Alcoholysis-resistant polypropylene composite material as well as preparation method and application thereof
Through the combination of components such as high-crystalline polypropylene, ethylene-octene block copolymer and modified nanosilicon dioxide, the alcoholylation problem of traditional nylon materials in high-temperature ethylene glycol environment is solved, and alcoholylation resistant poly(ethanolylation) is prepared Apropylene composite material improves its performance in water chamber applications in new energy vehicles.
Patent Information
- Application Number
- CN202310614646.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional glass fiber reinforced nylon materials are prone to alcoholylation in high-temperature ethylene glycol soaking environment, resulting in a decline in mechanical properties and cannot meet the use requirements of water chamber materials for new energy vehicles.
Using high crystalline, high modulus polypropylene material, ethylene-octene block copolymer, silane coupling agent to modify nanosilia and glass fiber, the double screw extrusion process is used to prepare alcohol-resistant polypropylene Composite materials improve their heat, water, glycol and corrosion resistance.
It significantly improves the tensile strength and mechanical properties of the material, delays the penetration of water/alcohol media, enhances the resistance to alcoholylation, and makes it suitable for water chamber materials in new energy vehicles.
Smart Images

Figure BDA0004253434820000011 
Figure BDA0004253434820000021 
Figure BDA0004253434820000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material modification and processing, and particularly relates to an alcoholysis-resistant polypropylene composite material and a preparation method and application thereof. Background Art
[0002] With the increasing awareness of environmental protection and the deepening of the energy crisis, the energy power system of automobiles has changed, and new energy vehicles have become a hot spot in the global automotive industry. New energy vehicles use unconventional automotive fuels as their power source. In the new power system, the temperature of the radiator has been significantly reduced compared to before. The traditional high-temperature water chamber test temperature is as high as 130°C, and the low-temperature water chamber test temperature is only 70-100°C. The reduction in radiator temperature has brought new opportunities and challenges to the lightweighting of water chamber materials.
[0003] The main component of the cooling medium in the radiator water chamber is ethylene glycol. Traditional water chamber materials are mostly glass fiber reinforced nylon materials. However, nylon materials have many polar groups on the polymer chain, which is prone to alcoholysis, resulting in a decrease in the mechanical properties of nylon materials.
[0004] Polypropylene is a thermoplastic with low density, good chemical stability, and natural water and alcoholysis resistance. Glass fiber reinforced polypropylene has low density and high strength, and is widely used in automobiles. It is the best alternative to glass fiber reinforced nylon. However, when glass fiber reinforced polypropylene is immersed in ethylene glycol for a long time at high temperature (120℃ / 1000 hours), ethylene glycol will invade the interface between glass fiber and polypropylene, causing the degradation of polypropylene molecular segments, resulting in a certain degree of performance degradation, which cannot meet the use requirements. Summary of the invention
[0005] In order to solve the above problems, the present invention designs a polypropylene composite material resistant to alcoholysis and its preparation method and application. The material has high strength and has the advantages of heat resistance, water resistance, ethylene glycol resistance, corrosion resistance and the like, and is suitable for water chamber materials of new energy vehicles.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] The first object of the present invention is to provide an alcoholysis-resistant polypropylene composite material, which is composed of the following components in parts by weight:
[0008]
[0009]
[0010] In a further embodiment, the polypropylene is a homopolymerized high-crystalline, high-modulus polypropylene; the crystallinity of the polypropylene is ≥70%, the flexural modulus is ≥1600Mpa, and the melt index is 8-40g / 10min under the test conditions of 230°C and 2.16kg.
[0011] In a further embodiment, the compatibilizer is maleic anhydride grafted polypropylene;
[0012] In a further embodiment, the olefin block copolymer is an ethylene-octene block copolymer, which has a melting point of 100-120°C and a glass transition temperature of below -60°C.
[0013] In a further embodiment, the glass fiber is flat glass fiber with a thickness-to-width ratio of 1:(3-5).
[0014] In a further embodiment, the preparation method of the silane coupling agent modified nano-silica is as follows:
[0015] (1) dispersing nano-silicon dioxide in a dispersant to obtain a suspension; preferably, the dispersant is one or more of n-hexane, cyclohexane, and heptane;
[0016] (2) Adding a silane coupling agent to the suspension, heating to 60-100°C and stirring for 4-6 hours, separating the obtained mixture after the reaction, washing and drying the separated solid to obtain silane coupling agent modified nano-silica. Preferably, the silane coupling agent is at least one of an epoxy silane coupling agent, a long-chain alkyl silane coupling agent, and an amino silane coupling agent; the mass ratio of the silane coupling agent to the nano-silica is (0.01-0.02):1.
