Photosensitive drum, image forming device, and photosensitive drum regeneration method
By stacking the photosensitive layer and the protective layer on the photosensitive drum and grinding with abrasive film that condenses abrasive particles to control the surface roughness and corrugation, the problem of difficulty in recovering characteristics after grinding the photosensitive drum is solved, and good cleaning and image are achieved Form an effect.
Patent Information
- Application Number
- CN202010907883.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-02
- Filing Date
- 2020-09-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-09-02
AI Technical Summary
The prior art is difficult to restore its original characteristics after grinding the photosensitive drum, resulting in surface damage and poor cleaning, affecting the quality of image formation.
The photosensitive layer and the protective layer are laminated on the outer periphery of the hollow cylindrical sleeve. By grinding with an abrasive film of condensed abrasive particles, the arithmetic average roughness Ra of the control protective layer is less than 0.03 μm and the arithmetic average wrigor degree Wa is more than 0.05 μm. Ensure the cleaning characteristics of the cleaning blade and the quality of image formation.
It effectively reduces the impact of surface damage, inhibits poor cleaning and stripe-like contamination, extends the service life of the photosensitive drum, and maintains good image formation quality.
Smart Images

Figure CN112445089B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a photosensitive drum, an image forming device and a photosensitive drum regeneration method. Background Art
[0002] Generally, in an image forming device, an electrostatic latent image is formed on a photosensitive drum by an optical writing device, and the electrostatic latent image is developed into a toner image by a developing device, and the toner image is transferred to a transfer belt. Then, the toner remaining on the surface of the photosensitive drum is removed by a cleaning device. In this way, the surface of the photosensitive drum may be damaged by repeated formation of the toner image and removal of the toner.
[0003] Therefore, a photoreceptor recycling device that grinds and recycles the surface of a photoreceptor has been proposed (for example, see Patent Document 1). In the photoreceptor recycling device described in Patent Document 1, the surface roughness Rmax of the photoreceptor after grinding is reduced to 4.5 μm or less, thereby removing the attached matter on the surface of the photoreceptor.
[0004] However, simply polishing the photoreceptor to reduce its surface roughness may not provide the same properties as an unused photoreceptor, and further improvement of the properties of the polished photoreceptor is desired.
[0005] An object of the present invention is to provide a photosensitive drum capable of obtaining good characteristics even after polishing, an image forming apparatus including the photosensitive drum, and a photosensitive drum regenerating method.
[0006] [Patent Document 1] (Japan) Patent Publication No. 2002-351098 Summary of the invention
[0007] Technical Solution 1 involves a photosensitive drum in which a photosensitive layer and a protective layer are sequentially stacked on the outer peripheral surface of a hollow cylindrical sleeve in order to solve the above-mentioned problem, and is characterized in that: in the surface of the protective layer, the arithmetic mean roughness Ra defined by JIS B0601:2001 is less than 0.03 μm when the cutoff value is 0.25 mm, and the arithmetic mean waviness Wa defined by JIS B0601:2001 is greater than 0.05 μm when the cutoff value is 2.5 mm.
[0008] According to the photosensitive drum of the present invention, the arithmetic mean roughness Ra is less than 0.03 μm, so even if damage is formed on the surface by using the photosensitive drum, the influence of the damage can be reduced by grinding. Therefore, when the surface of the photosensitive drum is cleaned by a cleaning scraper, poor cleaning caused by surface damage can be suppressed, and streak-shaped pollution caused by surface damage during image formation can be suppressed. In addition, by making the arithmetic mean waviness Wa above 0.05 μm, while ensuring the cleaning characteristics of the cleaning scraper, the one-sided contact of the cleaning scraper can also be suppressed. In this way, by reducing the surface roughness at a relatively microscopic level and leaving the undulating shape of the surface at a larger level, even a photosensitive drum after grinding can obtain good characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 FIG. 1 is a cross-sectional view of a photosensitive drum according to an embodiment of the present invention.
[0010] Figure 2 Shown is a cross-sectional view of the surface state of the unused photosensitive drum.
[0011] Figure 3 Shown is a cross-sectional view of the surface state of the photosensitive drum after use.
[0012] 4(a) and 4(b) are perspective views showing a grinding device for grinding the photosensitive drum.
[0013] Figure 5 Shown is a cross-sectional view of the surface state of the photosensitive drum being ground by a grinding mechanism having free abrasive grains.
[0014] Figure 6 Shown is a cross-sectional view of the surface state of the photosensitive drum being ground by a grinding mechanism having fixed abrasive grains.
