Dicing tape and dicing die-bonding film
By using a resin film structure with low heat shrinkage and suitable bending hardness in the cutting tape, combined with a nano-indenter to determine the optimized adhesive layer characteristics, the problem of chip floating after the cutout maintenance process is solved, and a better chip is achieved Inter-distance maintenance and cutting properties.
Patent Information
- Application Number
- CN202011171730.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-07
- Filing Date
- 2020-10-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-10-28
AI Technical Summary
In the prior art, the chip float suppression effect after the cut-up maintenance process is poor and it is difficult to effectively solve it.
The cutting tape consisting of a resin film of a single structure or a laminated structure is adopted. The heat shrinkage rate of the substrate layer in the MD direction at 100°C is less than 20%, and the bending hardness of the product of the elastic modulus and the moment of inertia of the cross-section is 40N. ·mm2 or less, and nano-indenter measurement is carried out on the surface of the adhesive layer to optimize elastic recovery and hardness.
The chip float after the cut-up maintenance process is effectively suppressed, the distance between semiconductor chips is maintained and the cutting properties of the cutting tape is ensured, the resistance after heat shrinkage is reduced, and the bending deformation ability in the expansion process is improved.
Smart Images

Figure CN112778921B_ABST
Abstract
Description
[0001] Cross-references to related applications
[0002] This application claims the priority of Japanese Patent Application No. 2019-202484, which is incorporated by reference into the description of the present application specification. Technical Field
[0003] The present invention relates to a dicing tape and a dicing die-bonding film. Background Art
[0004] Conventionally, it is known that a dicing tape or a dicing die-bonding film is used to obtain a semiconductor chip for die bonding in the production of a semiconductor device.
[0005] The dicing tape is configured by laminating an adhesive layer on a base material layer, and the dicing die-bonding film is configured by laminating a die-bonding layer on the adhesive layer of the dicing tape in a releasable manner.
[0006] Furthermore, as a method for obtaining a semiconductor chip (Die) for chip bonding using the aforementioned cutting chip bonding film, a method having the following steps is known: a half-cutting step of forming a groove on a semiconductor wafer to be processed into a chip (Die) by cutting the semiconductor wafer; a back grinding step of grinding the semiconductor wafer after the half-cutting step to reduce the thickness; a mounting step of attaching one side of the semiconductor wafer after the back grinding step (for example, the side opposite to the circuit side) to the chip bonding layer and fixing the semiconductor wafer to the cutting tape; an expansion step of enlarging the interval between the semiconductor chips processed by half-cutting; a cut maintaining step of maintaining the interval between the semiconductor chips; a picking-up step of peeling off the chip bonding layer and taking out the semiconductor chip in a state where the chip bonding layer is attached; and a chip bonding step of bonding the semiconductor chip in a state where the chip bonding layer is attached to an adherend (for example, a mounting substrate, etc.).
[0007] It should be noted that in the aforementioned cut maintaining process, hot air (e.g. 100-130°C) is blown onto the dicing tape to cause thermal shrinkage (after thermal shrinkage), and then the dicing tape is cooled and solidified to maintain the distance (cut) between adjacent semiconductor chips being cut.
[0008] Furthermore, in the expansion step, the die bonding layer is cut into a size corresponding to the size of the plurality of singulated semiconductor chips.
[0009] However, after the cutout maintaining step, the outer peripheral portion of the semiconductor chip with the die-bonding layer may swell from the surface of the adhesive layer (chip lifting may occur).
[0010] In order to suppress such chip floating, for example, Patent Document 1 describes the use of a dicing tape having specific properties.
[0011] The invention describes in detail the use of a dicing tape having a stress relaxation rate of 45% or more after 1000 seconds after being stretched 30% at 23°C in at least one direction, and a stress value of 4 MPa or less after 1000 seconds after being stretched 30% at 23°C in at least one direction.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: Japanese Patent Application Publication No. 2019-16633 Summary of the invention
[0015] Problem that the invention aims to solve
[0016] However, it is difficult to say that sufficient research has been conducted on the suppression of chip floating after the above-mentioned notch maintaining step.
[0017] Therefore, an object of the present invention is to provide a dicing tape and a dicing die-bonding film capable of relatively suppressing chip floating after a cut maintaining step.
[0018] Solutions for solving problems
[0019] The dicing tape of the present invention is a dicing tape having an adhesive layer laminated on a base material layer.
[0020] The substrate layer is composed of a resin film having a single structure or a laminated structure.
[0021] The heat shrinkage of the substrate layer in the MD direction at 100°C is 20% or less, and the bending hardness calculated as the product of the elastic modulus of the substrate layer and the cross-sectional inertia moment of the substrate layer measured at 25°C using a nanoindenter is 40 N·mm 2 the following.
[0022] For the aforementioned cutting belt,
[0023] The elastic recovery rate of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is preferably 75% or less when measured at 25° C. using a nanoindenter.
[0024] For the aforementioned cutting belt,
[0025] The hardness of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is to be laminated is preferably 40 MPa or less when measured at 25° C. using a nanoindenter.
[0026] The dicing die bonding film of the present invention comprises:
[0027] A dicing tape having an adhesive layer laminated on a base material layer; and
[0028] a die bonding layer laminated on the adhesive layer of the dicing tape,
[0029] The substrate layer is composed of a resin film having a single structure or a laminated structure.
[0030] The heat shrinkage of the substrate layer in the MD direction at 100°C is 20% or less, and the bending hardness calculated as the product of the elastic modulus of the substrate layer and the cross-sectional inertia moment of the substrate layer measured at 25°C using a nanoindenter is 40 N·mm 2 the following. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a cross-sectional view showing the structure of a dicing tape according to one embodiment of the present invention.
[0032] Figure 2 It is a cross-sectional view showing the structure of a dicing die-bonding film according to one embodiment of the present invention.
[0033] Figure 3A This is a cross-sectional view schematically showing a state of half-cutting processing in a method of manufacturing a semiconductor integrated circuit.
[0034] Figure 3B The figure is a cross-sectional view schematically showing a half-cut process in a method for manufacturing a semiconductor integrated circuit.
[0035] Figure 3C The figure is a cross-sectional view schematically showing a backside grinding process in a method for manufacturing a semiconductor integrated circuit.
[0036] Figure 3D The figure is a cross-sectional view schematically showing a backside grinding process in a method for manufacturing a semiconductor integrated circuit.
[0037] Figure 4A It is a cross-sectional view schematically showing a mounting step in a method of manufacturing a semiconductor integrated circuit.
[0038] Figure 4B It is a cross-sectional view schematically showing a mounting step in a method of manufacturing a semiconductor integrated circuit.
[0039] Figure 5A This is a cross-sectional view schematically showing a state of a low-temperature expansion step in a method of manufacturing a semiconductor integrated circuit.
[0040] Figure 5BThis is a cross-sectional view schematically showing a state of a low-temperature expansion step in a method of manufacturing a semiconductor integrated circuit.
[0041] Figure 5C This is a cross-sectional view schematically showing a state of a low-temperature expansion step in a method of manufacturing a semiconductor integrated circuit.
[0042] Fig. 6A It is a cross-sectional view schematically showing a state of an expansion process at room temperature in a method for manufacturing a semiconductor integrated circuit.
[0043] Figure 6B It is a cross-sectional view schematically showing a state of an expansion process at room temperature in a method for manufacturing a semiconductor integrated circuit.
[0044] Figure 7 This is a cross-sectional view schematically showing a state of a cutout maintaining step in a method of manufacturing a semiconductor integrated circuit.
[0045] Figure 8 This is a cross-sectional view schematically showing a pickup step in a method of manufacturing a semiconductor integrated circuit.
[0046] Description of Reference Numerals
[0047] 1. Substrate layer
[0048] 2 Adhesive layer
[0049] 3. Chip bonding layer
[0050] 10 Cutting tape
[0051] 20 Cutting die bonding film
[0052] 1a First resin layer
[0053] 1b Second resin layer
[0054] 1c The third resin layer
[0055] G Back Grinding Tape
[0056] H retainer
[0057] J Suction fixture
[0058] P pin component
[0059] R cutting ring
[0060] T Wafer Processing Tape
[0061] U lifting member
[0062] W Semiconductor Wafer DETAILED DESCRIPTION
[0063] Hereinafter, one embodiment of the present invention will be described.
[0064] [Cutting tape]
[0065] like Figure 1 As shown, the dicing tape 10 according to the present embodiment is a dicing tape in which the adhesive layer 2 is laminated on the base material layer 1 .
[0066] In the dicing tape 10 according to the present embodiment, the base layer 1 is composed of a resin film having a single structure or a laminated structure.
[0067] In the dicing tape 10 according to the present embodiment, the heat shrinkage rate of the base material layer 1 in the MD direction (resin flow direction) at 100° C. is 20% or less.
[0068] In the dicing tape 10 according to the present embodiment, the bending hardness of the base layer 1 obtained as the product of the elastic modulus of the base layer 1 measured at 25° C. using a nanoindenter and the cross-sectional inertia moment of the base layer 1 is 40 N·mm 2 The bending hardness is preferably 30 N·mm 2 Less than, more preferably 20N·mm 2 the following.
[0069] In this specification, the heat shrinkage rate of the substrate layer 1 in the MD direction at 100°C refers to the shrinkage rate after a test piece of the substrate layer 1 cut out along a specified size (width 20 mm, length 120 mm) in such a way that the MD direction becomes the longitudinal direction is exposed to an environment with a temperature of 100°C for 60 seconds.
[0070] In addition, the MD direction refers to the winding direction when the base material layer 1 is wound into a roll.
[0071] The heat shrinkage in the MD direction can be obtained by the following procedure.
[0072] (1) Markings were made at locations 10 mm away from both ends in the longitudinal direction of the test piece before heating.
[0073] (2) The distance L0 between the marks of the test piece before heating (ie, the initial length in the MD direction) is measured.
[0074] (3) The test piece was exposed to an environment at a temperature of 100° C. for 60 seconds with the portion outside the marked portion (ie, the end portion in the longitudinal direction) fixed by a clamp.
[0075] (4) After the test piece is cooled to room temperature (23±2° C.), the length L1 is measured at the same location as in (2).
