Precipitated χ iron carbide composition, preparation method, catalyst and application thereof, and Fischer-Tropsch synthesis method
By preparing a composition containing precipitated χ iron carbide, the problems of high by-product selectivity and impurities in the Fischer-Tropsch synthesis of iron-based catalysts are solved, the preparation of high-purity catalysts and the improvement of reaction stability are achieved, and it is suitable for use under high temperature and high pressure conditions. Fischer-Tropsch synthesis.
Patent Information
- Application Number
- CN202011064107.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing iron-based catalysts have high selectivity for CO2 and CH4 by-products in Fischer-Tropsch synthesis reactions, and it is impossible to obtain pure phase iron carbide without Fe impurities, which affects reaction stability and efficiency.
A composition containing precipitated χ iron carbide is used, which contains 95-100 mol% of precipitated χ iron carbide and 0-5 mol% of Fe-containing impurities, and is prepared by co-precipitation, reduction, surface passivation and carbonization treatment. A high-purity χ iron carbide catalyst is prepared, and the Fischer-Tropsch synthesis reaction is performed under high temperature and high pressure conditions.
A high-purity χ iron carbide catalyst is achieved, which reduces the selectivity of CO2 and CH4, improves reaction stability and effective product selectivity, is suitable for high-temperature and high-pressure continuous reactors, and maintains reaction stability for more than 400 hours.
Smart Images

Figure CN112569992B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of Fischer-Tropsch synthesis reaction, in particular to a precipitated chi iron carbide composition and a preparation method, a catalyst and application thereof, and a Fischer-Tropsch synthesis method. Background Art
[0002] The characteristics of my country's primary energy structure are rich in coal, lack of oil and little gas. With the development of my country's economy, the dependence on foreign oil has continued to rise.
[0003] Fischer-Tropsch synthesis is an increasingly important energy conversion pathway in recent years, which can convert synthesis gas of carbon monoxide and H2 into liquid fuels and chemicals.
[0004] The reaction equation of Fischer-Tropsch synthesis is as follows:
[0005] (2n+1)H2+nCO→C n H 2n+2 +nH2O (1),
[0006] 2nH2+nCO→C n H 2n +nH2O (2).
[0007] In addition to alkanes and olefins, industrial Fischer-Tropsch synthesis can also produce by-products carbon dioxide (CO2) and methane (CH4). The Fischer-Tropsch synthesis reaction mechanism is complex and has many steps, such as CO dissociation, carbon (C) hydrogenation, CH x Chain growth, as well as hydrogenation and dehydrogenation reactions leading to desorption of hydrocarbon products and removal of oxygen (O).
[0008] Iron is the cheapest transition metal used to make Fischer-Tropsch synthesis catalysts. Traditional iron-based catalysts have high water-gas shift (CO+H2O→CO2+H2) activity, so traditional iron-based catalysts usually have high byproduct CO2 selectivity, usually accounting for 25%-45% of the converted raw carbon monoxide. This has become one of the main disadvantages of iron-based catalysts for Fischer-Tropsch synthesis reactions.
[0009] The changes in the active phase of iron-based catalysts are very complex, which has led to considerable controversy on the nature of the active phase and the Fischer-Tropsch synthesis reaction mechanism of iron-based catalysts.
[0010] CN104399501A discloses a method for preparing nanoparticles of ε-Fe2C suitable for low-temperature Fischer-Tropsch synthesis reaction. The initial precursor is skeleton iron, and the reaction system is an intermittent non-continuous reaction of polyethylene glycol solvent. The CO2 selectivity of this catalyst is 18.9%, and the CH4 selectivity is 17.3%. Its disadvantage is that it can only be applied to low temperatures below 200°C, and the reaction cannot be completed continuously. This means that this catalyst is not suitable for continuous production under modern Fischer-Tropsch synthesis industrial conditions. However, since skeleton iron cannot be completely carbonized at low temperatures, the ε-Fe2C nanoparticles recorded in the document contain a considerable amount of non-carburized iron-type iron impurity components. In fact, the prior art cannot obtain a carburized ultra-pure phase material without iron impurities. The Fe impurities here refer to various Fe (element)-containing phase components of non-carburized iron.
[0011] Therefore, the iron-based catalyst used in the Fischer-Tropsch synthesis reaction needs to be improved. Summary of the invention
[0012] The purpose of the present invention is to solve the problem of how to obtain a pure phase iron carbide material without Fe impurities from an iron-based catalyst, improve the stability of the Fischer-Tropsch synthesis reaction, and reduce the problem of excessive selectivity of CO2 or CH4 by-products. A precipitated χ-iron carbide composition and its preparation method, catalyst and application, and a Fischer-Tropsch synthesis method are provided.
[0013] In order to achieve the above-mentioned object, the first aspect of the present invention provides a precipitated χ iron carbide composition, which comprises 95-100 mol% of precipitated χ iron carbide and 0-5 mol% of Fe-containing impurities, wherein the Fe-containing impurities are iron-containing substances other than χ iron carbide; wherein the specific surface area of the composition is 20-280 m 2 / g.
[0014] A second aspect of the present invention provides a method for preparing a composition containing precipitated x-iron carbide, comprising:
[0015] (1) mixing an aqueous solution containing an iron salt with an alkaline precipitant for co-precipitation, washing and separating the obtained precipitate, and then drying and calcining the obtained solid to obtain a precursor;
[0016] (2) reducing the precursor with H2 at a temperature of 450-610°C;
[0017] (3) subjecting the material obtained in step (2) to surface passivation treatment with an O2-containing gas at a temperature of 0-50° C., wherein the volume concentration of O2 in the O2-containing gas is 1-5%;
[0018] (4) preparing carbides by reacting the material obtained in step (3) with H2 and CO at a temperature of 260-430° C., wherein the molar ratio of H2 to CO is 7-110:1, to obtain precipitated χ iron carbide;
[0019] (5) mixing 95-100 mole parts of precipitated x-iron carbide and 0-58 mole parts of Fe-containing impurities under the protection of an inert gas;
[0020] Wherein, the Fe-containing impurities are iron-containing substances other than x-iron carbide.
