Film forming method and film forming device

By alternately supplying disiloxane hexachloride and nitride gas to form a thin SiN layer, and after modification, using plasma nitride gas for nitriding, the problem of inconsistent silicon nitride film thickness in semiconductor manufacturing is solved, and the film is realized Thick consistency and yield improvement.

CN112391607BActive Publication Date: 2024-11-05TOKYO ELECTRON LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010789975.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-19
Filing Date
2020-08-07
Publication Date
2024-11-05
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

During semiconductor manufacturing, when a silicon nitride film is formed on a substrate with Si and SiO2 films exposed on the surface, it is difficult to suppress the film thickness inconsistency caused by different incubation times, which affects the yield rate.

Method used

The SiN thin layer is formed by alternately supplying disilic hexachloride and unplasmic nitrided gas, and after modification, the plasma nitrided gas is used for nitriding, ensuring the consistent incubation time of each membrane, thereby achieving the membrane Thick consistency.

Benefits of technology

It effectively suppresses the influence of different incubation times, ensures high uniformity of the silicon nitride film, improves the yield of semiconductor products, and reduces the dependence on plasma treatment, avoids excessive nitriding and damage of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112391607B_ABST
    Figure CN112391607B_ABST
Patent Text Reader

Abstract

The present invention relates to a film forming method and a film forming device. [Subject] When forming a silicon nitride film on a substrate with a first film and a second film exposed on the surface, nitridation of the first film or the second film is suppressed, and the film thickness of each silicon nitride on the first film and the second film is made uniform. [Solution] The following steps are implemented: a step of supplying a processing gas composed of a silicon halide having a Si-Si bond to the substrate; a step of supplying a second nitriding gas that has not been plasma-formed to the substrate; a step of repeating the step of supplying the processing gas and the step of supplying the second nitriding gas in sequence to form a thin layer of silicon nitride covering the first film and the second film; a step of supplying a plasma-formed modifying gas to the substrate in order to modify the thin layer of silicon nitride; and a step of supplying a raw material gas and a first nitriding gas to the aforementioned substrate to form a silicon nitride film on the modified thin layer of silicon nitride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a film forming method and a film forming apparatus. Background Art

[0002] In the semiconductor manufacturing process, a film forming process of forming a SiN (silicon nitride) film on a semiconductor wafer (hereinafter referred to as a wafer) serving as a substrate is sometimes performed. Sometimes, films with different incubation times described later are exposed on the surface of the wafer, but even in the above case, it is required to form the above-mentioned SiN film with a highly uniform film thickness in each part of the surface of the wafer. Patent document 1 describes the following scheme: NH3 (ammonia) is supplied and adsorbed to a wafer with a Si (silicon) film and a SiO2 (silicon oxide) film exposed on the surface, and then the wafer is exposed to Ar (argon) gas plasma to nitride the above-mentioned films. Then, after the nitridation, a raw material gas containing silicon and a plasma-formed NH3 gas are alternately supplied to the wafer to form a SiN (silicon nitride) film.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-175106 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] The present disclosure provides a technology that can suppress nitridation of the first film or the second film when forming a silicon nitride film on a substrate with a first film and a second film exposed on the surface, and can make the film thickness of silicon nitride on the first film and the second film uniform.

[0008] Solutions for solving problems

[0009] The film forming method disclosed herein is a film forming method for forming a silicon nitride film on a substrate having a first film and a second film on the surface of which the incubation times required until the growth of the silicon nitride film start are different from each other when a raw material gas containing silicon and a first nitriding gas for nitriding the silicon are supplied.

[0010] The film forming method comprises the following steps:

[0011] A step of supplying a processing gas composed of silicon halide having Si-Si bonds to the substrate;

[0012] A step of supplying a second nitriding gas that has not been converted into plasma to the substrate;

[0013] a step of sequentially repeating the step of supplying the aforementioned processing gas and the step of supplying the aforementioned second nitriding gas to form a thin layer of silicon nitride covering the aforementioned first film and the aforementioned second film;

[0014] In order to modify the thin layer of silicon nitride, a step of supplying a plasma-formed modifying gas to the substrate; and

[0015] A step of supplying the source gas and the first nitriding gas to the substrate to form the silicon nitride film on the modified silicon nitride thin layer.

[0016] Effects of the Invention

[0017] According to the present disclosure, a technology is provided: when a silicon nitride film is formed on a substrate with a first film and a second film exposed on the surface, nitridation of the first film or the second film can be suppressed and the film thickness of each silicon nitride on the first film and the second film can be made uniform. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a longitudinal side view of a film forming apparatus as one embodiment of the present disclosure.