[0076] (5) Calculate the dimensional change rate R of the test piece in the longitudinal direction (MD direction) according to the following formula: C .
[0077] R C =(L0-L1) / L0×100
[0078] The heat shrinkage rate of the dicing tape 10 according to the present embodiment in the MD direction (resin flow direction) at 100° C. is preferably 0.01% or more, more preferably 0.1% or more, and even more preferably 1% or more.
[0079] By setting the heat shrinkage rate to 1% or more, after dicing the semiconductor wafer into semiconductor chips, the distance between the semiconductor chips (that is, the kerf) can be more sufficiently maintained.
[0080] The elastic modulus of the base material layer 1 for calculating the bending hardness of the base material layer 1 can be obtained as follows.
[0081] Measurement apparatus and measurement conditions
[0082] · Device: Tribo Indenter (manufactured by Hysitron Inc.)
[0083] ·Indenter used: Berkovich type diamond indenter (triangular pyramid type)
[0084] ·Measurement method: Single press measurement
[0085] ·Measurement temperature: 25℃
[0086] Pressing depth setting: 200nm
[0087] ·Measurement atmosphere: Air
[0088] Load (pressing) speed: 20nm / sec
[0089] ·Unloading (pulling) speed: 20nm / sec
[0090] Measurement sample
[0091] The entire diced tape (length l: 5 mm, width w: 5 mm, thickness t: 125 μm) was embedded with an embedding resin, and then the embedded diced tape was cut into a cross section (exposed cross section) along the width direction using a microtome to prepare a measurement sample.
[0092] As the embedding resin, for example, DEV-TUBE S-31 (manufactured by ITW PP&F JAPAN) can be used.
[0093] Determination method
[0094] (1) The measurement sample is kept at 25°C for 1 hour.
[0095] (2) The measurement sample is arranged so that the pressing direction of the Berkovich-type diamond indenter is perpendicular to the surface of the base material layer 1 of the measurement sample.
[0096] (3) After the tip of the Berkovich diamond indenter was brought into contact with the surface of the substrate layer 1 of the measurement sample, the Berkovich diamond indenter was pressed from the surface of the substrate layer 1 to a depth of 200 nm at a load speed of 20 nm / s.
[0097] (4) After the Berkovich-type diamond indenter was pressed from the surface of the substrate layer 1 to a depth of 200 nm, the Berkovich-type diamond indenter was returned to the position at the start of the pressing at a deloading speed of 20 nm / s.
[0098] (5) Using the analysis software "Triboscan Ver.9.2.12.0", the elastic modulus is calculated based on the displacements of the substrate layer 1 when the indenter is unloaded from the deepest pressing position, the load applied to the substrate layer 1 when the aforementioned displacements are reached, and the theoretically calculated indentation area at the aforementioned displacements (the contact area (contact projection area) between the indenter and the substrate layer 1 when the aforementioned displacements are reached).
[0099] The above measurement is performed at three different locations of the base material layer 1 , and the elastic modulus calculated at the three locations is arithmetic averaged to determine the elastic modulus of the base material layer 1 .
[0100] When the base material layer 1 has a laminated structure, the elastic modulus is determined for each layer.
[0101] In addition, assuming that the cross section of the base layer 1 is a rectangular shape, the cross-sectional moment of inertia I of the base layer 1 can be calculated using the following formula.
[0102] I=w×h 3 / 12 (where w is the width of the cutting tape and h is the thickness of the substrate layer 1)
[0103] In addition, when the base material layer 1 has a laminated structure, the cross-sectional moment of inertia is calculated for each layer.
[0104] The bending hardness of the base layer 1 can be obtained by calculating the product of the elastic modulus of the base layer 1 and the cross-sectional moment of inertia of the base layer 1 .
[0105] When the base material layer 1 has a laminated structure, the bending hardness can be obtained by calculating the product of the elastic modulus and the cross-sectional inertia moment for each layer and adding them together.
[0106] The substrate layer 1 is a two-layer structure consisting of a first layer and a second layer laminated on one side of the first layer. When the adhesive layer 2 is laminated on the other side of the first layer, the elastic modulus of the first layer measured using a nanoindenter at 25°C is preferably greater than 350 MPa and less than 800 MPa, and the elastic modulus of the second layer measured using a nanoindenter at 25°C is preferably greater than 10 MPa and less than 120 MPa.
[0107] In addition, when the substrate layer 1 has a three-layer structure consisting of a second layer serving as a central layer, a first layer laminated on one side of the central layer and laminated with the adhesive layer 2, and a third layer laminated on the other side of the central layer, the elastic modulus of the first layer and the third layer measured at 25°C using a nanoindenter is preferably greater than 350 MPa and less than 800 MPa, and the elastic modulus of the second layer measured at 25°C using a nanoindenter is preferably greater than 10 MPa and less than 200 MPa.
[0108] The bending hardness of the base material layer 1 is preferably 3N·mm 2 More preferably, 10 N·mm 2 By making the bending hardness 3N·mm 2 As described above, in the product form, the individualized dicing tape can be smoothly peeled off from the long separator (for example, PET separator).
[0109] The thermal shrinkage rate of the substrate layer 1 made of the resin film in the MD direction at 100°C is set to 20% or less, and the bending hardness obtained as the product of the elastic modulus of the substrate layer 1 measured at 25°C using a nanoindenter and the cross-sectional inertia moment of the substrate layer 1 is set to 40 N·mm 2 The chip lifting (the swelling of the adhesive layer 2 from the outer peripheral portion of the semiconductor chip) after the cutout maintaining step can be relatively suppressed, and the reason for this is considered to be as follows.
[0110] In order to obtain multiple semiconductor chips from a semiconductor wafer using a dicing tape 10, a method comprising the following steps is usually adopted: a half-cutting step of forming grooves on the semiconductor wafer to be processed into a chip (die) by dicing the semiconductor wafer; a back grinding step of grinding the semiconductor wafer after the half-cutting step to reduce the thickness; a mounting step of adhering one side of the semiconductor wafer after the back grinding step (for example, the side opposite to the circuit side) to the adhesive layer 2 of the dicing tape 10 to fix the semiconductor wafer to the dicing tape 10; an expansion step of increasing the interval between the semiconductor chips processed by the half-cutting; a cut maintaining step of maintaining the interval between the semiconductor chips; and a picking-up step of peeling off the semiconductor chip from the adhesive layer 2 to remove the semiconductor chip.
[0111] Here, a circuit is generally formed on the circuit surface of a semiconductor wafer by photolithography, and therefore, the semiconductor wafer is likely to warp toward the circuit surface side due to the circuit formation by the photolithography.
[0112] In addition, as described later, the expansion process often uses an expansion device equipped with a lifting member, and the dicing tape 10 fixed with the semiconductor wafer formed with the groove is lifted up by the lifting member and stretched downward (diagonally downward). In this case, in the expansion process, the force that lifts the dicing tape 10 upward acts on the dicing tape 10.
[0113] Then, as a force resisting the force (lifting force) that pushes the dicing tape 10 upward, the dicing tape 10 generates a force in the opposite direction to the lifting force, that is, a downward resistance force.
[0114] On the other hand, when the cutting tape 10 is lifted up and stretched, the force (tensile force) in the direction (diagonally downward) in which the cutting tape 10 is stretched acts on the semiconductor wafer with the grooves formed therein. As a force to resist the tensile force acting on the cutting tape 10, the semiconductor wafer with the grooves generates a force in the opposite direction to the tensile force, i.e., a resistance force diagonally upward.
[0115] Furthermore, in the cut-off maintaining step, after the dicing tape 10 is cooled and solidified, the downward resistance force generated in the dicing tape 10 and the oblique upward resistance force generated in the semiconductor wafer having the groove formed therein are retained. It is therefore considered that due to these retained forces, the outer periphery of the cut semiconductor chip bulges relative to the dicing tape 10 after the cut-off maintaining step.
[0116] Furthermore, the thickness of the semiconductor wafer cut into semiconductor chips by stretching is about 0.055 mm, which is relatively thin. Therefore, it is considered that the cut semiconductor chips are easily affected by the resistance generated in the dicing tape 10 and the resistance generated in the semiconductor wafer after the dicing tape 10 is cooled and solidified and preserved. Therefore, it is considered that the peripheral part of the semiconductor chip is easy to float from the adhesive layer 2 after the incision maintenance process.
[0117] However, in the dicing tape 10 according to the present embodiment, since the heat shrinkage rate of the base layer 1 in the MD direction at 100° C. is 20% or less, the heat shrinkage of the base layer 1 in the incision maintaining step can be relatively reduced.
[0118] As described above, after the cut maintaining step, resistance is generated in the dicing tape 10 . However, when the thermal shrinkage of the base layer 1 is small, it is possible to suppress the resistance remaining in the base layer after the thermal shrinkage from increasing.
[0119] As a result, it is possible to suppress the outer peripheral portion of the semiconductor chip from swelling out from the adhesive layer 2 due to the resistance generated in the dicing tape 10 .
[0120] In addition, in the dicing tape 10 according to the present embodiment, since the bending hardness of the base material layer 1 is 40 N·mm 2 Therefore, the bending deformation is easier to occur in the expansion process. That is, even if the outer peripheral portion of the semiconductor chip is displaced in the swelling direction, the base material layer 1 is easier to follow the displacement.
[0121] From the above, it can be considered that chip floating after the cutout maintaining step can be relatively suppressed.
[0122] As will be described later, the thickness of the base material layer 1 of the dicing tape 10 is usually as thin as 55 μm or more and 195 μm or less.
[0123] Therefore, it is considered that when the characteristics of the base material layer 1 are to be improved by physical properties, it is beneficial to study physical properties suitable for evaluation in a micro region.
[0124] Here, in the present invention, the bending hardness, which is a physical property used to determine the base material layer 1, is calculated using the elastic modulus measured by a nanoindenter, which is a device particularly suitable for measuring a micro region.
[0125] That is, it is considered that the bending hardness is particularly suitable as a physical property to be studied in order to improve the characteristics of the base material layer 1 of the dicing tape 10 .
