Battery
By designing sealing parts in the battery to ensure that there is no solid electrolyte layer on the side of the negative active material layer, and arranging sealing parts in the stacking direction, the problem of insufficient reliability of the battery in terms of impact and mechanical strength is solved, and higher battery stability is achieved. properties and mechanical strength.
Patent Information
- Application Number
- CN201980067204.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-08-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-08-05
AI Technical Summary
Existing batteries suffer from shortcomings in reliability, especially in terms of impact and mechanical strength, leading to problems with micro-short circuits and interlayer delamination.
By designing the sealing member in the battery to ensure that no solid electrolyte layer is formed on the side of the negative electrode active material layer, and arranging the sealing member between the positive electrode current collector and the negative electrode current collector in the stacking direction, the insulation of the sealing member is utilized. and elastic properties to firmly join the negative electrode current collector and the positive electrode current collector, prevent impact and the influence of external gas, and provide space buffering to absorb mechanical impact when necessary.
Significantly improves the reliability of the battery, prevents micro short circuits and interlayer peeling, enhances mechanical strength, and ensures the stability of the battery during impact and charge and discharge processes.
Smart Images

Figure CN112840495B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to batteries. Background Art
[0002] Patent Document 1 discloses a battery having an insulating resin around a battery element.
[0003] Prior Art Literature
[0004] Patent Document 1: Japanese Patent Application Publication No. 2007-273350 Summary of the invention
[0005] Problems to be solved by the invention
[0006] In the prior art, it is expected that the reliability of batteries will be further improved.
[0007] Therefore, the present disclosure provides a battery with further improved reliability.
[0008] Means for solving problems
[0009] A battery according to a technical solution of the present disclosure comprises: a positive electrode collector; a positive electrode active material layer arranged in contact with the positive electrode collector; a solid electrolyte layer arranged in a manner covering the positive electrode active material layer; a negative electrode active material layer arranged in contact with the solid electrolyte layer; a negative electrode collector arranged in contact with the negative electrode active material layer; and a sealing component. The area of the negative electrode active material layer is larger than the area of the solid electrolyte layer when viewed from above. The area of each of the positive electrode collector and the negative electrode collector is larger than the area of the negative electrode active material layer when viewed from above. The sealing component is located outside the solid electrolyte layer when viewed from above, and is arranged in a cross section perpendicular to the stacking direction in a region sandwiched by a portion of the positive electrode collector and a portion of the negative electrode active material layer in the stacking direction, and in a region sandwiched by another portion of the positive electrode collector and a portion of the negative electrode collector in the stacking direction.
[0010] Effects of the Invention
[0011] According to the present disclosure, the reliability of the battery can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 This is a diagram showing an example of a schematic structure of a battery in the first embodiment.
[0013] Figure 2 This is a diagram showing an example of a schematic structure of a battery in Modification 1 of Embodiment 1.
[0014] Figure 3 This is a diagram showing an example of a schematic structure of a battery in a second modification of the first embodiment.
[0015] Figure 4 This is a diagram showing an example of a schematic structure of a battery in Modification 3 of Embodiment 1.
[0016] Figure 5 This is a diagram showing an example of a schematic structure of a battery in Modification 4 of Embodiment 1.
[0017] Figure 6 This is a diagram showing an example of a schematic structure of a battery in a fifth modification of the first embodiment.
[0018] Figure 7 This is a diagram showing an example of a schematic structure of a battery in Modification 6 of Embodiment 1.
[0019] Figure 8 It is a diagram showing a schematic structure of a battery of a comparative example.
[0020] Fig. 9 This is a diagram showing an example of a battery forming process in the first embodiment.
[0021] Fig.10 This is a diagram showing an example of a schematic structure of a battery in the second embodiment.
[0022] Fig.11 This is a diagram showing another example of the schematic structure of the battery in the second embodiment.
[0023] Fig.12 This is a diagram showing another example of the schematic structure of the battery in the second embodiment. DETAILED DESCRIPTION
[0024] (Overview of the present disclosure)
[0025] A battery in a technical solution of the present disclosure comprises: a positive electrode collector; a positive electrode active material layer arranged in contact with the positive electrode collector; a solid electrolyte layer arranged in a manner covering the positive electrode active material layer; a negative electrode active material layer arranged in contact with the solid electrolyte layer; a negative electrode collector arranged in contact with the negative electrode active material layer; and a sealing component. The area of the negative electrode active material layer is larger than the area of the solid electrolyte layer when viewed from above. The area of each of the positive electrode collector and the negative electrode collector is larger than the area of the negative electrode active material layer when viewed from above. The sealing component is located outside the solid electrolyte layer when viewed from above, and is arranged in a cross section perpendicular to the stacking direction in a region sandwiched by a portion of the positive electrode collector and a portion of the negative electrode active material layer in the stacking direction, and in a region sandwiched by another portion of the positive electrode collector and a portion of the negative electrode collector in the stacking direction.
[0026] Thus, there is an area on the side of the negative electrode active material layer where no solid electrolyte layer is formed. The portion where the solid electrolyte layer is formed on the side of the negative electrode active material layer is more likely to have problems with mechanical strength caused by uneven film thickness and film density than the portion where the solid electrolyte layer is formed on the stacked surface of the negative electrode active material layer that is closer to the side. Thus, according to the present disclosure, since no solid electrolyte layer is formed on the side of the negative electrode active material layer, when the battery is impacted, the occurrence of a small short circuit caused by proximity to the portion where the solid electrolyte layer is formed on the side of the positive electrode active material layer is suppressed. Thus, the reliability of the battery can be further improved.
[0027] In addition, for example, the sealing member may be arranged in contact with the positive electrode current collector, the negative electrode active material layer, and the negative electrode current collector.
[0028] Thus, the negative electrode collector and the positive electrode collector can be firmly joined by the sealing component. By joining the outer periphery of the negative electrode collector and the positive electrode collector by the sealing component, the positive electrode active material layer, the solid electrolyte layer and the negative electrode active material layer contained in the power generation element of the battery can be sealed to protect the power generation element from impact or external gas. Thus, the reliability of the battery can be further improved.
[0029] In addition, for example, the sealing member may be in contact with a portion of the stacking surface of the negative electrode active material layer.
[0030] Thus, the sealing component is arranged in contact with the stacked surface of the negative electrode active material layer in the area outside the solid electrolyte layer, and the negative electrode active material layer is firmly held by the sealing component. Therefore, in the case where an impact is applied to the battery and the negative electrode active material layer expands and contracts during charging and discharging, the peeling of the negative electrode active material layer and the solid electrolyte layer can be suppressed. Thus, the reliability of the battery can be further improved.
[0031] In addition, for example, the sealing member may have a shape that protrudes outward from at least one of the positive electrode current collector and the negative electrode current collector in a plan view.
[0032] Thus, the sealing component protrudes outwards further than the side surface of at least one of the negative electrode collector and the positive electrode collector. Therefore, when subjected to external force impact, it is easy to avoid the negative electrode collector and the positive electrode collector from being directly subjected to force, and the elastic performance of the sealing material can be used to absorb part of the impact force, thereby suppressing the damage of the battery. Thus, the reliability of the battery can be further improved.
