Method and apparatus for determining the effect of one or more pixels of a substrate to be introduced into a photolithography mask

By measuring the birefringence change of the lithographic mask substrate, determining the pixel effect and correcting the lithographic mask error, the complexity of error correction and EUV mask transmission calibration in lithographic mask manufacturing are solved, and the photoresist is realized High accuracy and uniformity of patterns.

CN112639612BActive Publication Date: 2024-12-06CARL ZEISS SMS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880095686.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-07-17
Publication Date
2024-12-06
Estimated Expiration
2038-07-17

AI Technical Summary

Technical Problem

There are many types of errors in the manufacturing process of existing photolithography masks, including registration error, optical intensity unevenness, coverage defects and substrate bending, resulting in inconsistent photoresist pattern sizes, and future EUV masks cannot use traditional light Transmission calibration is performed by diluting wavelengths, resulting in changes in the defect correction workflow.

Method used

By measuring the birefringence change of the lithographic mask substrate, the introduced pixel effect is determined to correct the error of the lithographic mask, using stress birefringence as the main effect of the calibration procedure, independent of the actinic wavelength, using transmission or reflective optical bi-folds The refractive measurement system, combined with the control of laser beam parameters, ensures the accuracy of the pixel writing program.

Benefits of technology

Effectively correct the defects of lithography masks, avoid indirect calibration problems caused by stress in traditional methods, and are suitable for traditional and EUV masks, improving the pattern uniformity and resolution of lithography masks, ensuring photoresist patterns accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112639612B_ABST
    Figure CN112639612B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for determining an effect of one or more pixels to be introduced into a substrate (110, 310) of a lithography mask (100, 300), the lithography mask (100, 300) having one or more pattern elements (120, 360), wherein the one or more pixels are used to at least partially correct one or more errors (190, 390) of the lithography mask (100, 300), the method comprising: determining the effect of the one or more introduced pixels by determining a birefringence change of the substrate (110, 310) of the lithography mask (100, 300) having the one or more pattern elements (120, 360).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims priority to U.S. Patent No. 9,658,527 B2, entitled “Correction of errors of a photolithographic mask using a joint optimization process,” the entire contents of which are expressly incorporated herein by reference. Technical Field

[0002] The present invention relates to the field of determining the effect of one or more pixels of a substrate to be introduced into a lithography mask. In particular, the present invention relates to a method and apparatus for determining a calibration procedure for correcting errors of a lithography mask. Background Art

[0003] As the integration density in the semiconductor industry continues to increase, the photolithography mask must project smaller and smaller structures onto the photosensitive layer, i.e., the photoresist on the wafer. In order to meet this demand, the exposure wavelength of the photolithography mask has been shifted from the near-ultraviolet to the far-ultraviolet region of the electromagnetic spectrum across the mid-ultraviolet. At present, a wavelength of 193nm is generally used for the exposure of the photoresist on the wafer. In the future, the photolithography mask will use significantly smaller wavelengths in the extreme ultraviolet (EUV) wavelength range (about 10nm to 15nm) of the electromagnetic spectrum.

[0004] As a result, the manufacture of photolithography masks that meet the ever-increasing resolution requirements is becoming increasingly complex and, therefore, more expensive. It is not uncommon for photolithography masks, photomasks or simply masks, to have defects at the end of their manufacturing process. Since the mask manufacturing process is time-consuming, photomask defects should be repaired whenever possible.

[0005] A photolithography mask can have several kinds or types of errors. One important type of defect in a photolithography mask is a mask image placement error or registration error. This type of error or defect occurs when one or more pattern elements of a pattern configured on a photolithography mask are not positioned precisely at their locations as predetermined by the layout data of the mask.

[0006] WO 2013 / 123973 describes a method for compensating polarization defects of an optical element in an optical system caused by birefringence of the material of the optical component by introducing one or more configurations of pixels into the optical element, preferably into optically irrelevant parts of the optical element.

[0007] Another type of error is the non-uniformity of light transmission across the area of ​​the photolithography mask, which results in corresponding variations in the optical intensity dose or simple dose applied to the photoresist on the wafer when the wafer is illuminated through the mask. Variations in the locally applied optical intensity dose or simple dose result in fluctuations or variations in the feature dimensions of the pattern elements in the developed photoresist. The uniformity of the imaging of the pattern elements across the area of ​​the photolithography mask is called critical dimension uniformity (CDU).

[0008] In addition, another important type of defect is overlay defect or on product overlay (OPO). This error type is related to the offset of the feature elements on the wafer that are imaged by two or more subsequent illumination steps using two or more different masks. In addition, the bow of the substrate of the photomask is another error type.

[0009] The applicant has described methods for correcting these and other errors of photolithography masks by introducing or writing pixels into the substrate of the photomask. For example, some of these methods are described in the applicant's US patent US 9 658 527 B2. In addition, the applicant has constructed several tools These tools have been routinely used to reliably correct several types of photomask errors. However, there is still room for further improvement in these defect correction procedures.

[0010] Therefore, an object of the present invention is to provide a method and an apparatus to improve the above-mentioned method for correcting defects of a lithography mask. Summary of the invention

[0011] According to an aspect of the present invention, there is provided a method as claimed in claim 1. In one embodiment, there is provided a method for determining an effect of one or more pixels to be introduced into a substrate of a lithography mask, wherein the lithography mask has one or more pattern elements, and wherein the one or more pixels are used to at least partially correct one or more errors of the lithography mask, the method comprising: determining the effect of the one or more introduced pixels by determining a birefringence change of the substrate of the lithography mask having the one or more pattern elements.

[0012] The pixels introduced into the substrate of the lithography mask to correct various types of errors or defects of the lithography mask can locally change the optical transmittance of the mask substrate. In the following, the benefits of the method of the present invention are shown by taking the correction of the registration errors of the mask as an example. However, the method of the present invention is not limited to the correction of the registration errors of the lithography mask.

[0013] Pixels introduced or written into the mask substrate to correct, for example, registration errors create small scattering centers for optical radiation transmitted through the mask substrate. For example, when a repaired mask having pixels in its substrate is operated in a photolithography illumination system, pixels that correct one or more registration defects may introduce localized non-uniformities in the optical transmission of the mask. Thus, pixels introduced to correct registration errors will cause critical dimension (CD) variations across the photomask or critical dimension uniformity (CDU) issues for the photolithography mask.

[0014] In order to avoid CDU problems when correcting registration errors, the distribution of the second type of pixels can be determined at the same time as the first type of pixels that correct the registration errors. The second type of pixels mainly scatters the optical radiation impinging on one or more pixels locally in a defined manner. The second type of pixels does not substantially change the density of the substrate locally. Generally speaking, the second type of pixels will be introduced into the mask substrate together with the first type of pixels, wherein the first type of pixels corrects the registration errors of, for example, a lithography mask.

[0015] In general, neither the first type of pixels nor the second type of pixels are uniformly distributed in the substrate of the lithographic mask to be corrected. The effect of the correction of one or more pixels depends on the details of the pixel writing procedure. Therefore, the laser beam parameters of the laser system introduced into the pixel must be precisely controlled. In addition, there is a maximum allowed optical transmission variation, which can be corrected by a scanner or stepper, which uses the corrected mask in the lithographic procedure to project the pattern elements of the mask onto the photoresist arranged on the wafer. Therefore, the pixel writing procedure must be calibrated to ensure that the allowed optical transmission variation is not exceeded at the mask position.