[0015] Figure 7 FIG. 1 is a graph showing the relationship between primary particles and average polishing speed when the surface of a photosensitive drum is polished by a polishing mechanism having agglomerated abrasive particles.
[0016] Figure 8 Shown is a graph of the arithmetic mean waviness Wa of the photosensitive drum before and after grinding.
[0017] Fig. 9 Shown is a graph of the electrostatic capacitance of the photosensitive drum before and after grinding. DETAILED DESCRIPTION
[0018] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. Figure 1As shown, the photosensitive drum 1 of this embodiment includes a hollow cylindrical sleeve member 2, a photosensitive layer 3 laminated on the outer peripheral surface of the sleeve member 2, and a protective layer 4 laminated on the outer peripheral surface of the photosensitive layer 3. That is, the photosensitive layer 3 and the protective layer 4 are laminated on the outer peripheral surface of the sleeve member 2 in sequence. The photosensitive drum 1 is used in an image forming device such as a copier or a fax machine, a laser printer, or a multi-function peripheral device thereof, and an electrostatic latent image is formed on the surface by an optical writing device, and the electrostatic latent image is developed into a toner image by a developing device, and the toner image is transferred to a transfer belt.
[0019] The photosensitive layer 3 is composed of, for example, an undercoat layer, a charge generating layer, and a charge transporting layer. The protective layer 4 is composed of, for example, a binder resin such as polycarbonate constituting the charge transporting layer in which a filler such as a resin is dispersed. The structure and material of the photosensitive layer 3 and the protective layer 4 can be appropriately selected.
[0020] Figure 2 FIG. 2 schematically shows the surface shape of the protective layer 4 in the photosensitive drum 1 in an unused state (new product). Figure 2 FIG. 1 schematically shows the surface shape of the protective layer 4 of the photosensitive drum 1 after being used a predetermined number of times.
[0021] like Figure 2 , 3 As shown in the enlarged view in FIG. 1 (see the dotted line), when the photosensitive drum 1 is used, rough surface degradation occurs due to wear or film formation. In addition, when the photosensitive drum 1 is used, damage 41 to 43 is formed due to one-sided contact of the cleaning blade or the developer material. In addition, before or after the use of the photosensitive drum 1, the surface of the protective layer 4 also has an undulating shape.
[0022] As described above, the photosensitive drum 1 deteriorated by use is subjected to grinding as described below, so that the photosensitive drum 1 can be recycled.
[0023] 4 shows a grinding device (grinding mechanism) 100 for grinding the photosensitive drum 1. The grinding device 100 has a cylindrical elastic member 101 and a grinding film 102 attached to the top surface of the elastic member 101, and is configured to rotate by a power source with the height direction of the cylindrical elastic member 101 as the axial direction.
[0024] The elastic member 101 is made of, for example, foamed polyurethane, foamed EVA sponge, suede, nonwoven fabric, or the like.
[0025] The polishing film 102 has agglomerated abrasive grains as polishing abrasive grains and functions as a polishing mechanism. The agglomerated abrasive grains are agglomerates composed of many fine primary particles, and many primary particles gradually combine with each other while partially forming voids to form a granular porous body.
[0026] In order to obtain such agglomerated abrasive grains, a spray dryer is first used to granulate the grains to obtain grains (secondary grains) with a grain size of about 1 to 300 μm. Then, the grains are heat-treated to form a porous structure. The compression failure strength of the agglomerated abrasive grains after the heat treatment is preferably 20 MPa or less. If the compression failure strength is too high, scratches are easily generated during grinding.
[0027] The average particle size of the primary particles of the aggregated abrasive is preferably 4 μm or less. In addition, the primary particles are preferably inorganic oxides such as alumina, zirconia, silica, cerium oxide, silicon dioxide, and iron oxide.
[0028] Next, the abrasive obtained as described above is mixed with a liquid polyurethane resin, and methyl ethyl ketone is added as a solvent. After adjusting the viscosity of the solution, a stirrer is used to mix and stir for about 10 minutes to prepare a mixture. The stirring is carried out at room temperature, and the rotation speed is 100 rpm, which is not enough to damage the abrasive. The mixture is applied to a base material (for example, a PET film with a thickness of about 75 μm) using a wire rod coater, and then dried in a thermostatic bath maintained at 60°C for 1 hour to obtain a polishing film.
