Sheath with improved performance
By using multimodal ethylene copolymer composition and Ziegler-Natta catalyst in cable sheath materials, the balance problem of existing materials between flexibility and mechanical strength is solved, achieving higher flexibility and hardness , suitable for high-demand applications of underground facilities.
Patent Information
- Application Number
- CN202110224803.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-05-31
- Filing Date
- 2017-05-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2037-05-29
AI Technical Summary
Existing cable sheath materials are difficult to take into account high flexibility and high mechanical strength, especially in underground facilities that require higher hardness and wear resistance.
Using a multimodal ethylene copolymer composition, a multimodal ethylene copolymer with a density of between 920 and 949 kg/m3 is prepared by using a multimodal ethylene copolymer composition and a specific catalyst component during the polymerization process, combined with a continuous operation process and liquid reaction mixture technology optimizes polymerization conditions to improve the flexibility and mechanical properties of the material.
It achieves the improvement of the flexibility and hardness of the material on the basis of maintaining processability and high mechanical properties, and meets the high demanding cable sheath application needs, especially in underground facilities to provide better mechanical impact resistance.
Smart Images

Figure BDA0002956816160000031 
Figure BDA0002956816160000051 
Figure BDA0002956816160000151
Abstract
Description
[0001] This application is a divisional application of an invention patent application with an application date of May 29, 2017, application number 201780028963.4 (international application number PCT / EP2017 / 062883), and name “Sheath with improved performance”. Technical Field
[0002] The present invention relates to a multimodal ethylene copolymer composition having a molecular weight of 920 to 949 kg / m 3 The multimodal ethylene copolymer composition according to the invention can be used in cable sheathing. Background Art
[0003] Cables usually include a conductor, which is surrounded by one or more layers, depending on the field of application. For example, a power cable has several layers of polymeric material, which include an inner semiconducting layer, followed by an insulating layer, and then an outer semiconducting layer. One or more additional auxiliary layers may also be added to these layers. The outer protective polymer layer is called a sheath layer. Other types of cables are communication cables, which also include several layers and a sheath layer.
[0004] One goal in polyethylene material development is to maximize its flexibility while maintaining other mechanical properties, such as high Shore D for linear low density polyethylene (LLDPE) jacket layer applications.
[0005] Since the outer sheath layer provides external protection for the cable, it plays an important role in providing functionality. Safety, reliability and long-term operation are important key factors in sheath application requirements. On the other hand, the sheath layer has a great influence on the overall flexibility of the cable. Therefore, the flexibility of the sheath layer is the most important factor in obtaining a flexible cable. Flexible cables are easy to handle and install, especially in buildings and conduits.
[0006] Linear low density polyethylene (LLDPE) is known typically (ia) as a jacket layer material. The mechanical properties of the jacket layer can be improved by using polyethylene with a higher density, such as a high density polyethylene (HDPE) polymer. HDPE polymers typically (ia) provide improved mechanical strength and abrasion resistance for the cable layer. However, HDPE has the disadvantage of limited flexibility.
[0007] Multimodal sheathing ethylene polymer compositions are well known in the art, for example EP907682 B1 and EP892979 B1. EP2353169, EP2351049 and EP2182525 disclose flexible polyethylene compositions for cable sheathing, which are prepared using a single site catalyst.
[0008] In the polymer field, there is a continuous need to find polymers that are suitable for demanding applications, especially W&C applications, where the cable materials must meet high demands and strict government regulations.
[0009] In the field of cable sheathing, there is a particular need to provide a material that combines high flexibility with high mechanical strength.
[0010] It is therefore an object of the present invention to provide a bimodal sheath having improved flexibility relative to density while maintaining processability, ie maintaining MFR properties.
[0011] Another object of the invention is to achieve higher or at least similar levels of Shore D(1s) values. Shore D indicates the hardness of a material. This parameter is particularly important for underground installations, where the cables are subjected to a more severe environment. Summary of the invention
[0012] definition
[0013] "Multimodal copolymer" means a copolymer containing different fractions having different average molecular weights or different comonomer contents or both. Multimodal copolymers are produced by copolymerizing ethylene and comonomers in two or more polymerization stages, wherein the polymerization conditions are sufficiently different to allow the production of different polymers in the different stages. Alternatively, multimodal copolymers may be produced in a single polymerization stage by using two or more different catalysts or by using a multicomponent catalyst comprising compounds of at least two different transition metals.
[0014] "Continuously operating process" means a process or process stage into which raw materials are continuously or intermittently introduced and products are continuously or intermittently removed. Continuous addition or removal means an uninterrupted stream flows into or out of a process or process stage. Intermittent addition or removal means that small batches of raw materials are constantly added or small batches of product are constantly removed from a process or process stage during the operation. The cycle time between these batches is short compared to the total average residence time of the process or process stage, for example, not more than 10% of the total average residence time.
[0015] "Liquid reaction mixture" refers to the fluid phase (liquid, gas or supercritical) in which the reactants (ethylene, comonomer and hydrogen) are dissolved. Particles including catalyst and polymer are then suspended in the fluid reaction mixture.
[0016] The term "cable" includes all types of wires and cables used in wire and cable (W&C) applications, such as power cables and communication cables.
[0017] The multimodal ethylene copolymer composition of the present invention has a density of 920 to 949 kg / m 3 , where the flexural modulus is given by the following equation:
[0018] Flexural modulus [MPa] < 21.35 × density [kg / m 3 ]–19585 [1]
[0019] The multimodal ethylene copolymer composition according to the present invention has an optimal compromise between high flexibility and favourable mechanical properties.
[0020] The solid catalyst component for ethylene copolymerization is a solid Ziegler-Natta catalyst component for ethylene polymerization, which comprises magnesium, titanium, halogen and an internal organic compound. The internal organic compound (donor) is selected from a bis-(oxygen-containing ring) compound of formula (I) or an isomer or mixture thereof,
[0021]
[0022] Wherein, in formula (I), R1 to R5 are identical or different, and may be hydrogen, linear or branched C1 to C8-alkyl, or C3-C8-alkylene, or two or more of R1 to R5 may form a ring, and the two oxygen-containing rings are each saturated or partially unsaturated or unsaturated. "Isomers and mixtures" refers to all possible stereoisomers and mixtures derived from the structure of formula (I), depending on the substituents R1 to R5.
[0023] The catalyst used in the present invention comprises a component supported on solid MgCl2, which is prepared by a method comprising the following steps:
[0024] a) providing solid support particles of MgCl2*mROH adduct;
[0025] b) pretreating the solid support particles in step a) with a Group 13 metal compound;
[0026] c) treating the solid support particles pretreated in step b) with a Group 4 to 6 transition metal compound;
[0027] d) Reduction of solid catalyst component
[0028] Wherein, before the treatment of the solid carrier particles in step c), the solid carrier particles are contacted with an internal organic compound of formula (I) or its isomers or mixtures, and in formula (I) or its isomers or mixtures, R1 to R5 are the same or different, and can be hydrogen, linear or branched C1 to C8-alkyl, or C3-C8-alkylene, or two or more of R1 to R5 can form a ring, and the two oxygen-containing rings are each saturated or partially unsaturated or unsaturated, and R in the adduct MgCl2*mROH is a linear or branched alkyl having 1 to 12 carbon atoms, and m is 0 to 6.
[0029] Accordingly, the internal organic compound of formula (I) is contacted with the solid support particles before the solid support particles are treated with the Group 4 to 6 transition metal compound. Thus, the internal organic compound is contacted with the solid support particles before step b), i.e. before pre-treating the solid support particles with the Group 13 metal compound, or simultaneously with the pre-treatment step, or after step b), but before treating the solid support particles with the Group 4 to 6 transition metal compound.
[0030] According to the present invention, the above catalyst is used as disclosed above in the process for producing linear low density polyethylene in a multi-stage process.
[0031] The catalyst will be described in more detail below. In this article, the term Ziegler Natta (ZN) catalyst component is intended to cover a catalyst component comprising a transition metal compound from Groups 4 to 6 of the Periodic Table of the Elements (IUPAC, Nomenclature of Inorganic Chemistry, 1989), a Group 13 metal compound, and an internal organic compound supported on a MgCl2-based support.