[0016] Currently, the pixel writing process is calibrated using the optical transmission variation of the photolithography at the actinic wavelength and the maximum value of the allowed optical transmission variation caused by the error correction process is determined by introducing one or more pixels into the substrate of the photolithography mask.

[0017] This approach has two disadvantages: (a) The main parameter associated with the change of the mask substrate caused by the introduction of one or more pixels into the substrate is not the optical transmission, but the stress generated by the error correction pixels. This means that the calibration procedure of the present invention uses indirect quantities to describe the effect of one or more pixels and to determine the maximum tolerable optical transmission change. (b) Moreover, and more importantly, future EUV masks will be reflective optical elements. Actinic wavelengths can no longer be used to calibrate the transmission of the error correction procedure based on the introduction of pixels into the substrate of the lithography mask. Therefore, using the currently established calibration procedure also for EUV masks will lead to a change in the workflow of defect correction, since the optical transmission calibration must be performed on an uncoated EUV mask substrate.

[0018] The method of the present invention takes into account the changes in birefringence caused by stress in the mask substrate due to writing one or more pixels used to correct mask defects. By using the main effect of the error correction pixels, namely stress birefringence, to calibrate the defect correction procedure, two disadvantages of current calibration procedures can be avoided.

[0019] Determining the change in birefringence may include measuring the birefringence of the substrate before introducing the one or more pixels and after introducing the one or more pixels to the substrate.

[0020] Typically, optically isotropic materials are used for the substrates of photomasks, such as quartz substrates or LTE (low temperature expansion) materials. For these materials, the induced birefringence is proportional to the stress optical coefficient K (unit: [mm2 / N]). It can be measured as the difference Δ in the optical path length or delay between two incident flat waves passing through the sample parallel and perpendicular to the principal axis of stress at the measurement position.

[0021] The one or more errors may include at least one of: a registration error, a variation in optical transmission across the substrate, an overlay defect, and a bow of the substrate of the lithography mask.

[0022] This list of correctable defects is not complete. For example, polarization defects of a lithography mask can also be corrected by introducing pixels into the substrate of the lithography mask.

[0023] In this application, the term "photolithography mask" also includes templates used in nanoimprint technology.

[0024] One or more introduced pixels may not have an effect on the polarization of optical radiation that has been modified by one or more pattern elements of the lithographic mask. This is true for EUV masks; EUV photons will not pass through the layer where the pixel is configured.

[0025] Determining the effect of the one or more introduced pixels may include determining a change in birefringence as a function of at least one laser beam parameter of a laser system used to introduce the one or more pixels into the substrate of the lithography mask.

[0026] The method of the present invention may further comprise the step of controlling at least one laser beam parameter of a laser system based on the determined birefringence change to correct one or more errors of the lithography mask when writing one or more pixels into the substrate of the lithography mask.

[0027] By determining the stress-induced change or variation in birefringence introduced into one or more pixels in the substrate based on one or more laser beam parameters, a calibration curve can be determined that can be used to control the pixel writing process.

[0028] Determining the birefringence change may include using a transmission optical birefringence measurement system using a wavelength greater than the actinic wavelength of the lithography mask. Additionally, determining the birefringence change may include using a reflection optical birefringence measurement system using a wavelength greater than the actinic wavelength of the lithography mask.

[0029] Using stress birefringence as the quantity used to determine the stress caused by writing an error correction pixel to the mask substrate allows the determination of the pixel effect to be decoupled from the actinic wavelength. Thus, the wavelength used to measure the stress birefringence can be selected independently of the actinic wavelength. However, the wavelength used to measure the stress birefringence can be adapted to the optical properties of the mask substrate so that the stress birefringence can be determined with high accuracy.

[0030] The wavelength of the transmission optical birefringence measurement system can be in the visible wavelength range.

[0031] The substrate of an EUV mask is not transmissive to EUV photons, but is typically at least partially transmissive in the visible wavelength range. Therefore, for conventional transmissive lithography masks (regardless of their actinic wavelength) as well as for future EUV masks (also independent of their specific actinic wavelength), the method of the present invention can be used to directly determine the stress birefringence induced by a defect correction process written into one or more pixels.

[0032] The at least one laser beam parameter may include at least one of: power, pulse length, pulse density, focal width, focal depth, wavelength, wavefront, and polarization of the laser beam.

[0033] The wavefront describes the shape of the wavefront of electromagnetic radiation that produces one or more pixels in the substrate of a lithographic mask.

[0034] The defined method may further comprise the step of correlating the change in birefringence to a stress model for one or more pixels to be introduced into the substrate of the lithography mask.

[0035] The method as defined above may comprise determining a variation in optical transmission of the substrate as a function of at least one laser beam parameter.

[0036] This step allows to connect the conventional calibration procedure with the new calibration procedure explained in this application. This step is also necessary to connect the stress birefringence with the optical transmission change.

[0037] The pulse length, pulse density, focal width, focal depth, wavefront, and polarization of the laser beam may be fixed, and the power of the laser beam may be varied as a parameter.

[0038] The defined method may further comprise the step of coupling the change in birefringence to a change in optical transmission caused by one or more pixels to be introduced into the substrate, wherein at least one laser beam parameter is a parameter.

[0039] For each substrate type of photolithographic mask, it is possible to establish a relationship between stress birefringence and the induced optical transmission change. This means that the optical transmission change of the mask substrate can be derived as the amount of stress introduced into the substrate during the pixel writing process.

[0040] Controlling at least one laser beam parameter may include limiting a value of the at least one laser beam parameter such that introduction of one or more pixels into the substrate does not locally exceed a predetermined critical value of a variation in optical transmission of the substrate of the lithography mask.

[0041] Based on a calibration procedure, in which the stress birefringence is determined as a function of the optical transmission variation and with at least one laser beam parameter as a parameter, it can be ensured that the defects of the lithography mask are effectively corrected by an error correction procedure of writing pixels to the mask substrate, without introducing one or more new errors that cannot be corrected by writing additional pixels to the substrate in a second error correction procedure.

[0042] The defined method may further comprise the step of determining a change in optical transmission of the substrate at a wavelength used by a laser system to introduce one or more pixels into the substrate.The substrate may comprise a substrate for a photolithography mask in the extreme ultraviolet (EUV) wavelength range.

[0043] As described above, the stress introduced into the mask substrate by introducing one or more pixels into the substrate depends on at least one laser beam parameter. The at least one laser beam parameter may be the power of the laser beam if the other above-mentioned laser beam parameters are fixed. When determining at least one laser beam parameter, the substrate, in particular the substrate of an EUV mask, may have optical absorptions which cannot be ignored at the wavelength at which the laser system generating the pixel operates. In particular, the optical absorption of the photomask may vary from batch to batch. If this effect is not taken into account, at the location where the pixel is generated, at least one actual laser beam parameter may deviate from the determined laser beam parameter. As a result, the error correction procedure is not optimal and may even fail completely.

[0044] Determining a change in optical transmission of the substrate may include determining a change in optical transmission as a function of a lateral position of the substrate of a lithography mask.

