Toner and two-component developer
By using a combination of crystalline and non-crystalline resins in the toner and adding inorganic fine particles to the particle surface to form a domain-matrix structure, the problem of poor charge stability under high temperature and high humidity conditions is solved, achieving rapid charge rise and low temperature fixing, adapting to the image requirements of different printing rates.
Patent Information
- Application Number
- CN202011454471.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-13
- Filing Date
- 2020-12-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-12-10
AI Technical Summary
Existing toners have poor electrical stability in high temperature and high humidity environments, leading to variations in image density. This is especially true when a high-print-rate image is followed immediately by a low-print-rate image, resulting in uneven image density due to the difference in charge between the existing toner and the new toner in the developing unit.
By employing a binder resin combination containing both crystalline and non-crystalline resins, and by adding inorganic fine particles to the surface of the toner particles and controlling the acid value and resistivity of the resin, a domain-matrix structure is formed to improve the charge rise rate and stability.
It achieves electrical stability and rapid charge rise in high temperature and high humidity environments, reduces image density changes, improves the low temperature fixing and heat-resistant stain resistance of toners, and adapts to the image requirements of different printing rates.
Smart Images

Figure BDA0002828042330000031 
Figure BDA0002828042330000032 
Figure BDA0002828042330000051
Abstract
Description
Technical Field
[0001] The present disclosure relates to a toner used in an electrophotographic system, an electrostatic recording system, an electrostatic printing system, and a toner jetting system, and a two-component developer using the toner. Background Art
[0002] With the popularity of full-color electrophotographic copiers in recent years, there has been an increasing demand for high-speed printing and high energy saving. In order to achieve high-speed printing, a technology for melting toner more quickly in the fixing step has been studied. A technology for shortening various control times within and between jobs has been studied to improve productivity. As an energy-saving strategy, a technology for fixing toner at low temperatures has been studied to reduce energy consumption in the fixing step.
[0003] A method for achieving high-speed printing while improving the low-temperature fixability of a toner includes lowering the glass transition temperature or softening point of a binder resin in the toner and using a binder resin having rapid melting properties. In recent years, many toners containing crystalline polyesters as resins having rapid melting properties have been proposed. However, crystalline polyesters have problems with charging stability in a high-temperature and high-humidity environment, particularly problems with maintaining charging performance after being left in a high-temperature and high-humidity environment.
[0004] Various toners using a crystalline vinyl resin as other crystalline resin having a sharp melting property have also been proposed.
[0005] For example, Japanese Patent Application Laid-Open No. 2013-097321 proposes a toner that achieves both low-temperature fixability and charging stability by using an acrylic resin having crystallinity.
[0006] Japanese Patent Application Laid-Open No. 2017-58604 proposes a toner that achieves both low-temperature fixability and charging uniformity by using a binder resin including a non-crystalline vinyl resin chemically linked to a crystalline vinyl resin.
[0007] In addition, WO 2019 / 073731 proposes a toner using a binder resin combining a crystalline vinyl resin and a polyester resin cross-linked by a carbon-carbon bond. Summary of the invention
[0008] The toners of these patent documents can provide some improvement in low temperature fixability and charge stability, which has been a weak point of toners using crystalline polyester resins. However, it has been found that these toners using crystalline vinyl resins as binder resins have slow charge rising.
[0009] For this reason, it has been found that when an image with a small print rate is printed immediately after an image with a large print rate is printed, the image density changes gradually due to the difference in charge amount between the toner existing in the developing device and the new toner supplied to the developing device. This tendency is particularly noticeable in a low humidity environment.
[0010] The present disclosure provides a toner having both low-temperature fixing property and hot offset resistance as well as charging stability and rapid charging rise in a high-temperature and high-humidity environment, and further, showing resistance to density fluctuation regardless of image printing rate, and also provides a two-component developer using the toner.
[0011] A toner comprising:
[0012] Toner particles containing a binder resin including a first resin and a second resin; and
[0013] The inorganic fine particles on the surface of the toner particles, wherein
[0014] The first resin is a crystalline resin,
[0015] The second resin is a non-crystalline resin,
[0016] The first resin has a first monomer unit represented by the following formula (1),
[0017] The content ratio of the first monomer unit in the first resin is 30.0 mass % to 99.9 mass %,
[0018] The acid value of the first resin is 0.1 mg KOH / g to 30 mg KOH / g,
[0019] The acid value of the second resin is 0.5 mg KOH / g to 40 mg KOH / g,
[0020] A domain-matrix structure formed of a matrix containing the first resin and domains containing the second resin appears in cross-sectional observation of the toner,
[0021] A compound having an alkyl group is present on the surface of the inorganic fine particles, and
[0022] The volume resistivity of inorganic fine particles is 1.0×10 5 Ω·cm to 1.0×10 13 Ω·cm:
[0023] In the following formula (1), R Z1 represents a hydrogen atom or a methyl group, and R represents C 18-36 alkyl.
[0024]
[0025] The present disclosure can provide a toner which has both low-temperature fixing property and hot offset resistance as well as charging stability and rapid charging rise in a high-temperature and high-humidity environment, and furthermore, which shows resistance to density fluctuation regardless of image printing rate.
[0026] Further features of the present invention will become apparent from the following description of exemplary embodiments. DETAILED DESCRIPTION
[0027] Unless otherwise stated, the description of a numerical range in the present disclosure, such as "from X to Y" or "X to Y", includes the numerical values at the upper and lower limits of the range.
[0028] In the present disclosure, (meth)acrylate refers to acrylate and / or methacrylate.
[0029] When numerical ranges are described in stages, each upper and lower limit of each numerical range can be combined arbitrarily.
[0030] The term "monomer unit" describes the reaction form of a monomer material in a polymer. For example, a carbon-carbon bond in the main chain of a polymerized vinyl monomer in a polymer is considered a unit. A vinyl monomer can be represented by the following formula (Z):
[0031]
[0032] [In (Z), R Z1 represents a hydrogen atom or an alkyl group (preferably C 1-3 alkyl, or more preferably methyl), and R Z2 represents any substituent].
[0033] The crystalline resin is a resin that shows a clear endothermic peak in differential scanning calorimetry (DSC) measurement.
[0034] The present inventors consider that the mechanism by which the effects of the present invention are produced is as follows.
[0035] It is believed that the charge increase speed of the toner is determined by the speed at which the charge is transferred from the inorganic fine particles on the surface of the toner particles to the surface of the toner particles and saturated on the entire toner particles. Generally, low resistivity inorganic fine particles such as titanium oxide have been used to increase the charge transfer speed from the inside of the inorganic fine particles, thereby increasing the charge increase speed of the toner.
[0036] However, the present inventors' studies have revealed that when a crystalline vinyl resin is used as a binder resin, the charge rise speed is not sufficiently increased by itself. This is considered to be because the charge transfer from the inorganic fine particles to the toner particle surface is limited.
[0037] As a result of studying different compositions of the binder resin, it was found that the use of a crystalline resin having a monomer with an acid value resulted in an increase in charge rise. The inventors believe that the use of a monomer having an acid value allows charge transfer to be faster due to the presence of an electric dipole caused by charge localization. However, with certain compositions, low-temperature fixability and hot offset resistance are reduced.
[0038] The present inventors subsequently discovered, as a result of intensive studies, that these problems can be solved by controlling the states of the crystalline resin and the non-crystalline resin in the toner, the acid value of the crystalline resin, the acid value of the non-crystalline resin, and the resistivity and surface treatment of the inorganic fine particles on the toner surface within specific ranges.
[0039] In these disclosures, a domain-matrix structure consisting of a matrix (sea portion) containing a first resin as a crystalline resin and a domain (island portion) containing a second resin as a non-crystalline resin appears in cross-sectional observation of the toner. When such a domain-matrix structure is formed, the fixing temperature range of the toner can be greatly extended.
[0040] Since the matrix (sea portion) is composed of a crystalline resin and the domain (island portion) is composed of a non-crystalline resin in the domain-matrix structure of the toner cross section, excellent low-temperature fixability is achieved.
[0041] On the other hand, in the case where the crystalline resin and the non-crystalline resin are blended together without forming a uniform structure of a domain-matrix structure, since the rapid melting property of the crystalline resin is lost, the low-temperature fixability is reduced. In addition, if the toner has a structure in which the matrix is composed of a non-crystalline resin and the domain is composed of a crystalline resin, the rapid melting property of the crystalline resin cannot be fully obtained, and since the crystalline resin controls the melting property, the low-temperature fixability is reduced.
[0042] Preferably, the matrix is exposed on at least a portion of the toner particle surface, and at least a portion of the inorganic fine particles is in contact with the exposed portion of the matrix.
[0043] The first resin is a crystalline resin having a first monomer unit represented by formula (1).
[0044] The content ratio of the first monomer unit in the first resin is 30.0 mass % to 99.9 mass %. The acid value of the first resin is 0.1 mg KOH / g to 30 mg KOH / g. Since the first resin has such a first monomer unit, the binder resin has crystallinity and the low temperature fixability of the toner is improved.
[0045] When the content ratio of the first monomer unit in the first resin is 30.0% by mass to 99.9% by mass, low-temperature fixability and charge increase in a low-humidity environment are good.
[0046] If the content ratio of the first monomer unit is less than 30.0% by mass, the low temperature fixability is reduced. The range is more preferably 40.0% to 90.0% by mass, or even more preferably 45.0% to 75.0% by mass. If the content ratio of the first monomer unit exceeds 99.9% by mass, since most of the first resin can be occupied by the non-polar part having a low SP value, the charge rise performance in a low humidity environment will be reduced.
[0047] The acid value of the first resin (crystalline resin) is 0.1 mg KOH / g to 30 mg KOH / g. If the acid value is within this range, the charge-raising performance of the toner is improved because the toner particle surface more easily receives the charge from the inorganic fine particles.
[0048] If the acid value of the first resin is less than 0.1 mg KOH / g, the charge transfer from the inorganic fine particles to the surface of the toner particles is not smooth, so the effect of improving the charging performance of the toner cannot be obtained. If the acid value of the first resin exceeds 30 mg KOH / g, the hydrophobicity of the surface of the toner particles becomes lower, so the charging maintenance performance in a high humidity environment is reduced. More preferably, the acid value is in the range of 5 mg KOH / g to 15 mg KOH / g.
[0049]
[0050] [In formula (1), R Z1 represents a hydrogen atom or a methyl group, and R represents C 18-36 Alkyl (preferably C 18-30 Straight chain alkyl).]
[0051] The first monomer unit represented by formula (1) is preferably derived from a monomer selected from 18-36 The monomer unit is at least one monomer unit selected from the group consisting of alkyl (meth)acrylates.
[0052] Each has C 18-36 Examples of the alkyl (meth)acrylates include 18-36 (meth)acrylates of linear alkyl groups [(stearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, heneicosyl (meth)acrylate, docosyl (meth)acrylate, tetracosyl (meth)acrylate, hexacosyl (meth)acrylate, octacosyl (meth)acrylate, triacontyl (meth)acrylate, triacontyl (meth)acrylate, etc.] and each having C 18-36 Branched alkyl (meth)acrylates [2-decyltetradecyl (meth)acrylate, etc.].
[0053] Among them, from the viewpoint of low temperature fixing property, charging rise performance and charging stability of the toner, it is preferable to select 18-36 At least one (meth)acrylate of a linear alkyl group, more preferably selected from 18-30 At least one kind of linear alkyl (meth)acrylate, and still more preferably at least one kind selected from linear stearyl (meth)acrylate and behenyl (meth)acrylate.
[0054] One monomer may be used alone or a combination of at least two monomers may be used to form the first monomer unit.
[0055] The first resin is preferably a vinyl polymer. The vinyl polymer may be, for example, a polymer of a monomer containing an ethylenically unsaturated bond. An ethylenically unsaturated bond is a free radical polymerizable carbon-carbon double bond, and examples include vinyl, acryl, acryl, and methacryloyl.
[0056] The first resin preferably has a second monomer unit different from the first monomer unit and is at least one selected from the group consisting of a monomer unit represented by the following formula (2) and a monomer unit represented by the following formula (3).
[0057] The content ratio of the second monomer unit in the first resin is preferably 1.0% by mass to 70.0% by mass, or more preferably 10.0% by mass to 60.0% by mass, or still more preferably 15.0% by mass to 30.0% by mass.
[0058]
[0059] (In formula (2), X represents a single bond or C 1-6 Alkylene,
[0060] R 1 represents a nitrile group (-C≡N),
[0061] Amide (-C(=O)NHR 10 (where R 10 Represents a hydrogen atom or C 1-4 alkyl)),
[0062] Hydroxyl,
[0063] -COOR 11 (where R 11 Represents C 1-6 (Preferred C 1-4 ) alkyl or C 1-6 (Preferred C 1-4 )hydroxyalkyl),
[0064] Urea (-NH-C(=O)-N(R 13 )2(Two R 13independently represent hydrogen atoms or C 1-6 (Preferred C 1-4 )alkyl)),
[0065] -COO(CH2)2NHCOOR 14 (where R 14 Represents C 1-4 alkyl) or
[0066] -COO(CH2)2-NH-C(=O)-N(R 15 )2(Two R 15 independently represent hydrogen atoms or C 1-6 (Preferred C 1-4 )alkyl), and
[0067] R 2 represents a hydrogen atom or a methyl group. )
[0068] (In formula (3), R 3 Represents C 1-4 Alkyl and R 4 represents a hydrogen atom or a methyl group. )
[0069] Given SP 21 SP value as the second monomer unit (J / cm 3 ) 0.5 From the perspective of charging performance, SP 21 It is preferably 21.00 or more, or more preferably 25.00 or more. The upper limit is not particularly limited, but is preferably 40.00 or less, or more preferably 30.00 or less.
[0070] If the SP value of the second monomer unit is within this range, charge transfer from the inorganic fine particles occurs rapidly, and the charge rise speed of the toner increases.
[0071] The content ratio of the first resin (crystalline resin) in the binder resin is preferably 30.0% by mass or more.
[0072] Within this range, since a domain-matrix structure consisting of a matrix containing the first resin and a domain containing the second resin is easily formed, both low temperature fixability and hot offset resistance can be achieved. The content is more preferably 50.0% by mass or more, or still more preferably 55.0% by mass or more.
[0073] The upper limit is not particularly limited, but is preferably 97.0% by mass or less, or more preferably 75.0% by mass or less.
[0074] The content of the second resin (non-crystalline resin) in the binder resin is preferably 3.0% by mass or more, or more preferably 25.0% by mass or more. The upper limit is preferably 70.0% by mass or less, or more preferably 50.0% by mass or less, or still more preferably 40.0% by mass or less.
[0075] One feature is that the acid value of the second resin (non-crystalline resin) is 0.5 mg KOH / g to 40 mg KOH / g. Within this range, the toner particle surface easily receives charge from the inorganic fine particles, and the charge rise performance of the toner is improved.
[0076] If the acid value of the second resin is less than 0.5 mg KOH / g, the charge transfer from the inorganic fine particles to the surface of the toner particles is not smooth, so the effect of improving the charge raising performance of the toner cannot be obtained. If the acid value of the second resin exceeds 40 mg KOH / g, the hydrophobicity of the surface of the toner particles is low, so the charge maintenance performance in a high humidity environment is reduced. The acid value is more preferably 1 mg KOH / g to 30 mg KOH / g, or more preferably 6 mg KOH / g to 25 mg KOH / g, or further more preferably from 3 mg KOH / g to 20 mg KOH / g.
[0077] Examples of the second resin include the following resins: single polymers of styrene and substituted styrenes, such as poly-p-chlorostyrene and polyvinyltoluene; styrene-based copolymers, such as styrene-p-chlorostyrene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-acrylate copolymers, styrene-methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-acrylonitrile copolymers, styrene-vinyl methyl ether copolymers, styrene-vinyl ethyl ether copolymers, styrene-vinyl methyl ketone copolymers and styrene-acrylonitrile-indene copolymers; and polyvinyl chloride, phenolic resins, natural resin-modified phenolic resins, natural resin-modified maleic acid resins, acrylic resins, methacrylic resins, polyvinyl acetate, silicone resins, polyester resins, polyurethane resins, polyamide resins, furan resins, epoxy resins, xylene resins, polyvinyl butyral, terpene resins, coumarone-indene resins and petroleum resins.
[0078] Among them, from the viewpoint of charge-raising performance, the second resin is preferably at least one selected from the group consisting of a vinyl resin (e.g., a styrene copolymer), a polyester resin, and a hybrid resin comprising a vinyl resin connected to a polyester resin. The connection here may refer to a connection through a covalent bond. The second resin more preferably contains a polyester resin, and is more preferably a polyester resin.
[0079] The second resin is explained below using an example of a polyester resin.
[0080] The polyester resin is preferably a polycondensate of an alcohol component and a carboxylic acid component.
[0081] The acid value of the second resin can be controlled, for example, by changing the contents and kinds of the alcohol unit and the carboxylic acid unit in the non-crystalline resin.
