Liquid crystal alignment agent, liquid crystal alignment film and liquid crystal element
By using a liquid crystal alignment agent containing a polymer and solvent with a specific structure, the solubility and coatability problems caused by the polarity of amide groups were solved, thereby improving the uniformity and electrical properties of the liquid crystal alignment film.
Patent Information
- Application Number
- CN202011124991.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-10-20
AI Technical Summary
The high polarity of amide groups in liquid crystal alignment agents leads to poor solubility, affecting coating properties and the uniformity of liquid crystal alignment films. Furthermore, the solvent components penetrate into the lower layers, resulting in a decrease in the electrical properties of liquid crystal elements.
A liquid crystal alignment agent containing polymers, cyclic carbonate compounds, and dialkyl glycol monoalkyl ethers is used. The polymers contain amide groups, protected amide groups, urea groups, and other structures. Combined with dialkyl glycol dialkyl esters, the solubility and coatability are improved, and a liquid crystal alignment film is formed by light irradiation or rubbing treatment.
This improved the coatability of the liquid crystal alignment agent and the electrical properties of the liquid crystal element, reduced the impact of solvent penetration into the lower layer, and ensured film thickness uniformity and electrical property stability.
Smart Images

Figure BDA0002733300860000021 
Figure BDA0002733300860000041 
Figure BDA0002733300860000051
Abstract
Description
Technical Field
[0001] The invention relates to a liquid crystal alignment agent, a liquid crystal alignment film and a liquid crystal element. Background Art
[0002] In recent years, liquid crystal elements are not only used in display devices such as personal computers or liquid crystal televisions, car navigation systems, mobile phones, smart phones, and information displays, but also in various applications such as optical compensation films and dimming films. With such multi-purpose applications, liquid crystal elements are required to be further improved in quality, and improvements in driving methods or element structures, as well as improvements in liquid crystal alignment films, which are one of the components of liquid crystal elements, are being promoted.
[0003] In order to further improve the performance of liquid crystal elements, it is proposed to use polyimide having a nitrogen-containing structure such as an amide group (-NH-CO-) for an alignment film material (for example, see Patent Document 1). Patent Document 1 discloses that a liquid crystal alignment agent contains polyamic acid, which is obtained by reacting tetracarboxylic dianhydride containing 1,2,3,4-cyclobutanetetracarboxylic dianhydride with a diamine compound containing a diamine having an amide group (-NH-CO-).
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2009-294274 Summary of the invention
[0007] [Problems to be solved by the invention]
[0008] The polarity of the amide group is high, and the solubility in the solvent component of the liquid crystal alignment agent is not very good. Therefore, the liquid crystal alignment agent prepared with a polymer having a nitrogen-containing structure such as an amide group has poor coating properties on the substrate, and the film thickness of the alignment film formed using the liquid crystal alignment agent is sometimes uneven.
[0009] The liquid crystal alignment film is generally formed by coating a liquid crystal alignment agent containing a polymer component and a solvent on a substrate laminated with a color filter or a transparent conductive film, and removing the solvent from the coating film. At this time, since the solvent component in the liquid crystal alignment agent penetrates into the lower layer, the low molecular components contained in the lower layer (such as the colored hardened film) sometimes dissolve and mix into the liquid crystal alignment film or the liquid crystal layer. In this case, there is a concern that the electrical properties of the liquid crystal element will be reduced due to the dissolution from the lower layer.
[0010] The present invention has been made in view of the above-mentioned problems, and one object of the present invention is to provide a liquid crystal aligning agent which is excellent in coating properties and can obtain a liquid crystal element having good electrical characteristics.
[0011] [Technical means to solve the problem]
[0012] The present invention adopts the following means to solve the above-mentioned problems.
[0013] <1> A liquid crystal alignment agent comprising: a polymer [P] having at least one selected from the group consisting of an amide group, a protected amide group, a urea group, and a protected urea group; a cyclic carbonate compound; and a dialkyl glycol monoalkyl ether.
[0014] <2> The liquid crystal aligning agent according to <1>, further comprising a dialkyl diol ester.
[0015] <3> A liquid crystal aligning film formed using the liquid crystal aligning agent according to <1> or <2>.
[0016] <4> A liquid crystal element including the liquid crystal alignment film according to <3>.
[0017] [Effects of the Invention]
[0018] The liquid crystal aligning agent of this invention is excellent in coating property, and can obtain the liquid crystal element which is favorable in electric characteristics. DETAILED DESCRIPTION
[0019] Hereinafter, each component contained in the liquid crystal aligning agent of the present disclosure and other components arbitrarily prepared as needed will be described. The liquid crystal aligning agent contains a polymer component and a solvent component, and is preferably a liquid polymer composition in which the polymer component is dissolved in the solvent component.
[0020] In addition, in this specification, the so-called "hydrocarbon group" refers to the meaning of chain hydrocarbon groups, alicyclic hydrocarbon groups and aromatic hydrocarbon groups. The so-called "chain hydrocarbon group" refers to a straight-chain hydrocarbon group and a branched hydrocarbon group that does not contain a cyclic structure in the main chain and is only composed of a chain structure. Among them, it can be saturated or unsaturated. The so-called "alicyclic hydrocarbon group" refers to a hydrocarbon group that only contains the structure of alicyclic hydrocarbon as a ring structure and does not contain an aromatic ring structure. Among them, it is not necessary to be composed only of the structure of alicyclic hydrocarbons, and a group having a chain structure in a part thereof is also included. The so-called "aromatic hydrocarbon group" refers to a hydrocarbon group that contains an aromatic ring structure as a ring structure. Among them, it is not necessary to be composed only of an aromatic ring structure, and a chain structure or an alicyclic hydrocarbon structure may be contained in a part thereof.
[0021] 《Polymer composition》
[0022] <Polymer [P]>
[0023] The liquid crystal alignment agent of the present disclosure contains a polymer [P] having at least one partial structure (hereinafter also referred to as a "specific structure") selected from the group consisting of an amide group, a protected amide group, a urea group, and a protected urea group. The specific structure of the polymer [P] is represented by the following formula (1), for example.
[0024] [Chemistry 1]
[0025]
[0026] (In formula (1), R 1 and R 2 Each is independently a hydrogen atom or a monovalent organic group. m is 0 or 1. "*" represents a bond to a hydrocarbon group.
[0027] In the formula (1), R 1 and R 2 The monovalent organic group is preferably a monovalent hydrocarbon group or a protecting group having 1 to 20 carbon atoms. Examples of the monovalent hydrocarbon group include monovalent chain hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups, among which alkyl groups, cycloalkyl groups, or phenyl groups having 1 to 3 carbon atoms are preferred. Here, the protecting group is a functional group that makes the group represented by the formula (1) inert in advance. The "protected amide group" is a group formed by the removal of the protecting group to form a "*" group. 1 -CO-NH-* 1 "(in,* 1 In addition, the "protected urea group" is a group formed by the detachment of the protecting group. 2 -NH-CO-NH-* 2 "(in,* 2 represents a bond to a hydrocarbon group).
[0028] The protecting group in the formula (1) is preferably a monovalent group that is detached by heat or light, and examples thereof include: carbamate protecting groups, amide protecting groups, imide protecting groups, sulfonamide protecting groups, etc. Among them, in terms of high thermal detachability, carbamate protecting groups are preferred, and specific examples thereof include: tert-butoxycarbonyl, benzyloxycarbonyl, 1,1-dimethyl-2-haloethoxycarbonyl, allyloxycarbonyl, 2-(trimethylsilyl)ethoxycarbonyl, etc. Among them, in terms of excellent thermal detachability and the ability to reduce the residual amount of the deprotected part in the film, tert-butoxycarbonyl is particularly preferred.
[0029] R 1 and R 2 A hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a protecting group is preferred, and a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a tert-butoxycarbonyl group is particularly preferred.
[0030] As polymer [P], there can be cited polymers with a main skeleton of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, polyenamine, polyester, polyamide, polyamideimide, polybenzoxazole precursor, polybenzoxazole, cellulose derivative, polyacetal, polymer having a structural unit derived from a monomer containing a polymerizable unsaturated bond (hereinafter also referred to as "polymer Q"), etc. In terms of being able to form a liquid crystal alignment film with high affinity for liquid crystal, high mechanical strength and high reliability, polymer [P] preferably includes at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, polyamide and polymer Q, and particularly preferably includes at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.
[0031] The polymer [P] may have a specific structure in the main chain and in any one of the side chains. From the viewpoint of making the electrical properties of the liquid crystal element more excellent, the polymer [P] preferably has a specific structure in the main chain. In addition, the so-called "having a specific structure in the main chain" refers to the case where the specific structure is only in the main chain, and the case where the specific structure is in the main chain and the side chain. Here, the so-called "main chain" refers to the part of the "trunk" containing the longest atomic chain in the polymer. In addition, the part of the "trunk" is allowed to contain a ring structure. Therefore, the so-called "having a specific structure in the main chain" means that the specific structure constitutes a part of the main chain. The so-called "side chain" refers to the part branching from the "trunk" of the polymer.
[0032] As a method for obtaining a polymer having a specific structure, a method of polymerizing using a monomer having a specific structure can be cited. In this case, in the polymer [P], the content of the structural unit derived from the monomer having the specific structure is preferably 5 mol% or more, more preferably 10 mol% or more, further preferably 15 mol% or more, and particularly preferably 20 mol% or more, relative to the total amount of the monomer units possessed by the polymer [P]. In addition, the content of the structural unit derived from the monomer having the specific structure is preferably 90 mol% or less, more preferably 80 mol% or less, and further preferably 70 mol% or less, relative to the total amount of the monomer units possessed by the polymer [P].
[0033] ·Specific base A
[0034] The polymer [P] preferably further has at least one group selected from the group consisting of a group having a polymerizable carbon-carbon unsaturated bond, a photoinitiator group, and a photo-alignment group (hereinafter also referred to as "specific group A"). By having such a specific group A, a more stable liquid crystal alignment film can be formed, and a liquid crystal alignment film that can obtain a liquid crystal element showing excellent electrical properties can be formed, which is preferred in this respect.
[0035] In the specific group A, the group having a polymerizable carbon-carbon unsaturated bond is preferably a functional group that can be polymerized by heat or light. Specific examples of the group having a polymerizable carbon-carbon unsaturated bond include: (meth)acryloyl, vinyl, allyl, vinylphenyl, maleimide, vinyloxy, ethynyl, etc. Among them, in terms of high reactivity based on heat, preferably (meth)acryloyl, vinyl, allyl, ethynyl or vinylphenyl, more preferably (meth)acryloyl.
[0036] In the polymer [P], the content of the group having a polymerizable carbon-carbon unsaturated bond is preferably 1 mol% or more, more preferably 5 mol% or more, and further preferably 10 mol% or more, relative to the total amount of the monomer units possessed by the polymer [P]. In addition, the content of the group having a polymerizable carbon-carbon unsaturated bond is preferably 60 mol% or less, more preferably 50 mol% or less, relative to the total amount of the monomer units possessed by the polymer [P].
