Electrolyte for lithium secondary battery and lithium secondary battery including the same
LiPF6 decomposition is solved by using electrolytes of non-aqueous organic solvents, lithium salts and specific additives, including compounds and negative electrode film forming agents, in lithium secondary batteries, forming an ionic conductive film and SEI layer of polar-SO3-groups. The side reaction problems caused by improve the high temperature stability and cycle life of lithium secondary batteries.
Patent Information
- Application Number
- CN201980053485.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-07
- Filing Date
- 2019-06-18
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-06-18
AI Technical Summary
LiPF6 lithium salt commonly used in existing lithium secondary batteries will generate gas when decomposed, resulting in poor battery stability and deterioration of high-temperature performance. An electrolyte that can suppress side reactions is needed to improve battery performance.
Using electrolytes including nonaqueous organic solvents, lithium salts and specific additives, the additives consist of a compound represented by chemical formula 1 and a negative electrode film forming agent. The compound has excellent solubility and control, and can form polar-SO3- groups rich in polarity. The ion conductive film captures F-, prevents the decomposition of the positive electrode, and forms a SEI layer on the surface of the negative electrode to suppress rapid reaction.
The high-temperature stability and cycle life characteristics of lithium secondary batteries at high temperatures are improved, reducing internal gas generation and increasing resistance, and extending the cycle life of the battery.
Smart Images

Figure CN112567558B_ABST
Abstract
Description
Technical Field
[0001] Disclosed are an electrolyte for a lithium secondary battery and a lithium secondary battery including the same. Background Art
[0002] Lithium secondary batteries are rechargeable, and have an energy density per unit weight that is three or more times higher than that of conventional lead storage batteries, nickel-cadmium batteries, nickel-metal hydride batteries, nickel-zinc batteries, etc. They can also be charged at a high rate, and therefore are commercially manufactured for notebook computers, mobile phones, power tools, electric bicycles, etc., and research on increasing the additional energy density has been actively conducted.
[0003] Such a lithium secondary battery is manufactured by injecting an electrolyte into a battery cell including a positive electrode including a positive electrode active material capable of intercalating / deintercalating lithium ions and a negative electrode including a negative electrode active material capable of intercalating / deintercalating lithium ions.
[0004] In particular, the electrolyte includes an organic solvent in which a lithium salt is dissolved, and critically determines the stability and performance of a lithium secondary battery.
[0005] LiPF6, the most commonly used electrolyte lithium salt, has the problem of reacting with electrolytic solvents to promote solvent consumption and generate a large amount of gas. When LiPF6 decomposes, it generates LiF and PF5, resulting in electrolyte consumption in the battery, resulting in high temperature performance degradation and poor safety.
[0006] There is a need for an electrolyte that suppresses the side reactions of such lithium salts and improves the performance of the battery. Summary of the invention
[0007]
Technical issues
[0008] Embodiments provide an electrolyte for a lithium secondary battery having improved cycle-life characteristics while ensuring high-temperature stability.
[0009] Another embodiment provides a lithium secondary battery including the electrolyte for a lithium secondary battery.
[0010]
Technical solution
[0011] An embodiment of the present invention provides an electrolyte for a lithium secondary battery, which includes a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive includes a compound represented by Chemical Formula 1 and a negative electrode film-forming agent.
[0012] [Chemical formula 1]
[0013]
[0014] In Chemical Formula 1,
[0015] R1 To R 6 are independently hydrogen, substituted or unsubstituted C1 to C10 alkyl, substituted or unsubstituted C1 to C10 alkoxy, substituted or unsubstituted C2 to C10 alkenyl, substituted or unsubstituted C2 to C10 alkynyl, substituted or unsubstituted C3 to C10 cycloalkyl, or substituted or unsubstituted C3 to C10 cycloalkenyl, and
[0016] n is an integer of 1 to 10.
[0017] Chemical Formula 1 may be represented by Chemical Formula 1A.
[0018] [Chemical Formula 1A]
[0019]
[0020] In Chemical Formula 1A,
[0021] R 1 and R 2 are independently hydrogen, substituted or unsubstituted C1 to C10 alkyl, substituted or unsubstituted C1 to C10 alkoxy, substituted or unsubstituted C2 to C10 alkenyl, substituted or unsubstituted C2 to C10 alkynyl, substituted or unsubstituted C3 to C10 cycloalkyl, or substituted or unsubstituted C3 to C10 cycloalkenyl, and
[0022] n is an integer of 1 to 10.
[0023] R 1 and R 2 They may independently be substituted or unsubstituted C1 to C4 alkyl groups, or substituted or unsubstituted C2 to C4 alkenyl groups.
[0024] R 1 and R 2 They may independently be C1 to C4 alkyl groups which may be substituted by halogen or cyano, or C2 to C4 alkenyl groups which may be substituted by halogen or cyano.
[0025] R 1 and R 2 may be independently methyl, ethyl or vinyl, and R 3 To R 6 The groups may independently be substituted or unsubstituted C1 to C5 alkyl groups.
