Electroluminescent device and display device including the same
By adopting a double-layer luminescent structure in quantum dot electroluminescent devices, the hole-electron balance is ensured by using n-type metal oxides, which solves the problem of unstable holes and electron flow in electroluminescent devices, and improves the luminescent efficiency and lifetime .
Patent Information
- Application Number
- CN202011201636.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-30
- Filing Date
- 2020-11-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-11-02
AI Technical Summary
The flow of holes and electrons in quantum dot electroluminescent devices is unstable, resulting in excitons recombining in non-luminescent layers, with low efficiency and short lifetime.
A double-layer luminescent structure is adopted, one of which contains n-type metal oxides, ensuring stable hole-electron equilibrium in the luminescent layer, and improving luminescent efficiency and lifetime by adjusting the recombination position of electrons and holes.
The improvement of luminescence efficiency and lifetime in quantum dot electroluminescent devices is achieved, and the hole-electron balance is ensured through the double-layer luminescent structure, reducing the capture and quenching of excitons in the non-luminescent layer.
Smart Images

Figure CN112750966B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2019-0137993, filed on October 31, 2019, and Korean Patent Application No. 10-2020-0142938, filed on October 30, 2020, in the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference. Technical Field
[0003] Disclosed are an electroluminescent device and a display apparatus including the same. Background Art
[0004] Quantum dots are nanocrystals of semiconductor materials with a diameter of about several nanometers to tens of nanometers, which exhibit a quantum confinement effect. Compared with commonly used phosphors, quantum dots produce stronger light in a narrow wavelength region. When excited electrons transition from the conduction band to the valence band, quantum dots emit light, and the wavelength varies depending on the particle size, even in the same material. Since quantum dots emit shorter wavelength light with smaller particle sizes, quantum dots can provide light in a desired wavelength region by adjusting the size.
[0005] In other words, compared to an organic light emitting diode using a light emitting layer including phosphorescent and / or fluorescent materials, a light emitting layer including quantum dots and various types of electronic devices including the same can generally save manufacturing costs, and can emit desirable colors by changing the size of the quantum dots without using other organic materials in the light emitting layer to emit light of other colors.
[0006] The luminous efficiency of the light-emitting layer including quantum dots is determined by the quantum efficiency of the quantum dots, the balance of charge carriers, the light extraction efficiency, etc. In particular, in order to improve the quantum efficiency, the excitons may be confined in the light-emitting layer, but when the excitons are not confined in the light-emitting layer due to various factors, it may cause problems such as exciton quenching. Summary of the invention
[0007] Embodiments provide an electroluminescent device having improved luminous efficiency and lifespan, and a display apparatus including the same.
[0008] According to one embodiment, an electroluminescent device includes: a first electrode and a second electrode facing each other; and a light-emitting layer arranged between the first electrode and the second electrode; wherein the light-emitting layer includes a first light-emitting layer arranged on the first electrode side and including first quantum dots, and a second light-emitting layer arranged on the second electrode side and including second quantum dots and an n-type metal oxide.
[0009] The second quantum dots may emit a first light belonging to a predetermined wavelength region, and may include the n-type metal oxide in an amount greater than about 0 wt % and less than or equal to about 20 wt % based on the total weight of the second light emitting layer.
[0010] The n-type metal oxide may include an oxide of a metal including zinc (Zn), magnesium (Mg), tin (Sn), zirconium (Zr), titanium (Ti), aluminum (Al), or a combination thereof.
[0011] The n-type metal oxide may be dispersed in the second light emitting layer.
[0012] The n-type metal oxide may include a hydrophobic organic material attached (connected) to at least a portion of a surface thereof.
[0013] The n-type metal oxide may have an average particle diameter of about 1 nm to about 10 nm.
[0014] The first light emitting layer may further include a p-type semiconductor.
[0015] The p-type semiconductor may include a p-type single-molecule organic semiconductor, a p-type oxide semiconductor, or a combination thereof.
[0016] The p-type organic material may be included in an amount greater than about 0 wt % and less than or equal to about 20 wt % based on the total weight of the first light emitting layer.
[0017] The light emitting layer may have a charge balance factor, which is a ratio (HT / ET) of hole transport capability (HT) to electron transport capability (ET), of greater than about 0.20 and less than about 0.56.
[0018] The light emitting layer may have a thickness of about 10 nm to about 60 nm.
[0019] At least one of the first quantum dot and the second quantum dot may include a core including a first semiconductor nanocrystal, and a shell including a second semiconductor nanocrystal having a different composition from the first semiconductor nanocrystal and disposed on the core.
[0020] A ligand may be attached to at least one of the first quantum dot and the second quantum dot, the ligand including a moiety derived from a metal halide compound, a moiety derived from a carboxylic acid-based compound, a moiety derived from a thiol compound, or a combination thereof.
[0021] The electroluminescent device may or may not further include a hole transport layer disposed between the first electrode and the light emitting layer.
[0022] The electroluminescent device may further include the hole transport layer, and the hole transport layer may include poly(3,4-ethylenedioxythiophene) derivatives, poly(styrene sulfonate) derivatives, poly-N-vinylcarbazole derivatives, polyphenylene vinylene derivatives such as poly-p-phenylene vinylene derivatives, polymethacrylate derivatives, polyarylamine (polyarylamine) derivatives, polyaniline derivatives, polypyrrole derivatives, poly(9,9-dioctylfluorene) derivatives, poly(spiro-bifluorene) derivatives, tris(4-carbocyanine) derivatives, poly(vinyl)sulfonate ... oxazol-9-ylphenyl)amine (TCTA), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine (NPB), tris(3-methylphenylamino)triphenylamine (m-MTDATA), poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine (poly-TPD), NiO, MoO 3 , or a combination thereof.
[0023] The electroluminescent device may or may not further include an electron transport layer disposed between the second electrode and the light emitting layer.
[0024] The electroluminescent device may further include the electron transport layer, and the electron transport layer may include inorganic material nanoparticles, quinolone compounds, triazine-based compounds, quinoline-based compounds, triazole-based compounds, naphthalene-based compounds, or a combination thereof.
[0025] The inorganic material nanoparticles may include a salt of a metal including zinc (Zn), magnesium (Mg), tin (Sn), zirconium (Zr), titanium (Ti), aluminum (Al), or a combination thereof.
[0026] The electroluminescent device may further include a hole transport layer disposed between the first electrode and the first light-emitting layer and including an organic material, and an electron transport layer disposed between the second electrode and the second light-emitting layer and including an inorganic material, and wherein the first light-emitting layer may include a p-type organic material.
[0027] According to another embodiment, a display device including the electroluminescent device is provided.
[0028] Provided are an electroluminescent device having improved luminous efficiency and lifespan and a display apparatus including the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a schematic cross-sectional view of an electroluminescent device according to one embodiment,
[0030] Figure 2Schematically displayed Figure 1 The energy level diagram of
[0031] Figure 3 To schematically show a cross-sectional view of an electroluminescent device according to another embodiment,
[0032] Figure 4 Schematically displayed Figure 3 The energy level diagram of
[0033] Figure 5 is a voltage-current density diagram of a hole-only device (HOD) according to Verification Example 1 and Verification Comparative Example 1,
[0034] Figure 6 is a voltage-current density diagram of the electronic device (EOD) only according to Verification Examples 2-4 and Verification Comparative Example 2,
[0035] Figure 7 is the voltage-brightness (unit: cd / m 2 )picture,
[0036] Figure 8 is a time-voltage (unit: V) diagram of the electroluminescent devices according to Comparative Examples 1, 4, and 5,
[0037] Fig. 9 is a T50-initial voltage diagram for an electroluminescent device including a blue double-emitting layer and an electroluminescent device including a blue single-emitting layer,
[0038] Fig.10 and 11 To show the external quantum efficiency ( Fig.10 ) and maximum brightness (unit: cd / cm 2 )( Fig.11 ) diagram of the changes in
[0039] Fig.12 and 13 To show the external quantum efficiency ( Fig.12 ) and maximum brightness (unit: cd / cm 2 )( Fig.13 ) diagram of the changes in
[0040] Fig.14 is the brightness of the electroluminescent devices according to Example 7 and Comparative Example 6 (unit: cd / cm 2 )-EQE diagram,
[0041] Fig.15is a voltage-current density diagram of the electroluminescent device according to Example 7 and Comparative Example 6,
[0042] Fig.16 is a time-brightness (unit: %) graph of the electroluminescent device according to Example 7 and Comparative Example 6,
[0043] Fig.17 is a time-voltage diagram of the electroluminescent device according to Example 7 and Comparative Example 6,
[0044] Fig.18 is a voltage-current density graph of the electroluminescent devices according to Examples 8 to 10, Comparative Example 1 and Comparative Example 7, and
[0045] Fig.19 is the brightness of the electroluminescent devices according to Examples 9 and 10 and Comparative Example 1 (unit: cd / cm 2 )-EQE diagram. DETAILED DESCRIPTION
[0046] Hereinafter, example embodiments of the present disclosure will be described in detail and can be easily implemented by persons with ordinary skills in the relevant field. However, the present disclosure can be embodied in many different forms and will not be construed as limited to the example embodiments set forth herein.
[0047] In the accompanying drawings, the thickness of layers, films, panels, regions, etc. is exaggerated for clarity. Throughout the specification, the same reference numerals represent the same elements. It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it may be directly on the other element, or there may be intermediate elements. On the contrary, when an element is referred to as being "directly on" another element, there are no intermediate elements.
[0048] As used herein, when no definition is otherwise provided, "thickness" refers to "average thickness".
[0049] The “average thickness” means the arithmetic mean of the thickness of a measurement object (eg, a layer, etc.) obtained from several to several tens of random scanning electron microscope images.
[0050] As used herein, for the average diameter of particles in the present disclosure, although it can be numerated by measurement to show the average size of a group, methods generally used include a mode diameter showing the maximum value of the distribution, a median diameter corresponding to the central value of the integrated distribution curve, a variety of average diameters (number average, length average, area average, mass average, volume average, etc.), etc. As used herein, unless otherwise specifically mentioned, the average particle diameter in the present disclosure means a quantitative average diameter, and it is obtained by measuring D50 (particle diameter at the position of 50% of the distribution rate).
[0051] As used herein, "Group" refers to a Group of the Periodic Table.
[0052] As used herein, “Group II” refers to Group IIA and Group IIB, and examples of Group II metals may be Cd, Zn, Hg, and Mg, but are not limited thereto.
[0053] As used herein, “Group II metal excluding Cd” refers to Group II metals other than Cd, such as Zn, Hg, Mg, and the like.
[0054] As used herein, “Group III” refers to Group IIIA and Group IIIB, and examples of Group III metals may be Al, In, Ga, and Tl, but are not limited thereto.
[0055] As used herein, "Group IV" refers to Group IVA and Group IVB, and examples of Group IV metals may be Si, Ge, and Sn, but are not limited thereto. As used herein, the term "metal" may include semimetals such as Si.
[0056] As used herein, “Group I” refers to Group IA and Group IB, and examples may include Li, Na, K, Rb, and Cs, but are not limited thereto.
[0057] As used herein, “Group V” refers to Group VA, and examples may include nitrogen, phosphorus, arsenic, antimony, and bismuth, but are not limited thereto.
[0058] As used herein, "Group VI" refers to Group VIA, and examples may include sulfur, selenium, and tellurium, but are not limited thereto.
[0059] An electroluminescent device including quantum dots (hereinafter referred to as a quantum dot electroluminescent device) is attracting attention as a next-generation display device due to high color reproducibility and ease of solution processing of quantum dots.
[0060] However, in a quantum dot electroluminescent device, the flow of holes in a light-emitting layer including quantum dots is generally not smooth (smooth) compared to the flow of electrons in an electric field of constant intensity. Therefore, a quantum dot electroluminescent device may require improvements in the following matters.
[0061] For example, the charges (electrons, holes) injected toward the light-emitting layer tend to recombine mainly at the interface between the hole transport layer and the light-emitting layer or inside the hole transport layer and / or the light-emitting layer near the interface. Here, the excitons inside the quantum dot electroluminescent device can be captured and quenched by several energy levels generated at the interface between the hole transport layer and the light-emitting layer and / or in the internal conduction band of the hole transport layer and / or the light-emitting layer near the interface.
[0062] Alternatively, the injected electrons and holes may not be in the light-emitting layer, but in the non-light-emitting layer (hole transport layer) to recombine and thus form excitons. Here, the excitons formed in the non-light-emitting layer do not contribute to the light emission of the device, but are quenched and thus can deteriorate the efficiency of the quantum dot electroluminescent device.
[0063] Alternatively, uncombined excess electrons among the injected electrons and holes continuously (persistently) exist at the interface between the hole transport layer and the light-emitting layer, and thus may cause deterioration of the material included in the light-emitting layer and / or the hole transport layer. In addition, excess electrons may cause surface defects at the interface between the hole transport layer and / or the light-emitting layer. These surface defects may quench excitons and, in addition, accelerate the deterioration of the device when driven at a constant current.
[0064] Therefore, the present inventors have conducted research on a method for ensuring a stable hole-electron balance inside a quantum dot electroluminescent device and thereby improving the luminous efficiency and lifetime characteristics of the device.
[0065] As a result, the inventors found that when the light-emitting layer of a quantum dot electroluminescent device is configured to have two or more layers, and when the light-emitting layer adjacent to the electron transport layer among the two or more light-emitting layers includes an n-type metal oxide, a stable hole-electron balance within the light-emitting layer can be ensured, and the recombination position of electrons and holes can be adjusted from the interface or periphery of the light-emitting layer to the interior of the light-emitting layer to achieve improved luminous efficiency and lifetime characteristics, thereby completing the present invention.
[0066] Therefore, refer to Figure 1 , a schematic configuration of an electroluminescent device according to an embodiment will be described.
[0067] Figure 1FIG. 1 is a cross-sectional view schematically showing an electroluminescent device according to an embodiment. The electroluminescent device 10 according to an embodiment includes a first electrode 110 and a second electrode 160 facing each other, and a light emitting layer 140 disposed between the first electrode 110 and the second electrode 160 .
[0068] In an embodiment, the electroluminescent device 10 may or may not further include a hole transport layer 130 disposed between the first electrode 110 and the light-emitting layer 140, a hole injection layer 120 disposed between the first electrode 110 and the hole transport layer 130 and optionally omitted in consideration of the relationship with each constituent element, and an electron transport layer 150 disposed between the second electrode 160 and the light-emitting layer 140.