[0037] The photoinitiator group is a site that generates polymerization initiation ability by light or a site with photosensitization, and is a group having a structure after one or more hydrogen atoms are removed from the photoinitiator. Here, the photoinitiator refers to a compound that can initiate the polymerization of polymerizable components by irradiation with radiation such as visible light, ultraviolet rays, far ultraviolet rays, electron beams, and X-rays. The photoinitiator group possessed by the polymer [P] is preferably a group having a structure after hydrogen atoms are removed from a free radical polymerization initiator that can generate free radicals by light irradiation, specifically, preferably a group having an acetophenone structure, an oxime ester structure, a dibenzoyl structure, a benzoin structure, a dibenzophenone structure, an alkyl phenone structure, or an acylphosphine oxide structure. Among them, the photoinitiator group is preferably a group having an alkyl phenone structure or an acetophenone structure.
[0038] As further specific examples of the photoinitiator group, for example, there can be mentioned a group having a structure obtained by removing a hydrogen atom from the following substances: 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, phenyl 2-(meth)acryloyloxy-2-propyl ketone, 4-isopropylphenyl 2-(meth)acryloyloxy-2-propyl ketone, 4-(2-(meth)acryloyloxyethoxy)-benzoin, 4-(meth)acryloyloxyphenyl 2-(meth)acryloyloxy-2-propyl ketone, 4-(meth)acryloyloxybenzophenone, etc.
[0039] In the polymer [P], the content of the photoinitiator group is preferably 1 mol% or more, more preferably 3 mol% or more, and further preferably 5 mol% or more, relative to the total amount of the monomer units of the polymer [P]. In addition, the content of the photoinitiator group is preferably 50 mol% or less, more preferably 40 mol% or less, relative to the total amount of the monomer units of the polymer [P].
[0040] The photo-orientation group is a functional group that imparts anisotropy to the film by a photoisomerization reaction or a photodimerization reaction, a photodecomposition reaction, or a photoFries rearrangement reaction caused by light irradiation. As a specific example of the photo-orientation group, for example, it can be cited: a group containing azobenzene as a basic skeleton, a group containing cinnamic acid structure containing cinnamic acid or its derivatives as a basic skeleton, a group containing chalcone as a basic skeleton, a group containing benzophenone or its derivatives as a basic skeleton, a group containing benzophenone as a basic skeleton, a group containing coumarin or its derivatives as a basic skeleton, a structure containing cyclobutane or its derivatives as a basic skeleton, etc. Among them, in terms of high sensitivity to light, it is preferably a group containing a cinnamic acid structure, for example, a group having a partial structure represented by the following formula (6) can be cited.
[0041] [Chemistry 2]
[0042]
[0043] (In formula (6), R 21 and R 22 are each independently a hydrogen atom, a fluorine atom, a cyano group, an alkyl group having 1 to 3 carbon atoms, or a fluoroalkyl group having 1 to 3 carbon atoms, and R 23 is an alkyl group, alkoxy group, fluoroalkyl group or fluoroalkoxy group having 1 to 10 carbon atoms, a fluorine atom or a cyano group. k is an integer of 0 to 4. When k is 2 or more, a plurality of R 23 The same base or different bases. "*" indicates a bond. )
[0044] In the structure represented by the formula (6), R 21 and R 22 Preferably, both are hydrogen atoms, or one of them is a hydrogen atom and the other (preferably R 22 ) is an alkyl group having 1 to 3 carbon atoms. 23 It is preferably a fluorine atom, a cyano group or an alkyl group having 1 to 5 carbon atoms, and more preferably a fluorine atom, a cyano group or an alkyl group having 1 to 3 carbon atoms. k is preferably 0 to 2, and more preferably 0 or 1.
[0045] In terms of more preferably controlling the pretilt angle of the resulting liquid crystal element, one of the two bonds "*" in the formula (6) is preferably bonded to an alkyl group, alkoxy group, fluoroalkyl group, fluoroalkoxy group, cyano group-containing alkyl group or cyano group-containing alkoxy group having 3 to 20 carbon atoms, or a group having at least one of a benzene ring and a cyclohexane ring.
[0046] In the polymer [P], the content of the photo-alignment group is preferably 1 mol% or more, more preferably 5 mol% or more, and further preferably 10 mol% or more, relative to the total amount of the monomer units of the polymer [P]. In addition, the content of the photo-alignment group is preferably 60 mol% or less, more preferably 50 mol% or less, relative to the total amount of the monomer units of the polymer [P].
[0047] ·Specific base B
[0048] The polymer [P] preferably further has at least one group selected from the group consisting of a tertiary amine structure, a protected amino group, and a nitrogen-containing aromatic heterocyclic group (hereinafter also referred to as a "specific group B"). By having such a specific group B, a liquid crystal element showing more excellent electrical properties can be obtained, which is preferred in this respect.
[0049] In the specific group B, the tertiary amine structure is preferably a partial structure represented by the following formula (7).
[0050] [Chemistry 3]
[0051]
[0052] (In formula (7), R 51 is a divalent hydrocarbon group. 52 and R 53 Represents R 52 is a divalent hydrocarbon group and R 53 is a monovalent hydrocarbon group, or R 52 and R 53 Combined with R 52 and R 53 The nitrogen atoms bonded together form a ring structure. "*" indicates a bond. )
[0053] In the formula (7), R 51 and R 52 Examples of divalent hydrocarbon groups include alkanediyl, cyclohexylene, and phenylene. 53 Examples of the monovalent hydrocarbon group include an alkyl group, a cyclohexyl group, and a phenyl group. 52 With R 53 Combined with R 52 and R 53 Examples of the ring structure formed together with the nitrogen atoms to which the ring is bonded include a piperidine structure, a piperazine structure, a pyrrolidine structure, and a hexamethyleneimine structure.
[0054] In the protected amino group, the amino group is protected by a protecting group, and the protecting group is preferably detached by heat to generate a primary amino group or a secondary amino group. In addition, the primary amino group or the secondary amino group generated by the detachment of the protecting group is bonded to a hydrocarbon group. The protecting group is preferably a group detached by heat, for example, carbamate protecting groups, amide protecting groups, imide protecting groups, sulfonamide protecting groups, etc. Among them, the protecting group is preferably a tert-butoxycarbonyl group in terms of high detachability based on heat and the amount of residue in the film of the deprotected part can be reduced.
[0055] The nitrogen-containing aromatic heterocyclic group is an n-valent group obtained by removing n hydrogen atoms from the ring part of the nitrogen-containing aromatic heterocyclic ring. The nitrogen-containing aromatic heterocyclic ring can be an aromatic ring containing one or more nitrogen atoms in the ring skeleton. In addition, as a heteroatom, it can contain only nitrogen atoms, or it can contain nitrogen atoms and heteroatoms other than nitrogen atoms (oxygen atoms, sulfur atoms, etc.).
[0056] Specific examples of heterocyclic rings constituting nitrogen-containing aromatic heterocyclic groups include, for example, pyrrole rings, imidazole rings, pyrazole rings, triazole rings, pyridine rings, pyrimidine rings, pyridazine rings, pyrazine rings, indole rings, benzimidazole rings, purine rings, quinoline rings, isoquinoline rings, naphthyridine rings, quinoxaline rings, phthalazine rings, triazine rings, azepine rings, diazepine rings, acridine rings, phenazine rings, phenanthroline rings, oxazole rings, thiazole rings, carbazole rings, thiadiazole rings, benzothiazole rings, phenothiazine rings, oxadiazole rings, etc. In nitrogen-containing aromatic heterocyclic groups, substituents may also be introduced into the ring moiety. As the substituents, for example, halogen atoms, alkyl groups, alkoxy groups, etc. may be included. Among them, the nitrogen-containing aromatic heterocyclic group is preferably a group obtained by removing a hydrogen atom from a ring portion of a pyrrole ring, an imidazole ring, a pyrazole ring, a triazole ring, a pyridine ring, a pyrimidine ring, a pyridazine ring or a pyrazine ring.
[0057] In the polymer [P], the content of the specific group B is preferably 1 mol% or more, more preferably 5 mol% or more, and further preferably 10 mol% or more relative to the total amount of the monomer units possessed by the polymer [P]. In addition, the content of the specific group B is preferably 60 mol% or less, more preferably 50 mol% or less relative to the total amount of the monomer units possessed by the polymer [P]. In addition, the specific group B possessed by the polymer [P] may be only one type, or may be two or more types.
[0058] Next, preferred examples of the polymer [P] are described in detail.
[0059] <Polyamic acid>
[0060] When the polymer [P] is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [P]") can be obtained by reacting tetracarboxylic dianhydride with a diamine compound. As a method for obtaining a polymer having a specific structure, there can be cited: (1) a method of polymerizing using tetracarboxylic anhydride having a specific structure, (2) a method of polymerizing using a diamine having a specific structure (hereinafter also referred to as "specific diamine"), etc. Among them, the method (2) is preferred in terms of the high degree of freedom of selection of the monomer.
[0061] (Tetracarboxylic dianhydride)
[0062] Examples of the tetracarboxylic dianhydride used in the synthesis of the polyamic acid [P] include aliphatic tetracarboxylic dianhydride, alicyclic tetracarboxylic dianhydride, aromatic tetracarboxylic dianhydride, etc. Specific examples thereof include aliphatic tetracarboxylic dianhydride, such as 1,2,3,4-butanetetracarboxylic dianhydride;
[0063] Alicyclic tetracarboxylic dianhydrides include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 2,4, 6,8-tetracarboxy bicyclo[3.3.0]octane-2:4,6:8-dianhydride, cyclopentanetetracarboxylic dianhydride, cyclohexanetetracarboxylic dianhydride, etc.; aromatic tetracarboxylic dianhydride can be exemplified by pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, ethylene glycol ditriphthalic anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 4,4'-carbonyldiphthalic anhydride, etc. In addition to the above tetracarboxylic dianhydride, the tetracarboxylic dianhydride described in Japanese Patent Laid-Open No. 2010-97188 can also be used. As tetracarboxylic dianhydride, one kind can be used alone or two or more kinds can be used in combination.
[0064] As the tetracarboxylic dianhydride used in the synthesis of the polyamic acid [P], in terms of obtaining a polymer [P] having higher solubility in a solvent, it is preferred to include at least one compound selected from the group consisting of aliphatic tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride, more preferably include alicyclic tetracarboxylic dianhydride, and further preferably include alicyclic tetracarboxylic dianhydride having at least one ring structure selected from the group consisting of a cyclobutane ring, a cyclopentane ring, and a cyclohexane ring. The usage ratio of aliphatic tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride (total amount when two or more are included) relative to the total amount of tetracarboxylic dianhydride used in the synthesis of the polyamic acid [P] is preferably set to 20 mol% or more, more preferably set to 40 mol% or more, and further preferably set to 50 mol% or more.
[0065] (Diamine compound)
[0066] ·Specific diamine
[0067] Examples of the diamine compound used in the synthesis of the polyamic acid include aliphatic diamines, alicyclic diamines, aromatic diamines, diaminoorganosiloxanes, etc. The specific diamine is preferably an aromatic diamine, and specifically includes compounds represented by the following formula (5A) and compounds represented by the following formula (5B).
