Surface treated copper foil, copper foil with carrier, copper clad laminate and printed circuit board

By giving a unique surface profile to the surface of the resin substrate and controlling the deflection Ssk of the resin film, the problem of circuit entrapment in the SAP method is solved, the adhesion between the circuit and the insulating layer is improved, and the stability and reliability of the circuit are enhanced. .

CN112969824BActive Publication Date: 2024-10-18MITSUI MINING & SMELTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201980073918.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-02
Publication Date
2024-10-18
Estimated Expiration
2039-10-02

AI Technical Summary

Technical Problem

In the manufacturing process of printed circuit boards, when using the SAP method, circuit entrapment is prone to occur during the etching process of the electroless copper plating layer, resulting in a reduction in the adhesion between the circuit and the insulating layer, thereby affecting the stability and reliability of the circuit.

Method used

By imparting a unique surface profile to the surface of the resin substrate, specifically by processing the surface to thermally press the resin film and removing the surface-treated copper foil by etching, the deflection Ssk of the remaining resin film is controlled below -0.6 to suppress the sinking occur.

Benefits of technology

It effectively suppresses the occurrence of sinking in the circuit, improves the adhesion between the circuit and the insulating layer, and enhances the stability and reliability of the circuit. Especially under the finer circuit pattern width, it significantly improves the effect of the etching process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112969824B_ABST
    Figure CN112969824B_ABST
Patent Text Reader

Abstract

Provided is a surface-treated copper foil, which, when used in a SAP method, can impart a surface profile to a resin substrate, and the surface profile can effectively suppress the occurrence of sinking that may occur in a circuit during the etching process of a chemical copper plating layer. The surface-treated copper foil is a surface-treated copper foil having a treated surface on at least one side, and when a resin film is thermally pressed onto the treated surface to transfer the surface shape of the treated surface to the surface of the resin film, and the surface-treated copper foil is removed by etching, the skewness Ssk of the surface of the remaining resin film measured in accordance with ISO25178 is less than -0.6.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a surface treated copper foil, a copper foil with a carrier, a copper clad laminate and a printed circuit board. Background Art

[0002] In recent years, the semi-additive process (SAP process) has been widely used as a method for manufacturing printed circuit boards suitable for miniaturization of circuits. The SAP process is a method suitable for forming extremely fine circuits. As an example, the SAP process is performed using a roughened copper foil with a carrier. For example, Figure 1 and Figure 2 As shown, a prepreg 12 and a primer 13 are used to press an ultra-thin copper foil 10 having a roughened surface onto an insulating resin substrate 11 to make it close, and the insulating resin substrate 11 has a lower circuit 11b on a base substrate 11a (process (a)). After peeling off the carrier (not shown), a via 14 is formed by laser perforation as needed (process (b)). Then, the ultra-thin copper foil is removed by etching to expose the primer 13 with a roughened surface profile (process (c)). After chemical copper plating 15 is applied to the roughened surface (process (d)), a dry film 16 is used to mask with a prescribed pattern by exposure and development (process (e)), and electroplating copper 17 is applied (process (f)). After removing the dry film 16 and forming a wiring portion 17a (process (g)), the unnecessary chemical copper plating 15 between adjacent wiring portions 17a, 17a is removed by etching (process (h)), and a wiring 18 having a prescribed pattern is obtained.

[0003] The SAP method using such a roughened copper foil removes the roughened copper foil itself by etching after laser perforation (process (c)). Thus, the concavo-convex shape of the roughened surface of the roughened copper foil is transferred to the surface of the laminate from which the roughened copper foil is removed, so that in the subsequent process, the closeness between the insulating layer (e.g., the primer layer 13, or the prepreg 12 when the primer layer is not present) and the plated circuit (e.g., the wiring 18) can be ensured. It should be noted that the modified semi-additive method (MSAP method) that does not perform the copper foil removal process equivalent to process (c) is also widely used, but in the etching process (equivalent to process (h)) after the dry film is removed, the copper foil layer and the chemical copper plating layer must be removed by etching. Therefore, compared with the SAP method that can remove one layer of the chemical copper plating layer by etching, it is necessary to perform etching in depth. Therefore, considering the larger etching amount, there is a need to make the circuit space narrower, so it can be said that in terms of fine circuit formability, the MSAP method is slightly inferior to the SAP method. That is, the SAP method is more advantageous for the purpose of forming a finer circuit.

[0004] In addition, in the etching step (corresponding to step (h)) after the dry film is removed, the interface between the circuit (e.g., wiring 18) and the insulating layer is etched, and as a result, a phenomenon called "sinking" occurs in which the base of the circuit is etched in a collapsed manner. When this sinking occurs, the adhesion between the circuit and the insulating layer decreases, which causes the circuit to peel off.

[0005] On the other hand, there is known a roughened copper foil in which the shape of the roughened particles is controlled. For example, in Patent Document 1 (Japanese Patent No. 6293365), in a roughened copper foil having a roughened surface with a plurality of substantially spherical protrusions, the average height of the substantially spherical protrusions is set to 2.60 μm or less, and the average maximum diameter b of the substantially spherical protrusions is set to 2.60 μm or less. ave Average bottleneck diameter a relative to the roughly spherical protrusion ave The ratio ave / a ave When the ratio is 1.2 or more, when used in the SAP method, the laminate can be provided with a surface profile that is excellent in not only plated circuit adhesion but also excellent in etching properties against chemical copper plating.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1; Japanese Patent No. 6293365 Summary of the invention

[0009] In recent years, as the circuits have become more miniaturized, the application of the SAP method, which is beneficial to the formation of fine circuits, has expanded. For the second point, it can be said that as the width of the circuit pattern becomes narrower, the allowable sinking width is relatively reduced. In addition, in the SAP method, in the etching process after the dry film is removed, only the chemical copper plating layer is etched away. Therefore, an etching solution that does not remove electrolytic copper but selectively removes chemical copper plating can be used. In this way, the circuit, which is mostly composed of electrolytic copper, can be suppressed from becoming thinner. Therefore, from the perspective of fine circuit formation, it can be said that the SAP method is more advantageous than the MSAP method. On the other hand, since the bottom part of the circuit formed by the SAP method is composed of chemical copper plating, it becomes easier to sink when using the above-mentioned etching solution.

[0010] The present inventors have obtained the following knowledge: by giving the surface of a resin substrate a unique surface profile defined by the skewness Ssk measured in accordance with ISO25178, the occurrence of sinking that may occur in the circuit during the etching process of the chemical copper plating layer in the SAP method can be effectively suppressed. In addition, the present inventors have obtained the following knowledge: a surface-treated copper foil capable of giving the above-mentioned unique surface profile to a resin substrate when used in the SAP method can be provided.

[0011] Therefore, an object of the present invention is to provide a surface-treated copper foil which, when used in a SAP method, can provide a resin substrate with a surface profile that can effectively suppress the occurrence of depressions that may occur in a circuit during an etching step of an electroless copper plating layer.

