one of the radical polymerizable compounds is a compound that is compatible with liquid crystal and has one polymerizable unsaturated bond in one molecule.
[0061]
[11] The method according to
[10] , wherein the polymerization reactive group of the radical polymerizable compound is selected from the following structures:
[0062]
Compound 9
[0063]
[0064] (wherein, * represents a site bonded to a portion other than a polymerizable unsaturated bond of a compound molecule; R b represents a straight-chain alkyl group having 2 to 8 carbon atoms, and E represents a single bond, -O-, -NR c -, -S-, ester bonds and amide bonds in the bonding group; R c represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms).
[0065]
[12] A method according to any one of [1] to
[11] , wherein the liquid crystal composition containing a liquid crystal and a radically polymerizable compound comprises a liquid crystal composition containing a radically polymerizable compound such that the Tg of the polymer obtained by polymerizing the radically polymerizable compound is below 100°C.
[0066]
[13] A method for producing a liquid crystal cell, wherein the method described in any one of [1] to
[12] is used, and the method for producing a liquid crystal cell comprises:
[0067] A step of preparing a first substrate having a radical generating film and a second substrate having or not having a radical generating film;
[0068] a step of manufacturing a unit in such a manner that the radical generating film on the first substrate faces the second substrate; and
[0069] A step of filling a liquid crystal composition containing a liquid crystal and a radical polymerizable compound between the first substrate and the second substrate.
[0070]
[14] The method for manufacturing a liquid crystal cell according to
[13] , wherein the second substrate is a second substrate that does not have a radical generating film.
[0071]
[15] The method for manufacturing a liquid crystal unit according to
[14] , wherein the second substrate is a substrate coated with a liquid crystal alignment film having uniaxial alignment properties.
[0072]
[16] The method for producing a liquid crystal unit according to
[15] , wherein the liquid crystal alignment film having uniaxial alignment properties is a liquid crystal alignment film for horizontal alignment.
[0073]
[17] The method for manufacturing a liquid crystal cell according to any one of
[13] to
[16] , wherein the first substrate having a radical generating film is a substrate having a comb-tooth electrode.
[0074]
[18] A liquid crystal composition comprising a liquid crystal and a radical polymerizable compound,
[0075] At least one of the radical polymerizable compounds is a compound that is compatible with liquid crystal and has one polymerizable unsaturated bond in one molecule,
[0076] The polymerizable reactive group is selected from the following structures,
[0077]
Compound 10
[0078]
[0079] (wherein, * represents a site bonded to a portion other than a polymerizable unsaturated bond of a compound molecule; R b represents a straight-chain alkyl group having 2 to 8 carbon atoms, and E represents a single bond, -O-, -NR c -, -S-, ester bonds and amide bonds in the bonding group; R c represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms).
[0080]
[19] A method for manufacturing a liquid crystal display element, wherein a film produced in a zero-plane anchoring state is used, wherein the film produced in a zero-plane anchoring state is obtained using the method described in any one of [1] to
[17] .
[0081]
[20] A liquid crystal display element obtained using the method described in
[19] .
[0082]
[21] The liquid crystal display element according to
[20] , wherein the first substrate or the second substrate has an electrode.
[0083]
[22] A liquid crystal display element according to
[20] or
[21] , wherein the liquid crystal display element is a low voltage driven lateral electric field liquid crystal display element.
[0084] Effects of the Invention
[0085] According to the present invention, a zero-plane anchoring film can be made industrially with a high yield. The method of the present invention can be used to easily manufacture a liquid crystal display element similar to the zero-plane anchoring IPS mode liquid crystal display element described in Patent Documents 1 and 2 using cheap raw materials and existing manufacturing methods. In addition, the liquid crystal display element obtained by the manufacturing method of the present invention can provide a liquid crystal display element with the following excellent characteristics: compared with the previous technology, the response speed of the liquid crystal when turned off (Off) is faster, and the driving voltage is low, there are no bright spots, the Vcom offset can be suppressed in the IPS mode, and the fineness can be higher in the FFS mode. BRIEF DESCRIPTION OF THE DRAWINGS
[0086] Figure 1TN cell with a substrate having a film with zero plane anchoring regions and non-zero plane anchoring regions by having UV irradiated regions and non-UV irradiated regions. In the cell, transparent regions are not UV irradiated and opaque regions are UV irradiated regions. DETAILED DESCRIPTION
[0087] The present invention is a method for producing a film having a zero-plane anchor region and a strong anchor region patterned therein, characterized in that, after forming a radical generating film having an anchoring force on a substrate, irradiating the radical generating film with radiation in a region where the anchoring force is to be maintained, the polymerizing compound is polymerized by UV or heat while a liquid crystal containing a specific polymerizing compound is in contact with the radical generating film. More specifically, the present invention is a method for producing a film having a zero-plane anchor region and a strong anchor region patterned therein, comprising: a step of preparing a cell having a liquid crystal composition containing a liquid crystal and a radical polymerizing compound between a first substrate having a radical generating film treated with radiation and a second substrate having or not having a radical generating film; and a step of giving energy sufficient to polymerize the radical polymerizing compound to the cell. Preferably, the method is a method for producing a liquid crystal cell, comprising: a step of preparing a first substrate having a radical generating film treated with radiation and a second substrate having no radical generating film; a step of preparing the cell in a manner that the radical generating film and the second substrate face each other; and a step of filling a liquid crystal composition containing a liquid crystal and a radical polymerizing compound between the first substrate and the second substrate. For example, in a method for manufacturing a low-voltage driven IPS liquid crystal display element, the second substrate is a substrate (substrate) that does not have a free radical generating film and has a liquid crystal alignment film that has been uniaxially oriented, and the first substrate is a substrate that has a comb-tooth electrode.
[0088] In the present invention, "zero-plane anchoring film" refers to a film that has no orientation-restricting force on liquid crystal molecules in the in-plane direction, or even if there is, it is weaker than the intermolecular force between liquid crystals, and the liquid crystal molecules cannot be uniaxially oriented in any direction using only this film. In addition, the zero-plane anchoring film is not limited to a solid film, but also includes a liquid film covering the surface of a solid. Usually, in a liquid crystal display element, a film that restricts the orientation of liquid crystal molecules, i.e., a liquid crystal orientation film, is used in pairs to orient the liquid crystal, but when the zero-plane anchoring film and the liquid crystal orientation film are used in pairs, the liquid crystal can also be oriented. This is because the orientation-restricting force of the liquid crystal orientation film is also transmitted in the thickness direction of the liquid crystal layer due to the intermolecular force between the liquid crystal molecules, and as a result, the liquid crystal molecules close to the zero-plane anchoring film are also oriented. Therefore, when a liquid crystal orientation film for horizontal orientation is used in the liquid crystal orientation film, a horizontal orientation state can be produced in the liquid crystal unit as a whole. Horizontal orientation refers to a state in which the long axes of the liquid crystal molecules are arranged roughly parallel to the surface of the liquid crystal orientation film, and an inclined orientation of several degrees is also included in the category of horizontal orientation.
[0089] [Radical Generating Film-Forming Composition]
[0090] The radical-generating film-forming composition used to form the radical-generating film used in the present invention contains a polymer as a component, and contains a group that can generate free radicals. At this time, the composition can be a composition of a polymer formed by bonding a group that can generate free radicals, or a composition of a compound having a group that can generate free radicals and a polymer as a base resin. Such a composition is applied and cured to form a film, thereby obtaining a radical-generating film obtained by fixing the group that can generate free radicals in the film. The group that can generate free radicals is preferably an organic group that induces free radical polymerization.
[0091] Examples of such an organic group that induces radical polymerization include an organic group represented by any one of [X-1] to [X-18], [W], [Y], and [Z] represented by the following structures.
[0092]
Compound 11
[0093]
[0094] (In formulas [X-1] to [X-18], * represents a site bonded to a portion other than a polymerizable unsaturated bond of a compound molecule, S1 and S2 each independently represent -O-, -NR-, or -S-, R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, and R1 and R2 each independently represent a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms)
[0095]
Compound 12
[0096]
[0097] (In the formulas [W], [Y], and [Z], * represents a site bonded to a portion other than the polymerizable unsaturated bond of the compound molecule, Ar represents an aromatic hydrocarbon group selected from phenylene, naphthylene, and biphenylene groups which may have an organic group and / or a halogen atom as a substituent, and R 9 and R 10 Each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and R 9 and R 10 In the case of an alkyl group, the terminals may be bonded to each other to form a ring structure or may not be bonded to each other to form a ring structure; Q represents any of the following structures,
[0098]
Compound 13
[0099]
[0100] (Where R 11 represents -CH2-, -NR-, -O- or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a site bonded to a part other than Q of the compound molecule.
[0101] R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms).
[0102] As the polymer, for example, at least one polymer selected from the group consisting of a polyimide precursor, polyimide, polyurea, polyamide, polyacrylate, polymethacrylate, polyorganosiloxane, and the like is preferred.
[0103] In order to obtain the free radical generating film used in the present invention, when using the above-mentioned polymer having an organic group that induces free radical polymerization, it is preferred to use the following monomers as monomer components to produce a polymer having a group that can generate free radicals: a monomer having a photoreactive side chain containing at least one selected from methacrylic, acryl, vinyl, allyl, coumarin, styryl and cinnamoyl groups, or a monomer having a free radical generating site on the side chain that is decomposed by ultraviolet irradiation. On the other hand, considering the problem that the monomer that generates free radicals itself will spontaneously polymerize and eventually form an unstable compound, it is preferred to use a polymer derived from a diamine having a free radical generating site in terms of ease of synthesis, and more preferably a polyimide precursor such as polyamic acid and polyamic acid ester, polyimide, polyurea, polyamide, etc.
[0104] Specifically, such a radical generating site-containing diamine is, for example, a diamine having a side chain capable of generating radicals and polymerizing, and examples thereof include diamines represented by the following general formula (6), but are not limited thereto.
[0105]
Compound 14
[0106]
[0107] (In formula (6), R 6 represents a single bond, -CH2-, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-,
[0108] R 7represents a single bond, or an alkylene group having 1 to 20 carbon atoms which is unsubstituted or substituted with a fluorine atom, wherein at least one of any -CH2- or -CF2- of the alkylene group is independently substituted with or not substituted with a group selected from -CH=CH-, a divalent carbocyclic ring and a divalent heterocyclic ring, and is substituted with or not substituted with any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH- or -NH-, provided that they are not adjacent to each other;
[0109] R 8 represents a radical polymerizable group selected from the following formulae.
[0110]
Compound 15
[0111]
[0112] (In formulas [X-1] to [X-18], * represents a site bonded to a portion other than the radical polymerization reactive group of the compound molecule, S1 and S2 each independently represent -O-, -NR-, or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and R 12 represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, and R1 and R2 each independently represent a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms)
[0113] The bonding positions of the two amino groups (-NH2) in formula (6) are not limited. Specifically, relative to the bonding group of the side chain, the positions 2,3, 2,4, 2,5, 2,6, 3,4, and 3,5 on the benzene ring can be cited. Among them, from the viewpoint of reactivity when synthesizing polyamic acid, the positions 2,4, 2,5, or 3,5 are preferred. If the ease of synthesizing diamine is also considered, the positions 2,4 or 3,5 are more preferred.
