Method and device for preparing polymer composite piezoelectric material dispersed with boron nitride nanotubes, and polymer composite piezoelectric material prepared by the method
Arranging boron nitride nanotubes and polymer fibers in the same direction through electrospinning solves the problems of preparing high-purity boron nitride nanotubes and improving piezoelectric properties, achieving efficient piezoelectric material preparation and reducing production costs. and energy consumption.
Patent Information
- Application Number
- CN201980016278.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-09
- Filing Date
- 2019-05-14
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2039-05-14
AI Technical Summary
The existing technology has the problems of high-temperature synthesis difficulty and low purity when preparing high-purity boron nitride nanotubes. Moreover, boron nitride nanotubes have low efficiency in the electrical polarization process and require high voltage or repeated mechanical processes, which limits the Improvement of its piezoelectric properties.
The electrospinning method is used to arrange boron nitride nanotubes and polymer fibers in the same direction, and are aligned through electromagnetic fields to avoid a separate polarization process and improve the polarization effect and piezoelectric properties.
It achieves efficient column polarization of boron nitride nanotubes in polymer composite materials, improves piezoelectric properties and polarization efficiency, and reduces production costs and energy consumption.
Smart Images

Figure CN112585774B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method and device for preparing a polymer composite piezoelectric material dispersed with boron nitride nanotubes and a polymer composite piezoelectric material prepared by the method. More specifically, the present invention relates to a method and device for preparing a polymer composite piezoelectric material dispersed with boron nitride nanotubes and a polymer composite piezoelectric material prepared by the method, which can improve the polarization effect and piezoelectric properties because the boron nitride nanotubes can be arranged in the same direction as the fibers by an electrospinning method without the need for a separate polarization alignment process, and a polymer composite piezoelectric material prepared by the method. Background Art
[0002] Boron nitride nanotubes (BNNTs) are similar to the well-known carbon nanotubes (CNTs) in mechanical properties and thermal conductivity. However, carbon nanotubes are electrically made of a mixture of conductors and semiconductors and have the characteristic of being oxidized in air above 400°C, while boron nitride nanotubes have electrical insulation properties and have the advantages of thermal stability and chemical stability that they will not be oxidized even in high-temperature air atmospheres above 800°C.
[0003] Due to the high thermal conductivity and electrical insulation, boron nitride nanotubes dispersed in the polymer composite material can be used flexibly as a highly efficient electrical insulating heat shielding material while maintaining the electrical insulation and thermal conductivity characteristics.
[0004] At the same time, boron nitride nanotubes have very outstanding thermal neutron absorption capabilities, so they are highly useful in the atomic energy / aerospace industry. In particular, in the case of aluminum composites dispersed with boron nitride nanotubes, they have the same strength as stainless steel and only half the density, so they are valuable as lightweight, high-strength metal alloys that have both radiation protection and mechanical strength.
[0005] Boron nitride nanotubes are known to have other characteristics, namely, they have piezoelectricity due to the potential difference caused by external pressure or vibration, or due to the asymmetry of the crystal structure caused by internal defects, so they have attracted much attention as a new type of piezoelectric material. As a widely used piezoelectric material in the past, ceramic lead zirconate titanate (PZT: Lead Zirconate Titanate, Pb(Zr,Ti)O 3) has high piezoelectricity and reliability, but has disadvantages such as high density, lead toxicity, inflexibility and impact resistance. Therefore, it is limited in many industries, especially in the application of wearable sensors / robots, medical and environmental fields. In addition, it has the disadvantage of requiring a separate polarization process to ensure high-quality polarization characteristics. Therefore, the polymer composite piezoelectric material with dispersed boron nitride nanotubes can be flexibly used as an environmentally friendly piezoelectric material, which is non-cytotoxic, large in area and flexible, and resistant to moisture and impact.
[0006] In addition, as a method for synthesizing / producing boron nitride nanotubes, arc discharge, laser plasma, vapor deposition (CVD), and ball milling-heat treatment have been developed so far, but laser plasma and ball milling-heat treatment are mainly used in commercial applications. These preparation methods have been improved and developed by various methods according to the type and atmosphere of the reaction gas, the type and form of the precursor, and the characteristics of the synthesis and preparation equipment. However, unlike carbon nanotubes, which can be synthesized at a temperature of about 800°C, boron nitride nanotubes have process difficulties such as synthesis at a high temperature of at least 1200°C and at most 5000°C, depending on the preparation method, and the current mass production technology is not yet mature. In addition, depending on the type of process, impurities based on the precursor and reaction gas are generated simultaneously with the boron nitride nanotubes, so it has the disadvantage of relatively low purity.
