Improved temperature-stable soft magnetic powder
By forming a fluorine-containing silicon-based coating on soft magnetic powder, the problem of easy cracking of the insulating layer at high temperature is solved, and soft magnetic powder with high permeability and high resistivity at high temperature is realized, which is suitable for manufacturing high-temperature durable electronic components.
Patent Information
- Application Number
- CN201980046009.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-07-11
- Filing Date
- 2019-07-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-07-09
AI Technical Summary
The insulating layer of existing soft magnetic powder is prone to cracking at high temperatures, which leads to increased eddy current losses and decreased resistivity, making it difficult to achieve a balance between high permeability and high resistivity in high-frequency applications.
Fluorine-containing silicon-based coatings are used, which are formed by mixing soft magnetic powder with soluble fluorinating agents and silicon-based solutions to create uniform or non-uniform silicon-based coatings. This improves temperature stability and resistivity, and reduces eddy current losses.
A soft magnetic powder that maintains high permeability and high resistivity at high temperatures has been developed, making it suitable for manufacturing high-temperature durable electronic components and improving batch-to-batch consistency and reliability.
Smart Images

Figure BDA0002889014810000181 
Figure BDA0002889014810000191 
Figure BDA0002889014810000201
Abstract
Description
[0001] Description of the invention
[0002] The present invention relates to soft magnetic powders and methods for coating soft magnetic powders. The present invention further relates to the use of such soft magnetic powders and electronic components comprising such soft magnetic powders.
[0003] Common applications of soft magnetic powders include magnetic core components, which are used as magnetic material workpieces with high magnetic permeability for confining and guiding magnetic fields in electrical, electromechanical and magnetic devices such as electromagnets, transformers, motors, inductors and magnetic assemblies. These components are usually made in different shapes and sizes by molding soft magnetic powders in molds under high pressure.
[0004] In electronic applications, especially in alternating current (AC) applications, two key properties of magnetic core components are the magnetic permeability and core loss characteristics. In this case, the magnetic permeability of a material provides an indication of its ability to be magnetized or its ability to carry magnetic flux. Magnetic permeability is defined as the ratio of the induced magnetic flux to the magnetizing force or field strength. When a magnetic material is exposed to a rapidly changing field, the total energy of the core is reduced due to the occurrence of hysteresis losses and / or eddy current losses. Hysteresis losses are caused by the energy dissipation required to overcome the retained magnetic forces within the core component. Eddy current losses are caused by the generation of currents in the core component due to the changing flux caused by AC conditions, and essentially result in resistive losses.
[0005] Typically, devices for high frequency applications are sensitive to core losses, and good insulation of the soft magnetic powder particles is desirable in order to reduce eddy current induced losses. The simplest way to achieve this is to thicken the insulating layer of each particle. However, the thicker the insulating layer, the lower the core density of the soft magnetic particles, and the magnetic flux density decreases. Thus, in order to produce a soft magnetic powder core with optimal key properties, both the resistivity and density of the core must be increased.
[0006] Another aspect of insulation relates to the temperature performance and durability of the insulation layer. Particularly high temperatures can lead to degradation of the insulation layer by creating cracks that promote eddy current losses. Thus, temperature stability is a further requirement for manufacturing soft magnetic powder cores with optimal properties. Ideally, the particles would be covered with a thin insulation layer that provides high resistivity and high density as well as stable temperature performance.
[0007] Known methods of forming an insulating layer on magnetic particles usually deal with one of the key properties, namely density or resistivity. However, if the particles coated with the insulating layer are subjected to temperatures exceeding 120°C, preferably exceeding 150°C, for several hours, the insulating layer may crack, which results in higher eddy currents and lower resistivity values.
[0008] EP 2 871 646 A1 provides a soft magnetic powder coated with a silicon-based coating, which exhibits good properties in terms of temperature stability and resistivity. This is achieved by a specific silicon-based coating containing fluorine in a certain amount. EP 2 871 646 A1 also discloses a method for preparing the coated soft magnetic powder. However, considering the increasing demand for coated soft magnetic powders, especially in terms of thermal stability, there is still a need in the art to further improve the insulating layer of soft magnetic powders in order to achieve the best results for magnetic core components prepared from such powders. In addition, it is desirable to improve the method for coating soft magnetic powders.
[0009] It is therefore an object of the present invention to provide an improved coated soft magnetic powder and a corresponding method for coating a soft magnetic powder, which method helps to achieve good temperature stability, high resistivity and high magnetic permeability when used in magnetic core components. In addition, it is an object of the present invention to provide a method that can achieve the aforementioned goals in a simple, cost-effective and uncomplicated manner. Another object of the present invention is to provide an electronic component comprising a soft magnetic powder having good temperature stability, high resistivity and high magnetic permeability.
[0010] These objects are achieved by a soft-magnetic powder coated with a silicon-based coating, wherein the silicon-based coating comprises at least one fluorine-containing composition of formula (I):
[0011] Si 1-0.75c M c O 2-0.5c F d (I)
[0012] in
[0013] c is in the range of 0.01 to 0.5,
[0014] d is in the range of 0.04 to 2, and
[0015] M is B or Al.
[0016] The invention further relates to a method for coating a soft magnetic powder, wherein the soft magnetic powder is mixed with a silicon-based solution containing a soluble fluorinating agent. The invention further relates to a soft magnetic powder obtained by the coating method or a soft magnetic powder coated according to the method. The invention also relates to the use of the coated soft magnetic powder for the manufacture of electronic components, in particular magnetic core components, and electronic components, in particular magnetic core components, comprising the coated soft magnetic powder.
[0017] The following description relates to the coated soft magnetic powder and the method for coating the soft magnetic powder proposed by the present invention. In particular, the embodiments of the soft magnetic powder, the fluorine-containing composition and the soluble fluorinating agent are applicable to the coated soft magnetic powder, the method for coating the soft magnetic powder and the coated soft magnetic compound obtained by the method, etc.
[0018] The present invention provides a method for coating soft magnetic powders and corresponding coated powders, which are most suitable for manufacturing electronic components. In particular, when used to manufacture electronic components such as magnetic core components, the soft magnetic powders coated according to the present invention can achieve high temperature durability, high resistivity and high magnetic permeability. In addition, due to the simple and uncomplicated manner of the proposed method, high batch-to-batch consistency can be achieved, which in turn enables reliable production of electronic components. In summary, the soft magnetic powders coated according to the present invention help to prepare electronic components with unique electromagnetic performance characteristics and high temperature durability, especially for temperatures >120°C, preferably >150°C, such as >175°C.