[0082] The alcohol unit in the second resin is a structure obtained by polycondensation of a monomer as an alcohol component, or in other words, a monomer unit derived from an alcohol component. In addition, the carboxylic acid unit in the second resin is a structure obtained by polycondensation of a monomer as a carboxylic acid component, or in other words, a monomer unit derived from a carboxylic acid component.
[0083] From the viewpoint of charge enhancement performance, the structure obtained by polycondensation of bisphenol A alkylene oxide adduct preferably constitutes at least 75 mol%, or more preferably at least 80 mol%, or still more preferably at least 90 mol% of the alcohol unit. An example of bisphenol A alkylene oxide adduct is a compound represented by the following formula (A):
[0084]
[0085] (In formula (A), each R is independently an ethylene group or a propylene group, x and y are each an integer of 0 or greater, and the average value of x+y is 0 to 10).
[0086] In view of the charge-raising performance, the bisphenol A alkylene oxide adduct is preferably a bisphenol A propylene oxide adduct and / or an ethylene oxide adduct, more preferably a propylene oxide adduct. The average value of x+y is preferably 1 to 5, more preferably 1.6 to 2.8.
[0087] The following polyol components may be used as components other than the bisphenol A alkylene oxide adduct for forming the alcohol unit.
[0088] Ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,4,5-pentanetriol, glycerol, 2-methylpropylenetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, 1,3,5-trimethylolbenzene.
[0089] The peak molecular weight Mp of the second resin is preferably 3,000 to 30,000, or more preferably 5,000 to 20,000, or still more preferably 10,000 to 15,000, from the viewpoint of low-temperature fixability and hot offset resistance.
[0090] The carboxylic acid unit preferably includes at least one selected from the group consisting of an aromatic dicarboxylic acid polycondensation structure, a saturated aliphatic dicarboxylic acid polycondensation structure, and an unsaturated dicarboxylic acid polycondensation structure.
[0091] Examples of the aromatic dicarboxylic acids include phthalic acid, isophthalic acid, and terephthalic acid, and anhydrides thereof.
[0092] From the viewpoint of charge-increasing performance, alkyl dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, adipic acid, suberic acid, azelaic acid, and sebacic acid, and anhydrides thereof are desirable as the saturated aliphatic dicarboxylic acid.
[0093] It is expected that such as fumaric acid, maleic acid, citraconic acid, itaconic acid and C 6-18 Unsaturated dicarboxylic acids such as alkenyl-substituted succinic acid and anhydrides thereof are used as unsaturated dicarboxylic acids. It is particularly desirable to include dodecenylsuccinic acid. It is more desirable to combine at least two of the above-mentioned saturated aliphatic dicarboxylic acids and unsaturated dicarboxylic acids.
[0094] That is, it is preferred that the second resin is a polyester resin, and the polyester resin has a polycondensation structure of dodecenylsuccinic acid or its anhydride. In addition, the polyester resin preferably has a polycondensation structure of other carboxylic acid components other than the polycondensation structure of dodecenylsuccinic acid or its anhydride. If the polyester resin has a polycondensation structure of dodecenylsuccinic acid or its anhydride, it is more likely to interact with inorganic fine particles, thereby causing good charge-raising performance of the toner.
[0095] The content of the polycondensation structure of dodecenylsuccinic acid or its anhydride in the carboxylic acid unit is preferably 10 mol % to 30 mol %, or more preferably 15 mol % to 20 mol %.
[0096] In view of charge-raising performance and hot offset resistance, the carboxylic acid unit preferably includes a polycondensation structure of an aromatic tricarboxylic acid or an aromatic tetracarboxylic acid.
[0097] Examples of the aromatic tricarboxylic acid include trimellitic acid and trimellitic anhydride.Examples of the aromatic tetracarboxylic acid include pyromellitic acid and pyromellitic anhydride.
[0098] The polycondensation structure of the aromatic carboxylic acid preferably constitutes 50 mol% to 80 mol%, or more preferably 60 mol% to 75 mol% of the carboxylic acid unit.
[0099] It is desirable to increase the content ratio of the aromatic carboxylic acid to the aliphatic dicarboxylic acid to improve the charge retention property.
[0100] Examples of the aromatic carboxylic acid include the aforementioned aromatic dicarboxylic acids, aromatic tricarboxylic acids, and aromatic tetracarboxylic acids.
[0101] Other carboxylic acids useful in forming the carboxylic acid unit include 6-18 Alkyl-substituted succinic acid or its anhydride, and polycarboxylic acids such as 1,2,3,4-butanetetracarboxylic acid and benzophenonetetracarboxylic acid and its anhydride.
[0102] The non-crystalline polyester resin can be produced using any commonly used catalyst including metals such as tin, titanium, antimony, manganese, nickel, zinc, lead, iron, magnesium, calcium and germanium, and compounds containing these metals.
[0103] Among them, tin compounds are expected to be used to improve charging performance. Examples of tin compounds include organic tin compounds such as dibutyltin dichloride, dibutyltin oxide, and diphenyltin oxide. The organic tin compound here is a compound having a Sn-C bond.
[0104] Inorganic tin compounds without Sn-C bonds can also be used advantageously. The inorganic tin compound here is a compound without Sn-C bonds.
[0105] Examples of the inorganic tin compound include unbranched alkyl tin carboxylates such as tin diacetate, tin dihexanoate, tin dioctanoate, and tin distearate, branched alkyl tin carboxylates such as tin dipivalate and tin di(2-ethylhexanoate), tin carboxylates such as tin oxalate, and dialkoxytin such as dioctanoate and distearoxytin.
[0106] Among these tin compounds, tin alkylcarboxylates or tin dialkoxides are preferred, and tin dioctoate, tin di(2-ethylhexanoate), and tin distearate, which are tin alkylcarboxylates having a carboxyl residue in the molecule, are particularly desirable.
[0107] The dielectric constant of the second resin (non-crystalline resin) at 2kHz is preferably 2.0 pF / m to 3.0 pF / m. Within this range, the charge transfer of the inorganic fine particles is improved, so the charge rise performance is improved. More preferably, it is 2.2 pF / m to 2.8 pF / m. The dielectric constant of the second resin can be controlled by changing the monomer composition and the acid value.
[0108] The binder resin preferably contains a third resin. The third resin preferably comprises a resin in which a first resin (crystalline resin) and a second resin (non-crystalline resin) are connected, and more preferably a resin in which a first resin and a second resin are connected. When such a third resin is contained, good charge rise performance, low temperature fixing property and heat offset resistance are obtained. The third resin preferably has a structure in which, for example, at least a portion of the first resin and the second resin are connected together.
[0109] Methods of connecting the first resin to the second resin include a method of crosslinking by applying a radical initiator to a mixture obtained by melting or dissolving the first resin and the second resin, a method of crosslinking using a crosslinking agent having a functional group reactive with the first resin and the second resin, and the like.
[0110] The radical initiator used in the method of cross-linking using a radical initiator is not particularly limited, and may be an inorganic peroxide, an organic peroxide, or an azo compound, etc. These radical reaction initiators may also be combined.
[0111] When both the first resin and the second resin have carbon-carbon unsaturated bonds, these bonds are broken when the first resin and the second resin are cross-linked. When either or both of the first resin and the second resin do not have carbon-carbon unsaturated bonds, the two are cross-linked by extracting hydrogen atoms bonded to carbon atoms contained in the first resin and / or the second resin. In this case, the free radical initiator is more preferably an organic peroxide having a strong hydrogen abstraction ability.
[0112] There is no particular limitation on the cross-linking agent having a functional group that reacts with both the first resin and the second resin, and known reagents can be used, such as a cross-linking agent having an epoxy group, a cross-linking agent having an isocyanate group, a cross-linking agent having an oxazoline group, a cross-linking agent having a carbodiimide group, a cross-linking agent having a hydrazide group, or a cross-linking agent having an aziridine group.
[0113] In the method of cross-linking using a cross-linking agent having a functional group reactive with both the first resin and the second resin, both the first resin and the second resin must have a functional group reactive with the cross-linking agent.
[0114] A resin in which at least a part of the first resin and the second resin are crosslinked together by the above method (ie, a resin composition containing the first resin and the second resin, and a third resin obtained by crosslinking the first resin and the second resin) can be used to manufacture a toner.
[0115] When the toner is produced by a melt-kneading method, toner particles containing a resin including a first resin linked to a second resin can be produced by melt-kneading a raw material mixture containing the first resin and the second resin in the presence of the above-mentioned radical initiator or crosslinking agent.
[0116] The content of the third resin in the binder resin is preferably 1.0% by mass to 20.0% by mass, or more preferably 5.0% by mass to 15.0% by mass.
[0117] For example, the third resin is preferably a resin obtained by adding a radical reaction initiator while melt-kneading a non-crystalline polyester resin (second resin) having a carbon-carbon double bond and the first resin to thereby perform a crosslinking reaction.
[0118] When the third resin is made using the first resin and the second resin, at least a portion of the first resin and the second resin are connected together to form the third resin. This produces a binder resin containing the first resin, the second resin, and the third resin.
[0119] The binder resin containing the first resin, the second resin and the third resin can also be obtained by connecting at least a portion of the first resin and the second resin. The binder resin can also be obtained by separately manufacturing the third resin and then mixing it with the first resin and the second resin.
[0120] The radical reaction initiator used in the crosslinking reaction is not particularly limited, and may be an inorganic peroxide, an organic peroxide, or an azo compound, etc. These radical reaction initiators may be used in combination.
[0121] The inorganic peroxide is not particularly limited, and examples include hydrogen peroxide, ammonium peroxide, potassium peroxide, sodium peroxide, and the like.
[0122] The organic peroxide is not particularly limited, and examples include benzoyl peroxide, di-tert-butyl peroxide, tert-butylcumyl peroxide, dicumyl peroxide, α,α-di(tert-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, di-tert-hexyl peroxide, 2,5-dimethyl-2,5-di-t-butylperoxyhexine-3, Acetyl peroxide, isobutyryl peroxide, octanoyl peroxide, decanoyl peroxide, lauroyl peroxide, 3,3,5-trimethylhexanoyl peroxide, m-toluoyl peroxide, tert-butyl peroxyisobutyrate, tert-butyl peroxyneodecanoate, cumyl peroxyneodecanoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylethylhexanoate, tert-butyl peroxylaurate, tert-butyl peroxybenzoate, tert-butyl peroxyisopropyl monocarbonate, and tert-butyl peroxyacetate, etc.
[0123] The azo compound or diazo compound is not particularly limited, and examples include 2,2′-azobis-(2,4-dimethylvaleronitrile), 2,2′-azobisisobutyronitrile, 1,1′-azobis(cyclohexane-1-carbonitrile), 2,2′-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile.
[0124] Among them, organic peroxides are desirable because they have high initiator efficiency and do not produce toxic byproducts such as cyanide compounds.
[0125] Reaction initiators having high hydrogen abstraction ability are desirable because the cross-linking reaction can be efficiently carried out using a smaller amount of initiator, and free radical reaction initiators having high hydrogen abstraction ability such as isopropyl tert-butyl peroxide monocarbonate, benzoyl peroxide, di-tert-butyl peroxide, tert-butylcumyl peroxide, dicumyl peroxide, α,α-di(tert-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane or di-tert-hexyl peroxide are even more desirable.
[0126] The amount of the radical reaction initiator used is not particularly limited, but is preferably 0.1 to 50 parts by mass, or more preferably 0.2 to 5 parts by mass, relative to 100 parts by mass of the binder resin to be crosslinked.
[0127] The mass ratio X / Y of the content X of the first resin to the content Y of the second resin in the binder resin is preferably 0.2 to 2.5, or more preferably 2.0 to 2.4, from the viewpoints of low temperature fixing property, hot offset resistance and charge build-up performance.
[0128] The number average diameter of domains in cross-sectional observation of the toner is preferably 0.1 μm to 2.0 μm, or more preferably 0.5 μm to 1.5 μm, from the viewpoint of low-temperature fixability and hot offset resistance.
[0129] If the number average diameter of the domain is 2.0 μm or less, the fixing performance is improved because the crystalline resin of the matrix and the non-crystalline resin of the domain are more easily melted when the toner particles are fixed. In addition, since the viscosity of the molten matrix is maintained at an appropriate level in a high temperature region, hot offset is suppressed.
[0130] If the number average diameter of the domains is 0.1 μm or more, since the rapid melting property of the crystalline resin can be appropriately obtained, the low-temperature fixing property is improved.
[0131] The number average diameter of the domains can be controlled by the monomer composition of the crystalline resin and the non-crystalline resin, the production conditions, and the like.
[0132] The toner is characterized by containing a volume resistivity of 1.0×10 5 Ω·cm to 1.0×1013 Inorganic fine particles of Ω·cm.
[0133] If the volume resistivity of the inorganic fine particles is within this range, charge transfer of the inorganic fine particles occurs more rapidly and the charge rise is improved. 5 Ω·cm, the electrical resistivity is too low, so the charging performance is reduced in a high temperature and high humidity environment. On the other hand, if it exceeds 1.0×10 13 Ω·cm, the charge rises slowly due to the high resistance.
[0134] The volume resistivity of the inorganic fine particles is preferably 1.0×10 8 Ω·cm to 7.0×10 12 Ω·cm. The volume resistivity can be controlled by controlling the type of inorganic fine particles, the type of surface treatment, the concentration of the surface treatment agent, and the like.
[0135] The following is the volume resistivity of 1.0×10 5 Ω·cm to 1.0×10 13 Examples of inorganic fine particles of Ω·cm:
[0136] Fine particles of metal titanates such as strontium titanate fine particles, calcium titanate fine particles, and magnesium titanate fine particles; and fine particles of metal oxides such as titanium oxide fine particles, magnesium oxide fine particles, zinc oxide fine particles, and cerium oxide fine particles.
[0137] Among them, at least one selected from the group consisting of titanium oxide fine particles, strontium titanate fine particles, calcium titanate fine particles and zinc oxide fine particles is preferred. At least one selected from the group consisting of titanium oxide fine particles and strontium titanate fine particles is more preferred. Inorganic fine particles containing titanium oxide fine particles are still more preferred, and further preferably the inorganic fine particles are titanium oxide fine particles.
[0138] Particle characteristics such as particle size, resistivity and dielectric constant are relatively easily controlled by manufacturing conditions. Strontium titanate preferably has a perovskite crystal structure. If strontium titanate has a perovskite crystal structure, electron transfer of the second monomer unit is relatively fast.
[0139] Strontium titanate fine particles, calcium titanate fine particles and magnesium titanate fine particles can be obtained, for example, by a normal pressure heating reaction method. In this case, an inorganic acid peptized product of a hydrolyzate of a titanium compound is used as a titanium oxide source, and a water-soluble acidic metal compound is used as a metal oxide source. It can be produced by reacting a mixture of these while adding an alkaline aqueous solution at 60° C. or above, and then treating with an acid.
[0140] The production method of the titanium dioxide fine particles is not particularly limited, and examples include titanium dioxide fine particles produced by conventional sulfuric acid method and chlorine method, and titanium dioxide fine particles produced by a gas phase oxidation method in which titanium tetrachloride as a raw material reacts with oxygen in a gas phase. Titanium dioxide fine particles obtained by a sulfuric acid method are more preferred because the number average particle size of primary particles of the obtained titanium dioxide fine particles can be easily controlled.
[0141] It is desirable to use either rutile or anatase titanium dioxide fine particles. To obtain anatase titanium dioxide fine particles, it is desirable to add phosphoric acid, a phosphate, or a potassium salt as a rutile transition inhibitor when firing metatitanic acid.
[0142] On the other hand, in order to obtain rutile titanium oxide fine particles, it is desirable to add a salt such as a lithium salt, a magnesium salt, a zinc salt or an aluminum salt as a rutile transition accelerator, or a seed such as a slurry containing rutile microcrystals.
[0143] The production methods of metal oxide fine particles of magnesium oxide, zinc oxide and cerium oxide include a dry method in which metal vapor is oxidized in air to produce zinc oxide, and a wet method in which a metal salt is neutralized by reacting with an alkali in an aqueous solution, then washed with water, dried, and fired to produce zinc oxide. Among them, the wet method is preferred because it is more likely to produce fine particles with a relatively small particle size that can be added to the toner surface.
[0144] The dielectric constant of the inorganic fine particles at 2kHz is preferably 20pF / m to 60pF / m. Since the inorganic fine particles with a dielectric constant within this range have fast charge transfer with the second monomer unit, the inorganic fine particles are desirable. It is believed that since the dielectric constant originates from polarization within or between atoms, it is closely related to charge transfer.
[0145] The dielectric constant can be controlled by selecting inorganic fine particles, or by controlling the conditions and operations for changing the crystallinity of the particles when producing the inorganic fine particles, such as by changing the reaction temperature or water pressure in a dry method or the pH or temperature in a wet method, or by, for example, ultrasonic treatment or bubbling treatment during crystal formation.
[0146] The dielectric constant is more preferably 20 pF / m to 40 pF / m, or still more preferably 25 pF / m to 30 pF / m.
[0147] The compound having an alkyl group is present on the surface of the inorganic fine particles. Such inorganic fine particles can be obtained, for example, by surface-treating the inorganic fine particles with a compound having an alkyl group.