[0021] The third aspect of the present invention provides a precipitated x-iron carbide composition obtained by the method provided by the present invention.
[0022] The fourth aspect of the present invention provides a catalyst comprising the precipitated x-iron carbide composition provided by the present invention.
[0023] A fifth aspect of the present invention provides an application of the precipitated x-iron carbide composition or catalyst provided by the present invention in a Fischer-Tropsch synthesis reaction.
[0024] In a sixth aspect, the present invention provides an application of a precipitated x-iron carbide composition or catalyst of the present invention in the synthesis of C, H fuels and / or chemicals based on the Fischer-Tropsch synthesis principle.
[0025] A seventh aspect of the present invention provides a method for Fischer-Tropsch synthesis, comprising: under Fischer-Tropsch synthesis reaction conditions, contacting synthesis gas with the precipitated x-iron carbide composition or catalyst provided by the present invention.
[0026] An eighth aspect of the present invention provides a method for Fischer-Tropsch synthesis, comprising: under Fischer-Tropsch synthesis reaction conditions, contacting synthesis gas with a Fischer-Tropsch catalyst, wherein the Fischer-Tropsch catalyst comprises a Mn component and a precipitated x-iron carbide composition provided by the present invention.
[0027] Through the above technical solution, the present invention has the following technical effects:
[0028] (1) The required raw materials are easy to obtain and low in cost: the main raw material iron source of the synthetic precursor can be a commercially available iron salt. When synthesizing the active phase carbide, only the original reaction gas (carbon monoxide and hydrogen) of the Fischer-Tropsch synthesis reaction system can be used, without involving any inorganic or organic reaction raw materials, which is greatly simplified compared with the existing literature technology;
[0029] (2) The operation steps are simple. In a preferred embodiment, the entire process of preparing precipitated x-iron carbide only requires three steps: precursor reduction, surface passivation treatment, and carbide preparation. The preparation of the active phase can be achieved in situ in the same reactor.
[0030] (3) The present invention can prepare 100% pure precipitated x-iron carbide through the steps included in the method, which can be combined with Fe-containing impurities to form a composite, and further combined with an auxiliary agent to form a catalyst. The 100% pure precipitated χ iron carbide or composition or catalyst can be used in a high-temperature and high-pressure (for example, a temperature of 235-250°C and a pressure of 2.3-2.5MPa) continuous reactor, has extremely high reaction stability, and breaks the theoretical and technical barrier of traditional literature theory that "pure phase χ iron carbide cannot exist stably under reaction conditions", and can achieve a stable temperature of up to 320°C, and extremely low CO2 selectivity: under industrial Fischer-Tropsch synthesis reaction conditions, a high-pressure continuous reactor can be used to maintain continuous and stable reaction for more than 400 hours, and its CO2 selectivity is below 12% (preferably, it can reach below 8%); at the same time, its by-product CH4 selectivity is also maintained at 12% (preferably, it can reach below 8%), and the effective product selectivity can reach above 73% (preferably, it can reach above 85%), which is very suitable for use in modern coal chemical Fischer-Tropsch synthesis large-scale industry to efficiently output oil wax products. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is an in-situ XRD spectrum of the process of preparing precipitated x-iron carbide in Example 1 provided in the present invention; wherein, A-before reduction of the precursor, B-after reduction of the precursor, C-after surface passivation treatment, and D-iron carbide preparation is completed. DETAILED DESCRIPTION
[0032] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0033] The first aspect of the present invention provides a precipitated x-iron carbide composition, wherein the composition comprises 95-100 mol% of precipitated x-iron carbide and 0-5 mol% of Fe-containing impurities, wherein the Fe-containing impurities are iron-containing substances other than x-iron carbide; wherein the specific surface area of the composition is 20-280 m 2 / g.
[0034] The present invention provides a composition containing precipitated x-iron carbide, wherein the precipitated x-iron carbide is x-iron carbide with a purity of 100%. Further, the precipitated x-iron carbide can form a composition with other Fe-containing impurities. Under the above-mentioned content limit, the composition containing precipitated x-iron carbide provided by the present invention can be applied to a Fischer-Tropsch synthesis catalyst, used alone or with other components, and can improve the stability of the Fischer-Tropsch synthesis catalyst in the Fischer-Tropsch synthesis reaction, and significantly reduce the selectivity of CO2 or CH4 by-products.
[0035] In some embodiments of the present invention, the composition contains high-purity precipitated x-iron carbide, and XRD and Mössbauer spectroscopy analysis can be performed, and the crystal phase can be observed to be pure x-iron carbide in the obtained XRD spectrum and Mössbauer spectroscopy results. Preferably, the specific surface area of the composition is 27-210 m 2 / g. The specific surface area can be measured by the BET adsorption-desorption method of N2. The composition comprises monoclinic x-iron carbide.
[0036] In some embodiments of the present invention, it is further preferred that, based on the total amount of the composition, the composition comprises 97-100 mol% of precipitated x-iron carbide and 0-3 mol% of Fe-containing impurities, which can be determined by XRD and Mössbauer spectroscopy analysis, or by the amount of materials used in the preparation of the composition.
[0037] In some embodiments of the present invention, the Fe-containing impurities are at least one of iron carbide, iron, iron oxide, iron hydroxide, iron sulfide, and iron salt other than x-iron carbide. The Fe-containing impurities can be introduced by solution impregnation, sputtering, atomic deposition, or mixing.
[0038] The second aspect of the present invention provides a method for preparing a composition containing precipitated x-iron carbide, comprising:
[0039] (1) mixing an aqueous solution containing an iron salt with an alkaline precipitant for co-precipitation, washing and separating the obtained precipitate, and then drying and calcining the obtained solid to obtain a precursor;
[0040] (2) reducing the precursor with H2 at a temperature of 450-610°C;
[0041] (3) subjecting the material obtained in step (2) to surface passivation treatment with an O2-containing gas at a temperature of 0-50° C., wherein the volume concentration of O2 in the O2-containing gas is 1-5%;
[0042] (4) preparing carbides by reacting the material obtained in step (3) with H2 and CO at a temperature of 260-430° C., wherein the molar ratio of H2 to CO is 7-110:1, to obtain precipitated χ iron carbide;
[0043] (5) mixing 95-100 mol parts of precipitated x-iron carbide and 0-5 mol parts of Fe-containing impurities under the protection of an inert gas;
[0044] Wherein, the Fe-containing impurities are iron-containing substances other than x-iron carbide.