[0069] In an embodiment, the light-emitting layer 140 may be a multilayer (particularly a double layer) including: a first light-emitting layer 141 disposed on the hole transport layer 130 and including first quantum dots 141a, and a second light-emitting layer 142 disposed on the first light-emitting layer 141 and including second quantum dots 142a and an n-type metal oxide 142b.
[0070] That is, the electroluminescent device 10 may have a stacked structure in which the hole injection layer 120, the hole transport layer 130, the light emitting layer 140 including the first and second light emitting layers 141 and 142, and the electron transport layer 150 are sequentially between the first and second electrodes 110 and 160 facing each other.
[0071] In an embodiment, the first electrode 110 may be directly connected to a driving power source, and thus may play a role in causing current to flow to the light emitting layer 140. The first electrode 110 may include a material having light transmittance (transmittance) in at least a visible light wavelength region, but is not necessarily limited thereto. The first electrode 110 may include a material having light transmittance in an infrared or ultraviolet (UV) wavelength region. For example, the first electrode 110 may be an optically transparent material.
[0072] In an implementation, the first electrode 110 may include molybdenum oxide, tungsten oxide, vanadium oxide, rhenium oxide, niobium oxide, tantalum oxide, titanium oxide, zinc oxide, nickel oxide, copper oxide, cobalt oxide, manganese oxide, chromium oxide, indium oxide, or a combination thereof.
[0073] However, according to one embodiment, the first electrode 110 is not necessarily limited thereto, but may include a material that is further light-transmissive with respect to light in an infrared or ultraviolet (UV) wavelength region, or a semi-transmissive material that selectively transmits light in a specific wavelength region, and implements the function of reflecting light in the visible light wavelength region and returning it toward the second electrode 160.
[0074] Meanwhile, in an embodiment, the first electrode 110 may be disposed on the substrate 100, such as Figure 1 As shown in . The substrate 100 may be a transparent insulating substrate or may be made of a tough material. The substrate 100 may include a polymer material or glass in the form of a film having a glass transition temperature (Tg) greater than about 150° C. For example, it includes a material based on COC (cyclic olefin copolymer) or COP (cyclic olefin polymer (homopolymer)).
[0075] In an embodiment, the substrate 100 may support the hole injection layer 120, the hole transport layer 130, the light emitting layer 140, and the electron transport layer 150 disposed between the first electrode 110 and the second electrode 160. However, the substrate 100 of the electroluminescent device 10 according to an embodiment may not be disposed under the first electrode 110, but the substrate 100 may be disposed on the second electrode 160 or may be omitted, as desired.
[0076] The second electrode 160 includes an optically transparent material and may function as a light-transmitting electrode to transmit light generated in the light-emitting layer 140. In an embodiment, the second electrode 160 may include at least one selected from the group consisting of silver (Ag), aluminum (Al), copper (Cu), gold (Au), and alloys thereof, molybdenum oxide, tungsten oxide, vanadium oxide, rhenium oxide, niobium oxide, tantalum oxide, titanium oxide, zinc oxide, nickel oxide, copper oxide, cobalt oxide, manganese oxide, chromium oxide, indium oxide, or a combination thereof.
[0077] However, the second electrode 160 according to the embodiment is not necessarily limited thereto but may include a semi-transmissive material that selectively transmits light in a specific wavelength region and implements a function of reflecting light in a visible light wavelength region and returning it toward the first electrode 110 .
[0078] When the second electrode 160 functions as a reflective electrode, the first electrode 110 may be a light-transmitting electrode formed of a material that transmits light in at least a visible wavelength region or a semi-transmitting electrode that selectively transmits light in a specific wavelength region.
[0079] Each of the first electrode 110 and the second electrode 160 may be formed by depositing a material for forming an electrode on the substrate 100 or an organic layer by a method such as sputtering.
[0080] On the other hand, Figure 1 As shown in , the electroluminescent device 10 according to one embodiment may have a general structure in which a substrate 100 and each of constituent elements are disposed in the above stacking order.
[0081] However, the electroluminescent device 10 according to an embodiment is not necessarily limited thereto, but may have various structures within the range satisfying the above-mentioned order of arranging each constituent element. For example, when the substrate 100 is not disposed under the first electrode 110 but disposed on the second electrode 160, the electroluminescent device 10 may have an inverted structure.
[0082] The hole injection layer 120 may be directly disposed on the first electrode 110. The hole injection layer 120 may supply holes into the light emitting layer 140 together with the hole transport layer 130. However, the hole injection layer 120 may be omitted in consideration of the thickness and material of the hole transport layer 130.
[0083] On the other hand, the hole injection layer 120 may be formed of a p-type semiconductor or a material doped with a p-type semiconductor. Examples of the hole injection layer 120 may include poly(3,4-ethylenedioxythiophene) (PEDOT) or a derivative thereof, poly(styrene sulfonate) (PSS) or a derivative thereof, poly-N-vinylcarbazole (PVK) or a derivative thereof, polyphenylene vinylene or a derivative thereof such as poly-p-phenylene vinylene (PPV) or a derivative thereof, polymethacrylate or a derivative thereof, poly(9,9-dioctylfluorene) or a derivative thereof, poly(spiro-bifluorene) or a derivative thereof, tris(4-carbazol-9-ylphenyl)amine (TCTA), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine (NPB), tris(3-methylphenylphenylamino)triphenylamine (m-MTDATA), poly-TPD, a metal oxide such as NiO or MoO 3 , or a combination thereof, but is not necessarily limited thereto.
[0084] The hole transport layer 130 may be disposed on the first electrode 110, for example, on the first electrode 110 and the hole injection layer 120. The hole transport layer 130 may provide and transport holes into the light emitting layer 140. The hole transport layer 130 may be formed directly under the light emitting layer 140, particularly the first light emitting layer 141, to directly contact the light emitting layer 140.
[0085] In an embodiment, the hole transport layer 130 may include a material having a hole transport property. The material having a hole transport property may be a p-type semiconductor or a material doped with a p-type semiconductor. The material having a hole transport property is not limited to a specific material, but may be a polymer, an oligomer, a metal oxide, or a combination thereof.
[0086] Examples of the material having hole transport properties may include poly(3,4-ethylenedioxythiophene) derivatives, poly(styrene sulfonate) derivatives, poly-N-vinylcarbazole derivatives, polyphenylene vinylene derivatives such as poly-p-phenylene vinylene derivatives, polymethacrylate derivatives, polyarylamine derivatives, polyaniline derivatives, polypyrrole derivatives, poly(9,9-dioctylfluorene) derivatives (e.g., poly[(9,9-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-4-butylene)]-4-yl)-1,2-di ... phenyl) diphenylamine)] (TFB)), poly (spiro-bifluorene) derivatives, tri (4-carbazol-9-ylphenyl) amine (TCTA), N, N'-diphenyl-N, N'-bis (3-methylphenyl) - (1, 1'-biphenyl) -4, 4'-diamine (TPD), N, N'-di (naphthalene-1-yl) -N, N'-diphenylbenzidine (NPB), tri (3-methylphenylphenylamino) triphenylamine (m-MTDATA), poly-TPD, NiO, MoO 3 , or a combination thereof, but is not necessarily limited thereto.
[0087] In embodiments, the thickness of the hole transport layer 130 may vary in consideration of the hole-electron balance with the hole injection layer 120, the hole transport layer 130, and / or the light emitting layer 140 in the device. It may be, for example, greater than or equal to about 10 nm, for example, greater than or equal to about 15 nm, or greater than or equal to about 20 nm and, for example, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, or less than or equal to about 50 nm, for example, about 10 nm to about 80 nm, about 10 nm to about 70 nm, about 10 nm to about 60 nm, about 10 nm to about 50 nm, about 10 nm to about 40 nm, or about 20 nm to about 40 nm.
[0088] For example, the hole transport layer 130 may be formed by a wet coating method such as spin coating, etc. For example, both the hole transport layer 130 and the light emitting layer 140, and in particular, both the hole transport layer 130 and the first light emitting layer 141 may be formed by a wet coating method. In this way, the hole transport layer 130 and / or the first light emitting layer 141 may be formed by a simple process.
[0089] In addition, in an embodiment, the hole transport layer 130 and the first light emitting layer 141 may be made of materials having relatively different solubilities. For example, the hole transport layer 130 may be prepared using a material having excellent solubility for an aromatic non-polar solvent, and the first light emitting layer 141 may be prepared using a material having excellent solubility for an aliphatic non-polar solvent. Therefore, even if the hole transport layer 130 and the first light emitting layer 141 are directly contacted using a solution process, due to the different solubilities of the hole transport layer 130 and the first light emitting layer 141, the first light emitting layer 141 may be formed without damaging the surface of the hole transport layer 130.
[0090] For example, when forming a poly[(9,9-dioctylfluorene-2,7-diyl)-co-(4,4′-(N-4-butylphenyl)diphenylamine)] (TFB) polymer film as the hole transport layer 130, a precursor solution including a TFB precursor polymer and an aromatic non-polar solvent (e.g., toluene, xylene, etc.) is spin-coated on the first electrode 110 or the hole injection layer 120. 2 The hole transport layer 130 made of TFB is formed by heat treatment in an inert gas atmosphere or in a vacuum at a temperature of about 150°C to about 180°C for about 30 minutes, and the first light-emitting layer 141 can be easily formed thereon by a solution process using an aliphatic non-polar solvent (e.g., octane, nonane, cyclohexane, etc.).
[0091] In this way, when the hole transport layer 130 and the first light-emitting layer 141 are configured to have different relative solubilities, the formation of the hole transport layer 130 and the first light-emitting layer 141 using a solution process is more easily performed, and during the subsequent formation of the first light-emitting layer 141, surface damage of the hole transport layer 130 caused by the organic solvent can be minimized.
[0092] The light emitting layer 140 may be disposed on the hole transport layer 130 and may include quantum dots. In an embodiment, the light emitting layer 140 may include a first light emitting layer 141 and a second light emitting layer 142 as described above. In an embodiment, the first light emitting layer 141 and the second light emitting layer 142 may each include a quantum dot. Hereinafter, the quantum dots included in the first light emitting layer 141 are referred to as first quantum dots 141a, and the quantum dots included in the second light emitting layer 142 are referred to as second quantum dots 142a.
[0093] The light emitting layer 140 is a location where electrons and holes transmitted by current supplied from the first electrode 110 and the second electrode 160 are recombined to generate excitons, and the generated excitons transition from an excited state to a ground state to emit light of a wavelength corresponding to the size of the quantum dots. That is, the quantum dots can impart an electroluminescent function to the light emitting layer 140.
[0094] In particular, the quantum dots have a discontinuous energy band gap through a quantum confinement effect, and incident light can be converted into light having a specific wavelength and then radiated. Therefore, the light emitting layer 140 including the quantum dots can generate light having excellent color reproducibility and color purity.
[0095] In an embodiment, the light emitting layer 140 may emit light belonging to a predetermined wavelength region through the quantum dots. In an embodiment, the first light emitting layer 141 and the second light emitting layer 142 may each emit a first light belonging to a predetermined wavelength region, respectively. The light emitted by the first and second light emitting layers 141 and 142 may be light belonging to the same wavelength region. That is, the first quantum dot 141a and the second quantum dot 142a may each emit a first light belonging to the same wavelength region. In an embodiment, the first light may be in a wavelength region belonging to the visible light region, such as a first wavelength region of about 380nm-about 488nm, a second wavelength region of about 490nm-about 510nm, a third wavelength region of about 510nm-about 580nm, a fourth wavelength region of about 582nm-about 600nm, and one of a fifth wavelength region of about 620nm-about 680nm.
[0096] In an embodiment, each of the first quantum dot 141a and the second quantum dot 142a may emit blue light belonging to a first wavelength region of about 380 nm to about 488 nm. In this case, the light emitting layer 140 may be a blue light emitting layer.
[0097] In an embodiment, each of the first quantum dot 141a and the second quantum dot 142a may emit red light belonging to a fifth wavelength region of about 620 nm to about 680 nm. In this case, the light emitting layer 140 may be a red light emitting layer.
[0098] In an embodiment, the material of the first and second quantum dots 141 a and 142 a is not particularly limited and known or commercially available quantum dots may be used.
[0099] In an embodiment, at least one of the first quantum dot 141a and the second quantum dot 142a may include: a core including a first semiconductor nanocrystal, and a shell including a second semiconductor nanocrystal disposed on the core, and the second semiconductor nanocrystal may have a composition different from that of the first semiconductor nanocrystal. That is, only one of the first quantum dot 141a and the second quantum dot 142a may have a core-shell structure, or both of the first quantum dot 141a and the second quantum dot 142a may have a core-shell structure.
[0100] In an embodiment, the interface between the core and the shell may have a concentration gradient, wherein the concentration of the element in the shell decreases toward the center. In an embodiment, the quantum dot may have a structure including a core and a shell layer surrounding it (core-single shell structure). In this case, the single shell structure may have a single composition or concentration gradient.
[0101] However, the embodiment is not necessarily limited thereto. At least one of the first quantum dot 141a and the second quantum dot 142a may have a structure including a core and a multilayer shell surrounding the core. Here, the multilayer shell structure has a structure of two or more shells, and each layer may have a single composition or alloy or may have a concentration gradient.
[0102] In this way, when at least one of the first quantum dot 141a and the second quantum dot 142a has a core-shell structure, the material composition constituting the shell may have a band gap energy greater than the band gap energy of the core, and thus has a structure in which a quantum confinement effect is effectively exhibited. However, the embodiment is not necessarily limited to this. On the other hand, even in the case of configuring a multi-layer shell, the shell away from the core may have a larger band gap energy than the shell close to the core. In this case, the quantum dots having a core-multi-layer shell structure among the first quantum dot 141a and the second quantum dot 142a may emit light having a wavelength range from ultraviolet (UV) to infrared.
[0103] In an embodiment, the first semiconductor nanocrystal included in the core and the second semiconductor nanocrystal included in the shell may independently include a II-VI compound, a III-V compound, a IV-VI compound, a IV element or compound, an I-III-VI compound, an I-II-IV-VI compound, or a combination thereof that does not include Cd. That is, each of the first and second quantum dots 141a and 142a may be a quantum dot that does not contain cadmium. Like this, when the first and second quantum dots 141a and 142a are composed of materials that do not contain cadmium, they are not toxic compared to conventional cadmium-based quantum dots, and therefore are not dangerous and are environmentally friendly.