[0019] Figure 2 It is a cross-sectional top view of the aforementioned film forming device.

[0020] Figure 3 It is a longitudinal side view of the aforementioned nozzle.

[0021] Figure 4 It is a bottom view of the nozzle arranged in the aforementioned film forming device.

[0022] Figure 5 This is a longitudinal side view of a wafer processed by the aforementioned film forming apparatus.

[0023] Figure 6 This is a longitudinal side view of the aforementioned wafer.

[0024] Figure 7 This is a longitudinal side view of the aforementioned wafer.

[0025] Figure 8 This is a longitudinal side view of the aforementioned wafer.

[0026] Fig. 9 It is a flowchart showing the flow of one embodiment of a film forming method performed by the above-mentioned film forming apparatus.

[0027] Fig.10 It is a graph showing the results of the evaluation test.

[0028] Fig.11 It is a graph showing the results of the evaluation test.

[0029] Description of Reference Numerals

[0030] B Wafer

[0031] 1 Film forming device

[0032] 10. Control Unit

[0033] 12 Rotating table

[0034] 2 Nozzles

[0035] 3A~3C Plasma formation unit

[0036] 61 Si film

[0037] 62, 64 SiO2 film, SiO2 film

[0038] 63 W film

[0039] 66 Si thin layer

[0040] 67 Thin layer of SiN

[0041] 68 SiN film DETAILED DESCRIPTION

[0042] The film forming method of one embodiment of the present disclosure is first described in its outline. The embodiment is as follows: a SiN film is formed on a wafer B having a Si (silicon) film, a SiO2 (silicon oxide) film, and a W (tungsten) film as a metal film exposed on the surface. It should be noted that W is easily oxidized, and the process is performed in a state where oxygen atoms exist on the surface of the W film.

[0043] Here, the incubation time of the SiN film is described in advance. The incubation time of the SiN film refers to the time required from the start of supplying one of the gases until the start of forming the SiN film when a raw material gas containing silicon and a nitriding gas for nitriding the silicon are supplied to form the SiN film. More specifically, by supplying the raw material gas and the nitriding gas respectively, a plurality of island-shaped SiN cores are formed on the film of the base of the SiN film. The SiN cores expand and grow along the surface of the base film, and when a thin layer is formed in contact with each other, the thin layer grows as a SiN film (the film thickness increases). Therefore, the timing of the start of the growth of the above-mentioned film is the timing of the formation of the thin layer of SiN. As the base of the SiN film, depending on the type of film in contact with the SiN film, the time required for the formation and growth of the above-mentioned cores is different from each other.

[0044] Moreover, the different incubation times of the SiN films between the films means that when the raw material gas and the nitriding gas are supplied between the films under the same conditions to form the SiN films in contact with the films, the times from the start of supplying these gases to the formation of the above-mentioned thin layer are different. To be further supplemented, it means that the comparison is made without any treatment other than adsorption of the raw material gas and nitridation of silicon in the raw material gas by the nitriding gas, and the time until the above-mentioned thin layer is formed is different. That is, it means that the comparison is made without performing the treatment such as reduction and modification by hydrogen plasma as performed in the present embodiment, and the time until the above-mentioned thin layer is formed is different. It should be noted that the nitriding gas referred to here includes plasma-formed nitriding gas in addition to non-plasma-formed nitriding gas.

[0045] When the raw material gas and the nitriding gas are supplied to the base films having different incubation times, the thickness of the SiN films formed in contact with the base films fluctuates due to the difference in incubation time. Moreover, the incubation time of the SiN film is different between the W film, the SiO2 film, and the Si film formed on the wafer B of the present embodiment. Specifically, when the W film and the SiO2 film are the first film and the Si film is the second film, the incubation time of the first film is longer than the incubation time of the second film.

[0046] In this way, when forming each film of the SiN film with different incubations, as shown in the evaluation test described later, by exposing the wafer B to the plasma of N2 gas, a pretreatment is sometimes performed to make the surface state of each film consistent. After the pretreatment of exposure to the plasma of N2 gas, for example, a SiN film is formed by ALD, but the nitriding power of the plasma of N2 gas is high. Therefore, when the above-mentioned wafer B is treated with the plasma of N2 gas in this way, for example, the Si film is nitrided from the surface to the depth, and becomes SiN, and there is a concern that the yield of the semiconductor product manufactured by the wafer B will be reduced.

