Metal oxide electrode compositions

By using niobium tungsten oxide as an electrode material in lithium-ion batteries, the problem of lithium dendrites and inhomogeneity in high-rate applications of lithium-ion batteries is solved, high energy density and fast charge and discharge are achieved, and the battery manufacturing process is simplified And provides a safe battery management system.

CN112585780BActive Publication Date: 2024-10-29CAMBRIDGE ENTERPRISE LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201980053477.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-06-07
Publication Date
2024-10-29
Estimated Expiration
2039-06-07

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have problems with lithium dendrite formation, particle cracking and inhomogeneity in high-rate applications, leading to risks of short circuits, fires and explosions. Moreover, the synthesis of nanostructures is complex, time-consuming and suffers from loss of energy density, making it difficult to achieve high energy. density and fast charge and discharge.

Method used

Niobium tungsten oxide is used as the electrode material to achieve high-rate lithium-ion battery performance through its good lithium diffusion performance and less solid electrolyte dielectric reaction, and is optimized by adjusting the molar ratio of Nb2O5 to WO3 and mixing with LTO. Electrode structure.

Benefits of technology

It achieves high energy density and fast charge and discharge rates, reduces the risk of lithium dendrite formation, simplifies the battery manufacturing process, and provides a simple battery management system suitable for high-power fast charging applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112585780B_ABST
    Figure CN112585780B_ABST
Patent Text Reader

Abstract

The present invention provides a method for charging and / or discharging an electrochemical cell at a high rate, wherein the electrochemical cell has a working electrode comprising niobium tungsten oxide and / or niobium molybdenum oxide. The present invention also provides an electrode comprising niobium tungsten oxide wherein the ratio of Nb2O5 to WO3 is from 8:5 to 11:20, and an electrode comprising niobium molybdenum oxide wherein the ratio of Nb2O5 to MoO3 is from 6:1 to 1:3.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application is related to and claims the benefit of GB 1809467.2 filed on June 8, 2018 (08.06.2018) and GB 1905218.2 filed on April 12, 2019 (12.04.2019), the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present invention provides electrodes and electrochemical cells including the electrodes, such as lithium ion batteries, and methods of using the electrodes in the electrochemical cells. Background Art

[0004] High-rate lithium-ion battery electrode materials can store large amounts of charge in minutes rather than hours of charging. These materials are needed to ease the technical challenges associated with the adoption of electric vehicles and grid-scale batteries and to enable new power-hungry devices.

[0005] The most intuitive and commonly used approach to improve the rate performance of electrode materials is to create nano-sized or porous (often hierarchical) structures. This minimizes the solid-state diffusion distance of lithium ions, allowing lithium ions to be transported more quickly through the electrode and increasing the surface area of ​​the electrode material in contact with the electrolyte. Carbonaceous hierarchical structures and carbon coatings are also often used to improve electronic conductivity, another prerequisite for high-rate applications.

[0006] In practice, despite its excellent lithium ion mobility, graphite cannot be used at high rates due to the risk of particle fracture and lithium dendrite formation, resulting in short circuits and the risk of fire and explosion (Zhao et al.; Downie et al.). The latter problem inherently limits the use of low-voltage anodes in high-rate applications, as electrode inhomogeneities or any increased overpotential sources may lead to lithium plating potentials on the low-voltage electrode surface (Downie et al.).

[0007] Li4Ti5O 12 (Lithium titanate; LTO) relative to Li + The average voltage of 1.55 V for Li / Li allows high-rate intercalation (deintercalation) without the risk of Li dendrites or extensive solid-electrolyte interphase (SEI) formation, which, although undesirable, necessitates a reduction in the full-cell voltage and, therefore, in energy density. However, even in this putatively “high-rate” anode, the capacity of 1 μm particles from solid-state synthesis is only 60–65 mA·h·g at a rate of 10 C. -1 (Kim et al.).

[0008] Many strategies have been proposed to improve the capacity of LTO electrodes at high charge-discharge rates (C-rates). Currently, carbon-coated nanoparticles of LTO can achieve at least 150 mA h g at 10 C. -1 (Wang et al.; Odziomek et al.). This is equivalent to each transition metal (Li + / TM) is about 0.5 lithium ions.

[0009] However, the use of nanostructures and porous materials for electrochemical energy storage applications inherently results in severe losses in terms of volumetric energy density. In addition, these well-designed porous and nanostructures are time-consuming and expensive to synthesize, characterize and manufacture. Synthesis methods often result in relatively low yields and / or large amounts of chemical waste generation (Oszajca et al.). In addition, these porous and nanostructures are also susceptible to degradation during electrochemical cycling due to processes such as catalytic decomposition of electrolytes (Palacin et al.), morphological changes that result in loss of nanostructures (Wu et al.), and higher first cycle capacity loss (Kasnatscheew et al.).

[0010] Another problem with using nano-LTO electrodes in whole cells is gas evolution during repeated charge and discharge cycles, accompanied by swelling or pressure rise. This is caused by heterogeneous catalysis between the metal oxide surface and the organic electrolyte (He et al.; Lv et al.). The small particle size required to compensate for the lack of lithium ions and electron diffusion in LTO increases the reactive surface area, exacerbating this problem.

[0011] Fast charging or high power delivery from a full cell also requires a cathode to match the anode. LiFePO4 has been used as a promising high-rate cathode (Zaghib et al.). However, both LiFePO4 and LTO have exceptionally flat voltage curves. This combination provides a constant voltage but presents severe challenges in terms of battery management systems (BMS). A simple and accurate BMS is a critical factor for battery applications in electric vehicles and mobile technology, and is even more important at high rates to prevent dangerous and destructive over-discharge while maximizing practicality. A BMS relies on the ability to measure the state of charge, which cannot be simply done by charge counting alone as the battery degrades and electron-consuming side reactions occur.

[0012] In view of the above challenges, there is a need to provide new electrode materials for lithium-ion batteries that can operate at high rates. Summary of the invention

[0013] The present invention generally provides an electrode comprising niobium tungsten oxide, an electrochemical cell comprising the electrode, and use of the cell in a lithium ion battery during charge and / or discharge, for example at high charge and discharge rates (C-rates) of 5C or higher (e.g., 10C or higher).

[0014] The present inventors have determined that the use of electrode materials comprising niobium tungsten oxide in high-rate lithium-ion batteries can achieve extremely high volumetric energy density and impressive charge and discharge rates. Niobium tungsten oxide has good lithium diffusion properties and therefore exhibits excellent performance. + / Li above 1.0 V, there is minimal SEI formation, which means that lithium is not lost in side reactions with the electrolyte.

[0015] In addition, high-rate lithium-ion batteries using electrode materials containing niobium tungsten oxide can be operated at higher than 1.3 V. (e.g., relative to Li + / L,Nb 16 W5W 55 The average voltage is 1.57V, which is + / L,Nb 18 W 16 O 93 The average voltage of the battery is 1.67V. Operating in this voltage range eliminates the need to perform an initial formation cycle, thereby simplifying the battery manufacturing process. Typical lithium-ion batteries including graphite electrodes operate at voltages below 1.3V and must undergo an initial formation cycle before sealing the battery. Typically, this formation cycle is performed at an elevated temperature, such as 60°C, to allow degassing to occur. This adds time and cost to the battery manufacturing process.

[0016] In addition, in full cells such as LiFePO4, LiN(CF3SO2)2 (LiTFSI) can be used to replace the more toxic LiPF6 electrolyte salt commonly used in standard commercial electrolytes. In addition, aluminum can replace more expensive copper as a current collector while avoiding the LiAl alloying potential (relative to Li + / Li≤0.3V).

[0017] Using niobium tungsten oxide as an electrode material, for example in high-rate lithium batteries, the open circuit voltage can be used as a measure of the state of charge. This has the potential to provide a simple and reliable BMS, which could prove to be an important advantage for high-power / fast-charging applications.

[0018] In a first aspect of the present invention, a method of charging and / or discharging an electrochemical cell having a working electrode comprising niobium tungsten oxide at a charge and discharge rate (C-rate) of at least 5C (eg, at least 10C) is provided.

[0019] The electrochemical cell may comprise a counter electrode and an electrolyte, and optionally the electrode may be connected to or in communication with a power source.

[0020] The method may be carried out at a rate of at least 750 mA·g -1 , for example at least 800 mA g -1 A method for charging and / or discharging an electrochemical cell at a current density of 1000 Å.

[0021] The method may include cycling the electrochemical cell to charge and discharge, or discharge and charge, and the method may include 2 or more cycles, 5 or more cycles, 10 or more cycles, 50 or more cycles, 100 or more cycles, 500 or more cycles, 1,000 or more cycles, or 2,000 or more cycles.

[0022] In one embodiment, the working electrode does not have a porous structure or a layered structure.

[0023] The working electrode may include niobium tungsten oxide in particle form. For example, the niobium tungsten oxide may have a primary particle size of at least 1 μm.

[0024] The smaller surface area of ​​the particulate niobium tungsten oxide reduces side reactions and alleviates gas evolution problems and the associated swelling or pressure rise problems observed with nano-LTO electrodes. In addition, the particulate niobium tungsten oxide can be quickly and easily prepared using solid-state synthesis.

[0025] The working electrode can have a temperature of less than 10 14 m 2 ·s -1 The solid-state lithium diffusion coefficient (DLi) is, for example, less than 10 at 298K. -15 m 2 ·s -1 .

[0026] Good lithium diffusion properties enable micron-sized niobium tungsten oxide particles to be used at extremely high rates.

[0027] The working electrode can have 50 mA·h·g at 20C -1 For example, at 20C it is 75mA·h·g -1 or 50mA·h·g at 60°C -1 .

[0028] The molar ratio of Nb2O5 to WO3 in the working electrode may be 6:1 to 1:15, for example, 8:5 to 11:20.

[0029] The working electrode may include a niobium tungsten oxide selected from the group consisting of: Nb 12 WO 33 , Nb 26 W4O 77 , Nb 14 W3O 44 , Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 , Nb 22 W 20 O 115 、Nb8W9O 47 , Nb 54 W 82 O 381 , Nb 20 W 31 O 143 、Nb4W7O 31 or Nb2W 15 O 50 For example, Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 or Nb 22 W 20 O 115 .

[0030] In addition, the working electrode may include a mixture of niobium tungsten oxide and an additional active material. For example, the working electrode may include a mixture of niobium tungsten oxide and LTO. The ratio of niobium tungsten oxide to LTO may be 95:5 to 5:95 by weight. For example, the ratio may be 90:10 to 10:90 by weight, 80:20 to 20:80 by weight, 70:30 to 30:70 by weight, 60:40 to 40:60 by weight, or the ratio of niobium tungsten oxide to LTO may be 1:1 by weight.

[0031] In another aspect of the present invention, an electrode is provided, which may be referred to as a working electrode, comprising niobium tungsten oxide, for example wherein the molar ratio of Nb2O5 to WO3 in the electrode is 8:5 to 11:20. The working electrode is suitable for lithium ion batteries.

[0032] The working electrode may include Nb 16 W5W 55 , Nb 18 W8O69 、Nb2WO8、Nb 18 W 16 O 93 or Nb 22 W 20 O 115 Niobium tungsten oxide. For example, Nb 16 W5W 55 or Nb 18 W 16 O 93 .