[0032] Magnesium dihalide is used as the starting material for the production of the carrier. The solid carrier is a carrier in which ethanol is complexed with magnesium dihalide, preferably MgCl2. MgCl2 is mixed with an alcohol (ROH) and a solid carrier MgCl2*mROH is formed according to a well-known method. For example, a spray drying method or a spray crystallization method can be used to prepare the magnesium halide. Spherical or granular MgCl2*mROH carrier materials of different sizes (5-100 μm) are suitable for the present invention. The alcohol for producing the MgCl2*mROH carrier material is an alcohol ROH, wherein R is a straight or branched alkyl containing 1 to 12 carbon atoms, preferably 1 to 8 carbon atoms, more preferably 1 to 4 carbon atoms. Ethanol is generally used. In MgCl2*mROH, m is 0 to 6, preferably 1 to 4, more preferably 2.7 to 3.3.
[0033] MgCl2*mROH is available from commercial sources or can be prepared by methods described in the prior art. The preparation methods of MgCl2*mROH supports are described in a number of patents, such as EP-A-376936, EP-A-424049, EP-A-655073 and EP-A-614467.
[0034] The Group 13 metal compound used in step b) is preferably an aluminum compound.
[0035] Particularly preferred aluminum compounds are those of the formula Al(alkyl) x X 3-x wherein each alkyl is independently an alkyl of 1 to 12 carbon atoms, preferably 1 to 8 carbon atoms, more preferably 1 to 6 carbon atoms, X is a halogen, preferably chlorine, and 1 < x < 3. The alkyl can be straight-chain, branched-chain or cyclic, or a mixture of these groups.
[0036] Preferred aluminum compounds are dialkylaluminum chlorides or trialkylaluminum compounds, such as dimethylaluminum chloride, diethylaluminum chloride, diisobutylaluminum chloride, and triethylaluminum or mixtures thereof. Most preferred aluminum compounds are trialkylaluminum compounds, especially triethylaluminum compounds.
[0037] The Group 4 to 6 transition metal compounds are preferably Group 4 transition metal compounds or vanadium compounds, more preferably titanium compounds. Particularly preferred titanium compounds are halogen-containing titanium compounds of the formula X y Ti(OR 8 ) 4-y wherein R 8 is a C 1-20 alkyl, preferably a C 2-10 alkyl and more preferably a C 2-8 alkyl, X is a halogen, preferably chlorine, and y is 1, 2, 3 or 4, preferably 3 or 4, and more preferably 4.
[0038] Suitable titanium compounds include trialkoxy titanium monochloride, dialkoxy titanium dichloride, alkoxy titanium trichloride and titanium tetrachloride. Titanium tetrachloride is preferably used.
[0039] The internal organic compound is selected from bicyclic ether compounds of the formula (I) or isomers or mixtures thereof:
[0040]
[0041] wherein, in formula (I), R1 to R5 are the same or different and can be hydrogen, straight-chain or branched-chain C1 to C8-alkyl, or C3-C8-alkylene, or two or more of R1 to R5 can form a ring, and each of the two oxygen-containing rings is saturated or partially unsaturated or unsaturated.
[0042] Preferred examples of straight-chain or branched C1 to C8-alkyl are methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, pentyl and hexyl.
[0043] Preferred examples of C3-C8-alkylene are pentylene and butylene.
[0044] The two R1s are preferably the same and are both straight-chain C1 to C4-alkyl, more preferably methyl or ethyl, most preferably both R1s are methyl; or the two R1s form a ring with the carbon atom to which they are attached, preferably a ring having 3 to 7 carbon atoms, more preferably a cyclopentyl ring or a cyclohexyl ring.
[0045] R2 to R5 are identical or different and are preferably all H or C1 to C2 alkyl, or two or more of the residues R2 to R5 may form a ring. If one or more rings are formed by the residues R2 to R5, these rings are more preferably formed by R3 and R4 and / or R4 and R5.
[0046] Preferably, the R2 to R5 residues do not form a ring, and more preferably at most two of the R2 to R5 residues are methyl, and the others are hydrogen. Most preferably, R2 to R5 are hydrogen.
[0047] The two oxygen-containing rings may both be saturated or partially unsaturated or unsaturated. Each partially unsaturated or unsaturated oxygen-containing ring may have one or two double bonds. More preferably, both oxygen-containing rings are saturated.
[0048] In the most preferred embodiment, 2,2-bis(2-tetrahydrofuryl)propane (DTHFP) and its isomers are used together. DTHFP is usually a 1:1 mol / mol mixture of diastereoisomers of D,L-(rac)-DTHFP and meso-DTHFP.
[0049] When preparing the supported catalyst component used in the present invention, it is particularly preferred that the above internal organic compound is added to the catalyst mixture before, during or after pre-treating MgCl2*mROH with a Group 13 metal compound, but before treating MgCl2*mROH with a Group 4 to 6 transition metal compound.
[0050] Therefore, according to the present invention, the solid catalyst component can be prepared by a method comprising the steps of:
[0051] i) providing a solid MgCl2*mROH support, wherein m is 1 to 4 and R is a linear or branched alkyl group containing 1 to 8 carbon atoms;
[0052] ii) pretreating the solid support particles in step i) with an aluminum compound,
[0053] iii) adding the internal organic compound represented by formula (I) to the solid support pretreated in step ii),
[0054] iii') adding an internal organic compound of formula (I) to the solid support simultaneously with step ii),
[0055] iv) treating the solid support particles pretreated in step iii) or iii') with TiCl4, and
[0056] v) recovering the solid catalyst component.
[0057] According to the present invention, the solid catalyst component can also be prepared by a method comprising the steps of:
[0058] i) providing a solid MgCl2*mROH support, wherein m is 1 to 4 and R is a linear or branched alkyl group containing 1 to 8 carbon atoms;
[0059] ii-1) adding an internal organic compound represented by formula (I) to the solid support in step i),
[0060] iii-1) pretreating the solid support particles in step ii-1) with an aluminum compound,
[0061] iv-1) treating the solid support particles pretreated in step iii-1) with TiCl4, and
[0062] v-1) Recovering the solid catalyst component.
[0063] According to any of the above methods, the aluminum compound may be added to the solid support before or after the addition of the internal organic compound, or simultaneously with the internal organic compound.
[0064] In the above embodiment, most preferably, m=2.7 to 3.3, ROH is ethanol, the aluminum compound is a trialkylaluminum compound, such as triethylaluminum, and the internal organic compound is 2,2-bis(2-tetrahydrofuranyl)propane, or 2,2-bis(2-furanyl)propane, in particular 2,2-bis(2-tetrahydrofuranyl)propane or an isomer or mixture thereof.
[0065] According to the catalyst preparation method of the present invention, the pretreatment with a Group 13 metal compound, preferably an aluminum compound, can be completed by adding a solution of an aluminum compound dissolved in an inert organic solvent, preferably an inert aliphatic hydrocarbon solvent such as heptane. The method of the present invention allows the use of concentrated aluminum compound solutions. In the case of using triethylaluminum (TEA), a 15-100% by weight TEA solution dissolved in an inert hydrocarbon, preferably a 25-100% by weight TEA solution dissolved in an inert aliphatic hydrocarbon solvent such as heptane, can be used. It has been found that by using these more concentrated solutions, the morphology is still favorable and the amount of waste generated is reduced.
[0066] The final solid catalyst component generally has a Mg / Ti mol / mol ratio of 1 to 10, preferably 2 to 8, particularly preferably 3 to 7, an Al / Ti mol / mol ratio of 0.01 to 1, preferably 0.1 to 0.5 and a Cl / Ti mol / mol ratio of 5 to 20, preferably 10 to 17.
[0067] The particles of the solid catalyst component of the present invention may be uniform in particle size without fines or agglomerates.
[0068] Above-mentioned supported catalyst component allows to produce the polymer with the molecular weight of increase.The increase of molecular weight is not at the expense of the productivity of catalyst.With using similar type catalyst component but using different internal organic compounds, and / or by using TiCl during or after the treatment step to add the internal organic compound preparation, or using the organic compound as the situation of external additive to compare, productivity maintains an acceptable high level or even is improved.Therefore, the performance of the catalyst prepared according to the inventive method makes it possible to widen the preparation window of polyethylene, makes it possible to polymerize with higher amount and lower amount of hydrogen while keeping good productivity.
