Metal-clad laminate and circuit board

By adopting a multi-layer structure of a transmission loss suppression layer and a dimensional accuracy maintenance layer with low dielectric loss tangent in the flexible printed wiring board, the problems of large transmission loss and poor dimensional stability in high-frequency signal transmission are solved, and the high-frequency signal is realized Low loss and high dimensional stability.

CN113043690BActive Publication Date: 2024-11-26NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011550852.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-24
Publication Date
2024-11-26
Estimated Expiration
2040-12-24

AI Technical Summary

Technical Problem

The prior art has problems of large transmission loss and poor dimensional stability in high-frequency signal transmission, especially in flexible printed wiring boards (FPCs), which are difficult to simultaneously reduce transmission loss and maintain dimensional stability.

Method used

Using a multi-layer structure of a transmission loss suppression layer and a dimensional accuracy maintenance layer with low dielectric loss tangent, the thickness ratio of the resin layer is controlled to ensure the reduction of the transmission loss of high-frequency signals by setting up a multi-layer resin laminate and an intermediate transmission loss suppression layer. and maintain dimensional accuracy.

Benefits of technology

It effectively reduces the transmission loss of high-frequency signals and maintains high dimensional stability. It is suitable for high-frequency signal circuit boards above 10GHz.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113043690B_ABST
    Figure CN113043690B_ABST
Patent Text Reader

Abstract

The present invention provides a metal-clad laminate and a circuit substrate that can reduce transmission loss even in high-frequency transmission and have excellent dimensional stability. The metal-clad laminate includes: a first metal layer, a first transmission loss suppression layer connected to one side of the first metal layer, a second metal layer, a second transmission loss suppression layer connected to one side of the second metal layer, and a multilayer resin layer interposed between the first transmission loss suppression layer and the second transmission loss suppression layer. The resin laminate has a first transmission loss suppression layer and a second transmission loss suppression layer, and at least two or more dimensional accuracy maintaining layers and an intermediate transmission loss suppression layer stacked between the dimensional accuracy maintaining layers. In the metal-clad laminate, when the dielectric loss tangent of the first transmission loss suppression layer and the second transmission loss suppression layer at 10 GHz is set to Df1, and the dielectric loss tangent of the dimensional accuracy maintaining layer is set to Df2, Df1<Df2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metal-clad laminate and a circuit board which are effectively used as electronic parts. Background Art

[0002] In recent years, with the progress of miniaturization, lightness and space saving of electronic devices, the demand for flexible printed circuits (FPCs) that are thin, light, flexible and have excellent durability even when bent repeatedly has increased. FPCs can be installed three-dimensionally and at high density even in a limited space, so their use is gradually expanding in the wiring or cables, connectors and other parts of the movable parts of electronic devices such as hard disk drives (HDDs), digital video disks (DVDs), and smart phones.

[0003] In addition to the high density mentioned above, the high performance of the equipment is being promoted, so it is also necessary to deal with the high frequency of the transmission signal. When transmitting high-frequency signals, if the transmission loss in the transmission path is large, the loss of electrical signals or the delay time of the signal will be prolonged. Therefore, in the future, it will also be important to reduce the transmission loss in FPC.

[0004] In order to improve high-frequency transmission characteristics, it has been proposed to use a laminated body formed by laminating films containing fluororesins on both sides of a polyimide film as an insulating resin layer (Patent Document 1). The insulating resin layer of Patent Document 1 uses a fluororesin, and thus has excellent dielectric properties, but has problems with dimensional stability. In particular, when applied to FPC, there is a concern that the dimensional change before and after circuit processing caused by etching and the dimensional change before and after heat treatment will become larger.

[0005] In order to improve high-frequency transmission characteristics, it is proposed to laminate two single-sided metal-clad laminates by introducing an adhesive layer having a specific diamine residue, and to control the thickness of the entire resin layer and the adhesive layer (Patent Document 2). However, in Patent Document 2, the distance between the adhesive layer with a low dielectric loss tangent and the metal layer (wiring) is far due to the insulating layer of the single-sided metal-clad laminate, so there is room for further improvement in the effect of reducing transmission loss.