[0033] In one embodiment, the working electrode does not have a porous structure or a layered structure.

[0034] The working electrode may include niobium tungsten oxide in particle form. For example, the niobium tungsten oxide may have a primary particle size of at least 1 μm.

[0035] In addition, the working electrode may include a mixture of niobium tungsten oxide and an additional active material. For example, the working electrode may include a mixture of niobium tungsten oxide and LTO. The ratio of niobium tungsten oxide to LTO may be 95:5 to 5:95 by weight. For example, the ratio may be 90:10 to 10:90 by weight, 80:20 to 20:80 by weight, 70:30 to 30:70 by weight, 60:40 to 40:60 by weight, or the ratio of niobium tungsten oxide to LTO may be 1:1 by weight.

[0036] In another aspect of the present invention, an electrochemical cell is provided, which comprises a working electrode of the present invention.

[0037] In another aspect of the present invention, a lithium ion battery is provided, which comprises one or more electrochemical cells of the present invention. In the case of multiple cells, these cells can be arranged in series or in parallel.

[0038] In another aspect of the invention, there is provided the use of a working electrode comprising niobium tungsten oxide in a high rate electrochemical cell, for example wherein the cell is operated at a charge and discharge rate (C-rate) of at least 5C, for example at least 10C.

[0039] In another aspect of the present invention, a method of charging and / or discharging an electrochemical cell having a working electrode comprising niobium molybdenum oxide at a charge and discharge rate (C-rate) of at least 5C (e.g., at least 10C) is provided.

[0040] The inventors have found that using electrode materials containing niobium molybdenum oxide in high-rate lithium-ion batteries can achieve high energy density and considerable rate. Compared with common high-rate anode materials, niobium molybdenum oxide shows a higher average voltage, thus avoiding or minimizing the reaction with the electrolyte.

[0041] In another aspect of the present invention, an electrode is provided, which may be referred to as a working electrode, comprising niobium molybdenum oxide, for example, wherein the molar ratio of Nb2O5 to MoO3 in the electrode is 6:1 to 1:3, for example 1:3. The working electrode is suitable for lithium ion batteries.

[0042] The working electrode may include Nb2Mo3O 14 , Nb 14 Mo3O 44 or Nb 12 MoO 44 Niobium molybdenum oxide. For example, Nb2Mo3O 14 .

[0043] These and other aspects and embodiments of the invention are described in further detail below. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 is (A) Nb 16 W5W 55 and (B)Nb 18 W 16 O 93 Wide field SEM images at low magnification, showing roughly uniform particle size and the presence of agglomerates. The background of (A) is a Cu grid, and the background of (B) is binder carbon. In both images, the scale bar is 50 μm.

[0045] Figure 2 is the atomic structure and SEM image showing that (AC)Nb 16 W5W 55 and (DF)Nb 18 W 16 O 93 The scale bars shown in (B) and (E) are 5 μm. The scale bars shown in (C) and (F) are 10 μm.

[0046] Figure 3 It shows that Nb 18 W 16 O 93 Diagram of the bronze-like structure of and its relationship to classic tetragonal tungsten bronze (TTB). The partially filled spheres represent K + ions, which are not present in Nb 18 W 16 O 93 middle.

[0047] FIG. 4 shows a block Nb 16 W5W 55 and Nb 18 W 16 O 93 Figure 2 shows the rate performance of Nb.16 W5W 55 Constant current discharge and charge curves from 60C (the leftmost curve at 1.0V and 3.0V) to 0.2C (the rightmost curve at 1.0V and 3.0V); (B) Nb 16 W5W 55 From 0.2C (50mA·h·g -1 The leftmost curve below) to 60C (50mA·h·g -1 (C) Nb 18 W 16 O 93 Constant current discharge and charge curves from 100C (the leftmost curve at 1.0V and 3.0V) to 0.2C (the rightmost curve at 1.0V and 3.0V); (D) Nb 18 W 16 O 93 From 0.2C (50mA·h·g -1 The leftmost curve below) to 100C (50mA·h·g -1 (E) Summary of rate performance and (F) high rate cycling of 250 cycles at 10C followed by 750 cycles at 20C.

[0048] Figure 5 shows that Li4Ti5O 12 (curve with a flat peak at 1.55 V), Nb 16 W5W 55 (curves crossing at 1.57V) and Nb 18 W 16 O 93 Voltage curves of (curves crossing at 1.65 V). Discharge and charge voltage curves normalized to (A) gravimetric capacity and (B) lithium ions transferred per transition metal atom. Li4Ti5O 12 , Nb 16 W5W 55 and Nb 18 W 16 O 93 The average voltages are 1.55 V, 1.57 V, and 1.65 V, respectively. 12 Electrochemistry (adapted from WebPlotDigitizer2017, Ankit Rohatgi) represents the best performance, consisting of 5-20 nm particles on 15-20 nm carbon nanofibers (CNFs) with a mass loading of 1 mg cm -2 .

[0049] FIG. 6 is a comparison of Cu foil and carbon-coated Al foil current collectors. Fig. 6A Figure 2 shows the Nb cycled for 1000 cycles under constant current discharge and charge at 10C (first 200 cycles) and 20C (last 800 cycles). 16 W5W 55 ; Copper foil at 1.0V (top line); Copper foil at 1.2V (second from the top); C-Al at 1.0V (third from the top) and C-Al at 1.2V (bottom line). Figure 6B The discharge and charge curves between 3.0 and 1.0 V for the 100th cycle at 10 C are shown; at 100 mA·h·g -1 The order of the curves below: C-Al charge curve (top); Cu foil charge curve (second from the top); Cu foil discharge curve (third from the top) and C-Al discharge curve (bottom).

[0050] Figure 7 shows the long term cycling as a function of the minimum cutoff voltage. (A) Nb on Cu foil cycled at C / 5 (first 50 cycles) and 1C (second 50 cycles) 16 W5W 55 , keep constant potential at the top of the charge for 1h; V min =1.2V (top curve); V min = 1.0 V (lowest curve). (B) Nb on aluminum foil cycled at C / 5 16 W5W 55 , without a constant potential charging step.

[0051] Figure 8 The overpotential as a function of current density in a Li||Li symmetric cell is shown.

[0052] Fig. 9 shows the measurement 7 The stimulated echo pulsed field gradient sequence of Li diffusivity shows the radio frequency ( 7 Li) and magnetic field gradient (G z Here, the gradient pulse duration (t g ) includes the rising slope, opening time and falling slope of the opt compound gradient pulse.

[0053] Fig.10 A representative 7 Li decay curves showing (A) Li 10.2 Nb 18 W 16 O 93 At 453K, (B)Li 6.8 Nb 18 W 16O9 at 453K, (C)Li 3.4 Nb 18 W 16 O 93 At 453K, (D)Li 6.3 Nb 16 W5W 55 At 353K and (E)Li 8.4 Nb 16 W5W 55 Normalized NMR signal intensity as a function of gradient strength at 383 K. Black circles represent experimental data points and red lines represent (AC; E) single or (D) double exponential fits of the data to the Stejskal-Tanner equation.

[0054] Fig.11 Shown by 7 Lithium diffusion measured by Li pulsed field gradient nuclear magnetic resonance (PFG NMR) spectroscopy. 6.3 Nb 16 W5W 55 and Li x Nb 18 W 16 O 93 The lithium diffusion coefficients (x = 3.4, 6.8, 10.2) were measured in the temperature range 333-453 K. 6.3 Nb 16 W5W 55 The solid symbols (85% signal contribution) and open symbols (15% signal contribution) correspond to the observed two-component diffusion.

[0055] Fig.12 Shown are (A) the relative change in lithium diffusion as a function of open circuit voltage (Voc), and (B) open circuit voltage versus closed circuit voltage (Vcc) from constant current intermittent titration technique (GITT) measurements, showing the “thermodynamic” electrochemical curve at a C / 20 rate with a 12-hour rest period at each point, reaching full discharge in approximately one month.

[0056] Figure 13 shows (A) the Nb content of this work compared with the high-rate electrode formulations in the literature. 16 W5W 55 and Nb 18 W 16 O 93 The volumetric capacities at 1C and 20C were determined based on the reported capacities and the reported, measured, or estimated tap densities. (B) Ragone (log-log) plot of energy density and power density based on the anode active material versus the cathode at 4.0V. Here, the mass loading of niobium tungsten oxide is 2.6 mg cm -2, the mass loading of other titanium and niobium-based materials is usually about 1 mg cm -2 Graphite was included as a reference, although it cannot be used for high rate applications due to lithium plating risks and particle breakage. Literature values ​​for the Ragone plot were extracted using WebPlotDigitizer.

[0057] Fig.14 Theoretical volumetric capacities, assuming one electron reaction per transition metal, and crystallographic (single crystal) densities are shown. 12 The well-established reaction of Li4T i5 O 12 The capacity of graphite is based on the reaction of one electron per C6 unit.

[0058] Fig.15 It shows that Nb2Mo3O 14 Capacity vs. cycle number at 0.05C and relative to Li + / Li is 1.0 to 3.0V.

[0059] Fig.16 It shows that Nb2Mo3O 14 Discharge and charge voltage curves in three different voltage windows (1.0 V, 1.2 V, and 1.4 V). The discharge and charge curves were normalized to the gravimetric capacity; at 200 mA·h·g -1 The order of the curves below: 1.4V charge curve (top); 1.2V charge curve (second from the top); 1.0V charge curve (third from the top); 1.2V discharge curve (third from the bottom); 1.0V discharge curve and 1.4V discharge curve (overlap; bottom).

[0060] Figure 17 shows the relationship between Li / Li + (A) NMC622(LiNi 0.6 Co 0.2 Mn 0.2 O2), (B) LiFePO4 and (C) LiMn2O4 discharge and charge voltage curves.

[0061] Fig.18 Compared with Nb 16 W5W 55 and the capacities at different charge and discharge rates for different separators, binders, binder amounts, conductive carbon types, and electrodes with electrode calendaring.

[0062] FIG. 19 shows a diagram including Nb 16 W5W 55The discharge and charge voltage curves of the full cell with (A) LiFePO4 anode, (B) LiMn2O4 and (C) NMC622 cathode. 16 W5W 55 Rate performance of cells with NMC622 anode and NMC622 cathode; order of curves in (E): capacity (top, sloping); Coulombic efficiency (lower, horizontal).

[0063] FIG. 20 shows (A) a 16 W5W 55 Long-term cycling of a cell with a NMC622 anode and NMC622 cathode at 1C charge and discharge rates; capacity (ramp); coulombic efficiency (horizontal). (B) shows the extracted NMC622 electrode relative to Li + / Li performance. (C) shows the extracted electrode relative to Li + / Li performance.

