Polyamides with side chain pigments and related methods
By functionalizing pigment particles with metal oxide particles and reacting them with polyamide, PP-polyamide with side chain epoxy or carboxylic acid groups is generated, solving the problem of uneven pigment dispersion in 3D printing and realizing polyamide materials with uniform coloring, which are suitable for demanding applications such as power tools, automotive parts and gears.
Patent Information
- Application Number
- CN202010907512.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-30
- Filing Date
- 2020-09-02
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-09-02
AI Technical Summary
During the 3D printing process, microparticle pigments are difficult to disperse evenly in polyamide, resulting in uneven coloring of the final product, especially in demanding applications such as power tools, automotive parts and gears.
By functionalizing pigment particles with metal oxide particles to form side-chain epoxy or carboxylic acid groups, and then reacting them with polyamide, polyamide with pigments attached from the main chain (PP-polyamide) is generated. The polyamide is then mixed with a carrier fluid at a high shear rate to form uniformly dispersed particles.
It achieves uniform dispersion of pigments in polyamide, ensuring the color uniformity and stability of 3D printed items, making it suitable for harsh applications.
Smart Images

Figure CN112457488B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to compositions, synthesis methods and uses of polyamides having pigments pendant from the backbone of the polyamide.For example, a particle may comprise a polyamide having pigments pendant from the backbone of the polyamide. Background Art
[0002] Thermoplastic polymers are commonly used to make extruded articles, such as films, bags, particles and filaments. An example of a thermoplastic polymer is polyamide. Polyamides, such as nylon, are off-white polymers that have the ability to withstand high or low temperatures without losing physical properties. Therefore, articles formed from polyamides can be used in demanding applications, such as power tools, automotive parts, gears and appliance parts. In some cases, applications may require that parts made from polyamides be colored. Because the pigment is a microparticle, the pigment may be difficult to evenly mix in the polyamide, which results in uneven coloring of the resulting parts.
[0003] One application where uniform incorporation of pigments is particularly important is the rapidly growing field of three-dimensional (3D) printing technology, also known as additive manufacturing. Although 3D printing has traditionally been used for rapid prototyping activities, the technology is increasingly being used to produce commercial and industrial objects that may have structural and mechanical tolerances that are completely different from those of rapid prototypes.
[0004] 3D printing operates by depositing either (a) small droplets or streams of molten or solidifiable material or (b) powder particles in precise deposition locations for subsequent consolidation into a larger object, which may have any number of complex shapes. Such deposition and consolidation processes are typically performed under computer control to provide a layer-by-layer buildup of the larger object. In a specific example, consolidation of powder particles may be performed in a 3D printing system using a laser to facilitate selective laser sintering (SLS).
[0005] Powder particles that can be used for 3D printing include thermoplastic polymers (including thermoplastic elastomers), metals, and other solidifiable substances. An exemplary thermoplastic polymer is nylon. Nylon is an off-white polymer that has the ability to withstand high or low temperatures without losing physical properties. Therefore, nylon can be used in demanding applications such as power tools, automotive parts, gears, and appliance parts.
[0006] When using micro-particle pigments in 3D printing, the particles should be evenly dispersed throughout the molten droplets or powder particles, otherwise the coloration of the final object will be uneven. Summary of the invention
[0007] The present disclosure relates to compositions, synthesis methods and uses of polyamides having pigments pendant from the backbone of the polyamide.For example, a particle may comprise a polyamide having pigments pendant from the backbone of the polyamide.
[0008] The method described herein comprises: functionalizing metal oxide particles bonded to pigment particles with a compound having epoxy groups to produce a surface-treated pigment having pendant epoxy groups; and reacting the pendant epoxy groups with a polyamide to produce a pigment pendant polyamide (PP-polyamide).
[0009] The method described herein includes: functionalizing metal oxide particles bonded to pigment particles with silica particles having a carboxylic acid surface treatment to produce a surface-treated pigment having a pendant carboxylic acid; converting the pendant carboxylic acid into a pendant acid chloride; and reacting the pendant acid chloride with a polyamide to produce a PP-polyamide.
[0010] The compositions described herein include a polyamide having a pigment pendant from the backbone of the polyamide, wherein the pigment includes metal oxide particles on the surface of the pigment particles.
[0011] The articles described herein also comprise the aforementioned compositions.
[0012] The method described herein comprises mixing a mixture comprising a polyamide having the PP-polyamide, the carrier fluid immiscible with the PP-polyamide, and an optional emulsion stabilizer at a temperature greater than the melting point or softening temperature of the PP-polyamide and at a shear rate high enough to disperse the PP-polyamide in a carrier fluid; and cooling the mixture to below the melting point or softening temperature of the PP-polyamide to form solidified particles comprising the PP-polyamide and, when present, the emulsion stabilizer associated with the outer surface of the solidified particles.
[0013] The compositions described herein include particles comprising a polyamide having a PP-polyamide and having a roundness of from about 0.90 to about 1.0. The particles may also include one or more emulsion stabilizers associated with the outer surface of the particles.
[0014] The method disclosed herein also includes: depositing the particles (including the PP-polyamide), optionally in combination with other thermoplastic polymer particles, on a surface in a specified shape; and once deposited, heating at least a portion of the particles to promote their consolidation and form a consolidated body. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The following drawings are included to illustrate certain aspects of the disclosure and should not be construed as exclusive configurations. The disclosed subject matter is capable of considerable modification, alteration, combination, and equivalents in form and function, as will occur to those skilled in the art having the benefit of this disclosure.
[0016] Figure 1 is a flow chart of a non-limiting example method 100 of the present disclosure. DETAILED DESCRIPTION
[0017] The present disclosure relates to compositions, synthesis methods and application methods of polyamides having pigments pendant from the backbone of the polyamide (also referred to herein as polyamides with pendant pigments or PP-polyamides). Because the polyamide is functionalized with pigment particles, articles incorporating the PP-polyamide will have more uniformly dispersed pigments.
[0018] The present disclosure also relates to particles comprising polyamides having pigments pendant from the backbone of the polyamide (also referred to herein as pigment-pendant polyamides or PP-polyamides) and related methods. More specifically, the present disclosure includes methods of making highly spherical polymer particles comprising one or more PP-polyamides and optionally one or more other thermoplastic polymers. The polymer particles can be used, among other things, as feedstock for additive manufacturing.
[0019] The polymer particles described herein can be produced, for example, by a melt emulsification process, wherein one or more PP-polyamides and optionally one or more additional thermoplastic polymers are dispersed as a melt in a carrier fluid that is immiscible with the PP-polyamide and the additional thermoplastic polymer (if used). Sufficient shear is applied to the mixture to cause the polymer melt to form droplets in the carrier fluid.
[0020] Because the pigment is pendant from the backbone of the polyamide, articles produced via additive manufacturing methods that include these particles should maintain a uniform color over time because the pigment cannot migrate within the article.
[0021] Definition and test methods
[0022] As used herein, the term "pigment" refers to particles that absorb and / or refract ultraviolet or visible light. As used herein, "surface treated pigment" refers to a pigment having oxide particles chemically and / or physically bonded to the surface of the pigment particles.
[0023] As used herein, the term "immiscible" refers to a mixture of components that, when combined, form two or more phases that have less than 5 weight % solubility in each other at ambient pressure and room temperature or the melting points of the components if they are solid at room temperature. For example, polyethylene oxide having a molecular weight of 10,000 g / mol is solid at room temperature and has a melting point of 65° C. Thus, if a material that is liquid at room temperature and the polyethylene oxide have less than 5 weight % solubility in each other at 65° C., the polyethylene oxide is immiscible with the material.
[0024] As used herein, the term "thermoplastic polymer" refers to a plastic polymer material that can reversibly soften and harden when heated and cooled. Thermoplastic polymers encompass thermoplastic elastomers.
[0025] As used herein, the term "elastomer" refers to a copolymer comprising a crystalline "hard" segment and an amorphous "soft" segment. For example, in the case of a polyurethane, the crystalline segment may include a portion of a polyurethane having carbamate functional groups and optional chain extender groups, and the soft segment may include a polyol.
[0026] As used herein, the term "polyurethane" refers to the polymer reaction product between a diisocyanate, a polyol, and an optional chain extender.
[0027] As used herein, the term "oxide" refers to both metal oxides and non-metal oxides. For the purposes of this disclosure, silicon is considered a metal.
[0028] As used herein, the terms "associated," "associated," and grammatical variations thereof between an emulsion stabilizer and a surface refer to chemical bonding and / or physical adhesion of the emulsion stabilizer to the surface. Without being limited by theory, it is believed that the association between the polymers described herein and the emulsion stabilizer is primarily physical adhesion via hydrogen bonding and / or other mechanisms. However, chemical bonding may occur to some extent.
[0029] As used herein, the term "embedded" with respect to nanoparticles and polymer particle surfaces means that the nanoparticles extend at least partially into the surface such that the polymer contacts the nanoparticles to a greater extent than would occur if the nanoparticles were simply laid down on the polymer particle surface.
[0030] As used herein, D10, D50, D90 and diameter span are primarily used herein to describe particle size. As used herein, the term "D10" refers to the diameter at which 10% of the sample (on a volume basis unless otherwise specified) consists of particles with a diameter less than the stated diameter value. As used herein, the term "D50" refers to the diameter at which 50% of the sample (on a volume basis unless otherwise specified) consists of particles with a diameter less than the stated diameter value. As used herein, the term "D90" refers to the diameter at which 90% of the sample (on a volume basis unless otherwise specified) consists of particles with a diameter less than the stated diameter value.
[0031] As used herein, the terms "diameter span" and "span" and "span size" when referring to diameter provide an indication of the breadth of the particle size distribution and are calculated as (D90-D10) / D50 (again unless otherwise indicated, each D value is based on volume).
[0032] By using the Malvern MASTERSIZERTM Particle size was determined by light scattering techniques or analysis of optical digital micrographs of the ATmega 3000. Unless otherwise specified, light scattering techniques were used to analyze particle size.
[0033] For light scattering techniques, the control sample is the product of the trade name Quality Audit Standards QAS4002 TM Glass microspheres with diameters ranging from 15 μm to 150 μm were purchased from Malvern Analytical Ltd. Samples were analyzed as dry powders unless otherwise specified. TM The particles to be analyzed were dispersed in air and analyzed using the 3000. The particle size was derived from a plot of bulk density versus size using the instrument software.
[0034] Particle size measurements and diameter spans can also be determined by optical digital microscopy.Optical images were obtained using a Keyence VHX-2000 digital microscope and version 2.3.5.1 software for particle size analysis (system version 1.93).
[0035] As used herein, when referring to sieving, the hole / sieve size is described in terms of United States Standard Sieve (ASTM E11-17).
[0036] As used herein, the terms "roundness" and "sphericity" with respect to particles refer to how close a particle is to a perfect sphere. To determine roundness, an optical microscopic image is taken of the particle. The perimeter (P) and area (A) of the particle in the plane of the microscopic image are calculated (e.g., using a SYSMEX FPIA 3000 particle shape and size analyzer, available from Malvern Instruments). The roundness of a particle is C EA / P, where C EA It is the circumference of a circle whose area is equal to the area (A) of the actual particle.
[0037] As used herein, the term "sintering window" refers to the difference between the melting temperature (Tm) onset and the crystallization temperature (Tc) onset or (Tm-Tc) onset. Tm, Tm (onset), Tc, and Tc (onset) are determined by differential scanning calorimetry at a ramp rate of 10 ° C / min and a cooling rate of 10 ° C / min according to ASTM E794-06 (2018).
[0038] As used herein, the term "shear" refers to stirring or similar processes that cause mechanical agitation in a fluid.
[0039] As used herein, the term "aspect ratio" refers to the length divided by the width, wherein the length is greater than the width.
[0040] Unless otherwise indicated, the melting point of the polymers was determined by ASTM E794-06 (2018) with a 10°C / min ramp rate and cooling rate.
[0041] Unless otherwise indicated, the softening temperature or softening point of a polymer is determined by ASTM D6090-17.The softening temperature can be measured by using a cup and ball apparatus from Mettler-Toledo using a 0.50 gram sample at a heating rate of 1°C / min.
[0042] The angle of repose is a measure of the flowability of a powder. Angle of repose measurements were determined using ASTM D6393-14 "Standard Test Method for Bulk Solids Characterized by Carr Indices" using a Hosokawa Micron Powder Characterization Tester PT-R.
[0043] Hausner ratio (Hausner ratio, H r ) is a measure of the flowability of the powder and is determined by H r =ρ 振实 / ρ 堆积 Calculate, where ρ 堆积 is the bulk density according to ASTM D6393-14, and ρ 振实 It is the tap density according to ASTM D6393-14.
[0044] As used herein, unless otherwise specified, the viscosity of the carrier fluid is the kinematic viscosity at 25° C., measured in accordance with ASTM D445-19. For commercially available carrier fluids (e.g., PDMS oil), the kinematic viscosity data cited herein are provided by the manufacturer, whether measured in accordance with the aforementioned ASTM or another standard measurement technique.
[0045] Pigment-side-mounted polyamide
[0046] In general, the compositions, synthesis methods, and use methods of the present disclosure use a linker that chemically bonds the oxide particles of the surface treated pigment to the nitrogen of the polyamide. The result is PP-polyamide. Because the surface treated pigment has several oxide particles on the surface, the surface treated pigment particles can be used as a crosslinker for the polyamide.
[0047] Examples of polyamides include, but are not limited to, polycaprolactam (nylon 6, polyamide 6, or PA6), poly(hexamethylene succinamide) (nylon 4,6, polyamide 4,6, or PA4,6), polyhexamethylene adipamide (nylon 6,6, polyamide 6,6, or PA6,6), polypentamethylene adipamide (nylon 5,6, polyamide 5,6, or PA5,6), polyhexamethylene sebacamide (nylon 6,10, polyamide 6,10, or PA6,10), polyundecanamide (nylon 11, polyamide 11, or PA11), polydodecaneamide (nylon 12, polyamide 12, or PA12), polyhexamethylene terephthalamide (nylon 6T, polyamide 6T, or PA6T), Nylon 10,10 (polyamide 10,10 or PA10,10), nylon 10,12 (polyamide 10,12 or PA10,12), nylon 10,14 (polyamide 10,14 or PA10,14), nylon 10,18 (polyamide 10,18 or PA10,18), nylon 6,18 (polyamide 6,18 or PA6,18), nylon 6,12 (polyamide 6,12 or PA6,12), nylon 6,14 (polyamide 6,14 or PA6,14), nylon 12,12 (polyamide 12,12 or PA12,12), semi-aromatic polyamide, aromatic polyamide (aramid), etc. and any combination thereof. Copolyamides can also be used. Examples of copolyamides include, but are not limited to, PA 11 / 10,10, PA 6 / 11, PA 6,6 / 6, PA 11 / 12, PA 10,10 / 10,12, PA 10,10 / 10,14, PA 11 / 10,36, PA 11 / 6,36, PA 10,10 / 10,36, PA 6T / 6,6, etc. and any combination thereof. Examples of polyamide elastomers include, but are not limited to, polyesteramides, polyetheresteramides, polycarbonate-esteramides, and polyether-block-amide elastomers. Herein, a polyamide followed by a single number is a polyamide having that number of main chain carbons between each nitrogen. A polyamide followed by a first number comma second number is a polyamide having a first number of main chain carbons between nitrogens for segments without pendant =O and a second number of main chain carbons between two nitrogens for segments with pendant =O. As a non-limiting example, nylon 6,10 is [NH-(CH 2 ) 6 -NH-CO-(CH 2 ) 8 -CO] n A polyamide followed by a quantitative backslash number is a copolymer of the polyamide indicated by the numbers before and after the backslash.
[0048] Pigments can impart color, metallic color, and / or pearlescent color to the polyamide, such as gold, silver aluminum, bronze, gold bronze, stainless steel, zinc, iron, tin, and copper pigments. Examples of pigments include, but are not limited to, synthetic mica (e.g., fluorphlogopite), natural mica (e.g., muscovite), talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments (e.g., BiOCl, colored glass fibers, α-Fe 2 O 3 and α-FeOOH), CaSO 4 , iron oxide, chromium oxide, carbon black, metal effect pigments (e.g., Al flakes and bronze), optional optically variable pigments (OVP), liquid crystal polymer pigments (LCP), holographic pigments, etc. and any combination thereof.
[0049] Examples of metal oxides that can be coated on the surface of the pigment include, but are not limited to, titanium dioxide, titanium suboxide, titanium oxynitride, Al 2 O 3 , Fe 2 O 3 , Fe 3 O 4 SnO 2 Cr 2 O 3 , ZnO, CuO, NiO, zirconium oxide, titanium iron oxide (titanium iron), other metal oxides, etc. and any combination thereof. Preferred metal oxides include TiO 2 and / or Fe 2 O 3 .
[0050] The surface treated pigments may be any combination of the above pigments and one or more metal oxides, which are present alone or in a mixture of uniform layers or continuous layers. For example, the surface treated pearlescent pigments may be pigments based on a flake-like, transparent or translucent substrate such as silicate, which are coated with colored or colorless metal oxides such as titanium oxide and iron oxide alone or in a mixture of uniform layers or continuous layers. Particularly preferred surface treated pigments include TiO 2 Coated mica, Fe 2 O 3 Coated mica, TiO 2 / Fe2O 3 Coated micas and any combinations thereof.