[0012] According to one embodiment of the present invention, there is provided a surface-treated copper foil having a treated surface on at least one side.

[0013] When a resin film is thermally pressed onto the treated surface to transfer the surface shape of the treated surface to the surface of the resin film, and the surface treated copper foil is removed by etching, the skewness Ssk measured according to ISO25178 on the surface of the remaining resin film is less than -0.6.

[0014] According to another aspect of the present invention, there is provided a copper foil with a carrier, comprising: a carrier; a release layer provided on the carrier; and the surface-treated copper foil provided on the release layer with the treated surface facing the outside.

[0015] According to another aspect of the present invention, there is provided a copper-clad laminate including the surface-treated copper foil or the copper foil with a carrier.

[0016] According to another aspect of the present invention, there is provided a printed wiring board obtained by using the surface-treated copper foil or the copper foil with a carrier.

[0017] According to another aspect of the present invention, there is provided a resin substrate having a skewness Ssk of -0.6 or less as measured in accordance with ISO 25178 on at least one surface thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a process flow chart for explaining the SAP method, and is a diagram showing the first half of the processes (process (a) to process (d)).

[0019] Figure 2 This is a process flow chart for explaining the SAP method, and is a diagram showing the latter half of the processes (process (e) to process (h)).

[0020] Figure 3A This is a diagram for explaining the skewness Ssk determined in accordance with ISO 25178, and is a diagram showing a surface and its height distribution when Ssk<0.

[0021] Figure 3B This is a diagram for explaining the skewness Ssk determined in accordance with ISO 25178, and is a diagram showing a surface and its height distribution when Ssk>0.

[0022] Figure 4This is a diagram for explaining the load curve and load area ratio determined in accordance with ISO25178.

[0023] Figure 5 This is a diagram for explaining the load area ratio Smr1 separating the protruding peak portion from the center portion and the load area ratio Smr2 separating the protruding valley portion from the center portion, which are determined in accordance with ISO25178.

[0024] Figure 6 This is a diagram for explaining the pole height Sxp determined in accordance with ISO25178.

[0025] Figure 7 This is a diagram for explaining the solid volume Vmc of the center portion determined in accordance with ISO25178.

[0026] Fig. 8A This is a process flow chart showing an example of circuit formation based on the MSAP method, and is a diagram for explaining the occurrence of circuit thinning.

[0027] Figure 8B This is a process flow chart showing an example of circuit formation by the SAP method and is a diagram for explaining the occurrence of a trap.

[0028] Fig. 9A Schematic cross-sectional views showing the states before and after the occurrence of sinking in a laminated body on which a circuit is formed on a resin-coated sample having small Ssk and Spc and large Spd and Vmc / Sxp.

[0029] Fig. 9B Schematic cross-sectional views showing the states before and after the occurrence of sinking in a laminated body on which a circuit is formed on a resin replica sample having large Ssk and Spc and small Spd and Vmc / Sxp.

[0030] Fig. 10A To show the extraction Fig. 9A A diagram showing a resin replica of a sample in a laminate and correction of the height of the convex portion.

[0031] Fig. 10B To show the extraction Fig. 9B A diagram showing a resin replica of a sample in a laminate and correction of the height of the convex portion.

[0032] Fig.11 It is a figure for demonstrating the measurement method of the penetration amount. DETAILED DESCRIPTION

[0033] definition

[0034] Definitions of terms and parameters used to define the present invention are shown below.

[0035] In this specification, "skewness Ssk" is a parameter that indicates the symmetry of the height distribution, measured in accordance with ISO25178. When this value is 0, it means that the height distribution is symmetrical in the upper and lower parts. Figure 3A As shown in , when the value is less than 0, it indicates a surface with many fine valleys. Figure 3B As shown in FIG. 1 , when the value is greater than 0, it indicates a surface with many fine peaks. The skewness Ssk can be measured by using a commercially available laser microscope to measure a predetermined measurement area (e.g., 57074.677 μm 2 It is calculated by the surface contour of the two-dimensional area.

[0036] In this specification, "arithmetic mean curvature Spc of the peak vertex" is a parameter that is measured in accordance with ISO25178 and represents the arithmetic mean of the principal curvatures of the peak vertices of the surface. A small value indicates that the point in contact with other objects has rounded corners. On the other hand, a large value indicates that the point in contact with other objects is sharp. In simple terms, the arithmetic mean curvature Spc of the peak vertex can be considered to be a parameter that represents the rounded corners of the protrusions that can be measured by a laser microscope. The arithmetic mean curvature Spc of the peak vertex can be measured by using a commercially available laser microscope to measure a specified measurement area (e.g., 57074.677 μm 2 It is calculated by the surface contour of the two-dimensional area.

[0037] In this specification, "peak vertex density Spd" is a parameter indicating the number of peak vertices per unit area measured in accordance with ISO25178. A larger value indicates a greater number of contact points with other objects. The peak vertex density Spd can be measured by using a commercially available laser microscope to measure a specified measurement area (e.g., 57074.677 μm 2 It is calculated by the surface contour of the two-dimensional area.

[0038] In this specification, the "surface load curve" (hereinafter referred to as "load curve") is a curve indicating the height of the load area ratio of 0% to 100% measured in accordance with ISO25178. Figure 4 As shown in Figure 2, the load area ratio is a parameter that represents the area of ​​a region above a certain height c. The load area ratio at height c is equivalent to Figure 4 Smr(c) in Figure 5As shown, along the load curve from the load area rate of 0%, take the load area rate difference set to 40% and draw the secant of the load curve, move the secant of the load curve from the load area rate of 0%, and the position where the slope of the secant is the most gentle is called the central part of the load curve. Relative to the central part, the straight line with the smallest sum of the squares of the deviations from the vertical axis direction is called the equivalent straight line. The part included in the range of heights of the load area rate of 0% to 100% of the equivalent straight line is called the central part. The part higher than the central part is called the protruding peak, and the part lower than the central part is called the protruding valley. The central part represents the height of the area in contact with other objects after the initial wear is completed.

[0039] like Figure 6 As shown, in this specification, "pole height Sxp" is a parameter indicating the height difference between the load area ratio p% and the load area ratio q% measured in accordance with ISO25178. Sxp represents the difference between the average surface of the surface and the peak of the surface after removing the particularly high peaks in the surface. In this specification, Sxp represents the difference in height between the load area ratio of 2.5% and the load area ratio of 50%. The pole height Sxp can be measured by using a commercially available laser microscope to measure a specified measurement area (e.g., 57074.677μm 2 It is calculated by the surface contour of the two-dimensional area.

