Semiconductor devices

By using indium and oxygen semiconductor layers in semiconductor devices, controlling the gallium content, and combining a multilayer insulating structure, the mobility and reliability issues of metal oxide semiconductor devices were solved, resulting in semiconductor devices with high mobility and high reliability.

CN112514079BActive Publication Date: 2024-10-15SEMICON ENERGY LAB CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980050350.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-27
Filing Date
2019-07-24
Publication Date
2024-10-15
Estimated Expiration
2039-07-24

AI Technical Summary

Technical Problem

In the prior art, metal-oxide-semiconductor devices have shortcomings in terms of high field-effect mobility and reliability, especially in oxide semiconductor layers containing gallium, where high interface defect state density leads to electrical characteristic and reliability problems.

Method used

By employing a semiconductor layer containing indium and oxygen, and controlling the ratio of indium to gallium to reduce gallium content, combined with a multilayer insulating structure and a metal oxide layer, the deposition conditions are optimized to reduce interface defects and improve carrier mobility and reliability.

Benefits of technology

This technology enables semiconductor devices with high field-effect mobility and high reliability, reduces threshold voltage variation, and improves device stability and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112514079B_ABST
    Figure CN112514079B_ABST
Patent Text Reader

Abstract

A semiconductor device with good electrical characteristics is provided. A semiconductor device with high reliability is provided. A semiconductor device with stable electrical characteristics is provided. The semiconductor device includes a first insulating layer, a second insulating layer, a semiconductor layer and a first conductive layer. The semiconductor layer, the second insulating layer and the first conductive layer are stacked in sequence on the first insulating layer. The second insulating layer has a stacked structure in which a first insulating film, a second insulating film and a third insulating film are stacked in sequence. The first insulating film, the second insulating film and the third insulating film each include an oxide. The first insulating film includes a portion in contact with the semiconductor layer. The semiconductor layer includes indium, gallium and oxygen, and includes a region in which the content of indium is higher than the content of gallium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a semiconductor device and a method for manufacturing a semiconductor device. One embodiment of the present invention relates to a display device.

[0002] Note that one embodiment of the present invention is not limited to the above-mentioned technical field. Examples of the technical field of one embodiment of the present invention disclosed in this specification and the like include semiconductor devices, display devices, light-emitting devices, power storage devices, storage devices, electronic devices, lighting devices, input devices, input-output devices, driving methods of these devices, or manufacturing methods of these devices. Semiconductor devices refer to all devices that can work by utilizing semiconductor characteristics. Background Art

[0003] As a semiconductor material that can be used for transistors, oxide semiconductors containing metal oxides have attracted attention. For example, Patent Document 1 discloses a semiconductor device in which a plurality of oxide semiconductor layers are stacked, in which an oxide semiconductor layer used as a channel contains indium and gallium, and the proportion of indium is higher than that of gallium, so that field effect mobility (sometimes referred to as mobility or μFE) is improved.

[0004] Since the metal oxide that can be used for the semiconductor layer can be formed by sputtering or the like, it can be used for the semiconductor layer of the transistor in the large display device. In addition, since part of the production equipment of the transistor containing polycrystalline silicon or amorphous silicon can be improved and used, the equipment investment can also be suppressed. Compared with the transistor containing amorphous silicon, the transistor containing metal oxide has a high field effect mobility, so a high-performance display device provided with a driving circuit can be realized.

[0005] [References]

[0006] [Patent Document]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 2014-7399 Summary of the invention

[0008] One of the purposes of one embodiment of the present invention is to provide a semiconductor device with good electrical characteristics. One of the purposes of one embodiment of the present invention is to provide a semiconductor device with high reliability. One of the purposes of one embodiment of the present invention is to provide a semiconductor device with stable electrical characteristics. One of the purposes of one embodiment of the present invention is to provide a display device with high reliability.

[0009] Note that the description of these purposes does not prevent the existence of other purposes. Note that one embodiment of the present invention does not need to achieve all of the above purposes. In addition, purposes other than the above can be extracted from the description of the specification, drawings, claims, etc.

[0010] One embodiment of the present invention is a semiconductor device including a first insulating layer, a second insulating layer, a semiconductor layer and a first conductive layer. The semiconductor layer, the second insulating layer and the first conductive layer are stacked in sequence on the first insulating layer. The second insulating layer has a stacked structure in which a first insulating film, a second insulating film and a third insulating film are stacked in sequence. The first insulating film, the second insulating film and the third insulating film each contain an oxide. The first insulating film includes a portion in contact with the semiconductor layer. The semiconductor layer contains indium and oxygen.

[0011] In the above, the semiconductor layer preferably does not contain gallium.

[0012] Among the above, the semiconductor layer preferably contains zinc.

[0013] Another embodiment of the present invention is a semiconductor device including a first insulating layer, a second insulating layer, a semiconductor layer and a first conductive layer. A semiconductor layer, a second insulating layer and a first conductive layer are stacked in sequence on the first insulating layer. The second insulating layer has a stacked structure in which a first insulating film, a second insulating film and a third insulating film are stacked in sequence. The first insulating film, the second insulating film and the third insulating film each include an oxide. The first insulating film includes a portion in contact with the semiconductor layer. The semiconductor layer includes indium, gallium and oxygen, and includes a region in which the content of indium is higher than the content of gallium.

[0014] In the above, the semiconductor layer preferably contains zinc. In this case, the semiconductor layer preferably includes a region where the content of zinc is higher than the content of gallium.

[0015] Another embodiment of the present invention is a semiconductor device including a first insulating layer, a second insulating layer, a first semiconductor layer, a second semiconductor layer and a first conductive layer. The second semiconductor layer, the first semiconductor layer, the second insulating layer and the first conductive layer are stacked in sequence on the first insulating layer. The second insulating layer has a stacked structure in which a first insulating film, a second insulating film and a third insulating film are stacked in sequence. The first insulating film, the second insulating film and the third insulating film each contain an oxide. The first insulating film includes a portion in contact with the first semiconductor layer. The first semiconductor layer contains indium and oxygen. The second semiconductor layer contains indium, zinc, gallium and oxygen. The first semiconductor layer includes a region in which the content of indium is higher than that of the second semiconductor layer.

[0016] In the above, the first semiconductor layer preferably contains zinc and gallium. The first semiconductor layer preferably includes a region where the gallium content is lower than the indium content and the zinc content is higher than the gallium content. The first semiconductor layer preferably includes a region where the zinc content is higher than or equal to the zinc content of the second semiconductor layer.

[0017] In the above, it is preferred that a metal oxide layer is provided between the second insulating layer and the first conductive layer. In this case, the metal oxide layer preferably contains one or more elements selected from aluminum, hafnium, indium, gallium and zinc. It is particularly preferred that the metal oxide layer contains indium. In addition, the metal oxide layer and the first semiconductor layer preferably have substantially the same indium content.

[0018] In the above, the first insulating film is preferably formed at a lower deposition rate than the second insulating film.

[0019] In the above, it is preferred that a second conductive layer is included, and a third insulating layer is included instead of the first insulating layer. In this case, it is preferred that the second conductive layer includes a region overlapping the first semiconductor layer via the third insulating layer, and the third insulating layer has a stacked structure in which a fourth insulating film, a fifth insulating film, a sixth insulating film, and a seventh insulating film are stacked in sequence. It is preferred that the seventh insulating film contains oxygen, and the fourth insulating film, the fifth insulating film, and the sixth insulating film each contain nitrogen.

[0020] In the above, it is preferable that the seventh insulating film includes silicon oxide, and the fourth insulating film, the fifth insulating film, and the sixth insulating film each include silicon nitride.

[0021] According to one embodiment of the present invention, a semiconductor device having good electrical characteristics can be provided. A semiconductor device having high reliability can be provided. A semiconductor device having stable electrical characteristics can be provided. A display device having high reliability can be provided.

[0022] Note that the description of these effects does not prevent the existence of other effects. In addition, one embodiment of the present invention does not need to have all of the above effects. In addition, effects other than the above can be extracted from the description of the specification, drawings, claims, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In the diagram:

[0024] Figure 1A and Figure 1B Each shows a structural example of a transistor;

[0025] Figure 2A and Figure 2B Each shows a structural example of a transistor;

[0026] FIG. 3A to FIG. 3C An example of the structure of a transistor is shown;

[0027] FIG. 4A to FIG. 4C An example of the structure of a transistor is shown;

[0028] FIG. 5A to FIG. 5C An example of the structure of a transistor is shown;

[0029] FIG. 6A to FIG. 6C An example of the structure of a transistor is shown;

[0030] 7A to 7D Each shows a structural example of a transistor;

[0031] FIG. 8A to FIG. 8D Each shows a structural example of a transistor;

[0032] 9A to 9E A method of manufacturing a transistor is shown;

[0033] FIG. 10A to FIG. 10D A method of manufacturing a transistor is shown;

[0034] Fig.11A and Fig. 11B A method of manufacturing a transistor is shown;

[0035] FIG. 12A to FIG. 12D A method of manufacturing a transistor is shown;

[0036] FIG. 13A to FIG. 13C is a top view of the display device;

[0037] Fig.14 is a cross-sectional view of a display device;

[0038] Fig.15 is a cross-sectional view of a display device;

[0039] Fig.16 is a cross-sectional view of a display device;

[0040] Fig.17 is a cross-sectional view of a display device;

[0041] Fig.18A is a block diagram of a display device, Fig.18B and Fig.18C is a circuit diagram of the display device;

[0042] Fig.19A , Fig.19C and Fig.19D is a circuit diagram of the display device, Fig.19B It is a timing diagram;

[0043] Fig. 20A and Fig. 20B An example of the structure of the display module is shown;

[0044] Fig.21A and Fig.21B An example of the structure of an electronic device is shown;

[0045] FIG. 22A to FIG. 22E An example of the structure of an electronic device is shown;

[0046] FIG. 23A to FIG. 23G An example of the structure of an electronic device is shown;

[0047] FIG. 24A to FIG. 24D An example of the structure of an electronic device is shown;

[0048] FIG. 25A to FIG. 25D The Id-Vg characteristics of the transistor are shown. Fig.25E shows the reliability test results of transistors;

[0049] Fig.26A The Id-Vg characteristics of the transistor are shown. Fig.26B shows the reliability test results of transistors;

[0050] Fig. 27 Shows TDS analysis results;

[0051] Fig.28A and Fig.28B Shows TDS analysis results;

[0052] FIG. 29A to FIG. 29C The ESR measurement results are shown;

[0053] Fig. 30A The Id-Vg characteristics of the transistor are shown. Fig. 30B shows the reliability test results of transistors;

[0054] Fig.31A The Id-Vg characteristics of the transistor are shown. Fig.31B shows the reliability test results of transistors;

[0055] Fig.32A The Id-Vg characteristics of the transistor are shown. Fig.32B shows the reliability test results of transistors;

[0056] Fig.33A is a schematic diagram of the segmentation structure. Fig.33B shows the density of states of an oxide semiconductor having a segmented structure;

[0057] Fig.34A is a schematic diagram of the Ga-O structure. Fig.34B shows the density of states of an oxide semiconductor having a Ga—O structure;

[0058] Fig.35A and Fig.35B Each shows the energy change of the reaction path. DETAILED DESCRIPTION

[0059] The following describes the embodiments with reference to the accompanying drawings. However, the embodiments can be implemented in a number of different ways, and a person skilled in the art can easily understand that the methods and details can be transformed into various forms without departing from the purpose and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the contents described in the embodiments shown below.

[0060] In the drawings described in this specification, the size of each component, the thickness of a layer, or a region may be exaggerated for the sake of clarity of description.

[0061] The ordinal numbers such as “first”, “second” and “third” used in this specification and the like are added to avoid confusion among constituent elements and are not intended to limit the number.

[0062] In this specification, for the sake of convenience, words and phrases such as "upper" and "lower" are used to indicate the positional relationship of the components with reference to the drawings. In addition, the positional relationship of the components is appropriately changed according to the direction in which each structure is described. Therefore, the words and phrases described in the specification are not limited, and the words and phrases can be appropriately changed according to the situation.

[0063] In addition, in this specification, when transistors with different polarities are used or the direction of current changes during circuit operation, the functions of the source and drain included in the transistor may be interchanged. Therefore, "source" and "drain" may be interchanged.

[0064] Note that in this specification, etc., the channel length direction of a transistor refers to one of the directions parallel to the straight line connecting the source region and the drain region at the shortest distance. That is, the channel length direction is equivalent to one of the directions of the current flowing through the semiconductor layer when the transistor is in the on state. In addition, the channel width direction refers to a direction orthogonal to the channel length direction. In addition, depending on the structure and shape of the transistor, the channel length direction and the channel width direction are sometimes not limited to one direction.

[0065] In this specification, "electrical connection" includes connection through "an element having some kind of electrical function". Here, "an element having some kind of electrical function" is not particularly limited as long as it can transmit and receive electrical signals between the connected objects. For example, "an element having some kind of electrical function" includes not only electrodes and wiring, but also switching elements such as transistors, resistors, inductors, capacitors, and other elements having various functions.

[0066] In addition, in this specification, "film" and "layer" may be interchanged. For example, "conductive layer" may be replaced with "conductive film". Also, for example, "insulating layer" may be replaced with "insulating film".

[0067] In addition, in this specification, etc., unless otherwise specified, the off-state current refers to the drain current when the transistor is in the off state (also called the non-conducting state or the blocking state). Unless otherwise specified, in an n-channel transistor, the off state refers to the voltage V between the gate and the source. gs Below the threshold voltage V th (In a p-channel transistor, V gs Higher than V th ) status.

[0068] In this specification, etc., a display panel which is one form of a display device refers to a panel which can display (output) an image etc. on a display surface. Therefore, a display panel is one form of an output device.

[0069] In addition, in this specification, etc., a structure in which a connector such as an FPC (Flexible Printed Circuit) or TCP (Tape Carrier Package) is installed on a display panel substrate, or a structure in which an IC (Integrated Circuit) is directly installed on a substrate using a COG (Chip On Glass) method, etc. is sometimes referred to as a display panel module or display module, or simply as a display panel, etc.

[0070] Note that in this specification, a touch panel, which is one form of a display device, has the following functions: a function of displaying an image on a display surface; and a function of acting as a touch sensor that detects when a detected object, such as a finger or a stylus pen, touches, presses, or approaches the display surface. Therefore, a touch panel is one form of an input / output device.

[0071] A touch panel may also be referred to as a display panel (or display device) having a touch sensor, or a display panel (or display device) having a touch sensor function. A touch panel may also include a display panel and a touch sensor panel. Alternatively, a structure may have a touch sensor function inside or on the surface of a display panel.

[0072] In this specification and the like, a structure in which a connector or an IC is mounted on a substrate of a touch panel may be referred to as a touch panel module, a display module, or simply as a touch panel.

[0073] (Implementation Method 1)

[0074] In this embodiment, a semiconductor device and a method for manufacturing the semiconductor device according to one embodiment of the present invention are described. In particular, in this embodiment, a transistor using an oxide semiconductor in a semiconductor layer forming a channel is described as an example of a semiconductor device.

[0075] [Structural Example 1]

[0076] <Structural Example 1-1>

[0077] Figure 1A A schematic cross-sectional view along the channel length direction of the transistor 10 is shown.

[0078] The transistor 10 includes an insulating layer 103, a semiconductor layer 108, an insulating layer 110, a metal oxide layer 114, and a conductive layer 112. The insulating layer 110 serves as a gate insulating layer, and the conductive layer 112 serves as a gate electrode.

[0079] The conductive layer 112 is preferably formed using a conductive film containing a metal or an alloy because resistance can be suppressed. Note that a conductive film containing an oxide can also be used as the conductive layer 112.

[0080] The metal oxide layer 114 has a function of supplying oxygen to the insulating layer 110. Further, when a conductive film including an easily oxidizable metal or alloy is used as the conductive layer 112, the metal oxide layer 114 can be used as a barrier layer for preventing the conductive layer 112 from being oxidized by oxygen in the insulating layer 110. Note that the conductive layer 112 can be made to be in contact with the insulating layer 110 by removing the metal oxide layer 114 before forming the conductive layer 112.

[0081] The insulating layer 103 is preferably formed of an insulating film containing an oxide. In particular, an oxide film is preferably used for a portion in contact with the semiconductor layer 108.

[0082] The semiconductor layer 108 includes a metal oxide (hereinafter also referred to as an oxide semiconductor) having semiconductor characteristics. The semiconductor layer 108 preferably includes at least indium and oxygen. When the semiconductor layer 108 includes an indium oxide, carrier mobility can be improved. For example, a transistor capable of passing a larger current than a transistor using amorphous silicon can be realized.

[0083] The region of the semiconductor layer 108 overlapping the conductive layer 112 is used as a channel formation region. In addition, the semiconductor layer 108 preferably includes a pair of low resistance regions 108n sandwiching the channel formation region. The low resistance regions 108n each have a higher carrier concentration than the channel formation region and are used as a source region and a drain region.

[0084] The low resistance region 108n may be referred to as a region having lower resistance than the channel formation region, a region having a higher carrier concentration, a region having a larger amount of oxygen vacancies, a region having a higher hydrogen concentration, or a region having a higher impurity concentration.

[0085] The insulating layer 110 has a stacked structure in which an insulating film 110a, an insulating film 110b, and an insulating film 110c are stacked in this order from the insulating layer 103. The insulating film 110a has a region in contact with the channel formation region of the semiconductor layer 108. The insulating film 110c has a region in contact with the metal oxide layer 114. The insulating film 110b is located between the insulating film 110a and the insulating film 110c.

[0086] The insulating film 110a, the insulating film 110b, and the insulating film 110c are preferably insulating films each containing an oxide. At this time, the insulating film 110a, the insulating film 110b, and the insulating film 110c are preferably formed continuously in the same deposition apparatus.

[0087] As each of the insulating films 110a, 110b and 110c, for example, an insulating layer including one or more of a silicon oxide film, a silicon oxynitride film, a silicon nitride oxide film, an aluminum oxide film, a hafnium oxide film, a yttrium oxide film, a zirconium oxide film, a gallium oxide film, a tantalum oxide film, a magnesium oxide film, a lanthanum oxide film, a cerium oxide film and a neodymium oxide film can be used.

[0088] The insulating layer 110 in contact with the semiconductor layer 108 preferably has a stacked structure of oxide insulating films. In addition, the insulating layer 110 more preferably has a region containing oxygen exceeding the stoichiometric composition. In other words, the insulating layer 110 includes an insulating film capable of releasing oxygen. For example, oxygen can be supplied to the insulating layer 110 by forming the insulating layer 110 in an oxygen atmosphere; by performing heat treatment, plasma treatment, etc. on the formed insulating layer 110 in an oxygen atmosphere; or by forming an oxide film on the insulating layer 110 in an oxygen atmosphere.

[0089] Each of the insulating film 110a, the insulating film 110b, and the insulating film 110c can be formed by any method such as sputtering, chemical vapor deposition (CVD: Chemical Vapor Deposition), vacuum evaporation, pulsed laser deposition (PLD: Pulsed Laser Deposition), atomic layer deposition (ALD: Atomic Layer Deposition), etc. As the CVD method, a plasma enhanced chemical vapor deposition (PECVD: Plasma Enhanced CVD) method, a thermal CVD method, etc. can be used.

[0090] In particular, the insulating film 110 a , the insulating film 110 b , and the insulating film 110 c are preferably formed by a PECVD method.

[0091] Since the insulating film 110a is formed on the semiconductor layer 108, it is preferable to form it under the condition that the semiconductor layer 108 is damaged as little as possible. For example, the insulating film 110a can be formed under the condition that the deposition rate is sufficiently low.

[0092] For example, when a silicon oxynitride film is formed as the insulating film 110 a by the PECVD method, damage to the semiconductor layer 108 can be minimized by forming the film under low power conditions.

[0093] As a formation gas for forming a silicon oxynitride film, for example, a deposition gas containing silicon such as silane or disilane and a source gas containing an oxidizing gas such as oxygen, ozone, nitrous oxide, or nitrogen dioxide may be used. In addition to the source gas, a diluent gas such as argon, helium, or nitrogen may be included.

[0094] For example, by reducing the ratio of the flow rate of the deposition gas to the total flow rate of the formation gas (hereinafter referred to simply as flow rate ratio), the deposition rate can be reduced, thereby forming a dense film with few defects.

[0095] The insulating film 110b is preferably formed under a condition where its deposition rate is higher than that of the insulating film 110a. Thus, productivity can be improved.

[0096] For example, when a condition of increasing the flow rate ratio of the deposition gas compared to the insulation film 110 a is adopted, the insulation film 110 b can be formed under the condition of increasing the deposition rate.

[0097] The insulating film 110c is preferably a very dense film with reduced surface defects and less prone to adsorbing impurities such as water contained in the atmosphere. For example, the insulating film 110c can be formed under conditions of a sufficiently low deposition rate, similarly to the insulating film 110a.

[0098] Since the insulating film 110c is formed on the insulating film 110b, the influence on the semiconductor layer 108 when forming the insulating film 110c is small compared with the formation of the insulating film 110a. Therefore, the insulating film 110c can be formed under high power conditions compared with the insulating film 110a. By reducing the flow rate ratio of the deposition gas and forming the film at a higher power, a dense film with reduced surface defects can be achieved.

[0099] In other words, the insulating layer 110 can be formed using a stacked film formed under conditions where the deposition rate of the insulating film 110b is the highest, the insulating film 110a is the second highest, and the insulating film 110c is the lowest. In addition, in the insulating layer 110, when wet etching or dry etching is performed under the same conditions, the etching rate of the insulating layer 110b is the highest, the insulating film 110a is the second highest, and the insulating film 110c is the lowest.

[0100] The insulating film 110b is preferably formed thicker than the insulating film 110a and the insulating film 110c. By forming the insulating film 110b formed at the highest deposition rate thicker, the time required for the formation step of the insulating layer 110 can be shortened.

[0101] Here, since the boundary between the insulating film 110a and the insulating film 110b and the boundary between the insulating film 110b and the insulating film 110c are sometimes unclear, Figure 1A In the figure, the boundaries are indicated by dotted lines. Note that since the film density of the insulating film 110a is different from that of the insulating film 110b, the boundaries can sometimes be observed by the difference in contrast in a transmission electron microscope (TEM: Transmission Electron Microscopy) image of the cross section of the insulating layer 110. Similarly, the boundary between the insulating film 110b and the insulating film 110c can sometimes be observed by the difference in contrast.

[0102] Here, the composition of the semiconductor layer 108 is described. The semiconductor layer 108 preferably includes a metal oxide containing at least indium and oxygen. In addition, the semiconductor layer 108 may further include zinc. The semiconductor layer 108 may also include gallium.

[0103] Typically, indium oxide, indium zinc oxide (In-Zn oxide), indium gallium zinc oxide (also referred to as In-Ga-Zn oxide or IGZO), or the like can be used as the semiconductor layer 108. In addition, indium tin oxide (In-Sn oxide) or indium tin oxide containing silicon can be used. Note that the details of the material that can be used for the semiconductor layer 108 will be described later.

[0104] Here, the composition of the semiconductor layer 108 greatly affects the electrical characteristics and reliability of the transistor 10. For example, by increasing the indium content in the semiconductor layer 108, carrier mobility can be increased, thereby realizing a transistor with high field effect mobility.

[0105] Here, as one of the indicators for evaluating the reliability of transistors, there is a gate bias stress test (GBT) in which an electric field applied to the gate is maintained. The GBT test includes a PBTS (Positive Bias Temperature Stress) test in which a positive potential relative to the source potential and the drain potential is applied to the gate and maintained at a high temperature, and an NBTS (Negative Bias Temperature Stress) test in which a negative potential is applied to the gate and maintained at a high temperature. In addition, the PBTS test and the NBTS test performed under the state of irradiating light such as white LED light are respectively referred to as the PBTIS (Positive Bias Temperature Illumination Stress) test and the NBTIS (Negative Bias Temperature Illumination Stress) test.