[0033] In addition, for example, the battery may have a space between at least one of the positive electrode active material layer, the solid electrolyte layer, and the negative electrode active material layer and the sealing member, or may have a space inside the sealing member.
[0034] Thus, the sealing component has a space, so that when an external force is applied to the battery, even if the sealing component is deformed, by having a space between the power generation element including the positive electrode active material layer, the solid electrolyte layer and the negative electrode active material layer and the sealing component, or inside the sealing component, the impact can be eased in space, and the power generation element can be suppressed from being subjected to mechanical impact. Thus, the collapse of the power generation element due to mechanical impact such as external force can be suppressed, and the mechanical strength of the battery can be improved. In addition, when the power generation element is in contact with the space, even if gas is generated from the power generation element due to charging and discharging, the space can be used to ease the pressure of the gas, and the interlayer peeling of the power generation element caused by the generated gas can be suppressed. Thus, the reliability of the battery can be further improved.
[0035] In addition, for example, the sealing member may have a shape protruding toward the inside of the solid electrolyte layer.
[0036] Thus, the solid electrolyte layer is supported by the protruding portion of the sealing member, so even when an external force is applied to the battery, the collapse of the solid electrolyte layer can be suppressed. Therefore, the risk of damage to the power generation element can be reduced, and the reliability of the battery can be further improved.
[0037] Furthermore, the solid electrolyte layer may include a first solid electrolyte layer located on the negative electrode active material layer side and a second solid electrolyte layer located on the positive electrode active material layer side, and the sealing member may have a shape protruding between the first solid electrolyte layer and the second solid electrolyte layer.
[0038] Thus, the solid electrolyte layer is supported by the protruding portion of the sealing component, so even when an external force is applied to the battery, the collapse of the solid electrolyte layer can be suppressed. Therefore, the risk of damage to the power generation element can be reduced, and the reliability of the battery can be further improved. In addition, since the solid electrolyte layer is divided into two or more layers, the sealing component can easily form a shape protruding between the solid electrolyte layers, making the manufacture of the battery easy.
[0039] Furthermore, for example, the sealing member may include a first sealing member located on the negative electrode current collector side and containing a first material, and a second sealing member located on the positive electrode current collector side and containing a second material different from the first material.
[0040] This makes it possible to select the most suitable sealing material for each of the sealing members on the positive electrode side and the negative electrode side from the viewpoint of reactivity, mechanical characteristics, etc. This makes it possible to further improve the reliability of the battery.
[0041] In addition, for example, the sealing member may include a material having insulating properties and not having ion conductivity.
[0042] Thus, the material of the sealing component is insulating, so the conduction between the negative electrode collector and the positive electrode collector can be suppressed. In addition, the material of the sealing component does not have ion conductivity, for example, it is possible to suppress the reduction of battery characteristics caused by contact between the sealing material and other battery components. Thus, the reliability of the battery can be further improved.
[0043] In addition, for example, the sealing member may include a resin or a sealant.
[0044] Thus, the sealing member includes a resin or a sealant, so when an external force is applied to the battery or the battery is exposed to a humid atmosphere or a gas component, the flexibility, softness or gas barrier property of the sealing member can suppress adverse effects on the power generation element. Thus, the reliability of the battery can be further improved.
[0045] In addition, for example, the sealing member may include at least one selected from epoxy resin, acrylic resin, polyimide resin, and silsesquioxane.
[0046] Thus, epoxy resin, acrylic resin, polyimide resin and silsesquioxane are materials that have fluidity in the initial state and then lose fluidity and solidify by, for example, ultraviolet irradiation, heat treatment, etc., so that the sealing component can be formed using an easily solidified material. In addition, temporary curing by heat treatment or ultraviolet irradiation, or formal curing by heat treatment or ultraviolet irradiation can be performed as needed, thereby suppressing deformation of the sealing component at each stage of manufacturing.
[0047] In addition, for example, the sealing member may include a particulate metal oxide material.
[0048] This can further improve the characteristics of the sealing member, such as the ability to maintain the shape of the battery, the insulation, the thermal conductivity, and the moisture resistance.
[0049] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0050] Furthermore, the embodiments described below all represent general or specific examples. The numerical values, shapes, materials, components, configuration positions of components, connection methods, steps, and the order of steps shown in the following embodiments are only examples, and their purport does not limit the present disclosure. In addition, the components in the following embodiments that are not recorded in the independent claims are described as arbitrary components.
[0051] In addition, each figure is a schematic diagram and is not necessarily a strict illustration. Therefore, for example, the scales in each figure are not necessarily the same. In addition, the same reference numerals are attached to substantially the same structures in each figure, and repeated descriptions are omitted or simplified.
[0052] In the present specification, terms such as parallel indicating the relationship between elements, terms such as rectangle indicating the shape of elements, and numerical ranges do not have strict meanings but refer to substantially the same ranges, including, for example, a difference of several percent.
[0053] In addition, in this specification and the drawings, the x-axis, y-axis and z-axis represent the three axes of a three-dimensional rectangular coordinate system. In each embodiment, the z-axis direction is the thickness direction of the battery. In addition, in this specification, the "thickness direction" refers to the direction perpendicular to the surface of each layer stacked.
[0054] In addition, in this specification, "top view" refers to the situation of observing the battery along the stacking direction of the battery, and "thickness" in this specification refers to the length of the battery and each layer in the stacking direction. In addition, in this specification, "stacking surface" refers to the surface when observing the battery along the stacking direction of the battery. That is, the "stacking surface" is a surface that intersects the stacking direction. For example, the stacking surface is a surface that is substantially perpendicular to the stacking direction. In addition, in this specification, "side" refers to the surface when observing the battery from a direction perpendicular to the stacking direction of the battery. That is, "side" refers to a surface that intersects with a direction perpendicular to the stacking direction. For example, the side is a surface that is substantially parallel to the stacking direction.
[0055] In addition, the "inside" and "outside" in the present specification refer to the inside and outside when the battery is viewed along the stacking direction of the battery.
[0056] In addition, in this specification, the terms "upper" and "lower" in the structure of the battery do not refer to the upper direction (vertically above) and the lower direction (vertically below) in absolute spatial cognition, but are terms that are defined by relative positional relationships based on the stacking order of the stacked structure. In addition, the terms "upper" and "lower" are not only applicable to the case where two components are arranged with a gap between them and there is another component between them, but also to the case where two components are arranged to fit each other so that the two components are in contact.
[0057] (Implementation Method 1)
[0058] Figure 1 2 is a cross-sectional view showing a schematic structure of a battery 1000 in Embodiment 1. Specifically, Figure 1 (a) is a cross-sectional view showing the general structure of the battery 1000, showing Figure 1 A cross section at the position indicated by line 1A-1A in (b). Figure 1 (b) is a top perspective view showing a general structure of the battery 1000. Figure 1 In (b) of FIG. 1 , the planar shape of each component of the battery 1000 when the battery 1000 is viewed from above is indicated by a solid line or a dotted line.