[0045] In general, optical transmission can vary across an EUV mask blank. Therefore, for accurate defect correction by pixel writing, the variation in optical attenuation of the substrate at the pixel writing wavelength must be taken into account.

[0046] The lateral position of the mask is the position in the plane of the lithography mask (x-direction and y-direction). The z-direction is perpendicular to the plane of the mask.

[0047] The defined method may further comprise the step of determining a variation in optical transmission as a function of depth and / or lateral position of the substrate where one or more pixels are to be introduced into the substrate.

[0048] Depending on the type of error to be corrected in the lithography mask, one or more pixels may be introduced to different depths in the mask substrate. Thus, the attenuation of the laser beam within the substrate may depend on the type of error to be corrected. In order to optimize the defect correction procedure, it is advantageous to consider the depth of introduction parameters.

[0049] The substrate may have a coating on a rear surface of the substrate, wherein the coating is electrically conductive and at least partially optically transmissive at a wavelength at which one or more pixels are introduced into the substrate when determining at least one laser beam parameter.

[0050] The substrate of the EUV mask may have a coating on its rear surface. The coating is usually electrically conductive so that the EUV mask can be fixed to an electronic chuck. In order to correct defects of the EUV mask, pixels are usually introduced via the back side of the mask substrate. In general, a multilayer structure is arranged on the front side of the mask substrate, which acts as a reflective element for EUV radiation. Therefore, the front side of the EUV mask is usually not available for introducing pixels into the mask substrate. Therefore, the electrically conductive rear side coating needs to be at least partially optically transparent at the wavelength at which the pixels are introduced into the substrate of the EUV mask.

[0051] The coating may include at least one of the following materials: indium tin oxide (ITO), fluorine tin oxide (FTO), and antimony tin oxide (ATO). The thickness of the coating may be in the range of 1 nm to 200 nm, preferably 2 nm to 100 nm, more preferably 3 nm to 50 nm, and most preferably 4 nm to 30 nm. Alternatively, the conductive coating may include two layers. The first layer may include chromium nitride (CrN) with a thickness of 2 nm to 50 nm, preferably 4 nm to 30 nm, more preferably 6 nm to 20 nm, and most preferably 8 nm to 12 nm. The second layer may include a metal oxide layer, such as a tantalum oxynitride layer, with a thickness of 50 nm to 1000 nm, preferably 100 nm to 800 nm, and most preferably 200 nm to 600 nm.

[0052] The method defined above may further comprise the step of determining a change in the optical transmission of the substrate and / or the coating at a wavelength used by the laser system for introducing the plurality of pixels into the substrate.

[0053] Coatings are usually based on a compromise between low electrical resistance and high optical transmission. The optical absorptivity of the backside coating of the substrate can range from a few percent to tens of percent, depending on the material composition and thickness of the coating. Therefore, it is very beneficial to consider the optical attenuation of the coating when deciding at least one laser beam parameter used to write the pixel.

[0054] Determining the variation in optical transmission of the substrate and / or coating may include determining the variation in optical transmission as a function of the lateral position of the substrate of the lithography mask. Similar to the substrate, the optical transmission of the coating may fluctuate across the mask substrate. This may occur due to positional variations in coating depth and / or local variations in material composition, and / or local variations in doping of the coating.

[0055] Determining the change in optical transmission of the substrate may include determining the optical reflection of the substrate and determining the optical transmission of the substrate. In addition, determining the change in optical transmission of the substrate and the coating may include determining the optical reflection of the substrate and the coating and determining the optical transmission of the coating and the substrate. These three quantities, reflection, absorption and transmission, essentially characterize dielectric materials. By measuring two of them, the third quantity can be derived.

[0056] The method defined above may further comprise the step of determining the variation in optical transmission of the substrate and / or the coating as a function of the depth and / or lateral position of the substrate where one or more pixels are to be introduced into the substrate.

[0057] By adapting the pixel writing process to the optical properties of the mask substrate and the mask coating on the one hand and to the depth of the introduced pixel on the other hand, the error correction procedure can be optimized.

[0058] The one or more pixels may include a first written map having a first type of pixels for correcting the one or more errors, wherein the first written map describes a distribution of the one or more pixels to be introduced into the substrate of the lithography mask.

[0059] The defined method may further comprise the steps of determining a second write map having a second type of pixels for correcting the optical transmission variation of the substrate based on the determined birefringence variation and / or the determined optical transmission variation of the substrate and / or coating at the wavelength at which one or more pixels are introduced into the substrate.

[0060] The computer program may include instructions for causing a computer system to execute the steps of the method of the present invention and any of the aforementioned aspects.

[0061] According to another aspect of the invention, there is provided an apparatus as claimed in claim 16. In one embodiment, there is provided an apparatus for determining an effect to be introduced into one or more pixels of a substrate of a lithography mask, wherein the lithography mask has one or more pattern elements, wherein the one or more pixels are used to at least partially correct one or more errors of the lithography mask, the apparatus comprising: determining means for determining the effect of the one or more introduced pixels by determining a birefringence change of the substrate of the lithography mask having the one or more pattern elements.

[0062] The determining means for determining the birefringence change comprises at least one of the following: a polarizer, an ellipsometer, and a birefringence imaging system.

[0063] The means for determining the effect of one or more introduced pixels may comprise means for determining the stress distribution on the surface of the photolithography mask. The means for determining the stress distribution may comprise a device for determining surface plasmon resonances. When the response of the photomask to internal stresses is accurately modeled, it is possible to use information on the surface stresses on either side of the mask to determine the pixel effect.

[0064] Directly determining the stress distribution on the mask surface is an alternative method to determine the effect of pixels written into the mask substrate.

[0065] The apparatus according to the invention further comprises an optical measurement system which is suitable for determining the optical reflection and / or the optical transmission of the substrate and / or the coating arranged on the substrate.

[0066] The apparatus may further include a pixel writing system for correcting the one or more errors.

[0067] The means for determining the change in birefringence, the optical measurement system, and the laser system for correcting one or more errors may be combined into a single device.

[0068] Finally, the apparatus may be adapted to perform the steps of the method of the invention as well as the steps of any of the aforementioned aspects. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] In order to better understand the present invention and appreciate its practical application, the following drawings are provided and referenced below. It should be noted that the drawings are given only as examples and in no way limit the scope of the present invention.