[0047] Therefore, in this embodiment, the pretreatment for suppressing the influence of the difference in incubation time to make the film thickness of the SiN film uniform is performed as described above to suppress the nitridation of the Si film. Specifically, first, without plasma-forming disilicon hexachloride (Si2Cl6) gas and NH3 gas (second nitriding gas), disilicon hexachloride (Si2Cl6) gas and NH3 gas (second nitriding gas) are alternately supplied to wafer B to form a thin layer of SiN. Thereafter, plasma-formed NH3 gas is supplied to modify the thin layer of SiN.

[0048] Then, after such pretreatment, ALD (Atomic Layer Deposition) is performed using Si2Cl6 gas and plasma-formed NH3 gas (first nitriding gas) to form a SiN film on the above-mentioned thin layer of SiN. It should be noted that Si2Cl6 (hexachlorodisilane) is sometimes referred to as HCD hereinafter. As mentioned above, HCD gas is a processing gas used for pretreatment and a raw material gas for forming a SiN film. In addition, in this specification, silicon nitride is referred to as SiN regardless of the stoichiometric ratio. Therefore, the so-called SiN record includes, for example, Si3N4. Furthermore, the above-mentioned base film refers to the case where, in addition to the film formed on wafer B, it also includes wafer B itself. Therefore, for example, the above-mentioned Si film can be a film formed on a silicon wafer or can be the silicon wafer itself.

[0049] Hereinafter, a film forming apparatus 1 as one embodiment of an apparatus for implementing the above-mentioned film forming method will be described with reference to Figure 1 The longitudinal side view and Figure 2 The film forming device 1 is described with reference to a cross-sectional top view. The film forming device 1 has a flat, approximately circular vacuum container (processing container) 11, and the vacuum container 11 is composed of a container body 11A constituting side walls and a bottom, and a top plate 11B. In the figure, 12 is a circular turntable horizontally arranged in the vacuum container 11. In the figure, 12A is a support portion supporting the central portion of the back side of the turntable 12. In the figure, 13 is a rotating mechanism, which is used to rotate the turntable 12 clockwise in a top view along its circumferential direction by means of the support portion 12A. It should be noted that X in the figure represents the rotation axis of the turntable 12.

[0050] Six circular recesses 14 are provided on the upper surface of the turntable 12 along the circumferential direction (rotational direction) of the turntable 12, and wafers B are accommodated in each recess 14. That is, each wafer B is placed on the turntable 12 in such a manner that it revolves as the turntable 12 rotates. Figure 1 Reference numeral 15 denotes a heater, which is provided in plurality in a concentric circle at the bottom of the vacuum container 11 and heats the wafer B placed on the turntable 12 . Figure 2 Reference numeral 16 is a transfer port for wafer B opened in the side wall of the vacuum container 11 and can be opened and closed freely by a gate valve (not shown). The wafer B is transferred between the outside of the vacuum container 11 and the inside of the recess 14 via the transfer port 16 by a substrate transfer mechanism (not shown).

[0051] On the turntable 12, toward the downstream side of the rotation direction of the turntable 12, there are arranged in order along the rotation direction: a nozzle 2, a plasma forming unit 3A, a plasma forming unit 3B and a plasma forming unit 3C. The nozzle 2 as the first gas supply unit supplies the HCD gas used in the film formation and pre-treatment of the above-mentioned SiN film to the wafer B. The plasma forming units 3A to 3C as the second gas supply unit are as follows: the plasma forming gas supplied to the turntable 12 is plasma-formed, and the wafer B is plasma-treated, and is configured in a manner that can form a plasma of H2 gas alone, a plasma of NH3 gas and a plasma of H2 gas respectively. In addition, an exhaust port 51 for exhausting the plasma forming gas supplied by the plasma forming units 3A to 3C is opened below the outer side of the turntable 12 in the vacuum container 11 and outside the second plasma forming unit 3B. The exhaust port 51 is connected to the exhaust mechanism 50.

[0052] The showerhead 2, which is a processing gas supply unit and a raw material gas supply unit, is also shown with reference to the longitudinal side view. Figure 3 and as a bottom view Figure 4 The nozzle 2 is formed into a fan shape that expands from the center side of the turntable 12 to the peripheral side along the circumferential direction of the turntable 12 when viewed from above, and the lower surface of the nozzle 2 is adjacent to the upper surface of the turntable 12. The gas outlet 21, the exhaust port 22 and the purge gas outlet 23 are opened on the lower surface of the nozzle 2. For easy identification, Figure 4 In the figure, the exhaust port 22 and the purge gas exhaust port 23 are indicated by marking multiple points. The gas exhaust ports 21 are arranged in a plurality in a fan-shaped area 24 that is closer to the inner side than the peripheral edge of the lower surface of the shower head 2. Moreover, the gas exhaust ports 21 discharge HCD gas downward in a spraying manner during the rotation of the turntable 12, and open in a manner to supply the HCD gas to the entire surface of the wafer B.