[0059] like Figure 1 As shown, the battery 1000 in Embodiment 1 includes a power generation element 100, a negative electrode collector 210, a positive electrode collector 220, and a sealing member 310. Specifically, the battery 1000 includes: a positive electrode collector 220; a positive electrode active material layer 120 disposed in contact with the positive electrode collector 220; a solid electrolyte layer 130 disposed in a manner covering the positive electrode active material layer 120; a negative electrode active material layer 110 disposed in contact with the solid electrolyte layer 130; a negative electrode collector 210 disposed in contact with the negative electrode active material layer 110; and a sealing member 310.
[0060] The area of the negative electrode active material layer 110 is larger than the area of the solid electrolyte layer 130 when viewed from above. The area of each of the positive electrode collector 220 and the negative electrode collector 210 is larger than the area of the negative electrode active material layer 110 when viewed from above. The sealing member 310 is located outside the solid electrolyte layer 130 when viewed from above, and is arranged in a region sandwiched by a portion of the positive electrode collector 220 and a portion of the negative electrode active material layer 110 in the stacking direction, and in a cross section perpendicular to the stacking direction, in a region sandwiched by another portion of the positive electrode collector 220 and another portion of the negative electrode collector 210 in the stacking direction. Furthermore, in the present disclosure, "a cross section perpendicular to the stacking direction" refers to a region such as Figure 1 As shown in (a), a cross section parallel to the stacking direction is observed from a direction perpendicular to the stacking direction.
[0061] The sealing member 310 is disposed in contact with the positive electrode collector 220, the negative electrode active material layer 110, and the negative electrode collector 210. The sealing member 310 is in contact with the stacking surface of the negative electrode active material layer 110. In addition, a portion of the sealing member 310 may be disposed inside the solid electrolyte layer 130 in a plan view.
[0062] The power generation element 100 is disposed between the negative electrode current collector 210 and the positive electrode current collector 220. Figure 1As shown, the power generation element 100 includes a negative electrode active material layer 110 and a positive electrode active material layer 120. The power generation element 100 further includes a solid electrolyte layer 130. The negative electrode active material layer 110, the solid electrolyte layer 130, and the positive electrode active material layer 120 are stacked in order from the negative electrode collector 210 side along the thickness direction (z-axis direction) of the battery 1000.
[0063] The negative electrode active material layer 110 contains, for example, a negative electrode active material as an electrode material and is disposed facing the positive electrode active material layer 120 .
[0064] Graphite, metal lithium, or the like may be used as the negative electrode active material contained in the negative electrode active material layer 110. Various materials capable of desorbing and inserting ions of lithium (Li) or magnesium (Mg) may be used as the material of the negative electrode active material.
[0065] In addition, as the material contained in the negative electrode active material layer 110, for example, a solid electrolyte such as an inorganic solid electrolyte can be used. As the inorganic solid electrolyte, for example, a sulfide solid electrolyte or an oxide solid electrolyte can be used. As the sulfide solid electrolyte, for example, a mixture of lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) can be used. In addition, as the material contained in the negative electrode active material layer 110, for example, a conductive material such as acetylene black, Ketjen black, carbon black, graphite, carbon fiber, or a bonding adhesive such as polyvinylidene fluoride can be used. Examples of other adhesives include butadiene rubber, isoprene rubber, styrene-butadiene rubber (SBR), styrene-butadiene-styrene copolymer (SBS), styrene-ethylene-butadiene-styrene copolymer (SEBS), ethylene-propylene rubber, butyl rubber, chloroprene rubber, acrylonitrile-butadiene rubber, acrylic rubber, silicone rubber, synthetic rubbers such as fluororubber and polyurethane rubber, polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyimide, polyamide, polyamideimide, polyvinyl alcohol, and chlorinated polyethylene (CPE).
[0066] The negative electrode active material layer 110 can be prepared, for example, by kneading the materials contained in the negative electrode active material layer 110 with a solvent, applying the obtained paste coating on the surface of the negative electrode collector 210, and drying. In order to increase the density of the negative electrode active material layer 110, the negative electrode plate including the negative electrode active material layer 110 and the negative electrode collector 210 can be pressed after drying. The thickness of the negative electrode active material layer 110 is, for example, 5 μm or more and 300 μm or less, but is not limited thereto.
[0067] The positive electrode active material layer 120 is a layer containing a positive electrode material such as an active material. The positive electrode material is a material constituting a counter electrode of the negative electrode material. The positive electrode active material layer 120 contains, for example, a positive electrode active material.
[0068] As the positive electrode active material contained in the positive electrode active material layer 120, for example, lithium cobalt oxide composite oxide (LCO), lithium nickel oxide composite oxide (LNO), lithium manganese oxide composite oxide (LMO), lithium-manganese-nickel composite oxide (LMNO), lithium-manganese-cobalt composite oxide (LMCO), lithium-nickel-cobalt composite oxide (LNCO), lithium-nickel-manganese-cobalt composite oxide (LNMCO) and the like can be used.
[0069] As the material of the positive electrode active material, various materials that can extract and insert ions of lithium, magnesium, etc. can be used.
[0070] In addition, as a material contained in the positive electrode active material layer 120, for example, a solid electrolyte such as an inorganic solid electrolyte can be used. As an inorganic solid electrolyte, for example, a sulfide solid electrolyte or an oxide solid electrolyte can be used. As a sulfide solid electrolyte, for example, a mixture of lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) can be used. The surface of the positive electrode active material can be coated with a solid electrolyte. In addition, as a material contained in the positive electrode active material layer 120, for example, a conductive material such as acetylene black or a bonding adhesive such as polyvinylidene fluoride can be used. As a conductive material and an adhesive, the materials listed above as the materials used in the negative electrode active material layer 110 can be used.
[0071] The positive electrode active material layer 120 can be prepared, for example, by kneading the materials contained in the positive electrode active material layer 120 with a solvent, applying the obtained paste coating on the surface of the positive electrode collector 220, and drying. In order to increase the density of the positive electrode active material layer 120, the positive electrode plate including the positive electrode active material layer 120 and the positive electrode collector 220 can be pressed after drying. The thickness of the positive electrode active material layer 120 is, for example, 5 μm or more and 300 μm or less, but is not limited thereto.
[0072] The solid electrolyte layer 130 is disposed between the negative electrode active material layer 110 and the positive electrode active material layer 120. The solid electrolyte layer 130 is in contact with the negative electrode active material layer 110 and the positive electrode active material layer 120, respectively. The solid electrolyte layer 130 is a layer containing an electrolyte material. As the electrolyte material, a generally known electrolyte for a battery can be used. The thickness of the solid electrolyte layer 130 can be 5 μm or more and 300 μm or less, or can be 5 μm or more and 100 μm or less.
[0073] Solid electrolyte layer 130 may include a solid electrolyte. Battery 1000 including power generation element 100 may be, for example, an all-solid-state battery.
[0074] The solid electrolyte layer 130 is composed of a negative electrode side solid electrolyte layer 131 that mainly covers the negative electrode active material layer 110 and a positive electrode side solid electrolyte layer 132 that mainly covers the positive electrode active material layer 120. The negative electrode side solid electrolyte layer 131 and the positive electrode side solid electrolyte layer 132 may be formed integrally and used as the solid electrolyte layer 130. When the negative electrode side solid electrolyte layer 131 and the positive electrode side solid electrolyte layer 132 are formed integrally, the negative electrode side solid electrolyte layer 131 and the positive electrode side solid electrolyte layer 132 in the present embodiment are joined at an arbitrary internal plane parallel to the solid electrolyte layer 130.