[0106] In particular, in an n-type transistor including an oxide semiconductor, a positive potential is applied to the gate when the transistor is turned on (a state where current flows), so the variation in threshold voltage in the PBTS test is one of the important factors focusing on the reliability index of the transistor.

[0107] Here, a metal oxide film containing no gallium or having a low gallium content is used as the semiconductor layer 108, thereby reducing the variation of the threshold voltage in the PBTS test. In addition, when gallium is contained, the gallium content in the semiconductor layer 108 is preferably lower than the indium content. Thus, a transistor with high reliability can be realized.

[0108] One of the reasons for the change in threshold voltage in the PBTS test is the defect state at or near the interface between the semiconductor layer and the gate insulating layer. The greater the defect state density, the more significant the degradation in the PBTS test. The generation of the defect state can be suppressed by reducing the gallium content in the portion of the semiconductor layer that contacts the gate insulating layer.

[0109] The reason why PBTS degradation can be suppressed when the semiconductor layer 108 does not contain gallium or the gallium content is very low is, for example, as follows. Gallium contained in the semiconductor layer 108 is more likely to attract oxygen than other metal elements (such as indium or zinc). Therefore, when gallium is bonded to excess oxygen in the insulating layer 110 at the interface between the metal oxide film containing more gallium and the insulating layer 110 containing oxide, carrier (here, electron) trap sites are easily generated. Therefore, when a positive potential is applied to the gate and carriers are trapped at the interface between the semiconductor layer and the gate insulating layer, the threshold voltage changes.

[0110] Specifically, when In-Ga-Zn oxide is used as the semiconductor layer 108, a metal oxide film in which the atomic ratio of In is higher than the atomic ratio of Ga can be used as the semiconductor layer 108. It is more preferable to use a metal oxide film in which the atomic ratio of Zn is higher than the atomic ratio of Ga. In other words, a metal oxide film in which the atomic ratio of metal elements satisfies In>Ga and Zn>Ga is used as the semiconductor layer 108.

[0111] For example, as the semiconductor layer 108, a metal oxide film having an atomic number ratio of metal elements of In:Ga:Zn=2:1:3, In:Ga:Zn=3:1:2, In:Ga:Zn=4:2:3, In:Ga:Zn=4:2:4.1, In:Ga:Zn=5:1:6, In:Ga:Zn=5:1:7, In:Ga:Zn=5:1:8, In:Ga:Zn=6:1:6, In:Ga:Zn=5:2:5, and any atomic number ratio thereabouts can be used.

[0112] When a metal oxide film containing indium and gallium is used as the semiconductor layer 108, the ratio of gallium atoms contained in the metal oxide to atoms of the metal element (atomic ratio) is greater than 0 and less than 50%, preferably greater than 0.05% and less than 30%, more preferably greater than 0.1% and less than 15%, and further preferably greater than 0.1% and less than 5%. Note that when the semiconductor layer 108 contains gallium, oxygen vacancies are less likely to be generated.

[0113] As the semiconductor layer 108, a metal oxide film that does not contain gallium can also be used. For example, In-Zn oxide can be used for the semiconductor layer 108. At this time, when the atomic ratio of In contained in the metal oxide film relative to the metal element is increased, the field effect mobility of the transistor can be improved. On the other hand, when the atomic ratio of Zn contained in the metal oxide relative to the metal element is increased, the metal oxide film has high crystallinity, so the variation of the electrical characteristics of the transistor can be suppressed, and the reliability can be improved. In addition, as the semiconductor layer 108, a metal oxide film that does not contain gallium and zinc, such as indium oxide, can be used. By using a metal oxide film that does not contain gallium, the variation of the threshold voltage in the PBTS test can be made extremely small, especially.

[0114] In the transistor 10 according to one embodiment of the present invention, a metal oxide film having a low gallium content or a metal oxide film containing no gallium is used as the semiconductor layer 108, and a film formed by a deposition method that reduces damage to the semiconductor layer 108 is used as the insulating film 110a in contact with the top surface of the semiconductor layer 108. Therefore, the defect state density at the interface between the semiconductor layer 108 and the insulating layer 110 can be reduced, and thus the transistor 10 can have high reliability.

[0115] Although the case of using gallium is described as an example, the same contents can also be applied to the case of using element M (M is one or more of aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten and magnesium) instead of gallium. In particular, M is preferably one or more of gallium, aluminum, yttrium and tin.

[0116] In particular, a metal oxide film in which the atomic ratio of In is higher than the atomic ratio of the element M is preferably used as the semiconductor layer 108. In addition, a metal oxide film in which the atomic ratio of Zn is higher than the atomic ratio of the element M is preferably used.

[0117] A crystalline metal oxide film is preferably used as the semiconductor layer 108. For example, a metal oxide film having a CAAC (c-axis aligned crystal) structure, a polycrystalline structure, a microcrystalline structure, or the like described later can be used. By using a crystalline metal oxide film as the semiconductor layer 108, the defect state density in the semiconductor layer 108 can be reduced, thereby realizing a semiconductor device with high reliability.

[0118] The higher the crystallinity of the semiconductor layer 108 is, the lower the defect state density in the film. On the other hand, by using a metal oxide film with low crystallinity, a transistor capable of passing a large current can be realized.

[0119] When a metal oxide film is formed by sputtering, the higher the substrate temperature (stage temperature) during film formation, the higher the crystallinity of the metal oxide film can be. The higher the flow rate ratio of the oxygen gas relative to the entire forming gas used in film formation (also referred to as the oxygen flow rate ratio) is, the higher the crystallinity of the metal oxide film can be.

[0120] <Structural Example 1-2>

[0121] Figure 1B 1 is a schematic cross-sectional view of a transistor 10A. The transistor 10A is different from the above-described transistor 10 mainly in the structure of the semiconductor layer 108.

[0122] The semiconductor layer 108 included in the transistor 10A has a stacked-layer structure in which a semiconductor layer 108a and a semiconductor layer 108b are stacked from the insulating layer 103 side. It is preferable that a metal oxide film is used for each of the semiconductor layer 108a and the semiconductor layer 108b.

[0123] Note that for convenience, the low resistance region included in the semiconductor layer 108a and the low resistance region included in the semiconductor layer 108b are collectively referred to as a low resistance region 108n and are shown with the same hatching. In practice, since the semiconductor layer 108a and the semiconductor layer 108b have different compositions, the low resistance region 108n in the semiconductor layer 108a and the low resistance region 108n in the semiconductor layer 108b may differ in resistivity, carrier concentration, oxygen vacancy amount, hydrogen concentration, or impurity concentration.

[0124] The semiconductor layer 108b is in contact with the top surface of the semiconductor layer 108a and the bottom surface of the insulating film 110a. As the semiconductor layer 108b, the metal oxide film that can be used for the semiconductor layer 108 described in the above Structural Example 1-1 can be used.

[0125] On the other hand, the semiconductor layer 108a may use a metal oxide film having a higher atomic ratio of gallium than that of the semiconductor layer 108b.

[0126] Gallium has a stronger bonding force with oxygen than indium, so when a metal oxide film having a high atomic ratio of gallium is used as the semiconductor layer 108a, oxygen vacancies are less likely to form. A large amount of oxygen vacancies in the semiconductor layer 108a leads to a decrease in the electrical characteristics and reliability of the transistor. Therefore, when a metal oxide film having a higher atomic ratio of gallium than the semiconductor layer 108b is used as the semiconductor layer 108a, a transistor 10A having good electrical characteristics and high reliability can be realized.

[0127] Specifically, the semiconductor layer 108a can be formed using a metal oxide film containing indium, gallium, and zinc and including a region where the atomic ratio of gallium is higher than that of the semiconductor layer 108b and the atomic ratio of indium is lower than that of the semiconductor layer 108b. In other words, the semiconductor layer 108b can be formed using a metal oxide film including a region where the atomic ratio of indium is higher than that of the semiconductor layer 108a and the atomic ratio of gallium is lower than that of the semiconductor layer 108a.

[0128] As the semiconductor layer 108a, a metal oxide film including a region in which the atomic ratio of zinc is lower than or equal to the atomic ratio of zinc in the semiconductor layer 108b is preferably used.

[0129] For example, as the semiconductor layer 108a, a metal oxide film having an atomic ratio of metal elements of In:Ga:Zn=1:1:1, In:Ga:Zn=1:3:2, In:Ga:Zn=1:3:4, In:Ga:Zn=1:3:6, In:Ga:Zn=2:2:1 or a vicinity thereof can be used.

[0130] Typically, as the semiconductor layer 108a, a metal oxide film in which the atomic ratio of the metal elements is In:Ga:Zn=1:1:1 or thereabouts is preferably used, and as the semiconductor layer 108b, a metal oxide film in which the atomic ratio of the metal elements is In:Ga:Zn=4:2:3, In:Ga:Zn=5:1:6 or thereabouts is preferably used.

[0131] When a metal oxide film in which oxygen vacancies are less likely to be generated is used as the semiconductor layer 108 a , degradation in the above-mentioned NBTIS test can be reduced.

[0132] exist Figure 1B In the transistor 10A shown, a metal oxide film having a high gallium content is used as the semiconductor layer 108a located on the insulating layer 103 side, thereby reducing oxygen vacancies in the semiconductor layer 108. Furthermore, a metal oxide film having a low gallium content or containing no gallium is used as the semiconductor layer 108b located on the insulating layer 110 side, thereby reducing the interface defect density between the semiconductor layer 108 and the insulating layer 110. Therefore, the transistor 10A has extremely high electrical characteristics and extremely high reliability.

[0133] Here, the semiconductor layer 108b is preferably formed thinner than the semiconductor layer 108a. Even if the semiconductor layer 108b is an extremely thin film of, for example, 0.5 nm or more and 10 nm or less, the interface defect density with the insulating layer 110 can be reduced. On the other hand, by making the semiconductor layer 108a, in which oxygen vacancies are less likely to be generated, relatively thick, a transistor with higher reliability can be realized.

[0134] For example, the thickness of the semiconductor layer 108a may be 1.5 to 20 times the thickness of the semiconductor layer 108b, preferably 2 to 15 times, more preferably 3 to 10 times. The thickness of the oxide semiconductor layer 108b is preferably 0.5 nm to 30 nm, preferably 1 nm to 20 nm, more preferably 2 nm to 10 nm.

[0135] The above-mentioned metal oxide film having crystallinity is preferably used as each of the semiconductor layer 108a and the semiconductor layer 108b. A metal oxide film having high crystallinity or a metal oxide film having low crystallinity can be used as both the semiconductor layer 108a and the semiconductor layer 108b. Alternatively, the semiconductor layer 108a and the oxide semiconductor layer 108b may have different crystallinities. For example, the crystallinity of the semiconductor layer 108a may be higher than that of the semiconductor layer 108b, or the crystallinity of the semiconductor layer 108b may be higher than that of the semiconductor layer 108a. The crystallinity of the metal oxide film used as each of the semiconductor layer 108a and the semiconductor layer 108b can be determined based on the electrical characteristics and reliability of the required transistor and the specifications of the deposition device, etc.

[0136] <Structural Examples 1-3>

[0137] Figure 2A 10B is a schematic cross-sectional view of a transistor 10B. The difference between the transistor 10B and the transistor 10 is mainly in the structure of the insulating layer 103 and the presence of the conductive layer 106.

[0138] The conductive layer 106 includes a region overlapping with the semiconductor layer 108, the insulating layer 110, the metal oxide layer 114, and the conductive layer 112 via the insulating layer 103. The conductive layer 106 is used as a first gate electrode (also referred to as a back gate electrode). The insulating layer 103 is used as a first gate insulating layer. In this case, the conductive layer 112 is used as a second gate electrode, and the insulating layer 110 is used as a second gate insulating layer.

[0139] For example, when the same potential is applied to the conductive layer 112 and the conductive layer 106, the current that can flow through the transistor 10B in the on state can be increased. In addition, in the transistor 10B, a potential for controlling a threshold voltage can be supplied to one of the conductive layer 112 and the conductive layer 106, and a potential for controlling the on / off state of the transistor 10B can be supplied to the other of the conductive layer 112 and the conductive layer 106.

[0140] The insulating layer 103 has a stacked structure in which an insulating film 103a, an insulating film 103b, an insulating film 103c, and an insulating film 103d are stacked from the conductive layer 106 side. The insulating film 103a is in contact with the conductive layer 106. The insulating film 103d is in contact with the semiconductor layer 108.

[0141] The insulating layer 103 used as the second gate insulating layer preferably satisfies at least one of the following characteristics, and more preferably satisfies all of the following characteristics: high voltage resistance, low stress, not easy to release hydrogen and water, few defects, and prevention of diffusion of metal elements contained in the conductive layer 106.

[0142] Among the four insulating films included in the insulating layer 103, each of the insulating film 103a, the insulating film 103b, and the insulating film 103c located on the side of the conductive layer 106 is preferably formed using an insulating film containing nitrogen. On the other hand, the insulating film 103d in contact with the semiconductor layer 108 is preferably formed using an insulating film containing oxygen. The four insulating films included in the insulating layer 103 are preferably formed continuously without being exposed to the atmosphere using a plasma CVD apparatus.

[0143] Each of the insulating films 103a, 103b, and 103c can be made of an insulating film containing nitrogen, such as silicon nitride, silicon nitride oxide, aluminum nitride, or hafnium nitride. Alternatively, the insulating film 103c can be any insulating film that can be used as the insulating layer 110.

[0144] The insulating film 103a and the insulating film 103c are preferably dense films that prevent diffusion of impurities from the underlying layer. It is preferable that the insulating film 103a can block the metal elements contained in the conductive layer 106, and the insulating film 103c can block hydrogen and water contained in the insulating film 103b. Therefore, each of the insulating film 103a and the insulating film 103c can use an insulating film formed at a lower deposition rate than the insulating film 103b.

[0145] On the other hand, the insulating film 103b is preferably formed using an insulating film having low stress and formed at a high deposition rate. The insulating film 103b is preferably thicker than the insulating film 103a and the insulating film 103c.

[0146] For example, when silicon nitride films formed by PECVD are used as the insulating films 103a, 103b, and 103c, the film density of the insulating film 103b is smaller than that of the other two insulating films. Therefore, a difference in contrast is observed in the transmission electron microscope image of the cross section of the insulating layer 103, and these films can sometimes be distinguished. Since the boundaries between the insulating films 103a and 103b and the boundaries between the insulating films 103b and 103c are unclear, Figure 2A These boundaries are shown as dashed lines in FIG.

[0147] As the insulating film 103d in contact with the semiconductor layer 108, a dense insulating film whose surface is not easily adsorbed with impurities such as water is preferably used. In addition, it is preferable to use an insulating film with as few defects as possible and with reduced impurities such as water and hydrogen. For example, the insulating film 103d can be the same as the insulating film 110c included in the insulating layer 110 described above.

[0148] For example, when a metal film or alloy film whose constituent elements are not easily diffused into the insulating layer 103 is used as the conductive layer 106, a structure of three insulating films including the insulating film 103b, the insulating film 103c, and the insulating film 103d can be stacked instead of the insulating film 103a.

[0149] By using the insulating layer 103 having such a stacked-layer structure, the transistor can have extremely high reliability.

[0150] <Structural Examples 1-4>

[0151] Figure 2B 1 is a schematic cross-sectional view of a transistor 10C. The transistor 10C is an example in which the conductive layer 106 and the insulating layer 103 included in the transistor 10B shown in the above structural example 1-3 are applied to the transistor 10A shown in the above structural example 1-2.

[0152] By adopting this structure, a transistor having excellent electrical characteristics and extremely high reliability can be realized.

[0153] [Structural Example 2]

[0154] A more specific example of the structure of the transistor will be described below.

[0155] <Structural Example 2-1>

[0156] Figure 3A is a top view of transistor 100 . Figure 3B It is along Figure 3A The cross-sectional view cut along the dot-dash line A1-A2 shown in FIG. Figure 3C It is along Figure 3A The cross-sectional view is shown along the dashed line B1-B2. Figure 3A In the figure, some components of transistor 100 (gate insulating layer, etc.) are not shown. The dot-dash line A1-A2 direction corresponds to the channel length direction, and the dot-dash line B1-B2 direction corresponds to the channel width direction. Figure 3A Likewise, some components are not shown.

[0157] The transistor 100 is provided on a substrate 102 and includes an insulating layer 103, a semiconductor layer 108, an insulating layer 110, a metal oxide layer 114, a conductive layer 112, an insulating layer 118, and the like. The island-shaped semiconductor layer 108 is provided on the insulating layer 103. The insulating layer 110 is provided in a manner of contacting the top surface of the insulating layer 103 and the top surface and side surface of the semiconductor layer 108. The metal oxide layer 114 and the conductive layer 112 are provided on the insulating layer 110 in sequence and have a portion overlapping with the semiconductor layer 108. The insulating layer 118 is provided in a manner of covering the top surface of the insulating layer 110, the side surface of the metal oxide layer 114, and the top surface of the conductive layer 112.

[0158] The insulating layer 103 has a stacked-layer structure including insulating films 103a, 103b, 103c, and 103d stacked from the substrate 102 side. The insulating layer 110 has a stacked-layer structure including insulating films 110a, 110b, and 110c stacked from the semiconductor layer 108 side.

[0159] like Figure 3A and Figure 3B As shown, the transistor 100 may also include a conductive layer 120a and a conductive layer 120b on the insulating layer 118. The conductive layer 120a and the conductive layer 120b are used as a source electrode and a drain electrode. The conductive layer 120a and the conductive layer 120b are electrically connected to the low resistance region 108n through the openings 141a and the openings 141b provided in the insulating layer 118 and the insulating layer 110.

[0160] A portion of the conductive layer 112 is used as a gate electrode. A portion of the insulating layer 110 is used as a gate insulating layer. The transistor 100 is a so-called top-gate transistor in which a gate electrode is provided over the semiconductor layer 108 .

[0161] The conductive layer 112 and the metal oxide layer 114 are processed to have substantially the same top surface shapes.

[0162] In this specification, etc., "the top surface shapes are substantially consistent" means that at least a portion of the edges of each layer in the stack overlap. For example, it refers to the case where a part or all of the upper layer and the lower layer are processed using the same mask pattern. However, in reality, there are cases where the edges do not overlap, for example, the upper layer is located inside the lower layer or the upper layer is located outside the lower layer. In this case, it can also be said that "the top surface shapes are substantially consistent."

[0163] The metal oxide layer 114 located between the insulating layer 110 and the conductive layer 112 is used as a barrier film for preventing oxygen contained in the insulating layer 110 from diffusing toward the conductive layer 112. Furthermore, the metal oxide layer 114 is also used as a barrier film for preventing hydrogen and water contained in the conductive layer 112 from diffusing toward the insulating layer 110. The metal oxide layer 114 is preferably formed using a material that is less likely to transmit oxygen and hydrogen than the insulating layer 110, for example.

[0164] Even when a metal material that easily absorbs oxygen, such as aluminum or copper, is used for the conductive layer 112, the metal oxide layer 114 can prevent oxygen from diffusing from the insulating layer 110 to the conductive layer 112. Further, even when the conductive layer 112 contains hydrogen, hydrogen can be prevented from diffusing from the conductive layer 112 through the insulating layer 110 to the semiconductor layer 108. As a result, the carrier density in the channel formation region of the semiconductor layer 108 can be made extremely low.

[0165] An insulating material or a conductive material can be used as the metal oxide layer 114. When the metal oxide layer 114 has insulating properties, the metal oxide layer 114 is used as a part of a gate insulating layer. On the other hand, when the metal oxide layer 114 has conductive properties, the metal oxide layer 114 is used as a part of a gate electrode.

[0166] In particular, an insulating material having a higher dielectric constant than silicon oxide is preferably used as the metal oxide layer 114. In particular, an aluminum oxide film, a hafnium oxide film, a hafnium aluminate film, or the like is preferably used because a driving voltage can be reduced.

[0167] The metal oxide layer 114 may be formed using a conductive oxide such as indium oxide, indium tin oxide (ITO), or indium tin oxide containing silicon (ITSO). In particular, a conductive oxide containing indium is preferably used because it has high conductivity.

[0168] In addition, as the metal oxide layer 114, it is preferable to use an oxide material containing one or more elements of the semiconductor layer 108. In particular, it is preferable to use an oxide semiconductor material that can be used for the above-mentioned semiconductor layer 108. In this case, by using a metal oxide film formed using the same sputtering target as the semiconductor layer 108 as the metal oxide layer 114, it is possible to share equipment, which is preferable.

[0169] The metal oxide layer 114 is preferably formed using a sputtering device. For example, when an oxide film is formed using a sputtering device, oxygen can be appropriately added to the insulating layer 110 and the semiconductor layer 108 by forming the oxide film in an atmosphere including an oxygen gas.

[0170] The semiconductor layer 108 includes a region overlapping with the conductive layer 112 and a pair of low resistance regions 108n sandwiching the region. The region of the semiconductor layer 108 overlapping with the conductive layer 112 is used as a channel formation region of the transistor 100. The pair of low resistance regions 108n are used as a source region and a drain region of the transistor 100.

[0171] The low resistance region 108n may be a region having lower resistance than the channel formation region, a region having a higher carrier concentration, a region having a higher oxygen vacancy density, a region having a higher impurity concentration, or a region exhibiting n-type.

[0172] The low resistance region 108n of the semiconductor layer 108 contains an impurity element. Examples of the impurity element include hydrogen, boron, carbon, nitrogen, fluorine, phosphorus, sulfur, arsenic, aluminum, and rare gas elements. Typical examples of rare gas elements include helium, neon, argon, krypton, and xenon. In particular, it is preferred to contain boron or phosphorus. In addition, two or more of these elements may be contained.

[0173] As described later, impurities can be added to the low-resistance region 108n through the insulating layer 110 using the conductive layer 112 as a mask.

[0174] The low resistance regions 108n preferably each contain an impurity concentration of 1×10 19 atoms / cm 3 Above and 1×10 23 atoms / cm 3 Below, preferably 5×10 19 atoms / cm 3 Above and 5×10 22 atoms / cm 3 Below, more preferably 1×10 20 atoms / cm 3 Above and 1×10 22 atoms / cm 3 The following area.

[0175] For example, the concentration of impurities contained in the low resistance region 108n can be analyzed by using analysis methods such as secondary ion mass spectrometry (SIMS) and X-ray photoelectron spectroscopy (XPS). When XPS analysis is used, the concentration distribution in the depth direction can be obtained by combining ion sputtering from the surface side or the back side and XPS analysis.

[0176] In addition, the impurity elements in the low resistance region 108n are preferably oxidized. For example, as the impurity elements, it is preferable to use an element that is easily oxidized, such as boron, phosphorus, magnesium, aluminum, and silicon. Such an easily oxidized element can stably exist in a state of being bonded to oxygen in the semiconductor layer 108 and oxidized, so that even if a high temperature (for example, 400°C or more, 600°C or more, or 800°C or more) is applied in the subsequent process, the detachment of the element can be suppressed. In addition, the impurity element deprives the semiconductor layer 108 of oxygen, thereby generating many oxygen vacancies in the low resistance region 108n. The oxygen vacancies bond with hydrogen in the film to become a carrier supply source, so that the low resistance region 108n becomes an extremely low resistance state.

[0177] For example, when boron is used as an impurity element, the boron contained in the low resistance region 108n may be present in a state of being bonded to oxygen. This can be confirmed by observing a spectral peak due to B2O3 bonding in XPS analysis. In addition, in XPS analysis, a spectral peak due to elemental boron is not observed or its peak intensity is so small that it is buried in the background noise detected near the lower limit of detection.

[0178] The insulating layer 110 includes a region in contact with the channel formation region of the semiconductor layer 108, that is, a region overlapping the conductive layer 112. The insulating layer 110 also includes a region in contact with the low resistance region 108n of the semiconductor layer 108 and not overlapping the conductive layer 112.