[0040] like Figure 5 As shown in FIG. 1 , the “load area ratio Smr1 separating the protruding peak from the center” in this specification is a parameter indicating the load area ratio of the intersection of the height of the upper part of the center and the load curve measured in accordance with ISO 25178 (i.e., the load area ratio separating the center and the protruding peak). The larger the value, the larger the proportion of the protruding peak. In addition, as Figure 5 As shown, in this specification, "the load area ratio Smr2 separating the protruding valley and the center" is a parameter indicating the load area ratio of the intersection of the height of the lower part of the center and the load curve measured in accordance with ISO25178 (i.e., the load area ratio separating the center and the protruding valley). The larger the value, the larger the proportion of the protruding valley.

[0041] In this specification, the "central solid volume Vmc" is a parameter indicating the volume of the central part measured in accordance with ISO25178. Figure 7 As shown in FIG. 1 , Vmc represents the difference between the solid volume of the load area ratio Smr2 separating the protruding valley and the central part and the solid volume of the load area ratio Smr1 separating the protruding peak and the central part. The solid volume Vmc of the central part can be obtained by measuring a predetermined measurement area (e.g., 57074.677 μm) in the treated surface using a commercially available laser microscope. 2In this specification, the solid volume Vmc of the center portion is calculated by setting the load area ratio Smr1 separating the protruding peak and the center portion to 10% and the load area ratio Smr2 separating the protruding valley and the center portion to 80%.

[0042] In this specification, the "electrode surface" of the electrolytic copper foil refers to the surface on the side in contact with the cathode when the electrolytic copper foil is produced.

[0043] In this specification, the "deposition surface" of the electrolytic copper foil refers to the surface on the side where the electrolytic copper is deposited when the electrolytic copper foil is produced, that is, the surface on the side not in contact with the cathode.

[0044] Surface treated copper foil

[0045] The copper foil according to the present invention is a surface-treated copper foil. For the surface-treated copper foil, when a resin film is thermally pressed onto the treated surface to transfer the surface shape of the treated surface to the surface of the resin film, and the surface-treated copper foil is removed by etching, the skewness Ssk measured according to ISO25178 is less than -0.6 on the surface (hereinafter also referred to as the transfer surface) of the remaining resin film (hereinafter also referred to as the resin replica sample).

[0046] As mentioned above, with the demand for further miniaturization of circuits, the application of the SAP method, which is conducive to the formation of fine circuits, has expanded. In this regard, it can be said that as the circuit pattern width becomes narrower, the allowable indentation width is relatively reduced. That is, in a finer circuit pattern width (e.g., 10 μm), the allowable indentation width of the previous pattern width (e.g., 30 μm) may deviate from the standard due to reasons such as the increased risk of circuit collapse.

[0047] In addition, the SAP method is advantageous in terms of miniaturization of circuits compared to other methods such as the MSAP method, but is disadvantageous in terms of suppressing trapping. In this regard, for example, in circuit formation based on the MSAP method, Fig. 8A As illustrated, a laminate 110 is prepared in which a rust-proof layer 114 made of copper foil with a carrier and an electrolytic copper layer 116 are sequentially laminated on a resin substrate 112 (step (i)), and chemical copper plating 118 is formed with the electrolytic copper layer 116 remaining. Then, masking is performed with a dry film in a predetermined pattern, and then electrolytic copper plating is performed to form a wiring portion 120 (step (ii)). In this way, in the MSAP method, since the electrolytic copper layer 116 remains on the resin substrate 112, in the step of etching away the unnecessary portion between adjacent wiring portions 120, 120, the two layers of the electrolytic copper layer 116 and the chemical copper plating 118 must be removed by etching. Therefore, Fig. 8AAs shown in step (iii) of the method, the obtained wiring 122 is prone to circuit thinning. On the other hand, in the MSAP method, as described above, the electrolytic copper layer 116 is not completely removed, so the rust-proof layer 114 exists between the resin substrate 112 and the wiring 122, and the rust-proof layer 114 helps prevent the occurrence of sinking. In contrast, in the circuit formation based on the SAP method, Figure 8B As shown in the example, the following steps are performed in sequence: preparation of a laminate 110 having a rust-proof layer 114 and an electrolytic copper layer 116 formed in sequence on a resin substrate 112 (step (i)), complete removal of the electrolytic copper layer 116 (step (ii)), formation of chemical copper plating 118, masking by dry film, and formation of a wiring portion 120 by electrolytic copper plating (step (iii)). In this way, in the SAP method, no electrolytic copper layer 116 remains on the resin substrate 112, so in the etching step of the unnecessary portion between adjacent wiring portions 120, 120, only the chemical copper plating 118 is etched away, thereby suppressing the circuit thinning of the obtained wiring 122. On this basis, in the SAP method, an etching solution that can selectively remove chemical copper plating without removing electrolytic copper can be used, so that the thinning of the wiring 122, which is mostly composed of electrolytic copper, can be more effectively suppressed. Therefore, in terms of miniaturization of circuits, it can be said that the SAP method is advantageous compared to other methods such as the MSAP method. However, if Figure 8B As shown in step (iv) of the embodiment, the bottom of the wiring 122 formed by the SAP method is composed of the chemically plated copper 118. Therefore, when an etching solution that can selectively remove the chemically plated copper is used, the interface between the wiring 122 and the resin substrate 112 is easily sunken 124. In this regard, even when a surface-treated copper foil having an antirust layer 114 provided on an electrolytic copper layer 116 is used as a copper foil for SAP, since the electrolytic copper layer 116 is completely removed by etching in the SAP method, the antirust metal is also etched during the etching (see FIG. 1 ). Figure 8B Step (ii)). It should be noted that in Fig. 8A and 8B In the figure, the thickness of the rust-proof layer 114 is exaggerated for emphasis, but this does not necessarily reflect the actual thickness ratio in the laminate. Thus, in the SAP method, it is not easy to suppress the possible trapping in the circuit.

[0048] In this regard, by using the surface treated copper foil of the present invention in the SAP method, it is possible to impart a unique surface profile in which the skewness Ssk measured in accordance with ISO25178 is -0.6 or less to the surface of the resin substrate. As a result, in the etching process of the chemical copper plating layer, the occurrence of sinking that may occur in the circuit can be effectively suppressed. The mechanism by which the resin substrate surface has the above-mentioned surface profile and can suppress the sinking that occurs in the circuit has not yet been determined. As one of the reasons, the following reasons can be cited. That is, the convex portion of the surface of the resin substrate on which the circuit is to be formed (i.e., the transfer surface of the resin replica sample) functions as a protective wall to prevent the infiltration of the etching solution in the etching process of the chemical copper plating of the SAP method. Therefore, it can be said that the thicker the protective wall, the more difficult it is to sink. In this regard, based on the definition of the skewness Ssk mentioned above, as Fig. 9A and 9B As shown in FIG. 1 , it can be said that the resin replica sample 20 (refer to Fig. 9A ) and the resin replica sample 20 with large skewness Ssk (refer to Fig. 9B ) is thicker than the protrusion 20a (see the circled position in the figure). Therefore, it can be considered that by setting the skewness Ssk of the resin replica sample to a sufficiently small value of less than -0.6, the above-mentioned protective wall can be thickened, thereby effectively suppressing the sinking in the circuit 22.