[0064] FIG. 21 shows (A) Nb at ratios of 7:3, 1:1, and 3:7 normalized to gravimetric capacity. 16 W5W 55 -Charge and discharge curves of LTO blends, order of charge curves at 3.0V: 3:7 (leftmost), 5:5 (second from the left), 7:3 (rightmost); order of discharge curves at 1.0V: 3:7 (leftmost), 5:5 (second from the left), and 7:3 (rightmost). (B) Rate performance of blends, order at 0.2C: 7:3 (top), 5:5 (second from the top), 3:7 (bottommost). (C) Long-term cycling performance at 10C charge and discharge rates, 1C point: 7:3 (topmost), 5:5 (second from the top), 3:7 (bottommost); 10C curve: 3:7 (topmost), 5:5 (second from the top), 7:3 (bottommost).

[0065] FIG. 22 shows (A) a 3:7 (Nb 16 W5W 55 (A) Charge and discharge curves of a full cell with LTO anode and NMC622 cathode, and (B) the rate performance of the cell. DETAILED DESCRIPTION

[0066] The present invention generally provides an electrode comprising niobium tungsten oxide, an electrochemical cell comprising the electrode, and use of the cell in a lithium ion battery during charge and / or discharge at high charge and discharge rates (C-rates), such as 5C.

[0067] Nb 16 W5W 55The preparation of Nb has been previously described by Roth and Wadsley et al. 18 W 16 O 93 The preparation of Nb was previously described by Stephensen et al. However, these papers did not describe 16 W5W 55 and Nb 18 W 16 O 93 electrochemical properties.

[0068] Contains Nb8W9O 47 (Montemayor et al.); Nb 26 W4O 77 (Fuentes et al.); Nb 14 W3O 44 (Fuentes et al.); and Nb x W 1-x O 3-x / 2 Electrodes with 0≤x≤0.25 (Yamada et al.) have been described previously. However, the ability of the material to resist the charge-discharge rate (C-rate) was not measured.

[0069] Cruz et al. have described the inclusion of Nb 8-x W 9-x O 47 Electrodes with 1≤x≤6. However, electrochemical cells including the electrodes have been used under limited conditions, and no cells operating under high rate conditions have been disclosed. In addition, the authors report that irreversible structural transformations in the matrix-host lead to a loss of capacity after the first cycle.

[0070] Saritha et al. and Yan et al. have described Nb 12 WO 33 The electrode was used in the experiment. Yan et al. 1 (corresponding to a charge and discharge rate of 3.6C) 12 WO 33 Electrochemical cells containing Nb electrodes were tested by Saritha et al. at charge and discharge rates reported not exceeding 20C. 12 WO 33 electrochemical cell.

[0071] However, Saritha et al. apparently defined the charge / discharge rate as the reaction (i.e., removal or insertion) of one lithium ion per hour. This is equivalent to one electron transfer per formula unit. Therefore, using the law defined in this work, the Nb reported by Saritha et al. 12 WO 33The 20C rate corresponds to 1.54C (equivalent to 294mA·g -1 ).

[0072] The present inventors have developed an electrode comprising niobium tungsten oxide having favorable lithium ion diffusion properties, thus exhibiting excellent performance even for micron-sized particles. The electrode exhibits extremely high volumetric energy density and high capacity at high charge and discharge rates.

[0073] As is common in the art, the voltage values ​​described herein refer to Li + / Li to determine.

[0074] The charge / discharge rate is a measure of the rate at which a battery is discharged relative to its maximum capacity. The charge / discharge rate can be defined as the reciprocal of the number of hours to reach a defined theoretical capacity, e.g. 10C corresponds to 6 minutes of discharge or charge time. In this work, the charge / discharge rate is defined relative to one electron transfer per transition metal, e.g. for Nb 16 W5W 55 , 1C = 171.3 mA·h·g -1 , 20C=3426mA·h·g -1 The theoretical capacity is calculated by the following formula:

[0075]

[0076] Where n is the number of electrons transferred per formula unit, F is the Faraday constant, and 3.6 is the difference between coulombs and the conventional mA·h·g –1 , and m is the mass of each formula unit. Thus, 1C rate corresponds to each Nb in one hour. 16 W5W 55 The material can react (i.e., insert or remove) 21 lithium ions per formula unit because the material contains 21 transition metals per formula unit.

[0077] High rate applications may also be described with reference to the (gravimetric) current density, e.g. where the current density is at least 800 mA g -1 or 1000mA·g -1 The relationship between current density and charge and discharge rate is as follows:

[0078]

[0079] Therefore, for Nb 16 W5W 55 , using the law defined in this work, the current density is 800 mA g -1 Corresponding to a charge and discharge rate of 4.67C, and for Nb 18 W 16 O 93, current density is 800mA·g -1 This corresponds to a charge and discharge rate of 5.36C.

[0080] All (gravimetric) capacities are quoted based on the mass of active electrode material.

[0081] Working electrode

[0082] The present invention provides a working electrode comprising niobium tungsten oxide. The working electrode is electrically conductive and can be electrically connected to a counter electrode, such as in an electrochemical cell.

[0083] During the discharge step, for example in a lithium ion battery, the working electrode can be the anode or the cathode. Typically, the working electrode is the anode during the discharge step.

[0084] Typically, the working electrode used in the method comprises Nb2O5 and WO3 in a molar ratio of 6:1 to 1:15. Preferably, the molar ratio of Nb2O5 to WO3 in the working electrode is 8:5 to 11:20.

[0085] Typically, the working electrode used in this method comprises a Nb 12 WO 33 , Nb 26 W4O 77 , Nb 14 W3O 44 , Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 , Nb 22 W 20 O 115 、Nb8W9O 47 , Nb 54 W 82 O 381 , Nb 20 W 31 O 143 、Nb4W7O 31 or Nb2W 15 O 50 Or a combination thereof. Preferably, the working electrode comprises Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 or Nb 22 W 20 O115 or a combination thereof.

[0086] Typically, the molar ratio of Nb2O5 to WO3 in the working electrode is 8:5 to 11:20. Preferably, the molar ratio of Nb2O5 to WO3 in the working electrode is 8:5 or 9:16.

[0087] Typically, the working electrode comprises Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 or Nb 22 W 20 O 115 Or a combination thereof. Preferably, the working electrode comprises Nb 16 W5W 55 or Nb 18 W 16 O 93 or a combination thereof.

[0088] Optionally, the working electrode comprises a mixture of niobium tungsten oxide and an additional active material. The additional active material may be an additional metal oxide. For example, the working electrode may comprise a mixture of niobium tungsten oxide and an additional active material selected from lithium titanate (LTO; Li4Ti5O 12 ), titanium niobium oxide (such as TiNb2O7), titanium tantalum oxide (such as TiTa2O7), tantalum molybdenum oxide (such as Ta8W9O 47 ) and niobium molybdenum oxides (e.g. Nb2Mo3O 14 ).

[0089] Graphite may also be used as an additional active material. Working electrodes comprising a mixture of niobium tungsten oxide and graphite are relatively inexpensive to produce while maintaining the beneficial properties outlined above.

[0090] Preferably, the working electrode comprises a mixture of niobium tungsten oxide and LTO. The ratio of niobium tungsten oxide to LTO may be 95:5 to 5:95 by weight. For example, the ratio may be 90:10 to 10:90 by weight, 80:20 to 20:80 by weight, 70:30 to 30:70 by weight, 60:40 to 40:60 by weight, or the ratio of niobium tungsten oxide to LTO may be 1:1 by weight.

[0091] Preferably, the working electrode consists essentially of niobium tungsten oxide and the additional active material. For example, the working electrode consists essentially of a mixture of niobium tungsten oxide and LTO.

[0092] Typically, the working electrode does not have a porous structure or a layered structure. For example, the electrode material may have a structure less than 20 m 2 ·g -1 , less than 10m 2 ·g -1 , less than 5m 2 ·g -1 , less than 3m 2 ·g -1 , less than 2m 2 ·g -1 or less than 1m 2 ·g -1 Specific surface area.

[0093] The specific surface area of ​​the electrode material may be known or may be determined using standard techniques, such as N2 adsorption isotherm analysis and the Brunauer-Emmett-Teller (BET) theory.

[0094] Alternatively, the working electrode may have a porous structure. For example, the working electrode may have at least 50 m 2 ·g -1 , at least 60m 2 ·g -1 、70m 2 ·g -1 、80m 2 ·g -1 、90m 2 ·g -1 、100m 2 ·g -1 、150m 2 ·g -1 、200m 2 ·g -1 、300m 2 ·g -1 or 400m 2 ·g -1 Specific surface area.

[0095] The working electrode may have a thickness of at least 0.1 cm 3 ·g -1 , at least 0.2cm 3 ·g -1 , at least 0.4cm 3 ·g -1 , at least 0.5cm 3 ·g -1 , at least 0.7cm 3 ·g -1 , at least 0.8cm 3 ·g -1 , at least 0.9cm 3 ·g-1 , at least 1.0cm 3 ·g -1 , at least 1.5cm 3 ·g -1 or at least 2.0cm 3 ·g -1 of pore volume.

[0096] The pore volume of the electrode material may be known or may be determined using standard techniques such as N2 adsorption isotherm analysis and Barrett-Joyner-Halenda (BJH) theory.

[0097] The porous working electrode can have an average pore size (largest cross section) of at least 1 nm, at least 5 nm, at least 10 nm, at least 20 nm, at least 30 nm, at least 40 nm, at least 50 nm, or at least 100 nm.

[0098] The porous working electrode may have a macroporous structure. Thus, the porous working electrode may comprise pores having a maximum cross-section of at least 200 nm, at least 500 nm, at least 1 μm or at least 5 μm.

[0099] The pore size of the electrode material may be known or may be determined using standard techniques such as scanning electron microscopy (SEM).

[0100] The working electrode may additionally comprise porous carbon, such as porous reduced graphene oxide.

[0101] Electrodes containing porous carbon are generally light and conductive, and can provide a large pore volume, which can allow rapid transport of lithium ions and electrons to the active material. They can also increase the electrochemical capacity of a working device.

[0102] The working electrode may additionally comprise reduced graphene oxide, Ketjen black or Super P carbon.

[0103] Alternatively, the working electrode may have a layered structure. For example, the working electrode may further include layered reduced graphene oxide (rGO).

[0104] Typically, the working electrode comprises niobium tungsten oxide in particle form.The size of the niobium tungsten oxide particles of the working electrode may be known or it may be determined using standard techniques such as SEM.

[0105] Typically, the primary particle size of the niobium tungsten oxide particles of the working electrode is at least 1 μm. The primary particle size is the size of a single crystallite. It is the smallest identifiable subdivision in a particle system. For example, the primary particle size of the niobium tungsten oxide particles is at least 2 μm, 3 μm, 4 μm, 5 μm or 10 μm.

[0106] Individual niobium tungsten oxide particles may agglomerate to form secondary particles. Typically, the agglomerate (secondary) particle size of the niobium tungsten oxide particles is at least 5 μm. More preferably, the agglomerate particle size of the niobium tungsten oxide is at least 10 μm, 15 μm, 20 μm, 25 μm or 30 μm.

[0107] When present, the additional active material may be in the form of particles.The size of the additional active material particles may be known or may be determined using standard techniques such as SEM.

[0108] Preferably, the primary particle size of the additional active material particles is 1 μm or less. For example, the primary particle size of the additional active material particles is 800 nm or less, 750 nm or less, 700 nm or less, 600 nm or less, 500 nm or less, 400 nm or less, 300 nm or less, 200 nm or less or 150 nm or less. The particulate lithium titanate generally has a particle size within this range.