[0104] The II-VI group compound may be selected from: a binary compound selected from ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, MgSe, MgS, and mixtures thereof; a ternary compound selected from ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, HgZnS, HgZnSe, HgZnTe, MgZnSe, MgZnS, and mixtures thereof; and a quaternary compound selected from HgZnTeS, HgZnSeS, HgZnSeTe, HgZnSTe, and mixtures thereof. The II-VI group compound may further include a group III metal.
[0105] The III-V compound may be selected from: a binary compound selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, and mixtures thereof; a ternary compound selected from GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, InZnP, and mixtures thereof; and a quaternary compound selected from GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb, and mixtures thereof. The III-V compound may further include a Group II metal (e.g., InZnP).
[0106] The IV-VI group compound may be selected from: a binary compound selected from SnS, SnSe, SnTe, PbS, PbSe, PbTe, and mixtures thereof; a ternary compound selected from SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, and mixtures thereof; and a quaternary compound selected from SnPbSSe, SnPbSeTe, SnPbSTe, and mixtures thereof. An example of the I-III-VI group compound may be CuInSe 2 、CuInS 2 , CuInGaSe, and CuInGaS, but not limited thereto. Examples of the I-II-IV-VI group compound may be CuZnSnSe and CuZnSnS, but not limited thereto. Examples of the IV group compound may be: a simple substance selected from Si, Ge, and a mixture thereof; and a binary compound selected from SiC, SiGe, and a mixture thereof.
[0107] The binary compound, ternary compound or quaternary compound is present in a uniform concentration in the particle or in locally different concentrations in the same particle, respectively.
[0108] The first and second quantum dots 141a and 142a may independently have a quantum efficiency greater than or equal to about 10%, for example, greater than or equal to about 20%, greater than or equal to about 30%, greater than or equal to about 40%, greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 90%, or even 100%.
[0109] In the display, the first and second quantum dots 141a and 142a may have a relatively narrow emission wavelength spectrum to improve color purity or color reproducibility. The first and second quantum dots 141a and 142a may independently have, for example, a half width (FWHM) of an emission wavelength spectrum of less than or equal to about 45 nm, less than or equal to about 40 nm, or less than or equal to or about 30 nm. Within the range, the color purity or color reproducibility of the device (equipment) may be improved.
[0110] The first and second quantum dots 141a and 142a may independently have a particle diameter of about 1nm to about 100nm (the longest dimension for non-spherical particles). For example, the first and second quantum dots 141a and 142a may independently have, for example, a particle diameter of about 1nm to about 20nm, about 1nm to about 15nm, about 1nm to about 14nm, about 1nm to about 13nm, about 1nm to about 12nm, about 1nm to about 11nm, or about 1nm to about 10nm (the longest dimension for non-spherical particles).
[0111] In addition, the shapes of the first and second quantum dots 141a and 142a may be common shapes in the art, and therefore may not be particularly limited. For example, the quantum dots may be spherical, elliptical, tetrahedral, pyramidal, cuboctahedral, cylindrical, polyhedral, multi-arm or cubic nanoparticles, nanotubes, nanowires, nanofibers, nanosheets, or combinations thereof. The quantum dots may have any cross-sectional shape.
[0112] The first and second quantum dots 141a and 142a may be commercially available or may be synthesized by any method. For example, quantum dots of a few (several) nanometers in size may be synthesized according to a wet chemical process. In a wet chemical process, a precursor reacts in an organic solvent to grow crystal particles, and a surfactant or organic solvent for forming a ligand may coordinate to the surface of the quantum dots to control the growth of the crystal. Examples of the surfactant and organic solvent for forming a ligand are known.
[0113] The surfactant and organic solvent for forming the ligand can be appropriately selected. Examples of the organic solvent may include: C6-C22 primary amines such as hexadecylamine; C6-C22 secondary amines such as dioctylamine; C6-C40 tertiary amines such as trioctylamine; nitrogen-containing heterocyclic compounds such as pyridine; C6-C40 olefins such as octadecene; C6-C40 aliphatic hydrocarbons such as hexane, octane, hexadecane, octadecane or squalane; aromatic hydrocarbons substituted with C6-C30 alkyl groups such as phenyldodecane, phenyltetradecane or phenylhexadecane; primary, secondary or tertiary phosphine (e.g., trioctylphosphine) substituted with at least one (e.g., 1, 2, or 3) C6-C22 alkyl group; phosphine oxide (e.g., trioctylphosphine oxide) substituted with at least one (e.g., 1, 2, or 3) C6-C22 alkyl group; C12-C22 aromatic ethers such as phenyl ether or benzyl ether; or combinations thereof.
[0114] Examples of the surfactant used to form the ligand may include RCOOH, RNH 2 , R 2 NH, R 3 N, RSH, RH 2 PO, R 2 HPO, R 3 PO, RH 2 P.R 2 HP, R 3 P, ROH, RCOOR', RPO(OH) 2 , RHPOOH, R 2 POOH (wherein R and R' are independently hydrogen, a C1-C40 substituted or unsubstituted aliphatic hydrocarbon group, or a C6-C40 substituted or unsubstituted aromatic hydrocarbon group, or a combination thereof, and in each ligand, at least one R is not hydrogen), or a combination thereof, but is not limited thereto.
[0115] Since the organic solvent coordinated to the surface of the quantum dot can affect the stability in the device, the excess material (surfactant, organic solvent, or combination thereof for forming the ligand) that is not coordinated to the surface of the nanocrystal can be removed by pouring them into a non-solvent in excess and centrifuging the resulting mixture. Specific examples of the non-solvent include, but are not limited to, acetone, ethanol, and methanol. After removing the excess material, the amount of the material coordinated to the surface of the quantum dot can be less than or equal to about 50% by weight, such as less than or equal to about 30% by weight, less than or equal to about 20% by weight, or less than or equal to about 10% by weight of the weight of the quantum dot. The material coordinated to the surface of the quantum dot may include a ligand, an organic solvent, or a combination thereof. The material coordinated to the surface of the quantum dot, particularly the ligand, can impart dispersibility to the quantum dot.
[0116] In an embodiment, at least a portion of the surfaces of the first and second quantum dots 141a and 142a may have a ligand attached thereto. In an embodiment, examples of the ligand may be a moiety derived from a metal halide compound, a moiety derived from a carboxylic acid-based compound, a moiety derived from a thiol compound, or a combination thereof.
[0117] In an embodiment, the ligand may be a ligand having a hydrophobic portion (hereinafter referred to as a hydrophobic ligand). In an embodiment, the hydrophobic ligand may include a portion chemically bonded (bonded) to the surface of the quantum dot and a hydrophobic functional group providing hydrophobicity. In an embodiment, an example of the hydrophobic ligand may be a portion derived from a carboxylic acid-based compound, a portion derived from a thiol compound, or a combination thereof.
[0118] Examples of the hydrophobic portion may include a C4-C20 alkyl group, a C4-C20 alkenyl group, a C4-C20 alkynyl group, or a combination thereof, and examples of the portion forming a bond with the surface of the quantum dot may be a carboxylate group (-COO - ) part, thiol group (-SH - )(-S - ) part, etc.
[0119] In an embodiment, examples of the moiety derived from a carboxylic acid-based compound may include moieties derived from fatty acid-based compounds such as oleate, stearate, palmitate, etc. In an embodiment, examples of the moiety derived from a thiol compound may include C6-C20 aliphatic thiolate.
[0120] For example, when the first quantum dot 141a has a hydrophobic ligand as described above, the first light-emitting layer 141 including it can also exhibit non-polarity as a whole. In addition, the first quantum dot to which the hydrophobic ligand is attached has solvent selectivity for a non-polar solvent, particularly an aliphatic non-polar solvent. Therefore, even if the first light-emitting layer 141 is formed on the hole transport layer 130 having solvent selectivity for an aromatic non-polar solvent by using a solution process, damage to the surface of the hole transport layer 130 caused by the organic solvent during the formation of the first light-emitting layer 141 can be minimized.
[0121] However, the embodiment is not necessarily limited thereto. The second quantum dot 142a may have the above-mentioned hydrophobic ligand, or both the first and second quantum dots 141a and 142a may not have the above-mentioned hydrophobic ligand.
[0122] For example, the surface of at least one of the first and second quantum dots 141a and 142a may have a ligand having lower solubility in an organic solvent than a quantum dot having the above-mentioned hydrophobic ligand attached thereto. In this case, an example of the ligand may include a moiety derived from a metal halide compound.
[0123] The metal halide may include zinc, indium, gallium, magnesium, lithium, or a combination thereof, and / or may be in the form of chloride, bromide, iodide, or fluoride. The metal included in the metal halide may be the same as the metal included in the outermost layer of the quantum dot, or they may be different from each other.
[0124] Specific examples of the metal halide may be zinc fluoride, zinc chloride, zinc bromide, zinc iodide, indium fluoride, indium chloride, indium bromide, indium iodide, gallium fluoride, gallium chloride, gallium bromide, gallium iodide, magnesium fluoride, magnesium chloride, magnesium bromide, magnesium iodide, lithium fluoride, lithium chloride, lithium bromide, lithium iodide, or a combination thereof.
[0125] The moiety derived from the metal halide compound may include a moiety that chemically binds (bonds) to the surface of the attached quantum dot. Examples of the moiety that forms a bond on the surface of the quantum dot may include a halogen ion moiety (e.g., F - , Cl - Br - ,I - ). The halogen ion portion can be firmly bound to the surface of the quantum dot and can replace other ligands (e.g., hydrophobic ligands such as oleate, etc.) present on the surface of the quantum dot (e.g., replace them) to passivate the quantum dot.
[0126] The quantum dots having the attached portion derived from the metal halide compound can be obtained by reacting a metal halide solution on a light-emitting layer including quantum dots to which the above-mentioned hydrophobic ligand is attached. At least a portion of the hydrophobic ligand attached to the quantum dots can be partially replaced by the above-mentioned halogen ion. The ratio of the hydrophobic ligand attached to the surface of the quantum dots to the portion derived from the metal halide compound can be variously controlled by adjusting the concentration of the metal halide solution, the reaction time, etc.
[0127] Although not wishing to be bound by any theory, the above-mentioned hydrophobic ligands can reduce the luminescence efficiency of quantum dots because the hydrophobic moiety generally acts as a barrier to electron and hole injection. However, in embodiments, quantum dots having attached moieties derived from metal halide compounds can provide improved passivation and improved charge injection characteristics compared to quantum dots having attached hydrophobic ligands.
[0128] In an embodiment, the thickness of the light emitting layer 140, in particular, the total thickness of the first and second light emitting layers 141 and 142, may vary depending on the type and size of the first and second quantum dots included in each of the first and second light emitting layers 141 and 142, and the type of ligand attached thereto. However, it may be, for example, greater than or equal to about 10 nm, greater than or equal to about 11 nm, greater than or equal to about 12 nm, greater than or equal to about 13 nm, greater than or equal to about 14 nm, greater than or equal to about 15 nm, greater than or equal to about 16 nm, greater than or equal to about 17 nm, greater than or equal to about 18 nm, greater than or equal to about 19 nm, greater than or equal to about 20 nm, greater than or equal to about 25 nm, greater than or equal to about 30 nm, or greater than or equal to about 35 nm. The light emitting layer 140 may include two or more quantum dot monolayers, for example, three or more quantum dot layers, or four or more quantum dot layers. The thickness of the light emitting layer 140 may be less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, or less than or equal to about 40 nm. The thickness of the light emitting layer 140 may be, for example, about 10 nm to about 60 nm, about 15 nm to about 60 nm, about 20 nm to about 60 nm, about 25 nm to about 60 nm, or about 25 nm to about 50 nm.
[0129] The electroluminescent device 10 according to one embodiment may include a predetermined amount of quantum dots to improve the light emitting efficiency of the light emitting layer 140 .
[0130] For example, the total weight of the first and second quantum dots 141a and 142a can be included in an amount as follows: for example, greater than or equal to about 5 weight%, greater than or equal to about 10 weight%, greater than or equal to about 15 weight%, or greater than or equal to about 20 weight% and less than or equal to about 98 weight%, less than or equal to about 95 weight%, less than or equal to about 90 weight%, less than or equal to about 85 weight%, less than or equal to about 80 weight%, less than or equal to about 75 weight%, less than or equal to about 70 weight%, less than or equal to about 65 weight%, less than or equal to about 60 weight%, less than or equal to about 55 weight%, or less than or equal to about 50 weight%, for example, about 5 weight%-about 98 weight%, about 20 weight%-about 98 weight%, about 20 weight%-about 90 weight%, about 20 weight%-about 85 weight%, about 50 weight%-about 85 weight%, or about 50 weight%-about 80 weight%, based on 100 weight% of the light-emitting layer 140.
[0131] However, the embodiments are not necessarily limited thereto. The total amount of the first and second quantum dots 141a and 142a in the light emitting layer 140 may vary depending on the amount of other constituent elements in the light emitting layer 140, the type and / or amount of the ligand used, the material of the first and second quantum dots 141a and 142a, the wavelength range of the emitted light, the thickness of the hole transport layer 130, the light emitting layer 140 and / or the electron transport layer 150, etc.
[0132] In an embodiment, the first light emitting layer 141 may include the first quantum dots 141a described above. The first light emitting layer 141 may provide holes received from the adjacent hole transport layer 130 to the second light emitting layer 142, and the holes are combined with electrons to emit light in a predetermined wavelength region using the first quantum dots 141a.
[0133] In addition, the first light-emitting layer 141 functions as a space in which holes received from the hole transport layer 130 are not supplied to the second light-emitting layer 142. That is, since hole-electron recombination in the second light-emitting layer 142 is suppressed, electrons reaching the first light-emitting layer 141 can be increased. As a result, electron-hole recombination can be concentrated inside the light-emitting layer, particularly inside the first light-emitting layer, rather than at the interface between the light-emitting layer and the hole transport layer. More details about this will be described later with the description of the second light-emitting layer 142.
