A high-strength hollow brick and its preparation process

By combining aluminum ash, cinder ash and other materials with soy protein and carboxymethyl chitosan, phenolic resin is modified to form a three-dimensional network structure, which improves the compressive strength and yield of hollow bricks, and solves the poor crack resistance of hollow bricks. The problem.

CN116477876BActive Publication Date: 2024-11-29XUZHOU ZHENFENG NEW TYPE WALL MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310450216.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-25
Publication Date
2024-11-29
Estimated Expiration
2043-04-25

AI Technical Summary

Technical Problem

Hollow bricks have poor crack resistance, pose safety hazards, and are difficult to meet high-strength needs.

Method used

Using aluminum ash, cinder ash, coal gangue, silica fume, cast waste sand, clay, glass fiber and other materials, combined with soy protein and carboxymethyl chitosan, it is modified through phenolic resin to form a three-dimensional network structure material that intersects each other. , enhance the compressive strength of hollow bricks.

Benefits of technology

The compressive strength and yield of hollow bricks are significantly improved, the compressive strength reaches more than 26MPa, and the yield rate exceeds 98%, solving the problem of hollow bricks being prone to cracking.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of building materials, specifically to a high-strength hollow brick and a preparation process thereof. The present invention discloses a high-strength hollow brick and a preparation process thereof, wherein waste materials such as aluminum ash, coal slag ash, coal gangue, silica ash, and foundry waste sand in industrial production are blended with clay and glass fiber, and a hollow brick is prepared using a modified phenolic resin as an adhesive. Phenolic resin is water-resistant, heat-resistant, and has stable performance, but it is brittle and easy to crack, so it is modified using soy protein and carboxymethyl chitosan. Protein and carboxymethyl chitosan have good water solubility, and are combined into a protein-carboxymethyl chitosan polymer under the action of electrostatics, which is mixed with phenol and methanol, and cross-linked under the action of glutaraldehyde to form a three-dimensional network, thereby enhancing the bonding effect; at the same time, glutaraldehyde changes the connection of the aromatic nucleus in the phenolic resin, improves the toughness of the resin, and thus improves the strength of the hollow brick.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a high-strength hollow brick and a preparation process thereof. Background Art

[0002] Hollow bricks are made of pumice, volcanic slag, coal slag, ceramsite and other materials. They are a kind of filling material for construction, mainly used in non-load-bearing parts of walls. There are many types of hollow bricks, including concrete hollow blocks, ordinary concrete small hollow blocks, lightweight aggregate concrete blocks, single-row hole small blocks, double-row hole or multi-row hole blocks, etc. Among them, concrete hollow blocks and ordinary concrete small hollow blocks are the most common.

[0003] Hollow bricks have the advantages of light weight, heat preservation, sound insulation, etc. Compared with solid bricks, the use of hollow bricks can greatly reduce the total mass of the building, thereby reducing the load-bearing capacity of the building foundation and maintaining its original state. Although hollow bricks have many advantages, their poor crack resistance is a fatal disadvantage. They are prone to cracking after long-term use, posing a safety hazard. Therefore, it is necessary to modify the hollow bricks to improve their strength. Summary of the invention

[0004] The object of the present invention is to provide a high-strength hollow brick and a preparation process thereof to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a high-strength hollow brick and a preparation process thereof, comprising the following steps:

[0006] Step 1: crushing and mixing aluminum ash, coal slag ash, coal gangue, silica ash, foundry waste sand, clay and glass fiber to obtain a powder material;

[0007] Step 2: dissolving the isolated soy protein powder in deionized water, and performing ultrasonic dispersion to obtain a soy protein solution; adding a sodium hydroxide solution to the soy protein solution to adjust the pH, and stirring to obtain a soy protein modified solution; adding carboxymethyl chitosan to the soy protein modified solution, and stirring to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0008] Step 3: Mix phenol and glutaraldehyde, adjust the pH, heat the mixture for reaction, cool it down, add a mixed solution of soybean protein and carboxymethyl chitosan, stir, heat it up, add formaldehyde, stir and react to obtain a mixed material, and perform reduced pressure distillation to obtain a resin material;

[0009] Step 4: Mix the powder material, the resin material and the deionized water, stir and pour into a mold to solidify and shape, and demold to obtain the high-strength hollow brick.