[0075] As a solid electrolyte, for example, a solid electrolyte such as an inorganic solid electrolyte can be used. As an inorganic solid electrolyte, for example, a sulfide solid electrolyte, an oxide solid electrolyte, or a halide solid electrolyte can be used. As a sulfide solid electrolyte, for example, a mixture of lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) can be used. Furthermore, in addition to the electrolyte material, the solid electrolyte layer 130 may contain, for example, a bonding adhesive such as polyvinylidene fluoride. As the adhesive, the materials listed above as the materials used in the negative electrode active material layer 110 can be used.
[0076] In Embodiment 1, the negative electrode active material layer 110, the positive electrode active material layer 120, and the solid electrolyte layer 130 are maintained in parallel flat plate shape. Thus, the occurrence of cracks or collapse caused by bending can be suppressed. Furthermore, the negative electrode active material layer 110, the positive electrode active material layer 120, and the solid electrolyte layer 130 can be smoothly bent together.
[0077] The negative electrode collector 210 and the positive electrode collector 220 are each a conductive member. The negative electrode collector 210 and the positive electrode collector 220 may be, for example, a conductive film. As a material constituting the negative electrode collector 210 and the positive electrode collector 220, for example, a metal such as stainless steel (SUS), aluminum (Al), copper (Cu) or the like may be used.
[0078] The negative electrode current collector 210 is arranged in contact with the negative electrode active material layer 110. As the negative electrode current collector, for example, a metal foil such as SUS foil or Cu foil can be used. The thickness of the negative electrode current collector 210 is, for example, 5 μm or more and 100 μm or less, but is not limited thereto. Furthermore, the negative electrode current collector 210 may include, for example, a layer containing a conductive material, i.e., a current collector layer, in a portion in contact with the negative electrode active material layer 110.
[0079] The positive electrode current collector 220 is arranged in contact with the positive electrode active material layer 120. As the positive electrode current collector 220, for example, a metal foil such as SUS foil or Al foil can be used. The thickness of the positive electrode current collector 220 is, for example, 5 μm or more and 100 μm or less, but is not limited thereto. Furthermore, the positive electrode current collector 220 may include, for example, a layer containing a conductive material, i.e., a current collector layer, at a portion in contact with the positive electrode active material layer 120.
[0080] The sealing member 310 is disposed between the negative electrode current collector 210 and the positive electrode current collector 220. In addition, the sealing member 310 is disposed in contact with the side surface of the power generation element 100. In other words, the sealing member 310 is disposed so as to completely cover the power generation element 100. The sealing member 310 is formed of, for example, an electrically insulating material. The sealing member 310 functions as a spacer that maintains the gap between the negative electrode current collector 210 and the positive electrode current collector 220.
[0081] For example, the sealing member 310 is a member including the first material. For example, the sealing member 310 may be a member including the first material as a main component. For example, the sealing member 310 may be a member consisting of only the first material.
[0082] As the first material, for example, a generally known battery sealing component material such as a sealant can be used. As the sealant, a ceramic sealant, a resin sealant, etc. can be cited. Furthermore, the first material may include a material that has insulation and does not have ion conductivity. As the first material, for example, a resin material can be included. In addition, for example, the first material may include any one of a thermosetting resin, a photocurable resin such as an ultraviolet light, and a hot melt resin (thermoplastic resin). For example, the first material may include at least one of a thermosetting or photocurable epoxy resin, an acrylic resin, a polyimide resin, and silsesquioxane.
[0083] The sealing member 310 may include a particulate metal oxide material. As the metal oxide material, silicon oxide, aluminum oxide, titanium oxide, zinc oxide, cerium oxide, iron oxide, tungsten oxide, zirconium oxide, calcium oxide, zeolite, glass, etc. may be used. For example, the sealing member 310 may be formed using a resin material in which a plurality of particles composed of a metal oxide material are dispersed.
[0084] The particle size of the metal oxide material may be smaller than the distance between the negative electrode current collector 210 and the positive electrode current collector 220. The particle shape of the metal oxide material may be a perfect circle (sphere), an ellipsoid, a rod, or the like.
[0085] In a plan view, the formation region of the negative electrode active material layer 110 is formed to be smaller than the formation regions of the negative electrode collector 210 and the positive electrode collector 220, and is located inside the formation regions of the negative electrode collector 210 and the positive electrode collector 220. In a plan view, the formation region of the solid electrolyte layer 130 is formed to be smaller than the formation regions of the negative electrode collector 210, the positive electrode collector 220, and the negative electrode active material layer 110, and is located inside the formation regions of the negative electrode collector 210, the positive electrode collector 220, and the negative electrode active material layer 110.
[0086] In addition, in a plan view, the formation region of the positive electrode active material layer 120 is formed smaller than the formation region of the solid electrolyte layer 130, and is located inside the formation region of the solid electrolyte layer 130. In a plan view, the negative electrode collector 210 and the positive electrode collector 220 are formed at the same position. Thus, a portion of the positive electrode collector 220 is arranged at a position opposite to the region of the outer periphery of the negative electrode active material layer 110 that is not bonded to the solid electrolyte layer 130. In addition, another portion of the positive electrode collector 220 is arranged at a position opposite to the region of the outer periphery of the negative electrode collector 210 that is not bonded to the negative electrode active material layer 110.
[0087] According to the above technical configuration, when viewed from above, by forming the formation area of the negative electrode active material layer 110 smaller than the formation area of the negative electrode collector 210, the sealing component 310 can be placed in contact with the surface of the negative electrode collector 210 in the area outside the negative electrode active material layer 110. Thus, the negative electrode active material layer 110 can be protected from impact or external gas. In addition, when viewed from above, by forming the formation area of the negative electrode active material layer 110 smaller than the negative electrode collector 210, the sealing component 310 can be placed in contact with the side of the negative electrode active material layer 110. Thus, the negative electrode active material layer 110 can be supported by the sealing component 310, so that the side collapse of the negative electrode active material layer 110 can be suppressed.
[0088] In addition, in a plan view, by forming the formation region of the solid electrolyte layer 130 smaller than the formation region of the negative electrode active material layer 110, the sealing member 310 can be arranged in contact with a portion of the main surface (i.e., stacking surface) of the negative electrode active material layer 110 in the region outside the solid electrolyte layer 130. Thus, the vicinity of the end of the negative electrode active material layer 110 can be supported from both the side surface and the main surface (i.e., stacking surface), and the end surface collapse of the negative electrode active material layer 110 can be further suppressed.
[0089] In addition, when viewed from above, by forming the formation area of the positive electrode active material layer 120 smaller than the formation area of the solid electrolyte layer 130, the solid electrolyte 130 can be used to cover the entire side and stacking surface of the positive electrode active material layer 120 except the surface in contact with the positive electrode collector 220, and bonded to the negative electrode active material layer 110 via the solid electrolyte layer 130. As a result, the capacity of the battery can be accurately designed based on the area of the positive electrode active material layer 120, and the capacity accuracy of the battery can be improved. In addition, the electrochemical reaction can be uniformly generated throughout the positive electrode active material layer 120, so that the long-term reliability of the battery can be improved.