[0007] Therefore, there is a need for a technology and process as well as a preparation system that can overcome the process disadvantages of the aforementioned prior art and can mass-produce high-purity boron nitride nanotubes. At the same time, research related to the industrial application of high-purity boron nitride nanotubes is also needed.
[0008] According to the latest research results, it is known that an electrical or mechanical polarization process is performed in order to improve the pressure point characteristics of polymer composite materials dispersed with boron nitride nanotubes. However, since boron nitride nanotubes are electrically insulating, the efficiency of the electrical polarization process is reduced, and in particular, it has the disadvantage of having to apply a very high voltage. In addition, when dispersing polymers, the efficiency of the die-casting process using the physical polarization method of aligning boron nitride using mechanical shear force is very low, so it is not very effective in improving the piezoelectricity of the composite material. As a result, the polarization process through this alignment has the limitations of having to be performed at a very high voltage, or repeated mechanical processes that consume a lot of time and cost.
[0009] The alignment polarization process used to improve the piezoelectricity of a polymer composite material dispersed with boron nitride nanotubes is a process of physically aligning the boron nitride nanotubes inside the composite material, which can greatly improve the piezoelectric performance.
[0010] Therefore, it is necessary to develop a method for preparing a polymer composite piezoelectric material having dispersed boron nitride nanotubes in a novel structure, which can maximize the piezoelectric properties of the composite material by aligning and polarizing the boron nitride nanotubes without performing a separate polarization process.
[0011] The relevant prior art includes Korean Patent No. 10-1867905 (invention title: Apparatus for preparing boron nitride nanotubes and method for preparing boron nitride nanotubes using the same, authorization date: June 8, 2018). Summary of the invention
[0012] Technical issues
[0013] Embodiments of the present invention provide a method and device for preparing a polymer composite piezoelectric material dispersed with boron nitride nanotubes, and a polymer composite piezoelectric material prepared by the method. The method can maximize the polarization effect of the entire array because the boron nitride nanotubes are arranged in the same direction as the polymer fibers by an electrospinning method without the need for a separate polarization process.
[0014] Furthermore, embodiments of the present invention provide a method and apparatus for preparing a polymer composite piezoelectric material dispersed with boron nitride nanotubes, and a polymer composite piezoelectric material prepared by the method. The method prepares fibers by generating an electromagnetic field by applying voltage according to an electrospinning method, so that the boron nitride nanotubes can be arranged in the same direction as the fibers during spinning, and polarization of the polymer itself can be formed according to the type of polymer, so that the polarization effect of the polymer composite material can be maximized.
[0015] Furthermore, embodiments of the present invention provide a method and apparatus for preparing a polymer composite piezoelectric material having dispersed boron nitride nanotubes that can achieve improved piezoelectric properties, and a polymer composite piezoelectric material prepared by the method.
[0016] Furthermore, embodiments of the present invention provide a method and apparatus for preparing a polymer composite piezoelectric material dispersed with boron nitride nanotubes, and a polymer composite piezoelectric material prepared by the method. The method can arrange the boron nitride nanotubes in a certain direction inside the polymer fiber, and can also maximize the piezoelectric effect based on the polarization effect of the structural factors of the polymer itself.
[0017] At the same time, the embodiments of the present invention provide a polymer composite piezoelectric material. Since the material is prepared by dispersing and arranging boron nitride nanotubes in a polymer composite material, it can have flexibility and a high piezoelectric coefficient.
[0018] The technical problems to be solved by the present invention are not limited to the problems mentioned above, and practitioners in the relevant fields can clearly understand the unmentioned or other problems through the following description.
[0019] Technical Solution
[0020] According to an embodiment of the present invention, a method for preparing a polymer composite piezoelectric material dispersed with boron nitride nanotubes may include: a solution preparation step of preparing a polymer solution; a dispersion step of dispersing the boron nitride nanotubes in the above polymer solution; and an electrospinning step of preparing a composite piezoelectric material of a nanofiber phase by electrospinning the above polymer solution dispersed with the above boron nitride nanotubes using an electrospinning method.
[0021] Furthermore, in the electrospinning step according to an embodiment of the present invention, the boron nitride nanotubes may be dispersed in the polymer solution at a concentration of 0.01 weight percent to 20 weight percent.
[0022] Furthermore, in the electrospinning step according to an embodiment of the present invention, the boron nitride nanotubes may be dispersed in the polymer solution at a concentration of 2 weight percent.
[0023] Furthermore, in the electrospinning step according to an embodiment of the present invention, the external voltage applied to the polymer solution may be 5 kV to 30 kV.
[0024] Furthermore, in the solution preparation step according to an embodiment of the present invention, the prepared polymer solution may be a solution in which polyvinylidene fluoride (PVDF) as the polymer is dissolved in dimethylacetamide (DMA) acetone solution at 10-30 weight percent relative to the solution.