[0069] In addition to the solid catalyst component as defined above, the catalyst used in the method of the present invention may also include a cocatalyst, which is also referred to as an activator. Cocatalysts are organometallic compounds of Group 13 metals, typically aluminum compounds. These compounds include alkylaluminum halides, preferably alkylaluminum chlorides, such as ethylaluminum dichloride, diethylaluminum chloride, ethylaluminum sesquichloride, dimethylaluminum chloride, etc. They also include trialkylaluminum compounds, such as trimethylaluminum, triethylaluminum, triisobutylaluminum, trihexylaluminum and tri-n-octylaluminum. Other alkylaluminum compounds, such as isoprenylaluminum, may also be used. Particularly preferred cocatalysts are trialkylaluminums, wherein triethylaluminum, trimethylaluminum and triisobutylaluminum are particularly used.
[0070] The catalyst of the present invention may also contain external additives, such as external donors. The external additives that can be used include ether compounds, typically tetrahydrofuran, external donors of the siloxane or silane type and / or alkyl halides known in the prior art. The final solid catalyst component obtained according to any of the above methods, i.e. the ZN solid catalyst component, is mixed with an activator.
[0071] Suitable activators are optionally of the formula (C1-C4 alkyl) p -Al-X 3-p The haloalkylaluminum cocatalyst of the present invention is a halogenated alkylaluminum cocatalyst wherein X is chlorine, bromine, iodine or fluorine and p is 1, 2 or 3. The C1-C4 alkyl group may be straight chain or branched or cyclic, or a mixture of these groups. X is preferably chlorine or bromine, and X is most preferably chlorine.
[0072] Suitable activators are, for example, trimethylaluminum (TMA), triethylaluminum (TEA), dimethylaluminum chloride (DMAC), diethylaluminum chloride (DEAC), diisobutylaluminum chloride (DIBAC), ethylaluminum dichloride (EADC), methylaluminum dichloride (MADC). The preferred activator for the process of the invention is triethylaluminum.
[0073] The amount of activator used depends on the specific catalyst and activator. Generally, the amount of triethylaluminum used should be such that the molar ratio of aluminum to transition metal is Al / Ti from 1 to 1000, preferably from 3 to 100, especially from about 5 to about 30 mol / mol.
[0074] Aggregation methods
[0075] Polymerization process comprises the first polymerization stage and the second polymerization stage. In addition, the method may comprise other polymerization stages, for example, for the preparation of one or more other polymer components or for the stage of prepolymerization catalyst. Other polymerization stages can be carried out before or after any one in the first polymerization stage and the second polymerization stage. In addition, any one in the first polymerization stage and the second polymerization stage all can be divided into two or more steps, wherein the first homopolymer of ethene or multipolymer or the second multipolymer of ethene produce in two or more steps, wherein each such step is carried out under the condition of preparing the corresponding first homopolymer or multipolymer or the second multipolymer.
[0076] Prepolymerization
[0077] The polymerization step may be preceded by a prepolymerization step. The purpose of the prepolymerization is to polymerize a small amount of polymer onto the catalyst at low temperature and / or low monomer concentration. By prepolymerization, the performance of the catalyst in the slurry can be improved and / or the properties of the final polymer can be changed. The prepolymerization step is carried out in slurry.
[0078] Therefore, the prepolymerization step can be carried out in a loop reactor. The prepolymerization is then preferably carried out in an inert diluent, which is typically a hydrocarbon diluent, such as methane, ethane, propane, n-butane, isobutane, pentane, hexane, heptane, octane, etc., or a mixture thereof. Preferably, the diluent is a low boiling hydrocarbon having 1 to 4 carbon atoms or a mixture of these hydrocarbons.
[0079] The temperature in the prepolymerization step is usually 0 to 90°C, preferably 20 to 80°C, more preferably 55 to 75°C.
[0080] The pressure is not critical and is generally from 1 to 150 bar, preferably from 40 to 80 bar.
[0081] The amount of monomer is generally about 0.1-1000 grams of monomers per 1 gram of solid catalyst component in the prepolymerization step. As known to those skilled in the art, the catalyst particles recovered from the continuous prepolymerization reactor do not all contain the same amount of prepolymer. On the contrary, each particle has its own characteristic amount, which depends on the residence time of the particle in the prepolymerization reactor. Because some particles retain a relatively long time in the reactor and some particles retain a relatively short time, the amount of prepolymer on different particles is also different, and some individual particles may contain prepolymers that exceed the amount of the above-mentioned restriction. However, the average amount of prepolymer on the catalyst is usually within the scope of the above-mentioned regulation.
[0082] As is known in the art, the molecular weight of the prepolymer can be controlled by hydrogen.In addition, antistatic additives can be used to prevent the particles from sticking to each other or to the reactor walls, as disclosed in WO-A-96 / 19503 and WO-A-96 / 32420.
[0083] When a prepolymerization step is present, the catalyst components are preferably all introduced into the prepolymerization step (separately or together). However, in case the solid catalyst component and the cocatalyst can be fed separately, it is possible to introduce only a portion of the cocatalyst into the prepolymerization stage and the remainder into the subsequent polymerization stage. Also in this case, it is necessary to introduce so much cocatalyst into the prepolymerization stage that a sufficient polymerization reaction is obtained therein. Typically, the amount of hydrogen and comonomer is adjusted so that the presence of the prepolymer has no effect on the properties of the final multimodal polymer. In particular, it is preferred that the melt flow rate of the prepolymer is greater than the melt flow rate of the final polymer, but less than the melt flow rate of the polymer prepared in the first polymerization stage. It is further preferred that the density of the prepolymer is greater than the density of the final polymer. Preferably, the density is about the same as or greater than the density of the polymer produced in the first polymerization stage. Furthermore, typically the amount of prepolymer does not exceed about 5% by weight of the multimodal polymer comprising the prepolymer.
[0084] First polymerization stage
[0085] In the first polymerization stage, a first homopolymer or copolymer of ethylene is produced. This is done by introducing a polymerization catalyst into the first polymerization stage together with ethylene, hydrogen and optionally an alpha-olefin comonomer, optionally via a prepolymerization stage or a preceding polymerization stage as described above.
[0086] Hydrogen is introduced into the first polymerization stage to control the MFR2 of the first homopolymer or copolymer of ethylene. The amount of hydrogen is such that the molar ratio of hydrogen to ethylene in the fluid reaction mixture is in the range of 200 to 50000 mol / kmol (or mol / 1000 mol), preferably in the range of 200 to 1000 mol / kmol. If the first polymerization stage is carried out as a slurry polymerization stage, preferably in a loop reactor, the molar ratio of hydrogen to ethylene in the fluid reaction mixture is preferably 200-1000 mol / kmol, preferably 300-800 mol / kmol.
[0087] The first homopolymer or copolymer of ethylene can be a homopolymer. Therefore, there is no first alpha-olefin in the first polymerization stage. Hydrogen exists in an amount as described above. In addition, the first homopolymer or copolymer of ethylene can be a copolymer of ethylene and the first alpha-olefin. In this case, the molar ratio of the first alpha-olefin to ethylene in the fluid reaction mixture is 100-1000mol / kmol, preferably 200-800mol / kmol. The first alpha-olefin is preferably selected from 1-butene, 1-hexene and 4-methyl-1-pentene, more preferably selected from 1-butene and 1-hexene. Also in this embodiment, hydrogen exists in an amount as described above.
[0088] When produced under the conditions defined above, the melt flow rate MFR2 of the first homopolymer or copolymer of ethylene is typically 100-1000 g / 10 min, preferably 150-750 g / 10 min, more preferably 200-600 g / 10 min. In addition, the density of the first copolymer is typically 930 to 980 kg / m 3 , preferably 940 to 978 kg / m 3 , most preferably 945 to 976 kg / m 3 .
[0089] When the first homopolymer or copolymer of ethylene is a copolymer of ethylene, its density is preferably from 930 to 955 kg / m 3 , more preferably 940 to 953 kg / m 3 , most preferably 945 to 953 kg / m 3 .
[0090] As known to the skilled person, the MFR2 and density ranges apply to the first homopolymer or copolymer of ethylene. If the first polymerization stage is preceded by another polymerization stage producing a larger amount of polymer, the above MFR2 and density ranges for the first homopolymer or copolymer do not necessarily apply to the polymer mixture comprising the polymers produced in the preceding polymerization stage and the first polymerization stage.
[0091] The first polymerization stage is preferably carried out as a slurry polymerization. Slurry polymerization is usually carried out in an inert diluent, which is usually a hydrocarbon diluent, such as methane, ethane, propane, n-butane, isobutane, pentane, hexane, heptane, octane, etc., or a mixture thereof. Preferably, the diluent is a low boiling hydrocarbon having 1 to 4 carbon atoms or a mixture of these hydrocarbons. A particularly preferred diluent is propane, possibly containing small amounts of methane, ethane and / or butane.