[0179] The region of the insulating layer 110 overlapping the low resistance region 108n may contain the above-mentioned impurity element. In this case, the impurity element in the insulating layer 110 is preferably present in a state of being bonded to oxygen, as in the low resistance region 108n. Such an element that is easily oxidized can be stably present in a state of being bonded to oxygen in the insulating layer 110 and oxidized, so that even if a high temperature is applied in a subsequent process, the detachment of the element can be suppressed. In particular, when the insulating layer 110 contains oxygen that can be detached by heating (also called excess oxygen), the excess oxygen is bonded to the impurity element and stabilized, thereby suppressing the supply of oxygen from the insulating layer 110 to the low resistance region 108n. In addition, since oxygen is not easily diffused into a part of the insulating layer 110 containing the oxidized impurity element, the supply of oxygen from the insulating layer 110 through the insulating layer 110 to the low resistance region 108n can also be prevented from becoming high-resistance in the low resistance region 108n.

[0180] The insulating layer 118 is used as a protective layer for protecting the transistor 100. For example, an inorganic insulating material such as oxide or nitride can be used as the insulating layer 110. Specifically, an inorganic insulating material such as silicon oxide, silicon oxynitride, silicon nitride, silicon nitride oxide, aluminum oxide, aluminum oxynitride, aluminum nitride, hafnium oxide, or hafnium aluminate can be used.

[0181] <Structural Example 2-2>

[0182] Figure 4A is a top view of transistor 100A, Figure 4B is a cross-sectional view of the transistor 100A in the channel length direction. Figure 4C It is a cross-sectional view of the transistor 100A in the channel width direction.

[0183] The transistor 100A is different from the transistor of Structural Example 2-1 mainly in that a conductive layer 106 is included between the substrate 102 and the insulating layer 103. The conductive layer 106 includes a region overlapping with the semiconductor layer 108 and the conductive layer 112.

[0184] In the transistor 100A, the conductive layer 112 is used as a second gate electrode (also referred to as a top gate electrode), and the conductive layer 106 is used as a first gate electrode (also referred to as a bottom gate electrode). In addition, a portion of the insulating layer 110 is used as a second gate insulating layer, and a portion of the insulating layer 103 is used as a first gate insulating layer.

[0185] A portion of the semiconductor layer 108 that overlaps with at least one of the conductive layer 112 and the conductive layer 106 is used as a channel formation region. Below, for convenience of description, the portion of the semiconductor layer 108 that overlaps with the conductive layer 112 is sometimes referred to as a channel formation region, but in fact, a channel is sometimes formed in a portion of the semiconductor layer 108 that does not overlap with the conductive layer 112 but overlaps with the conductive layer 106 (including a portion of the low resistance region 108n).

[0186] In addition, if Figure 4C As shown, the conductive layer 106 can be electrically connected to the conductive layer 112 through the opening 142 provided in the metal oxide layer 114, the insulating layer 110, and the insulating layer 103. Thus, the conductive layer 106 and the conductive layer 112 can be supplied with the same potential.

[0187] The conductive layer 106 can be formed using the same material as the conductive layer 112, the conductive layer 120a, or the conductive layer 120b. In particular, when a material containing copper is used for the conductive layer 106, wiring resistance can be reduced, which is preferred.

[0188] In addition, if Figure 4A and Figure 4C As shown in FIG. 1 , it is preferred that the conductive layer 112 and the conductive layer 106 extend beyond the end of the semiconductor layer 108 in the channel width direction. Figure 4C As shown, the conductive layer 112 and the conductive layer 106 cover the entire semiconductor layer 108 in the channel width direction via the insulating layer 110 between the semiconductor layer 108 and the conductive layer 112 and the insulating layer 103 between the semiconductor layer 108 and the conductive layer 112 .

[0189] By adopting the above structure, the semiconductor layer 108 can be electrically surrounded by the electric field generated by the pair of gate electrodes. In this case, it is particularly preferable to supply the same potential to the conductive layer 106 and the conductive layer 112. Thus, the electric field for inducing the channel can be effectively applied to the semiconductor layer 108, and the on-state current of the transistor 100A can be increased. Therefore, the miniaturization of the transistor 100A can be achieved.

[0190] Note that the conductive layer 112 may not be connected to the conductive layer 106. In this case, a fixed potential may be supplied to one of the pair of gate electrodes, and a signal for driving the transistor 100A may be supplied to the other. In this case, the threshold voltage when the transistor 100A is driven by the other gate electrode can be controlled by using the potential supplied to one gate electrode.

[0191] <Structural Example 2-3>

[0192] Figure 5A is a top view of transistor 100B, Figure 5B is a cross-sectional view of the transistor 100B in the channel length direction. Figure 5CIt is a cross-sectional view of the transistor 100B in the channel width direction.

[0193] The difference between transistor 100B and transistor 100 shown in structural example 2-1 mainly lies in the structure of insulating layer 110 and the existence of insulating layer 116.

[0194] The insulating layer 110 is processed to have a top surface shape substantially identical to the top surface shapes of the conductive layer 112 and the metal oxide layer 114. The insulating layer 110 can be formed by using a resist mask used to process the conductive layer 112 and the metal oxide layer 114, for example.

[0195] The insulating layer 116 is provided in contact with the top surface and side surfaces of the semiconductor layer 108 that are not covered by the conductive layer 112, the metal oxide layer 114, and the insulating layer 110. The insulating layer 116 is provided to cover the top surface of the insulating layer 103, the side surfaces of the insulating layer 110, the side surfaces of the metal oxide layer 114, and the top surface and side surfaces of the conductive layer 112.

[0196] The insulating layer 116 has a function of lowering the resistance of the low resistance region 108n. The insulating layer 116 can be formed using an insulating film that supplies impurities to the low resistance region 108n by heating when the insulating layer 116 is formed or after the insulating layer 116 is formed. Alternatively, the insulating layer 116 can be formed using an insulating film that can generate oxygen vacancies in the low resistance region 108n by heating when the insulating layer 116 is formed or after the insulating layer 116 is formed.

[0197] For example, an insulating film used as a supply source for supplying impurities to the low resistance region 108n can be used as the insulating layer 116. In this case, the insulating layer 116 is preferably a film that releases hydrogen by heating. When such an insulating layer 116 is formed in contact with the semiconductor layer 108, impurities such as hydrogen can be supplied to the low resistance region 108n, thereby making the low resistance region 108n low-resistance.

[0198] The insulating layer 116 is preferably formed using a formation gas containing an impurity element such as hydrogen. In addition, by increasing the deposition temperature of the insulating layer 116, a large amount of impurity elements can be effectively supplied to the semiconductor layer 108. The deposition temperature of the insulating layer 116 can be, for example, 200° C. to 500° C., preferably 220° C. to 450° C., and more preferably 250° C. to 400° C.

[0199] When the insulating layer 116 is formed under reduced pressure while heating, oxygen can be released from the region to be the low resistance region 108n in the semiconductor layer 108. When impurities such as hydrogen are supplied to the semiconductor layer 108 in which many oxygen vacancies are formed, the carrier density of the low resistance region 108n is increased, and the resistance of the low resistance region 108n can be further effectively reduced.

[0200] As the insulating layer 116, for example, an insulating film containing a nitride such as silicon nitride, silicon nitride oxide, silicon oxynitride, aluminum nitride, or aluminum nitride oxide can be appropriately used. In particular, silicon nitride has a barrier property against hydrogen and oxygen, and thus can prevent both the diffusion of hydrogen from the outside into the semiconductor layer and the separation of oxygen from the semiconductor layer to the outside, thereby realizing a transistor with high reliability.

[0201] The insulating layer 116 can be an insulating film having a function of absorbing oxygen in the semiconductor layer 108 and generating oxygen vacancies. In particular, as the insulating layer 116, for example, a metal nitride such as aluminum nitride is preferably used.

[0202] When a metal nitride is used, a nitride of aluminum, titanium, tantalum, tungsten, chromium or ruthenium is preferably used. For example, aluminum or titanium is particularly preferably contained. For example, with respect to an aluminum nitride film formed by a reactive sputtering method using a sputtering target using aluminum and a forming gas containing nitrogen, by appropriately controlling the flow ratio of nitrogen gas relative to the total flow rate of the forming gas, a film having both extremely high insulation and extremely high barrier properties to hydrogen or oxygen can be formed. Therefore, by providing such an insulating film containing a metal nitride in contact with the semiconductor layer, not only can the resistance of the semiconductor layer be reduced, but also the oxygen detachment from the semiconductor layer and the diffusion of hydrogen into the semiconductor layer can be effectively prevented.

[0203] When aluminum nitride is used as the metal nitride, the thickness of the insulating layer containing aluminum nitride is preferably 5 nm or more. Even with such a thin film, it can have both high barrier properties to hydrogen and oxygen and the function of reducing the resistance of the semiconductor layer. In addition, there is no upper limit to the thickness of the insulating layer, but considering productivity, it is preferably 500 nm or less, more preferably 200 nm or less, and further preferably 50 nm or less.

[0204] When an aluminum nitride film is used as the insulating layer 116, it is preferable to use an aluminum nitride film satisfying the composition formula: AlN x (x is a real number greater than 0 and less than 2, preferably a real number greater than 0.5 and less than 1.5). In this case, a film having good insulation and high thermal conductivity can be obtained, thereby improving the heat dissipation performance when driving the transistor 100B.

[0205] Alternatively, as the insulating layer 116, a titanium aluminum nitride film, a titanium nitride film, or the like can be used.

[0206] Since the insulating layer 116 is provided in contact with the low resistance region 108n, the insulating layer 116 absorbs oxygen in the low resistance region 108n, and oxygen vacancies can be generated in the low resistance region 108n. In addition, when heat treatment is performed after the insulating layer 116 is formed, more oxygen vacancies can be formed in the low resistance region 108n, and the resistance can be further reduced. In the case of using a film containing a metal oxide as the insulating layer 116, the insulating layer 116 absorbs oxygen in the semiconductor layer 108, and thus a layer containing an oxide of a metal element (e.g., aluminum) contained in the insulating layer 116 is sometimes formed between the insulating layer 116 and the low resistance region 108n.

[0207] Here, when a metal oxide film containing indium is used as the semiconductor layer 108, a region where indium oxide is precipitated or a region with a high indium concentration may be formed near the interface of the low resistance region 108n on the insulating layer 116 side. Thus, a low resistance region 108n with extremely low resistance can be formed. Such a region may be observed by an analysis method such as XPS, for example.

[0208] <Structural Example 2-4>

[0209] Fig. 6A is a top view of transistor 100C, Figure 6B is a cross-sectional view of the transistor 100C in the channel length direction. Figure 6C It is a cross-sectional view of the transistor 100C in the channel width direction.

[0210] The transistor 100C is an example in which the transistor 100B shown in Structural Example 2-3 is provided with the conductive layer 106 used as the first gate electrode shown in Structural Example 2-2.

[0211] By adopting this structure, a transistor with high on-state current can be realized. Alternatively, a transistor capable of controlling threshold voltage can be provided.

[0212] [Modification Example 1 of Structural Example 2]

[0213] Although the semiconductor layer 108 is a single layer in the above-mentioned structural examples 2-1 to 2-4, the semiconductor layer 108 preferably has a stacked-layer structure in which the semiconductor layer 108a and the semiconductor layer 108b are stacked.

[0214] Fig. 7A The transistor 100_a shown in the structure example 2-1 is an example in which the semiconductor layer 108 of the transistor 100 has a stacked structure. Fig. 7A In FIG. 1 , a cross section in the channel length direction is shown on the left side of the dot-dashed line, and a cross section in the channel width direction is shown on the right side of the dot-dashed line.

[0215] Likewise, Figure 7B The transistor 100A_a shown in FIG. Figure 7C The transistor 100B_a and Fig.7D The transistor 100C_a shown is an example in which each of the semiconductor layers 108 of the transistor 100A, the transistor 100B, and the transistor 100C has a stacked-layer structure.

[0216] [Modification Example 2 of Structural Example 2]

[0217] As described above, the metal oxide layer 114 between the insulating layer 110 and the conductive layer 112 may be removed after oxygen is supplied to the insulating layer 110 .

[0218] Fig. 8A The transistor 100_b shown is removed. Fig. 7A An example of a metal oxide layer 114 of transistor 100_a is shown.

[0219] Likewise, Figure 8B The transistor 100A_b shown in FIG. Figure 8C The transistor 100B_b and Fig.8D The transistor 100C_b shown is an example in which the metal oxide layer 114 of the transistor 100A_a, the transistor 100B_a, and the transistor 100C_a is removed.

[0220] [Manufacturing method example 1]

[0221] Hereinafter, an example of a method for manufacturing a transistor according to an embodiment of the present invention will be described. Here, the transistor 100A shown in Structural Example 2-2 will be described as an example.

[0222] The thin film (insulating film, semiconductor film, conductive film, etc.) included in the semiconductor device can be formed by any method including sputtering, chemical vapor deposition (CVD: Chemical Vapor Deposition) method, vacuum evaporation method, pulsed laser deposition (PLD: Pulsed Laser Deposition) method, atomic layer deposition (ALD: Atomic Layer Deposition) method, etc. As CVD methods, there are plasma enhanced chemical vapor deposition (PECVD: Plasma Enhanced CVD) method and thermal CVD method. In addition, as one of the thermal CVD methods, there is metal organic chemical vapor deposition (MOCVD: Metal Organic CVD) method.

[0223] In addition, the thin films (insulating films, semiconductor films, conductive films, etc.) included in the semiconductor device can be formed by spin coating, dipping, spraying, inkjet, dispenser, screen printing, offset printing, doctor knife, slit coating, roll coating, curtain coating, doctor knife coating, or the like.

[0224] In addition, when processing a thin film included in a semiconductor device, photolithography or the like can be used. In addition to the above methods, the thin film can also be processed by nanoimprinting, sandblasting, lift-off, etc. In addition, an island-shaped thin film can be formed by forming a shadow mask such as a metal mask.

[0225] There are two typical photolithography methods. One is to form a resist mask on a thin film to be processed, process the thin film by etching, etc., and remove the resist mask. The other is to form a photosensitive thin film, then perform exposure and development to process the thin film into a desired shape.

[0226] In the photolithography method, as the light used for exposure, for example, i-line (wavelength of 365nm), g-line (wavelength of 436nm), h-line (wavelength of 405nm) or a mixture of these lights can be used. In addition, ultraviolet light, KrF laser or ArF laser, etc. can also be used. In addition, liquid immersion exposure technology can also be used for exposure. As the light used for exposure, extreme ultraviolet light (EUV: Extreme Ultra-Violet) or X-rays can also be used. In addition, an electron beam can also be used instead of the light used for exposure. When extreme ultraviolet light, X-rays or electron beams are used, extremely fine processing can be performed, so it is preferred. In addition, when exposure is performed by scanning a light beam such as an electron beam, a photomask is not required.

[0227] As a method for etching the thin film, a dry etching method, a wet etching method, a sand blast method, or the like can be used.

[0228] 9A to 9E , FIG. 10A to FIG. 10D as well as Fig.11A and Fig. 11B Each of the cross sections in the channel length direction and the channel width direction at each stage of the manufacturing process of the transistor 100A is shown.

[0229] <Formation of Conductive Layer 106>

[0230] A conductive film is formed on the substrate 102, and the conductive film is etched to form a conductive layer 106 ( Fig.9A ).

[0231] At this time, if Fig.9AAs shown in FIG. 1 , the conductive layer 106 is preferably processed so that its end has a tapered shape. This can improve the step coverage of the insulating layer 103 to be formed in the next step.

[0232] When a conductive film containing copper is used as the conductive film to be the conductive layer 106, wiring resistance can be reduced. For example, in the case of a large display device or a display device with high resolution, it is preferable to use a conductive film containing copper. Even if a conductive film containing copper is used as the conductive layer 106, diffusion of copper to the semiconductor layer 108 side can be suppressed by the insulating layer 103, thereby obtaining a transistor with high reliability.

[0233] <Formation of Insulating Layer 103>

[0234] Next, an insulating layer 103 is formed to cover the substrate 102 and the conductive layer 106. Fig. 9B ). The insulating layer 103 can be formed by a PECVD method, an ALD method, a sputtering method, or the like.

[0235] Here, the insulating layer 103 is formed by stacking an insulating film 103a, an insulating film 103b, an insulating film 103c, and an insulating film 103d.

[0236] In particular, each insulating film included in the insulating layer 103 is preferably formed by a PECVD method. The method for forming the insulating layer 103 can refer to the description of the above-mentioned Structural Example 1.

[0237] After forming the insulating layer 103, oxygen supply treatment may be performed on the insulating layer 103. For example, plasma treatment or heat treatment may be performed in an oxygen atmosphere. Alternatively, oxygen may be supplied to the insulating layer 103 by a plasma ion doping method or an ion implantation method.

[0238] <Formation of Semiconductor Layer 108>

[0239] Next, a metal oxide film 108f is formed on the insulating layer 103 ( Fig. 9C ).

[0240] The metal oxide film 108f is preferably formed by a sputtering method using a metal oxide target.

[0241] The metal oxide film 108f is preferably a dense film with as few defects as possible. The metal oxide film 108f is preferably a high-purity film in which impurities such as hydrogen and water are reduced as much as possible. In particular, a crystalline metal oxide film is preferably used as the metal oxide film 108f.

[0242] When forming a metal oxide film, an oxygen gas and an inert gas (e.g., helium gas, argon gas, xenon gas, etc.) may also be mixed. Note that the higher the ratio of the oxygen gas in the overall forming gas when forming the metal oxide film (hereinafter, also referred to as the oxygen flow ratio), the higher the crystallinity of the metal oxide film can be, and a transistor with high reliability can be realized. On the other hand, the lower the oxygen flow ratio, the lower the crystallinity of the metal oxide film, and a transistor with high on-state current can be realized.

[0243] When forming a metal oxide film, as the substrate temperature becomes higher, a denser metal oxide film with higher crystallinity can be formed. On the other hand, as the substrate temperature becomes lower, a metal oxide film with lower crystallinity and higher conductivity can be formed.

[0244] The metal oxide film is formed under the condition that the substrate temperature is higher than room temperature and lower than 250° C., preferably higher than room temperature and lower than 200° C., and more preferably higher than room temperature and lower than 140° C. For example, the substrate temperature is preferably higher than room temperature and lower than 140° C., thereby improving productivity. When the metal oxide film is formed when the substrate temperature is room temperature or when no intentional heating is performed, the metal oxide film can have low crystallinity.

[0245] Before forming the metal oxide film 108f, it is preferred to perform at least one of a treatment for removing water, hydrogen, organic matter, etc. adsorbed on the surface of the insulating layer 103 and a treatment for supplying oxygen to the insulating layer 103. For example, a heat treatment may be performed at a temperature of 70°C to 200°C in a reduced pressure atmosphere. Alternatively, a plasma treatment in an oxygen-containing atmosphere may be performed. Alternatively, oxygen may be supplied to the insulating layer 103 by performing a plasma treatment in an atmosphere containing an oxidizing gas such as nitrous oxide (N2O). When a plasma treatment using nitrous oxide gas is performed, organic matter on the surface of the insulating layer 103 can be appropriately removed and oxygen can be supplied to the insulating layer 103. Preferably, after such a treatment, the metal oxide film 108f is continuously formed in a manner that does not expose the surface of the insulating layer 103 to the atmosphere.

[0246] Note that in the case where the semiconductor layer 108 has a stacked-layer structure in which a plurality of semiconductor layers are stacked, it is preferable that an upper metal oxide film be formed continuously after a lower metal oxide film is formed so that a surface of the lower metal oxide film is not exposed to the atmosphere.

[0247] Next, the metal oxide film 108f is partially etched to form an island-shaped semiconductor layer 108 ( Fig.9D ).

[0248] The metal oxide film 108f is processed by wet etching and / or dry etching. At this time, a portion of the insulating layer 103 that does not overlap with the semiconductor layer 108 is sometimes etched to be thinner. For example, the insulating film 103d of the insulating layer 103 is sometimes removed by etching, exposing the surface of the insulating film 103c.

[0249] Here, it is preferable to perform heat treatment after forming the metal oxide film 108f or processing the semiconductor layer 108. By heat treatment, hydrogen or water contained in the metal oxide film 108f or the semiconductor layer 108 or attached to the surface of the metal oxide film 108f or the semiconductor layer 108 can be removed. In addition, by heat treatment, the film quality of the metal oxide film 108f or the semiconductor layer 108 is sometimes improved (for example, the amount of defects is reduced, the crystallinity is improved, etc.).

[0250] In addition, by heat treatment, oxygen can be supplied from the insulating layer 103 to the metal oxide film 108f or the semiconductor layer 108. At this time, it is more preferable to perform heat treatment before processing the semiconductor film 108f into the semiconductor layer 108.

[0251] Typically, the heat treatment can be performed at a temperature of 150° C. or higher and lower than the strain point of the substrate, 200° C. or higher and 500° C. or lower, 250° C. or higher and 450° C. or higher, or 300° C. or higher and 450° C. or lower.

[0252] The heat treatment may be performed in an atmosphere containing a rare gas or nitrogen. Alternatively, the heat treatment may be performed in the atmosphere and then in an atmosphere containing oxygen. Alternatively, the heating may be performed in a dry air atmosphere. Preferably, the atmosphere of the heat treatment does not contain hydrogen or water as much as possible. The heat treatment may be performed using an electric furnace or an RTA (Rapid Thermal Anneal) device. By using an RTA device, the heat treatment time may be shortened.

[0253] Note that this heat treatment does not necessarily need to be performed. It is not necessary to perform heat treatment in this step, and the heat treatment performed in a later step may be used as the heat treatment in this step. Sometimes, a treatment at a high temperature in a later step (e.g., a film formation step) may be used as the heat treatment in this step.

[0254] <Formation of Insulating Layer 110 >

[0255] Next, an insulating layer 110 is formed so as to cover the insulating layer 103 and the semiconductor layer 108 ( Fig.9E ).

[0256] Here, the insulating layer 110 is formed by stacking an insulating film 110 a , an insulating film 110 b , and an insulating film 110 c .

[0257] In particular, it is preferable that each insulating film included in the insulating layer 110 is formed by a PECVD method. As a method for forming each insulating film included in the insulating layer 110, the description of the above-mentioned structural example 1 can be referred to.

[0258] Preferably, the surface of the semiconductor layer 108 is subjected to plasma treatment before forming the insulating layer 110. By this plasma treatment, impurities such as water attached to the surface of the semiconductor layer 108 can be reduced. Therefore, impurities at the interface between the semiconductor layer 108 and the insulating layer 110 can be reduced, and a transistor with high reliability can be realized. In the case where the surface of the semiconductor layer 108 is exposed to the atmosphere during the formation of the semiconductor layer 108 to the formation of the insulating layer 110, plasma treatment is particularly preferred. The plasma treatment can be performed in an atmosphere of oxygen, ozone, nitrogen, nitrous oxide, argon, or the like. The plasma treatment and the formation of the insulating layer 110 are preferably performed continuously without being exposed to the atmosphere.

[0259] After forming the insulating layer 110, heat treatment is preferably performed. By heat treatment, hydrogen or water contained in the insulating layer 110 or adsorbed on the surface thereof can be removed. At the same time, the amount of defects in the insulating layer 110 can be reduced.

[0260] The conditions for the heat treatment can refer to the above description.

[0261] Note that this heat treatment does not necessarily need to be performed. It is not necessary to perform heat treatment in this step, and the heat treatment performed in a later step may be used as the heat treatment in this step. Sometimes, a treatment at a high temperature in a later step (e.g., a film formation step) may be used as the heat treatment in this step.

[0262] <Formation of Metal Oxide Film 114f>

[0263] Next, a metal oxide film 114f is formed on the insulating layer 110 ( Fig. 10A ).

[0264] The metal oxide film 114f is preferably formed in an atmosphere including oxygen, for example. In particular, the metal oxide film 114f is preferably formed by sputtering in an atmosphere including oxygen. Thus, oxygen can be supplied to the insulating layer 110 when the metal oxide film 114f is formed.

[0265] When the metal oxide film 114 f is formed by a sputtering method using an oxide target containing a metal oxide similarly to the semiconductor layer 108 , the above description can be applied.