[0148] If the inorganic fine particles have a compound containing an alkyl group on the surface thereof, it can interact with the alkyl group contained in the first monomer unit, improve adhesion and allow charges to be quickly transferred from the inorganic fine particles to the second monomer unit of the toner particles.
[0149] Examples of the compound having an alkyl group include fatty acids, fatty acid metal salts, silicone oils, silane coupling agents, titanium coupling agents, and fatty alcohols.
[0150] Among them, in order to easily obtain the effects of the present disclosure, at least one compound selected from the group consisting of fatty acids, fatty acid metal salts, silicone oils, and silane coupling agents is preferred.
[0151] Examples of the fatty acid and the fatty acid metal salt include lauric acid, stearic acid, behenic acid, lithium laurate, lithium stearate, sodium stearate, zinc laurate, zinc stearate, calcium stearate and aluminum stearate.
[0152] The following is a method for treating inorganic fine particles with fatty acid or its metal salt surface. For example, the slurry containing inorganic fine particles can be placed in a sodium fatty acid aqueous solution in Ar gas or N2 gas atmosphere, and the fatty acid is separated out on the calcium iron ore type crystal surface. The slurry containing inorganic fine particles can also be placed in a sodium fatty acid aqueous solution in Ar gas or N2 gas atmosphere, and under agitation, the desired metal salt aqueous solution is dripped and the fatty acid metal salt is separated out and adsorbed on the calcium iron ore type crystal surface. For example, aluminum stearate can be adsorbed by using aluminum sulfate and sodium stearate aqueous solution.
[0153] Examples of the silicone oil include dimethyl silicone oil, methylphenyl silicone oil, and alkyl-modified silicone oils such as α-methylstyrene-modified silicone oil and octyl-modified silicone oil.
[0154] The method of silicone oil treatment may be a known method. For example, the inorganic fine particles and silicone oil may be mixed using a mixer; or the silicone oil may be sprayed onto the inorganic fine particles using a sprayer; or the silicone oil may be dissolved in a solvent after the inorganic fine particles are mixed in the solvent. The treatment method is not limited to these.
[0155] Examples of the silane coupling agent include hexamethyldisilazane, trimethylsilane, trimethylethoxysilane, isobutyltrimethoxysilane, trimethylchlorosilane, dimethyldichlorosilane, methyltrichlorosilane, dimethylethoxysilane, dimethyldimethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, hexadecyltrimethoxysilane, and stearyltrimethoxysilane.
[0156] Examples of fatty alcohols include ethanol, n-propanol, 2-propanol, n-butanol, tert-butanol, n-octanol, stearyl alcohol and 1-tetracosanol. The method of treating with fatty alcohols may be, for example, a method of treating inorganic fine particles after heating and vaporizing at a temperature at or above the boiling point.
[0157] Among these compounds, in order to increase the charge rise, selected from the group consisting of 4-24 (Preferred C 4-18 ) alkyl group is desirable because it further improves the interaction with the alkyl group of the first monomer unit.
[0158] The compound having an alkyl group preferably has a 9 -COO) p M(OH) q (where each R 9 Independently represents C 4-24 (Preferred C 4-18 ) Straight or branched alkyl or C 4-24 (Preferred C 4-18 ) a structure represented by a straight chain or branched hydroxyalkyl group, M is Al, Zn, Mg, Ca, Sr, K or Na (preferably Ca or Na), p is an integer from 1 to 3 (preferably 1 or 2) and q is an integer from 0 to 2 (preferably 0)).
[0159] When Cx is the carbon number of the alkyl group represented by R in the first monomer unit and Cy is the carbon number of the alkyl group of the compound having an alkyl group, in order to further strengthen the interaction between the alkyl groups and make the charge transfer smooth, Cx / Cy is preferably 0.8 to 24.0. More preferably, it is 1.0 to 7.0. When a plurality of first monomer units or a plurality of compounds having an alkyl group are used, the average carbon number is calculated based on the molar ratio.
[0160] When Cz is the carbon number of the polycarboxylic acid in the polymerization (preferably polycondensation) structure of the polycarboxylic acid contained in the second resin (non-crystalline resin), (Cx+Cz) / Cy is preferably 0.8 to 10.0. Within this range, the interaction between the alkyl groups becomes stronger and charge transfer occurs smoothly. It is more preferably 1.0 to 5.0, and even more preferably 1.0 to 3.0.
[0161] When a plurality of first monomer units or a plurality of compounds having an alkyl group are used, the average carbon number is calculated based on a molar ratio.
[0162] The number average particle diameter of the primary particles of the inorganic fine particles is preferably 20nm to 300nm. It is desirable that the number average particle diameter of the primary particles is within this range because it makes it easier for the inorganic fine particles to interact with both the first monomer unit and the second monomer unit of the first resin having a block copolymer-like structure. More preferably 20nm to 200nm.
[0163] The content of the inorganic fine particles is preferably 0.1 to 15.0 parts by mass relative to 100 parts by mass of the toner particles.
[0164] In order to more easily obtain the effects of the present disclosure, the coverage of the toner particles by the inorganic fine particles is preferably 10 area % to 80 area %. More preferably, it is 15 area % to 75 area %, or still more preferably 20 area % to 70 area %. The coverage can be controlled by controlling the addition amount of the inorganic fine particles, external addition conditions, and the like.
[0165] The charge decay rate coefficient of the toner measured under a 30° C., 80% RH environment is preferably 3 to 100, or more preferably 3 to 50. The charge decay rate coefficient within this range is expected to be used for controlling the charge reduction in a high temperature and high humidity environment. The charge decay rate coefficient can be controlled by controlling the type and acid value of the binder resin, the type of inorganic fine particles, the inorganic fine particle surface treatment agent, and the coverage of the inorganic fine particles on the toner particles.
[0166] When Xε is the dielectric constant of the inorganic fine particles at 2 kHz and Yε is the dielectric constant of the second resin at 2 kHz, Xε / Yε is preferably 5.0 to 170.0.
[0167] Within this range, charge up in a low-temperature and low-humidity environment can be controlled. Xε / Yε is more preferably 8.0 to 13.0.
[0168] The first resin (crystalline resin) may contain a third monomer unit different from the first monomer unit represented by the above formula (1) and the second monomer unit represented by the above formula (2) or (3).
[0169] The polymerizable monomer capable of forming the third monomer unit includes styrenes such as styrene and o-methylstyrene and derivatives thereof, (meth)acrylates such as 2-ethylhexyl (meth)acrylate, and (meth)acrylic acid.
[0170] The content ratio of the third monomer unit in the first resin is preferably 1.0% by mass to 30.0% by mass, or more preferably 5.0% by mass to 20.0% by mass.
[0171] As described above, strontium titanate fine particles can be obtained by a normal pressure heating reaction method.
[0172] Normal pressure heating reaction method
[0173] The inorganic acid peptized product of the hydrolyzate of the titanium compound is used as the titanium oxide source. For example, metatitanic acid obtained by a sulfuric acid method and peptized by adjusting the pH to 0.8 to 1.5 with hydrochloric acid and preferably having an SO3 content of 1.0% by mass or less or more preferably 0.5% by mass or less can be used.
[0174] Nitrates, hydrochlorides, or the like can be used as the strontium oxide source, and for example, strontium nitrate or strontium hydrochloride can be used.
[0175] Caustic alkali may be used as the alkaline aqueous solution, preferably an aqueous sodium hydroxide solution.
[0176] Factors affecting the particle size of the obtained strontium titanate particles include the mixing ratio of the titanium oxide source and the strontium oxide source in the reaction, the concentration of the titanium oxide source at the start of the reaction, and the temperature and addition rate when the alkaline aqueous solution is added, which can be appropriately adjusted to obtain the target particle size and particle size distribution. It is desirable to prevent contamination by carbon dioxide gas during the reaction by, for example, conducting the reaction in a nitrogen atmosphere to prevent the generation of carbonates.
[0177] Factors affecting the dielectric constant of the obtained strontium titanate particles include conditions and operations that destroy the crystallinity of the particles. In order to obtain strontium titanate with a low dielectric constant, it is preferred to apply energy to destroy crystal growth in a state where the concentration of the reaction solution is high, and a specific method is, for example, microbubbling with nitrogen during crystal growth.
[0178] For the mixing ratio of the titanium oxide source and the strontium oxide source during the reaction, the molar ratio of SrO / TiO2 is preferably 0.9 to 1.4, or more preferably 1.05 to 1.20. If the SrO / TiO2 molar ratio is 0.9 or more, there is less possibility of residual unreacted titanium oxide. The concentration of the titanium oxide source in terms of TiO2 at the start of the reaction is preferably 0.05 to 1.3 mol / L, or more preferably 0.08 to 1.0 mol / L.
[0179] The temperature when adding the alkaline aqueous solution is preferably about 60° C. to 100° C. With regard to the addition rate of the alkaline aqueous solution, the slower the addition rate, the larger the particle size of the produced metal titanate particles, and the faster the addition rate, the smaller the particle size of the produced metal titanate particles. The addition rate of the alkaline aqueous solution is preferably 0.001 to 1.2 eq / h or more preferably 0.002 to 1.1 eq / h relative to the raw material, and can be appropriately adjusted according to the desired particle size.
[0180] Acid treatment
[0181] It is preferred to further acid-treat the metal titanate particles obtained by the normal pressure heating reaction. If the mixing ratio of the titanium oxide source and the strontium oxide source exceeds the SrO / TiO2 molar ratio of 1.0, when the metal titanate particles are synthesized by the normal pressure heating reaction, the unreacted metal source other than titanium remaining after the reaction is completed may react with the carbon dioxide gas in the air to produce impurities such as metal carbonate. Therefore, it is preferred to perform the acid treatment after adding the alkaline aqueous solution to remove the unreacted metal source.
[0182] In the acid treatment, the pH is preferably adjusted to 2.5 to 7.0, more preferably 4.5 to 6.0, with hydrochloric acid. In addition to hydrochloric acid, nitric acid, acetic acid, and the like can also be used as the acid.
[0183] Colorants
[0184] A colorant may also be used as the toner. Examples of the colorant include the following.
[0185] Examples of black colorants include carbon black and black products obtained by blending yellow, magenta and cyan colorants. Pigments can be used alone as colorants, but from the viewpoint of image quality of full-color images, it is desirable to combine dyes with pigments to improve clarity.
[0186] Examples of pigments for magenta toners include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75 7:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269 and 282; CI Pigment Violet 19; and CI Vat Red 1, 2, 10, 13, 15, 23, 29 and 35.
[0187] Examples of dyes for magenta toners include CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109 and 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; oil-soluble dyes such as CI Disperse Violet 1, and CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39 and 40; and basic dyes such as CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27 and 28.
[0188] Examples of the pigment for cyan toner include CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, and 17; CI Vat Blue 6; and CI Acid Blue 45, and copper phthalocyanine pigments having 1 to 5 phthalimidomethyl substituents in the phthalocyanine skeleton.
[0189] Examples of the dye for cyan toner include CI Solvent Blue 70.
[0190] Examples of the pigment for yellow toner include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181 and 185; and CI Vat Yellow 1, 3 and 20.
[0191] Examples of the dye for yellow toner include CI Solvent Yellow 162.
[0192] The content of the colorant is preferably from 0.1 to 30 parts by mass based on 100 parts by mass of the binder resin.
[0193] wax
[0194] Waxes can also be used in toners. Examples of waxes include the following: hydrocarbon waxes, such as microcrystalline waxes, paraffin waxes, and Fischer-Tropsch waxes; oxides of hydrocarbon waxes, such as oxidized polyethylene waxes, and block copolymers thereof; waxes composed mainly of fatty acid esters, such as carnauba wax; and waxes composed of partially or completely deoxygenated fatty acid esters, such as deoxygenated carnauba wax.
[0195] Other examples include the following: saturated straight-chain fatty acids, such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids, such as brassidic acid, eleostearic acid, and parinaric acid; saturated alcohols, such as stearyl alcohol, aralkyl alcohols, behenyl alcohol, carnaubyl alcohol, wax alcohol, and melissyl alcohol; polyols, such as sorbitol; esters of fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid with alcohols such as stearyl alcohol, aralkyl alcohols, behenyl alcohol, carnaubyl alcohol, wax alcohol, and melissyl alcohol. Fatty acid amides, such as linoleamide, oleamide and lauramide; saturated fatty acid bisamides, such as methylene bisstearamide, ethylene bisdecylamide, ethylene bislauramide and hexamethylene bisstearamide; unsaturated fatty acid amides, such as ethylene bisoleamide, hexamethylene bisoleamide, N,N'-dioleyl adipamide and N,N'-dioleylsebacamide; aromatic bisamides, such as meta-xylene bisstearamide and N,N'-distearyl isophthalamide. isophthalamide); fatty metal salts (commonly known as metal soaps), such as calcium stearate, calcium laurate, zinc stearate and magnesium stearate; waxes obtained by grafting vinyl monomers such as styrene and acrylic acid onto fatty hydrocarbon waxes; partial esterification products of polyols and fatty acids such as monoglyceride of behenic acid; methyl ester compounds having a hydroxyl group obtained by hydrogenating vegetable oils and fats.
[0196] The content of the wax is preferably 2.0 to 30.0 parts by mass relative to 100 parts by mass of the binder resin.
[0197] Charge control agent
[0198] If necessary, a charge control agent may also be contained in the toner. A known charge control agent may be contained in the toner, and a metal compound of an aromatic carboxylic acid is particularly desirable because the compound is colorless and can provide a fast charging speed and stably maintain a uniform charge amount.
[0199] Examples of negative charge control agents include salicylic acid metal compounds, naphthoic acid metal compounds, dicarboxylic acid metal compounds, polymer compounds having sulfonic acid or carboxylic acid in the side chain, polymer compounds having sulfonates or sulfonic esters in the side chain, polymer compounds having carboxylates or carboxylates in the side chain, and boron compounds, urea compounds, silicon compounds, and calixarene. The charge control agent may be added internally or externally to the toner particles.
[0200] The amount of the charge control agent added is preferably 0.2 parts by mass to 10 parts by mass based on 100 parts by mass of the binder resin.
[0201] Inorganic fine powder
[0202] In addition to the above-mentioned inorganic fine particles, another inorganic fine powder can be included in the toner if necessary. The inorganic fine powder can be added to the toner particles internally or externally. Inorganic fine powders such as silicon dioxide are expected to be used as external additives. Preferably, the inorganic fine powder is an inorganic fine powder that has been hydrophobized with a hydrophobic agent such as a silane compound or silicone oil or a mixture thereof.
[0203] For example, it is desirable to use a fine silica powder produced by any method, such as a precipitation method, a sol-gel method or other wet method for obtaining silica by neutralizing sodium silicate, or a flame melting method, an arc method or other dry method for obtaining silica in a gas phase. Among them, the fine silica powder produced by the sol-gel method or the flame melting method is more desirable because it makes it easier to control the number average particle size of the primary particles within a desired range.
[0204] The specific surface area is 50m 2 / g to 400m 2 / g of inorganic fine powder is expected to be used as an external additive to improve fluidity, and the specific surface area is 10m 2 / g to 50m 2 Inorganic fine powder having a specific surface area within these ranges may be combined in order to improve fluidity and stabilize durability.
[0205] Developer
[0206] The toner can be used as a single-component developer, but from the viewpoint of obtaining stable image quality over a long period of time, it is preferably mixed with a magnetic carrier and used as a two-component developer to improve dot reproducibility. That is, this is preferably a two-component developer containing a toner and a magnetic carrier, wherein the toner is the toner of the present invention.
[0207] Common well-known magnetic carriers can be used, and examples include surface-oxidized iron powder, unoxidized iron powder, metal particles of iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, chromium, and rare earth, their alloy particles and oxide particles, magnetic bodies such as ferrite, and resin carriers with dispersed magnetic bodies containing a binder resin that supports these magnetic bodies in a dispersed state (so-called resin carriers).
[0208] When the toner is mixed with a magnetic carrier and used as a two-component developer, good effects can generally be obtained if the carrier mixing ratio (toner concentration of the two-component developer) is 2% by mass to 15% by mass, or more preferably 4% by mass to 13% by mass.
[0209] Method for producing toner particles
[0210] The method for producing the toner particles is not particularly limited, and a conventionally known method such as a suspension polymerization method, an emulsion aggregation method, a melt kneading method, or a dissolution suspension method may be used.
[0211] The obtained toner particles can be used as toner as they are. If necessary, inorganic fine particles or other external additives can be mixed with the obtained toner particles to obtain a toner. The mixing of the toner particles with the inorganic fine particles and other external additives can be performed using a mixing device such as a double cone mixer, a V-type mixer, a drum mixer, a super mixer, a Henschel mixer, a Nauta mixer, a Mechano Hybrid (Nippon Coke and Engineering), or a Nobilta (Hosokawa Micron).
[0212] The amount of the external additive used is preferably 0.1 to 10.0 parts by mass relative to 100 parts by mass of the toner particles.