[0010] Furthermore, in step 1, the contents of each component in the powder material are, by weight, 10 to 15 parts of aluminum ash, 20 to 25 parts of coal slag ash, 18 to 27 parts of coal gangue, 10 to 12 parts of silica ash, 15 to 22 parts of foundry waste sand, 26 to 35 parts of clay, and 10 to 12 parts of glass fiber.

[0011] Furthermore, in step 2, the content of each component in the soy protein solution is, by weight, 20 to 30 parts of soy protein isolate powder and 100 to 120 parts of deionized water.

[0012] Furthermore, in step 2, the pH of the sodium hydroxide solution is adjusted to 7.5-8.0.

[0013] Furthermore, in step 2, the ultrasonic dispersion time is 15 to 30 minutes.

[0014] Furthermore, in step 2, the content of each component in the mixed solution of soybean protein and carboxymethyl chitosan is, by weight, 100 to 120 parts of soybean protein modified solution and 4 to 10 parts of carboxymethyl chitosan.

[0015] Furthermore, in step 3, the specific operating conditions are: mix phenol and glutaraldehyde, adjust the pH to 8-9, heat to 70-90°C and react for 30-60 minutes, cool to 50-60°C, add a mixed solution of soybean protein and carboxymethyl chitosan, stir and heat to 80-90°C, add formaldehyde and stir to react for 30-60 minutes to obtain a mixed material, and distill under reduced pressure to obtain a resin material.

[0016] Furthermore, in step 3, the contents of the components in the mixed material are, by weight, 15 to 18 parts of phenol, 0.5 to 0.8 parts of glutaraldehyde, 10 to 12 parts of soy protein and carboxymethyl chitosan, and 10 to 12 parts of formaldehyde.

[0017] Furthermore, in step 4, the amount of each component used, by weight, is 100 to 150 parts of powder material, 50 to 80 parts of resin material, and 20 to 24 parts of deionized water.

[0018] Furthermore, in step 4, the stirring time is 5 to 10 minutes.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention uses aluminum ash, coal slag ash, coal gangue, silica ash, foundry waste sand, clay, and glass fiber as raw materials, and uses modified phenolic resin as an adhesive to prepare hollow bricks, thereby achieving reasonable resource allocation and turning waste into treasure. Phenolic resin has the advantages of water resistance, heat resistance, and stable chemical properties, and is a common adhesive. However, due to its own brittleness, it is prone to cracking, which affects the compressive strength and yield rate of hollow bricks. Therefore, the present invention uses soybean protein and carboxymethyl chitosan to modify it. Protein and carboxymethyl chitosan have good water solubility, and are combined into protein-carboxymethyl chitosan polymers by electrostatic forces under alkaline conditions. The protein-carboxymethyl chitosan polymer is mixed with phenol and formaldehyde, and a co-condensation reaction occurs under the action of glutaraldehyde to form a three-dimensional mesh structure material that intersects each other; at the same time, glutaraldehyde can change the connection between the aromatic nuclei in the phenolic resin, further improve the toughness of the phenolic resin, and thus prepare high-strength hollow bricks. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The raw materials used in the following examples and their sources:

[0022] Aluminum ash, coal slag ash, coal gangue, silica ash and foundry waste sand are from industrial waste, among which the carbon content of coal gangue is 15-20% and the particle size is 0.5-0.8mm; clay was purchased from Guangao Biotechnology, the main component is kaolinite, with a purity of 99%; glass fiber was purchased from Asia Pacific Technology, with a fiber length of 25-300μm; soy protein isolate powder was purchased from Yuxin Biotechnology, model YX8000; carboxymethyl chitosan was purchased from Yuanye Biotechnology, item number S30948-500g, and sodium hydroxide (CAS number: 1310-73-2), phenol (CAS number: 108-95-2), glutaraldehyde (CAS number: 111-30-8) and formaldehyde (CAS number: 50-00-0) were purchased from Aladdin.