[0053] In the above-mentioned fan-shaped area 24, three areas 24A, 24B, and 24C are provided from the central side of the turntable 12 to the peripheral side of the turntable 12. In a manner that HCD gas can be independently supplied to the gas outlets 21 provided in each area 24A, area 24B, and area 24C, gas flow paths 25A, 25B, and 25C that are distinguished from each other are provided on the nozzle 2. The upstream sides of the gas flow paths 25A, 25B, and 25C are connected to the supply source 26 of HCD gas by means of pipes, and a gas supply device 27 composed of a valve and a mass flow controller is provided on each pipe. The gas supply device 27 is used to supply / cut off the HCD gas to the downstream side of the pipe and adjust the flow rate. It should be noted that each gas supply device other than the gas supply device 27 described later is also constructed in the same manner as the gas supply device 27, and the gas supply / cut off and the flow rate to the downstream side are adjusted.

[0054] The exhaust port 22 and the purge gas exhaust port 23 are respectively opened in an annular shape at the peripheral portion of the lower surface of the showerhead 2 in a manner of surrounding the fan-shaped area 24 and facing the upper surface of the turntable 12, and the purge gas exhaust port 23 is located outside the exhaust port 22 and is formed in a manner of surrounding the exhaust port 22. The inner area of ​​the exhaust port 22 on the turntable 12 forms an adsorption area R0 for adsorption of HCD on the surface of the wafer B. The purge gas exhaust port 23 discharges Ar (argon) gas, for example, as a purge gas onto the turntable 12.

[0055] While the HCD gas is being discharged from the gas discharge port 21, exhaust from the exhaust port 22 and purge gas from the purge gas discharge port 23 are being discharged simultaneously. Figure 3 As shown by the arrows, the raw material gas and the purge gas discharged toward the turntable 12 are exhausted from the exhaust port 22 on the upper surface of the turntable 12 toward the exhaust port 22. By discharging and exhausting the purge gas in this way, the atmosphere of the adsorption region R0 as the first region is separated from the external atmosphere, and the raw material gas can be limitedly supplied to the adsorption region R0. That is, the HCD gas supplied to the adsorption region R0 can be suppressed from mixing with the various gases supplied to the outside of the adsorption region R0 by the plasma forming units 3A to 3C as described later, and the above-mentioned ALD-based film forming process can be performed. Figure 3 Reference numeral 28 denotes an exhaust mechanism for exhausting the gas from the exhaust port 22 via a pipe. Figure 3 Reference numeral 29 denotes a supply source of Ar gas as a purge gas, and the Ar gas is supplied to the purge gas discharge port 23 via a pipe. A gas supply device 20 is provided on the pipe.

[0056] Next, with respect to the plasma forming unit 3B, while referring to Figure 1 , Figure 2The plasma forming unit 3B supplies microwaves to the plasma forming gas (H2 gas or a mixed gas of H2 gas and NH3 gas) discharged below the plasma forming unit 3B, and generates plasma on the rotating table 12. The plasma forming unit 3B includes an antenna 31 for supplying the microwaves, and the antenna 31 includes a dielectric plate 32 and a metal waveguide 33.

[0057] The dielectric plate 32 is formed in a substantially fan-shaped shape that expands from the center side toward the peripheral side when looking down at the turntable 12. A substantially fan-shaped through-hole is opened in the top plate 11B of the vacuum container 11 in a manner corresponding to the shape of the dielectric plate 32, and the inner peripheral surface of the lower end of the through-hole slightly protrudes toward the center side of the through-hole to form a support portion 34. The dielectric plate 32 blocks the fan-shaped through-hole from the upper side, faces the turntable 12, and the peripheral portion of the dielectric plate 32 is supported by the support portion 34.

[0058] The waveguide 33 is provided on the dielectric plate 32 and has an internal space 35 extending on the top plate 11B. In the figure, 36 is a slot plate constituting the lower side of the waveguide 33, which has a plurality of slots 36A and is provided in contact with the dielectric plate 32. The end of the waveguide 33 on the central side of the turntable 12 is blocked, and a microwave generator 37 for supplying microwaves of about 2.35 GHz to the waveguide 33 is connected to the end on the peripheral side of the turntable 12. The microwave reaches the dielectric plate 32 through the slots 36A of the slot plate 36, and the supplied plasma forming gas is supplied to the lower side of the dielectric plate 32, and plasma is limitedly formed below the dielectric plate 32 to process the wafer B. In this way, the lower side of the dielectric plate 32 is constituted as a plasma forming region, which is represented as R2.