[0029] The photosensitive drum 1 is rotated by a power source, and the grinding device 100 is rotated by the power source and moved back and forth in the vertical direction in the figure, thereby performing the grinding process. At this time, the grinding film 102 rotates together with the elastic member 101 in a state of biting into the surface of the photosensitive drum 1 by a certain amount, and the surface of the photosensitive drum 1 is ground.
[0030] The photosensitive drum 1 whose surface of the protective layer 4 has deteriorated due to use for a predetermined number of times is subjected to grinding treatment by the grinding device 100 as described above to obtain a regenerated photosensitive drum. On the surface of the protective layer 4 of the regenerated photosensitive drum, the arithmetic mean roughness Ra defined in JIS B0601:2001 is less than 0.03 μm at a cutoff value of 0.25 mm, the arithmetic mean waviness Wa defined in JIS B0601:2001 is greater than 0.05 μm at a cutoff value of 2.5 mm, and the maximum height roughness Rz defined in JIS B0601:2001 is less than 0.5 μm at a cutoff value of 0.25 mm. In addition, in the regenerated photosensitive drum, the average thickness of the protective layer 4 is greater than 0.2 μm.
[0031] According to this embodiment, the following effects are achieved. That is, since the arithmetic mean roughness Ra of the surface of the protective layer 4 is less than 0.03 μm, even if scratches 41 to 43 are formed on the surface of the photosensitive drum 1 by using the photosensitive drum 1, the influence of the scratches 41 to 43 can be reduced by grinding. When the photosensitive drum surface is cleaned by the cleaning blade, poor cleaning due to the scratches on the surface can be suppressed, and streak-like contamination and the like due to the scratches on the surface can be suppressed during image formation.
[0032] In addition, by making the arithmetic mean waviness Wa of the surface of the protective layer 4 not less than 0.05 μm, the cleaning properties of the cleaning blade can be ensured while the one-sided contact of the cleaning blade can be suppressed. Thus, by reducing the surface roughness at a relatively microscopic level and leaving the undulating shape of the surface at a relatively large level, even the photosensitive drum after grinding can obtain good properties.
[0033] Furthermore, by setting the maximum height roughness Rz of the surface of the protective layer 4 to 0.5 μm or less, it is possible to prevent new damage due to polishing from being generated.
[0034] Furthermore, by setting the average thickness of the protective layer 4 to 0.2 μm or more, it is possible to suppress changes in the electrostatic characteristics of the photosensitive layer 3 and extend the life of the photosensitive drum 1 after regeneration.
[0035] By polishing the surface of the protective layer 4 using the polishing film 102 having aggregated abrasive grains, the arithmetic mean roughness Ra of the polished surface of the protective layer 4 can be less than 0.03 μm and the arithmetic mean waviness Wa can be greater than 0.05 μm.
[0036] In contrast, when a grinding mechanism with free abrasive particles (e.g., a soft grinding pad such as a non-woven fabric or a sponge) is used for grinding, Figure 5 As shown (the solid line represents the surface S0 before grinding, and the dotted line represents the surface S1 after grinding), the undulating shape can be maintained and the reduction of the arithmetic mean waviness Wa can be suppressed. However, as the grinding progresses, damage 41 to 43 also progresses, and sometimes the deep damage among damage 41 to 43 cannot be removed.
[0037] In addition, when grinding using a grinding mechanism with fixed abrasive particles (such as grinding paper), Figure 6 As shown, although the flaws 41 to 43 are easily removed, the undulating shape cannot be maintained, resulting in a decrease in the arithmetic mean waviness Wa.
[0038] That is, by performing polishing using the polishing film 102 having aggregated abrasive grains as in the present embodiment, it is possible to maintain the undulating shape while removing the flaws 41 to 43 .
[0039] In addition, by using particles having an average primary particle size of 4 μm or less as agglomerated abrasive grains, it is possible to suppress the occurrence of grinding damage such as scratches on the processed surface, i.e., the surface of the protective layer 4. On the other hand, when the average primary particle size is too large, although the grinding efficiency is improved, grinding damage such as scratches is likely to occur on the processed surface, which may reduce the quality.
[0040] In addition, by using a coagulated abrasive grains with a compression failure strength of 20 MPa or less, the abrasive grains are gradually worn during grinding, and new cutting edges are easily generated, thereby improving the processing efficiency and quality when grinding the surface of the protective layer 4, and further, it is easy to maintain this state for a long time. On the other hand, if the compression failure strength of the coagulated abrasive grains is too high, new grinding damage may be imparted to the surface of the protective layer 4 during grinding, which may lead to a decrease in surface quality.