[0109] The electrode comprising the mixture of niobium tungsten oxide and the additional active material having a part size within the above range can be charged and discharged at very high charge and discharge rates and very high charge density.

[0110] To improve the conductivity on the working electrode, a conductive carbon material (e.g., carbon black, graphite, nanoparticle carbon powder, carbon fiber and / or carbon nanotube) is typically mixed with the working electrode material. Alternatively, the conductive carbon material can be coated on the working electrode material. In one embodiment, the working electrode includes porous carbon, such as porous reduced graphene oxide, which can encapsulate larger niobium oxide particles.

[0111] Typically, the working electrode contains 1-5 wt% binder.

[0112] The electrode may consist essentially of niobium tungsten oxide.

[0113] Alternatively, the working electrode is mixed with a binder or adhesive. Some examples of binders or adhesives include PVDF, PTFE, CMC, PAA, PMMA, PEO, SBR and copolymers thereof.

[0114] The working electrode is typically affixed to a current collector, such as a copper or aluminum current collector, which may be in the form of a plate.

[0115] The inventors used a lithium counter electrode with a geometry corresponding to that of a 2032-type button cell and used 1.0 M LiPF6 in ethylene carbonate / dimethyl carbonate as the electrolyte with a capacity of 2-3 mg·cm 2 of active material loading and 1.27cm 2The electrode area evaluated was a standard electrode configuration of 8:1:1 active material / carbon / binder including particulate niobium tungsten oxide as the working electrode.

[0116] Under these conditions, the inventors found that a working electrode comprising niobium tungsten oxide could sustain up to 150 mA·h·g at 10C. -1 The capacity is used for 1000 cycles and can sustain up to 125 mA·h·g at 20C. -1 The capacity is for 750 cycles.

[0117] Additionally, the inventors have discovered that a working electrode comprising niobium tungsten oxide has a sloped rather than a flat voltage curve.

[0118] The inventors have evaluated the solid-state lithium diffusion in niobium tungsten oxide using pulsed field gradient NMR (PFG NMR) and constant current intermittent titration technique (GITT). The inventors have found that the solid-state lithium diffusion coefficient (D) of niobium tungsten oxide at 298K is Li ) is 10 -13 Up to 10 -12 m 2 ·s -1 This corresponds to a characteristic diffusion length of about 10 μm for a 1-min discharge.

[0119] The present invention also provides a working electrode comprising niobium molybdenum oxide. The working electrode is electrically conductive and can be electrically connected to a counter electrode, such as in an electrochemical cell.

[0120] During the discharge step, for example in a lithium ion battery, the working electrode can be the anode or the cathode. Typically, the working electrode is the anode during the discharge step.

[0121] Typically, the working electrode used in the method comprises Nb2O5 and MoO3 in a molar ratio of 6:1 to 1:3. Preferably, the molar ratio of Nb2O5 to MoO3 in the working electrode is 1:3.

[0122] Typically, the working electrode used in this method comprises a Nb2Mo3O 14 , Nb 14 Mo3O 44 or Nb 12 MoO 44 Preferably, the working electrode comprises Nb2Mo3O 14 .

[0123] Typically, the working electrode does not have a porous structure or a layered structure. As described above, the working electrode may have a specific surface area, a pore volume, and an average pore diameter.

[0124] Typically, the working electrode comprises niobium molybdenum oxide in particle form. As described above, the niobium molybdenum oxide particles of the working electrode may have a primary or agglomerated particle size.

[0125] As described above, the working electrode may include a binder and a bonding agent.

[0126] Electrochemical Cells

[0127] The invention also provides an electrochemical cell comprising a working electrode of the invention. During the discharge step, for example in a lithium ion battery, the working electrode may be an anode or a cathode. Typically, the working electrode is an anode during the discharge step.

[0128] An electrochemical cell generally includes a counter electrode and an electrolyte. An electrochemical cell may include a current collecting plate. An electrochemical cell may be electrically connected to a power source. An electrochemical cell may be electrically connected to a measuring device, such as an ammeter or a voltmeter.

[0129] During the discharge step, for example in a lithium ion battery, the counter electrode can be the anode or the cathode. During the discharge step, the counter electrode is typically the cathode.

[0130] Suitable cathode materials include lithium-containing or lithium-intercalating materials such as lithium metal oxides, where the metal is typically a transition metal such as Co, Fe, Ni, V or Mn, or a combination thereof. Some examples of positive electrode materials include lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt oxide (NMC, LiNiMnCoO2, such as LiNi 0.6 Co 0.2 Mn 0.2 O2), lithium vanadium fluorophosphate (LiVPO4F), lithium nickel cobalt aluminum oxide (NCA, LiNiCoAlO2), lithium iron phosphate (LFP, LiFePO4), and manganese-based spinels (such as LiMn2O4).

[0131] To improve conductivity at the counter electrode, a conductive carbon material (eg, carbon black, graphite, nanoparticle carbon powder, or carbon nanotubes) is typically mixed with the counter electrode material. In one embodiment, the counter electrode comprises porous carbon, such as porous reduced graphene oxide.

[0132] In one embodiment, the counter electrode is substantially free of binder.

[0133] In an alternative embodiment, the counter electrode is mixed with a binder or adhesive. Some examples of binders or adhesives include PVDF, PTFE, CMC, PAA, PMMA, PEO, SBR and copolymers thereof.

[0134] The counter electrode is usually fixed to a current collecting substrate, such as an aluminum plate.

[0135] Typically, the electrolyte in an electrochemical cell is suitable for dissolving lithium ions.

[0136] Typically, the electrolyte in a battery that is charged and discharged contains lithium ions.

[0137] Typically, the electrolyte comprises a lithium salt such as LiTFSI, (lithium bis(trifluoromethane)sulfonyl imide, LiPF6, LiBF4, LiClO4, LiTF (lithium trifluoromethanesulfonate) or lithium bis(oxalato)borate (LiBOB).

[0138] The electrolyte may be a liquid electrolyte, for example a liquid at ambient temperature, for example 25°C.

[0139] The electrolyte may be a non-aqueous electrolyte. The electrolyte may include a polar aprotic solvent. The electrolyte may include an organic solvent. Solvents that dissolve lithium ions are well known in the art.

[0140] Suitable solvents include carbonate solvents, such as propylene carbonate (PC), ethylene carbonate (EC), butylene carbonate (BC), vinyl chloride carbonate, fluorocarbonate solvents (e.g., ethylene fluorocarbonate and trifluoromethyl propylene carbonate), and dialkyl carbonate solvents, such as dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), and ethyl propyl carbonate (EPC).

[0141] Suitable solvents also include sulfone solvents. For example, methyl sulfone, ethyl methyl sulfone, methyl phenyl sulfone, methyl isopropyl sulfone (MiPS), propyl sulfone, butyl sulfone, tetramethylene sulfone (cyclopentane sulfone), phenyl vinyl sulfone, allyl methyl sulfone, methyl vinyl sulfone, divinyl sulfone (vinyl sulfone), diphenyl sulfone (phenyl sulfone), dibenzyl sulfone (benzyl sulfone), vinylidene sulfone, butadiene sulfone, 4-methoxyphenyl methyl sulfone, 4-chlorophenyl methyl sulfone, 2-chlorophenyl methyl sulfone, 3,4-dichlorophenyl methyl sulfone, 4-(methylsulfonyl) toluene, 2-(methylsulfonyl) ethanol, 4-bromophenyl methyl sulfone, 2-bromophenyl methyl sulfone, 4-fluorophenyl methyl sulfone, 2-fluorophenyl methyl sulfone, 4-aminophenyl methyl sulfone, sultone (for example 1,3-propane sultone) and ether-containing sulfone solvents (for example, 2-methoxyethyl (methyl) sulfone and 2-methoxyethoxyethyl (ethyl) sulfone).

[0142] Suitable solvents also include silicon-containing solvents such as siloxanes or silanes. Examples include hexamethyldisiloxane (HMDS), 1,3-divinyltetramethyldisiloxane, polysiloxanes, and polysiloxane-polyoxyalkylene derivatives. Some examples of silane solvents include methoxytrimethylsilane, ethoxytrimethylsilane, dimethoxydimethylsilane, methyltrimethoxysilane, and 2-(ethoxy)ethoxytrimethylsilane.

[0143] Generally, additives may be included in the electrolyte to improve performance. For example, vinylene carbonate (VC), vinyl carbonate, allyl ethyl carbonate, tert-butylene carbonate, vinyl acetate, divinyl adipate, acrylic nitrile, 2-vinyl pyridine, maleic anhydride, methyl cinnamate, vinyl carbonate, halogenated vinyl carbonate, α-bromo-γ-butyrolactone, methyl chloroformate, 1,3-propane sultone, vinyl sulfite (ES), propylene sulfite (PS), vinylene sulfite (VES), fluoroethylene sulfite (FES), 12-crown-4 ether, carbon dioxide (CO2), sulfur dioxide (SO2) and sulfur trioxide (SO3).

[0144] The electrochemical cell may also include a solid porous membrane between the negative electrode and the positive electrode. The solid porous membrane may partially or completely replace the liquid electrolyte. The solid porous membrane may comprise a polymer (e.g., polyethylene, polypropylene, or a copolymer thereof) or an inorganic material, such as a transition metal oxide (e.g., titanium dioxide, zirconium oxide, yttrium oxide, hafnium dioxide, or niobium oxide) or a main group metal oxide, such as silicon oxide, which may be in the form of glass fibers.

[0145] Solid nonporous membranes may include lithium ion conductors such as LLZO (garnet series), LSPO (lithium zinc germanate series), LGPS (lithium zinc sulfide-germanate series), LATP / LAGP (sodium superionic conductor series), LLTO (perovskite series), and phosphide / sulfide glass ceramics.

[0146] The electrochemical cell can be charged or discharged at a charge and discharge rate of at least 5 C relative to one electron transfer per transition metal per formula unit of the working electrode material, for example, the electrochemical cell can be charged or discharged at a charge and discharge rate of at least 5 C. Preferably, the electrochemical cell can be charged or discharged at a charge and discharge rate of at least 10 C, 15 C, 20 C, 25 C, 30 C, 35 C, 40 C, 50 C, 60 C or 80 C.

[0147] Electrochemical cells can deliver at least 750 mA g -1 Preferably, the electrochemical cell can be charged or discharged at a current density of at least 800 mA g -1 、850mA·g -1 , 900mA·g -1 , 950mA·g -1 , 1000mA·g -1 , 1050mA·g -1 , 1100mA·g -1 , 1200mA·g -1 or 1300mA·g -1 The current density is charged or discharged.

[0148] The electrochemical cell may have a current of at least 200, 300, 400, 500, 600, or 700 A·h·L at 1C. -1 Typically, electrochemical cells have a volume charge density of up to 100, 200, 300, or 400 A·h·L at 20C. -1 The volume charge density of .

[0149] The electrochemical cell can have a capacity retention of at least 70%, 75%, 80%, 85%, 90%, 95%, 96%, 97%, 98%, 99% or 100% at 20C for at least 50, 100, 150, 200, 250, 300, 400, 500, 600, 700, 800, 900, 1,000, 1,200, 1,500, 1,800 or 2,000 cycles.

