High-temperature-cooking-resistant tank cover chromium-free passivator and preparation method thereof

By using a chromium-free passivator combined with fluorotitanic acid and other compounds, the safety and adhesion problems of the chromium-containing passivator in the aluminum can lid are solved, and efficient passivation film formation and corrosion resistance are achieved, which meets the Safety requirements in the field of food packaging.

CN119061390AActive Publication Date: 2024-12-03TAISHAN KEMEI CHEM IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411486021.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-03
Estimated Expiration
2044-10-23

AI Technical Summary

Technical Problem

The passivating agents for existing aluminum can lids are mostly chromium-containing materials, which have potential harm to human health and the environment. The chromium-free passivating agent has insufficient adhesion and corrosion resistance, making it difficult to meet the safety requirements in the food packaging field. .

Method used

Fluorotitanic acid is used as the main film forming component, combined with zirconium methacrylate, phosphoric acid and polyacrylic acid, ammonium tungstate or ammonium heptamolybdate is used as film forming promoter, and aminosilane coupling agent and hyperbranched surfactant are added , a high temperature cooking type chromium-free passivating agent is formed by a specific preparation method.

Benefits of technology

It achieves good adhesion between the chromium-free passivator and the aluminum can lid, improves the corrosion resistance and high temperature resistance of the passivation film, avoids the risk of chromium use, and improves the safety and environmental protection performance of beverage packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005098724200000051
    Figure BDA0005098724200000051
  • Figure BDA0005098724200000061
    Figure BDA0005098724200000061
  • Figure BDA0005098724200000071
    Figure BDA0005098724200000071
Patent Text Reader

Abstract

The invention discloses a chromium-free passivating agent for a high-temperature cooking resistant tank cover. The chromium-free passivating agent is prepared from the following raw materials in percentage by weight: 0.5-2% of organic zirconium, 1-5% of inorganic acid, 5-10% of a film material, 0.5-2% of a film-forming accelerant, 1-5% of a silane coupling agent, 3-10% of an auxiliary agent and the balance of pure water. The main component of the passivation film is fluotitanic acid, and the chromium-free passivation film is adopted, so that potential risks caused by using a chromium-containing passivator are avoided, the use safety is improved, no pollution is caused to the environment, and the modern environmental protection requirement is met. And the combination of zirconium methacrylate, phosphoric acid and polyacrylic acid is adopted, so that the adhesive force between the passivation film and the aluminum ring-pull can cover can be improved, the thickness of the passivation film is increased, and the corrosion resistance of the passivation film is improved. The chromium-free passivating agent is applied to the aluminum ring-pull can cover plate strip, and the water boiling resistance, the acid boiling resistance and the sulfur boiling resistance are excellent under the high-temperature condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of C09D coating compositions, and in particular to a chromium-free passivating agent for high-temperature resistant retorting can lids and a preparation method thereof. Background Art

[0002] The materials of aluminum can lids usually include 3104 aluminum alloy, 5052 aluminum alloy, and 5182 aluminum alloy, which are widely used in the field of food packaging. In the surface treatment of aluminum can lid strips, the aluminum strips will be cleaned, passivated, and coated. The aluminum can lid is coated with a passivator to prevent the beverage from directly contacting the aluminum, avoid aluminum ions from dissolving in the beverage, and maintain the quality and taste of the beverage. The passivators commonly used in existing aluminum can lids are mostly chromium (trivalent chromium) passivators, which have good corrosion resistance. Although trivalent chromium is safer than hexavalent chromium in food safety, trivalent chromium, as a heavy metal element, still poses a great hazard to human health and the natural environment. Therefore, it is crucial to develop a chromium-free passivator and maintain good adhesion between the chromium-free passivator and the can lid.