[0092] The ethylene content of the fluid reaction mixture can be 1 to about 50 mol%, preferably about 2 to about 20 mol%, and especially about 2 to about 10 mol%. The benefit of having a high ethylene concentration is that the productivity of the catalyst is increased, but the disadvantage is that more ethylene needs to be recycled than when the concentration is lower.
[0093] The temperature of the first polymerization stage is generally from 60 to 100° C., preferably from 70 to 95° C. Excessively high temperatures should be avoided to prevent partial dissolution of the polymer into the diluent and reactor fouling. The pressure is from 1 to 150 bar, preferably from 40 to 80 bar.
[0094] Slurry polymerization can be carried out in any known reactor for slurry polymerization. Such reactors include continuous stirred tank reactors and loop reactors. Particularly preferably, polymerization is carried out in a loop reactor. In such a reactor, the slurry is circulated along a closed pipeline at high speed by using a circulating pump. Loop reactors are generally known in the art, for example, examples given in US-A-4582816, US-A-15 3405109, US-A-3324093, EP-A-479186 and US-A-5391654. Therefore, in one or more loop reactors, the first polymerization stage is more preferably carried out in a loop reactor as a slurry polymerization.
[0095] The slurry can be taken out from the reactor continuously or intermittently. A preferred mode for intermittent removal is to use settling legs, wherein the slurry is concentrated before a batch of concentrated slurry is taken out from the reactor. Among them, the use of settling legs is disclosed in US-A-3374211, US-A-3242150 and EP-A-1310295. Among them, EP-A-891990, EP-A-1415999, EP-A-1591460 and WO-A-2007 / 025640 disclose continuous removal. As disclosed in EP-A-20 1310295 and EP-A-1591460, it is advantageous to combine continuous removal with a suitable concentration method. Preferably, the slurry is taken out continuously from the first polymerization stage.
[0096] If the first homopolymer or copolymer of ethylene is the first copolymer of ethylene, the first α-olefin comonomer is introduced into the first polymerization stage to control the density of the first copolymer of ethylene. The amount of comonomer required to achieve the desired density depends on the comonomer type, the catalyst used and the polymerization conditions, especially the H2 / C2 ratio.
[0097] As disclosed in WO-A-1996035936, WO-A-1994027134 and EP-A-460594, as known in the art, the content of hydrogen, ethylene and the first alpha-olefin comonomer can be measured by taking a sample stream from the reactor or by a sample stream taken from the reactor. Preferably, such a sample stream is taken from a decompression stage or flash distillation between the first polymerization stage and the second polymerization stage.
[0098] The average residence time of the first polymerization stage is generally 20 to 120 minutes, preferably 20 to 70 minutes. As is well known in the art, the average residence time τ can be calculated by the following formula:
[0099] τ=Vr / Qo
[0100] Where Vr is the volume of the reaction space (in the case of a loop reactor, the volume of the reactor; in the case of a fluidized bed reactor, the volume of the fluidized bed), and Qo is the volumetric flow rate of the product stream (including polymer product and fluid reaction mixture).
[0101] It is possible and sometimes preferred to carry out the first polymerization stage in more than one step, for example in two steps. When the first polymerization stage is carried out in more than one step, the first homopolymer or copolymer of ethylene is a mixture of two or more homopolymers or copolymers of ethylene. In this case, all of these steps should be carried out under the conditions as described above. In addition, the amount of the first homopolymer or copolymer of ethylene is the sum of the amounts of polymers produced in all of these steps.
[0102] Furthermore, as mentioned above, the first polymerization stage may be preceded by one or more further polymerization stages, in which a polymer different from the first homopolymer or copolymer of ethylene is produced.
[0103] Second polymerization stage
[0104] In the second polymerization stage, a polymer mixture comprising a first homopolymer or copolymer of ethylene and a second copolymer of ethylene is formed. This is accomplished by introducing particles of the first homopolymer or copolymer of ethylene (containing an active catalyst dispersed therein) into the second polymerization stage together with additional ethylene and a second alpha-olefin comonomer. Hydrogen may be introduced to control molecular weight. This results in the formation of a second copolymer of ethylene on particles comprising the first homopolymer or copolymer of ethylene.
[0105] The MFR5 of the ethylene copolymer may be from 0.3 to 12.0 g / 10 min. 21 Preferably it is 20-180 g / 10 min, more preferably 25-100 g / 10 min. In addition, its flow rate is FRR 21 / 5 It is preferably 10-50, more preferably 15-40.
[0106] The second α-olefin comonomer is selected from α-olefins containing 4 to 10 carbon atoms. If the first α-olefin comonomer is present, the second α-olefin comonomer may be the same or different from the first α-olefin comonomer. In a preferred embodiment of the present invention, the first α-olefin comonomer and the second α-olefin comonomer are the same, such as 1-butene or 1-hexene, and 1-butene is particularly preferred. In another preferred embodiment of the present invention, the first α-olefin comonomer is different from the second α-olefin comonomer. Then, the first α-olefin comonomer may be 1-butene, and the second α-olefin comonomer may be 1-hexene or 1-octene, more preferably 1-hexene. According to another embodiment, there is no first α-olefin comonomer, and the second α-olefin comonomer is 1-butene, 1-hexene or 1-octene, or a mixture thereof, preferably 1-hexene.
[0107] The density of the polymer mixture is 910 to 940 kg / m 3 , more preferably 915 to 930 kg / m 3 , most preferably 918 to 927 kg / m 3 .
[0108] The MFR of the second copolymer of ethylene cannot be measured 21 , because the second copolymer cannot be separated from the polymer mixture.
[0109] The hydrogen feed is regulated to obtain the required melt flow rate (or molecular weight) of the polymer mixture. Preferably, the hydrogen feed is controlled to maintain a constant ratio of hydrogen to ethylene in the fluid reaction mixture. The actual ratio depends on the type of catalyst and polymerization. In a fluidized bed reactor, by the ratio in the gas phase being maintained at 10 to 200mol / kmol, preferably 50 to 200mol / kmol, for example 100 to 175mol / kmol, in gas phase polymerization, desired polymer properties are obtained.
[0110] The second alpha-olefin comonomer is usually introduced to maintain a constant comonomer to ethylene ratio in the fluid reaction mixture. The comonomer to ethylene ratio required to produce a polymer having a desired density depends inter alia on the type of comonomer and the type of catalyst. Using 1-hexene as a comonomer, the desired polymer properties are obtained in a gas phase polymerization in a fluidized bed reactor by a 1-hexene to ethylene molar ratio in the gas phase of 50 to 400 mol / kmol, preferably 100 to 250 mol / kmol, and particularly 120 to 220 mol / kmol.
[0111] Preferably, the second polymerization stage is carried out as a fluidized bed gas phase polymerization. In a fluidized bed gas phase reactor, olefins are polymerized in the presence of a polymerization catalyst in an upwardly moving gas stream. The reactor typically contains a fluidized bed containing growing polymer particles containing an active catalyst located above a fluidizing grid.
[0112] The polymer bed is fluidized with the aid of a fluidizing gas comprising an olefin monomer, an optional comonomer, an optional chain growth controller or chain transfer agent, such as hydrogen and an optional inert gas. The fluidizing gas is introduced into an inlet chamber at the bottom of the reactor. In order to ensure that the gas flow is evenly distributed over the cross-sectional surface area of the inlet chamber, the inlet pipe may be equipped with a diverter element known in the art, such as US-A-4933149 and EP-A-684871. One or more of the above components may be added continuously to the fluidizing gas to compensate for losses caused by reaction or product removal.
[0113] From the inlet chamber, the gas flow passes upward through a fluidizing grid into the fluidized bed. The purpose of the fluidizing grid is to evenly distribute the gas flow across the cross-sectional area of the bed. Sometimes, as disclosed in WO-A-2005 / 087361, the fluidizing grid can be arranged to establish a gas flow to sweep along the reactor wall. Other types of fluidizing grids are disclosed in US-A-4578879, EP 600414 and EP-A-721798. Geldart and Bayens provide a review: Design of gas fluidized bed distributors, Powder Technology, Volume 42, 1985.