[0126] Furthermore, when the base layer 1 has a laminated structure, the bending hardness can be determined for each layer using a nanoindenter. Therefore, from this point of view, the bending hardness is considered to be particularly suitable as a physical property for evaluating the characteristics of the base layer 1 .
[0127] In the dicing tape 10 according to this embodiment, the elastic recovery rate of the surface layer of the substrate layer 1 on the side where the adhesive layer 2 is laminated is preferably 75% or less, more preferably 65% or less when measured at 25°C using a nanoindenter.
[0128] In the dicing tape 10 according to the present embodiment, the elastic recovery rate of the surface layer of the substrate layer 1 on the side where the adhesive layer 2 is laminated is preferably 50% or more, more preferably 60% or more when measured at 25°C using a nanoindenter.
[0129] When the elastic recovery rate measured at 25° C. using a nanoindenter is 50% or more, it is possible to more fully suppress appearance defects caused by deformation of the base material layer 1 .
[0130] The elastic recovery rate using a nanoindenter can be measured by using the same measuring device and measuring sample as those used in the measurement of the elastic modulus of the above-mentioned substrate layer 1, using the same conditions as the measurement conditions of the elastic modulus of the above-mentioned substrate layer 1, using the analysis software "Triboscan Ver.9.2.12.0", and using the same measurement method as the elastic modulus of the above-mentioned substrate layer 1.
[0131] It should be noted that if no load is applied to the substrate layer 1 when the pressure head presses the deepest position, the elastic recovery rate becomes 0%, and if a load is applied to the substrate layer 1 until the pressure head and the substrate layer 1 are about to stop contacting, the elastic recovery rate becomes 100%.
[0132] That is, the elastic recovery rate can be obtained by checking at what point the load is removed, with the pressing start position as a reference, until the base material layer 1 no longer bears the load.
[0133] In the dicing tape 10 according to the present embodiment, the hardness of the surface layer of the substrate layer 1 on the side where the adhesive layer 2 is laminated is preferably 40 MPa or less, more preferably 35 MPa or less when measured at 25° C. using a nanoindenter.
[0134] In the dicing tape 10 according to the present embodiment, the hardness of the surface layer of the substrate layer 1 on the side where the adhesive layer 2 is laminated is preferably 20 MPa or more, more preferably 30 MPa or more when measured at 25° C. using a nanoindenter.
[0135] When the hardness measured at 25° C. using a nano indenter is 20 MPa or more, dicing of the semiconductor wafer and the die bonding layer can be performed more satisfactorily.
[0136] The hardness measurement using a nanoindenter can be performed by using a measuring device and a measuring sample that are the same as those used in the measurement of the elastic modulus of the above-mentioned substrate layer 1, using the same conditions as the measurement conditions of the elastic modulus of the above-mentioned substrate layer 1, and using the analysis software "Triboscan Ver.9.2.12.0". The hardness of the substrate layer 1 can be calculated based on the load applied to the substrate layer 1 when the indenter is pressed deepest, and the indentation area theoretically calculated when the indenter is pressed deepest (the contact area (contact projection area) between the indenter and the substrate layer 1 when the indenter is pressed deepest). Other than that, the measurement is performed using the same method as the method for measuring the elastic modulus of the above-mentioned substrate layer 1.
[0137] The substrate layer 1 supports the adhesive layer 2. The substrate layer 1 is made of a resin film. Examples of the resin contained in the resin film include polyolefins, polyesters, polyurethanes, polycarbonates, polyetheretherketones, polyimides, polyetherimides, polyamides, wholly aromatic polyamides, polyvinyl chloride, polyvinylidene chloride, polyphenylene sulfide, fluororesins, cellulose resins, and silicone resins.
[0138] Examples of the polyolefin include homopolymers of α-olefins, copolymers of two or more α-olefins, block polypropylene, random polypropylene, and copolymers of one or more α-olefins and other vinyl monomers.
[0139] The homopolymer of α-olefin is preferably a homopolymer of α-olefin having a carbon number of 2 to 12. Examples of such a homopolymer include ethylene, propylene, 1-butene, and 4-methyl-1-pentene.
[0140] Examples of copolymers of two or more α-olefins include ethylene / propylene copolymers, ethylene / 1-butene copolymers, ethylene / propylene / 1-butene copolymers, ethylene / α-olefin copolymers having 5 to 12 carbon atoms, propylene / ethylene copolymers, propylene / 1-butene copolymers, and propylene / α-olefin copolymers having 5 to 12 carbon atoms.
[0141] Examples of the copolymer of one or more α-olefins and other vinyl monomers include ethylene-vinyl acetate copolymers (EVA) and the like.
[0142] The polyolefin may be a so-called α-olefin thermoplastic elastomer. Examples of the α-olefin thermoplastic elastomer include a combination of a propylene-ethylene copolymer and a propylene homopolymer, or a propylene-ethylene-α-olefin terpolymer having 4 or more carbon atoms.
[0143] Examples of commercially available α-olefin-based thermoplastic elastomers include Vistamaxx 3980 (manufactured by ExxonMobil Chemical Company), which is a propylene-based elastomer resin.
[0144] The resin film may contain one kind of the aforementioned resin, or may contain two or more kinds of the aforementioned resins.
[0145] When the adhesive layer 2 includes an ultraviolet curing adhesive described later, the resin film forming the base layer 1 is preferably configured to have ultraviolet transmittance.
[0146] The substrate layer 1 may be a single-layer structure or a laminated structure. The substrate layer 1 may be obtained by non-stretching forming or by stretching forming, preferably by stretching forming. When the substrate layer 1 is a laminated structure, the substrate layer 1 preferably has a layer containing an elastomer (hereinafter referred to as an elastomer layer) and a layer containing a non-elastic body (hereinafter referred to as a non-elastic body layer).
[0147] By making the base layer 1 have an elastic layer and a non-elastic layer, the elastic layer can function as a stress relaxation layer for relaxing tensile stress. That is, since the tensile stress generated in the base layer 1 can be relatively reduced, the base layer 1 can have appropriate hardness and be relatively easy to stretch.
[0148] This can improve the dicing performance of dicing a semiconductor wafer into a plurality of semiconductor chips.
[0149] Furthermore, it is possible to suppress the base material layer 1 from being cracked and damaged during cutting in the expanding step.
[0150] It should be noted that, in this specification, the elastomer layer refers to a low elastic modulus layer having a tensile storage modulus at room temperature lower than that of the non-elastic layer. As the elastomer layer, an elastomer layer having a tensile storage modulus at room temperature of 10 MPa or more and 200 MPa or less can be listed, and as the non-elastic layer, a non-elastic layer having a tensile storage modulus at room temperature of 200 MPa or more and 500 MPa or less can be listed.
[0151] The elastomer layer may contain one type of elastomer or two or more types of elastomers, and preferably contains an α-olefin-based thermoplastic elastomer or EVA (ethylene-vinyl acetate copolymer).
[0152] The non-elastic layer may contain one non-elastic layer or two or more non-elastic layers, and preferably contains the metallocene PP described below.
[0153] When the substrate layer 1 has an elastomer layer and a non-elastic layer, the substrate layer 1 is preferably formed into a three-layer structure (non-elastic layer / elastic layer / non-elastic layer) with the elastomer layer as the center layer and the non-elastic layers on the two opposite sides of the center layer (refer to Figure 1 ). It should be noted that Figure 1 , one non-elastic layer is shown as a first resin layer 1a, the elastic layer is shown as a second resin layer 1b, and the other non-elastic layer is shown as a third resin layer 3c.
[0154] In addition, as described above, in the incision maintaining process, since the dicing die bonding film is thermally shrunk by blowing hot air (e.g., 100-130°C) at room temperature (e.g., 23°C) to the dicing die bonding film maintained in an expanded state, and then cooled and solidified, the outermost layer of the base material layer 1 preferably contains a resin having a melting point close to the temperature of the hot air blown to the dicing tape. Thus, the outermost layer melted by blowing the hot air can be solidified more quickly.
[0155] As a result, the incision can be more fully maintained in the incision maintaining step.
[0156] The substrate layer 1 is a laminated structure of an elastomer layer and a non-elastic layer. When the elastomer layer includes an α-olefin thermoplastic elastomer and the non-elastic layer includes a polyolefin such as metallocene PP described later, the elastomer layer preferably includes an α-olefin thermoplastic elastomer of 50% by mass or more and 100% by mass or less relative to the total mass of the elastomer forming the elastomer layer, more preferably 70% by mass or more and 100% by mass or less, further preferably 80% by mass or more and 100% by mass or less, particularly preferably 90% by mass or more and 100% by mass or less, and most preferably 95% by mass or more and 100% by mass or less. By including an α-olefin thermoplastic elastomer in the aforementioned range, the affinity between the elastomer layer and the non-elastic layer becomes high, so that the substrate layer 1 can be extruded relatively easily. In addition, the elastomer layer can function as a stress relaxation layer, so that the semiconductor wafer attached to the dicing tape can be efficiently cut.
[0157] When the substrate layer 1 is a laminated structure of an elastomer layer and a non-elastic layer, the substrate layer 1 is preferably obtained by coextrusion molding of a laminated structure of an elastomer layer and a non-elastic layer by coextruding an elastomer and a non-elastic body. As coextrusion molding, any and appropriate coextrusion molding commonly performed in the manufacture of films, sheets, etc. can be adopted. Among the coextrusion molding, from the viewpoint of being able to efficiently and cheaply obtain the substrate layer 1, it is preferred to adopt an inflation method or a coextrusion T-die method.
[0158] When the substrate layer 1 forming a laminated structure is obtained by co-extrusion molding, the aforementioned elastomer layer and the aforementioned non-elastic layer are heated and contacted in a molten state, so it is preferred that the difference in melting point between the aforementioned elastomer and the aforementioned non-elastic body is small. By making the difference in melting point small, it is suppressed that the aforementioned elastomer or any of the aforementioned non-elastic body with a low melting point is overheated, so that it is possible to suppress the generation of by-products due to thermal degradation of the aforementioned elastomer or any of the aforementioned non-elastic body with a low melting point. In addition, it is also possible to suppress the occurrence of poor lamination between the aforementioned elastomer layer and the aforementioned non-elastic body layer due to excessive reduction in viscosity of the aforementioned elastomer or any of the aforementioned non-elastic body with a low melting point. The difference in melting point between the aforementioned elastomer and the aforementioned non-elastic body is preferably above 0°C and below 70°C, and more preferably above 0°C and below 55°C.