[0019] In the context of the present invention, the individual components of the fluorine-containing composition, for example Si, O, F, can be uniformly distributed in the whole silicon-based coating. In this case, the fluorine-containing composition described herein represents the composition of uniform silicon-based coating. Or, the silicon-based coating can be inhomogeneous. In such cases, the individual components of the fluorine-containing composition described herein represent the mean value of the composition of the silicon-based coating on the whole coating. For example, the silicon-based coating can contain one or more silicon dioxide (SiO 2 ) layers and one or more layers that further contain fluorine components. The fluorine-containing composition described herein thus represents the average composition of layered or inhomogeneous silicon-based coating.
[0020] In the context of the present invention, unless otherwise stated, weight % (wt.-%) refers to the fraction of the total weight of the soft magnetic powder. For example, the solution used to coat the soft magnetic powder comprises a soluble fluorinating agent as described above and optionally other components, such as a solvent. Unless otherwise expressly stated, weight % here refers to the fraction of the total weight of the soft magnetic powder to be treated with the solution. Therefore, the indicators in weight % are based on, for example, the total weight of the soft magnetic powder excluding other components from the solution.
[0021] The soft magnetic powder of the present invention comprises a plurality of particles consisting of soft magnetic material. Such powders comprise particles having an average size of 0.5 to 250 μm, preferably 2 to 150 μm, more preferably 2 to 10 μm. The shapes of these particles may be different. With regard to shape, many variants known to those skilled in the art are possible. The shape of the powder particles may be, for example, needle-shaped, cylindrical, plate-shaped, tear-shaped, flat or spherical. Soft magnetic particles with various particle shapes are commercially available. Spherical is preferred because such particles can be more easily coated, which in fact results in more effective insulation of the electric current.
[0022] As soft magnetic material, elemental metal, alloy or the mixture of one or more elemental metals and one or more alloys can be used.Typical elemental metal includes Fe, Co and Ni.Alloy can include Fe-based alloy (Fe-based alloys), such as Fe-Si alloy, Fe-Si-Cr alloy, Fe-Si-Ni-Cr alloy, Fe-Al alloy, Fe-N alloy, Fe-Ni alloy, Fe-C alloy, Fe-B alloy, Fe-Co alloy, Fe-P alloy, Fe-Ni-Co alloy, Fe-Cr alloy, Fe-Mn alloy, Fe-Al-Si alloy and ferrite, or rare earth based alloy (rare earth based alloy), particularly rare earth Fe-based alloy (rare earthFe-based alloy), such as Nd-Fe-B alloy, Sn-Fe-N alloy or Sm-Co-Fe-Cu-Zr alloy, or Sr-ferrite, or Sm-Co alloy.In a preferred embodiment, Fe or Fe-based alloy, such as Fe-Si-Cr, Fe-Si or Fe-Al-Si serve as soft magnetic material.
[0023] In a particularly preferred embodiment, Fe serves as the soft magnetic material and the soft magnetic powder is carbonyl iron powder (also referred to herein as CIP). Carbonyl iron can be obtained by thermal decomposition of pentacarbonyl iron in the gas phase according to known methods, as described, for example, in Ullmann's Encyclopedia of Industrial Chemistry, 5th edition, volume A14, page 599 or DE 3 428121 or DE 3 940 347, and contains particularly pure metallic iron.
[0024] Carbonyl iron powder is a grey, finely divided powder of metallic iron which has a low content of secondary constituents and consists essentially of spherical particles with an average particle size of up to 10 μm. Unreduced carbonyl iron powder, which is preferred in this case, has an iron content of >97% by weight (here based on the total weight of the powder), a carbon content of <1.5% by weight, a nitrogen content of <1.5% by weight and an oxygen content of <1.5% by weight. Reduced carbonyl iron powder, which is particularly preferred in the process according to the invention, has an iron content of >99.5% by weight (here based on the total weight of the powder), a carbon content of <0.1% by weight, a nitrogen content of <0.01% by weight and an oxygen content of <0.5% by weight. The average diameter of the powder particles is preferably 1 to 10 μm, and their specific surface area (BET of the powder particles) is preferably 0.1 to 2.5 m 2 / g.
[0025] In one embodiment, the silicon-based coating comprises a fluorine-containing composition of formula (I):
[0026] Si1-0.75c M c O 2-0.5c F d (I).
[0027] In the above formula (I), M is B or Al, preferably B.
[0028] In the fluorine-containing composition of formula (I), the index c is a number in the range of 0.01 to 0.5, preferably in the range of 0.05 to 0.3 and particularly preferably in the range of 0.085 to 0.2.
[0029] The index d is a number in the range from 0.04 to 2, preferably in the range from 0.2 to 1.2 and particularly preferably in the range from 0.34 to 0.8.
[0030] Preferably, the index c and the index d have the following relationship: d=4c.
[0031] The silicon-based coating may preferably comprise >5 to 45 wt. %, more preferably 10 to 40 wt. % and particularly preferably 20 to 35 wt. % of at least one fluorine-containing composition of the formula (I), based on the total weight of the silicon-based coating.
[0032] In addition to the above-mentioned silicon-based coatings, the coating can also be based on metal oxides, such as aluminum oxide (Al2O3), magnesium oxide (MgO) or titanium oxide (TiO2, TiO, Ti2O3). Such coatings can be prepared by decomposition of metal alkoxides. Metal alkoxides are generally represented by the formula M 2 (OR')(OR”)…(OR n ) is given by, where M 2 is a metal, and n is the valence of the metal. R', R", R n R represents an organic residue which may be identical or different. For example, R represents a linear or branched alkyl group or a substituted or unsubstituted aryl group. Here, R represents a C1-C8 alkyl group, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl or tert-butyl, n-hexyl, 2-ethylhexyl, or a C6-C8 12 Aryl, such as phenyl, 2-, 3- or 4-methylphenyl, 2,4,6-trimethylphenyl or naphthyl. Methyl, ethyl and isopropyl are preferred. Further details of the method for coating the soft magnetic powder with metal oxides (especially SiO2) are described below.
[0033] In addition, the fluorine component of this fluorine-containing composition can be embedded in SiO2 matrix and / or be attached to SiO2 on the surface of coating.The fluorine component of this fluorine-containing composition can be evenly or unevenly distributed in SiO2 matrix.For example, this silicon-based coating can comprise one or more layers of SiO2 coating and one or more layers of fluorine-containing SiO2 coating.Alternatively or additionally, the fluorine component of this fluorine-containing composition can be attached to the SiO2 that surrounds soft magnetic powder particles on the surface of coating, wherein this SiO2 coating also can contain the fluorine component of this fluorine-containing composition.
[0034] In a further embodiment, the silicon-based coating has an average thickness of 2 to 100 nm, preferably 5 to 70 nm and particularly preferably 10 to 50 nm. In addition, the ratio of the silicon-based coating to the soft magnetic material is not higher than 0.1, preferably not higher than 0.02, and preferably, the soft magnetic powder contains 0.1 to 10 wt. %, more preferably 0.2 to 3.0 wt. %, and in particular 0.3 to 1.8 wt. % of the silicon-based coating based on the total weight of the soft magnetic powder. Thus, a significant decrease in the magnetic flux density of the magnetic core obtained by molding the soft magnetic powder can be prevented.