[0049] From the above viewpoints, the surface treated copper foil of the present invention is preferably used for manufacturing a printed wiring board by the SAP method. In other words, the surface treated copper foil of the present invention is preferably used for transferring a concavo-convex shape to an insulating resin layer for a printed wiring board.

[0050] The surface treated copper foil of the present invention has a treated surface on at least one side. The treated surface is a surface that has been subjected to certain surface treatments, typically a roughened surface. The treated surface is typically formed with a plurality of protrusions (e.g., roughened particles). In either case, the surface treated copper foil may have treated surfaces (e.g., roughened surfaces) on both sides, or may have treated surfaces only on one side. In the case of having treated surfaces on both sides, when used in the SAP method, the surface on the laser irradiated side (the surface on the opposite side to the surface that is in close contact with the insulating resin) is also subjected to surface treatment, so that the laser absorbency is improved, and as a result, the laser permeability can also be improved.

[0051] For the surface treated copper foil of the present invention, when the surface shape of the treated surface is transferred to the surface of the resin film by hot pressing the resin film on the treated surface, and the surface treated copper foil is removed by etching, the skewness Ssk of the surface of the residual resin film (i.e., the transfer surface of the resin replica sample) is below -0.6, preferably above -1.7 and below -0.6, more preferably above -1.6 and below -0.7, further preferably above -1.5 and below -0.9, and particularly preferably above -1.5 and below -1.1. When it is within the above preferred range, the occurrence of sinking in the etching process of the SAP method can be further suppressed, and the protrusion of the treated surface of the surface treated copper foil can be controlled to a suitable shape that is not too slender, thereby effectively suppressing the occurrence of powder falling caused by bending, falling off, etc. of the protrusion of the surface treated copper foil. The resin film is preferably a thermosetting resin film, or it can be in the form of a prepreg. Examples of thermosetting resins include epoxy resins, cyanate resins, bismaleimide triazine resins (BT resins), polyphenylene ether resins, phenolic resins, polyimide resins, etc. Thermocompression bonding can be performed under conditions that allow the concavo-convex shape of the treated surface of the surface-treated copper foil to be transferred to the resin film, and is not particularly limited. For example, thermocompression bonding is preferably performed under conditions of a pressure of 3.0 MPa or more and 5.0 MPa or less, a temperature of 200° C. or more and 240° C. or less, and 60 minutes or more and 120 minutes or less.

[0052] For the surface-treated copper foil of the present invention, it is preferred that the arithmetic mean curvature Spc of the peak apex of the surface of the resin film remaining after etching (i.e., the transfer surface of the resin replica sample) is 5000 mm -1 Above and 13000mm -1 Below, more preferably 7000mm -1 Above and 13000mm -1 Below, more preferably 9000mm -1 Above and 13000mm -1 Below, particularly preferably 10000mm -1 Above and 13000mm -1 When the surface of the surface treated copper foil is within such a range, the protrusions on the treated surface of the surface treated copper foil can be controlled to an appropriate shape that is not too elongated, and the occurrence of powder falling caused by bending and falling of the protrusions of the surface treated copper foil can be effectively suppressed, and the occurrence of sinking in the etching process of the SAP method can be further suppressed. As one of the factors that can suppress the occurrence of sinking, the following reasons can be listed. That is, based on the definition of the arithmetic mean curvature Spc of the peak apex, as Fig. 9A and 9B As shown, the resin replica sample 20 (refer to Fig. 9A) and the arithmetic mean curvature Spc of the peak apex is greater than that of the resin replica sample 20 (reference Fig. 9B ) is compared to the top of the convex portion 20a. As a result, it is considered that the wall thickness of the convex portion 20a, which functions as a sinking protection wall, becomes thicker.

[0053] For the surface-treated copper foil of the present invention, the peak vertex density Spd of the surface of the resin film remaining after the etching (i.e., the transfer surface of the resin replica sample) is preferably 1.13×10 6 mm -2 Above and 1.50×10 6 mm -2 Below, more preferably 1.13×10 6 mm -2 Above and 1.40×10 6 mm -2 Below, more preferably 1.14×10 6 mm -2 Above and 1.30×10 6 mm -2 Below, particularly preferably 1.15×10 6 mm -2 Above and 1.20×10 6 mm -2 Below. Within such a range, the protrusions on the treated surface of the surface-treated copper foil can be controlled to an appropriate number, effectively suppressing the occurrence of powder falling, and further suppressing the occurrence of sinking in the etching process of the SAP method. That is, as mentioned above, the sinking of the circuit is prevented by the protrusions of the resin replica sample, so it can be said that the resin replica sample with a high frequency of protrusions can suppress the aggravation of sinking. In this regard, based on the definition of the peak vertex density Spd mentioned above, as Fig. 9A and 9B As shown, the resin replica sample 20 (refer to Fig. 9A ) and the resin replica sample 20 with a small peak density Spd (reference Fig. 9B ) compared to the convex portion 20a. Therefore, it can be considered that even if the sinking occurs, it can be prevented from being aggravated at an early stage.

[0054] For the surface-treated copper foil of the present invention, the solid volume Vmc (mL / m 2) relative to the peak height Sxp (μm) is preferably 0.39 or more and 0.44 or less, more preferably 0.39 or more and 0.43 or less, further preferably 0.39 or more and 0.42 or less, particularly preferably 0.39 or more and 0.41 or less, and most preferably 0.39 or more and 0.40 or less. Within such a range, the protrusions on the treated surface of the surface-treated copper foil can be controlled to be an appropriate shape that is not too elongated, and the occurrence of powder falling caused by bending, shedding, etc. of the protrusions of the surface-treated copper foil can be effectively suppressed, and the occurrence of sinking in the etching process of the SAP method can be further suppressed. On this basis, the adhesion between the substrate and the circuit can also be increased. That is, as mentioned above, the protrusions of the resin replica sample function as a protective wall to prevent the etching solution from penetrating. Based on the definition of the solid volume Vmc of the center portion, the larger the solid volume Vmc of the center portion, the larger the protrusions of the resin replica sample, and it can be said that sinking is further suppressed. On the other hand, based on the definition of the central part's solid volume Vmc and the extreme point height Sxp, as Fig. 10A and 10B As shown, the solid volume Vmc of the center portion also depends on the height of the protrusion 20a of the resin replica sample 20, so the size of the protrusion 20a can be evaluated by dividing the value of Vmc / Sxp by the extreme point height Sxp of the parameter related to the height of the protrusion 20a and comparing them. In addition, by increasing Vmc / Sxp (for example, 0.39 or more), the area of ​​the protrusion 20a of the resin replica sample 20 in which the circuit 22 is embedded will also increase (that is, the amount of resin surrounded and retained by the circuit 22 will increase), so that the adhesion between the substrate and the circuit will also increase by improving the anchoring effect.