[0090] By arranging a portion of the positive electrode collector 220 opposite to the region of the outer periphery of the negative electrode active material layer 110 that is not bonded to the solid electrolyte layer 130, the sealing member 310 can be arranged in contact with both a portion of the main surface (i.e., stacking surface) of the negative electrode active material layer 110 and a portion of the main surface (i.e., stacking surface) of the positive electrode collector 220. In addition, by arranging another portion of the positive electrode collector 220 opposite to the region of the outer periphery of the negative electrode collector 210 that is not bonded to the negative electrode active material layer 110, the sealing member 310 can be arranged in contact with both a portion of the main surface of the negative electrode collector 210 and another portion of the main surface of the positive electrode collector 220 that are opposite to each other. Thus, the negative electrode collector 210 and the positive electrode collector 220 can be firmly bonded by the sealing member 310. By firmly bonding the outer peripheries of the negative electrode current collector 210 and the positive electrode current collector 220 over the entire area with the sealing member 310 , the power generation element 100 of the battery can be sealed and protected from impact and external air.
[0091] Figure 8 is a diagram showing a schematic structure of a battery of a comparative example. Figure 8 In the case of the battery 1700, when the main surface (i.e., the stacking surface) of the negative electrode active material layer 110 opposite to the positive electrode collector 220 is completely covered by the solid electrolyte layer 130, there will be a portion where only the sealing member 310 exists and a portion where only the solid electrolyte layer 130 exists between the positive electrode collector 220 and the negative electrode collector 210 when viewed from above. At this time, when an impact is applied to the battery 1700 or when the negative electrode active material layer 110 expands and contracts during charge and discharge, force is applied between the negative electrode collector 210 and the solid electrolyte layer 130, and the bonding between the negative electrode collector 210 and the solid electrolyte layer 130 is likely to become insufficient, resulting in deterioration of the sealing structure.
[0092] In contrast to the above, Figure 1If the formation region of the solid electrolyte layer 130 is formed smaller than the negative electrode active material layer 110 in a plan view, as in the battery 1000 in the first embodiment of the present invention, the sealing member 310 can be arranged in contact with the stacked surface of the negative electrode active material layer 110 in the region outside the solid electrolyte layer 130. Thus, the negative electrode active material layer 110 is firmly held by the sealing member 310, and the peeling of the solid electrolyte layer 130 when an impact is applied to the battery or when the negative electrode active material layer 110 expands and contracts during charge and discharge can be suppressed, thereby improving the reliability of the battery.
[0093] In addition, as in the comparative example Figure 8 As in the battery 1700 of FIG. 1 , when the main surface of the negative electrode active material layer 110 facing the positive electrode current collector 220 is entirely covered by the solid electrolyte layer 130, the portion where the solid electrolyte layer 130 is formed on the side surface of the negative electrode active material layer 110 and the portion where the solid electrolyte layer 130 is formed on the side surface of the positive electrode active material layer 120 can be closely opposed to each other. The portion where the solid electrolyte layer 130 is formed on the side surface of the negative electrode active material layer 110 and the portion where the solid electrolyte layer 130 is formed on the main surface of the positive electrode active material layer 120 that is more inner than the side surface are more likely to have a problem of mechanical strength due to uneven film thickness and film density than the portion where the solid electrolyte layer 130 is formed on the main surface (i.e., stacking surface) of the negative electrode active material layer 110 and the portion where the solid electrolyte layer 130 is formed on the main surface (i.e., stacking surface) of the positive electrode active material layer 120. Therefore, when such portions exist in close proximity on both the positive electrode side and the negative electrode side, a micro short circuit is likely to occur when the battery 1700 receives an impact.
[0094] like Figure 1 As in the battery 1000 in the first embodiment, the formation area of the solid electrolyte layer 130 is formed to be smaller than the formation area of the negative electrode active material layer 110 when viewed from above. Since the solid electrolyte layer 130 is not formed on the side of the negative electrode active material layer 110, the reliability of the battery can be improved.
[0095] [Modifications]
[0096] Hereinafter, a plurality of modified examples of Embodiment 1 will be described. In the following description of the plurality of modified examples, the description will focus on the differences from Embodiment 1 or the differences between the modified examples, and the description of the common points will be omitted or simplified.
[0097] <Variation 1>
[0098] First, use Figure 2 Modification 1 of Implementation Example 1 will be described. Figure 21 is a diagram showing a schematic structure of a battery 1100 in a first variation of the first embodiment. Specifically, Figure 2 (a) is a cross-sectional view showing the general structure of the battery 1100, showing Figure 2 A cross section at the position indicated by line 2A-2A in (b). Figure 2 (b) is a top perspective view showing the general structure of the battery 1100. Figure 2 In (b), the planar shape of each component of the battery 1100 when the battery 1100 is viewed from above is indicated by a solid line or a dotted line.
[0099] like Figure 2 As shown, in the battery 1100, the sealing member 310 protrudes between the negative electrode side solid electrolyte layer 131 on the negative electrode active material layer 110 side and the positive electrode side solid electrolyte layer 132 on the positive electrode active material layer 120 side. Thus, the solid electrolyte layer 130 can be more firmly held, so that the reliability of the battery can be further improved.
[0100] <Variation 2>
[0101] use Figure 3 Modification 2 of the first embodiment will be described. Figure 3 1 is a diagram showing a schematic structure of a battery 1200 in a second variation of the first embodiment. Specifically, Figure 3 (a) is a cross-sectional view showing the general structure of the battery 1200, showing Figure 3 A cross section at the position indicated by line 3A-3A in (b). Figure 3 (b) is a top perspective view showing the general structure of the battery 1200. Figure 3 In (b), the planar shape of each component of the battery 1200 when the battery 1200 is viewed from above is indicated by a solid line or a dotted line.
[0102] like Figure 3 As shown, the battery 1200 has a gap 350 between the sealing member 310 and the solid electrolyte layer 130. A portion of the gap 350 is in contact with a portion of the negative electrode active material layer 110. The gap 350 is filled with a gas. As the gas filled, for example, it is air, but it can also be a rare gas such as argon or nitrogen. In addition, the gap 350 can be decompressed to be lower than the atmospheric pressure. In addition, the gap 350 is an example of a space.
[0103] The gaps 350 can partially release stress caused by external impact from the side of the battery 1200 and deformation caused by expansion and contraction of the negative electrode active material layer 110 and the positive electrode active material layer 120 during charge and discharge, thereby further improving battery reliability.
[0104] Furthermore, since the power generation element 100 is in contact with the gap 350 , even if gas is generated from the power generation element 100 due to charge and discharge, the pressure of the gas can be relieved by the gap 350 , thereby suppressing delamination of the power generation element 100 due to the generated gas.