[0035] The soluble fluorinating agent used in the method for coating soft magnetic powders is a fluorinating agent having a solubility in ethanol of more than 15% by weight, preferably more than 20% by weight, particularly preferably more than 25% by weight at 0°C. Alternatively, the fluorinating agent can be specified to have a very high solubility in water of more than 25% by weight, preferably more than 30% by weight, particularly preferably more than 35% by weight at 20°C. It has been found that fluorinating agents with lower solubility tend to precipitate from the solution if the solution is prepared in advance and stored at ambient temperature. This is usually observed for BF3·NH2-CH2-Ph - its solubility in ethanol at 0°C was found to be about 10% by weight. Fluorinating agents with sufficient solubility in ethanol are generally ionic fluorinating agents. Alternatively or additionally, it is also particularly preferred that the fluorinating agent is liquid at room temperature and / or can be prepared from components that are liquid at room temperature.
[0036] In a particularly preferred embodiment, the solution of the soluble fluorinating agent in ethanol has a pH of 0 to 10, preferably 6 to 9. Considering the potential corrosion of the equipment used for preparation (i.e., the reactor) during the coating process, a pH of 6 to 9, preferably 7 to 9 is preferred. In addition, the preferred pH range enables mild conditions for coating the soft magnetic powder.
[0037] Preferably, at least one fluorinating agent has formula (II):
[0038] [Q][MF4] (II)
[0039] in
[0040] M is B or Al; and
[0041] Q is selected from H + 、Na + , K + , Rb + , Cs + or [NR 1 4] + A cationic group, where R 1 Independently selected from -H, -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 6-18 -aryl groups, each of which may be substituted with at least one group of the formula -OR 2 The group represented by R 2 Independently selected from -H, -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 1-18 -Aryl.
[0042] In a preferred embodiment of the present invention, M is selected from B in formula (II).
[0043] Furthermore, preferred embodiments include the following: + or [NR 1 4] + The cationic group Q, where R 1 As defined above.
[0044] In one embodiment, at least one substituent R 1 Selected from -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 6-18 -aryl (ie, groups as defined above except -H), each of which may be substituted with at least one radical of the formula -OR 2 The group represented by R 2 As defined above. In an alternative embodiment, at least two substituents R 1 Selected from -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 6-18 -aryl groups (ie, other than -H), each of which may be substituted with at least one group of the formula -OR 2 The group represented by R 2 As defined above. In an alternative embodiment, at least three substituents R 1 Selected from -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 6-18 -aryl groups (ie, other than -H), each of which may be substituted with at least one group of the formula -OR 2 The group represented by R 2As defined above.
[0045] In a further preferred embodiment, the at least one fluorinating agent of formula (II) is selected from HBF4, [NH4] [BF4] and [(R 4 -OR 3 ) x -NH 3-x ][BF4], where R 3 Representative formula - (C n H 2n+p )-, wherein n is an integer from 1 to 6, and p is an integer selected from 0 and -2;
[0046] R 4 Selected from -H or -(C m H 2m+q )-CH3, wherein m is an integer from 0 to 6, q is an integer selected from 0 and -2, provided that when m=0, then q=0, and
[0047] x is an integer from 1 to 3.
[0048] In a preferred embodiment, n is an integer from 1 to 3.
[0049] In an alternative preferred embodiment, p is zero.
[0050] In a further alternative preferred embodiment, m is an integer selected from 0 to 2.
[0051] In a further alternative preferred embodiment, q is zero.
[0052] In one embodiment, R 3 It represents a group selected from -(CH2)-, -(C2H4)-, -(C3H6)-, -(CH3-CH(CH3))-, and preferably represents -(C2H4)-.
[0053] In one embodiment, R 4 represents a group selected from -H and -CH3, preferably represents -H.
[0054] In a particularly preferred embodiment, at least one fluorinating agent of formula (II) is represented by the formula [(R 4 -OR 3 ) x -NH 3-x ][BF4] means, where R 3 Representative formula - (C n H 2n+p )-, wherein n is an integer from 1 to 3, and p is 0; and R 4 is -H.
[0055] In a further particularly preferred embodiment, at least one fluorinating agent of formula (II) is of the formula [(R 4 -OR 3 ) x -NH 3-x ][BF4] represents, where R 3 represents a group selected from -(CH2)-, -(C2H4)-, -(C3H6)-, -(CH3-CH(CH3))-, and preferably represents -(C2H4)-, and R 4 is -H.
[0056] In a further embodiment, x is an integer selected from 1 and 2, and in a particularly preferred embodiment, x represents 1.
[0057] Particularly preferably, the soluble fluorinating agent is selected from HBF4, [NH4][BF4], [HOCH2-NH3][BF4], [HOC2H4-NH3][BF4], [HOC3H6-NH3][BF4], [HOC4H8-NH3][BF4], [HOC5H 10 -NH3][BF4] and [HOC6H 12 [-NH3][BF4]. In particular, [HOC2H4-NH3][BF4] is preferably used as a soluble fluorinating agent. These fluorinating agents combine solubility in ethanol, stability in solution, accessibility and excellent properties in terms of performance as fluorinating agents and the performance of silicon-based coatings obtained therewith. In addition, these fluorinating agents are characterized by having a lower toxicity than fluorinating agents such as H2SiF6 known from EP 2 871 646 A1.
[0058] Formula [(R 4 -OR 3 ) x -NH 3-x The compound of [BF4] can be easily prepared by mixing HBF4 and R in a ratio of 1:0.5 to 1:4, preferably 1:0.8 to 1:3, more preferably 1:0.9 to 1:2 and especially 1:1 to 1:1.5 in a suitable solvent (e.g. ethanol) at room temperature. 4 -OR 3 The resulting solution is generally stable at room temperature and can be stored without deterioration or sedimentation.
[0059] The soluble fluorinating agent according to the invention is characterized in particular by being a compound with good solubility in ethanol. In a preferred embodiment, the soluble fluorinating agent is preferably a liquid compound or is prepared in situ from a liquid compound, which is therefore easy to manage. The solution thus obtained is well compatible with corrosion-sensitive materials (e.g. reactor surfaces).
[0060] In order to coat the soft magnetic powder with silicon dioxide (SiO2), the silicon-based solution preferably contains a silicon alkoxide, which is added to the silicon-based solution in one or more steps. Suitable silicon alkoxides are, for example, tetramethyl orthosilicate (TMOS), tetraethyl orthosilicate (TEOS), tetrapropyl orthosilicate and tetraisopropyl orthosilicate or mixtures thereof. Such silicon alkoxides provide a soluble form of silicon that does not contain any water or hydroxyl groups. Thus, a controlled hydrolysis silicon product can be obtained. TEOS is preferably used as the silicon alkoxide. Also suitable are silicon alkoxides having two or three OR n silane radical, where R n are residues as given above, and two or one X 1 The groups are directly bonded to the silane, where X 1 are residues such as H, methyl, ethyl, C3 to C 18 or propylamine, or even more complex examples such as (3-glycidyloxypropyl)triethoxysilane and mixtures thereof, which may further be mixed with any of the above siliconates.