[0006] [Prior art literature]

[0007] [Patent Document]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 2004-216830

[0009] [Patent Document 2] Japanese Patent Application Publication No. 2018-170417 Summary of the invention

[0010] [Problems to be solved by the invention]

[0011] An object of the present invention is to provide a metal-clad laminate and a circuit board which can reduce transmission loss even in high-frequency transmission and have excellent dimensional stability.

[0012] [Technical means to solve the problem]

[0013] The inventors of the present invention have conducted intensive research and found that: by respectively providing transmission loss suppression layers with low dielectric loss tangent in contact with a pair of metal layers (wiring), and providing a structure in which a plurality of dimensional accuracy maintaining layers are stacked using intermediate transmission loss suppression layers between the transmission loss suppression layers, and by setting the ratio of the total thickness of the dimensional accuracy maintaining layers to the overall thickness of the resin layer to be above a certain level, even if the overall thickness of the resin layer is increased, the positional deviation of the wiring can be suppressed, and the reduction of transmission loss and the maintenance of dimensional accuracy can coexist.

[0014] The metal-clad laminate of the present invention includes: a first metal layer, a first transmission loss suppression layer arranged in contact with one side of the first metal layer, a second metal layer, a second transmission loss suppression layer arranged in contact with one side of the second metal layer, and a multilayer resin layer interposed between the first transmission loss suppression layer and the second transmission loss suppression layer.

[0015] In the metal-clad laminate of the present invention, a resin laminate is formed by the first transmission loss suppression layer, the second transmission loss suppression layer and the multi-layer resin layer, and the resin laminate has at least two or more dimensional accuracy maintaining layers and an intermediate transmission loss suppression layer stacked between the dimensional accuracy maintaining layers.

[0016] Furthermore, the metal-clad laminate of the present invention satisfies the following conditions i and ii;

[0017] i) when the dielectric loss tangent of the first transmission loss suppression layer and the second transmission loss suppression layer is set to Df1 and the dielectric loss tangent of the dimensional accuracy maintaining layer is set to Df2, the relationship of Df1<Df2 is maintained, and the dielectric loss tangent is the dielectric loss tangent at 10 GHz measured by a split post dielectric resonator (SPDR) after humidity adjustment for 24 hours under constant temperature and humidity conditions (normal state) of 23°C and 50%RH;

[0018] ii) The total thickness of the dimensional accuracy maintaining layers is within a range of 25% to 60% of the total thickness of the resin laminate.

[0019] The circuit substrate of the present invention includes: a first wiring layer, a first transmission loss suppression layer arranged in contact with one side of the first wiring layer, a second wiring layer, a second transmission loss suppression layer arranged in contact with one side of the second wiring layer, and a multilayer resin layer interposed between the first transmission loss suppression layer and the second transmission loss suppression layer.

[0020] In the circuit substrate of the present invention, the first transmission loss suppression layer, the second transmission loss suppression layer and the multi-layer resin layer form a resin laminate, and the resin laminate has at least two or more dimensional accuracy maintaining layers and an intermediate transmission loss suppression layer stacked between the dimensional accuracy maintaining layers.

[0021] Furthermore, the circuit substrate of the present invention satisfies the following conditions i and ii;

[0022] i) when the dielectric loss tangent of the first transmission loss suppression layer and the second transmission loss suppression layer is set to Df1 and the dielectric loss tangent of the dimensional accuracy maintaining layer is set to Df2, the relationship of Df1<Df2 is maintained, and the dielectric loss tangent is the dielectric loss tangent at 10 GHz measured by a separation dielectric resonator (SPDR) after humidity adjustment for 24 hours under constant temperature and humidity conditions (normal state) of 23°C and 50%RH;

[0023] ii) The total thickness of the dimensional accuracy maintaining layers is within a range of 25% to 60% of the total thickness of the resin laminate.

[0024] In the metal-clad laminate or circuit substrate of the present invention, the dimensional accuracy maintaining layer can be a low thermal expansion polyimide layer whose minimum storage elastic coefficient in the temperature range of 100°C to 250°C can be in the range of 1.0GPa to 8.0GPa and whose thermal expansion coefficient is in the range of 15ppm / K to 25ppm / K.