[0105] <Variation 3>
[0106] use Figure 4 Modification 3 of Implementation Example 1 will be described. Figure 4 1 is a diagram showing a schematic structure of a battery 1300 in a third variation of the first embodiment. Specifically, Figure 4 (a) is a cross-sectional view showing the general structure of the battery 1300, showing Figure 4 A cross section at the position indicated by line 4A-4A in (b). Figure 4 (b) is a top perspective view showing the general structure of the battery 1300. Figure 4 In (b), the planar shape of each component of the battery 1300 when the battery 1300 is viewed from above is indicated by a solid line or a dotted line.
[0107] like Figure 4 As shown, a portion of the sealing member 310 of the battery 1300 is bonded to the solid electrolyte layer 130, and there is a gap 352 between the sealing member 310 and the solid electrolyte layer 130 and between the sealing member 310 and the negative electrode active material layer 110. The gap 352 is a space surrounded by the sealing member 310 and the solid electrolyte layer 130 or the sealing member and the negative electrode active material layer 110. The gap 352 is filled with gas. As the gas filled, for example, it is air, but it can also be a rare gas such as argon or nitrogen. In addition, the gap 352 can be decompressed to below atmospheric pressure.
[0108] Thus, sealing member 310 can prevent collapse of solid electrolyte layer 130 and, through gap 352 , can reduce damage to power generation element 100 when battery 1400 is impacted, thereby improving the reliability of the battery against impact.
[0109] Furthermore, even when gas is generated from the power-generating element 100 due to charge and discharge, the pressure of the gas can be relieved by the gap 352 , thereby suppressing delamination of the power-generating element 100 due to the generated gas.
[0110] <Variation 4>
[0111] use Figure 5 Modification 4 of Implementation Example 1 will be described. Figure 5 1 is a diagram showing a schematic structure of a battery 1400 in a fourth variation of the first embodiment. Specifically, Figure 5(a) is a cross-sectional view showing the general structure of the battery 1400, showing Figure 5 A cross section at the position indicated by line 5A-5A in (b). Figure 5 (b) is a top perspective view showing the general structure of the battery 1400. Figure 5 In (b), the planar shape of each component of the battery 1400 when the battery 1400 is viewed from above is indicated by a solid line or a dotted line.
[0112] like Figure 5 As shown, the sealing member 310 of the battery 1400 has a tiny pore 354 whose diameter is smaller than the thickness and width of the power generation element. That is, the battery 1400 has a pore 354 inside the sealing member 310. The pore 354 is an independent pore inside the sealing member 310 and is completely surrounded by the sealing member 310. The pore 354 is filled with a gas. As the gas filled, for example, it is air, but it can also be a rare gas such as argon or nitrogen. In addition, the pore 354 can be depressurized to be lower than the atmospheric pressure. Furthermore, the pore 354 is an example of a space.
[0113] Thus, damage to the power generating element 100 when the battery 1400 is subjected to an impact can be reduced by deformation of the pores 354 in the sealing member 310 , thereby improving the reliability of the battery 1400 against impacts.
[0114] <Variant 5>
[0115] use Figure 6 Modification 5 of the first embodiment will be described. Figure 6 1 is a diagram showing a schematic structure of a battery 1500 in a fifth variation of the first embodiment. Specifically, Figure 6 (a) is a cross-sectional view showing the general structure of the battery 1500, showing Figure 6 A cross section at the position indicated by line 6A-6A in (b). Figure 6 (b) is a top perspective view showing the general structure of the battery 1500. Figure 6 In (b) of FIG. 1 , the planar shape of each component of the battery 1500 when the battery 1500 is viewed from above is indicated by a solid line or a dotted line.
[0116] like Figure 6 As shown, the sealing member 310 of the battery 1500 protrudes outward further than the side surfaces of the negative electrode collector 210 and the positive electrode collector 220. Thus, when an external force impact is applied, it is easy to avoid direct force on the negative electrode collector 210 and the positive electrode collector 220, and the elasticity of the sealing member 310 can be used to absorb a part of the impact force, so that the damage of the battery can be suppressed.
[0117] <Variant 6>
[0118] use Figure 7 Modification example 6 of embodiment 1 is described. Figure 7 1 is a diagram showing a schematic structure of a battery 1600 in a sixth variation of the first embodiment. Specifically, Figure 7 (a) is a cross-sectional view showing the general structure of the battery 1600, showing Figure 7 A cross section at the position indicated by line 7A-7A in (b). Figure 7 (b) is a top perspective view showing the general structure of the battery 1600. Figure 7 In (b), the planar shape of each component of the battery 1600 when the battery 1600 is viewed from above is indicated by a solid line or a dotted line.
[0119] like Figure 7 As shown, the battery 1600 has a first sealing member 311 and a second sealing member 312 instead of the sealing member 310. The first sealing member 311 is located on the side close to the negative electrode collector 210 and contains the first material. The second sealing member 312 is located on the side closer to the positive electrode collector 220 than the first sealing member 311 and contains the second material. The second material is a material different from the first material. The second material is, for example, a material having insulation and not having ion conductivity. The second material may contain a resin or a sealant. The second material may be, for example, a material selected from a plurality of materials that can be used as the first material and different from the material contained in the first sealing member 311. For example, the second material may be a material that is not contained in the first sealing member 311 among epoxy resins, acrylic resins, polyimide resins, and silsesquioxanes that are thermosetting or photocurable. The second material may contain a particulate metal oxide material.
[0120] The structure including the first sealing member 311 and the second sealing member 312 allows selection of the most suitable material for each of the sealing members on the positive electrode side and the negative electrode side from the viewpoint of reactivity, mechanical characteristics, etc. This can further improve the reliability of the battery 1600 .
[0121] [Battery manufacturing method]
[0122] Next, an example of a method for manufacturing a battery in the first embodiment and each modification example is described. Fig. 9 The following describes a method for manufacturing the battery 1300 in the above-mentioned modification 3. The same is true for the other batteries 1000 , 1100 , 1200 , 1400 , 1500 , and 1600 .
[0123] Fig. 9 It is a cross-sectional view showing an example of a method for manufacturing the battery 1300 .
[0124] First, a paste coating is prepared by kneading the positive electrode material and the solvent. The coating is applied to the positive electrode collector 220. That is, the positive electrode active material layer 120 is formed. Then, a paste coating is applied to the positive electrode collector 220 in a manner that covers the entire positive electrode active material layer 120 to be coated, and dried. That is, the positive electrode side solid electrolyte layer 132 is formed. In this way, a product such as Fig. 9 (a) shows the positive electrode plate. The positive electrode material and the solid electrolyte material may also be prepared using materials that do not contain a solvent.
[0125] Then, if Fig. 9 As shown in (b), a sealing material is applied to the peripheral portion of the positive electrode side solid electrolyte layer 132. That is, a sealing component 310 is formed. The thickness of the sealing component 310 is appropriately adjusted according to the thickness of the positive electrode active material layer 120, the positive electrode side solid electrolyte layer 132, the negative electrode active material layer 110 and the negative electrode side solid electrolyte layer 131, thereby being able to adjust the degree of expansion of the sealing material when the battery is formed. By adjusting the thickness of the formed sealing component 310, a part of the sealing component 310 can also become a protruding portion protruding toward the inside of the solid electrolyte layer 130 or the outside of the battery when the battery is formed. The method for forming the solid electrolyte layer 130 or the protruding portion of the solid electrolyte layer 130 is not limited to this.