[0023] Example 1

[0024] Step 1: 10g aluminum ash, 20g coal slag ash, 18g coal gangue, 10g silica ash, 15g foundry waste sand, 26g clay, and 10g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0025] Step 2: dissolving 20 g of soy protein isolate powder in 100 g of deionized water, and performing ultrasonic dispersion for 15 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 7.5, and stirring at a speed of 300 rpm for 10 min to obtain a soy protein modified solution; adding 4 g of carboxymethyl chitosan to 100 g of the soy protein modified solution, and stirring for 15 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0026] Step 3: 15 g of phenol and 0.5 g of glutaraldehyde were mixed, the pH was adjusted to 8, the temperature was raised to 70° C. for reaction for 30 min, the temperature was lowered to 50° C., 10 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 3 min, the temperature was raised to 80° C., 10 g of formaldehyde was added, the mixture was stirred for reaction for 30 min to obtain a mixed material, and the mixture was subjected to reduced pressure distillation to obtain a resin material;

[0027] Step 4: Mix 100 g of powder material, 50 g of resin material, and 20 g of deionized water, stir for 5 minutes, pour into a mold for curing and molding, and demold to obtain the high-strength hollow brick.

[0028] Example 2

[0029] Step 1: 11g aluminum ash, 22g coal slag ash, 19g coal gangue, 10g silica ash, 16g foundry waste sand, 27g clay, and 10.3g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0030] Step 2: dissolving 21 g of soy protein isolate powder in 103 g of deionized water, and performing ultrasonic dispersion for 24 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 7.6, and stirring at a speed of 390 rpm for 13 min to obtain a soy protein modified solution; adding 5 g of carboxymethyl chitosan to 112 g of the soy protein modified solution, and stirring for 20 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0031] Step 3: 15.2 g of phenol and 0.5 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 75° C. for reaction for 35 min, the temperature was lowered to 55° C., 10.2 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 3 min, the temperature was raised to 85° C., 10.2 g of formaldehyde was added, the mixture was stirred for reaction for 35 min to obtain a mixed material, and the resin material was obtained by vacuum distillation;

[0032] Step 4: 101 g of powder material, 53 g of resin material and 21 g of deionized water are mixed, stirred for 6 minutes, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0033] Example 3

[0034] Step 1: 11.3 g aluminum ash, 22.4 g coal slag ash, 19 g coal gangue, 10.3 g silica ash, 16 g foundry waste sand, 27 g clay, and 10.3 g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0035] Step 2: dissolving 23 g of soy protein isolate powder in 106 g of deionized water, and performing ultrasonic dispersion for 16 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 7.5, and stirring at a speed of 350 rpm for 12 min to obtain a soy protein modified solution; adding 5.6 g of carboxymethyl chitosan to 107 g of the soy protein modified solution, and stirring for 17 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0036] Step 3: 16.3 g of phenol and 0.58 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 80° C. for reaction for 38 min, the temperature was lowered to 55° C., 10.6 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 3.5 min, the temperature was raised to 85° C., 10.1 g of formaldehyde was added, the mixture was stirred for reaction for 40 min to obtain a mixed material, and the resin material was obtained by vacuum distillation;

[0037] Step 4: 110 g of powder material, 60 g of resin material and 21.3 g of deionized water are mixed, stirred for 6.5 min, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0038] Example 4

[0039] Step 1: 12.3 g aluminum ash, 20.5 g coal slag ash, 19 g coal gangue, 10.8 g silica ash, 18 g foundry waste sand, 28 g clay, and 10.7 g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0040] Step 2: dissolving 22 g of soy protein isolate powder in 107.5 g of deionized water, and performing ultrasonic dispersion for 20 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 8, and stirring at a speed of 360 rpm for 12 min to obtain a soy protein modified solution; adding 5.6 g of carboxymethyl chitosan to 108 g of the soy protein modified solution, and stirring for 20 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0041] Step 3: 15.8 g of phenol and 0.68 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 80° C. for reaction for 50 min, the temperature was lowered to 55° C., 11.2 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 4.5 min, the temperature was raised to 85° C., 11.3 g of formaldehyde was added, the mixture was stirred for reaction for 40 min to obtain a mixed material, and the resin material was obtained by vacuum distillation;