[0055] Method for producing surface treated copper foil

[0056] An example of a preferred method for producing the surface-treated copper foil according to the present invention is described below. However, the surface-treated copper foil according to the present invention is not limited to the method described below, and any surface-treated copper foil produced by any method may be used as long as the above-mentioned surface profile can be given to the surface of the resin film.

[0057] (1) Preparation of copper foil

[0058] As the copper foil used in the manufacture of the surface-treated copper foil, both electrolytic copper foil and rolled copper foil can be used. The thickness of the copper foil is not particularly limited, preferably 0.1 μm or more and 18 μm or less, more preferably 0.5 μm or more and 10 μm or less, further preferably 0.5 μm or more and 7 μm or less, particularly preferably 0.5 μm or more and 5 μm or less, and most preferably 0.5 μm or more and 3 μm or less. When the copper foil is prepared in the form of a copper foil with a carrier, the copper foil can be formed by a wet film forming method such as a chemical copper plating method and an electrolytic copper plating method, a dry film forming method such as sputtering and chemical vapor deposition, or a combination thereof.

[0059] (2) Surface treatment (roughening)

[0060] At least one surface of the copper foil is roughened using copper particles. The roughening is performed by electrolysis using a copper electrolytic solution for roughening treatment. The electrolysis is preferably performed through a 2-stage or 3-stage plating process, and more preferably through a 3-stage plating process. In the first stage plating process, it is preferred to use a copper sulfate solution containing a copper concentration of 5 g / L or more and 20 g / L or less, a sulfuric acid concentration of 30 g / L or more and 200 g / L or less, a chlorine concentration of 20 mg / L or more and 100 mg / L or less, and a 9-phenylacridine (9PA) concentration of 20 mg / L or more and 80 mg / L or less, at a liquid temperature of 20°C or more and 40°C or less, and a current density of 5 A / dm 2 Above and 25A / dm 2 Electrodeposition is performed under the plating conditions of 2 seconds or less and 10 seconds or less. The plating process of the first stage can be performed twice in total using two tanks, but it is preferably completed once in total. In the plating process of the second stage, it is preferred to use a copper sulfate solution containing a copper concentration of 65 g / L or more and 80 g / L or less and a sulfuric acid concentration of 200 g / L or more and 280 g / L or less, at a liquid temperature of 45°C or more and 55°C or less, and a current density of 1 A / dm 2 Above and 10A / dm 2 In the third stage of the plating process, it is preferred to use a copper sulfate solution containing a copper concentration of 10 g / L to 20 g / L, a sulfuric acid concentration of 30 g / L to 130 g / L, a chlorine concentration of 20 mg / L to 100 mg / L, and a 9PA concentration of 100 mg / L to 200 mg / L, at a liquid temperature of 20°C to 40°C, a current density of 10 A / dm 2 Above and 40A / dm 2Electrodeposition is performed under the plating conditions of 0.3 seconds to 1.0 seconds or less. In particular, the first stage plating process is preferably performed using additives such as 9PA, and the total amount of electricity (Q1+Q2) of the first stage plating process and the second stage plating process Q1 and Q2 is preferably 100C / dm 2 In terms of uniformity of treatment and workability, the distance between the positive electrode and the negative electrode in the first stage of the plating step is preferably set to 45 mm or more and 90 mm or less, and more preferably 50 mm or more and 80 mm or less.

[0061] (3) Anti-rust treatment

[0062] According to the expectation, the copper foil after the roughening treatment can also be subjected to rust-proof treatment. The rust-proof treatment preferably includes a plating treatment using zinc. The plating treatment using zinc can be a zinc plating treatment or a zinc alloy plating treatment, and the zinc alloy plating treatment is particularly preferably a zinc-nickel alloy treatment. The zinc-nickel alloy treatment is a plating treatment containing at least Ni and Zn, and may further contain other elements such as Sn, Cr, and Co. The Ni / Zn adhesion ratio in the zinc-nickel alloy plating is preferably 1.2 or more and 10 or less in terms of mass ratio, more preferably 2 or more and 7 or less, and further preferably 2.7 or more and 4 or less. In addition, the rust-proof treatment preferably also includes a chromate treatment, and the chromate treatment is more preferably performed on the plated surface containing zinc after the zinc plating treatment. Thus, the rust resistance can be further improved. A particularly preferred rust-proof treatment is a combination of a zinc-nickel alloy plating treatment and a subsequent chromate treatment.

[0063] (4) Silane coupling agent treatment

[0064] As desired, the copper foil may be treated with a silane coupling agent to form a silane coupling agent layer. This can improve moisture resistance, chemical resistance, and adhesion to adhesives, etc. The silane coupling agent layer can be formed by appropriately diluting the silane coupling agent, applying it, and drying it. Examples of silane coupling agents include epoxy-functional silane coupling agents such as 4-glycidylbutyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane; or 3-aminopropyltriethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, N-3-(4-(3-aminopropoxy)butoxy)propyl-3-aminopropyltrimethoxysilane, N-phenyl ... Amino-functional silane coupling agents such as oxysilane; or mercapto-functional silane coupling agents such as 3-mercaptopropyltrimethoxysilane; or olefin-functional silane coupling agents such as vinyltrimethoxysilane and vinylphenyltrimethoxysilane; or acrylic-functional silane coupling agents such as 3-methacryloxypropyltrimethoxysilane; or imidazole-functional silane coupling agents such as imidazole silane; or triazine-functional silane coupling agents such as triazine silane, etc.

[0065] Copper foil with carrier

[0066] The surface-treated copper foil of the present invention can be provided in the form of a copper foil with a carrier. In this case, the copper foil with a carrier comprises: a carrier; a peeling layer provided on the carrier; and the surface-treated copper foil of the present invention provided on the peeling layer with the treated surface (typically the roughened surface) as the outer side. Of course, the copper foil with a carrier can adopt a known layer structure in addition to using the surface-treated copper foil of the present invention.

[0067] The carrier is a layer (typically a foil) for supporting the surface treated copper foil and improving its handling properties. Examples of the carrier include aluminum foil, copper foil, resin films coated with metal such as copper on the surface, glass plates, etc., preferably copper foil. The copper foil may be either rolled copper foil or electrolytic copper foil. The thickness of the carrier is typically 200 μm or less, preferably 12 μm or more and 35 μm or less.

[0068] The surface on the peeling layer side of the carrier preferably has a microscopic roughness ten-point height Rz of 0.5 μm or more and 1.5 μm or less, and more preferably 0.6 μm or more and 1.0 μm or less. Rz can be determined in accordance with JIS B 0601-1994. By giving such a microscopic roughness ten-point height Rz to the surface on the peeling layer side of the carrier in advance, it is easy to give a desired surface profile to the surface-treated copper foil of the present invention produced by sandwiching the peeling layer thereon.