[0061] The soft magnetic powder is preferably mixed with a silicon-based solution, and the soluble fluorinating agent is added after the soft magnetic powder is at least partially treated with the silicon-based solution. For example, the soluble fluorinating agent is added immediately during and / or after the treatment with the silicon-based solution. Here, immediately after the treatment with the silicon-based solution refers to the step that directly follows the last step of the treatment with the silicon-based solution. The last step of the treatment with the silicon-based solution generally includes or consists of the distillation and drying of the coated soft magnetic powder, thereby providing a dry coated soft magnetic powder. In the step directly after the treatment with the silicon-based solution, a solvent containing the fluorinating agent can be added to the coated soft magnetic powder to provide a soft magnetic powder coated with a silicon-based coating containing one of the fluorine-containing compositions described herein.
[0062] In principle, the solution can also be based on other metals and contain corresponding metal alkoxides in order to coat the soft magnetic powder with metal oxides. For example, the solution can be based on titanium, magnesium (Mg) or aluminum to produce aluminum oxide (Al2O3), magnesium oxide (MgO) or titanium oxide (TiO2, TiO, Ti2O3) coatings. In addition, the solution can be based on a mixture of metals such as Si, Al, Mg or Ti and contain corresponding metal alkoxide mixtures to obtain a mixed coating. Preferably, the decomposition of the metal alkoxide is carried out by hydrolysis. For hydrolysis, the metal-based solution further contains an inert suspending agent, water and a possible catalyst.
[0063] The reaction mixture comprising soft magnetic powder, metal-based solution and optional fluorinating agent can be prepared stepwise or gradually in one or more steps. Preferably, the reaction mixture is prepared stepwise. In this case, stepwise refers to adding at least one component of the reaction mixture in one or more steps during the hydrolysis process, wherein the stepwise addition can also be included in adding at a certain rate within a specific time range. Thus, the component can be added once in one step. Alternatively, the component can be added at regular or irregular intervals in at least two steps. Gradually means adding components at a fixed rate or at regular intervals (e.g., per minute or per second) during the hydrolysis process. Preferably, metal alkoxide and / or fluorinating agent are added stepwise.
[0064] In the first process step, the soft magnetic powder can be mixed with an inert suspending agent, such as water and / or an organic solvent. Suitable organic solvents are protic solvents, preferably monovalent or divalent alcohols, such as methanol, ethanol, isopropanol, ethylene glycol, diethylene glycol or triethylene glycol, or aprotic solvents, preferably ketones, such as acetone, diketones, ethers, such as diethyl ether, di-n-butyl ether, dimethyl ether of ethylene glycol, diethylene glycol or triethylene glycol, or nitrogen-containing solvents, such as pyridine, piperidine, N-methylpyrrolidine or aminoethanol. Preferably, the organic solvent is miscible with water. The suspending agent can be an organic solvent or an organic solvent mixed with water. Preferred organic solvents are acetone, isopropanol and ethanol. Ethanol is particularly preferred. The content of the inert suspending agent in the metal-based solution can be up to 70 weight %. Preferably, the content of the inert suspending agent is 10 to 50 weight %.
[0065] The mixture of soft magnetic powder and suspending agent is selected to obtain a miscible solution. In order to improve the output per unit volume and time, a high solid fraction is advantageous. The optimal solid fraction can be easily obtained by conventional experiments that can find the optimal fraction of the reaction mixture. In addition, a mechanical agitator or a pump / nozzle device can be used to increase the solid fraction.
[0066] In the second process step, a metal alkoxide can be added to the mixture. The metal alkoxide can be added as is to the reaction mixture or dissolved in an organic solvent. If an organic solvent is used, the organic solvent contains 10 to 90% by weight, preferably 50 to 80% by weight, of the metal alkoxide. The metal alkoxide can be added stepwise or gradually. Preferably, the metal alkoxide is added stepwise in more than one step, preferably in two steps. For example, at most 90%, at most 50% or at most 20% of the total amount of metal alkoxide required for the hydrolysis is first added to the reaction mixture, and the remainder is added at a later stage of the process.
[0067] The total amount of metal alkoxide added to the metal-based solution depends on the desired coating thickness. According to the particle size distribution, the profile of the particles (needle-shaped or spherical) and the amount of powder particles that increase the total specific surface area can be easily determined. Alternatively, the specific surface area can be determined using known methods such as the BET method. According to the desired thickness of the coating and the density of the metal oxide, the required amount of the metal oxide can be calculated. The total amount of the required metal alkoxide can then be determined by the stoichiometry of the reaction.
[0068] After the addition of the metal alkoxide, hydrolysis occurs automatically as soon as water is added to the reaction mixture in the third step. Preferably, the total amount of water corresponds to at least two times, more preferably at least five times, the stoichiometric amount required for the hydrolysis of the metal alkoxide. Typically, the total amount of water is not more than one hundred times, preferably twenty times, the required stoichiometric amount. In the third step, a portion of water is added that corresponds to the portion of the metal alkoxide added to the reaction mixture in the second process step.
[0069] In order to further accelerate the hydrolysis, a catalyst such as an alkaline or acidic catalyst can be added to the reaction mixture. The amount of the added catalyst can also be adjusted to the fraction of the metal alkoxide added to the reaction mixture in the second process step. Suitable acidic catalysts are, for example, dilute mineral acids such as sulfuric acid, hydrochloric acid, nitric acid, and suitable basic catalysts are, for example, dilute alkaline lye such as caustic soda. Preferably, a dilute ammonia solution is used so that the catalyst and water are added simultaneously in one step.
[0070] The preferred molar ratio of catalyst to metal alkoxide, in particular ammonia to silicon alkoxide, is from 1:1 to 1:2, preferably from 1:1.1 to 1:1.8. This ratio enables the formation of a coating having good properties.
[0071] In the fourth process step, by heating the prepared reaction mixture, the decomposition of metal alkoxide (preferably silicon alkoxide) can be further promoted. The reaction mixture can be heated to a temperature just below the boiling point of the reaction mixture or up to reflux. For example, in the case of ethanol, the temperature remains below 80°C, for example, about 60°C. The reaction mixture can be kept for several hours, for example, 3 hours, at an increased temperature in reflux. Usually, the reaction mixture is dispersed by a mechanical stirrer. In addition, a dispersant such as anionic or ionic surfactants, acrylic resins, pigment dispersants or higher alcohols such as hexanol, octanol, nonanol or dodecanol can be added to the reaction mixture.