[0051] Examples of commercially available surface treated pigments include, but are not limited to, REFLEX TMPigment (synthetic mica-based pearlescent pigment, available from CQV), IRIODIN TM (Mica-based, metal oxide-coated pearlescent pigments available from Merck) (e.g., IRIODIN TM 300 "Gold Pearl" and IRIODIN TM 100 "Silver Pearl"), SUNGEM TM (glass flake-based pigment, available from Sun Chemical), SUNMICA TM (mica-based pigment, available from Sun Chemical), SYNCRYSTAL TM (metal oxide coated synthetic fluorphlogopite flakes, available from Eckart), etc. and any combination thereof. Other metallic pearlescent pigments available from Merck include those with a D50 volume average particle size (50% of the pigment has a volume size smaller than the specified size) of 22 to 37 microns. Bronze MP60, D50 size 22 microns to 37 microns Copper MP-65, D50 size 3 microns to 10 microns Oriental Beige, D50 size 18 microns to 25 microns Aborigine Amber, D50 size 18 microns to 25 microns Passion Orange, D50 size 7 microns to 14 microns Bronze Fine, D50 size 18 microns to 25 microns Bronze, D50 size 28 microns to 42 microns Bronze Sparkle, D50 size 7 microns to 14 microns Copper Fine, D50 size 18 microns to 25 microns Copper, D50 size 25 microns to 39 microns Copper Sparkle, D50 size 18 microns to 25 microns Red Brown, D50 size 18 microns to 25 microns Russet, D50 size 18 microns to 25 microns Tibetan Ochre, D50 size 7 microns to 14 microns Sienna Fine, D50 size 18 microns to 25 microns Sienna, D50 size 18 microns to 25 microns Bordeaux, Glitter Bordeaux, D50 size 18 microns to 25 microns Also suitable are Merck mica-based pigments with a coating of metal oxide particles, such as Merck silver white pigments, including those with a D50 size of 3 to 10 microns. Super Silk MP-1005, D50 size 7 microns to 14 microns Super Sheen MP-1001, D50 size 9 microns to 13 microns Super Silver Fine, D50 size 15 microns to 21 microns Pearl Sheen MP-30, D50 size 11 micron to 20 micron Satin MP-11171, D50 size 18 microns to 25 microns Ultra Luster MP-111, D50 size 18 microns to 25 microns Star Luster MP-111, D50 size 22 microns to 37 microns PearlFlake MP-10, D50 size 17 micron to 26 micron Super Silver, D50 size 28 microns to 38 microns Sparkle MP-47, D50 size 19 microns to 25 microns Arctic Silver, D50 size 15 microns to 22 microns Silver, D50 size 25 microns to 45 microns Silver, etc. and any combination thereof. For very bright colors, examples from Merck include D50 sizes of 10 microns to 60 microns. Carmine Red, produces a red gloss effect, with a D50 size of 18 microns to 25 microns Magenta, produces a pink-purple sheen effect, with a D50 size of 18 microns to 25 microns Light Blue, produces a light blue sheen effect, with a D50 size of 18 microns to 25 microns Dark Blue, produces a dark blue gloss effect, with a D50 size of 18 microns to 25 microns Majestic Green, produces a green sheen, D50 size 19 microns to 26 microns Brilliant Green, produces a golden green luster, D50 size is 18 microns to 25 microns Egyptian Emerald, produces a deep green sheen effect, with a D50 size of 18 microns to 25 microns Patagonian Purple, producing a purple sheen effect, etc. and any combination thereof. Mica-based special effect pigments such as PTFE® from Eckart Corporation having a D50 of about 18 microns to about 50 microns may also be used. PX 4001, PX 4261, PX 4271, PX4310, PX 4331, PX 4542, XT, XT2001, XT 3001, XT 4001, XT 5001, PX 1000, PX 1001, PX 1221, PX 1231, PX 1241, PX 1251, PX 1261, PX1271, PX 1310, PX 1320, PX 1502, PX 1522, PX 1542, PX 2000, PX 2000L, PX 2001, PX 2011, PX 2021, PX2221, PX 2231, PX 2241, PX 2251, PX 2261, PX 2271, PX 3001, PX 4000, PX 4001, PX 4221, PX 4231, PX4241, PX 4251, PX 4261, PX 4271, PX 4310, PX 4320, PX 4502, PX 4522, PX 4542, PX 5000, PX 5001, PX5310, PX 5331, etc. and any combination thereof. Special effect pigments may be used, such as aluminum flake pigments from Silberline, such as 16 micron DF-1667, 55 micron DF-2750, 27 micron DF-3500, 35 micron DF-3622, 15 micron DF-554, 20 micron DF-L-520AR, 20 micron LED-1708AR, 13 micron LED-2314AR, 55 micron SILBERCOTE TM PC 0452Z, 47 micron SILBERCOTE TM PC 1291X, 36 micron SILBERCOTE TM , 36 micron SILBERCOTE TM PC 3331X, 31 micron SILBERCOTE TM PC 4352Z, 33 micron SILBERCOTE TM PC 4852X, 20 micron SILBERCOTE TM PC 6222X, 27 micron SILBERCOTE TM PC6352Z, 25 micron SILBERCOTE TM PC 6802X, 14 micron SILBERCOTE TM PC 8152Z, 14 micron SILBERCOTE TM PC 8153X, 16 micron SILBERCOTE TMPC 8602X, 20 micron 890 series, 16 micron 950 series etc and any combination of them.
[0052] The surface treated pigments may have an average diameter (or D50) of from about 1 micron to about 500 microns (or from about 1 micron to about 25 microns, or from about 5 microns to about 50 microns, or from about 25 microns to about 200 microns, or from about 100 microns to about 300 microns, or from about 250 microns to about 500 microns). Without being limited by theory, it is believed that larger pigment particles impart greater coloration, metallic and / or pearlescent effects to the polyamide.
[0053] Scheme 1 below is a first non-limiting example synthesis of a PP-polyamide. More specifically, the bifunctional bonding agent comprises, for example, an alkoxysilane terminal group and a glycidyl functional group. The alkoxysilane group (in the form of Si(-OCH 3 ) 3 ) groups, one or more of which are hydrolyzable to -OH groups) are coupled to the surface of oxide particles (MOx particles) on the surface of the pigment. Although the silane is shown as being coupled only to the metal oxide particles, depending on the composition of the pigment, the silane may also be coupled to the surface of the pigment. The epoxy group of the glycidyl portion then reacts with the nitrogen of the amide in the polyamide (shown using nylon 6) to produce a PP-polyamide. Although the epoxy group is shown as a terminal epoxy group, the bifunctional bonding agent may have one or more glycidyl functional groups (or epoxy groups) that are terminal, side chain, or both terminal and side chain of such groups. As shown, the pigment is chemically bonded to four polyamide chains, indicating that the pigment may also be a crosslinking agent.
[0054] Solution 1
[0055]
[0056] Examples of silanes having a glycidyl moiety include, but are not limited to, (3-glycidyloxypropyl)trimethoxysilane, (3-glycidyloxypropyl)triethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane and 1,3-bis(3-glycidyloxypropyl)tetramethylsiloxane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidyloxypropylmethyldimethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, 5,6-epoxyhexyltriethoxysilane, and the like, and any combination thereof.
[0057] Silane coupling reaction can be carried out by known methods. For example, "Glycidyl Alkoxysilanc Reactivities Towards Simple Nucleophiles in Organic Media for Improved Molecular Structure Definition in Hybrid Materials" summarized in the references of X. Guillory et al., Royal Society of Chemistry Advances 2016, 6th edition, pp. 74087 to 74099. The result of the reaction is highly dependent on the reaction conditions; the choice of solvent (whether it is aqueous, organic or ionic liquid medium), temperature concentration, catalyst and acidic or basic conditions. Also from the cited U.S. Patent No. 7,998,649, a metal oxide coated mica pigment on the surface of the silica or titanium dioxide particles is reacted with (3-glycidoxypropyl)trimethoxysilane or (3-glycidoxypropyl)triethoxysilane or diethoxy(3-glycidoxypropyl)methylsilane or 1,3-bis(3-glycidoxypropyl)tetramethylsiloxane in a molar ratio of 0.85 to 0.15 with appropriate amounts of ethanol or methanol, water and ammonia to prepare an epoxide-containing component. The solution is then stirred at room temperature or slightly elevated to 40° C. for a period of about 2 hours to about 10 hours.
[0058] As another example, the silane coupling reaction can be carried out by hydrolysis deposition of silane (B. Arkles, CHEMTECH, 7th edition, page 766, 1977), wherein the silane oligomer is hydrogen bonded to the OH group of the substrate. During drying or curing, a covalent bond is formed with the substrate while losing water. The method for enhancing reactivity includes an ester exchange catalyst and an agent that increases the acidity of the hydroxyl groups on the substrate by hydrogen bonding. The ester exchange catalyst includes tin compounds such as dibutyl diacetoxytin and titanates such as titanium isopropoxide. In many cases, the incorporation of an ester exchange catalyst at about 2% to about 3% by weight of the silane effectively promotes the reaction and deposition, and other catalysts include tetrabutyl titanate, or the reaction can be promoted by adding a catalytic amount of an amine such as benzyl dimethylamine. The reaction conditions may include that the coupling agent may be present at about 0.1 wt % to about 5 wt % relative to the pigment, the reaction time may be about 4 hours to about 12 hours, the temperature may be about 50° C. to about 120° C., and ethanol solvent may be better than methanol, wherein the water content in the solvent is about 1 wt % to about 5 wt % to promote hydrolysis of the silane during attachment to the surface.
[0059] For another example, the silane coupling reaction can be carried out by anhydrous liquid phase deposition, wherein a toluene, tetrahydrofuran and / or hydrocarbon solution containing about 1% by weight to about 10% by weight of silane is prepared. The mixture is refluxed for about 12 hours to about 24 hours, wherein the substrate (in this case, the pigment) is to be treated. The treated pigment is washed with a solvent. The solvent is then removed by air or explosion-proof oven drying. No further curing is required.
[0060] The reaction of the epoxy groups on the metal pigment with the polyamide can be carried out at a temperature of about 70°C to about 200°C (or about 70°C to about 150°C, or about 125°C to about 200°C) in the presence of an organic solvent such as tetrahydrofuran, dimethylformamide or toluene, etc., under an atmosphere (nitrogen or argon). The mixture is then stirred at elevated temperature for about 24 hours. After the mixture is cooled to room temperature, the grafted polymer is filtered and washed to remove organic impurities and unreacted starting reagents.
[0061] Scheme 2 below is a second non-limiting example synthesis of a PP-polyamide. More specifically, silica particles having at least one surface functional group of a carboxylic acid (which may be terminal, pendant, or both terminal and pendant as shown) are grafted onto metal oxide particles (although some may be grafted onto pigments depending on the pigment composition). The carboxylic acid from the functionalized silica particles is then converted to an acid chloride, which reacts with the amide nitrogen in a polyamide (shown using nylon 6) to produce a PP-polyamide. As shown, the pigment is chemically bonded to four polyamide chains, which shows that the surface-coated pigment (the surface of the pigment and / or the surface of the metal oxide particles) can also be a crosslinking agent.
[0062] Solution 2
[0063]
[0064] Examples of functionalized silica particles include, but are not limited to, 3-aminopropyl-(3-oxobutyric acid) functionalized silica, 3-propylsulfonic acid functionalized silica, propylcarboxylic acid functionalized silica, triaminetetraacetic acid functionalized silica, propionyl chloride functionalized silica, 3-carboxypropyl functionalized silica, aminomethylphosphonic acid (AMPA) functionalized silica, 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid (DOTA) functionalized silica, and the like, and any combination thereof.
[0065] The grafting reaction of functionalized silica with pigments can be carried out by known methods. Similar to the glycidyl functionalized coated pigments in Scheme 1, silanes containing reactive alkoxy (OR) functional groups can react with the surface hydroxyl groups of metal oxide particles and / or pigments. When the silane solution is applied to the surface hydroxyl groups of metal oxide particles and / or pigments, the free silanol groups first form hydrogen bonds with the hydroxyl groups (-OH) on the metal oxide particles and / or pigments at ambient temperature. Then, the silanols are condensed with SiO 2 Bonds are formed between the -OH groups on the surface of SiO 2 key.
[0066] The conversion of carboxylic acids into more reactive acid chlorides can be carried out by known methods. For example, oxalyl chloride (COCl) 2 and / or thionyl chloride SOCl 2 It can be used as a chlorinating agent in combination with a catalyst. The solvent used in the reaction may include, but is not limited to, dimethylformamide, dichloromethane, etc. and any combination thereof.
[0067] The reaction of acid chloride / polyamide with polyamide can be carried out by known methods. For example, the pigment with acid chloride functional group can be melt mixed with polyamide at about 125°C to about 250°C (or about 125°C to about 200°C, or about 150°C to about 225°C, or about 200°C to about 250°C) for about 15 minutes to about 1 hour or more (or about 15 minutes to about 30 minutes, or about 20 minutes to about 40 minutes, or about 30 minutes to about 1 hour).
[0068] Schemes 1 and 2 include non-limiting examples of synthetic routes for preparing surface treated pigments having pendant epoxy or carboxylic acid moieties. Other reaction schemes will be apparent to those skilled in the art.
[0069] Surface treated pigments having pendant epoxy or carboxylic acid moieties are reacted with polyamides to produce the PP-polyamides described herein.
[0070] Whether by Scheme 1, Scheme 2 or another coupling reaction scheme, the PP-polyamide described herein can have a pigment to polyamide weight ratio of about 1:10 to about 1:1000 (or about 1:10 to about 1:200 or about 1:100 to about 1:500 or about 1:250 to about 1:1000).
[0071] Application of PP-polyamide
[0072] The PP-polyamide described herein can be used to produce a variety of articles (or products). The PP-polyamide described herein can be used alone or in combination with other thermoplastic polymers (eg, polyamide without light absorber and / or other thermoplastic polymers). Examples of thermoplastic polymers that can be used with one or more PP-polyamides of the present disclosure include, but are not limited to, polyamides (e.g., polyamides not coupled to a pigment), polyurethanes, polyethylenes, polypropylenes, polyacetals, polycarbonates, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polytrimethylene terephthalate (PTT), polyhexamethylene terephthalate, polystyrene, polyvinyl chloride, polytetrafluoroethylene, polyesters (e.g., polylactic acid), polyethers, polyethersulfones, polyetheretherketones, polyacrylates, polymethacrylates, polyimides, acrylonitrile butadiene styrene (ABS), polyphenylene sulfide, vinyl polymers, polyarylethers, polyarylene sulfides, polysulfones, polyetherketones, polyamide-imides, polyetherimides, polyetheresters, copolymers comprising polyether blocks and polyamide blocks (PEBA or polyetherblocks), and polyamide-imides. The invention can be used in the following embodiments of the present invention: a polyimide (segment amide), a grafted or non-grafted thermoplastic polyolefin, a functionalized or non-functionalized ethylene / vinyl monomer polymer, a functionalized or non-functionalized ethylene / (meth) acrylate alkyl ester, a functionalized or non-functionalized (meth) acrylic polymer, a functionalized or non-functionalized ethylene / vinyl monomer / (meth) acrylate alkyl ester terpolymer, an ethylene / vinyl monomer / carbonyl terpolymer, an ethylene / (meth) acrylate alkyl ester / carbonyl terpolymer, a methyl methacrylate-butadiene-styrene (MBS) core-shell polymer, a polystyrene-block-polybutadiene-block-poly(methyl methacrylate) (SBM) block terpolymer, a chlorinated or chlorosulfonated polyethylene, a polyvinylidene fluoride (PVDF), a phenolic resin, a poly(ethylene / vinyl acetate), a polybutadiene, a polyisoprene, a styrenic block copolymer, a polyacrylonitrile, a silicone, and the like, and any combination thereof. Copolymers comprising one or more of the foregoing can also be used in the methods and systems described herein.
[0073] If desired, a compatibilizer may be used when combining the PP-polyamide described herein with other thermoplastic polymers. A compatibilizer may improve the blending efficiency and / or efficacy of the polymers. Examples of polymer compatibilizers include, but are not limited to, PROPOLDER TM MPP2020 20 (polypropylene, available from Polygroup Inc.), PROPOLDER TM MPP2040 40 (polypropylene, available from Polygroup Inc.), NOVACOM TMHFS2100 (maleic anhydride functionalized high density polyethylene polymer, available from Polygroup Inc.), KEN-REACT TM CAPS TM L TM 12 / L (organic metal coupling agent, available from Kenrich Petrochemicals), KEN-REACT TM CAPOW TM L TM 12 / H (organic metal coupling agent, available from Kenrich Petrochemicals), KEN-REACT TM LICA TM 12 (organic metal coupling agent, available from Kenrich Petrochemicals), KEN-REACT TM CAPS TM KPR TM 12 / LV (organic metal coupling agent, available from Kenrich Petrochemicals), KEN-REACT TM CAPOW TM KPR TM 12 / H (organic metal coupling agent, available from Kenrich Petrochemicals), KEN-REACT TM Titanates and zirconates (organic metal coupling agents, available from Kenrich Petrochemicals), VISTAMAXX TM (ethylene-propylene copolymer, available from ExxonMobil), SANTOPRENE TM (a thermoplastic vulcanizate of EPDM and polypropylene, available from ExxonMobil), VISTALON TM (EPDM rubber, available from ExxonMobil), EXACT TM (plastomer, available from ExxonMobil), EXXELOR TM (polymer resin, available from ExxonMobil), FUSABOND TM M603 (random ethylene copolymer, available from DOW), FUSABOND TME226 (anhydride-modified polyethylene, available from Dow Chemical Company (DOW)), BYNEL TM 41E710 (co-extrudable adhesive resin, available from DOW), SURLYN TM 1650 (ionomer resin, available from DOW), FUSABOND TM P353 (chemically modified polypropylene copolymer, available from DOW), ELVALOY TM PTW (ethylene terpolymer, available from DOW), ELVALOY TM 3427AC (copolymer of ethylene and butyl acrylate, available from DOW Chemical Company (DOW)), LOTADER TM AX8840 (ethylene-acrylate based terpolymer, available from Arkema), LOTADER TM 3210 (ethylene-acrylate based terpolymer, available from Arkema), LOTADER TM 3410 (ethylene-acrylate based terpolymer, available from Arkema), LOTADER TM 3430 (ethylene-acrylate based terpolymer, available from Arkema), LOTADER TM 4700 (ethylene-acrylate based terpolymer, available from Arkema), LOTADER TM AX8900 (ethylene-acrylate based terpolymer, available from Arkema), LOTADER TM 4720 (ethylene-acrylate based terpolymer, available from Arkema), BAXXODUR TM EC 301 (amine of epoxy resin, available from BASF), BAXXODUR TM EC 311 (amine of epoxy resin, available from BASF), BAXXODUR TM EC 303 (amine of epoxy resin, available from BASF), BAXXODUR TM EC 280 (amine of epoxy resin, available from BASF), BAXXODUR TM EC 201 (amine of epoxy resin, available from BASF), BAXXODUR TMEC 130 (amine of epoxy resin, available from BASF), BAXXODUR TM EC 110 (amine of epoxy resin, available from BASF), styrene, polypropylene, polyamide, polycarbonate, EASTMAN TM G-3003 (maleic anhydride grafted polypropylene, available from Eastman), RETAIN TM (polymer modifier, available from DOW Chemical Company (DOW)), AMPLIFY TY TM (maleic anhydride grafted polymer, available from DOW Chemical Company (DOW)), INTUNE TM (olefin block copolymer, available from The Dow Chemical Company (DOW)), etc. and any combination thereof.