[0025] Furthermore, in the dispersing step according to the embodiment of the present invention, the boron nitride nanotubes may be uniformly dispersed in the polymer solution by utilizing the surface active effect of ultrasonic vibration.
[0026] Furthermore, in the dispersing step according to an embodiment of the present invention, a stirrer may be used to uniformly disperse the boron nitride nanotubes in the polymer solution.
[0027] Furthermore, in the dispersing step according to the embodiment of the present invention, the boron nitride nanotubes may be uniformly dispersed in the polymer solution by performing surface treatment on the boron nitride nanotubes.
[0028] Furthermore, in the electrospinning step according to an embodiment of the present invention, the polymer solution may be sprayed by the electrospinning method so that the boron nitride nanotubes and the polymer solution are arranged in the same direction to form a polymer film of a nanofiber phase.
[0029] Furthermore, according to an embodiment of the present invention, the injection speed of the polymer solution may be 15 μL / min to 70 μL / min, and the distance between the collector formed with the polymer film and the discharge part for electrospinning the polymer solution may be 5 cm to 20 cm.
[0030] In addition, the composite piezoelectric material preparation device according to an embodiment of the present invention includes: a solution supply part, which is used to store and supply a polymer solution dispersed with boron nitride nanotubes; a solution discharge part, which is used to discharge the polymer solution from the above-mentioned solution supply part; a collecting part, which collects the above-mentioned polymer solution discharged from the above-mentioned solution discharge part as a composite piezoelectric material of nanofiber phase; and a high voltage applying part, which applies a high voltage to the above-mentioned solution discharge part and the above-mentioned collecting part, so that the above-mentioned polymer solution is collected in the above-mentioned collecting part through an electrospinning method. The above-mentioned polymer solution can be electrospun from the above-mentioned solution discharge part to the above-mentioned collecting part through the above-mentioned electrospinning method, so that the above-mentioned boron nitride nanotubes are arranged in the same direction.
[0031] Furthermore, the boron nitride nanotubes may be dispersed in the polymer solution according to the embodiment of the present invention at a concentration of 2 weight percent.
[0032] Furthermore, according to an embodiment of the present invention, the solution supply part may be configured as a syringe type, the solution discharge part may be configured as a needle type combined with a front end of the solution supply part, and the collection part may be configured as a rotatable roller type.
[0033] Furthermore, when a high voltage is applied to the solution discharge part by the high voltage applying part according to an embodiment of the present invention, the polymer solution discharged from the solution discharge part forms a hemispherical shape at the end of the solution discharge part due to surface tension, and then a Taylor cone can be formed by the mutual electrostatic repulsion between surface charges and the external electric field. If an electric field higher than the preset electric field is applied, the polymer can be electrospun toward the collecting part to form a piezoelectric composite material of a nanofiber phase on the collecting part.
[0034] Furthermore, the external voltage applied to the polymer solution by the high voltage application part according to the embodiment of the present invention is 5kV to 30kV, the injection speed of the polymer solution is 15μL / min to 70μL / min, and the distance between the collector formed with the polymer film and the discharge part for electrospinning the polymer solution is 5cm to 20cm. The morphology of the nanofiber phase can be selectively determined by adjusting the external voltage, the injection speed or the distance.
[0035] In addition, according to the composite piezoelectric material of an embodiment of the present invention, after dispersing boron nitride nanotubes in a polymer solution containing a polymer, the polymer solution containing the boron nitride nanotubes is electrospun by an electrospinning method to prepare a nanofiber phase, and the boron nitride nanotubes can be arranged in the nanofiber phase along the direction of the nanofiber phase.
[0036] Technical Effects
[0037] According to an embodiment of the present invention, since boron nitride nanotubes are arranged in the same direction as polymer fibers through an electrospinning method without a separate polarization process, the polarization effect through the entire array can be maximized, thereby achieving improved piezoelectric characteristics.
[0038] Furthermore, according to an embodiment of the present invention, fibers are prepared by an electromagnetic field generated by applying voltage according to an electrospinning method, so that the boron nitride nanotubes can be arranged in the same direction as the fibers during spinning, and polarization of the polymer itself can be formed according to the type of polymer, thereby maximizing the polarization effect of the polymer composite material.
[0039] Also, according to the embodiments of the present invention, improved piezoelectric characteristics may be achieved.
[0040] Furthermore, according to the embodiments of the present invention, the boron nitride nanotubes can be arranged in a certain direction inside the polymer fiber, and the piezoelectric effect can be maximized according to the polarization effect of the structural factors of the polymer itself.