[0069] The peeling layer is a layer having the following functions: weakening the peeling strength of the carrier, ensuring the stability of the strength, and further inhibiting the mutual diffusion that may occur between the carrier and the copper foil during press forming at high temperature. The peeling layer is usually formed on one side of the carrier, but it can also be formed on both sides. The peeling layer can be an organic peeling layer or an inorganic peeling layer. Examples of organic components used in the organic peeling layer include nitrogen-containing organic compounds, sulfur-containing organic compounds, carboxylic acids, etc. Examples of nitrogen-containing organic compounds include triazole compounds, imidazole compounds, etc., among which triazole compounds are preferred from the perspective of easy and stable peeling properties. Examples of triazole compounds include 1,2,3-benzotriazole, carboxybenzotriazole, N',N'-bis(benzotriazolemethyl)urea, 1H-1,2,4-triazole and 3-amino-1H-1,2,4-triazole, etc. Examples of sulfur-containing organic compounds include mercaptobenzothiazole, trithiocyanate, 2-benzimidazolethiol, etc. Examples of carboxylic acids include monocarboxylic acids and dicarboxylic acids. On the other hand, examples of inorganic components used in the inorganic release layer include Ni, Mo, Co, Cr, Fe, Ti, W, P, Zn, chromate-treated films, and the like. It should be noted that the formation of the release layer can be carried out by contacting at least one surface of the carrier with a solution containing a release layer component and fixing the release layer component on the surface of the carrier. The contact between the carrier and the solution containing the release layer component can be carried out by immersing the carrier in the solution containing the release layer component, spraying the solution containing the release layer component, or letting the solution containing the release layer component flow down. In addition, the fixation of the release layer component on the surface of the carrier can be carried out by adsorption, drying, or electrodeposition of the release layer component in the solution containing the release layer component. The thickness of the release layer is typically greater than 1 nm and less than 1 μm, preferably greater than 5 nm and less than 500 nm.

[0070] As the surface treated copper foil, the surface treated copper foil of the present invention is used. The roughening treatment of the present invention is implemented by roughening using copper particles, and as a step, a copper layer is first formed in the form of copper foil on the surface of the peeling layer, and then at least roughening is performed. The details of the roughening are as described above. It should be noted that the copper foil is preferably formed in the form of an ultra-thin copper foil in order to give full play to the advantages of the copper foil with a carrier. The preferred thickness of the ultra-thin copper foil is 0.1 μm or more and 7 μm or less, more preferably 0.5 μm or more and 5 μm or less, and further preferably 0.5 μm or more and 3 μm or less.

[0071] Another functional layer may be provided between the release layer and the carrier and / or the copper foil. As an example of such another functional layer, an auxiliary metal layer may be cited. The auxiliary metal layer is preferably formed of nickel and / or cobalt. The thickness of the auxiliary metal layer is preferably set to be greater than 0.001 μm and less than 3 μm.

[0072] Copper Clad Laminated Board

[0073] The surface-treated copper foil and / or copper foil with a carrier of the present invention are preferably used for the production of copper-clad laminates for printed circuit boards. That is, according to a preferred embodiment of the present invention, a copper-clad laminate having the above-mentioned surface-treated copper foil or the above-mentioned copper foil with a carrier is provided. By using the surface-treated copper foil of the present invention or the copper foil with a carrier, a copper-clad laminate particularly suitable for the SAP method can be provided. The copper-clad laminate comprises a surface-treated copper foil of the present invention and a resin layer tightly arranged on the roughening treatment surface of the surface-treated copper foil, or a copper foil with a carrier of the present invention and a resin layer tightly arranged on the roughening treatment surface of the surface-treated copper foil of the copper foil with a carrier. The surface-treated copper foil or the copper foil with a carrier can be arranged on a single side of the resin layer or on both sides. The resin layer comprises a resin, preferably an insulating resin. The resin layer is preferably a prepreg and / or a resin sheet. Prepreg refers to a general term for composite materials obtained by impregnating a synthetic resin into a substrate such as a synthetic resin plate, a glass plate, a glass woven fabric, a glass nonwoven fabric, or paper. As preferred examples of insulating resins, epoxy resins, cyanate resins, bismaleimide triazine resins (BT resins), polyphenylene ether resins, phenolic resins, etc. can be cited. In addition, as examples of insulating resins constituting resin sheets, insulating resins such as epoxy resins, polyimide resins, and polyester resins can be cited. In addition, from the viewpoint of improving the insulation of the resin layer, filler particles formed by various inorganic particles such as silica and alumina can also be contained. The thickness of the resin layer is not particularly limited, preferably 1 μm or more and 1000 μm or less, more preferably 2 μm or more and 400 μm or less, and further preferably 3 μm or more and 200 μm or less. The resin layer can be composed of multiple layers. Resin layers such as prepregs and / or resin sheets can also be arranged on the surface-treated copper foil or the copper foil with a carrier by sandwiching a primer resin layer pre-coated on the roughened surface of the surface-treated copper foil.

[0074] Printed Circuit Board

[0075] The surface treated copper foil and / or copper foil with a carrier of the present invention is preferably used for the production of printed circuit boards, and is particularly preferably used for the production of printed circuit boards based on a semi-additive process (SAP). That is, according to a preferred embodiment of the present invention, a method for producing a printed circuit board characterized in that the printed circuit board is produced using the aforementioned surface treated copper foil or the aforementioned copper foil with a carrier, or a printed circuit board obtained using the aforementioned surface treated copper foil or the aforementioned copper foil with a carrier can be provided. By using the surface treated copper foil and / or copper foil with a carrier of the present invention, the above-mentioned surface profile can be given to the laminate, and in the etching process which is one of the processes in the production of the printed circuit board, sinking can be effectively suppressed. The printed circuit board based on this method includes a layer structure obtained by laminating a resin layer and a copper layer. In the case of the SAP method, the surface treated copper foil of the present invention is Figure 1 The surface treated copper foil of the present invention is removed in the process (c), so the printed circuit board made by the SAP method no longer contains the surface treated copper foil of the present invention, and only the surface profile transferred from the roughened surface of the surface treated copper foil remains. In addition, the copper-clad laminated board with the resin layer is as described above. In short, the printed circuit board can adopt a known layer structure. As a specific example involving a printed circuit board, there can be listed: a single-sided or double-sided printed circuit board in which a laminate is made by bonding and curing the surface treated copper foil of the present invention and / or the copper foil with a carrier on one or both sides of the prepreg, and a circuit is formed on this basis, and a multilayer printed circuit board formed by multilayering them, etc. In addition, as other specific examples, flexible printed circuit boards, COFs, TAB tapes, etc. in which the surface treated copper foil of the present invention and / or the copper foil with a carrier are formed on a resin film and a circuit is formed. As other specific examples, there are: a resin-coated copper foil (RCC) formed by coating the above-mentioned resin layer on the surface-treated copper foil and / or the copper foil with a carrier of the present invention, after laminating the resin layer as an insulating adhesive material layer on the above-mentioned printed circuit board, using the surface-treated copper foil as all or part of the wiring layer, and forming a circuit by a modified semi-additive (MSAP) method, a subtractive method, etc.; a laminated wiring board in which the surface-treated copper foil is removed and a circuit is formed by a semi-additive (SAP) method; a direct build-up on wafer in which the lamination of the resin-coated copper foil and the formation of the circuit are repeated alternately on a semiconductor integrated circuit, etc. As further specific examples, there are: an antenna element obtained by laminating the above-mentioned resin-coated copper foil on a substrate and forming a circuit, an electronic material for a panel / display in which a pattern is formed by laminating on a glass or a resin film via an adhesive layer, an electronic material for window glass, an electromagnetic wave shielding body / film obtained by coating a conductive adhesive on the surface-treated copper foil of the present invention, etc. The surface treated copper foil and / or the copper foil with carrier of the present invention is particularly suitable for the SAP method. For example, when forming a circuit by the SAP method, the following method can be used: Figure 1 and 2The composition shown.