[0074] Methods for making articles include, but are not limited to, melt extrusion, injection molding, compression molding, melt spinning, melt emulsification, spray drying (e.g., to form particles), cryogenic milling (or cryogenic grinding), freeze drying polymer dispersions, precipitation of polymer dispersions, and the like, and any mixtures thereof.
[0075] Examples of articles that can be produced by such methods in which the PP-polyamide can be all or part of the article include, but are not limited to, pellets, films, packaging, toys, household goods, automotive parts, aviation / aircraft related parts, containers (e.g., for food, beverages, cosmetics, personal care compositions, pharmaceuticals, etc.), shoe soles, furniture parts, decorative homewares, plastic gears, screws, nuts, bolts, cable ties, jewelry, artwork, sculptures, medical supplies, prostheses, orthopedic implants, production of artifacts to aid learning in education, 3D anatomical models to aid surgery, robotics, biomedical devices (orthotics), household appliances, dentistry, electronics, sporting goods, etc. In addition, the pellets can be used in applications including, but not limited to, paints, powder coatings, inkjet materials, electrophotographic toners, 3D printing, etc.
[0076] Additionally, the PP-polyamide described herein may have a specific chemical fingerprint for identifying an item, tracking an item, authenticating an item, and / or determining the health status of an item. Additionally, the location of the PP-polyamide in the item is another layer of fingerprinting the item for identifying the item, tracking the item, authenticating the item, and / or determining the health status of the item.
[0077] A method of identifying an item, tracking an item, authenticating an item, and / or determining the health status of an item may include (a) exposing an item comprising PP-polyamide to electromagnetic radiation; (b) sensing one or more spectra associated with absorbed and / or re-emitted electromagnetic radiation; and (c) comparing the spectrum of a light absorber used in the item or a portion thereof with a known spectrum. Optionally, the location of a spectral region on the item may be compared with a known location where the spectral region should be located. The comparison may be used to identify and / or authenticate the item. For tracking purposes, the detected spectra and / or spectral regions may be compared and / or recorded in a database along with the physical location of the item. In addition, the health status of worn and / or broken items may be detected. For example, a core portion of an article may include a light absorber, and an outer portion may cover the core portion and not include the light absorber (or include a different light absorber). Then, when the spectra are compared, the presence of a spectral signature of the light absorber in the core may indicate that the item is at or near the end of its life.
[0078] As a non-limiting example, the 3D printing process of the present disclosure may include: depositing particles comprising one or more PP-polyamides of the present disclosure (and optionally one or more other thermoplastic polymers and / or one or more compatibilizers) on a surface in a specified shape, and once deposited, heating at least a portion of the particles to promote consolidation thereof and form a consolidated body (article), such that the consolidated body has a void percentage of about 1% or less after consolidation. For example, the heating and consolidation of the thermoplastic polymer particles may be performed in a 3D printing device using a laser, such that the heating and consolidation are performed by selective laser sintering.
[0079] As a non-limiting example, the 3D printing process of the present disclosure may include: extruding a filament comprising one or more PP-polyamides of the present disclosure (and optionally one or more other thermoplastic polymers and / or one or more compatibilizers) and passing it through an orifice, wherein the filament becomes a polymer melt upon extrusion; depositing the polymer melt as a first layer on a platform; cooling the layer; depositing additional layers of the polymer melt on the first layer; cooling the additional layer; and repeatedly depositing and cooling at least one additional layer to produce a 3D shape.
[0080] Yet another non-limiting example is a process comprising extruding a polymer melt comprising one or more PP-polyamides of the present disclosure (and optionally one or more other thermoplastic polymers and / or one or more compatibilizers) and passing it through an orifice to produce films, fibers (or filaments), particles, pellets, etc.
[0081] Thermoplastic polymer particles and preparation method
[0082] The accompanying figure is a flow chart of a non-limiting exemplary method 100 of the present disclosure. A thermoplastic polymer 102 (comprising one or more PP-polyamides and optionally one or more other thermoplastic polymers), a carrier fluid 104, and an optional emulsion stabilizer 106 are combined 108 to produce a mixture 110. The components 102, 104, and 106 may be added in any order and include mixing and / or heating during the combination of the components 102, 104, and 106 at 108.
[0083] The mixture 110 is then processed at 112 by applying sufficiently high shear to the mixture 110 at a temperature greater than the melting point or softening temperature of the thermoplastic polymer 102 to form a molten emulsion 114. Since the temperature is above the melting point or softening temperature of the thermoplastic polymer 102, the thermoplastic polymer 102 becomes a polymer melt. The shear rate should be high enough to disperse the polymer melt in the carrier fluid 104 in the form of droplets (i.e., polymer emulsion 114). Without being limited by theory, it is believed that increasing shear should reduce the size of the droplets of polymer melt in the carrier fluid 104, all other factors being equal. However, at some point there may be diminishing returns to increasing shear and reducing droplet size, and / or there may be damage to the contents of the droplets, thereby reducing the quality of the particles produced therefrom.
[0084] The molten emulsion 114 inside and / or outside the mixing vessel is then cooled at 116 to solidify the polymer droplets into thermoplastic polymer particles (also referred to as solidified thermoplastic polymer particles). The cooled mixture 118 may then be processed at 120 to separate the thermoplastic polymer particles 122 from other components 124 (e.g., carrier fluid 104, excess emulsion stabilizer 106, etc.), and to wash or otherwise purify the thermoplastic polymer particles 122. The thermoplastic polymer particles 122 include the thermoplastic polymer 102 and, when included, at least a portion of the emulsion stabilizer 106 coating the outer surface of the thermoplastic polymer particles 122. The emulsion stabilizer 106, or a portion thereof, may be deposited on the thermoplastic polymer particles 122 as a uniform coating. In some cases, which may depend on non-limiting factors such as temperature (including cooling rate), type of thermoplastic polymer 102, and type and size of emulsion stabilizer 106, nanoparticles of emulsion stabilizer 106 may be at least partially embedded within the outer surface of thermoplastic polymer particles 122 during association with the outer surface of the thermoplastic polymer particles 122. Even if embedding does not occur, at least the nanoparticles within the emulsion stabilizer 106 may remain robustly associated with the thermoplastic polymer particles 122 to facilitate further use thereof. In contrast, dry blending already formed thermoplastic polymer microparticles (e.g., formed by cryogenic grinding or precipitation processes) with a flow aid (such as silica nanoparticles) does not produce a robust, uniform coating of the flow aid on the thermoplastic polymer microparticles.
[0085] Advantageously, the carrier fluid and wash solvent of the systems and methods described herein (eg, method 100) can be recycled and reused. One skilled in the art will recognize any necessary cleaning of the spent carrier fluid and solvent required during the recycling process.
[0086] The thermoplastic polymer 102 and the carrier fluid 104 should be selected so that they are immiscible at various processing temperatures (e.g., from room temperature to the processing temperature). An additional factor that may be considered is the difference (e.g., difference or ratio) in viscosity between the molten polyamide 102 and the carrier fluid 104 at the processing temperature. The viscosity difference may affect droplet breakup and particle size distribution. Without being limited by theory, it is believed that when the viscosities of the molten polyamide 102 and the carrier fluid 104 are too similar, the roundness of the product as a whole may be reduced, with the particles being more oval and more elongated structures observed.
[0087] Thermoplastic polymer 102 includes one or more PP-polyamides and optionally one or more other thermoplastic polymers. Examples of other thermoplastic polymers include, but are not limited to, polyamides, polyurethanes, polyethylenes, polypropylenes, polyacetals, polycarbonates, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polytrimethylene terephthalate (PTT), polyhexamethylene terephthalate, polystyrene, polyvinyl chloride, polytetrafluoroethylene, polyesters (e.g., polylactic acid), polyethers, polyethersulfones, polyetheretherketones, polyacrylates, polymethacrylates, polyimides, acrylonitrile butadiene styrene (ABS), polyphenylene sulfide, vinyl polymers, polyarylethers, polyarylene sulfide, polysulfones, polyetherketones, polyamide-imides, polyetherimides, polyetheresters, copolymers containing polyether blocks and polyamide blocks (PEBA or polyether block amides), grafted or non-grafted thermoplastic polyolefins. , functionalized or non-functionalized ethylene / vinyl monomer polymers, functionalized or non-functionalized ethylene / (meth) acrylate alkyl esters, functionalized or non-functionalized (meth) acrylic polymers, functionalized or non-functionalized ethylene / vinyl monomer / (meth) acrylate alkyl ester terpolymers, ethylene / vinyl monomer / carbonyl terpolymers, ethylene / (meth) acrylate alkyl ester / carbonyl terpolymers, methyl methacrylate-butadiene-styrene (MBS) core-shell polymers, polystyrene-block-polybutadiene-block-poly(methyl methacrylate) (SBM) block terpolymers, chlorinated or chlorosulfonated polyethylene, polyvinylidene fluoride (PVDF), phenolic resins, poly(ethylene / vinyl acetate), polybutadiene, polyisoprene, styrenic block copolymers, polyacrylonitrile, silicones, and the like, and any combination thereof. Copolymers comprising one or more of the foregoing substances may also be used in the methods and systems of the present disclosure.
[0088] Other thermoplastic polymers in the compositions and methods of the present disclosure may be elastomeric or non-elastomeric. Some of the foregoing examples of other thermoplastic polymers may be elastomeric or non-elastomeric, depending on the exact composition of the polymer. For example, polyethylene, which is a copolymer of ethylene and propylene, may be elastomeric and independent of the amount of propylene in the polymer.
[0089] Thermoplastic elastomers generally belong to one of six categories: styrenic block copolymers, thermoplastic polyolefin elastomers, thermoplastic vulcanizates (also called elastomer alloys), thermoplastic polyurethanes, thermoplastic copolyesters, and thermoplastic polyamides (generally block copolymers containing polyamides). Examples of thermoplastic elastomers can be found in the following literature: Handbook of Thermoplastic Elastomers, 2nd edition, edited by BMW Walker and CP Rader, Van Nostrand Reinhold, New York, 1988. Examples of thermoplastic elastomers include, but are not limited to, elastomeric polyamides, polyurethanes, copolymers containing polyether blocks and polyamide blocks (PEBA or polyether block amides), methyl methacrylate-butadiene-styrene (MBS) type core-shell polymers, polystyrene-block-polybutadiene-block-poly(methyl methacrylate) (SBM) block terpolymers, polybutadiene, polyisoprene, styrenic block copolymers and polyacrylonitrile, silicones, and the like. The elastic styrenic block copolymer may include at least one block selected from the group consisting of isoprene, isobutylene, butene, ethylene / butylene, ethylene-propylene, and ethylene-ethylene / propylene. More specific examples of elastic styrenic block copolymers include, but are not limited to, poly(styrene-ethylene / butylene), poly(styrene-ethylene / butylene-styrene), poly(styrene-ethylene / propylene), poly(styrene-ethylene / propylene-styrene), poly(styrene-ethylene / propylene-styrene-ethylene-propylene), poly(styrene-butadiene-styrene), poly(styrene-butylene-butadiene-styrene), and the like, and any combination thereof.
[0090] Examples of polyamides include, but are not limited to, those described above.Examples of polyamide elastomers include, but are not limited to, polyesteramides, polyetheresteramides, polycarbonate-esteramides, and polyether-block-amide elastomers.
[0091] Examples of polyurethanes include, but are not limited to, polyether polyurethanes, polyester polyurethanes, mixed polyether and polyester polyurethanes, and the like, and any combination thereof. Examples of thermoplastic polyurethanes include, but are not limited to, poly[4,4′-methylenebis(phenyl isocyanate)-alternative-1,4-butanediol / di(propylene glycol) / polycaprolactone], 1190A (a polyether polyurethane elastomer available from BASF), 1190A10 (a polyether polyurethane elastomer available from BASF), etc. and any combination thereof.
[0092] Compatibilizers may optionally be used to improve the blending efficiency and efficacy of the PP-polyamide with one or more thermoplastic polymers.Examples of polymer compatibilizers include, but are not limited to, the compatibilizers described above.
[0093] Thermoplastic polymer 102 (comprising one or more PP-polyamides and optionally one or more other thermoplastic polymers) may have a melting point or softening temperature of about 50°C to about 450°C (or about 50°C to about 125°C, or about 100°C to about 175°C, or about 150°C to about 280°C, or about 200°C to about 350°C, or about 300°C to about 450°C).
[0094] The thermoplastic polymer 102 may have a glass transition temperature (derived from ASTM E1356-08 (2014) using a 10°C / min ramp rate and cooling rate) of about -50°C to about 400°C (or about -50°C to about 0°C, or about -25°C to about 50°C, or about 0°C to about 150°C, or about 100°C to about 250°C, or about 150°C to about 300°C, or about 200°C to about 400°C).
[0095] The thermoplastic polymer 102 may optionally include an additive. Typically, the additive will be present before the thermoplastic polymer 102 is added to the mixture 110. Thus, the additive is dispersed throughout the thermoplastic polymer in the thermoplastic polymer melt droplets and the resulting thermoplastic polymer particles. Thus, for clarity, the additive is referred to herein as an "internal additive." The internal additive may be blended with the thermoplastic polymer just prior to preparing the mixture 110 or well in advance.
[0096] When describing the amounts of components in the compositions described herein (e.g., the mixture 110 and the thermoplastic polymer particles 122), internal additives are not accounted for based on the weight percentage of the thermoplastic polymer 102. For example, a composition comprising 1 wt% emulsion stabilizer is a composition comprising 0.9 g of emulsion stabilizer, 90 g of thermoplastic polymer, and 10 g of internal additive, based on the weight of 100 g of thermoplastic polymer 102 comprising 10 wt% of internal additive and 90 wt% of thermoplastic polymer.
[0097] The internal additive may be present in the thermoplastic polymer 102 at about 0.1 wt % to about 60 wt % (or about 0.1 wt % to about 5 wt %, or about 1 wt % to about 10 wt %, or about 5 wt % to about 20 wt %, or about 10 wt % to about 30 wt %, or about 25 wt % to about 50 wt %, or about 40 wt % to about 60 wt %) of the thermoplastic polymer 102. For example, the thermoplastic polymer 102 may include about 70 wt % to about 85 wt % of the thermoplastic polymer and about 15 wt % to about 30 wt % of the internal additive, such as glass fiber or carbon fiber.
[0098] Examples of internal additives include, but are not limited to, fillers, reinforcing agents, pigments, pH adjusters, and the like, and combinations thereof. Examples of fillers include, but are not limited to, glass fibers, glass particles, mineral fibers, carbon fibers, oxide particles (e.g., titanium dioxide and zirconium dioxide), metal particles (e.g., aluminum powder), and the like, and any combination thereof. Examples of pigments include, but are not limited to, organic pigments, inorganic pigments, carbon black, and the like, and any combination thereof.
[0099] Thermoplastic polymer 102 may be present in mixture 110 at about 5 wt % to about 60 wt % (or about 5 wt % to about 25 wt %, or about 10 wt % to about 30 wt %, or about 20 wt % to about 45 wt %, or about 25 wt % to about 50 wt %, or about 40 wt % to about 60 wt %) of the combined thermoplastic polymer 102 and carrier fluid 104.
[0100] Suitable carrier fluids 104 have a viscosity of about 1000 cSt to about 150,000 cSt (or about 1000 cSt to about 60,000 cSt, or about 40,000 cSt to about 100,000 cSt, or about 75,000 cSt to about 150,000 cSt) at 25°C.
[0101] Examples of the carrier fluid 104 include, but are not limited to, silicone oil, fluorinated silicone oil, perfluorinated silicone oil, polyethylene glycol, polyethylene glycol with an alkyl terminal (e.g., a C1-C4 terminal alkyl group such as tetraethylene glycol dimethyl ether (TDG)), paraffin, liquid petrolatum, vison oil, turtle oil, soybean oil, perhydrosqualene, sweet almond oil, calophyllum oil, palm oil, parleam oil, grape seed oil, sesame oil, corn oil, rapeseed oil, sunflower oil, cottonseed oil, almond oil, castor oil, avocado oil, jojoba oil, olive oil, corn germ oil, esters of lanolic acid, esters of oleic acid, esters of lauric acid, esters of stearic acid, fatty acid esters, higher fatty acids, fatty alcohols, polysiloxanes modified with fatty acids, polysiloxanes modified with fatty alcohols, polysiloxanes modified with polyoxyalkylenes, and the like, and any combination thereof. Examples of silicone oils include, but are not limited to, polydimethylsiloxane, methylphenylpolysiloxane, alkyl-modified polydimethylsiloxane, alkyl-modified methylphenylpolysiloxane, amino-modified polydimethylsiloxane, amino-modified methylphenylpolysiloxane, fluorine-modified polydimethylsiloxane, fluorine-modified methylphenylpolysiloxane, polyether-modified polydimethylsiloxane, polyether-modified methylphenylpolysiloxane, and the like, and any combination thereof. The carrier fluid 104 may have one or more phases. For example, a polysiloxane modified with a fatty acid and a polysiloxane modified with a fatty alcohol (preferably the fatty acid and the fatty alcohol have similar chain lengths) may form a single-phase carrier fluid 104. In another example, a carrier fluid 104 comprising a silicone oil and a polyethylene glycol terminated with an alkyl group may form a two-phase carrier fluid 104.
[0102] The carrier fluid 104 may be present in the mixture 110 at about 40 wt % to about 95 wt % (or about 75 wt % to about 95 wt %, or about 70 wt % to about 90 wt %, or about 55 wt % to about 80 wt %, or about 50 wt % to about 75 wt %, or about 40 wt % to about 60 wt %) of the combined thermoplastic polymer 102 and the carrier fluid 104.
[0103] In some cases, carrier fluid 104 may have a relative humidity of about 0.6 g / cm 3 To about 1.5g / cm 3 The thermoplastic polymer 102 has a density of about 0.7 g / cm 3 To about 1.7g / cm 3 wherein the thermoplastic polymer has a similar, lower or higher density than the density of the carrier fluid.
[0104] Emulsion stabilizers used in the methods and compositions of the present disclosure may include nanoparticles (eg, oxide nanoparticles, carbon black, polymer nanoparticles, and combinations thereof), surfactants, and the like, and any combination thereof.