[0159] The melting points of the elastomer and the non-elastic body can be measured by differential scanning calorimetry (DSC) analysis. For example, the melting points can be measured by using a differential scanning calorimeter (manufactured by TA INSTRUMENTS, model: DSC Q2000), heating to 200°C at a heating rate of 5°C / min under a nitrogen flow, and determining the peak temperature of the endothermic peak.
[0160] The thickness of the base material layer 1 is preferably 55 μm to 195 μm, more preferably 55 μm to 190 μm, further preferably 55 μm to 170 μm, and most preferably 60 μm to 160 μm. By making the thickness of the base material layer 1 within the above range, the dicing tape can be efficiently manufactured, and the semiconductor wafer attached to the dicing tape can be efficiently diced.
[0161] The thickness of the base material layer 1 can be determined by, for example, measuring the thickness at five points selected at random using a direct-reading thickness meter (manufactured by PEACOCK, model: R-205) and calculating the arithmetic average of these thicknesses.
[0162] In the base material layer 1 formed by laminating an elastomer layer and a non-elastic layer, the ratio of the thickness of the non-elastic layer to the thickness of the elastomer layer is preferably 1 / 25 or more and 1 / 3 or less, more preferably 1 / 25 or more and 1 / 3.5 or less, further preferably 1 / 25 or more and 1 / 4 or less, particularly preferably 1 / 22 or more and 1 / 4 or less, and most preferably 1 / 20 or more and 1 / 4 or less. By setting the ratio of the thickness of the non-elastic layer to the thickness of the elastomer layer to the above range, the semiconductor wafer attached to the dicing tape can be cut more efficiently.
[0163] The elastomer layer may be a single layer (1 layer) structure or a laminated structure. The elastomer layer is preferably a structure of 1 to 5 layers, more preferably a structure of 1 to 3 layers, further preferably a structure of 1 to 2 layers, and the best is a 1-layer structure. When the elastomer layer is a laminated structure, all layers may contain the same elastomer, or at least 2 layers may contain different elastomers.
[0164] The non-elastic layer may be a single layer (1 layer) structure or a laminated structure. The non-elastic layer is preferably a structure of 1 to 5 layers, more preferably a structure of 1 to 3 layers, further preferably a structure of 1 to 2 layers, and most preferably a 1-layer structure. When the non-elastic layer is a laminated structure, all layers may contain the same non-elastic body, or at least 2 layers may contain different non-elastic bodies.
[0165] The non-elastic layer preferably contains a polypropylene resin (hereinafter referred to as metallocene PP) as a polymerization product obtained by using a metallocene catalyst as a non-elastic. As the metallocene PP, a propylene / α-olefin copolymer as a polymerization product of a metallocene catalyst can be cited. By making the non-elastic layer contain metallocene PP, a dicing tape can be efficiently manufactured, and a semiconductor wafer attached to the dicing tape can be efficiently cut.
[0166] In addition, as a commercially available metallocene PP, WINTEC WFX4M (made by Japan Polypropylene Co., Ltd.) is mentioned.
[0167] Here, the metallocene catalyst is a catalyst comprising a transition metal compound of Group 4 of the periodic table (so-called metallocene compound), wherein the transition metal compound of Group 4 of the periodic table comprises a ligand having a cyclopentadienyl skeleton, and a cocatalyst capable of reacting with the metallocene compound to activate the metallocene compound into a stable ionic state, and the metallocene catalyst comprises an organic aluminum compound as required. The metallocene compound is a cross-linked metallocene compound capable of stereoregular polymerization of propylene.
[0168] Among the aforementioned propylene / α-olefin copolymers as polymerization products of metallocene catalysts, preferred are propylene / α-olefin random copolymers as polymerization products of metallocene catalysts. Among the aforementioned propylene / α-olefin random copolymers as polymerization products of metallocene catalysts, preferred are copolymers selected from propylene / α-olefin random copolymers having 2 carbon atoms as polymerization products of metallocene catalysts, propylene / α-olefin random copolymers having 4 carbon atoms as polymerization products of metallocene catalysts, and propylene / α-olefin random copolymers having 5 carbon atoms as polymerization products of metallocene catalysts. Among these, the most suitable is the propylene / ethylene random copolymer as a polymerization product of metallocene catalysts.
[0169] The propylene / α-olefin random copolymer as the polymerization product of the metallocene catalyst preferably has a melting point of 80°C to 140°C, particularly 100°C to 130°C, from the viewpoint of co-extrusion film-forming property with the elastomer layer and cutting property of the semiconductor wafer attached to the dicing tape.
[0170] The melting point of the propylene / α-olefin random copolymer which is a polymerization product of the metallocene catalyst can be measured by the above-mentioned method.
[0171] Here, if the aforementioned elastomer layer is arranged at the outermost layer of the substrate layer 1, when the substrate layer 1 is made into a roll, the aforementioned elastomer layers arranged at the outermost layer are easily adhered to each other (easy to stick together). Therefore, it becomes difficult to unwind the substrate layer 1 from the roll. In contrast, the preferred form of the substrate layer 1 of the aforementioned laminated structure is non-elastic layer / elastic layer / non-elastic layer, that is, the non-elastic layer is arranged at the outermost layer, so the substrate layer 1 of this form has excellent anti-blocking property. As a result, it is possible to suppress the delay caused by blocking in the manufacture of semiconductor devices using the dicing tape 10.
[0172] The non-elastic layer preferably contains a resin having a melting point of 100° C. to 130° C. and a molecular weight dispersion (mass average molecular weight / number average molecular weight) of 5 or less. Examples of such a resin include metallocene PP.
[0173] By making the non-elastic layer contain the resin as described above, the non-elastic layer can be cooled and solidified more quickly in the incision maintaining step, so that the shrinkage of the base layer 1 after the dicing tape is thermally shrunk can be more fully suppressed.
[0174] Thereby, in the incision maintaining step, the incision can be more fully maintained.
[0175] It should be noted that, by forming the resin film from the above-mentioned resin and making the thickness of the substrate layer 1 the above-mentioned thickness, the heat shrinkage of the substrate layer 1 in the MD direction at 100° C. can be made 20% or less, and the bending hardness calculated as the product of the elastic modulus of the substrate layer 1 and the cross-sectional moment of inertia of the substrate layer 1 measured at 25° C. using a nanoindenter is 40 N·mm 2 the following.
[0176] The adhesive layer 2 contains an adhesive. The adhesive layer 2 holds the semiconductor wafer to be singulated into semiconductor chips by bonding.
[0177] Examples of the adhesive include adhesives whose adhesive force can be reduced by an external action during use of the dicing tape 10 (hereinafter referred to as an adhesive-reducing type adhesive).
[0178] When an adhesive of an adhesion-reducing type is used as an adhesive, the adhesive layer 2 can be used separately in a state showing a higher adhesive force (hereinafter referred to as a high adhesive state) and a state showing a lower adhesive force (hereinafter referred to as a low adhesive state) during the use of the dicing tape 10. For example, when a semiconductor wafer attached to the dicing tape 10 is provided for cutting, the high adhesive state is used to suppress the floating or peeling of a plurality of semiconductor chips singulated by cutting the semiconductor wafer from the adhesive layer 2. In contrast, after cutting the semiconductor wafer, the low adhesive state is used to pick up a plurality of singulated semiconductor chips so that the plurality of semiconductor chips can be easily picked up from the adhesive layer 2.
[0179] Examples of the adhesion-reducing adhesive include an adhesive that can be cured by irradiation with radiation during use of the dicing tape 10 (hereinafter referred to as a radiation-curing adhesive).
[0180] Examples of the radiation-curable adhesive include adhesives that are cured by irradiation with electron beams, ultraviolet rays, α rays, β rays, γ rays, or X rays. Of these, adhesives that are cured by irradiation with ultraviolet rays (ultraviolet curable adhesives) are preferably used.
[0181] Examples of the radiation-curable adhesive include additive-type radiation-curable adhesives comprising a base polymer such as an acrylic polymer, and a radiation-polymerizable monomer component or a radiation-polymerizable oligomer component having a radiation-polymerizable carbon-carbon double bond or other functional group.
[0182] Examples of the acrylic polymer include acrylic polymers containing monomer units derived from (meth)acrylic acid esters, and examples of (meth)acrylic acid esters include alkyl (meth)acrylates, cycloalkyl (meth)acrylates, and aryl (meth)acrylates.
[0183] The adhesive layer 2 may contain an external crosslinking agent. As the external crosslinking agent, any type can be used as long as it can react with the acrylic polymer as the base polymer to form a crosslinked structure. As such an external crosslinking agent, for example, polyisocyanate compounds, epoxy compounds, polyol compounds, aziridine compounds, and melamine-based crosslinking agents can be cited.
[0184] Examples of the radiation-polymerizable monomer component include urethane (meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and 1,4-butanediol di(meth)acrylate. Examples of the radiation-polymerizable oligomer component include various oligomers such as urethane, polyether, polyester, polycarbonate, and polybutadiene. The content ratio of the radiation-polymerizable monomer component and the radiation-polymerizable oligomer component in the radiation-curable adhesive can be selected within a range that appropriately reduces the adhesiveness of the adhesive layer 2.
[0185] The radiation-curable adhesive preferably contains a photopolymerization initiator. Examples of the photopolymerization initiator include α-ketol compounds, acetophenone compounds, benzoin ether compounds, ketal compounds, aromatic sulfonyl chloride compounds, photoactive oxime compounds, benzophenone compounds, thioxanthone compounds, camphorquinone, haloketones, acylphosphine oxides, and acylphosphonates.
[0186] The pressure-sensitive adhesive layer 2 may contain, in addition to the above-mentioned components, a cross-linking accelerator, a tackifier, an antioxidant, a colorant such as a pigment or a dye, and the like.
[0187] The thickness of the adhesive layer 2 is preferably 1 μm or more and 50 μm or less, more preferably 2 μm or more and 30 μm or less, and further preferably 5 μm or more and 25 μm or less.