[0076] Resin base material

[0077] According to a preferred embodiment of the present invention, a resin substrate having a skewness Ssk of at least one surface measured according to ISO25178 of less than -0.6 is provided. The resin substrate is equivalent to a resin replica sample of the surface shape of the surface-treated copper foil of the present invention transferred. Therefore, the preferred embodiment of the resin replica sample of the surface shape of the surface-treated copper foil transferred (skewness Ssk, arithmetic mean curvature Spc of the peak vertex, peak vertex density Spd, and each parameter of the ratio Vmc / Sxp of the solid volume Vmc of the center relative to the pole height Sxp) is also directly applicable to the resin substrate of this embodiment. The resin substrate comprises a resin, preferably an insulating resin. The resin substrate is preferably a prepreg and / or a resin sheet. Prepreg refers to a general term for a composite material obtained by impregnating a substrate such as a synthetic resin plate, a glass plate, a glass woven fabric, a glass non-woven fabric, and paper with a synthetic resin. As preferred examples of insulating resins, epoxy resins, cyanate resins, bismaleimide triazine resins (BT resins), polyphenylene ether resins, phenolic resins, etc. can be cited. In addition, as examples of insulating resins constituting the resin substrate, insulating resins such as epoxy resins, polyimide resins, and polyester resins can be cited. In addition, from the viewpoint of improving insulation, the resin substrate may also contain filler particles formed by various inorganic particles such as silica and alumina. The thickness of the resin substrate is not particularly limited, and is preferably 1 μm or more and 1000 μm or less, more preferably 2 μm or more and 400 μm or less, and further preferably 3 μm or more and 200 μm or less. The resin substrate may also be composed of a plurality of layers. The resin substrate of the present invention can be preferably used as a starting material or an intermediate product in the manufacture of a printed circuit board based on the SAP method.

[0078] Example

[0079] The present invention is further described in detail by the following examples.

[0080] Examples 1 to 6

[0081] The copper foil with carrier and the resin replica samples were prepared and evaluated as follows.

[0082] (1) Preparation of carrier

[0083] As the cathode, a titanium electrode whose surface was polished with a #2000 polishing wheel was prepared. In addition, as the anode, a DSA (dimensional stability anode) was prepared. These electrodes were immersed in a copper sulfate solution with a copper concentration of 80 g / L and a sulfuric acid concentration of 260 g / L, and the solution temperature was 45°C and the current density was 55 A / dm 2Electrolysis was performed under the condition of 100 ℃ to obtain an electrolytic copper foil with a thickness of 18 μm as a carrier.

[0084] (2) Formation of the peeling layer

[0085] The electrode surface side of the acid-washed support was immersed in a CBTA (carboxybenzotriazole) aqueous solution having a CBTA concentration of 1 g / L, a sulfuric acid concentration of 150 g / L, and a copper concentration of 10 g / L at a liquid temperature of 30° C. for 30 seconds to allow the CBTA component to be adsorbed on the electrode surface of the support. In this way, a CBTA layer as an organic release layer was formed on the surface of the electrode surface of the support.

[0086] (3) Formation of auxiliary metal layer

[0087] The support with the organic release layer formed thereon was immersed in a solution of nickel sulfate with a nickel concentration of 20 g / L and the mixture was stirred at a temperature of 45°C, a pH of 3, and a current density of 5 A / dm 2 Under the conditions of , nickel was deposited on the organic release layer in an amount corresponding to a thickness of 0.001 μm. In this way, a nickel layer as an auxiliary metal layer was formed on the organic release layer.

[0088] (4) Ultra-thin copper foil formation

[0089] The support with the auxiliary metal layer was immersed in a copper sulfate solution with a copper concentration of 60 g / L and a sulfuric acid concentration of 200 g / L at a solution temperature of 50°C and a current density of 5 A / dm 2 Above and 30A / dm 2 Next, electrolysis was performed to form an ultra-thin copper foil having a thickness of 1.2 μm on the auxiliary metal layer.

[0090] (5) Roughening treatment

[0091] The precipitation surface of the above-mentioned ultra-thin copper foil is roughened. In the roughening treatment, the plating of the first stage is carried out twice. In the plating process of each stage, a copper sulfate solution having a copper concentration, a sulfuric acid concentration, a chlorine concentration and a 9-phenylacridine (9PA) concentration shown in Table 1 is used, and the electrodeposition is carried out at the liquid temperature shown in Table 1 and the current density and time shown in Table 2. In the plating treatment of the first stage, the distance between the positive electrode and the negative electrode is set to be greater than 50 mm and less than 80 mm. In this way, 6 kinds of roughened copper foils of Examples 1 to 6 are prepared.

[0092] [Table 1]

[0093] Table 1

[0094]

[0095] [Table 2]

[0096]

[0097] (6) Anti-rust treatment

[0098] The surface of the roughened copper foil with carrier was subjected to rust prevention treatment consisting of zinc-nickel alloy plating and chromate treatment. First, an electrolyte solution with a zinc concentration of 0.2 g / L, a nickel concentration of 2 g / L, and a potassium pyrophosphate concentration of 300 g / L was used at a liquid temperature of 40°C and a current density of 0.5 A / dm 2 The surface of the roughened layer and the carrier was plated with zinc-nickel alloy. Then, a 1 g / L aqueous solution of chromic acid was used at pH 11, liquid temperature 25°C, and current density 1 A / dm 2 The surface treated with zinc-nickel alloy plating was chromated under the conditions of .

[0099] (7) Silane coupling agent treatment

[0100] The silane coupling agent treatment was performed by adsorbing an aqueous solution containing 3 g / L 3-aminopropyltrimethoxysilane on the surface of the copper foil side of the copper foil with a carrier, and evaporating the water with an electric heater. At this time, the silane coupling agent treatment was not performed on the carrier side.