[0266] For example, the metal oxide film 114f can be formed by a reactive sputtering method using oxygen as a forming gas and a metal target. When aluminum is used as the metal target, an aluminum oxide film can be formed.

[0267] When forming the metal oxide film 114f, the higher the ratio of the oxygen flow rate to the total flow rate of the forming gas introduced into the deposition chamber of the deposition device (oxygen flow rate ratio) or the higher the oxygen partial pressure in the deposition chamber, the greater the amount of oxygen supplied to the insulating layer 110. The oxygen flow rate ratio or the oxygen partial pressure is, for example, 50% or more and 100% or less, preferably 65% ​​or more and 100% or less, more preferably 80% or more and 100% or less, and further preferably 90% or more and 100% or less. In particular, it is preferred to set the oxygen flow rate ratio to 100% to make the oxygen partial pressure in the deposition chamber as close to 100% as possible.

[0268] Thus, by forming the metal oxide film 114f by sputtering in an atmosphere containing oxygen, oxygen can be supplied to the insulating film 110 while the metal oxide film 114f is formed, and oxygen can be prevented from being released from the insulating layer 110. As a result, a large amount of oxygen can be confined in the insulating layer 110.

[0269] After the metal oxide film 114f is formed, heat treatment is preferably performed. By heat treatment, oxygen contained in the insulating layer 110 can be supplied to the semiconductor layer 108. When heat treatment is performed in a state where the metal oxide film 114f covers the insulating layer 110, oxygen can be prevented from being released from the insulating layer 110 to the outside, and a large amount of oxygen can be supplied to the semiconductor layer 108. Therefore, oxygen vacancies in the semiconductor layer 108 can be reduced, thereby realizing a transistor with high reliability.

[0270] The conditions for the heat treatment can refer to the above description.

[0271] Note that this heat treatment does not necessarily need to be performed. It is not necessary to perform heat treatment in this step, and the heat treatment performed in a later step may be used as the heat treatment in this step. Sometimes, a treatment at a high temperature in a later step (e.g., a film formation step) may be used as the heat treatment in this step.

[0272] After the formation of the metal oxide film 114f or the heat treatment, the metal oxide film 114f may be removed.

[0273] <Formation of Opening 142>

[0274] Next, the metal oxide film 114f, the insulating layer 110, and the insulating layer 103 are partially etched to form an opening 142 ( Fig. 10B). Thus, the conductive layer 106 can be electrically connected to the conductive layer 112 formed later through the opening 142.

[0275] <Formation of Conductive Layer 112 and Metal Oxide Layer 114>

[0276] Next, a conductive film 112f ( Fig. 10C ).

[0277] As the conductive film 112f, a low-resistance metal or a low-resistance alloy material is preferably used. The conductive film 112f is preferably formed using a material that does not easily release hydrogen and does not easily diffuse hydrogen. In addition, as the conductive film 112f, a material that is not easily oxidized is preferably used.

[0278] For example, the conductive film 112f is preferably formed by a sputtering method using a sputtering target containing a metal or an alloy.

[0279] For example, the conductive film 112f is preferably a stacked film including a conductive film that is not easily oxidized and does not easily diffuse hydrogen, and a low-resistance conductive film.

[0280] Next, the conductive film 112f and the metal oxide film 114f are partially etched to form the conductive layer 112 and the metal oxide layer 114. The conductive film 112f and the metal oxide film 114f are preferably processed using the same resist mask. Alternatively, the metal oxide film 114f may be etched using the conductive layer 112 obtained by etching as a hard mask.

[0281] In particular, as etching of the conductive film 112f and the metal oxide film 114f, it is preferable to use a wet etching method.

[0282] Thus, the conductive layer 112 and the metal oxide layer 114 can be formed to have substantially the same top surface shapes.

[0283] When the insulating layer 110 is not etched but covers the top and side surfaces of the semiconductor layer 108 and the insulating layer 103 , it is possible to prevent the semiconductor layer 108 and the insulating layer 103 from being partially etched and thinned when etching the conductive film 112 f and the like.

[0284] <Supply Processing of Impurity Elements>

[0285] Next, a process of supplying (adding or implanting) an impurity element 140 to the semiconductor layer 108 through the insulating layer 110 is performed using the conductive layer 112 as a mask ( Fig. 10D). Thus, a low resistance region 108n can be formed in a region of the semiconductor layer 108 that is not covered by the conductive layer 112. At this time, in a region of the semiconductor layer 108 that overlaps with the conductive layer 112, the conductive layer 112 is used as a mask, and the impurity element 140 is not supplied to the region.

[0286] The supply of the impurity element 140 may be appropriately performed by a plasma doping method or an ion implantation method. By using these methods, the concentration distribution in the depth direction can be controlled with high accuracy according to the ion acceleration voltage and the dose, etc. By using the plasma doping method, productivity can be improved. In addition, by using the ion implantation method using mass separation, the purity of the impurity element supplied can be improved.

[0287] It is preferable to control the conditions of the supply process of the impurity element 140 so that the highest concentration is achieved at the interface between the semiconductor layer 108 and the insulating layer 110, at a portion of the semiconductor layer 108 close to the interface, or at a portion of the insulating layer 110 close to the interface. Thus, the impurity element 140 having an optimum concentration can be supplied to both the semiconductor layer 108 and the insulating layer 110 by a single process.

[0288] As the impurity element 140, hydrogen, boron, carbon, nitrogen, fluorine, phosphorus, sulfur, arsenic, aluminum, magnesium, silicon, or a rare gas can be cited. Typical examples of the rare gas include helium, neon, argon, krypton, and xenon. In particular, boron, phosphorus, aluminum, magnesium, or silicon is preferably used.

[0289] As the source gas of the impurity element 140, a gas containing the above-mentioned impurity elements can be used. When boron is supplied, B2H6 gas or BF3 gas can be typically used. In addition, when phosphorus is supplied, PH3 gas can be typically used. In addition, a mixed gas in which these source gases are diluted with a rare gas can also be used.

[0290] In addition to the above, as source gases, CH4, N2, NH3, AlH3, AlCl3, SiH4, Si2H6, F2, HF, H2, (C5H5)2Mg and rare gases can be used. In addition, the ion source is not limited to gas, and solids or liquids that are heated and vaporized can also be used.

[0291] By setting conditions such as an acceleration voltage and a dose in consideration of the composition, density, thickness, and the like of the insulating layer 110 and the semiconductor layer 108 , addition of the impurity element 140 can be controlled.

[0292] When boron is added by ion implantation or plasma ion doping, the acceleration voltage may be, for example, 5 kV to 100 kV, preferably 7 kV to 70 kV, and more preferably 10 kV to 50 kV. In addition, the dose may be, for example, 1×10 13ions / cm 2 Above and 1×10 17 ions / cm 2 Below, preferably 1×10 14 ions / cm 2 Above and 5×10 16 ions / cm 2 Below, more preferably 1×10 15 ions / cm 2 Above and 3×10 16 ions / cm 2 the following.

[0293] When phosphorus ions are added by ion implantation or plasma ion doping, the acceleration voltage may be, for example, 10 kV to 100 kV, preferably 30 kV to 90 kV, and more preferably 40 kV to 80 kV. 13 ions / cm 2 Above and 1×10 17 ions / cm 2 Below, preferably 1×10 14 ions / cm 2 Above and 5×10 16 ions / cm 2 Below, more preferably 1×10 15 ions / cm 2 Above and 3×10 16 ions / cm 2 the following.

[0294] Note that the method of supplying the impurity element 140 is not limited to this, and for example, plasma treatment or treatment using thermal diffusion due to heating may be performed. In the case of using a plasma treatment method, the impurity element can be added by using plasma generated in a gas atmosphere containing the impurity element to be added. As an apparatus for generating the above-mentioned plasma, a dry etching apparatus, an ashing apparatus, a plasma CVD apparatus, a high-density plasma CVD apparatus, or the like can be used.

[0295] In one embodiment of the present invention, the impurity element 140 can be supplied to the semiconductor layer 108 through the insulating layer 110. Thus, even when the semiconductor layer 108 has crystallinity, damage to the semiconductor layer 108 when the impurity element 140 is supplied can be reduced, and thus loss of crystallinity can be suppressed. Thus, it is suitable for use in a case where resistance increases due to a decrease in crystallinity.

[0296] <Formation of Insulating Layer 118>

[0297] Next, an insulating layer 118 is formed to cover the insulating layer 110, the metal oxide layer 114, and the conductive layer 112. Fig.11A ).

[0298] When the insulating layer 118 is formed by the PECVD method at an excessively high deposition temperature, impurities contained in the low resistance region 108n and the like may diffuse to the peripheral portion including the channel formation region of the semiconductor layer 108 or the resistance of the low resistance region 108n may increase. Therefore, the deposition temperature of the insulating layer 118 is determined in consideration of these factors.

[0299] For example, the insulating layer 118 is preferably formed at a deposition temperature of 150° C. to 400° C., preferably 180° C. to 360° C., and more preferably 200° C. to 250° C. By forming the insulating layer 118 at a low temperature, even a transistor with a short channel length can have good electrical characteristics.

[0300] Heat treatment may be performed after forming the insulating layer 118. The heat treatment may sometimes make the low resistance region 108n more stable and low-resistance. For example, the heat treatment may appropriately diffuse the impurity element 140 and locally make it uniform, thereby forming a low resistance region 108n having an ideal concentration gradient of the impurity element. Note that when the temperature of the heat treatment is too high (for example, 500° C. or more), the impurity element 140 diffuses into the channel formation region, which may result in a decrease in the electrical characteristics or reliability of the transistor.

[0301] The conditions for the heat treatment can refer to the above description.

[0302] Note that this heat treatment does not necessarily need to be performed. It is not necessary to perform heat treatment in this step, and the heat treatment performed in a later step may be used as the heat treatment in this step. Sometimes, a treatment at a high temperature in a later step (e.g., a film formation step) may be used as the heat treatment in this step.

[0303] <Formation of Openings 141a and 141b>

[0304] Next, the insulating layer 118 and the insulating layer 110 are partially etched to form the opening 141 a and the opening 141 b reaching the low resistance region 108 n .

[0305] <Formation of Conductive Layer 120a, Conductive Layer 120b>

[0306] Next, a conductive film is formed on the insulating layer 118 so as to cover the openings 141a and 141b, and the conductive film is processed into a desired shape to form the conductive layers 120a and 120b ( Fig. 11B ).

[0307] Through the above steps, the transistor 100A can be manufactured. For example, when the transistor 100A is applied to a pixel of a display device, one or more steps of forming a protective insulating layer, a planarization layer, a pixel electrode, and a wiring may be added later.

[0308] The above is the description of Manufacturing Method Example 1.

[0309] Note that when manufacturing the transistor 100 described in Structural Example 2-1, the step of forming the conductive layer 106 and the step of forming the opening 142 in the above-mentioned Manufacturing Method Example 1 can be omitted. The transistor 100 and the transistor 100A can be formed over the same substrate by the same step.

[0310] [Manufacturing method example 2]

[0311] The following describes a manufacturing method example in which a portion of the steps are different from the above-mentioned manufacturing method example 1. Here, the transistor 100C shown in the above-mentioned structural example 2-4 is used as an example for description.

[0312] Note that the description of the same steps as those in the above-mentioned manufacturing method example 1 is omitted below, and different steps are described in detail.

[0313] First, similar to the manufacturing method example 1 described above, the conductive layer 106, the insulating layer 103, the semiconductor layer 108, the insulating layer 110, the metal oxide film 114f and the conductive film 112f are formed in sequence. Fig. 12A This is a cross-sectional view of this stage.

[0314] Next, the conductive film 112f and the metal oxide film 114f are partially etched to form the conductive layer 112 and the metal oxide layer 114, and the insulating layer 110 is also partially etched to expose a portion of the semiconductor layer 108 ( Fig. 12B ). Thus, the conductive layer 112, the metal oxide layer 114, and the insulating layer 110 can be formed to have substantially the same top surface shapes.

[0315] The insulating layer 110 is preferably etched using a resist mask used to etch the conductive film 112f. The insulating layer 110 may be etched in the same process as the conductive film 112f and the metal oxide film 114f, or may be etched by a different etching method after etching the conductive film 112f and the metal oxide film 114f.

[0316] For example, the conductive film 112f and the metal oxide film 114f are etched by a wet etching method using the same etchant, and then the insulating layer 110 may be etched by a dry etching method. In particular, when the conductive film 112f and the metal oxide film 114f are processed by the dry etching method, the semiconductor layer 108 and the insulating layer 110 are contaminated by the generation of reaction products containing metal. Therefore, before etching the insulating layer 110, it is preferable to process the conductive film 112f and the metal oxide film 114f by the wet etching method.

[0317] Depending on etching conditions, ends of the conductive layer 112, the metal oxide layer 114, and the insulating layer 110 may not be aligned. For example, at least one end of the conductive layer 112 and the metal oxide layer 114 may be located inside or outside an end of the insulating layer 110.

[0318] When etching the insulating layer 110, a part of the semiconductor layer 108 that is exposed may be etched and thinned. At this time, the semiconductor layer 108 may have a shape in which the thickness of the low resistance region 108n is smaller than the thickness of the channel formation region.

[0319] In the etching of the insulating layer 110, a part of the insulating layer 103 which is not covered by the semiconductor layer 108 may be etched and thinned. For example, the insulating film 103d of the insulating layer 103 may be removed.

[0320] Next, an insulating layer 116 is formed in contact with the exposed portion of the semiconductor layer 108, and then an insulating layer 118 is formed ( Fig. 12C ). By forming the insulating layer 116, the resistance of the exposed portion of the semiconductor layer 108 is reduced, thereby forming a low-resistance region 108n.

[0321] As the insulating layer 116, an insulating film that releases an impurity element having a function of reducing the resistance of the semiconductor layer 108 can be used. In particular, an inorganic insulating film that can release hydrogen, such as a silicon nitride film, a silicon nitride oxide film, or a silicon oxynitride film, is preferably used. In this case, a PECVD method using a formation gas containing hydrogen is preferred because hydrogen can be supplied to the semiconductor layer 108 when the insulating layer 116 is formed.

[0322] For example, when silicon nitride is used as the insulating layer 116, a PECVD method using a mixed gas of a silicon-containing gas such as silane and a nitrogen-containing gas such as ammonia or nitrous oxide as a forming gas is preferably used. In this case, it is preferable that the formed silicon nitride film contains hydrogen. Thus, by diffusing hydrogen in the insulating layer 116 into the semiconductor layer 108, a portion of the semiconductor layer 108 can be easily reduced in resistance.

[0323] Alternatively, an insulating film having a function of generating oxygen vacancies in the semiconductor layer 108 may be used. In particular, an insulating film containing a metal nitride is preferably used. For example, a reactive sputtering method using a sputtering target containing a metal and a mixed gas of nitrogen gas and a rare gas as a diluent gas is preferably used as a forming gas. Thus, by controlling the flow rate ratio of the forming gas, the film quality of the insulating layer 116 can be easily controlled.

[0324] For example, when an aluminum nitride film formed by reactive sputtering using an aluminum target is used as the insulating layer 116, the flow rate of nitrogen gas relative to the total flow rate of the forming gas is greater than 30% and less than 100%, preferably greater than 40% and less than 100%, and more preferably greater than 50% and less than 100%.

[0325] Here, the insulating layer 116 and the insulating layer 118 are preferably formed continuously without being exposed to the air.

[0326] Heat treatment may be performed after forming the insulating layer 116 or the insulating layer 118. Heat treatment can promote the reduction of resistance of the low-resistance region 108n.

[0327] The conditions for the heat treatment can refer to the above description.

[0328] Note that this heat treatment does not necessarily need to be performed. It is not necessary to perform heat treatment in this step, and the heat treatment performed in a later step may be used as the heat treatment in this step. Sometimes, a treatment at a high temperature in a later step (e.g., a film formation step) may be used as the heat treatment in this step.

[0329] Next, the opening 141 a and the opening 141 b reaching the low resistance region 108 n are formed in the insulating layer 118 and the insulating layer 116 .

[0330] Next, in the same manner as in the manufacturing method example 1, a conductive layer 120a and a conductive layer 120b are formed on the insulating layer 118 ( Fig.12D ).

[0331] Through the above-described steps, the transistor 100C can be manufactured.

[0332] Note that when manufacturing the transistor 100B described in Structural Example 2-3, the step of forming the conductive layer 106 and the step of forming the opening 142 in the above-mentioned Manufacturing Method Example 2 can be omitted. The transistor 100B and the transistor 100C can be formed over the same substrate by the same step.

[0333] [Components of a semiconductor device]

[0334] Hereinafter, components included in the semiconductor device of this embodiment will be described.

[0335] <Substrate>

[0336] Although there is no particular limitation on the material of the substrate 102, it is at least required to have heat resistance sufficient to withstand subsequent heat treatment. For example, a single crystal semiconductor substrate or polycrystalline semiconductor substrate made of silicon or silicon carbide, a compound semiconductor substrate such as silicon germanium, an SOI substrate, a glass substrate, a ceramic substrate, a quartz substrate, a sapphire substrate, or the like can be used as the substrate 102. In addition, any of the above substrates provided with a semiconductor element can also be used as the substrate 102.

[0337] In addition, a flexible substrate may be used as the substrate 102, and a semiconductor device or the like may be directly formed on the flexible substrate. Alternatively, a peeling layer may be provided between the substrate 102 and the semiconductor device or the like. The peeling layer may be used when a part or all of a semiconductor device is manufactured on the peeling layer, and then the semiconductor device or the like is separated from the substrate 102 and transferred to another substrate. In this case, the semiconductor device or the like may also be transferred to a substrate with low heat resistance or a flexible substrate.

[0338] <Conductive Film>

[0339] The conductive layer 112 and the conductive layer 106 used as the gate electrode, the conductive layer 120a used as one of the source electrode and the drain electrode, and the conductive layer 120b used as the other of the source electrode and the drain electrode can be formed respectively using a metal element selected from chromium, copper, aluminum, gold, silver, zinc, molybdenum, tantalum, titanium, tungsten, manganese, nickel, iron, and cobalt, or an alloy containing the above metal elements as components, or an alloy combining any of the above metal elements.

[0340] In addition, as each of the conductive layer 112, the conductive layer 106, the conductive layer 120a and the conductive layer 120b, an oxide conductor or a metal oxide film such as In-Sn oxide, In-W oxide, In-W-Zn oxide, In-Ti oxide, In-Ti-Sn oxide, In-Zn oxide, In-Sn-Si oxide, In-Ga-Zn oxide can be used.

[0341] Here, an oxide conductor (OC) is described. For example, by forming oxygen vacancies in a metal oxide having semiconductor properties and adding hydrogen to the oxygen vacancies, a donor energy level is formed near the conduction band. As a result, the conductivity of the metal oxide increases, and the metal oxide becomes a conductor. The metal oxide that becomes a conductor can also be called an oxide conductor.

[0342] In addition, as the conductive layer 112, a stacked structure of a conductive film containing the above-mentioned oxide conductor (metal oxide) or a conductive film containing a metal or alloy may be used. By using a conductive film containing a metal or an alloy, wiring resistance can be reduced. Here, it is preferred that the conductive film in contact with the insulating layer used as the gate insulating film is a conductive film containing an oxide conductor.

[0343] In addition, the conductive layer 112, the conductive layer 106, the conductive layer 120a, and the conductive layer 120b preferably contain any one or more selected from the above-mentioned metal elements, titanium, tungsten, tantalum, and molybdenum. In particular, a tantalum nitride film is preferably used. The tantalum nitride film has conductivity and high barrier properties against copper, oxygen, or hydrogen, and the amount of hydrogen released is small, so the tantalum nitride film can be suitably used as a conductive film in contact with the semiconductor layer 108 or a conductive film near the semiconductor layer 108.

[0344] <Semiconductor Layer>

[0345] When the semiconductor layer 108 is In-M-Zn oxide, the atomic number ratio of the metal elements in the sputtering target used to form In-M-Zn oxide can be In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=1:3:2, In:M:Zn=1:3:4, In:M:Zn=1:3:6, In:M:Zn=2:2:1, In:M:Zn=2:1:3, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, In:M:Zn=6:1:6, In:M:Zn=5:2:5, etc.

[0346] In addition, it is preferable to use a target containing a polycrystalline oxide as a sputtering target, thereby making it easy to form a semiconductor layer 108 having crystallinity. Note that the atomic number ratio of the metal element in the formed semiconductor layer 108 varies within the range of ±40% of the atomic number ratio of the metal element in the above-mentioned sputtering target. For example, when the composition of the sputtering target used for forming the semiconductor layer 108 is In:Ga:Zn=4:2:4.1 [atomic number ratio], the composition of the formed semiconductor layer 108 may be In:Ga:Zn=4:2:3 [atomic number ratio] or its vicinity.

[0347] Note that the atomic number ratio of In:Ga:Zn=4:2:3 or its vicinity includes the following cases: when In is 4, Ga is 1 or more and 3 or less, and Zn is 2 or more and 4 or less. In addition, the atomic number ratio of In:Ga:Zn=5:1:6 or its vicinity includes the following cases: when In is 5, Ga is greater than 0.1 and 2 or less, and Zn is 5 or more and 7 or less. In addition, the atomic number ratio of In:Ga:Zn=1:1:1 or its vicinity includes the following cases: when In is 1, Ga is greater than 0.1 and 2 or less, and Zn is greater than 0.1 and 2 or less.

[0348] The energy gap of the semiconductor layer 108 is 2 eV or more, preferably 2.5 eV or more. Thus, by using a metal oxide having a wider energy gap than silicon, the off-state current of the transistor can be reduced.

[0349] In addition, the semiconductor layer 108 preferably has a non-single crystal structure. The non-single crystal structure includes, for example, a CAAC structure, a polycrystalline structure, a microcrystalline structure, or an amorphous structure described below. Among the non-single crystal structures, the amorphous structure has the highest defect state density, and the CAAC structure has the lowest defect state density.

[0350] CAAC (c-axis aligned crystal) is described below. CAAC is an example of a crystal structure.

[0351] The CAAC structure refers to one of the crystalline structures of a film including multiple nanocrystals (crystalline regions with a maximum diameter of less than 10 nm). The c-axis of each nanocrystal is oriented in a specific direction, and its a-axis and b-axis are not oriented. The nanocrystals do not form grain boundaries with each other but are continuously connected in the a-axis and b-axis directions. In particular, in a film having a CAAC structure, the c-axis of each nanocrystal is easily oriented in the thickness direction of the film, the normal direction of the formed surface of the film, or the normal direction of the film surface.

[0352] CAAC-OS (Oxide Semiconductor) is an oxide semiconductor with high crystallinity. On the other hand, no clear grain boundaries are observed in CAAC-OS, so it is not easy to cause a decrease in electron mobility due to grain boundaries. In addition, the crystallinity of oxide semiconductors is sometimes reduced due to the mixing of impurities or the generation of defects, so it can be said that CAAC-OS is an oxide semiconductor with few impurities or defects (oxygen vacancies, etc.). Therefore, the physical properties of oxide semiconductors containing CAAC-OS are stable. Therefore, oxide semiconductors containing CAAC-OS have high heat resistance and high reliability.

[0353] Here, in crystallography, a general method for determining a unit lattice formed by three axes (crystal axes) of the a-axis, the b-axis, and the c-axis is to determine a unit lattice with a more specific axis as the c-axis. In particular, in a crystal having a layered structure, a general method for determining a unit lattice is to determine a unit lattice in which two axes parallel to the plane direction of the layer are the a-axis and the b-axis, and an axis intersecting the layer is the c-axis. As a typical example of such a crystal having a layered structure, there is graphite classified as a hexagonal system, in which the a-axis and the b-axis of the unit lattice are parallel to the cleavage plane, and the c-axis is orthogonal to the cleavage plane. For example, InGaZnO4 having a layered structure and a YbFe2O4 type crystal structure can be classified as a hexagonal system, in which the a-axis and the b-axis of the unit lattice are parallel to the plane direction of the layer, and the c-axis is orthogonal to the layer (i.e., orthogonal to the a-axis and the b-axis).