[0213] In the gel permeation chromatography measurement of a tetrahydrofuran soluble matter of the toner, the weight average molecular weight is Mw(A), and the number average molecular weight is Mn(A).
[0214] Mw(A) is preferably 25,000 to 60,000, or more preferably 32,000 to 48,000.
[0215] Mw(A) / Mn(A) is preferably 5-10, or more preferably 7-8.
[0216] Mn(A) is preferably 3,000 to 8,500, or more preferably 4,000 to 6,000.
[0217] Mw(A) can be controlled by controlling the monomer composition and molecular weight of the binder resin and the production conditions.
[0218] Mw(A) / Mn(A) can be controlled by controlling the monomer composition and molecular weight of the binder resin and the production conditions.
[0219] Within these ranges, low temperature fixability and hot offset resistance are improved.The peak molecular weight in the molecular weight distribution curve obtained by GPC measurement of THF solubles of toner particles is preferably 7,000 to 11,000, or more preferably 8,200 to 10,500.
[0220] If the peak molecular weight is within this range, low-temperature fixability and hot offset resistance are improved.
[0221] When the molecular weight distribution curve has a plurality of peaks, the peak molecular weight in the molecular weight distribution curve obtained by GPC measurement of THF solubles of toner particles is the molecular weight of the highest peak.
[0222] Methods for measuring various physical properties of toner and raw materials are explained below.
[0223] Measurement method of volume resistivity of inorganic fine particles
[0224] The volume resistivity of the inorganic fine particles was measured as follows. A Keithley Instruments 6517 electrometer / high resistance system was used as the apparatus. Electrodes of 25 mm in diameter were connected, the inorganic fine particles were placed between the electrodes to a thickness of about 0.5 mm, and the distance between the electrodes was measured under a load of about 2.0 N.
[0225] The resistance value was measured when a voltage of 1,000 V was applied to the inorganic fine particles for 1 minute, and the volume resistivity was calculated according to the following formula.
[0226] Volume resistivity (Ω·cm) = R×L
[0227] R: resistance value (Ω)
[0228] L: distance between electrodes (cm)
[0229] Separation of inorganic fine particles from toner
[0230] The inorganic fine particles can also be separated from the toner and measured by the following method.
[0231] 200g sucrose (Kishida Chemical) is added to 100mL ion exchange water, and dissolved in a hot water bath to prepare a concentrated sucrose solution. 31g concentrated sucrose solution and 6mL Contaminon N (10% by mass pH 7 neutral detergent aqueous solution for washing precision instruments, which comprises nonionic surfactant, anionic surfactant and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) are added to a centrifuge tube to prepare a dispersion. 1g toner is added to the dispersion, and toner lumps are broken with a spatula or the like.
[0232] The centrifuge tube was shaken at a speed of 350 reciprocating times per minute for 20 minutes in a shaking table (KM Shaker (model: V.SX) IWAKI CO., LTD.). After shaking, the solution was transferred to a glass tube (50 mL) for a rotating rotor and centrifuged in a centrifuge for 30 minutes at 3500 rpm. After centrifugation, toner was present in the uppermost layer in the glass tube, and inorganic fine particles were present in the aqueous solution of the lower layer. The aqueous solution of the lower layer was collected and centrifuged to separate sucrose from inorganic fine particles, and inorganic fine particles were collected. Centrifugation was repeated as needed, and once the separation was sufficient, the dispersion was dried, and inorganic fine particles were collected.
[0233] When a plurality of types of inorganic fine particles have been added, these inorganic fine particles may be selected by centrifugation or the like.
[0234] Measuring method of dielectric constant of inorganic fine particles and second resin
[0235] The complex dielectric constant was measured at a frequency of 2 kHz using a 284A precision LCR meter (Hewlett Packard) after calibration at frequencies of 1 kHz and 1 MHz. A pressure of 39200 kPa (400 kg / cm 2 ) for 5 minutes to form a disk-shaped measurement sample having a diameter of 25 mm and a thickness of 1 mm or less (preferably 0.5 to 0.9 mm). The measurement sample is mounted on an ARES (Rheometric Scientific FE) equipped with a dielectric constant measurement fixture (electrode) having a diameter of 25 mm, and measured at a frequency of 2 kHz under a load of 0.49 N (50 g) in an atmosphere of 25°C.
[0236] Measurement of the Charge Decay Rate Coefficient of Toner
[0237] The charge decay rate coefficient of the toner is measured using an NS-D100 static diffusivity measuring device (Nano Seeds).
[0238] First, place about 100 mg of toner in a sample pan and scrape it to make the surface smooth. Expose the sample pan to X-rays for 30 seconds with an X-ray static eliminator to remove the charge from the toner. Place the de-charged sample pan on the measurement board. Also install a metal plate as a reference to zero-calibrate the surface voltmeter. Before measurement, place the measurement panel equipped with the sample in an environment of 30°C, 80%RH for more than 1 hour.
[0239] The measurement conditions were set as follows.
[0240] Charging time: 0.1 seconds
[0241] Measuring time: 1800 seconds
[0242] Measuring interval: 1 second
[0243] Discharge polarity:-
[0244] Electrode: Yes
[0245] The initial potential was set to -600 V, and the surface potential change immediately after charging was measured. The results were fitted into the following equation to determine the charge decay rate coefficient α.
[0246] V t =V0exp(-αt 1 / 2 )
[0247] V t : Surface potential at time t (V)
[0248] V0: Initial surface potential (V)
[0249] t: time after charging (seconds)
[0250] α: Charge decay rate coefficient
[0251] Number average particle size of primary particles of inorganic fine particles
[0252] The number average particle diameter of primary particles of the inorganic fine particles is measured using an S-4800 Hitachi ultra-high resolution field emission scanning electron microscope (FE-SEM) (Hitachi High-Technologies).
[0253] After the inorganic fine particles are mixed, the toner is measured.
[0254] The magnification was set to 50,000, a photograph was taken and further magnified twice, and the maximum diameter (long axis diameter) a and the minimum diameter (short axis diameter) b of the inorganic fine particles were measured from the resulting FE-SEM photograph, and (a+b) / 2 was regarded as the particle size of these particles. The diameters of 100 randomly selected inorganic fine particles were measured, and the average value was calculated and regarded as the number average diameter of the primary particles of the inorganic fine particles.
[0255] Method for measuring the content ratio of each monomer unit in the first resin
[0256] Pass under the following conditions 1 H-NMR measures the content ratio of each monomer unit in the first resin.
[0257] Measuring unit: FT NMR unit JNM-EX400 (JEOL Ltd.)
[0258] Measuring frequency: 400MHz
[0259] Pulse condition: 5.0μs
[0260] Frequency range: 10500Hz
[0261] Number of points: 64
[0262] Measuring temperature: 30℃
[0263] Sample: 50 mg of a measurement sample was placed in a sample tube with an inner diameter of 5 mm, deuterated chloroform (CDCl3) was added as a solvent, and it was dissolved in a constant temperature bath at 40°C to prepare.
[0264] In the obtained 1 In the H-NMR chart, among the peaks attributable to the constituent elements of the first monomer unit, a peak independent of peaks attributable to constituent elements of monomer units from other sources is selected, and the integrated value S1 of the peak is calculated.
[0265] Similarly, a peak independent of peaks of constituent elements attributed to monomer units of other origins is selected from the peaks of constituent elements attributed to the second monomer unit, and the integrated value S2 of the peak is calculated.
[0266] When the first resin contains the third monomer unit, a peak independent of peaks of constituent elements attributed to monomer units of other origins is selected from peaks of constituent elements attributed to the third monomer unit, and an integrated value S3 of the peak is calculated.
[0267] The content of the first monomer unit is determined as follows using the integrated values S1, S2, and S3: n1, n2, and n3 are the numbers of hydrogen atoms of the constituent element to which the observed peaks for each segment are attributed.
[0268] Content of the first monomer unit (mol%) =
[0269] {(S1 / n1) / ((S1 / n1)+(S2 / n2)+(S3 / n3))}×100.
[0270] The second and third monomer units are similarly determined as shown below.
[0271] Content of the second monomer unit (mol%) =
[0272] {(S2 / n2) / ((S1 / n1)+(S2 / n2)+(S3 / n3))}×100.
[0273] Content of the third monomer unit (mol%) =
[0274] {(S3 / n3) / ((S1 / n1)+(S2 / n2)+(S3 / n3))}×100.
[0275] When a polymerizable monomer containing no hydrogen atom in the constituent elements other than the vinyl group is used as the first resin,13 C-NMR 13 C is used as the measurement core in single pulse mode and is measured with 1 The ratio was calculated in the same manner as in H-NMR.
[0276] When a toner is manufactured by a suspension polymerization method, since the peaks of a release agent and other resins overlap, an independent peak may not be observed. Therefore, the ratio of monomer units derived from each polymerizable monomer in the first resin may not be calculated. In this case, the first resin ' can be manufactured and analyzed by performing similar suspension polymerization without using a release agent or other resins.
[0277] SP value calculation method
[0278] Such as SP 21 The equivalent SP value is determined as follows according to the calculation method proposed by Fedors.
[0279] The evaporation energy (Δei) (cal / mol) and molar volume (Δvi) (cm2) of the atoms or atomic groups in the molecular structure of each polymerizable monomer were determined from the table described in "Polym. Eng. Sci., 14 (2), 147-154 (1974)". 3 / mol), and (4.184×ΣΔei / ΣΔvi) 0.5 Considered as SP value (J / cm 3 ) 0.5 .
[0280] For the same atoms or atomic groups in the molecular structure of the polymerizable monomer having double bonds that are broken by polymerization, SP is calculated by a similar method. 21 .
[0281] Melting point measurement method
[0282] For example, the melting point of the resin is measured using DSC Q1000 (TA Instruments) under the following conditions.
[0283] Heating rate: 10℃ / min
[0284] Measurement start temperature: 20°C
[0285] Measurement end temperature: 180℃
[0286] The melting points of indium and zinc are used for temperature correction of the detection portion of the device, and the heat of fusion of indium is used for correction of the calorific value.
[0287] Specifically, 5 mg of the sample was accurately weighed into an aluminum pan and subjected to differential scanning calorimetry. An empty silver pan was used as a reference.
[0288] The peak temperature of the maximum endothermic peak during the first temperature increase was regarded as the melting point.
[0289] When there are multiple peaks, the maximum endothermic peak is the peak at which the amount of endothermic heat is the largest.
[0290] Method for measuring the peak molecular weight and weight average molecular weight of THF soluble matter of resin by GPC
[0291] The peak molecular weight and weight average molecular weight (Mw) of the THF-soluble matter of the resin such as the first resin or the second resin are measured by gel permeation chromatography (GPC) as follows.
[0292] First, the sample was dissolved in tetrahydrofuran (THF) at room temperature over a 24-hour period. The resulting solution was filtered through a solvent-resistant membrane filter (Maishori Disk, Tosoh Corp.) having a pore size of 0.2 μm to obtain a sample solution. The concentration of THF-solubles in the sample solution was adjusted to about 0.8% by mass. The sample solution was used for measurement under the following conditions.
[0293] System: HLC8120 GPC (Detector: RI) (Tosoh Corp.)
[0294] Chromatographic columns: Shodex KF-801, 802, 803, 804, 805, 806, 807 (7 in total) (Showa Denko)
[0295] Eluent: Tetrahydrofuran (THF)
[0296] Flow rate: 1.0mL / min
[0297] Oven temperature: 40.0℃
[0298] Sample injection volume: 0.10mL
[0299] A molecular weight calibration curve prepared using standard polystyrene resin (product name: TSK standard polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500, Tosoh Corp.) was used to calculate the molecular weight of the sample.
[0300] Method for measuring molecular weight of THF-soluble matter of toner
[0301] 0.5 mg of the toner to be tested is dissolved in 1 g of THF and dispersed by ultrasonication, and then the concentration is adjusted to 0.5%, and the dissolved components are measured by GPC.
[0302] HLC-8120GPC and SC-8020 (Tosoh) were used as GPC units, two TSK gels and Super HM-H columns (Tosoh, 6.0 mm ID×15 cm) were used as columns, and THF was used as an eluent.
[0303] As for the test conditions, the test was performed using a refractive index (RI) detector at a sample concentration of 0.5%, a flow rate of 0.6 ml / min, a sample injection amount of 10 μl, and a measurement temperature of 40°C.
[0304] A calibration curve was also prepared using Tosoh TSK standard polystyrenes A-500, F-1, F-10, F-80, F-380, A-2500, F-4, F-40, F-128 and F-700 (10 samples in total).
[0305] Method for measuring the softening point of resin
[0306] The softening point of the resin is measured using a constant load extrusion capillary rheometer (Shimadzu Corporation, CFT-500D Flowtester flow characteristics evaluation device) according to the attached manual. Using this device, the temperature of the measurement sample contained in the barrel is raised to melt the sample, and a certain load is applied to the measurement sample from above with a piston, and the molten measurement sample is extruded through a die at the bottom of the barrel, and then a flow curve can be obtained, which shows the relationship between the temperature and the amount of descent of the piston during this process.
[0307] In the present invention, the "1 / 2 method melting temperature" as described in the manual attached to the CFT-500D Flowtester flow characteristics evaluation apparatus is taken as the softening point.
[0308] The melting temperature of the 1 / 2 method is calculated as follows.
[0309] Half of the difference between the piston descent at the end of outflow (outflow end point, given as "Smax") and the piston descent at the start of outflow (lowest point, given as "Smin") is determined and given as X (X = (Smax-Smin) / 2). The temperature in the flow curve when the piston descent is the sum of X and Smin is the melting temperature of the 1 / 2 method.
[0310] For the measurement sample, about 1.0 g of the resin is compression-molded with a tablet molding press (eg, NPa Systems Co., Ltd., NT-100H) at about 10 MPa for about 60 seconds at 25° C. to obtain a cylindrical sample with a diameter of about 8 mm.
[0311] The specific operation of the measurement is carried out according to the device manual.
[0312] The measurement conditions of CFT-500D are as follows.
[0313] Test mode: Heating method
[0314] Starting temperature: 50℃
[0315] Reaching temperature: 200℃
[0316] Measuring interval: 1.0℃
[0317] Heating rate: 4.0℃ / min
[0318] Piston cross-sectional area: 1.000cm 2
[0319] Test load (piston load): 10.0kgf (0.9807MPa)
[0320] Warm-up time: 300 seconds
[0321] Die hole diameter: 1.0mm
[0322] Mold length: 1.0mm
[0323] Measurement of glass transition temperature (Tg) of resin
[0324] The glass transition temperature (Tg) was measured using a differential scanning calorimeter (TA Instruments, Q2000) according to ASTM D3418-82.
[0325] The melting points of indium and zinc are used for temperature correction of the detection part of the device, and the heat of fusion of indium is used for calibrating the calorimetric value.
[0326] Specifically, 3 mg of a sample was accurately weighed, placed in an aluminum pan, and measured using an empty aluminum pan as a reference under the following conditions.
[0327] Heating rate: 10℃ / min
[0328] Measurement start temperature: 30°C
[0329] Measurement end temperature: 180℃
[0330] During the measurement, the temperature was first raised to 180°C and held for 10 minutes, then lowered to 30°C at a rate of 10°C / min, and then raised again. During this second temperature increase, the specific heat change was obtained in the temperature range of 30°C to 100°C. The glass transition temperature (Tg) is the intersection of the differential thermal curve and the midline between the baselines before and after the specific heat change occurs.
[0331] Acid value measurement method
[0332] The acid value is the number of mg of potassium hydroxide required to neutralize the acid component contained in 1 g of a sample. According to JIS K 0070-1992, the acid value is measured as follows.
[0333] (1) Reagent preparation
[0334] A phenolphthalein solution was obtained by dissolving 1.0 g of phenolphthalein in 90 mL of ethanol (95% by volume), and adding ion-exchanged water to a total of 100 mL.
[0335] 7g of special grade potassium hydroxide is dissolved in 5mL water, and by adding ethanol (95 volume %), it is made into 1L.It is placed in an alkali-resistant container, avoid contact with carbon dioxide etc. simultaneously, stand for 3 days, filter to obtain potassium hydroxide solution.The potassium hydroxide solution obtained is stored in an alkali-resistant container.The factor of this potassium hydroxide solution is determined by the amount of potassium hydroxide solution required for neutralization when 25mL of 0.1mol / L hydrochloric acid is put into a conical flask, adding a few drops of phenolphthalein solution and titrating with potassium hydroxide solution.0.1mol / L hydrochloric acid is prepared according to JIS K 8001-1998.
[0336] (2) Operation
[0337] (A) Main test
[0338] 2.0 g of the crushed sample was accurately weighed into a 200 mL conical flask, and 100 mL of a mixed solution of toluene: ethanol (2:1) was added to dissolve the sample over a 5-hour period. A few drops of phenolphthalein solution were then added as an indicator, and titration was performed using potassium hydroxide solution. The titration endpoint was considered to be when the light pink color of the indicator lasted for 30 seconds.
[0339] (B) Blank test
[0340] Titration was performed by the same procedure, but without using any sample (ie, only using a toluene:ethanol (2:1) mixed solution).