[0041] When the boron nitride nanotubes are composited in the same direction inside the polymer fiber, the elastic modulus of the polymer composite material can be increased, and finally the stress is increased by applying pressure to increase the local deformation, thereby improving the piezoelectric properties of the boron nitride nanotube polymer composite material. In addition, when the boron nitride nanotubes are arranged in a polymer composite material by an electric field applied during the electrospinning process, the polarization properties of the pure polymer can be further improved, and the polarization properties based on the composite arrangement can be maximized, thereby having the advantage of further improving the piezoelectric properties.
[0042] Finally, according to the embodiments of the present invention, boron nitride nanotubes can be dispersed and arranged in a polymer composite material to prepare a material having flexibility and a high piezoelectric coefficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 FIG. 1 is a sequence diagram of a method for preparing a composite piezoelectric material dispersed with boron nitride nanotubes using an electrospinning method according to an embodiment of the present invention.
[0044] Figure 2FIG. 1 is a schematic structural diagram of a device for preparing a composite piezoelectric material dispersed with boron nitride nanotubes using an electrospinning method according to an embodiment of the present invention.
[0045] Figure 3 To confirm the Figure 1 Image of the composite piezoelectric material prepared by the preparation method.
[0046] Figure 4 To confirm the Figure 1 Image of the composite piezoelectric material prepared by the preparation method.
[0047] Figure 5 For the purpose of illustration, the preparation for evaluation is carried out by Figure 1 FIG. 1 is a diagram of the various structures used in the preparation method of the composite piezoelectric material sensor.
[0048] Figure 6 To show the use of Figure 1 Preparation method for preparing composite piezoelectric material Figure 5 Figure 1. An example of a voltage signal generated on an oscilloscope after a sensor is inserted.
[0049] Figure 7a 1 is a diagram showing structures of α-phase, β-phase, and γ-phase according to arrangement of structural elements of polyvinylidene fluoride used as a composite piezoelectric material.
[0050] Figure 7b FIG. 5 is a graph showing a Fourier transform infrared absorption spectrometer (FTIR) spectrum of a composite piezoelectric material film prepared by electrospinning.
[0051] Figure 7c The figure shows the Fourier transform infrared absorption spectrometer spectrum of the polyvinylidene fluoride composite piezoelectric material prepared by the die casting method using ordinary mechanical shear force to attempt to align and polarize the boron nitride nanotubes.
[0052] Figure 7d The figure shows the calculation of the structural ratio of the α-phase and the β-phase of each prepared composite piezoelectric material using the peak of the Fourier transform infrared absorption spectrometer spectrum.
[0053] Explanation of symbols:
[0054] 100: Preparation device of composite piezoelectric material dispersed with boron nitride nanotubes
[0055] 110: Solution supply department
[0056] 111: Polymer solution
[0057] 120: Solution discharge part
[0058] 130: High voltage applying unit
[0059] 140: Collection Department
[0060] 150: Composite piezoelectric materials of nanofiber phase DETAILED DESCRIPTION
[0061] The advantages and / or features of the present invention and methods for achieving them can be clarified by referring to the accompanying drawings and the embodiments described below. However, the present invention is not limited to the embodiments described below, and can be implemented in various different ways. This embodiment is only used to complete the disclosure of the present invention and to enable ordinary technicians in the technical field to which the present invention belongs to fully understand the scope of the present invention. The present invention is only limited by the scope of the invention. Throughout the specification, the same figure numerals refer to the same structural elements.
[0062] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0063] Figure 1 FIG. 1 is a sequence diagram of a method for preparing a composite piezoelectric material dispersed with boron nitride nanotubes using an electrospinning method according to an embodiment of the present invention. Figure 2 FIG. 1 is a schematic structural diagram of a device for preparing a composite piezoelectric material dispersed with boron nitride nanotubes using an electrospinning method according to an embodiment of the present invention. Figure 3 To confirm the Figure 1 Image of the composite piezoelectric material prepared by the preparation method. Figure 4 To confirm the Figure 1 Image of the composite piezoelectric material prepared by the preparation method.
[0064] First refer to Figure 1 According to an embodiment of the present invention, a method for preparing a composite piezoelectric material dispersed with boron nitride nanotubes may include: a solution preparation step (S100), preparing a polymer solution containing a polymer; a dispersion step (S200), dispersing the boron nitride nanotubes in the above polymer solution; an electrospinning step (S300), preparing a composite piezoelectric material of a nanofiber phase by electrospinning the above polymer solution dispersed with the above boron nitride nanotubes using an electrospinning method; and a characteristic evaluation step (S400), evaluating the piezoelectric characteristics of the composite piezoelectric material.
[0065] With this step-by-step structure, boron nitride nanotubes can be arranged in the same direction as the fibers by electrospinning without a separate polarization alignment process, so a composite piezoelectric material with improved piezoelectric properties can be prepared. It is also possible to maximize the polarization effect by regularly arranging the elements that make up the polymer.