[0072] If the metal alkoxide is added gradually in more than one step, the metal alkoxide, water and the remainder of the catalyst may be added in one or more steps while the reaction mixture is maintained at an elevated temperature. A two-step addition of the metal alkoxide is preferred, wherein the remainder of the metal alkoxide, water and catalyst are added in one step while the reaction mixture is maintained at an elevated temperature.
[0073] After the hydrolysis, the reaction mixture is distilled and dried in the fifth and sixth process steps. The point in time at which the hydrolysis is finished can be detected by monitoring the decrease in the water content in the reflux. If the water content is low enough, the mixture can be distilled and dried, leaving a soft magnetic powder coated with SiO2. In this case, the level of the water content can be easily determined by routine experiments.
[0074] In one embodiment of the method, the soluble fluorinating agent is added during the treatment with the silicon-based solution. Thus, the soluble fluorinating agent is added before the end of the treatment with the silicon-based solution, ie before the distillation and drying of the reaction mixture.
[0075] In a further embodiment, based on the total amount of soft magnetic powder, 1.0×10 -2 Up to 5.5×10 -2 % fluorinating agent is added to the silicon-based solution. Preferably, 1.5×10 -2 Up to 3.5×10 -2 mol% of fluorinating agent, especially 1.7×10 -2 to 2.7×10 -2 mol % of fluorinating agent.
[0076] In a further embodiment, 0.1 to 10 mmol of fluorinating agent per kg of soft magnetic powder is added to the silicon-based solution. Preferably, 1 to 7 mmol of fluorinating agent, in particular 3 to 5 mmol of fluorinating agent, per kg of soft magnetic powder is used.
[0077] In a further embodiment, 0.25 to 5 mol % of fluorinating agent is added to the silicon-based solution, based on the total amount of Si in the silicon-based solution. Preferably, 1 to 4.5 mol % of fluorinating agent is used, in particular 1.5 to 3.5 mol % of fluorinating agent.
[0078] The fluorinating agent can be added in solid or solution form. Preferably, the solution of the fluorinating agent has a concentration of about 5 to 30% by weight, in particular 10 to 20% by weight. Typically, the solvent is water, ethanol or the aforementioned inert suspending agent. In a particularly preferred embodiment, the solution comprises at least one fluorinating agent and at least ethanol.
[0079] In a further preferred embodiment, only a portion of the silicon alkoxide is added together with the fluorinating agent. For example, 100% of the silicon alkoxide is required to form 1-2% by weight of SiO2 on the iron powder, and 25%, 50% or 75% is added together with the fluorinating agent.
[0080] The preferred molar ratio of fluorine atoms added in the soluble fluorinating agent to silicon in the added silicon alkoxide (molar ratio F:Si) is 1:3 to 1:18, preferably 1:5 to 1:15, in particular 1:8 to 1:13, wherein the molar ratio refers to the ratio of the entire coating. The molar ratio F:Si can be, for example, 1:9.1. With this ratio, the coating can be suitable for providing high magnetic permeability due to the thickness of the coating and good temperature stability.
[0081] In addition, during the treatment with the silicon-based solution, the soluble fluorinating agent can be added gradually in one or more steps. Preferably, the soluble fluorinating agent is added in one step. The time point for adding the soluble fluorinating agent can be selected after the second process step, that is, after the addition of the metal alkoxide, and before the fifth process step, that is, somewhere before distillation and drying. Preferably, the soluble fluorinating agent is added while the reaction mixture is maintained at an elevated temperature. Particularly preferably, the soluble fluorinating agent is added before the addition of the remaining part of the metal alkoxide, while the reaction mixture is maintained at an elevated temperature. Thus, the soluble fluorinating agent can be added after at least 20%, preferably at least 50%, and particularly preferably at least 70% of the hydrolysis reactants (e.g., metal alkoxides) have been added.
[0082] The above method is a preferred embodiment. However, the order of the process steps can be varied. The metal alkoxide can, for example, be added simultaneously to a reaction mixture comprising a soft magnetic powder, an inert suspending agent, water and a catalyst, or water and the metal alkoxide can be added simultaneously. However, in such embodiments, it is preferred to gradually add the metal alkoxide in more than one step, wherein the soluble fluorinating agent is added once as described above.
[0083] Alternatively or additionally, a soluble fluorinating agent is added immediately after treatment with a silicon-based solution. If a soluble fluorinating agent is added immediately after treatment with a silicon-based solution, the soft magnetic powder is treated with a silicon-based solution containing or not containing a soluble fluorinating agent. In a process step after the alkoxide coating process, the coated soft magnetic powder can be mixed with a solvent (such as ethanol) and a soluble fluorinating agent.
[0084] The soft magnetic powder coated according to the above method and the above coated soft magnetic powder are characterized by an improved magnetic permeability and an unchanged or even improved temperature stability compared to the prior art material disclosed in EP 2 871 646 A1.
[0085] The soft magnetic powder coated according to the above method and the soft magnetic powder of the above-mentioned coating are particularly suitable for manufacturing electronic components. Electronic components (such as magnetic cores) can be obtained by, for example, compression molding or injection molding of the soft magnetic powder coated. In order to manufacture such electronic components, the soft magnetic powder coated is usually mixed with one or more types of resins, such as epoxy resins, carbamate resins, polyurethane resins, phenolic resins, amino resins, silicone resins, polyamide resins, polyimide resins, acrylic resins, polyester resins, polycarbonate resins, norbornene resins, styrene resins, polyether sulfone resins, silicone resins, polysiloxane resins, fluororesins, polybutadiene resins, vinyl ether resins, polyvinyl chloride resins or vinyl ester resins. The method for mixing these components is not limited, and mixing can be carried out by mixing machine, such as ribbon mixer, drum mixer, Nauta mixer, Henschel mixer or super mixer or kneader, such as Banbury mixer, kneader, roller, kneading-extruder (kneader-ruder), paddle mixer, planetary mixer or single shaft or twin shaft extruder.
[0086] In order to manufacture molded products, the soft magnetic powder can be mixed with one or more types of resins to provide molded powders or instant press powders. For molded powders, the mixture of the coated soft magnetic powder and the resin can be heated and melted at the melting point of the resin (preferably a thermoplastic resin), and then molded into an electronic component (such as a magnetic core) of a desired shape. Preferably, the mixture is pressed in a mold to obtain a magnetic or magnetizable molded product. The compression produces a molded product with high strength and good temperature stability.
[0087] Another method for making molded articles includes ready to press powder, which contains a coated soft magnetic powder further coated with a resin. Such ready to press powder can be pressed in a mold at a pressure of up to 1000 MPa, preferably up to 500 MPa, with or without heating. After compression, the molded article is cured. The method of coating the soft magnetic powder with a resin includes, for example, the following steps: dissolving a resin (e.g., an epoxy resin) in a solvent, adding the soft magnetic powder to the mixture, removing the solvent from the mixture to obtain a dry product, and grinding the dry product to obtain a powder. Ready to press powder is used to produce magnetic or magnetizable molded articles.