[0150] An electrochemical cell can be considered fully charged when the voltage passes a threshold. For example, when the voltage rises above a practical level, such as when the voltage is above a certain level relative to Li / Li + When raised above 2.0 V (eg, above 2.25 V or above 2.5 V), the electrochemical cell including a lithium metal anode and a niobium tungsten oxide cathode can be considered fully charged.

[0151] An electrochemical cell can be considered fully discharged when the voltage passes a threshold. For example, when the voltage drops below a practical level, such as when the voltage relative to Li / Li + An electrochemical cell including a lithium metal anode and a niobium tungsten oxide cathode may be considered fully discharged when the voltage drops below 1.5 V (eg, below 1.25 V or below 1.0 V).

[0152] The electrochemical cell may be a lithium ion cell.

[0153] method

[0154] The present invention provides a method for charging and / or discharging an electrochemical cell at a charge and discharge rate of at least 5C, for example, the electrochemical cell can be charged or discharged at a charge and discharge rate of at least 5C relative to one electron transfer per transition metal per formula unit of working electrode material. The electrochemical cell includes a working electrode, the working electrode including niobium tungsten oxide and / or niobium molybdenum oxide. Preferably, the electrochemical cell includes a counter electrode and an electrolyte.

[0155] Preferably, the method is a method of charging and / or discharging an electrochemical cell at a charge and discharge rate of at least 10C, 15C, 20C, 25C, 30C, 35C, 40C, 50C, 60C or 80C.

[0156] The method may be carried out at a rate of at least 750 mA·g-1 , for example at least 800 mA g -1 Preferably, the method is to charge and / or discharge an electrochemical cell at a current density of at least 800 mA g -1 , 850mA g -1 , 900mA·g -1 , 950mA·g -1 , 1000mA·g -1 , 1050mA·g -1 , 1100mA·g -1 , 1200mA·g -1 or 1300mA·g -1 A method for charging and / or discharging an electrochemical cell at a current density of 1000 Å.

[0157] The method may include cycles of charging and discharging, or discharging and charging, the electrochemical cell. The cycle may be repeated more than once. Thus, the method includes 2 or more cycles, 5 or more cycles, 10 or more cycles, 50 or more cycles, 100 or more cycles, 500 or more cycles, 1,000 or more cycles, or 2,000 or more cycles.

[0158] Battery

[0159] The present invention also provides a battery comprising one or more electrochemical cells of the present invention. The battery may be a lithium ion battery.

[0160] Where there are multiple batteries, the batteries may be arranged in series or in parallel.

[0161] The battery of the present invention may be arranged in a road vehicle, such as a car, moped or truck. Alternatively, the battery of the present invention may be arranged in a rail vehicle such as a train or tram. The battery of the present invention may also be arranged in an electric bicycle (ebike).

[0162] The battery of the present invention may be provided in a regenerative braking system.

[0163] The battery of the present invention may be provided in a portable electronic device such as a mobile phone, a notebook computer or a tablet computer.

[0164] The battery of the present invention may be provided in a power management system.

[0165] use

[0166] The present invention generally provides the use of a working electrode comprising niobium tungsten oxide in a high rate electrochemical cell (e.g., an electrochemical cell as described herein). Typically, the electrochemical cell can be charged or discharged at a charge and discharge rate of at least 5C relative to one electron transfer per transition metal per formula unit of the working electrode material, for example, the electrochemical cell can be charged or discharged at a charge and discharge rate of at least 5C. Preferably, the electrochemical cell can be charged or discharged at a charge and discharge rate of at least 10C, 15C, 20C, 25C, 30C, 35C, 40C, 50C, 60C, or 80C.

[0167] Electrochemical cells can deliver at least 750 mA g -1 Preferably, the electrochemical cell can be charged or discharged at a current density of at least 800 mA g -1 、850mA·g -1 , 900mA·g -1 , 950mA·g -1 , 1000mA·g -1 , 1050mA·g -1 , 1100mA·g -1 , 1200mA·g -1 or 1300mA·g -1 The current density is charged or discharged.

[0168] A working electrode may find use in the methods described herein.

[0169] Other options

[0170] Each and every compatible combination of the embodiments described above is expressly disclosed herein, as if each and every combination were individually and expressly recited.

[0171] Various other aspects and embodiments of the present invention will be apparent to those skilled in the art in view of the present disclosure.

[0172] As used herein, "and / or" is considered to be a specific disclosure of each of the two indicated features or components with or without the other. For example, "A and / or B" is considered to be a specific disclosure of each of (i) A, (ii) B, and (iii) A and B, just as each is individually set forth herein.

[0173] Unless the context dictates otherwise, the descriptions and definitions of the features above are not limited to any particular aspect or embodiment of the invention, and apply equally to all aspects and embodiments described.

[0174] Certain aspects and embodiments of the invention will now be described by way of example and with reference to the above-described drawings.

[0175] experiment

[0176] The following examples are provided merely to illustrate the present invention and are not intended to limit the scope of the invention, as described herein.

[0177] Nb 16 W5W 55 and Nb 18 W 16 O 93 Synthesis

[0178] Nb 16 W5W 55 and Nb 18 W 16 O 93 Synthesized by co-thermal oxidation of dark blue NbO2 (Alfa Aesar, 99+%) and brown WO2 (Alfa Aesar, 99.9%) in approximately one to five gram batches. The partially reduced oxides were quantified to within 0.001 g of a 16:5 or 18:16 molar ratio, hand-ground with an agate mortar and pestle, pressed into pellets at 10 MPa, and heated in a platinum crucible at 10 K min -1 The sample was heated to 1473 K at a rate of 1.25 °C and cooled naturally in the furnace over about 2 h.

[0179] oeLh 47 and Nb 12 WO 33 Synthesis

[0180] oeLh 47 and Nb 12 WO 33 Synthesized by co-thermal oxidation of dark blue NbO2 (Alfa Aesar, 99+%) and brown WO2 (Alfa Aesar, 99.9%) in approximately one to five gram batches. The partially reduced oxides were quantified to within 0.001 g of a molar ratio of 8:9 or 12:1, hand-ground with an agate mortar and pestle, pressed into pellets at 10 MPa, and heated in a platinum crucible at 10 K min -1 The sample was heated to 1473 K at a rate of 1.25 °C and cooled naturally in the furnace over about 2 h.

[0181] Nb2Mo3O 14 Synthesis

[0182] Nb2Mo3O 14It is synthesized by co-thermal oxidation of dark blue NbO2 (Alfa Aesar, 99+%) and dark brown MoO2 (Sigma, 99%), or co-thermal oxidation of white Nb2O5 (Sigma, 99.9985%) and pale white MoO3 (Sigma, ≥99.5%) in batches of about one to five grams. The partially reduced oxides are quantified to within 0.001 g of a 2:3 or 1:3 molar ratio, ground by hand with an agate mortar and pestle, pressed into pellets at 10 MPa, and heated in a platinum or alumina crucible at 10 K min -1 The samples were heated to 873K, 923K or 973K at a rate of 1000 K and quenched on a metal plate outside the furnace in air.

[0183] Microscopic characterization

[0184] Scanning electron microscopy (SEM) images were taken using a Σigma VP instrument (Zeiss) at 3.0 kV and a MIRA3 instrument (TESCAN) at 5.0 kV using secondary electron detection. Tap density was recorded at 257 taps min -1 Tap density was measured according to ASTM International Standard B527-15, modified to accommodate 5 to 10 cm 3 of measuring cylinder.

[0185] Nb 16 W5W 55 and Nb 18 W 16 O 93 Both form semi-shaped particles with primary particles of about 3 to 10 μm, which appear to grow / "glue" into larger secondary particles of about 10 to 30 μm in electron microscopy (Figures 1 and 2). The bulk compound is a series of complex "blocks" (Nb 16 W5W 55 ) or "bronze" (Nb 18 W 16 O 93 )Oxide structure( Figure 2 ), which is mainly composed of corner- and edge-sharing NbO6 and WO6 octahedra.

[0186] Nb 16 W5W 55 It has a monoclinic structure consisting of corner-sharing octahedral subunits arranged in ReO3-like blocks, four octahedra wide by five octahedra long, infinite in the third dimension ( Figure 2 A). The block subunits are connected by crystal shear planes along the edges and tetrahedra at each corner, resulting in the notation (4×5)1, where in (m×n)p In the equation, m and n represent the block length in units of octahedrons and p is related to the connectivity of the blocks, which can also be connected in pairs (p = 2) or in infinite bands (p = ∞).

[0187] Nb 18 W 16 O 93 It is an orthorhombic crystal system, which is the 1×3×1 upper structure of the classic tetragonal tungsten bronze (TTB) ( Figure 2 D and 3). The TTB structure is sometimes stabilized by cations (e.g., K+, Figure 3 partially filled spheres in the 18 W 16 O 93 Stabilized by -MO- chains, which partially occupy the tunnel and form a pentagonal bipyramid. The ionic and electronic meanings for lithium insertion are Nb 18 W 16 O 93 The layer is still completely open and unoccupied by cations (i.e., around the plane (x, y, 1 / 2)), and all metal cations are in the desired d 0 The electronic configuration is in the traditional TTB structure, and neither of these two criteria is met.

[0188] Nb 16 W5W 55 and Nb 18 W 16 O 93 Electrochemical characterization of

[0189] Electrochemical characterization was performed using stainless steel 2032 button cells with conical springs (Cambridge Energy Solutions), two 0.5 mm stainless steel diaphragms, plastic spacers, and glass microfiber diaphragms (Whatman). To form niobium tungsten oxide electrodes, niobium tungsten oxide and conductive carbon (Super P, TIMCAL) were manually ground in an agate mortar and pestle at a mass ratio of 8:1. The powder was ground with polyvinylidene fluoride (PVDF, Kynar) dispersed in N-methylpyrrolidone (NMP, Sigma-Aldrich, anhydrous, 99.5%) at a mass ratio of 9:1. The slurry was coated onto aluminum or copper foil with a scraper (rod coater). NMP was removed by heating in an oven at 60°C for 24 hours. Although a standard, Super P carbon is a nanoparticle powder and NMP is a hazardous organic solvent, so an appropriate nanoparticle cabinet / fume hood should be used.

[0190] The 80 / 10 / 10 metal oxide / carbon / polymer electrode served as cathode relative to a Li metal disc (LTS Research, 99.95%) anode in a half-cell geometry. In the electrochemical tests, the electrolyte was 1 M LiPF6 dissolved in 1:1 v / v ethylene carbonate / dimethyl carbonate (EC / DMC; Sigma-Aldrich, battery grade; also known as LP30). No additives were used. The electrochemistry was performed in a temperature controlled chamber at 293 K. Electrochemical measurements were performed using a Biologic galvanostat / potentiostat with EC-Lab software.

[0191] The current density test was 2 to 3 mg cm-1, which was equivalent to a discharge time of several hours to tens of seconds. -2 Dense electrodes with large particles of active material loading. Nb 16 W5W 55 The Nb 18 W 16 O 93 Cycle without this step and at 60C (i.e., within <60s) at 100mA·h·g -1 Both oxides were cycled at high rate for 1000 cycles at 10C / 20C constant current without any potentiostatic step.