[0105] Oxide nanoparticles can be metal oxide nanoparticles, non-metal oxide nanoparticles or their mixtures. Examples of oxide nanoparticles include, but are not limited to, silicon dioxide, titanium dioxide, zirconium oxide, aluminum oxide, iron oxide, copper oxide, tin oxide, boron oxide, cerium oxide, thallium oxide, tungsten oxide, etc. and any combination thereof. Mixed metal oxides and / or non-metal oxides such as aluminosilicates, borosilicates and aluminoborosilicates are also included in the term metal oxide. Oxide nanoparticles can be hydrophilic or hydrophobic, which may be natural to the particles or the result of surface treatment of the particles. For example, silicon dioxide nanoparticles with hydrophobic surface treatment (such as dimethylsilyl, trimethylsilyl, etc.) can be used in the methods and compositions of the present invention. In addition, silicon dioxide with functional surface treatment (such as methacrylate functionality) can be used in the methods and compositions of the present invention. Non-functionalized oxide nanoparticles may also be suitable for use.
[0106] Commercially available examples of silica nanoparticles include, but are not limited to, those available from Evonik Particles (e.g. R812S (with hydrophobic modified surface and 260±30m 2 / g BET surface area of about 7nm average diameter silica nanoparticles), RX50 (with hydrophobic modified surface and 35±10m 2 / g BET surface area of about 40nm average diameter silica nanoparticles), 380 (with hydrophilic modified surface and 380±30m 2 / g of BET surface area of silica nanoparticles)) and the like and any combination thereof.
[0107] Carbon black is another type of nanoparticle that can be present as an emulsion stabilizer in the compositions and methods disclosed herein. Various grades of carbon black are familiar to those of ordinary skill in the art, and any of these grades of carbon black can be used herein. Other nanoparticles that can absorb infrared radiation can similarly be used.
[0108] Polymer nanoparticles are another type of nanoparticles that can be present in the form of emulsion stabilizers in the present disclosure. Suitable polymer nanoparticles can include one or more polymers that are thermosetting and / or crosslinked so that they do not melt when processed by melt emulsification according to the present disclosure. High molecular weight thermoplastic polymers with high melting points or decomposition points can similarly include suitable polymer nanoparticle emulsion stabilizers.
[0109] The nanoparticles can have an average diameter (D50 based on volume) of about 1 nm to about 500 nm (or about 10 nm to about 150 nm, or about 25 nm to about 100 nm, or about 100 nm to about 250 nm, or about 250 nm to about 500 nm).
[0110] Nanoparticles can have a size of about 10 m 2 / g to about 500m 2 / g(or about 10m 2 / g to about 150m 2 / g, or about 25m 2 / g to about 100m 2 / g, or about 100m 2 / g to about 250m 2 / g, or about 250m 2 / g to about 500m 2 / g) of BET surface area.
[0111] The nanoparticles can be included in the mixture 110 at a concentration of about 0.01 wt % to about 10 wt % (or about 0.01 wt % to about 1 wt %, or about 0.1 wt % to about 3 wt %, or about 1 wt % to about 5 wt %, or about 5 wt % to about 10 wt %) based on the weight of the thermoplastic polymer 102.
[0112] The surfactant may be anionic, cationic, nonionic or zwitterionic. Examples of surfactants include, but are not limited to, sodium lauryl sulfate, sorbitan oleate, poly[dimethylsiloxane-co-[3-(2-(2-hydroxyethoxy)ethoxy)propylmethylsiloxane], sodium docusate (sodium 1,4-bis(2-ethylhexyloxy)-1,4-dioxobutane-2-sulfonate), and the like, and any combination thereof. Commercially available examples of surfactants include, but are not limited to, DB-45 (sodium dodecyl diphenyl ether disulfonate, available from Pilot Chemicals), 80 (Sorbitan maleate nonionic surfactant), Surfactants (available from Stepan Company), TERGITOL TM TMN-6 (a water-soluble, nonionic surfactant available from DOW), TRITON TM X-100 (octylphenol ethoxylate, available from Sigma Aldrich), CA-520 (polyoxyethylene (5) isooctylphenyl ether, available from Sigma Aldrich), S10 (polyethylene glycol octadecyl ether, available from Sigma Aldrich), etc. and any combination thereof.
[0113] The surfactant may be included in the mixture 110 at a concentration of about 0.01 wt % to about 10 wt % (or about 0.01 wt % to about 1 wt %, or about 0.5 wt % to about 2 wt %, or about 1 wt % to about 3 wt %, or about 2 wt % to about 5 wt %, or about 5 wt % to about 10 wt %) based on the weight of the polyamide 102. Alternatively, the mixture 110 may not include (or be absent) a surfactant.
[0114] The weight ratio of nanoparticles to surfactant may be from about 1:10 to about 10:1 (or from about 1:10 to about 1:1, or from about 1:5 to about 5:1, or from about 1:1 to about 10:1).
[0115] As described above, the components 102, 104, and 106 may be added in any order and include mixing and / or heating during the process of combining the components 102, 104, and 106 at 108. For example, the emulsion stabilizer 106 may be dispersed in the carrier fluid 104 prior to adding the thermoplastic polymer 102, and the dispersion may be optionally heated. In another non-limiting example, the thermoplastic polymer 102 may be heated to produce a polymer melt, to which the carrier fluid 104 and the emulsion stabilizer 106 are added together or in any order. In yet another non-limiting example, the thermoplastic polymer 102 and the carrier fluid 104 may be mixed at a temperature greater than the melting point or softening temperature of the thermoplastic polymer 102 and at a sufficient shear rate to disperse the thermoplastic polymer melt in the carrier fluid 104. The emulsion stabilizer 106 may then be added to form a mixture 110 and maintained under suitable processing conditions for a set period of time.
[0116] The components 102, 104, and 106 may be combined at 108 in any combination in a mixing device and / or another suitable container for processing 112. As a non-limiting example, the thermoplastic polymer 102 may be heated to a temperature greater than the melting point or softening temperature of the thermoplastic polymer 102 in a mixing device for processing 112, and the emulsion stabilizer 106 may be dispersed in the carrier fluid 104 in another container. The dispersion may then be added to the melt of the thermoplastic polymer 102 in the mixing device for processing 112.
[0117] The mixing apparatus used for processing 112 to produce molten emulsion 114 should be capable of maintaining molten emulsion 114 at a temperature greater than the melting point or softening temperature of thermoplastic polymer 102 and applying sufficient shear rate to disperse the polymer melt in the carrier fluid 104 in the form of droplets.
[0118] Examples of mixing devices for use in processing 112 to produce molten emulsion 114 include, but are not limited to, extruders (e.g., continuous extruders, batch extruders, etc.), stirred reactors, mixers, reactors with in-line homogenizer systems, and the like, and devices derived therefrom.
[0119] The molten emulsion 114 is processed 112 and formed under suitable processing conditions (eg, temperature, shear rate, etc.) for a set period of time.
[0120] The temperature of processing 112 and forming molten emulsion 114 should be a temperature greater than the melting point or softening temperature of thermoplastic polymer 102 and less than the decomposition temperature of any component 102, 104, and 106 in mixture 110. For example, the temperature of processing 112 and forming molten emulsion 114 can be about 1°C to about 50°C (or about 1°C to about 25°C, or about 5°C to about 30°C, or about 20°C to about 50°C) greater than the melting point or softening temperature of thermoplastic polymer 102, provided that the temperature of processing 112 and forming molten emulsion 114 is less than the decomposition temperature of any component 102, 104, and 106 in mixture 110.
[0121] The shear rate of processing 112 and forming molten emulsion 114 should be high enough to disperse the polymer melt in the form of droplets in carrier fluid 104. The droplets should include droplets having a diameter of about 1000 μm or less (or about 1 μm to about 1000 μm, or about 1 μm to about 50 μm, or about 10 μm to about 100 μm, or about 10 μm to about 250 μm, or about 50 μm to about 500 μm, or about 250 μm to about 750 μm, or about 500 μm to about 1000 μm).
[0122] The time for maintaining the temperature and shear rate for processing 112 and forming molten emulsion 114 can be from 10 seconds to 18 hours or longer (or 10 seconds to 30 minutes, or 5 minutes to 1 hour, or 15 minutes to 2 hours, or 1 hour to 6 hours, or 3 hours to 18 hours). Without being limited by theory, it is believed that a steady state of droplet size will be reached, at which time processing 112 can be stopped. This time can also depend on the temperature, shear rate, thermoplastic polymer 102 composition, carrier fluid 104 composition, and emulsion stabilizer 106 composition, among other things.
[0123] The molten emulsion 114 may then be cooled at 116. Cooling 116 may range from slow (e.g., allowing the molten emulsion to cool under ambient conditions) to fast (e.g., quenching). For example, the cooling rate may range from about 10°C / hour to about 100°C / second to almost instantaneous when quenching (e.g., in dry ice) (or about 10°C / hour to about 60°C / hour, or about 0.5°C / minute to about 20°C / minute, or about 1°C / minute to about 5°C / minute, or about 10°C / minute to about 60°C / minute, or about 0.5°C / second to about 10°C / second, or about 10°C / second to about 100°C / second).
[0124] During cooling, little or no shear may be applied to the molten emulsion 114. In some cases, the shear applied during heating may also be applied during cooling.
[0125] The cooled mixture 118 resulting from cooling 116 the molten emulsion 114 comprises solidified thermoplastic polymer particles 122 (or simply thermoplastic polymer particles) and other components 124 (e.g., carrier fluid 104, excess emulsion stabilizer 106, etc.). The thermoplastic polymer particles may be dispersed in the carrier fluid or settled in the carrier fluid.
[0126] The cooled mixture 118 may then be processed at 120 to separate the thermoplastic polymer particles 122 (or simply thermoplastic polymer particles 122) from other components 124. Suitable processing includes, but is not limited to, washing, filtering, centrifuging, decanting, and the like, and any combination thereof.
[0127] The solvent used to wash the thermoplastic polymer particles 122 should generally be (a) miscible with the carrier fluid 104 and (b) non-reactive with (e.g., non-swelling and non-dissolving) the thermoplastic polymer 102. The choice of solvent will depend on, among other things, the composition of the carrier fluid and the composition of the thermoplastic polymer 102.
[0128] Examples of solvents include, but are not limited to, hydrocarbon solvents (e.g., pentane, hexane, heptane, octane, cyclohexane, cyclopentane, decane, dodecane, tridecane and tetradecane), aromatic hydrocarbon solvents (e.g., benzene, toluene, xylene, 2-methylnaphthalene and cresol), ether solvents (e.g., diethyl ether, tetrahydrofuran, diisopropyl ether and dioxane), ketone solvents (e.g., acetone and methyl ethyl ketone), alcohol solvents (e.g., methanol, ethanol, isopropanol and n-propanol), ester solvents (e.g., ethyl acetate, methyl acetate, butyl acetate, butyl propionate and butyl butyrate), halogenated solvents (e.g., chloroform, bromoform, 1,2-dichloromethane, 1,2-dichloroethane, carbon tetrachloride, chlorobenzene and hexafluoroisopropanol), water, the like and any combination thereof.
[0129] The solvent may be removed from the thermoplastic polymer particles 122 by drying using an appropriate method such as air drying, heat drying, reduced pressure drying, freeze drying, or a mixture thereof. Heating may preferably be performed at a temperature below the glass transition point of the thermoplastic polymer (e.g., about 50°C to about 150°C).
[0130] The thermoplastic polymer particles 122 separated from the other components 124 may optionally be further classified to prepare purified thermoplastic polymer particles 128. For example, in order to narrow the particle size distribution (or reduce the diameter span), the thermoplastic polymer particles 122 may be passed through a sieve having a pore size of about 10 μm to about 250 μm (or about 10 μm to about 100 μm, or about 50 μm to about 200 μm, or about 150 μm to about 250 μm).
[0131] In another exemplary purification technique, the thermoplastic polymer particles 122 may be washed with water to remove the surfactant while retaining substantially all of the nanoparticles associated with the surface of the thermoplastic polymer particles 122. In yet another exemplary purification technique, the thermoplastic polymer particles 122 may be blended with additives to achieve a desired final product. For clarity, such additives are referred to herein as "external additives" because they are blended with the thermoplastic particles 122 or other particles obtained by the methods described herein after the particles have solidified. Examples of external additives include glidants, other polymer particles, fillers, and the like, and any combination thereof.
[0132] In some cases, the surfactant used to prepare the thermoplastic polymer particles 122 may be undesirable in downstream applications. Thus, yet another exemplary purification technique may include at least substantially removing the surfactant from the thermoplastic polymer particles 122 (eg, by washing and / or pyrolysis).
[0133] Thermoplastic polymer particles 122 and / or purified thermoplastic polymer particles 128 (referred to as particles 122 / 128 ) can be characterized by composition, physical structure, and the like.
[0134] As described above, the emulsion stabilizer is at the interface between the polymer melt and the carrier fluid. Thus, when the mixture is cooled, the emulsion stabilizer remains at or near the interface. Thus, the structure of the particles 122 / 128 typically includes an emulsion stabilizer that is (a) dispersed on the outer surface of the particles 122 / 128 and / or (b) embedded in the outer portion (e.g., the outer 1 volume %) of the particles 122 / 128.
[0135] In addition, in the case where voids are formed inside the polymer melt droplets, the emulsion stabilizer 106 should generally be at the interface between the interior of the void and the thermoplastic polymer (and / or embedded in the interface). The void generally does not contain a thermoplastic polymer. Instead, the void may contain, for example, a carrier fluid, air, or be empty. The particles 122 / 128 may contain a carrier fluid at about 5% by weight or less (or about 0.001% by weight to about 5% by weight, or about 0.001% by weight to about 0.1% by weight, or about 0.01% by weight to about 0.5% by weight, or about 0.1% by weight to about 2% by weight, or about 1% by weight to about 5% by weight) of the particles 122 / 128.
[0136] Thermoplastic polymer 102 may be present in particle 122 / 128 at about 90% to about 99.5% by weight (or about 90% to about 95% by weight, or about 92% to about 97% by weight, or about 95% to about 99.5% by weight) of particle 122 / 128.
[0137] When included, the emulsion stabilizer 106 may be present in the particles 122 / 128 at about 10% by weight or less (or about 0.01% by weight to about 10% by weight, or about 0.01% by weight to about 1% by weight, or about 0.5% by weight to about 5% by weight, or about 3% by weight to about 7% by weight, or about 5% by weight to about 10% by weight) of the particles 122 / 128. When purified to at least substantially remove a surfactant or another emulsion stabilizer, the emulsion stabilizer 106 may be present in the particles 128 at less than 0.01% by weight (or 0% by weight to about 0.01% by weight, or 0% by weight to 0.001% by weight).
[0138] After forming thermoplastic microparticles according to the disclosure herein, at least a portion of nanoparticles (such as silica nanoparticles) can be disposed on the outer surface of the thermoplastic microparticles in the form of a coating. At least a portion of the surfactant (if used) can also be associated with the outer surface. The coating can be substantially uniformly disposed on the outer surface. As used herein with respect to the coating, the term "substantially uniform" refers to a uniform coating thickness in the surface position (particularly the entire outer surface) covered by the coating composition (e.g., nanoparticles and / or surfactant). The emulsion stabilizer 106 can form a coating covering at least 5% (or about 5% to about 100%, or about 5% to about 25%, or about 20% to about 50%, or about 40% to about 70%, or about 50% to about 80%, or about 60% to about 90%, or about 70% to about 100%) of the surface area of the particles 122 / 128. When purified to at least substantially remove a surfactant or another emulsion stabilizer, the emulsion stabilizer 106 may be present in the particle 128 at less than 25% (or 0% to about 25%, or about 0.1% to about 5%, or about 0.1% to about 1%, or about 1% to about 5%, or about 1% to about 10%, or about 5% to about 15%, or about 10% to about 25%) of the surface area of the particle 128. Image analysis of scanning electron microscope images (SEM micrographs) may be used to determine the coverage of the emulsion stabilizer 106 on the outer surface of the particle 122 / 128. The emulsion stabilizer 106 may form a coating covering at least 5% (or about 5% to about 100%, or about 5% to about 25%, or about 20% to about 50%, or about 40% to about 70%, or about 50% to about 80%, or about 60% to about 90%, or about 70% to about 100%) of the surface area of the particle 122 / 128. When purified to at least substantially remove a surfactant or another emulsion stabilizer, the emulsion stabilizer 106 may be present in the particles 128 at less than 25% (or 0% to about 25%, or about 0.1% to about 5%, or about 0.1% to about 1%, or about 1% to about 5%, or about 1% to about 10%, or about 5% to about 15%, or about 10% to about 25%) of the surface area of the particles 128. Image analysis of SEM micrographs may be used to determine the coverage of the emulsion stabilizer 106 on the exterior surfaces of the particles 122 / 128.
[0139] The particles 122 / 128 can have a D10 of about 0.1 μm to about 125 μm (or about 0.1 μm to about 5 μm, about 1 μm to about 10 μm, about 5 μm to about 30 μm, or about 1 μm to about 25 μm, or about 25 μm to about 75 μm, or about 50 μm to about 85 μm, or about 75 μm to about 125 μm), a D50 of about 0.5 μm to about 200 μm (or about 0.5 μm to about 10 μm, or about 5 μm to about 50 μm, or about 30 μm to about 100 μm, or about 30 μm to about 70 μm, or about 25 μm to about 50 μm, or about 50 μm to about 100 μm, or about 75 μm to about 150 μm, or about 100 μm to about 200 μm), and a D90 of about 3 μm to about 300 μm (or about 3 μm to about 15 μm, or about 10 μm to about 50 μm, or about 25 μm to about 75 μm, or about 70 μm to about 200 μm, or about 60 μm to about 150 μm, or about 150 μm to about 300 μm), where D10 < D50 < D90. The particles 122 / 128 can also have a diameter span of about 0.2 to about 10 (or about 0.2 to about 0.5, or about 0.4 to about 0.8, or about 0.5 to about 1.0, or about 1 to about 3, or about 2 to about 5, or about 5 to about 10). Without limitation, a diameter span value of 1.0 or greater is considered wide, and a diameter span value of 0.75 or less is considered narrow. Without limitation, a diameter span value of 1.0 or greater is considered wide, and a diameter span value of 0.75 or less is considered narrow.
[0140] In a first non - limiting example, the particles 122 / 128 can have a D10 of about 0.1 μm to about 10 μm, a D50 of about 0.5 μm to about 25 μm, and a D90 of about 3 μm to about 50 μm, where D10 < D50 < D90. The particles 122 / 128 can have a diameter span of about 0.2 to about 2.