[0026] The negative electrode film-forming agent may include at least one of vinylene carbonate (VC), vinylethylene carbonate (VEC), and fluoroethylene carbonate (FEC).
[0027] The compound represented by Chemical Formula 1 may be included in an amount of 0.05 to 5 wt % based on the total amount of the electrolyte for a lithium secondary battery, and the negative electrode film-forming agent may be included in an amount of 0.05 to 20 wt % based on the total amount of the electrolyte for a lithium secondary battery.
[0028] The compound represented by Chemical Formula 1 may be included in an amount of 0.1 to 2 wt % based on the total amount of the electrolyte for a lithium secondary battery, and the negative electrode film-forming agent may be included in an amount of 0.5 to 5 wt % based on the total amount of the electrolyte for a lithium secondary battery.
[0029] The additive may further include a nitrile-based compound.
[0030] The nitrile-based compound may include at least one of succinonitrile, adiponitrile, and glutaronitrile.
[0031] The nitrile-based compound may be included in an amount of 0.2 wt % to 5 wt % based on the total amount of the electrolyte for a lithium secondary battery.
[0032] Another embodiment of the present invention provides a lithium secondary battery including a positive electrode; a negative electrode, and an electrolyte.
[0033] A solid electrolyte interface (SEI) layer may be further included on the surface of the negative electrode, and the SEI layer may include a reaction product of the additive.
[0034]
Beneficial effects
[0035] While ensuring high temperature stability, it is possible to realize a lithium secondary battery having further improved cycle-life characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 is a schematic diagram showing a lithium secondary battery according to an embodiment of the present invention.
[0037] Figure 2 Nyquist plot showing the initial impedance analysis results of a lithium secondary battery cell.
[0038] Figure 3 Nyquist plot showing the impedance analysis results of a lithium secondary battery cell after being left at high temperature (2 weeks).
[0039] Figure 4 It is a graph showing the discharge capacity retention rate at 25° C. according to the cycle of the lithium secondary battery.
[0040] Figure 5 Shown are the results of measuring the amount of gas generated after a lithium secondary battery was stored at high temperature for 2 weeks.
[0041] <symbol description>
[0042] 100: Lithium secondary battery
[0043] 112: Negative electrode
[0044] 113: Partition
[0045] 114: Positive electrode
[0046] 120: Battery housing
[0047] 140: Sealing member DETAILED DESCRIPTION OF THE INVENTION
[0049] Hereinafter, embodiments of the present invention are described in detail. However, these embodiments are exemplary, the present invention is not limited thereto, and the present invention is defined by the scope of the claims.
[0050] In the present specification, when no definition is otherwise provided, "substituted" means that the hydrogen of the compound is substituted by a substituent selected from a halogen atom (F, Br, Cl or I), a hydroxyl group, an alkoxy group, a nitro group, a cyano group, an amino group, an azido group, an amidino group, a hydrazine group, a hydrazone group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphoric acid or a salt thereof, a C1 to C20 alkyl group, a C2 to C20 alkenyl group, a C2 to C20 alkynyl group, a C6 to C30 aryl group, a C7 to C30 arylalkyl group, a C1 to C4 alkoxy group, a C1 to C20 heteroalkyl group, a C3 to C20 heteroarylalkyl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C15 cycloalkynyl group, a C2 to C20 heterocycloalkyl group, and a combination thereof.
[0051] Hereinafter, an electrolyte for a lithium secondary battery according to an embodiment is described.
[0052] An electrolyte for a lithium secondary battery according to an embodiment includes a non-aqueous organic solvent, a lithium salt, and an additive, wherein the additive includes a compound represented by Chemical Formula 1 and a negative electrode film-forming agent.
[0053] [Chemical formula 1]
[0054]
[0055] In Chemical Formula 1,
[0056] R 1 To R 6 are independently hydrogen, substituted or unsubstituted C1 to C10 alkyl, substituted or unsubstituted C1 to C10 alkoxy, substituted or unsubstituted C2 to C10 alkenyl, substituted or unsubstituted C2 to C10 alkynyl, substituted or unsubstituted C3 to C10 cycloalkyl, or substituted or unsubstituted C3 to C10 cycloalkenyl, and
[0057] n is an integer of 1 to 10.
[0058] The compound represented by Chemical Formula 1 is a neutral compound having no charge, and has excellent solubility in a solvent, and its content is easily controlled.
[0059] In addition, the compound represented by Chemical Formula 1 has an anodic oxidation decomposition reaction or interacts with LiPF6 during charging, and thereby forms a strong ion conductive CEI (cathode-electrolyte interface) film rich in chemical substances having polar -SO3- groups, and the -Si-O- groups of the compound represented by Chemical Formula 1 can react with F-containing electrolytes in the electrolyte. - reacts with the chemical (e.g., HF) and captures F - , and thereby forming a compound with a strong Si-F bond, and thus preventing the positive electrode from being dissolved or decomposed by HF. Therefore, undesirable side reactions between the electrode and the electrolyte can be suppressed, and therefore, the amount of gas generated inside the battery can be reduced, and the resistance increase rate inside the lithium secondary battery can be reduced.