[0114] Specific examples of the diamine having a photoreactive group including at least one selected from the group consisting of a methacryloyl group, an acryloyl group, a vinyl group, an allyl group, a coumarin group, a styryl group, and a cinnamoyl group include the following compounds, but are not limited thereto.
[0115]
Compound 16
[0116]
[0117] (Where J 1 is a bonding group selected from a single bond, -O-, -COO-, -NHCO-, or -NH-, J 2 represents a single bond or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms)
[0118] The diamine having a site as a side chain that decomposes by ultraviolet irradiation to generate a radical includes, but is not limited to, diamines represented by the following general formula (7).
[0119]
Compound 17
[0120]
[0121] (In formula (7), T1 and T2 are each independently a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-,
[0122] S 0 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, wherein at least one of any -CH2- or -CF2- of the alkylene group is independently substituted by or is not substituted by a group selected from -CH=CH-, a divalent carbocyclic ring and a divalent heterocyclic ring, and is substituted by or is not substituted by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH- or -NH-, provided that they are not adjacent to each other,
[0123] J is an organic group represented by any one of the following formulae,
[0124]
Compound 18
[0125]
[0126] (In the formulas [W], [Y], and [Z], * represents a bonding site with T2, Ar represents an aromatic hydrocarbon group selected from phenylene, naphthylene, and biphenylene groups which may have an organic group and / or a halogen atom as a substituent, and R 9 and R 10 Each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and Q represents any of the following structures;
[0127]
Compound 19
[0128]
[0129] (Where R 11 represents -CH2-, -NR-, -O- or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a site bonded to a portion other than Q of the compound molecule)
[0130] R 12represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms).
[0131] The bonding positions of the two amino groups (-NH2) in the above formula (7) are not limited. Specifically, relative to the bonding group of the side chain, the positions 2,3, 2,4, 2,5, 2,6, 3,4, and 3,5 on the benzene ring can be cited. Among them, from the viewpoint of reactivity when synthesizing polyamic acid, the positions 2,4, 2,5, or 3,5 are preferred. If the ease of synthesizing diamine is also considered, the positions 2,4 or 3,5 are more preferred.
[0132] In particular, in view of ease of synthesis, high versatility, properties, etc., a structure represented by any of the following formulae is most preferred, but the present invention is not limited thereto.
[0133]
Compound 20
[0134]
[0135] (where n is an integer from 2 to 8)
[0136] The above-mentioned diamines may be used alone or in combination of two or more, depending on the liquid crystal orientation, polymerization reaction sensitivity, voltage holding characteristics, stored charge and other characteristics when used as a radical generating film.
[0137] The diamine having such a radical polymerization-generating site is preferably used in an amount of 5 to 50 mol %, more preferably 10 to 40 mol %, and particularly preferably 15 to 30 mol % based on the total diamine component used for polymer synthesis contained in the radical generating film-forming composition.
[0138] Furthermore, when the polymer used for the radical generating film of the present invention is obtained from a diamine, other diamines other than the above-mentioned diamine having a radical generating site may be used in combination as a diamine component unless the effects of the present invention are impaired. Specific examples thereof include p-phenylenediamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,5-dimethyl-p-phenylenediamine, m-phenylenediamine, 2,4-dimethyl-m-phenylenediamine, 2,5-diaminotoluene, 2,6-diaminotoluene, 2,5-diaminophenol, 2,4-diaminophenol, 3,5-diaminophenol, 3,5-diaminobenzyl alcohol, 2,4-diaminobenzyl alcohol, 4,6-diaminoresorcinol, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 3,3'-dicarboxy-4 ,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-biphenyl, 3,3'-trifluoromethyl-4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 2,2'-diaminobiphenyl, 2,3'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,2'-diaminodiphenylmethane, 2,3'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 2,2'-diaminodiphenyl ether, 2,3'-diaminodiphenyl ether, 4, 4'-Sulfonyl diphenylamine, 3,3'-Sulfonyl diphenylamine, bis(4-aminophenyl)silane, bis(3-aminophenyl)silane, dimethyl-bis(4-aminophenyl)silane, dimethyl-bis(3-aminophenyl)silane, 4,4'-thiodiphenylamine, 3,3'-thiodiphenylamine, 4,4'-diaminodiphenylamine, 3,3'-diaminodiphenylamine, 3,4'-diaminodiphenylamine, 2,2'-diaminodiphenylamine, 2,3'-diaminodiphenylamine, N-methyl(4,4'-diaminodiphenyl)amine, N-methyl(3,3'-diaminodiphenyl)amine, N-methyl(3,4'-diaminodiphenyl)amine, N-methyl(2 ,2'-diaminodiphenyl)amine, N-methyl (2,3'-diaminodiphenyl)amine, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 1,4-diaminonaphthalene, 2,2'-diaminobenzophenone, 2,3'-diaminobenzophenone, 1,5-diaminonaphthalene, 1,6-diaminonaphthalene, 1,7-diaminonaphthalene, 1,8-diaminonaphthalene, 2,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,7-diaminonaphthalene, 2,8-diaminonaphthalene, 1,2-bis(4-aminophenyl)ethane, 1,2-bis(3-aminophenyl)ethane, 1,3-bis(4-aminophenyl)propane, 1,3-Bis(3-aminophenyl)propane, 1,4-bis(4-aminophenyl)butane, 1,4-bis(3-aminophenyl)butane, bis(3,5-diethyl-4-aminophenyl)methane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(4-aminobenzyl)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-[1,4-phenylenebis(methylene)]diphenylamine, 4,4'-[1,3-phenylenebis(methylene)]diphenylamine, 3,4'-[1,4-phenylenebis(methylene)]diphenylamine, 3,4'-[1,3-phenylenebis(methylene)]diphenylamine 1,3-phenylenebis(3-aminophenyl)ketone], 1,4-phenylenebis(4-aminobenzoate), 1,4-phenylenebis(3-aminobenzoate), 1,3-phenylenebis(4-aminobenzoate), 1,3-phenylenebis(3-aminobenzoate), bis(4-aminobenzoate), bis(4-aminophenyl)terephthalate, bis(3-aminophenyl)terephthalate, bis(4-aminophenyl)terephthalate, Bis(4-aminophenyl)phthalate, bis(3-aminophenyl)isophthalate, N,N'-(1,4-phenylene)bis(4-aminobenzamide), N,N'-(1,3-phenylene)bis(4-aminobenzamide), N,N'-(1,4-phenylene)bis(3-aminobenzamide), N,N'-(1,3-phenylene)bis(3-aminobenzamide), N,N'-bis(4-aminophenyl)terephthalamide, N,N'-bis(3-aminophenyl)terephthalamide, N,N'-bis(4-aminophenyl)isophthalamide, N,N'-bis(3-aminophenyl)isophthalamide, 9,10-bis(4-aminophenyl)anthracene, 4,4'-bis(4-aminophenoxy) 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis(4-aminophenyl)hexafluoropropane, 2,2'-bis(3-aminophenyl)hexafluoropropane, 2,2'-bis(3-amino-4-methylphenyl)hexafluoropropane, 2,2'-bis(4-aminophenyl)propane, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(3-amino-4-methylphenyl)propane, trans-1,4-bis(4-aminophenyl)cyclohexane, 3,5-diaminobenzoic acid, 2,5-diaminobenzoic acid, bis(4-aminophenoxy)methane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,3-bis(3-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,4-bis(3-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,5-bis(3-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,6-bis(3-aminophenoxy)hexane, 1,7-bis(4-aminophenoxy)heptane, 1,7-bis(3-aminophenoxy) )heptane, 1,8-bis(4-aminophenoxy)octane, 1,8-bis(3-aminophenoxy)octane, 1,9-bis(4-aminophenoxy)nonane, 1,9-bis(3-aminophenoxy)nonane, 1,10-bis(4-aminophenoxy)decane, 1,10-bis(3-aminophenoxy)decane, 1,11-bis(4-aminophenoxy)undecane, 1,11-bis(3-aminophenoxy)undecane, 1,12-bis(4-aminophenoxy)dodecane , 1,12-bis(3-aminophenoxy)dodecane and other aromatic diamines; bis(4-aminocyclohexyl)methane, bis(4-amino-3-methylcyclohexyl)methane and other alicyclic diamines; 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diamino Aliphatic diamines such as dodecane; diamines with urea structure such as 1,3-bis[2-(p-aminophenyl)ethyl]urea and 1,3-bis[2-(p-aminophenyl)ethyl]-1-tert-butoxycarbonylurea; diamines with nitrogen-containing unsaturated heterocyclic structure such as N-p-aminophenyl-4-p-aminophenyl(tert-butoxycarbonyl)aminomethylpiperidine; diamines with N-Boc group such as N-tert-butoxycarbonyl-N-(2-(4-aminophenyl)ethyl)-N-(4-aminobenzyl)amine, etc.
[0139] The above other diamines may be used alone or in combination of two or more, depending on the liquid crystal orientation, polymerization reaction sensitivity, voltage holding characteristics, stored charge and other characteristics when forming a radical generating film.
[0140] In the synthesis when the polymer is a polyamic acid, the tetracarboxylic dianhydride reacted with the above-mentioned diamine component is not particularly limited. Specifically, pyromellitic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 1,2,5,6-naphthalenetetracarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, 2,3,6,7-anthracenetetracarboxylic acid, 1,2,5,6-anthracenetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, bis(3,4-dicarboxyphenyl)ether, 3,3',4,4'-benzophenonetetracarboxylic acid, bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)methane, 2,2-bis(3,4-dicarboxyphenyl)propane, 1,1,1,3,3,3-hexafluoro-2,2-bis(3,4-dicarboxyphenyl)propane alkane, bis(3,4-dicarboxyphenyl)dimethylsilane, bis(3,4-dicarboxyphenyl)diphenylsilane, 2,3,4,5-pyridinetetracarboxylic acid, 2,6-bis(3,4-dicarboxyphenyl)pyridine, 3,3',4,4'-diphenylsulfonetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, 1,3-diphenyl-1,2,3,4-cyclobutanetetracarboxylic acid, oxydiphthalic acid, 1,2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, 1,2,4,5-cyclohexanetetracarboxylic acid, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic acid, 1,2-dimethyl-1,2,3,4-cyclo Butanetetracarboxylic acid, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic acid, 1,2,3,4-cycloheptanetetracarboxylic acid, 2,3,4,5-tetrahydrofurantetracarboxylic acid, 3,4-dicarboxy-1-cyclohexylsuccinic acid, 2,3,5-tricarboxycyclopentylacetic acid, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalenesuccinic acid, bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic acid, bicyclo[4,3,0]nonane-2,4,7,9-tetracarboxylic acid, bicyclo[4,4,0]decane-2,4,7,9-tetracarboxylic acid, bicyclo[4,4,0]decane-2,4,8,10-tetracarboxylic acid, tricyclo[6.3.0. Dianhydrides of tetracarboxylic acids such as 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid, bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic acid, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexane-1,2-dicarboxylic acid, tetracyclo[6,2,1,1,0<2,7>]dodecane-4,5,9,10-tetracarboxylic acid, 3,5,6-tricarboxynorbornane-2:3,5:6-dicarboxylic acid and 1,2,4,5-cyclohexanetetracarboxylic acid.
[0141] Of course, one or more tetracarboxylic dianhydrides may be used in combination depending on the liquid crystal orientation, polymerization reaction sensitivity, voltage holding characteristics, stored charge and other characteristics when used as a radical generating film.