[0192] Nb 16 W5W 55 Reaction with lithium ( Figure 4A ) in three regions from 2.5 V to 1.0 V, with an average voltage of 1.57 V (Figure 5), which is similar to that of Li4Ti5O 12 The average voltage is 1.55 V. The three regions that are more easily observed in the derivative plot ( Figure 4B ) is characterized by its slope and is reminiscent of other crystallographic shear structures (e.g., H-Nb2O5, PNb9O 25 , TiNb2O7 and Nb 12 WO 33 ) in the three regions observed in the C / 5 (34.3 mA·g -1 ) to 60C (10.3A·g -1 ) when examining the kinetics in the current density range, Nb 16 W5W 55 Demonstrating unprecedented volumetric rate performance ( Figure 4A and 4C ). At C / 5, each transition metal can reversibly insert about 1.3 lithium ions, with a gravimetric capacity of about 225 mA·h·g -1 When the rate increases 25 times to 5C, Nb16 W5W 55 Maintain 1.0Li + / TM(171mA·h·g -1 ) capacity. At 20C, it is equivalent to a discharge time of three minutes, and 0.86Li can still be exchanged. + / TM and access 148mA·h·g -1 In Nb 16 W5W 55 The rate tests on the 2000-volt FET were measured using a constant potential hold at the top of the charge to ensure a reliable discharge starting point. To test performance under more demanding conditions, 1000 cycles were measured using a fixed constant current discharge and 250 cycles were performed at 10C charge conditions followed by 750 cycles at 20C (no hold) ( Figure 4F ). Under these conditions, 0.90 Li was reversibly inserted at 10C. + / TM(average 155mA·h·g -1 ) 95% capacity retention after 250 cycles on an unoptimized or calendered electrode. At 20C, the capacity is 0.75Li + / TM(average 128mA·h·g -1 ); at 750 cycles at 20C, the capacity retention is again 95%.

[0193] Nb 18 W 16 O 93 The average voltage is 1.67V ( Figure 4D -F). In terms of gravimetric capacity, due to the higher molar mass of the tungsten-rich bronze phase, Nb 18 W 16 O 93 Storage: about 20mA·h·g -1 , less than Nb at C / 5 and 1C 16 W5W 55 However, at 20°C, Nb 18 W 16 O 93 Still able to accommodate a full cell of Li+ / TM for a capacity of about 150 mA·h·g -1 At 60C and 100C (14.9A·g –1 ) the capacities are still 105 and 70 mA·h·g respectively. -1 .

[0194] Comparison of Copper Foil and Carbon-Coated Aluminum Foil Current Collectors

[0195] Figure 6 shows the effect of the current collector, which cannot be ignored at high rates.

[0196] For Nb2O3 cycled for 1000 cycles under constant current discharge and charge at 10C / 20C 16 W5W 55 , Cu foil current collector shows higher capacity than carbon-coated Al (C@Al) foil ( Fig. 6A ). Untreated Al foil has been shown to be insufficient to achieve high current densities (Griffith et al.); C@Al shows significant improvement compared to untreated Al. 16 W5W 55 The lower voltage region is the source of excess capacity beyond 1.0 Li+ / TM at low rates, but effectively shifts below 1.0 V at moderate rates. Only in the dQ / dV plot is a second discharge peak (centered at 1.2 V) observed at C / 5 ( Figure 4B ). As a result, the capacity observed when cycling at a minimum voltage limit of 1.2 V versus 1.0 V becomes less critical with increasing rate, and safety can be further improved by avoiding lower voltages. Figure 6B The discharge and charge curves between 3.0 and 1.0 V for the 100th cycle at 1OC are shown.

[0197] Relationship between long-term cycling and minimum cut-off voltage

[0198] Figure 7 shows the effect of long term cycling at C / 5.

[0199] As in ( Fig. 7A ), constant current constant voltage charging is a common method to maximize capacity without overcharging, but the extra time required means that the cycle can be considered as C / 5 and 1C discharge, but C / 6 and C / 2 charge. For minimum voltages of 1.2 and 1.0V, Fig. 7A The 2nd to 50th cycle retention rates are 96% and 93%, respectively. The 51st to 100th cycles at 1C show that the capacity retention rates at 1.2V and 1.0V are 99% and 101%, respectively. For 1.1V, 1.0V and 0.9V, Figure 7B The cycle retention rates of the 2nd to 50th cycles of C / 5 in the embodiment are 88%, 90% and 40% respectively. The cycle time is about one month.

[0200] Overpotential in Li||Li symmetric cells as a function of current density

[0201] As a control, the Li||Li symmetric cell corresponds to Figure 4A -E( Figure 8) were cycled at current densities equal to those in ). The cell configuration was identical to that used for the metal oxide tests, except that a second Li disk replaced the composite electrode. Rate tests were performed at 100 μA (C / 5), 500 μA (1C), 1 mA (2C), 2.5 mA (5C), 5 mA (10C) for 5 cycles and at 10 mA (20C), 20 mA (40C), 30 mA (60C), and 50 mA (100C) for 10 cycles. The "rate" in parentheses indicates the reciprocal of the amount of time (in hours) that the current was applied to simulate the rate test. At low current densities (less than 1 mA (2C)), the overpotential was less than 100 mV; however, at 5 mA (10C), it rose to 200 mV and increased to approximately 700 mV at 100C.

[0202] The overpotential in a symmetric cell ( Figure 8 )and Figure 4A and 4D This suggests that the extremely high rates of bulk electrodes at room temperature are close to the limits of lithium metal plating / stripping and / or lithium ion desolvation and migration in carbonate electrolytes, i.e., a large portion of the ohmic drop seen during fast charging results from lithium metal rather than complex oxide electrode materials.

[0203] 7 Li pulsed field gradient NMR spectrum

[0204] Recorded on a Bruker Avance III 300 MHz spectrometer using a Diff50 probe equipped with extended variable temperature capability 7 Li NMR diffusion spectrum. Fig. 9 The spectra were recorded with the stimulated echo pulsed field gradient (PFG) sequence shown in to minimize spin-spin relaxation (T2) losses. After the first 90° radio frequency (rf) pulse, the net magnetization loses coherence due to T2 relaxation; therefore, the time period following this pulse, which includes the first PFG pulse (used to encode spin positions), must be shorter than T2. ​​In the stimulated echo sequence used here, a second 90° rf pulse is applied, which stores the net magnetization along the z-axis before the diffusion time Δ, so that the time for the observed material diffusion is commensurate with the relatively long spin lattice (T1) value because no T2 relaxation occurs. During Δ, a short spoiler gradient (SINE.100) is applied to eliminate residual transverse magnetization. Then, a third 90° rf pulse is applied, followed by a PFG pulse to decode the spin positions. A sufficiently long delay (≥0.5ms) is used between the PFG and rf pulses to minimize eddy currents in the diffusion measurement.

[0205] In this sequence, the gradient strength g varies from 0.87 to 1800 or 2300 G·cm -1 , and 16 gradient steps are obtained using an "opt" shaped pulse with 1024-4096 transients. The opt shape is a composite pulse that starts with a quarter of a sine wave, followed by a constant gradient, and ends with a ramp down ( Fig. 9 ). The “opt” gradient pulse provides the largest gradient integral over a given time period, thereby maximizing the range of diffusion coefficients that we can evaluate in this experiment.

[0206] The spectra were analyzed in phase-sensitive mode and the Stejskal-Tanner equation describes the response of the NMR signal intensity I to changes in g:

[0207]

[0208] where I0 is the intensity without gradient, γ is the gyromagnetic ratio (γ 7Li =103.962×10 6 ·s -1 ·T -1 ), δ is the effective gradient pulse duration, and D is the diffusion coefficient. Here, the NMR signal intensity and integral give similar 7 Li diffusivity, but the NMR signal intensity gives more reliable data as assessed by the standard deviation of the fit. Typical δ values ​​range from 0.8 ms to 1.5 ms for bronze and bulk phase samples, and Δ values ​​range from 50-100 ms.

[0209] Due to the increase in T2 observed at high temperatures (e.g., Li 3.4 Nb 18 W 16 O 93 The T2 of the spectral spectrum was about 700 μs at room temperature and 1.9 ms at 453 K, so the diffusion spectra were recorded at elevated temperatures (333-453 K). (Note that due to the use of a single-tuned 7 Li coils and conventionally have no reliable 7 The Li reference was used for temperature calibration, so no attempt was made to calibrate the temperature used for this experimental setup. The Bruker manual states that for static measurements, the temperature calibration should be within ±7 degrees of the set value.) The increase in T2 allows the use of longer gradient pulses δ, which are necessary for measuring diffusion coefficients in solid oxides.

[0210] Representative 7 The Li diffusion decay curve is shown in Fig.10 The data quality is related to the Li content and the subsequent 7 The Li NMR spectrum signal-to-noise ratio (SNR) is directly related to Fig.10A(Li 10.2 Nb 18 W 16 O 93 )、10B(Li 6.8 Nb 18 W 16 O 93 )、10C(Li 3.4 Nb 18 W 16 O 93 ) and 10D(Li 6.3 Nb 16 W5W 55 ) are 95, 56, 10, and 12, respectively. We note that although the low Li content Li 3.4 Nb 18 W 16 O 93 The SNR of the sample is low, and the signal attenuation is only about 60%. 7 The Li diffusion rate and activation energy trends are consistent with those observed in more lithiated bronze structures.

[0211] Li 6.3 Nb 16 W5W 55 The two-component behavior of lithium at 333 K is shown with a transport rate of up to 4.3 × 10 -12 m 2 ·s -1 ( Fig.11 ). Assuming Arrhenius behavior and a measured activation energy of 0.23 eV, the room temperature lithium diffusion coefficient is estimated to be 2.1 × 10 -12 m 2 ·s -1 (Table 1).

[0212] Li x Nb 18 W 16 O 93 (x=3.4, 6.8, 10.2) show similar diffusion and activation energies, and the room temperature diffusion coefficient is 1.1×10 -13 m 2 ·s -1 And E a In the range of 0.27 to 0.30 eV.

[0213] Table 1 - D of selected niobium tungsten oxide materials Li and E a Measurement

[0214]

[0215] In about 10 -16-10 -15 m 2 ·s -1 Under these conditions, lithium diffusion in the two niobium tungsten oxide structures is significantly faster than that in Li 4+x Ti5O 12 or Li x TiO2, and is close to the best-known lithium solid electrolytes (Table 2).

[0216] PFG NMR( Fig.11 ) The results show that the initial lithium ion diffusion is about 10 -12 Up to 10 -13 m 2 ·s -1 , while the galvanostatic intermittent titration technique (GITT) measures ( Fig.12 ) indicates that niobium tungsten oxide retains this rapid movement to high capacity (≥1.5Li + / TM), and then diffuses down about two orders of magnitude toward 2.0Li + This indicates that the intrinsic range of niobium tungsten oxide electrode materials for high-rate multi-redox extends to about 1.5Li + / TM. The diffusion coefficients measured for these materials are about 10 -12 Up to 10 -13 m 2 ·s -1 , consistent with the value required to achieve full lithiation of 6 to 19 μm particles on a 60 C timescale.