[0134] In an embodiment, the portion derived from the metal halide compound described above may be attached to the first quantum dot 141a. In an embodiment, greater than or equal to about 10%, for example, greater than or equal to about 20%, greater than or equal to about 30%, greater than or equal to about 40%, greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 90%, greater than or equal to about 91%, greater than or equal to about 92%, greater than or equal to about 93%, greater than or equal to about 94%, greater than or equal to about 95%, greater than or equal to about 96%, greater than or equal to about 97%, or greater than or equal to about 98% of the ligand attached to the surface of the first quantum dot 141a may be the portion derived from the metal halide compound. When the ratio of the portion derived from the metal halide compound attached to the surface of the first quantum dot 141a satisfies the above range, the first light emitting layer 141 may exhibit low solubility in an organic solvent. As a result, even if the second light emitting layer 142 is formed directly on the first light emitting layer 141 by using a solution process, damage to the first light emitting layer 141 may be minimized.
[0135] However, embodiments are not necessarily limited thereto, and the type and / or ratio of ligands attached to the surface of the first quantum dot 141a may vary depending on the presence or absence, type and / or ratio of ligands attached to the surface of the second quantum dot 142a.
[0136] The second light emitting layer 142 is directly formed on the first light emitting layer 141 and may include a second quantum dot 142a and an n-type metal oxide 142b. The second light emitting layer 142 may provide electrons received from the adjacent electron transport layer 150 to the first light emitting layer 141, and the electrons are combined with holes to emit light in a predetermined wavelength region by using the second quantum dot 142a.
[0137] In an embodiment, the first light emitting layer 141 and the second light emitting layer 142 may be separate layers different from each other. For example, the first light emitting layer 141 and the second light emitting layer 142 may be distinguished by the type of the first quantum dots 141a and the second quantum dots 142a, the type of attached ligands, the type of doped materials, etc. They may be distinguished by the amount of the n-type oxide 142b, or may be distinguished by the electron-hole recombination site.
[0138] Figure 2 Schematically displayed Figure 1 Energy level diagram.
[0139] Reference Figure 2 In an embodiment, the n-type metal oxide 142b included in the second light emitting layer 142 may have electron transfer characteristics and / or hole blocking characteristics. Therefore, the second light emitting layer 142 may exhibit improved electron transport properties and / or may serve as an energy barrier for the movement of holes from the first light emitting layer 141 to the second light emitting layer 142.
[0140] In particular, the absolute value of the LUMO (Lowest Unoccupied Molecular Orbital) energy level of the n-type metal oxide 142b may vary depending on the material constituting the electron transport layer 150, the material of the second quantum dot 142a, etc. However, it may be equal to or less than the absolute value of the LUMO energy level of the electron transport layer 150, and may be equal to or greater than the absolute value of the LUMO energy level of the second quantum dot 142a. Therefore, the n-type metal oxide 142b can reduce the energy required for electrons supplied to the second light-emitting layer 142 to move within the second light-emitting layer 142.
[0141] On the other hand, the absolute value of the HOMO (highest occupied molecular orbital) energy level of the n-type metal oxide 142b may be equal to or greater than the absolute value of the HOMO energy level of the second quantum dot 142a. Therefore, the n-type metal oxide 142b may adjust the holes in the first light-emitting layer 141 so that they are not easily transferred to the second light-emitting layer 142 and remain in the first light-emitting layer 141.
[0142] As a result, the electroluminescent device 10 according to one embodiment of the present disclosure can adjust the recombination position of holes and electrons to be inside the light-emitting layer 140, in particular, at the interface between the first light-emitting layer 141 and the second light-emitting layer 142 and / or near the interface, such as Figure 2 as shown in .
[0143] Meanwhile, as the content of the n-type metal oxide 142b included in the second light emitting layer 142 increases, the hole blocking property of the second light emitting layer 142 can be increased proportionally. Even if the second quantum dots 142a and the n-type metal oxide 142b are mixed in the second light emitting layer 142, the energy bands of the second quantum dots 142a and the n-type metal oxide 142b are independently maintained. Therefore, the hole blocking property of the second light emitting layer 142 can be enhanced.
[0144] In this case, the electroluminescent device 10 may not include the electron transport layer 150. By including the second light emitting layer 142 of the n-type metal oxide 142b, the leakage current of the electroluminescent device 10 can be reduced, and the light emission efficiency can be improved. In addition, by not forming the electron transport layer 150, the manufacturing process of the electroluminescent device 10 can be simplified.
[0145] In an embodiment, the n-type metal oxide 142b is not particularly limited as long as it has electron transfer properties and / or hole blocking properties. Examples of the n-type metal oxide 142b may include oxides of metals including zinc (Zn), magnesium (Mg), tin (Sn), zirconium (Zr), titanium (Ti), aluminum (Al), or a combination thereof.
[0146] In an embodiment, the n-type metal oxide 142b may include a compound represented by Chemical Formula 1:
[0147] Chemical formula 1
[0148] Zn 1-x M x O
[0149] In Chemical Formula 1, M is Mg, Sn, Ca, Zr, W, Li, Ti, Y, Al, or a combination thereof, and 0≤x≤0.5.
[0150] In an embodiment, in Chemical Formula 1, M may be magnesium (Mg). In an embodiment, in Chemical Formula 1, x may be greater than or equal to about 0.01 and less than or equal to about 0.3, for example, less than or equal to about 0.15.
[0151] In an embodiment, the n-type metal oxide 142b may be dispersed in the second light emitting layer 142. In an embodiment, the n-type metal oxide 142b may include particles having a size ranging from several nanometers to tens of nanometers.
[0152] The average particle diameter of the n-type metal oxide 142b may vary depending on the size of the second quantum dots 142a in the second light-emitting layer 142, the target thickness of the second light-emitting layer 142, etc., but may be, for example, greater than or equal to about 1 nm, greater than or equal to about 2 nm, or greater than or equal to about 3 nm and, for example, less than or equal to about 10 nm, less than or equal to about 9 nm, less than or equal to about 8 nm, less than or equal to about 7 nm, less than or equal to about 6 nm, or less than or equal to about 5 nm, or, for example, from about 1 nm to about 10 nm, from about 1 nm to about 5 nm, or from about 2 nm to about 5 nm.
[0153] The n-type metal oxide 142b may have a hydrophobic organic material attached to at least a portion of its surface in order to improve dispersibility inside the second light emitting layer 142. For example, the hydrophobic organic material may be coordinated to the surface of the n-type metal oxide 142b.
[0154] Examples of the hydrophobic organic material may include C6-C40 aliphatic hydrocarbons such as hexane, octane, hexadecane, octadecane, or squalane; C6-C20 carboxylic acid-based compounds such as oleate, stearate, or palmitate; and the like.
[0155] In this case, since the n-type metal oxide 142 b is generally hydrophobic due to the hydrophobic organic material, the n-type metal oxide 142 b together with the second quantum dots 142 a to which the hydrophobic ligand is attached may have improved dispersibility with respect to the hydrophobic organic solvent.
[0156] Even if the hydrophobic organic material is attached to the n-type metal oxide 142b, the resistance increased by the hydrophobic organic material is insignificant or has no effect compared to the n-type metal oxide without the hydrophobic organic material attached to the surface. In other words, even if the hydrophobic organic material is attached to the n-type metal oxide 142b, the electron transport characteristics and / or hole blocking characteristics of the n-type metal oxide are not significantly deteriorated.
[0157] For example, when ZnO is used as the n-type metal oxide, the conductivity of ZnO without attached hydrophobic organic material is about 2.2×10 -5 S / cm, while the conductivity of ZnO with attached hexane is about 5.1×10 -4 S / cm; and when ZnMgO is used as the n-type metal oxide, the conductivity of ZnMgO without attached hydrophobic organic material is about 2.4×10 - 9 S / cm, while the conductivity of ZnMgO with attached hexane is about 5.6×10 -9 S / cm.
[0158] However, the embodiments are not necessarily limited thereto, but an n-type metal oxide having no hydrophobic organic material attached to the surface may be used, or a mixture of an n-type metal oxide having a hydrophobic organic material attached to the surface and an n-type metal oxide having no hydrophobic organic material attached to the surface may be used.
[0159] In an embodiment, the content of the n-type metal oxide 142b may vary depending on the wavelength of light emitted from the second light emitting layer 142, but may be, for example, less than or equal to about 20 wt%, less than or equal to about 19 wt%, less than or equal to about 18 wt%, less than or equal to about 17 wt%, less than or equal to about 16 wt%, less than or equal to about 15 wt%, less than or equal to about 12 wt%, less than or equal to about 11 wt%, less than or equal to about 10.5 wt%, or less than or equal to about 10 wt% and, for example, greater than about 0 wt%, greater than or equal to about 1 wt%, greater than or equal to about 2 wt%, or greater than or equal to about 3 wt%, or, for example, greater than about 0 wt% and less than or equal to about 20 wt%, greater than about 0 wt% and less than or equal to about 15 wt%, about 1 wt%-about 11 wt%, or about 2 wt%-about 11 wt%, based on the total weight of the second light emitting layer 142, so that the second light emitting layer 142 can exhibit the above-mentioned electron transfer characteristics and / or hole blocking characteristics. For example, when the second light-emitting layer 142 emits blue light (i.e., includes quantum dots that emit blue light), the content of the n-type metal oxide 142b may be greater than about 0 wt% to about 12 wt%, about 1 wt% to about 11 wt%, about 2 wt% to about 11 wt%, or about 3 wt% to about 10 wt% based on the total weight of the second light-emitting layer 142. When the second light-emitting layer 142 emits red light (i.e., includes quantum dots that emit red light), the content of the n-type metal oxide 142b may be greater than about 0 wt% to about 20 wt%, about 1 wt% to about 17 wt%, or about 3 wt% to about 15 wt% based on the total weight of the second light-emitting layer 142.
[0160] The light-emitting layer 140 is formed of a multilayer of a first light-emitting layer 141 and a second light-emitting layer 142, wherein the electron-hole recombination position is controlled to the interface between the first and second light-emitting layers 141 and 142 and / or near the interface by ensuring the electron-hole balance through the n-type metal oxide 142b included in the second light-emitting layer 142, so that the electroluminescent device 10 including it can show improved luminous efficiency and life characteristics.
[0161] In an embodiment, each of the first and second light emitting layers 141 and 142 may include at least one or more monolayers of at least quantum dots, for example, at least 1.5 or more monolayers.
[0162] The thickness of each of the first and second light-emitting layers 141 and 142 may vary depending on the material of the first and second quantum dots 141a and 142a, the type of ligand, and the amount of other components of each light-emitting layer, but may be, for example, less than or equal to about 50 nm, less than or equal to about 40 nm, less than or equal to about 30 nm, or less than or equal to about 20 nm and, for example, greater than or equal to about 5 nm, greater than or equal to about 6 nm, greater than or equal to about 7 nm, greater than or equal to about 8 nm, greater than or equal to about 9 nm, greater than or equal to about 10 nm, greater than or equal to about 11 nm, greater than or equal to about 12 nm, greater than or equal to about 13 nm, greater than or equal to about 14 nm, or greater than or equal to about 15 nm, or, for example, about 5 nm-about 50 nm, about 5 nm-about 40 nm, about 5 nm-about 30 nm, or about 10 nm-about 30 nm.
[0163] In an embodiment, the first and second light emitting layers 141 and 142 may each have a different thickness range. For example, the first light emitting layer 141 may have a thickness of about 20 nm to about 40 nm, about 20 nm to about 35 nm, about 25 nm to about 35 nm, or about 25 nm to about 30 nm, and the second light emitting layer 142 may have a thickness of about 5 nm to about 20 nm, about 5 nm to about 15 nm, or about 10 nm to about 15 nm.
[0164] In an implementation, the electron transport layer 150 may be disposed between the light emitting layer 140 and the second electrode 160 and, in particular, directly on the second light emitting layer 142 to transport electrons to the light emitting layer 140 .
[0165] In an embodiment, the thickness of the electron transport layer 150 may vary in consideration of the electron-hole balance with the hole injection layer 120, the hole transport layer 130, and / or the light emitting layer 140 in the device, but may be, for example, greater than or equal to about 10 nm, greater than or equal to about 15 nm, or greater than or equal to about 20 nm and, for example, less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, or less than or equal to about 40 nm, or, for example, from about 10 nm to about 100 nm, from about 10 nm to about 60 nm, from about 10 nm to about 50 nm, from about 10 nm to about 40 nm, or from about 15 nm to about 40 nm.
[0166] When the electron transport layer 150 has a thickness exceeding the above range, voids, cracks, etc. on the electron transport layer 150 have a greater influence on the electron transport properties and thus greatly deteriorate the device characteristics, and electron-hole balance with other constituent elements in the electroluminescent device 10 is hardly achieved.
[0167] In an implementation, the electron transport layer 150 may be formed of an electron transport material that does not emit light by an electric field and thus does not internally quench electrons.
[0168] Meanwhile, the electron transport layer 150 may include inorganic material nanoparticles or may be an organic layer formed by deposition. For example, the electron transport layer 150 may include inorganic material nanoparticles, quinolone-based compounds, triazine-based compounds, quinoline-based compounds, triazole-based compounds, naphthalene-based compounds, or a combination thereof.
[0169] In an embodiment, the electron transport layer 150 may include inorganic material nanoparticles. The inorganic material nanoparticles may impart electron transport properties to the electron transport layer 150 and do not exhibit luminescent properties. Examples of the inorganic material nanoparticles may be salts of metals including zinc (Zn), magnesium (Mg), tin (Sn), zirconium (Zr), titanium (Ti), aluminum (Al), or a combination thereof. The inorganic material nanoparticles may be made of the same material as the above-mentioned n-type metal oxide, or may be made of a material different from the above-mentioned n-type metal oxide.
[0170] In an embodiment, the electron transport layer 150 may include two or more inorganic material nanoparticles. In an embodiment, the electron transport layer 150 may include a cluster layer composed of a plurality of inorganic material nanoparticles. In an embodiment, the electron transport layer 150 may be a cluster layer composed of two or more inorganic material nanoparticles.
[0171] Meanwhile, an electron injection layer for facilitating injection of electrons and / or a hole blocking layer for preventing movement of holes may be further formed between the electron transport layer 150 and the second electrode 160 .
[0172] The thickness of the electron injection layer and the hole blocking layer may be appropriately selected. For example, the thickness of each of the layers may be greater than or equal to about 1 nm and less than or equal to about 500 nm, but is not limited thereto. The electron injection layer may be an organic layer formed by deposition.