[0354] In the image observed by TEM, the crystal part of the oxide semiconductor film (microcrystalline oxide semiconductor film) having a microcrystalline structure cannot be clearly confirmed. The crystal part of the microcrystalline oxide semiconductor film is mostly greater than 1nm and less than 100nm or greater than 1nm and less than 10nm. In particular, the microcrystals whose size is greater than 1nm and less than 10nm or greater than 1nm and less than 3nm are called nanocrystals (nc: nanocrystal). The oxide semiconductor film containing nanocrystals is called nc-OS (nanocrystalline Oxide Semiconductor: nanocrystalline oxide semiconductor) film. For example, in the image obtained using TEM, the grain boundaries in the nc-OS film cannot be clearly confirmed.

[0355] In the nc-OS film, the atomic arrangement in a tiny area (for example, an area with a size of 1 nm or more and 10 nm or less, and in particular, an area with a size of 1 nm or more and 3 nm or less) is periodic. In addition, the nc-OS film has no regularity of crystal orientation between different crystalline parts. Therefore, no orientation is observed in the entire film. Therefore, sometimes the nc-OS film is no different from the amorphous oxide semiconductor film in certain analysis methods. For example, when the nc-OS film is structurally analyzed by an out-of-plane method using an XRD device using an X-ray whose beam diameter is larger than that of the crystalline part, no peak representing the crystalline plane is detected. In addition, in the selected area electron diffraction pattern of the nc-OS film obtained using an electron beam whose beam diameter is larger than the diameter of the crystalline part (for example, more than 50 nm), a halo pattern is observed. On the other hand, sometimes when the nc-OS film is subjected to electron diffraction (also called nanobeam electron diffraction) using an electron beam whose electron beam diameter is close to the diameter of the crystalline portion or smaller than the diameter of the crystalline portion (for example, greater than 1 nm and less than 30 nm), a ring-shaped (annular) region with high brightness is observed, and multiple spots are observed within the annular region.

[0356] The defect state density of the nc-OS film is lower than that of the amorphous oxide semiconductor film. However, the nc-OS film has no regularity of crystal orientation between different crystalline parts. Therefore, the defect state density of the nc-OS film is higher than that of the CAAC-OS film. Therefore, the nc-OS film sometimes has a higher carrier density and electron mobility than the CAAC-OS film. Therefore, a transistor including the nc-OS film sometimes has a higher field effect mobility.

[0357] The nc-OS film can be formed at a lower oxygen flow rate than when the CAAC-OS film is formed. In addition, the nc-OS film can be formed at a lower substrate temperature than when the CAAC-OS film is formed. For example, the nc-OS film can be formed when the substrate temperature is a relatively low temperature (e.g., a temperature below 130°C) or when the substrate is not heated, so it is suitable for use in cases where a large glass substrate, a resin substrate, etc. is used, and productivity can be improved.

[0358] Below, an example of the crystal structure of a metal oxide is described. A metal oxide formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]) at a substrate temperature of 100°C or higher and 130°C or lower tends to have either a nc structure or a CAAC structure, or a structure in which these two structures are mixed. On the other hand, a metal oxide formed at a substrate temperature of room temperature (RT) tends to have a nc crystal structure. Note that the room temperature (RT) here refers to a temperature including a temperature when the substrate is not intentionally heated.

[0359] [Composition of Metal Oxides]

[0360] Hereinafter, the configuration of a CAC (Cloud-Aligned Composite)-OS that can be used for the transistor disclosed in one embodiment of the present invention will be described.

[0361] Note that CAAC refers to an example of a crystal structure, and CAC refers to an example of a function or a material composition.

[0362] CAC-OS or CAC-metal oxide has a conductive function in a part of the material, an insulating function in another part of the material, and has a semiconductor function as a whole. In addition, when CAC-OS or CAC-metal oxide is used in the active layer of a transistor, the conductive function is to allow electrons (or holes) used as carriers to flow through, and the insulating function is to prevent electrons used as carriers from flowing through. Through the complementary effects of the conductive function and the insulating function, CAC-OS or CAC-metal oxide can have a switching function (on / off function). By separating each function in CAC-OS or CAC-metal oxide, each function can be maximized.

[0363] In addition, CAC-OS or CAC-metal oxide includes a conductive region and an insulating region. The conductive region has the function of the above-mentioned conductivity, and the insulating region has the function of the above-mentioned insulation. In addition, in the material, the conductive region and the insulating region are sometimes separated at a nanoparticle level. In addition, the conductive region and the insulating region are sometimes unevenly distributed in the material. In addition, sometimes the conductive region is observed to be fuzzy at its edge and connected in a cloud shape.

[0364] In CAC-OS or CAC-metal oxide, the conductive region and the insulating region may each be dispersed in the material with a size of 0.5 nm to 10 nm, preferably 0.5 nm to 3 nm.

[0365] In addition, CAC-OS or CAC-metal oxide is composed of components with different band gaps. For example, CAC-OS or CAC-metal oxide contains a component with a wide gap caused by an insulating region and a component with a narrow gap caused by a conductive region. In the case of such a structure, carriers mainly flow through the component with a narrow gap. In addition, the component with a narrow gap and the component with a wide gap complement each other, and carriers flow through the component with a wide gap in conjunction with the component with a narrow gap. Therefore, when the above-mentioned CAC-OS or CAC-metal oxide is used in the channel formation region of a transistor, a high current driving force, that is, a large on-state current and a high field effect mobility can be obtained in the on-state of the transistor.

[0366] That is, CAC-OS or CAC-metal oxide may also be referred to as a matrix composite material (matrix composite) or a metal matrix composite material (metal matrix composite).

[0367] The above is the description of the structure of the metal oxide.

[0368] At least a part of the structural examples described in this embodiment mode and the drawings and the like corresponding to these examples can be implemented in combination with other structural examples or drawings and the like as appropriate.

[0369] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.

[0370] (Implementation Method 2)

[0371] In this embodiment, an example of a display device including any of the transistors described in the above embodiment will be described.

[0372] [Structure example]

[0373] Fig.13A 7 shows a top view of a display device 700. The display device 700 includes a first substrate 701 and a second substrate 705 bonded together by a sealant 712. In a region sealed by the first substrate 701, the second substrate 705, and the sealant 712, a pixel portion 702, a source driver circuit portion 704, and a gate driver circuit portion 706 are formed on the first substrate 701. A plurality of display elements are provided in the pixel portion 702.

[0374] In addition, an FPC terminal portion 708 connected to an FPC 716 is provided in a portion of the first substrate 701 that does not overlap with the second substrate 705. Various signals are provided from the FPC 716 to the pixel portion 702, the source driver circuit portion 704, and the gate driver circuit portion 706 through the FPC terminal portion 708 and the signal line 710.

[0375] A plurality of gate driver circuits 706 may be provided. In addition, the gate driver circuit 706 and the source driver circuit 704 are separately formed on a semiconductor substrate or the like to obtain a packaged IC chip. The IC chips may be mounted on the first substrate 701 or mounted on the FPC 716 .

[0376] As transistors included in the pixel portion 702 , the source driver circuit portion 704 , and the gate driver circuit portion 706 , any transistor among transistors of the semiconductor device according to one embodiment of the present invention can be used.

[0377] As display elements provided in the pixel portion 702, liquid crystal elements and light-emitting elements can be cited. As liquid crystal elements, transmissive liquid crystal elements, reflective liquid crystal elements, semi-transmissive liquid crystal elements, etc. can be used. In addition, as light-emitting elements, self-luminous light-emitting elements such as LED (Light Emitting Diode), OLED (Organic LED), QLED (Quantum-dot LED), semiconductor lasers, etc. can be cited. In addition, as display elements, shutter-type or light interference-type MEMS (Micro Electro Mechanical Systems) elements or display elements using microcapsule method, electrophoresis method, electrowetting method, or electronic powder fluid (registered trademark) method can be used.

[0378] Fig. 13B The display device 700A shown is an example of a display device that can be used as a flexible display and includes a resin layer 743 having flexibility instead of the first substrate 701.

[0379] The pixel portion 702 of the display device 700A is not a rectangular shape but has arc-shaped corners. Fig. 13B As shown in the area P1 in FIG. 1 , the display device 700A has a notch portion where a portion of the pixel portion 702 and a portion of the resin layer 743 are cut off. A pair of gate drive circuit portions 706 are provided on both sides of the pixel portion 702. The gate drive circuit portion 706 is provided at the corner of the pixel portion 702 along the inner side of the arc-shaped contour.

[0380] The resin layer 743 has a protruding portion provided with the FPC terminal portion 708. A portion of the resin layer 743 including the FPC terminal portion 708 may be provided along Fig. 13B By folding a portion of the resin layer 743 to the back, the display device 700A can be mounted on an electronic device in a state where the FPC 716 overlaps the back of the pixel portion 702, thereby miniaturizing the electronic device.

[0381] The FPC 716 connected to the display device 700A is mounted with an IC 717. The IC 717 has, for example, a function of a source driver circuit. Here, the source driver circuit section 704 in the display device 700A may include at least one of a protection circuit, a buffer circuit, a demultiplexer circuit, and the like.

[0382] Fig. 13C The display device 700B shown is a display device that can be applied to electronic devices with large screens. For example, the display device 700B can be applied to television devices, monitor devices, personal computers (including notebook and desktop), tablet terminals, digital signage, etc.

[0383] The display device 700B includes a plurality of source driver ICs 721 and a pair of gate driver circuit units 722 .

[0384] The plurality of source driver ICs 721 are mounted on the FPCs 723. In addition, one terminal of each of the plurality of FPCs 723 is connected to the first substrate 701, and the other terminal is connected to the printed circuit board 724. By bending the FPCs 723, the printed circuit board 724 can be arranged on the back side of the pixel portion 702, and the display device 700B can be mounted on an electronic device, thereby miniaturizing the electronic device.

[0385] On the other hand, the gate driving circuit portion 722 is provided on the first substrate 701. Thus, an electronic device with a narrow frame can be realized.

[0386] By adopting the above structure, a large and high-definition display device can be realized. For example, a display device with a screen size of 30 inches or more, 40 inches or more, 50 inches or more, or 60 inches or more in diagonal can be realized. In addition, a display device with extremely high resolution such as 4K2K and 8K4K can be realized.

[0387] [Cross-section structure example]

[0388] Refer to the following Fig.14 , Fig.15 , Fig.16 and Fig.17 A structure using a liquid crystal element or an EL element as a display element is described. Fig.14 , Fig.15 , Fig.16 It is along Fig.13A A cross-sectional view along the dashed line QR is shown. Fig.17 It is along Fig. 13B A cross-sectional view taken along dashed line ST in the display device 700A is shown. Fig.14 and Fig.15 They all have structures including liquid crystal elements as display elements. Fig.16 and Fig.17 All of them have a structure including an EL element as a display element.

[0389] <Description of the Same Parts of the Display Device>

[0390] Fig.14 , Fig.15 , Fig.16 and Fig.17 The display devices shown each include a routing wiring section 711, a pixel section 702, a source driver circuit section 704, and an FPC terminal section 708. The routing wiring section 711 includes a signal line 710. The pixel section 702 includes a transistor 750 and a capacitor 790. The source driver circuit section 704 includes a transistor 752. Fig.15 There is no case where capacitor 790 is provided.

[0391] The transistor 750 and the transistor 752 can use the transistor described in Embodiment 1.

[0392] The transistor used in this embodiment includes a highly purified oxide semiconductor film in which the formation of oxygen vacancies is suppressed. The transistor can have a low off-state current. Therefore, the retention time of an electrical signal such as an image signal can be extended, and the interval between writing operations of the image signal and the like can be extended. Therefore, the frequency of the refresh operation can be reduced, thereby achieving the effect of reducing power consumption.

[0393] In addition, the transistor used in this embodiment can obtain a higher field effect mobility, so it can be driven at high speed. For example, by using such a high-speed transistor in a display device, a switching transistor of a pixel portion and a driving transistor of a driving circuit portion can be formed on the same substrate. That is, there is no need to use a driving circuit formed by a silicon wafer, etc., thereby reducing the number of components of the display device. In addition, by also using a high-speed transistor in the pixel portion, a high-quality image can be provided.

[0394] Fig.14 , Fig.16 and Fig.17 Each capacitor 790 includes a lower electrode formed by processing the same film as the first gate electrode of the transistor 750 and an upper electrode formed by processing the same metal oxide as the film used for the semiconductor layer. The upper electrode is low-resistance in the same manner as the source region or drain region of the transistor 750. In addition, a portion of an insulating film used as the first gate insulating layer of the transistor 750 is provided between the lower electrode and the upper electrode. That is, the capacitor 790 has a stacked structure in which an insulating film used as a dielectric film is sandwiched between a pair of electrodes. In addition, the upper electrode is electrically connected to a wiring formed by processing the same film as the source electrode and drain electrode of the transistor.

[0395] In addition, a planarization insulating film 770 is provided over the transistor 750 , the transistor 752 , and the capacitor 790 .

[0396] In addition, the transistor 750 included in the pixel portion 702 and the transistor 752 included in the source driver circuit portion 704 may have different structures. For example, one of the transistor 750 and the transistor 752 may use a top-gate transistor and the other may use a bottom-gate transistor. Note that, similar to the source driver circuit portion 704, a transistor having the same structure as the transistor 750 or a different structure may be used in the gate driver circuit portion 706.

[0397] The signal line 710 is formed of the same conductive film as the source electrode and the drain electrode of the transistor 750 and the transistor 752. Here, a low-resistance material such as a material containing copper is preferably used, thereby reducing signal delay caused by wiring resistance, thereby achieving a large-screen display.

[0398] The FPC terminal portion 708 includes a wiring 760, a portion of which is used as a connection electrode, an anisotropic conductive film 780, and an FPC 716. The wiring 760 is electrically connected to the terminal of the FPC 716 via the anisotropic conductive film 780. Here, the wiring 760 is formed of the same conductive film as the source electrode and the drain electrode of the transistor 750 and the transistor 752.

[0399] A flexible substrate such as a glass substrate or a plastic substrate can be used as the first substrate 701 and the second substrate 705. When a flexible substrate is used as the first substrate 701, an insulating layer having a barrier property against water or hydrogen is preferably provided between the first substrate 701 and the transistor 750 or the like.

[0400] In addition, a light-shielding film 738, a coloring film 736, and an insulating film 734 in contact with these are provided on the second substrate 705 side.

[0401] <Structural Example of Display Device Using Liquid Crystal Element>

[0402] Fig.14 The display device 700 shown includes a liquid crystal element 775. The liquid crystal element 775 includes a conductive layer 772, a conductive layer 774, and a liquid crystal layer 776 between the conductive layer 772 and the conductive layer 774. The conductive layer 774 is provided on the second substrate 705 side and serves as a common electrode. In addition, the conductive layer 772 is electrically connected to a source electrode or a drain electrode included in the transistor 750. The conductive layer 772 is formed on the planarization insulating film 770 and serves as a pixel electrode.

[0403] A material that is translucent or reflective to visible light can be used for the conductive layer 772. As the translucent material, for example, an oxide material containing indium, zinc, tin, or the like can be used. As the reflective material, for example, a material containing aluminum, silver, or the like can be used.

[0404] When a reflective material is used as the conductive layer 772, the display device 700 is a reflective liquid crystal display device. When a light-transmitting material is used as the conductive layer 772, the display device 700 is a transmissive liquid crystal display device. In a reflective liquid crystal display device, a polarizing plate is provided on the viewing side. On the other hand, in a transmissive liquid crystal display device, a pair of polarizing plates are provided so as to sandwich a liquid crystal element.

[0405] Fig.15The display device 700 shown is an example of a liquid crystal element 775 using a lateral electric field method (e.g., FFS mode). A conductive layer 774 serving as a common electrode is provided on the conductive layer 772 via an insulating layer 773. The alignment state of the liquid crystal layer 776 can be controlled by an electric field generated between the conductive layer 772 and the conductive layer 774.

[0406] exist Fig.15 In the embodiment, a storage capacitor can be formed by stacking the conductive layer 774, the insulating layer 773, and the conductive layer 772. Therefore, there is no need to provide a separate capacitor, and the aperture ratio can be increased.

[0407] In addition, although Fig.14 and Fig.15 Although not shown in the figure, an alignment film may be provided in contact with the liquid crystal layer 776. In addition, an optical member (optical substrate) such as a polarizing member, a phase difference member, an antireflection member, and a light source such as a backlight or a sidelight may be provided as appropriate.

[0408] The liquid crystal layer 776 may use thermotropic liquid crystal, low molecular liquid crystal, polymer liquid crystal, polymer dispersed liquid crystal (PDLC: Polymer Dispersed Liquid Crystal), polymer network liquid crystal (PNLC: Polymer Network Liquid Crystal), ferroelectric liquid crystal, antiferroelectric liquid crystal, etc. In addition, when the lateral electric field method is adopted, liquid crystal exhibiting a blue phase that does not require an alignment film may also be used.

[0409] In addition, as the mode of the liquid crystal element, a TN (Twisted Nematic) mode, a VA (Vertical Alignment) mode, an IPS (In-Plane-Switching) mode, an FFS (Fringe Field Switching) mode, an ASM (Axially Symmetric aligned Micro-cell) mode, an OCB (Optically Compensated Birefringence) mode, an ECB (Electrically Controlled Birefringence) mode, a guest-host mode, or the like can be used.

[0410] The liquid crystal layer 776 may be a dispersed liquid crystal such as a polymer dispersed liquid crystal or a polymer network liquid crystal. In this case, a structure may be used for displaying black and white images without providing the color film 736, or a structure may be used for displaying colors using the color film 736.

[0411] In addition, as a driving method of the liquid crystal element, a time-sharing display method (also called a field sequential driving method) that uses a sequential additive color mixing method to perform color display can be applied. In this case, a structure without a color film 736 can be adopted. When the time-sharing display method is adopted, for example, there is no need to provide sub-pixels that respectively display R (red), G (green), and B (blue), so there is an advantage that the aperture ratio and clarity of the pixel can be improved.

[0412] <Display device including light-emitting element>

[0413] Fig.16 The display device 700 shown includes a light-emitting element 782. The light-emitting element 782 includes a conductive layer 772, an EL layer 786, and a conductive film 788. The EL layer 786 includes a light-emitting material such as an organic compound or an inorganic compound.

[0414] Examples of the light-emitting material include fluorescent materials, phosphorescent materials, thermally activated delayed fluorescence (TADF) materials, and inorganic compounds (quantum dot materials, etc.).

[0415] Fig.16 The display device 700 shown in the figure has an insulating film 730 covering a portion of a conductive layer 772 provided on a planarizing insulating film 770. Here, the light emitting element 782 is a top emission type light emitting element including a light-transmitting conductive film 788. Alternatively, the light emitting element 782 may have a bottom emission structure in which light is emitted from the conductive layer 772 side or a double-sided emission structure in which light is emitted from both the conductive layer 772 side and the conductive film 788 side.

[0416] In addition, the coloring film 736 is provided at a position overlapping with the light emitting element 782, and the light shielding film 738 is provided at a position overlapping with the routing wiring portion 711, the source driver circuit portion 704, and the insulating film 730. In addition, the coloring film 736 and the light shielding film 738 are covered by the insulating film 734. In addition, the space between the light emitting element 782 and the insulating film 734 is filled with the sealing film 732. In addition, when the EL layer 786 is formed into an island shape in each pixel or the EL layer 786 is formed into a strip shape in each pixel column, that is, when the EL layer 786 is formed by separate coating, the coloring film 736 may not be provided.

[0417] Fig.17 The structure of a display device suitable for a flexible display is shown. Fig.17 It is along Fig. 13B A cross-sectional view taken along dashed line ST in the display device 700A is shown.

[0418] Fig.17The display device 700A shown in the figure adopts a structure in which a first supporting substrate 745, an adhesive layer 742, a resin layer 743 and an insulating layer 744 are stacked to replace Fig.16 A substrate 701 is shown. A transistor 750, a capacitor 790, and the like are provided on an insulating layer 744 provided on a resin layer 743.

[0419] The support substrate 745 includes an organic resin, glass, or the like and is thin enough to be flexible. The resin layer 743 is a layer including an organic resin such as a polyimide resin or an acrylic resin. The insulating layer 744 includes an inorganic insulating film such as silicon oxide, silicon oxynitride, or silicon nitride. The resin layer 743 and the support substrate 745 are bonded together by an adhesive layer 742. The resin layer 743 is preferably thinner than the support substrate 745.

[0420] also, Fig.17 The display device 700A shown includes a protective layer 740 instead of Fig.16 The second substrate 705 is shown. The protective layer 740 is bonded to the sealing film 732. The protective layer 740 can be made of a glass substrate, a resin film, etc. In addition, the protective layer 740 can also be made of an optical component such as a polarizing plate, a scattering plate, an input device such as a touch sensor panel, or a stacked structure of two or more of the above optical components and the above input devices.

[0421] In addition, the EL layer 786 included in the light-emitting element 782 is provided in an island shape on the insulating film 730 and the conductive layer 772. By forming the EL layer 786 separately in a manner that the luminescent color of the EL layer 786 in each sub-pixel is different, color display can be achieved without using the coloring film 736. In addition, a protective layer 741 is provided to cover the light-emitting element 782. The protective layer 741 has a function of preventing impurities such as water from diffusing into the light-emitting element 782. The protective layer 741 is preferably formed using an inorganic insulating film. In addition, it is more preferable to adopt a stacked structure in which the inorganic insulating film and the organic insulating film are each one or more.

[0422] also, Fig.17 7 shows a foldable region P2. The region P2 includes a portion where no inorganic insulating film such as a supporting substrate 745, an adhesive layer 742, and an insulating layer 744 is provided. In addition, in the region P2, a resin layer 746 is provided to cover the wiring 760. By not providing an inorganic insulating film in the foldable region P2 as much as possible and only stacking a conductive layer containing a metal or alloy and a layer containing an organic material, cracks can be prevented from being generated when the region P2 is bent. In addition, by not providing a supporting substrate 745 in the region P2, a portion of the display device 700A can be bent with an extremely small radius of curvature.

[0423] <Configuration Example of Providing Input Device in Display Device>

[0424] In addition, it is also possible to Fig.14 , Fig.15 , Fig.16 or Fig.17 The display device 700 or the display device 700A shown in the figure is provided with an input device. As the input device, for example, a touch sensor or the like can be cited.

[0425] For example, various sensor types can be used, such as electrostatic capacitance type, resistance type, surface acoustic wave type, infrared type, optical type, pressure sensitive type, etc. In addition, two or more of the above types can be used in combination.

[0426] In addition, the touch panel has the following structures: a so-called In-Cell touch panel in which the input device is formed between a pair of substrates; a so-called On-Cell touch panel in which the input device is formed on the display device 700; a so-called Out-Cell touch panel in which the input device is bonded to the display device 700; and the like.

[0427] At least a part of the structural examples described in this embodiment mode and the drawings and the like corresponding to these examples can be implemented in combination with other structural examples or drawings and the like as appropriate.

[0428] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.

[0429] (Implementation 3)

[0430] In this embodiment, reference is made to 18A to 18C A display device including a semiconductor device according to one embodiment of the present invention will be described.

[0431] Fig.18A The display device shown includes a pixel portion 502, a driver circuit portion 504, a protection circuit 506, and a terminal portion 507. Note that the protection circuit 506 may not be provided.

[0432] The transistor of one embodiment of the present invention can be used as a transistor included in the pixel portion 502 or the driver circuit portion 504. Furthermore, the transistor of one embodiment of the present invention can also be used in the protection circuit 506.

[0433] The pixel portion 502 includes a plurality of pixel circuits 501 that drive a plurality of display elements arranged in X rows and Y columns (X and Y independently represent a natural number greater than or equal to 2).