[0070] Figure 1 A schematic cross-sectional view showing a transmissive photolithography mask;

[0071] Figure 2 A cross-sectional view of a template used for nanoimprint lithography is schematically depicted;

[0072] Figure 3 A cross-sectional view of a reflective extreme ultraviolet (EUV) mask is schematically shown;

[0073] Figure 4 A block diagram schematically shows some components of an apparatus that can be used to determine stress birefringence;

[0074] Figure 5 Some components of an optical measurement system allowing the optical reflection and optical transmission of a sample to be measured are shown;

[0075] Figure 6 The upper half of the figure shows the variation of the transmission of the mask substrate of the EUV mask on the substrate, and the lower half of the figure shows the variation of the reflection of the coating on the back side of the substrate of the reflective mask, wherein both images are composed of Figure 5 Determined by the optical measurement system;

[0076] Figure 7 A cross-sectional view schematically shows some components of a pixel writing system;

[0077] Figure 8 Schematically shows the Figure 4 equipment, Figure 5 Optical measurement systems, and Figure 7 A cross-sectional view of a device incorporating a pixel writing system;

[0078] Fig. 9 shows the change in optical transmission at an actinic wavelength caused by the introduction of a pixel into a substrate of a photolithographic mask as a function of the laser power of the laser system used to write the pixel into the substrate;

[0079] Fig.10 shows the variation of optical transmission at actinic wavelength and stress birefringence caused by introducing pixels into the substrate of a photolithographic mask as a function of the laser power of the laser system used to write the pixels into the substrate;

[0080] Fig.11 shows a representation of stress birefringence (ordinate) versus optical transmission change (abscissa) for various laser powers used to introduce pixels into the mask substrate; and

[0081] Fig.12 A flow chart of the inventive method of the present application is shown. DETAILED DESCRIPTION

[0082] Hereinafter, the present invention will be described more fully with reference to the accompanying drawings, in which exemplary embodiments of the present invention are shown. However, the present invention can be implemented in different forms and should not be construed as being limited to the embodiments set forth herein. Rather, these embodiments are provided to make the present disclosure more thorough and to convey the scope of the present invention to those skilled in the art.

[0083] In particular, the method of the invention is described in the context of a lithography mask. However, the skilled person will appreciate that the method defined is not limited to the application of correcting defective lithography masks. The method of the invention can also be used to correct defective templates 200 to be used in nanoimprint lithography. In general, the method of the invention can be applied to all transmissive optical elements that can be corrected by introducing one or more stress-causing pixels. It is applicable to optical elements for which optical transmission uniformity is not a critical parameter.

[0084] Figure 1 A schematic cross-sectional view of a transmissive photolithography mask 100 is shown. The mask 100 comprises a substrate 110 having a first or front surface 150 and a second or rear surface 160. The substrate 110 must be transparent to the wavelength used to illuminate the photoresist on the wafer. This wavelength is called the actinic wavelength. The exposure wavelength 180 may be in the deep ultraviolet (DUV) spectral range of the electromagnetic spectrum, particularly around 193 nm. In general, the substrate material comprises quartz. The substrate 110 typically has lateral dimensions of 152 mm x 152 mm and a depth or height of substantially 6.35 mm. The substrate 110 of the photolithography mask 100 has a pattern element 120 of a pattern 130, typically made of chrome, on its front surface 150, which images the pattern element 120 predetermined by the layout data into the photoresist disposed on the wafer.

[0085] exist Figure 1 In the example shown, the mask 100 has an error 190 in the form of a registration error, i.e., the distance of two or more pattern elements 120 deviates from the position predetermined by the layout data. The error 190 may also be a flatness error of the mask substrate 110, an overlay error, or an inhomogeneity of light transmission over the mask substrate 110 ( Figure 1 not shown).

[0086] The portion of the substrate 110 of the photolithography mask 100 with the pattern elements 120 is referred to as the active region 170 of the mask 100, while the boundary portion without the pattern elements 120 is referred to as the inactive region 175. A laser beam having an actinic exposure or illumination wavelength illuminates the substrate 110 of the mask 100 via the second or rear surface 160 of the substrate 110.

[0087] In the context of this application, the term "substantially" refers to a reference to a measured variable being within its error range when the variable is measured using state-of-the-art metrological tools.

[0088] Figure 2 A template 200 is schematically shown for transferring pattern elements onto a wafer in nanoimprint lithography. The template 200 comprises a material 210 which is transparent in the UV and DUV spectral range, typically fused silica is used as template material. Figure 2The exemplary template 200 has an error 290. The pattern elements on the front template side 220 are in the same Figure 1 The pattern elements 120 of the photolithography mask 100 are manufactured in a very similar procedure. Therefore, the principles of the present invention can also be applied to correct various errors of the template 200 used in nanoimprint lithography. The template 200 is illuminated by electromagnetic radiation 280 passing through the back side 230 of the template.

[0089] Figure 3 A schematic cross-sectional view of a photolithography mask 300 is shown for an exposure wavelength of 13.5 nm. Figure 1 Unlike the photolithography mask of the present invention, the EUV mask 300 is a reflective optical element based on a multilayer structure 305. The multilayer structure 305 acts as a reflector, which selectively reflects incident EUV photons 350. The multilayer structure 305 of the EUV mask 300 is deposited on a front substrate surface 315 of a suitable substrate 310 (e.g., a fused silica substrate). Other transparent dielectrics, glass materials, or semiconductor materials can also be used as substrates for photolithography masks, such as or It is advantageous for the material of the substrate 310 to have a very low coefficient of thermal expansion (LTE).

[0090] The multilayer film or multilayer structure 305 includes 20 to 60 pairs of alternating molybdenum (Mo) layers 320 and silicon (Si) layers 325. The thickness of each Mo layer 320 is 4.15 nm, and the thickness of the Si layer 325 is 2.80 nm. In order to protect the multilayer structure 305, a silicon capping layer 330 having a native oxide with a depth of 7 nm is disposed on top of the multilayer structure 305. Other materials may also be used to form the capping layer 330, such as ruthenium.

[0091] In the multilayer 305, the Mo layer 320 functions as a scattering layer, and the Si layer 325 functions as a separation layer. Instead of Mo, other elements having a high Z value may be used as scattering layers, such as cobalt (Co), nickel (Ni), tungsten (W), rhenium (Re), and iridium (Ir).

[0092] As already mentioned, the multilayer structure 305 on the substrate 310 of the EUV mask 300 acts as a reflector for EUV electromagnetic radiation. To form the EUV mask 300, a buffer structure 335 and an absorption pattern structure 340 are additionally deposited on the cover layer 330. The buffer layer 335 may be deposited to protect the multilayer structure 305 during processing (e.g. during etching and / or repair of the absorption pattern structure 340). Possible buffer structure materials are, for example, fused silica (SiO 2), silicon oxynitride (SiON), ruthenium (Ru), chromium (Cr) and / or chromium nitride (CrN). The absorption structure 340 includes a material having a large absorption constant for photons in the EUV wavelength range. Examples of these materials are chromium (Cr), titanium nitride (TiN) and / or tantalum nitride (TaN).

[0093] An anti-reflection (AR) layer 345 may be additionally disposed on the absorption pattern structure 340 to ensure that no photons are reflected by the surface of the absorption pattern 340. Tantalum oxynitride (TaON) may be used to make the AR layer. A thickness of about 50 nm is sufficient to substantially absorb all EUV photons 350 incident on the absorption structure 340. In contrast, most of the photons 350 incident on the capping layer 330 are reflected as photons 355.

[0094] exist Figure 3 In the example of , the pattern element 360 has an error 390 in the form of a registration error. The portion of the pattern element 360 indicated by the dashed line 395 should be free of absorbing material.