[0068] [Chemistry 4]
[0069]
[0070] (In formula (5A), R 10 , R 11 and R 12 Each independently represents a single bond, a divalent hydrocarbon group having 1 to 20 carbon atoms, or a divalent group having 2 to 20 carbon atoms having -O- between carbon-carbon bonds. j is an integer from 1 to 3. When j = 2 or 3, R 11 It will not become a single bond. 13 and R 14 p1 and p2 are each independently a monovalent organic group having 1 to 5 carbon atoms. p1 and p2 are each independently an integer of 0 to 2. 1 , R 2 and m has the same meaning as in the above formula (1).
[0071] [Chemistry 5]
[0072]
[0073] (In formula (5B), L 3 is a single bond or a divalent linking group, R 17 is a monovalent organic group having 1 to 40 carbon atoms. m1 and m2 are each independently 0 or 1. However, m1 and m2 are not 0 at the same time. 1 and R2 It has the same meaning as the above formula (1).
[0074] In the above formula (5A), from the viewpoint of improving the electrical properties of the liquid crystal element, R 10 , R 11 and R 12 The divalent hydrocarbon group is preferably a divalent chain hydrocarbon group or an alicyclic hydrocarbon group, more preferably a divalent chain hydrocarbon group, and further preferably an alkanediyl group. 10 , R 11 and R 12 When the divalent hydrocarbon group is an alkanediyl group, R 10 , R 11 and R 12 The carbon number of R is preferably 1 to 10, more preferably 1 to 6. 10 , R 11 and R 12 In the case of a divalent group having 2 to 20 carbon atoms and having -O- between carbon-carbon bonds, the divalent group is preferably -R 15 -(OR 16 )r-(where R 15 and R 16 Each is independently an alkanediyl group, and r is an integer of 1 to 3. )
[0075] R 13 and R 14 It is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably a methyl group or an ethyl group. p1 and p2 are preferably 0 or 1. j is preferably 1 or 2.
[0076] In the formula (5B), L 3 The divalent linking group of is preferably an alkanediyl group having 1 to 5 carbon atoms, and more preferably an alkanediyl group having 1 to 3 carbon atoms. 17 The monovalent organic group may include a monovalent hydrocarbon group having 1 to 40 carbon atoms, a group containing a heteroatom between carbon-carbon bonds of the hydrocarbon group, a group having a heterocyclic group, and the like. 17 It is preferably a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms or a monovalent group having a nitrogen-containing aromatic heterocyclic ring.
[0077] As specific examples of specific diamines, the compound represented by the formula (5A) may be compounds represented by the following formulas (5-1) to (5-17), etc.; the compound represented by the formula (5B) may be compounds represented by the following formulas (5-18) to (5-31), etc. In addition, by using compounds represented by the following formulas (5-18) to (5-22), (5-28), (5-29), and (5-31), a polymer [P] having a nitrogen-containing aromatic heterocyclic group as a specific group B can be obtained.
[0078] [Chemistry 6]
[0079]
[0080] [Chemistry 7]
[0081]
[0082] (Wherein, "TMS" represents trimethoxysilyl.)
[0083] [Chemistry 8]
[0084]
[0085] Other diamines
[0086] The diamine compound used in the synthesis of the polyamic acid [P] may be only a specific diamine, or a specific diamine and a diamine different from the specific diamine (hereinafter also referred to as "other diamines") may be used together. Examples of other diamines include aliphatic diamines, alicyclic diamines, aromatic diamines, and diaminoorganosiloxanes.
[0087] Specific examples of other diamines include p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4-aminophenyl-4-aminobenzoate, 4,4'-diaminoazobenzene, 3,5-diaminobenzoic acid, 1,5-bis(4-aminophenoxy)benzene, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,6-bis(4-aminophenoxy)hexane, bis[2-(4-aminophenyl)ethyl]hexanediacid, 4,4'-diaminodiphenyl ether, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2, Main chain diamines such as 2-bis(4-aminophenyl)hexafluoropropane, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenylamine, 1,5-bis(4-aminophenyl)benzene, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 4,4'-(phenylene diisopropylidene) dianiline, 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, m-xylene diamine, hexamethylene diamine, and 4,4'-methylene bis(cyclohexylamine);
[0088] Dodecyloxy-2,4-diaminobenzene, pentadecyloxy-2,4-diaminobenzene, hexadecyloxy-2,4-diaminobenzene, octadecyloxy-2,4-diaminobenzene, pentadecyloxy-2,5-diaminobenzene, octadecyloxy-2,5-diaminobenzene, cholesteryloxy-3,5-diaminobenzene, cholesteryloxy-3,5-diaminobenzene, cholesteryloxy-2,4-diaminobenzene, cholesteryloxy-2,4-diaminobenzene, cholesteryloxy-3,5-diaminobenzoate, 3,5-diamino Side chain type diamines such as cholesteryl benzoate, lanostanyl 3,5-diaminobenzoate, 3,6-bis(4-aminobenzoyloxy)cholestane, 3,6-bis(4-aminophenoxy)cholestane, 4-(4'-trifluoromethoxybenzoyloxy)cyclohexyl-3,5-diaminobenzoate, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-butylcyclohexane, 5ξ-cholestane-3-yl 3,5-diaminobenzoate, and compounds represented by the following formula (E-1),
[0089] [Chemistry 9]
[0090]
[0091] (In formula (E-1), X I and X II are independently a single bond, -O-, *-COO- or *-OCO- (wherein "*" indicates the I The bond of I is an alkanediyl group having 1 to 3 carbon atoms, R II is a single bond or an alkanediyl group having 1 to 3 carbon atoms, a is 0 or 1, b is an integer of 0 to 2, c is an integer of 1 to 20, and d is 0 or 1. Wherein a and b are not 0 at the same time. ).
[0092] Examples of the compound represented by the formula (E-1) include compounds represented by the following formulae (E-1-1) to (E-1-4), respectively.
[0093] [Chemistry 10]
[0094]
[0095] By using a diamine having a specific group A as another diamine, a polyamic acid [P] having a specific group A can be produced, and by using a diamine having a specific group B, a polyamic acid [P] having a specific group B can be produced. Specific examples of the diamine having a specific group A include compounds represented by the following formulas (a-1) to (a-11), respectively. Specific examples of the diamine having a specific group B include 2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole, N-ethyl-3,6-diaminocarbazole, N-phenyl-3,6-diaminocarbazole, 3,6-diaminoacridine, compounds represented by the above formulas (5-18) to (5-22), (5-28), (5-29) and (5-31), compounds represented by the following formulas (b-1) to (b-18), etc.
[0096] [Chemistry 11]
[0097]
[0098] (Where L 2 is a divalent linking group.)
[0099] [Chemistry 12]
[0100]
[0101] (Where R 40 It is an alkyl group having 1 to 20 carbon atoms. 1 is a divalent linking group.)
[0102] [Chemistry 13]
[0103]
[0104] [Chemistry 14]
[0105]
[0106] When synthesizing polyamic acid [P], in terms of the coating property of the liquid crystal alignment agent and the electrical characteristics of the liquid crystal cell that can be well balanced, relative to the total amount of the diamine compound used in the synthesis of polyamic acid [P], the use ratio of specific diamine is preferably 5 mol% or more, more preferably 10 mol% or more, and then preferably 15 mol% or more, and particularly preferably 20 mol% or more. In addition, with respect to the viewpoint of obtaining the effect of the performance improvement brought about by and using other diamines, the use ratio of specific diamine is preferably 90 mol% or less, more preferably 80 mol% or less, and then preferably 70 mol% or less. As a specific diamine, one can be used alone or two or more can be used in combination.
[0107] (Synthesis of Polyamic Acid)
[0108] Polyamic acid [P] can be obtained by reacting the tetracarboxylic dianhydride and the diamine compound with a molecular weight modifier as needed. In the synthesis reaction of polyamic acid [P], the use ratio of tetracarboxylic dianhydride and diamine compound is preferably a ratio in which the anhydride group of tetracarboxylic dianhydride is 0.2 equivalents to 2 equivalents relative to 1 equivalent of the amino group of the diamine compound. As molecular weight modifiers, for example, acid monoanhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride, monoamine compounds such as aniline, cyclohexylamine, and n-butylamine, monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate, etc. The use ratio of the molecular weight modifier is preferably set to 20 parts by mass or less relative to a total of 100 parts by mass of the tetracarboxylic dianhydride and diamine compound used.
[0109] The synthesis reaction of polyamic acid [P] is preferably carried out in an organic solvent. The reaction temperature at this time is preferably -20°C to 150°C, and the reaction time is preferably 0.1 hour to 24 hours. As the organic solvent used in the reaction, for example, aprotic polar solvents, phenolic solvents, alcohols, ketones, esters, ethers, halogenated hydrocarbons, hydrocarbons, etc. can be cited. As a specific example, it is preferred to use one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphoric triamide, metacresol, dimethyl phenol and halogenated phenol as a reaction solvent, or use a mixture of one or more of them with other organic solvents (such as butyl cellosolve, diethylene glycol diethyl ether, etc.). The amount (a) of the organic solvent used is preferably set to an amount that makes the total amount (b) of tetracarboxylic dianhydride and diamine relative to the total amount (a+b) of the reaction solution 0.1% to 50% by mass.
[0110] In this manner, a polymer solution in which the polyamic acid [P] is dissolved is obtained. The polymer solution may be used directly for the preparation of a liquid crystal aligning agent, or may be used for the preparation of a liquid crystal aligning agent after the polyamic acid [P] contained in the polymer solution is separated.
[0111] <Polyamic acid ester>
[0112] When the polymer [P] is polyamic acid ester, the polyamic acid ester (hereinafter also referred to as "polyamic acid ester [P]") can be obtained, for example, by the following methods: [I] a method of reacting polyamic acid [P] with an esterifying agent; [II] a method of reacting a tetracarboxylic acid diester with a diamine compound; [III] a method of reacting a tetracarboxylic acid diester dihalide with a diamine compound. Polyamic acid ester [P] may have only an amic acid ester structure, or may be a partially esterified product of an amic acid structure and an amic acid ester structure. In [II] and [III], it is preferred to react a tetracarboxylic acid derivative with a diamine compound containing a specific diamine. The reaction solution formed by dissolving polyamic acid ester [P] can be directly used for the preparation of a liquid crystal aligning agent, or it can be used for the preparation of a liquid crystal aligning agent after separating the polyamic acid ester [P] contained in the reaction solution.
[0113] <Polyimide>
[0114] When the polymer [P] is a polyimide, the polyimide (hereinafter also referred to as "polyimide [P]") can be obtained, for example, by dehydrating and ring-closing the polyamic acid [P] synthesized in the above manner and imidizing it. The polyimide [P] may be a completely imidized product formed by dehydrating and ring-closing all the amic acid structures possessed by the polyamic acid [P] as its precursor, or a partially imidized product formed by dehydrating and ring-closing only a part of the amic acid structure so that the amic acid structure and the imide ring structure coexist. The imidization rate of the polyimide [P] is preferably 20% to 99%, and more preferably 30% to 90%. In addition, the imidization rate is expressed as a percentage of the ratio of the number of imide ring structures to the total number of amic acid structures and the number of imide ring structures of the polyimide. Here, a part of the imide ring may be an isoimide ring.