[0066] Specifically, since the boron nitride nanotubes can be orderly arranged in the polymer contained in the polymer solution, the charge movement and transfer efficiency can be improved compared to the case where the boron nitride nanotubes are randomly distributed. In particular, the polarization of the boron nitride nanotubes dispersed throughout the polymer can be maximized, thereby improving the piezoelectric properties.
[0067] Specifically, the fibers or nanofibers generated by ejection from a jet in electrospinning are stretched, thereby allowing the boron nitride nanotubes contained in the fibers to be arranged in a certain preferential manner.
[0068] At the same time, in the nanofiber composite piezoelectric material, the boron nitride nanotubes can be aligned inside the nanofiber phase formed by the polymer along the length direction of the nanofiber phase.
[0069] Each step is described. First, the solution preparation step (S100) is a step of preparing a polymer solution by dissolving a polymer in a pre-prepared solution. In the solution preparation step (S100), the polymer used can be polyvinylidene fluoride (PVDF). Moreover, the solution can be a mixed solution of dimethylacetamide and acetone. In this solution, 10 to 30 weight percent of the polymer, i.e., polyvinylidene fluoride, can be dissolved relative to 100 weight percent of the solution. More preferably, 14 to 20 weight percent can be dissolved to prepare the polymer solution.
[0070] However, the type of polymer in the polymer solution and the type and proportion of the solution are not limited thereto, and other types of polymers and solutions may be used, and the polymers may be mixed in the solution in other proportions.
[0071] In addition, the dispersing step (S200) of this embodiment is a step of dispersing the boron nitride nanotubes in the polymer solution prepared in the solution preparation step (S100), that is, the boron nitride nanotubes are uniformly dispersed in the polymer solution.
[0072] In the dispersing step (S200), the boron nitride nanotubes can be uniformly dispersed in the polymer solution by utilizing the surface active effect of ultrasonic vibration. When the boron nitride nanotubes are dispersed in the polymer solution, ultrasonic vibration is applied so that the boron nitride nanotubes can be uniformly dispersed in the polymer solution.
[0073] However, the invention is not limited thereto, and of course a stirrer can be used to evenly disperse the boron nitride nanotubes in the polymer solution.
[0074] Furthermore, the present invention is not limited thereto. Of course, the surface treatment of the boron nitride nanotubes can be used to uniformly disperse the boron nitride nanotubes in the polymer solution and to enhance the bonding force between the polymer and the boron nitride nanotubes.
[0075] In addition, the polymer solution in which the boron nitride nanotubes are uniformly dispersed in the dispersing step ( S200 ) can be electrospun in the electrospinning step ( S300 ) to prepare a composite piezoelectric material of a nanofiber phase.
[0076] In the electrospinning step ( S300 ) of this embodiment, the boron nitride nanotubes dispersed in the polymer solution can be arranged in the same direction as the polyvinylidene fluoride by the electrospinning method to form a polymer film of a nanofiber phase.
[0077] pass Figure 2 This is illustrated by the preparation device 100.
[0078] Reference Figure 2 The composite piezoelectric material preparation device 100 dispersed with boron nitride nanotubes of this embodiment may include: a solution supply part 110, used to store and supply a polymer solution 111 dispersed with boron nitride nanotubes; a solution discharge part 120, used to discharge the polymer solution from the solution supply part 110; a collecting part 140, which collects the polymer solution 111 discharged from the solution discharge part 120 as a composite piezoelectric material of a nanofiber phase 150; and a high voltage applying part 130, which applies a high voltage to the solution discharge part 120 and the collecting part 140, so as to collect the polymer solution 111 in the collected part 140 through an electrospinning method.
[0079] According to this structure, the polymer solution can be electrospun from the solution discharge part 120 to the collection part 140 by the electrospinning method, so that the boron nitride nanotubes are arranged in the same direction on the polymers of the polymer solution.
[0080] like Figure 2 As shown, the solution supply part 110 may be provided in a syringe type. Therefore, the push rod portion of the solution supply part 110 may be pushed to discharge the polymer solution through the solution discharge part 120.
[0081] The solution discharge part 120 may be provided as a needle type combined with the front end of the solution supply part, and the collection part 140 may be provided as a rotatable roller type. However, the structure of the collection part 140 is not limited thereto, and two rods may be provided in parallel for use.
[0082] When a high voltage is applied to the solution discharge portion 120 and the collection portion 140 through the high voltage application portion 130, the polymer solution 111 discharged from the solution discharge portion 120 forms a hemispherical shape at the end of the solution discharge portion 120 due to surface tension, and then forms a Taylor cone by the mutual electrostatic repulsion between surface charges and the external electric field.