[0114] The fluidizing gas is passed through the fluidized bed. The superficial velocity of the fluidizing gas must be greater than the minimum fluidizing velocity of the particles contained in the fluidized bed, otherwise fluidization will not occur. On the other hand, the velocity of the gas should be lower than the starting velocity of the pneumatic transport, otherwise the entire bed will be entrained by the fluidizing gas. When the particle characteristics are known by conventional engineering practice, the minimum fluidizing velocity and the starting velocity of the pneumatic transport can be calculated. A review is provided by Geldart: Gas Fluidization Technology, J. Wiley & Sons, 1986.
[0115] When the fluidizing gas contacts the bed containing the active catalyst, the reactive components of the gas, such as monomers, comonomers and chain transfer agents, react in the presence of the catalyst to form polymer product. At the same time, the gas is heated by the heat of reaction.
[0116] Unreacted fluidizing gas is removed from the reactor top and cooled in a heat exchanger to remove the heat of reaction. The gas is cooled to a temperature below the bed temperature to prevent the bed from heating due to the reaction. The gas can be cooled to a temperature at which a portion of it condenses. When the droplets enter the reaction zone, they evaporate. Then the heat of evaporation helps to remove the heat of reaction. This operation is referred to as concentrated mode, and its variants are disclosed in WO-A-2007 / 025640, US-A-4543399, EP-A-699213 and WO-A-94 / 25495. As disclosed in EP-A-696293, condensing agents can also be added to the circulating gas stream. Condensing agents are non-polymerizable components, such as n-pentane, isopentane, n-butane or isobutane, which are at least partially condensed in a cooler.
[0117] The gas is then compressed and recycled into the inlet chamber of the reactor. Before entering the reactor, fresh reactants are introduced into the fluidizing gas stream to compensate for losses caused by the reaction and product withdrawal. It is generally known to analyze the composition of the fluidizing gas and introduce gas components to keep the composition constant. The actual composition is determined by the desired properties of the product and the catalyst used in the polymerization.
[0118] The catalyst can be introduced into the reactor continuously or intermittently in various ways. Among others, WO-A-01 / 05845 and EP-A-499759 disclose these processes.
[0119] In case the gas phase reactor is part of a reactor cascade, the catalyst is usually dispersed within polymer particles from the preceding polymerisation stage.Polymer particles may be introduced into a gas phase reactor as disclosed in EP-A-1415999 and WO-A-00 / 26258.
[0120] The polymer product can be withdrawn from the gas phase reactor continuously or intermittently. Combinations of these methods can also be used. Among them, continuous withdrawal is disclosed in WO-A-00 / 29452. Among them, intermittent withdrawal is disclosed in US-A-4621952, EP-A-188125, EP-A-250169 and EP-A-579426.
[0121] The top of a gas phase reactor may include a so-called disengagement zone. In such a zone, the diameter of the reactor is increased to reduce the gas velocity and allow particles entrained from the bed with the fluidizing gas to settle back into the bed.
[0122] The bed level can be observed by different techniques known in the art. For example, the pressure difference between the bottom of the reactor and a certain height of the bed can be recorded over the entire length of the reactor, and the bed level can be calculated based on the pressure difference. Such a calculation produces a time-averaged level. Ultrasonic sensors or radioactive sensors can also be used. Using these methods, instantaneous levels can be obtained, which can then of course be averaged over time to obtain a time-averaged bed level.
[0123] In addition, if desired, an antistatic agent can be introduced into the gas phase reactor. Suitable antistatic agents and methods of using them are disclosed in US-A-5026795, US-A-4803251, US-A-4532311, US-A-4855370 and EP-A-560035. They are usually polar compounds, including water, ketones, aldehydes and alcohols.
[0124] The reactor may also include a mechanical agitator to further promote mixing within the fluidised bed. An example of a suitable agitator design is given in EP-A-707513.
[0125] Typically, the fluidized bed polymerization reactor is operated at a temperature of from 50 to 100° C., preferably from 65 to 90° C. The pressure is preferably from 10 to 40 bar, preferably from 15 to 30 bar.
[0126] The average residence time in the second polymerization stage is generally from 40 to 240 minutes, preferably from 60 to 180 minutes.
[0127] As stated above, the second polymerisation stage is preferably carried out in gas phase in one or more gas phase reactors, more preferably in a fluidised bed reactor.
[0128] The polymer mixture typically comprises 25 to 57% by weight of the first homopolymer or copolymer and 43 to 75% by weight of the second copolymer. Preferably, the polymer mixture comprises 35 to 57% by weight of the first homopolymer or copolymer of ethylene and 43 to 65% by weight of the second copolymer of ethylene. In addition to the first homopolymer or copolymer of ethylene and the second copolymer of ethylene, the polymer mixture may contain other polymers, but the content of the first homopolymer or copolymer of ethylene and the second copolymer of ethylene must be within the above limits.
[0129] Most preferably, the polymerization process of the present invention is carried out in a cascade sequence comprising at least one loop reactor followed by at least one gas phase reactor.
[0130] Extrusion
[0131] When the polymer mixture has been taken out of the polymerization reactor, it is subjected to process steps for removing residual hydrocarbons from the polymer. These methods are well known in the art and may include a decompression step, an air purging step, a stripping step, an extraction step, etc. Moreover, a combination of different steps is possible.
[0132] After removal of residual hydrocarbons, the polymer is preferably mixed with additives, as are well known in the art. Such additives include antioxidants, processing stabilizers, neutralizers, lubricants, nucleating agents, pigments, and the like.
[0133] According to the present invention, 0.1 to 5 wt% of carbon black can be added to the ethylene copolymer composition during the extrusion process, preferably 2 to 3 wt%. The carbon black is preferably N220 type carbon black.
[0134] The polymer particles are mixed with additives and extruded into pellets as known in the art.Preferably, a counter-rotating twin-screw extruder is used for the extrusion step.
[0135] Polymer composition
[0136] Ethylene copolymers can be prepared according to the process described above and according to all disclosed embodiments. The copolymers according to the invention are those having a molecular weight of 920 to 949 kg / m 3 A multimodal ethylene copolymer composition having a density and a flexural modulus of 1000 Å, wherein the flexural modulus is as expressed by the following equation:
[0137] Flexural modulus [MPa] < 21.35 × density [kg / m 3 ]–19585 [1]
[0138] The ethylene copolymer is preferably LLDPE.The ethylene copolymer is preferably produced in at least two polymerisation stages, preferably in a continuously operated process.
[0139] The multimodal ethylene copolymer composition may comprise at least one C4-C 10 The ethylene copolymer preferably comprises at least 1-butene and 1-hexene comonomers.
[0140] The multimodal ethylene copolymer composition preferably comprises at least 80 wt%, more preferably at least 90 wt% of the ethylene copolymer.
[0141] The ethylene copolymers of the present invention can be prepared using a Ziegler-Natta catalyst, preferably using an internal organic compound having the general formula (1):
[0142]
[0143] Wherein, in formula (I), R1 to R5 are the same or different, and can be hydrogen, linear or branched C1 to C8-alkyl, or C3-C8-alkylene, or two or more of R1 to R5 can form a ring, and the two oxygen-containing rings are each saturated or partially unsaturated or unsaturated.
[0144] The MFR2 of the multimodal ethylene copolymer composition may be from 0.1 to 4 g / 10min, preferably from 0.5 to 2 g / 10min, most preferably from 0.7 to 1.5 g / 10min.
[0145] The MFR5 of the multimodal ethylene copolymer composition may be from 0.3 to 12 g / 10 min, more preferably from 2 to 7 g / 10 min, most preferably from 2 to 5 g / 10 min.
[0146] MFR of the multimodal ethylene copolymer composition 21 It may be 20 to 180 g / 10 min, more preferably 40 to 120 g / 10 min, most preferably 60 to 100 g / 10 min.
[0147] FRR of multimodal ethylene copolymer compositions 21 / 5 It may be 10 to 50, more preferably 15 to 40.
[0148] The multimodal ethylene copolymer composition may have a Shore D(ls) of at least 50, more preferably at least 53. The higher the Shore D(ls), the more resistant the surface of the multimodal ethylene copolymer composition is to mechanical impact.
[0149] The multimodal ethylene copolymer composition according to the invention may have a flexural modulus of the following equation:
[0150] Flexural modulus [MPa] < 21.35 × density [kg / m3 ]–19610 [2]
[0151] The multimodal ethylene copolymer composition preferably has a density of 930 to 949 kg / m 3 , preferably 930 to 940 kg / m 3 One object of the present invention is to minimize density, thereby increasing flexibility, while maintaining Shore D(ls).
