Single photon avalanche detector, method of use and method of manufacturing the same
Through the planar germanium-on-silicon SPAD architecture that provides lateral confinement of the electric field in the Ge absorber layer, the problem of high cost of single-photon avalanche detectors in the existing technology is solved, and efficient detection and detection in the wavelength range of 1310nm to 1600nm are achieved. Low noise equivalent power, suitable for low-cost, mass production needs of LIDAR systems for automobiles and autonomous vehicles.
Patent Information
- Application Number
- CN201980067264.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-09-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-09-09
AI Technical Summary
The cost of existing single photon avalanche detectors (SPAD) in the wavelength range of 1310nm to 1550nm is high, and it is difficult to achieve low-cost, mass production with existing technology, especially in LIDAR systems for automobiles and autonomous vehicles. The high cost and large refrigerators of InGaAs/InP SPAD and superconducting single-photon detectors limit their applications.
Using a planar germanium-on-silicon SPAD architecture, by providing lateral confinement of the electric field in the Ge absorber layer, combined with a cheap germanium-on-silicon platform, single-photon avalanche diode (SPAD) devices and arrays with high performance are designed, including The avalanche layer of Si, the p-type charge sheet layer and the absorber layer of Ge optimize the electric field distribution to reduce the dark count rate and noise equivalent power.
It achieves high single-photon detection efficiency and low dark count rate in the wavelength range of 1310nm to 1600nm, reduces noise equivalent power, and has low cost. It is suitable for mass production and its performance is close to or exceeds that of commercial InGaAs/InP SPAD.
Smart Images

Figure CN112840466B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to single photon avalanche detectors (SPADs), in particular but not exclusively to single photon avalanche detectors designed to operate at wavelengths between 1300 nm and 1600 nm (SWIR) or 1300 nm and 1700 nm. The present invention relates to arrays of such detectors, and to methods of using such detectors or arrays and methods of making such detectors or arrays. Background Art
[0002] Single-photon detectors at 1310 nm and 1550 nm are in demand for a wide range of applications, including quantum optics, quantum-enhanced imaging, quantum communications over optical fiber, and LIDAR (light detection and ranging) for automobiles and autonomous vehicles. For imaging and ranging applications, operation between 1500 nm and 1600 nm is particularly important because this is an atmospheric window in which water vapor does not absorb or scatter light as strongly as at shorter wavelengths comprising the visible portion of the spectrum. Smoke
[54] , smog
[15] , and haze
[16] all have improved transparency in this window compared to visible light. Solar radiation, which is a background signal in visible wavelengths, is significantly reduced at 1550 nm compared to visible wavelengths
[14] . Since wavelengths above 1400 nm have an increased laser safety threshold compared to visible and near-infrared light
[13] , the optical power of the light source in an active system such as LIDAR can also be increased by at least 20 times at 1550 nm compared to visible wavelengths, thereby improving the signal-to-noise ratio in the system. Therefore, LIDAR performance at 1550nm is greatly improved compared to visible wavelengths, especially in the presence of most obstructions.
[0003] Some reports indicate that the LIDAR market was worth $580 million in 2016 (primarily geographic and information systems plus military systems with CMOS image sensors and robotics, which account for about 40% of the market) and is expected to grow to $1.2 billion by 2022, with automotive LIDAR accounting for 16% of the market. Being able to provide a $50 automotive LIDAR system for a vehicle would be of significant commercial interest. Many visible or near-visible (e.g., 905nm or 940nm) LIDAR systems utilizing all-silicon optical detectors are already available for automotive and autonomous vehicles.
[0004] Silicon CMOS SPADs are commercially available and operate in the visible range up to 940 nm, where the single photon detection efficiency (SPDE) is low (≤10%) due to the silicon indirect bandgap
[12] . Currently, the only commercially available single photon detectors for wavelengths between 1310 nm and 1550 nm are InGaAs / InP SPAD devices operating at 233 K using a Peltier cooler, with a single pixel module costing around £20,000. Imaging arrays of these InGaAs / InP SPAD devices cost ≥ £100,000 and are subject to ITAR (US regulatory regime) restrictions. Superconducting single photon detectors, which require cryogenic operation below 8 K and typically cost £80,000 each, are also commercially available, but the cryo-coolers are bulky and require large amounts of power, which limits their use in portable applications. Both technologies are expensive, and the market demand, particularly for automotive and autonomous vehicles, is typically for low-cost (~$50) systems, which will be difficult to achieve with existing technologies, even in large volumes.
[0005] It would be desirable to be able to produce single photon detector devices that can be manufactured in large quantities to mass produce inexpensive products having the performance required by the above-mentioned markets.
[0006] The present invention has been designed in view of the above considerations. Summary of the invention
[0007] The inventors have recognised that the use of a planar germanium-on-silicon SPAD architecture can provide significant performance. This forms an overall aspect of the present invention. It is known that a planar germanium-on-silicon SPAD architecture provides better performance than a mesa-type planar germanium-on-silicon SPAD architecture by providing lateral confinement of the electric field in the Ge absorber layer while exploiting an inexpensive germanium-on-silicon platform.
[0008] Therefore, in a first preferred aspect, the present invention provides a single photon avalanche diode (SPAD) device comprising:
[0009] A Si-based avalanche layer formed on the n-type semiconductor contact layer;
[0010] A p-type charge sheet layer formed in or on the avalanche layer, the p-type charge sheet layer having an in-plane width;
[0011] a Ge-based absorber layer formed on and overlapping the charge sheet layer and / or the avalanche layer, the Ge-based absorber layer having an in-plane width;
[0012] The in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type charge sheet layer in at least one in-plane direction.
[0013] In a second preferred aspect, the present invention provides a SPAD array comprising at least 1×2 arranged SPAD devices, each of which is according to the first aspect and formed on a common substrate.
[0014] In a third preferred aspect, the present invention provides a LIDAR system, comprising a light source with a wavelength in the range of 1.3 μm to 1.6 μm and a SPAD device according to the first aspect or a SPAD array according to the second aspect.
[0015] In a fourth preferred aspect, the present invention provides the use of the SPAD device according to the first aspect or the SPAD array according to the second aspect in the detection of at least one photon having a wavelength in the range of 0.9 μm to 2.0 μm. The SPAD device according to the first aspect or the SPAD array according to the second aspect can be used to detect at least one photon having a wavelength in the range of 1.3 μm to 1.6 μm.
[0016] In a fifth preferred aspect, the present invention provides a method of manufacturing a SPAD device according to the first aspect or a method of manufacturing a SPAD array according to the second aspect, wherein a p-type charge sheet is formed by selective region implantation into a Si-based avalanche layer.
[0017] Optional features of the present invention will now be described.
[0018] Preferably, the in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type charge sheet layer in all in-plane directions. This helps ensure that the electric field distribution in the device is tailored to avoid "hot spots" in one or more regions. This will also help reduce or avoid the effects of sidewall surface states on the dark count rate (DCR).
[0019] The SPAD device may further include:
[0020] a p-type semiconductor contact layer formed on the absorber layer, the p-type semiconductor contact layer having an in-plane width,
[0021] Therein, at least a portion of the p-type semiconductor contact layer is formed to be substantially aligned with at least a portion of the p-type charge sheet layer with a Ge-based absorber layer interposed therebetween.
[0022] In this case, preferably, the in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type semiconductor contact layer in at least one in-plane direction. More preferably, the in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type semiconductor contact layer and greater than the in-plane width of the p-type charge sheet layer in all in-plane directions.
[0023] Preferably, the entire p-type semiconductor contact layer is formed to be substantially aligned with at least a portion of the p-type charge sheet layer. Alternatively, preferably, at least a portion of the p-type semiconductor contact layer is formed to be substantially aligned with the entire p-type charge sheet layer.
[0024] The Ge-based absorber may have side walls in the in-plane direction. The charge sheet may have side edges in the in-plane direction. When the Ge-based absorber has a thickness of at least 1 μm, the distance between the side edge of the charge sheet and the side wall of the Ge-based absorber in the in-plane direction is preferably at least 1 μm greater than the thickness of the Ge-based absorber. It is known that this provides an appropriate overlap of the Ge-based absorber on the p-type charge sheet to provide the technical advantages discussed above and below.
[0025] Alternatively, when the Ge-based absorber has a thickness of less than 1 μm, the distance between the side edge of the charge sheet and the sidewall of the Ge-based absorber in the in-plane direction may be at least 1.0 μm.
[0026] In some embodiments, the distance between the side edge of the charge sheet and the sidewall of the Ge-based absorber in the in-plane direction is at least 5 μm.
[0027] In some embodiments, when the width of the charge sheet is at least 25 μm, the distance between the side edge of the charge sheet layer and the side edge of the p-type semiconductor contact layer in the in-plane direction may be at least 25 μm. Alternatively, when the width of the charge sheet is less than 25 μm, the distance between the side edge of the charge sheet layer and the side edge of the p-type semiconductor contact layer in the in-plane direction may be at least 1 μm.
[0028] In the present disclosure, the expression "width" is generally used to refer to the size of a device in the in-plane direction. The in-plane directions are those directions parallel to the main surface of the substrate (usually a single crystal Si substrate) on which the device is formed. The expression "diameter" is used to refer to the width of certain features of the device (usually features with an island structure). The use of the expression "diameter" does not necessarily indicate that the feature has a circular shape in a plan view (although this is possible and may be preferred in some cases). The feature may have a square, rectangle, rounded square or rectangle, ellipse, racetrack or other similar shape in a plan view, and its "diameter" is intended to refer to its width in the in-plane direction of interest.
[0029] The charge sheet typically has a doping concentration that varies with depth from the surface of the Si-based avalanche layer. Thus, a depth corresponding to the depth of the maximum doping concentration can be identified. Preferably, the charge sheet has a maximum doping concentration at a depth in the range of 30 nm to 100 nm from the surface of the Si-based avalanche layer. This configuration is known to help avoid loss of dopants by diffusion to the surface and subsequent cleaning prior to deposition of the Ge-based absorber layer.