[0115] The dehydration ring-closure of polyamic acid [P] is preferably carried out by the following method: dissolving polyamic acid [P] in an organic solvent, adding a dehydrating agent and a dehydration ring-closure catalyst to the solution, and heating as needed. In the method, as a dehydrating agent, for example, an anhydride such as acetic anhydride, propionic anhydride, trifluoroacetic anhydride, etc. can be used. The amount of the dehydrating agent used is preferably set to 0.01 mol to 20 mol relative to 1 mol of the amic acid structure of polyamic acid [P]. As a dehydration ring-closure catalyst, for example, a tertiary amine such as pyridine, trimethylpyridine, dimethylpyridine, triethylamine, etc. can be used. The amount of the dehydration ring-closure catalyst used is preferably set to 0.01 mol to 10 mol relative to 1 mol of the dehydrating agent used. As the organic solvent used in the dehydration ring-closure reaction, the organic solvent exemplified as the organic solvent used in the synthesis of polyamic acid [P] can be cited. The reaction temperature of the dehydration ring-closure reaction is preferably 0°C to 180°C. The reaction time is preferably 1.0 hour to 120 hours. Moreover, the reaction solution containing the polyimide [P] may be used for preparation of a liquid crystal aligning agent as it is, or may be used for preparation of a liquid crystal aligning agent after isolating the polyimide [P].
[0116] Regarding the solution viscosity of the polymer [P] used in the preparation of the liquid crystal alignment agent, when a solution with a concentration of 10% by mass is prepared, it is preferably a solution viscosity of 10mPa·s to 800mPa·s, and more preferably a solution viscosity of 15mPa·s to 500mPa·s. In addition, the solution viscosity (mPa·s) is a value measured at 25°C using an E-type rotational viscometer for a polymer solution with a concentration of 10% by mass prepared using a good solvent for the polymer [P] (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.).
[0117] The weight average molecular weight (Mw) of the polymer [P] measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1,000 to 500,000, and more preferably 2,000 to 300,000. In addition, the molecular weight distribution (Mw / Mn) represented by the ratio of Mw to the number average molecular weight (Mn) in terms of polystyrene measured by GPC is preferably 7 or less, and more preferably 5 or less. In addition, when preparing a liquid crystal alignment agent, the polymer [P] may be used alone or in combination of two or more.
[0118] The liquid crystal aligning agent of the present disclosure may also contain polymers other than polymer [P] (hereinafter also referred to as "other polymers") as polymer components. As long as other polymers do not have a specific structure, there is no particular limitation on the main skeleton. As other polymers, for example, polymers with structural units of polymers such as polyamic acid, polyamic acid ester, polyimide, polysiloxane, polyester, polyenamine, polyurea, polyamide, polyamideimide, polybenzoxazole precursor, polybenzoxazole, cellulose derivatives, polyacetals, and monomers containing polymerizable unsaturated bonds as the main skeleton can be cited.
[0119] For example, when polymer [P] is at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide, polyorganosiloxane may be deployed as other polymers. In this case, functional functional groups such as photo-alignment groups or pretilt angle imparting groups are introduced into the side chains of polyorganosiloxane so that they are included in the liquid crystal alignment agent together with polymer [P], thereby the functional functional groups possessed by polyorganosiloxane can be used to impart the desired characteristics to the liquid crystal alignment film. In the case of containing other polymers in the liquid crystal alignment agent, the content of other polymers is preferably 30% by mass or less, more preferably 20% by mass or less, relative to the total amount of polymer [P] and other polymers. Other polymers can be used alone or in combination of two or more.
[0120] Solvent composition
[0121] The liquid crystal aligning agent disclosed herein contains a cyclic carbonate compound and a dialkylene glycol monoalkyl ether. By using the cyclic carbonate compound and the dialkylene glycol monoalkyl ether in combination as the solvent component of the liquid crystal aligning agent containing the polymer [P], a liquid crystal aligning agent showing good coating properties can be obtained, and a liquid crystal element with a sufficiently high voltage holding rate can be obtained.
[0122] <Cyclic carbonate compounds>
[0123] The cyclic carbonate compound may be any compound having a carbonate structure (-O-CO-O-) in the ring skeleton, and the number of ring members and the presence or absence of substituents are not particularly limited. As the cyclic carbonate compound, a compound represented by the following formula (2) can be preferably used.
[0124] [Chemistry 15]
[0125]
[0126] (In formula (2), R 3 ~R 6 are each independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 5 carbon atoms. n is an integer of 1 to 5. When n is 2 or more, the plurality of R 5 and multiple R6 Each independently has the above definition.)
[0127] In the formula (2), R 3 ~R 6 The monovalent hydrocarbon group having 1 to 5 carbon atoms is preferably a monovalent straight-chain or branched hydrocarbon group having 1 to 5 carbon atoms. Specific examples thereof include alkyl groups having 1 to 5 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and n-pentyl; alkenyl groups having 2 to 5 carbon atoms, such as vinyl and allyl; and alkynyl groups having 2 to 5 carbon atoms, such as ethynyl and prop-2-yn-1-yl.
[0128] R 3 ~R 6 It is preferably a hydrogen atom or a chain hydrocarbon group having 1 to 3 carbon atoms, more preferably a hydrogen atom or a chain hydrocarbon group having 1 or 2 carbon atoms, and still more preferably a hydrogen atom, a methyl group, an ethyl group or a vinyl group.
[0129] n is preferably 1 to 4, more preferably 1 to 3, and even more preferably 1 or 2.
[0130] In the compound represented by the formula (2), the number of substituents on the ring portion (i.e., R 3 ~R 6 The number of the monovalent hydrocarbon groups having 1 to 5 carbon atoms in the moiety is preferably 0 to 3, more preferably 0 to 2.
[0131] As the specific example of cyclic carbonate compound, can be listed: ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, vinyl ethylene carbonate, 4-propyl-1,3-dioxolane-2-one, 1,3-dioxane-2-one, 4-methyl-1,3-dioxane-2-one, 4-ethyl-1,3-dioxane-2-one, 4,6-dimethyl-1,3-dioxane-2-one etc.As cyclic carbonate compound, can use one alone, can also use two or more in combination.Among them, as cyclic carbonate compound, preferably be selected from at least one of the group consisting of ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, 2,3-butylene carbonate, vinyl ethylene carbonate and 1,3-dioxane-2-one.
[0132] In liquid crystal aligning agent, with respect to the viewpoint of the electrical characteristic of the coating property and liquid crystal cell that improves liquid crystal aligning agent with good balance, relative to the total amount of the solvent contained in liquid crystal aligning agent, the containing ratio of cyclic carbonate compound is preferably more than 0.5 mass %.The containing ratio of cyclic carbonate compound is more preferably more than 2 mass %, and then preferably more than 3 mass %, and particularly preferably more than 5 mass %.In addition, with respect to described viewpoint, the containing ratio of cyclic carbonate compound is preferably less than 50 mass %, more preferably less than 40 mass %, and then preferably less than 30 mass %, and particularly preferably less than 20 mass %.
[0133] <Dialkyl glycol monoalkyl ether>
[0134] The dialkylene glycol monoalkyl ether can be represented by the following formula (3).
[0135] [Chemistry 16]
[0136]
[0137] (In formula (3), R 7 is an alkyl group having 1 to 4 carbon atoms. a1 and a2 are each independently an integer of 1 to 4.
[0138] In the formula (3), R 7 It is preferably a linear alkyl group, and particularly preferably a linear alkyl group having 1 to 3 carbon atoms. a1 and a2 are preferably 1 to 3, and more preferably 2 or 3.
[0139] Specific examples of dialkylene glycol monoalkyl ethers include dimethylene glycol monomethyl ether, dimethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol mono-n-butyl ether, etc. In addition, as dialkylene glycol monoalkyl ethers, one kind may be used alone or two or more kinds may be used in combination.
[0140] In the liquid crystal alignment agent, from the viewpoint of improving the coating property of the liquid crystal alignment agent and the electrical characteristics of the liquid crystal cell with good balance, the content ratio of dialkyl glycol monoalkyl ether is preferably 1% by mass or more relative to the total amount of the solvent contained in the liquid crystal alignment agent. The content ratio of dialkyl glycol monoalkyl ether is more preferably 5% by mass or more, and further preferably 10% by mass or more, and particularly preferably 15% by mass or more. In addition, from the viewpoint, the content ratio of dialkyl glycol monoalkyl ether is preferably 70% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less, and particularly preferably 40% by mass or less.
[0141] <Dialkyl glycol dialkyl ether>
[0142] The liquid crystal aligning agent disclosed herein preferably contains a cyclic carbonate compound and a dialkylene glycol monoalkyl ether and a dialkylene glycol dialkyl ether. By using a dialkylene glycol dialkyl ether in combination, the coating property (printability) of the liquid crystal aligning agent can be made more excellent. In addition, the effect of suppressing the intermixing (intermixing) of the lower layer of the liquid crystal aligning film is high, and the electrical properties of the obtained liquid crystal element can be made excellent, which is suitable in this respect. The dialkylene glycol dialkyl ether can be represented by the following formula (4).
[0143] [Chemistry 17]
[0144]
[0145] (In formula (4), R 8 and R 9 b1 and b2 are each independently an integer of 1 to 4.
[0146] In the formula (4), R 8 and R 9 b1 and b2 are preferably 1 to 3, more preferably 2 or 3.
[0147] Specific examples of dialkyl glycol dialkyl ethers include dimethylene glycol dimethyl ether, dimethylene diethyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, dipropylene glycol dimethyl ether, dipropylene glycol methyl ethyl ether, dipropylene glycol diethyl ether, dipropylene glycol dipropyl ether, and dipropylene glycol di-n-butyl ether. In addition, as dialkyl glycol dialkyl ethers, one kind may be used alone or two or more kinds may be used in combination.
[0148] From the viewpoint of improving the coating property of the liquid crystal alignment agent and the electrical characteristics of the liquid crystal cell with good balance, the content ratio of dialkyl glycol dialkyl ether is preferably 1% by mass or more relative to the total amount of the solvent contained in the liquid crystal alignment agent. The content ratio of dialkyl glycol dialkyl ether is more preferably 5% by mass or more, and further preferably 10% by mass or more, and particularly preferably 15% by mass or more. In addition, from the viewpoint, the content ratio of dialkyl glycol dialkyl ether is preferably 70% by mass or less, more preferably 60% by mass or less, and further preferably 50% by mass or less, and particularly preferably 40% by mass or less.
[0149] When a dialkylene glycol monoalkyl ether and a dialkylene glycol dialkyl ether are used as the solvent component, the ratio (D1 / D2) of the dialkylene glycol monoalkyl ether (D1) to the dialkylene glycol dialkyl ether (D2) is preferably in the range of 80 / 20 to 20 / 80, more preferably in the range of 70 / 30 to 30 / 70, further preferably in the range of 65 / 35 to 35 / 65, and particularly preferably in the range of 60 / 40 to 40 / 60 in terms of mass ratio, from the viewpoint of further enhancing the effect of improving the coating properties.