[0141] In a second non - limiting example, the particles 122 / 128 can have a D10 of about 5 μm to about 30 μm, a D50 of about 30 μm to about 70 μm, and a D90 of about 70 μm to about 120 μm, where D10 < D50 < D90. The particles 122 / 128 can have a diameter span of about 1.0 to about 2.5.
[0142] In a third non - limiting example, the particles 122 / 128 can have a D10 of about 25 μm to about 60 μm, a D50 of about 60 μm to about 110 μm, and a D90 of about 110 μm to about 175 μm, where D10 < D50 < D90. The particles 122 / 128 can have a diameter span of about 0.6 to about 1.5.
[0143] In a fourth non-limiting example, the particles 122 / 128 may have a D10 of from about 75 μm to about 125 μm, a D50 of from about 100 μm to about 200 μm, and a D90 of from about 125 μm to about 300 μm, where D10 < D50 < D90. The particles 122 / 128 may have a diameter span of from about 0.2 to about 1.2.
[0144] In a fifth non-limiting example, the particles 122 / 128 may have a D10 of from about 1 μm to about 50 μm (or from about 5 μm to about 30 μm, or from about 1 μm to about 25 μm, or from about 25 μm to about 50 μm), a D50 of from about 25 μm to about 100 μm (or from about 30 μm to about 100 μm, or from about 30 μm to about 70 μm, or from about 25 μm to about 50 μm, or from about 50 μm to about 100 μm), and a D90 of from about 60 μm to about 300 μm (or from about 70 μm to about 200 μm, or from about 60 μm to about 150 μm, or from about 150 μm to about 300 μm), where D10 < D50 < D90. The particles 122 / 128 may also have a diameter span of from about 0.4 to about 3 (or from about 0.6 to about 2, or from about 0.4 to about 1.5, or from about 1 to about 3).
[0145] The particles 122 / 128 may have a roundness of about 0.9 or greater (or from about 0.90 to about 1.0, or from about 0.93 to about 0.99, or from about 0.95 to about 0.99, or from about 0.97 to about 0.99, or from about 0.98 to 1.0).
[0146] The particles 122 / 128 may have an angle of repose of from about 25° to about 45° (or from about 25° to about 35°, or from about 30° to about 40°, or from about 35° to about 45°).
[0147] The particles 122 / 128 may have a Hausner ratio of from about 1.0 to about 1.5 (or from about 1.0 to about 1.2, or from about 1.1 to about 1.3, or from about 1.2 to about 1.35, or from about 1.3 to about 1.5).
[0148] The particles 122 / 128 may have a bulk density of from about 0.3 g / cm 3 to about 0.8 g / cm 3 (or from about 0.3 g / cm 3 to about 0.6 g / cm 3 , or from about 0.4 g / cm 3 to about 0.7 g / cm 3 , or from about 0.5 g / cm 3 to about 0.6 g / cm 3 , or from about 0.5 g / cm 3 to about 0.8 g / cm 3 ).
[0149] Depending on the temperature and shear rate of processing 112 and the composition and relative concentration of components 102, 104 and 106, different shapes of structures constituting particles 122 / 128 have been observed. Typically, particles 122 / 128 include substantially spherical particles (having a roundness of about 0.97 or greater). However, other structures have been observed in particles 122 / 128, including discs and elongated structures. Therefore, particles 122 / 128 may include one or more of the following: (a) substantially spherical particles with a roundness of 0.97 or greater, (b) disc structures with an aspect ratio of about 2 to about 10, and (c) elongated structures with an aspect ratio of 10 or greater. Each of the (a), (b) and (c) structures has an emulsion stabilizer dispersed on the outer surface of the (a), (b) and (c) structures and / or embedded in the exterior of the (a), (b) and (c) structures. At least some of the (a), (b) and (c) structures may be agglomerated. For example, (c) elongated structures may be laid on the surface of (a) substantially spherical particles.
[0150] The particles 122 / 128 may have a sintering window within 10°C, preferably within 5°C, of the sintering window of the thermoplastic polymer 102 (comprising one or more PP-polyamides and optionally one or more other thermoplastic polymers).
[0151] 3D Printing
[0152] The particles comprising PP-polyamide described herein can be used in a variety of applications, including 3D printing. The 3D printing process of the present disclosure may include: depositing the PP-polyamide of the present disclosure (e.g., particles comprising one or more PP polyamides and optionally one or more other thermoplastic polymers) onto a surface in a specified shape, and once deposited, heating at least a portion of the particles to promote consolidation thereof and form a consolidated body (article), so that the consolidated body has a void percentage of about 1% or less after consolidation. For example, the heating and consolidation of the thermoplastic polymer particles can be performed in a 3D printing device using a laser, so that the heating and consolidation are performed by selective laser sintering.
[0153] Examples of items that can be 3D printed using the thermoplastic polymer particles of the present disclosure include, but are not limited to, containers (e.g., for food, beverages, cosmetics, personal care compositions, pharmaceuticals, etc.), shoe soles, toys, furniture parts and decorative household items, plastic gears, screws, nuts, bolts, cable ties, automotive parts, medical supplies, prostheses, orthopedic implants, aviation / aircraft related parts, preparation of artifacts to aid learning in education, 3D anatomical models to assist surgery, robots, biomedical devices (orthotics), household appliances, dentistry, electronic devices, sporting goods, etc.
[0154] Other applications for particles comprising one or more of the disclosed PP-polyamides may include, but are not limited to, use as fillers in paints and powder coatings, inkjet materials, and electrophotographic toners, among others.
[0155] Example Implementation
[0156] The method of the first non-limiting exemplary embodiment includes: functionalizing metal oxide particles bonded to pigment particles with a compound having epoxy groups (terminal, pendant, or both terminal and pendant including such groups) to produce a surface-treated pigment having pendant epoxy groups; and reacting the pendant epoxy groups with a polyamide to produce a pigment pendant polyamide (PP-polyamide). The first non-limiting exemplary embodiment may also include one or more of the following: Element 1: wherein the compound having an epoxide is selected from: (3-glycidyloxypropyl)trimethoxysilane, (3-glycidyloxypropyl)triethoxysilane, diethoxy(3-glycidyloxypropyl)methylsilane and 1,3-bis(3-glycidyloxypropyl)tetramethylsiloxane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidyloxypropylmethyldimethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, 5,6-epoxyhexyltriethoxysilane and any combination thereof; Element 2: wherein the metal oxide particles comprise one or more selected from: titanium dioxide, sub-valent titanium oxide, titanium oxynitride, Al 2 O 3 , Fe 2 O 3 , Fe 3 O 4 SnO 2 Cr 2 O 3 , ZnO, CuO, NiO, zirconium oxide and titanium iron oxide; Element 3: wherein the pigment particles contain one or more selected from the following: synthetic mica, natural mica, talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments, CaSO 4, iron oxide, chromium oxide, carbon black, metallic effect pigments, optically variable pigments, liquid crystal polymer pigments and holographic pigments; Element 4: wherein the polyamide is selected from: polycaprolactam, poly(hexamethylene succinamide), polyhexamethylene adipamide, polypentamethylene adipamide, polyhexamethylene sebacamide, polyundecanamide, polydodecaneamide, polyhexamethylene terephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semi-aromatic polyamide, aromatic polyamide, any copolymers thereof and any combination thereof; Element 5: wherein the reaction of the side chain epoxy group with the polyamide is carried out at about 70°C to about 200°C; and Element 6: wherein the weight ratio of the pigment to the polyamide is about 1:10 to about 1:1000. Examples of combinations include, but are not limited to, a combination of element 1 with one or more of elements 2 to 6; a combination of element 2 with one or more of elements 3 to 6; a combination of element 3 with one or more of elements 4 to 6; and a combination of two or more of elements 4 to 6.
[0157] The second non-limiting exemplary embodiment is a PP-polyamide prepared according to the method of the first non-limiting exemplary embodiment (optionally including one or more of elements 1 to 6).
[0158] The method of the third non-limiting exemplary embodiment includes: functionalizing the metal oxide particles bonded to the pigment particles with silica particles having a surface treatment with carboxylic acid (terminally, pendantly, or both terminally and pendantly comprising such groups) to produce a surface treated pigment having pendant carboxylic acid; converting the pendant carboxylic acid into a pendant acid chloride; and reacting the pendant acid chloride with a polyamide to produce a pigment pendant polyamide (PP-polyamide). The third non-limiting exemplary embodiment may also include one or more of the following: Element 7: wherein the metal oxide particles comprise one or more selected from the group consisting of titanium dioxide, titanium suboxide, titanium oxynitride, Al 2 O 3 , Fe 2 O 3 , Fe 3 O 4 SnO 2 Cr 2 O 3 , ZnO, CuO, NiO, zirconium oxide and titanium iron oxide; Element 8: wherein the pigment particles contain one or more selected from the following: synthetic mica, natural mica, talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments, CaSO 4, iron oxide, chromium oxide, carbon black, metal effect pigments, optically variable pigments, liquid crystal polymer pigments and holographic pigments; Element 9: wherein the silica particles having a carboxylic acid surface treatment comprise one or more selected from the following: 3-aminopropyl-(3-oxobutyric acid) functionalized silica, 3-propylsulfonic acid functionalized silica, propylcarboxylic acid functionalized silica, triaminetetraacetic acid functionalized silica, propionyl chloride functionalized silica, 3-carboxypropyl functionalized silica, aminomethylphosphonic acid (AMPA) functionalized silica and 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid (DOTA) functionalized silica; Element 10: wherein the polyamide is selected from the group consisting of polycaprolactam, poly(succinyl adipate); amine), polyhexamethylene adipamide, polypentamethylene adipamide, polyhexamethylene sebacamide, polyundecanamide, polydodecaneamide, polyhexamethylene terephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semi-aromatic polyamide, aromatic polyamide, any copolymers thereof, and any combination thereof; Element 11: wherein the reaction of the side chain acid chloride with the polyamide comprises melt mixing the pigment particles having side chain acid chloride functional groups with the polyamide at about 125° C. to about 250° C. for 15 minutes to about 1 hour; and Element 12: wherein the weight ratio of the pigment to the polyamide is about 1:10 to about 1:1000. Examples of combinations include, but are not limited to, a combination of element 7 with one or more of elements 8 to 12; a combination of element 8 with one or more of elements 9 to 12; a combination of element 9 with one or more of elements 10 to 12; and a combination of two or more of elements 10 to 12.
[0159] The fourth non-limiting exemplary embodiment is a PP-polyamide prepared according to the method of the third non-limiting exemplary embodiment (optionally including one or more of elements 7 to 12).
[0160] A composition of a fifth non-limiting exemplary embodiment comprises: a polyamide having a pigment pendant from a backbone of the polyamide, wherein the pigment comprises metal oxide particles on surfaces of the pigment particles. The third non-limiting exemplary embodiment may also include one or more of the following: Element 13: wherein the polyamide is selected from the group consisting of polycaprolactam, poly(hexamethylene succinamide), polyhexamethylene adipamide, polypentamethylene adipamide, polyhexamethylene sebacamide, polyundecanamide, polydodecaneamide, polyhexamethylene terephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semi-aromatic polyamide, aromatic polyamide, any copolymers thereof, and any combination thereof; Element 14: wherein the weight ratio of the pigment to the polyamide is from about 1:10 to about 1:1000; and Element 15: wherein the pigment particles comprise one or more selected from the group consisting of synthetic mica, natural mica, talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments, CaSO 4 , iron oxide, chromium oxide, carbon black, metallic effect pigments, optically variable pigments, liquid crystal polymer pigments and holographic pigments.
[0161] The sixth non-limiting exemplary embodiment is an article comprising the composition of the fifth non-limiting exemplary embodiment (optionally including one or more of elements 13 to 15), which composition can be produced from the first non-limiting exemplary embodiment or the third non-limiting exemplary embodiment.
[0162] The method of the seventh non-limiting exemplary embodiment comprises: depositing particles in a specified shape on a surface, and once deposited, wherein the particles comprise the composition of the fifth non-limiting exemplary embodiment (optionally including one or more of elements 13 to 15); and heating at least a portion of the particles to promote their consolidation and form a consolidated body. In addition, the particles of the seventh non-limiting exemplary embodiment may also include a thermoplastic polymer selected from the group consisting of polyurethane, polyethylene, polypropylene, polyacetal, polycarbonate, polybutylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, polytrimethylene terephthalate, polyhexamethylene terephthalate, polystyrene, polyvinyl chloride, polytetrafluoroethylene, polyester, polyether, polyethersulfone, polyetheretherketone, polyacrylate, polymethacrylate, polyimide, acrylonitrile butadiene styrene, polyphenylene sulfide, vinyl polymer, polyarylether, polyarylene sulfide, polysulfone, polyetherketone, polyamide-imide, polyetherimide, polyetherester, copolymers comprising polyether blocks and polyamide blocks, grafted or non-grafted thermoplastic polyolefins, functionalized or non-functionalized Ethylene / vinyl monomer polymers, functionalized or non-functionalized ethylene / alkyl (meth)acrylate, functionalized or non-functionalized (meth)acrylic acid polymers, functionalized or non-functionalized ethylene / vinyl monomer / alkyl (meth)acrylate terpolymers, ethylene / vinyl monomer / carbonyl terpolymers, ethylene / alkyl (meth)acrylate / carbonyl terpolymers, methyl methacrylate-butadiene-styrene type core-shell polymers, polystyrene-block-polybutadiene-block-poly(methyl methacrylate) block terpolymers, chlorinated or chlorosulfonated polyethylene, polyvinylidene fluoride), phenolic resins, poly(ethylene / vinyl acetate), polybutadiene, polyisoprene, styrene-based block copolymers, polyacrylonitrile, silicones, and any combination thereof.
[0163] The method of an eighth non-limiting exemplary embodiment comprises: mixing a mixture comprising a polyamide having a pigment pendant from a backbone of the polyamide (PP-polyamide), a carrier fluid immiscible with the PP-polyamide, and an optional emulsion stabilizer at a temperature greater than the melting point or softening temperature of the PP-polyamide and at a shear rate high enough to disperse the PP-polyamide in the carrier fluid; and cooling the mixture to below the melting point or softening temperature of the PP-polyamide to form solidified particles comprising the PP-polyamide and, when present, the emulsion stabilizer associated with the outer surfaces of the solidified particles.
[0164] The composition of a ninth non-limiting exemplary embodiment comprises: coagulated particles comprising a polyamide (PP-polyamide) having a pigment pendant from the backbone of the polyamide and having a roundness of about 0.90 to about 1.0.
[0165] The eighth exemplary embodiment and the ninth exemplary embodiment may include one or more of the following: Element 16: wherein an emulsion stabilizer is included in the mixture (or wherein the solidified particles also include an emulsion stabilizer), and wherein the emulsion stabilizer is associated with the outer surface of the solidified particles; Element 17: Element 16 and wherein at least some of the solidified particles have voids that contain the emulsion stabilizer at the void / thermoplastic polymer interface; Element 18: Element 17 and wherein the voids contain a carrier fluid; Element 19: Element 17 and wherein the emulsion stabilizer includes nanoparticles and the nanoparticles are embedded in the void / polymer interface; Element 20: Element 16 and wherein the solidified particles further include elongated structures on the surface of the solidified particles, wherein the elongated structures comprise PP-polyamide and the emulsion stabilizer is associated with the outer surface of the elongated structures; Element 21: Element 16 and wherein the emulsion stabilizer forms a coating that covers less than 5% of the surface of the solidified particles; Element 22: Element 16 and wherein the emulsion stabilizer forms a coating that covers at least 5% of the surface of the solidified particles; Element 23: Element 16 and wherein the emulsion stabilizer forms a coating that covers at least 25% of the surface of the solidified particles; Element 24: Element 16 and wherein the emulsion The stabilizer forms a coating that covers at least 50% of the surface of the solidified particles; Element 25: Element 16 and wherein the emulsion stabilizer is present in the mixture (or solidified particles) at 0.05 wt % to 5 wt % based on the weight of the PP-polyamide; Element 26: Element 16 and wherein the emulsion stabilizer comprises nanoparticles and the nanoparticles have an average diameter of 1 nm to 500 nm; Element 27: Element 16 and wherein the emulsion stabilizer comprises nanoparticles and the nanoparticles comprise oxide nanoparticles; Element 28: Element 16 and wherein the emulsion stabilizer comprises nanoparticles and the nanoparticles comprise carbon nanoparticles. black; Element 29: Element 16 and wherein the emulsion stabilizer comprises nanoparticles, and the nanoparticles comprise polymer nanoparticles; Element 30: wherein the mixture further comprises a thermoplastic polymer that is not PP-polyamide (or wherein the solidified particles further comprise a thermoplastic polymer that is not PP-polyamide); Element 31: wherein the mixture further comprises a polyamide of PP-polyamide but without a pigment pendant therefrom (or wherein the solidified particles further comprise a polyamide of PP-polyamide but without a pigment pendant therefrom); Element 32: wherein the pigment is selected from the group consisting of: synthetic mica, natural mica, talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments, CaSO 4, iron oxide, chromium oxide, carbon black, metallic effect pigments, optically variable pigments, liquid crystal polymer pigments, holographic pigments, and any combination thereof; Element 33: wherein the polyamide is selected from: polycaprolactam, poly(butylene succinyl adipamide), polyhexamethylene adipamide, polypentamethylene hexanediamide, polydecamethylene adipamide, polyundecanamide, polydodecanamide, polyhexamethylene terephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semi-aromatic polyamides, aromatic polyamides, any copolymers thereof, and any combination thereof; Element 34: wherein the weight ratio of the pigment to the polyamide is from about 1:10 to about 1:1000; Element 35: wherein the solidified particles have a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, and a D90 of about 3 μm to about 300 μm, where D10 < D50 < D90; Element 36: wherein the solidified particles have a diameter span of about 0.2 to about 10; Element 37: wherein the solidified particles have a D10 of about 5 μm to about 30 μm, a D50 of about 30 μm to about 70 μm, and a D90 of about 70 μm to about 120 μm, where D10 < D50 < D90; Element 38: Element 37 and wherein the solidified particles have a diameter span of about 1.0 to about 2.5; Element 39: wherein the solidified particles have a D10 of about 25 μm to about 60 μm, a D50 of about 60 μm to about 110 μm, and a D90 of about 110 μm to about 175 μm, where D10 < D50 < D90; Element 40: Element 39 and wherein the solidified particles have a diameter span of about 0.6 to about 1.5; Element 41: wherein the solidified particles have a D10 of about 75 μm to about 125 μm, a D50 of about 100 μm to about 200 μm, and a D90 of about 125 μm to about 300 μm, where D10 < D50 < D90; Element 42: Element 41 and wherein the solidified particles have a diameter span of about 0.2 to about 1.2; Element 43: wherein the solidified particles have a roundness of about 0.90 to about 1.0; and Element 44: wherein the solidified particles have a value from about 1.0 to about 1.5; examples of combinations include, but are not limited to, a combination of element 16 with one or more of elements 17 to 19; a combination of element 16 with one of elements 20 to 24, optionally further combined with one or more of elements 17 to 19; a combination of element 16 (optionally in combination with one of elements 20 to 24 and / or optionally in combination with one or more of elements 17 to 19) with one or more of elements 25 to 29; a combination of element 16 (optionally in combination with one or more of elements 17 to 29) with one or more of elements 30 to 44; a combination of two or more of elements 30 to 34; a combination of one or more of elements 30 to 34 with one or more of elements 35 to 44; and a combination of element 43 and / or element 44 with one or more of elements 35 to 42. .