[0142] In the synthesis when the polymer is polyamic acid ester, the structure of the tetracarboxylic acid dialkyl ester reacted with the above-mentioned diamine component is not particularly limited, and specific examples thereof are given below.
[0143] Specific examples of the aliphatic tetracarboxylic acid diester include 1,2,3,4-cyclobutanetetracarboxylic acid dialkyl ester, 1,2-dimethyl-1,2,3,4-cyclobutanetetracarboxylic acid dialkyl ester, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic acid dialkyl ester, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic acid dialkyl ester, 1,2,3,4-cyclopentanetetracarboxylic acid dialkyl ester, 2,3,4,5-tetrahydrofurantetracarboxylic acid dialkyl ester, 1,2,4,5-cyclohexanetetracarboxylic acid dialkyl ester, 3,4-dicarboxy-1-cyclohexylsuccinic acid dialkyl ester, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalenesuccinic acid dialkyl ester, 1,2,3,4-butanetetracarboxylic acid dialkyl ester, bicyclo[3,3,0 ] octane-2,4,6,8-tetracarboxylic acid dialkyl ester, 3,3',4,4'-dicyclohexyltetracarboxylic acid dialkyl ester, 2,3,5-tricarboxycyclopentylacetic acid dialkyl ester, cis-3,7-dibutylcycloocta-1,5-diene-1,2,5,6-tetracarboxylic acid dialkyl ester, tricyclo[4.2.1.0<2,5>]nonane-3,4,7,8-tetracarboxylic acid 3 ,4:7,8-dialkyl ester, hexacyclo[6.6.0.1<2,7>.0<3,6>.1<9,14>.0<10,13>]hexadecane-4,5,11,12-tetracarboxylic acid 4,5:11,12-dialkyl ester, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid dialkyl ester, etc.
[0144] Examples of the aromatic tetracarboxylic acid dialkyl esters include pyromellitic acid dialkyl esters, 3,3',4,4'-biphenyltetracarboxylic acid dialkyl esters, 2,2',3,3'-biphenyltetracarboxylic acid dialkyl esters, 2,3,3',4-biphenyltetracarboxylic acid dialkyl esters, 3,3',4,4'-benzophenonetetracarboxylic acid dialkyl esters, 2,3,3',4'-benzophenonetetracarboxylic acid dialkyl esters, bis(3,4-dicarboxyphenyl)ether dialkyl esters, bis(3,4-dicarboxyphenyl)sulfone dialkyl esters, 1,2,5,6-naphthalenetetracarboxylic acid dialkyl esters, and 2,3,6,7-naphthalenetetracarboxylic acid dialkyl esters.
[0145] In the synthesis when the polymer is polyurea, the diisocyanate to be reacted with the diamine component is not particularly limited, and can be used depending on availability, etc. The specific structure of the diisocyanate is shown below.
[0146]
Compound 21
[0147]
[0148] In the formula, R2 and R3 represent aliphatic hydrocarbons having 1 to 10 carbon atoms.
[0149] The aliphatic diisocyanates represented by K-1 to K-5 have poor reactivity, but have the advantage of improving solvent solubility. The aromatic diisocyanates represented by K-6 to K-7 have the effect of being rich in reactivity and improving heat resistance, but have the disadvantage of reducing solvent solubility. In terms of versatility and characteristics, K-1, K-7, K-8, K-9, and K-10 are particularly preferred. From the viewpoint of electrical characteristics, K-12 is particularly preferred. From the viewpoint of liquid crystal orientation, K-13 is particularly preferred. Diisocyanates may also be used in combination of more than one, preferably for various applications according to the desired characteristics.
[0150] Furthermore, part of the diisocyanate may be replaced with the above-described tetracarboxylic dianhydride, and the polyamide acid and polyurea copolymer may be used. The polyamide acid and polyurea copolymer may also be used by chemical imidization.
[0151] In the synthesis when the polymer is a polyamide, the structure of the dicarboxylic acid to be reacted is not particularly limited, and specific examples are given below. Specific examples of aliphatic dicarboxylic acids include malonic acid, oxalic acid, dimethylmalonic acid, succinic acid, fumaric acid, glutaric acid, adipic acid, succinic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, 2,2-dimethylglutaric acid, 3,3-diethylsuccinic acid, azelaic acid, sebacic acid, and suberic acid.
[0152] Examples of the alicyclic dicarboxylic acid include 1,1-cyclopropanedicarboxylic acid, 1,2-cyclopropanedicarboxylic acid, 1,1-cyclobutanedicarboxylic acid, 1,2-cyclobutanedicarboxylic acid, 1,3-cyclobutanedicarboxylic acid, 3,4-diphenyl-1,2-cyclobutanedicarboxylic acid, 2,4-diphenyl-1,3-cyclobutanedicarboxylic acid, 1-cyclobutene-1,2-dicarboxylic acid, 1-cyclobutene-3,4-dicarboxylic acid, 1,1-cyclopentanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,1-cyclohexanedicarboxylic acid, and 1,2-cyclohexanedicarboxylic acid. dicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,4-(2-norbornene)dicarboxylic acid, norbornene-2,3-dicarboxylic acid, bicyclo[2.2.2]octane-1,4-dicarboxylic acid, bicyclo[2.2.2]octane-2,3-dicarboxylic acid, 2,5-dioxo-1,4-bicyclo[2.2.2]octanedicarboxylic acid, 1,3-adamantanedicarboxylic acid, 4,8-dioxo-1,3-adamantanedicarboxylic acid, 2,6-spiro[3.3]heptanedicarboxylic acid, 1,3-adamantanedicarboxylic acid, camphoric acid, and the like.
[0153] Examples of the aromatic dicarboxylic acid include phthalic acid, isophthalic acid, terephthalic acid, 5-methylisophthalic acid, 5-tert-butylisophthalic acid, 5-aminoisophthalic acid, 5-hydroxyisophthalic acid, 2,5-dimethylterephthalic acid, tetramethylterephthalic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-anthracenedicarboxylic acid, 1,4-anthraquinonedicarboxylic acid, 2,5-biphenyldicarboxylic acid, 4 ,4'-biphenyl dicarboxylic acid, 1,5-biphenyl dicarboxylic acid, 4,4"-terphenyl dicarboxylic acid, 4,4'-diphenyl methane dicarboxylic acid, 4,4'-diphenyl ethane dicarboxylic acid, 4,4'-diphenyl propane dicarboxylic acid, 4,4'-diphenyl hexafluoro propane dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, 4,4'-bibenzyl dicarboxylic acid, 4,4'-stilbene dicarboxylic acid, 4,4'-diphenyl ethynyl dicarboxylic acid (4,4'-tolandicarboxylic dicarboxylic acids such as 4,4'-diphenylene glycol, ...
[0154] Examples of the dicarboxylic acid containing a heterocyclic ring include 1,5-(9-oxofluorene)dicarboxylic acid, 3,4-furandicarboxylic acid, 4,5-thiazoledicarboxylic acid, 2-phenyl-4,5-thiazoledicarboxylic acid, 1,2,5-thiadiazole-3,4-dicarboxylic acid, 1,2,5-oxadiazole-3,4-dicarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 2,5-pyridinedicarboxylic acid, 2,6-pyridinedicarboxylic acid, 3,4-pyridinedicarboxylic acid, and 3,5-pyridinedicarboxylic acid.
[0155] The above-mentioned various dicarboxylic acids can be dicarboxylic acids of acid dihalides or acid anhydrides. From the aspect of maintaining the orientation of liquid crystal molecules, these dicarboxylic acids are particularly preferably dicarboxylic acids that can give polyamides of linear structures. Among them, terephthalic acid, isophthalic acid, 1,4-cyclohexanedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 4,4'-diphenylmethanedicarboxylic acid, 4,4'-diphenylethanedicarboxylic acid, 4,4'-diphenylpropanedicarboxylic acid, 4,4'-diphenylhexafluoropropanedicarboxylic acid, 2,2-bis(phenyl)propanedicarboxylic acid, 4,4-terphenyldicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,5-pyridinedicarboxylic acid or their acid dihalides are preferably used. These compounds sometimes have isomers, or mixtures containing them. In addition, more than two compounds can also be used in combination. It should be noted that the dicarboxylic acids used in the present invention are not limited to the above-mentioned exemplified compounds.
[0156] When polyamic acid, polyamic acid ester, polyurea, and polyamide are obtained by reacting a diamine as a raw material (also recorded as "diamine component") with a component selected from tetracarboxylic dianhydride (also recorded as "tetracarboxylic dianhydride component"), a tetracarboxylic diester, a diisocyanate, and a dicarboxylic acid as a raw material, a known synthesis means can be used. Generally speaking, it is a method for reacting a diamine component with one or more components selected from tetracarboxylic dianhydride components, tetracarboxylic diesters, diisocyanates, and dicarboxylic acids in an organic solvent.
[0157] The reaction of the diamine component and the tetracarboxylic dianhydride component is advantageous in that it is relatively easy to proceed in an organic solvent and no by-product is generated.
[0158] As the organic solvent used for the above-mentioned reaction, there is no particular limitation as long as it is an organic solvent that dissolves the generated polymer. Furthermore, even if it is an organic solvent that does not dissolve the polymer, it can be mixed with the above-mentioned solvent in the range that the generated polymer does not precipitate. It should be noted that since the moisture in the organic solvent becomes the cause of hindering the polymerization reaction and hydrolyzing the generated polymer, the organic solvent is preferably an organic solvent that has been dehydrated.
[0159] Examples of the organic solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N,N-dimethylpropaneamide, N-methylcaprolactam, dimethyl sulfoxide, tetramethyl urea, pyridine, dimethyl sulfone, hexamethyl sulfoxide, γ-butyrolactone, isopropyl alcohol, methoxymethylpentanol, dipentene, ethyl 1-Butyl ketone, ... Diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, dioxane, n-hexane, n- Pentane, n-octane, diethyl ether, cyclohexanone, ethylene carbonate, propylene carbonate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol monoethyl acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, diethylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, 2-ethyl-1-hexanol, etc. These organic solvents may be used alone or in combination.
[0160] When the diamine component and the tetracarboxylic dianhydride component are reacted in an organic solvent, the following methods can be cited: a method of stirring a solution obtained by dispersing or dissolving the diamine component in an organic solvent, and adding the tetracarboxylic dianhydride component directly or by dispersing or dissolving it in an organic solvent; a method of adding the diamine component to a solution obtained by dispersing or dissolving the tetracarboxylic dianhydride component in an organic solvent; a method of alternately adding the tetracarboxylic dianhydride component and the diamine component, etc. Any of these methods can be used. In addition, when the diamine component or the tetracarboxylic dianhydride component is composed of a plurality of compounds, they can be reacted in a pre-mixed state, or they can be reacted in sequence, or the low molecular weight bodies obtained by the separate reactions can be further mixed to form a high molecular weight body.
[0161] The temperature for reacting the diamine component and the tetracarboxylic dianhydride component can be selected at any temperature, for example, in the range of -20 to 100° C., preferably -5 to 80° C. The reaction can be performed at any concentration, for example, the total amount of the diamine component and the tetracarboxylic dianhydride component is 1 to 50% by mass, preferably 5 to 30% by mass, relative to the reaction solution.