[0188] [Dicing Die Bonding Film]
[0189] Afterwards, refer to Figure 2 The dicing die-bonding film 20 will be described. In the description of the dicing die-bonding film 20 , the parts that overlap with the dicing tape 10 will not be described repeatedly.
[0190] like Figure 2 As shown, the dicing die-bonding film 20 of the present embodiment includes a dicing tape 10 in which an adhesive layer 2 is laminated on a base layer 1 , and a die-bonding layer 3 laminated on the adhesive layer 2 of the dicing tape 10 .
[0191] In the dicing die-bonding film 20 , a semiconductor wafer is attached to the die-bonding layer 3 .
[0192] When the semiconductor wafer is cut using the dicing die-bonding film 20, the die-bonding layer 3 is also cut together with the semiconductor wafer. The die-bonding layer 3 is cut into a size corresponding to the size of the plurality of singulated semiconductor chips. Thus, a semiconductor chip with the die-bonding layer 3 can be obtained.
[0193] Regarding the dicing tape 10 for dicing the die bonding film 20, as described above, the base layer 1 is composed of a resin film having a single structure or a laminated structure, the base layer 1 of the dicing tape 10 has a heat shrinkage rate in the MD direction at 100° C. of 20% or less, and a bending hardness calculated as a product of an elastic modulus of the base layer 1 and a cross-sectional moment of inertia of the base layer 1 measured at 25° C. using a nano indenter is 40 N·mm 2 the following.
[0194] In the dicing tape 10 for dicing the die-bonding film 20, as described above, the heat shrinkage rate of the substrate layer 1 in the MD direction at 100° C. is preferably 0.01% or more, more preferably 0.1% or more, and further preferably 1% or more, and the bending hardness calculated as the product of the elastic modulus of the substrate layer 1 measured at 25° C. using a nanoindenter and the cross-sectional inertia moment of the substrate layer 1 is preferably 3 N·mm 2 More preferably, 10 N·mm 2 above.
[0195] In addition, in the dicing tape 10 for dicing the die-bonding film 20, as described above, the elastic recovery rate when measured at 25°C using a nanoindenter on the surface layer portion on the side of the laminated adhesive layer 2 of the base layer 1 is preferably 75% or less, more preferably 65% or less. The elastic recovery rate is preferably 50% or more, more preferably 60% or more.
[0196] Furthermore, in the dicing tape 10 for dicing the die-bonding film 20, as described above, the hardness of the surface on the side of the laminated adhesive layer 2 of the base layer 1 when measured at 25°C using a nanoindenter is preferably 40 MPa or less, more preferably 35 MPa or less. The hardness is preferably 20 MPa or more, more preferably 30 MPa or more.
[0197] The die bonding layer 3 preferably has thermosetting properties. The die bonding layer 3 can be given thermosetting properties by including at least one of a thermosetting resin and a thermoplastic resin having a thermosetting functional group.
[0198] When the die bonding layer 3 contains a thermosetting resin, examples of such thermosetting resins include epoxy resins, phenolic resins, amino resins, unsaturated polyester resins, polyurethane resins, silicone resins, and thermosetting polyimide resins, etc. Among these, epoxy resins are preferably used.
[0199] Examples of the epoxy resin include bisphenol A type, bisphenol F type, bisphenol S type, brominated bisphenol A type, hydrogenated bisphenol A type, bisphenol AF type, biphenyl type, naphthalene type, fluorene type, phenol novolac type, o-cresol novolac type, trihydroxyphenylmethane type, tetraphenolethane type, hydantoin type, triglycidyl isocyanurate type, and glycidylamine type epoxy resins.
[0200] Examples of the phenol resin used as a curing agent for the epoxy resin include novolac-type phenol resins, resol-type phenol resins, and polyoxystyrene such as polyparaoxystyrene.
[0201] When the die bonding layer 3 includes a thermoplastic resin having a thermosetting functional group, such a thermoplastic resin may include, for example, an acrylic resin containing a thermosetting functional group. Among the acrylic resins containing a thermosetting functional group, an acrylic resin containing a monomer unit derived from a (meth)acrylate may be included.
[0202] For a thermosetting resin having a thermosetting functional group, a curing agent can be selected according to the type of the thermosetting functional group.
[0203] The die bonding layer 3 may contain a thermal curing catalyst from the viewpoint of sufficiently advancing the curing reaction of the resin component or increasing the curing reaction rate. Examples of the thermal curing catalyst include imidazole compounds, triphenylphosphine compounds, amine compounds, and trihaloborane compounds.
[0204] The chip bonding layer 3 may include a thermoplastic resin. The thermoplastic resin acts as a binder. As thermoplastic resins, for example, natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylate copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide 6, polyamide 6,6 and other polyamide resins, phenoxy resins, acrylic resins, saturated polyester resins such as PET and PBT, polyamide-imide resins, fluororesins, etc. The above-mentioned thermoplastic resins may be used alone or in combination of two or more. As the above-mentioned thermoplastic resin, acrylic resins are preferred from the viewpoint of having few ionic impurities and high heat resistance, thereby easily ensuring the connection reliability based on the chip bonding layer.
[0205] The acrylic resin is preferably a polymer containing monomer units derived from (meth)acrylate as the largest monomer units in terms of mass ratio. Examples of (meth)acrylate include alkyl (meth)acrylate, cycloalkyl (meth)acrylate, and aryl (meth)acrylate. The acrylic resin may include monomer units derived from other components that can be copolymerized with (meth)acrylate. Examples of other components include functional group-containing monomers such as carboxyl-containing monomers, anhydride monomers, hydroxyl-containing monomers, glycidyl-containing monomers, sulfonic acid-containing monomers, phosphoric acid-containing monomers, acrylamide, and acrylonitrile, and various multifunctional monomers. From the viewpoint of achieving high cohesion in the chip bonding layer, the above-mentioned acrylic resin is preferably a copolymer of (meth)acrylate (especially (meth)acrylate alkyl ester having an alkyl group with a carbon number of 4 or less) and a carboxyl group-containing monomer, a nitrogen atom-containing monomer, or a polyfunctional monomer (especially a polyglycidyl-based polyfunctional monomer), and more preferably a copolymer of ethyl acrylate and butyl acrylate, acrylic acid, acrylonitrile, or polyglycidyl (meth)acrylate.
[0206] The die bonding layer 3 may contain one or more other components as necessary. Examples of other components include flame retardants, silane coupling agents, and ion scavengers.
[0207] The thickness of the die bond layer 3 is not particularly limited, and is, for example, 1 μm to 200 μm. The thickness may be 3 μm to 150 μm, or 5 μm to 100 μm.
[0208] The dicing die-bonding film 20 of the present embodiment can be used as an auxiliary tool for manufacturing a semiconductor integrated circuit, for example. A specific example of using the dicing die-bonding film 20 will be described below.
[0209] Hereinafter, an example using the dicing die-bonding film 20 including a single base material layer 1 will be described.
[0210] The method for manufacturing a semiconductor integrated circuit has the following steps: a half-cutting step of forming grooves in a semiconductor wafer to be processed into a die by dicing the semiconductor wafer; a back grinding step of grinding the semiconductor wafer after the half-cutting step to reduce the thickness; a mounting step of attaching one side (e.g., the side opposite to the circuit side) of the semiconductor wafer after the back grinding step to a die bonding layer 3 and fixing the semiconductor wafer to a dicing tape 10; an expansion step of expanding the interval between the semiconductor chips processed by the half-cutting process; a cut-out maintaining step of maintaining the interval between the semiconductor chips; a pick-up step of peeling the die bonding layer 3 from the adhesive layer 2 and taking out the semiconductor die with the die bonding layer 3 attached; and a die bonding step of attaching the semiconductor die with the die bonding layer 3 attached to an adherend. When implementing these steps, the dicing tape (dicing die bonding film) of the present embodiment is used as a manufacturing auxiliary tool.
[0211] In the half-cutting process, Figure 3A and Figure 3B As shown in FIG. 1 , a half-cutting process is performed to cut the semiconductor integrated circuit into small pieces (dies). Specifically, a wafer processing tape T (see FIG. 1 ) is attached to the surface of the semiconductor wafer W opposite to the circuit surface. Figure 3A ). In addition, the dicing ring R is mounted on the wafer processing tape T (refer to Figure 3A ). A groove for dividing is formed in a state where the wafer processing tape T is attached (refer to Figure 3B ). In the back grinding process, such as Figure 3C and Figure 3D Specifically, the back grinding tape G is attached to the surface where the grooves are formed, and the wafer processing tape T attached initially is peeled off (see Figure 3C ). Grinding is performed with the back grinding tape G attached until the semiconductor wafer W reaches a predetermined thickness (see Figure 3D ).
[0212] During the installation process, Figure 4A to Figure 4B As shown, after the dicing ring R is attached to the adhesive layer 2 of the dicing tape 10, the semiconductor wafer W (see FIG. 1 ) which has been half-cut is attached to the exposed surface of the die bonding layer 3. Figure 4A ). Thereafter, the back grinding tape G is peeled off from the semiconductor wafer W (see Figure 4B ).
[0213] In the expansion process, Figure 5A to Figure 5CAs shown, the dicing ring R is fixed to the holder H of the expansion device. The dicing die bonding film 20 is lifted from the lower side using the lifting member U provided in the expansion device, thereby stretching the dicing die bonding film 20 and expanding it in the surface direction (see Figure 5B ). Thus, the semiconductor wafer W that has been half-cut is cut under a specific temperature condition. The temperature condition is, for example, -20 to 5°C, preferably -15 to 0°C, and more preferably -10 to -5°C. The extended state is released by lowering the lifting member U (see Figure 5C ).
[0214] Furthermore, in the expansion process, Figure 6A to Figure 6B As shown, the dicing tape 10 is stretched under a higher temperature condition (for example, room temperature (23° C.)) to expand the area. Thus, the cut adjacent semiconductor chips W are separated in the plane direction of the film surface, and the interval is further increased.
[0215] It should be noted that, in the expansion step, as described above, resistance is generated in the base material layer 1 in the direction away from the semiconductor chip.