[0341] (3) The acid value was calculated by substituting the obtained result into the following formula:
[0342] A=[(CB)×f×5.61] / S
[0343] Where A is the acid value (mg KOH / g), B is the amount of potassium hydroxide solution added in the blank test (mL), C is the amount of potassium hydroxide solution added in the main test (mL), f is the factor of potassium hydroxide solution, and S is the mass of the sample (g).
[0344] Measuring method of coverage of inorganic fine particles
[0345] To determine the coverage of the inorganic fine particles, surface images of toner particles taken using an S-4800 Hitachi ultra-high resolution field emission scanning electron microscope (SEM, Hitachi High-Technologies) were analyzed using image analysis software (Image-Pro Plus ver. 5.0, Nippon Roper).
[0346] The inorganic fine particles present on the surfaces of the toner particles are observed using the SEM apparatus.
[0347] During observation, a position where the surface of the toner particles is as smooth as possible is selected.
[0348] An image in which inorganic fine particles are extracted only on the toner particle surface is binarized, and the ratio of the area occupied by the inorganic fine particles relative to the area of the toner particle surface is calculated. The same operation is performed for 10 toner particles, and the arithmetic mean is calculated.
[0349] When the toner contains a plurality of external additives, specific inorganic fine particles can be distinguished by the following method.
[0350] The inorganic fine particles are separated from the toner by the above method.
[0351] When various inorganic fine particles are added, they are classified by centrifugation.
[0352] The collected inorganic fine particles can be measured by FT-IR and NMR to sort out the inorganic fine particles in which a compound having an alkyl group is present.
[0353] Weight average particle size of toner particles (D4)
[0354] A Multisizer (registered trademark) 3 CoulterCounter precision particle size distribution analyzer (Beckman Coulter, Inc.) based on the pore resistance method and equipped with a 100 μm orifice tube was used. The accompanying dedicated Beckman Coulter Multisizer 3 software version 3.51 (Beckman Coulter, Inc.) was used to set the measurement conditions and analyze the measurement data. The measurement was performed using 25,000 effective measurement channels, and the measurement data was analyzed to calculate the weight-average particle size (D4) of the colorant particles (or colorant).
[0355] The aqueous electrolyte solution used in the measurement may be, for example, a solution of special grade sodium chloride dissolved in ion exchange water to a concentration of about 1% by mass, such as ISOTON II (Beckman Coulter, Inc.).
[0356] Prior to measurement and analysis, dedicated software settings were performed as follows.
[0357] On the "Standard Measurement Method (SOM) Change" screen of the dedicated software, the total count in the control mode was set to 50,000 particles, the number of measurements was set to 1, and the Kd value was set to the value obtained using "Standard Particles 10.0 μm" (Beckman Coulter, Inc.). The threshold noise level was automatically set by pressing the "Threshold / Noise Level Measurement Button". The current was set to 1600 μA, the gain was set to 2, the electrolyte solution was set to ISOTON II, and the inlet tube flushing was checked after the measurement.
[0358] On the "Conversion Settings from Pulse to Particle Size" screen of the dedicated software, the element interval is set to logarithmic particle size, the particle size element is 256, and the particle size range is 2 μm to 60 μm.
[0359] The specific measurement method is as follows.
[0360] (1) Add about 200 mL of electrolyte aqueous solution to a 250 mL round-bottom beaker dedicated to Multisizer 3, place the beaker on the sample stage, and stir it counterclockwise at 24 rpm with a stirring rod. Then use the "mouth tube flushing" function of the dedicated software to remove contaminants and bubbles in the mouth tube.
[0361] (2) 30 mL of the same aqueous electrolyte solution was placed in a 100 mL flat-bottom glass beaker, and about 0.3 mL of "Contaminon N" (a 10 mass % aqueous solution of a pH 7 neutral detergent for washing precision instruments, containing a nonionic surfactant, an anionic surfactant and an organic builder, manufactured by Wako Pure Chemical Industries) diluted 3 times by mass with ion exchange water was added.
[0362] (3) A specific amount of ion-exchanged water was placed in the water tank of an ultrasonic disperser (Ultrasonic Dispersion System Tetora 150, Nikkaki Bios), and then about 2 mL of Contaminon N was added to the water tank. The ultrasonic disperser had an electrical output of 120 W and was equipped with two built-in oscillators with an oscillation frequency of 50 kHz and phases shifted by 180° from each other.
[0363] (4) The beaker of (2) above is placed in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. The height position of the beaker is adjusted so that the resonance state of the liquid surface of the aqueous electrolyte solution in the beaker is maximized.
[0364] (5) While about 10 mg of the toner is added little by little to the electrolyte aqueous solution and dispersed, the electrolyte aqueous solution in the beaker of (4) is exposed to ultrasonic waves. Then, ultrasonic dispersion is continued for another 60 seconds. During the ultrasonic dispersion, the water temperature in the tank is appropriately adjusted to 10° C. to 40° C.
[0365] (6) The electrolyte aqueous solution of (5) in which the toner is dispersed is dropped into the round bottom beaker of (1) placed on the sample stage with a pipette and adjusted to a measurement concentration of about 5%. Then, measurement is performed until the number of particles measured reaches 50,000.
[0366] (7) Analyze the measurement data using the dedicated software included with the device, and calculate the weight average particle size (D4). When setting the graph / volume % in the dedicated software, the weight average particle size (D4) is the "average diameter" on the "Analysis / Volume Statistics (Arithmetic Mean)" screen.
[0367] Method for observing toner cross section and method for analyzing matrix and domain
[0368] First prepare the slices as a reference sample for abundance.
[0369] First, the first resin (crystalline resin) is fully dispersed in a visible light curable resin (Aronix LCR series D800) and cured by exposure to short wavelength light. The resulting cured resin is cut with an ultrathin slicer equipped with a diamond knife to prepare a 250 nm sample slice. A sample of the second resin (non-crystalline resin) is prepared in the same manner.
[0370] The first resin and the second resin were mixed at a ratio of 0 / 100, 30 / 70, 70 / 30 and 0 / 100, and melt-kneaded to prepare a kneaded mixture. They were similarly dispersed in a visible light curable resin and cut to prepare a sample slice.
[0371] Next, these reference samples were observed in cross section by TEM-EDX using a transmission electron microscope (JEOL Ltd., JEM-2800 electron microscope), and element mapping was performed by EDX. The mapped elements were carbon, oxygen, and nitrogen.
[0372] The mapping conditions are as follows.
[0373] Accelerating voltage: 200 kV
[0374] Electron beam exposure size: 1.5nm
[0375] Live time limit: 600 seconds
[0376] Dead time: 20 to 30
[0377] Mapping resolution: 256×256
[0378] Based on the spectral intensity of each element (average of 10 nm square area), (oxygen element intensity / carbon element intensity) and (nitrogen element intensity / carbon element intensity) were calculated, and a calibration curve of the mass ratio of the first and second resins was prepared. When the monomer unit of the first resin contained nitrogen, the subsequent test was performed using the (nitrogen element intensity / carbon element intensity) calibration curve.
[0379] The toner samples were then analyzed.
[0380] First, the toner is fully dispersed in a visible light curable resin (Aronix LCR Series D800) and cured by exposure to short wavelength light. The resulting cured resin is cut with an ultrathin slicer equipped with a diamond knife to prepare a 250nm sample slice. Then a transmission electron microscope (JEOL Ltd., JEM-2800 electron microscope) is used to observe the cut sample by TEM-EDX. The cross-sectional image of the toner particles is obtained and element mapping is performed by EDX. The mapped elements are carbon, oxygen and nitrogen.
[0381] The toner cross section for observation is selected as follows. First, the cross-sectional area of the toner is determined from the cross-sectional image, and the diameter of a circle having the same area as the cross-sectional area (equivalent circle diameter) is determined. Observation is limited to toner cross-sectional images in which the absolute value of the difference between the equivalent circle diameter and the weight-average particle size (D4) is within 1.0 μm.
[0382] For the domain confirmed in the observed image, (oxygen element intensity / carbon element intensity) and / or (nitrogen element intensity / carbon element intensity) are calculated based on the spectral intensity of each element (average of 10 nm squares), and the ratio of the first resin to the second resin is calculated based on comparison with the calibration curve. A domain in which the ratio of the second resin is 80% or more is considered to be a domain in the present disclosure.
[0383] The domain confirmed in the observed image was specified and binarized to determine the particle size of the domain present in the toner cross section. The particle size was taken as the domain diameter. It was measured at 10 points in each toner, and the calculated average value of the domains of the 10 toners was taken as the number average diameter. Image Pro PLUS (Nippon Roper KK) was used for binarization.
[0384] Method for separating materials in toner
[0385] Each material contained in the toner can be separated from the toner by utilizing the difference in solubility of each material in the solvent.
[0386] First separation: The toner is dissolved in methyl ethyl ketone (MEK) at 23° C., and the soluble matter (second resin) is separated from the insoluble matter (first resin, releasing agent, colorant, inorganic fine particles, etc.).
[0387] Second separation: The insoluble matter (first resin, releasing agent, colorant, inorganic fine particles, etc.) obtained in the first separation is dissolved in 100°C MEK, and the soluble matter (first resin, releasing agent) is separated from the insoluble matter (colorant, inorganic fine particles, etc.).
[0388] Third separation: The soluble matter (first resin, release agent) obtained in the second separation was dissolved in chloroform at 23° C. and separated into a soluble matter (first resin) and an insoluble matter (release agent).
[0389] Including the third resin
[0390] First separation: The toner is dissolved in methyl ethyl ketone (MEK) at 23° C., and solubles (second resin, third resin) are separated from insolubles (first resin, release agent, colorant, inorganic fine particles, etc.).
[0391] Second separation: The soluble matter (second resin, third resin) obtained in the first separation was dissolved in toluene at 23° C. and separated into a soluble matter (third resin) and an insoluble matter (second resin).
[0392] Third separation: The insoluble matter (first resin, release agent, colorant, inorganic fine particles, etc.) obtained in the first separation was dissolved in 100°C MEK and separated into soluble matter (first resin, release agent) and insoluble matter (colorant, inorganic fine particles, etc.).
[0393] Fourth separation: The soluble matter (first resin, release agent) obtained in the third separation was dissolved in chloroform at 23° C. and separated into a soluble matter (first resin) and an insoluble matter (release agent).
[0394] Measurement of Contents of First Resin and Second Resin in Binder Resin in Toner
[0395] The masses of the soluble matter and the insoluble matter obtained in the above separation step are measured to calculate the contents of the first resin and the second resin in the binder resin in the toner.
[0396] Example
[0397] The present invention is illustrated using the following examples. However, these are by no means limiting the present invention in any way. Unless otherwise stated, the parts in the following formulations are based on mass.
[0398] Production Example of Inorganic Fine Particles 1
[0399] The metatitanic acid obtained by the sulfuric acid method was subjected to iron removal bleaching, sodium hydroxide aqueous solution was added to make the pH reach 9.0, desulfurization was carried out, and then the pH was neutralized to 5.8 with hydrochloric acid, and the product was filtered and washed. Water was added to the washed filter cake to obtain a slurry containing 1.5 mol / L of TiO2, and hydrochloric acid was added to adjust the pH to 1.5 for peptization treatment.
[0400] The desulfurized and peptized metatitanic acid was collected as TiO2 and placed in a 3L reaction vessel. An aqueous strontium chloride solution was added to the peptized metatitanic acid slurry to obtain a SrO / TiO2 molar ratio of 1.15, and then the TiO2 concentration was adjusted to 0.8 mol / L. It was then heated to 90°C with stirring and mixing, and 444 mL of a 10 mol / L sodium hydroxide aqueous solution was added over a 45 minute period while nitrogen was microbubbled at 600 mL / min, after which the slurry was stirred at 95°C for 1 hour while nitrogen was microbubbled at 400 mL / min.
[0401] The reaction slurry was then stirred and cooled to 15° C. while passing cooling water at 10° C. through the jacket of the reaction vessel, hydrochloric acid was added until the pH was 2.0, and stirring was continued for 1 hour. The resulting precipitate was washed by decantation, and 5.0% by mass of sodium stearate was dissolved in water relative to the solid content and added in the form of an aqueous solution, stirring was continued for 2 hours, and then the pH was adjusted to 6.5 with hydrochloric acid, and stirring was continued for 1 hour to precipitate stearic acid on the surface of strontium titanate.
[0402] It was then filtered and washed, and the resulting filter cake was left in an atmosphere at 120° C. for 10 hours and pulverized in a jet mill until no aggregates remained, thereby obtaining Inorganic Fine Particles 1. In the measurement of Inorganic Fine Particles 1 by powder X-ray diffraction, a diffraction peak of strontium titanate was observed. The physical properties are shown in Table 1.
[0403] Production Example of Inorganic Fine Particles 2
[0404] The aqueous titanium oxide slurry obtained by hydrolyzing the titanium sulfate aqueous solution was washed with an alkali aqueous solution. Next, hydrochloric acid was added to the aqueous titanium oxide slurry to adjust the pH to 0.65, obtaining a titanium dioxide sol dispersion. NaOH was added to the titanium dioxide sol dispersion to adjust the pH of the dispersion to 4.5, and washing was repeated until the conductivity of the supernatant was 70 μS / cm.
[0405] 0.97 times the molar amount of Sr(OH)2.8H2O was added to the hydrous titanium oxide, which was then placed in a SUS reaction vessel and replaced with nitrogen. Distilled water was then added to obtain a concentration of 0.1 to 2.0 mol / liter (in terms of SrTiO3).
[0406] The dispersion was sprayed into an 80-liter combustion reaction tank through a fine particle nozzle together with oxygen and propane gas and burned, and then collected by a filter to obtain fine particles. Pure water was added to the obtained fine particles, 6 mol / liter hydrochloric acid was added to the obtained slurry to adjust the pH to 2.0, 3.6 parts of calcium stearate were added relative to 100 parts of solids, and the mixture was stirred for 18 hours. It was then neutralized with a 4 mol / liter sodium hydroxide aqueous solution, stirred for 2 hours, and then separated by filtration, followed by drying in an atmosphere at 120°C for 8 hours to obtain inorganic fine particles 2.
[0407] In powder X-ray analysis, the inorganic fine particles 2 showed a strontium titanate diffraction peak. The physical properties are shown in Table 1.
[0408] Production Example of Inorganic Fine Particles 3
[0409] Inorganic fine particles 3 were obtained according to the production example of inorganic fine particles 1, except that calcium chloride was used instead of strontium chloride and nitrogen microbubbling was not performed. The physical properties are shown in Table 1.
[0410] Production Example of Inorganic Fine Particles 4
[0411] 200 parts of zinc oxide were added to an aqueous hydrochloric acid solution consisting of 500 parts of 35 mass % hydrochloric acid and 700 parts of pure water, and the zinc oxide was completely dissolved to prepare an aqueous zinc chloride solution. At the same time, 460 parts of ammonium carbonate were dissolved in 3000 parts of pure water to prepare an aqueous solution of ammonium bicarbonate, respectively. The aqueous zinc chloride solution was added to the aqueous ammonium bicarbonate solution over a period of 60 minutes to produce a precipitate. The precipitate was fully washed, separated from the liquid phase, and dried at 130° C. for 5 hours.
[0412] Next, the dried powder was crushed in an agate mortar. While supplying a mixed gas of 0.21 L / min of nitrogen and 0.09 L / min of hydrogen, the crushed powder was heated to 500° C. at a rate of 200° C. / hour. It was kept as it was for 2 hours, then cooled to room temperature, after which sodium stearate was dissolved in water in an amount of 5.0% by mass of the obtained zinc oxide fine particles and added in the form of an aqueous solution, stirring was continued for 2 hours, hydrochloric acid was added to adjust the pH to 6.5, and stirring was continued for 1 hour to allow stearic acid to precipitate on the surface of the zinc oxide fine particles.
[0413] It was then filtered and washed to obtain a filter cake, which was subsequently dried in an atmosphere of 120° C. for 10 hours and pulverized in a jet mill until no aggregates remained to obtain Inorganic Fine Particles 4. The physical properties are shown in Table 1.
[0414] Production Example of Inorganic Fine Particles 5
[0415] The hydrated titanium oxide slurry obtained by thermal hydrolysis of an aqueous titanyl sulfate solution was neutralized to pH 7 with aqueous ammonia, filtered and washed to obtain a filter cake, and the titanium oxide of the filter cake was peptized with hydrochloric acid to obtain an anatase-type titanium dioxide sol having an average primary particle size of 7 nm.
[0416] Ilmenite ore containing 50% by mass of TiO2 equivalent was used as a raw material, which was dried at 150°C for 2 hours and dissolved by adding sulfuric acid to obtain a TiOSO4 aqueous solution. It was concentrated, and 4.0 parts of the above-mentioned anatase-type titanium dioxide sol in terms of TiO2 equivalent was added as a seed to 100 parts of TiO2 equivalent, and hydrolyzed at 120°C to obtain a slurry of TiO(OH)2 containing impurities.
[0417] The slurry was repeatedly washed with water at pH 5 to 6 to sufficiently remove sulfuric acid, FeSO4 and impurities. Thus, a slurry of high-purity metatitanic acid [TiO(OH)2] was obtained.