[0173] The electron injection layer may include, for example, at least one selected from the group consisting of 1,4,5,8-naphthalene-tetracarboxylic dianhydride (NTCDA), bathocuproin (BCP), tris[3-(3-pyridyl)- yl]borane (3TPYMB), LiF, Alq 3 , Gaq 3 、Inq 3 、Znq 2 、Zn(BTZ) 2 、BeBq 2, ET204 (8-(4-(4,6-di(naphthalene-2-yl)-1,3,5-triazine-2-yl)phenyl)quinolone), 8-hydroxyquinoline lithium (Liq), n-type metal oxides (e.g., ZnO, HfO 2 etc.), Bphen, and combinations thereof, but are not limited thereto.
[0174] The hole blocking layer may include, for example, at least one selected from the group consisting of 1,4,5,8-naphthalene-tetracarboxylic dianhydride (NTCDA), bathocuproin (BCP), tris[3-(3-pyridyl)- yl]borane (3TPYMB), LiF, Alq 3 , Gaq 3 、Inq 3 、Znq 2 、Zn(BTZ) 2 、BeBq 2 , and combinations thereof, but are not limited thereto.
[0175] As described above, in the electroluminescent device 10 according to an embodiment, the light emitting layer 140 includes a plurality of first and second light emitting layers 141 and 142, wherein the electron-hole recombination position can be controlled to the interface between the first and second light emitting layers 141 and 142 and / or near the interface by ensuring electron-hole balance through the n-type metal oxide 142b included in the second light emitting layer 142. As a result, the electroluminescent device 10 can show improved light emitting efficiency and life characteristics.
[0176] In the following, reference is made to Figure 3-4 An electroluminescent device 10' according to another embodiment is described. In order to describe an electroluminescent device 10' according to another embodiment, detailed descriptions about the same constituent elements as those in the electroluminescent device 10 are omitted.
[0177] Figure 3 2 is a cross-sectional view schematically showing an electroluminescent device according to another embodiment. Figure 4 Schematically displayed Figure 3 Energy level diagram.
[0178] Reference Figure 3-4 The electroluminescent device 10 ′ according to another embodiment has the same constituent elements as those of the electroluminescent device 10 according to one embodiment, except that the first light emitting layer 141 further includes a p-type semiconductor 141 b in addition to the first quantum dots 141 a .
[0179] In another embodiment, the p-type semiconductor 141 b included in the first light emitting layer 141 is not particularly limited as long as it has a hole transfer property and / or an electron blocking property.
[0180] In another embodiment, examples of the p-type semiconductor 141 b may include a p-type single-molecule organic semiconductor, a p-type oxide semiconductor, or a combination thereof.
[0181] Examples of the p-type single-molecule organic semiconductor may be tris(4-carbazol-9-ylphenyl)amine (TCTA), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-2,7-diamino-9,9-spiro-bifluorene (spiro-TPD), N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-9,9-dioctylfluorene (DOFL-TPD), N,N'-di(naphthalene-1-yl)-N,N'-diphenyl-benzidine (NPB), N2,N7-di(naphthalene-1-yl)-9,9-dioctyl-N2,N7-diphenyl-9H-fluorene-2,7-diamine (DOFL-NPB), Tris(3-methylphenylphenylamino)-triphenylamine (m-MTDATA), dipyrazino[2,3-f:2',3'-h]quinoxaline-2,3,6,7,10,11-hexanitrile (HAT-CN), di-[4-(N,N-di-p-tolylamino)-phenyl]cyclohexane (TAPC), N,N'-(4,4'-(cyclohexane-1,1-diyl)bis(4,1-phenylene))bis(N-(4-(6-(2-ethyloxetane-2-yloxy)hexyl)phenyl)-3,4,5-trifluoroaniline) (X-F6-TAPC), 4,4'-bis(N-carbazolyl)-1,1'-biphenyl (CBP), 2,6-bis(3-(9H-carbazol-9-yl)phenyl)pyridine (26DCzPPy), or a combination thereof.
[0182] Examples of the p-type oxide semiconductor may include oxides including vanadium (V), molybdenum (MO), nickel (Ni), copper (Cu), chromium (Cr), graphene, or a combination thereof.
[0183] In an embodiment, the p-type semiconductor 141b may be, for example, in the following amount: for example, less than or equal to about 20 wt%, less than or equal to about 15 wt%, less than or equal to about 14 wt%, less than or equal to about 13 wt%, less than or equal to about 12 wt%, less than or equal to about 11 wt%, or less than or equal to about 10 wt% and, for example, greater than 0 wt%, greater than or equal to about 1 wt%, greater than or equal to about 2 wt%, or greater than or equal to about 3 wt%, or, for example, greater than about 0 wt% and less than or equal to about 20 wt%, greater than about 0 wt% and less than or equal to about 15 wt%, greater than about 0 wt% and less than or equal to about 12 wt%, greater than about 0 wt% and less than or equal to about 11 wt%, about 1 wt%-about 11 wt%, or about 2 wt%-about 11 wt%, based on the total weight of the first light emitting layer 141, so that the first light emitting layer 141 can exhibit the above-mentioned hole transfer characteristics and / or electron blocking characteristics.
[0184] According to another embodiment, although it may differ depending on the material used for the hole transport layer 130, the material used for the first quantum dot 141a, etc., the absolute value of the LUMO (Lowest Unoccupied Molecular Orbital) energy level of the p-type semiconductor 141b may be equal to or lower than the absolute value of the LUMO energy level of the hole transport layer 130, and may be the same as or smaller than the absolute value of the LUMO energy level of the first quantum dot 141a. Thus, the p-type semiconductor 141b can reduce the energy required to transfer holes supplied to the first light emitting layer 141 in the first light emitting layer 141.
[0185] On the other hand, the absolute value of the HOMO (highest occupied molecular orbital) energy level of the p-type semiconductor 141b may be equal to or lower than the absolute value of the HOMO energy level of the second quantum dot 142a. Therefore, the p-type semiconductor 141b may adjust the electrons in the second light-emitting layer 142 to not be easily transferred to the first light-emitting layer 141 and remain in the second light-emitting layer 142.
[0186] As a result, the electroluminescent device 10' according to another embodiment can adjust the recombination position of holes and electrons to be inside the light-emitting layer 140, in particular, at the interface between the first light-emitting layer 141 and the second light-emitting layer 142 and / or near the interface, such as Figure 4 That is, the electroluminescent device 10' according to another embodiment may be configured to form a pn junction of a first light emitting layer 141 including a p-type semiconductor 141b and a second light emitting layer 142 including an n-type metal oxide 142b, and thus the electron-hole recombination position may be adjusted to be at the interface between the first and second light emitting layers 141 and 142 and / or near the interface.
[0187] In addition, as the content of the p-type semiconductor 141b included in the first light emitting layer 141 increases, the electron blocking property of the first light emitting layer 141 can be increased proportionally. Even if the first quantum dot 141a and the p-type semiconductor 141b are mixed in the first light emitting layer 141, the energy bands of the first quantum dot 141a and the p-type semiconductor 141b are independently maintained. Therefore, the electron blocking property of the first light emitting layer 141 can be enhanced.
[0188] In this case, the electroluminescent device 10 may not include the hole transport layer 130. Even if the electroluminescent device 10 does not include the hole transport layer 130, the first light emitting layer 141 including the p-type semiconductor 141b may replace the hole transport layer 130.
[0189] As a review of the above, the electroluminescent device 10, 10' is formed by including first and second light emitting layers 141, wherein the second light emitting layer 142 includes at least an n-type metal oxide 142b, or in addition, the first light emitting layer 141 further includes a p-type semiconductor 141b, so that it can show improved light emitting characteristics and life characteristics.
[0190] In an embodiment, the light emitting layer 140 has a charge balance factor greater than about 0.20 and less than about 0.56, which is a ratio (HT / ET) of a hole transport capability (HT) measured at a predetermined voltage (e.g., at about 1 volt to about 12 volts or at 3.5 volts) to an electron transport capability (ET) measured at a predetermined voltage (e.g., at about 1 volt to about 12 volts or at 3.5 volts).
[0191] In order to obtain the charge balance factor of the light emitting layer 140 including the first light emitting layer 141 and the second light emitting layer 142, the more dominant carrier transport capability is measured in each of the first light emitting layer 141 and the second light emitting layer 142. That is, in the second light emitting layer 142 including the n-type metal oxide 142b, the electron transport capability (ET) is measured, and in the first light emitting layer 141 which may or may not further include the p-type semiconductor 141b, the hole transport capability (HT) is measured.
[0192] Electron transport capability (ET) can be obtained by an electron-only device (hereinafter referred to as EOD) in which the second light-emitting layer 142 including an n-type metal oxide 142b is formed as a single emission layer, and hole transport capability (HT) can be obtained by a hole-only device (hereinafter referred to as HOD) in which the first light-emitting layer 141 may or may not further include a p-type semiconductor 141b is formed as a single emission layer.
[0193] For example, the structure of the EOD may be electrode / lower electron auxiliary layer (e.g., electron injection layer, electron transport layer (ETL), or a combination thereof) / second light-emitting layer 142 / upper electron auxiliary layer (electron injection layer, electron transport layer, or a combination thereof) / electrode (as a non-limiting example, ITO 200nm / ZnMgO 30-50nm / QD light-emitting layer 20-30nm including n-type metal oxide / ZnMgO 30-50nm / Al 100nm). The material of the upper electron auxiliary layer, the lower electron auxiliary layer, or a combination thereof may include the same material as the material used in the electroluminescent device to be measured. The material of the upper electron auxiliary layer, the lower electron auxiliary layer, or a combination thereof may include a material different from the material used in the electroluminescent device to be measured.
[0194] The electron transport capability (ET) can be obtained from the voltage-current density diagram of the EOD. For example, the electron transport capability (ET) can be increased in proportion to the content of the n-type metal oxide 142b included in the second light emitting layer 142. The electron transport capability can be measured at a voltage greater than or equal to about 1 volt, greater than or equal to about 2 volts, or greater than or equal to about 3 volts and less than or equal to about 12 volts, less than or equal to about 11 volts, less than or equal to about 10 volts, less than or equal to about 9 volts, less than or equal to about 8 volts, or less than or equal to about 7 volts. The electron transport capability can be measured at a voltage of about 3.5 volts.
[0195] For example, the structure of the HOD may be electrode / lower hole auxiliary layer (e.g., hole injection (delay) layer, hole transport layer (HTL), or a combination thereof) / first light emitting layer 141 / upper hole auxiliary layer (e.g., hole injection layer, hole transport layer, or a combination thereof) / electrode (as a non-limiting example, ITO 200nm / poly (3,4-ethylenedioxythiophene) polystyrene sulfonate (PEDOT:PSS) 30nm / poly (9,9-dioctyl-fluorene-co-N-(4-butylphenyl)-diphenylamine) (TFB) 25nm / QD light emitting layer with or without p-type semiconductor 20-30nm / GSH0137 (a compound including bicarbazolyl and biphenyl, available from Samsung SDI is commercially available) 36nm / dipyrazino[2,3-f:2',3'-h]quinoxaline-2,3,6,7,10,11-hexacarbonitrile (HAT-CN) 10nm / Ag 100nm). The material of the upper hole auxiliary layer, the lower hole auxiliary layer, or a combination thereof may include the same material as the material used in the electroluminescent device to be measured. The material of the upper hole auxiliary layer, the lower hole auxiliary layer, or a combination thereof may include a material different from the material used in the electroluminescent device to be measured.
[0196] The hole transport capability (HT) may be obtained from a voltage-current density graph of the HOD. For example, the hole transport capability (HT) may increase in proportion to the content of the p-type semiconductor 141b included in the first light emitting layer 141. The hole transport capability may be measured at a voltage greater than or equal to about 1 volt, greater than or equal to about 2 volts, or greater than or equal to about 3 volts and less than or equal to about 12 volts, less than or equal to about 11 volts, less than or equal to about 10 volts, less than or equal to about 9 volts, less than or equal to about 8 volts, or less than or equal to about 7 volts. The hole transport capability may be measured at a voltage of about 3.5 volts.
[0197] For example, HT and ET values are measured a predetermined number of times (e.g., three times) at a predetermined rate (e.g., 0.2 volt units) at a predetermined voltage interval (e.g., an interval from -2 volts to 8 volts). HT and ET values can be selected from three values at a predetermined voltage (e.g., 3.5 volts).
[0198] When the electroluminescent device 10, 10' includes an n-type metal oxide 142b in the second light-emitting layer 142 and may further include a p-type semiconductor 141b in the first light-emitting layer 141, the light-emitting layer 140 has a value greater than about 0.20, greater than or equal to about 0.21, greater than or equal to about 0.22, greater than or equal to about 0.23, greater than or equal to about 0.24, or greater than or equal to about 0.25 and less than about 0.56, less than or equal to about 0.55, less than or equal to about 0.54, less than or equal to, etc. The charge balance factor may be about 0.53 or less, about 0.52 or less, about 0.51 or less, about 0.50 or less, about 0.49 or less, about 0.48 or less, about 0.47 or less, about 0.46 or less, or about 0.45 or less, such as about 0.20 or more and about 0.56 or less, about 0.21 or less, about 0.55 or less, about 0.25 or less, about 0.45 or less, about 0.25 or less, about 0.40 or less, or about 0.25 or less. When the charge balance factor is within the above range, the electroluminescent device 10 may exhibit improved light emission and lifetime characteristics (e.g., T50).
[0199] In this case, HT may be less than about 3.0 mA / cm 2 , less than or equal to about 2.5mA / cm 2 , less than or equal to about 2.0mA / cm 2 , or less than or equal to about 1.5 mA / cm 2 and greater than about 0.5 mA / cm 2 , greater than or equal to about 1.0 mA / cm 2 , or greater than or equal to about 1.5 mA / cm 2 ET may be less than or equal to about 5.4 mA / cm 2, or less than or equal to about 5.0 mA / cm 2 and greater than or equal to about 1 mA / cm 2 or greater than or equal to about 4.0 mA / cm 2 .
[0200] In an embodiment, the hole transport layer 130 may include an organic material such as the p-type semiconductor, the first light-emitting layer 141 may include an organic material such as the p-type single-molecule organic semiconductor (hereinafter referred to as the p-type organic material), the second light-emitting layer 142 may include an inorganic material such as an n-type metal oxide 142b (hereinafter referred to as the n-type inorganic material), and the electron transport layer 150 may include an inorganic material such as the inorganic material nanoparticles.