[0152] Carbon black may be added to the multimodal ethylene copolymer composition, preferably in an amount of 0.1-5 wt%, more preferably 0.5-3 wt%, most preferably 1-3 wt%. The carbon black is preferably UV carbon black, such as N220 type carbon black. The carbon black may be added during the extrusion process immediately after the polymerization reactor or in a separate step. The carbon black may also be added directly to the cable sheath extruder via a carbon black masterbatch. MFR2, MFR5, MFR 21 and FRR were almost unchanged by the addition of carbon black.
[0153] The multimodal ethylene copolymer composition of the present invention may further comprise conventional additives such as antioxidants, pigments, UV additives and processing aids, typically in amounts of 0.1 to 5 wt%.
[0154] The multimodal ethylene copolymer composition according to the present invention may be produced in at least two polymerisation stages.
[0155] The present invention also relates to a cable sheathing comprising the multimodal ethylene copolymer composition according to the above disclosure.
[0156] The present invention also relates to a power cable or a communication cable comprising a cable sheath comprising the multimodal ethylene copolymer composition; preferably to a power cable comprising an inner semiconductive layer followed by an insulating layer and then an outer semiconductive layer. The cable sheath preferably consists of the multimodal ethylene copolymer composition of the present invention. DETAILED DESCRIPTION
[0157] Test Method
[0158] Melt flow rate
[0159] The melt flow rate (MFR) is determined at 190°C according to ISO 1133. The load under which the measurement is made is given as a subscript. Thus, the MFR under a load of 2.16 kg is denoted as MFR2. Correspondingly, the melt flow rate MFR 21 It is measured at 190°C and 21.6 kg load, and MFR5 is measured at 5 kg load.
[0160] density
[0161] Polymer density was measured according to ISO 1183-1:2004 Method A by using compression molded specimens produced according to EN ISO 1872-2 (February 2007) and is expressed in kg / m 3 Given.
[0162] Reactor gas composition
[0163] As is well known in the art, the reactor gas composition in a slurry reactor may be measured from the flash gas after the reactor by using on-line gas chromatography, for example as disclosed in WO-A-1996035936.
[0164] As is well known in the art, the reactor gas composition in a gas phase reactor can be analyzed from the recycle gas by using on-line chromatography.
[0165] As is known in the art, the instrument is calibrated using a calibration gas mixture having a known composition close to the gas mixture present during the polymerization process.
[0166] Flexural test (modulus)
[0167] The flexural modulus reflects the flexibility of a material. The higher the flexural modulus, the less flexible the material is, i.e., it is more difficult for the material to deform under a given load.
[0168] The flexural tests were carried out according to the method of ISO 178 by using compression moulded test specimens produced according to EN ISO 1872-2.
[0169] A rectangular sample with dimensions of 80×4×10 mm is placed between two supports. The sample is then pressed at a speed of 2 mm / min towards the edge of a load placed in the middle of the sample. In this case, only the flexural modulus is studied, so the flexural strain is determined between 0.05% and 0.25%, from which the flexural modulus is calculated.
[0170] Tensile test (strength)
[0171] The tensile test was measured according to ISO 527.
[0172] The crosshead speed for testing tensile strength and elongation was 50 mm / min.
[0173] Test specimens produced as described in EN ISO 1872-2, specimen type: 5A to ISO 527-2 were used.
[0174] Shaw D
[0175] Shore D (1s) is determined on molded specimens with a thickness of 4 mm according to IS0868. Shore hardness is determined 1 second after the pressure foot has been in firm contact with the test specimen. Samples are molded according to EN IS01872-2.
[0176] Quantification of microstructure by nuclear magnetic resonance (NMR) spectroscopy
[0177] Quantitative nuclear magnetic resonance (NMR) spectroscopy is used to quantify the comonomer content of the polymer. 1 H and 13 Quantitative measurements of the melt state were recorded using a Bruker Advance III 500 NMR spectrometer operating at 500.13 MHz and 125.76 MHz, respectively. 13 C{ 1 H} NMR spectrum. At 150°C, nitrogen was used for all atmospheres. 13 All spectra were recorded using a C-optimal 7 mm magic angle spinning (MAS) probe. Approximately 200 mg of material was packed into a 7 mm outer diameter zirconium oxide MAS rotor and spun at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification {klimke06, parkinson07, castignolles09}. Standard single pulse excitation was employed, which utilized NOE {pollard04, klimke06} and RS-HEPT decoupling scheme {fillip05, griffin07} at a short recirculation delay. A total of 1024 (1k) transients were acquired for each spectrum.
[0178] For quantitative 13 C{ 1 H} NMR spectra were processed, integrated and the relevant quantitative properties determined from the integration. All chemical shifts were internally referenced to the bulk methylene signal (δ+) at 30.00 ppm {randall89}.
[0179] The ethylene content is quantified using the integral of the number of methylene (δ+) sites over the number of reporter sites per monomer at 30.00 ppm:
[0180] E=I δ+ / 2
[0181] Correction for the presence of isolated comonomer units is based on the number of isolated comonomer units present:
[0182] E total = E + (3 × B + 2 × H) / 2
[0183] wherein B and H are defined as their respective comonomers. Correction for incorporated continuous and non-continuous comonomers, when present, is performed in a similar manner.
[0184] Characteristic signals corresponding to the incorporation of 1-butene were observed, and the comonomer fraction was calculated as the fraction of 1-butene in the polymer relative to all monomers in the polymer:
[0185] fB total = B total / (E total + B total + H total)
[0186] The amount of isolated 1-butene incorporated into the EEBEE sequence was quantified using the integral of the *B2 site over the number of reported sites per comonomer at 38.3 ppm:
[0187] B=I *B2
[0188] The amount of continuously incorporated 1-butene in the EEBBEE sequence was quantified using the integral of the ααB2B2 sites over the number of reporter sites per comonomer at 39.4 ppm:
[0189] BB=2×I ααB2B2
[0190] The amount of non-continuously incorporated 1-butene in the EEBEBEE sequence was quantified using the integral of the ββB2B2 sites over the number of reporter sites per comonomer at 24.7 ppm:
[0191] BEB=2×I ββB2B2
[0192] Due to the overlap of the *B2 and *βB2B2 sites of isolated (EEBEE) 1-butene and discontinuously bound (EEBEBEE) 1-butene, the total amount of bound isolated 1-butene was corrected based on the amount of discontinuous 1-butene present:
[0193] B=I *B2 -2×I ββB2B2
[0194] The total 1-butene content was calculated based on the sum of isolated, continuous and non-continuously combined 1-butene:
[0195] Total B=B+BB+BEB
[0196] The total mole fraction of 1-butene in the polymer is then calculated:
[0197] fB=B total / (E total+B total+H total)
[0198] A characteristic signal corresponding to the incorporation of 1-hexene was observed, and the comonomer fraction was calculated as the fraction of 1-hexene in the polymer relative to all monomers in the polymer:
[0199] fHtotal=Htotal / (Etotal+Btotal+Htotal)
[0200] The amount of isolated 1-hexene incorporated in the EEHEE sequence was quantified using the integral of the *B4 site at 39.9 ppm over the number of reporter sites per comonomer:
[0201] H=I *B4
[0202] The amount of continuously incorporated 1-hexene in the EEHHEE sequence was quantified using the integral of the ααB4B4 site over the number of reporter sites per comonomer at 40.5 ppm:
[0203] HH=2×I ααB4B4
[0204] The amount of non-continuously incorporated 1-hexene in the EEHEHEE sequence was quantified using the integral of the ββB4B4 sites over the number of reporter sites per comonomer at 24.7 ppm:
[0205] HEH=2×I ββB4B4
[0206] The total mole fraction of 1-hexene in the polymer is then calculated:
[0207] fH=H total / (E total+B total+H total)
[0208] The mole percent of comonomer incorporated is calculated from the mole fraction:
[0209] B [mol%] = 100 × fB
[0210] H[mol%]=100×fH
[0211] The weight percent of comonomer incorporated is calculated from the mole fraction:
[0212] B [weight %] = 100 × (fB × 56.11) / ((fB × 56.11) + (fH × 84.16) + ((1-(fB + fH)) × 28.05))
[0213] H [weight %] = 100 × (fH × 84.16) / ((fB × 56.11) + (fH × 84.16) + ((1-(fB + fH)) × 28.05))
[0214] References
[0215] klimke06
[0216] Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2006; 207:382.
[0217] parkinson07
[0218] Parkinson, M., Klimke, K., Spiess, H.W., Wilhelm, M., Macromol. Chem. Phys. 2007; 208: 2128.