[0030] The Si based avalanche layer may be at least 0.5 μm thick. Preferably it is at least 1 μm thick and may be up to 2 μm thick.
[0031] The Si-based avalanche layer may be i-Si.
[0032] The n-type semiconductor contact layer may be n++Si.
[0033] The Ge-based absorber may be i-Ge. The Ge-based absorber may include i-Ge. The Ge-based absorber may include at least 80% Ge, at least 85% Ge, at least 90% Ge, at least 95% Ge, or at least 99% Ge. The Ge-based absorber may be a Ge alloy-based absorber layer. The Ge alloy-based absorber may include an alloy of Ge with Sn (tin), Si (silicon), or C (carbon). For example, the Ge alloy-based absorber may include Ge x Si 1-x ,Ge 1-x Sn x ,Ge x Si 1-x-y Sn y or Si 1-x Ge x C y .
[0034] The p-type semiconductor contact layer may have a thickness in the range of 10 nm to 100 nm.The p-type semiconductor contact layer may be p++Ge.
[0035] At least one upper surface and / or side surface of the Ge-based absorber layer may be passivated. The passivation may be provided by a GeO2 layer. For example, the GeO2 layer may be thermally grown. The GeO2 layer may be protected by an Al2O3 layer. A suitable Al2O3 layer may be deposited by atomic layer deposition. The Al2O3 layer may help prevent the GeO2 layer from being etched by water from the atmosphere.
[0036] In a graph of doping concentration versus in-plane distance from the maximum doping concentration in the charge sheet to the doping concentration in the avalanche layer, the side edge of the charge sheet can be defined as the position of 0.5 times the maximum doping concentration in the charge sheet.
[0037] Typically, the p-type semiconductor contact layer is formed by photolithography. The contact layer may be formed by etching or implantation. The side edge of the p-type semiconductor contact layer may be defined as a lateral position corresponding to half of the maximum height of the p-type semiconductor contact layer from the Ge-based absorber layer.
[0038] Preferably, the Ge-based absorber has sidewalls in at least one in-plane direction, the width of the Ge-based absorber being measured from one sidewall to the other sidewall.
[0039] Generally, it is preferred that the device have a separate absorption and multiplication (SACM) architecture.
[0040] Preferably, the device has less than 100 counts / s / μm at 100K 2 The dark count rate (DCR) of
[0041] Preferably, the device has a single photon detection efficiency (SPDE) of at least 10% at 100K for photons having a wavelength of 1.3 μm to 1.45 μm.
[0042] Preferably, the device has no more than 2x10 -15 W / Hz 1 / 2 The noise equivalent power (NEP) of the
[0043] Preferably, the device has a thermal conductivity of no more than 3x10 -15 W / Hz 1 / 2 The noise equivalent power (NEP) of the
[0044] Preferably, the device has a maximum of 7x10 -15 W / Hz 1 / 2 The noise equivalent power (NEP) of the
[0045] In a SPAD array, it is preferred that the SPAD devices have a planar architecture, which is superior to a mesa architecture.
[0046] In a SPAD array, it is preferred that the array has at least 2x2 SPAD devices, at least 4x4 SPAD devices, or any other suitable array of SPAD devices, optionally including a large number of SPAD devices such as for imaging applications.
[0047] In a SPAD array, the respective Ge-based absorber layers of adjacent SPAD devices can be laterally isolated by:
[0048] (i) etching a continuous Ge-based absorber layer to at least the depth of the p-type charge sheet layer to form respective Ge-based absorber layers of adjacent SPAD devices; or
[0049] (ii) doping a continuous Ge-based absorber layer to at least the depth of the p-type charge sheet layer to form respective Ge-based absorber layers of adjacent SPAD devices; or
[0050] (iii) Selectively growing respective Ge-based absorber layers within the patterned electrically insulating layer to form respective Ge absorber layers of adjacent SPAD devices.
[0051] With respect to (iii) above, it should be noted that selective area growth is beneficial in reducing the dislocation density at the Si-Ge heterojunction interface.
[0052] The SPAD array (or SPAD device) can be mounted on a Peltier cooler for use. For low-cost implementations, it is preferred to use a Peltier cooler to maintain the SPAD device at a suitable operating temperature.
[0053] It is preferred to use the SPAD device for detecting at least one photon having a wavelength in the range of 0.9 μm to 2.0 μm, or for detecting at least one photon having a wavelength in the range of 1.3 μm to 1.7 μm. The inventors have observed that indirect absorption increases at the 1.7 μm tail.
[0054] In use, as will be understood for a SPAD, the device is biased above its avalanche breakdown voltage. This is in contrast to a related but different device known as an avalanche photodiode (APD). After a photon is detected, the SPAD device is typically quenched by reducing the bias voltage below the breakdown voltage and reset by subsequently increasing the bias voltage above the breakdown voltage.
[0055] In a method of fabricating the device, the charge sheet may be activated by annealing at a temperature of at least 850° C. prior to depositing a Ge-based absorber layer.
[0056] The invention includes the described aspects and combinations of preferred or optional features unless such a combination is clearly impermissible or explicitly avoided.The remainder of the disclosure sets out further optional features of the invention.
[0057] Preferred embodiments of the present invention provide the following significant advantages: allowing the manufacture of germanium-on-silicon single-photon avalanche detectors (SPADs) in a planar process using a silicon foundry. This enables the technology to be manufactured in complementary metal oxide semiconductor (CMOS) or micro-electromechanical system (MEMS) foundries, with the potential to integrate electronic devices on the same small chip. As discussed in more detail below, this new design and manufacturing method has demonstrated single photon detection efficiency (SPDE) of up to 38% at 1310nm and 125K, which is nearly an order of magnitude higher than the previous best germanium-on-silicon SPAD devices
[29]
[28]
[30] . Devices with a diameter of 100μm operate at up to 175K and scaling down to smaller sizes allows operation on Peltier coolers such as those used in currently commercial InGaAs / InP SPAD devices. The SPDE performance is comparable to or better than commercially available InGaAs / InP SPADs, while the DCR is much lower than any other germanium-on-silicon SPAD
[29] , but still higher than the state-of-the-art InGaAs / InP SPAD
[44] . The DCR is roughly proportional to the area of the device, so scaling down to smaller diameter devices advantageously reduces the DCR. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Implementation and experiments illustrating the principles of the present invention will now be discussed with reference to the accompanying drawings, in which:
[0059] Figure 1 A schematic diagram of a device according to an embodiment of the present invention is shown.
[0060] 2(a) and 2(b) show simulated electric field distributions for a planar device (Design 1) according to an embodiment of the present invention.
[0061] Figures 3(a) and 3(b) show the simulated electric field distribution of a comparative mesa-type device (Design 2).
[0062] Figure 4 Shows Figure 2a-2b The device shown (Design 1) and Figure 3a-Figure 3b Dark current of the device shown (Design 2) at 100K.
[0063] Figure 5 The dark current and photocurrent responses when illuminated with 1310 nm wavelength light at 78 K are shown. The breakdown of the sheet charge layer is evident at 20 V.
[0064] Figure 6The single photon detection efficiency (SPDE) and dark count rate (DCR) of a 100 μm diameter Ge SPAD of Design 1 at 78 K and 1310 nm wavelength are shown, demonstrating a 700-fold reduction in DCR compared to a mesa-type device (Design 2).
[0065] Figure 7 The single photon detection efficiency (SPDE) and dark count rate (DCR) of a 100 μm diameter Ge SPAD of Design 1 at 100 K and 1310 nm wavelength are shown, demonstrating a 700-fold reduction in DCR compared to a mesa-type device (Design 2).
[0066] Figure 8 The single photon detection efficiency (SPDE) and dark count rate (DCR) of a 100 μm diameter Ge SPAD of Design 1 at 125 K and 1310 nm wavelength are shown, demonstrating a 700-fold reduction in DCR compared to a mesa-type device (Design 2).
[0067] Fig. 9 A scanning transmission electron microscope (STEM) image of a selectively grown Ge absorber on top of Si inside a window etched into a SiO2 mask is shown. Although misfit dislocations (black dots) are evident at the heterojunction interface between Si and Ge, no threading dislocations are evident across the 10 μm wide Ge pixel. The residual strain due to the transmission electron microscope (TEM) sample formation process causes the warping shown between a portion of the Si layer and a portion of the Ge layer.
[0068] Fig.10 The capacitance-voltage behavior of the GeO2 passivation process on a flat Ge surface using an atomic layer deposited Al2O3 protective cap by thermal oxidation is shown.
[0069] Fig.11 The timing histogram for a SPAD with a diameter of 100 μm is shown at an excess bias of 5.5% and a temperature of 78 K and incident radiation λ = 1310 nm. The full width at half maximum (FWHM) jitter is 310 ps.
[0070] Fig.12a and Figure 12b Shown is the normalized SPDE as a function of incident wavelength for a SPAD with a diameter of 100 μm at temperatures of 125 K (squares), 150 K (circles), and 175 K (triangles).
[0071] Fig.13 The experimental (squares) and theoretical (lines) Ge cutoff wavelengths are shown as a function of temperature.
[0072] Fig.14 Shown are the estimated cut-off wavelength and fit for a germanium-on-silicon SPAD with a 2 μm thick Ge absorption region.
[0073] Fig.15 Shown is the variation of parasitic pulse probability with gate delay time for a 100 μm diameter germanium-on-silicon SPAD (open squares) compared to a 25 μm diameter commercially available InGaAs / InP SPAD (closed squares) when measured at λ=1310 nm and operated at 17% SPDE and 125 K.