[0201] In this case, holes are injected from the hole transport layer 130 including an organic material into the first light emitting layer 141 including a p-type organic material, and electrons are injected from the electron transport layer 150 including an inorganic material into the second light emitting layer 142 including an n-type inorganic material. Since holes are efficiently injected from the organic material to the organic material and electrons are efficiently injected from the inorganic material to the inorganic material, the on-voltage can be significantly reduced, the external quantum efficiency (EQE) and the brightness can be significantly improved, and the lifespan characteristics (e.g., T50) can be improved.
[0202] Hereinafter, a display apparatus including the above-described electroluminescent devices 10 and 10 ′ is described.
[0203] A display apparatus according to an embodiment includes: a substrate; a driving circuit formed on the substrate; and first, second, and third electroluminescent devices spaced apart from each other at predetermined intervals and disposed on the driving circuit.
[0204] At least one (eg, one, two, or all) of the first to third electroluminescent devices may have the same structure as the electroluminescent device 10 or 10', but wavelengths of light emitted from respective quantum dots may be different from each other.
[0205] In an embodiment, the first electroluminescent device is a red device that emits red light, the second electroluminescent device is a green device that emits green light, and the third electroluminescent device is a blue device that emits blue light. In other words, the first to third electroluminescent devices may be pixels that express red, green, and blue, respectively, in the display device.
[0206] However, the embodiment is not necessarily limited thereto, but the first to third electroluminescent devices may express magenta, yellow, and cyan, respectively, or may express other colors.
[0207] Meanwhile, only one of the first to third electroluminescent devices may be the above-mentioned electroluminescent device 10 or 10'. In this case, the third electroluminescent device showing at least blue may desirably be the above-mentioned electroluminescent device 10 or 10'.
[0208] In a display device according to an embodiment, a hole injection layer, a hole transport layer, an electron transport layer, an electron injection layer, and a hole blocking layer other than the light-emitting layer of each pixel may be integrated to form a common layer. However, the embodiment is not limited thereto. The hole injection layer, the hole transport layer, the electron transport layer, the electron injection layer, and the hole blocking layer may be independently formed in each pixel of the display device, or at least one of the hole injection layer, the hole transport layer, the electron transport layer, the electron injection layer, and the hole blocking layer may form a common layer and the remaining layers may form separate independent layers.
[0209] The substrate may be a transparent insulating substrate or may be made of a tough material. The substrate may include a polymer material or glass in the form of a film having a glass transition temperature (Tg) greater than about 150°C. For example, it includes a material based on COC (cyclic olefin copolymer) or COP (cyclic olefin polymer). All of the first to third electroluminescent devices are formed on the substrate. That is, the substrate of the display device according to the embodiment provides a common layer.
[0210] The driving circuit is disposed on the substrate and is independently connected to each of the first to third electroluminescent devices. The driving circuit may include: at least one line including a scan line, a data line, a driving power line, a common power line, etc.; at least two thin film transistors (TFTs) connected to the line and corresponding to one organic light emitting diode; and at least one capacitor, etc. The driving circuit may have a variety of known structures.
[0211] As described above, the display apparatus according to the embodiment may exhibit improved device efficiency and thus improved lifespan and light emitting efficiency.
[0212] Hereinafter, the embodiments are described in more detail with reference to Examples. However, these Examples shall not be construed as limiting the scope of the present invention in any sense.
[0213] Synthesis of Metal Oxides (as used herein, "Zn 1-x Mg x O" is referred to as "ZnMgO")
[0214] Zinc acetate dihydrate and magnesium acetate tetrahydrate were added to dimethyl sulfoxide in a reactor so as to provide a molar ratio of the following chemical formula, and the reactor was heated at 60° C. in air. Subsequently, an ethanol solution of tetramethylammonium hydroxide pentahydrate was added thereto dropwise at a rate of 3 milliliters per minute (mL / min). The obtained mixture was stirred for 1 hour, and the Zn generated therein was 1-x Mgx O nanoparticles were centrifuged and dispersed in ethanol to obtain Zn 1-x Mg x O nanoparticles (x=0.15).
[0215] The obtained nanoparticles were subjected to X-ray diffraction analysis to confirm the formation of ZnMgO crystals. The obtained nanoparticles were subjected to transmission electron microscopy analysis, and the results showed that the particles had an average size of about 3 nm.
[0216] Verification Example 1
[0217] After the glass substrate on which the first electrode (anode) i.e. ITO was deposited was surface treated with UV-ozone for 15 minutes, a PEDOT:PSS solution (HOMO energy level: -5.35 eV, HC Starks) was spin-coated thereon and heat-treated at 150°C in a nitrogen atmosphere for 30 minutes to form a 30 nm thick first hole injection layer.
[0218] Then, a solution in which poly[(9,9-dioctylfluorene-2,7-diyl-co-(4,4'-(N-4-butylphenyl)diphenylamine] (TFB, HOMO energy level: -5.56 eV, LUMO energy level: -2.69 eV, Sumitomo Co., Ltd.) was dissolved in o-xylene was spin-coated on the first hole injection layer and heat-treated at 150°C for 30 minutes to form a 25 nm thick first hole transport layer.
[0219] Subsequently, the following composition for forming a blue light-emitting layer (a layer emitting blue light) was coated thereon and then heated at 80° C. to provide a blue light-emitting layer having a thickness of 20 nm (CBP content in the blue light-emitting layer: 8 wt %): wherein 4,4′-bis(N-carbazolyl)-1,1′-biphenyl (CBP, HOMO level: −5.7 eV, LUMO level: −2.6 eV) and ZnTeSe / ZnSeS core-shell blue quantum dots (average particle diameter: 10 nm, peak emission wavelength: about 451 nm, HOMO level: −5.7 eV, LUMO level: −3.0 eV) having attached oleate groups as hydrophobic ligands were dispersed in octane.
[0220] Then, a bicarbazole-based compound (GSH0137, manufacturer: Samsung SDI) was deposited on the blue light emitting layer to provide a second hole transport layer having a thickness of 36 nm.
[0221] Then, 1,4,5,8,9,11-hexaazabenzo[9,10]phenanthrenehexacarbonitrile (HAT-CN) was deposited on the second hole transport layer to form a second hole injection layer with a thickness of 10 nm.
[0222] Then, 100 nm of aluminum was vacuum deposited on the second hole injection layer to provide a second electrode, so that the HOD (hole only device) according to Verification Example 1 (ITO / PEDOT:PSS / TFB / blue QD:CBP (8 wt %) / GSH0137 / HAT-CN / Ag) was obtained.
[0223] Verification Comparative Example 1
[0224] HOD (ITO / PEDOT:PSS / TFB / blue QD / GSH0137 / HAT-CN / Ag) according to Verification Comparative Example 1 was obtained according to the same procedure as in Verification Example 1, except that the blue light emitting layer was formed using a composition for forming a blue light emitting layer that did not include CBP.
[0225] The voltage-current density of each HOD according to Verification Example 1 and Verification Comparative Example 1 was measured, and the results are shown in Figure 5 middle.
[0226] Figure 5 Graphs of voltage-current density of hole-only devices (HODs) according to Verification Example 1 and Verification Comparative Example 1.
[0227] Reference Figure 5 , it was confirmed that Verification Example 1 including CBP in the blue light emitting layer showed more excellent current density with respect to voltage than Verification Comparative Example 1 not including CBP.
[0228] Therefore, by Figure 5 As a result, it is understood that when a predetermined amount of CBP is included when forming the blue light emitting layer, the charge transport capability (specifically, the hole transport capability) of the device is improved.
[0229] Verification Example 2
[0230] After the glass substrate on which the first electrode (anode) i.e. ITO was deposited was surface treated with UV-ozone for 15 minutes, a solution for forming an electron transport layer in which ZnMgO (average particle diameter: 3 nm) was dispersed in ethanol was spin-coated thereon and heated at 80°C for 30 minutes to provide a first electron transport layer having a thickness of 20 nm.
[0231] Subsequently, the following composition for forming a blue light-emitting layer was coated thereon and then heated at 80°C to provide a blue light-emitting layer having a thickness of 20 nm: ZnTeSe / ZnSeS core-shell blue quantum dots (average particle diameter: 10 nm, peak emission wavelength: about 451 nm, HOMO energy level: -5.7 eV, LUMO energy level: -3.0 eV) having attached oleate groups as hydrophobic ligands and ZnMgO (average particle diameter: 3 nm, HOMO energy level: -7.7 eV, LUMO energy level: -4.3 eV) having attached oleate groups on the surface were dispersed in hexane.
[0232] Subsequently, a solution for forming an electron transport layer in which ZnMgO (average particle diameter: 3 nm) was dispersed in ethanol was spin-coated on the light emitting layer and heated at 80° C. for 30 minutes to provide a second electron transport layer having a thickness of 20 nm.
[0233] Subsequently, 100 nm of aluminum was vacuum-deposited on the second electron transport layer to provide a second electrode, so that the EOD (electronic device only) according to Verification Example 2 (ITO / ZnMgO / blue QD: ZnMgO (3 wt %) / ZnMgO / Al) was obtained.
[0234] Verification Example 3
[0235] The EOD according to Verification Example 3 (ITO / ZnMgO / blue QD: ZnMgO (5 wt %) / ZnMgO / Al) was obtained according to the same procedure as in Verification Example 2, except that the addition amount of ZnMgO was adjusted so that the ZnMgO content in the blue light emitting layer was 5 wt %.
[0236] Verification Example 4
[0237] The EOD according to Verification Example 4 (ITO / ZnMgO / blue QD: ZnMgO (10 wt %) / ZnMgO / Al) was obtained according to the same procedure as in Verification Example 2, except that the addition amount of ZnMgO was adjusted so that the ZnMgO content in the blue light emitting layer was 10 wt %.
[0238] Verification Comparative Example 2
[0239] The EOD (ITO / ZnMgO / blue QD / ZnMgO / Al) according to Verification Comparative Example 2 was obtained according to the same procedure as in Verification Example 2, except that the blue light emitting layer was formed using a composition for forming a blue light emitting layer that did not include ZnMgO.
[0240] The voltage-current density of the EOD according to each of the Verification Examples 2-4 and the Verification Comparative Example 2 was measured, and the results are shown in Figure 6 middle.
[0241] Figure 6 Graphs of voltage-current density of the electron-only device (EOD) according to Verification Examples 2-4 and Verification Comparative Example 2.
[0242] Reference Figure 6 , it was confirmed that Verification Examples 2-4, in which ZnMgO was included in the blue light emitting layer, showed more excellent current density relative to voltage than Verification Comparative Example 2. At the same time, it was confirmed that as ZnMgO in the blue light emitting layer gradually increased from 3 wt % to 5 wt % and 10 wt %, the current density relative to voltage also gradually increased.
[0243] Therefore, by Figure 6 As a result, it is understood that when a predetermined amount of ZnMgO is included when forming a blue light emitting layer, the charge transport capability (specifically, electron transport capability) of the device is improved.
[0244] Example 1
[0245] After the glass substrate on which the first electrode (anode) i.e. ITO (work function: -4.850 eV) was deposited was surface treated with UV-ozone for 15 minutes, a PEDOT solution (HOMO energy level: -5.3 eV, HC Starks) was spin-coated thereon and heat-treated at 150°C in a nitrogen atmosphere for 30 minutes to form a 30 nm thick hole injection layer.
[0246] Then, a solution in which poly[(9,9-dioctylfluorene-2,7-diyl-co-(4,4'-(N-4-butylphenyl)diphenylamine] (TFB, HOMO energy level: -5.56 eV, LUMO energy level: -2.69 eV, Sumitomo Co., Ltd.) was dissolved in toluene was spin-coated on the hole injection layer and heat-treated at 150°C for 30 minutes to form a 25 nm thick hole transport layer.
[0247] Subsequently, ZnTeSe / ZnSeS core-shell blue quantum dots (average particle diameter: 10 nm, peak emission wavelength: about 451 nm, HOMO energy level: -5.7 eV, LUMO energy level: -3.0 eV) having oleate groups attached as hydrophobic ligands on the surface were added to octane and stirred for 5 minutes to provide a composition for a first blue light-emitting layer. Then, the composition for a first blue light-emitting layer was spin-coated on the hole transport layer and heated at 120° C. for 30 minutes under a nitrogen atmosphere to provide a 28 nm thick first blue light-emitting layer.
[0248] At the same time, ZnTeSe / ZnSeS core-shell quantum dots having chloride (Cl) attached on the surface (average particle diameter: 10 nm, peak emission wavelength: about 451 nm, HOMO energy level: -5.9 eV, LUMO energy level: -3.2 eV) and ZnMgO having oleate groups attached on the surface (average particle diameter: 3 nm, HOMO energy level: -7.7 eV, LUMO energy level: -4.3 eV) were added to hexane and stirred for 5 minutes to provide a composition for a second blue light-emitting layer.
[0249] Subsequently, the composition for a second blue light emitting layer was spin-coated on the first blue light emitting layer and heated at 120° C. for 30 minutes under a nitrogen atmosphere to provide a 13 nm thick second blue light emitting layer (ZnMgO content in the second blue light emitting layer: 3 wt %).
[0250] Then, a solution for forming an electron transport layer in which ZnMgO (average particle diameter: 3 nm) was dispersed in ethanol was spin-coated on the second blue light-emitting layer and heated at 80° C. for 30 minutes to provide a 20 nm-thick electron transport layer.
[0251] Then, 100 nm of aluminum (work function: -4.3 eV) was vacuum deposited on the electron transport layer to provide a second electrode, so that the electroluminescent device according to Example 1 [ITO / PEDOT / TFB / blue QD / blue QD:ZnMgO (3 wt %) / ZnMgO / Al] was obtained.
[0252] Example 2
[0253] An electroluminescent device according to Example 2 [ITO / PEDOT / TFB / blue QD / blue QD:ZnMgO (5 wt %) / ZnMgO / Al] was obtained according to the same procedure as in Example 1, except that the addition amount of ZnMgO in the composition for forming the second blue light-emitting layer was adjusted so that the ZnMgO content in the second blue light-emitting layer was 5 wt %.
[0254] Example 3
[0255] An electroluminescent device according to Example 3 [ITO / PEDOT / TFB / blue QD / blue QD:ZnMgO (10 wt %) / ZnMgO / Al] was obtained according to the same procedure as in Example 1, except that the amount of ZnMgO added in the composition for forming the second blue light-emitting layer was adjusted so that the ZnMgO content in the second blue light-emitting layer was 10 wt %.