[0045] In some embodiments of the present invention, the iron salt can be a water-soluble iron salt commonly used in the art, selected from water-soluble iron salts, and can be a commercially available product. For example, the iron salt is at least one of ferric nitrate, ferric chloride, ferrous ammonium sulfate and ferric ammonium citrate.
[0046] In some embodiments of the present invention, the alkaline precipitant can be a conventional choice in the art, for example, the alkaline precipitant is at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, sodium hydroxide, potassium hydroxide and ammonia water.
[0047] In a preferred embodiment of the present invention, the drying and calcining process comprises: first drying the solid at a temperature of 35-80°C and a vacuum degree of 250-1200Pa for 6-10 hours; drying the dried material at 75-180°C for 3-24 hours, and then calcining the obtained material at a temperature of 250-580°C for 1-10 hours. The drying process can be carried out in an oven, and the calcining process can be carried out in a muffle furnace.
[0048] In some embodiments of the present invention, step (2) can simultaneously generate nano iron powder from the iron element in the precursor in situ and reduce the generated nano iron powder.
[0049] In some embodiments of the present invention, the H2 in step (2) can be introduced into the reaction system in the form of an H2 flow. At the same time, the pressure of the precursor reduction is controlled by controlling the pressure of the H2 flow. Preferably, in step (2), the pressure of the precursor reduction is 0.1-15atm, preferably 0.3-2.6atm, and the time is 0.7-15h, preferably 1-12h.
[0050] In some embodiments of the present invention, the amount of H2 can be selected according to the amount of the precursor to be treated. Preferably, in step (2), the gas flow rate of H2 is 600-25000 mL / h / g, more preferably 2800-22000 mL / h / g.
[0051] In step (3) of the method provided by the present invention, the O2-containing gas is a mixture of O2 and an inert gas. The inert gas may be at least one of nitrogen, helium, argon, krypton and xenon. The O2-containing gas is introduced to participate in the surface passivation treatment process; at the same time, the pressure of the surface passivation treatment is controlled by controlling the pressure of the O2-containing gas. Preferably, in step (3), the pressure of the surface passivation treatment is 0-1.6 atm, preferably 0-0.09 atm, and the time is 5-72 h, preferably 10-56 h.
[0052] In some embodiments of the present invention, preferably, in step (3), the gas flow rate of the O2-containing gas is 400-12000 mL / h / g, more preferably 1400-8500 mL / h / g.
[0053] In step (4) of the method provided by the present invention, conditions for achieving the preparation of the carbide are provided to obtain precipitated x iron carbide. H2 and CO can be introduced into the process of preparing the carbide in the form of a mixed gas flow of (H2+CO); at the same time, the pressure of the carbide preparation process is controlled by controlling the pressure of the mixed gas flow of (H2+CO). Preferably, in step (4), the pressure of the carbide preparation is 0.08-12atm, preferably 0.15-2.5atm, and the time is 0.3-30h, preferably 0.5-2.4h.
[0054] In some embodiments of the present invention, preferably, in step (4), the total gas flow rate of H2 and CO is 250-21000 mL / h / g, more preferably 2000-18000 mL / h / g.
[0055] In a preferred embodiment of the present invention, the carbide preparation further comprises: performing a heating operation simultaneously in step (4), heating from the temperature of the surface passivation treatment to 250-430°C at a heating rate of 0.2-5°C / min. In this preferred embodiment, the precipitated χ iron carbide obtained can specifically have better effective product selectivity in the Fischer-Tropsch synthesis reaction. Further preferably, the temperature is heated from the temperature of the surface passivation treatment to 260-400°C at a heating rate of 0.2-2.5°C / min. In the heating operation, the temperature of the surface passivation treatment refers to the temperature of 0-50°C in step (3). That is, the heating operation is: heating from 0-50°C at a heating rate of 0.2-5°C / min to the temperature of 250-430°C in step (4), preferably from 0-50°C at a heating rate of 0.2-2.5°C / min to 260-400°C.
[0056] In the present invention, unless otherwise specified, in the process of preparing iron carbide, "mL / h / g" refers to the intake volume per gram of material per hour.
[0057] In another preferred embodiment of the present invention, the processes of precursor reduction, surface passivation treatment and carbide preparation can be performed continuously in the same reactor. During the preparation process, in-situ characterization equipment can be used to track the crystal phase transformation of the material.
[0058] In the present invention, through the process of steps (1) to (4), it is possible to obtain precipitated x-iron carbide, which can be determined by XRD and / or Mössbauer spectroscopy analysis.
[0059] In some embodiments of the present invention, the Fe-containing impurities contained in the precipitated x-iron carbide composition may be mixed in by external addition. Preferably, in step (5), 97-100 molar parts of precipitated x-iron carbide are mixed with 0-3 molar parts of Fe-containing impurities.
[0060] In one embodiment of the present invention, in step (5), the mixing comprises mixing the precipitated x-iron carbide powder and the Fe impurity-containing powder in a glove box according to the required amount under inert gas protection conditions.
[0061] The third aspect of the present invention provides a precipitated x-iron carbide composition obtained by the method of the present invention. The composition comprises 95-100 mol% of precipitated x-iron carbide and 0-5 mol% of Fe-containing impurities, wherein the Fe-containing impurities are iron-containing substances other than x-iron carbide.
[0062] Preferably, the composition comprises 97-100 mol% of precipitated x-iron carbide and 0-3 mol% of Fe-containing impurities.
[0063] Preferably, the specific surface area of the composition is 20-280 m 2 / g, preferably 27-210m 2 / g.