[0162] The ratio of the total molar number of the tetracarboxylic dianhydride component to the total molar number of the diamine component in the above-mentioned polymerization reaction can be selected as an arbitrary value according to the molecular weight of the polyamic acid to be obtained. As in the usual polycondensation reaction, the closer the molar ratio is to 1.0, the greater the molecular weight of the generated polyamic acid. As a preferred range, it is 0.8 to 1.2.
[0163] The method for synthesizing the polymer used in the present invention is not limited to the above method. In the case of synthesizing polyamic acid, it is the same as the synthesis method of common polyamic acid, and the above-mentioned tetracarboxylic dianhydride is replaced with tetracarboxylic acid or tetracarboxylic acid dihalide and other tetracarboxylic acid derivatives of the corresponding structure, and a known method is used to react to obtain the corresponding polyamic acid. In addition, in the case of synthesizing polyurea, diamines are reacted with diisocyanates. When manufacturing polyamic acid esters or polyamides, diamines are reacted with components selected from tetracarboxylic acid diesters and dicarboxylic acids in the presence of a known condensing agent, or after being derived into acid halides using a known method, it is reacted with diamines.
[0164] As a method for making polyimide by imidizing the above-mentioned polyamic acid, thermal imidization by directly heating a solution of polyamic acid and catalytic imidization by adding a catalyst to a solution of polyamic acid can be cited. It should be noted that from the viewpoint of improving the voltage holding rate, the imidization rate of polyamic acid to polyimide is preferably more than 30%, more preferably 30 to 99%. On the other hand, from the viewpoint of whitening characteristics, that is, the viewpoint of suppressing the precipitation of polymers in varnish, it is preferably less than 70%. Considering the two characteristics, it is more preferably 40 to 80%.
[0165] The temperature when the polyamic acid is thermally imidized in a solution is usually 100 to 400° C., preferably 120 to 250° C., and the imidization reaction is preferably carried out while removing water generated by the imidization reaction to the outside of the system.
[0166] The catalytic imidization of polyamic acid can be carried out by adding a basic catalyst and anhydride to a solution of polyamic acid, usually stirring at -20 to 250°C, preferably at 0 to 180°C. The amount of the basic catalyst is usually 0.5 to 30 times the molar amount of the amic acid group, preferably 2 to 20 times the molar amount, and the amount of the anhydride is usually 1 to 50 times the molar amount of the amic acid group, preferably 3 to 30 times the molar amount. As a basic catalyst, pyridine, triethylamine, trimethylamine, tributylamine, trioctylamine, etc. can be mentioned, among which pyridine has the appropriate alkalinity for the reaction to proceed, so it is preferred. As anhydrides, acetic anhydride, trimellitic anhydride, pyromellitic anhydride, etc. can be mentioned, among which, if acetic anhydride is used, the purification after the reaction is completed becomes easy, so it is preferred. The imidization rate based on catalytic imidization can be controlled by adjusting the amount of catalyst, reaction temperature, reaction time, etc.
[0167] In the case of recovering the generated polymer from the reaction solution of the polymer, the reaction solution can be put into a poor solvent to precipitate it. As the poor solvent used in the precipitation generation, methanol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, benzene, water, etc. can be mentioned. The polymer put into the poor solvent to precipitate can be filtered and recovered, and then dried at normal pressure or reduced pressure, at room temperature or heated. In addition, if the operation of re-dissolving the polymer recovered by precipitation in an organic solvent and re-precipitating and recovering is repeated 2 to 10 times, the impurities in the polymer can be reduced. As the poor solvent at this time, for example, alcohols, ketones, hydrocarbons, etc. can be mentioned. If more than 3 poor solvents selected from them are used, the efficiency of purification is further improved, so it is preferred.
[0168] In addition, when the radical generating film contains a polymer containing an organic group that induces radical polymerization, the radical generating film forming composition used in the present invention may contain other polymers in addition to the polymer containing an organic group that induces radical polymerization. In this case, the content of the other polymer in the total polymer component is preferably 5 to 95% by mass, more preferably 30 to 70% by mass.
[0169] Taking into account the strength of the free radical generating film obtained by coating the free radical generating film, the workability during film formation, the uniformity of the film, etc., the molecular weight of the polymer possessed by the free radical generating film forming composition is preferably 5,000 to 1,000,000, and more preferably 10,000 to 150,000, based on the weight average molecular weight measured by the GPC (Gel Permeation Chromatography) method.
[0170] As the polymer used in the free radical generating film of the present invention, when the composition of the compound having a group generating free radicals and the polymer is applied and cured to form a film, and then fixed in the film, at least one polymer selected from the polyimide precursor produced by the above-mentioned production method, and polyimide, polyurea, polyamide, polyacrylate, polymethacrylate, etc. can be used, and the above polymer is obtained using a diamine component, and the above diamine component is a diamine component having a site for generating free radical polymerization, and the diamine component accounts for 0 mol% of the total diamine components in the synthesis of the polymer contained in the composition for forming the free radical generating film. As the compound having a group generating free radicals added at this time, the following can be mentioned.
[0171] The compound that generates free radicals by heat is a compound that generates free radicals by heating to a temperature higher than the decomposition temperature. Examples of the above-mentioned free radical thermal polymerization initiator include ketone peroxides (methyl ethyl ketone peroxide, cyclohexanone peroxide, etc.), diacyl peroxides (acetyl peroxide, benzoyl peroxide, etc.), hydroperoxides (hydrogen peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, etc.), dialkyl peroxides (di-tert-butyl peroxide, dicumyl peroxide, dilauroyl peroxide, etc.), peroxyacetals (dibutyl peroxide cyclohexane, etc.), peroxyalkyl esters (tert-butyl peroxyneodecanoate, tert-butyl peroxypivalate, tert-amyl peroxy 2-ethylcyclohexane, etc.), persulfates (potassium persulfate, sodium persulfate, ammonium persulfate, etc.), and azo compounds (azobisisobutyronitrile and 2,2'-bis(2-hydroxyethyl)azobisisobutyronitrile, etc.). Such radical thermal polymerization initiators may be used alone or in combination of two or more.
[0172] As a compound that generates free radicals by light, there is no particular limitation as long as it is a compound that initiates free radical polymerization by light irradiation. As such a free radical photopolymerization initiator, benzophenone, Michler's ketone, 4,4'-bis(diethylamino)benzophenone, xanthone, thioxanthone, isopropylxanthone, 2,4-diethylthioxanthone, 2-ethylanthraquinone, acetophenone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-2-methyl-4'-isopropylpropiophenone, 1-hydroxycyclohexyl phenyl ketone, isopropylbenzoin ether, isobutylbenzoin ether, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, camphorquinone, benzanthraquinone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl) ... 4-Dimethylaminobenzoic acid ethyl ester, 4-Dimethylaminobenzoic acid isopentyl ester, 4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4,4'-tri(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-(4'-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(3',4'-dimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2',4'-dimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2'-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4' -pentyloxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 4-[p-N,N-bis(ethoxycarbonylmethyl)]-2,6-bis(trichloromethyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(2'-chlorophenyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(4'-methoxyphenyl)-s-triazine, 2-(p-dimethylaminophenyl)benzoxazole, 2-(p-dimethylaminophenyl)benzothiazole, 2-mercaptobenzothiazole, 3,3'-carbonylbis(7-diethylaminocoumarin), 2-(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2-chlorophenyl)-4,4 ',5,5'-Tetrakis(4-ethoxycarbonylphenyl)-1,2'-biimidazole, 2,2'-bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4-dibromophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 3-(2-methyl-2-dimethylaminopropionyl)carbazole, 3,6-bis(2-methyl-2-morpholinopropionyl)-9-n-dodecylcarbazole, 1-hydroxycyclohexyl phenyl ketone, bis(5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-hexylperoxycarbonyl)benzophenone, 3,3'-di(methoxycarbonyl)-4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4'-di(methoxycarbonyl)-4,3'-di(tert-butylperoxycarbonyl)benzophenone, 4,4'-di(methoxycarbonyl)-3,3'-di(tert-butylperoxycarbonyl)benzophenone, 2-(3-methyl-3H-benzothiazol-2-ylidene)-1-naphth-2-yl-ethanone or 2-(3-methyl-1,3-benzothiazol-2(3H)-ylidene)-1-(2-benzoyl)ethanone, etc. These compounds may be used alone or in combination of two or more.
[0173] In addition, when the radical generating film contains a polymer containing an organic group that induces radical polymerization, the compound having a group that generates radicals may be contained in order to promote radical polymerization when energy is applied.
[0174] The free radical generation film forming composition may contain organic solvents containing other components other than the free radical generating agent used as needed and dissolved or dispersed polymer components. Such organic solvents are not particularly limited, and for example, the organic solvents exemplified in the synthesis of the above-mentioned polyamic acid can be cited. Among them, from the viewpoint of solubility, preferably N-methyl-2-pyrrolidone, γ-butyrolactone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, 3-methoxy-N, N-dimethylpropaneamide, etc. are particularly preferred. Particularly preferably, N-methyl-2-pyrrolidone or N-ethyl-2-pyrrolidone, two or more mixed solvents can also be used.
[0175] Furthermore, it is preferred to use a solvent that improves the uniformity and smoothness of the coating film and an organic solvent in which the components of the radical-generating film-forming composition have high solubility as a mixture.
[0176] Examples of the solvent for improving the uniformity and smoothness of the coating film include isopropyl alcohol, methoxymethylpentyl alcohol, methyl cellosolve, ethyl cellosolve, butyl cellosolve, methyl cellosolve acetate, butyl cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethyl carbitol acetate, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol monobutyl ether, propylene glycol tert-butyl ether, and the like. Ether, dipropylene glycol monomethyl ether, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, di ...ethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate Isobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methyl cyclohexene, propyl ether, dihexyl ether, n-hexane, n-pentane, n-octane, diethyl ether, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol acetate monoethyl ether, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, 3-methoxybutyl propionate, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 1-butoxy-2-propanol, 1-phenoxy-2-propanol, propylene glycol monoacetate, propylene glycol diacetate, propylene glycol-1-monomethyl ether-2-acetate, propylene glycol-1-monoethyl ether-2-acetate, dipropylene glycol, 2-(2-ethoxypropoxy) propanol, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isopentyl lactate, 2-ethyl-1-hexanol, etc. These solvents can be mixed in multiple ways. When using these solvents, it is preferably 5 to 80% by mass of the total solvent contained in the liquid crystal alignment agent, and more preferably 20 to 60% by mass.
[0177] The radical-generating film-forming composition may contain ingredients other than those mentioned above, and examples thereof include compounds that improve the uniformity of film thickness and surface smoothness when the radical-generating film-forming composition is applied, compounds that improve the adhesion between the radical-generating film-forming composition and the substrate, and compounds that further improve the film strength of the radical-generating film-forming composition.
[0178] As compounds that improve the uniformity of film thickness and surface smoothness, fluorine-based surfactants, silicone-based surfactants, nonionic surfactants, etc. can be cited. More specifically, for example, Eftop EF301, EF303, EF352 (manufactured by Tohkem Products Co., Ltd.), MEGAFAC F171, F173, R-30 (manufactured by Dainippon Ink Co., Ltd.), FLUORAD FC430, FC431 (manufactured by Sumitomo 3M Co., Ltd.), AsahiGuard AG710, SURFLON S-382, SC101, SC102, SC103, SC104, SC105, SC106 (manufactured by Asahi Glass Co., Ltd.), etc. can be cited. When using these surfactants, the use ratio thereof is preferably 0.01 to 2 parts by mass, and more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of the total amount of the polymer contained in the free radical generating film-forming composition.