[0017] In a further embodiment, the heat-resistant auxiliary agent is a compound composed of antioxidant 1010 and antioxidant 168. In a further embodiment, the mass ratio of antioxidant 1010 to antioxidant 168 is 1:1.
[0018] The second object of the present invention is to provide a method for preparing the alcoholysis-resistant polypropylene composite material as described in the first object above, comprising the following steps:
[0019] Polypropylene, a compatibilizer, an olefin block copolymer, silane coupling agent-modified nano-silica and a heat-resistant additive are placed in a high-speed mixer according to a proportion and mixed for 3 to 5 minutes to obtain a mixture; then the mixture is added to a twin-screw extruder, glass fiber is added from a glass fiber port, and an alcoholysis-resistant polypropylene composite material is obtained through extrusion and pelletization; the aspect ratio of the twin-screw extruder is 48:1, and the processing temperature of the twin-screw extruder is 190-230°C.
[0020] The third object of the present invention is to provide an application of the alcoholysis-resistant polypropylene composite material as described in the first object, wherein the composite material can be used for automobile water chamber materials.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention adopts a high-crystallization, high-modulus polypropylene material and short-cut glass fibers to effectively improve the tensile strength of the material, so that its performance can meet the requirements of the water chamber material of new energy vehicles.
[0023] (2) The olefin block copolymer used in the present invention is an ethylene-octene block copolymer, which is composed of a crystallizable ethylene-octene segment (hard segment) with a low comonomer content and a high melting temperature and an amorphous ethylene-octene segment (soft segment) with a high comonomer content and a low glass transition temperature. The crystallizable segment is dispersed in the polypropylene matrix and entangled with the polypropylene segment, affecting the crystallization orientation of the polypropylene; the amorphous segment is dispersed in the polypropylene matrix and in the interface between the polypropylene matrix and the glass fiber, filling the crystallization defects, slowing down the crystallization rate of the polypropylene, making it have a more suitable crystallization rate, reducing the probability of crystallization defects, and improving the material performance.
[0024] (3) The silane coupling agent modified nano-silica added in the present invention is evenly dispersed in the polypropylene resin, and plays the role of a nucleation fulcrum, so that the polypropylene molecular segments are orderly arranged and crystallized around the nucleation fulcrum, the crystal form is more uniform, and the crystal defects are less, and the mechanical properties of the obtained product are further improved. At the same time, the inventors have also studied the addition amount of the silane coupling agent modified nano-silica. If the addition amount of the silane coupling agent modified nano-silica is too large, it is easy to aggregate in the polymer melt matrix, and it is not easy to be evenly dispersed, and it is difficult to achieve ideal performance.
[0025] (4) The silane coupling agent modified nano-silica added in the present invention has excellent hydrophobic properties. It can effectively improve the hydrophobic properties of the material when dispersed in the polypropylene matrix, delay the penetration of media such as water / alcohol into the composite material, protect the interface between polypropylene and glass fiber, and thus improve the alcoholysis resistance of the composite material. At the same time, the silane coupling agent on the surface of the nano-silica can react with alcohol, thereby improving the alcoholysis resistance of the material.
[0026] (5) The material of the present invention has high strength and has the advantages of heat resistance, water resistance, ethylene glycol resistance, corrosion resistance, etc., and is suitable for water chamber materials of new energy vehicles. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with the embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The types and suppliers of reagents used in the following examples and comparative examples are only for illustrating the sources and components of the reagents used in the experiments of the present invention so as to fully disclose the information, and do not mean that the present invention cannot be realized by using other similar reagents or reagents provided by other suppliers.