[0088] Powder injection molding enables the cost-effective and efficient production of complex metal parts. Powder injection molding generally involves molding soft magnetic powders into the desired shape together with a polymer as a binder, followed by removal of the binder and compacting the powder into a solid metal part in a sintering stage. This is particularly effective with carbonyl iron powders, as the spherical iron particles can be packed very closely together.
[0089] The soft magnetic powder treated according to the above method or containing the above-mentioned silicon-based coating with a fluorine-containing composition can be used for electronic components. This type of molded product is particularly useful as a coil core or coil frame used in electrical engineering. Coils with corresponding coil cores or coil frames are used, for example, as electromagnets, generators, transformers, inductors, laptops, notebook computers, mobile phones, motors, AC inverters, electronic components in the automotive industry, toys and magnetic field concentrators. Electronic components are particularly used for core components in electrical, electromechanical and magnetic devices such as electromagnets, transformers, motors, inductors and magnetic components. Other uses of coated soft magnetic powders include the manufacture of radio frequency identification (RFID) tags and elements for reflecting or shielding electromagnetic radiation. In the production of RFID tags, soft magnetic powders can be used in printed RFID structures, which are rice-sized tags for automatic target positioning or identification. Finally, electronic components made of soft magnetic powders can be used to shield electronic devices. In such applications, the radiated alternating magnetic field causes the powder particles to rearrange themselves continuously. Due to the friction caused, the powder particles convert the energy of electromagnetic waves into heat. Example
[0090] Coating of Metal Powders - General Procedure A (Prepared using a Planetary Mixer)
[0091] In a heatable planetary mixer, 2700 kg of carbonyl iron powder (e.g. available from BASF, with a purity of 99.5 g per 100 g of iron and an average particle size of d 50 4.5 to 5 μm). The mixer was equipped with a condenser and flushed with argon to obtain an inert atmosphere. While stirring, 480 grams of ethanol were added. Subsequently, 75% by weight of the total amount of TEOS was added (the total amount of TEOS used in each experiment is given in Tables 1 to 6 below). Subsequently, 80% by weight of the total amount of NH3 aqueous solution was added, which had an NH3 concentration of 5% by weight (the total amount of NH3 aqueous solution used in each experiment is given in Tables 1 to 6 below). The temperature was now raised to 60° C. while stirring. After stirring at this temperature for about 2 hours, a fluorinating agent was added to the reaction mixture in the form of an ethanol solution with a concentration of about 10 to 15% by weight. The temperature was maintained while adding the remaining 25% by weight of TEOS and the remaining 20% by weight of NH3 solution over a period of about one hour. The mixture was stirred for another 45 minutes. The condenser was removed and the product was stirred for another hour. During this period, the inert gas flow was increased to 600 l / h, and some solvents had been removed. After one hour, the temperature was raised to 90° C. and the product was stirred under an increased inert gas flow until dry. The coated carbonyl iron powder was obtained in the form of a grey powder.
[0092] Coating of Metal Powders - General Procedure B (Preparation in Flask)
[0093] 355 g of ethanol was added to a homogenizer (rotor / stator homogenizer, available from ) and a condenser flask and flushed with argon to obtain an inert atmosphere. The homogenizer was set to 2000 rpm. While stirring, 500 grams of carbonyl iron powder (e.g., available from BASF, with a purity of 99.5 grams per 100 grams of iron and an average particle size of d 50 4.5 to 5 μm). The homogenizer speed is increased to 6000 rpm. Subsequently, 68 wt% of the total amount of TEOS is added (the total amount of TEOS used in each experiment is given in Table 7 below). Subsequently, 100 wt% of the total amount of NH3 aqueous solution with an NH3 concentration of 2.5 wt% is added (the total amount of NH3 aqueous solution used in each experiment is given in Table 7 below). The temperature is now raised to 45°C for 20 minutes, then to 55°C for 20 minutes, and finally to 65°C for 20 minutes while stirring. After stirring for about another hour at this temperature, a fluorinating agent is added to the reaction mixture in the form of an ethanol solution with a concentration of about 10 to 15 wt%. The temperature is maintained while the remaining 32 wt% of TEOS is quickly added. The mixture is stirred for another hour. In a planetary mixer, the product is stirred at 95°C for about 3 hours at an inert gas flow of 600 l / h and 47 rpm until the solvent is removed. A coated carbonyl iron powder is obtained in the form of a gray powder.
[0094] Mix with epoxy resin
[0095] The epoxy resin was prepared by dissolving 2.8 g of epoxy resin in 15 to 20 ml of solvent (methyl ethyl ketone or acetone) and adding 0.14 g of dicyandiamide (e.g., available from Alzchem). 100 g of coated carbonyl iron powder (CIP) was mixed with an epoxy resin (e.g. Epikotet TM 1004). In a glass beaker, the coated CIP was stirred with the epoxy formulation at 1000 rpm using a dissolver mixer. After mixing, the slurry was poured into an aluminum plate, which was then placed in a fume hood for 8 hours, and the resulting dry CIP epoxy resin plate was ground in a knife grinder for 10 seconds to obtain a ready-to-press powder. It contains 2.8% by weight of epoxy resin.
[0096] Toroidal core molding and wiring
[0097] 6.8 g (± 0.1 g) of the ready-to-press powder is placed in a steel mold of a ring with an outer diameter of 20.1 mm and an inner diameter of 12.5 mm to obtain a height of about 5-6 mm. The ready-to-press powder is molded at 440 MPa for a few seconds. The density of the toroidal core is calculated from the exact mass and height of the ring. The toroidal core is wound with 20 turns of insulated 0.85 mm copper wire, such as Isoladrht available from Multogan 2000MH 62, to determine the magnetic permeability and resistivity.
[0098] Measuring magnetic permeability and resistivity
[0099] An LRC meter was used to measure the magnetic permeability of the toroidal core. All measurements were performed at 100kHz with a 0V DC bias. A test AC current of 10mA was applied to the toroidal core.
[0100] To measure the resistivity of the pressed part, a power supply was connected in series with the voltmeter and the sample. A voltage of 298 volts was applied to the multimeter and sample connected in series. The voltage reading of the multimeter was used to estimate the resistance of the sample using the following equation.
[0101] R 样品 =R 仪表 ×(V PS –V 仪表 ) / V 仪表
[0102] Where R 样品 is the resistance of the cylinder, R 仪表 is the internal resistance of the instrument, V PS is the applied voltage from the power supply (=298V), and V 仪表 is the reading from the voltmeter.
[0103] Temperature stability
[0104] Before the temperature stability test can begin, the epoxy is cured. This is done by placing the toroidal core in an oven set at 70°C. After 2 hours, the toroidal core is placed in a second oven set at 155°C. After 2 hours, the toroidal core is removed for resistivity testing.