[0059] Furthermore, the plasma forming unit 3B has a gas discharge hole 41 and a gas discharge hole 42 located in the above-mentioned support portion 34. The gas discharge hole 41 discharges the plasma forming gas from the central part side to the peripheral part side of the turntable 12, and the gas discharge hole 42 discharges the plasma forming gas from the peripheral part side to the central part side of the turntable 12. The gas discharge hole 41 and the gas discharge hole 42 are respectively connected to the H2 gas supply source 43 and the NH3 gas supply source 44 via a piping system having a gas supply device 45. It should be noted that the plasma forming units 3A and 3C are configured in the same manner as the plasma forming unit 3B, and the regions corresponding to the plasma forming region R2 in the plasma forming units 3A and 3C are respectively represented as plasma forming regions R1 and R3. The plasma forming regions R1 to R3 are the second regions, and the plasma forming units 3A to 3C constitute a reforming gas supply unit, a nitriding gas supply unit, and a plasma forming mechanism.

[0060] like Figure 1As shown, the film forming apparatus 1 is provided with a control unit 10 composed of a computer, and a program is stored in the control unit 10. The program sends control signals to each part of the film forming apparatus 1 to control the operation of each part, and is incorporated into a step group in a manner of performing the above-mentioned pre-processing and film forming processing of the SiN film. Specifically, the rotation speed of the turntable 12 based on the rotating mechanism 13, the operation of each gas supply device, the exhaust volume based on each exhaust mechanism 28, 50, the supply / cutoff of microwaves from the microwave generator 37 to the antenna 31, and the power supply to the heater 15 are controlled by the program. The control of the power supply to the heater 15 is the control of the temperature of the wafer B, and the control of the exhaust volume based on the exhaust mechanism 50 is the control of the pressure in the vacuum container 11. The program is stored in a storage medium such as a hard disk, an optical disk, a DVD, a memory card, etc., and is installed in the control unit 10.

[0061] The following will describe the pre-processing and SiN film forming process performed by the film forming apparatus 1, with reference to FIG. Figures 5 to 8 , and a flowchart of the operation of the film forming apparatus 1 Fig. 9 While explaining. Figure 5 An example of a wafer B conveyed to the film forming apparatus 1 is shown, on which a stacked body is formed in which the Si film 61, the SiO2 film 62, the W film 63, and the SiO2 film 64 are stacked in this order upward. A recess 65 is formed in the stacked body, and the side surface of the recess 65 is composed of the SiO2 film 62, the W film 63, and the SiO2 film 64, and the bottom surface of the recess 65 is composed of the Si film 61. Therefore, as described above, the Si film, the SiO2 film, and the W film are exposed on the surface of the wafer B, respectively.

[0062] Six sheets of the same are placed on the concave portion 14 of the rotating table 12. Figure 5 The wafer B shown is then closed at the transfer port 16 of the vacuum container 11, the vacuum container 11 is airtight, and the wafer B is heated to, for example, 200°C to 600°C, more specifically, 550°C, by the heater 15. Then, by exhausting from the exhaust port 51, a vacuum atmosphere of, for example, 53.3 Pa to 666.5 Pa is formed in the vacuum container 11, and the turntable 12 is rotated at, for example, 3 rpm to 60 rpm, and each wafer B revolves.

[0063] The plasma forming units 3A to 3C supply NH3 gas to the plasma forming regions R1 to R3. However, microwaves are not supplied, and the NH3 gas is not converted into plasma. On the other hand, in the shower head 2, HCD gas is discharged from the gas outlet 21, Ar gas is discharged from the purge gas outlet 23, and exhaust is performed from the exhaust port 22. Fig. 9In this way, the shower head 2 and the plasma forming units 3A to 3C operate, so that the supply of HCD gas and the supply of NH 3 gas are alternately and repeatedly performed on each of the revolving wafers B.

[0064] Si in the raw material gas is easily adsorbed to the SiO2 films 62, 64, the Si constituting the Si film 61, and the W constituting the W film 63. That is, there are oxygen atoms on the surfaces of the SiO2 films 62, 64, and the W film 63, but the HCD gas as the raw material gas contains two Si atoms, and thus has a high adsorption property to these SiO2 films 62, 64, the Si film 61, and the W film 63. Therefore, in the adsorption area R0, the HCD gas can be efficiently adsorbed to these films. Then, NH3 gas is supplied to the adsorbed HCD gas in the plasma forming areas R1 to R3, and they react with each other through heat to form a thin layer 66 of SiN. As the wafer B continues to revolve, the thickness of the thin layer 66 of SiN increases ( Figure 6 ).