[0095] Similar to the transmissive mask 100, the substrate 310 of the EUV mask 300 typically has lateral dimensions of 152 mm×152 mm and a thickness or height of substantially 6.35 mm. The rear surface 370 or rear substrate surface 370 of the substrate 310 has a thin coating 375. The coating 375 should be conductive so that the EUV mask 300 can be fixed by electrostatic forces, that is, it can be electrically stuck on the sample stage of the lithography illumination system. In addition, the coating should be at least partially optically transparent near the wavelength used by the laser system to introduce pixels into the substrate 310. Materials that meet these two requirements are, for example, indium tin oxide (ITO), fluorine tin oxide (FTO), and / or antimony tin oxide (ATO). The coating 375 may have a thickness of 10 nm to 50 nm. Alternatively, the coating may include a chromium nitride (CrN) layer with a thickness of 10 nm to 20 nm. In addition, alternative coatings may also include CrN layers and metal oxide layers with thicknesses ranging up to 600 nm.

[0096] In another alternative, a very thin metal layer may be used for coating 375. For example, coating 375 may include at least one metal from the following group: nickel (Ni), chromium (Cr), aluminum (Al), gold (Au), silver (Ag), copper (Cu), titanium (Ti), tungsten (W), indium (In), platinum (Pt), molybdenum (Mo), rhodium (Rh), and / or zinc (Zn), and / or a mixture of at least two of these metals. The thickness of the metal layer is typically less than 30 nm.

[0097] Figure 4A cross section of an apparatus 400 is shown, which can be used to determine stress birefringence caused by introducing pixels into a substrate 110, 310 of a lithography mask 100, 300. The apparatus 400 includes a light source 420, which can be a laser light source 420. The light source can emit light in the visible range of the electromagnetic spectrum. For example, in Figure 4 In the embodiment, a Helium Neon laser is used as a light source. The light beam 430 generated by the light source 420 passes through a photoelastic modulator (PEM) 440. The PEM 440 includes a polarizer ( Figure 4 The photoelastic modulator 440 is not shown in the figure and typically comprises a piezoelectric transducer that periodically compresses and expands an optical medium (which is typically a quartz glass plate). Typically, the modulation frequency is 50 kHz. Thus, the photoelastic modulator 440 modulates the polarization of the light beam leaving the polarizer.

[0098] The modulated light beam 450 is transmitted through the sample 410. The sample 410 may be a mask substrate 110, 310 of a photolithography mask 100, 300, or may be a template 200 applied to nanoimprint lithography. Figure 1 and Figure 3 As discussed in the context of , the substrate of the lithography mask is typically an optically isotropic material. However, stress may be introduced into the mask substrate 110, 310 by the mask manufacturing process (i.e., by manufacturing the pattern 130 for the transmissive mask 100, or by manufacturing the pattern elements 360 on the front side 315 and / or the coating 375 on the back surface 370 for the reflective mask 300). Therefore, after the lithography mask 100, 300 is manufactured based on the substrate 110, 310, the defect-free substrate 110, 310 may have induced stress. Therefore, the lithography mask 100, 300 may show stress birefringence. In order to eliminate this stress birefringence contribution, the measurement of stress birefringence is a difference measurement, that is, the stress birefringence is measured before and after the pixels are introduced into the mask substrate 110, 310.

[0099] Furthermore, stress may be temporarily applied to the photolithography mask 100, 300, for example, by improper fixation of the mask 100, 300. Such temporary stress due to improper operation of the photomask 100, 300 is not considered in the present application.

[0100] Introducing pixels into the substrate 100, 310 of the mask 100, 300 will introduce a local permanent stress into the mask substrate 100, 300 in a defined manner. It is known that induced stress will cause or induce a change in opacity Δβ ij , which varies linearly depending on the stress induced in the material of the mask substrate 100 , 300 , where the relationship between the impermeability β and the dielectric constant ε is as follows:

[0101]

[0102] This dependence can be expressed in terms of the components of the stress-optical matrix:

[0103]

[0104] Where q is the stress optical coefficient matrix and σ is the stress tensor. Therefore, the stress induced in the material of the mask substrate 110, 310 by introducing or writing a pixel to the substrate 110, 310 will be directly related to the delay Δ of the light beam in the material of the substrate 110, 310 and is given by the following equation:

[0105]

[0106] Wherein, d is the thickness of the mask substrate 110, 310, n 0 is the refractive index of the isotropic material of the substrates 110 and 310, and β ij is a component of the opaque matrix of the substrate material of the photomask 100 , 300 . Equation 3 describes the delay in a two-dimensional deformation model in the plane of the photolithography mask 100 , 300 .

[0107] The delay Δ caused by the stress birefringence introduced into the mask substrate 110, 310 is connected in a simple manner to a quantity that can be precisely measured. The delay Δ of the lithography mask 100, 300 with material birefringence depends on the thickness d of the substrate 110, 310 of the mask 100, 300 and the fast axis n of the substrate 110, 310. F and slow axis n S The refractive index is given by the following equation:

[0108] Δ=d.(n S -n F )=d.Δn=d.δ (4)

[0109] where δ is called birefringence. The retardation is measured in meters; usually expressed in nanometers.

[0110] The retardation Δ caused by the material birefringence of the mask substrate 110 , 310 results in a change in the polarization of the laser beam 460 exiting the sample 410 relative to the polarization of the incident laser beam 450 .

[0111] Light beam 460 exiting sample 410 enters detection system 470. Detection system 470 may include a beam splitter mirror that separates modulated light beam 460 into two beams of substantially equal light intensity. Each portion of the light beam passes through a combination of an analyzer and a filter and is then detected by a photodetector. Components within detection system 470 are not shown. Figure 4 middle.

[0112] The lateral resolution of the device 400 is determined by the focal width of the modulated laser beam 450 in the sample 410. Currently, the lateral resolution for determining stress birefringence is in the range of 4 μm.

[0113] Computational Unit ( Figure 4 The device 400 (not shown) can convert the measurement signals of the two photodetectors into parameters from which the birefringence of the sample 410 can be determined. The device 400 or the calculation unit provides the retardation Δ and the fast axis angle as output signals. In general, the resolution limit of the device 400 is in the range of a few picometers. The resolution may be as low as 1 pm, with a typical repeatability of about ±10 pm.

[0114] The light source 420, PEM 440, and detection system 470 of the device 400 may have an interface 480. The device 400 may output the data of the calculation unit via the interface 480. It is possible to control the device 400 externally via the interface 480 and to transmit its measurement data via the interface 480 to an external computer system.

[0115] Figure 4 The device 400 determines the stress birefringence caused by introducing pixels into the substrate 110, 310 of the photolithography mask 100, 300 by transmitting light through the substrate 110, 310. However, it is also possible to use a device ( Figure 4 Therefore, the apparatus can be used to analyze the stress birefringence of the EUV mask 300.

[0116] Figure 5 Schematically shown are some components of an optical measurement system 500, which can be used to determine the optical absorption of a mask substrate 100, 300, in particular the substrate 310 of the EUV mask 300. The optical measurement system 500 comprises a light source 520, which can be a laser system. The wavelength of the light source 520 can be adapted to the wavelength of the laser system used to introduce pixels into the mask substrate 110, 310. Figure 5 In the example of FIG. 5 , the light source is a light emitting diode (LED). The light source 520 is connected to the control unit ( Figure 5 5. The light generated by the light source 520 is connected to the projection system 530 through the optical fiber 525, which directs the light beam 535 onto the sample 510. The sample 510 may be a photolithography mask 100, 300 or may be a template 200.