[0003] Chinese invention patent CN201410389381.7 discloses a chromium-free composite passivator for hot-dip galvanized steel plate and its preparation and use method. First, the organosilane is dissolved in water, stirred until completely dissolved, and then the main salt compound is added. After dissolving, an inorganic acid is added to measure the pH value, and then sulfate and inorganic zirconium salt are added under stirring. After completely dissolved, a water-based resin is added. The passivator does not contain chromium and is non-toxic and harmless. The thickness of the passivation film can reach 8-1.0 mg / m 2 , the corrosion resistance is close to the level of hexavalent chromium passivation solution, but resin is required, and the safety performance is not high in beverage packaging. Chinese invention patent CN201410081359.6 discloses a chromium-free composite passivator for galvanized sheet of steel plant continuous annealing line and its preparation method. The passivator includes coupling agent, silicate, emulsifier, corrosion inhibitor. The prepared passivator has uniform and stable appearance and significantly improved corrosion resistance, but it cannot meet the safety requirements of food packaging. Summary of the invention

[0004] In order to develop a chromium-free passivator and maintain good adhesion between the chromium-free passivator and the can lid, the first aspect of the present invention provides a high-temperature resistant cooking type can lid chromium-free passivator, and the preparation raw materials include, by weight percentage: 0.5-2% organic zirconium, 1-5% inorganic acid, 5-10% film material, 0.5-2% film-forming promoter, 1-5% silane coupling agent, 3-10% auxiliary agent, and pure water is supplemented to 100%.

[0005] As a preferred embodiment, the organic zirconium is selected from at least one of zirconium methacrylate, butyl zirconate, zirconium acetylacetonate, zirconium isobutoxide, zirconium acetate, tetraethoxy zirconium, and tetrabenzyl zirconium.

[0006] As a preferred embodiment, the organic zirconium is zirconium methacrylate.

[0007] As a preferred embodiment, the inorganic acid is selected from at least one of phosphoric acid, sulfuric acid, nitric acid, hydrochloric acid, boric acid and carbonic acid.

[0008] As a preferred embodiment, the inorganic acid is phosphoric acid.

[0009] As a preferred embodiment, the film material is a fluorine compound, and the fluorine compound is selected from at least one of fluorotitanic acid, fluorozirconic acid, ammonium bifluoride, fluoroboric acid, and hydrofluoric acid.

[0010] As a preferred implementation, the membrane material is fluorotitanic acid.

[0011] The applicant found in the experiment that the coating on the surface of the aluminum can lid also has a certain adhesion when using fluorotitanic acid as the main film-forming component, which can replace the chromium-containing passivator and improve the safety of use in beverage packaging. The reason may be that the chromium-containing passivator usually contains trivalent chromium. When the passivation film structure is unstable, it may be converted into hexavalent chromium, which is unsafe to use in beverage packaging, and the chromium-containing passivator still has great harm to the environment. Therefore, using fluorotitanic acid as the main film-forming component can avoid the use of chromium and improve the safety of use. However, the chromium-free passivator still has a certain lack of bonding with the aluminum lid during the film-forming process.

[0012] As a preferred implementation, the film-forming promoter is a high-valent metal compound, and the high-valent metal compound is selected from at least one of ammonium tungstate, ammonium heptamolybdate, ammonium tetramolybdate, and ammonium heptatungstate.

[0013] As a preferred implementation, the film-forming promoter is ammonium tungstate or ammonium heptamolybdate.

[0014] As a preferred embodiment, the silane coupling agent is an aminosilane coupling agent or an acyloxysilane coupling agent, and the aminosilane coupling agent is selected from at least one of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl-trimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyl-methyl-trimethoxysilane. The acyloxysilane coupling agent is γ-methacryloxypropyltrimethoxysilane.

[0015] As a preferred embodiment, the silane coupling agent is selected from at least one of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and γ-methacryloxypropyltrimethoxysilane.

[0016] As a preferred embodiment, the auxiliary agent includes at least one of a stabilizer and a wetting and dispersing agent, the stabilizer is polyacrylic acid, and the average molecular weight of the polyacrylic acid is 2000-5000 Da.

[0017] The applicant discovered during the experiment that by introducing zirconium methacrylate and phosphoric acid into the polyacrylic acid system, the adhesion between the passivation film and the substrate can be improved, and the thickness of the passivation film can be increased. The possible reasons are speculated to be: in the polyacrylic acid system, zirconium methacrylate reacts with phosphoric acid to generate a nano-scale microparticle suspension, and the nano-scale microparticles produce slight protrusions on the surface of the fluorine titanium passivation film, increasing the roughness of the passivation film and improving the adhesion to the smooth substrate surface. In addition, the polyacrylic acid system contains more polar groups, which further improves the adhesion to the aluminum can cover. At the same time, the nano-scale microparticles generated by the reaction of zirconium methacrylate and phosphoric acid increase the thickness of the passivation film, and the structure of the passivation film is more stable, and the corrosion resistance of the passivation film is also improved.