[0083] Furthermore, if an electric field greater than a preset electric field is applied, the polymer solution 111 may be electrospun toward the collecting portion 140 to form a piezoelectric composite material 150 of a nanofiber phase on the collecting portion.
[0084] In the electrospinning step (S300), the external voltage applied to the polymer solution 111 may be 5 kV to 30 kV. Moreover, the ejection speed of the polymer solution 111 may be 15 μL / min to 70 μL / min, and the distance between the collecting part 140 for forming the polymer film and the discharge part of the electrospun polymer solution 111 may be adjusted between 5 cm and 20 cm. That is, the morphology of the composite piezoelectric material 150 according to various characteristics may be selectively determined by adjusting the external voltage, the ejection speed or the distance.
[0085] In addition, in the electrospinning step (S300), as the polymer solution is electrospun through the solution discharge unit 120, the effect of fiber or nanofiber stretching can be produced. Figure 3 As shown, the internal boron nitride nanotubes can be well aligned along the fiber direction.
[0086] pass Figure 3 The following results were confirmed by observation with a transmission electron microscope (TEM) that the aligned structure of polyvinylidene fluoride and boron nitride nanotubes as polymers in the nanofiber phase composite piezoelectric material formed by applying the electrospinning method of this example.
[0087] It can be seen that the boron nitride nanotubes are uniformly arranged along the length direction of the polyvinylidene fluoride, so the charge polarization efficiency can be improved compared to the case where the boron nitride nanotubes are randomly distributed in the polyvinylidene fluoride. In addition, since the polarization of the entire array of boron nitride nanotubes distributed in the entire polymer can be maximized, the piezoelectric properties can be improved.
[0088] In this way, by electrospinning a polymer solution using an electrospinning method, a composite piezoelectric material having the same directionality (tendency) can be prepared. Figure 4 This is a polymer image observed by scanning electron microscopy (SEM), which shows that they have the same directionality. Therefore, the boron nitride nanotubes are well aligned inside the polymer to maximize the polarization of the charge without the need for a separate boron nitride nanotube polarization process, thereby improving the piezoelectric efficiency.
[0089] In addition, in the characteristic evaluation step ( S400 ) of this embodiment, a piezoelectric constant detector (Piezometer) can be used to evaluate the piezoelectric characteristics of the composite piezoelectric material in which the boron nitride nanotubes are arranged in the same direction by the aforementioned electrospinning step ( S300 ).
[0090] In the characteristic evaluation step (S400) of the present embodiment, a piezoelectric constant detector is used to confirm the piezoelectric coefficient of the d33 mode showing the piezoelectric effect in the vertical direction of the piezoelectric material. The evaluation of the piezoelectric properties can be implemented according to the concentration of the boron nitride nanotubes. For example, it can be confirmed that in the case of the piezoelectric material of the electrospinning of pure polyvinylidene fluoride polymer without boron nitride nanotubes, it is 50pC / N, and in the case of the concentration of the boron nitride nanotubes being 2 weight percent, it is 250pC / N. It can be seen that in the polyvinylidene fluoride polymer suitable for boron nitride nanotubes, the piezoelectric properties are increased by more than 5 times.
[0091] From these results, it can be seen that, compared with the case of preparing by electrospinning polyvinylidene fluoride alone, the piezoelectric coefficient of the d33 mode is increased from 50 pC / N to 250 pC / N in the case of electrospinning mixed boron nitride nanotubes, which is increased by more than about 5 times. It can be seen that since the boron nitride nanotubes are well arranged inside the composite piezoelectric material in which the boron nitride nanotubes prepared by the electrospinning method are dispersed, the piezoelectric properties are improved.
[0092] In addition, a piezoelectric sensor using the composite piezoelectric material according to the present embodiment will be described below with reference to the drawings.
[0093] Figure 5 For the purpose of illustrating the preparation for evaluation by Figure 1 FIG. 1 is a diagram of the various structures used in the preparation method of the composite piezoelectric material sensor.
[0094] Reference Figure 5 As can be seen, the structure of the piezoelectric sensor 200 is prepared using the composite piezoelectric material 150 prepared by the aforementioned method. The piezoelectric sensor 200 is formed by stacking a plurality of polyimide films 210a, 210b, and 210c, and has a platinum (Pt) electrode 221 and an aluminum (Al) electrode 225 inside, and the composite piezoelectric material 150 of this embodiment can be provided between them. Furthermore, a copper (Cu) strip 230 is disposed between the upper polyimide film 210a and the lower polyimide film 210b, so that the piezoelectric sensor 200 can be prepared.