[0179] Specific examples of compounds that improve the adhesion between the radical-generating film-forming composition and the substrate include compounds containing functional silanes and compounds containing epoxy groups. For example, 3-aminopropyl trimethoxysilane, 3-aminopropyl triethoxysilane, 2-aminopropyl trimethoxysilane, 2-aminopropyl triethoxysilane, N-(2-aminoethyl)-3-aminopropyl trimethoxysilane, N-(2-aminoethyl)-3-aminopropyl methyl dimethoxysilane, 3-ureidopropyl trimethoxysilane, 3-ureidopropyl triethoxysilane, N-ethoxycarbonyl-3-aminopropyl trimethoxysilane, N-ethoxycarbonyl-3-aminopropyl triethoxysilane, and the like are mentioned. Alkane, N-triethoxysilylpropyl triethylenetriamine, N-trimethoxysilylpropyl triethylenetriamine, 10-trimethoxysilyl-1,4,7-triazadecane, 10-triethoxysilyl-1,4,7-triazadecane, 9-trimethoxysilyl-3,6-diazanonyl acetate, 9-triethoxysilyl-3,6-diazanonyl acetate, N-benzyl-3-aminopropyl trimethoxysilane, N-benzyl-3-aminopropyl triethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, N-bis(ethylene oxide)-3-aminopropyltrimethoxysilane, N-bis(ethylene oxide)-3-aminopropyltriethoxysilane, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol diglycidyl ether, 2 ,2-dibromoneopentyl glycol diglycidyl ether, 1,3,5,6-tetraglycidyl-2,4-hexanediol, N,N,N',N'-tetraglycidyl-m-phenylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, 3-(N-allyl-N-glycidyl)aminopropyltrimethoxysilane, 3-(N,N-diglycidyl)aminopropyltrimethoxysilane, etc.
[0180] In order to further improve the film strength of the radical generating film, phenol compounds such as 2,2'-bis(4-hydroxy-3,5-dihydroxymethylphenyl)propane and tetrakis(methoxymethyl)bisphenol may be added. When these compounds are used, the amount is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, relative to 100 parts by mass of the total amount of the polymer contained in the radical generating film forming composition.
[0181] Furthermore, in addition to the above, a dielectric or conductive substance for changing the electrical properties such as the dielectric constant and conductivity of the radical generating film may be added to the radical generating film forming composition as long as the effects of the present invention are not impaired.
[0182] [Free Radical Generating Film]
[0183] The radical generating film of the present invention is obtained by using the above-mentioned radical generating film forming composition. For example, a cured film obtained by applying the radical generating film forming composition used in the present invention to a substrate, drying and sintering the cured film can also be used directly as a radical generating film. In addition, the cured film can also be rubbed, or irradiated with polarized light or light of a specific wavelength, or treated with ion beams, or irradiated with UV on a liquid crystal display element filled with liquid crystal as an alignment film for PSA.
[0184] The substrate to which the radical-generating film-forming composition is applied is not particularly limited as long as it is a substrate with high transparency, but is preferably a substrate on which a transparent electrode for driving liquid crystal is formed.
[0185] If specific examples are given, there can be mentioned substrates in which transparent electrodes are formed on glass plates, polycarbonate, poly(meth)acrylate, polyethersulfone, polyarylate, polyurethane, polysulfone, polyether, polyetherketone, trimethylpentene, polyolefin, polyethylene terephthalate, (meth)acrylonitrile, triacetyl cellulose, diacetyl cellulose, cellulose acetate butyrate and other plastic plates.
[0186] On a substrate that can be used for an IPS-type liquid crystal display element, an electrode pattern such as a standard IPS comb-tooth electrode, a PSA herringbone electrode, or a protrusion pattern such as an MVA can also be used.
[0187] In addition, in a high-performance element such as a TFT type element, a component in which an element such as a transistor is formed between an electrode for driving liquid crystal and a substrate can be used.
[0188] When a transmissive liquid crystal display element is used as the target, the substrate as described above is usually used, but when a reflective liquid crystal display element is used as the target, an opaque substrate such as a silicon wafer can also be used if only a single-sided substrate is used. In this case, a material such as aluminum that reflects light can also be used in the electrode formed on the substrate.
[0189] Examples of the method for coating the radical generating film-forming composition include spin coating, printing, ink jetting, spraying, and roll coating. Transfer printing is widely used industrially from the viewpoint of productivity and is also preferably used in the present invention.
[0190] The drying process after applying the radical generating film forming composition is not necessarily necessary, but when the time from application to sintering is not uniform for each substrate or when sintering is not performed immediately after application, it is preferred to include a drying process. The drying process is not particularly limited as long as the solvent is removed to the extent that the shape of the coating film is not deformed due to the transportation of the substrate, etc. For example, the following method can be cited: drying on a hot plate at a temperature of 40°C to 150°C, preferably 60°C to 100°C for 0.5 to 30 minutes, preferably 1 to 5 minutes.
[0191] The coating film formed by applying the free radical generating film-forming composition by the above method can be sintered to form a cured film. At this time, the sintering temperature can usually be carried out at any temperature of 100°C to 350°C, preferably 140°C to 300°C, more preferably 150°C to 230°C, and further preferably 160°C to 220°C. The sintering time can usually be sintered within any time of 5 minutes to 240 minutes. It is preferably 10 to 90 minutes, and more preferably 20 to 90 minutes. Heating can usually be carried out using known methods, such as a hot plate, a hot air circulation oven, an IR oven, a belt furnace, etc.
[0192] The thickness of the cured film can be selected as required, and when it is preferably more than 5 nm, more preferably more than 10 nm, the reliability of the liquid crystal display element can be easily obtained, so it is preferred. In addition, when the thickness of the cured film is preferably less than 300 nm, more preferably less than 150 nm, the power consumption of the liquid crystal display element will not become extremely large, so it is preferred.
[0193] The first substrate having the radical generating film can be obtained in the above manner, but the radical generating film can also be subjected to uniaxial orientation treatment. Examples of methods for uniaxial orientation treatment include photo-orientation, oblique deposition, friction, and uniaxial orientation treatment using a magnetic field.
[0194] In the case of performing the orientation treatment by rubbing treatment in one direction, for example, the substrate is moved in a manner such that the rubbing cloth contacts the film while a rubbing roller wound with the rubbing cloth is rotated. In the case of the first substrate of the present invention having comb-tooth electrodes formed thereon, the direction can be selected according to the electrical properties of the liquid crystal, but in the case of using liquid crystal having positive dielectric anisotropy, the rubbing direction is preferably set to be substantially the same direction as the extension direction of the comb-tooth electrodes.
[0195] As a process for making a zero anchoring part and a strong anchoring part, a method of irradiating radiation in an arbitrary pattern through a photomask or the like can be cited. This is a process in which the free radical generating part is eliminated by irradiating the free radical generating film with radiation in advance, and a zero anchoring state is not formed. As radiation when performing this step, polarized light or light of a specific wavelength, ion beam, etc. can be cited. It is particularly preferred to irradiate the light free radical generating part with light of a wavelength at which the absorbance of the corresponding part reaches the highest.
[0196] The second substrate of the present invention is the same as the first substrate except that it does not have a radical generating film, and is preferably a substrate having a conventionally known liquid crystal alignment film.
[0197] <Liquid Crystal Unit>
[0198] After forming a radical generating film on a substrate by the above method, the liquid crystal cell of the present invention is obtained by placing the substrate (first substrate) having the radical generating film and the known substrate (second substrate) having a liquid crystal alignment film so that the radical generating film and the liquid crystal alignment film face each other, clamping a spacer, fixing with a sealant, injecting a liquid crystal composition containing a liquid crystal and a radical polymerizable compound and sealing. At this time, the size of the spacer used is usually 1 to 30 μm, preferably 2 to 10 μm.
[0199] There is no particular limitation on the method of injecting a liquid crystal composition containing a liquid crystal and a free radical polymerizable compound, and examples thereof include: a vacuum method in which the pressure in the prepared liquid crystal unit is reduced and then a mixture containing a liquid crystal and a polymerizable compound is injected; a dropping method in which a mixture containing a liquid crystal and a polymerizable compound is dropped and then sealed.
[0200] <Liquid Crystal Composition Containing Liquid Crystal and Radical Polymerizable Compound>
[0201] In the preparation of the liquid crystal display element of the present invention, the polymerizable compound used with the liquid crystal is not particularly limited as long as it is a free radical polymerizable compound, for example, a compound having one or more polymerizable unsaturated bonds in one molecule. Preferably, it is a compound having one polymerizable unsaturated bond in one molecule (hereinafter, sometimes referred to as "a compound having a monofunctional polymerizable reactive group", "a compound having a monofunctional polymerizable reactive group", etc.). The polymerizable unsaturated bond is preferably a free radical polymerizable unsaturated bond, such as a vinyl bond.
[0202] At least one of the radical polymerizable compounds is preferably a compound having compatibility with liquid crystal and having one polymerizable unsaturated bond in one molecule, that is, a compound having a monofunctional radical polymerizable group.
[0203] Furthermore, the polymerizable reactive group of the radical polymerizable compound is preferably a polymerizable group selected from the following structures.
[0204]
Compound 22
[0205]
[0206] (wherein, * represents a site bonded to a portion other than a polymerizable unsaturated bond of a compound molecule; R b represents a straight-chain alkyl group having 2 to 8 carbon atoms, and E represents a single bond, -O-, -NR c -, -S-, ester bonds and amide bonds in the bonding group; R c represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms).
[0207] Furthermore, the liquid crystal composition containing a liquid crystal and a radical polymerizable compound preferably contains a radical polymerizable compound such that a polymer obtained by polymerizing the radical polymerizable compound has a Tg of 100° C. or less.
[0208] The compound having a monofunctional free radical polymerization reactive group has an unsaturated bond that can be free radically polymerized in the presence of an organic free radical, and examples thereof include methacrylate monomers such as tert-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, lauryl methacrylate, and n-octyl methacrylate; acrylate monomers such as tert-butyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, benzyl acrylate, lauryl acrylate, and n-octyl acrylate; styrene, styrene derivatives (e.g., o-, m-, p-methoxystyrene, o-, m-, p-tert-butoxystyrene, o-, m-, p-tert-butoxystyrene, o-, m-, p-tert-butoxystyrene, The present invention relates to vinyl monomers such as vinyl esters (e.g., vinyl acetate, vinyl propionate, vinyl benzoate, vinyl acetate, etc.), vinyl ketones (e.g., vinyl methyl ketone, vinyl hexyl ketone, methyl isopropenyl ketone, etc.), N-vinyl compounds (e.g., N-vinyl pyrrolidone, N-vinyl pyrrole, N-vinyl carbazole, N-vinyl indole, etc.), (meth) acrylic acid derivatives (e.g., acrylonitrile, methacrylonitrile, acrylamide, isopropyl acrylamide, methacrylamide, etc.), vinyl halides (e.g., vinyl chloride, vinylidene chloride, tetrachloroethylene, hexachlorobutadiene, vinyl fluoride, etc.), but are not limited to these. These various free radical polymerizable monomers can be used alone or in combination of two or more. In addition, these compounds are preferably compatible with liquid crystals.