[0025] In the metal-clad laminate or circuit substrate of the present invention, the resin constituting the first transmission loss suppression layer and the second transmission loss suppression layer may be a polyimide formed by reacting an acid anhydride component with a diamine component, and contains 50 mol parts or more of a dimer diamine in which the two terminal carboxylic acid groups of a dimer acid are substituted with a primary aminomethyl group or an amino group, relative to 100 mol parts of the total amount of the diamine component.

[0026] [Effects of the Invention]

[0027] The metal-clad laminate of the present invention is provided with a transmission loss suppression layer of low dielectric loss tangent in a manner connected to a pair of metal layers (wiring), so the transmission loss in high-frequency signal transmission can be effectively suppressed. In addition, since a structure formed by stacking a multilayer dimensional accuracy maintenance layer and an intermediate transmission loss suppression layer is provided between the transmission loss suppression layers, and the ratio of the total thickness of the dimensional accuracy maintenance layer to the thickness of the entire resin layer is set to a certain value or more, high dimensional stability can be ensured, and low dielectricization is achieved at the same time. Therefore, the metal-clad laminate of the present invention, for example, can effectively reduce transmission loss when applied to a circuit substrate of a high-frequency signal having a transmission frequency of more than 10 GHz. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram showing the structure of a metal-clad laminate according to one embodiment of the present invention.

[0029] Figure 2 This is a schematic cross-sectional view showing the structure of a metal-clad laminate according to another embodiment of the present invention.

[0030] Figure 3 This is a schematic cross-sectional view showing the structure of a metal-clad laminate according to still another embodiment of the present invention.

[0031] Figure 4 This is a schematic cross-sectional view showing a structural example of the dimensional accuracy maintaining layer.

[0032] Explanation of symbols

[0033] 10: Metal-clad laminate

[0034] 20: Resin laminate

[0035] M1: First metal layer

[0036] M2: Second metal layer

[0037] BS1: First transmission loss suppression layer

[0038] BS2: Second transmission loss suppression layer

[0039] BS3: Intermediate transmission loss suppression layer

[0040] PL: Dimensional Precision Maintaining Layer

[0041] 31: Non-thermoplastic polyimide layer

[0042] 33: Thermoplastic polyimide layer DETAILED DESCRIPTION

[0043] Embodiments of the present invention will be described with reference to the accompanying drawings as appropriate.

[0044] [Metal-clad laminate]

[0045] Figure 1 Schematic diagram showing the structure of a metal-clad laminate according to an embodiment of the present invention. The metal-clad laminate 10 of this embodiment includes:

[0046] The first metal layer M1,

[0047] A first transmission loss suppression layer BS1 connected to one side of the first metal layer M1,

[0048] The second metal layer M2,

[0049] A second transmission loss suppression layer BS2 disposed in contact with one side of the second metal layer M2, and

[0050] A plurality of resin layers are interposed between the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 .

[0051] The metal-clad laminate 10 is provided with a first transmission loss suppression layer BS1 and a second transmission loss suppression layer BS2 with low dielectric loss tangent at the positions closest to a pair of metal layers (the first metal layer M1 and the second metal layer M2 that become wiring), thereby effectively suppressing the transmission loss in high-frequency signal transmission.

[0052] Here, the first transmission loss suppression layer BS1, the second transmission loss suppression layer BS2, and a plurality of resin layers form a resin laminate 20. The resin laminate 20 includes at least two or more dimensional accuracy maintenance layers PL and an intermediate transmission loss suppression layer BS3 laminated between the dimensional accuracy maintenance layers PL in addition to the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2.

[0053] As described above, by providing the stacked structure of the dimensional accuracy maintaining layer PL and the intermediate transmission loss suppression layer BS3 between the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 , it is possible to achieve low dielectric constant while ensuring high dimensional stability.

[0054] In addition, the resin laminate 20 may have any resin layer other than the above, but is preferably formed only of resin layers having the above functions.

[0055] like Figure 1As shown, the first metal layer M1 and the second metal layer M2 are located at the outermost sides, and the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 are arranged in contact with their inner sides, and further, a multi-layer resin layer including a multi-layer dimensional accuracy maintaining layer PL and an intermediate transmission loss suppression layer BS3 is arranged between the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2. Here, the first transmission loss suppression layer BS1 is adjacent to one dimensional accuracy maintaining layer PL, and the second transmission loss suppression layer BS2 is in contact with another dimensional accuracy maintaining layer PL.