[0074] Fig.16 The time constant extracted from the parasitic pulse probability of a germanium-on-silicon SPAD is shown as a function of 1 / kT for excess bias of 2.0% (black squares), 2.5% (red circles), 3.5% (blue upper triangles), and 4.5% (pink lower triangles).
[0075] Fig.17 The activation energy of a germanium-on-silicon SPAD is shown as a function of excess bias.
[0076] Fig.18 The band structure at 125K at a Ge-Si heterojunction interface showing trapped defect states of dislocations (dashed lines) is shown.
[0077] Fig.19 The single photon characterization setup is shown - the black lines represent electrical connections, the solid red lines represent fiber optical connections, and the dashed red lines represent free space optical connections.A broadband imaging system (not shown) is used to aim the laser spot at the optical region of the SPAD.
[0078] Fig. 20 The single photon detection efficiency (SPDE) of the Ge SPAD of Design 1 with a diameter of 100 μm and the Ge SPAD of Design 1 with a diameter of 26 μm at 78 K, 100 K, 125 K and 150 K and a wavelength of 1310 nm is shown.
[0079] Fig.21 The dark count rates (DCR) of the Ge SPAD of Design 1 with a diameter of 100 μm and the Ge SPAD of Design 1 with a diameter of 26 μm at 78 K, 100 K, 125 K and 150 K and a wavelength of 1310 nm are shown.
[0080] Fig. 22 The noise equivalent power (NEP) of a design 1 Ge SPAD with a diameter of 100 μm and a design 1 Ge SPAD with a diameter of 26 μm are shown. DETAILED DESCRIPTION
[0081] Various aspects and embodiments of the present invention will now be discussed with reference to the accompanying drawings. Other aspects and embodiments will be apparent to those skilled in the art. The contents of all files mentioned herein are incorporated herein by reference. These files are listed and numbered at the end of the specification and indicated in square brackets in the text below.
[0082] Introduction and Overview
[0083] We have designed, fabricated, and characterized a new generation of planar Germanium-on-Si single-photon avalanche detectors (SPADs) for picosecond resolution timing applications in the wavelength range of 0.9 μm to 2.0 μm. The use of this novel planar geometry has resulted in a significant step change in the performance of this class of SPDs, allowing the application of larger excess bias voltages above avalanche breakdown and yielding a single-photon detection efficiency (SPDE) of 38% at 125 K and a detection wavelength of 1310 nm. This compares favorably to alternative semiconductor-based SPDs operating in this wavelength range and, combined with the low dark count rate (DCR), results in a 2×10- -16 WHz -1 / 2 The record low noise equivalent power (NEP) of 1.5 GHz is 50 times better than the previous best result. For the first time, InGaAs / InP and Ge-on-Si SPADs have been compared under similar operating conditions, with the Ge-on-Si SPADs showing very low parasitic pulse effects, indicating potential for use at very high count rates. Using an inexpensive Ge-on-Si platform, these results provide a path toward developing large arrays of high-efficiency, high-count-rate Ge-on-Si SPADs operating at telecom wavelengths for eye-safe automotive and autonomous vehicle LIDAR, as well as a range of future quantum technology applications.
[0084] Compact, near-room-temperature semiconductor-based single-photon detectors (SPADs) have become an established optical detection method in the visible and short-wave infrared spectral regions for a variety of emerging applications [1][2][3]. SPAD detectors are avalanche photodiodes that are biased above avalanche breakdown in the field in Geiger mode, where a self-sustaining avalanche current can be triggered by an incident single photon. After a photo-induced avalanche, the detector must be reset or "quenched" before the next detection event. Such detectors typically have a temporal jitter of hundreds of picoseconds, allowing ultrasensitive measurements of fast optical transients. At wavelengths below 1 μm, silicon-based SPADs have been used in a range of quantum photonic applications, including experiments in quantum fundamentals [4] and demonstrations of optical fiber and free-space quantum communications [5][6]. In more traditional applications such as light detection and ranging (LIDAR), silicon-based SPAD detectors have also become candidate technologies due to their high sensitivity and picosecond temporal response, which yields enhanced ranging and improved resolution from surface to surface [7]. Si SPAD detectors have been integrated with standard Si CMOS processes to produce ultra-sensitive, large-format detector arrays with integrated electronics [8]. This low-cost technology has allowed time-of-flight systems to be adapted and developed for use in the automotive industry [9]
[10]
[11] and the smartphone industry
[12] .
[0085] There are many obvious advantages as follows: Extending the spectral range of SPAD detectors into the short-wave infrared (SWIR) region, beyond the detection spectrum of Si-based SPADs. First, compatibility with the low-loss telecommunication window of optical fibers is a fundamental requirement for most fiber-based applications (including quantum communications). Second, in free-space applications such as LIDAR and ranging, the optical power of laser sources is limited to relatively low levels due to the laser eye safety threshold. When the laser wavelength is increased from 850nm to 1550nm, this threshold increases by about 20 times
[13] , allowing increased optical power while maintaining human eye safety in active imaging applications. Therefore, this leads to an increase in the maximum achievable range and / or a potential improvement in depth resolution. Third, solar radiation, which is usually the background level in most single-photon LIDAR systems, is significantly reduced in the SWIR
[14] . Finally, operation in the SWIR will mean enhanced atmospheric transmission, especially through obscurants such as smoke, smog
[15] , and haze
[16] .
[0086] In the SWIR region, the most widely used single photon detectors are InGaAs / InP SPADs and superconducting nanowire single photon detectors (SNSPDs) [1][2]. In general, SNSPD devices have excellent single photon detection performance, but the low operating temperature (usually below 3K) limits the use of SNSPD devices in certain key application areas. InGaAs / InP SPADs are the main single photon detectors in the SWIR region and have been used in a range of quantum communication experiments, especially for long-distance quantum key distribution demonstrations
[17] . More recently, InGaAs / InP SPADs have been used in LIDAR and depth profiling experiments with good results over kilometer ranges
[18]
[19] . Arrays of InGaAs / InP SPADs have been developed and show high performance detection at telecommunication wavelengths
[20] , but two-dimensional arrays may be expensive for the low-cost, high-volume automotive and autonomous vehicle LIDAR markets. One challenging issue with the use of InGaAs / InP SPADs is the effect of parasitic pulses (described below), which severely limit the possible count rates of these SPADs in many different application scenarios.
[0087] An alternative to using an InGaAs absorber layer is to use the semiconductor material Ge. At room temperature, Ge is sensitive to incident radiation with wavelengths up to 1650 nm and can be integrated with Si CMOS
[21] , offering the potential for integrated electronics, high yields, and low cost in volume. SPADs made entirely of Ge have been used for laboratory-based single-photon applications such as time-resolved photoluminescence
[22] , but Ge's narrow direct bandgap of about 0.8 eV means that avalanche gain is limited by band-to-band tunneling. Loudon et al. reported the first Ge-containing SPAD with a Si avalanche region
[23] , using Si 0.7 Ge 0.3 / Si multiple quantum wells to absorb 1210nm radiation. The efficiency and wavelength range of this detector are limited by the use of relatively thin strained superlattice absorption layers. Although the detector has poor efficiency in the short-wave infrared, it is an early example of a separate absorption, charge, and product (SACM) structure for Si-based SPAD detectors and is conceptually similar to previous SACM designs used in InGaAs / InP SPADs and avalanche photodiodes. To avoid tunneling and impact ionization, Si 0.7 Ge 0.3The absorber region has a low electric field, where the thin Si charge sheet allows for a larger electric field in the Si multiplication layer. The large direct Si bandgap of 3.66 eV (3.53 eV) at 300 K (78 K)
[24] significantly reduces the noise from band-to-band tunneling in the high-field avalanche region, which is essential for high-performance SPADs. In the past decade, thicker epitaxial Ge layers have become available on Si substrates. Kang et al. proposed monolithic Ge-on-Si avalanche photodiodes (APDs) operating with a high gain-bandwidth product
[25] . CMOS-compatible Ge waveguide photodiodes
[26] and APDs
[27] have also been developed. Lu et al.
[28] and Warburton et al.
[29] proposed Geiger-mode Ge-on-Si SPADs, the latter reporting a noise equivalent power (NEP) of 1 × 10 at 100 K using a detection wavelength of 1310 nm. -14 WHz -1 / 2 Recently, Martinez et al. fabricated a waveguide germanium-on-silicon SPAD
[30] with a reported single-photon detection efficiency (SPDE) of 5.27% at 1310 nm and 80 K. Although promising, none of these SPADs have performance close enough to that of InGaAs / InP SPAD alternatives and have dark count rates that prevent their effective use in many applications.
[0088] To date, normal incidence Ge-on-Si SPADs have used a mesa design in which the sidewalls of the device are exposed. The inventors have recognised that the use of a mesa design imposes severe limitations on detector performance due to surface effects that result in extremely high dark count rates. The inventors have also recognised that these limitations can be avoided by using a planar design in which the high field regions are located well away from any sidewalls, alleviating the need for high quality passivation layers. Here we report the first planar Ge-on-Si SPAD at normal incidence and demonstrate high performance operation, illustrating the clear potential of integration with Si CMOS for low cost, high performance SPAD array imaging in the SWIR band.
[0089] Design, fabrication and characterization results
[0090] Figure 1 A schematic cross section of a device according to the invention is shown, the device having the following features indicated by reference numerals:
[0091] 1–p ++ Ge top ohmic contact layer;
[0092] 2–i-Ge absorber;
[0093] 3 – p-doped Si sheet charge layer;
[0094] 4 – i-Si avalanche gain multiplication region;
[0095] 5 – Bottom N ++ Si ohmic contact layer;
[0096] 6 – Silicon substrate;
[0097] 7-Electrical insulators, such as SiO2, Si3N4, SiO x N y , hydrogen silsesquioxane, TEOS, BPSG, polyimide, benzocyclobutene based polymer or others;
[0098] 8 – Metal interconnect to the top electrical contact of the germanium-on-silicon SPAD device;
[0099] 9 – Metal interconnect to the bottom electrical contact of the germanium-on-silicon SPAD device;
[0100] 10 – lateral distance between the outer side of the top ohmic contact layer (1) and the outer side of the p-doped sheet charge layer (3);
[0101] 11 – thickness of the Ge absorber;
[0102] 12 – distance between the outer edge of the doped sheet charge layer (3) and the outer edge of the Ge absorber layer (2);
[0103] 13 – thickness of the i-Si avalanche multiplication gain region;
[0104] 14 – Width of the doped sheet charge layer (3).