[0041] Furthermore, by using primary particles composed of an inorganic oxide as aggregated abrasive grains, contamination and damage on the surface of the protective layer 4 can be easily removed.
[0042] In addition, the present invention is not limited to the above-described embodiment, and includes other configurations that can achieve the object of the present invention. Modifications such as those described below are also included in the present invention.
[0043] For example, in the above-mentioned embodiment, the maximum height roughness Rz in the surface of the protective layer 4 is set to be less than 0.5 μm at the cutoff value of 0.25 mm, but if the arithmetic mean roughness Ra is less than 0.03 μm at the cutoff value of 0.25 mm, the maximum height roughness Rz may be greater than 0.5 μm.
[0044] In the above embodiment, the average thickness of the protective layer is set to 0.2 μm or more. However, for example, when it is desired to improve the initial image quality, the average thickness of the protective layer may be set to less than 0.2 μm.
[0045] In addition, in the above-mentioned embodiment, as the agglomerated abrasive, particles with an average primary particle size of less than 4 μm, a compression failure strength of less than 20 MPa, and primary particles composed of inorganic oxides are used, but the grinding mechanism only needs to have agglomerated abrasives that can remove scratches on the surface of the protective layer 4 and maintain the corrugated shape, and the average primary particle size, compression failure strength, and material of the primary particles can be appropriately selected.
[0046] In addition, although the best configuration and method for implementing the present invention are as described above, the present invention is not limited thereto. That is, the present invention mainly illustrates and describes a specific embodiment, and those skilled in the art may apply various modifications to the above-described embodiment without departing from the technical concept and scope of the present invention.
[0047] Therefore, the description of the limitation of the shapes, materials, etc. disclosed above is only for illustrative purposes to facilitate understanding of the present invention, and is not intended to limit the present invention. The description of the names of the components after removing some or all of the limitations of the shapes, materials, etc. is also included in the present invention.
[0048] [Example]
[0049] [Surface conditions before and after grinding]
[0050] The abrasive film having an average primary particle size of 3 μm and a compression failure strength of 7.7 MPa was used to polish an unused photosensitive drum and a used photosensitive drum, and the arithmetic mean roughness Ra and the maximum height roughness Rz before and after polishing were measured. The Form Talysurf S4C manufactured by the old Taylor Hobson Company was used in the measurement. In addition, the measurement was performed at 4 locations (90° apart) in the circumferential direction of the surface of the photosensitive drum. The results are shown in Table 1.
[0051] Table 1
[0052]
[0053] The arithmetic mean roughness Ra and the maximum height roughness Rz both increase as the photosensitive drum is used. In addition, the arithmetic mean roughness Ra decreases as the photosensitive drum is polished in both the unused photosensitive drum and the used photosensitive drum. The maximum height roughness Rz of the unused photosensitive drum increases slightly as the photosensitive drum is polished. The maximum height roughness Rz decreases as the photosensitive drum is polished after use, but it is larger than the value before the polishing of the unused photosensitive drum.
[0054] [Types of grinding mechanisms and grinding results]
[0055] Using the polishing mechanisms of Examples 1 to 5 and Comparative Examples 1 to 3 shown in Table 2, the surfaces of the used photosensitive drums were polished.
[0056] Table 2
[0057]
[0058]
[0059] The ultra-precision polishing film of Comparative Example 1 is a 1200# film of the LAPIKA series manufactured by KOVAX. The ultra-precision polishing film of Comparative Example 2 is a 10000# film of the LAPIKA series manufactured by KOVAX, and the particle size is finer than that of Comparative Example 1. The polishing pad of Comparative Example 3 is a suede type SURFIN018-3 manufactured by FUJIMI INCORPORATED, and the alumina slurry is obtained by mixing abrasive grains with an average particle size of 0.5 μm manufactured by FUJIMI INCORPORATED with water at a weight ratio of 5 wt%. In Comparative Example 3, the alumina slurry is supplied to the polishing pad at a supply rate of 20 cc / min during polishing.
[0060] Table 3 shows the results of grinding using the grinding mechanisms of Examples 1 to 5 and Comparative Examples 1 to 3.
[0061] Table 3
[0062]
[0063] In each of Examples 1 to 6, the occurrence of new damage due to grinding can be suppressed. In particular, in Examples 1 to 4, the occurrence of new damage due to grinding can be suppressed. In Comparative Example 1, new damage was generated due to grinding. In addition, the occurrence of new damage was evaluated by visual observation.
[0064] In each of Examples 1 to 6, the generated damage could be removed by using the photosensitive drum. In Comparative Examples 2 and 3, the generated damage could not be removed by using the photosensitive drum.