[0060] In addition, since the compound represented by Chemical Formula 1 includes two -SO2-O-Si- groups in one molecule, the above-mentioned effect can be further maximized at the same molar concentration as that of the compound including one -SO2-O-Si- group in one molecule.
[0061] In addition, a negative electrode film-forming agent is added thereto to form a film on the surface of the negative electrode of the lithium secondary battery, which can inhibit the rapid reaction between the negative electrode and the non-aqueous electrolyte, especially at high temperatures during charging and discharging, and thereby prevent thermal runaway of the lithium secondary battery in advance and thus improve the cycle life characteristics.
[0062] For example, Chemical Formula 1 may be represented by Chemical Formula 1A.
[0063] [Chemical Formula 1A]
[0064]
[0065] In Chemical Formula 1A, R 1 , R 2 and n are the same as above.
[0066] For example, R 1 and R 2 They may independently be substituted or unsubstituted C1 to C4 alkyl groups, or substituted or unsubstituted C2 to C4 alkenyl groups.
[0067] For example, R 1 and R 2 They may independently be C1 to C4 alkyl groups which may be substituted by halogen or cyano, or C2 to C4 alkenyl groups which may be substituted by halogen or cyano.
[0068] As an example, R 1 and R 2 may be independently methyl, ethyl or vinyl, and R 3 To R 6 The groups may independently be substituted or unsubstituted C1 to C5 alkyl groups.
[0069] The negative electrode film-forming agent may include at least one of vinylene carbonate (VC), vinylethylene carbonate (VEC), and fluoroethylene carbonate (FEC).
[0070] The double bonds included in the negative electrode film-forming agent are supplied with electrons from the dissociated anions of the non-aqueous organic solvent and from the surface of the negative electrode and are thereby reduced to anion radicals, and these anion radicals react with another double bond and thereby have a polymerization reaction, and the negative electrode film-forming agent can form an SEI (solid electrolyte interface) layer that is insoluble in the electrolyte on the surface of the negative electrode.
[0071] When the SEI layer grows beyond a certain thickness, the negative electrode film-forming agent does not diffuse into the lithium metal to complete the polymerization reaction, and thus a protective layer with a predetermined thickness remains on the lithium surface. Therefore, a lithium secondary battery with an SEI layer can have excellent cycle life characteristics.
[0072] For example, the compound represented by Chemical Formula 1 may be included in an amount of 0.05 wt % to 5 wt % based on the total amount of the electrolyte for a lithium secondary battery, and the negative electrode film-forming agent may be included in an amount of 0.05 wt % to 20 wt % based on the total amount of the electrolyte for a lithium secondary battery.
[0073] For example, the compound represented by Chemical Formula 1 may be included in an amount of 0.05 wt % to 3 wt %, or 0.1 wt % to 3 wt %.
[0074] In addition, the negative electrode film-forming agent may be included in an amount of 0.1 wt % to 20 wt %, or 0.1 wt % to 15 wt %.
[0075] As the most specific example, the compound represented by Chemical Formula 1 may be included in an amount of 0.1 wt % to 2 wt %, and the negative electrode film-forming agent may be included in an amount of 0.5 wt % to 5 wt %.
[0076] When the content range of the compound represented by Chemical Formula 1 is within the above range, resistance increase and gas formation during high-temperature storage may be suppressed, thereby realizing a lithium secondary battery having improved charge-discharge characteristics.
[0077] That is, when the amount of the compound represented by Chemical Formula 1 is less than 0.05 wt %, storage characteristics at high temperatures may be deteriorated, and when it is greater than 5 wt %, interface resistance may increase, and thus cycle life may be deteriorated.
[0078] In addition, when the content of the negative electrode film-forming agent is within the above range, a film having a sufficient thickness to protect the surface of the negative electrode can be formed within a range in which the conductivity of lithium ions is not reduced.
[0079] That is, when the content of the negative electrode film-forming agent is less than 0.05 wt %, a film having a sufficient thickness cannot be formed, and when it exceeds 20 wt %, lithium ion conductivity may be disturbed due to excessive film formation.
[0080] The additive according to the embodiment may further include a nitrile-based compound in addition to the compound represented by Chemical Formula 1 and the negative electrode film-forming agent.
[0081] The nitrile-based compound may include at least one of succinonitrile, adiponitrile, and glutaronitrile.
[0082] The nitrile-based compound forms a stable passivation film on the surface of the positive electrode, which can improve the performance of the battery and increase the flame retardancy to ensure stability.
[0083] The nitrile-based compound may be included in an amount of 0.2 wt % to 5 wt % based on the total amount of the electrolyte for a lithium secondary battery.
[0084] For example, the nitrile group compound may be included in an amount of 0.5 wt % to 5 wt %, for example, the nitrile group compound may be included in an amount of 1 wt % to 5 wt %.
[0085] The non-aqueous organic solvent serves as a medium for transporting ions participating in the electrochemical reaction of the battery.
[0086] The non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based or aprotic solvent.