[0219] pollard04
[0220] Pollard, M., Klimke, K., Graf, R., Spiess, H.W., Wilhelm, M., Sperber, O., Piel, C., Kaminsky, W., Macromolecules 2004; 37: 813.
[0221] filip05
[0222] Filip, X., Tripon, C., Filip, C., J. Mag. Resn. 2005, 176, 239
[0223] griffin07
[0224] Griffin, J.M., Tripon, C., Samoson, A., Filip, C., and Brown, S.P., Mag. Res. in Chem. 2007 45, S1, S198
[0225] castignolles09
[0226] Castignolles, P., Graf, R., Parkinson, M., Wilhelm, M., Gaborieau, M., Polymer 50(2009)2373
[0227] busico01
[0228] Busico, V., Cipullo, R., Prog. Polym. Sci. 26(2001)443
[0229] busico97
[0230] Busico, V., Cipullo, R., Monaco, G., Vacatello, M., Segre, A.L., Macromoleucles 30(1997)6251
[0231] zhou07
[0232] Zhou,Z.,Kuemmerle,R.,Qiu,X.,Redwine,D.,Cong,R.,Taha,A.,Baugh,D.Winniford,B.,
[0233] J.Mag.Reson.187(2007)225
[0234] busico07
[0235] Busico,V.,Carbonniere,P.,Cipullo,R.,Pellecchia,R.,Severn,J.,Talarico,G.,Macromol.
[0236] Rapid Commun.2007,28,1128
[0237] resconi00
[0238] Resconi,L.,Cavallo,L.,Fait,A.,Pimontesi,F.,Chem.Rev.2000,100,1253
[0239] Material
[0240] Catalyst 1
[0241] Complex preparation
[0242] Toluene (87 kg) was added to a 100 liter reactor. Bomag A (45.5 kg, 20 wt% butyloctyl magnesium solution in heptane) supplied by Chemtura was then added to the reactor. 2-ethyl-1-hexanol (161 kg, 99.8 wt%) was then introduced into the reactor at a flow rate of 24-40 kg / h. The molar ratio of BOMAG-A to 2-ethyl-1-hexanol was 1:1.83.
[0243] Preparation of solid catalyst components
[0244] 10 275 kg silica (ES747JR of Crossfield, average particle size of 20 μm) activated in nitrogen at 600° C. was added to the catalyst preparation reactor. Then, 411 kg 20% EADC (2.0 mmol / g silica) diluted in 555 liters of pentane was added to the reactor within 1 hour at ambient temperature. The temperature was then raised to 35° C. while the treated silica was stirred for 1 hour. The silica was dried at 50° C. for 8.5 hours. Then 655 kg of the complex prepared as described above (2 mmol Mg / g silica) was added within 10 minutes at 23° C. 86 kg pentane was added to the reactor within 10 minutes at 22° C. The slurry was stirred at 50° C. for 8 hours. Finally, 52 kg TiCl4 was added within 0.5 hours at 45° C. The slurry was stirred at 40° C. for 5 hours. The catalyst was then dried by purging with nitrogen.
[0245] Catalyst 2
[0246] Preparation of pretreated support material
[0247] A 160 dm jacketed 3 The stainless steel reactor was pressurized to 2.0 bar with N2 and decompressed to 0.2 bar until the O2 level was less than 3 ppm. Heptane (20.5 kg) and 2,2-bis(tetrahydrofuryl)propane (0.512 kg; 79 mol; DTHFP) were then added to the vessel. The resulting mixture was stirred at 40 rpm for 20 minutes. MgCl2·3EtOH carrier (6.5 kg; DTHFP / Mg=0.1 mol / mol; 27.2 mol Mg; Mg 10.18 wt%, d10=9.5 μm, d50=17.3 μm, d90=28.5 μm, granular) was stirred into the reactor. The suspension was cooled to about -20°C and a 33 wt% solution of triethylaluminum (29.4 kg, 85.0 mol of Al; Al / EtOH=1.0 mol / mol) dissolved in heptane was added in aliquots over 2.5 hours while keeping the temperature below 10°C. After adding TEA, the reaction mixture was gradually heated to 80°C in 2.4 hours and maintained at this temperature for another 20 minutes at 40 rpm. The suspension was allowed to settle for 10 minutes and the mother liquor was removed by a 10 μm filter at the bottom of the reactor within 15 minutes. Warm toluene (43 kg) was added to the container and then stirred at 40 rpm for 38 minutes at 55 to 70°C. The suspension was allowed to settle for 10 minutes at 50 to 55°C and the liquid was removed by a 10 μm filter at the bottom of the reactor within 15 minutes.
[0248] Catalyst preparation
[0249] Toluene (43 kg) was added to the container containing the pretreated support material and then cooled to about 30° C. Pure TiCl4 (5.17 kg, 27.5 mol; Ti / Mg=1.0 mol / mol) was added. The resulting suspension was heated to about 90° C. over 2 hours and maintained at this temperature for another hour while stirring at 40 rpm. The suspension was allowed to settle at about 90° C. for 10 minutes and the mother liquor was removed over 15 minutes through a 10 μm filter at the bottom of the reactor. The resulting solid material was washed twice with toluene (43 kg each) at about 90° C. and once with heptane (34 kg) at about 40° C. All three washing steps used the same sequence of events: addition of preheated (90 or 40° C.) solvent, followed by stirring at 40 rpm for 30 minutes, allowing the solid to settle for 10 minutes, and then removing the liquid over 15 minutes through a 10 μm filter at the bottom of the reactor.
[0250] The catalyst obtained was mixed with 20 kg of white oil and dried at 40-50° C. for 4 hours with a nitrogen stream (2 kg / h) and vacuum (-1 barg). The catalyst was removed from the reactor, rinsed with another 20 kg of oil and removed to the same drum. The dry catalyst yield was 3.60 kg (82.2% based on Mg).
[0251] polymerization
[0252] Example
[0253] Volume: 50dm 3 The loop reactor was operated at a temperature of 60° C. and a pressure of 58 bar. Ethylene, 1-butene, propane diluent and hydrogen were added to the reactor so that the feed rate of ethylene was 4.0 kg / h, the feed rate of 1-butene was 50 g / h, the feed rate of hydrogen was 10 g / h, and the feed rate of propane was 52 kg / h. In addition, 3 g / h of a solid polymerization catalyst component prepared as described above in the “Catalyst Preparation” section was introduced into the reactor together with triethylaluminum cocatalyst so that the molar ratio of Al / Ti was about 15. The estimated productivity was 3.8 kg / h.
[0254] The slurry stream was intermittently withdrawn from the reactor and introduced into a 350 dm 3 The reactor was operated at a temperature of 85°C and a pressure of 56 bar. 116 kg / h of fresh propane, ethylene and hydrogen were further added to the reactor so that the ethylene content in the fluid reaction mixture was 3.8 mol% and the molar ratio of hydrogen to ethylene was 500 mol / kmol. The MFR2 of the ethylene copolymer removed from the reactor was 300 g / 10 min and the density was 972 kg / m 3 . The productivity is 38kg / h.
[0255] The slurry was intermittently withdrawn from the loop reactor and introduced into a flash vessel, which was operated at a temperature of 50° C. and a pressure of 3 bar. From there the polymer was introduced into a fluidized bed gas phase reactor, which was operated at a pressure of 20 bar and a temperature of 75° C. Additional ethylene, 1-hexene comonomer, nitrogen as an inert gas and hydrogen were added so that the ethylene content in the fluid reaction mixture was 20 mol %, the ratio of hydrogen to ethylene was 150 mol / kmol and the molar ratio of 1-hexene to ethylene was 210 mol / kmol. The polymer production rate in the gas phase reactor was 55 kg / h, so that the total polymer extraction rate from the gas phase reactor was about 97 kg / h. The polymer had a melt flow rate MFR5 of 3.0 g / 10 min and a density of 920 kg / m 3 The yield split (prepolymer weight % / first stage component weight % / second stage component weight %) was 4 / 44 / 52.
[0256] The polymer powder was compounded with 0.2 wt% Irganox B141, 6.6 wt% carbon black masterbatch based on LDPE (MFR 190°C / 2.16 kg=2 g / 10 min) containing about 40% N220 type carbon black, 0.1 wt% Irganox B 225FF and 0.05 wt% calcium stearate and pelletized.
[0257] The procedure of Example 1 of the present invention was repeated using the conditions shown in Table 1.