[0209] The radical polymerizable compound is preferably a compound represented by the following formula (1).
[0210]
Compound 23
[0211]
[0212] In formula (1), R a and R b Each independently represents a linear alkyl group having 2 to 8 carbon atoms, and E represents a single bond, -O-, -NR c -, -S-, ester bonds, amide bonds, bonding groups, R c It represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0213] At least one of the radical polymerizable compounds is preferably a compound having compatibility with liquid crystal and having one polymerizable unsaturated bond in one molecule, that is, a compound having a monofunctional radical polymerizable group.
[0214] In addition, as the free radical polymerizable compound represented by the above formula (1), from the viewpoint of ease of synthesis, compatibility with liquid crystals, and polymerization reactivity, it is preferably a compound in which E is an ester bond (a bond represented by -C(=O)-O- or -OC(=O)-), and specifically preferably a compound having the following structure, without any particular restriction.
[0215]
Compound 24
[0216]
[0217] In the formulae (1-1) and (1-2), Ra and Rb each independently represent a linear alkyl group having 2 to 8 carbon atoms.
[0218] The liquid crystal composition containing a liquid crystal and a radical polymerizable compound preferably contains a radical polymerizable compound such that a polymer obtained by polymerizing the radical polymerizable compound has a Tg of 100° C. or less.
[0219] These various radical polymerizable monomers may be used alone or in combination of two or more. Furthermore, they preferably have compatibility with liquid crystals.
[0220] The content of the radical polymerizable compound in the liquid crystal composition is preferably 3% by mass or more, more preferably 5% by mass or more, and preferably 50% by mass or less, more preferably 20% by mass or less, based on the total mass of the liquid crystal and the radical polymerizable compound.
[0221] The Tg of the polymer obtained by polymerizing the radical polymerizable compound is preferably 100° C. or lower.
[0222] It should be noted that liquid crystal generally refers to a substance in a state showing both solid and liquid properties. Representative liquid crystal phases include nematic liquid crystal and smectic liquid crystal. The liquid crystal that can be used in the present invention is not particularly limited. If an example is given, it is 4-pentyl-4'-cyanobiphenyl.
[0223] Next, the liquid crystal cell into which the mixture (liquid crystal composition) containing the liquid crystal and the radical polymerizable compound is introduced is given energy sufficient to cause the radical polymerizable compound to undergo a polymerization reaction. This can be implemented, for example, by applying heat or UV irradiation, and the radical polymerizable compound is polymerized at that time, thereby exhibiting the desired characteristics. Among them, UV irradiation is preferred in that the use of UV can form an oriented pattern and that a polymerization reaction occurs in a short time.
[0224] The heating temperature during UV irradiation is preferably within the temperature range where the introduced liquid crystal exhibits liquid crystallinity, usually 40° C. or higher, and preferably below the temperature at which the liquid crystal enters the isotropic phase.
[0225] Here, the UV irradiation wavelength during UV irradiation is preferably selected to be a wavelength with the best reaction quantum yield of the polymerizable compound being reacted, and the UV irradiation amount is generally 0.01 to 30 J, preferably less than 10 J. A small UV irradiation amount can suppress the reduction in reliability of damage to components constituting the liquid crystal display, and can improve the production cycle in manufacturing by reducing the UV irradiation time, so it is preferred.
[0226] When polymerizing by heating without UV irradiation, heating is preferably performed at a temperature at which the polymerizable compound reacts, that is, at a temperature lower than the decomposition temperature of the liquid crystal, specifically, at 100° C. to 150° C., for example.
[0227] When sufficient energy is given to cause the radical polymerizable compound to undergo a polymerization reaction, a no-electric-field state in which no voltage is applied is preferred.
[0228] <Liquid Crystal Display Element>
[0229] A liquid crystal display element can be produced using the liquid crystal cell obtained in this manner.
[0230] For example, a reflective liquid crystal display element can be produced by providing a reflective electrode, a transparent electrode, a λ / 4 plate, a polarizing film, a color filter layer, etc. in the liquid crystal cell according to a conventional method as needed.
[0231] In addition, a backlight, a polarizing plate, a λ / 4 plate, a transparent electrode, a polarizing film, a color filter layer, etc. can be arranged in the liquid crystal unit according to conventional methods as needed to produce a transmissive liquid crystal display element.
[0232] Example
[0233] The present invention will be specifically described with reference to Examples, but the present invention is not limited to these Examples. The abbreviations of the compounds used in the polymerization of the polymer and the preparation of the film-forming composition and the methods of evaluating the properties are as follows.
[0234]
Compound 25
[0235]
[0236] NMP: N-methyl-2-pyrrolidone,
[0237] GBL: γ-butyl lactone,
[0238] BCS: Butyl Cellosolve
[0239] <Viscosity measurement>
[0240] The viscosity of the polyamic acid solution at 25° C. was measured using an E-type viscometer TVE-22H (manufactured by Toki Sangyo Co., Ltd.) with a sample amount of 1.1 mL and a cone rotor TE-1 (1°34′, R24).
[0241] <Determination of Imidization Ratio>
[0242] 20 mg of polyimide powder was added to an NMR sample tube (NMR sampling tube standard φ5 manufactured by Kusano Scientific Co., Ltd.), 0.53 ml of deuterated dimethyl sulfoxide (DMSO-d6, 0.05 mass% TMS (tetramethylsilane) mixture) was added, and ultrasound was applied to completely dissolve it. The 500 MHz proton NMR of the solution was measured using a measuring device (manufactured by JEOL DATUM Co., Ltd., JNW-ECA500).
[0243] The imidization rate was determined by the following mathematical formula using the peak cumulative value of a proton derived from a structure that does not change before and after imidization as a reference proton and the proton peak cumulative value derived from NH of an amide group appearing around 9.5 to 10.0 ppm.
[0244] Imidization rate (%) = (1-α·x / y) × 100
[0245] Wherein, x is the peak cumulative value of protons derived from NH of an amide group, y is the peak cumulative value of reference protons, and α is the number ratio of reference protons to NH protons of one amide group in the case of polyamic acid (imidization ratio 0%).
[0246] <Polymerization and Preparation of Radical Generating Film-Forming Composition>
[0247] Synthesis example 1
[0248] Polymerization of TC-1, TC-2(50) / DA-1(50), DA-2(50) polyimide
[0249] In a 100ml 4-necked flask with a nitrogen inlet tube, an air cooling tube, and a mechanical stirrer, 1.62g (15.00mmol) of DA-1 and 3.96g (15.00mmol) of DA-2 were measured, and 48.2g of NMP was added, and stirred under a nitrogen atmosphere to completely dissolve. After confirming the dissolution, 3.75g (15.00mmol) of TC-2 was added, and the mixture was reacted at 60°C for 3 hours under a nitrogen atmosphere. The mixture was returned to room temperature again, and 2.71g (13.80mmol) of TC-1 was added, and the mixture was reacted at 40°C for 12 hours under a nitrogen atmosphere. The polymerization viscosity was confirmed, and TC-1 was further added in such a way that the polymerization viscosity reached 1000mPa·s to obtain a polymerization solution having a polyamic acid concentration of 20% by mass.
[0250] In a 200ml conical flask with a magnetic stirrer, 60g of the polyamic acid solution obtained above was measured, 111.4g of NMP was added to prepare a 7% by mass solution, while stirring, 9.10g (88.52mmol) of acetic anhydride and 3.76g (47.53mmol) of pyridine were added, and after stirring at room temperature for 30 minutes, the reaction was stirred at 55°C for 3 hours. After the reaction was completed, the solution was returned to room temperature, and the reaction solution was injected while stirring in 500ml of methanol to precipitate solids. The solid was recovered by filtration, and the solid was further put into 300ml of methanol and stirred and cleaned for 30 minutes. The above operation was performed twice in total, and the solid was recovered by filtration. After air-drying, it was dried in a vacuum oven at 60°C, thereby obtaining a polyimide (PI-1) having a number average molecular weight of 11300, a weight average molecular weight of 32900, and an imidization rate of 53%.
[0251] Synthesis example 2
[0252] Polymerization of TC-1, TC-2(50) / DA-1(50), DA-3(50) polyimide
[0253] In a 100 ml four-necked flask equipped with a nitrogen inlet tube, an air cooling tube, and a mechanical stirrer, 1.62 g (15.00 mmol) of DA-1 and 4.96 g (15.00 mmol) of DA-3 were weighed, 51.90 g of NMP was added, and the mixture was stirred under a nitrogen atmosphere to completely dissolve. After dissolution was confirmed, 3.75 g (15.00 mmol) of TC-2 was added, and the mixture was reacted at 60° C. for 3 hours under a nitrogen atmosphere. The mixture was returned to room temperature, 2.64 g (13.5 mmol) of TC-1 was added, and the mixture was reacted at 40° C. for 12 hours under a nitrogen atmosphere. The polymerization viscosity was confirmed, and TC-1 was further added in such a manner that the polymerization viscosity reached 1000 mPa·s to obtain a polymerization solution having a polyamic acid concentration of 20% by mass.
[0254] In a 200ml conical flask with a magnetic stirrer, 60g of the polyamic acid solution obtained above was measured, 111.4g of NMP was added, and a 7% by mass solution was prepared. 8.38g (81.4mmol) of acetic anhydride and 3.62g (45.8mmol) of pyridine were added while stirring. After stirring at room temperature for 30 minutes, it was reacted by stirring at 55°C for 3 hours. After the reaction was completed, the solution was returned to room temperature, and the reaction solution was injected while stirring in 500ml of methanol to precipitate solids. The solid was recovered by filtration, and the solid was further put into 300ml of methanol and stirred and cleaned for 30 minutes. The above operation was performed twice in total, and the solid was recovered by filtration. After air-drying, it was dried in a vacuum oven at 60°C, thereby obtaining a polyimide (PI-2) having a number average molecular weight Mn of 13100, a weight average molecular weight Mw of 34000, and an imidization rate of 55%.
[0255] Synthesis example 3
[0256] Polymerization of TC-1, TC-2(50) / DA-1(50), DA-4(50) polyimide
[0257] In a 100ml 4-necked flask with a nitrogen inlet tube, an air cooling tube, and a mechanical stirrer, 1.62g (15.00mmol) of DA-1 and 5.65g (15.00mmol) of DA-4 were measured, 55.4g of NMP was added, and it was stirred under a nitrogen atmosphere to completely dissolve. After confirming the dissolution, 3.75g (15.00mmol) of TC-2 was added, and the mixture was reacted at 60°C for 3 hours under a nitrogen atmosphere. The mixture was returned to room temperature again, and 2.82g (14.40mmol) of TC-1 was added, and the mixture was reacted at 40°C for 12 hours under a nitrogen atmosphere. The polymerization viscosity was confirmed, and TC-1 was further added in such a way that the polymerization viscosity reached 1000mPa·s to obtain a polymerization solution having a polyamic acid concentration of 20% by mass.