[0087] Carbonate-based solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. Ester-based solvents may include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanoic acid lactone, mevalonate lactone, caprolactone, etc. Ether-based solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc. In addition, ketone-based solvents may include cyclohexanone, etc. Alcohol-based solvents may include ethanol, isopropanol, etc., and aprotic solvents may include nitriles such as R-CN (wherein R is a hydrocarbon group having a C2 to C20 linear, branched or cyclic structure and may include a double bond, an aromatic ring or an ether bond), etc., dioxolanes such as 1,3-dioxolane, etc., cyclopentane, etc.
[0088] The non-aqueous organic solvent may be used alone or in a mixture. When the organic solvent is used in a mixture, the mixing ratio may be controlled according to the desired battery performance.
[0089] The carbonate-based solvent is prepared by mixing a cyclic carbonate and a linear carbonate. When the cyclic carbonate and the linear carbonate are mixed together in a volume ratio of 1:1 to 1:9, the electrolyte performance can be improved.
[0090] The non-aqueous organic solvent may further include an aromatic hydrocarbon-based organic solvent in addition to the carbonate-based solvent. Herein, the carbonate-based solvent and the aromatic hydrocarbon-based organic solvent may be mixed in a volume ratio of 1:1 to 30:1.
[0091] The aromatic hydrocarbon-based organic solvent may be an aromatic hydrocarbon-based compound of Chemical Formula 2.
[0092] [Chemical formula 2]
[0093]
[0094] In chemical formula 2, R 7 To R 12 are the same or different and are selected from hydrogen, halogen, C1 to C10 alkyl, haloalkyl, and combinations thereof.
[0095] Specific examples of the aromatic hydrocarbon-based organic solvent may be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluoroform, Benzene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene and combinations thereof.
[0096] The electrolyte may further include vinylene carbonate or an ethylene carbonate-based compound represented by Chemical Formula 3 in order to improve the cycle life of the battery.
[0097] [Chemical formula 3]
[0098]
[0099] In chemical formula 3, R 13 and R 14 are the same or different and are selected from hydrogen, halogen, cyano (CN), nitro (NO2), and fluorinated C1 to C5 alkyl, provided that R 13 and R 14 At least one of is halogen, cyano (CN), nitro (NO2) and fluorinated C1 to C5 alkyl and R 13 and R 14 Not hydrogen at the same time.
[0100] Examples of the ethylene carbonate-based compound may be difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. The amount of the additive for improving the cycle life may be used within an appropriate range.
[0101] The lithium salt dissolved in the non-organic solvent supplies lithium ions in the battery, enables the basic operation of the lithium secondary battery, and improves the transport of lithium ions between the positive electrode and the negative electrode. Examples of lithium salts include those selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are natural numbers, for example, integers ranging from 1 to 20), at least one supporting salt of LiCl, LiI, and LiB(C2O4)2 (lithium bis(oxalato)borate; LiBOB). The lithium salt may be used in a concentration ranging from 0.1 M to 2.0 M. When the lithium salt is included in the above concentration range, the electrolyte may have excellent performance and lithium ion mobility due to optimal electrolyte conductivity and viscosity.
[0102] Another embodiment provides a lithium secondary battery including a positive electrode; a negative electrode; and the above-described electrolyte.
[0103] For example, the negative electrode may further include a SEI (solid electrolyte interface) layer on the surface, and the SEI layer may include a reaction product of the additive.
[0104] The SEI layer on the electrode surface of the lithium secondary battery according to the embodiment may have a thickness of 0.05nm to 100nm, for example, 0.1nm to 80nm, and specifically, 0.5nm to 50nm. When the SEI layer has a thickness in this range, the SEI layer may not adversely affect the transmission of lithium ions, and effectively prevents direct contact between the electrode and the electrolyte.
[0105] The SEI layer may not be a film formed by an additional process such as coating, but may be derived from some additives of the electrolyte.
[0106] For example, the SEI layer may be derived from a negative electrode film former, and the negative electrode film former may include, for example, at least one of vinylene carbonate (VC), vinylethylene carbonate (VEC), and fluoroethylene carbonate (FEC).
[0107] Specifically, the negative electrode film-forming agent may be used alone or together with a nitrile-based compound, a positive electrode passivation film-forming agent, and the nitrile-based compound may include at least one of succinonitrile, adiponitrile, and glutaronitrile.
[0108] More specifically, the negative electrode film-forming agent may be vinylene carbonate (VC) or vinylethylene carbonate (VEC) alone or a mixture of fluoroethylene carbonate (FEC) and a succinonitrile compound, but is not limited thereto.
[0109] The positive electrode includes a current collector and a positive active material layer disposed on the current collector and including a positive active material.
[0110] The positive active material may include a lithiated intercalation compound that reversibly intercalates and deintercalates lithium ions.
[0111] Specifically, at least one composite oxide of metals of cobalt, manganese, nickel, or a combination thereof and lithium may be used.
[0112] Examples of the positive electrode active material may include a compound represented by one of the following chemical formulas.