[0217] Table 2 - D of known materials Li Measurement

[0218]

[0219]

[0220] Abbreviations: bcc = body-centered cubic, μ+-SR = μ-meson spin resonance

[0221] Galvanostatic Intermittent Titration Technique (GITT)

[0222] In principle, information about electrode thermodynamics, including phase transitions and lithium kinetics, can be extracted from GITT measurements by following the voltage evolution after a brief current pulse as lithium diffuses and the chemical potential reaches equilibrium within the electrode / particle. However, it is difficult to extract reliable quantitative diffusion coefficients D from GITT alone. Li. In order to determine the diffusion coefficient from GITT measurements, the diffusion length (L) must be defined, but the battery electrode is a heterogeneous system. First, it is a composite of active material (here, metal oxide), porous carbon, and polymer binder. In such a composite, there will be a particle size distribution (unless single crystals or well-defined particles are used; even then, diffusion will vary with the lattice direction). In addition, due to the presence of solid / liquid interfaces and porous electrode structures, different diffusion modes must exist. However, in electrodes that have not undergone severe comminution (e.g., insertion electrodes), L is a fixed quantity throughout the experiment. Variations in L (the parameter that relates relaxation rate to diffusion) lead to variations in D Li The values ​​of also vary significantly between reports, even for the same material. Thus, while a physically meaningful diffusion coefficient may not be extracted, a relative measure of diffusion is readily obtained. We therefore use the extracted proxy for lithium diffusion (D Li ·L –2 , Fig.12 ), which eliminates the uncertainty in L and enables a self-consistent analysis of a single electrode and electrodes prepared under identical conditions. The addition of quantitative information from another method, such as NMR spectroscopy, allows us to + The relative changes in kinetics are calibrated to quantitative diffusion values ​​over the entire lithiation range.

[0223] like Fig.12 As shown, in Nb 16 W5W 55 From the dilution limit to Li 4.5(5) Nb 16 W5W 55 The diffusion is fastest when more than one Li + / TM in the low voltage window dropped by two orders of magnitude. GITT data show that Nb 16 W5W 55 The second electrochemical region of is broader than that usually observed for two-phase reactions, but the D Li ·L– 2 The discontinuity in the value of Nb indicates that it is approaching two-phase behavior. 18 W 16 O 93 The average diffusion coefficient in is similar to that of Nb 16 W5W 55 Bronze also shows discontinuities at 2.1, 1.85, and 1.7 V. In both stages, the low voltage region (below 1.25 V, well above 1 Li + / TM) are characterized by increased overpotential and suppressed kinetics.

[0224] Energy comparison diagram of anode materials (Ragone Plot)

[0225] Energy comparison graph of anode materials: The energy density of cathode materials is the product of capacity (Q) and voltage (V); however, this product does not work when comparing anode materials, as energy and voltage have an inverse relationship. In the calculations for the energy comparison graph of anode materials in Figure 13, energy (E) was calculated based on the voltage difference relative to the 4.0V cathode. Therefore, normalized to the anode, E 阳极 =(V 阴极 –V 阳极 )*Q 阳极 .

[0226] When compared strictly based on the theoretical 1.0 Li+ / TM reaction and the crystallographic density of the active materials, titanium dioxide, niobium oxide, and graphite all show theoretical charge densities greater than 800 A·h·L -1 ( Fig.14 Once the experimental capacity and tap density are taken into account ( Fig.13A ), the unoptimized bulk niobium tungsten oxide provided herein maintains greater than 500 A·h·L at 1C -1 The volume charge density can reach up to 400A·h·L at 20C. -1 , even the volumetric performance of the most optimized versions of TiO2, Nb2O5, LTO cannot be achieved. This is not to say that the presented compounds cannot be improved by methods such as nanostructuring, calendering or carbon coating, as demonstrated by e.g. Sun et al. using porous graphene scaffolds, but demonstrates that large micron-sized particles can be used for high-rate electrodes and illustrates that nanostructuring is not always the most appropriate strategy for improving performance. This is evident in the energy comparison diagram ( Fig. 13B ), which shows the higher energy density of the new bulk niobium tungsten oxide compared to the latest high-rate anode materials and graphite.

[0227] Commercial Materials - Half-Cell Testing

[0228] In addition, in order to test the applicability of niobium tungsten oxide as a high-rate anode material, a commercially available high-rate cathode material NMC622 (LiNi 0.6 Mn 0.2 Co 0.2 O2; Targray), lithium iron phosphate (LiFePO4; Johnson Matthey), and LiMn2O4 (MTI Corp). These commercial materials were first characterized in half-cell geometries resistant to lithium metal. Stainless steel 2032 button cells and glass microfiber separators were used to match the above-mentioned Nb 16 W5W 55 and Nb 18 W 16 O 93Electrochemical measurements were performed in the same manner. Commercial cathode materials, conductive carbon (Li-250 carbon; Deka Chemicals) and PVDF were ground together in the same manner as above to prepare an 80 / 10 / 10 electrode (containing 80 wt% active material, 10 wt% carbon and 10 wt% polymer), which was used as the cathode relative to the Li metal disk anode in a half-cell geometry. The electrolyte was 150 μL LP30. No additives were used.

[0229] Under these conditions, the NMC622 showed an average voltage of 3.8 V and an actual capacity of 175 mA·h·g -1 ( Fig.17A ). LiFePO4 shows an average voltage of 3.4V and an actual capacity of 165mA·h·g -1 ( Fig. 17B ), and LiMn2O4 shows an average voltage of 4.0V and an actual capacity of 120mA·h·g -1 ( Fig. 17C ).

[0230] Electrode Optimization-Nb 16 W5W 55

[0231] In order to optimize Nb 16 W5W 55 Electrode Performance A series of electrodes were fabricated according to the specifications listed in Table 3 below. Electrochemical characterization was performed using stainless steel 2032 button cells and glass microfiber separators as described previously. Li metal disks were used as anodes in half-cell geometry. The electrolyte was 150 μL LP30. No additives were used.

[0232] Table 3 - Electrode Optimization

[0233]

[0234] 1 Celgard; 2 Styrene-butadiene rubber (Zeon); 3 Carboxymethyl cellulose (Sigma Aldrich); 4 Carbon nanotubes (Sigma Aldrich)

[0235] In the case of 5wt% PVDF or 4wt% SRB and 1w% CMC as binder, it was confirmed that the volume ratio performance was improved ( Fig.18 ). Calendering can also continuously improve electrode performance.

[0236] Full cell operation using commercial electrode materials

[0237] To test the suitability of niobium tungsten oxide as a high-rate anode material, full cells were produced using commercially available high-rate cathode materials NMC622, LiFePO4, and LiMn2O4. Stainless steel 2032 button cells and glass microfiber separators were used to match the above-mentioned Nb 16 W5W 55 and Nb 18 W 16 O 93 Electrochemical measurements were performed in the same manner. Commercial cathode materials, Li-250 carbon, and PVDF were ground together as described above to prepare an 80 / 10 / 10 electrode (containing 80 wt% active material, 10 wt% carbon, and 10 wt% polymer), which was used as the cathode. 16 W5W 55 , Li-250 carbon and PVDF were ground together to prepare an 80 / 10 / 10 electrode (containing 80 wt% active material, 10 wt% carbon and 10 wt% polymer), which was used as the anode. When the cathode contained NMC622, the anode contained Nb in a ratio of 80 / 15 / 5. 16 W5W 55 , Li-250 carbon, and PVDF. In all cases, the electrolyte was 150 μL of LP30. No additives were used. The capacity ratio of the anode and cathode was 1:1. For full cell balancing, the theoretical capacity of NMC622 was taken as 175 mA·h·g -1 .

[0238] The full cells were evaluated between 1.0 and 3.0 V. The initial charge / discharge curves of the full cells with LiFePO4 and LiMn2O4 cathodes are shown in Figure 2. Fig.19A and 19B At a low C / 5 rate, the full cell of LiMn2O4 shows 120 mA·h·g -1 The capacity is close to the actual capacity of the cathode. Using LiFePO4 as the cathode, the measured capacity is 140mA·h·g -1 With NMC622 as cathode, the highest capacity is 165mA·h·g -1 ( Fig.19C ). Capacities are quoted based on the mass of active cathode material.

[0239] The rate performance of NMC622 full cells was evaluated in the current density range from C / 5 to 20C. The NMC622 full cell maintained 125 mA·h·g at 20C. -1 The capacity retention rate is greater than 75% relative to the capacity at C / 5 ( Fig.19D). To test long-term cycling, the NMC622 full cells were cycled for 300 cycles at 10C charge and 10C discharge rates. Under these conditions, a capacity of 120 mA·h·g was observed after 300 cycles. -1 , corresponding to a capacity retention of more than 80% ( Fig.19E At lower rates, a very high capacity retention of over 98% was achieved over 100 cycles at 1C charge and 1C discharge ( Fig.19F ).

[0240] Study of electrode degradation

[0241] To investigate the cause of capacity loss, Nb 16 W5W 55 The full cell with NMC622 anode and cathode was cycled for 500 cycles at 1C charge and 1C discharge. A capacity retention of 71.1% was observed ( Fig. 20A ). The battery is disassembled and the cathode and anode are reassembled into a half-cell geometry with respect to the lithium metal electrode. Fig. 20B As shown, the extracted NMC622 electrode shows a capacity of 0.48 mAh. In this configuration, the initial capacity of the NMC622 half-cell is 0.72 mAh. Therefore, the NMC622 electrode shows a capacity retention of 67% (capacity loss of 33%). In contrast, in this configuration, the extracted Nb 16 W5W 55 The electrode showed a capacity of 0.62 mAh ( Fig. 20C ). This corresponds to a capacity retention of 85% (15% capacity loss). 16 W5W 55 More than half of the capacity loss observed in full cells with NMC622 anode and NMC622 cathode is caused by degradation of the NMC622 cathode. This suggests that Nb 16 W5W 55 The material is particularly an elastic electrode material.

[0242] Nb 16 W5W 55 A mixture of LTO and

[0243] Additional experiments were performed to test Nb 16 W5W 55 and LTO as an electrode material. 16 W5W 55 and Nb 18 W 16 O 93 In the same way, a Li metal anode containing Nb was prepared and measured.16 W5W 55 The constant current charge-discharge curves of the electrodes with three different ratios of LTO are shown in Fig.21A , normalized to gravimetric capacity. The average voltage of 1.55V is close to the average voltage of pure LTO ( Figure 5A ). With 7:3(Nb 16 W5W 55 :LTO), the gravimetric capacity observed at C / 5 was 225 mA·h·g -1 , while at 20C it is 125mA·h·g -1 ( Fig. 21B ). For 3:7(Nb 16 W5W 55 :LTO), the gravimetric capacity observed at C / 5 was 190 mA·h·g -1 , while at 20C it is 130mA·h·g -1 ( Fig. 21B ). To test long-term cycling, the cells were cycled for 500 cycles at 10C charge and 10C discharge rates. Under these conditions, a capacity of 150 mA·h·g was observed. -1 , showing a capacity retention of more than 93% ( Fig. 21C ).