[0095] The piezoelectric sensor 200 is designed to maximize the piezoelectric characteristics by using the composite piezoelectric material 150 having certain directionality. In order to improve the durability of the piezoelectric sensor 200 and maintain flexibility, a plurality of polyimide films 210a, 210b, 210c may be used to cover the front and rear surfaces.
[0096] Meanwhile, in order to detect a signal emitted from the composite piezoelectric material 150 , a platinum electrode 221 and an aluminum electrode 225 may be used as upper and lower electrodes, and a copper ribbon 230 may be used as an electric wire.
[0097] in addition, Figure 6 To show the use of Figure 1 The composite piezoelectric material prepared by the preparation method is prepared as follows: Figure 5 Figure 1. An example of a voltage signal generated on an oscilloscope after a sensor is inserted.
[0098] In other words, it is the result of detecting the output voltage of the piezoelectric sensor.
[0099] When a certain force is applied to the aforementioned piezoelectric sensor 200 in the vertical direction, it can be confirmed that the signal outputted due to the piezoelectric effect is at most 28Vpp (peak-to-peak). This shows the high performance of the composite piezoelectric material of this embodiment, and this piezoelectric property is generated by the boron nitride nanotubes and polyvinylidene fluoride polymer used as flexible elements in the composite piezoelectric material prepared by the electrospinning method.
[0100] This improvement in piezoelectric properties can be considered to be the result of an increase in the β-phase contents of polyvinylidene fluoride in the sample prepared by the electrospinning method and the influence of the boron nitride nanotubes thereon, which can be understood from FIG. 7 .
[0101] Figure 7a : is a diagram showing the structures of the α phase, β phase, and γ phase according to the arrangement of structural elements of polyvinylidene fluoride used as a composite piezoelectric material, Figure 7b 1 is a graph showing the Fourier transform infrared absorption spectrometer (FTIR) spectrum of the composite piezoelectric material prepared by electrospinning, Figure 7c This is a diagram showing the Fourier transform infrared absorption spectrometer spectrum of a polyvinylidene fluoride composite piezoelectric material prepared by a die casting method in which a common mechanical shear force is used to attempt to align and polarize boron nitride nanotubes. Figure 7d The figure shows the calculation of the structural ratio of the α-phase and the β-phase of each prepared composite piezoelectric material using the peak of the Fourier transform infrared absorption spectrometer spectrum.
[0102] exist Figure 7aIn the figure, the structures of the α phase, β phase and γ phase of polyvinylidene fluoride are shown. It is generally known that the α phase polyvinylidene fluoride has low piezoelectricity, while the β phase polyvinylidene fluoride has excellent piezoelectricity. Therefore, a polarization process needs to be added to convert the α phase polyvinylidene fluoride into the β phase polyvinylidene fluoride in order to improve the piezoelectricity.
[0103] pass Figure 7b and Figure 7c , it can be confirmed that the spectral results of Fourier transform infrared absorption spectrometer (FTIR) are those of the composite piezoelectric material of the nanofiber phase formed by using the electrospinning method of this embodiment and the composite piezoelectric material prepared by using the existing die-casting method.
[0104] Therefore, if Figure 7d As shown, the β-phase content of the polyvinylidene fluoride polymer is 40% when prepared by the die casting method, while it can be increased to 55% when prepared by the electrospinning method. In particular, in the case of polyvinylidene fluoride / boron nitride nanotubes (20 weight percent) prepared by the die casting method, it can be seen that the β-phase content is reduced by about 30% compared with the pure polyvinylidene fluoride polymer, which is known to be due to the disordered distribution of the boron nitride nanotubes in the polymer.
[0105] In contrast, it was confirmed that the β-phase content of the polyvinylidene fluoride / boron nitride nanotubes prepared by the electrospinning method increased to about 75%. It can be expected that in the case of preparation by the electrospinning method, the boron nitride nanotubes are distributed in the same direction inside the polymer, so that the polymer structure also contributes to the conversion to the β-phase.
[0106] The results of evaluating the piezoelectric coefficient of the d33 mode of the composite piezoelectric material prepared by the die casting method confirmed that it was 5 pC / N in the case of pure polyvinylidene fluoride polymer, and 40 pC / N in the case of 20 weight percent polyvinylidene fluoride / boron nitride nanotubes.
[0107] Compared with the piezoelectric coefficient (250pC / N) of the polyvinylidene fluoride / boron nitride nanotube (2 weight percent) composite piezoelectric material prepared by the electrospinning method, a difference of more than 6 times can be confirmed, which can be regarded as the result of the above-mentioned improvement in piezoelectricity based on the β-phase content of polyvinylidene fluoride and the maximization of the polarization effect based on the entire array of boron nitride nanotubes.