[0065] Since the supply of HCD gas from the nozzle 2 and the supply of NH3 gas based on the plasma forming units 3A to 3C are started, when the turntable 12 is rotated a preset number of times, for example, 30 times, the supply of HCD gas from the nozzle 2 is stopped. In this way, the supply of HCD gas is stopped, and on the other hand, H2 gas and NH3 gas are supplied to the plasma forming regions R1 to R3, and microwaves are supplied to form plasma of these gases (step S2). Then, the revolution of wafer B is continued, and each wafer B repeatedly passes through the plasma forming regions R1 to R3. As a result, the active substances (NH2 radicals, NH radicals, etc.) of the NH3 gas constituting the plasma act on the thin layer 66 of SiN, impurities such as chlorine constituting the HCD gas are released, and the thin layer 66 is modified to be solidified. Through this modification, the characteristics of the thin layer 66 become close to the characteristics of the SiN film 67 formed later.

[0066] After the formation of the plasma of H2 gas and NH3 gas begins, when the rotating table 12 is rotated a preset number of times, the supply of HCD gas from the shower head 2 to the adsorption region R0 is restarted. In addition, in the plasma formation regions R1 and R2, the supply of NH3 gas is stopped, while H2 gas is continuously supplied to form the plasma of the H2 gas. In the plasma formation region R3, H2 gas and NH3 gas are continuously supplied to form the plasma of these gases (step S3).

[0067] Then, wafer B continues to revolve, and the supply of HCD gas in adsorption region R0, the supply of plasma-formed H2 gas in plasma forming regions R1 and R2, and the supply of plasma-formed H2 gas and NH3 gas in plasma forming region R3 are repeated in sequence. Si in the HCD gas adsorbed on wafer B in adsorption region R0 is nitrided in plasma forming region R3 to become SiN. Then, in plasma forming regions R1 and R2, the deposited SiN is modified by plasma of H2 gas. Specifically, H bonding of dangling bonds in SiN and removal of Cl from deposited SiN are performed, thereby forming dense SiN with low impurity content.

[0068] As described above, the formation and growth of SiN nuclei are caused, and the substrate is a thin layer of SiN 66 that is the same as the nuclei. Therefore, the formation and growth of the nuclei proceed relatively quickly. Then, on each of the Si film 61, the SiO2 films 62, 64, and the W film 63, such a thin layer of SiN 66 that is the same as that of the nuclei is formed. It can be said that the surface states of these films are consistent. Therefore, the formation and growth of nuclei are similarly caused on each of these films, and a thin layer of SiN (SiN film 67) is formed. That is, on each of the Si film 61, the SiO2 films 62, 64, and the W film 63, the SiN film 67 is formed as if the incubation time is unified. Figure 7 ).

[0069] As the wafer B continues to revolve, the film thickness of the SiN film 67 increases, and the modification of the SiN film 67 proceeds. As described above, the film formation of the SiN film 67 is started at the same time on each of the Si film 61, the SiO2 films 62, 64, and the W film 63, so that the SiN film 67 grows with a highly uniform film thickness between these films. After the supply of the HCD gas in step S3 and the plasmaization of each gas in the plasma forming regions R1 to R3 are started, the rotating table 12 is rotated a preset number of times. When the SiN film 67 having the desired film thickness is formed, the film formation process of the SiN film 67 is completed ( Figure 8 That is, the supply of each gas, the supply of microwaves, and the rotation of the turntable 12 are stopped, and the film forming process is completed. Then, the wafer B is carried out of the vacuum container 11 by the substrate conveying mechanism.

[0070] According to the process using the film forming apparatus 1 in this way, the influence of the difference in the incubation time of the SiN film 67 between the Si film 61, the SiO2 films 62, 64 and the W film 63 is suppressed, and the timing of starting film formation can be made consistent. As a result, the SiN film 67 can be formed in a manner that the film thickness is highly uniform on each film. In addition, when forming the thin layer 66 of SiN for suppressing the influence of the incubation time, the HCD adsorbed on the wafer B is nitrided by the NH3 gas that has not been plasma-formed, and then modified by the NH3 gas that has been plasma-formed. That is, plasma is not used in the formation of the thin layer 66, so the time for the wafer B to be exposed to the NH3 gas that has been plasma-formed can be suppressed, or when the NH3 plasma is formed, the thin layer 66 is sandwiched between the plasma and each film 61 to 64. Therefore, the nitridation of each film 61 to 64 is suppressed. In particular, as shown in the evaluation test described later, the Si film 61 has the property of being easily nitrided, but the nitridation of the Si film 61 can be suppressed. In addition, as described above, the time during which the wafer B is exposed to the plasma-formed gas can be reduced, and therefore there is an advantage that damage to the films 61 to 64 caused by the plasma can be reduced.