[0105] Although not shown, the device may also include an antireflective coating (ARC - such as silicon nitride or other transparent material with a refractive index of about 2); graded etching of the top ohmic contact layer to reduce hot spots; and a doped sheet charge layer (3) that may be embedded at a non-zero distance from the Ge-Si heterojunction surface.
[0106] Without wishing to be bound by theory, the inventors suggest that the features discussed below, either alone or, more preferably, in combination, provide significant differences in the technology compared to known devices.
[0107] First, a specific portion of the active device is covered with a selectively implanted sheet charge layer 3. This provides lateral confinement of the high field Si avalanche region and helps to laterally confine the field within the Ge absorber. After implantation, the Ge absorber 2 and the top p ++The sheet charge layer 3 is activated by annealing at 950°C before contacting layer 1. This method allows high levels of activation of dopants in the supply layer using temperatures above the melting point of Ge to reduce point defects that can increase DCR. The sheet charge layer 3 is implanted to have a maximum doping at about 60nm below the silicon surface so that little dopant will be lost by diffusion to the surface and subsequent cleaning before growing the Ge absorber.
[0108] Secondly, a planar device process is designed in which selective area doping 3 is combined with a germanium absorber 2. The germanium layer is then etched to a depth approximating the charge sheet in a “superpixel” design where the pixel size is larger than the charge sheet size. Distances 12 and 10 are preferably larger than the Ge thickness 11 (approximately 1.1 μm deep in the device shown) to drive the electric field at the “superpixel” sidewalls to near zero to reduce the contribution of sidewall surface states to the DCR. This results in a 700-fold reduction in dark count rate (DCR) compared to published mesa-type devices for the same area, temperature, and voltage overbias
[29] . Figure 6 , Figure 7 and Figure 8 As shown, avalanche breakdown ( Figure 4 ) and DCR (for 78K to 125K Figure 6 , Figure 7 and Figure 8 ) enables the device to operate with significantly higher single photon detection efficiency (SPDE). This is equivalent to a 10-fold improvement in SPDE over previous mesa-type devices
[29] using the new planar device design and process. Figure 2a-2b and Figure 3a-Figure 3b The electric field modeling shown in illustrates that Design 1 has significantly lower electric fields at the sidewalls.
[0109] Third, a Ge absorber 2 is regrown on top of the implanted silicon 3, 4. This Ge absorber can be a bulk epitaxially grown layer, or a selectively grown epitaxial layer within a patterned electrically insulating (e.g. silicon dioxide or silicon nitride) layer 7 - see Fig. 9 The selected area approach also provides lateral electrical isolation of the devices allowing array implementation. A 4×4 test array was produced that demonstrated this isolation. ++ This use of a "superpixel" design of a Ge absorber with a -Ge ohmic contact layer 1 is designed to minimize hot spots in the avalanche region of the device that cause premature onset of avalanche breakdown at the edge of the device (i.e., edge breakdown). Hot spots will reduce the SPDE because the device will have lower efficiency in the center of the active area and effectively force the device to operate at higher bias levels, resulting in high dark count rates.
[0110] Fourth, an alternative method of electrically isolating the pixels after bulk Ge epitaxial growth of the absorber. This means etching the superpixel sidewalls over the full depth of the Ge layer 2 to provide lateral electrical isolation between pixels. This is similar to shallow trench isolation because combined with typical background doping levels (>10 15 cm -3 ) requires a method to laterally electrically isolate the device. The etched edge of the trench is preferably located at a lateral distance from the active area of the device of at least the depth of the Ge heterogeneous layer 2. ++ The electric field distribution between the surface ohmic contact 1 and the buried p-type sheet charge layer 3 can be considered the active area. The purpose of this method is to prevent any surface state trapped charges from being accelerated by the electric field into the avalanche region, otherwise it will increase the dark current and DCR. Alternatively, doping can be used to form lateral pn electrical isolation.
[0111] Fifth, thermally grown GeO2 (not shown) is used on the Ge surface 2 and the etched surface to produce a passivated Ge surface. In some embodiments, the GeO2 is protected by an atomic layer deposited Al2O3 layer to prevent the GeO2 from being etched by water from the atmosphere. Fig.10 The electrical characterization of a passivated GeO2 layer and an Al2O3 layer of equal thickness as part of a capacitor with a diameter of 100 μm is provided. The CV shows a 10 11 cm -2 The trap charge level nearby.
[0112] Sixth, limited area growth is used to reduce the number of dislocations to reduce dark current and DCR in the device. Fig. 9 The lack of any dark threading dislocation lines extending from the Si-Ge heterojunction face to the surface of Ge demonstrates how limited area growth can reduce threading dislocation density. This may help to further reduce or eliminate the deleterious effects of parasitic pulses if the trapped charge causing the effect is shown to be dislocation-related.
[0113] The embodiment devices described herein generally use the SACM structure modeled in FIG. 2( a) and FIG. 2( b) (otherwise referred to herein as "Design 1"). Design 1 is a device whose p-Ge contact has a smaller diameter than the p-Si sheet charge layer, while the i-Ge absorber has a much wider diameter than both the p-Ge and p-Si. The electric field distribution indicates that the device will have relatively low dark current and dark count rate. Note that in Figure 2a , the horizontal axis has a different ratio to the vertical axis. Figure 2b Shows Figure 2a is a portion of the device shown in Figure 2a The horizontal scale is expanded to more clearly show the device and p +Map of the electric field intensity in the region corresponding to the edge of the Si charge sheet.
[0114] A comparative mesa structure (otherwise referred to herein as "Design 2") is shown in Figures 3(a) and 3(b). Design 2 is a device whose p-Ge contact has the same diameter as the i-Ge absorber, and both of which are smaller than (or optionally equal to) the diameter of the p-Si sheet charge layer. The electric field distribution indicates that the high electric field hot spots on the sides of the etched Ge mesa indicate an early onset of avalanche (i.e., edge breakdown), which will reduce the SPDE and effectively force the device to operate at a higher bias level, resulting in a high dark count rate.
[0115] For the Design 1 device (and indeed for the Design 2 device), the incident SWIR radiation is absorbed in the Ge absorption region, and signal amplification occurs in the Si multiplication region. Between these regions, a charge sheet is used to modulate the electric field so that the field is high enough in the multiplication region to ensure that the excited carriers cause avalanche breakdown, and low enough in the absorption region to prevent inter-band and trap-assisted tunneling. However, a moderate electric field is maintained in the Ge layer to allow photogenerated electrons to drift efficiently into the multiplication region. The SPAD is biased above the avalanche breakdown voltage, and the process begins when the incident photon is absorbed in the Ge absorption region, creating an electron-hole pair. The photoexcited electron then drifts under a moderate electric field until it reaches the Si multiplication region. In the Si multiplication region, the photoexcited electron is accelerated under a high electric field, gaining sufficient kinetic energy for impact ionization, thereby forming an electron-hole pair. Secondary electrons and holes are accelerated and impact ionized in turn, creating additional electron-hole pairs. This process continues, generating a large avalanche current that can become self-sustaining if the device is biased above avalanche breakdown. Under these conditions, this results in a detectable electronic signal that can be timed relative to the initial laser pulse. After detection, it is necessary to temporarily bias the SPAD below avalanche breakdown to quench the avalanche, after which the SPAD can return to its quiescent state, ready to detect additional incident photons. The Design 2 device operates in a generally similar manner.
[0116] like Figure 2a and Figure 2b As shown, finite element analysis modeling using Silvaco ATLAS software was used to design the SPAD. The charge sheet doping level and the thickness of the multiplication and absorber regions as well as the preferred overall design dimensions of the SPAD were determined. As mentioned above, it is necessary to ensure that the electric field distribution throughout the SPAD is suitable to produce high performance. Figure 2a-2b The simulations for planar devices shown in Figure 3a-Figure 3bIn the simulation for a comparative mesa-type device shown in , the electric field distribution is shown for a potential held 5% above the avalanche breakdown voltage or 5% excess bias. Figure 2a and Figure 2b It is clear that a low electric field exists in the Ge absorber upon breakdown, and that the high electric field is confined to the center of the SPAD, preventing carriers originating from the sidewalls from causing a breakdown event.
[0117] The superpixel radius minus the charge sheet radius (in Figure 1 Dimension 12 in the figure should preferably be approximately 2 μm or larger in order to minimize the electric field at the sidewalls and reduce the electric field hotspot just below the corner at the lowest portion of the sidewalls (at Figure 1 For a very thin Ge absorber ( Figure 1 If the thickness of the Ge absorber is greater than 1 μm, the following equation gives a suitable minimum value for dimension 12.
[0118] Size 12 = Size 11 + 1 μm
[0119] Preferably, if Figure 1 As shown by dimension 10 in FIG, the radius of the contact layer is smaller than the radius of the charge sheet. Preferably, dimension 10 should be greater than 2 μm. Assuming a typical device active area of 25 μm or greater (the active area is defined as the diameter of the charge sheet, i.e. Figure 1 When dimension 14 is much smaller than 25 μm, dimension 10 may be smaller than 2 μm.