[0258] In a 200ml conical flask with a magnetic stirrer, 60g of the polyamic acid solution obtained above was measured, 111.4gNMP was added, and a 7% by mass solution was prepared. While stirring, 8.36g (81.2mmol) of acetic anhydride and 3.65g (46.1mmol) of pyridine were added, and stirred at room temperature for 30 minutes, and then stirred at 55°C for 3 hours to react. After the reaction was completed, the solution was returned to room temperature, and the reaction solution was injected while stirring in 500ml of methanol to precipitate solids. The solid was recovered by filtration, and the solid was further put into 300ml of methanol and stirred and cleaned for 30 minutes. The above operation was performed twice in total, and the solid was recovered by filtration. After air-drying, it was dried in a vacuum oven at 60°C, thereby obtaining a polyimide (PI-3) having a number average molecular weight Mn of 12900, a weight average molecular weight Mw of 31000, and an imidization rate of 51%.
[0259] Preparation of free radical generating film forming composition: AL1
[0260] In a 50 ml conical flask with a magnetic stirrer, 2.0 g of the polyimide powder (PI-1) obtained in Synthesis Example 1 was weighed, 18.0 g of NMP was added, and the mixture was stirred at 50° C. to completely dissolve. 6.7 g of NMP and 6.7 g of BCS were further added, and the mixture was stirred for another 3 hours to obtain a free radical generating film forming composition according to the present invention: AL1 (solid content: 6.0% by mass, NMP: 66% by mass, BCS: 30% by mass).
[0261] Preparation of free radical generating film forming composition: AL2
[0262] In a 50 ml conical flask with a magnetic stirrer, 2.0 g of the polyimide powder (PI-2) obtained in Synthesis Example 2 was weighed, 18.0 g of NMP was added, and the mixture was stirred at 50° C. to completely dissolve. 6.7 g of NMP and 6.7 g of BCS were further added, and the mixture was stirred for another 3 hours to obtain a free radical generating film forming composition according to the present invention: AL2 (solid content: 6.0% by mass, NMP: 66% by mass, BCS: 30% by mass).
[0263] Preparation of non-radical generating film-forming composition: AL3
[0264] In a 50 ml conical flask with a magnetic stirrer, 2.0 g of the polyimide powder (PI-3) obtained in Synthesis Example 3 was weighed, 18.0 g of NMP was added, and the mixture was stirred at 50° C. to completely dissolve. 6.7 g of NMP and 6.7 g of BCS were further added, and the mixture was stirred for another 3 hours to obtain a non-radical-generating film-forming composition AL3 (solid content: 6.0% by mass, NMP: 66% by mass, BCS: 30% by mass) as a comparative object.
[0265]
Table 1
[0266] Table 1 Composition of polyimide
[0267]
[0268]
Table 2
[0269] Table 2 Composition of film-forming composition
[0270]
[0271]
Table 3
[0272] Table 3 Composition of liquid crystal used
[0273] Using LCD liquid crystal additive LC-1 MLC-3018U none LC-2 MLC-3018U HMA 10wt% LC-3 MLC-3018U IDHex 7wt% LC-4 MLC-3018U C2C6 5wt% LC-5 MLC-3019 none LC-6 MLC-3019 HMA 10wt% LC-7 MLC-3019 IDHex 7wt% LC-8 MLC-3019 C2C6 5wt%
[0274] <Production of polymerizable compound>
[0275] Polymerizable compound synthesis example 1
[0276] Synthesis of Ethyl 2-(Heptanoyloxymethyl)acrylate
[0277]
Compound 26
[0278]
[0279] Step 1: Synthesis of 2-hydroxyethyl methacrylate
[0280] In a 500ml four-necked flask equipped with a nitrogen inlet tube, 10mg of 4-methoxyphenol and 21.88g (195.1mmol) of DABCO (1,4-diazabicyclo [2.2.2] octane) were measured, 50ml of pure water was added, and 11.52g (390.1mmol) of paraformaldehyde was added while stirring at 10°C or below under a nitrogen atmosphere, and stirred for 1 hour. Confirm that the slurry state has changed to a solution state, add 300ml of acetonitrile, and add 19.53g (195.1mmol) of ethyl acrylate while adding dropwise, and react at 50°C for 5 hours. After the reaction is completed, the reaction solution is transferred to a separatory funnel and 50ml of n-hexane is added. Confirm that it is divided into 3 layers, recover the lower 2 layers, and perform this operation 3 times. Furthermore, hydrochloric acid is added to bring the pH to 4-5, and extraction is performed using ethyl acetate. Anhydrous magnesium sulfate was added to the extracted solution, stirred to dryness, and then filtered and concentrated to obtain 22.9 g (175.6 mmol, yield 90%) of a colorless, transparent oily liquid. The structure was determined by nuclear magnetic resonance spectroscopy ( 1 The target compound was confirmed by H-NMR spectrum. The measurement data are shown below.
[0281] 1 H NMR (400MHz, CDCl3) δ: 6.81 (1H), 5.80 (1H), 4.31 (2H), 4.17 (1H), 1.98 (1H), 0.93 (3H)
[0282] Step 2: Synthesis of ethyl 2-(heptanoyloxymethyl)acrylate
[0283] In a 500 ml four-necked flask equipped with a nitrogen inlet tube, 19.9 g (152.9 mmol) of 2-hydroxymethylacrylic acid obtained by the above method was weighed, 300 ml of THF and 23.2 g (229.3 mmol) of triethylamine were added, and 25.0 g (168.2 mmol) of heptanoyl chloride was added dropwise while maintaining the temperature below 10°C under a nitrogen atmosphere, and the mixture was reacted for 6 hours. After the reaction, the precipitated triethylamine hydrochloride was removed by filtration, the reaction solution was concentrated, redissolved with 300 ml of ethyl acetate, washed 3 times with 10% potassium carbonate aqueous solution 100 ml, washed 3 times with 50 ml of pure water, dried with anhydrous magnesium sulfate, filtered and concentrated to obtain a light yellow viscous body. Further, it was purified by flash column chromatography (eluting solvent: ethyl acetate: n-hexane = 20:80), and the solvent was removed and vacuum dried to obtain 32.2 g (133.0 mmol: yield 87%) of a colorless transparent oily liquid. The structure was determined by NMR spectroscopy ( 1 The target compound was confirmed by H-NMR spectrum. The measurement data are shown below.
[0284] 1H NMR (400MHz, CDCl3) δ: 6.37(1H), 5.80(1H), 3.80(2H), 4.23-4.21(2H), 2.39-2.37(2H), 1.64-1.58(2H), 1.30-1.27(9H), 0.86(3H)
[0285] Polymerizable compound synthesis example 3
[0286] Synthesis of Dihexyl Itaconate
[0287]
Compound 27
[0288]
[0289] In a 4-necked flask equipped with a Dean-Stark tube, 23.8 g (182.9 mmol) of itaconic acid and 35.5 g (347.5 mmol) of 1-hexanol were measured, and 500 ml of cyclohexane, 0.9 g (9.1 mmol) of concentrated sulfuric acid and 0.04 g (1.82 mmol) of butylated hydroxytoluene (BHT) were added. A nitrogen atmosphere was set and a dehydration condensation reaction was carried out at 110°C for 24 hours. After the reaction, 100 ml of n-hexane was added to the reaction solution, and the solution was washed three times with 100 g of a 10% aqueous sodium carbonate solution, washed three times with 100 ml of pure water, and dried with anhydrous magnesium sulfate. After filtration and concentration, vacuum drying was performed to obtain 48.6 g (162.8 mmol: yield 89%) of a colorless and transparent oily liquid. The structure was determined by nuclear magnetic resonance spectroscopy ( 1 The target compound was confirmed by H-NMR spectrum. The measurement data are shown below.
[0290] 1 H NMR (400MHz, CDCl3) δ: 6.30 (1H), 5.65 (1H), 4.20-4.00 (4H), 3.32 (2H), 1.64-1.58 (4H), 1.40-1.25 (12H), 0.96-0.83 (6H)
[0291] <Production of Liquid Crystal Display Element>
[0292] A liquid crystal display element was produced with the configuration shown in Table 3 using AL1 to AL3 obtained above and SE-6414 (manufactured by Nissan Chemical Industries, Ltd.), which was a liquid crystal aligning agent for horizontal alignment.
[0293] (First Substrate)
[0294] The first substrate (hereinafter also referred to as IPS substrate) is an alkali-free glass substrate with a size of 30 mm × 35 mm and a thickness of 0.7 mm. ITO (Indium-Tin-Oxide) electrodes with a comb-shaped pattern with an electrode width of 10 μm and an interval of 10 μm between electrodes are formed on the substrate to form pixels. The size of each pixel is 10 mm in length and about 5 mm in width.
[0295] AL1 to AL3 or SE-6414 were filtered through a 1.0 μm filter, applied to the electrode formation surface of the IPS substrate by spin coating, and dried on a hot plate at 80° C. for 1 minute. Then, AL1 to AL3 were sintered at 220° C. for 20 minutes, and SE-6414 was sintered at 220° C. for 20 minutes, and each was formed into a coating film with a film thickness of 100 nm.
[0296] The coated substrate was shielded from light by a metal plate so that half of the substrate was not irradiated with light, and ultraviolet light was irradiated using a high-pressure mercury lamp through a bandpass filter with a wavelength of 313 nm to an exposure amount of 5000 mJ. This operation is hereinafter referred to as primary UV treatment.
[0297] After the exposure treatment, the rubbing direction was rubbed at an angle of 5° from the longitudinal direction of the comb-tooth electrode. The rubbing was performed using a rayon cloth YA-20R manufactured by Yoshikawa Chemical Industry Co., Ltd. under the conditions of a roller diameter of 120 mm, a rotation speed of 300 rpm, a moving speed of 50 mm / sec, and an intrusion amount of 0.4 mm. After the rubbing treatment, ultrasonic irradiation was performed in pure water for 1 minute and dried at 80°C for 10 minutes.
[0298] (Second Substrate)
[0299] The second substrate (also called the back ITO substrate) is an alkali-free glass substrate of 30 mm × 35 mm in size and 0.7 mm in thickness, with an ITO film formed on the back side (the surface facing the outside of the cell). In addition, a columnar spacer with a height of 4 μm is formed on the front side (the surface facing the inside of the cell).
[0300] SE-6414 was filtered through a 1.0 μm filter on the glass surface of the above-mentioned back ITO substrate, and then applied by spin coating, and dried on a hot plate at 80°C for 1 minute. Next, AL1 and AL2 were sintered at 220°C for 20 minutes, and SE-6414 was sintered at 220°C for 20 minutes. After each was formed into a coating film with a film thickness of 100 nm, a friction treatment was performed. The friction treatment was performed using a rayon cloth: YA-20R manufactured by Yoshikawa Chemical Industry, and the friction was performed under the conditions of a roller diameter of 120 mm, a rotation speed of 1000 rpm, a moving speed of 50 mm / sec, and an intrusion amount of 0.4 mm. After the friction treatment, ultrasonic irradiation was performed in pure water for 1 minute, and then dried at 80°C for 10 minutes.
[0301] (Fabrication of Liquid Crystal Cell)
[0302] The two substrates (first substrate and second substrate) with liquid crystal alignment films were used, leaving a liquid crystal injection port and sealing the periphery to produce an empty cell with a cell spacing of about 4 μm. At this time, the rubbing directions of the first substrate and the second substrate were respectively produced to be anti-parallel and crossed at 85°.