[0064] The fourth aspect of the present invention provides a catalyst, comprising the precipitated x-iron carbide composition provided by the present invention. Preferably, the catalyst may also contain other components, such as an additive.
[0065] In the specific embodiment provided by the present invention, preferably, based on the total amount of the catalyst, the content of the precipitated x-iron carbide composition is greater than 75wt% and less than 100wt%, and the content of the auxiliary agent is greater than 0wt% and less than 25wt%.
[0066] In the specific embodiment provided by the present invention, preferably, the catalyst can be prepared by introducing the auxiliary agent through impregnation, atomic deposition, sputtering or chemical deposition.
[0067] A fifth aspect of the present invention provides an application of the precipitated x-iron carbide composition or catalyst provided by the present invention in a Fischer-Tropsch synthesis reaction.
[0068] In a sixth aspect, the present invention provides an application of a precipitated x-iron carbide composition or catalyst provided by the present invention in the synthesis of C, H fuels and / or chemicals based on the Fischer-Tropsch synthesis principle.
[0069] A seventh aspect of the present invention provides a method for Fischer-Tropsch synthesis, comprising: under Fischer-Tropsch synthesis reaction conditions, contacting synthesis gas with the precipitated x-iron carbide composition or catalyst provided by the present invention.
[0070] The Fischer-Tropsch synthesis reaction can be carried out by using the precipitated x-iron carbide composition or catalyst of the present invention, and the Fischer-Tropsch synthesis reaction can be carried out at high temperature and high pressure, for example, the conditions of the Fischer-Tropsch synthesis reaction include: temperature of 250-320°C and pressure of 1.5-2.5MPa. And better selectivity of effective products can be obtained; the effective products are carbon-containing products other than CH4 and CO2 produced by the reaction of CO and H2, including but not limited to hydrocarbons, alcohols, aldehydes, ketones, esters, etc. of C2 and above.
[0071] In the present invention, unless otherwise specified, the pressure refers to the gauge pressure.
[0072] In some embodiments of the present invention, preferably, the Fischer-Tropsch synthesis reaction is carried out in a high-temperature and high-pressure continuous reactor. The catalyst containing the precipitated x-iron carbide composition of the present invention can achieve a continuous and stable reaction of the Fischer-Tropsch synthesis reaction in a high-temperature and high-pressure continuous reactor for more than 400 hours.
[0073] An eighth aspect of the present invention provides a method for Fischer-Tropsch synthesis, comprising: under Fischer-Tropsch synthesis reaction conditions, contacting synthesis gas with a Fischer-Tropsch catalyst, wherein the Fischer-Tropsch catalyst comprises a Mn component and a precipitated x-iron carbide composition provided by the present invention.
[0074] In a specific embodiment provided by the present invention, the composition of the Fischer-Tropsch catalyst can be further based on the total amount of the Fischer-Tropsch catalyst, the content of the precipitated x-iron carbide composition is greater than 75wt% and less than 100wt%, and the content of Mn is greater than 0wt% and less than 25wt%. In the Fischer-Tropsch catalyst, Mn can exist in the form of oxides and can be introduced into the Fischer-Tropsch catalyst by methods including but not limited to impregnation, chemical deposition, sputtering, and atomic deposition.
[0075] The present invention will be described in detail below by way of examples. In the following examples and comparative examples,
[0076] In-situ XRD detection during the preparation of iron carbide uses an X-ray diffractometer (Rigaku, model D / max-2600 / PC) to monitor the crystal phase changes of the material;
[0077] The obtained iron carbide and iron carbide composite were analyzed by Mössbauer spectrometer (Transmission 57 Fe, 57 Co(Rh) source sinusoidal velocity spectrometer) for Mössbauer spectroscopy detection;
[0078] The BET specific surface area of the iron carbide composition was measured by nitrogen adsorption method;
[0079] During the Fischer-Tropsch synthesis reaction:
[0080] The products obtained by the reaction were analyzed by gas chromatography (Agilent 6890 gas chromatograph);
[0081] The reaction effect is calculated by the following formula:
[0082] CO2 selectivity % = [CO2 mole number in the discharge / (CO mole number in the feed - CO mole number in the discharge)] × 100%;
[0083] CH4 selectivity % = [mole number of CH4 in the discharge / (mole number of CO in the feed - mole number of CO in the discharge)] × 100%;
[0084] Effective product selectivity % = [1-CO2 selectivity %-CH4 selectivity %] × 100%;
[0085] Raw material CO space-time conversion rate (mmol / h / g- Fe ) = (CO mole number in feed - CO mole number in discharge) / reaction time / Fe element weight;
[0086] Space-time yield of effective product formation (mmol / h / g- Fe ) = number of carbon moles of C2 and C2 hydrocarbons produced / reaction time / weight of Fe element.
[0087] Example 1
[0088] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0089] (2) reducing the precursor with H2 at a pressure of 2.6 atm, a flow rate of H2 of 22000 mL / h / g, and a temperature of 610°C for 1 h;
[0090] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 5%, the pressure is 0.09 atm, the gas flow rate is 8500 mL / h / g, and the treatment time is 10 h;
[0091] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 2.5 atm, total gas flow rate 18000 mL / h / g, H2 to CO molar ratio 110:1, heating from 30°C to 400°C at a heating rate of 2.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 0.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 1;
[0092] (5) Under Ar gas protection, 97 mol parts of precipitated x-iron carbide 1 and 3 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 1.
[0093] Example 2
[0094] (1) 1.2 mol / L ferric nitrate and 0.7 mol / L sodium carbonate solution were mixed at 50°C and pH = 6.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 h and calcined at 400°C for 10 h to obtain a precursor.
[0095] (2) reducing the precursor with H2 at a pressure of 0.3 atm, a flow rate of H2 of 2800 mL / h / g, and a temperature of 350°C for 12 h;
[0096] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 1%, the pressure is 0.01 atm, the gas flow rate is 1400 mL / h / g, and the treatment time is 56 h;
[0097] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 0.15 atm, total gas flow rate 2000 mL / h / g, H2 to CO molar ratio 7:1, and then heating from 30°C to 260°C at a heating rate of 0.2°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 2.4 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 2;
[0098] (5) Under Ar gas protection, 99 mol parts of precipitated x-iron carbide 2 and 1 mol part of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 2.