[0434] The driving circuit unit 504 includes a gate driver 504a that outputs a scanning signal to the gate lines GL_1 to GL_X, a source driver 504b that supplies a data signal to the data lines DL_1 to DL_Y, and the like. The gate driver 504a includes at least a shift register. In addition, the source driver 504b is composed of, for example, a plurality of analog switches. In addition, the source driver 504b may also include a shift register, etc.

[0435] The terminal portion 507 is a portion where terminals for inputting power, control signals, image signals, and the like from an external circuit into the display device are provided.

[0436] The protection circuit 506 is a circuit that electrically connects a wiring connected thereto to another wiring when a potential outside a predetermined range is supplied thereto. Fig.18A The protection circuit 506 shown is connected to, for example, a gate line GL that is a wiring between the gate driver 504 a and the pixel circuit 501 , or a data line DL that is a wiring between the source driver 504 b and the pixel circuit 501 .

[0437] In addition, a structure in which the gate driver 504a and the source driver 504b are each provided on a substrate provided with a pixel portion 502 can be adopted, or a structure in which a substrate formed with a gate driving circuit or a source driving circuit (for example, a driving circuit board formed using a single crystal semiconductor film or a polycrystalline semiconductor film) is installed on a substrate provided with a pixel portion 502 by COG or TAB (Tape Automated Bonding).

[0438] also, Fig.18A The plurality of pixel circuits 501 shown may be, for example, Fig.18B , Fig.18C The structure shown.

[0439] Fig.18B The pixel circuit 501 shown includes a liquid crystal element 570, a transistor 550, and a capacitor 560. In addition, the pixel circuit 501 is connected to a data line DL_n, a gate line GL_m, a potential supply line VL, and the like.

[0440] The potential of one of the pair of electrodes of the liquid crystal element 570 is appropriately set according to the specifications of the pixel circuit 501. The orientation state of the liquid crystal element 570 depends on the data to be written. In addition, a common potential may be supplied to one of the pair of electrodes of the liquid crystal element 570 of each of the plurality of pixel circuits 501. In addition, a different potential may be supplied to one of the pair of electrodes of the liquid crystal element 570 of each of the pixel circuits 501 of each row.

[0441] also, Fig.18CThe pixel circuit 501 shown includes a transistor 552, a transistor 554, a capacitor 562, and a light emitting element 572. In addition, the pixel circuit 501 is connected to a data line DL_n, a gate line GL_m, a potential supply line VL_a, a potential supply line VL_b, and the like.

[0442] In addition, a high power supply potential VDD is applied to one of the potential supply line VL_a and the potential supply line VL_b, and a low power supply potential VSS is applied to the other of the potential supply line VL_a and the potential supply line VL_b. According to the potential applied to the gate of the transistor 554, the current flowing through the light-emitting element 572 is controlled, thereby controlling the brightness of the light emitted from the light-emitting element 572.

[0443] At least a part of the structural examples described in this embodiment mode and the drawings and the like corresponding to these examples can be implemented in combination with other structural examples or drawings and the like as appropriate.

[0444] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.

[0445] (Implementation 4)

[0446] A pixel circuit including a memory for correcting grayscale displayed by a pixel and a display device including the pixel circuit are described below. Any of the transistors described in Embodiment Mode 1 can be used as a transistor of a pixel circuit described below.

[0447] [Circuit structure]

[0448] Fig.19A : shows a circuit diagram of a pixel circuit 400. The pixel circuit 400 includes a transistor M1, a transistor M2, a capacitor C1, and a circuit 401. In addition, the pixel circuit 400 is connected to a wiring S1, a wiring S2, a wiring G1, and a wiring G2.

[0449] The gate of the transistor M1 is connected to the wiring G1, one of the source and the drain of the transistor M1 is connected to the wiring S1, and the other of the source and the drain of the transistor M1 is connected to one electrode of the capacitor C1. The gate of the transistor M2 is connected to the wiring G2, one of the source and the drain of the transistor M2 is connected to the wiring S2, and the other of the source and the drain of the transistor M2 is connected to the other electrode of the capacitor C1 and the circuit 401.

[0450] The circuit 401 includes at least one display element. Various display elements can be used, and typically, there are light-emitting elements such as organic EL elements and LED elements, liquid crystal elements, or MEMS elements.

[0451] A node connecting the transistor M1 and the capacitor C1 is referred to as a node N1 , and a node connecting the transistor M2 and the circuit 401 is referred to as a node N2 .

[0452] The pixel circuit 400 can maintain the potential of the node N1 by turning the transistor M1 off. In addition, the potential of the node N2 can be maintained by turning the transistor M2 off. In addition, by writing a predetermined potential to the node N1 through the transistor M1 when the transistor M2 is in the off state, the potential of the node N2 can be changed in accordance with the potential change of the node N1 due to capacitive coupling through the capacitor C1.

[0453] Here, as one or both of the transistor M1 and the transistor M2, the transistor using the oxide semiconductor illustrated in Embodiment 1 can be used. Due to the extremely low off-state current, the potential of the node N1 or the node N2 can be maintained for a long time. In addition, when the potential holding period of each node is short (specifically, when the frame frequency is 30 Hz or more, etc.), a transistor using a semiconductor such as silicon can also be used.

[0454] [Drive method example]

[0455] Next, refer to Fig.19B An example of an operation method of the pixel circuit 400 will be described. Fig.19B 4 is a timing chart of the operation of the pixel circuit 400. Note that for the sake of convenience, the influence of various resistances such as wiring resistance, parasitic capacitance of transistors and wiring, and threshold voltage of transistors are not considered here.

[0456] exist Fig.19B In the operation shown, one frame period is divided into a period T1 and a period T2. The period T1 is a period for writing a potential to the node N2, and the period T2 is a period for writing a potential to the node N1.

[0457] <Period T1>

[0458] During the period T1, a potential that turns the transistor on is supplied to the wiring G1 and the wiring G2. In addition, a fixed potential V is supplied to the wiring S1. ref , providing the first data potential V to the wiring S2 w .

[0459] The node N1 is supplied with a potential V from the wiring S1 via the transistor M1. ref In addition, the node N2 is supplied with the first data potential V through the transistor M2. w Therefore, capacitor C1 maintains the potential difference V w -V ref .

[0460] <Period T2>

[0461] Next, in period T2, a potential for turning on the transistor M1 is supplied to the wiring G1, a potential for turning off the transistor M2 is supplied to the wiring G2, and a second data potential V is supplied to the wiring S1. data Furthermore, the wiring S2 may be provided with a predetermined constant potential or be in a floating state.

[0462] The node N1 is supplied with the second data potential V via the transistor M1. data At this time, due to the capacitive coupling through the capacitor C1, the corresponding second data potential V data The potential of the node N2 changes, and the change is only the potential dV. That is, the circuit 401 is input with the first data potential V w The potential is the sum of the potential dV. Note that although Fig.19B The potential dV is shown as a positive value, but the potential dV can also be a negative value. That is, the second data potential V data It can also be compared with the potential V ref Low.

[0463] Here, the potential dV is mainly determined by the capacitance value of the capacitor C1 and the capacitance value of the circuit 401. When the capacitance value of the capacitor C1 is sufficiently greater than the capacitance value of the circuit 401, the potential dV is close to the second data potential V data .

[0464] As described above, since the pixel circuit 400 can combine two types of data signals to generate a potential supplied to the circuit 401 including a display element, grayscale correction can be performed within the pixel circuit 400 .

[0465] In addition, the pixel circuit 400 can generate a potential exceeding the maximum potential that can be supplied to the source driver connected to the wiring S1 and the wiring S2. For example, when a light-emitting element is used, a high dynamic range (HDR) display can be performed. In addition, when a liquid crystal element is used, overdriving can be achieved.

[0466] [Application Examples]

[0467] <Example of Using Liquid Crystal Element>

[0468] Fig.19C The pixel circuit 400LC shown includes a circuit 401LC. The circuit 401LC includes a liquid crystal element LC and a capacitor C2.

[0469] One electrode of the liquid crystal element LC is connected to the node N2 and one electrode of the capacitor C2, and the other electrode of the liquid crystal element LC is connected to the node N2 and one electrode of the capacitor C2. com2 The other electrode of capacitor C2 is connected to the supply potential V com1 Wiring connections.

[0470] Capacitor C2 is used as a storage capacitor. In addition, capacitor C2 can be omitted when not needed.

[0471] Since a high voltage can be supplied to the liquid crystal element LC in the pixel circuit 400LC, high-speed display can be realized by overdriving, and a liquid crystal material with a high driving voltage can be used. In addition, by supplying a correction signal to the wiring S1 or the wiring S2, grayscale correction can be performed according to the use temperature or the degradation state of the liquid crystal element LC.

[0472] <Example of using light-emitting elements>

[0473] Fig.19D The pixel circuit 400EL shown includes a circuit 401EL. The circuit 401EL includes a light emitting element EL, a transistor M3, and a capacitor C2.

[0474] The gate of the transistor M3 is connected to the node N2 and one electrode of the capacitor C2, and one of the source and the drain of the transistor M3 is connected to the supplied potential V H The other of the source and drain of the transistor M3 is connected to one electrode of the light emitting element EL. The other electrode of the capacitor C2 is connected to the supply potential V com The other electrode of the light emitting element EL is connected to the wiring supplied with the potential V L Wiring connections.

[0475] The transistor M3 has a function of controlling the current supplied to the light emitting element EL. The capacitor C2 is used as a storage capacitor. The capacitor C2 may be omitted when not required.

[0476] In addition, although the transistor M3 can also be connected to the anode side of the light emitting element EL, the transistor M3 can also be connected to the cathode side. In this case, the potential V can be appropriately changed. H With potential V L The value of .

[0477] In the pixel circuit 400EL, a high potential can be applied to the gate of the transistor M3 to allow a large current to flow through the light emitting element EL, thereby realizing HDR display, etc. In addition, the electrical characteristic deviation of the transistor M3 or the light emitting element EL can be corrected by providing a correction signal to the wiring S1 or the wiring S2.

[0478] In addition, not limited to Fig.19C and Fig.19D The circuit shown may also be supplemented with transistors or capacitors.

[0479] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.

[0480] (Implementation method 5)

[0481] In this embodiment, a display module that can be manufactured using one embodiment of the present invention is described.

[0482] Fig. 20A The display module 6000 shown includes a display device 6006 connected to an FPC 6005 , a frame 6009 , a printed circuit board 6010 , and a battery 6011 between an upper cover 6001 and a lower cover 6002 .

[0483] For example, a display device manufactured using one embodiment of the present invention can be used as the display device 6006. By using the display device 6006, a display module with extremely low power consumption can be implemented.

[0484] The shapes and sizes of the upper cover 6001 and the lower cover 6002 may be appropriately changed according to the size of the display device 6006 .

[0485] The display device 6006 may also function as a touch panel.

[0486] The frame 6009 can have the function of protecting the display device 6006, the function of blocking electromagnetic waves generated by the operation of the printed circuit board 6010, the function of a heat sink, and the like.

[0487] The printed circuit board 6010 has a power supply circuit, a signal processing circuit for outputting a video signal and a clock signal, a battery control circuit, and the like.

[0488] Fig. 20B FIG. 6 is a schematic cross-sectional view of a display module 6000 having an optical touch sensor.

[0489] The display module 6000 includes a light emitting portion 6015 and a light receiving portion 6016 provided on a printed circuit board 6010. In addition, a pair of light guide portions (light guide portion 6017a, light guide portion 6017b) are provided in the area surrounded by the upper cover 6001 and the lower cover 6002.

[0490] The display device 6006 overlaps with the printed circuit board 6010 and the battery 6011 via the frame 6009. The display device 6006 and the frame 6009 are fixed to the light guide portions 6017a and 6017b.

[0491] Light 6018 emitted from the light emitting unit 6015 passes through the top of the display device 6006 through the light guiding unit 6017a and reaches the light receiving unit 6016 through the light guiding unit 6017b. For example, when the light 6018 is blocked by a detected object such as a finger or a stylus pen, it can be detected as a touch operation.

[0492] For example, a plurality of light emitting units 6015 are provided along two adjacent sides of the display device 6006. A plurality of light receiving units 6016 are arranged at positions facing the light emitting units 6015. Thus, information on the position of the touch operation can be obtained.

[0493] As the light emitting unit 6015, a light source such as an LED element can be used, and in particular, a light source that emits infrared rays is preferably used. As the light receiving unit 6016, a photoelectric element that receives the light emitted by the light emitting unit 6015 and converts it into an electrical signal can be used. Preferably, a photodiode that can receive infrared rays is used.

[0494] By using the light guide 6017a and the light guide 6017b that transmit the light 6018, the light emitting unit 6015 and the light receiving unit 6016 can be arranged on the lower side of the display device 6006, and it is possible to prevent external light from reaching the light receiving unit 6016 and causing malfunction of the touch sensor. In particular, it is preferable to use a resin that absorbs visible light and transmits infrared light, thereby more effectively suppressing malfunction of the touch sensor.

[0495] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.

[0496] (Implementation 6)

[0497] In this embodiment, an example of electronic equipment in which a display device according to one embodiment of the present invention can be used is described.

[0498] Fig.21A The electronic device 6500 shown is a portable information terminal device that can be used as a smartphone.

[0499] The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, a button 6504, a speaker 6505, a microphone 6506, a camera 6507, a light source 6508, and the like. The display portion 6502 has a touch panel function.

[0500] As the display portion 6502 , a display device according to one embodiment of the present invention can be used.

[0501] Fig.21B 65 is a schematic cross-sectional view of an end portion of a housing 6501 on one side of a microphone 6506 .

[0502] A light-transmitting protective component 6510 is provided on the display surface side of the housing 6501, and a display panel 6511, an optical component 6512, a touch sensor panel 6513, a printed circuit board 6517, a battery 6518, etc. are provided in the space surrounded by the housing 6501 and the protective component 6510.

[0503] The display panel 6511 , the optical member 6512 , and the touch sensor panel 6513 are fixed to the protective member 6510 using an adhesive layer (not shown).

[0504] In addition, a portion of the display panel 6511 is folded in a region outside the display portion 6502. The folded portion is connected to an FPC 6515. An IC 6516 is mounted on the FPC 6515. The FPC 6515 is connected to a terminal provided on a printed circuit board 6517.

[0505] The display panel 6511 may use a flexible display panel of one embodiment of the present invention. Thus, an extremely lightweight electronic device may be realized. In addition, since the display panel 6511 is extremely thin, a large-capacity battery 6518 may be mounted while suppressing an increase in the thickness of the electronic device. In addition, by folding a portion of the display panel 6511 to provide a connection portion with the FPC 6515 on the back of the pixel portion, an electronic device with a narrow frame may be realized.

[0506] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.

[0507] (Implementation 7)

[0508] In this embodiment, various electronic devices including a display device manufactured using one embodiment of the present invention are described.

[0509] Each electronic device described below includes a display device according to one embodiment of the present invention in a display portion, and thus can realize high definition. In addition, it can realize both high definition and a large screen.

[0510] On the display unit of the electronic device according to one embodiment of the present invention, for example, images having a resolution of full HD, 4K2K, 8K4K, 16K8K or higher can be displayed.

[0511] Electronic devices include, for example, television devices, notebook personal computers, display devices, digital signage, pinball machines, game consoles, and other large electronic devices with relatively large screens, as well as digital cameras, digital video cameras, digital photo frames, mobile phones, portable game consoles, portable information terminals, and sound reproduction devices.

[0512] An electronic device using one embodiment of the present invention can be assembled along a flat or curved surface such as an inner wall or outer wall of a house or building, an interior decoration or exterior decoration of a car, etc.

[0513] Fig.22A This is an external view of a camera 8000 equipped with a viewfinder 8100 .

[0514] The camera 8000 includes a housing 8001 , a display portion 8002 , operation buttons 8003 , a shutter button 8004 , etc. In addition, the camera 8000 is equipped with a detachable lens 8006 .

[0515] Lens 8006 may also be included in the housing of camera 8000.

[0516] The camera 8000 can perform imaging by pressing a shutter button 8004 or touching a display portion 8002 serving as a touch panel.

[0517] The housing 8001 includes an embedder having electrodes so that it can be connected to a viewfinder 8100, a flash device, etc.

[0518] The viewfinder 8100 includes a housing 8101 , a display portion 8102 , a button 8103 , and the like.

[0519] The housing 8101 is attached to the camera 8000 via an inserter that is fitted into an inserter of the camera 8000. The viewfinder 8100 can display an image received from the camera 8000 on the display portion 8102.

[0520] Button 8103 is used as a power button or the like.

[0521] The display device according to one embodiment of the present invention can be used for the display portion 8002 of the camera 8000 and the display portion 8102 of the viewfinder 8100. Alternatively, the camera 8000 may include a built-in viewfinder.

[0522] Fig. 22B This is an appearance diagram of the head mounted display 8200.

[0523] The head mounted display 8200 includes a mounting portion 8201 , a lens 8202 , a main body 8203 , a display portion 8204 , a cable 8205 , and the like. In addition, a battery 8206 is built in the mounting portion 8201 .

[0524] Power is supplied from a battery 8206 to a main body 8203 via a cable 8205. The main body 8203 includes a wireless receiver and the like, and can display received image data and the like on a display portion 8204. In addition, the main body 8203 includes a camera, thereby making it possible to use the movement of the user's eyeballs and eyelids as an input method.

[0525] In addition, multiple electrodes may be provided at the position of the mounting portion 8201 touched by the user to detect the current flowing through the electrodes according to the movement of the user's eyeballs, thereby realizing recognition of the user's line of sight. In addition, the mounting portion 8201 may also have a function of monitoring the user's pulse according to the current flowing through the electrodes. The mounting portion 8201 may have various sensors such as a temperature sensor, a pressure sensor, and an acceleration sensor, and may also display the user's biological information on the display portion 8204 and change the image displayed on the display portion 8204 in synchronization with the movement of the user's head.

[0526] The display device according to one embodiment of the present invention can be used for the display portion 8204 .

[0527] FIG. 22C to FIG. 22E 8300 is an external view of a head mounted display 8300. The head mounted display 8300 includes a housing 8301, a display portion 8302, a belt-shaped fixing tool 8304, and a pair of lenses 8305.

[0528] The user can see the display on the display unit 8302 through the lens 8305. Preferably, the display unit 8302 is configured to be curved. This is because the user can experience a high sense of reality. In addition, by seeing the images displayed on different areas of the display unit 8302 through the lens 8305, three-dimensional display using parallax can be performed. In addition, an embodiment of the present invention is not limited to a structure in which one display unit 8302 is provided, and two display units 8302 can also be provided to configure two different display units for a pair of eyes of the user.

[0529] The display device of one embodiment of the present invention can be used for the display portion 8302. Since the display device including the semiconductor device of one embodiment of the present invention has extremely high resolution, even if Fig.22E By using lens 8305 to enlarge in this way, a more realistic image can be displayed without causing the user to see the pixels.

[0530] FIG. 23A to FIG. 23G The electronic device shown includes a housing 9000, a display portion 9001, a speaker 9003, operation keys 9005 (including a power switch or an operation switch), a connecting terminal 9006, a sensor 9007 (the sensor has the function of measuring the following factors: force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, electricity, radiation, flow, humidity, inclination, vibration, smell or infrared), a microphone 9008, etc.

[0531] FIG. 23A to FIG. 23GThe electronic device shown has various functions. For example, it may have the following functions: a function of displaying various information (static images, dynamic images, text images, etc.) on a display unit; a function of a touch panel; a function of displaying a calendar, date, or time, etc.; a function of controlling processing by using various software (programs); a function of wireless communication; a function of reading out programs or data stored in a storage medium for processing; etc. Note that the functions of the electronic device are not limited to the above functions, but may have various functions. The electronic device may include a plurality of display units. In addition, a camera or the like may be provided in the electronic device so that it has the following functions: a function of taking a static image or a dynamic image to store the taken image in a storage medium (an external storage medium or a storage medium built into the camera); a function of displaying the taken image on a display unit; etc.

[0532] Below, we explain in detail FIG. 23A to FIG. 23G Electronic equipment shown.

[0533] Fig.23A 9100 is a perspective view of a television set 9100. The television set 9100 can be incorporated with a large display portion 9001 having a size of, for example, 50 inches or more or 100 inches or more.

[0534] Fig. 23B 9101 is a perspective view of a portable information terminal 9101. The portable information terminal 9101 can be used as a smart phone, for example. The portable information terminal 9101 can also be provided with a speaker 9003, a connection terminal 9006, a sensor 9007, etc. In addition, the portable information terminal 9101 can display text or image information on multiple surfaces thereof. Fig. 23B An example of displaying three icons 9050 is shown. In addition, information 9051 represented by a dotted rectangle may be displayed on the other surface of the display unit 9001. Examples of information 9051 include information indicating that an email, SNS, or phone call has been received; a title of the email or SNS; a sender's name; a date; a time; a remaining battery level; and an antenna receiving signal strength. Alternatively, icon 9050 may be displayed at a location where information 9051 is displayed.

[0535] Fig.23C9102 is a three-dimensional diagram of a portable information terminal 9102. The portable information terminal 9102 has a function of displaying information on three or more surfaces of the display unit 9001. Here, an example is shown in which information 9052, information 9053, and information 9054 are displayed on different surfaces. For example, the user can also check the information 9053 displayed at a position that can be viewed from above the portable information terminal 9102 while the portable information terminal 9102 is placed in a jacket pocket. The user can check the display without taking the portable information terminal 9102 out of the pocket, thereby being able to determine, for example, whether to answer a call.

[0536] Fig.23D It is a stereoscopic diagram of a watch-type portable information terminal 9200. The portable information terminal 9200 can be used as a smart watch, for example. In addition, the display surface of the display unit 9001 is curved, and display can be performed on the curved display surface. For example, by communicating with a headset capable of wireless communication, the portable information terminal 9200 can make a hands-free call. In addition, the portable information terminal 9200 includes a connection terminal 9006, which can exchange data with other information terminals or charge. In addition, the charging work can also be performed using wireless power supply.

[0537] Fig.23E , Fig.23F and Figure 23G 9201 is a three-dimensional diagram of a foldable portable information terminal. Fig.23E is a perspective view of the portable information terminal 9201 in an unfolded state. Figure 23G is a perspective view of the portable information terminal 9201 in a folded state, and Fig.23F The portable information terminal 9201 is from Fig.23E and Figure 23G The portable information terminal 9201 is a three-dimensional diagram of a state in which one state changes to another state. The portable information terminal 9201 has good portability in the folded state, and has excellent display overview in the unfolded state because it has a large display area with seamless splicing. The display unit 9001 included in the portable information terminal 9201 is supported by three housings 9000 connected by hinges 9055. For example, the display unit 9001 can be bent with a curvature radius of more than 1 mm and less than 150 mm.

[0538] Fig.24A 100 shows an example of a television set. A display portion 7500 of a television set 7100 is incorporated in a housing 7101. Here, a structure in which the housing 7101 is supported by a stand 7103 is shown.

[0539] The operation can be performed by using the operation switch provided in the housing 7101 or the remote control operation machine 7111 provided separately. Fig.24AThe television set 7100 shown in the figure can be operated. Alternatively, a touch panel may be used for the display portion 7500, and the television set 7100 can be operated by touching the display portion 7500 with a finger or the like. Furthermore, the remote control unit 7111 may include a display portion in addition to the operation buttons.

[0540] Alternatively, the television set 7100 may include a television broadcast receiver or a communication device for connecting to a communication network.

[0541] Fig. 24B The notebook personal computer 7200 is shown. The notebook personal computer 7200 includes a housing 7211 , a keyboard 7212 , a pointing device 7213 , an external connection port 7214 , and the like. A display portion 7500 is incorporated in the housing 7211 .

[0542] Fig.24C and Fig.24D An example of digital signage is shown.

[0543] Fig.24C The digital signage 7300 shown includes a housing 7301, a display unit 7500, a speaker 7303, etc. In addition, it may also include an LED lamp, operation keys (including a power switch or an operation switch), a connection terminal, various sensors, a microphone, etc.