[0018] However, the generated nano-scale microparticle suspension is prone to precipitation during storage. The weight ratio of zirconium methacrylate, phosphoric acid, and polyacrylic acid is (0.5-2): (1-5): (3-8), which can increase the dispersibility of the passivator system, avoid precipitation during storage, and improve the storage stability of the passivator system.

[0019] As a preferred embodiment, the wetting and dispersing agent is a nonionic surfactant, and the nonionic surfactant is a hyperbranched surfactant with a central hydrophilic group.

[0020] As a preferred implementation, the wetting and dispersing agent is BASF WE 3323.

[0021] The applicant found in the experiment that the use of ammonium tungstate or ammonium heptamolybdate as a film-forming promoter and the addition of an aminosilane coupling agent can accelerate the film formation of the passivating agent, improve the corrosion resistance of the passivating film, and make the passivating film have certain high temperature resistance and water resistance. The possible reasons are speculated to be: ammonium tungstate or ammonium heptamolybdate can accelerate the film formation of the passivating agent under acidic conditions, and ammonium tungstate or ammonium heptamolybdate is a high-valent metal compound that can achieve multivalent state conversion to improve the corrosion resistance of the passivating film. In addition, with the use of an aminosilane coupling agent, the drying temperature of the passivating film can be reduced. When the aluminum strip passes through the drying plate, the film can be quickly formed at 60-65°C. The passivating film and the aluminum strip have a good bonding effect under low-temperature film formation, and the passivating film can achieve the technical effects of water boiling resistance, acid boiling resistance, and high-temperature vulcanization resistance.

[0022] The second aspect of the present invention provides a method for preparing a chromium-free passivating agent for a high temperature resistant retort can lid, comprising the following steps:

[0023] S1: dissolve the inorganic acid in pure water, start the disperser, control the reaction temperature, slowly add the silane coupling agent, continue to disperse for 20-30 minutes, adjust the pH, and disperse again for 20-40 minutes to obtain a mixed solution I;

[0024] S2 accelerates the dispersion of the mixed solution I, controls the reaction temperature, adds the additive, disperses for 5-15 minutes, slowly adds the organic zirconium, and continues to disperse for 1-3 hours;

[0025] S3 slows down and disperses, cooling to room temperature;

[0026] S4 slowly adds membrane material and film-forming accelerator and disperses for 20-40 minutes.

[0027] As a preferred embodiment, the dispersion speed of step S1 is 300-400 r / min, and the dispersion speed of step S2 is 800-1000 r / min.

[0028] As a preferred embodiment, the pH of step S1 is 2-3; the reaction temperature of step S1 is 15-25°C.

[0029] As a preferred embodiment, the speed of adding the silane coupling agent in step S1 is 3-7% of the formula amount of the silane coupling agent per minute.

[0030] As a preferred embodiment, the reaction temperature in step S2 is 35-40° C., and the adding speed of organic zirconium in step S2 is 1-2% of the formula amount of organic zirconium per minute.

[0031] As a preferred embodiment, after dispersion in step S2, the solution is slightly turbid, and a sample is taken and cooled to room temperature and allowed to stand for 20-40 minutes until there is no obvious floating matter or precipitation in the solution.

[0032] As a preferred embodiment, the film material and the film-forming accelerator are added at a speed of 10-15% of the formulated amount of the film material and the film-forming accelerator per minute in step S4.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The chromium-free passivating agent for the high-temperature cooking-resistant can lid of the present invention has a passivating film whose main component is fluorotitanic acid. The use of a chromium-free passivating film avoids the potential risks of using a chromium-containing passivating agent, improves safety in use, does not pollute the environment, and meets modern environmental protection requirements.

[0035] (2) The chromium-free passivating agent for the high temperature resistant retort can lid of the present invention adopts a combination of zirconium methacrylate, phosphoric acid and polyacrylic acid, which can improve the adhesion between the passivation film and the aluminum can lid, increase the thickness of the passivation film, and improve the corrosion resistance of the passivation film.