[0166] In addition, the eighth non-limiting exemplary embodiment may also include one or more of the following: Element 45: wherein the PP-polyamide is present in the mixture at 5% to 60% by weight of the mixture; Element 46: wherein the carrier fluid is selected from the group consisting of silicone oil, fluorinated silicone oil, perfluorinated silicone oil, polyethylene glycol, paraffin, liquid petrolatum, vison oil, turtle oil, soybean oil, perhydrosqualene, sweet almond oil, calophyllum oil, palm oil, parleam oil, grape seed oil, sesame oil, corn oil, rapeseed oil, sunflower oil, cottonseed oil, almond oil, castor oil, avocado oil, jojoba oil, olive oil, cereal germ oil, lanolic acid, 47: wherein the silicone oil is selected from the group consisting of: polydimethylsiloxane, methylphenylpolysiloxane, alkyl-modified polydimethylsiloxane, alkyl-modified methylphenylpolysiloxane, amino-modified polydimethylsiloxane, amino-modified methylphenylpolysiloxane, fluorine-modified polydimethylsiloxane, fluorine-modified methylphenylpolysiloxane, polyether-modified polydimethylsiloxane, polyether-modified methylphenylpolysiloxane, and any combination thereof; Element 48: wherein the carrier fluid has a viscosity of 1000 cSt to 150,000 cSt at 25°C; and Element 49: wherein the carrier fluid has a viscosity of 0.6 g / cm 3 Up to 1.5g / cm 3 density; examples of combinations include, but are not limited to, a combination of one or more of elements 16 to 44 and one or more of elements 45 to 49; and two or more of elements 45 to 49.
[0167] Terms
[0168] Item 1. A method comprising: functionalizing metal oxide particles bonded to pigment particles with a compound having epoxy groups (terminal, pendant, or both terminal and pendant including such groups) to produce a surface-treated pigment having pendant epoxy groups; and reacting the pendant epoxy groups with a polyamide to produce a pigment pendant polyamide (PP-polyamide).
[0169] Clause 2. The method according to clause 1, wherein the compound having the epoxide is selected from: (3-glycidoxypropyl)trimethoxysilane, (3-glycidoxypropyl)triethoxysilane, diethoxy(3-glycidoxypropyl)methylsilane and 1,3-bis(3-glycidoxypropyl)tetramethylsiloxane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 5,6-epoxyhexyltriethoxysilane and any combination thereof.
[0170] Item 3. The method according to Item 1, wherein the metal oxide particles comprise one or more selected from the group consisting of titanium dioxide, titanium suboxide, titanium oxynitride, Al 2 O 3 , Fe 2 O 3 , Fe 3 O 4 SnO 2 Cr 2 O 3 , ZnO, CuO, NiO, zirconium oxide and titanium iron oxide.
[0171] Clause 4. The method according to clause 1, wherein the pigment particles comprise one or more selected from the group consisting of synthetic mica, natural mica, talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments, CaSO 4 , iron oxide, chromium oxide, carbon black, metallic effect pigments, optically variable pigments, liquid crystal polymer pigments and holographic pigments.
[0172] Clause 5. The method according to clause 1, wherein the polyamide is selected from the group consisting of polycaprolactam, poly(hexamethylene succinamide), polyhexamethylene adipamide, polypentamethylene adipamide, polyhexamethylene sebacamide, polyundecanamide, polydodecaneamide, polyhexamethylene terephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semiaromatic polyamide, aromatic polyamide, any copolymers thereof, and any combination thereof.
[0173] Clause 6. The method of Clause 1, wherein the reaction of the pendant epoxy groups with polyamide is conducted at about 70°C to about 200°C.
[0174] Clause 7. The method of Clause 1, wherein the weight ratio of the pigment to the polyamide is from about 1:10 to about 1:1000.
[0175] Item 8. A method comprising: functionalizing metal oxide particles bound to pigment particles with silica particles having a surface treatment with a carboxylic acid (terminally, pendantly, or both terminally and pendantly comprising such groups) to produce a surface-treated pigment having a pendant carboxylic acid; converting the pendant carboxylic acid into a pendant acid chloride; and reacting the pendant acid chloride with a polyamide to produce a pigment pendant polyamide (PP-polyamide).
[0176] Item 9. The method according to Item 8, wherein the metal oxide particles comprise one or more selected from the group consisting of titanium dioxide, titanium suboxide, titanium oxynitride, Al 2 O 3 , Fe 2 O 3 , Fe 3 O 4 SnO 2 Cr 2 O 3 , ZnO, CuO, NiO, zirconium oxide and titanium iron oxide.
[0177] Clause 10. The method according to clause 8, wherein the pigment particles comprise one or more selected from the group consisting of synthetic mica, natural mica, talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments, CaSO 4 , iron oxide, chromium oxide, carbon black, metallic effect pigments, optically variable pigments, liquid crystal polymer pigments and holographic pigments.
[0178] Item 11. A method according to Item 8, wherein the silica particles having the carboxylic acid surface treatment comprise one or more selected from the following: 3-aminopropyl-(3-oxobutyric acid) functionalized silica, 3-propylsulfonic acid functionalized silica, propylcarboxylic acid functionalized silica, triaminetetraacetic acid functionalized silica, propionyl chloride functionalized silica, 3-carboxypropyl functionalized silica, aminomethylphosphonic acid (AMPA) functionalized silica and 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid (DOTA) functionalized silica.
[0179] Clause 12. The method of clause 8, wherein the polyamide is selected from the group consisting of polycaprolactam, poly(hexamethylene succinamide), polyhexamethylene adipamide, polypentamethylene adipamide, polyhexamethylene sebacamide, polyundecanamide, polydodecaneamide, polyhexamethylene terephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semiaromatic polyamide, aromatic polyamide, any copolymers thereof, and any combination thereof.
[0180] Clause 13. The method of Clause 8, wherein the reacting of the pendant acid chloride with the polyamide comprises melt mixing the pigment particles having the pendant acid chloride functional groups with the polyamide at about 125°C to about 250°C for 15 minutes to about 1 hour.
[0181] Clause 14. The method of Clause 8, wherein the weight ratio of the pigment to the polyamide is from about 1:10 to about 1:1000.
[0182] Item 15. A composition comprising: a polyamide having a pigment pendant from a backbone of the polyamide, wherein the pigment comprises metal oxide particles on surfaces of the pigment particles.
[0183] Item 16. The composition of Item 15, wherein the polyamide is selected from the group consisting of polycaprolactam, poly(hexamethylene succinamide), polyhexamethylene adipamide, polypentamethylene adipamide, polyhexamethylene sebacamide, polyundecanamide, polydodecaneamide, polyhexamethylene terephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semiaromatic polyamide, aromatic polyamide, any copolymers thereof, and any combination thereof.
[0184] Clause 17. The composition of Clause 15, wherein the weight ratio of the pigment to the polyamide is from about 1:10 to about 1:1000.
[0185] Clause 18. The composition according to clause 15, wherein the pigment particles comprise one or more selected from the group consisting of synthetic mica, natural mica, talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments, CaSO 4 , iron oxide, chromium oxide, carbon black, metallic effect pigments, optically variable pigments, liquid crystal polymer pigments and holographic pigments.
[0186] Clause 19. An article comprising: the composition according to Clause 15.
[0187] Clause 20. A method comprising: depositing particles in a specified shape on a surface, and once deposited, wherein the particles comprise a polyamide according to any one of clauses 15 to 18; and heating at least a portion of the particles to promote consolidation thereof and form a consolidated body.
[0188] Item 21. The method according to Item 20, wherein the particles further comprise: polyurethane, polyethylene, polypropylene, polyacetal, polycarbonate, polybutylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, polytrimethylene terephthalate, polyhexylene terephthalate, polystyrene, polyvinyl chloride, polytetrafluoroethylene, polyester, polyether, polyethersulfone, polyetheretherketone, polyacrylate, polymethacrylate, polyimide, acrylonitrile butadiene styrene, polyphenylene sulfide, vinyl polymer, polyarylene ether, polyarylene sulfide, polysulfone, polyetherketone, polyamide-imide, polyetherimide, polyetherester, copolymers comprising polyether blocks and polyamide blocks, grafted or non-grafted thermoplastic polyolefins, functionalized or non-functionalized ethylene / Vinyl monomer polymers, functionalized or non-functionalized ethylene / alkyl (meth)acrylate, functionalized or non-functionalized (meth)acrylic polymers, functionalized or non-functionalized ethylene / vinyl monomer / alkyl (meth)acrylate terpolymers, ethylene / vinyl monomer / carbonyl terpolymers, ethylene / alkyl (meth)acrylate / carbonyl terpolymers, methyl methacrylate-butadiene-styrene core-shell polymers, polystyrene-block-polybutadiene-block-poly(methyl methacrylate) block terpolymers, chlorinated or chlorosulfonated polyethylene, polyvinylidene fluoride), phenolic resins, poly(ethylene / vinyl acetate), polybutadiene, polyisoprene, styrene block copolymers, polyacrylonitrile, silicones, and any combination thereof.
[0189] Item 22. A method comprising: mixing a mixture comprising a polyamide having a pigment pendant from the backbone of the polyamide (PP-polyamide), a carrier fluid immiscible with the PP-polyamide, and an optional emulsion stabilizer at a temperature greater than the melting point or softening temperature of the PP-polyamide and at a shear rate high enough to disperse the PP-polyamide in a carrier fluid; and cooling the mixture to below the melting point or softening temperature of the PP-polyamide to form solidified particles, the solidified particles comprising the PP-polyamide and, when present, the emulsion stabilizer associated with the outer surface of the solidified particles.
[0190] Clause 23. The method of Clause 22, wherein the emulsion stabilizer is included in the mixture, and wherein the emulsion stabilizer is associated with the outer surface of the solidified particles.
[0191] Clause 24. The method of Clause 23, wherein the emulsion stabilizer comprises nanoparticles, and wherein the nanoparticles are embedded in the outer surface of the solidified particles.
[0192] Clause 25. The method according to Clause 22, wherein the mixture further comprises a thermoplastic polymer that is not the PP-polyamide.
[0193] Clause 26. The method of Clause 22, wherein the mixture further comprises the polyamide of the PP-polyamide but without pigment pendant therefrom.
[0194] Clause 27. The method according to clause 22, wherein the pigment is selected from the group consisting of synthetic mica, natural mica, talc, sericite, kaolin, glass, SiO 2 Thin sheet, Al 2 O 3 Flakes, glass flakes, needle-shaped pigments, CaSO 4 , iron oxide, chromium oxide, carbon black, metallic effect pigments, optically variable pigments, liquid crystal polymer pigments, holographic pigments, and any combination thereof.
[0195] Clause 28. The method of clause 22, wherein the polyamide is selected from the group consisting of polycaprolactam, poly(hexamethylene succinamide), polyhexamethylene adipamide, polypentamethylene adipamide, polyhexamethylene sebacamide, polyundecanamide, polydodecaneamide, polyhexamethylene terephthalamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semiaromatic polyamide, aromatic polyamide, any copolymers thereof, and any combination thereof.
[0196] Clause 29. The method of Clause 22, wherein the weight ratio of the pigment to the polyamide is from about 1:10 to about 1:1000.
[0197] Clause 30. The method of Clause 22, wherein at least some of the solidified particles have voids comprising the emulsion stabilizer at a void / polymer interface.
[0198] Clause 31. The method of Clause 30, wherein the emulsion stabilizer comprises nanoparticles and the nanoparticles are embedded in the void / polymer interface.
[0199] Clause 32. The method of Clause 30, wherein the void contains the carrier fluid.
[0200] Clause 33. The method of Clause 22, wherein the solidified particles further comprise elongated structures on the surface of the solidified particles, wherein the elongated structures comprise the PP-polyamide and the emulsion stabilizer is associated with an outer surface of the elongated structures.
[0201] Clause 34. The method of Clause 22, wherein the emulsion stabilizer is included and forms a coating that covers less than 5% of the surface of the solidified particles.
[0202] Clause 35. The method of Clause 22, wherein the emulsion stabilizer is included and forms a coating that covers at least 5% of the surface of the solidified particles.
[0203] Clause 36. The method of Clause 22, wherein the emulsion stabilizer is included and forms a coating that covers at least 25% of the surface of the solidified particles.
[0204] Clause 37. The method of Clause 22, wherein the emulsion stabilizer is included and forms a coating that covers at least 50% of the surface of the solidified particles.
[0205] Clause 38. The method of Clause 22, wherein the PP-polyamide is present in the mixture at 5% to 60% by weight of the mixture.
[0206] Clause 39. The method of Clause 22, wherein the emulsion stabilizer is included and is present in the mixture at 0.05 wt % to 5 wt % based on the weight of the PP-polyamide.
[0207] Clause 40. The method of Clause 22, wherein the emulsion stabilizer is included and comprises nanoparticles, and the nanoparticles have an average diameter of 1 nm to 500 nm.
[0208] Item 41. A method according to Item 22, wherein the carrier fluid is selected from: silicone oil, fluorinated silicone oil, perfluorinated silicone oil, polyethylene glycol, paraffin, liquid petrolatum, vison oil, turtle oil, soybean oil, perhydrosqualene, sweet almond oil, calophyllum oil, palm oil, parleam oil, grape seed oil, sesame oil, corn oil, rapeseed oil, sunflower oil, cottonseed oil, almond oil, castor oil, avocado oil, jojoba oil, olive oil, cereal germ oil, esters of lanolic acid, esters of oleic acid, esters of lauric acid, esters of stearic acid, fatty acid esters, higher fatty acids, fatty alcohols, polysiloxanes modified with fatty acids, polysiloxanes modified with fatty alcohols, polysiloxanes modified with polyoxyalkylenes, and any combination thereof.
[0209] Item 42. The method according to Item 41, wherein the silicone oil is selected from: polydimethylsiloxane, methylphenylpolysiloxane, alkyl-modified polydimethylsiloxane, alkyl-modified methylphenylpolysiloxane, amino-modified polydimethylsiloxane, amino-modified methylphenylpolysiloxane, fluorine-modified polydimethylsiloxane, fluorine-modified methylphenylpolysiloxane, polyether-modified polydimethylsiloxane, polyether-modified methylphenylpolysiloxane and any combination thereof.
[0210] Clause 43. The method of Clause 22, wherein the carrier fluid has a viscosity of 1000 cSt to 150,000 cSt at 25°C.
[0211] Clause 44. The method of clause 22, wherein the carrier fluid has a viscosity of 0.6 g / cm 3 Up to 1.5g / cm 3 density.
[0212] Clause 45. The method of Clause 22, wherein the mixing is performed in an extruder.
[0213] Clause 46. The process according to Clause 22, wherein the mixing is carried out in a stirred reactor.
[0214] Clause 47. The method of Clause 22, wherein the mixture further comprises a surfactant.
[0215] Clause 448. The method of Clause 22, wherein the solidified particles have a D10 of about 0.1 μm to about 125 μm, a D50 of about 0.5 μm to about 200 μm, and a D90 of about 3 μm to about 300 μm, wherein D10 <D50<D90。
[0216] Clause 49. The method of Clause 22, wherein the solidified particles have a diameter span of about 0.2 to about 10.
[0217] Clause 50. The method of Clause 22, wherein the solidified particles have a D10 of about 5 μm to about 30 μm, a D50 of about 30 μm to about 70 μm, and a D90 of about 70 μm to about 120 μm, wherein D10 <D50<D90。
[0218] Clause 51. The method of Clause 50, wherein the solidified particles have a diameter span of about 1.0 to about 2.5.
[0219] Clause 52. The method of Clause 22, wherein the solidified particles have a D10 of about 25 μm to about 60 μm, a D50 of about 60 μm to about 110 μm, and a D90 of about 110 μm to about 175 μm, wherein D10 <D50<D90。
[0220] Clause 53. The method of Clause 52, wherein the solidified particles have a diameter span of about 0.6 to about 1.5.
[0221] Clause 54. The method of Clause 22, wherein the solidified particles have a D10 of about 75 μm to about 125 μm, a D50 of about 100 μm to about 200 μm, and a D90 of about 125 μm to about 300 μm, wherein D10 <D50<D90。
[0222] Clause 55. The method of Clause 54, wherein the solidified particles have a diameter span of about 0.2 to about 1.2.
[0223] Clause 56. The method of Clause 22, wherein the solidified particles have a roundness of about 0.90 to about 1.0.
[0224] Clause 57. The method of Clause 22, wherein the solidified particles have a Hausner ratio of about 1.0 to about 1.5.
[0225] Clause 58. The method of Clause 22, wherein the emulsion stabilizer comprises nanoparticles, and the nanoparticles comprise oxide nanoparticles.
[0226] Clause 59. The method of Clause 22, wherein the emulsion stabilizer comprises nanoparticles, and wherein the nanoparticles comprise carbon black.
[0227] Clause 60. The method of Clause 22, wherein the emulsion stabilizer comprises nanoparticles, and the nanoparticles comprise polymer nanoparticles.
[0228] Clause 61. A composition comprising: particles comprising a polyamide (PP-polyamide) having a pigment pendant from the backbone of the polyamide, and the particles having a roundness of about 0.90 to about 1.0.
[0229] Clause 62. The composition according to Clause 61, wherein the particles further comprise a thermoplastic polymer that is not the PP-polyamide.
[0230] Clause 63. The composition of Clause 61, wherein the particles further comprise the polyamide of the PP-polyamide but without a pigment pendant therefrom.