[0101] (8) Fabrication of copper-clad laminates

[0102] A copper-clad laminate was made using a copper foil with a carrier. First, a BT resin prepreg (manufactured by Mitsubishi Gas Chemical Co., Ltd., GHPL-830NS, thickness 0.1 mm) as a resin film was sandwiched on the surface of the inner substrate, and an ultra-thin copper foil with a carrier was laminated, and after thermocompression bonding at a pressure of 4.0 MPa and a temperature of 220° C. for 90 minutes, the carrier was peeled off to make a copper-clad laminate.

[0103] (9) Preparation of resin replica specimens

[0104] The copper foil on the surface of the copper-clad laminate was completely removed using a sulfuric acid / hydrogen peroxide-based etching solution to obtain a resin replica sample.

[0105] (10) Surface profile measurement of resin replica specimens

[0106] The transfer surface of the resin replica sample (the surface to which the surface profile of the roughened surface is transferred) was measured by surface roughness analysis using a laser microscope (VK-X100 manufactured by KEYENCE Co., Ltd.) in accordance with ISO 25178. Specifically, the transfer surface of the resin replica sample with an area of ​​57074.677 μm was measured using the laser microscope at an objective magnification of 50 times. 2The surface profile of the area. After the surface profile of the transfer surface of the obtained resin replication sample is subjected to surface tilt correction (automatic) as a pre-processing, it is analyzed by laser method to calculate various parameters (skewness Ssk, arithmetic mean curvature Spc of the peak vertex, peak vertex density Spd, and the ratio of the solid volume Vmc of the center to the pole height Sxp Vmc / Sxp). At this time, the S filter and L filter are not used to measure the numerical value. The above operation is performed 3 times for each example, and the average value is used as the value of each parameter in each example. The results are shown in Table 3.

[0107] (11) Preparation of laminate for SAP evaluation

[0108] The resin replica sample was degreased, provided with a Pd-based catalyst, and activated. Thus, the activated surface was electrolessly plated with copper (thickness: 1 μm) to obtain a laminate before the dry film was attached in the SAP method (hereinafter referred to as a laminate for SAP evaluation). These steps were performed under the known conditions of the SAP method.

[0109] (12) Evaluation of laminate for SAP evaluation

[0110] The SAP evaluation laminate obtained above was evaluated for various properties as follows.

[0111] <Falling into Evaluation>

[0112] A dry film is adhered to the surface of the SAP evaluation laminate, and exposure, dry film removal, and electrolytic plating are performed to form a circuit with a circuit width of 22μm, a height of 22μm, and a length of 150μm (at this stage, the lower part of each circuit is electrically connected through a chemical copper plating layer). The resulting circuit is treated with an etching solution (manufactured by JCU CORPORATION, SAC-700W3C) to dissolve and remove the chemical copper plating layer remaining between the circuits, thereby insulating the circuits. Regarding the etching amount at this time, the etching rate of the copper foil is measured in advance, and the etching is performed under the condition of so-called over-etching that further etches 4μm beyond the so-called appropriate etching. After the etching process, the circuit is washed with water and dried. Using an optical microscope, the cross-section of the circuit is observed to determine the amount of sinking. Specifically, as Fig.11 As shown in FIG. 3 , the upper width x (μm) and the lower width y (μm) of the circuit 22 formed on the resin replica sample 20 were measured, and the difference (xy) was taken as the sinking amount (μm). Each example was measured in two fields of view, and the average value was taken as the sinking amount of each example. The results are shown in Table 3.

[0113] <Plating circuit adhesion (peel strength)>

[0114] A dry film was attached to the SAP evaluation laminate, and then exposed and developed. The copper layer was precipitated from the laminate masked by the dry film by pattern plating, and then the dry film was peeled off. The precipitated chemical copper plating was removed with an etching solution (SAC-700W3C made by JCU CORPORATION), and a peel strength measurement sample with a height of 20 μm and a width of 10 mm was prepared. According to JIS C 6481 (1996), the peel strength when the copper layer was peeled off from the evaluation sample was measured. The results are shown in Table 3.

[0115] [Table 3]

[0116] Table 3

[0117]

[0118] * indicates a comparative example.

[0119] According to Table 3, although the value of Vmc / Sxp is large in Example 5, the peel strength does not increase accordingly. As for the reason, "powder falling" is considered to be one of the reasons. That is, when powder falling occurs, the anchoring effect can no longer be obtained, and a tendency of reduced peel strength can be observed. When Vmc / Sxp is too large, powder falling occurs. It is believed that slight powder falling occurred in Example 5, resulting in a lower peel strength.

Claims

1. A surface-treated copper foil having a treated surface on at least one side, When a resin film is bonded to the treated surface by thermocompression to transfer the surface shape of the treated surface to the surface of the resin film, and the surface treated copper foil is removed by etching, the skewness Ssk measured in accordance with ISO25178 on the surface of the remaining resin film is -0.6 or less, The resin film is a bismaleimide triazine resin prepreg, The thermal compression bonding was performed under the conditions of a pressure of 4.0 MPa, a temperature of 220° C., and 90 minutes.

2. The surface-treated copper foil according to claim 1, wherein The skewness Ssk is greater than or equal to -1.7 and less than or equal to -0.

6.

3. The surface-treated copper foil according to claim 1 or 2, wherein The arithmetic mean curvature Spc of the peak apex of the surface of the resin film remaining after the etching, measured in accordance with ISO25178, is 5000 mm -1 Above and 13000mm -1 the following.

4. The surface-treated copper foil according to claim 1 or 2, wherein The peak top density Spd of the surface of the resin film remaining after the etching, measured in accordance with ISO25178, was 1.13×10 6 mm -2 Above and 1.50×10 6 mm -2 the following.

5. The surface-treated copper foil according to claim 1 or 2, wherein A ratio Vmc / Sxp of a substantial volume Vmc of a center portion of the surface of the resin thin film remaining after the etching measured in accordance with ISO 25178 to a peak height Sxp measured in accordance with ISO 25178 is greater than or equal to 0.39 and less than or equal to 0.

44. 6 . The surface-treated copper foil according to claim 1 , which is used for transferring a concavo-convex shape to an insulating resin layer for a printed wiring board.

7. The surface-treated copper foil according to claim 1 or 2, which is used for the production of printed circuit boards based on a semi-additive process (SAP). 8 . A copper foil with a carrier, comprising: a carrier; a release layer provided on the carrier; and the surface-treated copper foil according to claim 1 provided on the release layer with the treated surface facing the outside. 9 . A copper-clad laminate comprising the surface-treated copper foil according to claim 1 or the copper foil with a carrier according to claim 8 . 10 . A printed wiring board obtained by using the surface-treated copper foil according to claim 1 or the copper foil with a carrier according to claim 8 .

11. A method for manufacturing a printed circuit board, characterized in that: A printed wiring board is produced using the surface-treated copper foil according to any one of claims 1 to 7 or the copper foil with a carrier according to claim 8.

Citation Information

Patent Citations

  • Surface-treated copper foil and laminated board using same

    CN104603333A

  • Metal material for printed circuit board

    JP2006339304A