[0117] A first, typically small portion of the incident light beam 535 is reflected at the front side of the sample 510. For example, the front side 575 of the sample 510 may be the back side 160 of the substrate 110 of the transmissive mask 100, or may be the surface of the front side of the coating 375 of the substrate 310 of the photolithography mask 300. A second portion of the light beam 535 is reflected from the back side 580 of the sample 510. The back side 580 of the sample 510 may be the front side 190 of the substrate 110 of the transmissive mask 100, or may be the front side 315 of the substrate 310 of the EUV mask 300.

[0118] The first reflection portion 555 and the second reflection portion 565 may be separated by an aperture 550, such as by a pinhole 550. In addition, the light beam transmitted through the aperture 550 is filtered by a filter 560 and then measured by a photodetector 570. Therefore, the first reflection portion 555 and the second reflection portion 565 may be measured sequentially by the photodetector 570. It is also possible to use two different photodetectors 570 to detect the first reflection portion 555 and the second reflection portion 565 simultaneously.

[0119] A second photodetector 540 is disposed behind the sample 510 and detects a portion 545 of the incident light 535 that has passed through the sample 510 and has not been reflected at the back side 580 of the sample 510. The photodetectors 540, 570 may include photodiodes, such as PIN diodes or avalanche diodes. Alternatively, photomultiplier tubes may be used as the photodetectors 540, 570.

[0120] The lateral resolution of the detection of the reflected portions 555, 565 and the transmitted radiation depends on the focal width of the incident light beam 535, which is determined by the projection system 530 and the aperture 550 of the photodetectors 540 and 570. The lateral resolution of the optical measurement system 500 is in the range of 100 μm to 1 mm. When using an aperture 550 with a smaller opening, a higher lateral resolution can be obtained, but the signal-to-noise ratio of the signal of the photodetectors 540, 570 is sacrificed.

[0121] Based on the measurements of the photodetectors 540 and 570, the reflected portions 555, 565 and the transmitted portions 545 of the light beam 535 incident on the sample 510 can be determined. Based on these measurements, the absorption or attenuation of the substrate 110, 310 can be calculated. In addition, the data measured by the photodetectors 540, 570 can also determine the absorption of the coating 375 of the EUV mask 300. In addition, the photodetectors 540, 570 can measure the reflected portions 555, 565 and the transmitted portions 545 of the incident light beam 535 as a function of the lateral position of the mask substrate 110, 310. Therefore, the measurement system 500 can determine the absorption or attenuation of both the substrate 110, 310 and / or the coating 375 with high spatial resolution.

[0122] Figure 6 The upper half of the image 600 shows the variation of the transmitted portion 545 of the incident light beam 535 across the photolithography mask 300 as a function of lateral position. The light source 520 has a wavelength of 532 nm. As can be seen from the image 600, the absolute transmission variation across the mask 300 is approximately 3%.

[0123] Figure 6 The lower image 650 of shows the variation of the first reflected portion 555 of the incident light beam 535 on the coating 375 of the substrate 300 of the EUV mask 300, again for a wavelength of the incident light beam 535 of 532 nm. The maximum absolute variation is about 0.7%.

[0124] Those skilled in the art will recognize that images 600 and 650 show the absolute values ​​of the transmitted portion 545 and the reflected portion 555 of the light beam on the substrate 310 of the EUV mask 330. This indicates that the substrate 310 and the coating 375 of the EUV mask 300 are Figure 6 In the example shown, approximately 20% of the incident light beam 535 is transmitted. Figure 6 In the example of , the first order reflected light 555 from the front side 575 of the sample 510 accounts for about 29%. Figure 6 In the example of , according to A=1-RT, about 50% of the incident light 535 is absorbed in the substrate 310 and the coating 375 of the EUV mask 300. Generally speaking, the first order reflection value is in the range of 30% to 60%. In addition, generally speaking, 15% to 25% of the incident light 535 is transmitted through the substrate 310 and the coating 375 of the EUV mask 300. Therefore, in Figure 6 In the example of FIG. 3 , the absorption of the substrate 310 and the coating 375 of the EUV mask comprises a range of 15% to 55%. However, as described, this is only an example. Figure 6 Other coatings and substrates may not be significantly absorptive, or may have higher or lower optical transmittance, or may have higher and lower values ​​of reflectivity than the examples shown.

[0125] Figure 7 A schematic block diagram of an exemplary pixel writing device 700 is shown, which can be used to correct Figure 1 and Figure 3 The photolithography masks 100, 300 and Figure 2 The pixel writing apparatus 700 includes a chuck 720 that can move in three dimensions. The sample 710 can be fixed to the chuck 720 by using various techniques (such as clamping). The sample 710 is mounted upside down on the chuck 720 so that its rear substrate surface faces the objective lens 740. The sample 710 can be a photolithography mask 100, 300, or can be a template 200.

[0126] The pixel writing device 700 includes a pulsed laser source 730, which generates a beam or light beam 735 of pulses or light pulses. The laser source 730 generates light pulses with variable duration. The pulse duration can be as low as 10fs (femtoseconds), but can also be continuously increased to 100ps (picoseconds). The pulse energy of the light pulses generated by the pulsed laser source 730 can also be adjusted in a huge range from 0.01μJ per pulse to 10mJ per pulse. In addition, the repetition rate of the light pulses includes a range from 1Hz to 100MHz. For example, the light pulses can be generated by a titanium: sapphire (Ti: Sapphire) laser operating at a wavelength of 800nm. However, the error correction method by introducing pixels into the mask substrate 110, 310 is not limited to this laser type. In principle, all laser types having photon energy less than the band gap of the substrate 110, 310 or template 200 of the photolithography mask 100, 300 and capable of generating pulses with a duration in the femtosecond range can be used. Thus, for example, Nd-YAG lasers or dye laser systems ( Figure 7 not shown).

[0127] The mirror 790 is steered to direct the pulsed laser beam 735 into the focusing objective 740. The objective 740 focuses the pulsed laser beam 735 through the rear substrate surface 160, 370 into the substrate 110, 310 of the lithography mask 100, 300. The NA (numerical aperture) of the applied objective 740 depends on the predetermined spot size of the focal point and the position of the focal point within the substrate 110, 310 of the lithography mask 100, 300 relative to the rear substrate surface 160, 370. The NA of the objective 740 can be as high as 0.9, which results in a focal spot diameter of substantially 1 μm and a maximum intensity of substantially 10 20 W / cm 2 .

[0128] The pixel writing apparatus 700 also includes a controller 780 and a computer system 760, which manage the translation (x and y directions) of the two-axis positioning stage of the sample holder 720 within the plane of the sample 710. The controller 780 and the computer system 760 also control the translation (z direction) of the objective lens 740 perpendicular to the plane of the chuck 720 via the single-axis positioning stage 750 to which the objective lens 740 is fixed. It should be noted that in other embodiments of the pixel writing apparatus 700, the chuck 720 can be equipped with a three-axis positioning system to move the sample 710 to a target position and the objective lens 740 can be fixed, or the chuck 720 can be fixed and the objective lens 740 can be movable in three dimensions.

[0129] The computer system 760 may be a microprocessor, a general purpose processor, a special purpose processor, a CPU (central processing unit), etc. It may be configured in the controller 780, or may be a separate unit, such as a PC (personal computer), a workstation, a mainframe computer, etc. The computer system 760 may further include an interface that connects the computer system 760 to the controller 780 via the connection 755. Figure 4 In addition, the computer system 760 can control the laser source 520 via the connection 515 and the laser source 520 via the connection 795. Figure 5 Photodetectors 540 and 570 of the optical measurement system 500 .