[0231] Clause 64. The composition of Clause 61, wherein the particle further comprises an emulsion stabilizer associated with an outer surface of the particle.
[0232] Clause 65. The composition of Clause 61, wherein at least some of the particles have voids comprising the emulsion stabilizer at the void / polymer interface.
[0233] Clause 66. The composition of Clause 65, wherein the emulsion stabilizer comprises nanoparticles and the nanoparticles are embedded in the void / polymer interface.
[0234] Clause 67. The composition of Clause 65, wherein the voids contain the carrier fluid.
[0235] Clause 68. The composition of Clause 61, wherein the particle further comprises elongated structures on the surface of the particle, wherein the elongated structures comprise the PP-polyamide and the emulsion stabilizer is associated with an outer surface of the elongated structures.
[0236] Clause 69. The composition of Clause 61, wherein the emulsion stabilizer forms a coating that covers less than 5% of the surface of the solidified particles.
[0237] Clause 70. The composition of Clause 61, wherein the emulsion stabilizer forms a coating that covers at least 5% of the surface of the solidified particles.
[0238] Clause 71. The composition of Clause 61, wherein the emulsion stabilizer forms a coating that covers at least 25% of the surface of the solidified particles.
[0239] Clause 72. The composition of Clause 61, wherein the emulsion stabilizer forms a coating that covers at least 50% of the surface of the solidified particles.
[0240] Clause 73. The composition of Clause 61, wherein the emulsion stabilizer comprises nanoparticles having an average diameter of 1 nm to 500 nm.
[0241] Clause 74. The composition of Clause 61, wherein the solidified particles have a D10 of about 0.5 μm to about 125 μm, a D50 of about 1 μm to about 200 μm, and a D90 of about 70 μm to about 300 μm, wherein D10 <D50<D90。
[0242] Clause 75. The composition of Clause 61, wherein the solidified particles have a diameter span of about 0.2 to about 10.
[0243] Clause 76. The composition of Clause 61, wherein the solidified particles have a D10 of about 5 μm to about 30 μm, a D50 of about 30 μm to about 70 μm, and a D90 of about 70 μm to about 120 μm, wherein D10 <D50<D90。
[0244] Clause 77. The composition of Clause 76, wherein the solidified particles have a diameter span of about 1.0 to about 2.5.
[0245] Clause 78. The composition of Clause 61, wherein the solidified particles have a D10 of about 25 μm to about 60 μm, a D50 of about 60 μm to about 110 μm, and a D90 of about 110 μm to about 175 μm, wherein D10 <D50<D90。
[0246] Clause 79. The composition of Clause 78, wherein the solidified particles have a diameter span of about 0.6 to about 1.5.
[0247] Clause 80. The composition of Clause 61, wherein the solidified particles have a D10 of about 75 μm to about 125 μm, a D50 of about 100 μm to about 200 μm, and a D90 of about 125 μm to about 300 μm, wherein D10 <D50<D90。
[0248] Clause 81. The composition of Clause 80, wherein the solidified particles have a diameter span of about 0.2 to about 1.2.
[0249] Clause 82. The composition of Clause 61, wherein the solidified particles have a Hausner ratio of about 1.0 to about 1.5.
[0250] Clause 83. A method comprising: depositing the composition according to Clause 61, optionally in combination with other thermoplastic polymer particles, on a surface in a specified shape; and once deposited, heating at least a portion of the particles to promote consolidation thereof and form a consolidated body.
[0251] Unless otherwise indicated, all numbers used in this specification and the associated claims expressing the quantity of ingredients, properties (such as molecular weight), reaction conditions, etc. should be understood as being modified in all cases by the term "about". Therefore, unless otherwise indicated, the numerical parameters listed in the following specification and the attached claims are approximate values, which may vary depending on the desired properties typically sought to be obtained by the present invention. At a minimum, and without attempting to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should at least be interpreted in light of the number of reported significant digits and by applying customary rounding techniques.
[0252] One or more exemplary typical examples of incorporating one or more inventive elements are presented herein. For the sake of clarity, all features of physical implementation are not described or shown in this application. It should be understood that in the development of the physical implementation scheme of one or more elements of the present invention, many specific decisions must be made to achieve the goal of the developer, such as meeting system-related constraints, business-related constraints, government-related constraints and other constraints, which vary and change over time due to implementation. Although the efforts made by the developer may be time-consuming, such efforts will be a routine task for those of ordinary skill in the art who benefit from the disclosure.
[0253] Although compositions and methods are described herein as "comprising" various components or steps, the compositions and methods may also "consist essentially of" or "consist of" the various components and steps.
[0254] In order to facilitate a better understanding of the embodiments of the present invention, the following examples of preferred or representative embodiments are given. The following examples should in no way be construed as limiting or defining the scope of the present invention.
[0255] Example
[0256] Hypothetical Example 1: Reaction with (3-glycidyloxypropyl)trimethoxysilane and polyamide resin Solution cross-linked 100 Silver Pearl Pigment
[0257] A 2-liter glass reactor equipped with an overhead mechanical stirrer and a heating mantle was charged with 100 g of 100 Silver Pearl pigment (available from E. Merck KGaA, Darmstadt, Germany) was added and heated to 40° C. with vigorous stirring. The pH of the suspension was adjusted to 3.3 using 2.5% hydrochloric acid and the temperature was raised to 75° C.
[0258] Subsequently, 3.0 g of (3-glycidyloxypropyl)trimethoxysilane (available from Millipore Sigma) were added over 10 minutes, and the pH was kept constant using a 2.5% hydrochloric acid solution. At the end of the addition, stirring was continued at 75° C. for 2 hours, during which the silane hydrolyzed and the resulting silanols associated with the inorganic pigment surface.
[0259] Subsequently, the system was adjusted to pH 8.0 while maintaining a reaction temperature of 75°C very slowly using 2.5% sodium hydroxide solution over a period of 1 hour, during which a condensation reaction occurred and the resulting siloxane bonded to the pigment surface, leaving unreacted epoxy end groups unavailable for subsequent functionalization. Stirring was continued at 75°C for another hour to complete the reaction and the pH dropped to 7.0. The product was filtered off using vacuum filtration, washed with deionized water, and dried at 140°C for about 16 hours.
[0260] Subsequently, 100 g of a polyamide resin such as nylon 6,6 is dissolved in N-methyl-2-pyrrolidone (NMP) under vigorous stirring. To this mixture is added 10 g of the epoxide-functionalized 100 SilverPearl pigment, and the reaction mixture was increased to 150°C for 2 hours under continuous agitation to promote the amino functional groups of the polyamide resin to react with the coating 100 Silver Pearl pigment surface glycidyl ether oxypropyl (epoxide) curing reaction. After the polyamide resin has been cured and coated with suspended 100 Silver Pearl pigment was then removed by filtering the particles using vacuum filtration to remove the solvent and the material was thoroughly dried in a vacuum oven for 24 hours. A portion of this mixture was then mixed with non-pigmented pendant polyamide in a Haake reaction with PDMS to form particles.
[0261] 2.5 g of polyamide resin cross-linked to the pigment surface was used. 100g Silver Pearl pigment side hanging agent and 27.5g nylon 6,6 were melt mixed with 150g 60,000 specific viscosity polydimethylsiloxane (PDMS) by hot melt emulsification in a Haake mixer equipped with a 300ml mixing container. The stirrer was heated to 230°C and mixed at 200rpm for 20 minutes. The mixture was then discharged from the Haake onto a cold surface to provide rapid quench cooling. It was then passed through a 90mm The resulting mixture was filtered through #1 filter paper (available from Sigma Aldrich) to separate the PP-polyamide particles from the carrier fluid. The PP-polyamide particles were washed three times with 1000 mL of ethyl acetate. The PP-polyamide particles were then air dried overnight in an aluminum pan in a fume hood. Optionally, the dried PP-polyamide particles may be screened through a 150 μm sieve. The Malvern MASTERSIZER was then used to sieve the dried PP-polyamide particles. TM The size of the PP-polyamide particles was characterized using a 3000 and the morphology was characterized using SEM micrographs. The D50 (μm) was estimated to be about 50 μm and the span was about 0.85.
[0262] Hypothetical Example 2: Reaction with (3-glycidyloxypropyl)trimethoxysilane and polyamide resin Cross-linked Metallic Super Gold Pigment
[0263] A 2-liter glass reactor equipped with an overhead mechanical stirrer and a heating mantle was charged with 100 g of Metallic Super Gold pigment, product number N-2002S (available from Creation of Quality Value) was added and heated to 40° C. with vigorous stirring. The pH of the suspension was adjusted to 3.3 using 2.5% hydrochloric acid and the temperature was raised to 75° C.
[0264] Subsequently, 3.0 g of (3-glycidyloxypropyl)trimethoxysilane (available from Millipore Sigma) were added over 10 minutes, and the pH was kept constant using a 2.5% hydrochloric acid solution. At the end of the addition, stirring was continued at 75° C. for 2 hours, during which the silane hydrolyzed and the resulting silanols associated with the inorganic pigment surface.
[0265] Subsequently, the system was adjusted to pH 8.0 while maintaining a reaction temperature of 75°C very slowly using 2.5% sodium hydroxide solution over a period of 1 hour, during which a condensation reaction occurred and the resulting siloxane bonded to the pigment surface, leaving unreacted epoxy end groups unavailable for subsequent functionalization. Stirring was continued at 75°C for another hour to complete the reaction and the pH dropped to 7.0. The product was filtered off using vacuum filtration, washed with deionized water, and dried at 140°C for about 16 hours.
[0266] Subsequently, 50 g of a polyamide resin such as nylon 6,6 is mixed with 10 g of the above-mentioned epoxy surface functionalized mica pigment. Metallic Super Gold was melt mixed in a Haake mixer at 150°C to 200°C for 20 to 30 minutes to promote the crosslinking reaction of the epoxide with the amino groups of the polyamide resin. The resulting pigmented polyamide resin concentrate was discharged from the Haake mixer, cooled and ground into a fine powder for subsequent incorporation into the colored polyamide microparticles.
[0267] 1.5 g of polyamide resin cross-linked to the pigment surface was used. Metallic Super Gold pigment pendant and 28.5 g nylon 6,6 were melt mixed with 150 g 30,000 specific viscosity polydimethylsiloxane (PDMS) by hot melt emulsification in a Haake mixer equipped with a 300 ml mixing vessel. The stirrer was heated to 230°C and mixed at 200 rpm for 20 minutes.
[0268] The mixture is then discharged from the Haake onto a cold surface to provide rapid quench cooling. The resulting mixture was filtered through #1 filter paper (available from Sigma Aldrich) to separate the PP-polyamide particles from the carrier fluid. The particles were washed three times with 1000 mL of ethyl acetate. The particles were then air dried overnight in an aluminum pan in a fume hood. Optionally, the dried particles may be screened through a 150 μm sieve. The Malvern MASTERSIZER was then used. TM The size of the PP-polyamide particles was characterized using a 3000 and the morphology was characterized using SEM micrographs. The D50 (μm) was estimated to be about 65 μm and the span was about 1.20.
[0269] Hypothetical Example 3: Reaction with (3-glycidyloxypropyl)trimethoxysilane and polyamide resin Solution cross-linked 100 Sparkle Violet Pigment
[0270] A 2-liter glass reactor equipped with an overhead mechanical stirrer and a heating mantle was charged with 100 g of 100 Sparkle Violet R-706E pigment (available from Creation of Quality Value) was added and heated to 40° C. with vigorous stirring. The pH of the suspension was adjusted to 3.3 using 2.5% hydrochloric acid and the temperature was raised to 75° C.
[0271] Subsequently, 3.0 g of (3-glycidyloxypropyl)trimethoxysilane (available from Millipore Sigma) were added over 10 minutes, and the pH was kept constant using a 2.5% hydrochloric acid solution. At the end of the addition, stirring was continued at 75° C. for 2 hours, during which the silane hydrolyzed and the resulting silanols associated with the inorganic pigment surface.
[0272] Subsequently, the system was adjusted to pH 8.0 while maintaining a reaction temperature of 75°C very slowly using 2.5% sodium hydroxide solution over a period of 1 hour, during which a condensation reaction occurred and the resulting siloxane bonded to the pigment surface, leaving unreacted epoxy end groups unavailable for subsequent functionalization. Stirring was continued at 75°C for another hour to complete the reaction and the pH dropped to 7.0. The product was filtered off using vacuum filtration, washed with deionized water, and dried at 140°C for about 16 hours.
[0273] Subsequently, 100 g of a polyamide resin such as nylon 6,6 is dissolved in N-methyl-2-pyrrolidone (NMP) under vigorous stirring. To this mixture is added 10 g of the epoxide-functionalized 100 SparkleViolet R-706E pigment, and the reaction mixture was increased to 150°C for 2 hours under continuous agitation to promote the amino functional groups of the polyamide resin to the coating 100 Sparkle Violet R-706E is a pigment that has been cured and coated with a suspended 100 Sparkle Violet R-706E pigment was then removed by filtering the particles using vacuum filtration to remove the solvent and the material was thoroughly dried in a vacuum oven for 24 hours. A portion of this mixture was then mixed with non-pigmented pendant polyamide in a Haake reaction with PDMS to form particles.
[0274] Use 50g of polyamide resin cross-linked to the pigment surface 100 Sparkle Violet R-706E pigment pendant and 550g nylon 6,6 were melt mixed with 2000g 10,000 specific viscosity polydimethylsiloxane (PDMS) by hot melt emulsification in a 25mm twin screw extruder (Werner & Pfleiderer ZSK-25). The polymer pellets were first added to the extruder, the temperature reached 230°C and the rotation speed was 900, and then the A preheated carrier fluid of R812S silica nanoparticles (1.1 wt. % relative to the PP-polyamide) was added to the molten polymer in the extruder.
[0275] The mixture was then discharged into a container and allowed to cool to room temperature over several hours. The resulting mixture was filtered through #1 filter paper (available from Sigma Aldrich) to separate the PP-polyamide particles from the carrier fluid. The particles were washed three times with 2000 mL of ethyl acetate. The particles were then dried overnight in a vacuum oven at ambient temperature. Optionally, the dried particles may be screened through a 150 μm sieve. The Malvern MASTERSIZER TM The size of the PP-polyamide particles was characterized using a 3000 and the morphology was characterized using SEM micrographs. The D50 (μm) was estimated to be about 75 μm and the span was about 1.30.
[0276] Hypothetical Example 4: Reaction with (3-glycidyloxypropyl)trimethoxysilane and polyamide resin Cross-linked Glitter Blue R-781E Pigment
[0277] A 2-liter glass reactor equipped with an overhead mechanical stirrer and a heating mantle was charged with 100 g of Glitter Blue pigment, product number R-781E (available from Creation of Quality Value), was heated to 40° C. with vigorous stirring. The pH of the suspension was adjusted to 3.3 using 2.5% hydrochloric acid, and the temperature was raised to 75° C.
[0278] Subsequently, 3.0 g of (3-glycidyloxypropyl)trimethoxysilane (available from Millipore Sigma) were added over 10 minutes, and the pH was kept constant using a 2.5% hydrochloric acid solution. At the end of the addition, stirring was continued at 75° C. for 2 hours, during which the silane hydrolyzed and the resulting silanols associated with the inorganic pigment surface.
[0279] Subsequently, the system was adjusted to pH 8.0 while maintaining a reaction temperature of 75°C very slowly using 2.5% sodium hydroxide solution over a period of 1 hour, during which a condensation reaction occurred and the resulting siloxane bonded to the pigment surface, leaving unreacted epoxy end groups unavailable for subsequent functionalization. Stirring was continued at 75°C for another hour to complete the reaction and the pH dropped to 7.0. The product was filtered off using vacuum filtration, washed with deionized water, and dried at 140°C for about 16 hours.
[0280] Subsequently, 50 g of a polyamide resin such as nylon 6,6 is mixed with 10 g of the above-mentioned epoxy surface functionalized mica pigment. Glitter Blue R-871E was melt mixed in a Haake mixer at 150°C to 200°C for 20 to 30 minutes to promote the crosslinking reaction of the epoxide with the amino groups of the polyamide resin. The resulting pigmented polyamide resin concentrate was discharged from the Haake mixer, cooled and ground into a fine powder for subsequent incorporation into the colored polyamide microparticles.
[0281] Use 30g of polyamide resin cross-linked to the pigment surface Glitter Blue R-871E pigment pendant and 570g nylon 6,6 were melt mixed with 2000g 10,000 specific viscosity polydimethylsiloxane (PDMS) by hot melt emulsification in a 25mm twin screw extruder (Werner & Pfleiderer ZSK-25). The polymer pellets were first added to the extruder, the temperature reached 230°C and the rotation speed was 900, and then the A preheated carrier fluid of R812S silica nanoparticles (1.1 wt. % relative to the PP-polyamide) was added to the molten polymer in the extruder.
[0282] The mixture was then discharged into a container and allowed to cool to room temperature over several hours. The resulting mixture was filtered through #1 filter paper (available from Sigma Aldrich) to separate the PP-polyamide particles from the carrier fluid. The particles were washed three times with 2000 mL of ethyl acetate. The particles were then dried overnight in a vacuum oven at ambient temperature. Optionally, the dried particles may be screened through a 150 μm sieve. The Malvern MASTERSIZER TM The size of the PP-polyamide particles was characterized using a 3000 and the morphology was characterized using SEM micrographs. The D50 (μm) was estimated to be about 65 μm and the span was about 1.10.
[0283] Hypothetical Example 5: Reaction of Silica Nanoparticles Functionalized with 3-Aminopropyl-(3-oxobutyric Acid) and Reaction of In-situ cross-linking of polyamide resin 100 Silver Pearl Pigment
[0284] A 2-liter glass reactor equipped with an overhead mechanical stirrer and a heating mantle was charged with 100 g of 100 Silver Pearl pigment (available from E. Merck KGaA, Darmstadt, Germany) and 100 mL of 3-aminopropyl-(3-oxobutanoic acid) functionalized silica nanoparticles (available from Millipore Sigma) at 2.5 wt% loading in dimethylformamide (DMF) as a colloidal dispersion. The mixture was heated to 40° C. with vigorous stirring for 4 hours to promote adsorption of the silica nanoparticles onto the surface of the pigment. The suspension was cooled to room temperature and filtered to remove water and DMF solvent. The functionalized pigment particles with free carboxylic acid functional groups were dried in a vacuum oven at 40° C. for 24 hours to produce a functionalized pigment powder.