[0099] Example 3
[0100] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 65°C and pH = 6.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0101] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 450°C for 6 h;
[0102] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0103] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 3;
[0104] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 3 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 3.
[0105] Example 4
[0106] (1)-(4) According to the method of Example 1, the difference is that "precursor and H2 at a pressure of 3 atm" is replaced by "precursor and H2 at a pressure of 2.6 atm", and precipitated iron carbide is obtained, which is determined by Mössbauer spectroscopy to be pure χ iron carbide, recorded as precipitated χ iron carbide 4.
[0107] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 4 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 4.
[0108] Example 5
[0109] (1)-(4) The method of Example 1 was followed, except that "precursor and H2 at a pressure of 0.08 atm" was used instead of "precursor and H2 at a pressure of 2.6 atm", to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and was recorded as precipitated χ iron carbide 5.
[0110] (5) Under Ar gas protection, 97 mol parts of precipitated x-iron carbide 5 and 3 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 5.
[0111] Example 6
[0112] (1) Mix 0.4 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution at 55°C and pH = 6.9 to obtain a precipitate slurry, wash with deionized water, filter to obtain a filter cake, dry at 110°C for 24 hours, and calcine at 500°C for 10 hours to obtain a precursor.
[0113] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 23000 mL / h / g, and a temperature of 500°C for 6 h;
[0114] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0115] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 6;
[0116] (5) Under Ar gas protection, 99 mol parts of precipitated x-iron carbide 6 and 1 mol part of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 6.
[0117] Example 7
[0118] (1) 1.1 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 75°C and pH = 6.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0119] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 500 mL / h / g, and a temperature of 500°C for 12 h;
[0120] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0121] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 7;
[0122] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 7 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 7.
[0123] Example 8
[0124] (1) 1.0 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 hours and calcined at 350°C for 6 hours to obtain a precursor.
[0125] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 13 h;
[0126] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0127] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 8;
[0128] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 8 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 8.
[0129] Example 9
[0130] (1) 1.4 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0131] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0132] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 9;
[0133] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 9 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 9.
[0134] Example 10
[0135] (1) 1.2 mol / L ferric nitrate and 0.5 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 105°C for 24 hours and calcined at 340°C for 9 hours to obtain a precursor.
[0136] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0137] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 10000 mL / h / g, and the treatment time is 12 h;
[0138] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 0.05 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 10;
[0139] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 10 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 10.
[0140] Embodiment 11
[0141] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 7.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0142] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0143] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 300 mL / h / g, and the treatment time is 24 h;
[0144] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 11;
[0145] (5) Under Ar gas protection, 97 mol parts of precipitated x-iron carbide 11 and 3 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 11.
[0146] Example 12
[0147] (1) 1.7 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 5.9 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0148] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0149] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 58 h;
[0150] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 12;
[0151] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 12 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 12.
[0152] Example 13
[0153] (1) 1.2 mol / L ferric nitrate and 0.3 mol / L sodium carbonate solution were mixed at 65°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 h and calcined at 400°C for 10 h to obtain a precursor.
[0154] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 450°C for 6 h;
[0155] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 4 h;
[0156] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 13;
[0157] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 13 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 13.
[0158] Embodiment 14
[0159] (1) 1.2 mol / L ferric nitrate and 0.6 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.3 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 90°C for 24 h and calcined at 340°C for 12 h to obtain a precursor.
[0160] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0161] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0162] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 3 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, recorded as precipitated iron carbide 14;
[0163] (5) Under Ar gas protection, 97 mol parts of precipitated x-iron carbide 14 and 3 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 14.
[0164] Embodiment 15
[0165] (1) Mix 0.6 mol / L ferric nitrate and 0.5 mol / L sodium carbonate solution at 45°C and pH=6.9 to obtain a precipitate slurry, wash with deionized water, filter to obtain a filter cake, dry at 110°C for 24 hours, and calcine at 380°C for 10 hours to obtain a precursor.
[0166] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0167] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.06 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0168] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 0.07 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 15;
[0169] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 15 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 15.
[0170] Example 16
[0171] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 h and calcined at 400°C for 10 h to obtain a precursor.
[0172] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0173] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0174] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 4 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 16;
[0175] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 16 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 16.
[0176] Embodiment 17
[0177] (1) 0.8 mol / L ferric nitrate and 0.5 mol / L sodium carbonate solution were mixed at 65°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 h and calcined at 320°C for 10 h to obtain a precursor.
[0178] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0179] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0180] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 0.2 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 17;
[0181] (5) Under Ar gas protection, 97 mol parts of precipitated x-iron carbide 17 and 3 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 17.
[0182] Embodiment 18
[0183] (1) 1.1 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 h and calcined at 500°C for 10 h to obtain a precursor.
[0184] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0185] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0186] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 19000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 18;
[0187] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 18 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 18.
[0188] Embodiment 19
[0189] (1) 1.0 mol / L ferric nitrate and 0.7 mol / L sodium carbonate solution were mixed at 55° C. and pH=6.1 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130° C. for 24 h and calcined at 410° C. for 10 h to obtain a precursor.
[0190] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0191] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0192] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 200 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 19;
[0193] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 19 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 19.
[0194] Embodiment 20
[0195] (1) 1.8 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.5 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 110°C for 24 h and calcined at 270°C for 10 h to obtain a precursor.
[0196] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0197] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 2%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0198] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 3°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 20;
[0199] (5) Under the protection of Ar gas, 98 mol parts of precipitated x-iron carbide 20 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) are mixed. The mixed mixture is recorded as iron carbide composition 20.
[0200] Embodiment 21
[0201] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L ammonium carbonate solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 h and calcined at 400°C for 10 h to obtain a precursor.
[0202] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0203] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 2%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0204] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 0.1°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 0.2 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 21;
[0205] (5) Under Ar gas protection, 97 mol parts of precipitated x-iron carbide 21 and 3 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 21.