[0113] Li a A 1-b X b D2(0.90≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a E 1-b X b O 2-c D c (0.90≤a≤1.8, 0, 0≤b≤0.5, 0≤c≤0.05); Li a E 2-b X b O 4- c D c (0.90≤a≤1.8, 0, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b-c Co b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni 1-b-c Co b X c O2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);Li a Nor 1-b-c Mn b X c D α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05\0<α≤2);Li a Nor 1-b-c Mn b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05\0<α<2);Li a Nor 1-b-c Mn b X c O 2-α T2(0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05,0<α<2);Li a Nor b E c G d O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0.001≤d≤0.1);Li a Nor b Co c Mn d G e O2(0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0.001≤e≤0.1);Li a NiG b O2(0.90≤a≤1.8,0.001≤b≤0.1);Li a CoG b O2(0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 1-b G b O2(0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn2G b O4(0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 1-g G g PO4(0.90≤a≤1.8,0≤g≤0.5);QO2;QS2;LiQS2;V2O5;LiV2O5;LiZO2;LiVO4;Li (3-f)J2(PO4)3(0≤f≤2);Li (3-f) Fe2(PO4)3(0≤f≤2);Li a FePO4(0.90≤a≤1.8)
[0114] In the chemical formula, A is selected from Ni, Co, Mn and combinations thereof; X is selected from Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements and combinations thereof; D is selected from O, F, S, P and combinations thereof; E is selected from Co, Mn and combinations thereof; T is selected from F, S, P and combinations thereof; G is selected from Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V and combinations thereof; Q is selected from Ti, Mo, Mn and combinations thereof; Z is selected from Cr, V, Fe, Sc, Y and combinations thereof; and J is selected from V, Cr, Mn, Co, Ni, Cu and combinations thereof.
[0115] The compound may have a coating on the surface, or may be mixed with another compound having a coating. The coating may include at least one coating element compound selected from oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compound used for the coating may be amorphous or crystalline. The coating elements included in the coating may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. By using these elements in the compound, the coating can be set in a way that has no adverse effect on the performance of the positive active material. For example, the method may include any coating method (e.g., spraying, dipping, etc.). However, it is not described in more detail because it is well known to those skilled in the relevant art.
[0116] As a specific example of the positive electrode active material according to the embodiment of the present invention, LiNi 1-x- y Co x Mn y O2(0≤x≤0.5 and 0≤y≤0.5).
[0117] The positive active material may be included in an amount of 90 wt % to 98 wt % based on the total weight of the positive active material layer.
[0118] In an embodiment of the present invention, the positive active material layer may include a binder and a conductive material. Herein, the binder and the conductive material may be included in an amount of 1 wt % to 5 wt % respectively based on the total amount of the positive active material layer.
[0119] The binder improves the bonding properties between the positive electrode active material particles and the current collector. Examples thereof include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0120] A conductive material is included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes a chemical change, and examples of the conductive material may include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials of metal powder or metal fiber including copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0121] The current collector may use Al, but is not limited thereto.
[0122] The negative electrode includes a current collector and a negative active material layer formed on the current collector and including a negative active material.
[0123] The negative electrode active material may include a material that reversibly intercalates / deintercalates lithium ions, lithium metal, a lithium metal alloy, a material capable of doping / dedoping lithium, or a transition metal oxide.
[0124] The material for reversibly inserting / deinserting lithium ions may include a carbon material, which may be any commonly used carbon-based negative electrode active material in a lithium ion secondary battery, and examples thereof may be crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon may be non-shaped, or flaky, flake-shaped, spherical or fibrous natural graphite or artificial graphite, and the amorphous carbon may be soft carbon, hard carbon, a mesophase pitch carbonization product, fired coke, etc.
[0125] Lithium metal alloys include alloys of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.
[0126] The materials that can be doped / dedoped with lithium can be Si, Si-C composite materials, SiO x(0 < x < 2), Si-Q alloy (where Q is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, but not Si), Sn, SnO2, Sn-R (where R is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, but not Sn), etc., and at least one of these materials can be mixed with SiO2. Elements Q and R can be selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof.
[0127] The transition metal oxide can be vanadium oxide, lithium vanadium oxide, or lithium titanium oxide.
[0128] In the negative electrode active material layer, based on the total weight of the negative electrode active material layer, the negative electrode active material can be included in an amount of 95 wt% to 99 wt%.
[0129] In an embodiment of the present invention, the negative electrode active material layer includes a binder and an optional conductive material. In the negative electrode active material layer, based on the total weight of the negative electrode active material layer, the content of the binder can be 1 wt% to 5 wt%. When the negative electrode active material layer includes a conductive material, the negative electrode active material layer includes approximately 90 wt% to approximately 98 wt% of the negative electrode active material, 1 wt% to 5 wt% of the binder, and 1 wt% to 5 wt% of the conductive material.
[0130] The binder improves the binding properties between the negative electrode active material particles and between the particles and the current collector. The binder includes a water-insoluble binder, a water-soluble binder, or a combination thereof.
[0131] The water-insoluble binder can be selected from polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.