[0056] Figure 1 The metal-clad laminate 10 shown has two dimensional accuracy maintaining layers PL and one intermediate transmission loss suppression layer BS3, but the dimensional accuracy maintaining layers PL only need to be two or more layers, and the number of layers of the intermediate transmission loss suppression layer BS3 is not particularly limited. Figure 2 As shown, the structure having three dimensional accuracy maintaining layers PL and two intermediate transmission loss suppression layers BS3 may also be as follows Figure 3 As shown, it has a structure of five dimensional accuracy maintaining layers PL and four intermediate transmission loss suppression layers BS3.

[0057] In the metal-clad laminate 10 , the first metal layer M1 and the second metal layer M2 may have the same or different structures, but are preferably made of the same material, have the same physical properties, and have the same thickness.

[0058] In addition, the structures of the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 may be the same or different, but are preferably made of the same material, physical properties, and thickness. For example, by making the dielectric loss tangent or thickness of the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 the same, it becomes easier to design a transmission loss reduction when manufacturing a circuit substrate for high-frequency transmission.

[0059] Furthermore, the structures of the first transmission loss suppression layer BS1, the second transmission loss suppression layer BS2 and the intermediate transmission loss suppression layer BS3 may be the same or different, but in order to improve the dielectric properties of the entire resin laminate 20 and effectively suppress the transmission loss of high-frequency signals, they are preferably made of the same material and have the same physical properties.

[0060] The structures of the multiple dimensional accuracy maintaining layers PL may be the same or different, but are preferably the same material, same physical properties, same thickness, and same layer structure in terms of easy design of mechanical strength or dimensional accuracy when manufacturing the circuit board.

[0061] The metal-clad laminate 10 satisfies the following conditions i and ii.

[0062] Condition i:

[0063] When the dielectric loss tangent of the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 is Df1 and the dielectric loss tangent of the dimensional accuracy maintaining layer PL is Df2 , a relationship of Df1 < Df2 exists.

[0064] By designing the dielectric loss tangent Df1 of the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2, which are respectively connected to the first metal layer M1 and the second metal layer M2, which are the transmission paths of the high-frequency signal, to be lower than the dielectric loss tangent Df2 of the dimensional accuracy maintaining layer PL, the transmission loss of the high-frequency signal can be effectively suppressed. Furthermore, even if the dielectric loss tangents of the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 are different, they are both required to satisfy the relationship of Df1<Df2. In the present invention, unless otherwise specified, the dielectric constant and dielectric loss tangent refer to the dielectric constant and dielectric loss tangent at 10 GHz measured by a separated dielectric resonator (SPDR) after humidification for 24 hours under constant temperature and humidity conditions (normal state) of 23°C and 50%RH.

[0065] From the viewpoint of achieving suppression of the transmission loss of high-frequency signals, the dielectric loss tangent Df1 at 10 GHz of the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 is preferably 0.005 or less, and more preferably 0.003 or less.

[0066] Furthermore, from the perspective of achieving suppression of transmission loss of high-frequency signals, the dielectric loss tangent Df3 of the intermediate transmission loss suppression layer BS3 at 10 GHz measured in the same manner as condition i is preferably less than 0.005, more preferably less than 0.003, and most preferably the same as the dielectric loss tangent Df1 of the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2.

[0067] In addition, the dielectric loss tangent Df2 of the dimensional accuracy maintaining layer PL is ideally as low as possible, but since it is a layer whose main purpose is to maintain dimensional accuracy and mechanical strength, it is preferably 0.012 or less as long as the condition i is satisfied, and more preferably 0.010 or less. The reason is that even if the dielectric loss tangent Df2 of the dimensional accuracy maintaining layer PL is slightly higher, by laminating with the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 and the intermediate transmission loss suppression layer BS3 having lower dielectric loss tangents, and considering the thickness ratio with them, the overall low dielectric property of the resin laminate 20 can be ensured.