[0244] Same as above for Nb 16 W5W 55 and Nb 18 W 16 O 93 In the same way, a stainless steel 2032 button cell with a glass microfiber separator was prepared comprising 3:7 (Nb 16 W5W 55 :LTO) anode and NMC622 cathode. 16 W5W 55 , LTO, Super P carbon and PVDF were ground together to prepare an 80 / 15 / 5 active material / carbon / polymer anode. NMC622, Li250 carbon and PVD were ground together as described above to prepare an 80 / 10 / 10 active material / carbon / polymer electrode used as a cathode. The electrolyte was 150 μL LP30. No additives were used.

[0245] like Fig.22A As shown, the full cell was evaluated between 1.0 and 3.25 V. At a low C / 5 rate, a capacity of 200 mA·h·g was observed. -1 The average voltage was 2.25 V. The rate performance of the full cell was evaluated in the current density range from C / 5 to 20 C. The full cell maintained 160 mA·h·g at 20 C. -1The capacity retention rate is greater than 78% relative to the capacity at C / 5 ( Fig. 22B ).

[0246] Nb2Mo3O 14 Electrochemical characterization of

[0247] Same as above for Nb 16 W5W 55 and Nb 18 W 16 O 93 The same method is used for Nb2Mo3O 14 Electrochemical characterization of the 2032 stainless steel button cells (Cambridge Energy Solutions) with conical springs, two 0.5 mm stainless steel spacer disks, a plastic washer and a glass microfiber diaphragm (Whatman) were used. The metal oxides and conductive carbon (Super P, TIMCAL) were hand-ground in an agate mortar and pestle at a mass ratio of 8:1. The powder was ground with polyvinylidene fluoride (PVDF, Kynar) dispersed in N-methylpyrrolidone (NMP, Sigma-Aldrich, anhydrous, 99.5%) at a mass ratio of 9:1. The metal oxide / carbon / polymer electrode acted as a cathode relative to a Li metal disc (LTS Research, 99.95%) anode in a half-cell geometry. The electrolyte was 1 M LiPF6 dissolved in 1:1 v / v ethylene carbonate / dimethyl carbonate (EC / DMC, Sigma-Aldrich, battery grade). No additives were used. The electrochemistry was performed in a temperature-controlled chamber at 293K. Electrochemical measurements were performed using a Biologic galvanostat / potentiostat with EC-Lab software.

[0248] At C / 20, it can maintain about 200mA·h·g -1 Gravimetric capacity ( Fig.15 ). Nb2Mo3O 14 The average voltage is about 2.0 V. Therefore, Nb2Mo3O 14 It can be used in a voltage window of, for example, 3.0 to 1.4 V or 3.0 to 1.8 V and still provide high capacity at high rates while avoiding or minimizing reactions with the electrolyte. This is advantageous because many prospective solid electrolyte materials will react with low voltage anodes, and this can be achieved using Nb2Mo3O 14 Anode to relieve.

[0249] References

[0250] All documents mentioned in this specification are incorporated herein by reference in their entirety.

[0251] Allpress and Roth,J.Solid State Chem.1971,3,209-216.

[0252] Arbi,et al.,MRS Online Proc.Libr.Arch.2011,1313.

[0253] Bork and Heitjans,J.Phys.Chem.B 1998,102,7303-7306.

[0254] Cruz,at al.,Mater.Res.Bull.2003,38,525-531.

[0255] Downiem et al.,J.Electochem.Soc.2013,160,A588-A570.

[0256] Fuentes,et al.,Solid State lon.1996,92,103-111.

[0257] Fuentes,et al.,Solid State lon.1997,93,245-253.

[0258] Gobet,et al.,Chem.Mater.2014,26,3558-3564.

[0259] Griffith,et al.,lnorg.Chem.2017,56,4002-4010.

[0260] Hayamizu,et al.,Solid State lon.2013,238,7-14.

[0261] Hayamizu,et al.,Solid State Nucl.Magn.Reson.2015,70,21-27.

[0262] Hayamizu,et al.,Solid State lon.2016,285,51-58.

[0263] Hayamizu,et al.,Phys.Chem.Chem.Phys.2017,19,23483-23491.

[0264] Holzmann,et al.Energy Environ.Sci.2016,9,2578-2585.

[0265] He at al.,Sci.Rep.2012,2,913.

[0266] Ishiyama,et al.,Jpn.J.Appl.Phys.2014,53,110303.

[0267] Ishiyama,et al.,Nucl.Instrum.Methods Phys.Res.Sect.B BeamInteract.Mater.At.2016,376,379-381.

[0268] Kasnatscheew,et al.,J.Electrochem.Soc.2017,164,A2479-A2486.

[0269] Kim,et al.,Adv.Funct.Mater.2013,23,1214-1222.

[0270] Kuhn,et al.,Phys.Rev.B 2011,83,094302.

[0271] Kuhn,et al.,Energy Environ.Sci.2013,6,3548-3552.

[0272] Kuhn,et al.,Phys.Chem.Chem.Phys.2014,16,14669-14674.

[0273] Langer et al.,Phys.Rev.B 2013,88,094304.

[0274] Lv,et al.,J.Electrochem.Soc.2017,164,A2213-A2224.

[0275] Mali,et al.,J.Phys.F Met.Phys.1988,18,403.

[0276] Montemayor,et al.,J.Mater.Chem.1998,8,2777-2781.

[0277] Odziomek,et al.,Nat.Commun.2017,8,15636.

[0278] Oszajca,et al.,Chem.Mater.2014,26,5422-5432.

[0279] Palacin,et al.,Acta Chim.Solv.2016,63,417-423.

[0280] Roth and Wadsley,Acta Crystallogr.1965,19,26-32.

[0281] Roth and Wadsley,Acta Crystallogr.1965,19,32-38.

[0282] Ruprecht,et al.,Phys.Chem.Chem.Phys.2012,14,11974-11980.

[0283] Ruprecht and Heitjans,Diffusion Fundamentals2010,12,101.

[0284] Saritha,et al.,J.Solid State Chem.2010,183,988-993.

[0285] Stephenson,Acta Crystallogr.B 1968,24,673-653.

[0286] Sugiyama,et al.,Phys.Rev.B 2015,92,014417.

[0287] Sun,et al.,Science 2017,356,599-604.

[0288] Toby and Von Dreele,J.Appl.Crystallogr.2013,46,544-549.

[0289] Verhoevenm,et al.Phys.Rev.Lett.2001,86,4314-4317.

[0290] Wagemaker,et al.,J.Am.Chem.Soc.2001,123,11454-11461.

[0291] Wagemaker,et al.,Chem.-Eur.J.2007,13,2023-2028.

[0292] Wang,et al.,Nano Energy,2016,21,133-144.

[0293] Waring,et al.,J.Res.Nat.Bur.Stand.Sec.A 1966,70A,281-303.

[0294] Wilkening,et al.Phys.Chem.Chem.Phys.2007,9,6199-6202.

[0295] Wu,at al.,Nat.Nanotechnol.2012,7,310-315.

[0296] Yamada,et al.Solid State lon.2001,140,249-255.

[0297] Yamada,et al.,Mater.Res.Bull.1999,34,955-962.

[0298] Yan,et al.,J.Mater.Chem.A 2017,5,8972-8980.

[0299] Zaghib,et al.,Mater.Basel Switz.2013,6,1028-1049.

[0300] Zhao,at al.,J.Appl.Phys.2010,108,073517。

Claims

1. A method for charging and / or discharging an electrochemical cell, wherein the electrochemical cell has a working electrode comprising niobium tungsten oxide, wherein the niobium tungsten oxide is selected from Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 , Nb 22 W 20 O 115 or a combination thereof, wherein during discharge of the electrochemical cell, the working electrode is an anode.

2. The method according to claim 1, wherein the method is a method of charging and / or discharging an electrochemical battery at a charge and discharge rate of at least 5C.

3. The method according to claim 1 or 2, wherein the method is to provide a flow rate of at least 750 mA·g -1 A method for charging and / or discharging an electrochemical cell at a current density of 1000 Å.

4. The method of claim 1, wherein the working electrode comprises Nb 16 W5W 55 or Nb 18 W 16 O 93 .

5. The method of claim 1, wherein the ratio of Nb2O5 to WO3 in the working electrode is 8:5 to 11:

20.

6. The method according to claim 1, wherein the working electrode further comprises Nb 12 WO 33 , Nb 26 W4O 77 , Nb 14 W3O 44 , Nb 18 W8O 69 、Nb2WO8、Nb 22 W 20 O 115 、Nb8W9O 47 , Nb 54 W 82 O 381 , Nb 20 W 31 O 143 、Nb4W7O 31 or Nb2W 15 O 50 Niobium tungsten oxide or a combination thereof.

7. The method of claim 1, wherein the working electrode comprises a mixture of niobium tungsten oxide and an additional active material.

8. The method according to claim 7, wherein the additional active material is Li4Ti5O 12 .

9. The method of claim 1, wherein the method comprises cycling the electrochemical cell to charge and discharge, or discharge and charge, and wherein the method comprises 2 or more cycles.

10. The method of claim 1, wherein the method comprises 500 or more cycles.

11. An electrochemical cell comprising a working electrode, wherein the working electrode comprises niobium tungsten oxide, the niobium tungsten oxide being selected from Nb 16 W5W 55 , Nb 18 W8O 69 、Nb2WO8、Nb 18 W 16 O 93 , Nb 22 W 20 O 115 or a combination thereof, wherein during discharge of the electrochemical cell, the working electrode is an anode.

12. The electrochemical cell of claim 11, wherein the working electrode comprises Nb 16 W5W 55 or Nb 18 W 16 O 93 .

13. An electrochemical cell according to claim 11 or 12, wherein the ratio of Nb2O5 to WO3 in the working electrode is from 8:5 to 11:

20.

14. The electrochemical cell according to claim 11, wherein the working electrode further comprises Nb 12 WO 33 , Nb 26 W4O 77 , Nb 14 W3O 44 , Nb 18 W8O 69 、Nb2WO8、Nb 22 W 20 O 115 、Nb8W9O 47 , Nb 54 W 82 O 381 , Nb 20 W 31 O 143 、Nb4W7O 31 or Nb2W 15 O 50 Niobium tungsten oxide or a combination thereof.

15. The electrochemical cell of claim 11, wherein the working electrode comprises a mixture of niobium tungsten oxide and an additional active material.

16. The electrochemical cell of claim 15, wherein the additional active material is Li4Ti5O 12 .

17. The electrochemical cell of claim 11, wherein the electrode does not have a porous structure or a layered structure.

18. The electrochemical cell of claim 11, wherein the electrode comprises niobium tungsten oxide in particle form.

19. A lithium ion battery comprising one or more electrochemical cells according to any one of claims 11 to 18.

20. A vehicle comprising the lithium ion battery according to claim 19.

Citation Information

Patent Citations

  • Coupled hydrocarbon polymers and process for their preparation

    EP0002012A1

  • Process for isolating rubbers

    EP0002015A1

  • Negative pole used for lithium battery, and preparation and application thereof

    CN106558692A

  • Electrode composition

    CN114730861A