[0206] Embodiment 22
[0207] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L ammonium bicarbonate solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0208] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0209] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0210] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 410°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 22;
[0211] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 22 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) are mixed. The mixed mixture is recorded as iron carbide composition 22.
[0212] Embodiment 23
[0213] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L sodium bicarbonate solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0214] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0215] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0216] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 240°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 23;
[0217] (5) Under Ar gas protection, 98 mol parts of precipitated x-iron carbide 23 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 23.
[0218] Embodiment 24
[0219] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L sodium hydroxide solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 h and calcined at 400°C for 10 h to obtain a precursor.
[0220] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0221] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.12 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0222] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, which was determined to be pure χ iron carbide by Mössbauer spectroscopy and recorded as precipitated χ iron carbide 24;
[0223] (5) Under Ar gas protection, 97 mol parts of precipitated x-iron carbide 24 and 3 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition 24.
[0224] Comparative Example 1
[0225] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L potassium hydroxide solution were mixed at 55° C. and pH=6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130° C. for 24 h and calcined at 400° C. for 10 h to obtain a precursor.
[0226] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 620°C for 6 h;
[0227] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0228] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, recorded as iron carbide D1;
[0229] (5) Under the protection of Ar gas, 98 mol parts of iron carbide D1 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition D1.
[0230] Comparative Example 2
[0231] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L ammonia solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 h and calcined at 400°C for 10 h to obtain a precursor.
[0232] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0233] (3) cooling the product obtained in step (2) to 60° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0234] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 60°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, recorded as iron carbide D2;
[0235] (5) Under the protection of Ar gas, 98 mol parts of iron carbide D2 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition D2.
[0236] Comparative Example 3
[0237] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L sodium carbonate solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 h and calcined at 400°C for 10 h to obtain a precursor.
[0238] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 500°C for 6 h;
[0239] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 7%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0240] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, recorded as iron carbide D3;
[0241] (5) Under the protection of Ar gas, 99 mol parts of iron carbide D3 and 1 mol part of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition D3.
[0242] Comparative Example 4
[0243] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L potassium hydroxide solution were mixed at 55° C. and pH=6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130° C. for 24 h and calcined at 400° C. for 10 h to obtain a precursor.
[0244] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 450°C for 6 h;
[0245] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0246] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 5:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, recorded as iron carbide D4;
[0247] (5) Under the protection of Ar gas, 98 mol parts of iron carbide D4 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition D4.
[0248] Comparative Example 5
[0249] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L sodium bicarbonate solution were mixed at 75°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0250] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 450°C for 6 h;
[0251] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 0.5%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0252] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, and then heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbides from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, recorded as iron carbide D5;
[0253] (5) Under the protection of Ar gas, 98 mol parts of iron carbide D5 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition D5.
[0254] Comparative Example 6
[0255] (1) 1.2 mol / L ferric nitrate and 0.9 mol / L potassium bicarbonate solution were mixed at 55°C and pH = 6.2 to obtain a precipitate slurry, which was washed with deionized water and filtered to obtain a filter cake, which was dried at 130°C for 24 hours and calcined at 400°C for 10 hours to obtain a precursor.
[0256] (2) reducing the precursor with H2 at a pressure of 1.5 atm, a flow rate of H2 of 12000 mL / h / g, and a temperature of 300°C for 6 h;
[0257] (3) cooling the product obtained in step (2) to 30° C. and contacting it with an inert gas containing O2 at this temperature for surface passivation treatment, wherein the volume concentration of O2 in the gas is 3%, the pressure is 0.05 atm, the gas flow rate is 4000 mL / h / g, and the treatment time is 24 h;
[0258] (4) replacing the mixed gas containing O2 with a mixed gas of H2 and CO under the following conditions: pressure 1.5 atm, total gas flow rate 10000 mL / h / g, H2 to CO molar ratio 70:1, heating from 30°C to 350°C at a heating rate of 1.5°C / min under the same conditions, and then preparing carbide from the product obtained in step (3) for a carbonization time of 1.5 h to obtain precipitated iron carbide, recorded as iron carbide D6;
[0259] (5) Under the protection of Ar gas, 98 mol parts of iron carbide D6 and 2 mol parts of ferrous oxide (i.e., containing Fe impurities) were mixed. The mixed mixture was recorded as iron carbide composition D6.
[0260] Comparative Example 7
[0261] The method of Example 1 is followed, except that (5) under the protection of Ar gas, 91 mole parts of precipitated x-iron carbide 1 and 9 mole parts of ferrous oxide (i.e. containing Fe impurities) are mixed. The mixed mixture is recorded as iron carbide composition D7.
[0262] Examples 25-48
[0263] Take the iron carbide composition 1-24 respectively, add the manganese citrate solution respectively by impregnation method under N2 protection, and dry it with N2 gas flow at 25°C for 24 hours to obtain Fischer-Tropsch catalysts 1-24 accordingly. The amount of manganese citrate solution added by impregnation is such that the obtained Fischer-Tropsch catalysts 1-24 respectively contain 85wt% of the iron carbide composition 1-24 and 15wt% of MnO2.
[0264] Comparative Examples 8-14
[0265] Take the iron carbide compositions D1-D7 respectively, add manganese citrate solution respectively by impregnation method under N2 protection, and dry with N2 gas flow at 25°C for 24 hours to obtain Fischer-Tropsch catalysts D1-D7 accordingly. The amount of manganese citrate solution added by impregnation is such that the obtained Fischer-Tropsch catalysts D1-D7 respectively contain 85wt% of the iron carbide compositions D1-D7 and 15wt% of MnO2.
[0266] Test Case
[0267] XRD and Mössbauer spectrometry were performed on iron carbides 1-24 and D1-D6, and the results of the Fe compound content are shown in Table 1. The unit of the Fe compound content is molar percentage.