[0216] Here, in the dicing tape 10 for dicing the die-bonding film 20 according to the present embodiment, the bending hardness of the base layer 1 obtained as the product of the elastic modulus of the base layer 1 measured at 25° C. using a nanoindenter and the cross-sectional inertia moment of the base layer 1 is 40 N·mm 2 Therefore, in the expansion step, the base layer 1 is relatively easy to bend and deform. That is, even if the outer peripheral portion of the semiconductor chip is displaced in the swelling direction, the base layer 1 is relatively easy to follow the displacement.
[0217] In the incision maintenance process, Figure 7 As shown, hot air (eg, 100 to 130° C.) is blown toward the dicing tape 10 to heat-shrink the dicing tape 10 , and then the dicing tape 10 is cooled and solidified, thereby maintaining the distance (kerf) between the cut adjacent semiconductor chips.
[0218] Here, in the dicing tape 10 for dicing the die-bonding film 20 according to the present embodiment, the heat shrinkage rate of the base layer 1 in the MD direction at 100° C. is 20% or less, so the heat shrinkage of the base layer 1 in the incision maintaining step can be relatively reduced. Therefore, as described above, in the expansion step, even if resistance in the direction away from the semiconductor chip is generated in the base layer 1, the resistance remaining in the base layer after heat shrinkage can be made small. As a result, the peripheral portion of the semiconductor chip can be relatively suppressed from bulging from the adhesive layer 2.
[0219] In the picking process, Figure 8As shown, the semiconductor chip W with the die bonding layer 3 attached thereto is peeled off from the adhesive layer 2 of the dicing tape 10. Specifically, the pin member P is raised to lift up the semiconductor chip W to be picked up through the dicing tape 10. The lifted semiconductor chip is held by the suction jig J.
[0220] In the die bonding step, the semiconductor chip W with the die bonding layer 3 attached thereto is bonded to an adherend.
[0221] In the above-mentioned manufacture of the semiconductor integrated circuit, an example in which the dicing die-bonding film 20 is used as an auxiliary tool is described. However, when the dicing tape 10 is used as an auxiliary tool, the semiconductor integrated circuit can be manufactured in the same manner as described above.
[0222] Matters disclosed by this specification include the following. (1)
[0224] A dicing tape comprising a base material layer and an adhesive layer laminated thereon.
[0225] The substrate layer is composed of a resin film having a single structure or a laminated structure.
[0226] The heat shrinkage of the substrate layer in the MD direction at 100°C is 20% or less, and the bending hardness calculated as the product of the elastic modulus of the substrate layer and the cross-sectional inertia moment of the substrate layer measured at 25°C using a nanoindenter is 40 N·mm 2 the following.
[0227] According to this configuration, since the thermal shrinkage rate of the substrate layer in the MD direction at 100° C. is 20% or less, the thermal shrinkage of the substrate layer in the incision maintaining step can be relatively reduced. Therefore, in the expansion step, even if resistance in the direction away from the semiconductor chip is generated in the substrate layer, the resistance remaining in the substrate layer after thermal shrinkage can be reduced. As a result, the peripheral portion of the semiconductor chip can be relatively suppressed from bulging from the adhesive layer.
[0228] In addition, the bending hardness of the substrate layer, which is obtained by the product of the elastic modulus of the substrate layer measured at 25° C. using a nanoindenter and the cross-sectional inertia moment of the substrate layer, is 40 N·mm 2 Therefore, in the expansion step, the base layer is relatively easy to bend and deform. That is, even if the peripheral portion of the semiconductor chip is displaced in the swelling direction, the base layer is relatively easy to follow the displacement.
[0229] This can relatively suppress chip floating after the cutout maintaining step.
[0230] (2) The cutting tape according to (1) above, wherein:
[0231] The substrate layer has a heat shrinkage in the MD direction at 100° C. of 1% or more.
[0232] According to this configuration, after the semiconductor wafer is cut into semiconductor chips, the distance between the semiconductor chips (ie, the kerf) can be more sufficiently maintained.
[0233] (3) The cutting tape according to (1) or (2) above, wherein:
[0234] The bending hardness of the substrate layer, which is obtained by the product of the elastic modulus of the substrate layer measured at 25° C. using a nanoindenter and the cross-sectional inertia moment of the substrate layer, is 3 N·mm 2 above.
[0235] According to this configuration, the individualized dicing tape can be smoothly peeled off from the long separator in the product form.
[0236] (4) The cutting tape according to any one of (1) to (3) above, wherein
[0237] The elastic recovery rate of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is 75% or less when measured at 25° C. using a nanoindenter.
[0238] According to this configuration, the elastic recovery rate of the surface layer of the substrate layer on the side where the adhesive layer is stacked is 75% or less when measured at 25°C using a nanoindenter. Therefore, even if resistance in the direction away from the semiconductor chip is generated in the substrate layer during the expansion process, the resistance remaining in the substrate layer can be further reduced after heat shrinkage. As a result, it is possible to further suppress the peripheral portion of the semiconductor chip from bulging from the adhesive layer.
[0239] This can further suppress chip floating after the cutout maintaining step.
[0240] (5) The cutting tape according to (4) above, wherein:
[0241] The elastic recovery rate of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is 50% or more when measured at 25° C. using a nanoindenter.
[0242] According to this configuration, it is possible to more fully suppress the appearance defect caused by the deformation of the base material layer.
[0243] (6) The cutting tape according to any one of (1) to (5) above, wherein:
[0244] The hardness of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is 40 MPa or less when measured at 25° C. using a nanoindenter.
[0245] According to this configuration, the hardness of the surface portion of the substrate layer on the side where the adhesive layer is stacked is 40 MPa or less when measured at 25°C using a nanoindenter. Therefore, even if resistance in the direction away from the semiconductor chip is generated in the substrate layer during the expansion process, the resistance remaining in the substrate layer after heat shrinkage can be further reduced. As a result, the peripheral portion of the semiconductor chip can be further suppressed from bulging from the adhesive layer.
[0246] This can further suppress chip floating after the cutout maintaining step.
[0247] (7) The cutting tape according to (6) above, wherein:
[0248] The hardness of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is 20 MPa or more when measured at 25° C. using a nanoindenter.
[0249] According to this configuration, the semiconductor wafer and the die bonding layer can be diced more satisfactorily.
[0250] (8) A dicing die-bonding film comprising:
[0251] A dicing tape having an adhesive layer laminated on a base material layer; and
[0252] a die bonding layer laminated on the adhesive layer of the dicing tape,
[0253] The substrate layer is composed of a resin film having a single structure or a laminated structure.
[0254] The heat shrinkage of the substrate layer in the MD direction at 100°C is 20% or less, and the bending hardness calculated as the product of the elastic modulus of the substrate layer and the cross-sectional inertia moment of the substrate layer measured at 25°C using a nanoindenter is 40 N·mm 2 the following.
[0255] According to this configuration, even if resistance in a direction away from the semiconductor chip is generated in the base layer during the expansion step, the resistance remaining in the base layer after heat shrinkage can be reduced, and the base layer can be elastically deformed more easily during the expansion step.
[0256] This can relatively suppress chip floating after the cutout maintaining step.
[0257] (9) The dicing die-bonding film according to (8) above, wherein
[0258] The elastic recovery rate of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is 75% or less when measured at 25° C. using a nanoindenter.
[0259] (10) The dicing die-bonding film according to (8) or (9) above, wherein
[0260] The hardness of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is 40 MPa or less when measured at 25° C. using a nanoindenter.
[0261] According to this configuration, chip floating after the cutout maintaining step can be further suppressed.
[0262] It should be noted that the dicing tape and dicing die bonding film of the present invention are not limited to the aforementioned embodiments. In addition, the dicing tape and dicing die bonding film of the present invention are not limited by the aforementioned effects. The dicing tape and dicing die bonding film of the present invention can be variously modified within the scope of the present invention.
[0263] Example
[0264] The following examples are provided to further illustrate the present invention in detail, but are not intended to limit the scope of the present invention.
[0265] [Example 1]
[0266] <Formation of Base Material Layer>
[0267] Two types of three-layer extrusion T-die molding machines were used to mold a base material layer having a three-layer structure of layer A / layer B / layer C (a three-layer structure in which layer B is the center layer and layers A and C are laminated on both sides of layer B as outer layers). Metallocene PP (trade name: WINTEC WFX4M, manufactured by Japan Polypropylene Co., Ltd.) was used as the resin for layer A and layer C, and EVA (trade name: Ultrathene (registered trademark) 626, manufactured by Tosoh Corporation) was used as the resin for layer B.
[0268] The extrusion molding was performed at a die temperature of 190°C. That is, the A layer, the B layer, and the C layer were extruded at 190°C. The thickness of the substrate layer obtained by extrusion molding was 80 μm. It should be noted that the thickness ratio (layer thickness ratio) of the A layer, the B layer, and the C layer was A layer: B layer: C layer = 1:10:1.
[0269] After the formed base material layer is sufficiently cured, the cured base material layer is wound into a roll to obtain a roll body.
[0270] <Production of cutting tape>
[0271] The adhesive composition was applied from the roll substrate layer to one surface of the substrate layer using an applicator to a thickness of 10 μm. The substrate layer coated with the adhesive composition was heated and dried at 110° C. for 3 minutes to form an adhesive layer, thereby obtaining a dicing tape.
[0272] The above-mentioned adhesive composition was prepared as follows.
[0273] First, 173 parts by mass of INA (isononyl acrylate), 54.5 parts by mass of HEA (hydroxyethyl acrylate), 0.46 parts by mass of AIBN (2,2′-azobisisobutyronitrile), and 372 parts by mass of ethyl acetate were mixed to obtain a first resin composition.
[0274] Thereafter, the first resin composition was added to the round-bottomed separable flask of the polymerization experimental apparatus equipped with a round-bottomed separable flask (capacity 1 L), a thermometer, a nitrogen inlet tube and a stirring blade, and the liquid temperature of the first resin composition was brought to room temperature (23° C.) while stirring the first resin composition, and the atmosphere in the round-bottomed separable flask was purged with nitrogen for 6 hours.