[0042] Step 4: 120 g of powder material, 65 g of resin material, and 22.5 g of deionized water are mixed, stirred for 7.5 min, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0043] Example 5

[0044] Step 1: 11.4 g aluminum ash, 23.4 g coal slag ash, 23.3 g coal gangue, 11.4 g silica ash, 17.8 g foundry waste sand, 28.6 g clay, and 11.3 g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0045] Step 2: dissolving 26.3 g of soy protein isolate powder in 110 g of deionized water, and performing ultrasonic dispersion for 21 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 7.7, and stirring at a speed of 400 rpm for 13 min to obtain a soy protein modified solution; adding 5.6 g of carboxymethyl chitosan to 107 g of the soy protein modified solution, and stirring for 22 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0046] Step 3: 17.5 g of phenol and 0.62 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 85° C. for reaction for 48 min, the temperature was lowered to 55° C., 11.8 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 5 min, the temperature was raised to 86° C., 10.9 g of formaldehyde was added, the mixture was stirred for reaction for 49 min to obtain a mixed material, and the resin material was obtained by vacuum distillation;

[0047] Step 4: 130 g of powder material, 72 g of resin material and 22 g of deionized water are mixed, stirred for 7.5 min, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0048] Example 6

[0049] Step 1: 13.8 g aluminum ash, 23.6 g coal slag ash, 25.3 g coal gangue, 11.6 g silica ash, 21.5 g foundry waste sand, 32.2 g clay, and 11.5 g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0050] Step 2: dissolving 28.3 g of soy protein isolate powder in 115 g of deionized water, and performing ultrasonic dispersion for 26 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 8, and stirring at a speed of 490 rpm for 13 min to obtain a soy protein modified solution; adding 8.6 g of carboxymethyl chitosan to the 115 g soy protein modified solution, and stirring for 27 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0051] Step 3: 17.1 g of phenol and 0.68 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 85° C. for reaction for 50 min, the temperature was lowered to 50° C., 11.3 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 3.5 min, the temperature was raised to 90° C., 12 g of formaldehyde was added, the mixture was stirred for reaction for 55 min to obtain a mixed material, and the resin material was obtained by vacuum distillation;

[0052] Step 4: 140 g of powder material, 75 g of resin material and 23 g of deionized water were mixed, stirred for 9 minutes, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0053] Example 7

[0054] Step 1: 15g aluminum ash, 23g coal slag ash, 24g coal gangue, 11g silica ash, 19g foundry waste sand, 29g clay, and 11.3g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0055] Step 2: dissolving 28 g of soy protein isolate powder in 118 g of deionized water, and performing ultrasonic dispersion for 27 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 8, and stirring at a speed of 500 rpm for 14 min to obtain a soy protein modified solution; adding 8 g of carboxymethyl chitosan to the 118 g soy protein modified solution, and stirring for 28 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0056] Step 3: 17.8 g of phenol and 0.78 g of glutaraldehyde were mixed, the pH was adjusted to 9, the temperature was raised to 90° C. for reaction for 40 min, the temperature was lowered to 55° C., 11.6 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 4.3 min, the temperature was raised to 86° C., 11.8 g of formaldehyde was added, the mixture was stirred for reaction for 48 min to obtain a mixed material, and the resin material was obtained by vacuum distillation;

[0057] Step 4: 143 g of powder material, 76 g of resin material, and 23.7 g of deionized water were mixed, stirred for 9 minutes, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0058] Example 8

[0059] Step 1: 14 g aluminum ash, 24.7 g coal slag ash, 26.3 g coal gangue, 11.6 g silica ash, 21.6 g foundry waste sand, 33 g clay, and 10.9 g glass fiber were crushed, mixed, and stirred to obtain a powder material;