[0268] Table 1
[0269] Iron Carbide Number χIron carbide content (mol%) Other Fe-containing impurities (mol%) 1-24 100.0 0.0 D1 45.0 55.0 D2 57.0 43.0 D3 39.0 61.0 D4 41.0 59.0 D5 38.0 62.0 D6 56.0 44.0
[0270] The whole process of preparing the iron carbide 1 in Example 1 was monitored by in-situ XRD detection technology, using an X-ray diffractometer (Rigaku, model D / max-2600 / PC) to monitor the crystal phase change of the material. Figure 1 As shown, curve A in the figure is before the precursor reduction in step (1), curve B is after the precursor reduction in step (1), curve C is after the surface passivation treatment in step (2), and curve D is after the carbide preparation in step (3). Among them, curve A is α-Fe2O3, and its characteristic peaks 2θ=33.3°, 35.7°, 41.0°, 49.5°, 54.2°, 57.6°, 62.7°, etc. are completely consistent with the standard card PDF-02-0919. B is the α-Fe crystal phase, and curve C is the α-Fe crystal phase with an oxide passivation layer generated on the surface, and their characteristic peaks 2θ=44.7°, 65.0°, 82.3° are consistent with the XRD standard card PDF-65-4899 of α-Fe. Curve D is χ-Fe5C2 with 100% purity, i.e. χ iron carbide. The main peaks of 2θ shown in curve D are 35.7°, 39.3°, 40.8°, 41.1°, 42.7°, 43.4°, 44.0°, 44.6°, 45.0°, 45.6°, 47.2°, and 50.2°. All characteristic peaks are completely consistent with the χ-Fe5C2 standard card PDF-89-8968. The obtained spectrum can clearly see the change process from nano iron powder to target carbide. The generated target product χ iron carbide has good crystallinity, corresponds well to all characteristic peaks of χ iron carbide, is extremely pure, and does not contain any other impurities.
[0271] The pure phase χ iron carbide obtained in other examples also has similar spectra as above, which will not be described in detail. However, the iron carbide obtained in Comparative Examples 1-6 cannot have pure phase χ iron carbide, and cannot be obtained as Figure 1 Spectrum of .
[0272] The iron carbide compositions 1-24 and D1-D7 were subjected to Mössbauer spectroscopy and BET specific surface area measurements, and the results are shown in Table 2.
[0273] Table 2
[0274]
[0275]
[0276] Note: In the iron carbide compositions D1-D6, the iron carbides D1-D6 are not precipitated 100% pure x-iron carbides. Table 1 shows the x-iron carbide content in the iron carbides D1-D6. The x-iron carbide content in the iron carbide compositions D1-D6 is determined based on the data on the iron carbides D1-D6 in Comparative Examples 1-6 and the data on the x-iron carbide in Table 1.
[0277] Evaluation Example
[0278] In a fixed bed continuous reactor, the catalytic reaction performance of Fischer-Tropsch catalysts 1-24, Fischer-Tropsch catalysts D1-D7, and iron carbide compositions 1-3 were evaluated respectively. The catalyst loading amount was 10.0 g.
[0279] Evaluation conditions: T = 255 ° C, P = 2.45 MPa, H2: CO = 1.7: 1, (H2 + CO) total amount = 45000 mL / h / g- Fe (Standard state flow rate, relative to Fe element) The reaction was carried out, and the reaction product was analyzed by gas chromatography. The reaction performance evaluation data after 24h and 400h of reaction are shown in Tables 3 and 4.
[0280] Table 3
[0281]
[0282]
[0283] Table 4
[0284]
[0285]
[0286] It can be seen from the above examples, comparative examples and the data in Tables 1-4 that the precipitated x-iron carbide or the composition or the catalyst prepared by the present invention is subjected to the Fischer-Tropsch synthesis reaction under industrial conditions, and exhibits a high space-time conversion rate of the raw material CO within the limited conditions, better reaction performance, and ultra-low CO2 selectivity. At the same time, the CH4 selectivity is low and the effective product selectivity is high.
[0287] Further long-term experiments were conducted. From the data of 400 hours of reaction in Table 4, it can be seen that after long-term operation of the precipitated x-iron carbide composition or catalyst prepared under the limited conditions of the present invention, both the CO conversion rate and the product selectivity remained stable without significant changes, and the stability was much better than that of the iron carbide in the prior art.
[0288] The precipitated iron carbide or composite or catalyst prepared under the conditions specified in the present invention can be applied to high-temperature and high-pressure continuous reactors, and has high reaction stability and extremely low CO2 selectivity: under industrial Fischer-Tropsch synthesis reaction conditions, a high-pressure continuous reactor can be used to maintain continuous and stable reaction for more than 400 hours, and its CO2 selectivity is below 15% (preferably 8% or less); at the same time, its by-product CH4 selectivity is also maintained below 12% (preferably below 8%), and the effective product selectivity can reach more than 73% (preferably more than 85%). The effective product generation space-time yield of the catalyst under the preferred conditions can reach 140mmol / h / g- Fe The above is very suitable for the modern coal chemical Fischer-Tropsch synthesis industry to efficiently produce oil and wax products.
[0289] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various specific technical features in any suitable manner. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. However, these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a composition containing precipitated x-iron carbide, include: (1) mixing an aqueous solution containing an iron salt with an alkaline precipitant for co-precipitation, washing and separating the obtained precipitate, and then drying and calcining the obtained solid to obtain a precursor; (2) mixing the precursor with H 2 Reducing the precursor at a temperature of 450-610°C; (3) the material obtained in step (2) is mixed with 2 The surface is passivated at a temperature of 0-50°C. 2 O in gas 2 The volume concentration is 1-5%; (4) The material obtained in step (3) is mixed with H 2 , CO is used to prepare carbides at a temperature of 260-430°C, H 2 The molar ratio of CO to 7-110:1 is 7-110:1, and precipitated χ iron carbide is obtained; (5) mixing 95-100 mol parts of precipitated x-iron carbide and 0-5 mol parts of Fe-containing impurities under the protection of an inert gas; Wherein, the Fe-containing impurities are iron-containing substances other than x-iron carbide.