[0120] To characterize these devices, a 150 mm diameter ++ Five structures were grown on a doped Si substrate. A 1.5μm thick Si multiplication region was first grown using a commercial reduced pressure-chemical vapor deposition (RP-CVD) system. The charge sheet region was defined using photolithography, which was then implanted with boron acceptors at an energy of 10keV. Different charge sheet doses were implanted into each of the five wafers to account for manufacturing tolerances and ensure that the best electric field distribution was obtained. After implantation, the boron dopant was activated at 950°C for 30s using a rapid thermal annealer. After RCA cleaning, a 1μm thick nominally undoped Ge absorption region was grown on top of the selectively implanted Si layer using RP-CVD along with 50nm of p-type Ge. ++ Ge top contact layer. To electrically isolate each SPAD, a trench etch through the Ge was performed at a lateral distance of 10 μm from the charge sheet. This isolation was deemed necessary in this embodiment due to the background doping levels found in the Ge layer. Figure 3aA mesa design with exposed sidewalls is shown and used as a control during characterization. Metal contacts, GeO2 passivation, anti-reflective (AR) coatings, and pads are subsequently deposited. To ensure rapid and high-throughput manufacturing, device diameters range from 100 μm to 200 μm, resulting in very large device cross-sectional areas compared to previous germanium-on-silicon SPADs
[28]
[29] . However, the present disclosure is intended to be applicable to SPADs that are significantly smaller than the device described - for example, to further reduce dark count rates, devices with a diameter of approximately 10 μm are suitable.
[0121] After fabrication, the SPADs were cooled in a Janis micromanipulator cryoprobe system. Figure 4 The dark current of both a planar SPAD structure and a mesa-etched SPAD structure made from the same wafer at 100 K is shown. The mesa-etched structure has Figure 2a-2b The microstructure is similar in geometry to the planar geometry in FIG, except that an etching process is used to create a mesa with a diameter smaller than the diameter of the ion-implanted charge sheet, which is etched to a depth just below the charge sheet and into the multiplication layer ( Figure 3a-Figure 3b ). The planar SPAD has a sharp breakdown indicating a low multiplicative dark current, which was previously found to be a strong indicator of the desired low dark count rate performance
[31] and demonstrates that the surface generation effects are negligible as predicted by electric field modeling. The mesa-etched SPAD has a softer breakdown, with the dark current 50 times higher than the planar structure immediately before breakdown. This indicates that there is significant surface generation as expected based on the present disclosure, and suggests that the mesa-etched SPAD will have a high dark count rate compared to the planar SPAD. In fact, it is impossible to characterize the mesa-etched SPAD above breakdown due to its excessively high DCR. Figure 5 Dark current and photocurrent as a function of reverse bias are shown for a planar SPAD at 78K. The dark current before breakdown is less than 1 nA and the SPAD exhibits good uniformity with little variation in dark current between devices. Photocurrent measurements at λ = 1310 nm show a clear breakdown at 20 V where the electric field reaches the absorption region and the photoexcited electrons can drift into the multiplication region. The device yield is over 90%, which is very encouraging at this early stage for the final realization of germanium-on-silicon SPAD focal plane arrays.
[0122] As described in more detail in the Methods section, after preliminary characterization, SPDE, DCR and jitter measurements were performed using the time-correlated single photon counting (TCSPC) technique. In these measurements, an electrical gating method was used to switch the detector above avalanche breakdown, into Geiger mode, for a duration of 50ns, synchronously with the arrival of an attenuated laser pulse. This gated detector method was used at a low frequency of 1kHz in order to completely quench the avalanche and avoid the effects of parasitic pulses (described below). The SPAD detector was first cooled to 78K to perform SPDE, DCR and jitter measurements using laser radiation at λ=1310nm. Figure 6 , Figure 7 and Figure 8 The SPDE and DCR are shown as a function of excess bias at 78 K, 100 K and 125 K. It should be noted that the detector used has a large area (100 μm in diameter) and it is fully expected that using a reduced area device will significantly reduce the DCR, as previously reported for all-Si SPADs
[32] .
[0123] The measured DCR shows a dramatic improvement over previous work on germanium on silicon. Warburton et al. reported a mesa-geometry germanium-on-silicon SPAD with a 5.5 MHz DCR for a 25 μm diameter SPAD at 100 K. This corresponds to 11,200 counts / s / μm. 2 , which is higher than the 18.3 counts / s / μm reported in this work. 2 , which is about 3 orders of magnitude higher. It should also be noted that under these conditions, the SPDE reported in that paper is 4%, compared to 26% for the SPAD reported in this paper. A similar relationship exists when comparing our results with those from Martinez et al., who reported a DCR of 500kHz for a 1μm x 15.9μm rectangular waveguide SPAD at 80K
[30] . This is equivalent to 31400 counts / s / μm 2 , which is higher than the 6.37 counts / s / μm reported in this paper. 2 They report 5% for SPDEs compared to 22% for SPADs reported in this paper. This large reduction in dark count rate arises from the carefully designed electric field distribution of these planar geometry detectors, which means that the high electric fields are confined within the SPAD, preventing surface states from contributing significantly to the DCR.
[0124] Figure 6 , Figure 7 and Figure 8The SPDE is shown to increase with excess bias to a maximum of 38% at 125K, significantly higher than previously reported SPDEs for Ge SPADs and germanium-on-silicon SPADs
[22]
[28]
[29]
[30] and comparable to the highest values recorded for InGaAs / InP SPADs at 225K
[33]
[34]
[35] . This is due in part to the high excess bias applied to the SPAD that is achievable due to the low DCR, thereby increasing the breakdown probability in the multiplication region. The breakdown probability is also increased by the relatively thick 1.5μm Si multiplication region, which reduces the probability of carriers leaving the multiplication region before impact ionization and the breakdown chain begin. The uniform electric field in the multiplication region caused by minimal residual doping in the lower part of the Si multiplication layer leads to a uniform impact ionization rate throughout the region, further increasing the breakdown probability. The optimized electric field also ensures that photoexcited electrons will drift into the multiplication region with low recombination probability. Significantly, there is no conduction band barrier between the Ge absorption region and the Si charge sheet, ensuring that photoexcited electrons can easily enter Si from Ge. In fact, if the deformation potentials in reference
[36] are used for calculation, the Si Δ-type valley at the conduction band edge is 235 meV lower than the Ge L-type valley conduction band edge in the absorber. This is an advantage over InGaAs / InP SPADs, which have an energy barrier step that the photoexcited carriers must overcome to reach the InP multiplication region. These SPADs require an InGaAsP graded layer between the InGaAs and InP regions to reduce carrier accumulation at the absorber-charge sheet interface. It is preferred to include an AR coating on the device to reduce reflection from the top surface of the SPAD to less than 1% of the incident radiation. For these samples, measurements at higher temperatures are limited by the increased DCR rate due to the increased heat generation rate, but the reduction in detector area further reduces the DCR and allows significantly higher operating temperatures.
[0125] The high SPDE is achieved despite the use of a relatively thin Ge absorption region. Using the absorption coefficient of single crystal Ge at 77K
[37] , we calculate that less than 50% of the radiation at 1310nm wavelength is absorbed in a Ge absorber with a thickness of 1μm over the entire operating temperature range. The Beer-Lambert law indicates that a Ge absorber with a thickness of 2μm will increase the absorptivity to over 70%, which results in a SPDE greater than 55% at 125K. This figure is significantly higher than the SPDE reported for InGaAs / InP SPADs
[33]
[34]
[35] . Even thicker Ge layers still provide higher absorptivity.
[0126] Noise equivalent power (NEP) is the figure of merit of the SPAD calculated from the SPDE and DCR of the detector using the following formula:
[0127]
[0128] where h is Planck's constant and v is the frequency of the incident radiation. This can be used to compare detectors, with lower values indicating improved performance. At 78K, we measured 1.9×10 -16 W / Hz 1 / 2 The NEP of the GaN-based SPAD is 50 times lower than that of the Ge-on-Si SPAD reported in
[29] . The NEP values of 3×10 -16 WHz -1 / 2 and 7×10 -16 WHz -1 / 2 .
[0129] Fig.11 The timing histogram obtained at 5.5% excess bias and 78K when measured at λ = 1310nm is shown. The jitter FWHM is 310ps, which is a reasonable value considering the increased width of the multiplication region
[38]
[39] . A wider multiplication region generally improves SPDE, but the increased variance of the avalanche build-up time increases the jitter. As previously found in SiSPADs
[40] , the jitter is expected to decrease with decreasing device diameter by improving the electronic packaging that cools the device.
[0130] The wavelength dependence of germanium-on-silicon SPAD detector efficiency varies over the SWIR as the Ge bandgap changes with temperature. Fig.12a and Figure 12b The wavelength dependence of the SPDE of a germanium-on-silicon SPAD as a function of temperature is shown. The efficient SPDE region and the direct bandgap absorption between the conduction and valence bands at the Γ-point are associated with the absorption at longer wavelengths, which is associated with significantly weaker indirect absorption into the L-type valley and valence bands. At room temperature, the direct bandgap of Ge is 0.80 eV
[36] , but this value increases to 0.88 eV at 78 K, thereby reducing the detection cutoff wavelength
[36] . Using a tunable NKT supercontinuum laser, we are able to vary the wavelength of the radiation incident on the SPAD from 1310 nm to 1550 nm to obtain the precise cutoff wavelength at various temperatures. As Fig.13 As shown, by changing the cut-off wavelength λ c Defined as the wavelength at which the detector's SPDE is 50% of the 1450nm wavelength value, λ can be observed cThe wavelength of the SPAD increases from 1468 nm at 125 K to 1495 nm at 175 K, at a rate of approximately 0.54 nm / K, which is consistent with the value calculated using Varshni's temperature-dependent bandgap parameter in
[41] . If the operating temperature of the SPAD is increased above 180 K, the cutoff wavelength can be extended to reach an atmospheric transmission window of 1500 nm to 1800 nm. This is thought to be readily achievable using smaller diameter devices with lower DCR rates and allowing higher temperature operation (as discussed above). In addition, increasing the thickness of the Ge absorption region increases the SPDE and increases λ c Move to longer wavelengths. Fig.14 The estimated cut-off wavelength for a germanium-on-silicon SPAD with a 2 μm thick Ge absorption region is shown. This reduces the temperature required to detect 1550 nm wavelength radiation to 220 K.