[0029] The specific information of the raw materials used in the following examples and comparative examples is as follows:
[0030] Polypropylene-1: homopolymer polypropylene, grade HP840N, purchased from CNOOC Shell Petrochemical Co., Ltd.;
[0031] Polypropylene-2: homopolymer polypropylene, grade HJ730, purchased from Hanwha Total Petrochemical;
[0032] Compatibilizer: brand BONDYRAM 1001, purchased from Plyram Industries Ltd.;
[0033] Olefin block copolymer-1, brand INFUSE 9807, purchased from Dow Chemical, USA;
[0034] Olefin block copolymer-2, brand INFUSE 9507, purchased from Dow Chemical, USA;
[0035] Flat glass fiber-1: thickness to width ratio is 1:3, purchased from Chongqing International Composite Materials Co., Ltd.;
[0036] Flat glass fiber-2: the ratio of thickness to width is 1:4, purchased from Chongqing International Composite Materials Co., Ltd.;
[0037] Nano-silicon dioxide: purchased from Shanghai Waidian International Trading Co., Ltd.
[0038] Talc: brand HTP1L, purchased from Liaoning Aihai Talc Co., Ltd.;
[0039] Heat-resistant additive: It is prepared from antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1, and the antioxidants are purchased from BASF AG.
[0040] The silane coupling agent modified nano silicon dioxide used in the following embodiments is prepared by the following preparation method:
[0041] (1) dispersing nano-silicon dioxide in n-hexane to obtain a suspension;
[0042] (2) adding an aminosilane coupling agent to the suspension, heating it to 80° C. and stirring it for 4 hours, separating the resulting mixture after the reaction is completed, washing and drying the separated solid to obtain silane coupling agent-modified nano-silica; wherein the mass ratio of the aminosilane coupling agent to the nano-silica is 0.02:1.
[0043] The preparation methods used in the following examples and comparative examples are as follows:
[0044] According to the proportion, polypropylene, compatibilizer, olefin block copolymer, silane coupling agent modified nano-silica and heat-resistant additive are placed in a high-speed mixer and mixed for 3 to 5 minutes, and then the mixture is added to an extruder, and flat glass fiber is added from the glass fiber port, extruded and pelletized to obtain alcoholysis-resistant polypropylene material. In comparative example 5, unmodified nano-silica is used to replace silane coupling agent modified nano-silica.
[0045] The length-to-diameter ratio of the twin-screw extruder is 48:1, and the temperatures of the barrel sections of the twin-screw extruder are set to: 190°C for zone 1, 195°C for zone 2, 205°C for zone 3, 210°C for zone 4, 220°C for zone 5, 230°C for zone 6, and 230°C for the die head.
[0046] Examples 1 to 10: The components and amounts of the alcoholysis-resistant polypropylene material described in each example are shown in Table 1;
[0047] Comparative Examples 1 to 5: The components and amounts of the alcoholysis-resistant polypropylene materials in each comparative example are shown in Table 2;
[0048] Table 1 Formulation of polypropylene composition of Examples 1 to 10
[0049]
[0050] Table 2 Formula of polypropylene composition of comparative examples 1 to 5
[0051]
[0052] After the particles prepared in each embodiment and comparative example are injection molded into standard specimens, performance tests are carried out. The tensile strength is carried out in accordance with ISO 527, the test speed is 5mm / min, the specimen is dumbbell-shaped, and the specimen size is 170mm*10mm*4mm; the cantilever beam notched impact strength is carried out in accordance with ISO 180, the test is carried out at room temperature (23°C), the specimen is rectangular (V-shaped molding notch), and the specimen size is 80mm*10mm*4mm. The specimens are soaked in an ethylene glycol-based solvent (ethylene glycol coolant and water in a volume ratio of 50:50) and placed at 120°C for 1000 hours. The tensile strength and notched impact strength of the specimens before and after immersion are tested respectively, and the performance retention rate is calculated. Performance retention rate = (test data after ethylene glycol immersion / test data before ethylene glycol immersion) * 100%. The test results of each product are shown in Tables 3 and 4.
[0053] Table 3 Performance test results of the products obtained in Examples 1 to 10
[0054]
[0055] Table 4 Performance test results of the products obtained in Comparative Examples 1 to 4
[0056] Test items Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Tensile strength retention rate (%) 73.6 72.1 75.2 65.9 72.2 Notched impact strength retention rate (%) 71.8 72.9 70.9 70.2 71.9
[0057] It can be seen from Examples 1 to 10 that after the polypropylene composite material prepared by the present invention is immersed in an ethylene glycol-based solvent at 120°C for 1000 hours, the tensile strength and the Izod notched impact strength retention rate of the material are both
[0058] ≥80%, excellent alcoholysis resistance.