[0071] In the above step S1, nitridation is not limited to using NH3 gas, and for example, N2 gas may be used. In addition, as the processing gas containing silicon used in the step S1, in order to ensure high adsorption to each film as described above, a halogenated silicon gas having a plurality of Si atoms in one molecule due to Si-Si bonds may be used. As such a halogenated silicon gas, in addition to HCD gas, for example, octachlorotrisilane (Si3Cl8) gas may be used.

[0072] In addition, the exposure to plasma in the above step S2 can be used as long as the SiN thin layer 66 can be modified as described above, so it is not limited to the plasma using NH3 gas. However, it is preferred to treat the thin layer 66 using NH3 gas plasma so that the film quality of the thin layer 66 can be formed to be equivalent to the SiN film 67 to be formed later.

[0073] Furthermore, the formation of the modified SiN film 67 of the SiN thin layer 66 is not limited to ALD, but may be performed by CVD (Chemical Vapor Deposition). In the formation of the SiN film 67, as long as the silicon in the raw material gas can be nitrided, it is not limited to the use of plasma-formed NH3 gas, and for example, non-plasma-formed NH3 gas may be used. In addition, as the raw material gas for forming the SiN film 67, a gas without Si-Si bonds, such as DCS (dichlorosilane) gas, may be used.

[0074] In the above processing example, a SiN film is formed on a W film 63 as a metal film, but it is not limited to the W film 63. For example, when a SiN film 68 is formed on a metal film such as Ti (titanium) or Ni (nickel), this method is also effective. That is, the metal film that serves as the base of the SiN film is not limited to the W film. It should be noted that the embodiments disclosed this time are examples in all aspects and should be considered as non-limiting. The above embodiments can be omitted, replaced, and changed in various forms without departing from the attached claims and their main purpose.

[0075] Hereinafter, evaluation tests conducted on the present technology will be described.

[0076] As an evaluation test 1, a plurality of wafers made of Si and with exposed surfaces (bare wafers) and wafers made of Si and with SiO2 films formed on the surfaces (referred to as SiO2 wafers) are prepared. Then, a series of treatments (pretreatment and film forming treatment of SiN film 67) including steps S1 to S3 described in the above embodiment are respectively performed on the bare wafer and the SiO2 wafer. The time for the film forming treatment of SiN film 67 in step S3 of the series of treatments is set to 180 seconds or 360 seconds. After the series of treatments are completed, the film thickness of the formed SiN film 67 is measured.

[0077] Furthermore, as a comparative test 1, N2 gas was supplied to the plasma forming regions R1 to R3 instead of performing the process of step S1, and the N2 gas was turned into plasma to perform a process of nitriding the surfaces of the bare wafer and the SiO2 wafer. After the nitridation, the processes of step S2 and step S3 were performed on each wafer, and DCS gas was used instead of HCD gas as the raw material gas of step S3. Except for such a difference, the process of comparative test 1 was the same as that of evaluation test 1.

[0078] Respectively, Fig.10 The figure shows the results of evaluation test 1, Fig.11 The graphs of FIG. 1 show the results of the comparative test 1. In each graph, the horizontal axis represents the film forming time (unit: seconds) of the SiN film 67 in step S3, and the vertical axis represents the film thickness of the SiN film 67. In each figure, the measured film thickness of the SiN film 67 is plotted and shown, and a straight line connecting each point plotted for the bare wafer and a straight line connecting each point plotted for the SiO2 wafer are shown. In the further figure, the straight lines of the above-mentioned solid lines are extended to the position where the film forming time on the horizontal axis becomes 0 seconds or the film thickness of the SiN film 67 on the vertical axis becomes It should be noted that the film incubation time is defined as the time required for the SiN film to start film formation when the SiN film is formed in direct contact with the film. Regardless of its definition, in this evaluation test, the extension line of the above dotted line is observed and the film thickness is The film formation time was taken as the incubation time.