[0131] A key difference between Germanium-on-Silicon SPADs and their InGaAs / InP SPAD alternatives is believed to be the significantly reduced deleterious effects of parasitic pulses in the detector. Parasitic pulses occur when carriers are trapped and subsequently released after an avalanche event, leading to elevated background levels. This can be mitigated by using a long hold-off time (typically >10 μs) after each event so that the trapped carriers can be released before reactivating the detector. However, this approach increases dead time and limits the maximum possible count rate. Parasitic pulses are considered to be one of the main limitations on the performance of InGaAs / InP SPADs, severely degrading their performance even at modest count rates. Parasitic pulses in InGaAs / InP detectors originate primarily from deep level trap states in the InP multiplication layer
[42]
[43]
[44] , and the expectation for Germanium-on-Silicon SPAD detectors is that high quality Si multiplication layers will have a low density of such states. We show for the first time a comparison of InGaAs / InP SPADs with Germanium-on-Silicon SPADs under similar operating conditions.
[0132] Parasitic pulse measurements have been performed using a time-dependent carrier counting method
[45] on a 100 μm diameter germanium-on-silicon SPAD at temperatures between 78 K and 175 K, where the SPAD underwent an intentional avalanche. The device was then immediately quenched and then activated a second time via an electrical gate shortly after. By varying the time between the two detector gates, we examined the probability of an avalanche in the second gate, thereby giving the parasitic pulse probability as a function of time after the initial avalanche. The obtained results have been compared with a commercial state-of-the-art InGaAs / InP SPAD operated at the same temperature and with a specific excess bias applied to each detector in order to obtain the same SPDE for both detectors. Fig.15The variation of the parasitic pulse probability of the two SPADs at a temperature of 125K is shown when an excess bias corresponding to an SPDE of 17% is applied in both detectors. It can be observed that for a particular holdoff time, the parasitic pulse probability of the germanium-on-silicon SPAD is significantly reduced. For example, using a holdoff time of 10μs, the germanium-on-silicon SPAD exhibits 20% of the parasitic pulse probability of the InGaAs / InP SPAD detector. A similar trend is shown at 150K. It should be noted that although the absolute parasitic pulse probability will be affected by operating conditions (e.g., gate duration), these results help to provide a comparison between the two detector types under nominally identical operating conditions. These preliminary results show great promise for future germanium-on-silicon developments, and in particular, the improvement in parasitic pulse probability will be further improved as the quality of the Si epilayer materials is further developed to optimize this particular detector characteristic.
[0133] In an attempt to identify the parasitic pulse mechanism in germanium-on-silicon SPADs, we studied the parasitic pulses as a function of temperature in the range of 78K to 125K and fitted an exponential decay. By fitting an Arrhenius curve, we derived activation energies in the range of 80 to 90 meV for a range of overbias levels in an attempt to identify the origin of the traps. GeO at native Si surface, native Ge surface, and Ge surface x Trap states have been demonstrated to be close to 420 meV
[46] , 130 meV
[46] , and from 200 meV to 300 meV
[47] , respectively. This provides additional evidence that the planar geometry is reducing the effects of traps and other impurities at the exposed surface. Therefore, the parasitic pulses are unlikely to be related to surface states on the passivated Ge or any exposed Si surface.
[0134] Fig.18 The band structure of the Ge-Si heterojunction calculated at 125 K using the deformation potential from
[24] is shown without any applied electric field for clarity, and includes the three main trap states of dislocations in Ge drawn as dashed lines within the band gap
[48] . Fig.17The activation energies of 80 meV to 90 meV extracted from are close to the 70 meV acceptor and 90 meV donor trap states at the valence band edge of the dislocations in Ge, but it is unclear what mechanism might be responsible for the parasitic pulses of these states. Metallic impurities in Ge with energies close to these values are Co (90 meV acceptor), Zn (90 meV acceptor), Hg (87 meV acceptor), and Cr (70 meV acceptor)
[49] , none of which are expected to be present at any trace levels in the present device. Metallic impurities in Si with similar energies are Bi (69 meV acceptor), Ga (72 meV acceptor), and Al (67 meV acceptor)
[49] . Although Al has been used for contacts and pads, these are at the top of the Ge and on the back of the Si wafer, and the avalanche region of the device is buried, so there should be no trace levels of aluminum near the avalanche region of the device.
[0135] Fig. 20 , Fig.21 and Fig. 22 It is demonstrated that 26μm diameter Ge-on-Si SPAD devices have significantly reduced SPDE, DCR and NEP compared to 100μm diameter Ge-on-Si SPADs at 78K, 100K, 125K and 150K. A slight decrease in SPDE is evident in the 26μm diameter device, but this is most likely due to the uneven lateral efficiency distribution of the device used. It is further demonstrated that the 26μm diameter Ge-on-Si SPAD has significantly reduced jitter (149±10ps cf. 310±10ps) compared to the 100μm diameter Ge-on-Si SPAD.
[0136] Dislocation traps in Si have been measured to be centered at 807 meV, 870 meV, 940 meV, and 1001 meV above the valence band at 12 K for the D1 to D4 trap states, respectively
[50] . The last of these dislocation trap states corresponds to about 130 meV below the Si conduction band at 125 K
[50] (see Fig.18 ), and at this temperature, the line width has a thermal broadening of at least 10 meV. It is well known that Ge or Si grown on a Si substrate to a critical thickness 1-x Ge xDuring the relaxation of the heterolayer, some threading dislocations can be injected into the Si substrate
[51] , and a certain degree of strain will be transferred to the Si near the heterojunction interface, which will reduce the energy between the trap state and the conduction band edge. The Si D4 trap state has been identified as coming from the relaxed dislocation
[52] , and the uncertainty in thermal broadening and strain together with the uncertainty in the parasitic pulse excitation energy extracted from three temperatures make this D4 dislocation trap in Si a good candidate for the origin of the parasitic pulse. Limited area growth of Ge on Si has demonstrated a significant reduction in the threading dislocation density both into the Ge heterolayer and into the Si substrate
[53] . Therefore, it can be determined whether the parasitic pulse can be further reduced, thereby determining whether the D4 trap state is the origin of the parasitic pulse mechanism, thereby further reducing the possibility of parasitic pulses.
[0137] in conclusion
[0138] We have reported high performance Ge-on-Si SPADs designed using a novel planar geometry. The 100 μm diameter SPAD shows a 38% SPDE at 125 K and a detection wavelength of 1310 nm, a significant step change in performance level improvement from all previous Ge-on-Si SPAD reports and now outperforming commercial InGaAs / InP SPADs. At 78 K, the 1.9×10 -16 WHz -1 / 2 The NEP is 50 times higher than previously reported for germanium-on-silicon SPADs. The parasitic pulse performance was analyzed using a time-correlated carrier counting method and compared to commercial InGaAs SPADs. Under the same conditions, this initial germanium-on-silicon SPAD detector can be operated with a 50% to 75% reduction in dead time compared to commercial InGaAs / InP SPADs, resulting in operation with higher maximum count rates. These results point to a clear path to smaller detectors: combined with thicker Ge absorbers that can operate at low dark count rates at or near room temperature and high count rate operation. The elevated temperature enables these detectors to operate efficiently in the relatively eye-safe 1550nm wavelength range. Using a Si platform provides a low-cost path to single-photon 3D imaging and sensing in the eye-safe short-wave infrared region. This can have important implications for a range of common applications such as automotive and autonomous vehicle LIDAR, security and environmental LIDAR monitoring, and in addition, can be used for a range of quantum technology applications using important telecommunication wavelengths.
[0139] method
[0140] The device is made of a 150 mm diameter n ++The Si(001) wafers were fabricated on which 1.5μm of undoped Si was grown. Finite element analysis modeling using Silvaco ATLAS software was used to determine the optimal charge sheet density to provide low electric fields in the Ge absorber and high electric fields in the Si avalanche region. Photolithography was then used with boron ion implantation at 10kV to selectively create the charge sheets. After an activation anneal at 950°C, five different wafers were produced with sheet densities ranging from 1x10 11 cm -2 With 5x10 11 cm -2 1 μm thick undoped Ge was then grown with the top 50 nm doped with boron in situ for the top ohmic contact. Photolithography was used with a fluorine dry etch to etch an electrically isolating trench into the Ge before depositing the SiO2 passivation and planarization layers. Al was deposited on the back side of the wafer to form the bottom ohmic contact. A set of devices for which characterization results are presented here used back contacts. As is well understood and as shown in the accompanying drawings, a device such as Figure 1 The bottom ohmic contact is formed by vias 9 shown. The manner of contact to the lower n-contact is not considered critical to device performance. The top contact approach is considered suitable for industrial implementation, while the back contact is more suitable for laboratory scale manufacturing and testing and is reported here. Note that the top contact approach also allows illumination through the substrate, which is advantageous for some applications.
[0141] Then, photolithography is used to etch holes in the oxide to the top ohmic contact before depositing Ni / Al and annealing the Ni / Al to form the top metal contact. The SiO2 is etched away on top of the device and a Si3N4 anti-reflective coating is deposited by PECVD.