[0059] Compared with Example 1, Comparative Example 1 does not add olefin block copolymers, the composite material has many crystal defects, and after ethylene glycol immersion, the material performance decreases significantly. Compared with Example 2, Comparative Example 3 increases the addition ratio of silane coupling agent modified nano-silica. When the content of silane coupling agent modified nano-silica is too high, it is easy to aggregate in the polymer melt matrix, not easy to disperse evenly, and the alcoholysis resistance decreases. Compared with Example 2, Comparative Example 3 does not add silane coupling agent modified nano-silica, which cannot effectively delay and prevent water / alcohol and other media from penetrating into the composite material, and the alcoholysis resistance of the material decreases. Compared with Example 8, Comparative Example 4 replaces silane coupling agent modified nano-silica with talcum powder, which does not have hydrophobicity, and has poor compatibility with glass fiber, and has many composite material interface defects, and alcoholysis resistance decreases significantly. Compared with Example 8, Comparative Example 5 is unmodified, has reduced compatibility with glass fiber, increased composite material interface defects, and alcoholysis resistance decreases significantly.
[0060] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A polypropylene composite material resistant to alcoholysis, Features: It is composed of the following components by weight:
2. The alcoholysis-resistant polypropylene composite material according to claim 1, Features: The polypropylene is a homopolymerized high-crystallization, high-modulus polypropylene, the crystallinity of the polypropylene is ≥70%, the bending modulus is ≥1600Mpa, and the melt index is 8-40g / 10min under the test conditions of 230°C and 2.16kg.
3. The alcoholysis-resistant polypropylene composite material according to claim 1, Features: The compatibilizer is maleic anhydride grafted polypropylene.
4. The alcoholysis-resistant polypropylene composite material according to claim 1, Features: The olefin block copolymer is an ethylene-octene block copolymer, the melting point of which is 100-120° C. and the glass transition temperature is below -60° C.
5. The alcoholysis-resistant polypropylene composite material according to claim 1, Features: The glass fiber is flat glass fiber with a thickness-to-width ratio of 1:(3-5).
6. The alcoholysis-resistant polypropylene composite material according to claim 1, Features: The preparation method of the silane coupling agent modified nano silicon dioxide is as follows: (1) dispersing nano silicon dioxide in a dispersant to obtain a suspension; (2) adding a silane coupling agent to the suspension, heating to 60-100° C. and stirring for a reaction for 4-6 hours; separating the obtained mixture after the reaction is completed; and washing and drying the separated solid to obtain silane coupling agent-modified nano-silica.
7. The alcoholysis-resistant polypropylene composite material according to claim 6, Features: The dispersant is one or more of n-hexane, cyclohexane, and heptane; the silane coupling agent is at least one of an epoxy silane coupling agent, a long-chain alkyl silane coupling agent, and an amino silane coupling agent; and the mass ratio of the silane coupling agent to nano-silicon dioxide is (0.01-0.02):
1.
8. The alcoholysis-resistant polypropylene composite material according to claim 1, Features: The heat-resistant auxiliary agent is a compound composed of antioxidant 1010 and antioxidant 168.
9. The method for preparing the alcoholysis-resistant polypropylene composite material according to any one of claims 1 to 8, Features The following steps are involved: Polypropylene, a compatibilizer, an olefin block copolymer, silane coupling agent-modified nano-silica and a heat-resistant additive are placed in a high-speed mixer according to a proportion and mixed for 3 to 5 minutes to obtain a mixture; then the mixture is added to a twin-screw extruder, glass fiber is added from a glass fiber port, and an alcoholysis-resistant polypropylene composite material is obtained through extrusion and pelletization; the aspect ratio of the twin-screw extruder is 48:1, and the processing temperature of the twin-screw extruder is 190-230°C.
10. The alcoholysis-resistant polypropylene composite material according to any one of claims 1 to 8 is used in automobile water chamber materials.
Citation Information
Patent Citations
Hydrolysis and alcoholysis resistant modified nylon 66 material for automotive water chamber and preparation method of modified nylon 66 material
CN108948738A
Polypropylene composition for automobile water chambers and preparation method thereof
CN110845792A
Glass fiber reinforced PP / PA66 composite material for new energy automobile water chamber and preparation method
CN112375297A
Polypropylene composition as well as preparation method and application thereof
CN114773728A
Method for Preparing Silane Coupling Agent / Silica / Plant Fiber Composite
US20230043739A1