[0418] The metatitanic acid was heat treated at 270°C for 6 hours and then fully pulverized to obtain a product having a BET specific surface area of 50 m 2 / g and anatase type crystalline titanium oxide fine particles with a number average particle size of 50 nm.
[0419] Next, sodium stearate in an amount of 5.0 mass % of anatase-type titanium oxide fine particles was added in the form of an aqueous solution dissolved in water, stirring was continued for 2 hours, hydrochloric acid was added to adjust the pH to 6.5, and stirring was continued for 1 hour to allow stearic acid to precipitate on the surface of the titanium oxide fine particles.
[0420] It was then filtered and washed, and the resulting filter cake was dried in an atmosphere of 120° C. for 10 hours and then pulverized in a jet mill until no aggregates remained to obtain Inorganic Fine Particles 5. The physical properties are shown in Table 1.
[0421] Production Example of Inorganic Fine Particles 6
[0422] After obtaining anatase type titanium oxide fine particles in the production example of inorganic fine particles 5, the following operation was performed. Hydrochloric acid was added to the dispersion liquid of anatase type titanium oxide fine particles to adjust the pH to 6.5, 0.5 parts of octyl-modified silicone oil (FZ-3196, Dow Corning Corp.) was added relative to 100 parts of anatase type titanium oxide fine particles, and the mixture was kept under stirring for 1 hour.
[0423] It was then filtered and washed to obtain a filter cake, which was then dried in an atmosphere at 120° C. for 10 hours and pulverized in a jet mill to eliminate aggregates of titanium particles and obtain Inorganic Fine Particles 6. The physical properties are shown in Table 1.
[0424] Production Example of Inorganic Fine Particles 7
[0425] After obtaining anatase type titanium oxide fine particles in Production Example of Inorganic Fine Particles 5, the following operation was performed. The dispersion of anatase type titanium oxide fine particles was adjusted to 50° C., and hydrochloric acid was added to adjust the pH to 2.5, then 5 parts of stearyl trimethoxysilane was added relative to 100 parts of the solid, and the mixture was kept under stirring for 6 hours.
[0426] The pH was then adjusted to 6.5 with an aqueous sodium hydroxide solution, stirring was continued for 1 hour, and the mixture was filtered to obtain a filter cake, which was dried in an atmosphere at 120° C. for 10 hours. This was pulverized in a jet mill until the aggregates of the titanium oxide fine particles were eliminated to obtain Inorganic Fine Particles 7. The physical properties are shown in Table 1.
[0427] Production Example of Inorganic Fine Particles 8
[0428] Inorganic fine particles 8 were obtained according to the production example of inorganic fine particles 7 except that isobutyltrimethoxysilane was used instead of stearyltrimethoxysilane.
[0429] Production Example of Inorganic Fine Particles 9
[0430] After obtaining anatase-type titanium oxide fine particles in the manufacturing example of inorganic fine particles 5, the following operation is performed. The anatase-type titanium oxide fine particles are placed in an autoclave together with a 20 / 80 vol% 1-tetracosanol / n-hexane mixed solution. It is heated at 240°C and a pressure of 2.8 MPa for 1 hour. It is then filtered and washed to obtain a filter cake, which is dried in an atmosphere at 120°C for 10 hours. It is pulverized in a jet mill until the aggregates of the titanium oxide fine particles are eliminated to obtain inorganic fine particles 9. The physical properties are shown in Table 1.
[0431] Production Example of Inorganic Fine Particles 10
[0432] The inorganic fine particles 10 were obtained according to the production example of the inorganic fine particles 9 except that n-octacosanol was used instead of 1-tetracosanol.
[0433] Production Example of Inorganic Fine Particles 11
[0434] Inorganic fine particles 11 were obtained according to the production example of inorganic fine particles 9 except that n-propanol was used instead of 1-tetracosanol.
[0435] Production Example of Inorganic Fine Particles 12
[0436] In the production example of inorganic fine particles 4, the production was carried out by the following method using zinc oxide fine particles before adding 5.0 mass % of sodium stearate aqueous solution.
[0437] The zinc oxide fine particles were placed in an autoclave together with a 20 / 80 volume % n-propanol / n-hexane mixed solution. They were heated at 240° C. and a pressure of 2.8 MPa for 1 hour. They were then filtered and washed to obtain a filter cake, which was dried in an atmosphere at 120° C. for 10 hours. They were then pulverized in a jet mill until the aggregates of the zinc oxide fine particles were eliminated to obtain inorganic fine particles 12.
[0438] Production Example of Inorganic Fine Particles 13
[0439] Inorganic fine particles 13 were obtained according to the production example of inorganic fine particles 11 except that the ratio of the mixed solution of n-propanol / n-hexane was changed to 5 / 95.
[0440] Production Example of Inorganic Fine Particles 14
[0441] Inorganic fine particles 14 were obtained according to the production example of inorganic fine particles 5 except that the treatment with the sodium stearate aqueous solution was not performed. The physical properties are shown in Table 1.
[0442] Production Example of Inorganic Fine Particles 15
[0443] The physical properties are shown in Table 1, except that antimony-doped tin oxide fine particles (SN-100P, Ishihara Sangyo Kaisha, Ltd.) were used instead of anatase-type titanium oxide fine particles.
[0444] Production Example of Inorganic Fine Particles 16
[0445] Inorganic fine particles 16 were obtained according to the production example of inorganic fine particles 11 except that silica fine particles produced by the following method were used instead of anatase type titanium oxide fine particles.
[0446] A double-tube hydrocarbon-oxygen mixed burner capable of forming inner and outer flames is used as a combustion furnace. A dual-fluid nozzle for slurry injection is installed at the center of the burner, and a raw silicon compound is introduced. Hydrocarbon-oxygen combustion gas is sprayed from around the dual-fluid nozzle to form outer and inner flames as a reducing atmosphere.
[0447] The atmosphere, temperature, flame length, etc. are adjusted by controlling the amount and flow of combustion gas and oxygen. Silica fine particles are formed from silicon compounds in the flame and melted until the desired particle size is obtained. They are then cooled and collected in a bag filter to obtain silica fine particles.
[0448] [Table 1]
[0449]
[0450] In the table, “1.0E+10” means “1.0×10 10 ”.
[0451] Production Example of Crystalline Resin C1
[0452] Solvent: 100.0 parts of toluene
[0453] Monomer composition: 100.0 parts
[0454] (The monomer composition is a mixture of the following behenyl acrylate, methacrylonitrile, styrene and acrylic acid in the following proportions)
[0455] (Behenyl acrylate (first polymerizable monomer): 67.0 parts (28.9 mol%))
[0456] (Methacrylonitrile (second polymerizable monomer): 21.5 parts (52.7 mol%))
[0457] (Styrene (third polymerizable monomer): 11.0 parts (17.3 mol%))
[0458] (Acrylic acid: 0.5 parts (1.1 mol%))
[0459] Polymerization initiator: 0.5 parts of tert-butyl peroxypivalate (NOF Corp. Perbutyl PV)
[0460] These materials are placed in a nitrogen atmosphere in a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer and a nitrogen inlet tube. The interior of the reaction vessel is stirred at 200 rpm while the mixture is heated to 70 ° C, and the polymerization reaction is carried out for 12 hours to obtain a solution of a polymer of the monomer composition dissolved in toluene. Next, the solution is cooled to 25 ° C, and then 1000.0 parts of methanol are added under stirring, and the methanol insoluble matter is precipitated. The resulting methanol insoluble matter is filtered out, washed with methanol, and vacuum dried at 40 ° C for 24 hours to obtain crystalline resin C1. The weight average molecular weight of crystalline resin C1 is 68400, the melting point is 62 ° C, and the acid value is 10 mg KOH / g.
[0461] In NMR analysis, the crystalline resin C1 contained 28.9 mol% of monomer units derived from behenyl acrylate, 53.8 mol% of monomer units derived from methacrylonitrile, and 17.3 mol% of monomer units derived from styrene. The content ratio of the first monomer unit was 67.0 mass%.
[0462] The SP value of the monomer unit derived from the second polymerizable monomer is 29.13 (J / cm 3 ) 0.5 .
[0463] Production Example of Crystalline Resin C2
[0464] 470 parts of toluene were placed in an autoclave, replaced with nitrogen, and the temperature was raised to 105° C. in a sealed state with stirring. While the internal temperature of the autoclave was controlled at 105° C., a mixture of 500 parts of behenyl acrylate (C22), 250 parts of styrene, 250 parts of acrylonitrile, 20 parts of methacrylic acid, 5 parts of alkylallyl sulfosuccinic acid sodium salt, 19 parts of 2-isocyanatoethyl acrylate, 3.7 parts of tert-butylperoxy-2-ethylhexanoate and 240 parts of toluene was dropped thereinto and polymerized over a period of 2 hours.
[0465] The reaction was continued for another 4 hours at the same temperature to complete the reaction, and then 16 parts of di-n-butylamine and 5 parts of bismuth catalyst (Nitto Kasei Co., Ltd., Neostann U-600) were added, and the mixture was reacted at 90°C for 6 hours. The solvent was then removed at 100°C to obtain crystalline resin C2. The weight average molecular weight of crystalline resin C2 was 100000, the melting point was 46°C, and the acid value was 10 mg KOH / g. The content ratio of the first monomer unit was 49.0% by mass.
[0466] The SP value of the monomer unit derived from acrylonitrile is 22.75 (J / cm 3 ) 0.5 .
[0467] Production Example of Crystalline Resin C3
[0468] 138 parts of xylene were placed in an autoclave, replaced with nitrogen, and heated to 170° C. in a sealed state with stirring. While the internal temperature of the autoclave was controlled at 170° C., a mixed solution of 200 parts of behenyl acrylate (C22), 150 parts of styrene, 300 parts of acrylonitrile, 600 parts of vinyl acetate, 1.5 parts of di-tert-butyl peroxide and 100 parts of xylene was dropped therein over a period of 3 hours and polymerized.
[0469] After the dropwise addition, the drip line was washed with 12 parts of xylene. The polymerization was then completed by maintaining at the same temperature for 4 hours. The solvent was removed at 100° C. for 3 hours under a reduced pressure of 0.5 to 2.5 kPa to obtain a crystalline resin C3.
[0470] The crystalline resin C3 had a weight average molecular weight of 45,000, a melting point of 60° C., an acid value of 10 mg KOH / g, and a content ratio of the first monomer unit of 23.5% by mass.
[0471] The SP value of the monomer unit derived from vinyl acetate is 18.31 (J / cm 3 ) 0.5 .
[0472] Production Example of Crystalline Resin C4
[0473] Dodecanediol: 34.5 parts (0.29 mol; 100.0 mol % relative to the total molar number of the polyol)
[0474] Sebacic acid: 65.5 parts (0.28 mol; 100.0 mol % relative to the total molar number of the polycarboxylic acid)
[0475] These materials were weighed into a reaction tank equipped with a cooling tube, a stirrer, a nitrogen inlet tube and a thermocouple. The flask was then purged with nitrogen, the temperature was gradually raised under stirring, and the mixture was reacted at 140° C. for 3 hours while stirring.
[0476] ·2-Ethylhexanoate Tin: 0.5 parts
[0477] Then, the material was added, the pressure in the reaction container was reduced to 8.3 kPa, and the mixture was reacted for 4 hours while maintaining the temperature at 200° C., and then the reaction container was gradually opened to return the pressure to normal pressure, and crystalline resin C4 was obtained. The weight average molecular weight of crystalline resin C4 was 30,000, the melting point was 50° C., and the acid value was 10 mg KOH / g. The content ratio of the first monomer unit was 0% by mass.
[0478] Production Example of Crystalline Resin C5
[0479] 138 parts of xylene were placed in an autoclave and then purged with nitrogen, after which the temperature was raised to 170° C. with stirring in a sealed state. While the internal temperature of the autoclave was controlled at 170° C., a mixed solution of 450 parts of behenyl acrylate (C22), 150 parts of styrene, 150 parts of acrylonitrile, 1.5 parts of di-tert-butyl peroxide and 100 parts of xylene was dropped thereinto and polymerized over a period of 3 hours.
[0480] After the dropping, the dripping line was washed with 12 parts of xylene and then maintained at the same temperature for 4 hours to complete the polymerization. The solvent was removed at 100° C. for 3 hours under a reduced pressure of 0.5 to 2.5 kPa to obtain a crystalline resin C5.
[0481] The weight average molecular weight of the crystalline resin C5 was 14,000, the melting point was 60° C., the acid value was 0 mg KOH / g, and the content ratio of the first monomer unit was 60.0% by mass.
[0482] The SP value of the monomer unit derived from acrylonitrile is 22.75 (J / cm 3 )0.5 .
[0483] Production Example of Crystalline Resin C6
[0484] Crystalline resin C6 was obtained according to the production example of crystalline resin C3 except that the amount of behenyl acrylate (C22) was changed to 500 parts.
[0485] The weight average molecular weight of the crystalline resin C6 was 46,000, the melting point was 55° C., the acid value was 8 mg KOH / g, and the content ratio of the first monomer unit was 32.3% by mass.
[0486] Production Example of Crystalline Resin C7
[0487] Crystalline resin C7 was obtained according to the production example of crystalline resin C3 except that 200 parts of behenyl acrylate (C22) was changed to 500 parts of stearyl acrylate (C18).
[0488] The weight average molecular weight of the crystalline resin C7 was 38,000, the melting point was 50° C., the acid value was 3 mg KOH / g, and the content ratio of the first monomer unit was 32.3% by mass.
[0489] Production Example of Crystalline Resin C8
[0490] Crystalline resin C8 was obtained according to the production example of crystalline resin C3 except that the amount of behenyl acrylate (C22) was changed to 700 parts.
[0491] The crystalline resin C8 had a weight average molecular weight of 28,000, a melting point of 65° C., an acid value of 30 mg KOH / g, and a content ratio of the first monomer unit of 40.0% by mass.
[0492] Production Example of Non-Crystalline Resin A1
[0493] Polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: 73.4 parts (0.186 mol; 100.0 mol% relative to the total molar number of the polyol)
[0494] Terephthalic acid: 11.6 parts (0.070 mol; 45.0 mol% relative to the total moles of polycarboxylic acid)
[0495] Adipic acid: 6.8 parts (0.047 mol; 30.0 mol% relative to the total moles of polycarboxylic acid)
[0496] ·Di(2-ethylhexyl)tin: 0.5 parts
[0497] These materials were weighed into a reaction tank equipped with a cooling tube, a stirrer, a nitrogen introduction tube, and a thermocouple. The inside of the flask was purged with nitrogen, the temperature was gradually increased under stirring, and the mixture was reacted while stirring at 200° C. for 2 hours.
[0498] The pressure in the reaction tank was then reduced to 8.3 kPa and maintained for 1 hour, after which the temperature was reduced to 180° C. and the pressure was returned to atmospheric pressure (first reaction step).
[0499] Trimellitic anhydride: 8.2 parts (0.039 mol; 25.0 mol% relative to the total moles of polycarboxylic acid)
[0500] Tert-butyl catechol (polymerization inhibitor): 0.1 part
[0501] Then, the above materials were added, the pressure in the reaction tank was reduced to 8.3 kPa, and the temperature was maintained at 160° C. while the mixture was reacted for 15 hours. The temperature was lowered to stop the reaction (second reaction step), and non-crystalline resin A1 was obtained. The obtained non-crystalline resin A1 had a peak molecular weight Mp of 11000, a glass transition temperature Tg of 58° C., and an acid value of 20 mgKOH / g.
[0502] Production Examples of Non-Crystalline Resins A2 and A4 to A9
[0503] Amorphous resins A2 and A4 to A9 were obtained by performing the same reaction as in the manufacturing example of the non-crystalline resin A1, except that the alcohol component or the carboxylic acid component and the molar ratio were changed as shown in Table 1. The mass parts of the raw materials were adjusted so that the total molar number of the alcohol component and the carboxylic acid component was the same as in the manufacturing example of the non-crystalline resin A1. The physical properties of the obtained non-crystalline resins are shown in Tables 2-1 and 2-2.
[0504] Production Example of Non-Crystalline Resin A3
[0505] Polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane: 75.4 parts (0.192 mol; 100.0 mol% relative to the total molar number of the alcohol component)
[0506] Terephthalic acid: 17.8 parts (0.111 mol; 70.0 mol % relative to the total moles of the carboxylic acid component)
[0507] Succinic acid: 3.4 parts (0.024 mol; 15.0 mol % relative to the total moles of the carboxylic acid component)
[0508] Oxalic acid: 3.4 parts (0.024 mol; 15.0 mol % relative to the total moles of the carboxylic acid component)
[0509] ·Di(2-ethylhexyl)tin: 1.0 part per 100 parts of the total monomer components
[0510] These materials were weighed into a reaction tank equipped with a cooling tube, a stirrer, a nitrogen introduction tube and a thermocouple. The inside of the flask was purged with nitrogen, the temperature was gradually increased under stirring, and the mixture was reacted while stirring at 200° C. for 5 hours to obtain non-crystalline resin A3.