[0150] As solvent, only cyclic carbonate compounds and dialkylene glycol monoalkyl ethers can be used, or only cyclic carbonate compounds, dialkylene glycol monoalkyl ethers and dialkylene glycol dialkyl ethers can be used, but solvents different from cyclic carbonate compounds, dialkylene glycol monoalkyl ethers and dialkylene glycol dialkyl ethers (hereinafter also referred to as "other solvents") can also be further contained in their mixed solvents. As other solvents, the known solvents used in the preparation of liquid crystal aligning agents can be used. As the specific example of other solvents, solvents (hereinafter also referred to as "the first solvent") and solvents (hereinafter also referred to as "the second solvent") with good wetting and expansibility can be listed that can improve the solubility and leveling properties of polymers.
[0151] Specific examples of the first solvent include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 4-hydroxy-4-methyl-2-pentanone, diisobutyl ketone, 1,3-dimethyl-2-imidazolidinone, etc.;
[0152] The second solvent may include alcohol solvents such as methanol, ethanol, propanol, butanol, pentanol, 3-methyl-1-butanol, 1-hexanol, 2-hexanol, heptanol, phenol, cyclohexanol, methylcyclohexanol, diacetone alcohol, propane-1,2-diol, and 3-methoxy-1-butanol;
[0153] Ether solvents such as ethylene glycol monomethyl ether, ethylene glycol monobutyl ether (butyl cellosolve), propylene glycol monobutyl ether, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol n-propyl ether, ethylene glycol isopropyl ether, ethylene glycol dimethyl ether, propylene glycol monomethyl ether (PGME), and diisoamyl ether;
[0154] Ester solvents such as methyl acetate, ethyl acetate, propyl acetate, n-butyl acetate, isobutyl acetate, sec-butyl acetate, tert-butyl acetate, 3-methoxybutyl acetate, methyl acetoacetate, ethyl acetoacetate, ethyl propionate, n-butyl propionate, methyl lactate, ethyl lactate, n-butyl lactate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol ethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol diethyl ether acetate, propylene glycol monomethyl ether acetate (PGMEA), isopentyl propionate, isopentyl isobutyrate, and propylene glycol diacetate;
[0155] Ketone solvents such as acetone, methyl ethyl ketone, methyl n-propyl ketone, methyl n-butyl ketone, diethyl ketone, di-n-butyl ketone, methyl isobutyl ketone, methyl n-amyl ketone, ethyl n-butyl ketone, methyl n-hexyl ketone, diisobutyl ketone, trimethyl nonanone, cyclobutanone, cyclopentanone, cyclohexanone, and cycloheptanone. In addition, as other solvents, one kind may be used alone, or two or more kinds may be used in combination.
[0156] Among the solvents, as other solvents, it is preferred to use at least one selected from the group consisting of alcoholic solvents and ether solvents. In addition, from the perspective of heating during film formation at low temperatures as much as possible, the liquid crystal alignment agent of the present disclosure is preferably substantially free of the first solvent. Specifically, relative to the total amount of the solvent contained in the liquid crystal alignment agent, the first solvent content is preferably 5% by mass or less, more preferably 1% by mass or less, and further preferably 0.5% by mass or less, and particularly preferably 0% by mass.
[0157] When other solvents are used as solvents, the content ratio of other solvents relative to the total amount of solvents contained in the liquid crystal alignment agent (the total amount when two or more solvents are used) is preferably 90 mass % or less, more preferably 80 mass % or less, further preferably 70 mass % or less, further more preferably 60 mass % or less, and particularly preferably 50 mass % or less.
[0158] 《Other ingredients》
[0159] The liquid crystal aligning agent may contain other components as needed, in addition to the polymer component and the solvent component.
[0160] <Compounds containing a cross-linkable group>
[0161] The liquid crystal alignment agent of the present disclosure may further include a compound having a crosslinking group (hereinafter also referred to as a "compound containing a crosslinking group"). If a compound containing a crosslinking group is included, a liquid crystal element with better electrical properties can be obtained, which is suitable in this respect. As the crosslinking group possessed by the compound containing a crosslinking group, it is preferably a compound having at least one selected from the group consisting of a cyclic ether group, a cyclic carbonate group, an isocyanate group, a protected isocyanate group, an oxazoline group, a β-hydroxyalkylamide group, a Meldrum'sacid group, a hydroxymethyl group and an alkylhydroxymethyl group and a molecular weight of 1000 or less. The number of crosslinking groups possessed by one molecule of the compound containing a crosslinking group is preferably two or more, more preferably three or more. Among them, the compound containing a crosslinking group is preferably a compound having at least one selected from the group consisting of a cyclic ether group, a protected isocyanate group, a β-hydroxyalkylamide group, a hydroxymethyl group and an alkylhydroxymethyl group, and more preferably a compound having at least one selected from the group consisting of a protected isocyanate group, a β-hydroxyalkylamide group, a hydroxymethyl group and an alkylhydroxymethyl group.
[0162] Specific examples of the crosslinkable group-containing compound include compounds having a cyclic ether group, such as ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, N,N,N',N'-tetraglycidyl-m-xylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N-diglycidyl-benzylamine, N,N-diglycidyl-aminomethylcyclohexane, and N,N-diglycidyl-cyclohexylamine. Examples of the compound having a cyclic carbonate group include N,N,N',N'-tetrakis[(2-oxo-1,3-dioxolan-4-yl)ethyl]-4,4'-diaminodiphenylmethane.
[0163] Examples of the compound having an isocyanate group or a protected isocyanate group include toluene diisocyanate, xylene diisocyanate, chlorophenylene diisocyanate, hexamethylene diisocyanate, tetramethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, and protected isocyanate compounds obtained by protecting these polyisocyanates with a protecting group; examples of the compound having an oxazoline group include 2,2'-bis(4-propyl-2-oxazoline), 2,2'-bis(4-phenyl-2-oxazoline), 1,2-bis(2-oxazolin-2-yl)ethane, 1,4-bis(2-oxazolin-2-yl)cyclohexane, 1,3-bis(2-oxazolin-2-yl)benzene, 1,3 -bis(4,5-dihydro-2-oxazolyl)benzene, 1,3-bis(4-methyl-2-oxazolin-2-yl)benzene, etc.; compounds having a β-hydroxyalkylamide group include, for example, N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide, etc.; compounds having a hydroxymethyl group or an alkylhydroxymethyl group include, for example, trimethylolpropane, bis[2-ethyl-2,2-bis(hydroxymethyl)ethyl]ether, 2,2'-[oxybis(methylene)]bis[2-ethyl-1,3-propanediol], 2,2-bis(4-hydroxymethylphenyl)propane, 2,2-bis(2,3,4-trihydroxymethylphenyl)propane, 2,4,6-tris[bis(methoxymethyl)amino]-1,3,5-triazine, etc. As the crosslinking group-containing compound, one kind may be used alone, or two or more kinds may be used in combination.
[0164] In the case of using a compound containing a crosslinking group, from the viewpoint of forming a stable liquid crystal alignment film and further improving the effect of improving the electrical properties of the obtained liquid crystal element, the content ratio of the compound containing a crosslinking group in the liquid crystal alignment agent is preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, relative to the total amount of 100 parts by mass of the polymer [P]. In addition, from the viewpoint of suppressing the performance degradation caused by excessive addition, the content ratio of the compound containing a crosslinking group is preferably 40 parts by mass or less, and more preferably 30 parts by mass or less, relative to the total amount of 100 parts by mass of the polymer component in the liquid crystal alignment agent. In addition, as a compound containing a crosslinking group, one may be used alone or two or more may be used in combination.
[0165] As other components contained in the liquid crystal alignment agent, not only the above compounds can be listed, but also antioxidants, metal chelate compounds, curing accelerators, surfactants, fillers, dispersants, photosensitizers, etc. The proportion of other components can be appropriately selected according to each compound within the range that does not damage the effect of the present invention.
[0166] The solid content concentration in the liquid crystal aligning agent (the total mass of the components of the liquid crystal aligning agent other than the solvent accounts for the total mass of the liquid crystal aligning agent) is appropriately selected in consideration of viscosity, volatility, etc., preferably in the range of 1% to 10% by mass. If the solid content concentration is 1% by mass or more, the film thickness of the coating can be fully ensured, and it is easy to obtain a liquid crystal alignment film showing good liquid crystal orientation. On the other hand, if the solid content concentration is 10% by mass or less, the coating can be made into a moderate thickness, and it is easy to obtain a liquid crystal alignment film showing good liquid crystal orientation. In addition, the viscosity of the liquid crystal aligning agent becomes moderate, and there is a tendency to make the coating property good.
[0167] 《Liquid crystal alignment film and liquid crystal element》
[0168] The liquid crystal alignment film of the present invention is formed by a liquid crystal alignment agent prepared in the manner described above. In addition, the liquid crystal element of the present invention includes a liquid crystal alignment film formed using the liquid crystal alignment agent described above. The operating mode of the liquid crystal in the liquid crystal element is not particularly limited, for example, it can be applied to twisted nematic (TN) type, super twisted nematic (STN) type, vertical alignment (VA) type (including vertical alignment-multi-domain vertical alignment (VA-MVA) type, vertical alignment-patterned vertical alignment (VA-PVA) type, etc.), in-plane switching (IPS) type, fringe field switching (FFS) type, optically compensated bend (OCB) type, polymer stabilized alignment (PSA) type and other modes. The liquid crystal element can be manufactured, for example, by a method including the following steps 1 to 3. Regarding step 1, different substrates are used depending on the desired operation mode. Steps 2 and 3 are common to each operation mode.
[0169] <Step 1: Formation of coating film>
[0170] First, a liquid crystal alignment agent is applied to a substrate, and the applied surface is preferably heated to form a coating film on the substrate. As a substrate, for example, glass such as float glass and soda glass can be used; a transparent substrate containing plastics such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, and poly(alicyclic olefin). As a transparent conductive film disposed on one side of the substrate, a NESA film (registered trademark of PPG, USA) containing tin oxide (SnO2) and an indium tin oxide (indium tin oxide, ITO) film containing indium oxide-tin oxide (In2O3-SnO2) can be used. In the case of manufacturing a TN type, STN type or VA type liquid crystal element, two substrates provided with a patterned transparent conductive film are used. On the other hand, in the case of manufacturing an IPS type or FFS type liquid crystal element, a substrate provided with electrodes patterned into a comb-tooth shape and an opposing substrate without an electrode are used.
[0171] The method for coating the liquid crystal alignment agent on the substrate is not particularly limited, and can be carried out by, for example, spin coating, printing (for example, offset printing, flexographic printing, etc.), inkjet, slit coating, rod coater, extrusion die, direct gravure coater, chamber doctor coater, offset gravure coater, impregnation coater, MB coater, etc.