[0132] The water-soluble adhesive can be a rubber-based adhesive or a polymer resin adhesive. The rubber-based adhesive can be selected from styrene-butadiene rubber, acrylated styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber and combinations thereof. The polymer resin adhesive can be selected from polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene copolymer, polyethylene oxide, polyvinyl pyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polystyrene, ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol and combinations thereof.
[0133] When a water-soluble binder is used as a negative electrode binder, a cellulose compound may be further used as a thickener to provide viscosity. The cellulose compound includes carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or one or more of their alkali metal salts. The alkali metal may be Na, K or Li. Such a thickener may be included in an amount of 0.1 to 3 parts by weight based on 100 parts by weight of the negative electrode active material.
[0134] A conductive material is included to provide electrode conductivity, and any electrically conductive material can be used as the conductive material unless it causes a chemical change, and examples of the conductive material include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.; metal-based materials of metal powder or metal fiber include copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0135] The current collector may include one selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.
[0136] Depending on the type of lithium secondary battery, the lithium secondary battery may further include a separator between the negative electrode and the positive electrode. Examples of suitable separator materials include polyethylene, polypropylene, polyvinylidene fluoride and multilayers thereof, such as polyethylene / polypropylene double-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, and polypropylene / polyethylene / polypropylene three-layer separators.
[0137] refer to Figure 1 According to an embodiment, a lithium secondary battery 100 includes a battery cell, which includes a negative electrode 112, a positive electrode 114 facing the negative electrode 112, a separator 113 inserted between the negative electrode 112 and the positive electrode 114, and an electrolyte (not shown) of the lithium secondary battery for impregnating the negative electrode 112, the positive electrode 114 and the separator 113, a battery case 120 accommodating the battery cell, and a sealing member 140 sealing the battery case 120. DETAILED DESCRIPTION
[0138] Hereinafter, examples of the present invention and comparative examples are described. However, these examples should not be interpreted as limiting the scope of the present invention in any sense.
[0139] Manufacturing of lithium secondary battery cells
[0140] Preparation Example 1: Synthesis of Compound 1-1
[0141] [Compound 1-1]
[0142]
[0143] Under cooling conditions, trimethylsilyl sulfonyl chloride (38.47.53g, 0.204mol) was added dropwise to 1,4-divinyl-1,1,4,4,-tetramethyl-1,4-disilabutane (19.94g, 0.101mol) for 2 hours. Subsequently, the reaction mixture was maintained at room temperature (20°C) for 15 hours. Then, the reaction mixture was heated to 110°C and maintained at the same temperature for 5 hours, and at the same time, the reaction product was distilled to remove trimethylsilyl chloride produced as a by-product. The resulting product was cooled to room temperature, and then, the remaining reaction product was distilled under vacuum by a short Vigreux column.
[0144] The obtained product was redistilled at a fractionation temperature of 184°C to 188°C / 0.05 Torr to obtain the product as a colorless oil (21.78 g, 60.4%). The corresponding material is very sensitive to moisture.
[0145] 1H NMR (400MHz, CDCl3), δ0.40 (s, 12H), 0.82 (s, 4H), 5.97 (d, 2H), 6.32 (d, 2H), 6.62 (dd, 2H).
[0146] 13C NMR (100MHz, CDCl3), δ-1.74(s), 7.59(s), 127.23(s), 135.24(s).
[0147] 29Si NMR (80MHz, CDCl3), δ33.62(s).
[0148] Preparation Example 2: Synthesis of Compound 1-2
[0149] [Compound 1-2]
[0150]
[0151] A mixture of 1,2-bis(chlorodimethylsilyl)ethane (21.53 g, 0.1 mol) and methanesulfonic acid (19.22 g, 0.2 mol) was heated to 65 ° C for 30 minutes and maintained at the same temperature for about 1 hour until the reaction with HCl was completed. Subsequently, the temperature of the reaction mixture was raised to 120 ° C and then maintained for 24 hours. The product was cooled to room temperature and distilled under vacuum by Vigreux column distillation. In this article, the distillation condenser was kept warm to prevent clogging the column due to recrystallization of the product therein. The product was processed by split flow at 162 ° C to 164 ° C / 0.05 to obtain a colorless oily product (23.19 g, 69.3%).
[0152] 1H NMR (400MHz, CDCl3), δ0.33 (s, 12H), 0.75 (s, 4H), 2.93 (s, 6H).
[0153] 13C NMR (100MHz, CDCl3), δ-1.83(s), 7.45(s), 40.08(s).
[0154] 29Si NMR (80MHz, CDCl3), δ32.39(s)
[0155] Preparation Example 3: Synthesis of Compound 1-3
[0156] [Compound 1-3]
[0157]
[0158] Compound 1-3 (22.14 g, 67.03%) was obtained as a colorless oily product according to the same method as in Preparation Example 2, except that ethanesulfonic acid (22.03 g, 0.2 mol) was used instead of methanesulfonic acid in Preparation Example 2.