[0130] In addition, the pixel writing apparatus 700 may also provide an observation system including a CCD (charge coupled device) camera 765, which receives light from an illumination source disposed in the chuck 720 via a dichroic mirror 745. The observation system helps to navigate the sample 710 to a target position. In addition, the observation system may also be used to observe the formation of a modified area on the rear substrate surface of the sample 710 by a pulsed laser beam 735 of the light source 730.

[0131] The computer system 760 may include a processing unit that determines laser beam parameters of the laser beam 735 based on error data and measurement data obtained from the apparatus 400 via the interface 480 and from the measurement system 500 via the interface 515. By taking into account experimental data from both the apparatus 400 and the measurement system 500, one of a plurality of errors of the photolithography mask 100, 300 may be effectively corrected without the risk that the error correction procedure will introduce new defects in the photomask 100, 300. More details of the pixel writing procedure are described in US 9 658 527 B2.

[0132] Figure 8 A cross-sectional view of a bonding device 800 is schematically shown, which Figure 4 Equipment 400, Figure 5 The optical measurement system 500, and Figure 7 The pixel writing device 700 is combined in a single device. The control and processing unit 850 controls the device 400 via the connection 810, controls the measuring system 500 via the connection 820, and controls the pixel writing device via the connection 830. Furthermore, the control and processing unit 850 is connected to an external interface 860 via a connection 840.

[0133] The control and processing unit 850 controls the measurement of stress birefringence via the device 400 and obtains experimental data from the device 400 via the connection 810. In addition, the control and processing unit controls the measurement of optical reflection and optical transmission of the substrate 310 and / or the coating 375 and receives the measured data. For example, based on these data, the control and processing unit 850 can determine the power of the laser beam 735 incident on the coating 375 of the mask substrate 110, 310 as a function of depth within the substrate 310. Since the correction effect of a pixel strongly depends on the local energy density at the location where the pixel is generated, the error correction procedure of the pixel writing device can be accurately controlled by the pixel writing device 700.

[0134] The control and processing unit 850 may receive error data of the mask 100, 300 from the defect metrology system via the interface 860 and the connection 840. Based on the obtained error data, the determined stress birefringence of the substrate 110, 310, and the determined reflective and transmissive properties of the substrate 110, 310, the control and processing unit may determine the laser beam parameters of the pixel writing device 700. The control and processing unit 850 may be implemented in hardware, software, firmware, and combinations thereof. The control and processing unit 850 may include an algorithm that calculates the parameters of the laser beam 735 of the laser system 730 of the pixel writing device 700 based on the measurement data received from the device 400 and the optical measurement system 500.

[0135] Fig. 9 Graph 900 shows the measurement results of the optical transmission variation of substrate 110 into which photolithography mask 100 with multiple pixel arrangements has been introduced. Fig. 9 and the subsequent Fig.10 In the embodiment, the pixels in each pixel arrangement in the plurality of pixel arrangements have a fixed density. Fig. 9 In the example of , the lateral dimensions of the pixel arrangement are 3 mm x 3 mm, and the pixels have a pitch of about 4 μm in both directions. All pixel arrangements have been written into the center of the substrate 110, at a depth of 3.175 mm. Various pixel arrangements have been introduced into the substrate 110 using different power levels of the laser system 730 of the pixel writing apparatus 700. The laser beam parameters used to introduce the pixel arrangements into the mask substrate 110 are shown in the table below.

[0136] Table 1: Numerical values ​​of selected laser beam parameters

[0137]

[0138] To obtain Fig. 9 At the measurement point shown, the substrate 110 with the pixel arrangement has been irradiated with a DUV (deep ultraviolet) lamp in CW (continuous wave) mode. The DUV radiation has been filtered using a narrow band filter. Alternatively, Fig. 9The measurement data of can also be measured at the actinic wavelength (ie, 193 nm) of the mask 100. Therefore, the light source of the lithography illumination system can be used for this measurement. Generally speaking, the light source of the lithography illumination system irradiates the substrate 110 in a CW mode or a quasi-CW mode.

[0139] As can be seen from graph 900, the attenuation of optical radiation in the deep ultraviolet (DUV) wavelength range increases almost linearly with the laser power used during the pixel writing process. Fig. 9 Details of the curve 910 fitted to the measurement points 920 are shown. Based on the curve 910, a lookup table can be established that can be used to determine a second pixel arrangement including second type pixels that compensate for variations in optical transmission or DUV attenuation across the substrate 110 of the photomask 100. Based on the lookup table, the laser beam parameters of the laser system 730 can be fixed to write a second type pixel arrangement having at least one second type pixel to compensate for variations in optical transmission of the photolithography mask 100.

[0140] exist Fig. 9 In the example shown, the maximum value of the allowable optical attenuation of the mask substrate 110 is 3%. The amount of optical attenuation of the substrate 110 can be compensated by a scanner or a stepper, which projects the pattern 130 of the mask 100 onto the photoresist disposed on the wafer using the corrected photolithography mask 100. Therefore, during the pixel writing process (which corrects, for example, the error 190 of the photolithography mask 100), the maximum allowable optical attenuation determines the maximum power of the laser beam 735. The dot-dash line 930 shows this relationship.

[0141] Fig. 9 A conventional calibration procedure for a defect correction procedure or RegC procedure is described, which introduces pixels into the substrate 110 of the lithography mask 100. As described above, this calibration procedure can no longer be used for the EUV mask 300. The substrate 310 of the EUV mask 300 is not transparent for the actinic wavelength. Furthermore, the conventional calibration procedure indirectly infers the effect of the pixels introduced into the mask substrate 110 from the induced changes in the optical transmission of the substrate 110. Furthermore, the optical transmission is not a relevant parameter for the EUV mask 300. It does not have to be kept at a constant level, but can be freely selected.

[0142] Fig.10 Again, the optical transmission variation or light attenuation of a pixel arrangement written into the mask substrate 110 at different power levels of the laser beam 735 of the pixel writing system 700 is shown. Fig.10 , the pixel arrangement is written to the bare mask substrate 110. The measurement point 1020 is represented by a rotated square. For the measurement point 1020, the coordinates are given on the right side of the graph 1000. The fitted curve 1010 is given by equation 1050.

[0143] Fig.10 Also shown is a stress birefringence measurement of the same pixel arrangement in a bare mask substrate 110. Measurement point 1040 is represented by Fig.10 The result of fitting curve 1030 is given by 1060 in graph 1000 . Fig.10 The stress birefringence measurements shown in are difference measurements. This means that the stress birefringence of the substrate 110 has been measured before the pixel arrangement is introduced into the mask substrate 110. Therefore, Fig.10 The data shown does not include the effects of stress birefringence that may have been present in the substrate 110 prior to introduction of the pixel arrangement.

[0144] Graph 1000 clearly shows that the pixel arrangement induces stress birefringence. Fig.10 It is also revealed that the stress birefringence varies with the laser power used to introduce the pixel arrangement into the substrate 110. Furthermore, the measured points 1120 and 1040 and the calculated curves 1010 and 1030 show a correlation between the stress birefringence variation and the attenuation of the optical radiation in the DUV wavelength range.