[0172] After applying the liquid crystal alignment agent, it is preferred to perform preheating (prebaking) for the purpose of preventing the applied liquid crystal alignment agent from sagging. The prebaking temperature is preferably 30°C to 200°C, and the prebaking time is preferably 0.25 minutes to 10 minutes. Thereafter, the solvent is completely removed, and a calcination (post-baking) process is performed as needed for the purpose of thermal imidization of the amide acid structure present in the polymer. The calcination temperature (post-baking temperature) at this time is preferably 80°C to 280°C, and more preferably 80°C to 250°C. The post-baking time is preferably 5 minutes to 200 minutes. The film thickness of the formed film is preferably 0.001μm to 1μm.
[0173] <Step 2: Orientation treatment>
[0174] In the case of manufacturing TN type, STN type, IPS type or FFS type liquid crystal elements, the coating formed in the process 1 is subjected to a process (orientation treatment) of imparting liquid crystal orientation ability. Thus, the orientation ability of the liquid crystal molecules is imparted to the coating to form a liquid crystal orientation film. As an orientation treatment, it is preferred to use a friction treatment in which the surface of the coating formed on the substrate is wiped with cotton wool or the like, or to irradiate the coating with light to impart a light orientation treatment of liquid crystal orientation ability. On the other hand, in the case of manufacturing a vertically oriented liquid crystal element, the coating formed in the process 1 can be directly used as a liquid crystal orientation film, or the coating can be subjected to an orientation treatment in order to further improve the liquid crystal orientation ability.
[0175] Light irradiation for photo-orientation can be carried out by the following methods: a method of irradiating the coating after the post-baking process; a method of irradiating the coating after the pre-baking process and before the post-baking process; a method of irradiating the coating during the heating process of the coating in at least any one of the pre-baking process and the post-baking process, etc. As radiation irradiated to the coating, for example: ultraviolet rays and visible light containing light with a wavelength of 150nm to 800nm can be used. Preferably, ultraviolet rays containing light with a wavelength of 200nm to 400nm are used. In the case where the radiation is polarized, it can be linearly polarized or partially polarized. In the case where the radiation used is linearly polarized or partially polarized, the irradiation can be carried out from a direction perpendicular to the substrate surface, from an oblique direction, or these directions can be combined. The irradiation direction for non-polarized radiation is set to an oblique direction.
[0176] Examples of the light source include a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, and an excimer laser. The radiation dose is preferably 400 J / m 2 ~50,000J / m 2 , more preferably 1,000 J / m 2 ~20,000J / m 2 After irradiation with light for imparting alignment ability, the substrate surface may be cleaned using water, an organic solvent (e.g., methanol, isopropanol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, etc.) or a mixture thereof, or the substrate may be heated.
[0177] <Step 3: Construction of liquid crystal cell>
[0178] Prepare two substrates with liquid crystal alignment films formed in the above manner, and arrange liquid crystal between the two substrates arranged opposite to each other, thereby manufacturing a liquid crystal unit. When manufacturing a liquid crystal unit, for example, the following methods can be listed: arrange the two substrates opposite to each other with a gap in a manner that the liquid crystal alignment films face each other, use a sealant to bond the peripheral portions of the two substrates, and inject the filling liquid crystal into the cell gap surrounded by the substrate surface and the sealant and seal the injection hole; use a method of using a liquid crystal drop (one dropfill, ODF) method, etc. As a sealant, for example, an epoxy resin containing a hardener and alumina balls as a spacer can be used. As liquid crystals, nematic liquid crystals and discotic liquid crystals can be listed, among which nematic liquid crystals are preferred.
[0179] In the PSA mode, the following treatment is performed: a liquid crystal and a polymerizable compound (e.g., a multifunctional (meth)acrylate compound, etc.) are filled into a cell gap together, and after constructing a liquid crystal cell, a voltage is applied between conductive films on a pair of substrates, and the liquid crystal cell is irradiated with light. When a liquid crystal element of the PSA mode is manufactured, the polymerizable compound is used in an amount of 0.01 to 3 parts by mass, preferably 0.1 to 1 part by mass, relative to a total of 100 parts by mass of the liquid crystal.
[0180] When the liquid crystal element is used as a display device, a polarizing plate is then attached to the outer surface of the liquid crystal unit as needed to prepare the liquid crystal element. Examples of the polarizing plate include a polarizing plate formed by sandwiching a polarizing film called "H film" between cellulose acetate protective films, or a polarizing plate including the H film itself, wherein the H film is formed by absorbing iodine while stretching and orienting polyvinyl alcohol.
[0181] The liquid crystal element of the present invention described in detail above can be effectively applied to various purposes. Specifically, for example, it can be used as various display devices or dimming devices, phase difference films, such as clocks, portable game consoles, word processors, notebook personal computers, car navigation systems, camcorders, personal digital assistants (PDAs), digital cameras, mobile phones, smart phones, various monitors, liquid crystal televisions, information displays, etc.
[0182] [Example]
[0183] Hereinafter, the embodiment will be described in more detail based on examples, but the present invention is not to be construed as being limitative by the following examples.
[0184] In the following examples, the weight average molecular weight Mw of the polymer, the imidization ratio of the polyimide in the polymer solution, the solution viscosity of the polymer solution, and the epoxy equivalent are measured by the following methods. The necessary amounts of the raw material compounds and polymers used in the following examples are ensured by repeatedly performing the synthesis under the synthesis scale shown in the following synthesis examples as needed.
[0185] [Weight average molecular weight Mw of polymer]
[0186] The weight average molecular weight Mw is a polystyrene-equivalent value measured by GPC under the following conditions.
[0187] Column: Made by Tosoh Corporation, TSKgelGRCXLII
[0188] Solvent: Tetrahydrofuran (polyorganosiloxane, binder resin)
[0189] N,N-dimethylformamide solution containing lithium bromide and phosphoric acid (polyamic acid)
[0190] Temperature: 40℃
[0191] Pressure: 68kgf / cm 2
[0192] [Imidization ratio of polyimide]
[0193] The polyimide solution was poured into pure water, the obtained precipitate was fully dried under reduced pressure at room temperature, and then dissolved in deuterated dimethyl sulfoxide. The hydrogen nuclear magnetic resonance (HNMR) spectra were measured at room temperature using tetramethylsilane as a reference substance. 1 H-nuclear magnetic resonance, 1 H-NMR). According to the obtained 1 The imidization ratio [%] was determined from the H-NMR spectrum using the following formula (1).
[0194] Imidization rate [%] = (1-(A 1 / (A 2 ×α)))×100…(1)
[0195] (In equation (1), A 1 A is the peak area of protons originating from NH groups appearing near the chemical shift of 10 ppm. 2 is the peak area derived from other protons, and α is the ratio of the number of other protons to one proton of the NH group in the polymer precursor (polyamic acid).
[0196] [Solution viscosity of polymer solution]
[0197] The solution viscosity (mPa·s) of the polymer solution was measured at 25° C. using an E-type rotational viscometer.
[0198] [Epoxy equivalent]
[0199] The epoxy equivalent is measured by the hydrochloric acid-methyl ethyl ketone method described in Japanese Industrial Standards (JIS) C 2105.
[0200] The abbreviations of the compounds are as follows: In addition, hereinafter, the compound represented by the formula (X) may be simply referred to as "compound (X)".
[0201] [Chemistry 18]
[0202]
[0203] [Chemistry 19]
[0204]
[0205] [Chemistry 20]
[0206]
[0207] [Chemistry 21]
[0208]
[0209] [Chemistry 22]
[0210]
[0211] [Chemistry 23]
[0212]
[0213] <Polymer Synthesis>
[0214] 1. Synthesis of polyamic acid
[0215] [Synthesis example 1]
[0216] 100 mol parts of 2,3,5-tricarboxycyclopentylacetic dianhydride (tc-1) as a tetracarboxylic dianhydride, 20 mol parts of cholesteryloxy-2,4-diaminobenzene (da-13) as a diamine, 40 mol parts of compound (da-2), and 40 mol parts of 4,4'-diaminobenzanilide (da-1) were dissolved in N-methyl-2-pyrrolidone (NMP), and reacted at 60°C for 6 hours to obtain a solution containing 30% by mass of polyamic acid. A small amount of the obtained polyamic acid solution was taken, and NMP was added to prepare a solution with a polyamic acid concentration of 20% by mass. The solution viscosity measured as this solution was 800 mPa·s. Subsequently, the reaction solution was injected into a large amount of excess methanol to precipitate the reaction product. The precipitate was washed with methanol and dried at 40°C for 15 hours under reduced pressure to obtain a polymer (PAA-1).
[0217] [Synthesis Example 2 to Synthesis Example 6]
[0218] Except having changed the kind and amount of the tetracarboxylic dianhydride and the diamine used as described in the following Table 1, the same operation as in Synthesis Example 1 was carried out to obtain polyamic acids (polymers (PAA-2) to (PAA-6)).
[0219] 2. Synthesis of polyimide
[0220] [Synthesis Example 7]
[0221] 100 mol parts of 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride (tc-2) as tetracarboxylic dianhydride, 30 mol parts of compound (da-14) as diamine, and 70 mol of 3,5-diaminobenzoic acid (da-16) were dissolved in NMP, and reacted at 60°C for 6 hours to obtain a solution containing 30% by mass of polyamic acid. A small amount of the obtained polyamic acid solution was taken, and NMP was added to prepare a solution with a polyamic acid concentration of 20% by mass. The solution viscosity measured as this solution was 800 mPa·s.
[0222] Then, NMP was added to the obtained polyamic acid solution to prepare a solution with a polyamic acid concentration of 7% by mass, and pyridine and acetic anhydride were added to carry out a dehydration ring-closure reaction at 110°C for 4 hours. After the dehydration ring-closure reaction, the solvent in the system was replaced with new NMP to obtain a solution containing 26% by mass of a polyimide (referred to as "polymer (PI-1)") with an imidization rate of about 80%. A small amount of the obtained polyimide solution was taken, and NMP was added to prepare a solution with a polyimide concentration of 15% by mass, and the solution viscosity measured as this solution was 120mPa·s. Then, the reaction solution was injected into a large amount of excess methanol to precipitate the reaction product. The precipitate was washed with methanol and dried at 40°C under reduced pressure for 15 hours to obtain a polymer (PI-1).
[0223] [Table 1]
[0224]
[0225] 3. Synthesis of epoxy-containing polyorganosiloxane
[0226] [Synthesis example 8]
[0227] In a reaction container including a stirrer, a thermometer, a dropping funnel and a reflux cooling tube, 100.0 g of 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (the compound represented by the formula (es-1)), 500 g of methyl isobutyl ketone and 10.0 g of triethylamine were added and mixed at room temperature. Subsequently, 100 g of deionized water was dripped from the dropping funnel over 30 minutes, and the mixture was reacted at 80°C for 6 hours while stirring under reflux. After the reaction was completed, the organic layer was taken out and washed with a 0.2% by mass aqueous solution of ammonium nitrate until the washed water became neutral, and then the solvent and water were distilled off under reduced pressure to obtain an epoxy-containing polyorganosiloxane (referred to as "polymer (ESSQ-1)") in the form of a viscous transparent liquid. The polymer (ESSQ-1) was subjected to 1 H-NMR analysis revealed that a peak due to epoxy groups was obtained at a chemical shift (δ) of about 3.2 ppm. The weight average molecular weight Mw of the obtained polymer (ESSQ-1) was 3,500, and the epoxy equivalent was 180 g / mol.