[0159] 1H NMR (400MHz, CDCl3), δ0.55 (S, 12H), 1.27 (t, 4H), 2.72 (s, 6H)
[0160] 13C NMR (100MHz, CDCl3), δ1.30(s), 10.3(s), 41.1(s)
[0161] 29Si NMR (80MHz, CDCl3), δ34.50(s)
[0162] Comparative Preparation Example 1: Synthesis of Compound 2a
[0163] [Compound 2a]
[0164]
[0165] Compound 2a (10.54 g, 64.21%) was obtained according to the same method as in Preparation Example 1-1, except that trimethylsilyl chloride (10.01 g, 0.1 mol) and ethanesulfonic acid (10.86 g, 0.1 mol) were used.
[0166] Example 1
[0167] LiNi as the positive electrode active material 1 / 3 Co 1 / 3 Mn 1 / 3 O2, polyvinylidene fluoride as a binder, and Ketjen black as a conductive material were mixed in a weight ratio of 90:5:5, and then dispersed in N-methylpyrrolidone to prepare a positive electrode active material slurry.
[0168] The positive electrode active material slurry was coated on a 15 μm thick Al foil, dried at 100° C., and pressed to produce a positive electrode.
[0169] Graphite as a negative electrode active material, polyvinylidene fluoride as a binder, and Ketjen black as a conductive material were mixed at a weight ratio of 90:5:5, and then dispersed in N-methylpyrrolidone to prepare a negative electrode active material slurry.
[0170] The negative electrode active material slurry was coated on a 10 μm thick Cu foil, dried at 100° C., and pressed to produce a negative electrode.
[0171] Positive and negative electrodes, a 25 μm thick polyethylene separator, and an electrolyte were used to fabricate a lithium secondary battery cell.
[0172] The electrolyte had the following composition.
[0173] (Electrolyte composition)
[0174] Salt: LiPF6 1.15M
[0175] Solvent: Ethylene carbonate / ethyl methyl carbonate / dimethyl carbonate (EC:EMC:DMC=1:1:1 volume ratio)
[0176] Additives: 0.5wt% of compound 1-1 / 2wt% of vinylene carbonate
[0177] (Herein, in the electrolyte composition, "wt%" is based on the total amount of the electrolyte (lithium salt + non-aqueous organic solvent + additives))
[0178] Examples 2 to 4, Reference Examples and Comparative Examples 1 and 2
[0179] A lithium secondary battery cell was manufactured according to the same method as in Example 1, except that the additive composition was changed as shown in Table 1.
[0180] [Table 1]
[0181]
[0182]
[0183] Battery characteristics evaluation
[0184] Evaluation 1: Measuring initial impedance and impedance spectrum after storage at high temperature (60°C)
[0185] The circular full battery cells according to Examples 1 to 4 and Comparative Examples 1 and 2 were measured for initial impedance spectra at room temperature (25° C.) and impedance spectra after being placed in an oven at a high temperature of 60° C. for 2 weeks, and the results are shown in Figure 2 and Figure 3 And in Table 2 and Table 3. Impedance spectrum detected by electrochemical impedance spectroscopy (EIS) was used to measure impedance. The impedance meter used herein was VMP3B-10 manufactured by BioLogic Science Instruments.
[0186] Initial impedance measurements of a circular full cell are shown in Figure 2 and Table 2.
[0187] Figure 2 Nyquist plot showing the initial impedance analysis results of a lithium secondary battery cell.
[0188] [Table 2]
[0189] Rs Comparative Example 1 0.81 Example 1 0.63 Comparative Example 2 0.70
[0190] In Table 2, R S Indicates the solution resistance (bulk resistance).
[0191] refer to Figure 2 and Table 2, the initial resistance of Example 1 including the novel additive of the present invention and VC is reduced compared to Comparative Example 1 including only VC and Comparative Example 2 including additives different from the novel additive together with VC.
[0192] In addition, the impedance measurement results of the circular full battery cell after being placed at 60°C are shown in Figure 3 and Table 3.
[0193] Figure 3 Nyquist plots showing impedance analysis results of the lithium secondary battery cells according to Examples 1 to 4 and Comparative Examples 1 and 2 after being left at high temperature (2 weeks).
[0194] [Table 3]
[0195]
[0196]
[0197] In Table 3, R S Represents solution resistance (body resistance), R CT+SEI represents the interface resistance, and R 总 Represents the overall resistance.
[0198] refer to Figure 3 As shown in Table 3, when the additives of the present invention (new additives and VC) are included, when placed at high temperature, the initial resistance or interface resistance is reduced, so the overall resistance is reduced, and as a result, the resistance increase rate thereof is greatly reduced. Therefore, the output characteristics of the lithium secondary battery cell are expected to be improved.
[0199] Evaluation 2: Evaluation of cycle life characteristics
[0200] The lithium secondary battery cells according to Examples 1 to 4, Reference Example and Comparative Examples 1 and 2 were charged for 10 minutes at room temperature (25° C.) under the conditions of CC-CV 4A, 4.2V and 100mA cutoff value, and discharged for 30 minutes under the conditions of CC 10A and 2.8V cutoff value as one cycle, and their capacity retention rates after 100 cycles were evaluated, as shown in FIG. Figure 4 show.