[0544] also, Fig.24D The digital signage 7400 is shown to be disposed on a cylindrical pillar 7401. The digital signage 7400 includes a display portion 7500 disposed along a curved surface of the pillar 7401.

[0545] The larger the display unit 7500 is, the more information can be provided at one time and the easier it is to attract people's attention, thereby improving the advertising effect, for example.

[0546] A touch panel is preferably used for display portion 7500 so that the user can operate digital signage 7300 or digital signage 7400. Thus, digital signage 7300 or digital signage 7400 can be used not only for advertisements but also for providing information required by users, such as route information, traffic information, and guidance of commercial facilities.

[0547] like Fig.24C and Fig.24D As shown, the digital signage 7300 or the digital signage 7400 can be linked with the information terminal device 7311 such as a smartphone carried by the user preferably through wireless communication. For example, the advertisement information displayed on the display unit 7500 can be displayed on the screen of the information terminal device 7311, and the display of the display unit 7500 can be switched by operating the information terminal device 7311.

[0548] Furthermore, the game can be executed on the digital signage 7300 or the digital signage 7400 using the information terminal device 7311 as an operation unit (controller). Thus, an unspecified number of users can participate in the game at the same time and enjoy the game.

[0549] A display device according to an embodiment of the present invention can be applied to Fig.24A and Fig.24D Display unit 7500 is shown.

[0550] Although the electronic device of this embodiment has a structure including a display portion, one embodiment of the present invention can also be applied to an electronic device that does not have a display portion.

[0551] At least a part of this embodiment mode can be implemented in combination with other embodiment modes described in this specification as appropriate.

[0552] [Example 1]

[0553] The following describes the results of manufacturing transistors having semiconductor layers with different structures and evaluating their electrical characteristics and reliability.

[0554] [Production of samples]

[0555] For the structure of the transistor to be manufactured, reference can be made to the transistor 100 described in Embodiment 1. Note that here, the transistor 100 is manufactured through the same process as that of the transistor 100A including a back gate electrode.

[0556] First, a tungsten film with a thickness of about 100 nm is formed on a glass substrate by sputtering, and the tungsten film is processed to form a first gate electrode. Next, as a first gate insulating layer, a first silicon nitride film with a thickness of about 240 nm, a second silicon nitride film with a thickness of about 60 nm, and a silicon oxynitride film with a thickness of about 3 nm are stacked by PECVD.

[0557] The first silicon nitride film is formed under the following conditions: flow rates of silane gas, nitrogen gas, and ammonia gas are 290 sccm, 2000 sccm, and 2000 sccm, respectively; the pressure is 200 Pa; the deposition power is 3000 W; and the substrate temperature is 350°C.

[0558] The second silicon nitride film was formed under the following conditions: flow rates of silane gas, nitrogen gas, and ammonia gas were 200 sccm, 2000 sccm, and 100 sccm, respectively; the pressure was 100 Pa; the deposition power was 2000 W; and the substrate temperature was 350°C.

[0559] The silicon oxynitride film was formed under the following conditions: flow rates of silane gas and nitrous oxide gas were 20 sccm and 3000 sccm, respectively; the pressure was 40 Pa; the deposition power was 3000 W; and the substrate temperature was 350°C.

[0560] Next, a metal oxide film having a thickness of about 30 nm was formed on the first gate insulating layer, and the metal oxide film was processed to form a semiconductor layer. Here, five samples (Samples A1 to A5) including metal oxide films formed under different deposition conditions were manufactured.

[0561] The metal oxide film of sample A1 was formed by sputtering using a metal oxide target, and the atomic ratio of the metal elements was In:Ga:Zn=5:1:6. A mixed gas of argon gas and oxygen gas was used as the forming gas, and the flow rate ratio of the oxygen gas was set to 2%. The film formation was performed without heating the substrate.

[0562] The metal oxide film of sample A2 was formed by sputtering using a metal oxide target, and the atomic ratio of the metal elements was In:Ga:Zn=4:2:3. A mixed gas of argon gas and oxygen gas was used as the forming gas, and the flow rate ratio of the oxygen gas was set to 10%. The film formation was performed without heating the substrate.

[0563] The metal oxide film of sample A3 was formed by sputtering using a metal oxide target, and the atomic ratio of the metal elements was In:Ga:Zn=1:1:1. A mixed gas of argon gas and oxygen gas was used as the forming gas, and the flow rate ratio of the oxygen gas was set to 30%. The film formation was performed without heating the substrate.

[0564] The metal oxide film of sample A4 was formed by sputtering using a metal oxide target, and the atomic ratio of the metal elements was In:Ga:Zn=1:3:4. A mixed gas of argon gas and oxygen gas was used as the forming gas, and the flow rate ratio of the oxygen gas was set to 10%. The film formation was performed without heating the substrate.

[0565] Sample A5 includes a stack of a first metal oxide film and a second metal oxide film. First, the first metal oxide film is formed by a sputtering method using a metal oxide target, and the atomic number ratio of the metal elements is In:Ga:Zn=1:1:1, and the thickness is about 25nm. Next, the second metal oxide film is formed by a sputtering method using a metal oxide target, and the atomic number ratio of the metal elements is In:Ga:Zn=5:1:6, and the thickness is about 5nm. A mixed gas of argon gas and oxygen gas is used as a forming gas, and the flow ratio of the oxygen gas is set to 30% in the formation of the first metal oxide film and to 2% in the formation of the second metal oxide film. The formation of the first metal oxide film and the second metal oxide film is performed without heating the substrate.

[0566] After the semiconductor layer is formed, heat treatment is performed at 350° C. for 1 hour in a nitrogen gas atmosphere, and then another heat treatment is performed at 350° C. for 1 hour in a mixed atmosphere of nitrogen gas and oxygen gas.

[0567] Next, as a second gate insulating layer, a first silicon oxynitride film with a thickness of approximately 5 nm, a second silicon oxynitride film with a thickness of approximately 140 nm, and a third silicon oxynitride film with a thickness of approximately 5 nm were formed by a PECVD method.

[0568] The first silicon oxynitride film was formed under the following conditions: flow rates of silane gas and nitrous oxide gas were 24 sccm and 18,000 sccm, respectively; the pressure was 200 Pa; the deposition power was 130 W; and the substrate temperature was 350° C.

[0569] The second silicon oxynitride film was formed under the following conditions: flow rates of silane gas and nitrous oxide gas were 200 sccm and 4000 sccm, respectively; pressure was 300 Pa; deposition power was 750 W; and substrate temperature was 350°C.

[0570] The third silicon oxynitride film was formed under the following conditions: flow rates of silane gas and nitrous oxide gas were 20 sccm and 3000 sccm, respectively; the pressure was 40 Pa; the deposition power was 500 W; and the substrate temperature was 350°C.

[0571] Next, a metal oxide film with a thickness of about 20 nm is formed on the second gate insulating layer by sputtering. The metal oxide film is formed using a metal oxide target in an oxygen-containing atmosphere, and the atomic ratio of the metal elements is In:Ga:Zn=4:2:3. Then, a heat treatment is performed at 350°C for 1 hour in a nitrogen-containing atmosphere.

[0572] Next, a molybdenum film with a thickness of about 100 nm is formed on the metal oxide film by sputtering, and then a portion of the molybdenum film and a portion of the metal oxide film are removed by etching to form a second gate electrode and a metal oxide layer.

[0573] Next, boron is added as an impurity element using the second gate electrode as a mask. A plasma ion doping device is used for adding the impurity. B2H6 gas is used as a gas for supplying boron.

[0574] Next, as a protective insulating layer covering the transistor, a silicon oxynitride film with a thickness of about 300 nm was formed by PECVD. Then, the protective insulating layer and the second gate insulating layer were partially etched to form an opening, and a molybdenum film was formed by sputtering, which was then processed to form a source electrode and a drain electrode. Then, as a planarizing layer, an acrylic resin film with a thickness of about 1.5 μm was formed, and heat treatment was performed at a temperature of 250° C. for 1 hour in a nitrogen atmosphere.

[0575] Through the above-described processes, samples A1 to A5 including transistors formed on a glass substrate were obtained.

[0576] [Id-Vg characteristics of transistor]

[0577] Next, the Id-Vg characteristics of the transistor manufactured as described above were measured.

[0578] The Id-Vg characteristics of the transistor were measured under the following conditions. The voltage applied to the gate electrode (hereinafter also referred to as the gate voltage (Vg)) was changed from -15V to +20V by 0.25V. In addition, the voltage applied to the source electrode (hereinafter also referred to as the source voltage (Vs)) was 0V (comm), and the voltage applied to the drain electrode (hereinafter also referred to as the drain voltage (Vd)) was 0.1V or 10V.

[0579] Each of the transistors to be measured had a single-gate structure with a designed channel length of 3 μm and a designed channel width of 50 μm. The number of transistors to be evaluated was 20 per sample.

[0580] [Reliability evaluation]

[0581] Next, in order to evaluate the reliability of the above transistor, a GBT test is performed. In the GBT test, the substrate on which the transistor is formed is kept at 60°C, a voltage of 0V is applied to the source and drain of the transistor, and a voltage of 20V or -20V is applied to the gate, and this state is maintained for 1 hour. Here, the PBTS test and the NBTIS test are particularly shown. Note that in the NBTIS test, white LED light of approximately 10,000 lx is irradiated on the sample.

[0582] [Result 1]

[0583] FIG. 25A to FIG. 25D The Id-Vg characteristics of the measured transistors are shown. Each graph shows two Id-Vg characteristics with different drain voltages (Vd) and field effect mobility (μFE) calculated from the Id-Vg characteristics when Vd=10V.

[0584] FIG. 25A to FIG. 25D The Id-Vg characteristics of sample A1, sample A2, sample A3, and sample A4 are shown. In each figure and the following description, the composition of the metal oxide film included in each sample is simply described as IGZO (516) or the like.

[0585] like FIG. 25A to FIG. 25D As shown, at the same Vg, the on-state current value is the largest in sample A1, followed by sample A2, sample A3, and sample A4. This may be related to the content of In. In addition, the unevenness of the electrical characteristics of sample A4 is greater than that of the other samples.

[0586] Fig.25E The variation (ΔVth) of the threshold voltage of samples A1 to A4 after the PBTS test and the NBTIS test is shown. Fig.25E As shown, ΔVth varies depending on the composition of the semiconductor layer.

[0587] When focusing on the PBTS test, the variation of the threshold voltage is the smallest in sample A1 (ie, sample A1 has good reliability), followed by sample A2, sample A3, and sample A4. In particular, the variation of the threshold voltage in sample A4 is significantly larger than that in other samples.

[0588] On the other hand, when focusing on the NBTIS test, the variation in threshold voltage of sample A1 is slightly larger than that of other samples, but the variation in threshold voltage of all samples is 2 V or less, which means that this sample has good reliability.

[0589] The above results show that the lower the gallium content in the metal oxide film used as the semiconductor layer, the more reliable the transistor can be. In particular, the results show that the change in threshold voltage in the PBTS test can be reduced by using a metal oxide film with a low gallium content. Furthermore, it can be seen that by using a metal oxide film with a higher indium content than gallium content and a higher zinc content than gallium content, a transistor with both high field effect mobility and high reliability can be realized.

[0590] [Result 2]

[0591] Fig.26A The Id-Vg characteristics of sample A5 are shown. As described above, the semiconductor layer of the transistor of sample A5 is a stacked film in which the second metal oxide film (IGZO (516)) is stacked on the first metal oxide film (IGZO (111)).

[0592] like Fig.26A As shown, it can be confirmed that sample A5 has less unevenness than sample A1 (IGZO (516)) and thus has good electrical characteristics. In addition, it can be confirmed that sample A5 has higher on-state current and higher field effect mobility than sample A3 (IGZO (111)).

[0593] Fig.26B The results of ΔVth after the reliability test of sample A5 are shown. Here, the results of the above-mentioned samples A1 and A3 are shown for comparison.

[0594] In the PBTS test, the variation of the threshold voltage of sample A5 is smaller than that of sample A1. In the NBTIS test, the variation of the threshold voltage of sample A5 is smaller than that of sample A3. In other words, it can be seen that sample A5 has higher reliability than the sample including a single film of a metal oxide film.

[0595] Here, the defect state at or near the interface between the gate insulating layer and the semiconductor layer is considered to be one of the causes of the variation of the threshold voltage in the PBTS test. Fig.26B The results show that by configuring a metal oxide film having a higher indium content than gallium content on one side of the gate insulating layer, defect states at or near the interface between the gate insulating layer and the semiconductor layer can be reduced.

[0596] Defect states caused by oxygen vacancies in the semiconductor layer are considered to be one of the causes of the variation in threshold voltage in NBTIS testing. Fig.26B The results show that by stacking a first metal oxide film having a higher gallium content than the second metal oxide film on the second metal oxide film in contact with the gate insulating layer, the defect state density can be reduced. Furthermore, since gallium is more easily bonded to oxygen than indium and zinc, oxygen vacancies are less likely to be generated in the first metal oxide film containing relatively more gallium.

[0597] In sample A5, the second metal oxide film, which has a low gallium content and is relatively easy to generate oxygen vacancies, is much thinner than the first metal oxide film, and sufficient oxygen is supplied from the gate insulating layer to the second metal oxide film by heat treatment. As a result, it is likely that the oxygen vacancies in the entire semiconductor layer are sufficiently reduced, and Fig.26A The unevenness shown is small and the transistor characteristics are good.

[0598] The above results show that by using a semiconductor layer formed by stacking a second metal oxide film that is in contact with a gate insulating layer and has a higher indium content than gallium, and a first metal oxide film that is thicker than the second metal oxide film and has a higher gallium content, a transistor with extremely good electrical characteristics and extremely high reliability can be realized.

[0599] [Example 2]

[0600] In this example, samples in which a metal oxide layer is formed on an insulating layer under different deposition conditions are manufactured, and the results of measuring the amounts of oxygen and argon desorbed from the insulating layer by thermal desorption spectroscopy (TDS) analysis are described.

[0601] [Production of samples]

[0602] First, as insulating layers on a glass substrate, a first oxynitride silicon film with a thickness of approximately 5 nm, a second oxynitride silicon film with a thickness of approximately 130 nm, and a third oxynitride silicon film with a thickness of approximately 5 nm are formed by a PECVD method under the same conditions as the second gate insulating layer shown in the above-mentioned embodiment 1.

[0603] Next, heat treatment was performed at 370° C. for 1 hour in a nitrogen atmosphere.

[0604] Next, a metal oxide film with a thickness of about 20 nm is formed on the insulating layer by sputtering. The metal oxide film is formed using a metal oxide target, and the atomic number ratio of the metal elements is In:Ga:Zn=4:2:4.1.

[0605] Here, five samples (samples B1 to B5) were manufactured using different forming gases when forming the metal oxide film.

[0606] Samples B1 to B4 were each formed using a mixed gas of argon gas and oxygen gas as a forming gas. Sample B1 was formed under the condition that the flow ratio of oxygen gas in the total flow of the forming gas (hereinafter referred to as the flow ratio) was 10%. Sample B2 was formed under the condition that the flow ratio of oxygen gas was 30%. Sample B3 was formed under the condition that the flow ratio of oxygen gas was 50%. Sample B4 was formed under the condition that the flow ratio of oxygen gas was 70%. Sample B5 was formed using only oxygen gas as a forming gas, which means that the flow ratio of oxygen gas was 100%.

[0607] Next, each sample was subjected to a heat treatment at 370° C. for 1 hour in a mixed atmosphere of oxygen gas and nitrogen gas.

[0608] Then, the metal oxide film of each sample was removed by a wet etching method.

[0609] Samples B1 to B5 were manufactured through the above-mentioned process.

[0610] [TDS analysis]

[0611] The TDS analysis was performed on the samples B1 to B5. The TDS analysis was performed at a heating rate of 30°C / min.

[0612] Fig. 27 The TDS analysis results of each sample are shown. Fig. 27 The results corresponding to the mass-to-charge ratio (M / z) of oxygen molecules 32 and the results corresponding to the mass-to-charge ratio of argon 40 are shown. The horizontal axis represents the substrate temperature (Sub.Temp.), and the vertical axis represents the detection intensity (Intensity).

[0613] like Fig. 27 As shown, in each sample, the oxygen molecule release is obvious at a temperature range of about 150° C. to 300° C., and there is a peak at a temperature range of 200° C. to 250° C. In addition, it can be confirmed that the higher the oxygen flow rate ratio when forming the metal oxide film, the greater the amount of oxygen released from the insulating layer.

[0614] On the other hand, the desorption of argon is obvious at a temperature in the range of about 250°C to 450°C, and there is a peak at a temperature in the range of 350°C to 400°C. In addition, it can be confirmed that the higher the oxygen flow rate ratio when forming the metal oxide film, the smaller the desorption amount of argon tends to be. In particular, under the condition of an oxygen flow rate of 100%, the desorption of argon is almost not confirmed, which means that argon is desorbed in the TDS analysis because it is a gas forming the metal oxide film.

[0615] Fig.28A and Fig.28B Shown from Fig. 27 The quantitative value of the desorption of oxygen molecules and argon calculated from the TDS analysis results.

[0616] from Fig.28A It can be confirmed that the higher the oxygen flow rate when the metal oxide film is formed, the greater the amount of oxygen molecules released from the insulating layer. In other words, it can be confirmed that when the insulating layer is used as the second gate insulating layer, the higher the oxygen flow rate when the metal oxide film is formed, the more oxygen is supplied to the semiconductor layer.

[0617] from Fig.28B It was confirmed that the amount of argon released from the insulating layer can be controlled by the oxygen flow ratio when the metal oxide film is formed.

[0618] [Example 3]

[0619] In this example, samples (samples C1 to C4) each having a stacked structure of an insulating film and a metal oxide film were manufactured, and the influence of the formation of the metal oxide film on the insulating film was evaluated.

[0620] [Production of samples]

[0621] First, a first silicon nitride film with a thickness of approximately 50 nm, a second silicon nitride film with a thickness of approximately 200 nm, a third silicon nitride film with a thickness of approximately 50 nm, and an oxynitride silicon film with a thickness of approximately 3 nm are stacked on a quartz substrate by a PECVD method.

[0622] The first silicon nitride film is formed under the following conditions: flow rates of silane gas, nitrogen gas, and ammonia gas are 200 sccm, 2000 sccm, and 100 sccm, respectively; the pressure is 100 Pa; the deposition power is 2000 W; and the substrate temperature is 350°C.

[0623] The second silicon nitride film was formed under the following conditions: flow rates of silane gas, nitrogen gas, and ammonia gas were 290 sccm, 2000 sccm, and 2000 sccm, respectively; the pressure was 200 Pa; the deposition power was 3000 W; and the substrate temperature was 350°C.

[0624] The third silicon nitride film is formed under the following conditions: flow rates of silane gas, nitrogen gas, and ammonia gas are 200 sccm, 2000 sccm, and 100 sccm, respectively; the pressure is 100 Pa; the deposition power is 2000 W; and the substrate temperature is 350°C.

[0625] The silicon oxynitride film was formed under the following conditions: flow rates of silane gas and nitrous oxide gas were 20 sccm and 3000 sccm, respectively; the pressure was 40 Pa; the deposition power was 3000 W; and the substrate temperature was 350°C.

[0626] Next, a metal oxide film with a thickness of about 30 nm is formed on the silicon oxynitride film. The metal oxide film is formed by a sputtering method using a metal oxide target, and the atomic number ratio of the metal elements is In:Ga:Zn=4:2:4.1. A mixed gas of argon gas and oxygen gas is used as a forming gas, and the flow rate ratio of the oxygen gas is set to 10%. The metal oxide film is formed under the following conditions: pressure of 0.6 Pa; power of 2.5 kW; and no heating of the substrate.

[0627] Next, heat treatment was performed. Sample C2 was heat treated at 350°C for 1 hour in a nitrogen gas atmosphere, and then another heat treatment was performed at 350°C for 1 hour in a mixed atmosphere of nitrogen gas and oxygen gas. Sample C3 was heat treated at 370°C for 1 hour in a nitrogen gas atmosphere, and then another heat treatment was performed at 370°C for 1 hour in a mixed atmosphere of nitrogen gas and oxygen gas. Sample C4 was heat treated at 400°C for 1 hour in a nitrogen gas atmosphere, and then heat treated at 400°C for 1 hour in a mixed atmosphere of nitrogen gas and oxygen gas. Sample C1 was not heat treated. Note that the volume ratio of nitrogen gas and oxygen gas in the mixed atmosphere is 4:1.

[0628] [ESR measurement]

[0629] Next, samples C1 to C4 were evaluated by an electron spin resonance method (ESR: Electron Spin Resonance).

[0630] In the ESR measurement, the measurement temperature was 85K, the high frequency power (microwave power) of 9.2 GHz was 10 mW, and the direction of the magnetic field was parallel to the film surface of each sample. The detection limit was 3.5×10 17 spins / cm 3 .

[0631] Fig.29A The ESR spectra of samples C1 to C4 are shown. Fig.29A In the figure, the horizontal axis represents the g-factor and the vertical axis represents the ESR signal intensity. Fig.29A As shown, a signal was observed in sample C1. The signal intensities of samples C2, C3, and C4 were below the detection limit.

[0632] Fig.29B This is an enlarged view of the ESR spectrum of sample C1. From the shape of the signal, it is considered that the signal caused by peroxide radicals (POR: Peroxide Radical) in the silicon oxynitride film overlaps with the signal caused by nitrogen dioxide (NO2) in the silicon oxynitride film.

[0633] Here, an asymmetric signal due to POR was observed at a g value of about 2.00. On the other hand, the signal due to NO2 was split into three signals according to the nuclear spin of nitrogen, and the three signals were observed at g values ​​of about 2.04, about 2.00, and about 1.96.

[0634] For reference, Fig.29C An ESR spectrum of a reference sample (Ref.) in which a silicon oxynitride film is formed on a quartz substrate is shown. Fig.29C FIG. 2 shows a typical example of a signal caused by NO2 in a silicon oxynitride film. Fig.29B and Fig.29C As shown, in the ESR spectrum of sample C1, the signal due to POR and the signal of NO2 may overlap.

[0635] Based on the shape of the signal due to NO2, the spin density of the signal due to NO2 in sample C1 was calculated to be 9.9×10 18 spins / cm 3 Since the signal due to POR overlaps with the signal due to NO2, the spin density of the signal due to POR cannot be calculated.

[0636] The above results show that when a metal oxide film is formed on a silicon oxynitride film, POR is formed in the silicon oxynitride film, and this POR is reduced by heat treatment. It is also known that NO2 in the silicon oxynitride film is reduced by heat treatment.

[0637] [Example 4]

[0638] In this example, the results of manufacturing a transistor according to one embodiment of the present invention and evaluating its electrical characteristics and reliability are described.

[0639] [Production of samples]

[0640] The structure of the transistor to be manufactured can refer to the transistor 100 and the transistor 100A described in Embodiment 1. That is, here, the transistor 100A including the back gate electrode and the transistor 100 not including the back gate electrode are manufactured by the same process.

[0641] First, a tungsten film with a thickness of about 100 nm is formed on a glass substrate by sputtering, and the tungsten film is processed to form a first gate electrode. Next, a stacked film of a first silicon nitride film with a thickness of about 240 nm, a second silicon nitride film with a thickness of about 60 nm, and a silicon oxynitride film with a thickness of about 5 nm is used as a first gate insulating layer by PECVD.

[0642] The first to third silicon nitride films are formed under the same conditions as those in the first embodiment described above.

[0643] Next, a single-layer metal oxide film or a stacked metal oxide film is formed on the first gate insulating layer to a total thickness of about 30 nm, and processed to form a semiconductor layer. Here, five samples including metal oxide films of different structures are manufactured.

[0644] The metal oxide films of Sample D1 and Sample E1 were formed by sputtering using a metal oxide target, and the atomic ratio of the metal elements was In:Ga:Zn=1:1:1. A mixed gas of argon gas and oxygen gas was used as the forming gas, and the flow rate ratio of the oxygen gas was set to 30%. The film formation was performed without heating the substrate.