[0142] Single-photon characterization. SPDE, DCR, and jitter measurements are performed using the time-correlated single-photon counting (TCSPC) technique, where Fig.19A schematic diagram of the setup used for this characterization is shown. The SPAD detector is mounted on a liquid nitrogen cryostat from Oxford Instruments that enables measurements between 78K and 175K. The cryostat has optical access, which allows a short working distance between the detector and the external optical system. A picosecond pulsed laser is used to measure the SPDE of the SPAD, where the output is attenuated to a level far less than one photon per pulse in order to reduce the possibility that a single pulse contains more than one photon. Two lasers are used, a PicoQuant laser diode emitting a wavelength of 1310nm and a NKT supercontinuum laser tunable over a wavelength range between 1150nm and 2000nm. The laser output is coupled into a single mode fiber (SMF-28) and then to a 50:50 fiber beam splitter. One beam splitter output is connected to a calibrated power meter to provide an in-situ power reading that is continuously monitored during the measurement. The other output is connected to a programmable optical attenuator in which the output can be attenuated by up to 100dB. The attenuator output is inserted into a reflective collimator for free space collimation. The collimated beam passes through two thin film beam splitters (splitting ratio of 92:8), which allows broadband illumination channels and imaging channels to reach the SWIR camera for aligning and focusing the laser spot on the SPAD. Before each SPDE measurement, the laser power reaching the SPAD is measured and compared with the power measured by the field power meter. This ratio is used to calculate the number of photons per pulse incident on the SPAD for a given power meter reading. The device is operated in gated mode, where a DC source biases the SPAD to just below the breakdown voltage. The master clock controls the timing of the laser trigger, the detector gate, and the start signal of the TCC900 photon counting card of Edinburgh Instruments. A detector gate with a duration of 50ns is used in the experiments described in this disclosure. The detector gate is combined with a DC bias using a Tektronix 5530 biaser, where the output is connected to the anode of the SPAD. The SPAD cathode is connected to the photon counting card stop signal. The timing histogram with a timing bin interval of 19.5 ps recorded by the photon counting card is used to calculate SPDE, DCR and device jitter.
[0143] ***
[0144] The features disclosed in the foregoing description or in the attached claims or in the drawings may be used alone or in any combination of such features to implement the invention in its different forms, whereby the features are appropriately expressed in their specific form or in terms of means for performing the disclosed functions or in terms of methods or processes for obtaining the disclosed results.
[0145] Although the present invention has been described in conjunction with the above exemplary embodiments, many equivalent modifications and variations will be apparent to those skilled in the art when present disclosure is given. Therefore, the exemplary embodiments of the present invention set forth above are considered to be illustrative rather than restrictive. Various changes may be made to the described embodiments without departing from the spirit and scope of the present invention.
[0146] For the avoidance of any doubt, any theoretical explanations provided herein are provided for the purpose of enhancing the reader's understanding. The inventors do not wish to be bound by any of these theoretical explanations.
[0147] Any section headings used herein are for organizational purposes only and are not to be construed as limiting the subject matter described.
[0148] Throughout this specification, including the appended claims, unless the context requires otherwise, the words "comprise" and "comprising" and variations such as "comprises", "comprising" and "including", will be understood to imply the inclusion of a stated integer or step or group of integers or steps without excluding any other integer or step or group of integers or steps.
[0149] It must be noted that, as used in the specification and the appended claims, the singular forms "a", "an", and "the" include plural referents unless the context clearly dictates otherwise. Ranges may be expressed herein as from "about" one particular value and / or to "about" another particular value. When such a range is expressed, another embodiment includes from the one particular value and / or to the other particular value. Similarly, when a value is expressed as an approximation by using the antecedent "about", it will be understood that the particular value forms another embodiment. The term "about" with respect to a numerical value is optional and means, for example, + / - 10%.
[0150] References
[0151] Many publications are cited above in order to more fully describe and disclose the present invention and the state of the art to which the present invention belongs. The complete citations of these references are provided below. Each of these references is incorporated herein in its entirety.
[0152] [1] Buller, GS & Collins, RJ Single-photon generation and detection. Meas. Sci. Technol. 21, 012002 (2010).
[0153] [2]Hadfield,R.H.Single-photon detectors for optical quantuminformation applications.Nature Photon.3,696–705(2009).
[0154] [3]Cova,S.,Ghioni,M.,Lotito,A.,Rech,I.&Zappa,F.Evolution andprospects for single-photon avalanche diodes and quenching circuits.J.ModOptics 51,1267-1288(2004).
[0155] [4]Shadbolt,P.,Matthews,J.C.F.,Laing,A.&J.L.O’Brien Testingfoundations of quantum mechanics with photons.Nature Phys.10,278-286(2014).
[0156] [5]Gordon,K.J.,Fernandez,V.,Townsend,P.D.&Buller,G.S.Ashortwavelength gigahertz clocked fiber-optic quantum key distribution system.IEEEJ.Quant.Electron.40,900-908(2004).
[0157] [6]Pugh,C.J.et al.Airborne demonstration of a quantum keydistribution receiver payload.Quantum Science and Technology 2,024009(2017).
[0158] [7]Buller,G.S.&Wallace,A.M.,Recent advances in ranging and three-dimensional imaging using time-correlated single-photon counting.IEEEJ.Sel.Top.Quantum Electron.13,1006-1015(2007).
[0159] [8]Charbon,E.&Donati,S.,SPAD sensors come of age.Optics and PhotonicsNews 36,(2010).
[0160] [9]Niclass,C.,Inoue,D.,Matsubara,H.,Ichikawa,T.&Soga,M.Development ofautomotive LIDAR.Elec..Comm.Japan 98,1476-1480(2015).
[0161]
[10] Gyongy,I.,Dutton,N.A.W.&Henderson R.K.,Single-photon tracking forhigh-speed vision.Sensors 18,323(2018).
[0162]
[11] Takai,I.et al.Single-photon avalanche diode with enhanced NIR-sensitivity for automotive LIDAR systems.Sensors 16,459(2016).
[0163]
[12] Pellegrini et al.Industrialised SPAD in 40 nm technology,2017IEEE Int.Electron Dev.Meeting 8268404(2017).
[0164]
[13] IEC-60825-1 standard
[0165]
[14] Bird,R.E.,Hulstrom,R.L.&Lewis,L.J.Terrestrial solar spectral datasets.Solar Energy 30,563-573(1983).
[0166]
[15] Christnacher,F.et al.Influence of gating and of the gate shape onthe penetration capacity of range-gated active imaging in scatteringenvironments.Opt.Express 23,32897-32908(2015).
[0167]
[16] Arnulf,A.,Bricard,J.,Curé,E.&Véret,C.Transmission by haze and fogin the spectral region 0.35 to 10 microns.J.Opt.Soc.Am.47,491-498(1957).[A]Dumont,M.,Brissaud,O.,Picard,G.,Schmitt,B.,Gallet,J.-C.&.Arnaud,Y.,High-accuracy measurements of snow bidirectional reflectance distribution functionat visible and NIR wavelengths–comparison with modellingresults.Atmos.Chem.Phys.10,2507–2520(2010).
[0168]
[17] Korzh,B.et al.Provably secure and practical quantum keydistribution over 307 km of optical fibre.Nature Photon.9,163-168(2015).
[0169]
[18] McCarthy,A.et al.Kilometer-range depth imaging at 1550 nmwavelength using an InGaAs / InP single-photon avalanche diodedetector.Opt.Express 21,19,pp.22098-22113(2013)
[0170]
[19] Pawlikowska,A.M.,Halimi,A.,Lamb,R.A.&Buller,G.S.Single–photonthree–dimensional imaging at up to 10 kilometers range.Opt.Express 25,11919-11931(2017).
[0171]
[20] Jiang,X.et al.InP-based single photon detectors and geiger-modeAPD arrays for quantum communication applications.IEEE J.Sel.Top.QuantumElectron.21,3800112(2015).
[0172]
[21] Sammak,A.,Aminian,M.,Nanver,L.K.&Charbon,E.CMOS-CompatiblePureGaB Ge-on-Si APD pixel arrays.IEEE Trans.Electron Dev.63,92-99(2016).
[0173]
[22] Buller,G.S.et al.Time-resolved photoluminescence measurements ofInGaAs / InP multiple-quantum-well structures at 1.3μm wavelengths by use ofgermanium single-photon avalanche photodiodes.Appl.Opt.35,916–921(1996).
[0174]
[23] Loudon,A.Y.et al.Enhancement of the infrared detection efficiencyof silicon photon-counting avalanche photodiodes by use of silicon germaniumabsorbing layers.Opt.Lett.27,219–221(2002).
[0175]
[24] Paul,D.J.8-band k·p modelling of mid-infrared intersubbandabsorption in Ge quantum wells.J.Appl.Phys.120,043103(2016).
[0176]
[25] Kang,Y.et al.Monolithic germanium / silicon avalanche photodiodeswith340 GHz gain–bandwidth product.Nature Photon.3,59–63(2009).
[0177]
[26] Derose,C.T.et al.Ultra compact 45 GHz CMOS compatible germaniumwaveguide photodiode with low darkcurrent.Opt.Express 19,527–534(2011).
[0178]
[27] Martinez,N.J.D.et al.High performance waveguide-coupled Ge-on-Silinear mode avalanche photodiodes.Opt.Express 24,19072–19081(2016).
[0179]
[28] Lu,Z.et al.Geiger-mode operation of Ge-on-Si avalanchephotodiodes.IEEE J.Quantum Electron.47,731–735(2011).
[0180]
[29] Warburton,R.E.et al.Ge-on-Si single-photon avalanche diodedetectors:design,modeling,fabrication,and characterization at wavelengths1310 and 1550 nm.IEEE Trans.Electron Dev.60,3807-3813(2013).
[0181]
[30] Martinez,N.J.D.et al.Single photon detection in a waveguide-coupled Ge-on-Si lateral avalanche photodiode.Opt.Express 25,16130–16139(2017).
[0182]
[31] Webster,E.A.G.&Henderson,R.K.A TCAD and spectroscopy study ofdark count mechanisms in single-photon avalanche diodes.IEEE Trans.ElectronDev.60,4014-4019(2013).
[0183]
[32] Sciacca,E.et al.Silicon planar technology for single-photonoptical detectors.IEEE Trans.Elec.Dev.50,918-925(2003).