[0228] 4. Synthesis of polyorganosiloxane containing specific groups
[0229] [Synthesis Example 9]
[0230] In a 200 mL three-necked flask, 10.0 g of polymer (ESSQ-1), 30.28 g of methyl isobutyl ketone as a solvent, 20 mol% of compound (ca-1) and 10 mol% of compound (ca-2) as a modifying component (carboxylic acid having an oriented group) based on the total amount of epoxy groups in polymer (ESSQ-1), and 0.10 g of UCAT 18X (trade name, manufactured by San-Apro Co., Ltd.) as a catalyst were added, and the mixture was stirred at 100° C. for 48 hours to react. After the reaction was completed, ethyl acetate was added to the reaction mixture, the resulting solution was washed with water three times, the organic layer was dried with magnesium sulfate, and the solvent was distilled off to obtain polymer (PSQ-1). The weight average molecular weight Mw of the obtained polymer was 6,800.
[0231] [Synthesis Example 10]
[0232] A polymer (PSQ-2) was obtained by performing the same operation as in Synthesis Example 9, except that the modifying components used were changed to compound (ca-1) in an amount equivalent to 30 mol % and compound (ca-3) in an amount equivalent to 10 mol % relative to the total amount of epoxy groups possessed by the polymer (ESSQ-1).
[0233] [Example 1]
[0234] 1. Preparation of Liquid Crystal Alignment Agent
[0235] Propylene carbonate (PC), diethylene glycol monomethyl ether (B1), diethylene glycol dimethyl ether (C1), and 3-methoxybutanol (MB) were added to 100 parts by mass of the polymer (PAA-1) obtained in Synthesis Example 1 and 5 parts by mass of the polymer (PSQ-1) obtained in Synthesis Example 9 to prepare a solution having a solid content concentration of 4.0% by mass and a solvent mixing ratio of PC: B1: C1: MB = 15: 20: 30: 35 (mass ratio). After the solution was fully stirred, it was filtered using a filter with a pore size of 0.2 μm to prepare a liquid crystal aligning agent (S-1).
[0236] 2. Preparation of Coloring Composition
[0237] (1) Preparation of pigment dispersion
[0238] A pigment dispersion (a-1) was prepared by treating with a bead mill using 15 parts by mass of Color Index (CI) Pigment Blue 15:6 as a colorant, 12.5 parts by mass of BYK-LPN21116 (manufactured by BYK) as a dispersant (solid content concentration: 40% by mass), and 72.5 parts by mass of propylene glycol monomethyl ether acetate as a solvent.
[0239] (2) Preparation of dye solution
[0240] 5 parts by mass of a colorant represented by the following formula (A-1) and 95 parts by mass of cyclohexanone as a solvent were mixed to prepare a dye solution (A-1). In addition, the compound represented by the following formula (A-1) was obtained by the method described in Synthesis Example 3 of Japanese Patent Laid-Open No. 2013-122577.
[0241] [Chemistry 24]
[0242]
[0243] (3) Synthesis of binder resin
[0244] 100 parts by mass of propylene glycol monomethyl ether acetate was added to a flask including a cooling tube and a stirrer and purged with nitrogen. The mixture was heated to 80°C, and a mixed solution of 100 parts by mass of propylene glycol monomethyl ether acetate, 20 parts by mass of methacrylic acid, 10 parts by mass of styrene, 5 parts by mass of benzyl methacrylate, 15 parts by mass of 2-hydroxyethyl methacrylate, 23 parts by mass of 2-ethylhexyl methacrylate, 12 parts by mass of N-phenylmaleimide, 15 parts by mass of mono(2-acryloyloxyethyl)succinate, and 6 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) was added dropwise over 1 hour at this temperature, and polymerization was performed for 2 hours while maintaining the temperature. Thereafter, the temperature of the reaction solution was raised to 100°C, and polymerization was performed for further 1 hour, thereby obtaining a solution containing a binder resin (B1) (solid content concentration 33% by mass, hereinafter referred to as "binder resin (B1) solution"). The obtained binder resin had Mw of 12,200 and Mn of 6,500.
[0245] (4) Preparation of coloring composition
[0246] 46.0 parts by mass of the pigment dispersion (a-1), 24.3 parts by mass of the dye solution (A-1), 24.6 parts by mass of the binder resin (B1) solution, 7.1 parts by mass of M-402 (a mixture of dipentaerythritol hexaacrylate and dipentaerythritol pentaacrylate) manufactured by Toagosei Co., Ltd. as a crosslinking agent, 2.1 parts by mass of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one (manufactured by Ciba Specialty Chemicals, trade name IRGACURE 369) as a photopolymerization initiator, 0.05 parts by mass of Megafac F-554 (manufactured by DIC Corporation) as a surfactant, and ethyl lactate as a solvent were mixed to prepare a coloring composition (G-1) having a solid content concentration of 20% by mass.
[0247] 3. Formation of colored hardened film
[0248] After the coloring composition (G-1) was applied to a glass substrate using a spin coater, it was pre-baked for 100 seconds using a 90°C hot plate to form a coating. In addition, during coating, the rotation speed of the spin coater was adjusted so that the film thickness after baking was 2.5 μm. Then, after the substrate was cooled to room temperature, a high-pressure mercury lamp was used to pattern the electrode portion for measurement, and radiation with wavelengths of 365 nm, 405 nm, and 436 nm was used at 400 J / m 2 The coating film was exposed to an exposure amount of . Thereafter, a developer containing a 0.04 mass % potassium hydroxide aqueous solution at 23°C was sprayed on the substrate under the conditions of a development pressure of 110 kPa and a developer flow rate of 1.2 liters / minute for a time equivalent to 1.5 times the time until the film of the unexposed part disappears and the substrate surface is seen, thereby performing spray development. Thereafter, the substrate was washed with ultrapure water and air-dried, and then further baked in a clean oven at 230°C for 20 minutes to form a colored cured film (film thickness 2.5 μm). An ITO film (film thickness 50 nm) was formed on the obtained colored cured film by sputtering.
[0249] 4.Manufacturing of vertical liquid crystal display elements
[0250] On the transparent electrode surface of the glass substrate with a transparent electrode including the laminated film of the colored cured film and the ITO film obtained in 3. above, the liquid crystal alignment agent (S-1) prepared in 1. above was applied using a spinner, and pre-baked on a hot plate at 80°C for 1 minute. Thereafter, in an oven in which the inside of the box was substituted with nitrogen, it was heated at 230°C for 1 hour to form a coating film with a film thickness of 0.1 μm. Subsequently, the same operation was repeated to prepare a pair (two sheets) of substrates having a colored cured film, an ITO film, and a liquid crystal alignment film.
[0251] On the periphery of the surface with a liquid crystal alignment film of one of the substrates, an epoxy resin adhesive with alumina balls of 3.5 μm in diameter is applied by screen printing, and then the liquid crystal alignment film surfaces of a pair of substrates are made to face each other, and the optical axes of the ultraviolet rays of each substrate are pressed in a manner that is antiparallel to the projection direction of the substrate surface, and the adhesive is thermally cured at 150°C for 1 hour. Then, after negative liquid crystal (Merck, MLC-6608) is filled into the gap between the substrates from the liquid crystal injection port, the liquid crystal injection port is sealed with an epoxy adhesive. Furthermore, in order to remove the flow orientation during liquid crystal injection, it is heated at 130°C and then slowly cooled to room temperature to manufacture a liquid crystal display element.
[0252] 5. Evaluation of electrical properties
[0253] After the produced liquid crystal display element was placed in an oven at 60°C, the VHR was measured using a VHR measuring device manufactured by Toyo Technica under the conditions of 1V and 167msec. As an evaluation standard, when the VHR is less than 100% and higher than 98%, it is set to "◎", when it is less than 98% and higher than 95%, it is set to "○", when it is less than 95% and higher than 90%, it is set to "△", and when it is less than 90%, it is set to "×". In addition, it can be said that the higher the VHR, the more it can suppress the reduction of electrical properties caused by the solvent in the liquid crystal alignment agent penetrating into the lower layer (specifically, the colored cured film), and thus the better. As a result, the VHR was 92.0%, which was evaluated as "△".
[0254] 6. Evaluation of coating properties (printing properties)
[0255] Liquid crystal alignment agent (S-1) was filled in an inkjet device manufactured by Shibaura, and inkjet coating was performed on a silicon wafer. Then, pre-baking was performed on a hot plate at 80°C for 1 minute. Thereafter, heating was performed at 230°C for 1 hour in an oven purged with nitrogen to form a film with a thickness of 0.1 μm and a coating area of 100 cm. 2 (=10cm×10cm) of the coating film. For a distance of 1mm in the center of the coating film, the Alpha-Step is used to measure the uniformity of the film thickness along the direction orthogonal to the direction of travel of the inkjet head. The difference between the maximum film thickness and the minimum film thickness of the obtained film thickness profile is defined as the roughness to judge the quality of the printability. As an evaluation standard, when the roughness is greater than 0 and less than 2nm, it is set to "◎", when it is greater than 2nm and less than 5nm, it is set to "○", when it is greater than 5nm and less than 10nm, it is set to "△", and when it is greater than 10nm, it is set to "×". As a result, the roughness was 0.7nm, which was evaluated as "◎".
[0256] [Examples 3 to 6, 8, 10 and Comparative Examples 1 to 4]
[0257] The liquid crystal alignment agent was prepared in the same manner as in Example 1 except that the composition of the liquid crystal alignment agent was changed as shown in Table 2 below. In addition, a vertical liquid crystal display element was manufactured in the same manner as in Example 1 using the obtained liquid crystal alignment agent, and electrical properties and coating properties were evaluated. The results are shown in Table 3 below.
[0258] [Example 7]
[0259] 1. Preparation of Liquid Crystal Alignment Agent
[0260] Except changing the preparation prescription as described in the following Table 2, it carried out similarly to Example 1, and prepared a liquid crystal aligning agent (S-7).
[0261] 2. Fabrication and evaluation of vertical light-type liquid crystal display elements
[0262] The composition of the liquid crystal alignment agent was changed as shown in Table 2 below. In the same manner as in Example 1, the liquid crystal alignment agent was applied by a spinner on the transparent electrode surface of the glass substrate with a transparent electrode including a laminated film of a colored cured film and an ITO film, and pre-baking and post-baking were performed to form a coating film. Subsequently, the coating film surface was irradiated with 1,000 J / m2 of polarized ultraviolet light containing a bright line of 313 nm from a direction inclined at 40° relative to the normal line of the substrate using a Hg-Xe lamp and a Glan Taylor prism. 2 The same operation is repeated to prepare a pair (two sheets) of substrates having a colored hardened film, an ITO film and a liquid crystal alignment film.