[0256] Comparative Example 1
[0257] An electroluminescent device (ITO / PEDOT / TFB / blue QD / ZnMgO / Al) according to Comparative Example 1 was obtained according to the same procedure as in Example 1, except that a blue single light-emitting layer was formed with a thickness of 28 nm using a composition for the first blue light-emitting layer that did not include ZnMgO, instead of forming the first and second blue light-emitting layers.
[0258] Comparative Example 2
[0259] An electroluminescent device according to Comparative Example 2 [ITO / PEDOT / TFB / blue QD / blue QD:ZnMgO (15 wt %) / ZnMgO / Al] was obtained according to the same procedure as in Example 1, except that the addition amount of ZnMgO in the composition for forming the second blue light-emitting layer was adjusted so that the ZnMgO content in the second blue light-emitting layer was 15 wt %.
[0260] Evaluation 1: Luminescence and lifetime characteristics of a blue double-emitting layer including ZnMgO
[0261] The light emitting characteristics of the electroluminescent devices according to Examples 1 and 2 and Comparative Examples 1-2 and the lifespan characteristics of the electroluminescent devices according to Examples 1 and 2 and Comparative Examples 1-2 were each measured, and the results are shown in Table 1-2.
[0262] (Table 1)
[0263]
[0264]
[0265] (Table 2)
[0266]
[0267] T95 and T50 in Table 2 respectively mean the time at which 95% (in the case of T95) and 50% (in the case of T50) of the initial brightness (e.g., 4500 nits) are shown. Meanwhile, the term initial P. current represents the value of the current converted from the light emitted by the device when the device is driven by the light receiving sensor (photodiode), which reflects the intensity of the light emitted from the device. The measurement of the initial P. current was started for the electroluminescent devices according to the embodiment and the comparative example at substantially equal light intensity.
[0268] First, referring to Table 1, it is confirmed that the electroluminescent devices according to Examples 1 and 2 show more excellent driving efficiency and luminous efficiency than the electroluminescent devices according to Comparative Examples 1-2.
[0269] In addition, referring to Table 2, it was confirmed that the electroluminescent devices according to Examples 1 and 2 had excellent life characteristics.
[0270] Therefore, from the results of Tables 1-2, it is understood that the electroluminescent device according to the embodiment shows more excellent light emitting characteristics and / or lifespan characteristics compared with an electroluminescent device having a blue single light emitting layer or including an excess of ZnMgO in the second blue light emitting layer.
[0271] Example 4
[0272] After the glass substrate on which the first electrode (anode) i.e. ITO (work function: -4.850 eV) was deposited was surface treated with UV-ozone for 15 minutes, a PEDOT solution (HOMO energy level: -5.35 eV, HC Starks) was spin-coated thereon and heat-treated at 150°C in a nitrogen atmosphere for 30 minutes to form a 30 nm thick hole injection layer.
[0273] Then, a solution in which poly[(9,9-dioctylfluorene-2,7-diyl-co-(4,4'-(N-4-butylphenyl)diphenylamine] (TFB, HOMO energy level: -5.56 eV, LUMO energy level: -2.69 eV, Sumitomo Co., Ltd.) was dissolved in toluene was spin-coated on the hole injection layer and heat-treated at 150°C for 30 minutes to form a 25 nm thick hole transport layer.
[0274] Subsequently, ZnTeSe / ZnSeS core-shell blue quantum dots (average particle diameter: 10 nm, peak emission wavelength: about 451 nm, HOMO level: -5.7 eV, LUMO level: -3.0 eV) having oleate groups attached as hydrophobic ligands on the surface and 4,4'-bis(N-carbazolyl)-1,1'-biphenyl (CBP, HOMO level: -5.7 eV, LUMO level: -2.6 eV) were added to octane and stirred for 5 minutes to provide a composition for forming a first blue light-emitting layer. Then, the composition for forming a first blue light-emitting layer was spin-coated on the hole transport layer and heated at 120°C for 30 minutes under a nitrogen atmosphere to provide a 28 nm thick first blue light-emitting layer. Then, a zinc chloride ethanol solution (concentration: 10 mg / mL) was added dropwise onto the first blue light-emitting layer and reacted for 1 minute to replace a portion of the oleate groups of the quantum dots attached to the first blue light-emitting layer with chloride groups (CBP content in the first blue light-emitting layer: 8 wt %).
[0275] At the same time, ZnTeSe / ZnSeS core-shell blue quantum dots (average particle diameter: 10 nm, peak emission wavelength: about 451 nm, HOMO energy level: -5.7 eV, LUMO energy level: -3.0 eV) having oleate groups attached on the surface as hydrophobic ligands and ZnMgO (average particle diameter: 3 nm, HOMO energy level: -7.7 eV, LUMO energy level: -4.3 eV) having oleate groups attached on the surface were added to hexane and stirred for 5 minutes to provide a composition for forming a second blue light-emitting layer.
[0276] The composition for forming a second blue light-emitting layer was then spin-coated on the chloride-substituted first blue light-emitting layer and then heated at 120° C. for 30 minutes in a nitrogen atmosphere to provide a 13 nm thick second blue light-emitting layer (ZnMgO content in the second blue light-emitting layer: 5 wt %).
[0277] Subsequently, a solution for forming an electron transport layer in which ZnMgO (average particle diameter: 3 nm) was dispersed in ethanol was spin-coated on the second blue light-emitting layer and heated at 80° C. for 30 minutes to provide a 20 nm-thick electron transport layer.
[0278] Subsequently, 100 nm aluminum (work function: -4.3 eV) was vacuum deposited on the electron transport layer to provide a second electrode, so that an electroluminescent device according to Example 4 [ITO / PEDOT / TFB / blue QD:CBP (8 wt %) / blue QD:ZnMgO (5 wt %) / ZnMgO / Al] was obtained.
[0279] Example 5
[0280] An electroluminescent device according to Example 5 [ITO / PEDOT / TFB / blue QD:CBP (10 wt %) / blue QD:ZnMgO (3 wt %) / ZnMgO / Al] was obtained according to the same procedure as in Example 4, except that the addition amounts of CBP and ZnMgO in the compositions for forming the first and second blue light-emitting layers were respectively adjusted so that the CBP content in the first blue light-emitting layer was 10 wt % and the ZnMgO content in the second blue light-emitting layer was 3 wt %.
[0281] Example 6
[0282] An electroluminescent device according to Example 6 [ITO / PEDOT / TFB / blue QD:CBP (8 wt %) / blue QD:ZnMgO (3 wt %) / ZnMgO / Al] was obtained according to the same procedure as in Example 4, except that the amount of ZnMgO added in the composition for forming the second blue light-emitting layer was adjusted so that the ZnMgO content in the second blue light-emitting layer was 3 wt %.
[0283] Comparative Example 3
[0284] An electroluminescent device according to Comparative Example 3 (ITO / PEDOT / TFB / blue QD (thickness: 41 nm) / ZnMgO / Al) was obtained according to the same procedure as in Example 4, except that a blue single light-emitting layer was formed with a thickness of 41 nm using a composition for forming a first blue light-emitting layer that did not include ZnMgO, instead of forming the first and second blue light-emitting layers.
[0285] Evaluation 2: Luminescence and lifetime characteristics of a pn junction blue double-light-emitting layer comprising ZnMgO and CBP
[0286] The light emitting characteristics and lifespan characteristics were measured for the electroluminescent devices according to Examples 4 to 6 and Comparative Example 3, and the results are shown in Tables 3 to 4, respectively.
[0287] (Table 3)
[0288]
[0289] (Table 4)
[0290]
[0291] Referring to Table 3, it was confirmed that the electroluminescent devices having a blue double emission layer according to Examples 4-6 showed more excellent driving efficiency and luminous efficiency than the electroluminescent device having a blue single emission layer according to Comparative Example 3. In addition, referring to Table 4, it was confirmed that the electroluminescent device having a blue double emission layer according to Example 6 showed more excellent life characteristics than the electroluminescent device having a blue single emission layer according to Comparative Example 3.
[0292] Therefore, from the results of Tables 3-4, it is understood that the electroluminescent device having a blue double emission layer according to the embodiment shows more excellent light emission and life characteristics than the electroluminescent device having a blue single emission layer.
[0293] Comparative Example 4
[0294] After the glass substrate on which the first electrode (anode) i.e. ITO (work function: -4.850 eV) was deposited was surface treated with UV-ozone for 15 minutes, a PEDOT solution (HOMO energy level: -5.3 eV, HC Starks) was spin-coated thereon and heat-treated at 150°C in a nitrogen atmosphere for 30 minutes to form a 30 nm thick hole injection layer.
[0295] Then, a solution in which poly[(9,9-dioctylfluorene-2,7-diyl-co-(4,4'-(N-4-butylphenyl)diphenylamine] (TFB, HOMO energy level: -5.56 eV, LUMO energy level: -2.69 eV, Sumitomo Co., Ltd.) was dissolved in toluene was spin-coated on the hole injection layer and heat-treated at 150°C for 30 minutes to form a 25 nm thick hole transport layer.
[0296] Subsequently, ZnTeSe / ZnSeS core-shell blue quantum dots (average particle diameter: 10 nm, peak emission wavelength: about 451 nm, HOMO level: -5.7 eV, LUMO level: -3.0 eV) having oleate attached on the surface as a hydrophobic ligand and ZnMgO (average particle diameter: 3 nm, HOMO level: -7.7 eV, LUMO level: -4.3 eV) having oleate attached on the surface were added to hexane and stirred for 5 minutes to provide a composition for forming a blue light-emitting layer. Then, the composition for forming a blue light-emitting layer was spin-coated on the hole transport layer and heat-treated at 120° C. for 30 minutes under a nitrogen atmosphere to provide a blue single light-emitting layer having a thickness of 28 nm. Then, zinc chloride ethanol solution (concentration: 10 mg / mL) was added dropwise onto the blue single emission layer and reacted for 1 minute to replace the oleate groups of the quantum dots attached to the blue single emission layer with chloride groups (ZnMgO content in the blue single emission layer: 3 wt %).
[0297] Subsequently, a solution for forming an electron transport layer in which ZnMgO (average particle diameter: 3 nm) was dispersed in ethanol was spin-coated on the blue single light emitting layer and heat-treated at 80° C. for 30 minutes to provide a 20 nm thick electron transport layer.
[0298] Subsequently, 100 nm of aluminum (work function: -4.3 eV) was vacuum deposited on the electron transport layer to provide a second electrode, so that an electroluminescent device according to Comparative Example 4 [ITO / PEDOT / TFB / blue QD:ZnMgO (3 wt %) / ZnMgO / Al] was obtained.
[0299] Comparative Example 5
[0300] An electroluminescent device according to Comparative Example 5 [ITO / PEDOT / TFB / blue QD:ZnMgO (5 wt %) / ZnMgO / Al] was obtained according to the same procedure as in Comparative Example 4, except that the addition amount of ZnMgO in the composition for forming the blue light-emitting layer was adjusted so that the ZnMgO content in the blue single light-emitting layer was 5 wt %.
[0301] Evaluation 3: Comparison of luminescence and lifetime characteristics of a blue single emitting layer depending on the ZnMgO content
[0302] The light emitting characteristics and life characteristics of the electroluminescent devices according to Comparative Examples 1, 4 and 5 were measured, and the results are each shown in Figure 7-8 middle.
[0303] Figure 7 is the voltage-brightness (unit: cd / m 2 ) diagram, and Figure 8 Graphs showing time-voltage (unit: V) of the electroluminescent devices according to Comparative Examples 1, 4 and 5.
[0304] Reference Figure 7-8 , it was confirmed that, in an electroluminescent device having a blue single light-emitting layer, even the driving voltage was increased by adding ZnMgO to the light-emitting layer, and the lifespan characteristics were deteriorated.
[0305] In addition, together with the results of Evaluation 1 based on Comparative Example 1, it was confirmed that the case of the electroluminescent device having a blue single light-emitting layer did not show the effect of improving the electron-hole balance in the entire device having a blue single light-emitting layer, although the electron transfer characteristics and / or hole blocking characteristics were improved by including ZnMgO.
[0306] Evaluation 4: Comparison of lifetime characteristics between blue double emission layer and blue single emission layer depending on ZnMgO content
[0307] For an electroluminescent device including a blue double emission layer and an electroluminescent device including a blue single emission layer, each T50-initial voltage relationship depending on changing the ZnMgO content in the emission layer is summarized and shown in Fig. 9 middle.
[0308] An electroluminescent device including a blue double emission layer was obtained by adjusting the ZnMgO content in the second blue emission layer to 0 wt%, 3 wt%, 5 wt%, and 7 wt%, respectively, by the manufacturing method according to Example 4; and an electroluminescent device including a blue single emission layer was obtained by adjusting the ZnMgO content to 0 wt%, 3 wt%, and 5 wt%, respectively, by the manufacturing method according to Comparative Example 3.
[0309] Fig. 9Graphs of T50-initial voltage for an electroluminescent device including a blue double-emitting layer and an electroluminescent device including a blue single-emitting layer. Fig. 9 In the above, T50 means the time when the electroluminescent device shows a luminance of 50% relative to the initial luminance.
[0310] Reference Fig. 9 , it was confirmed that the case of the electroluminescent device having a blue double emission layer substantially showed a more excellent T50-initial voltage than the electroluminescent device having a blue single emission layer. At the same time, it was confirmed that the case of the electroluminescent device in which the first and second blue emission layers formed a pn junction even with a blue double emission layer (i.e., the case having a blue double emission layer and having a ZnMgO content of 3 wt%, 5 wt%, or 7 wt% in the second blue emission layer) also showed a more improved T50 value than the case not including ZnMgO.
[0311] Therefore, by Fig. 9 The results confirmed that the electroluminescent device with a blue double emission layer (doped with an n-type semiconductor such as ZnMgO or undoped) showed better lifetime characteristics than the electroluminescent device with a blue single emission layer, and the electroluminescent device with a blue double emission layer in which the second blue emission layer was doped with an n-type semiconductor such as ZnMgO showed better lifetime characteristics than the electroluminescent device with a blue double emission layer in which the second blue emission layer was undoped.
[0312] Evaluation 5: Comparison of luminescence characteristics between blue double emission layer and blue single emission layer depending on ZnMgO content
[0313] For an electroluminescent device including a blue double-emitting layer and an electroluminescent device including a blue single-emitting layer, the relationship between the ZnMgO content in the emitting layer and the external quantum efficiency and the relationship between the ZnMgO content and the maximum brightness are summarized and the results are shown in Figure 10-13 middle.