[0275] Next, while nitrogen was flowing into the round-bottom separable flask, the first resin composition was kept at a liquid temperature of 62° C. for 3 hours while being stirred, and then further kept at 75° C. for 2 hours to polymerize the INA, HEA, and AIBN to obtain a second resin composition. Thereafter, the flow of nitrogen into the round-bottom separable flask was stopped.
[0276] The second resin composition was cooled until the liquid temperature reached room temperature, and then 52.5 parts by mass of 2-isocyanatoethyl methacrylate (manufactured by Showa Denko K.K., trade name "Karenz MOI (registered trademark)") as a compound having a polymerizable carbon-carbon double bond and 0.26 parts by mass of dibutyltin IV dilaurate (manufactured by Wako Pure Chemical Industries, Ltd.) were added to the second resin composition to obtain a third resin composition, and the obtained third resin composition was stirred in an air atmosphere at a liquid temperature of 50°C for 24 hours.
[0277] Thereafter, 0.75 parts by mass of CORONATE L (isocyanate compound) and 2 parts by mass of Omnirad 127 (photopolymerization initiator) were added to the third resin composition based on 100 parts by mass of the polymer solid content, and the third resin composition was diluted with ethyl acetate to a solid content concentration of 20% by mass to prepare an adhesive composition.
[0278] <Production of Dicing Die Bonding Film>
[0279] 100 parts by mass of an acrylic resin (manufactured by Nagase Chemical Co., Ltd., trade name "SG-P3", glass transition temperature 12°C), 46 parts by mass of an epoxy resin (manufactured by Mitsubishi Chemical Corporation, trade name "JER1001"), 51 parts by mass of a phenolic resin (manufactured by Meiwa Chemicals Co., Ltd., trade name "MEH-7851ss"), 191 parts by mass of spherical silica (manufactured by Admatechs, trade name "SO-25R"), and 0.6 parts by mass of a curing catalyst (manufactured by Shikoku Chemicals Co., Ltd., trade name "CUREZOL PHZ") are added to methyl ethyl ketone and mixed to obtain a chip bonding composition having a solid content concentration of 20% by mass.
[0280] Afterwards, the chip bonding composition is applied to the silicone-treated surface of a PET-based separator (50 μm thick) serving as a release liner using an applicator in a manner to a thickness of 10 μm, and the composition is dried at 130°C for 2 minutes to remove the solvent from the chip bonding composition, thereby obtaining a chip bonding sheet having a chip bonding layer stacked on the release liner.
[0281] Thereafter, the side of the die-bonding sheet on which the release sheet is not laminated is bonded to the pressure-sensitive adhesive layer of the dicing tape, and then the release liner is peeled from the die-bonding layer to obtain a dicing die-bonding film having a die-bonding layer.
[0282] (Bending hardness)
[0283] The bending hardness of the base material layer before forming the adhesive layer was determined.
[0284] The bending hardness is determined as the product of the elastic modulus of the substrate layer measured at 25° C. using a nanoindenter and the cross-sectional moment of inertia of the substrate layer.
[0285] The elastic modulus of the base material layer before forming the adhesive layer was determined as follows.
[0286] Measurement apparatus and measurement conditions
[0287] · Device: Tribo Indenter (manufactured by Hysitron Inc.)
[0288] ·Indenter used: Berkovich type diamond indenter (triangular pyramid type)
[0289] ·Measurement method: Single press measurement
[0290] ·Measurement temperature: 25℃
[0291] Pressing depth setting: 200nm
[0292] ·Measurement atmosphere: Air
[0293] Load (pressing) speed: 20nm / sec
[0294] Unloading speed (pulling): 20nm / sec
[0295] Measurement sample
[0296] The entire diced tape (length l: 5 mm, width w: 5 mm, thickness t: 125 μm) was embedded with an embedding resin, and then the embedded diced tape was cut into a cross section (exposed cross section) along the width direction using a microtome to prepare a measurement sample.
[0297] As the embedding resin, DEV-TUBE S-31 (manufactured by ITW PP&F JAPAN) can be used.
[0298] Determination method
[0299] (1) The measurement sample is kept at 25°C for 1 hour.
[0300] (2) The measurement sample is arranged so that the pressing direction of the Berkovich-type diamond indenter is perpendicular to the surface of the substrate layer of the measurement sample.
[0301] (3) After the tip of the Berkovich-type diamond indenter was brought into contact with the surface of the substrate layer of the measurement sample, the Berkovich-type diamond indenter was pressed from the surface of the substrate layer 1 to a depth of 200 nm at a load speed of 20 nm / s.
[0302] (4) After the Berkovich-type diamond indenter was pressed from the surface of the substrate layer to a depth of 200 nm, the Berkovich-type diamond indenter was returned to the position at the start of the pressing at a deloading speed of 20 nm / s.
[0303] (5) Using the analysis software "Triboscan Ver.9.2.12.0", the elastic modulus is calculated based on the displacements of the substrate layer 1 when the indenter is unloaded from the deepest pressing position, the load applied to the substrate layer when the aforementioned displacements are reached, and the theoretically calculated indentation area at the aforementioned displacements (the contact area (contact projection area) between the indenter and the substrate layer 1 when the aforementioned displacements are reached).
[0304] The above measurement is performed at three different locations on the base material layer, and the elastic modulus calculated at the three locations is arithmetic averaged to determine the elastic modulus of the base material layer.
[0305] Since the base material layer described in Example 1 has a three-layer structure, the elastic modulus was determined for each layer.
[0306] In addition, assuming that the cross section of the base layer is a rectangular shape, the cross-sectional moment of inertia of the base layer before the pressure-sensitive adhesive layer is formed is calculated using the following formula.
[0307] I=w×h 3 / 12 (where w is the width of the substrate layer and h is the thickness of the substrate layer)
[0308] Here, since the base material layer described in Example 1 has a three-layer structure, the area moment of inertia was calculated for each layer.
[0309] It should be noted that the first layer (A layer) of the substrate layer has a width of 300 mm and a thickness of 10.4 μm, the second layer (B layer) of the substrate layer has a width of 300 mm and a thickness of 10.4 μm, and the third layer (C layer) of the substrate layer has a width of 300 mm and a thickness of 10.4 μm.
[0310] It should be noted that the bending hardness of the base material layer described in Example 1 was determined by calculating the product of the elastic modulus and the cross-sectional moment of inertia for each layer and adding them together.
[0311] (Elastic recovery rate)
[0312] The elastic recovery rate was determined for the base material layer before the pressure-sensitive adhesive layer was formed.
[0313] The elastic recovery rate can be measured by using the same measuring device and measuring sample as the device and sample used in the measurement of the above-mentioned substrate layer, adopting the same measuring conditions as the measuring conditions of the elastic modulus of the above-mentioned substrate layer, using the analysis software "Triboscan Ver.9.2.12.0", and adopting the same measuring method as the elastic modulus of the above-mentioned substrate layer.
[0314] (hardness)
[0315] The hardness of the base material layer before the adhesive layer was formed was determined.
[0316] The hardness can be measured by using the same measuring device and measuring sample as those used in the measurement of the above-mentioned substrate layer, adopting the same measuring conditions as the measuring conditions of the elastic modulus of the above-mentioned substrate layer, and using the analysis software "Triboscan Ver.9.2.12.0", and calculating the hardness of the substrate layer based on the load applied to the substrate layer when the indenter is pressed deepest, and the indentation area theoretically calculated when the indenter is pressed deepest (the contact area between the indenter and the substrate layer when the indenter is pressed deepest (contact projection area)).
[0317] (Heat shrinkage)
[0318] A test piece having a predetermined size (width 20 mm, length 120 mm) was cut out from the base layer before forming the adhesive layer so that the MD direction became the longitudinal direction, and the heat shrinkage rate in the MD direction at 100°C was measured.
[0319] The thermal shrinkage ratio was determined according to the following procedure.
[0320] (1) Markings were made at locations 10 mm away from both ends in the longitudinal direction of the test piece before heating.
[0321] (2) The distance L0 between the marks of the test piece before heating (ie, the initial length in the MD direction) is measured.
[0322] (3) The test piece was exposed to an environment at a temperature of 100° C. for 60 seconds with the portion outside the marked portion (ie, the end portion in the longitudinal direction) fixed by a clamp.
[0323] (4) After the test piece is cooled to room temperature (23±2° C.), the length L1 is measured at the same location as in (2).
[0324] (5) Calculate the dimensional change rate R of the test piece in the longitudinal direction (MD direction) according to the following formula: C .
[0325] R C =(L0-L1) / L0×100
[0326] (Evaluation of chip floating)
[0327] A bare wafer (300 mm in diameter) and a dicing ring were attached to the dicing die-bonding film of Example 1 obtained as described above.
[0328] Next, the semiconductor wafer and the die bonding layer were diced using a die separation device DDS230 (manufactured by DISCO Corporation), and chip floating after dicing was evaluated. The bare wafer was cut into bare chips of a size of 10 mm in length×10 mm in width×0.055 mm in thickness.
[0329] It should be noted that a warped wafer was used as the bare wafer.
[0330] A warped wafer was produced as follows.
[0331] First, the following (a) to (f) were dissolved in methyl ethyl ketone to obtain a warpage control composition having a solid content concentration of 20% by mass.
[0332] (a) Acrylic resin (manufactured by Nagase Chemical Co., Ltd., trade name "SG-70L"): 5 parts by mass
[0333] (b) Epoxy resin (manufactured by Mitsubishi Chemical Corporation, trade name "JER828"): 5 parts by mass
[0334] (c) Phenolic resin (produced by Meiwa Chemicals Co., Ltd., trade name "LDR8210"): 14 parts by mass
[0335] (d) Epoxy resin (manufactured by Mitsubishi Chemical Corporation, trade name "MEH-8005"): 2 parts by mass
[0336] (e) Spherical silica (manufactured by Admatechs, trade name "SO-25R"): 53 parts by mass
[0337] (f) Phosphorus-based catalyst (TPP-K): 1 part by mass
[0338] Afterwards, the warp adjusting composition was applied to the silicone-treated surface of a PET-based separator (thickness 50 μm) serving as a release liner using an applicator at a thickness of 25 μm, and dried at 130°C for 2 minutes to remove the solvent from the warp adjusting composition, thereby obtaining a warp adjusting sheet having a warp adjusting layer laminated on the release liner.