[0263] On the periphery of the surface with a liquid crystal orientation film of one of the substrates, an epoxy resin adhesive with a diameter of 3.5 μm of alumina balls is applied by screen printing, and then the liquid crystal orientation film surfaces of a pair of substrates are made to face each other, and the optical axis of the ultraviolet rays of each substrate is pressed in a manner that is antiparallel to the projection direction of the substrate surface, and the adhesive is thermally cured at 150°C for 1 hour. Then, after filling the negative liquid crystal (Merck, MLC-6608) into the gap between the substrates from the liquid crystal injection port, the liquid crystal injection port is sealed with an epoxy adhesive. Furthermore, in order to remove the flow orientation during liquid crystal injection, it is heated at 130°C and then slowly cooled to room temperature to manufacture a liquid crystal display element. In addition, for the obtained liquid crystal display element, the electrical properties and coating properties are evaluated in the same manner as in Example 1. The evaluation results are shown in Table 3 below.
[0264] [Example 2]
[0265] 1. Preparation of Liquid Crystal Alignment Agent
[0266] Except changing the preparation prescription as described in the following Table 2, it carried out similarly to Example 1, and prepared a liquid crystal aligning agent (S-2).
[0267] 2. Preparation of Liquid Crystal Composition
[0268] To 10 g of nematic liquid crystal (MLC-6608, manufactured by Merck), 5% by mass of a liquid crystal compound represented by the following formula (L1-1) and 0.3% by mass of a photopolymerizable compound represented by the following formula (L2-1) were added and mixed to obtain a liquid crystal composition LC1.
[0269] [Chemistry 25]
[0270]
[0271] 3. Manufacturing of PSA type liquid crystal display elements
[0272] The liquid crystal orientation agent (S-2) prepared in 1. above is applied to the transparent electrode surface of the glass substrate with a transparent electrode of the laminated film including the colored hardened film and the ITO film using a rotator, and pre-baked on a heating plate at 80°C for 1 minute, and then heated at 200°C for 1 hour in an oven replaced with nitrogen to remove the solvent, thereby forming a coating film (liquid crystal orientation film) with a film thickness of 0.08 μm. For this coating film, a friction machine with a roller wound with rayon cloth is used, and the friction treatment is performed at a roller speed of 400 rpm, a platform moving speed of 3 cm / second, and a hair pressing length of 0.1 mm. Thereafter, ultrasonic cleaning is performed in ultrapure water for 1 minute, and then dried in a clean oven at 100°C for 10 minutes, thereby obtaining a substrate with a liquid crystal orientation film. Repeat the above operation to obtain a pair (two pieces) of substrates with a liquid crystal orientation film. In addition, the friction treatment is a weak friction treatment performed for the purpose of controlling the collapse of the liquid crystal and performing orientation segmentation using a simple method.
[0273] An epoxy resin adhesive containing alumina balls with a diameter of 3.5 μm was applied to the periphery of the surface of one of the substrates having a liquid crystal alignment film by screen printing, and then the liquid crystal alignment film surfaces of a pair of substrates were made to face each other, overlapped and pressed, and heated at 150° C. for 1 hour to thermally cure the adhesive. Subsequently, after the liquid crystal composition LC1 was filled into the gap between the substrates from the liquid crystal injection port, the liquid crystal injection port was sealed with an epoxy adhesive, and then, in order to remove the flow orientation during liquid crystal injection, it was heated at 150° C. for 10 minutes and then slowly cooled to room temperature.
[0274] Next, an alternating current of 10 V at a frequency of 60 Hz was applied between the electrodes of the obtained liquid crystal cell, and in a state where the liquid crystal was driven, an ultraviolet irradiation device using a metal halide lamp as a light source was used at a rate of 50,000 J / m 2 The ultraviolet rays were irradiated at an irradiation amount of . In addition, the irradiation amount was a value measured using a light meter measuring at a wavelength of 365 nm. A liquid crystal display element was manufactured by the method.
[0275] 4. Evaluation
[0276] The electrical characteristics and coating properties of the PSA type liquid crystal display element produced above were evaluated in the same manner as in Example 1. The results are shown in Table 3 below.
[0277] [Example 9]
[0278] 1. Preparation of Liquid Crystal Alignment Agent
[0279] Except changing the preparation prescription as described in the following Table 2, it carried out similarly to Example 1, and prepared a liquid crystal aligning agent (S-9).
[0280] 2. Manufacturing of rubbing FFS type liquid crystal display element
[0281] The coloring composition (G-1) is applied to a glass substrate having a flat electrode (bottom electrode), an insulating layer and a comb-shaped electrode (top electrode) stacked in sequence on one side, and to each surface of an opposing glass substrate without an electrode, and the same operation as "3. Formation of a colored cured film" of Example 1 is performed to form a colored cured film. Subsequently, a liquid crystal alignment agent (S-9) is applied to the formation surface side of the colored cured film in each substrate using a spinner, and heated (pre-baked) on a heating plate at 80°C for 1 minute. Thereafter, drying (post-baking) is performed for 1 hour in an oven at 200°C where nitrogen is substituted in the box to form a coating having an average film thickness of 0.08 μm. Subsequently, the surface of the coating is subjected to friction treatment using a friction machine having a roller wound with a rayon cloth, with a roller speed of 500 rpm, a platform moving speed of 3 cm / second, and a hair pressing length of 0.4 mm. Thereafter, ultrasonic cleaning was performed in ultrapure water for 1 minute, and then, drying was performed in a 100° C. clean oven for 10 minutes, thereby obtaining a substrate having a liquid crystal alignment film.
[0282] Then, for a pair of substrates with a liquid crystal orientation film, a liquid crystal injection port is reserved at the edge of the surface where the liquid crystal orientation film is formed, and an epoxy resin adhesive with alumina balls of 5.5 μm in diameter is applied by screen printing. Thereafter, the substrates are overlapped and crimped, and the adhesive is thermally cured at 150°C for 1 hour. Then, after filling the liquid crystal injection port between a pair of substrates with nematic liquid crystal (Merck, MLC-6221), the liquid crystal injection port is sealed with an epoxy adhesive. Furthermore, in order to remove the flow orientation during liquid crystal injection, it is heated at 120°C and then slowly cooled to room temperature to manufacture a liquid crystal unit. In addition, when a pair of substrates are overlapped, the friction method of each substrate is made antiparallel. In addition, for the top electrode, the line width of the electrode is set to 4 μm, and the distance between the electrodes is set to 6 μm. In addition, as the top electrode, 4 systems of driving electrodes of electrode A, electrode B, electrode C and electrode D are used. In this case, the bottom electrode functions as a common electrode acting on all of the four-system driving electrodes, and the regions of the four-system driving electrodes serve as pixel regions.
[0283] 3. Evaluation
[0284] The electrical characteristics and coating properties of the FFS liquid crystal display element produced above were evaluated in the same manner as in Example 1. The results are shown in Table 3 below.
[0285] [Table 2]
[0286]
[0287] In Table 2, the values in brackets of the polymer component and the cross-linking agent represent the blending ratio (parts by mass) of each compound relative to 100 parts by mass of the blending amount of the polymer (PAA-1) to the polymer (PAA-6) and the polymer (PI-1) used in the preparation of the liquid crystal aligning agent. The values in brackets of the solvent composition represent the blending ratio (mass ratio) of each solvent relative to the total amount of the solvent component used in the preparation of the liquid crystal aligning agent. In addition, regarding dialkylene glycol dialkyl ether, the blending ratio is shown in the columns of the base R4 and the base R6.
[0288] The abbreviations of the compounds are as follows.
[0289] <Solvent>
[0290] MB: 3-methoxy-1-butanol
[0291] BC: Ethylene glycol monobutyl ether
[0292] PB: Propylene glycol monobutyl ether
[0293] DAA: diacetone alcohol
[0294] NMP: N-methyl-2-pyrrolidone
[0295] [Table 3]
[0296]
[0297] As is clear from Table 3, in Examples 1 to 10, the roughness of the formed liquid crystal alignment film is small, and the coating (printing) is good. In addition, it can be seen that the voltage holding rate of the liquid crystal unit is higher than 90%, and a stable liquid crystal alignment film can be formed with good electrical properties. In particular, in Examples 1 to 9 in which dialkylene glycol dialkyl ether is formulated, the roughness of the liquid crystal alignment film is smaller than that of Example 10 in which dialkylene glycol dialkyl ether is not formulated, and the coating of the liquid crystal alignment agent on the substrate and the electrical properties of the liquid crystal element are well-balanced and improved.
[0298] On the other hand, in Comparative Example 3 using cyclic carbonate compound as solvent but not using dialkylene glycol monoalkyl ether, Comparative Example 2 using dialkylene glycol monoalkyl ether as solvent but not using cyclic carbonate compound and Comparative Example 1 not using polymer [P], the evaluation of the coating property of liquid crystal aligning agent is "○" or "◎", but the voltage holding rate of liquid crystal cell is about 80%, and the electrical property is poor. In addition, in Comparative Example 4 not using cyclic carbonate compound and dialkylene glycol monoalkyl ether as solvent, coating property and electrical property are the results worse than Examples 1 to 10.
Claims
1. A liquid crystal alignment agent, comprising: The polymer P has a specific structure derived from at least one selected from the group consisting of an amide group, a protected amide group, a urea group, and a protected urea group, and the specific structure is represented by the following formula (1): In formula (1), R 1 and R 2 are independently a hydrogen atom or a monovalent organic group, m is 0 or 1, and "*" represents a bond to the hydrocarbon group; Cyclic carbonate compounds; and Dialkyl glycol monoalkyl ether. 2 . The liquid crystal aligning agent according to claim 1 , further comprising a dialkyl diol ester.
3. The liquid crystal alignment agent according to claim 2, wherein: The content ratio of the dialkyl diol ester is 1 mass % or more and 70 mass % or less with respect to the total amount of the solvent contained in the said liquid crystal aligning agent.
4. The liquid crystal aligning agent according to any one of claims 1 to 3, wherein The polymer P further has at least one selected from the group consisting of a group having a polymerizable carbon-carbon unsaturated bond, a photoinitiator group, and a photo-alignment group.
5. The liquid crystal aligning agent according to any one of claims 1 to 3, wherein The polymer P further has at least one selected from the group consisting of a tertiary amine structure, a protected amino group, and a nitrogen-containing aromatic heterocyclic group. 6 . The liquid crystal aligning agent according to claim 1 , further comprising a compound having a crosslinkable group.
7. The liquid crystal aligning agent according to any one of claims 1 to 3, wherein The content ratio of the cyclic carbonate compound is 0.5 mass % or more and 50 mass % or less with respect to the total amount of the solvent contained in the said liquid crystal aligning agent.
8. The liquid crystal aligning agent according to any one of claims 1 to 3, wherein The content ratio of the dialkyl glycol monoalkyl ether is 1 mass % or more and 70 mass % or less with respect to the total amount of the solvent contained in the said liquid crystal aligning agent. 9 . A liquid crystal alignment film formed using the liquid crystal alignment agent according to claim 1 . 10 . A liquid crystal element comprising the liquid crystal alignment film according to claim 9 .
Citation Information
Patent Citations
Liquid crystal aligning agent, liquid crystal alignment layer, and liquid crystal display element
JP2009294274A
Liquid crystal aligning agent and liquid crystal display element
JP2010097188A
Colored photosensitive resin composition
JP2013122577A
Liquid crystal aligning agent, liquid crystal alignment film, manufacturing method of liquid crystal alignment film, and liquid crystal display element
WO2019103042A1