[0079] Regarding the evaluation test 1, when the film forming time of the SiN film 67 was 180 seconds or 360 seconds, the difference in the film thickness of the SiN film 67 between the SiO2 wafer and the bare wafer was small. The straight line obtained for the SiO2 wafer and the straight line obtained for the bare wafer were substantially parallel to each other. Furthermore, when the extension lines based on the dotted lines were observed, the film thickness of the SiN film 67 of the SiO2 wafer was When the incubation time is approximately 0 seconds, the thickness of the SiN film 67 of the bare wafer is

[0080] On the other hand, in Comparative Test 1, when the film forming time of SiN film 67 was 180 seconds and 360 seconds, a large difference was observed in the film thickness of SiN film 67 between the SiO2 wafer and the bare wafer. The solid line obtained for the SiO2 wafer and the solid line obtained for the bare wafer were approximately parallel to each other, but the interval between them was large. Moreover, when observing the extension line based on each dotted line, the incubation time for the SiO2 wafer was approximately 0 seconds, but for the bare wafer, when the film forming time was 0 seconds, the film thickness of SiN film 67 was 0.01%.

[0081] In the evaluation test 1 and the comparative test 1, the SiN film 67 was formed on the bare wafer when the film forming time was 0 seconds because nitridation had been performed in the process before the step S3 was performed. Moreover, according to the evaluation test 1, it can be seen that the nitridation was suppressed compared with the comparative test 1. Therefore, the effect of the above-mentioned embodiment can be confirmed from the results of the evaluation test.

Claims

1. A film forming method, comprising: forming a silicon nitride film on a substrate having a first film and a second film on the surface of which the incubation times required until the silicon nitride film starts to grow are different from each other, while supplying a raw material gas containing silicon and a first nitriding gas for nitriding the silicon, wherein the second film includes a metal film, The film forming method comprises the following steps: The step of supplying a processing gas composed of silicon halide having Si-Si bonds to the substrate; a step of supplying a second nitriding gas that has not been converted into plasma to the substrate; a step of repeatedly supplying the processing gas and the second nitriding gas to form a thin layer of silicon nitride covering the first film and the second film; A process of supplying a plasma-formed modifying gas to the thin layer of silicon nitride to release impurities in the processing gas in the thin layer of silicon nitride and solidify the thin layer of silicon nitride; and, The step of supplying the source gas and the first nitriding gas to the substrate to form the silicon nitride film on the modified silicon nitride thin layer.

2. The film forming method according to claim 1, in, The silicon halide constituting the process gas is disilicon hexachloride.

3. The film forming method according to claim 1 or 2, in, The plasma modified gas is plasma ammonia gas.

4. The film forming method according to claim 1 or 2, in, The first film is a silicon film.

5. The film forming method according to claim 4, in, The metal film included in the second film is a tungsten film.

6. A film forming apparatus for forming a silicon nitride film on a substrate having a first film and a second film on the surface of which the incubation times required until the silicon nitride film starts to grow are different from each other when a raw material gas containing silicon and a first nitriding gas for nitriding the silicon are supplied, wherein the second film includes a metal film, The film forming device comprises: a rotating table on which the substrate is placed and caused to revolve; a processing gas supply unit that supplies a processing gas composed of silicon halide having Si-Si bonds to the rotating table; a nitriding gas supply unit configured to supply the first nitriding gas and the second nitriding gas to the turntable; a raw material gas supply unit for supplying the raw material gas to the rotating table; a reforming gas supply unit that supplies reforming gas to the rotating table; a plasma forming mechanism for converting the reforming gas supplied to the rotating table into plasma; A control unit is configured to perform the following steps: a step of alternately and repeatedly supplying the processing gas and the second nitriding gas that has not been plasma-formed to the revolving substrate in order to form a thin layer of silicon nitride covering the first film and the second film, a step of supplying the modifying gas to the revolving substrate and plasma-forming the modifying gas to release impurities in the processing gas in the thin layer of silicon nitride and solidify the thin layer of silicon nitride, and a step of alternately and repeatedly supplying the raw material gas and the first nitriding gas to the revolving substrate in order to form the silicon nitride film on the modified thin layer of silicon nitride.

7. The film forming device according to claim 6, in, The following gas supply parts are provided: a first gas supply unit that supplies gas to a first area on the turntable; and a second gas supply unit for supplying gas to a second region on the turntable that is offset from the first region on the turntable and has a separated atmosphere and converting the gas into plasma; The raw gas supply unit and the processing gas supply unit are the first gas supply unit, The nitriding gas supply unit and the modifying gas supply unit are the second gas supply unit, The plasma generating mechanism is configured to convert the gas in the second region into plasma.