2. The method according to claim 1, in, The iron salt is selected from water-soluble iron salts; The alkaline precipitant is at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, sodium hydroxide, potassium hydroxide and ammonia water; And / or, the drying and roasting process includes: first drying the solid at a temperature of 35-80°C and a vacuum degree of 250-1200Pa for 6-10 hours; drying the dried material at 75-180°C for 3-24 hours, and then roasting the obtained material at a temperature of 250-580°C for 1-10 hours.
3. The method according to claim 2, in, The iron salt is selected from at least one of ferric nitrate, ferric chloride, ammonium ferrous sulfate and ammonium ferric citrate.
4. The method according to any one of claims 1 to 3, in, In step (2), the pressure of the precursor reduction is 0.1-15 atm, and the time is 0.7-15 h; And / or, in step (2), H 2 The gas flow rate is 600-25000mL / h / g.
5. The method according to claim 4, in, In step (2), the pressure of the precursor reduction is 0.3-2.6 atm, and the time is 1-12 h; And / or, in step (2), H 2 The gas flow rate is 2800-22000mL / h / g.
6. The method according to any one of claims 1 to 3, in, In step (3), the surface passivation treatment is performed at a pressure greater than 0 and less than or equal to 1.6 atm for a period of 5 to 72 hours; And / or, in step (3), the O-containing 2 The gas flow rate of the gas is 400-12000 mL / h / g.
7. The method according to claim 6, in, In step (3), the surface passivation treatment is performed at a pressure greater than 0 and less than or equal to 0.09 atm for a period of 10-56 hours; And / or, in step (3), the O-containing 2 The gas flow rate of the gas is 1400-8500 mL / h / g.
8. The method according to any one of claims 1 to 3, in, In step (4), the carbide is prepared at a pressure of 0.08-12 atm and a time of 0.3-30 h; And / or, in step (4), H 2 The total gas flow rate with CO is 250-21000 mL / h / g.
9. The method according to claim 8, in, In step (4), the carbide is prepared at a pressure of 0.15-2.5 atm and a time of 0.5-2.4 h; And / or, in step (4), H 2 The total gas flow rate with CO is 2000-18000mL / h / g.
10. The method according to any one of claims 1 to 3, in, The carbide preparation further comprises: performing a temperature increase operation simultaneously in step (4), from the temperature of the surface passivation treatment to 260-430° C. at a heating rate of 0.2-5° C. / min.
11. The method according to claim 10, in, The carbide preparation further comprises: performing a temperature increase operation simultaneously in step (4), from the temperature of the surface passivation treatment to 260-400° C. at a heating rate of 0.2-2.5° C. / min.
12. The method according to any one of claims 1 to 3, in, In step (5), 97-100 mol parts of precipitated x-iron carbide are mixed with 0-3 mol parts of Fe-containing impurities.
13. A composition containing precipitated x-iron carbide, wherein the composition comprises 95-100 mol% of precipitated x-iron carbide and 0-5 mol% of Fe-containing impurities, based on the total amount of the composition, wherein the Fe-containing impurities are iron-containing substances other than x-iron carbide; in, The specific surface area of the composition is 20-280 m 2 / g; The Fe-containing impurities are not 0; The preparation method of the composition comprises: (1) mixing an aqueous solution containing an iron salt with an alkaline precipitant for co-precipitation, washing and separating the obtained precipitate, and then drying and calcining the obtained solid to obtain a precursor; (2) mixing the precursor with H 2 Reducing the precursor at a temperature of 450-610°C; (3) the material obtained in step (2) is mixed with 2 The surface is passivated at a temperature of 0-50°C. 2 O in gas 2 The volume concentration is 1-5%; (4) The material obtained in step (3) is mixed with H 2 , CO is used to prepare carbides at a temperature of 260-430°C, H 2 The molar ratio of CO to 7-110:1 is 7-110:1, and precipitated χ iron carbide is obtained; (5) mixing 95-100 mol parts of precipitated x-iron carbide and 0-5 mol parts of Fe-containing impurities under the protection of an inert gas; Wherein, the Fe-containing impurities are iron-containing substances other than x-iron carbide.
14. The composition according to claim 13, in, The specific surface area of the composition is 27-210 m 2 / g.
15. The composition according to claim 13 or 14, in, The composition comprises 97-100 mol% of precipitated x-iron carbide and 0-3 mol% of Fe-containing impurities, based on the total amount of the composition.
16. The composition according to claim 13 or 14, in, The Fe-containing impurities are at least one of iron carbide, iron, iron oxide, iron hydroxide, iron sulfide, and iron salt other than x-iron carbide.
17. The composition according to claim 15, in, The Fe-containing impurities are at least one of iron carbide, iron, iron oxide, iron hydroxide, iron sulfide, and iron salt other than x-iron carbide.
18. A catalyst comprising the precipitated x-iron carbide composition according to any one of claims 13 to 17.
19. Use of the precipitated x-iron carbide composition according to any one of claims 13 to 17 or the catalyst according to claim 18 in a Fischer-Tropsch synthesis reaction.
20. Use of the precipitated x-iron carbide composition according to any one of claims 13 to 17 or the catalyst according to claim 18 in a synthesis reaction of C and H chemicals based on the Fischer-Tropsch principle.
21. The use according to claim 20, in, The chemical is a fuel.
22. A method for Fischer-Tropsch synthesis, include: Under Fischer-Tropsch synthesis reaction conditions, the synthesis gas is contacted with the precipitated x-iron carbide composition according to any one of claims 13 to 17 or the catalyst according to claim 18.
23. The method for Fischer-Tropsch synthesis according to claim 22, in, The Fischer-Tropsch synthesis is carried out in a high-temperature and high-pressure continuous reactor.
24. A method for Fischer-Tropsch synthesis, include: Under Fischer-Tropsch synthesis reaction conditions, the synthesis gas is contacted with a Fischer-Tropsch catalyst, wherein the Fischer-Tropsch catalyst comprises a Mn component and the precipitated x-iron carbide composition according to any one of claims 13 to 17.
Citation Information
Cited By
Fluidized bed Fischer-Tropsch synthesis method for catalyst containing chi iron carbide
CN120699658A