[0060] Step 2: dissolving 28.7 g of soy protein isolate powder in 116 g of deionized water, and performing ultrasonic dispersion for 30 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 7.5, and stirring at a speed of 330 rpm for 15 min to obtain a soy protein modified solution; adding 8.6 g of carboxymethyl chitosan to 108 g of the soy protein modified solution, and stirring for 28 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0061] Step 3: 17.1 g of phenol and 0.63 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 86° C. for reaction for 55 min, the temperature was lowered to 58° C., 12 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 5 min, the temperature was raised to 85° C., 11.7 g of formaldehyde was added, the mixture was stirred for reaction for 45 min to obtain a mixed material, and the mixture was subjected to reduced pressure distillation to obtain a resin material;

[0062] Step 4: 141 g of powder material, 72 g of resin material, and 21 g of deionized water were mixed, stirred for 8 minutes, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0063] Example 9

[0064] Step 1: 15g aluminum ash, 25g coal slag ash, 27g coal gangue, 12g silica ash, 22g foundry waste sand, 35g clay, and 12g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0065] Step 2: dissolving 30 g of soy protein isolate powder in 120 g of deionized water, and performing ultrasonic dispersion for 30 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 8, and stirring at a speed of 500 rpm for 15 min to obtain a soy protein modified solution; adding 10 g of carboxymethyl chitosan to the 120 g soy protein modified solution, and stirring for 15 to 30 min to obtain a mixed solution of soy protein and carboxymethyl chitosan;

[0066] Step 3: 18 g of phenol and 0.8 g of glutaraldehyde were mixed, the pH was adjusted to 9, the temperature was raised to 90° C. for reaction for 60 min, the temperature was lowered to 60° C., 12 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 5 min, the temperature was raised to 90° C., 12 g of formaldehyde was added, the mixture was stirred for reaction for 60 min to obtain a mixed material, and the mixture was distilled under reduced pressure to obtain a resin material;

[0067] Step 4: Mix 150 g of powder material, 80 g of resin material, and 24 g of deionized water, stir for 10 minutes, pour into a mold for curing and molding, and demold to obtain the high-strength hollow brick.

[0068] Comparative Example 1

[0069] Only phenolic resin was used as adhesive to prepare hollow bricks.

[0070] Step 1: 10g aluminum ash, 20g coal slag ash, 18g coal gangue, 10g silica ash, 15g foundry waste sand, 26g clay, and 10g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0071] Step 2: Mix 100 g of powder material, 50 g of phenolic resin material, and 20 g of deionized water, stir for 5 minutes, pour into a mold for curing and molding, and demold to obtain the high-strength hollow brick.

[0072] Comparative Example 2

[0073] Hollow bricks were prepared using only soy protein modified phenolic resin as adhesive.

[0074] Step 1: 11.3 g aluminum ash, 22.4 g coal slag ash, 19 g coal gangue, 10.3 g silica ash, 16 g foundry waste sand, 27 g clay, and 10.3 g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0075] Step 2: dissolving 23 g of soy protein isolate powder in 106 g of deionized water, and performing ultrasonic dispersion for 16 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 7.5, and stirring at a speed of 350 rpm for 12 min to obtain a soy protein modified solution;

[0076] Step 3: 16.3 g of phenol and 0.58 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 80° C. and the reaction was carried out for 38 min, the temperature was lowered to 55° C., 10.6 g of the soy protein modified solution was added, the mixture was stirred for 3.5 min, the temperature was raised to 85° C., 10.1 g of formaldehyde was added, the mixture was stirred and reacted for 40 min to obtain a mixed material, and the resin material was obtained by vacuum distillation;

[0077] Step 4: 110 g of powder material, 60 g of resin material and 21.3 g of deionized water are mixed, stirred for 6.5 min, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0078] Comparative Example 3

[0079] Only carboxymethyl chitosan modified phenolic resin was used as adhesive to prepare hollow bricks.