[0201] Figure 4 It is a graph showing the discharge capacity retention rate at 25° C. according to the cycle of the lithium secondary battery cell.
[0202] refer to Figure 4 , the capacity retention rates of Examples 1 to 4 according to the present invention were not deteriorated but maintained to a certain extent.
[0203] Therefore, as described above, the lithium secondary battery cell including the compound represented by Chemical Formula 1 and the negative electrode film-forming agent as an additive at the same time exhibits excellent cycle-life characteristics and certain high-temperature stability.
[0204] Assessment 3: Measurement of gas evolution after storage at high temperature
[0205] After the circular battery cells according to Examples 1 to 4, Reference Example and Comparative Examples 1 and 2 were stored at 60° C. for 2 weeks, the amount of internally generated gas was measured by punching holes in the bottom of the battery using a gas collecting jig and connecting it with a gas chromatograph (GC) without external leakage of the generated gas.
[0206] These gas volume measurements are shown in Figure 5 middle.
[0207] Figure 5 The measurement results of the amount of gas generated by the lithium secondary battery cells according to Examples 1 to 4, Reference Example, Comparative Examples 1 and 2 after being stored at high temperature for 2 weeks are shown.
[0208] like Figure 5 It is shown in Figure 1 that the amount of generated gas of the lithium secondary battery including the additive composition of the present invention according to Examples 1 to 4 is greatly reduced compared to the comparative example and the reference example not including some additive compositions of the present invention.
[0209] Therefore, the electrolyte according to the embodiment has a specific composition, thereby improving the stability of the lithium secondary battery cell.
[0210] While the invention has been described in connection with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but on the contrary is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.
Claims
1. An electrolyte for a lithium secondary battery, the electrolyte comprising: Non-aqueous organic solvents, lithium salts and additives, The additive comprises a compound represented by Chemical Formula 1 and a negative electrode film-forming agent: [Chemical formula 1] Wherein, in Chemical Formula 1, R 1 To R 6 are independently substituted or unsubstituted C1 to C10 alkyl or substituted or unsubstituted C2 to C10 alkenyl, and n is an integer of 1 to 10.
2. The electrolyte for a lithium secondary battery according to claim 1, wherein the compound represented by Chemical Formula 1 is represented by Chemical Formula 1A: [Chemical Formula 1A] in, In Chemical Formula 1A, R 1 and R 2 are independently substituted or unsubstituted C1 to C10 alkyl or substituted or unsubstituted C2 to C10 alkenyl, and n is an integer of 1 to 10.
3. The electrolyte for lithium secondary battery according to claim 2, wherein R 1 and R 2 are independently substituted or unsubstituted C1 to C4 alkyl, or substituted or unsubstituted C2 to C4 alkenyl.
4. The electrolyte for lithium secondary battery according to claim 2, wherein R 1 and R 2 They are independently C1 to C4 alkyl which may be substituted by halogen or cyano, or C2 to C4 alkenyl which may be substituted by halogen or cyano.
5. The electrolyte for a lithium secondary battery according to claim 1, wherein R 1 and R 2 are independently unsubstituted methyl, unsubstituted ethyl or unsubstituted vinyl, and R 3 To R 6 are independently substituted or unsubstituted C1 to C5 alkyl. 6 . The electrolyte for a lithium secondary battery according to claim 1 , wherein the negative electrode film-forming agent comprises at least one of vinylene carbonate (VC), vinylethylene carbonate (VEC), and fluoroethylene carbonate (FEC).
7. The electrolyte for a lithium secondary battery according to claim 1, wherein The compound represented by Chemical Formula 1 is included in an amount of 0.05 wt % to 5 wt % based on the total amount of the electrolyte for a lithium secondary battery, and The negative electrode film-forming agent is included in an amount of about 0.05 wt % to about 20 wt % based on the total amount of the electrolyte for the lithium secondary battery.
8. The electrolyte for a lithium secondary battery according to claim 1, wherein The compound represented by Chemical Formula 1 is included in an amount of 0.1 wt % to 2 wt % based on the total amount of the electrolyte for a lithium secondary battery, and The negative electrode film-forming agent is included in an amount of about 0.5 wt % to about 5 wt % based on the total amount of the electrolyte for the lithium secondary battery. 9 . The electrolyte for a lithium secondary battery according to claim 1 , wherein the additive further comprises a nitrile-based compound. 10 . The electrolyte for a lithium secondary battery according to claim 9 , wherein the nitrile-based compound comprises at least one of succinonitrile, adiponitrile, and glutaronitrile. 11 . The electrolyte for a lithium secondary battery according to claim 9 , wherein the nitrile-based compound is included in an amount of 0.2 wt % to 5 wt % based on the total amount of the electrolyte for the lithium secondary battery.
12. A lithium secondary battery, comprising: Positive electrode; Negative electrode; and The electrolyte according to any one of claims 1 to 11.
13. The lithium secondary battery according to claim 12, further comprising an SEI (solid electrolyte interface) layer on the surface of the negative electrode, and The SEI layer includes a reaction product of the additive.