[0126] Furthermore, by providing a minute space between the position where the sealing member 310 is formed and the positive electrode-side solid electrolyte layer 132 , a minute gap 352 can be formed between the sealing member 310 and the power generation element 100 after being joined.
[0127] In addition, after the sealing material is applied, heat treatment or ultraviolet irradiation may be performed. Thus, when the sealing material includes a thermosetting material or a photocurable material, the viscosity of the coating can be increased while maintaining the fluidity of the coating, thereby promoting the curing of the coating. By utilizing such viscosity increase and curing, the deformation of the sealing member 310 can be controlled.
[0128] Next, prepare a paste coating obtained by kneading the negative electrode material and the solvent together. Apply the coating to the negative electrode collector 210 in a larger area than the positive electrode side solid electrolyte layer 132. That is, form the negative electrode active material layer 110. Furthermore, apply the solid electrolyte material to the negative electrode active material layer 110 in a smaller area than the coated negative electrode active material layer 110, for example, in a manner having the same area as the positive electrode side solid electrolyte layer 132, and dry it. That is, form the negative electrode side solid electrolyte layer 131. Thus, a negative electrode plate is produced. Furthermore, the negative electrode material can also be prepared using a material that does not contain a solvent.
[0129] Then, if Fig. 9As shown in (c), a pressurizing fixture 500 having an upper fixture 510 and a lower fixture 520 is used to align the positions of the positive electrode side solid electrolyte layer 132 and the negative electrode side solid electrolyte layer 131, and to press the negative electrode plate and the positive electrode plate. Specifically, the negative electrode plate and the positive electrode plate are sandwiched between the upper fixture 510 and the lower fixture 520 for pressurization.
[0130] At this time, for example, by preheating the pressurizing jig and mixing a foaming source that generates gas due to heat into the sealing member, a plurality of minute pores 354 can be obtained in the sealing member 310 after bonding.
[0131] Therefore, if Fig. 9 As shown in (d), battery 1300 is manufactured.
[0132] Furthermore, for example, when the sealing material includes a thermosetting material or a photocurable material, the sealing member 310 may be completely cured by heat treatment or ultraviolet irradiation, etc. This can make the sealing state more firm.
[0133] In addition, the sealing material may be applied to the negative electrode current collector 210 and the negative electrode active material layer 110 instead of applying the sealing material to the positive electrode current collector 220 .
[0134] In addition, the sealing material can also be applied to the negative electrode collector 210 and the negative electrode active material layer 110, and the positive electrode collector 220. That is to say, after forming a part of the sealing component 310 on the negative plate and the positive plate, the negative plate and the positive plate can be bonded. As a result, the amount of the sealing component 310 formed at one time is reduced, so the sealing component 310 can be formed more quickly. In addition, by making the bonding between the negative plate and the sealing component 310 and the bonding between the positive plate and the sealing component 310 reliable, the bonding between the negative plate and the positive plate separated by the sealing component 310 can be made stronger. In addition, since the protrusion of the sealing component 310 becomes lower, the negative plate or the positive plate in the middle of the process can be easily wound up. In addition, by using the first material and the second material on the negative plate and the positive plate, respectively, the best different sealing materials can be selected for the negative plate and the positive plate.
[0135] Through the above steps, by crimping the negative electrode plate and the positive electrode plate, the negative electrode collector and the positive electrode collector can be prevented from short-circuiting by the sealing member 310, and the negative electrode collector and the positive electrode collector can be firmly joined. In addition, as the first material included in the sealing member 310, by using a material having better properties such as impact resistance and insulation than the solid electrolyte material, the impact resistance when an impact is applied to the battery can be improved.
[0136] As mentioned above, in Fig. 9The manufacturing method of the battery 1300 shown includes a step of forming a sealing member 310 in advance before bonding the positive electrode plate and the negative electrode plate. As a result, the sealing member 310 can be arranged between the negative electrode collector 210 and the positive electrode collector 220, and the risk of short circuit caused by direct contact between the negative electrode collector 210 and the positive electrode collector 220 can be greatly reduced without increasing the thickness of the battery 1300. At the same time, the bonding strength between the positive electrode plate and the negative electrode plate around the outer periphery of the power generation element 100 can be strengthened. In addition, since the sealing member 310 is also formed on the negative electrode active material layer 110, the negative electrode active material layer 110 is firmly held by the sealing member 310, and the peeling of the solid electrolyte layer 130 when the negative electrode active material layer 110 expands and contracts during charging and discharging can be suppressed.
[0137] Furthermore, the position where the sealing member 310 is formed, the shapes of the negative electrode active material layer 110, the positive electrode active material layer 120 and the solid electrolyte layer 130, the sizes of the negative electrode collector 210 and the positive electrode collector 220, etc. can also be adjusted. Thus, the batteries shown in the first embodiment and each modified example can be manufactured respectively. In addition, by stacking a plurality of batteries, the stacked batteries shown in the second embodiment described later can be manufactured respectively.
[0138] (Implementation Method 2)
[0139] Hereinafter, Embodiment 2 will be described. In the following description, differences from Embodiment 1 and each modification example described above will be mainly described, and description of common points will be appropriately omitted or simplified.
[0140] Fig.10 2 is a cross-sectional view schematically showing a structure of a laminated battery 2000 in Embodiment 2. The laminated battery 2000 in Embodiment 2 is a laminated battery in which a plurality of batteries 1000 in Embodiment 1 are laminated and electrically connected.
[0141] exist Fig.10 In the example shown, the stacked battery 2000 has a structure in which three batteries 2002, 2004, and 2006 are stacked in this order. For example, the batteries 2002, 2004, and 2006 each have the same structure as the battery 1000 in Embodiment 1. For example, at least one of the batteries 2002, 2004, and 2006 may be the battery 1000 in Embodiment 1, or may be at least one of the batteries 1100 to 1600 in Modifications 1 to 6 of Embodiment 1.
[0142] In the stacked battery 2000, a plurality of batteries can be stacked in series by joining the negative electrode collector 210 of a predetermined battery (e.g., a single cell) to the positive electrode collector 220 of another battery (e.g., a single cell). Fig.10 As shown, the positive and negative electrodes of the batteries 2002, 2004 and 2006 are the same above and below, the positive electrode collector 220 of the battery 2002 is joined to the negative electrode collector 210 of the battery 2004, and the positive electrode collector 220 of the battery 2004 is joined to the negative electrode collector 210 of the battery 2006, and the batteries 2002, 2004 and 2006 are connected in series. The joining of the negative electrode collector 210 and the positive electrode collector 220 can be directly joined, or can be joined by a conductive adhesive or welding method. It is also possible to use a negative electrode collector 210 and a positive electrode collector 220 that are previously integrated. By forming an outer seal 340 on the periphery of the stacked battery 2000, the stacked battery 2000 can be sealed as a whole, further improving the reliability of the battery.
[0143] The number of cells included in the stacked battery may be 3 or more, or may be only 2. By adjusting the number of stacked cells, desired battery characteristics can be obtained.