[0036] (3) The chromium-free passivator for the high-temperature resistant retort-type can lid of the present invention uses ammonium tungstate or ammonium heptamolybdate as a film-forming accelerator, and also includes an aminosilane coupling agent, which can accelerate the film formation of the passivator, improve the corrosion resistance of the passivation film, and make the passivation film have certain high temperature resistance and water resistance.

[0037] (4) The chromium-free passivator for high temperature resistant retort can lids of the present invention adopts a hyperbranched surfactant with a central hydrophilic group as a wetting and dispersing agent, which can increase the wetting speed of the passivator on the substrate, make the microparticles evenly dispersed, maintain the stability of the system, and prevent the passivator from polymerizing, precipitating or cross-linking under normal temperature conditions.

[0038] (5) The high temperature boiling resistant can lid chromium-free passivator of the present invention is applied to the aluminum can lid strip, and has excellent water boiling resistance, acid boiling resistance and sulfur boiling resistance under high temperature conditions. DETAILED DESCRIPTION

[0039] Example

[0040] A chromium-free passivating agent for high temperature resistant retorting can lids, the raw materials for preparation are shown in the following table 1 in terms of weight percentage:

[0041] Table 1

[0042]

[0043] The KH-792 is N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane; the KH-550 is γ-aminopropyltriethoxysilane; the KH-570 is γ-methacryloxypropyltrimethoxysilane. The average molecular weight of the polyacrylic acid is 2000-5000Da, and the CAS number is 9003-01-4.

[0044] A method for preparing a chromium-free passivating agent for a high-temperature resistant retort can lid comprises the following steps:

[0045] S1: dissolve the inorganic acid in pure water, start the disperser, control the reaction temperature, slowly add the silane coupling agent, continue to disperse for 20 minutes, adjust the pH, and disperse again for 30 minutes to obtain a mixed solution I;

[0046] S2 accelerates the dispersion of mixed solution I, controls the reaction temperature, adds additives, disperses for 10 min, slowly adds organic zirconium, and continues to disperse for 2 h;

[0047] S3 slows down and disperses, cooling to room temperature;

[0048] S4 slowly adds membrane material and film-forming accelerator and disperses for 30 minutes.

[0049] The dispersion speed of step S1 is 350 r / min, and the dispersion speed of step S2 is 900 r / min.

[0050] The pH of step S1 is 2.5; the reaction temperature of step S1 is 20°C.

[0051] The speed of adding the silane coupling agent in step S1 is 5% of the formula amount of the silane coupling agent per minute.

[0052] The reaction temperature in step S2 is 37.5° C., and the adding speed of organic zirconium in step S2 is 1% of the formula amount of organic zirconium per minute.

[0053] After dispersion in step S2, the solution is slightly turbid. Samples are taken and cooled to room temperature and allowed to stand for 30 minutes until there is no obvious floating matter or precipitation in the solution.

[0054] The adding speed of the film material and the film-forming accelerator in the step S4 is 10% of the formula amount of the film material and the film-forming accelerator per minute.

[0055] Comparative Example

[0056] A chromium-free passivating agent for high temperature resistant retorting can lids, the raw materials for preparation are shown in the following table 2 in terms of weight percentage:

[0057] Table 2

[0058]

[0059] A method for preparing a chromium-free passivating agent for high-temperature resistant retort can lids, the specific implementation method is the same as that of Example 1.

[0060] Performance Testing

[0061] The passivating agent prepared in the embodiment and the comparative example was diluted 6 times with deionized water, and coated on the inner side of the can lid by a roller, and dried at a plate temperature of 60° C. to obtain a passivation film.

[0062] The test was conducted according to the internal coating requirements of "YS / T726-2010 Aluminum Alloy Sheet and Strip for Can Cover and Ring Pull Materials". The test results are shown in Table 3.

[0063] High temperature sterilization: 121℃, 30min distillation, the coating is qualified if there is no whitening, loss of gloss, peeling or falling off;

[0064] Acid resistance: 121℃, 32min acid etching, the coating is qualified if there is no whitening, loss of gloss, peeling or falling off;

[0065] Sulfur resistance: 121℃, 31min sulfur corrosion, the coating is qualified if there is no whitening, loss of gloss, peeling or falling off;

[0066] Adhesion level 1 (no peeling or falling off in the 100-grid test of the coating) is qualified.