[0080] Step 1: 11.3 g aluminum ash, 22.4 g coal slag ash, 19 g coal gangue, 10.3 g silica ash, 16 g foundry waste sand, 27 g clay, and 10.3 g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0081] Step 2: 16.3 g of phenol and 0.58 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 80° C. and the mixture was reacted for 38 min, the temperature was lowered to 55° C., 10.6 g of carboxymethyl chitosan solution was added, the mixture was stirred for 3.5 min, the temperature was raised to 85° C., 10.1 g of formaldehyde was added, the mixture was stirred and reacted for 40 min to obtain a mixed material, and the mixture was subjected to reduced pressure distillation to obtain a resin material;

[0082] Step 3: Mix 110 g of powder material, 60 g of resin material, and 21.3 g of deionized water, stir for 6.5 min, pour into a mold for curing and molding, and demold to obtain the high-strength hollow brick.

[0083] Comparative Example 4

[0084] Chitosan was used as adhesive instead of carboxymethyl chitosan modified phenolic resin to prepare hollow bricks.

[0085] Step 1: 12.3 g aluminum ash, 20.5 g coal slag ash, 19 g coal gangue, 10.8 g silica ash, 18 g foundry waste sand, 28 g clay, and 10.7 g glass fiber are crushed, mixed, and stirred to obtain a powder material;

[0086] Step 2: dissolving 22 g of soy protein isolate powder in 107.5 g of deionized water, and performing ultrasonic dispersion for 20 min to obtain a soy protein solution; adding sodium hydroxide solution to the soy protein solution to adjust the pH to 5, and stirring at a speed of 360 rpm for 12 min to obtain a soy protein modified solution; adding 5.6 g of chitosan to 108 g of the soy protein modified solution, and stirring for 20 min to obtain a mixed solution of soy protein and chitosan;

[0087] Step 3: 15.8 g of phenol and 0.68 g of glutaraldehyde were mixed, the pH was adjusted to 8.5, the temperature was raised to 80° C. for reaction for 50 min, the temperature was lowered to 55° C., 11.2 g of a mixed solution of soybean protein and carboxymethyl chitosan was added, the mixture was stirred for 4.5 min, the temperature was raised to 85° C., 11.3 g of formaldehyde was added, the mixture was stirred for reaction for 40 min to obtain a mixed material, and the resin material was obtained by vacuum distillation;

[0088] Step 4: 120 g of powder material, 65 g of resin material, and 22.5 g of deionized water are mixed, stirred for 7.5 min, poured into a mold for curing and molding, and demolded to obtain the high-strength hollow brick.

[0089] experiment:

[0090] The hollow bricks prepared in Examples 1 to 9 and Comparative Examples 1 to 4 were tested for compressive strength and yield rate, wherein the compressive strength test method is: the hollow bricks are made into a size of 250×100×100mm, placed flat on a pressure plate, the load is increased at a uniform speed of 4kN / s, and the maximum breaking load is recorded. The compressive strength = maximum breaking load / stress area; the yield rate calculation method: yield rate = number of finished products / total number.

[0091] Example Compressive strength / MPa Yield rate / % Example 1 27.4 99.3 Example 2 27.9 98.9 Example 3 26.8 98.7 Example 4 28.1 99.1 Example 5 27.5 99.5 Example 6 26.6 98.6 Example 7 26.9 99.6 Example 8 27.3 98.4 Example 9 26.1 99.3 Comparative Example 1 18.3 95.5 Comparative Example 2 21.5 99.2 Comparative Example 3 19.7 96.3 Comparative Example 4 17.6 94.1

[0092] in conclusion:

[0093] The present invention mixes waste materials such as aluminum ash, coal slag ash, coal gangue, silica ash, and foundry waste sand in industrial production with clay and glass fiber, and uses modified phenolic resin as an adhesive to prepare hollow bricks. After testing, the data of Examples 1 to 9 show that the compressive strength of the hollow bricks prepared by the present invention reaches more than 26MPa, and the yield is more than 98%. Taking Example 1 as a reference, the data of Comparative Example 1 show that the compressive performance of the hollow bricks is poor, which is due to the brittleness and poor toughness of the phenolic resin itself; Comparative Example 2 uses soy protein to modify the phenolic resin. Soy protein is rich in amino groups and can be co-condensed to modify the phenolic resin, thereby forming a cross-linked network, which can improve the bonding strength of the phenolic resin, so the yield is higher, but due to the lack of carboxymethyl chitosan, the compressive strength of the prepared hollow bricks is not as good as that of Example 2; Comparative Example 3 uses carboxymethyl chitosan to modify the phenolic resin as As for the adhesive, carboxymethyl chitosan has certain film-forming property, but because its surface -NH2 group is replaced, it is difficult to connect with phenol and formaldehyde to form a co-condensation structure, and the modification effect on phenolic resin is not good, so the compressive performance of hollow bricks is not as good as that of Example 3; Comparative Example 4 uses chitosan instead of carboxymethyl chitosan. Since chitosan is only dissolved under acidic conditions and the dissolution amount is low, and the reaction environment is alkaline, it is difficult for chitosan to modify phenolic resin to achieve the modification effect of carboxymethyl chitosan, and the performance of the prepared hollow bricks is also worse than that of Example 4. In addition, the above experimental results show that the bonding strength of the modified phenolic resin is improved, so the yield rate of hollow bricks is also higher than that of Comparative Examples 1 to 4.

[0094] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for preparing high-strength hollow bricks, characterized in that: The following steps are involved: Step 1: crushing and mixing aluminum ash, coal slag ash, coal gangue, silica ash, foundry waste sand, clay and glass fiber to obtain a powder material; Step 2: dissolving the isolated soy protein powder in deionized water, and dispersing by ultrasonication to obtain a soy protein solution; adding a sodium hydroxide solution to the soy protein solution to adjust the pH, and stirring to obtain a soy protein modified solution; adding carboxymethyl chitosan to the soy protein modified solution, and stirring to obtain a mixed solution of soy protein and carboxymethyl chitosan; Step 3: Mix phenol and glutaraldehyde, adjust the pH to 8-9, heat to 70-90°C for reaction for 30-60min, cool to 50-60°C, add a mixed solution of soybean protein and carboxymethyl chitosan, stir and heat to 80-90°C, add formaldehyde and stir to react for 30-60min to obtain a mixed material, and perform reduced pressure distillation to obtain a resin material; Step 4: Mix the powder material, the resin material and the deionized water, stir and pour into a mold for curing and molding, and demold to obtain the high-strength hollow brick; wherein the amount of each component is, by weight, 100-150 parts of the powder material, 50-80 parts of the resin material, and 20-24 parts of deionized water.

2. The process for preparing a high-strength hollow brick according to claim 1, characterized in that: In step 1, the contents of the components in the powder material are, by weight, 10 to 15 parts of aluminum ash, 20 to 25 parts of coal slag ash, 18 to 27 parts of coal gangue, 10 to 12 parts of silica ash, 15 to 22 parts of foundry waste sand, 26 to 35 parts of clay, and 10 to 12 parts of glass fiber.

3. The process for preparing a high-strength hollow brick according to claim 1, characterized in that: In step 2, the content of each component in the soy protein solution is, by weight, 20 to 30 parts of soy protein isolate powder and 100 to 120 parts of deionized water.

4. The process for preparing a high-strength hollow brick according to claim 1, characterized in that: In step 2, the ultrasonic dispersion time is 15 to 30 minutes; and the pH value of the sodium hydroxide solution is adjusted to 7.5 to 8.

0.

5. The process for preparing a high-strength hollow brick according to claim 1, characterized in that: In step 2, the content of each component in the mixed solution of soybean protein and carboxymethyl chitosan is, by weight, 100-120 parts of soybean protein modified solution and 4-10 parts of carboxymethyl chitosan.

6. The process for preparing a high-strength hollow brick according to claim 1, characterized in that: In step 3, the contents of the components in the mixed material are, by weight, 15 to 18 parts of phenol, 0.5 to 0.8 parts of glutaraldehyde, 10 to 12 parts of a mixed solution of soy protein and carboxymethyl chitosan, and 10 to 12 parts of formaldehyde.

7. The process for preparing a high-strength hollow brick according to claim 1, characterized in that: In step 4, the stirring time is 5 to 10 minutes.

8. A hollow brick prepared according to the process for preparing a high-strength hollow brick according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • High-strength corrugated case binder and production method thereof

    CN109852341A