[0144] In addition, if Fig.11 As shown, while the stacked battery 2100 is constrained and pressed from both sides using the constraining and pressing upper jig 552 and the constraining and pressing lower jig 551 , the stacked battery 2100 can be charged and discharged from the negative electrode collector plate 571 and the positive electrode collector plate 572 .
[0145] In addition, when constructing a stacked battery, depending on the required characteristics, for example, Fig.12 As shown in the stacked battery 2200, multiple batteries are connected in parallel. Fig.12 In, with Fig.10 In contrast, the stacking direction of battery 2004 is opposite, and the positive electrode current collector 220 of battery 2002 is joined to the positive electrode current collector 220 of battery 2004. In addition, the negative electrode current collector 210 of battery 2004 is joined to the negative electrode current collector 210 of battery 2006. Multiple current collectors of the same polarity are connected by parallel current collectors 230, respectively.
[0146] In addition, the batteries included in the stacked battery may be a mixture of two or more batteries connected in parallel and two or more batteries connected in series. Thus, a stacked battery with a high battery capacity can be realized with a limited volume. Series connection, parallel connection or a mixture thereof can be easily realized by changing the connection method of the collectors between multiple single battery cells in the known technology.
[0147] According to the above technical configuration, a high voltage can be obtained by stacking a plurality of single cells in series. Therefore, a stacked battery of a series type with a low risk of short circuit can be realized. That is, a stacked battery with a bipolar structure stacked in series and a low risk of short circuit caused by contact between collectors can be formed. In addition, a stacked battery with a high battery capacity can be obtained by stacking a plurality of single cells in parallel. Therefore, a stacked battery of a parallel type with a low risk of short circuit can be realized. That is, a stacked battery with a structure stacked in parallel and a low risk of short circuit caused by contact between collectors can be formed.
[0148] Furthermore, the laminated battery may be enclosed in a sealed case. As the sealed case, for example, a laminate bag, a metal can, a resin case or the like may be used. By using a sealed case, it is possible to suppress the deterioration of the power generation element due to moisture.
[0149] (Other embodiments)
[0150] The above is a description of one or more battery solutions based on the embodiments, but the present disclosure is not limited to these embodiments. As long as it does not depart from the main purpose of the present invention, the various modifications that can be thought of by those skilled in the art to each embodiment, and the solutions constructed by combining the constituent elements in different embodiments are also included in the scope of the present invention.
[0151] In addition, various changes, substitutions, additions, omissions, etc. can be made to the above-mentioned embodiments within the scope of the claims or the scope equivalent thereto.
[0152] For example, in the above-mentioned embodiment, the solid electrolyte layer on the positive electrode side and the solid electrolyte layer on the negative electrode side have the same area when viewed from above and are formed in overlapping positions, but not limited to this, the area of either the solid electrolyte layer on the positive electrode side or the solid electrolyte layer on the negative electrode side can be made larger when viewed from above, and a sealing component can be formed on the surface where the solid electrolyte layers do not contact each other.
[0153] In the above embodiment, the entire stacking surface and side surfaces of the positive electrode current collector are covered with the solid electrolyte layer, but the present invention is not limited thereto and only the stacking surface side may be covered, with the side surface in contact with the sealing member.
[0154] Industrial Availability
[0155] The battery of the present disclosure can be used as a battery for electronic devices, electrical appliances, electric vehicles, and the like.
[0156] Description of Reference Numerals
[0157] 100 power generation elements
[0158] 110 negative electrode active material layer
[0159] 120 positive electrode active material layer
[0160] 130 Solid electrolyte layer
[0161] 131Solid electrolyte layer on the negative electrode side
[0162] 132Cathode side solid electrolyte layer
[0163] 210 negative electrode collector
[0164] 220 positive electrode collector
[0165] 310 sealing parts
[0166] 311 No.1 sealing component
[0167] 312 2nd sealing component
[0168] 340 Outer Seal
[0169] 350, 352 gaps
[0170] 354 empty hole
[0171] 500 Pressurized fixture
[0172] 510 upper fixture
[0173] 520 lower fixture
[0174] 551 Constrained Pressurized Fixture
[0175] 552 Constraint Pressurized Upper Fixture
[0176] 571 negative electrode collector plate
[0177] 572 positive collector plate
[0178] 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700 batteries
[0179] 2000, 2100, 2200 stacked batteries
Claims
1. A battery having: Positive electrode current collector; A positive electrode active material layer is disposed in contact with the positive electrode current collector; a solid electrolyte layer arranged so as to cover the side surfaces and stacking surface of the positive electrode active material layer; A negative electrode active material layer is disposed in contact with the solid electrolyte layer; A negative electrode current collector is disposed in contact with the negative electrode active material layer; and Sealing parts, The area of the negative electrode active material layer is larger than the area of the solid electrolyte layer when viewed from above. The positive electrode current collector and the negative electrode current collector each have an area larger than the area of the negative electrode active material layer when viewed from above. The sealing member is located outside the solid electrolyte layer in a plan view, and is arranged in a region sandwiched by a portion of the positive electrode collector and a portion of the negative electrode active material layer in the stacking direction, and in a region sandwiched by another portion of the positive electrode collector and a portion of the negative electrode collector in the stacking direction, in a cross section perpendicular to the stacking direction. There is a region on the side surface of the negative electrode active material layer where the solid electrolyte layer is not formed.
2. The battery according to claim 1, The sealing member is arranged in contact with the positive electrode current collector, the negative electrode active material layer, and the negative electrode current collector.
3. The battery according to claim 1 or 2, The sealing member is in contact with a portion of a stacked surface of the negative electrode active material layer.
4. The battery according to claim 1 or 2, The sealing member has a shape that protrudes outward from at least one of the positive electrode current collector and the negative electrode current collector in a plan view.
5. The battery according to claim 1 or 2, There is a space between at least one of the positive electrode active material layer, the solid electrolyte layer, and the negative electrode active material layer and the sealing member, or there is a space inside the sealing member.
6. The battery according to claim 1 or 2, The sealing member has a shape that protrudes toward the inside of the solid electrolyte layer.
7. The battery according to claim 1 or 2, The solid electrolyte layer has: a first solid electrolyte layer located on the negative electrode active material layer side; and a second solid electrolyte layer located on the positive electrode active material layer side, The sealing member has a shape protruding between the first solid electrolyte layer and the second solid electrolyte layer.
8. The battery according to claim 1 or 2, The sealing component has: a first sealing member located on the negative electrode current collector side and containing a first material; and A second sealing member is located on the positive electrode current collector side and includes a second material different from the first material.
9. The battery according to claim 1 or 2, The sealing member includes a material having insulating properties and not having ion conductivity.
10. The battery according to claim 1 or 2, The sealing member includes a resin or a sealant.
11. The battery according to claim 1 or 2, The sealing member includes at least one selected from epoxy resin, acrylic resin, polyimide resin, and silsesquioxane.
12. The battery according to claim 1 or 2, The sealing member includes a particulate metal oxide material.
Citation Information
Patent Citations
Stacked battery and manufacturing method therefor
JP2007273350A
Thin battery and manufacture thereof
JP1994052866A
Secondary battery and its manufacturing method
JP2003092092A
Lithium secondary battery and its manufacturing method
JP2007005219A
Stacked battery and manufacturing method therefor
JP2007273349A