[0258] Table 1: Trial production data
[0259]
[0260]
[0261] IE1 and IE2 were made from Catalyst 2. CE was made from Catalyst 1. CE was produced with similar process characteristics and CE had significantly higher flexibility than IE1 and IE2. IE1, IE2 and CE were prepared as described above on a pilot production scale compared to a control commercial product LE8707, available from Borealis, which is produced in a large-scale plant. The process parameters and catalyst selection were made to make the comparative example CE as close to the control commercial product as possible. It can be seen that the flexibility of the pilot scale material (CE) is significantly reduced compared to the commercial product. This shows that the present invention will produce better results in a large-scale plant.
[0262] Table 2 compares IE1, IE2, and CE to LE8707. Both IE1 and IE2 have lower flexural modulus than LE8707, but their hardness is comparable.
[0263] Table 2 Summary of analysis and testing of final materials
[0264]
[0265] As can be seen from Table 2, the comparative example and the inventive example have similar densities. Surprisingly, it can be seen that the inventive example has significantly higher flexibility than the comparative example, and an increased Shore D hardness. Other properties are similar to the ranges of the comparative example.
[0266] Figure 1 The flexural modulus is shown as a function of density. Figure 1 As can be seen from the above, the embodiments IE1 and IE2 of the present invention follow the equation as described above, namely
[0267] Flexural modulus [MPa] < 21.35 × density [kg / m 3 ]–19585
[0268] Although the present invention has been described by reference to various embodiments, those skilled in the art will recognize that changes can be made without departing from the scope of the present invention. It is intended that the detailed description be regarded as illustrative, and the appended claims including all equivalents are intended to define the scope of the present invention.
Claims
1. A multimodal ethylene copolymer composition comprising ethylene copolymers prepared by a process comprising a first polymerization stage, in which a first copolymer of ethylene is produced from ethylene, an α-olefin comonomer and hydrogen, and a second polymerization stage, in which a polymer mixture comprising the first copolymer of ethylene and a second copolymer of ethylene is produced, the second copolymer of ethylene being produced from ethylene and an α-olefin comonomer, the second copolymer of ethylene being formed on particles comprising the first copolymer of ethylene; Using a first α-olefin in a first polymerization stage and using a second α-olefin different from the first α-olefin in a second polymerization stage; The first α-olefin is selected from 1-butene, 1-hexene and 4-methyl-1-pentene, and the second α-olefin is selected from α-olefins containing 4 to 10 carbon atoms; The multimodal ethylene copolymer composition has a molecular weight of 920 to 949 kg / m 3 The density of the composite material is measured according to ISO 1183-1:2004 method A using compression molded test specimens prepared according to EN ISO 1872-2, February 2007; the flexural modulus is measured according to ISO 178 method using compression molded test specimens produced according to EN ISO 1872-2, February 2007; the flexural modulus in MPa and the flexural modulus in kg / m 3 The numerical value of the density in units follows the following relationship: Flexural modulus < 21.35 × density – 19585 [1], The multimodal ethylene copolymer composition has a Shore D of at least 53 on a specimen having a thickness of 4 mm, measured according to ISO 868 after the pressure foot has been in firm contact with the test specimen for 1 second, The multimodal ethylene copolymer composition further comprises carbon black; The ethylene copolymer is prepared by a Ziegler-Natta catalyst having an internal organic compound represented by formula (1), In formula (I), R1 to R5 are the same or different, and are hydrogen, a linear or branched C1 to C8 alkyl group, or a C3-C8 alkylene group, or two or more of R1 to R5 form a ring, and the two oxygen-containing rings are each saturated, partially unsaturated, or unsaturated.
2. The multimodal ethylene copolymer composition according to claim 1, wherein The multimodal ethylene copolymer composition has an MFR2 of 0.1 to 4 g / 10 min, measured according to ISO 1133 at 190°C and a load of 2.16 kg.
3. The multimodal ethylene copolymer composition according to claim 1, wherein The multimodal ethylene copolymer composition has an MFR2 measured according to ISO 1133 at 190°C and 2.16 kg load of 0.5 to 2 g / 10 min.
4. The multimodal ethylene copolymer composition according to claim 1, wherein The multimodal ethylene copolymer composition has an MFR5 of 0.3 to 12 g / 10 min, measured according to ISO 1133 at 190°C and 5 kg load.
5. The multimodal ethylene copolymer composition according to claim 1, wherein The MFR of the multimodal ethylene copolymer composition measured according to ISO 1133 at 190°C and 21.6 kg load is 21 20~180g / 10min.
6. The multimodal ethylene copolymer composition according to claim 1, wherein The flexural modulus in MPa and the 3 The numerical value of the density in units follows the following relationship: Flexural modulus <21.35×density–19610[2].
7. The multimodal ethylene copolymer composition according to claim 1, wherein The density of the compression molded sample of the multimodal ethylene copolymer composition prepared according to EN ISO 1872-2 published in February 2007 and measured according to ISO1183-1:2004 method A is 930-940 kg / m 3 .
8. A multimodal ethylene copolymer composition comprising an ethylene copolymer prepared by a process comprising a first polymerization stage, in which a first copolymer of ethylene is produced from ethylene, an α-olefin comonomer and hydrogen, and a second polymerization stage, in which a polymer mixture comprising the first copolymer of ethylene and a second copolymer of ethylene is produced, the second copolymer of ethylene being produced from ethylene, an α-olefin comonomer and hydrogen, the second copolymer of ethylene being formed on particles comprising the first copolymer of ethylene; a first α-olefin is used in the first polymerization stage and a second α-olefin different from the first α-olefin is used in the second polymerization stage; the first α-olefin is selected from 1-butene, 1-hexene and 4-methyl-1-pentene and the second α-olefin is selected from α-olefins containing 4 to 10 carbon atoms; The multimodal ethylene copolymer composition has a molecular weight of 920 to 949 kg / m 3 of density and has a flexural modulus, where The density is measured according to ISO 1183-1:2004 method A by using compression molded test specimens prepared according to EN ISO 1872-2, February 2007; the flexural modulus is measured according to ISO 178 method by using compression molded test specimens produced according to EN ISO 1872-2, February 2007; the flexural modulus in MPa and the flexural modulus in kg / m 3 The numerical value of the density in units follows the following relationship: Flexural modulus < 21.35 × density – 19585 [1], The multimodal ethylene copolymer composition has a Shore D of at least 53 on a specimen having a thickness of 4 mm, measured according to ISO 868 after the pressure foot has been in firm contact with the test specimen for 1 second, The multimodal ethylene copolymer composition further comprises carbon black; The ethylene copolymer is prepared by a Ziegler-Natta catalyst having an internal organic compound represented by formula (1), In formula (I), R1 to R5 are the same or different, and are hydrogen, a linear or branched C1 to C8 alkyl group, or a C3-C8 alkylene group, or two or more of R1 to R5 form a ring, and the two oxygen-containing rings are each saturated, partially unsaturated, or unsaturated.
9. The multimodal ethylene copolymer composition according to claim 8, wherein The multimodal ethylene copolymer composition has an MFR2 of 0.1 to 4 g / 10 min, measured according to ISO 1133 at 190°C and a load of 2.16 kg.
10. The multimodal ethylene copolymer composition according to claim 8, wherein The multimodal ethylene copolymer composition has an MFR2 measured according to ISO 1133 at 190°C and 2.16 kg load of 0.5 to 2 g / 10 min.
11. The multimodal ethylene copolymer composition according to claim 8, wherein The multimodal ethylene copolymer composition has an MFR5 of 0.3 to 12 g / 10 min, measured according to ISO 1133 at 190°C and 5 kg load.
12. The multimodal ethylene copolymer composition according to claim 8, wherein The MFR of the multimodal ethylene copolymer composition measured according to ISO 1133 at 190°C and 21.6 kg load is 21 20~180g / 10min.
13. The multimodal ethylene copolymer composition according to claim 8, wherein The flexural modulus in MPa and the 3 The numerical value of the density in units follows the following relationship: Flexural modulus <21.35×density–19610[2].
14. The multimodal ethylene copolymer composition according to claim 8, wherein The density of the compression molded sample of the multimodal ethylene copolymer composition prepared according to EN ISO 1872-2 published in February 2007 and measured according to ISO1183-1:2004 method A is 930-940 kg / m 3 .
15. A cable sheathing comprising the multimodal ethylene copolymer composition according to any one of claims 1 to 14.