[0339] Afterwards, a laminator (manufactured by MCK, model MRK-600) was used to stick the bare wafer to the side of the warp adjustment sheet on which the peeling liner was not stacked at 60°C, 0.1 MPa, and 10 mm / s, and the wafer was placed in an oven and heated at 175°C for 1 hour to thermally cure the resin of the warp adjustment layer, thereby shrinking the warp adjustment layer to obtain a warped bare wafer.
[0340] After shrinking the warp adjustment layer, a wafer processing tape (manufactured by Nitto Denko Corporation, trade name "V-12SR2") was attached to the side of the warped bare wafer on which the warp adjustment layer was not laminated, and then a dicing ring was fixed to the warped bare wafer via the wafer processing tape. Thereafter, the warp adjustment layer was removed from the warped bare wafer.
[0341] Using a dicing apparatus (manufactured by DISCO, Model 6361), grooves 100 μm deep from the warped bare wafer were formed in a grid pattern (20 μm wide) on the entire surface (hereinafter referred to as one surface) from which the warp adjusting layer was removed.
[0342] Thereafter, a back grinding tape is bonded to one surface of the warped bare wafer, and the wafer processing tape is removed from the other surface (the surface opposite to the one surface) of the warped bare wafer.
[0343] Thereafter, the warped bare wafer was ground from the other surface side using a back grinder (manufactured by DISCO Corporation, model DGP8760) until the thickness of the warped bare wafer reached 55 μm (0.055 mm), and the obtained wafer was referred to as a warped wafer.
[0344] Specifically, chip floating was evaluated as follows.
[0345] First, a cold expansion unit is used to cut the bare wafer and the chip bonding layer under the conditions of an expansion temperature of -5°C, an expansion speed of 100 mm / sec, and an expansion amount of 12 mm to obtain a semiconductor chip with a chip bonding layer.
[0346] After that, the expansion was carried out at room temperature, an expansion speed of 1 mm / sec, and an expansion distance of 5 mm. Then, while maintaining the expansion state, the dicing die bonding film at the boundary portion with the outer edge of the bare wafer was thermally shrunk at a heating temperature of 200°C, a heating distance of 18 mm, and a rotation speed of 5° / sec.
[0347] After that, the floating state of the semiconductor chip with the die bonding layer was photographed under a microscope on the surface of the substrate layer of the cut die bonding film and binarized to calculate the floating area. In addition, the floating area was evaluated as 0 when it was less than 4%, and as × when it was more than 4%.
[0348] [Example 2]
[0349] The dicing tape and dicing die-bonding film described in Example 2 were obtained in the same manner as in Example 1 except that the base material layer was set to 125 μm.
[0350] Furthermore, the same procedure as in Example 1 was carried out for the base material layer described in Example 2 to determine the bending hardness, elastic recovery rate, and hardness.
[0351] Furthermore, the base material layer described in Example 2 was evaluated for chip floating in the same manner as in Example 1.
[0352] [Example 3]
[0353] The dicing tape and dicing die-bonding film described in Example 3 were obtained in the same manner as in Example 1 except that the thickness of the base material layer was changed to 150 μm.
[0354] Furthermore, the same operation as in Example 1 was carried out for the base material layer described in Example 3 to determine the bending hardness, elastic recovery rate, and hardness.
[0355] Furthermore, the chip floating was evaluated in the same manner as in Example 1 with respect to the base material layer described in Example 3.
[0356] [Example 4]
[0357] The dicing tape and dicing die-bonding film described in Example 4 were obtained in the same manner as in Example 3 except that the thickness ratio (layer thickness ratio) of the A layer, the B layer, and the C layer was set to A layer:B layer:C layer=1:4:1.
[0358] Furthermore, the same procedure as in Example 1 was carried out for the base material layer described in Example 4 to determine the bending hardness, elastic recovery rate, and hardness.
[0359] Furthermore, the base material layer described in Example 4 was evaluated for chip floating in the same manner as in Example 1.
[0360] [Example 5]
[0361] The dicing tape and dicing die-bonding film described in Example 5 were obtained in the same manner as in Example 2 except that the base layer was composed of two layers, A layer and B layer, and the layer thickness ratio of the base layer was set to A layer:B layer=1:5.
[0362] Furthermore, the same procedure as in Example 1 was carried out for the base material layer described in Example 5 to determine the bending hardness, elastic recovery rate, and hardness.
[0363] Furthermore, the base material layer described in Example 5 was evaluated for chip floating in the same manner as in Example 1.
[0364] [Example 6]
[0365] The dicing tape and dicing die-bonding film described in Example 6 were obtained in the same manner as in Example 2 except that the resin of the A layer and the C layer (outer layer) constituting the base material layer was Novatec LC720.
[0366] Furthermore, the same procedure as in Example 1 was carried out for the base material layer described in Example 6 to determine the bending hardness, elastic recovery rate, and hardness.
[0367] Furthermore, the base material layer described in Example 6 was evaluated for chip floating in the same manner as in Example 1.
[0368] [Example 7]
[0369] The dicing tape and dicing die-bonding film described in Example 7 were obtained in the same manner as in Example 2 except that the resin of the A layer and the C layer (outer layer) constituting the base material layer was Nipolon Hard (registered trademark) 2000 (manufactured by Tosoh Corporation).
[0370] Furthermore, the same procedure as in Example 1 was carried out for the base material layer described in Example 7 to determine the bending hardness, elastic recovery rate, and hardness.
[0371] Furthermore, the base material layer described in Example 7 was evaluated for chip floating in the same manner as in Example 1.
[0372] [Comparative Example 1]
[0373] The dicing tape and dicing die-bonding film described in Comparative Example 1 were obtained in the same manner as in Example 2 except that the base layer was constituted by one layer A.
[0374] In addition, the same operation as in Example 1 was carried out for the base material layer described in Comparative Example 1 to determine the bending hardness, elastic recovery rate, and hardness.
[0375] Furthermore, the base material layer described in Comparative Example 1 was evaluated for chip floating in the same manner as in Example 1.
[0376] [Comparative Example 2]
[0377] The dicing tape and dicing die-bonding film described in Comparative Example 2 were obtained in the same manner as in Comparative Example 1 except that the resin of the layer A constituting the base layer was Nipolon Hard (registered trademark) 2000 (manufactured by Tosoh Corporation) and the layer thickness was 150 μm.
[0378] In addition, the same operation as in Example 1 was carried out for the base material layer described in Comparative Example 2 to determine the bending hardness, elastic recovery rate, and hardness.
[0379] Furthermore, the base material layer described in Comparative Example 2 was evaluated for chip floating in the same manner as in Example 1.
[0380] The bending hardness, elastic recovery rate and hardness results were obtained for the base material layer described in each example, and the die floating was evaluated for the dicing die-bonding film described in each example. The results are shown in Table 1 below.
[0381] [Table 1]
[0382]
[0383] It can be seen from Table 1 that the substrate layers described in Examples 1 to 7 all showed a pressure of 40 N·mm 2 The dicing die-bonding films of Examples 1 to 7 had a bending hardness of 0.0447 W / m and a thermal shrinkage of 20% or less, and were able to suppress chip floating.
[0384] In contrast, it can be seen that although the bending hardness of the base material layer in Comparative Example 1 is 40 N·mm 2 However, the heat shrinkage ratio exceeded 20%, and the dicing die-bonding film described in Comparative Example 1 could not sufficiently suppress chip floating.
[0385] In addition, it is found that although the thermal shrinkage of the base material layer described in Comparative Example 2 is 20% or less, the bending hardness exceeds 40 N·mm. 2 , the dicing die-bonding film described in Comparative Example 2 cannot sufficiently suppress chip floating.
[0386] It should be noted that although the results shown in Table 1 are about the dicing die-bonding film, it is expected that the same results as those shown in Table 1 can be obtained by using a dicing tape included in the dicing die-bonding film.
Claims
1. A dicing tape comprising a base material layer and an adhesive layer laminated thereon, The base layer is composed of a resin film having a laminated structure including an elastomer layer and a non-elastic layer, wherein the elastomer layer contains an elastomer and the non-elastic layer contains a polypropylene resin which is a polymerization product obtained using a metallocene catalyst. The base layer has a two-layer structure in which the elastomer layer and the non-elastic layer are stacked, or a three-layer structure in which two non-elastic layers are arranged on both sides of the elastomer layer. The heat shrinkage of the substrate layer in the MD direction at 100° C. is 20% or less, and the bending hardness calculated as the product of the elastic modulus of the substrate layer and the cross-sectional inertia moment of the substrate layer measured at 25° C. using a nanoindenter is 40 N·mm 2 the following.
2. The cutting tape according to claim 1, wherein: The elastic recovery rate of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is 75% or less when measured at 25° C. using a nanoindenter.
3. The cutting tape according to claim 1 or 2, wherein: The hardness of the surface layer portion of the substrate layer on the side where the pressure-sensitive adhesive layer is laminated is 40 MPa or less when measured at 25° C. using a nanoindenter.
4. A dicing die bonding film comprising: A dicing tape having an adhesive layer laminated on a base material layer; and a die bonding layer laminated on the adhesive layer of the dicing tape, The base layer is composed of a resin film having a laminated structure including an elastomer layer and a non-elastic layer, wherein the elastomer layer contains an elastomer and the non-elastic layer contains a polypropylene resin which is a polymerization product obtained using a metallocene catalyst. The base layer has a two-layer structure in which the elastomer layer and the non-elastic layer are stacked, or a three-layer structure in which two non-elastic layers are arranged on both sides of the elastomer layer. The heat shrinkage of the substrate layer in the MD direction at 100° C. is 20% or less, and the bending hardness calculated as the product of the elastic modulus of the substrate layer and the cross-sectional inertia moment of the substrate layer measured at 25° C. using a nanoindenter is 40 N·mm 2 the following.
Citation Information
Patent Citations
Dicing tape, dicing die-bonding film, and method of manufacturing semiconductor device
JP2019016633A
Film for manufacturing semiconductor device and method of manufacturing semiconductor device
CN102190973A
Adhesive sheet
CN105102565A
Semiconductor processing tape
CN107431002A
Dicing die bond film
CN109971376A