[0184]
[33] Zhang,J.,Itzler,M.A.,Zbinden,H.&Pan,J.-W.Advances in InGaAs / InPsingle-photon detector systems for quantum communication.Light:Science&Applications 4,e286(2015).
[0185]
[34] Tosi,A.,Calandri,N.,Sanzaro,M.&Acerbi,F.Low-noise,low-jitter,highdetection efficiency InGaAs / InP single-photon avalanche diode.IEEEJ.Sel.Top.Quantum Electron.20,3803406(2014).
[0186]
[35] Amri,E.,Boso,G.,Korzh,B.&Zbinden,H.Temporal jitter in free-running InGaAs / InP single-photon avalanche detectors.Optics Letters 41,5728-5731(2016).
[0187]
[36] Paul,D.J.8-band k.p modelling of the quantum confined Starkeffect in Ge quantum wells on Si substrates.Phys.Rev.B 77,155323(2008).
[0188]
[37] Dash,W.C.&Newman,R.Intrinsic optical absorption in single-crystalgermanium and silicon at 77Kand 300K.Phys.Rev.99,1151-1155(1955).
[0189]
[38] Itzler,M.A.et al.Single photon avalanche diodes(SPADs)for 1.5μmphoton counting applications.J.Modern Optics 54,283-304(2007).
[0190]
[39] Wang,S.,Ma,F.,Li,X.,Karve,G.,Zheng,X.&Campbell,J.C.Analysis ofbreakdown probabilities in avalanche photodiodes using a history-dependentanalytical model.Appl.Phys.Lett.82,1971-1973(2003).
[0191]
[40] Lacaita,A.&Mastrapasqua,M.Strong dependence of time resolution ondetector diameter in single photon avalanche diodes.Electron.Lett.26,2053-2054(1990).
[0192]
[41] Varshni,Y.P.Temperature dependence of the energy gap insemiconductors.Physica 34,149–154(1967).
[0193]
[42] Buller,G.S et al.Semiconductor avalanche diode detectors forquantum cryptography.IEEE LEOS Newsletter 20,(2006).
[0194]
[43] Jiang,X.,Itzler,M.A.,Ben-Michael,R.&Slomkowski,K.InGaAsP–InPavalanche photodiodes for single photon detection.IEEE J.Sel.Top.QuantumElectron.13,895-905(2007).
[0195]
[44] Korzh,B.,Lunghi,T.,Kuzmenko,K.,Boso,G.&Zbinden,H.Afterpulsingstudies of low-noise InGaAs / InP single-photon negative-feedback avalanchediodes.J.Modern Optics 62,1151-1157(2015).
[0196]
[45] Tosi,A.,Mora,A.D.,Zappa,F.&Cova,S.Single-photon avalanche diodesfor the near-infrared range:detector and circuit issues.J.Modern Optics 56,299-308(2009).
[0197]
[46] Statz,H.,deMars,G.,Davis Jr.,L.&Adams Jr.,A.Surface states onsilicon and germanium surfaces.Phys.Rev.106,455-464(1957).
[0198]
[47] Zhang,R.,Iwasaki,T.,Taoka,N.,Takenaka,M.&Takagi,S.Al2O3 / GeO x / Gegate stacks with low trap density fabricated by electron cyclotron resonanceplasma postoxidation.Appl.Phys.Lett.98,112902(2011).
[0199]
[48] Shevchenko,S.V.Electrical conductivity of germanium withdislocation grids.J.Exp.Theor.Phys.88,66-71(1999).
[0200]
[49] Sze,S.Physics of Semiconductor Devices.2 nd Ed.Wiley,New York(1981).
[0201]
[50] Binetti,S.,Pizzini,S.,Leoni,E.,Somaschini,R.,Castaldini,A.,&Cavallini,A.Optical properties of oxygen precipitates and dislocations insilicon.J.Appl.Phys.92,2437-2445(2002).
[0202]
[51] LeGoues,F.K.,Meyerson,B.S.,Morar,J.F.&Kirchner,P.D.Mechanism andconditions for anomalous strain relaxation in graded thin films andsuperlattices.J.Appl.Phys.71,4230-3243(1992).
[0203]
[52] Sauer,R.,Weber,J.,Soltz,J.Weber,E.R.,Küsters,K.-H.and Alexander,H.Dislocation-related photoluminescence in silicon.Appl.Phys.A 36,1-13(1985).
[0204]
[53] Noble,D.B.,Hoyt,J.L.,King,C.A.&Gibbons,J.F.,Reduction in misfitdislocation density by the selective growth of Si 1-x Ge x / Si in smallareas.Appl.Phys.Lett.56,51-53(1990).
[0205]
[54] R.Tobin,A.Halimi,A.McCarthy,M.Laurenzis,F.Christnacher andG.S.Buller,"Depth imaging through obscurants using time-correlated single-photon counting"Proc.SPIE,10659,106590S(2018).
Claims
1. A single photon avalanche diode (SPAD) device, comprising: A Si-based avalanche layer formed on the n-type semiconductor contact layer; a p-type charge sheet layer formed in or on the avalanche layer, the p-type charge sheet layer having an in-plane width; a Ge-based absorber layer formed on the charge sheet layer and / or the avalanche layer and overlapping the charge sheet layer, the Ge-based absorber layer having an in-plane width; Wherein, the in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type charge sheet layer in at least one in-plane direction.
2. The SPAD device according to claim 1, wherein: The in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type charge sheet layer in all in-plane directions.
3. The SPAD device according to claim 1 or claim 2, further comprising: a p-type semiconductor contact layer formed on the absorber layer, the p-type semiconductor contact layer having an in-plane width, Wherein, at least a portion of the p-type semiconductor contact layer is formed to be substantially aligned with at least a portion of the p-type charge sheet layer with the Ge-based absorber layer interposed therebetween.
4. The SPAD device according to claim 3, wherein: The in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type semiconductor contact layer in at least one in-plane direction.
5. The SPAD device according to claim 3, wherein: The in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type semiconductor contact layer in all in-plane directions.
6. The SPAD device according to claim 3, wherein: The in-plane width of the Ge-based absorber layer is greater than the in-plane width of the p-type semiconductor contact layer and greater than the in-plane width of the p-type charge sheet layer in all in-plane directions.
7. The SPAD device according to claim 3, wherein: The entire p-type semiconductor contact layer is formed to be substantially aligned with at least a portion of the p-type charge sheet layer.
8. The SPAD device according to claim 1 or 2, wherein: The Ge-based absorber has side walls in the in-plane direction and the charge sheet has side edges in the in-plane direction, and either: (a) when the Ge-based absorber has a thickness of at least 1 μm, the distance between the side edge of the charge sheet and the sidewall of the Ge-based absorber in the in-plane direction is at least 1 μm greater than the thickness of the Ge-based absorber; or (b) When the Ge-based absorber has a thickness of less than 1 μm, the distance between the side edge of the charge sheet and the sidewall of the Ge-based absorber in the in-plane direction is at least 1.0 μm.
9. The SPAD device according to claim 8, wherein: The distance between the side edge of the charge sheet and the side wall of the Ge-based absorber in the in-plane direction is at least 5 μm.
10. The SPAD device according to claim 3, wherein: The p-type semiconductor contact layer has a side edge in the in-plane direction and the charge sheet layer has a side edge in the in-plane direction, and either: (c) when the width of the charge sheet layer is at least 25 μm, the distance between the side edge of the charge sheet layer and the side edge of the p-type semiconductor contact layer in the in-plane direction is at least 2 μm; or (d) When the width of the charge sheet layer is less than 25 μm, the distance between the side edge of the charge sheet layer and the side edge of the p-type semiconductor contact layer in the in-plane direction is at least 1 μm.
11. The SPAD device according to claim 1 or 2, wherein: The charge sheet layer has a maximum doping concentration at a depth in a range of 10 nm to 100 nm from a surface of the Si-based avalanche layer.
12. A SPAD array comprising at least a 1x2 arrangement of SPAD devices, each of which is according to any one of claims 1 to 11 and formed on a common substrate.
13. The SPAD array according to claim 12, wherein: The respective Ge-based absorber layers of adjacent SPAD devices are laterally isolated by: (i) etching a continuous Ge-based absorber layer to at least the depth of the p-type charge sheet layer to form respective Ge-based absorber layers of adjacent SPAD devices; or (ii) doping a continuous Ge-based absorber layer to at least the depth of the p-type charge sheet layer to form respective Ge-based absorber layers of adjacent SPAD devices; or (iii) Selectively growing respective Ge-based absorber layers within the patterned electrically insulating layer to form respective Ge absorber layers of adjacent SPAD devices.
14. A LIDAR system comprising a light source with a wavelength in the range of 0.9 μm to 2.0 μm and a SPAD device according to any one of claims 1 to 11 or a SPAD array according to any one of claims 12 to 13.
15. Use of a SPAD device according to any one of claims 1 to 11 or a SPAD array according to any one of claims 12 to 13 in the detection of at least one photon having a wavelength in the range of 0.9 μm to 2.0 μm.
16. A method of manufacturing a SPAD device according to any one of claims 1 to 11, wherein: The p-type charge sheet is formed by selective area implantation into the Si-based avalanche layer.
17. The method according to claim 16, wherein: Prior to depositing the Ge-based absorber layer, the charge sheet is activated by annealing at a temperature of at least 850°C.
18. The method according to claim 16 or claim 17, wherein: At least one upper surface and / or side surface of the Ge-based absorber layer is passivated.
19. The method according to claim 18, wherein: The passivation is provided by a GeO2 layer which is thermally grown and protected by an Al2O3 layer.
Citation Information
Patent Citations
Avalanche Photodiode with Special Lateral Doping Concentration
US20120326259A1
Cited By
All-optical single-photon detector
US12683137B2
All-optical single-photon detector
US20240355602A1