[0511] The peak molecular weight of the obtained non-crystalline resin A3 by GPC was 4700. The glass transition temperature was 56° C. and the acid value was 7 mg KOH / g.
[0512] Production Example of Amorphous Resins A10 and A11
[0513] Amorphous resins A10 and A11 were obtained by performing the same reaction as in the manufacturing example of the amorphous resin A3, except that the alcohol component or the carboxylic acid component and the molar ratio were changed as shown in Table 1. The mass parts of the raw materials were adjusted so that the total number of moles of the alcohol component and the carboxylic acid component was the same as in the manufacturing example of the amorphous resin A3. The physical properties are shown in Tables 2-1 and 2-2.
[0514] Production Example of Non-Crystalline Resin A12
[0515] 50 parts of bisphenol A propylene oxide 2 mole adduct, 50 parts of bisphenol A ethylene oxide 2 mole adduct, 10 parts of fumaric acid, 65 parts of terephthalic acid, 10 parts of acrylic acid and 15 parts of tin (II) dioctoate were placed in a 4-necked flask equipped with a thermometer, a stirrer, a condenser and a nitrogen inlet tube, and polymerized at 230° C. for 4.5 hours under a nitrogen atmosphere.
[0516] Once it has cooled to 160°C, 25 parts of trimellitic acid are added.
[0517] Next, a mixture of 450 parts of styrene, 200 parts of 2-ethylhexyl acrylate and 30 parts of dicumyl peroxide as a polymerization initiator was dripped therein at 160° C. over a period of 2 hours. After the dripping was completed, the temperature was raised to 200° C. and the mixture was reacted for 3 hours to obtain a non-crystalline resin A12 having a softening point of 115° C.
[0518] The obtained non-crystalline resin A12 had a peak molecular weight of 9,000 as determined by GPC, a glass transition temperature of 60° C., and an acid value of 5 mg KOH / g.
[0519] Production Example of Non-Crystalline Resin A13
[0520] Low molecular weight polypropylene (Sanyo Chemical Industries, Ltd., Viscol 660P): 10.0 parts (0.02 mol; 2.4 mol% relative to the total molar number of constituent monomers)
[0521] Xylene: 25.0 parts
[0522] These materials were weighed into a reaction tank equipped with a cooling tube, a stirrer, a nitrogen inlet tube and a thermocouple. The flask was purged with nitrogen and the temperature was gradually raised to 175° C. under stirring.
[0523] Styrene: 68.0 parts (0.65 mol; 76.4 mol% relative to the total molar number of constituent monomers)
[0524] Cyclohexyl methacrylate: 5.0 parts (0.03 mol; 3.5 mol% relative to the total molar number of constituent monomers)
[0525] Butyl acrylate: 12.0 parts (0.09 mol; 11.0 mol% relative to the total molar number of constituent monomers)
[0526] Methacrylic acid: 5.0 parts (0.06 mol; 6.7 mol% relative to the total molar number of constituent monomers)
[0527] Xylene: 10.0 parts
[0528] ·Di-tert-butyl hexahydroperphthalate: 0.5 parts
[0529] These materials were then added dropwise over a period of 2.5 hours, and the mixture was stirred for a further 40 minutes. The solvent was then distilled off to obtain a non-crystalline resin A13 comprising a styrene acrylic polymer grafted onto a polyolefin.
[0530] The obtained non-crystalline resin A13 had a peak molecular weight of 11,000 as determined by GPC, a glass transition temperature of 62° C., and an acid value of 0.4 mg KOH / g.
[0531] [Table 2-1]
[0532]
[0533] The abbreviations in Table 2-1 are defined as follows.
[0534] BPA-PO (2.2): Bisphenol A propylene oxide 2.2 molar adduct
[0535] BPA-EO (2.2): Bisphenol A2 ethylene oxide 2.2 mole adduct
[0536] EG: Ethylene glycol
[0537] TFA: Terephthalic acid
[0538] TMA: trimellitic acid
[0539] FA: Fumaric acid
[0540] OA: Oxalic acid
[0541] SUA: Succinic Acid
[0542] AA: Adipic acid
[0543] SEA: Sebacic Acid
[0544] DCA: Dodecenylsuccinic anhydride
[0545] [Table 2-2]
[0546]
[0547] Tg is given in °C, acid value is given in mg KOH / g, and dielectric constant is pF / m at 2 kHz.
[0548] Production Example of Binder Resin 1
[0549] 32 parts of non-crystalline resin A6 and 68 parts of crystalline resin C1 were mixed and supplied to a twin-screw kneader (Kurimoto, Ltd., S5KRC kneader) at a rate of 52 kg / hour, and 1.0 part of tert-butyl peroxyisopropyl monocarbonate as a free radical reaction initiator (c) was supplied at a rate of 0.52 kg / hour, and the two were kneaded and extruded at 160°C, 90 rpm for 7 minutes to perform a crosslinking reaction, and then the pressure was reduced to 10 kPa from the exhaust port for mixing to remove the organic solvent. The mixed product was cooled to obtain a binder resin 1.
[0550] Production Examples of Binder Resins 2 to 21
[0551] Binder resins 2 to 21 were obtained according to the manufacturing example of the binder resin 1 except that the kinds and the mixing ratios of the non-crystalline resin and the crystalline resin were changed as shown in Table 3.
[0552] [Table 3]
[0553]
[0554] Preparation Example of Binder Resin 1 Fine Particle Dispersion Liquid
[0555] Toluene: (Wako Pure Chemical) 300 parts
[0556] ·Binder resin 1: 100 parts
[0557] These materials were weighed, mixed and dissolved at 90°C.
[0558] 5.0 parts of sodium dodecylbenzenesulfonate and 10.0 parts of sodium laurate were respectively added to 700 parts of ion exchange water and heated at 90° C. until dissolved.
[0559] The toluene solution and the aqueous solution were then mixed and stirred at 7000 rpm with a TK Robomix ultra-high speed stirring device (Primix Corp.), and thereafter emulsified at a pressure of 200 MPa with a high pressure impact disperser nanometer (Yoshida Kikai Co., Ltd.). Then, toluene was removed with an evaporator, and the concentration was adjusted with ion exchange water to obtain an aqueous dispersion of 20% by mass of fine particles of binder resin 1 (binder resin 1 fine particle dispersion).
[0560] The 50% particle diameter (D50) of the fine particles of the binder resin 1 based on volume distribution was measured using Nanotrac UPA-EX150 (Nikkiso Co., Ltd.) to find that it was 0.40 μm.
[0561] Preparation Example of Release Agent (Aliphatic Hydrocarbon Compound) Fine Particle Dispersion Liquid
[0562] Aliphatic hydrocarbon compound HNP-51 (Nippon Seiro) 100 parts
[0563] · Anionic surfactant Neogen RK (Daiichi Kogyo) 5 parts
[0564] ·395 parts of ion exchange water
[0565] These materials were accurately weighed, placed in a mixing container equipped with a stirrer, heated to 90°C, and then dispersed for 60 minutes by recirculation into Clearmix W-Motion (M Technique). The dispersion conditions were as follows.
[0566] Outer rotor diameter 3cm
[0567] · Clearance 0.3mm
[0568] Rotor speed 19000r / min
[0569] ·Screen rotation 19000r / min
[0570] After dispersion, it is cooled to 40°C under the conditions of a rotor speed of 1000 r / min, a sieve speed of 0 r / min, and a cooling rate of 10°C / min to obtain an aqueous dispersion (release agent (aliphatic hydrocarbon compound) fine particle dispersion) having a concentration of 20% by mass.
[0571] The 50% particle diameter (D50) on a volume basis of the fine particles of the releasing agent (aliphatic hydrocarbon compound) measured with a Nanotrac UPA-EX150 dynamic light scattering particle size distribution meter (Nikkiso) was 0.15 μm.
[0572] Production of colorant fine particle dispersion
[0573] ·Colorant 50.0 parts
[0574] (Cyan pigment, Dainichi Seika Pigment Blue 15:3)
[0575] ·Neogen RK anionic surfactant (Daiichi Kogyo Seiyaku) 7.5 parts
[0576] ·442.5 parts of ion exchange water
[0577] These materials were accurately weighed, mixed, dissolved and dispersed with a Nanomachine high pressure impact disperser (Yoshida Kikai) for about 1 hour to disperse the colorant and obtain an aqueous dispersion having a colorant fine particle concentration of 10 mass % (colorant fine particle dispersion).
[0578] The volume-based 50% particle diameter (D50) of the colorant fine particles measured with a Nanotrac UPA-EX150 dynamic light scattering particle size distribution analyzer (Nikkiso) was 0.20 μm.
[0579] Production Example of Toner Particles 1
[0580]
[0581] These materials were charged into a round bottom stainless steel flask and mixed. They were then dispersed using an Ultra Turrax T50 homogenizer (IKA) at a speed of 5000 r / min for 10 minutes. A 1.0% nitric acid aqueous solution was added to adjust the pH to 3.0, and the mixture was then heated to 58° C. in a heated water bath using a stirring blade while adjusting the number of revolutions so that the mixture could be stirred.
[0582] The volume average particle size of the formed aggregated particles was appropriately checked with Coulter Multisizer III, and once aggregated particles having a weight average particle size (D4) of about 6.00 μm were formed, the pH was adjusted to 9.0 with a 5% sodium hydroxide aqueous solution. The mixture was then heated to 75° C. while continuing to stir. The mixture was then kept at 75° C. for 1 hour to melt the aggregated particles.
[0583] It was then cooled to 50°C and kept for 3 hours to promote crystallization of the polymer.
[0584] The mixture was then cooled to 25° C., filtered and solid-liquid separated, and washed with ion-exchanged water. After washing, the mixture was dried with a vacuum dryer to obtain toner particles 1 having a weight average particle size (D4) of about 6.1 μm.
[0585] Production Examples of Toner Particles 2, 5 to 24 and 29 to 35
[0586] Toner particles 2, 5 to 24, and 29 to 35 were obtained according to the production example of toner particle 1 except that the binder resin was changed as shown in Table 4.
[0587] Production Example of Toner Particles 3
[0588]
[0589]
[0590] A mixture of the above materials was prepared. The mixture was placed in an attritor (Nippon Coke & Engineering Co., Ltd.) and dispersed with zirconia beads having a diameter of 5 mm at 200 rpm for 2 hours to obtain a raw material dispersion.
[0591] Meanwhile, 735.0 parts of ion exchanged water and 16.0 parts of trisodium phosphate (12 hydrate) were added to a container equipped with a homomixer high-speed stirrer (Primix) and a thermometer, and stirred at 12000 rpm while the temperature was raised to 60° C. A calcium chloride aqueous solution in which 9.0 parts of calcium chloride (2-hydrate) was dissolved in 65.0 parts of ion exchanged water was added, and stirred at 12000 rpm for 30 minutes while maintaining the temperature at 60° C. 10% hydrochloric acid was added to adjust the pH to 6.0, and an aqueous medium containing a dispersion stabilizer was obtained.
[0592] Next, the raw material dispersion was transferred to a container equipped with a stirrer and a thermometer, and stirred at 100 rpm while the temperature was raised to 60° C. Then, 8.0 parts of tert-butyl peroxypivalate (NOF: Perbutyl PV) was added as a polymerization initiator, and the mixture was stirred at 100 rpm for 5 minutes while maintaining the temperature at 60° C., and then added to the aqueous medium while stirring the medium at 12000 rpm with a high-speed stirring device.
[0593] Then, while maintaining the temperature at 60°C, stirring was continued at 12000rpm by a high-speed stirring device for 20 minutes to obtain a granulation liquid. The granulation liquid was transferred to a reactor equipped with a reflux condenser, a stirrer, a thermometer and a nitrogen inlet pipe, and stirred at 150rpm in a nitrogen atmosphere while the temperature was raised to 70°C. Then, a polymerization reaction was carried out at 150rpm for 10 hours while maintaining the temperature at 70°C. Then, the reflux condenser was removed from the reactor, the temperature of the reaction solution was raised to 95°C, and the solution was stirred at 150rpm for 5 hours while maintaining the temperature at 95°C to remove toluene and obtain a toner particle dispersion.
[0594] The obtained toner particle dispersion was cooled to 20° C. while stirring at 150 rpm, and then stirred while adding dilute hydrochloric acid to adjust the pH to 1.5 and dissolve the dispersion stabilizer. The solid was filtered out and washed thoroughly with ion exchange water, which was vacuum dried at 40° C. for 24 hours to obtain toner particles 3.
[0595] Production Example of Toner Particles 4
[0596]
[0597]
[0598] These materials were mixed with a Henschel mixer (FM-75, Nippon Coke & Engineering Co., Ltd.) for 20 s. -1 The mixture was mixed at a speed of 1000 rpm and a rotation time of 5 minutes, and then kneaded in a twin screw kneader (PCM-30, Ikegai) at a discharge temperature of 135°C, wherein the screw kneader was set to a screw speed of 200 rpm and a temperature of 120°C. The kneaded product was cooled at a cooling rate of 15°C / min and coarsely pulverized to less than 1 mm in a hammer mill to obtain a pulverized product. The pulverized product was then finely pulverized with a mechanical pulverizer (T-250, Freund-Turbo Corporation).
[0599] This was then classified using Faculty F-300 (Hosokawa Micron Corporation) to obtain toner particles 4. As for the operating conditions, the classification rotor speed was set to 130 s -1 , set the dispersion rotor speed to 120s -1 .
[0600] Production Example of Toner Particles 25
[0601] Toner particles 25 were obtained according to the production example of toner particles 4 except that the kind of binder resin was changed as shown in Table 4, the temperature of the twin-screw kneader was set to 120° C., and the screw rotation speed was changed to 300 rpm.
[0602] Production Example of Toner Particles 26
[0603] Toner particles 26 were obtained according to the production example of toner particles 4 except that the kind of binder resin was changed as shown in Table 4, the temperature of the twin-screw kneader was set to 120° C., and the screw rotation speed was changed to 150 rpm.
[0604] Production Example of Toner Particles 27
[0605] Toner particles 27 were obtained according to the production example of toner particles 4 except that the kind of binder resin was changed as shown in Table 4, the temperature of the twin-screw kneader was set to 100° C., and the screw rotation speed was changed to 350 rpm.
[0606] Production Example of Toner Particles 28
[0607] Toner particles 28 were obtained according to the production example of toner particles 4 except that the kind of binder resin was changed as shown in Table 4, the temperature of the twin-screw kneader was set to 140° C., and the screw rotation speed was changed to 100 rpm.
[0608] [Table 4]
[0609]
[0610] The abbreviations in Table 2-1 are defined as follows.
[0611] EA: Emulsion Polymerization
[0612] SP: Suspension polymerization
[0613] MK: Melt kneading
[0614] Production Example of Toner 1
[0615] ·Toner particles 1: 100 parts
[0616] Inorganic fine particles 5: 1.0 part
[0617] The above materials were mixed in a FM-10C Henschel mixer (Mitsui Miike Machinery Co., Ltd.) for 30 s. -1 The mixture was mixed at a rotation speed of 1000 rpm and a rotation time of 10 minutes to obtain Toner 1. The composition of Toner 1 is shown in Table 5. The weight average particle size (D4) of Toner 1 was 6.1 μm. The physical properties of Toner 1 are shown in Table 6.
[0618] Production Examples of Toners 2 to 36 and 45 to 54
[0619] Toners 2 to 36 and 45 to 54 were obtained according to the production example of Toner 1 except that the toner particles and the inorganic fine particles were changed as shown in Table 5. The physical properties of the obtained Toners 2 to 36 and 45 to 54 are shown in Table 6.
[0620] Production Examples of Toners 37 to 44
[0621] Toners 37 to 44 were obtained according to the production example of Toner 36 except that the kinds and addition amounts of toner particles and inorganic fine particles were changed as shown in Table 5. The physical properties of the obtained Toners 37 to 44 are shown in Table 6.
[0622] In cross-sectional observation of the obtained toners, Toners 1 to 44, 46 to 50, and 52 to 54 showed a domain-matrix structure composed of a matrix containing the first resin (crystalline resin) and a domain containing the second resin (non-crystalline resin).
[0623] On the other hand, Toners 45 and 51 show a domain-matrix structure composed of a matrix containing the second resin and domains containing the first resin.
[0624] [Table 5]
[0625]
[0626]
[0627] [Table 6]
[0628]
[0629]
[0630] The abbreviations in Table 6 are defined as follows.
[0631] DD: domain diameter
[0632] CR: Coverage
[0633] CDC: Charge decay rate coefficient
[0634] In the table, X is the content (mass %) of the first resin in the binder resin, and the domain diameter is the number average diameter (expressed in μm). The coverage is expressed in area %.
[0635] Production Example of Magnetic Carrier 1
[0636] Magnetite 1 with a number average particle size of 0.30 μm (magnetization intensity in a 1000 / 4π (kA / m) magnetic field is 65 Am 2 / kg)
[0637] Magnetite 2 with a number average particle size of 0.50 μm (magnetization intensity in a 1000 / 4π (kA / m) magnetic field is 65 Am 2 / kg)
[0638] 4.0 parts of a silane compound (3-(2-aminoethylaminopropyl)trimethoxysilane) was added to 100 parts of each of the above materials, and mixed and stirred at a high speed at 100° C. or more in a container to treat each fine particle.