[0645] In each of samples D2 to D5 and samples E2 to E5, a first metal oxide film having a thickness of about 25 nm and a second metal oxide film having a thickness of about 5 nm are stacked. The first metal oxide film of each sample is formed under the same conditions. The first metal oxide film is formed by a sputtering method using a metal oxide target, and the atomic number ratio of the metal element is In:Ga:Zn=1:1:1. A mixed gas of argon gas and oxygen gas is used as a forming gas, and the flow rate ratio of the oxygen gas is set to 30%. The film formation is performed without heating the substrate.

[0646] The second metal oxide film of each of the samples D2 and E2 was formed by a sputtering method using a metal oxide target, and the atomic number ratio of the metal elements was In:Ga:Zn=4:2:3. A mixed gas of argon gas and oxygen gas was used as a forming gas, and the flow rate ratio of the oxygen gas was 10%. The film formation was performed without heating the substrate. The second metal oxide film was continuously formed after the first metal oxide film was formed without being exposed to the atmosphere.

[0647] The second metal oxide film of each of the samples D3 and E3 was formed by a sputtering method using a metal oxide target, and the atomic number ratio of the metal elements was In:Ga:Zn=5:1:6. A mixed gas of argon gas and oxygen gas was used as a forming gas, and the flow rate ratio of the oxygen gas was set to 2%. The film formation was performed without heating the substrate. The second metal oxide film was continuously formed after the first metal oxide film was formed without being exposed to the atmosphere.

[0648] The second metal oxide film of each of the samples D4 and E4 was formed by a sputtering method using a metal oxide target, and the atomic number ratio of the metal element was In:Zn=2:3. A mixed gas of argon gas and oxygen gas was used as a forming gas, and the flow rate ratio of the oxygen gas was set to 2%. The film formation was performed without heating the substrate. The second metal oxide film was continuously formed after the first metal oxide film was formed without being exposed to the atmosphere.

[0649] The second metal oxide film of each of the samples D5 and E5 was formed by a sputtering method using a metal oxide target, and the atomic ratio of the metal elements was In:Sn:Si=80:9:11. A mixed gas of argon gas and oxygen gas was used as a forming gas, and the flow rate ratio of the oxygen gas was set to 6%. The film formation was performed without heating the substrate.

[0650] After the semiconductor layer is formed, heat treatment is performed at 350° C. for 1 hour in a nitrogen gas atmosphere, and then another heat treatment is performed at 350° C. for 1 hour in a mixed atmosphere of nitrogen gas and oxygen gas.

[0651] Next, as a second gate insulating layer, a first silicon oxynitride film with a thickness of approximately 5 nm, a second silicon oxynitride film with a thickness of approximately 140 nm, and a third silicon oxynitride film with a thickness of approximately 5 nm were formed by a PECVD method.

[0652] The first to third silicon oxynitride films are formed under the same conditions as those in the first embodiment described above.

[0653] Next, a metal oxide film is formed on the second gate insulating layer by a sputtering method. Here, the metal oxide film is formed under the following two conditions.

[0654] In samples D1 to D5, a metal oxide film having a thickness of about 20 nm was formed. The metal oxide film was formed using a metal oxide target in an oxygen-containing atmosphere, and the atomic number ratio of the metal elements was In:Ga:Zn=4:2:3.

[0655] In samples E1 to E5, a metal oxide film having a thickness of about 5 nm was formed The metal oxide film was formed by a reactive sputtering method using an aluminum target in an atmosphere containing oxygen.

[0656] After the metal oxide film was formed, heat treatment was performed at 350° C. for 1 hour in an atmosphere containing nitrogen and oxygen.

[0657] Next, a molybdenum film having a thickness of about 100 nm is formed on the metal oxide film by sputtering. Then, the molybdenum film is removed by etching to form a second gate electrode and a metal oxide layer. In samples D1 to D5, a portion of the molybdenum film and a portion of the metal oxide film are removed by etching. On the other hand, in samples E1 to E5, only the molybdenum film is removed by this etching.

[0658] Next, boron is added as an impurity element using the second gate electrode as a mask. A plasma ion doping device is used for adding the impurity. B2H6 gas is used as a gas for supplying boron.

[0659] Next, as a protective insulating layer covering the transistor, a silicon oxynitride film with a thickness of about 300 nm was formed by PECVD. Then, the protective insulating layer and the second gate insulating layer were partially etched to form an opening, and a molybdenum film was formed by sputtering, which was then processed to form a source electrode and a drain electrode. Then, as a planarizing layer, an acrylic resin film with a thickness of about 1.5 μm was formed, and heat treatment was performed at a temperature of 250° C. for 1 hour in a nitrogen atmosphere.

[0660] Through the above-described steps, samples D1 to D5 and samples E1 to E5 including transistors formed on a glass substrate were obtained.

[0661] [Id-Vg characteristics of transistor]

[0662] Next, the Id-Vg characteristics of the transistor manufactured as described above were measured.

[0663] The Id-Vg characteristics of the transistor were measured under the following conditions. The voltage applied to the gate electrode (hereinafter also referred to as the gate voltage (Vg)) was changed from -15V to +20V by 0.25V. In addition, the voltage applied to the source electrode (hereinafter also referred to as the source voltage (Vs)) was 0V (comm), and the voltage applied to the drain electrode (hereinafter also referred to as the drain voltage (Vd)) was 0.1V or 10V.

[0664] The transistors measured each have a designed channel length of 1.5 μm, 2 μm or 3 μm and a designed channel width of 50 μm. Single-gate transistors of samples D1 to D5, single-gate transistors of samples E1 to E5, and dual-gate transistors of samples E1 to E5 were measured. The number of transistors evaluated for each sample was 20.

[0665] [Reliability evaluation]

[0666] Next, in order to evaluate the reliability of the above transistor, a GBT test is performed. In the GBT test, the substrate on which the transistor is formed is kept at 60°C, a voltage of 0V is applied to the source and drain of the transistor, and a voltage of 20V or -20V is applied to the gate, and this state is maintained for 1 hour. Here, the PBTS test and the NBTIS test are particularly shown. Note that in the NBTIS test, white LED light of approximately 10,000 lx is irradiated on the sample.

[0667] [Result 1]

[0668] Fig. 30A The Id-Vg characteristics of transistors of samples D1 to D5 are shown. Each graph shows two Id-Vg characteristics with different drain voltages (Vd) and field effect mobility (μFE) calculated from the Id-Vg characteristics when Vd=10V.

[0669] exist Fig. 30A In the following description, the composition and type of the metal oxide film included in the semiconductor layer are simply referred to as IGZO (111), IGZO (423), IGZO (516), InZnO (2:3) or ITSO.

[0670] like Fig. 30A As shown, all samples exhibited good characteristics even when the channel length of the transistor was 1.5 μm. Furthermore, at the same Vg, samples D2 to D5 each including a semiconductor layer having a stacked structure flowed a larger current in the on state than sample D1 including a semiconductor layer having a single layer structure.

[0671] Fig. 30B The variation (ΔVth) of the threshold voltage of samples D1 to D5 after the PBTS test and the NBTIS test is shown.

[0672] When focusing on the PBTS test, sample D1 has the largest ΔVth, and each of samples D2 to D5 has a ΔVth that is less than half of that of sample D1.

[0673] On the other hand, when focusing on the NBTIS test, each of the samples D4 and D5 has a slightly larger ΔVth than the other samples, but the ΔVth of all the samples is 2 V or less, which means that the samples have good reliability.

[0674] [Result 2]

[0675] Fig.31A The Id-Vg characteristics of the transistors of samples E1 to E5 are shown. Similar to samples D1 to D5, samples E1 to E5 have good electrical characteristics.

[0676] Fig.31B ΔVth after the reliability test of Samples E1 to E5 is shown.

[0677] In sample E1, ΔVth in the PBTS test was large. This may be due to insufficient oxygen supply to the semiconductor layer because the metal oxide film formed on the gate insulating layer of sample E1 was different from that of sample D1.

[0678] However, in the PBTS test, ΔVth of samples E2 to E5 each including a semiconductor layer having a stacked structure is much smaller than that of sample E1. In particular, there is a tendency that the smaller the gallium content of the second metal oxide film is, the smaller ΔVth is in the PBTS test.

[0679] On the other hand, in the NBTIS test, ΔVth of each sample was small, and in particular, ΔVth of sample E4 was extremely small.

[0680] [Result 3]

[0681] Fig.32A and Fig.32B The results of the double-gate transistors of Samples E1 to E5 are shown.

[0682] from Fig.32A It can be confirmed that the variation in transistor characteristics of the double-gate transistor is much smaller than that of the single-gate transistor.

[0683] like Fig.32B As shown, it can be confirmed that ΔVth of the dual-gate transistor is particularly small in the NBTIS test.

[0684] The above results show that by using a semiconductor layer formed by stacking a second metal oxide film in contact with a gate insulating layer and having a higher indium content than gallium, and a first metal oxide film thicker than the second metal oxide film and having a higher gallium content, a transistor with extremely good electrical characteristics and extremely high reliability can be realized. In particular, it can be seen that by using a metal oxide film that does not contain gallium as the second metal oxide film, a transistor with extremely good electrical characteristics and extremely high reliability can be realized. In addition, it can be seen that gallium in the metal oxide film in contact with the gate insulating layer is the cause of the characteristic degradation in the PBTS test.

[0685] [Example 5]

[0686] [Study on the Change of Threshold Voltage in PBTS Test]

[0687] In this embodiment, the variation of the threshold voltage in the PBTS test is examined. Specifically, the reason why the variation of the threshold voltage in the PBTS test increases when a metal oxide film containing excess oxygen and a high gallium content is used as the semiconductor layer 108 is described using the results of first principle calculations.

[0688] It is expected that the increase in the variation of the threshold voltage in the PBTS test is caused by the formation of acceptor defects that capture electrons and the disappearance of donor defects that release electrons. Here, the formation of acceptor defects is considered as the mechanism of the increase in the variation of the threshold voltage in the PBTS test.

[0689] Here, the calculation model and calculation conditions used for the following calculations are described.

[0690] As a calculation model, a region corresponding to 6 atomic layers was cut out from the crystal structure of In-Ga-Zn oxide having an atomic number ratio of In:Ga:Zn:O=1:1:1:4. The total number of atoms included in this region is 56. Note that in the case where the calculation model has a structure including excess oxygen as described later, the total number of atoms included in the calculation model is 57.

[0691] Next, a vacuum layer is set in the c-axis direction of the above region. That is, the calculation model has a slab structure with periodicity in the a-axis direction and the b-axis direction and no periodicity in the c-axis direction. Note that the topmost layer of the slab structure is formed by O and one or two of Ga and Zn.

[0692] The calculation was performed using VASP (The Vienna Ab initio simulation Package), a first principle calculation software. Calculation conditions other than the above conditions are shown in Table 1. The Dipole Layer method was used for vacuum layer correction.

[0693] [Table 1]

[0694] software VASP Basis functions Plane Wave Functional GGA / PBE Pseudopotential PAW Cut-off energy 500eV k-point grid 4×4×1

[0695] In addition, the calculation of the subsequent reaction path adopts the nudged elastic band (NEB) method of chemical reaction path finding method. The NEB method is used to find the minimum energy path between the initial state and the final state. The energy height (energy difference) from the initial state to the minimum energy path is called the reaction barrier.

[0696] The above is the description of the calculation model and calculation conditions used for the following calculations.

[0697] Next, the possible defects before the PBTS test (in the initial state) and the defects in the PBTS test (in the final state) are described. In this embodiment, the defects in the initial state and the defects in the final state are caused by excess oxygen. Note that in this calculation, the defect is located in the topmost layer of the flat plate structure.

[0698] In the initial state, a structure without electron capture is adopted. As a structure without electron capture, a structure in which two oxygen atoms exist at the oxygen position is assumed. Note that a structure in which two oxygen atoms exist at the oxygen position is sometimes referred to as a split structure. Fig.33A is a schematic diagram of the segmentation structure.

[0699] Fig.33B The density of states obtained by calculating the computational model with a segmented structure is shown. Fig.33B In the figure, the horizontal axis represents energy (Energy) [eV], and the vertical axis represents the density of states (DOS) [states / eV]. The quasi-Fermi level is adjusted to 0 eV on the horizontal axis.

[0700] according to Fig.33B , the quasi-Fermi level is located on the upper side (high energy side) of the gap level. Therefore, it can be seen that the electrons are not captured by the split structure, that is, the split structure is not an acceptor. Therefore, the calculation model with the split structure is used as the initial state.

[0701] The final state is a structure that captures electrons (acceptor defect). As a structure that captures electrons, oxygen is assumed to be bonded to a gallium atom and has a dangling bond. Note that a structure in which oxygen is bonded to a gallium atom and has a dangling bond is sometimes referred to as a Ga-O structure. Fig.34A It is a schematic diagram of the Ga-O structure.

[0702] Fig.34B The density of states calculated for the calculation model with Ga-O structure is shown. Fig.34BIn the figure, the horizontal axis represents energy (Energy) [eV], and the vertical axis represents the density of states (DOS) [states / eV]. The quasi-Fermi level (the highest occupied energy level of electrons) is adjusted to 0 eV on the horizontal axis.

[0703] according to Fig.34B , the quasi-Fermi level is located on the lower side (low energy side) of the gap level. In other words, an acceptor defect is formed. Therefore, it can be known that the Ga-O structure is an acceptor that captures electrons. Therefore, the calculation model with the Ga-O structure is used as the end state.

[0704] Next, the energy change of the reaction path from the initial state to the final state before and during the PBTS test due to the different composition of the topmost layer of the calculation model and the change in the energy relationship between the initial state and the final state were evaluated by calculation.

[0705] Note that it is assumed that the transistor is turned off before the PBTS test. That is, carriers are not excited into the metal oxide film before the PBTS test. It is assumed that the transistor is turned on during the PBTS test. That is, carriers are excited into the metal oxide film during the PBTS test.

[0706] Note that the hydrogen enters the oxygen vacancy defect (this defect is denoted as V O H) generates carriers when it is formed. Therefore, in this calculation, by configuring a V O H, Reproduction of PBTS test. Note that V O H is located near the bottommost surface of the calculation model and at an oxygen position in a layer formed of In and O.

[0707] Here, two models (calculation model 1A and calculation model 2A) with different compositions of the top surface of the model are prepared. Calculation model 2A assumes a metal oxide film with a higher gallium content than calculation model 1A. In a metal oxide film with a high gallium content, the topmost layer is likely to be a layer with a high gallium content. Therefore, compared with the topmost layer of calculation model 1A, calculation model 2A includes a layer with a high gallium content as the topmost layer. Specifically, the topmost layer of calculation model 1A has an atomic number ratio of Ga:Zn:O=1:1:2. The topmost layer of calculation model 2A has an atomic number ratio of Ga:O=1:1. Note that by replacing Ga in a part of the layer formed by O and one or both of Ga and Zn with Zn, the atomic number ratio of calculation model 2A is consistent with that of calculation model 1A. This layer is located below the topmost layer, with a layer formed by In and O in between.

[0708] The calculation results of the energy change of the reaction path from the initial state to the final state and the change of the energy relationship between the initial state and the final state are described using the calculation model 1A.

[0709] The initial state is a calculation model 1A with a split structure, and the final state is a calculation model 1A with a Ga-O structure. The NEB method is used to calculate the change in the reaction path energy from the initial state to the final state before and during the PBTS test. The calculation conditions are the same as those shown in Table 1.

[0710] Fig.35A The calculation results of the energy change of the reaction path from the above initial state to the above end state when using the calculation model 1A are shown. Fig.35A The horizontal axis represents the reaction path. Note that Fig.35A The left side shows the initial state, and the right side shows the final state. The vertical axis represents energy [eV]. Fig.35A The dashed line in shows the calculation result assuming the state before the PBTS test. Fig.35A The solid line in shows the calculation result assuming the state in the PBTS test.

[0711] from Fig.35A It can be seen that, compared with the case of assuming the state before the PBTS test, the reaction barrier is lower and the final state is more stable when the state during the PBTS test is assumed. However, in the case of assuming the state before the PBTS test and the case of assuming the state during the PBTS test, the energy value of the initial state is smaller than the energy value of the final state. In other words, it can be seen that the initial state is more stable than the final state. Therefore, it can be inferred that the change in the threshold voltage during the PBTS test is smaller.

[0712] Next, the calculation results of the energy change of the reaction path from the initial state to the final state and the change of the energy relationship between the initial state and the final state are described using the calculation model 2A.

[0713] Fig.35B The calculation results of the energy change of the reaction path from the above initial state to the above end state when using the calculation model 2A are shown. Fig.35B The horizontal axis represents the reaction path. Note that Fig.35B The left side of shows the initial state. Fig.35B The right side of shows the end state. The vertical axis represents energy [eV]. Fig.35B The dashed line in shows the calculation result assuming the state before the PBTS test. Fig.35B The solid line in shows the calculation result assuming the state in the PBTS test.

[0714] from Fig.35BIt can be seen that, compared with the case of assuming the state before the PBTS test, when the state during the PBTS test is assumed, the reaction barrier is lower and the end state is more stable. Furthermore, when the state during the PBTS test is assumed, the energy value of the end state is smaller than the energy value of the initial state. In other words, it can be seen that the end state is more stable than the initial state. Therefore, it can be inferred that the variation of the threshold voltage in the PBTS test is large.

[0715] As described above, it is inferred that the variation of the threshold voltage increases by using a metal oxide film having a high gallium content as the semiconductor layer 108. In other words, it is inferred that the variation of the threshold voltage in the PBTS test is reduced by using a metal oxide film that does not contain gallium or has a low gallium content as the semiconductor layer 108.

[0716] Explanation of symbols

[0717] 10, 10A, 10B, 10C: transistor, 100, 100A, 100B, 100C: transistor, 102: substrate, 103: insulating layer, 103a, 103b, 103c, 103d: insulating film, 106: conductive layer, 108, 108a, 108b: semiconductor layer, 108f: metal oxide film, 108n: low resistance region, 110: insulating layer, 110a, 110b, 110c: insulating film, 112: conductive layer, 112f: conductive film, 114: metal oxide layer, 114f: metal oxide film, 116: insulating layer, 118: insulating layer, 120a, 120b: conductive layer, 140: impurity element, 141a, 141b, 142: opening

[0718] This application is based on Japanese Patent Application No. 2018-146787 accepted by the Japan Patent Office on August 3, 2018, Japanese Patent Application No. 2018-175352 accepted by the Japan Patent Office on September 19, 2018, Japanese Patent Application No. 2018-201126 accepted by the Japan Patent Office on October 25, 2018, and Japanese Patent Application No. 2019-061174 accepted by the Japan Patent Office on March 27, 2019, the entire contents of which are incorporated herein by reference.

Claims

1. A semiconductor device comprising: a first insulating layer; A semiconductor layer comprising indium, gallium and oxygen, the semiconductor layer being located on the first insulating layer; a second insulating layer having a stacked structure in which a first insulating film, a second insulating film and a third insulating film are stacked in sequence, the second insulating layer being located on the semiconductor layer; a first conductive layer on the second insulating layer; and a metal oxide layer between the second insulating layer and the first conductive layer, wherein the first insulating film, the second insulating film and the third insulating film each include an oxide, The first insulating film includes a portion in contact with the semiconductor layer, The semiconductor layer includes a region in which the content of indium is higher than the content of gallium. The metal oxide layer comprises one or more elements selected from aluminum, hafnium, indium, gallium and zinc, The metal oxide layer comprises indium, Furthermore, the metal oxide layer and the semiconductor layer have substantially the same indium content.

2. A semiconductor device comprising: a first insulating layer; A semiconductor layer comprising indium and oxygen, the semiconductor layer being located on the first insulating layer; a second insulating layer having a stacked structure in which a first insulating film, a second insulating film and a third insulating film are stacked in sequence, the second insulating layer being located on the semiconductor layer; a first conductive layer on the second insulating layer; as well as a metal oxide layer between the second insulating layer and the first conductive layer, wherein the semiconductor layer does not contain gallium, The first insulating film, the second insulating film, and the third insulating film each include an oxide, The first insulating film includes a portion in contact with the semiconductor layer, The metal oxide layer comprises one or more elements selected from aluminum, hafnium, indium, gallium and zinc, The metal oxide layer comprises indium, Furthermore, the metal oxide layer and the semiconductor layer have substantially the same indium content.

3. A semiconductor device comprising: a first insulating layer; a second semiconductor layer on the first insulating layer; a first semiconductor layer on the second semiconductor layer; a second insulating layer having a stacked structure in which a first insulating film, a second insulating film and a third insulating film are stacked in sequence, the second insulating layer being located on the first semiconductor layer; a first conductive layer on the second insulating layer; as well as a metal oxide layer between the second insulating layer and the first conductive layer, wherein the first insulating film, the second insulating film and the third insulating film each include an oxide, The first insulating film includes a portion in contact with the first semiconductor layer, The first semiconductor layer includes indium and oxygen, The second semiconductor layer comprises indium, zinc, gallium and oxygen, The first semiconductor layer includes a region having a higher indium content than that of the second semiconductor layer, The metal oxide layer comprises one or more elements selected from aluminum, hafnium, indium, gallium and zinc, The metal oxide layer comprises indium, Furthermore, the metal oxide layer and the first semiconductor layer have substantially the same indium content.

4. A semiconductor device comprising: a first insulating layer; a second semiconductor layer on the first insulating layer; a first semiconductor layer on the second semiconductor layer; a second insulating layer on the first semiconductor layer; a first conductive layer on the second insulating layer; as well as a metal oxide layer between the second insulating layer and the first conductive layer, The first insulating layer includes a portion in contact with the second semiconductor layer. The first semiconductor layer includes indium and oxygen, The second semiconductor layer comprises indium, zinc, gallium and oxygen, The first semiconductor layer includes a region having a higher indium content than that of the second semiconductor layer, The metal oxide layer comprises one or more elements selected from aluminum, hafnium, indium, gallium and zinc, The metal oxide layer comprises indium, Furthermore, the metal oxide layer and the first semiconductor layer have substantially the same indium content.

5. The semiconductor device according to claim 1, wherein the semiconductor layer comprises zinc, Furthermore, the semiconductor layer includes a region in which a content rate of zinc is higher than a content rate of gallium. 6 . The semiconductor device according to claim 1 , wherein the first insulating film is formed at a lower deposition rate than the second insulating film.

7. The semiconductor device according to claim 1 or 2, further comprising a second conductive layer, The second conductive layer includes a region overlapping the semiconductor layer via the first insulating layer. The first insulating layer has a stacked structure in which a fourth insulating film, a fifth insulating film, a sixth insulating film and a seventh insulating film are stacked in sequence, The seventh insulating film contains oxygen, And the fourth insulating film, the fifth insulating film, and the sixth insulating film each contain nitrogen.

8. The semiconductor device according to claim 3 or 4, further comprising a second conductive layer, The second conductive layer includes a region overlapping the second semiconductor layer via the first insulating layer. The first insulating layer has a stacked structure in which a fourth insulating film, a fifth insulating film, a sixth insulating film and a seventh insulating film are stacked in sequence, The seventh insulating film contains oxygen, And the fourth insulating film, the fifth insulating film, and the sixth insulating film each contain nitrogen.

9. The semiconductor device according to claim 7, wherein the seventh insulating film includes silicon oxide, Furthermore, the fourth insulating film, the fifth insulating film, and the sixth insulating film each include silicon nitride.

10. The semiconductor device according to claim 8, wherein the seventh insulating film includes silicon oxide, Furthermore, the fourth insulating film, the fifth insulating film, and the sixth insulating film each include silicon nitride.

11. The semiconductor device according to claim 2, wherein the semiconductor layer comprises zinc.

12. The semiconductor device according to claim 3 or 4, The first semiconductor layer comprises zinc and gallium, The first semiconductor layer includes a region in which the gallium content is lower than the indium content and the zinc content is higher than the gallium content. And the first semiconductor layer includes a region having a zinc content higher than or equal to a zinc content of the second semiconductor layer.