[0105] Now, the toroidal core is placed again in an oven set at 180° C. for a certain amount of time. For example, after an additional 24-hour temperature treatment at 180° C., the temperature stability after 24 hours is measured. If the voltage measured after 24 hours at 180° C. is approximately 0 V and the voltage measured after 48 hours at 180° C. is ≤30 V, preferably ≤25 V, in particular ≤20 V, the toroidal core is marked as temperature-stable. In a further preferred embodiment, the voltage measured after 120 hours at 180° C. is preferably ≤70 V, more preferably ≤30 V, in particular ≤10 V.
[0106] Test Results
[0107] After temperature treatment of the compacted samples, the magnetic permeability and resistivity were determined as described above. The results are given in Tables 1 to 7. The corrosion tests are summarized in Table 8.
[0108] Examples E-1 to E-3 and comparative examples C-1 and C-2 are summarized in Table 1. The examples and comparative examples allow the comparison of coated carbonyl iron powders (CIP) using different fluorinating agents under otherwise identical conditions. From the results it can be seen that all compounds show good to excellent properties in terms of magnetic permeability as well as heat resistance after the specified time.
[0109] As shown by Examples E-4 to E-8 shown in Table 2, the fluorinating agent according to the invention allows a significant reduction in the amount used to achieve excellent resistivity results. Starting from 9.6 mmol fluorinating agent / 1 kg CIP (the amount conventionally used in EP 2 871 646 A1), if HBF4 is used, the amount of fluorinating agent can be reduced by about 30% to 6.70 mmol / kg without adversely affecting the thermal stability. In fact, after 48 hours, this reduction leads to a slight improvement in resistivity.
[0110] Table 3 shows different reaction conditions by different ratios of TEOS, ammonia and fluorinating agent, which make it possible to influence the product properties. It can be seen that particularly good properties can be achieved in terms of resistivity and permeability if the molar ratio of ammonia to TEOS is in the range of 1:1.1 to 1:1.8.
[0111] Examples E-16 to E-19 in Table 4 demonstrate that the amount of fluorinating agent can be significantly reduced if [NH3EtOH][BF4] is used, compared to BF3·NH2-CH2-Ph (see Comparative Example CE-4).
[0112] Table 5 shows that the use of [NH3EtOH][BF4] as the fluorinating agent can further reduce the amount of SiO2 and the fluorinating agent compared to BF3·NH2-CH2-Ph. In particular, when [NH3EtOH][BF4] is used, the amount of the fluorinating agent can be reduced by about 65 mol%, the amount of TEOS can be reduced by 10 mol%, and the amount of NH3 solution can be reduced by 20 wt% compared to BF3·NH2-CH2-Ph, without significant deterioration in product properties.
[0113] Table 6 compares the use of [NH3EtOH][BF4] as a fluorinating agent with the known fluorinating agent BF3·NH2-CH2-Ph in different combinations in terms of the amounts of SiO2 and NH3 solution, while in the example pairs CE-6 / E25, CE-7 / E26, CE-8 / E-7 and CE-9 / E8, the amount of fluorine atoms remains approximately constant. It can be seen from these examples and comparative examples that the comparative examples using BF3·NH2-CH2-Ph generally result in higher voltages (i.e., higher resistivity) after exposing the prepared toroidal cores to elevated temperatures. On the other hand, the test samples using BF3·NH2-CH2-Ph generally exhibit lower magnetic permeability. In contrast, the examples using [NH3EtOH][BF4] according to the present invention exhibit a unique combination of relatively high magnetic permeability and low resistivity (i.e., measured voltage) after exposure to elevated temperatures. For example, by comparing the examples that exhibit a magnetic permeability of approximately 17 (+ / - 0.05) (i.e., Examples E-26, CE-8, and CE-9), it is apparent that similar magnetic permeabilities are achieved in accordance with the present invention while having significantly lower resistivities after 48 hours at 180°C (15 V for E-26, 143 V for CE-8, and 105 V for CE-9).
[0114] Table 7 shows the test results of two examples E-29 and E-30, both of which were exposed to 180° C. for 120 hours, and both examples showed excellent results in terms of magnetic permeability and resistivity.
[0115]
[0116]
[0117]
[0118]
[0119]
[0120]
[0121]
[0122] Corrosion test
[0123] The corrosion of different stainless steel materials was tested by exposing samples (size: 50×20×2 mm) of stainless steel materials (test materials include 1.4541, 1.4571, 1.4462, 1.0425) to the corresponding additive solution for 4×7 days at T=60°C, wherein the solution was replaced with fresh solution every week. The test was carried out in a PTFE container equipped. The test results are summarized in Table 8.
[0124] Table 8 Corrosion test results
[0125] Additive solution pH corrosion <![CDATA[[NH3EtOH][BF4] (15 wt% in ethanol)]]> 6 none <![CDATA[BF3·NH2-CH2-Ph (15 wt% in ethanol)]]> 4 None / Almost None <![CDATA[HBF4 (3 wt% in ethanol)]]> 3 Almost no <![CDATA[HBF4 (10 wt% in ethanol)]]> 3 Almost no / strong <![CDATA[HBF4 (10 wt% in water)]]> 0-1 powerful
[0126] It can be seen that the solution of HBF4 causes almost no corrosion to strong corrosion of the stainless steel material, depending on the solvent used. In contrast, BF3·NH2-CH2-Ph (15 wt % in ethanol) and [NH3EtOH][BF4] (15 wt % in ethanol) cause essentially no or almost no corrosion. Therefore, from the perspective of product purity, NH3EtOH][BF4] and BF3·NH2-CH2-Ph are preferred in the method of coating soft magnetic powders compared to HBF4. However, the latter can be used in low concentrations (i.e., 3 wt % in ethanol).
[0127] From the above, the advantages of the present invention can be summarized as follows.
[0128] The use of a fluorinating agent of formula (II) in a method for coating a soft magnetic powder, wherein the coating comprises at least one fluorine-containing composition comprising a composition of formula (I), can provide a coated soft magnetic powder having the following properties: a higher magnetic permeability at a comparable resistivity compared to known fluorinating agents. On the other hand, a higher resistivity can be achieved at a comparable magnetic permeability. In addition, the fluorinating agent according to the present invention is more stable in solution, less prone to precipitation from solution (i.e., has a higher solubility), shows improved material compatibility (particularly in terms of corrosion) and improved operability.
Claims
1. A method for coating a soft magnetic powder, wherein the coating formed comprises at least one fluorine-containing composition comprising a composition of formula (I), Si 1-0.75c M c O 2-0.5c F d (I) in c is in the range of 0.01 to 0.5, d is in the range of 0.04 to 2, and M is B or Al, The soft magnetic powder is mixed with a silicon-based solution containing at least one soluble fluorinating agent, wherein the at least one soluble fluorinating agent is a compound of formula (II): [Q][MF4] (II) in M is B or Al; and Q is selected from H + 、Na + , K + , Rb + , Cs + or [NR 1 4] + A cationic group, where R 1 Independently selected from -H, -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 6-18 -aryl, each of which is optionally substituted with at least one radical of the formula -OR 2 The group represented by R 2 Independently selected from -H, -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 1-18 -Aryl.