[0285] A clear viscous stock solution (1.5 moles) of thionyl chloride (5.46 mL, 0.075 mol) and benzotriazole (8.93 g, 0.075 mol) in 50 mL of anhydrous dichloromethane was prepared by stirring at room temperature. A portion of this solution (1.25 mmol) was slowly added to convert the side chain carboxylic acid functional groups on the surface of the mica pigment into acid chlorides to be able to cure with the amino polyamide groups in the polyamide resin.
[0286] Dry mica pigment functionalized with surface carboxylic acid 100 Silver Pearl (about 110g) was suspended in 500mL of anhydrous dichloromethane under constant stirring. At room temperature, 20mL of thionyl chloride-benzotriazole mixture was slowly added to the mixture over 30 minutes. As the reaction proceeded, benzotriazole hydrochloride began to separate out from the solution, indicating that the conversion of the carboxylic acid was converted into an acyl chloride. The reaction mixture was mixed for another 30 minutes, then the mixture was filtered to remove the solvent, and washed thoroughly with water, then dried in a vacuum oven for 24 hours.
[0287] Subsequently, 50 g of a polyamide resin such as nylon 6,6 is mixed with 10 g of the above-mentioned acyl chloride surface-functionalized mica pigment. 100 Silver Pearl was melt mixed in a Haake mixer at 150°C to 200°C for 20 to 30 minutes to promote the crosslinking reaction of the acid chloride with the amino groups of the polyamide resin. The resulting pigment-side-suspended polyamide resin concentrate was discharged from the Haake mixer, cooled and ground into a fine powder for subsequent incorporation into the colored polyamide microparticles.
[0288] 1.5 g of polyamide resin cross-linked to the pigment surface was used. 100g Silver Pearl pigment pendant and 28.5g nylon 6,6 were emulsified by hot melt in a Haake mixer equipped with a 300ml mixing container and 150g of a R812S silica nanoparticles (0.75 wt% relative to PP-polyamide) were melt mixed with polydimethylsiloxane (PDMS) of 30,000 specific viscosity. The stirrer was heated to 230° C. and mixed at 200 rpm for 15 minutes.
[0289] The mixture is then discharged from the Haake onto a cold surface to provide rapid quench cooling. The resulting mixture was filtered through #1 filter paper (available from Sigma Aldrich) to separate the PP-polyamide particles from the carrier fluid. The particles were washed three times with 1000 mL of ethyl acetate. The particles were then air dried overnight in an aluminum pan in a fume hood. Optionally, the dried particles may be screened through a 150 μm sieve. The Malvern MASTERSIZER was then used. TM The size of the PP-polyamide particles was characterized using a 3000 and the morphology was characterized using SEM micrographs. The D50 (μm) was estimated to be about 55 μm and the span was about 1.10.
[0290] Hypothetical Example 6: Silica nanoparticles functionalized with 3-aminopropyl-(3-oxobutyric acid) and in-situ crosslinked by polyamide resin Metallic Super Gold Pigment
[0291] A 2-liter glass reactor equipped with an overhead mechanical stirrer and a heating mantle was charged with 100 g of Metallic Super Gold (available from Creation of Quality Value) and 100 mL of 3-aminopropyl-(3-oxobutanoic acid) functionalized silica nanoparticles (available from Millipore Sigma) in a colloidal dispersion at 2.5 wt% loading in DMF. The mixture was heated to 40°C with vigorous stirring for 4 hours to promote adsorption of the silica nanoparticles onto the surface of the pigment. The suspension was cooled to room temperature and filtered to remove water and DMF solvent. The functionalized pigment particles with free carboxylic acid functional groups were dried in a vacuum oven at 40°C for 24 hours to produce a functionalized pigment powder.
[0292] A clear viscous stock solution (1.5 moles) of thionyl chloride (5.46 mL, 0.075 mol) and benzotriazole (8.93 g, 0.075 mol) in 50 mL of anhydrous dichloromethane was prepared by stirring at room temperature. A portion of this solution (1.25 mmol) was slowly added to convert the side chain carboxylic acid functional groups on the surface of the mica pigment into acid chlorides to be able to cure with the amino polyamide groups in the polyamide resin.
[0293] Dry mica pigment functionalized with surface carboxylic acid Metallic Super Gold (about 110 g) was suspended in 500 mL of anhydrous dichloromethane under constant stirring. At room temperature, 20 mL of thionyl chloride-benzotriazole mixture was slowly added to the mixture over 30 minutes. As the reaction proceeded, benzotriazole hydrochloride began to separate out from the solution, indicating that the conversion of the carboxylic acid was converted into an acyl chloride. The reaction mixture was mixed for another 30 minutes, then the mixture was filtered to remove the solvent, and thoroughly washed with water, then dried in a vacuum oven for 24 hours.
[0294] Subsequently, 50 g of a polyamide resin such as nylon 6,6 is mixed with 10 g of the above-mentioned acyl chloride surface-functionalized mica pigment. Metallic Super Gold was melt mixed in a Haake mixer at 150°C to 200°C for 20 to 30 minutes to promote the crosslinking reaction of the acid chloride with the amino groups of the polyamide resin. The resulting pigment-side-suspended polyamide resin concentrate was discharged from the Haake mixer, cooled and ground into a fine powder for subsequent incorporation into the colored polyamide microparticles.
[0295] 1.5 g of polyamide resin cross-linked to the pigment surface was used. Metallic Super Gold pigment pendant and 28.5 g nylon 6,6 were emulsified by hot melt in a Haake mixer equipped with a 300 ml mixing container and 150 g of the pigment dispersed therein. R812S silica nanoparticles (1.00 wt% relative to PP-polyamide) were melt mixed with polydimethylsiloxane (PDMS) of 30,000 specific viscosity. The stirrer was heated to 230° C. and mixed at 200 rpm for 15 minutes.
[0296] The mixture is then discharged from the Haake onto a cold surface to provide rapid quench cooling. The resulting mixture was filtered through #1 filter paper (available from Sigma Aldrich) to separate the PP-polyamide particles from the carrier fluid. The particles were washed three times with 1000 mL of ethyl acetate. The particles were then air dried overnight in an aluminum pan in a fume hood. Optionally, the dried particles may be screened through a 150 μm sieve. The Malvern MASTERSIZER was then used. TM The size of the PP-polyamide particles was characterized using a 3000 and the morphology was characterized using SEM micrographs. The D50 (μm) was estimated to be about 50 μm and the span was about 0.95.
[0297] Hypothetical Example 7: Silica nanoparticles functionalized with 3-aminopropyl-(3-oxobutyric acid) and in situ crosslinked by polyamide resin 100 Sparkle Violet Pigment
[0298] A 2-liter glass reactor equipped with an overhead mechanical stirrer and a heating mantle was charged with 100 g of 100 Sparkle Violet R-706E (available from Creation of QualityValue) and 100 mL of 3-aminopropyl-(3-oxobutanoic acid) functionalized silica nanoparticles (available from Millipore Sigma) in a colloidal dispersion at 2.5 wt% loading in DMF. The mixture was heated to 40°C with vigorous stirring for 4 hours to promote the adsorption of the silica nanoparticles onto the surface of the pigment. The suspension was cooled to room temperature and filtered to remove water and DMF solvent. The functionalized pigment particles with free carboxylic acid functional groups were dried in a vacuum oven at 40°C for 24 hours to produce a functionalized pigment powder.
[0299] A clear viscous stock solution (1.5 moles) of thionyl chloride (5.46 mL, 0.075 mol) and benzotriazole (8.93 g, 0.075 mol) in 50 mL of anhydrous dichloromethane was prepared by stirring at room temperature. A portion of this solution (1.25 mmol) was slowly added to convert the side chain carboxylic acid functional groups on the surface of the mica pigment into acid chlorides to be able to cure with the amino polyamide groups in the polyamide resin.
[0300] Dry mica pigment functionalized with surface carboxylic acid 100 Sparkle Violet R-706E (about 110g) was suspended in 500mL of anhydrous dichloromethane under constant stirring. At room temperature, 20mL of thionyl chloride-benzotriazole mixture was slowly added to the mixture in 30 minutes. Along with the reaction, benzotriazole hydrochloride began to separate out from the solution, which showed that the conversion of carboxylic acid was converted into acyl chloride. The reaction mixture was mixed for another 30 minutes, then the mixture was filtered to remove the solvent, and washed thoroughly with water, then dried in a vacuum oven for 24 hours.
[0301] Subsequently, 50 g of a polyamide resin such as nylon 6,6 is mixed with 10 g of the above-mentioned acyl chloride surface-functionalized mica pigment. 100 Sparkle Violet R-706E was melt mixed in a Haake mixer at 150°C to 200°C for 20 to 30 minutes to promote the crosslinking reaction of the acid chloride with the amino groups of the polyamide resin. The resulting pigmented polyamide resin concentrate was discharged from the Haake mixer, cooled and ground into a fine powder for subsequent incorporation into the colored polyamide microparticles.
[0302] Use 30g of polyamide resin cross-linked to the pigment surface 100 Sparkle Violet R-706E pigment pendant and 570g nylon 6,6 were melt mixed with 2000g 20,000 specific viscosity polydimethylsiloxane (PDMS) by hot melt emulsification in a 25mm twin screw extruder (Werner & Pfleiderer ZSK-25). The polymer pellets were first added to the extruder, the temperature reached 230°C and the rotation speed was 1100, and then the A preheated carrier fluid of R812S silica nanoparticles (1.1 wt. % relative to the PP-polyamide) was added to the molten polymer in the extruder.
[0303] The mixture was then discharged into a container and allowed to cool to room temperature over several hours. The resulting mixture was filtered through #1 filter paper (available from Sigma Aldrich) to separate the PP-polyamide particles from the carrier fluid. The particles were washed three times with 2000 mL of ethyl acetate. The particles were then dried overnight in a vacuum oven at ambient temperature. Optionally, the dried particles may be screened through a 150 μm sieve. The Malvern MASTERSIZER TM The size of the PP-polyamide particles was characterized using a 3000 and the morphology was characterized using SEM micrographs. The D50 (μm) was estimated to be about 55 μm and the span was about 1.30.
[0304] Hypothetical Example 8: Reaction of Silica Nanoparticles Functionalized with 3-Aminopropyl-(3-oxobutyric Acid) and Reaction of In-situ cross-linking of polyamide resin Glitter Blue R-781E Pigment
[0305] A 2-liter glass reactor equipped with an overhead mechanical stirrer and a heating mantle was charged with 100 g of Glitter Blue pigment, product number R-781E (available from Creation of Quality Value) and 100 mL of 3-aminopropyl-(3-oxobutanoic acid) functionalized silica nanoparticles (available from MilliporeSigma) at 2.5 wt% loading in DMF as a colloidal dispersion. The mixture was heated to 40° C. with vigorous stirring for 4 hours to promote adsorption of the silica nanoparticles onto the surface of the pigment. The suspension was cooled to room temperature and filtered to remove water and DMF solvent. The functionalized pigment particles with free carboxylic acid functional groups were dried in a vacuum oven at 40° C. for 24 hours to produce a functionalized pigment powder.
[0306] A clear viscous stock solution (1.5 moles) of thionyl chloride (5.46 mL, 0.075 mol) and benzotriazole (8.93 g, 0.075 mol) in 50 mL of anhydrous dichloromethane was prepared by stirring at room temperature. A portion of this solution (1.25 mmol) was slowly added to convert the side chain carboxylic acid functional groups on the surface of the mica pigment into acid chlorides to be able to cure with the amino polyamide groups in the polyamide resin.
[0307] Dry mica pigment functionalized with surface carboxylic acid Glitter Blue (about 110g) is suspended in 500mL anhydrous dichloromethane under constant stirring. At room temperature, in this mixture, 20mL thionyl chloride-benzotriazole mixture is slowly added in 30 minutes. Along with the carrying out of reaction, benzotriazole hydrochloride begins to separate out from solution, and this shows that the conversion of carboxylic acid is converted into acyl chloride. The reaction mixture is mixed for another 30 minutes, and the mixture is filtered then to remove solvent, and thoroughly washed with water, and then dried in a vacuum oven for 24 hours.
[0308] Subsequently, 50 g of a polyamide resin such as nylon 6,6 is mixed with 10 g of the above-mentioned acyl chloride surface-functionalized mica pigment. Glitter Blue was melt mixed in a Haake mixer at 150°C to 200°C for 20 to 30 minutes to promote the crosslinking reaction of the acid chloride with the amino groups of the polyamide resin. The resulting pigment-side-suspended polyamide resin concentrate was discharged from the Haake mixer, cooled and ground into a fine powder for subsequent incorporation into the colored polyamide microparticles.
[0309] 1.5 g of polyamide resin cross-linked to the pigment surface was used. Glitter Blue pigment pendant and 28.5 g nylon 6,6 were emulsified by hot melt in a Haake mixer equipped with a 300 ml mixing container and 150 g of the pigment dispersed therein. R812S silica nanoparticles (0.75 wt% relative to PP-polyamide) were melt mixed with polydimethylsiloxane (PDMS) of 60,000 specific viscosity. The stirrer was heated to 230° C. and mixed at 200 rpm for 20 minutes.
[0310] The mixture is then discharged from the Haake onto a cold surface to provide rapid quench cooling. The resulting mixture was filtered through #1 filter paper (available from Sigma Aldrich) to separate the PP-polyamide particles from the carrier fluid. The particles were washed three times with 1000 mL of ethyl acetate. The particles were then air dried overnight in an aluminum pan in a fume hood. Optionally, the dried particles may be screened through a 150 μm sieve. The Malvern MASTERSIZER was then used. TM The size of the PP-polyamide particles was characterized using a 3000 and the morphology was characterized using SEM micrographs. The D50 (μm) was estimated to be about 75 μm and the span was about 0.85.
[0311] Hypothetical Example 9: General Reaction Conditions of Epoxides and Polyamides
[0312] The reaction of the epoxy groups on the metal pigment with the polyamide can be carried out at a temperature of about 70°C to about 200°C (or about 70°C to about 150°C, about 125°C to about 200°C) in the presence of an organic solvent such as tetrahydrofuran, dimethylformamide, toluene, etc. and any combination thereof under an atmosphere (nitrogen or argon). The mixture is then stirred at elevated temperature for about 24 hours. After the mixture is cooled to room temperature, the grafted polymer is filtered and washed to remove organic impurities and unreacted starting reagents.
[0313] Therefore, the present invention is well suited to achieve the mentioned goals and advantages and those inherent therein. The specific embodiments and configurations disclosed above are exemplary only, because the present invention can be modified and implemented in different but equivalent ways that are obvious to those skilled in the art who benefit from the teachings herein. In addition, it is expected that there is no limitation on the details of construction or design shown herein, except as described in the following claims. Therefore, it is obvious that the specific exemplary embodiments disclosed above can be changed, combined or modified, and all such changes are considered to be within the scope and essence of the present invention. The present invention disclosed exemplarily herein can be appropriately implemented in the absence of any element not specifically disclosed herein and / or any optional element disclosed herein. Although compositions and methods are described by "comprising", "containing" or "including" various components or steps, compositions and methods can also be "essentially composed of various components and steps" or "composed of various components and steps". All numbers and ranges disclosed above may change by some amount. Whenever a numerical range with a lower limit and an upper limit is disclosed, any number and any included range falling within the range are specifically disclosed. Specifically, each value range disclosed herein (in the form of "about a to about b", or equivalently, "about a to b", or equivalently, "about ab") should be understood to set forth each numerical value and range encompassed within the broader value range. In addition, the terms in the claims have their plain, ordinary meaning unless otherwise explicitly and clearly defined by the patentee. In addition, the indefinite articles "a" or "an" used in the claims are defined herein to mean that there is one or more than one of the element it introduces.
Claims
1. A method, comprising: functionalizing metal oxide particles bonded to pigment particles with a compound having epoxy groups to produce a surface-treated pigment having pendant epoxy groups, wherein the metal oxide particles are particles distinct from the pigment particles; as well as The pendant epoxy groups are reacted with a polyamide to produce a pigment-pendent polyamide.
2. The method according to claim 1, wherein the compound having the epoxide is selected from the group consisting of: (3-glycidoxypropyl)trimethoxysilane, (3-glycidoxypropyl)triethoxysilane, diethoxy(3-glycidoxypropyl)methylsilane and 1,3-bis(3-glycidoxypropyl)tetramethylsiloxane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 5,6-epoxyhexyltriethoxysilane, and any combination thereof.
3. The method according to claim 1, wherein the metal oxide particles comprise one or more selected from the group consisting of titanium dioxide, titanium suboxide, Al2O3, Fe2O3, Fe3O4, SnO2, Cr2O3, ZnO, CuO, NiO, zirconium oxide, and titanium iron oxide.
4. The method of claim 1, wherein the pigment particles comprise one or more selected from the group consisting of synthetic mica, natural mica, talc, kaolin, glass, SiO2 flakes, Al2O3 flakes, acicular pigments, CaSO4, iron oxide, chromium oxide, carbon black, metallic effect pigments, optically variable pigments, liquid crystal polymer pigments, and holographic pigments. The method according to claim 4 , wherein the natural mica is sericite. The method of claim 4 , wherein the glass is a glass sheet.
7. The method of claim 1, wherein the polyamide is selected from the group consisting of polycaprolactam, polyhexamethylene succinamide, polyhexamethylene adipamide, polypentamethylene adipamide, polyhexamethylene sebacamide, polyundecanamide, polydodecaneamide, nylon 10,10, nylon 10,12, nylon 10,14, nylon 10,18, nylon 6,18, nylon 6,12, nylon 6,14, nylon 12,12, semiaromatic polyamide, aromatic polyamide, any copolymers thereof, and any combination thereof.
8. The method of claim 7, wherein the semiaromatic polyamide is polyhexamethylene terephthalamide.
9. The method of claim 1, wherein the reaction of the pendant epoxy group with polyamide is performed at 70°C to 200°C.
10. The method of claim 1, wherein the weight ratio of the pigment to the polyamide is 1:10 to 1:1000.
Citation Information
Patent Citations
Grafting functionalized pearlescent or metallic pigment onto polyester polymers for special effect images
US7998649B2
Thermoplastic silicone elastomers from compatibilized polyamide resins
CN1429253A
Thermoplastic silicone elastomers from compatibilized polyamide resins
CN1571818A
Compositions of polyhydric alcohols and polyamides
US20130228728A1
Polyarylene sulfide resin compositions
US6037422A