[0314] An electroluminescent device including a blue double emission layer and an electroluminescent device including a blue single emission layer are each obtained as follows: the ZnMgO content in the emission layer is adjusted by the exemplary method of Evaluation 4 (the ZnMgO content in the second blue emission layer in the case of the blue double emission layer, and the ZnMgO content in the entire blue single emission layer in the case of the blue single emission layer).
[0315] Reference Fig.10 and 11 , confirming that, in the case of an electroluminescent device comprising a blue single emitting layer, the external quantum efficiency and the maximum brightness tend to or even gradually decrease as the ZnMgO content increases.
[0316] On the contrary, refer to Fig.12 and13 , it was confirmed that, in the case of an electroluminescent device including a blue double-light-emitting layer, as the ZnMgO content increased until the ZnMgO content in the second blue light-emitting layer reached a predetermined amount (in Fig.12 and 13 However, it was confirmed that when the ZnMgO content was greater than a predetermined amount (e.g., greater than about 11 wt %), both the external quantum efficiency and the maximum brightness were even reduced as the ZnMgO content increased.
[0317] Therefore, by Figure 10-13 The results confirmed that in an electroluminescent device having a blue double emission layer, when the ZnMgO content in the second blue emission layer is greater than 0 to 11 wt %, it shows better luminescence characteristics than an electroluminescent device having a blue double emission layer and / or a blue single emission layer that does not include ZnMgO.
[0318] Example 7
[0319] An electroluminescent device according to Example 7 [ITO / PEDOT / TFB / red QD / red QD:ZnMgO (15 wt %) / ZnMgO / Al] was obtained according to the same procedure as in Example 1, except as follows: a red quantum dot solution in which InP / ZnSe / ZnS core-shell red quantum dots (average particle diameter: 12 nm, peak emission wavelength: about 630 nm, HOMO energy level: -5.55 eV, LUMO energy level: -3.58 eV) were dispersed in octane as a hydrophobic ligand on the surface instead of blue quantum dots was used to form a composition for forming the first and second red light-emitting layers (layers emitting red light), and the amount of ZnMgO added in the second red light-emitting layer was adjusted so that the ZnMgO content in the second red light-emitting layer was 15 wt %, wherein the first red light-emitting layer (thickness: 20 nm) and the second red light-emitting layer (thickness: 18 nm) were formed using the composition for forming the first and second red light-emitting layers.
[0320] Comparative Example 6
[0321] An electroluminescent device [ITO / PEDOT / TFB / red QD / ZnMgO / Al] according to Comparative Example 6 was obtained according to the same procedure as in Comparative Example 1, except that a red single light-emitting layer (thickness: 20 nm) was formed by using InP / ZnSe / ZnS core-shell red quantum dots (average particle diameter: 12 nm, peak emission wavelength: about 630 nm, HOMO level: -5.55 eV, LUMO level: -3.58 eV) having oleate groups attached on the surface as hydrophobic ligands instead of blue quantum dots.
[0322] Evaluation 6: Luminescence and lifetime characteristics of a red dual-emission layer including ZnMgO
[0323] The light emitting characteristics and life characteristics of the electroluminescent devices according to Example 7 and Comparative Example 6 were measured, and the results are shown in Figure 14-17 middle.
[0324] Fig.14 is the brightness of the electroluminescent devices according to Example 7 and Comparative Example 6 (unit: cd / m 2 )-EQE diagram, Fig.15 is a voltage-current density diagram of the electroluminescent device according to Example 7 and Comparative Example 6, Fig.16 is a time-brightness (unit: %) graph of the electroluminescent device according to Example 7 and Comparative Example 6, and Fig.17 2 is a time-voltage diagram of the electroluminescent devices according to Example 7 and Comparative Example 6.
[0325] Reference Figure 14-15 The electroluminescent device according to Example 7 shows more excellent driving efficiency and luminous efficiency than the electroluminescent device according to Comparative Example 6. In particular, the electroluminescent device according to Example 7 improves leakage current more than that in Comparative Example 6.
[0326] In addition, refer to Figure 16-17 , it was confirmed that the electroluminescent device according to Example 7 had more excellent life characteristics than the electroluminescent device according to Comparative Example 6 (red single light emitting layer).
[0327] Meanwhile, when the electroluminescent device includes red quantum dots, the appropriate ZnMgO content that can be included in the second red light emitting layer may be slightly different from Evaluation 5, which seems to be caused by the quantum dot difference between the blue light emitting element and the red light emitting element.
[0328] Therefore, by Figure 14-17 From the results, it is understood that the case of the electroluminescent device including the red double emission layer shows more excellent light emission and lifespan characteristics than the electroluminescent device including the red single emission layer.
[0329] Evaluation 7: Lifespan characteristics based on charge balance factor
[0330] In the electroluminescent device according to Example 4, the electron transport capacity (ET) and the hole transport capacity (HT) were measured while adjusting the content of CBP in the first blue light-emitting layer and the content of ZnMgO in the second blue light-emitting layer, the charge balance factor (CBF) was calculated, and the results are shown in Table 5.
[0331] In addition, after measuring the life characteristics (for example, T50) for each case, the results are also shown in Table 5.
[0332] (Table 5)
[0333] <![CDATA[HT(mA / cm 2 )]]> <![CDATA[ET(mA / cm 2 )]]> CBF(HT / ET) T50 (standardized) 1 0.5 3.7 0.14 1.5 2 0.8 4.0 0.20 1.5 3 0.8 4.0 0.20 1.3 4 1.5 4.0 0.38 2.1 5 1.5 4.0 0.38 1.9 6 1.5 5.0 0.30 2.2 7 1.5 5.4 0.28 2.6 8 0.5 4.0 0.13 1.4 9 0.5 4.0 0.13 1.3 10 3.0 5.4 0.56 1.6
[0334] In order to measure the hole transport ability, HOD [ITO (200 nm) / PEDOT: PSS (30 nm) / TFB (25 nm) / blue QD: CBP (20 nm) / GSH0137 (36 nm) / HAT-CN (10 nm) / Ag (100 nm)] was obtained according to the same procedure as in Verification Example 1, and the current density relative to voltage of the fabricated HOD was measured using a Keithley 2635B source meter to evaluate the hole transport ability.
[0335] In addition, in order to measure the electron transport capability, EOD [ITO (200 nm) / ZnMgO (20 nm) / blue QD: ZnMgO (20 nm) / ZnMgO (20 nm) / Al (100 nm)] was obtained according to the same procedure as in Verification Example 2, and the current density of the fabricated EOD relative to the voltage was measured using a Keithley 2635B source meter to evaluate the electron transport capability.
[0336] Referring to Table 5, when the charge balance factor is less than or equal to about 0.20 and greater than or equal to about 0.56, it can be seen that T50 is significantly reduced, and it is predicted that the charge balance factor of the light emitting layer is an important factor for the lifespan characteristics.
[0337] Example 8
[0338] An electroluminescent device according to Example 8 [ITO / PEDOT / TFB / blue QD / blue QD:ZnMgO (3 wt %) / Al] was obtained according to the same procedure as in Example 1, except that a second electrode was formed on the second blue light-emitting layer without an electron transport layer.
[0339] Example 9
[0340] An electroluminescent device according to Example 9 [ITO / PEDOT / TFB / blue QD / blue QD:ZnMgO (5 wt %) / Al] was obtained according to the same procedure as in Example 2, except that a second electrode was formed on the second blue light-emitting layer without an electron transport layer.
[0341] Example 10
[0342] An electroluminescent device according to Example 10 [ITO / PEDOT / TFB / blue QD / blue QD:ZnMgO (10 wt %) / Al] was obtained according to the same procedure as in Example 3, except that a second electrode was formed on the second blue light-emitting layer without an electron transport layer.
[0343] Comparative Example 7
[0344] An electroluminescent device [ITO / PEDOT / TFB / blue QD / Al] according to Comparative Example 7 was obtained according to the same procedure as in Comparative Example 1, except that a second electrode was formed on the blue light emitting layer without an electron transport layer.
[0345] Evaluation 8: Luminescent properties of electroluminescent devices without electron transport layers
[0346] The luminescent characteristics of the fabricated electroluminescent devices were evaluated using a Keithley 2200 source measurement instrument and a Minolta CS2000 spectroradiometer (current-voltage-luminance measurement instrument), and the results are shown in Fig.18 and Fig.19 middle.
[0347] Fig.18 is a voltage-current density diagram of the electroluminescent devices according to Examples 8-10, Comparative Example 1 and Comparative Example 7, and Fig.19 is the brightness of the electroluminescent devices according to Examples 9 and 10 and Comparative Example 1 (unit: cd / cm 2 )-EQE diagram.
[0348] Reference Fig.18 and Fig.19 Since the second light emitting layer includes an n-type metal oxide, the hole blocking property of the second light emitting layer 142 is improved, so that the electroluminescent device without an electron transport layer can have similar characteristics to the electroluminescent device with an electron transport layer.
[0349] While the present disclosure has been described with respect to what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but on the contrary is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.
[0350] <Description of symbols>
[0351] 10, 10': electroluminescent device 100: substrate
[0352] 110: first electrode 120: hole injection layer
[0353] 130: hole transport layer 140: light emitting layer
[0354] 141: first light emitting layer 141a: first quantum dot
[0355] 141b: p-type semiconductor 142: second light-emitting layer
[0356] 142a: second quantum dot 142b: n-type metal oxide
[0357] 150: electron transport layer 160: second electrode
Claims
1. Electroluminescent devices, include: a first electrode and a second electrode facing each other; as well as a light-emitting layer disposed between the first electrode and the second electrode; wherein the light emitting layer comprises a first light emitting layer disposed on the first electrode side and comprising first quantum dots, and a second light emitting layer disposed on the second electrode side and consisting of second quantum dots and an n-type metal oxide, and The second light-emitting layer emits blue light, and the content of the n-type metal oxide is 1 wt %-12 wt % based on the total weight of the second light-emitting layer, or the second light-emitting layer emits red light, and the content of the n-type metal oxide is 1 wt %-17 wt % based on the total weight of the second light-emitting layer.
2. The electroluminescent device according to claim 1, wherein The second light-emitting layer emits blue light, and the content of the n-type metal oxide is 3 wt %-11 wt % based on the total weight of the second light-emitting layer, or the second light-emitting layer emits red light, and the content of the n-type metal oxide is 3 wt %-15 wt % based on the total weight of the second light-emitting layer.
3. The electroluminescent device of claim 1, wherein the n-type metal oxide comprises an oxide of a metal comprising zinc (Zn), magnesium (Mg), tin (Sn), zirconium (Zr), titanium (Ti), aluminum (Al), or a combination thereof.
4. The electroluminescent device of claim 1, wherein the n-type metal oxide is dispersed in the second light emitting layer.
5. The electroluminescent device of claim 1, wherein the n-type metal oxide includes a hydrophobic organic material attached to at least a portion of a surface thereof. The electroluminescent device according to claim 1 , wherein the average particle diameter of the n-type metal oxide is 1 nm to 10 nm. The electroluminescent device of claim 1 , wherein the first light emitting layer further comprises a p-type semiconductor. 8 . The electroluminescent device of claim 7 , wherein the p-type semiconductor comprises a p-type single-molecule organic semiconductor, a p-type oxide semiconductor, or a combination thereof. 9 . The electroluminescent device of claim 7 , wherein the p-type semiconductor is included in an amount greater than 0 wt % and less than or equal to 20 wt % based on the total weight of the first light emitting layer.
10. The electroluminescent device of claim 1, wherein the light-emitting layer has a charge balance factor greater than 0.20 and less than 0.56, the charge balance factor being a ratio HT / ET of hole transport capacity HT to electron transport capacity ET.
11. The electroluminescent device of claim 1, wherein the light emitting layer has a thickness of 10 nm to 60 nm.
12. The electroluminescent device of claim 1, wherein at least one of the first quantum dot and the second quantum dot include: A core including a first semiconductor nanocrystal and a shell including a second semiconductor nanocrystal having a different composition than the first semiconductor nanocrystal and disposed on the core.
13. The electroluminescent device of claim 1, wherein at least one of the first quantum dot and the second quantum dot has a ligand attached to at least a portion of its surface, the ligand comprising a portion derived from a metal halide compound, a portion derived from a carboxylic acid-based compound, a portion derived from a thiol compound, or a combination thereof.
14. The electroluminescent device of claim 1, wherein the electroluminescent device further comprises or does not further comprise a hole transport layer disposed between the first electrode and the light emitting layer.
15. The electroluminescent device of claim 14, wherein the electroluminescent device further comprises the hole transport layer, and The hole transport layer includes poly(3,4-ethylenedioxythiophene) derivatives, poly(styrene sulfonate) derivatives, poly-N-vinyl carbazole derivatives, polyphenylene vinylene derivatives, poly-p-phenylene vinylene derivatives, polymethacrylate derivatives, polyarylamine derivatives, polyaniline derivatives, polypyrrole derivatives, poly(9,9-dioctylfluorene) derivatives, poly(spiro-bifluorene) derivatives, tri(4-carbazol-9-ylphenyl)amine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N'-di(naphthalene-1-yl)-N,N'-diphenylbenzidine, tri(3-methylphenylphenylamino)triphenylamine, poly[N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine, NiO, MoO 3 , or a combination thereof. 16 . The electroluminescent device of claim 1 , wherein the electroluminescent device further comprises or does not further comprise an electron transport layer disposed between the second electrode and the light emitting layer.
17. The electroluminescent device of claim 16, wherein the electroluminescent device further comprises the electron transport layer, and The electron transport layer includes inorganic material nanoparticles, a quinolone compound, a triazine-based compound, a quinoline-based compound, a triazole-based compound, a naphthalene-based compound, or a combination thereof.
18. The electroluminescent device of claim 17, wherein the inorganic material nanoparticles include salts of metals including zinc (Zn), magnesium (Mg), tin (Sn), zirconium (Zr), titanium (Ti), aluminum (Al), or combinations thereof.
19. The electroluminescent device of claim 1, wherein the electroluminescent device further comprises a hole transport layer disposed between the first electrode and the first light emitting layer and comprising an organic material, and an electron transport layer disposed between the second electrode and the second light emitting layer and including an inorganic material, and The first light-emitting layer includes a p-type organic material.
20. A display device comprising the electroluminescent device according to any one of claims 1 to 19.