2. The method of claim 1, wherein the soft magnetic powder is mixed with a silicon-based solution and the at least one soluble fluorinating agent is added after the soft magnetic powder has been at least partially treated with the silicon-based solution.
3. The method of claim 1, wherein the at least one soluble fluorinating agent is a compound of formula (II) [Q][MF4] (II) in M is selected from B, and Q is selected from H + or [NR 1 4] + The cationic group Where R 1 Independently selected from -H, -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 6-18 -aryl, each of which is optionally substituted with at least one radical of the formula -OR 2 The group represented by R 2 Independently selected from -H, -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 1-18 -Aryl.
4. The method of claim 2, wherein the at least one soluble fluorinating agent is a compound of formula (II) [Q][MF4] (II) in M is selected from B, and Q is selected from H + or [NR 1 4] + The cationic group Where R 1 Independently selected from -H, -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 6-18 -aryl, each of which is optionally substituted with at least one radical of the formula -OR 2 The group represented by R 2 Independently selected from -H, -C 1-12 -alkyl, -C 2-12 -alkenyl and -C 1-18 -Aryl.
5. The method of claim 1, wherein the soluble fluorinating agent is selected from the group consisting of HBF4, [NH4] [BF4] and [(R 4 -OR 3 ) x -NH 3-x ][BF4], in R 3 Representative formula - (C n H 2n+p )-group; n is an integer from 1 to 6, p is an integer selected from 0 and -2, R 4 Selected from -H or -(C m H 2m+q )-CH3, m is an integer from 0 to 6, q is an integer selected from 0 and -2, The condition is that when m = 0, then q = 0, and x is an integer selected from 1-3.
6. The method of claim 2, wherein the soluble fluorinating agent is selected from the group consisting of HBF4, [NH4] [BF4] and [(R 4 -OR 3 ) x -NH 3-x ][BF4], in R 3 Representative formula - (C n H 2n+p )-group; n is an integer from 1 to 6, p is an integer selected from 0 and -2, R 4 Selected from -H or -(C m H 2m+q )-CH3, m is an integer from 0 to 6, q is an integer selected from 0 and -2, The condition is that when m = 0, then q = 0, and x is an integer selected from 1-3.
7. The method of claim 3, wherein the soluble fluorinating agent is selected from the group consisting of HBF4, [NH4] [BF4] and [(R 4 -OR 3 ) x -NH 3-x ][BF4], in R 3 Representative formula - (C n H 2n+p )-group; n is an integer from 1 to 6, p is an integer selected from 0 and -2, R 4 Selected from -H or -(C m H 2m+q )-CH3, m is an integer from 0 to 6, q is an integer selected from 0 and -2, The condition is that when m = 0, then q = 0, and x is an integer selected from 1-3.
8. The method of claim 4, wherein the soluble fluorinating agent is selected from the group consisting of HBF4, [NH4] [BF4] and [(R 4 -OR 3 ) x -NH 3-x ][BF4], in R 3 Representative formula - (C n H 2n+p )-group; n is an integer from 1 to 6, p is an integer selected from 0 and -2, R 4 Selected from -H or -(C m H 2m+q )-CH3, m is an integer from 0 to 6, q is an integer selected from 0 and -2, The condition is that when m = 0, then q = 0, and x is an integer selected from 1-3.
9. The method according to any one of claims 1 to 8, wherein 0.1 to 10 mmol of fluorinating agent per kg of soft magnetic powder is added to the silicon-based solution.
10. Soft magnetic powder coated with a silicon-based coating, obtained by the method according to any one of claims 1 to 9.
11. The soft magnetic powder according to claim 10, comprising at least one fluorine-containing composition of formula (I), wherein M is B.
12. The soft magnetic powder according to claim 10 or 11, wherein the silicon-based coating comprises greater than 5 and less than or equal to 45% by weight of at least one fluorine-containing composition of formula (I).
13. The soft magnetic powder of claim 12, wherein the silicon-based coating comprises 10 to 40% by weight of at least one fluorine-containing composition of formula (I).
14. The soft magnetic powder of claim 12, wherein the silicon-based coating comprises 20 to 35% by weight of at least one fluorine-containing composition of formula (I).
15. The soft magnetic powder according to any one of claims 10 to 11, 13 to 14, wherein the fluorine component of the fluorine-containing composition is embedded in the SiO2 matrix and / or bonded to the surface of the SiO2 coating.
16. The soft magnetic powder according to any one of claims 10 to 11, 13 to 14, wherein the silicon-based coating has an average thickness of 2 to 100 nm.
17. The soft magnetic powder according to any one of claims 10 to 11, 13 to 14, wherein the soft magnetic powder comprises 0.1 to 10 wt% of a silicon-based coating layer based on the total weight of the soft magnetic powder.
18. A soft magnetic powder coated with a silicon-based coating, wherein the silicon-based coating comprises at least one fluorine-containing composition of formula (I): Si 1-0.75c M c O 2-0.5c F d (I) in c is in the range of 0.01 to 0.5, d is in the range of 0.04 to 2, The index c and the index d have the following relationship: d = 4c, and M is B or Al.
19. The soft magnetic powder of claim 18, comprising at least one fluorine-containing composition of formula (I), wherein M is B.
20. The soft magnetic powder of claim 19, wherein the silicon-based coating comprises greater than 5 and less than or equal to 45 weight percent of at least one fluorine-containing composition of formula (I).
21. The soft magnetic powder of claim 20, wherein the silicon-based coating comprises 10 to 40% by weight of at least one fluorine-containing composition of formula (I).
22. The soft magnetic powder of claim 20, wherein the silicon-based coating comprises 20 to 35% by weight of at least one fluorine-containing composition of formula (I).
23. The soft magnetic powder according to any one of claims 18 to 22, wherein the fluorine component of the fluorine-containing composition is embedded in the SiO2 matrix and / or bonded to the surface of the SiO2 coating.
24. The soft magnetic powder according to any one of claims 18 to 22, wherein the silicon-based coating has an average thickness of 2 to 100 nm.
25. The soft magnetic powder according to any one of claims 18 to 22, wherein the soft magnetic powder comprises 0.1 to 10 wt% of a silicon-based coating layer based on the total weight of the soft magnetic powder.
26. Use of the soft magnetic powder obtained by the method of any one of claims 1 to 9 or the soft magnetic powder of any one of claims 10 to 25 for manufacturing electronic components.
27. An electronic component comprising the soft magnetic powder obtained by the method of any one of claims 1 to 9 or the soft magnetic powder of any one of claims 10 to 25.