[0639] Phenol: 10% by mass
[0640] Formaldehyde solution: 6% by mass
[0641] (Formaldehyde 40% by mass, methanol 10% by mass, water 50% by mass)
[0642] Silane compound treated magnetite 1: 58 mass%
[0643] Silane compound treated magnetite 2: 26 mass%
[0644] 100 parts of these materials, 5 parts of 28 mass % ammonia aqueous solution and 20 parts of water were placed in a flask, stirred and mixed for 30 minutes while heating to 85° C. and maintained for 3 hours to perform polymerization reaction to harden the obtained phenolic resin.
[0645] Then, the hardened phenolic resin was cooled to 30°C, water was added, the supernatant was removed, and the precipitate was washed with water and air-dried. It was then dried at 60°C under reduced pressure (5 mmHg or less) to obtain a magnetic body dispersion type spherical magnetic carrier. The volume-based 50% particle size (D50) was 34.2 μm.
[0646] Production Example of Two-Component Developer 1
[0647] 92.0 parts of Magnetic Carrier 1 and 8.0 parts of Toner 1 were mixed in a V-type mixer (V-20, Seishin Enterprise Co., Ltd.) to obtain a two-component developer 1 .
[0648] Production Examples of Two-Component Developers 2 to 54
[0649] Except that the toner was changed as shown in Table 7, two-component developers 2 to 54 were obtained according to the manufacturing example of two-component developer 1.
[0650] [Table 7]
[0651]
[0652]
[0653] Toner Evaluation Method
[0654] Evaluation of live-lift performance
[0655] The charge-up performance is evaluated by measuring the density change when images with different image printing ratios and densities are output. An image with a low image ratio is output to saturate the charge of the toner in the developing unit, and an image with a high image ratio is output. The density change occurs as a result of the charge difference between the saturated toner already present in the developing unit and the new toner supplied to the developing unit.
[0656] Since the toner with rapid charge rise is quickly saturated after being supplied to the developing unit, the density changes little. On the other hand, the toner with slow charge rise takes time to become saturated after being supplied to the developing unit, reducing the charge amount of the entire toner and changing the density.
[0657] A Canon imagePress C800 full color copier was used as an image forming apparatus, a two-component developer to be evaluated was placed in a cyan developing device of the image forming apparatus, and a toner to be evaluated was placed in a cyan toner container, and evaluated as follows.
[0658] As an improvement, the mechanism for removing excess magnetic carrier from the inside of the developing device was removed. 2 , Canon Marketing Japan) was used as evaluation paper.
[0659] The toner load on the paper in the FFh image (solid image) was adjusted to 0.45 mg / cm 2 FFh is a value obtained by displaying 256 tones in hexadecimal notation, where 00h is the first of the 256 tones (white background) and FF is the 256th tone (solid part).
[0660] The image output test was conducted by outputting 1000 prints at an image ratio of 1%. During the continuous feeding of 1000 sheets, the developing conditions and the transfer conditions (without calibration) were the same as those of the first print.
[0661] Then, 1000 prints were output at an image ratio of 80% to conduct an image output test. During the continuous feeding of 1000 sheets, the developing conditions and the transfer conditions (without calibration) were the same as those of the first print.
[0662] The image density of the 1000th print printed at an image ratio of 1% was taken as the initial density. The density of the 1000th print printed at an image ratio of 80% was measured and evaluated according to the following evaluation criteria.
[0663] The test was performed in a high temperature and high humidity environment (H / H; 30° C., RH 80%) and a normal temperature and low humidity environment (N / L; 23° C., RH 5%).
[0664] (1) Measurement of image density changes
[0665] Using an X-Rite color reflection densitometer (500 series, X-Rite Inc.), the initial density and the density of the 1000th image printed at an image ratio of 80% were measured and graded according to the following criteria. Grade D or above means that the effect of the present invention has been obtained. The evaluation results are shown in Table 8.
[0666] (Concentration difference)
[0667] AA: less than 0.02
[0668] A: 0.02 or more and less than 0.04
[0669] BB: 0.04 or more and less than 0.06
[0670] B: 0.06 or more and less than 0.08
[0671] CC: 0.08 or more and less than 0.10
[0672] C: 0.10 or more and less than 0.12
[0673] D: 0.12 or more and less than 0.15
[0674] E: 0.15 or more
[0675] Evaluation method of charge retention characteristics in high temperature and high humidity environments
[0676] The toner on the electrostatic latent image bearing member is collected by suction using a metal cylindrical pipe and a cylindrical filter to measure the triboelectric charge amount of the toner.
[0677] Specifically, the friction charge amount of the toner on the electrostatic latent image bearing member is measured with a Faraday cage, which is a coaxial double cylinder in which the inner cylinder and the outer cylinder are insulated from each other. If a charged body with a charge amount Q is placed in the inner cylinder, electrostatic induction makes it seem as if there is a metal cylinder with a charge amount Q. The induced charge amount is measured with an electrometer (Keithley 6517A, Keithley), and the charge amount Q (mC) is divided by the mass M (kg) of the toner in the inner cylinder (Q / M), and is regarded as the friction charge amount of the toner.
[0678] Toner triboelectric charge (mC / kg) = Q / M
[0679] An image for evaluation is first formed on an electrostatic latent image bearing member, and then before it can be transferred to an intermediate transfer member, the rotation of the electrostatic latent image bearing member is stopped, and the toner on the electrostatic latent image bearing member is collected by suction with a metal cylindrical pipe and a cylindrical filter, and the "initial Q / M" is measured.
[0680] Next, the evaluation unit was left for two weeks, with the developing device still installed in a high temperature and high humidity environment (H / H), the same operation as before was performed, and the charge amount Q / M (mC / kg) per unit mass on the electrostatic latent image bearing member after the leaving was measured. The initial Q / M per unit mass on the electrostatic latent image bearing member was taken as 100%, and the maintenance rate of Q / M per unit mass on the electrostatic latent image bearing member after the leaving was calculated and evaluated according to the following standard ([Q / M after leaving] / [initial Q / M]×100). Grade D or above indicates that the effect of the present invention has been obtained. The evaluation results are shown in Table 8.
[0681] (Evaluation Criteria)
[0682] AA: Maintenance rate over 98%
[0683] A: Maintenance rate is above 95% and less than 98%
[0684] BB: Maintenance rate is above 90% and less than 95%
[0685] B: Maintenance rate is 85% or more and less than 90%
[0686] CC: Maintenance rate 80% or more and less than 85%
[0687] C: Maintenance rate 75% or more and less than 80%
[0688] D: Maintenance rate 70% or more and less than 75%
[0689] E: Maintenance rate is less than 70%
[0690] Evaluation method of low temperature fixability
[0691] Paper: GFC-081(81.0g / m 2 )(Sold by Canon Marketing Japan Inc.)
[0692] Toner loading on paper: 0.50mg / cm 2 (Adjusted by the DC voltage VDC of the developer bearing member, the charging voltage VD of the electrostatic latent image bearing member and the laser power)
[0693] Evaluation image: 2cm x 5cm image in the center of A4 paper
[0694] Test environment: 15°C, 10%RH low temperature and low humidity environment (hereinafter referred to as "L / L")
[0695] Fixing temperature: 130℃
[0696] Processing speed: 377mm / sec
[0697] The evaluation image was output and the low-temperature fixability was evaluated. The image density reduction rate was used as an evaluation standard for the low-temperature fixability.
[0698] For the image density reduction rate, the image density at the center of the image was first measured using an X-Rite color reflection densitometer (500 series, X-Rite Inc.). 2 ), the fixed image on the portion where the image density had been measured was rubbed with Silbon paper (5 reciprocations) under a load of 1.5 % and the image density was measured again.
[0699] Then, the image density reduction rate after rubbing was calculated by the following formula. The image density reduction rate was evaluated according to the following criteria. Grade D or above indicates that the effect of the present invention has been obtained. The evaluation results are shown in Table 8.
[0700] Image density reduction rate =
[0701] (Image density before rubbing - Image density after rubbing) / Image density before rubbing × 100
[0702] (Evaluation Criteria)
[0703] AA: Image density reduction rate is less than 3.0%
[0704] A: Image density reduction rate 3.0% or more and less than 5.0%
[0705] BB: Image density reduction rate 5.0% or more and less than 10.0%
[0706] B: Image density reduction rate 10.0% or more and less than 15.0%
[0707] CC: Image density reduction rate 15.0% or more and less than 20.0%
[0708] C: Image density reduction rate 20.0% or more and less than 25.0%
[0709] D: Image density reduction rate 25.0% or more and less than 30.0%
[0710] E: Image density reduction rate 30.0% or more
[0711] Evaluation method of hot fouling resistance (HO)
[0712] Using a modified Canon imagePRESS C800 full-color copier as an unfixed image forming unit, the above two-component developer was placed in a cyan station developing device and evaluated.
[0713] Use GFC-081 ordinary copy paper (A4, basis weight 81.4g / m 2 , Canon Marketing Japan Inc.) as the evaluation paper. An unfixed toner image (toner load 0.08 mg / cm) with a length of 2.0 cm and a width of 15.0 cm was formed at a portion 2.0 cm from the top of the paper in the paper feeding direction under a normal temperature and humidity environment (23°C, 60% RH) 2 ).
[0714] The fixing test was carried out using a fixing unit that had been taken out of an image RUNNER ADVANCE C5255 Canon full-color copier and modified so that the fixing temperature could be adjusted. In a normal temperature and humidity environment (23°C, 5% RH), the process speed was set to 265 mm / s, and the temperature was raised from 160°C to 210°C in 5°C increments, and a fixed image was obtained from a previous unfixed image at each temperature. The heat offset resistance of the resulting fixed image was then evaluated.
[0715] The hot offset in the fixed image was visually evaluated and judged according to the following criteria. A grade of D or higher indicates that the effect of the present invention has been obtained. The evaluation results are shown in Table 8.
[0716] (Evaluation Criteria)
[0717] AA: No thermal fouling even at 210°C
[0718] A: Thermal fouling at 205°C
[0719] BB: Thermal fouling at 200°C
[0720] B: Thermal fouling at 195°C
[0721] CC: Thermal fouling at 190°C
[0722] C: Thermal fouling at 180°C or above and less than 190°C
[0723] D: Thermal fouling at 170°C or above and less than 180°C
[0724] E: Thermal fouling below 170°C
[0725] Examples 1 to 44
[0726] The above-described evaluations were performed on Toners 1 to 44 (two-component developers 1 to 44).
[0727] Comparative Examples 1 to 10
[0728] The above-described evaluations were performed on Toners 45 to 54 (two-component developers 45 to 54).
[0729] [Table 8]
[0730]
[0731]
[0732] The abbreviations in Table 8 are defined as follows.
[0733] HOT: HO generation temperature
[0734] CD: Concentration Difference
[0735] While the present invention has been described with reference to exemplary embodiments, it is to be understood that the invention is not limited to the disclosed exemplary embodiments.The scope of the following claims is to be accorded the broadest interpretation so as to encompass all such modifications and equivalent structures and functions.
Claims
1. A toner comprising: Toner particles containing a binder resin including a first resin and a second resin; and Inorganic fine particles on the surface of the toner particles, It is characterized in that The first resin is a crystalline resin, The second resin is a non-crystalline resin, The first resin has a first monomer unit represented by the following formula (1), The content ratio of the first monomer unit in the first resin is 30.0 mass % to 99.9 mass %, The acid value of the first resin is 0.1 mg KOH / g to 30 mg KOH / g, The acid value of the second resin is 0.5 mg KOH / g to 40 mg KOH / g, A domain-matrix structure formed of a matrix containing the first resin and domains containing the second resin appears in cross-sectional observation of the toner, A compound having an alkyl group is present on the surface of the inorganic fine particles, and The volume resistivity of the inorganic fine particles is 1.0×10 5 Ω·cm to 1.0×10 13 Ω·cm: In formula (1), R Z1 represents a hydrogen atom or a methyl group, and R represents C 18-36 alkyl, The compound having an alkyl group has (R 9 -COO) p M(OH) q represents the structure, and In the formula, each R 9 Independently represents C 4-24 Straight or branched chain alkyl or C 4-24 A linear or branched hydroxyalkyl group, M is Al, Zn, Mg, Ca, Sr, K or Na, p is an integer from 1 to 3 and q is an integer from 0 to 2. 2 . The toner according to claim 1 , wherein a mass ratio X / Y of a content X of the first resin to a content Y of the second resin in the binder resin is 0.2 to 2.
5. 3 . The toner according to claim 1 , wherein a number average diameter of the domains in cross-sectional observation of the toner is from 0.1 μm to 2.0 μm. 4 . The toner according to claim 1 , wherein a coverage ratio of the inorganic fine particles to the toner particles is from 10 area % to 80 area %. 5 . The toner according to claim 1 , wherein the inorganic fine particles have a dielectric constant at 2 kHz of 20 pF / m to 60 pF / m.
6. The toner according to claim 1 or 2, wherein the compound having an alkyl group is selected from the group consisting of 4-24 At least one compound of the group consisting of alkyl compounds. 7 . The toner according to claim 1 , wherein the compound having an alkyl group is at least one compound selected from the group consisting of fatty acids, fatty acid metal salts, silicone oils, and silane coupling agents. 8 . The toner according to claim 1 , wherein the inorganic fine particles are at least one selected from the group consisting of titanium oxide fine particles, strontium titanate fine particles, calcium titanate fine particles, and zinc oxide fine particles. 9 . The toner according to claim 1 , wherein a charge decay rate coefficient of the toner measured at 30° C., 80% RH is from 3 to 100. 10 . The toner according to claim 1 , wherein when Xε is a dielectric constant of the inorganic fine particles at 2 kHz and Yε is a dielectric constant of the second resin at 2 kHz, Xε / Yε is 5.0 to 170.
0. 11 . The toner according to claim 1 or 2 , wherein the second resin has a dielectric constant at 2 kHz of 2.0 pF / m to 3.0 pF / m. 12 . The toner according to claim 1 , wherein when Cx in the first resin is the carbon number of the alkyl group represented by R in the first monomer unit and Cy is the carbon number of the alkyl group of the compound having an alkyl group, Cx / Cy is 0.8 to 24.
0.
13. The toner according to claim 1 or 2, wherein The binder resin contains a third resin, and The third resin includes a resin in which the first resin and the second resin are connected. 14 . The toner according to claim 1 , wherein the second resin contains at least one selected from the group consisting of a vinyl resin, a polyester resin, and a hybrid resin comprising a vinyl resin bonded to a polyester resin.
15. The toner according to claim 1 or 2, wherein The second resin is a polyester resin, and The polyester resin has a polycondensation structure of dodecenylsuccinic acid or its anhydride. 16 . The toner according to claim 15 , wherein the polyester resin has a polycondensation structure of a carboxylic acid component other than the polycondensation structure of the dodecenylsuccinic acid or its anhydride.
17. The toner according to claim 1 or 2, wherein in gel permeation chromatography measurement of tetrahydrofuran solubles of the toner, when Mw(A) is a weight average molecular weight and Mn(A) is a number average molecular weight, Mw(A) is 25,000 to 60,000 and Mw(A) / Mn(A) is 5 to 10. 18 . The toner according to claim 1 , wherein a content of the first resin in the binder resin is 30.0% by mass or more.
19. The toner according to claim 1 or 2, wherein The first resin has a second monomer unit different from the first monomer unit, and The second monomer unit is at least one selected from the group consisting of a monomer unit represented by the following formula (2) and a monomer unit represented by the following formula (3), and When SP 21 is the SP value (J / cm 3 ) 0.5 When the SP 21 For 21.00 and above: In formula (2), X is a single bond or C 1-6 Alkylene, R 1 For -C≡N, -C(=O)NHR 10 , where R 10 Represents a hydrogen atom or C 1-4 alkyl, Hydroxyl, -COOR 11 , where R 11 Represents C 1-6 Alkyl or C 1-6 Hydroxyalkyl, -NH-C(=O)-N(R 13 ) 2 , where two R 13 Each independently represents a hydrogen atom or a C 1-6 alkyl, -COO(CH 2 ) 2 NHCOOR 14 , where R 14 Represents C 1-4 Alkyl, or -COO(CH 2 ) 2 -NH-C(=O)-N(R 15 ) 2 , where two R 15 Each independently represents a hydrogen atom or a C 1-6 Alkyl, and R 2 represents a hydrogen atom or a methyl group; and In formula (3), R 3 Represents C 1-4 Alkyl and R 4 represents a hydrogen atom or a methyl group.
20. The toner according to claim 1 or 2, wherein The matrix is exposed on at least a portion of the surface of the toner particle, and At least a portion of the inorganic fine particles is in contact with the exposed portion of the matrix.
21. A two-component developer comprising a toner and a magnetic carrier, It is characterized in that The toner is the toner according to any one of claims 1 to 20.