[0108] Therefore, in the case of electrospinning, while increasing the β-phase content of pure polyvinylidene fluoride, the internal boron nitride nanotubes are polarized in an array, which can maximize the charge transfer effect. Based on this, it can be understood that this effect leads to an increase in piezoelectric properties. This can be understood through the following table.
[0109] Table 1
[0110]
[0111]
[0112] As described above, according to the embodiments of the present invention, since the boron nitride nanotubes can be arranged in the same direction as the fibers by the electrospinning method without a separate polarization alignment process, an efficient polymer composite piezoelectric material with improved piezoelectric properties can be realized. At the same time, since the boron nitride nanotubes can be orderly arranged in the polymer contained in the polymer solution, the polarization efficiency can be improved compared with the case where the boron nitride nanotubes are randomly distributed.
[0113] Specifically, the fibers are prepared by applying an electromagnetic field using an electrospinning method to apply voltage, so that the boron nitride nanotubes can be arranged in the same direction as the fibers during spinning. Depending on the type of polymer, the polarization of the polymer itself can also be formed, thereby maximizing the polarization effect of the polymer composite material, thereby achieving improved piezoelectric properties.
[0114] Furthermore, the boron nitride nanotubes can be aligned in a certain direction inside the polymer fiber, and the piezoelectric effect can be maximized by the polarization effect of the structural factors of the polymer itself.
[0115] Finally, since boron nitride nanotubes are prepared by dispersing and arranging them in a polymer composite material, they can have high piezoelectric coefficients while being flexible.
[0116] Although specific embodiments of the present invention have been described so far, various modifications may be made without departing from the scope of the present invention. Therefore, the scope of the present invention should not be defined by being limited to the described embodiments, but should be defined by the scope of the invention claims and the scope of equivalents.
[0117] As described above, although the present invention is described with limited embodiments and drawings, the present invention is not limited to the above embodiments, and ordinary technicians in the field of the present invention can make various modifications and variations through these descriptions. Therefore, the concept of the present invention should only be understood by the scope of the invention claims, and all equivalent or equivalent variations should fall within the scope of the concept of the present invention.
Claims
1. A piezoelectric sensor using a polymer composite piezoelectric material, characterized in that: include: a first electrode and a second electrode; as well as A polymer composite piezoelectric material in which boron nitride nanotubes are dispersed is provided between the first electrode and the second electrode. The polymer composite piezoelectric material is formed such that the boron nitride nanotubes are arranged in the nanofiber phase along the length direction of the nanofiber phase. Wherein, the polymer composite piezoelectric material is formed by the following steps: a solution preparation step, preparing a polymer solution; a dispersing step of dispersing the boron nitride nanotubes in the polymer solution; and an electrospinning step, wherein the polymer solution in which the boron nitride nanotubes are dispersed is electrospinned by an electrospinning method to prepare a composite piezoelectric material of a nanofiber phase; Wherein, the polymer in the polymer solution is polyvinylidene fluoride.
2. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 1, characterized in that: In the electrospinning step, the boron nitride nanotubes are dispersed in the polymer solution at a concentration of 0.01 weight percent to 20 weight percent.
3. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 2, characterized in that: In the electrospinning step, the boron nitride nanotubes are dispersed in the polymer solution at a concentration of 2 weight percent.
4. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 1, characterized in that: In the electrospinning step, the external voltage applied to the polymer solution is 5 kV to 30 kV.
5. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 1, characterized in that: In the solution preparation step, the prepared polymer solution is a solution in which the polyvinylidene fluoride is dissolved in a dimethylacetamide acetone solution at a weight percentage of 10 to 30 relative to the solution.
6. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 1, characterized in that: In the dispersing step, the boron nitride nanotubes are uniformly dispersed in the polymer solution by utilizing the surface activation effect of ultrasonic vibration.
7. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 1, characterized in that: In the dispersing step, a stirrer is used to uniformly disperse the boron nitride nanotubes in the polymer solution.
8. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 1, characterized in that: In the dispersing step, the boron nitride nanotubes are uniformly dispersed in the polymer solution by surface treating the boron nitride nanotubes.
9. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 1, characterized in that: In the electrospinning step, the polymer solution is sprayed by the electrospinning method, so that the boron nitride nanotubes and the polymer solution are arranged in the same direction to form a polymer film of a nanofiber phase.
10. The piezoelectric sensor using a polymer composite piezoelectric material according to claim 1, characterized in that: The ejection speed of the polymer solution is 15 μL / min to 70 μL / min, and the distance between the collector formed with the polymer composite piezoelectric material and the discharge part for electrospinning the polymer solution is 5 cm to 20 cm.
Citation Information
Cited By
Boron nitride-based piezoelectric material, preparation method and application of boron nitride-based piezoelectric material in underwater monitoring equipment
CN120157929A