[0145] Fig.11 A graph is shown in which the horizontal axis represents the power level of the laser used to write the pixel arrangement to the substrate 110. Fig.10 The light attenuation data is represented on the vertical axis. Fig.10 From curve 1110 it can be clearly seen that there is a linear relationship between optical attenuation and stress birefringence caused by pixel arrangements that have been written using laser beam 835 having different power levels.

[0146] therefore, Fig.11 1100 demonstrates that stress birefringence measurements can be used for calibration of the RegC procedure of the transmissive lithography mask 100. The determination of stress birefringence can be used in addition to the conventional calibration procedure. However, the RegC calibration procedure based on the determination of stress birefringence can also replace the present calibration method based on the measurement of the light attenuation caused by the pixels written to the substrate 110.

[0147] Even more importantly, Figure 4 As shown, the apparatus 400 uses a HeNe laser source as the light source 420, so that the stress birefringence is measured at a wavelength of 632 nm. Therefore, the stress birefringence can also be measured for the substrate 310 of the EUV mask 300, which is generally optically transparent in the visible wavelength range. By decoupling the RegC calibration from the actinic wavelength, the method described in this application can be used for both the transmissive lithography mask 100 and the reflective lithography mask 300.

[0148] at last, Fig.12A flow chart 1200 of the method of the present invention is shown. The method starts at 1210. At step 1220, the effect of one or more introduced pixels is determined by determining a change in birefringence of a substrate 110, 310 of a lithography mask 100, 300 having one or more pattern elements 120, 360. This step may be performed by an apparatus 400 designed to perform stress birefringence measurements.

[0149] At step 1230, at least one laser beam parameter is determined based on the determined effect of one or more introduced pixels. Step 1230 is an optional step of the method of the present invention. This is indicated by the dashed box in flowchart 1200. The method ends at step 1340.

Claims

1. A method for determining an effect to be introduced into one or more pixels of a substrate (110, 310) of a lithography mask (100, 300), the lithography mask (100, 300) having one or more pattern elements (120, 360), wherein the one or more pixels are used to at least partially correct one or more errors (190, 390) of the lithography mask (100, 300), the method comprising: determining an effect of the one or more pixels by determining a birefringence variation of the substrate (110, 310) of the lithography mask (100, 300) having the one or more pattern elements (120, 360), wherein determining the effect of the one or more pixels comprises determining the birefringence variation as a function of at least one laser beam parameter of a laser system (730) used to introduce the one or more pixels into the substrate (110, 310) of the lithography mask (100, 300), wherein determining the birefringence variation comprises using a transmission optical birefringence measurement system using a wavelength greater than an actinic wavelength; By determining the stress-induced change or variation in birefringence introduced into the substrate by one or more pixels based on one or more laser beam parameters, a calibration curve is determined for controlling the pixel writing process.

2. The method of claim 1 , further comprising the step of controlling at least one laser beam parameter of the laser system (730) based on the determined birefringence change to correct one or more errors (190, 390) of the photolithography mask (100, 300) when writing the one or more pixels into the substrate (110, 310) of the photolithography mask (100, 300).

3. The method of any of the preceding claims, wherein the at least one laser beam parameter comprises at least one of: power, pulse length, pulse density, focal width, focal depth, wavelength, wavefront, and polarization of the laser beam (735).

4. The method of claim 1 or 2, further comprising the step of determining a change in the optical transmission of the substrate (110, 310) as a function of the at least one laser beam parameter.

5. The method of claim 1 or 2, further comprising the step of coupling the birefringence variation to an optical transmission variation caused by one or more pixels introduced into the substrate (110, 310), the at least one laser beam parameter being a parameter.

6. The method of claim 2, wherein controlling the at least one laser beam parameter comprises limiting the value of the at least one laser beam parameter so that the one or more pixels introduced into the substrate (110, 310) does not locally exceed a predetermined critical value of the variation of the optical transmittance of the substrate (110, 310) through the photolithography mask (100, 300).

7. The method of claim 1 or 2, further comprising the step of determining the change in the optical transmission of the substrate (110, 310) at a wavelength used by the laser system (730) to introduce the one or more pixels into the substrate (110, 310).

8. The method of claim 1 or 2, further comprising the step of determining the optical transmission variation as a function of the depth and / or lateral position of the substrate (110, 310) at which the one or more pixels are to be introduced into the substrate (110, 310).

9. A method as claimed in any of the preceding claims, wherein the substrate (110, 310) has a coating (375) on a rear surface (370) of the substrate (310), the coating (375) being electrically conductive and at least partially optically transmissive at a wavelength at which the one or more pixels are introduced to the substrate (310).

10. The method of claim 9, further comprising the step of determining a change in optical transmission of the substrate (310) and / or the coating (375) at a wavelength used by the laser system (730) to introduce the plurality of pixels into the substrate (310).

11. The method of claim 10, wherein determining a change in optical transmission of the substrate (310) and / or the coating (375) comprises determining the change in optical transmission as a function of a lateral position of the substrate (310) of the photolithography mask (300).

12. The method of claim 10, further comprising the step of determining a change in optical transmission of the substrate (310) and the coating (375) as a function of the depth and / or lateral position of the substrate (310) at which the one or more pixels are to be introduced into the substrate (310).

13. A computer program product comprising instructions for causing a computer system (760) to perform the steps of any one of claims 1 to 12.

14. An apparatus (400, 800) for determining an effect to be introduced into one or more pixels of a substrate (110, 310) of a lithography mask (100, 300), the lithography mask (100, 300) having one or more pattern elements (120, 360), wherein the one or more pixels are used to at least partially correct one or more errors (190, 390) of the lithography mask (100, 300), the apparatus (400, 800) comprising: a determining device for determining an effect of the one or more pixels by determining a birefringence variation of a substrate (110, 310) of the photolithography mask (100, 300) having the one or more pattern elements (120, 360), wherein determining the effect of the one or more pixels comprises determining the birefringence variation as a function of at least one laser beam parameter of a laser system (730) for introducing the one or more pixels into the substrate (110, 310) of the photolithography mask (100, 300), wherein the determining device for determining the birefringence variation comprises using a transmission optical birefringence measurement system using a wavelength greater than the actinic wavelength of the photolithography mask (100, 300); By determining the stress-induced change or variation in birefringence introduced into the substrate by one or more pixels based on one or more laser beam parameters, a calibration curve is determined for controlling the pixel writing process.

15. The apparatus (400, 800) of claim 14, wherein the determining means for determining the effect of the one or more pixels by determining the birefringence variation comprises at least one of: a polarizer, an ellipsometer, or a birefringence imaging system (400).

16. The device (400, 800) of claim 14 or 15, further comprising an optical measurement system (500) adapted to determine an optical reflection and / or an optical transmission of the substrate (110, 310) and / or a coating (375) disposed on the substrate (110, 310).

17. The apparatus (400, 800) of claim 14 or 15, wherein the apparatus (900) further comprises a pixel writing system (700) for correcting the one or more errors (190, 390).

18. The apparatus (400, 800) of claim 14 or 15, wherein the apparatus (400, 800) is adapted to perform the steps of any one of claims 1 to 12.