[0065] That is, in any of Examples 1 to 6, both the suppression of the generation of new damage due to grinding and the removal of damage caused by use of the photosensitive drum can be achieved, but in Comparative Examples 1 to 3, both cannot be achieved. In addition, in any of Examples 1 to 6, the arithmetic mean roughness Ra is less than 0.03 μm at the cutoff value of 0.25 mm, and the arithmetic mean waviness Wa is greater than 0.05 μm at the cutoff value of 2.5 mm.
[0066] Table 4 shows the maximum height roughness Rz when the unused photosensitive drums were polished using the polishing mechanisms of Examples 1 to 6.
[0067] Table 4
[0068] Rz(μm) Example 1 0.25~0.35 Example 2 0.33~0.48 Example 3 0.25~0.35 Example 4 0.33~0.48 Example 5 0.6~0.11 Example 6 0.8~1.5
[0069] It can be seen that the larger the average particle size of the primary particles, the larger the maximum height roughness Rz, and the larger the compression failure strength, the larger the maximum height roughness Rz.
[0070] [Average particle size and grinding efficiency]
[0071] The average grinding speed (grinding efficiency) when grinding with different grinding mechanisms for primary particles with different average particle sizes was evaluated while keeping the compression failure strength approximately constant (8 MPa). Figure 7 The larger the average particle size of the primary particles, the higher the grinding efficiency. When the average particle size is 3 μm or more, good grinding efficiency is obtained.
[0072] [Change in arithmetic mean waviness due to grinding]
[0073] The used photosensitive drum was ground using the grinding mechanism of Example 3, and the arithmetic mean waviness Wa before and after grinding (before and after regeneration) was measured. Figure 8 In each sample, the arithmetic mean waviness Wa was reduced by grinding and reached 0.05 μm or more even after grinding.
[0074] [Thickness of protective layer after grinding]
[0075] The photosensitive drum after use was polished by the polishing mechanism of Example 3, and the average thickness of the protective layer became 0.2 μm. When the photosensitive drum after such polishing was assembled into an image forming apparatus and subjected to a life test, good results were obtained.
[0076] [Changes in electrostatic capacitance due to grinding]
[0077] The used photosensitive drum was ground using the grinding mechanism of Example 3, and the electrostatic capacitance of the surface of the photosensitive drum 1 was measured before and after grinding. Fig. 9 As shown in the figure, the electrostatic capacitance decreased by polishing, but no change that would affect the quality was observed.
Claims
1. A photosensitive drum having a photosensitive layer and a protective layer sequentially laminated on the outer peripheral surface of a hollow cylindrical sleeve, characterized in that: The surface of the protective layer has an arithmetic mean roughness Ra of less than 0.03 μm when the cutoff value is 0.25 mm, and an arithmetic mean waviness Wa of not less than 0.05 μm when the cutoff value is 2.5 mm. The photosensitive drum is produced by grinding a used photosensitive drum. wherein in the polishing process, a polishing mechanism having agglomerated abrasive grains is used as polishing abrasive grains to polish the surface of the protective layer, The agglomerated abrasive grains are agglomerates composed of a plurality of primary particles, and the plurality of primary particles are partially and gradually bonded to each other while forming voids to form a granular porous body.
2. The photosensitive drum according to claim 1, characterized in that: On the surface of the protective layer, the maximum height roughness Rz is 0.5 μm or less when the cutoff value is 0.25 mm.
3. The photosensitive drum according to claim 1 or 2, characterized in that: The average thickness of the protective layer is greater than 0.2 μm.
4. An image forming device, characterized in that: A photosensitive drum according to any one of claims 1 to 3.
5. A photosensitive drum regeneration method for producing the photosensitive drum according to any one of claims 1 to 3 by grinding a used photosensitive drum, characterized in that: In the polishing process, the surface of the protective layer is polished using a polishing mechanism having agglomerated abrasive grains as polishing abrasive grains. The agglomerated abrasive grains are agglomerates composed of a plurality of primary particles, and the plurality of primary particles are partially and gradually bonded to each other while forming voids to form a granular porous body.
6. The photosensitive drum regeneration method according to claim 5, characterized in that: As the agglomerated abrasive, the agglomerated abrasive used has an average primary particle size of 4 μm or less and a compressive fracture strength of 20 MPa or less.
7. The photosensitive drum regeneration method according to claim 5 or 6, characterized in that: As the agglomerated abrasive, a primary particle of the agglomerated abrasive is formed of an inorganic oxide.