[0303] In this empty cell, liquid crystal (obtained by adding various additives under optimal conditions to positive liquid crystal MLC-3019 for IPS manufactured by Merck and liquid crystal MLC3018U for TN manufactured by Merck) was vacuum injected at room temperature, and the injection port was sealed to form a liquid crystal cell. The obtained liquid crystal cell constitutes an IPS mode liquid crystal display element and a TN mode liquid crystal display element. Thereafter, the obtained liquid crystal cell was heat-treated at 120°C for 10 minutes.
[0304] As the secondary UV treatment, a high pressure mercury lamp was used to irradiate through a band pass filter with a wavelength of 313 nm. The liquid crystal cell was irradiated with ultraviolet light in such a way that the exposure amount was 5000 mJ. The details of the cell produced below are shown in Table 4 below.
[0305]
Table 4
[0306] Unit Number Free radical generating membrane liquid crystal Orientation Mode 1 AL-1 LC-1 TN 2 AL-2 LC-1 TN 3 AL-3 LC-1 TN 4 AL-1 LC-2 TN 5 AL-2 LC-2 TN 6 AL-3 LC-2 TN 7 AL-1 LC-3 TN 8 AL-2 LC-3 TN 9 AL-3 LC-3 TN 10 AL-1 LC-4 TN 11 AL-2 LC-4 TN 12 AL-3 LC-4 TN 13 AL-1 LC-5 level 14 AL-2 LC-5 level 15 AL-3 LC-5 level 16 AL-1 LC-6 level 17 AL-2 LC-6 level 18 AL-3 LC-6 level 19 AL-1 LC-7 level 20 AL-2 LC-7 level 21 AL-3 LC-7 level 22 AL-1 LC-8 level 23 AL-2 LC-8 level 24 AL-3 LC-8 level
[0307] ※SE-6414 is used for the back ITO side
[0308] <Visual Evaluation of Liquid Crystal Orientation>
[0309] The orientation of the TN mode liquid crystal unit is confirmed using a polarizing plate fixed to an orthogonal Nicol prism. In the absence of UV treatment, the orientation restriction force of the unilateral orientation film is lost (i.e., a zero anchoring state is formed), so the regulation force of the chiral dopant in the liquid crystal cannot fully twist it, and it changes to a horizontal orientation state. On the other hand, the UV-treated area loses its polymerization reactivity, so the anchoring force is maintained. Therefore, a twisted orientation is generated. As a result, two orientation states are generated within the pixel. As Figure 1 As shown, the case where the region of the film irradiated with UV was aligned (white) and the region not irradiated with UV was horizontally aligned (black) was marked as ○, and the case where there was no change in each region was marked as ×.
[0310]
Table 5
[0311] Table 5 Evaluation of orientation pattern formation characteristics
[0312] Example Unit Number Pattern formation Example 1 4 ○ Example 2 5 ○ Example 3 7 ○ Example 4 8 ○ Example 5 10 ○ Example 6 11 ○ Comparative Example 1 1 × Comparative Example 2 2 × Comparative Example 3 3 × Comparative Example 4 6 × Comparative Example 5 9 × Comparative Example 6 12 ×
[0313] When liquid crystal without additives is used in the liquid crystal, and when a material that does not generate free radicals due to light is used, even if UV treatment is performed once, the orientation patterning, i.e., the orientation restriction force, does not change. Therefore, it can be seen that the combination of the light free radical generating film and the additive of the present invention is important.
[0314] <Evaluation of electro-optical characteristics>
[0315] Using units 13 to 24 (horizontally aligned units), the change in threshold voltage and the measurement of mode efficiency are performed by measuring the VT curve. The white LED backlight and the brightness meter are fixed in the same way as the optical axis. During this period, the liquid crystal unit (liquid crystal display element) with a polarizer is fixed in a way that the brightness becomes minimum. The voltage is applied at intervals of 1V up to 8V, and the brightness during the voltage is measured to measure the VT curve. The value of the driving threshold voltage is estimated from the obtained VT curve. The measurement of mode efficiency is obtained by calculating the ratio of the brightness of the liquid crystal unit at Vmax to the brightness of the LED transmitted light when the polarizer is parallel to the Nicol prism.
[0316] The anchoring assay estimates the approximate value of the threshold voltage using the Fredericks shift method.
[0317]
Table 6
[0318] Table 6
[0319]
[0320] Units 13 to 24 are horizontally aligned units, so even if they become zero anchor alignment, there is no visual change. On the other hand, the threshold voltage and brightness of the VT curve are observed to change in the single UV exposure part and the unexposed part. According to this test, it can be seen that by performing a single exposure, regions with different anchoring forces are produced in the pixel.
[0321] Industrial Applicability
[0322] According to the present invention, different zero-plane regions anchored can be produced industrially with good yield from cheap raw materials. In addition, the liquid crystal display element obtained by the method of the present invention is useful as a liquid crystal display element of a vertical alignment mode such as a PSA type liquid crystal display, a SC-PVA type liquid crystal display, etc.
Claims
1. A method for manufacturing a patterned zero-plane anchoring film, characterized in that: include: a step of irradiating a specific region of the radical generating film with radiation to form a patterned radical generating film; as well as A step of bringing a liquid crystal composition containing a liquid crystal and a radical polymerizable compound into contact with the patterned radical generating film, and while maintaining this state, applying energy sufficient to cause the radical polymerizable compound to undergo a polymerization reaction to the liquid crystal composition, At least one of the radical polymerizable compounds is a compound that is compatible with liquid crystal and has one polymerizable unsaturated bond in one molecule, The radical generating film is a film in which organic groups inducing radical polymerization are fixed.
2. The method according to claim 1, wherein: The radical generating film is a radical generating film subjected to a uniaxial orientation treatment.
3. The method according to claim 1, wherein: The step of imparting energy is performed in the absence of an electric field.
4. The method according to claim 1, characterized in that: The radical generating film is obtained by applying a composition of a compound having a group generating a radical and a polymer, curing the composition to form a film, and thereby fixing the compound in the film.
5. The method according to claim 1, characterized in that The radical generating film includes a polymer containing an organic group that induces radical polymerization.
6. The method according to claim 5, characterized in that The polymer containing an organic group inducing free radical polymerization is at least one polymer selected from a polyimide precursor, polyimide, polyurea, and polyamide obtained using a diamine component, and the diamine component contains a diamine containing an organic group inducing free radical polymerization.
7. The method according to claim 1, wherein: The organic group inducing free radical polymerization is an organic group represented by any one of the following structures [X-1] to [X-18], [W], [Y] and [Z], In formulas [X-1] to [X-18], * represents a site bonded to a portion other than a polymerizable unsaturated bond of a compound molecule, S1 and S2 each independently represent -O-, -NR-, or -S-, R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, and R1 and R2 each independently represent a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms; In the formulas [W], [Y], and [Z], * represents a site bonded to a portion other than the polymerizable unsaturated bond of the compound molecule, Ar represents an aromatic hydrocarbon group selected from phenylene, naphthylene, and biphenylene which may have an organic group and / or a halogen atom as a substituent, and R 9 and R 10 Each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and R 9 and R 10 In the case of an alkyl group, the terminals may be bonded to each other to form a ring structure or may not be bonded to each other to form a ring structure; Q represents the following structure; In the formula, R 11 represents -CH2-, -NR-, -O- or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a site bonded to a portion other than Q of the compound molecule; R 12 It represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms.
8. The method according to claim 6, characterized in that The diamine containing an organic group inducing free radical polymerization is a diamine having a structure represented by the following general formula (6) or the following general formula (7), In formula (6), R 6 represents a single bond, -CH2-, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-, R 7 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, wherein at least one of any -CH2- or -CF2- in the alkylene group is independently substituted by or is not substituted by a group selected from -CH=CH-, a divalent carbocyclic ring and a divalent heterocyclic ring, and is substituted by or is not substituted by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH- or -NH-, provided that they are not adjacent to each other; R 8 represents a radical polymerizable group selected from the following formulae, In formulae [X-1] to [X-18], * represents a site bonded to a portion other than the radical polymerizable group of the compound molecule, and S 1 , S 2 Each independently represents -O-, -NR-, or -S-, R represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms, and R1 and R2 each independently represent a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms; In formula (7), T1 and T2 are each independently a single bond, -O-, -S-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CH2O-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-, S 0 represents a single bond, or an unsubstituted or fluorine-substituted alkylene group having 1 to 20 carbon atoms, wherein at least one of any -CH2- or -CF2- of the alkylene group is independently substituted by or is not substituted by a group selected from -CH=CH-, a divalent carbocyclic ring and a divalent heterocyclic ring, and is substituted by or is not substituted by any of the following groups, i.e., -O-, -COO-, -OCO-, -NHCO-, -CONH- or -NH-, provided that they are not adjacent to each other, J is an organic group represented by any one of the following formulae, In the formulas [W], [Y], and [Z], * represents a site bonded to T2, Ar represents an aromatic hydrocarbon group selected from phenylene, naphthylene, and biphenylene which may have an organic group and / or a halogen atom as a substituent, and R 9 and R 10 Each independently represents an alkyl group having 1 to 10 carbon atoms or an alkoxy group having 1 to 10 carbon atoms, and Q represents any of the following structures; In the formula, R 11 represents -CH2-, -NR-, -O- or -S-, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and * represents a site bonded to a portion other than Q of the compound molecule; R 12 It represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms.
9. The method according to claim 1, wherein: The polymerization reactive group of the free radical polymerizable compound is selected from the following structures, In the formula, * represents the site bonded to the part other than the polymerizable unsaturated bond of the compound molecule; R b represents a straight-chain alkyl group having 2 to 8 carbon atoms, and E represents a single bond, -O-, -NR c -, -S-, ester bonds and amide bonds in the bonding group; R c It represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
10. The method according to claim 1, wherein: The liquid crystal composition containing a liquid crystal and a radical polymerizable compound is a liquid crystal composition containing a radical polymerizable compound such that a polymer obtained by polymerizing the radical polymerizable compound has a Tg of 100° C. or less.
11. A method for manufacturing a liquid crystal unit, characterized in that: Using the method according to any one of claims 1 to 10, The method for manufacturing the liquid crystal unit comprises: The step of preparing a first substrate and a second substrate, wherein the first substrate has a free radical generating film, and the second substrate is a substrate covered with a liquid crystal alignment film having uniaxial alignment; a step of manufacturing a unit in such a manner that the radical generating film on the first substrate faces the second substrate; and A step of filling a liquid crystal composition containing a liquid crystal and a radical polymerizable compound between the first substrate and the second substrate.
12. The method for manufacturing a liquid crystal unit according to claim 11, characterized in that: The liquid crystal alignment film having uniaxial alignment properties is a liquid crystal alignment film for horizontal alignment.
13. The method for manufacturing a liquid crystal cell according to claim 11, wherein: The first substrate having the radical generating film is a substrate having comb-teeth electrodes.
14. A method for manufacturing a liquid crystal display element, characterized in that: A film having a zero-plane anchoring state is used, wherein the film having a zero-plane anchoring state is obtained by the method according to any one of claims 1 to 13.
15. A liquid crystal display element, characterized in that: The liquid crystal display element is obtained using the method according to claim 14.
16. The liquid crystal display element according to claim 15, wherein The first substrate or the second substrate has an electrode.
17. The liquid crystal display element according to claim 15, wherein The liquid crystal display element is a low voltage driven transverse electric field liquid crystal display element.