[0067] Table 3

[0068]

Claims

1. A chromium-free passivating agent for high temperature resistant retort can lids, characterized in that: The raw materials for preparation include, by weight percentage: 0.5-2% organic zirconium, 1-5% inorganic acid, 5-10% film material, 0.5-2% film-forming accelerator, 1-5% silane coupling agent, 3-10% auxiliary agent, and pure water is added to 100%.

2. The chromium-free passivating agent for high temperature resistant retort can lids according to claim 1, characterized in that: The organic zirconium is selected from at least one of zirconium methacrylate, butyl zirconate, zirconium acetylacetonate, zirconium isobutoxide, zirconium acetate, tetraethoxy zirconium, and tetrabenzyl zirconium.

3. The chromium-free passivating agent for high temperature resistant retort can lids according to claim 1, characterized in that: The inorganic acid is selected from at least one of phosphoric acid, sulfuric acid, nitric acid, hydrochloric acid, boric acid and carbonic acid.

4. The chromium-free passivating agent for high temperature resistant retort can lids according to claim 1, characterized in that: The film material is a fluorine compound, and the fluorine compound is selected from at least one of fluorotitanic acid, fluorozirconic acid, ammonium bifluoride, fluoroboric acid, and hydrofluoric acid.

5. The chromium-free passivating agent for high temperature resistant retort can lids according to claim 1, characterized in that: The film-forming promoter is a high-valent metal compound, and the high-valent metal compound is selected from at least one of ammonium tungstate, ammonium heptamolybdate, ammonium tetramolybdate, and ammonium heptatungstate.

6. The chromium-free passivating agent for high temperature resistant retort can lids according to claim 1, characterized in that: The silane coupling agent is an aminosilane coupling agent or an acyloxysilane coupling agent, and the aminosilane coupling agent is selected from at least one of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl-trimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyl-methyl-trimethoxysilane.

7. The chromium-free passivating agent for high temperature resistant retort can lids according to claim 1, characterized in that: The auxiliary agent includes at least one of a stabilizer and a wetting and dispersing agent. The stabilizer is polyacrylic acid, and the average molecular weight of the polyacrylic acid is 2000-5000Da.

8. The chromium-free passivating agent for high temperature resistant retort can lids according to claim 7, characterized in that: The wetting and dispersing agent is a nonionic surfactant, and the nonionic surfactant is a hyperbranched surfactant with a central hydrophilic group.

9. A method for preparing the chromium-free passivating agent for high temperature resistant retort can lids according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: dissolve the inorganic acid in pure water, start the disperser, control the reaction temperature, slowly add the silane coupling agent, continue to disperse for 20-30 minutes, adjust the pH, and disperse again for 20-40 minutes to obtain a mixed solution I; S2 accelerates the dispersion of the mixed solution I, controls the reaction temperature, adds the additive, disperses for 5-15 minutes, slowly adds the organic zirconium, and continues to disperse for 1-3 hours; S3 slows down and disperses, cooling to room temperature; S4 slowly adds membrane material and film-forming accelerator and disperses for 20-40 minutes.

10. The method for preparing the chromium-free passivating agent for high temperature resistant retort can lids according to claim 9, characterized in that: The dispersion speed of step S1 is 300-400 r / min, and the dispersion speed of step S2 is 800-1000 r / min.

Citation Information

Patent Citations

  • Chromium-free coating agent and preparation method thereof

    CN103938199A

  • Titanium-zirconium coloured chromium-free passivation solution for surface treatment of aluminium alloy, method for treating aluminium alloy surface using same, and use thereof

    CN107429404A

  • Chrome-free environmental-friendly passivator for tank cover packaging material pretreatment and preparation method thereof

    CN108866526A

  • Aluminum alloy template surface layer passivating liquid as well as preparation method and passivation treatment process thereof

    CN109468626A

  • Cr-free sealing solution and method of fabricating phosphated electro-galvanized steel sheet using the same

    KR1020090073908A