[0068] Condition ii:

[0069] Total thickness T of the dimensional accuracy maintaining layer PL PLIt is within the range of 25% to 60% of the total thickness T of the resin laminate 20 (ie, the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2, one or more intermediate transmission loss suppression layers BS3, and multiple dimensional accuracy maintaining layers PL).

[0070] By maintaining the total thickness T of the multi-layer dimensional accuracy layer PL PL When the ratio of the total thickness T of the resin laminate 20 is within the above range, the dimensional accuracy and mechanical strength of the metal-clad laminate 10 during circuit processing can be maintained, while the transmission loss of high-frequency signals can be reduced. PL The ratio to the total thickness T is preferably in the range of 25% to 50%.

[0071] Here, the thickness of each layer in the resin laminate 20 can be appropriately set according to the intended use and is not particularly limited, but can be exemplified as follows.

[0072] The thickness of one layer of the first transmission loss suppression layer BS1 and the second transmission loss suppression layer BS2 is preferably within a range of 2 μm to 100 μm, and more preferably within a range of 5 μm to 75 μm.

[0073] The thickness of one layer of the dimensional accuracy maintaining layer PL is preferably within a range of 10 μm to 100 μm, and more preferably within a range of 12 μm to 50 μm.

[0074] The thickness of one layer of the intermediate transmission loss suppression layer BS3 is preferably within a range of 12 μm to 150 μm, and more preferably within a range of 25 μm to 100 μm.

[0075] The total thickness T of the resin laminate 20 is preferably within a range of 50 μm to 300 μm, and more preferably within a range of 75 μm to 200 μm.

[0076] In order to achieve a low dielectric constant of the entire resin laminate 20, the total thickness T of the first transmission loss suppression layer BS1, the second transmission loss suppression layer BS2, and the intermediate transmission loss suppression layer BS3 is B The ratio is preferably within a range of 40% to 75%, more preferably within a range of 50% to 75%, relative to the total thickness T of the resin laminate 20 .

[0077] Hereinafter, each layer constituting the metal-clad laminate 10 will be described.

[0078] [Metal layer]

[0079] The material of the first metal layer M1 and the second metal layer M2 is not particularly limited, and examples thereof include copper, stainless steel, iron, nickel, beryllium, aluminum, zinc, indium, silver, gold, tin, zirconium, tantalum, titanium, lead, magnesium, manganese, and alloys thereof. Among them, copper or copper alloys are particularly preferred. Furthermore, the material of the wiring layer in the circuit substrate of the present embodiment described later is also the same as that of the first metal layer M1 and the second metal layer M2.

[0080] The thickness of the first metal layer M1 and the second metal layer M2 is not particularly limited. For example, when using a metal foil such as copper foil, it is preferably 35 μm or less, and more preferably within the range of 5 μm to 25 μm. From the perspective of production stability and handling properties, the lower limit of the thickness of the metal foil is preferably set to 5 μm. Furthermore, when using copper foil, it can be a rolled copper foil or an electrolytic copper foil. In addition, as the copper foil, a commercially available copper foil can be used.

[0081] The metal foil may be subjected to surface treatment using, for example, siding, aluminum alcoholate, aluminum chelate, silane coupling agent, etc., for the purpose of rust prevention or improvement of adhesive strength.

[0082] [Transmission loss suppression layer]

[0083] The glass transition temperature (Tg) of the resin constituting the first transmission loss suppression layer BS1, the second transmission loss suppression layer BS2, and the intermediate transmission loss suppression layer BS3 (hereinafter, they are sometimes collectively referred to as "transmission loss suppression layer BS1 to transmission loss suppression layer BS3") is preferably 180°C or less, and more preferably 160°C or less. By setting the glass transition temperature of the transmission loss suppression layer BS1 to the transmission loss suppression layer BS3 to be 180°C or less, thermocompression bonding at a low temperature can be performed, thereby alleviating the internal stress generated during lamination and suppressing dimensional changes after circuit processing. If the Tg of the transmission loss suppression layer BS1 to the transmission loss suppression layer BS3 exceeds 180°C, the temperature during bonding between the dimensional accuracy maintaining layers PL becomes high, which may impair the dimensional stability after circuit processing.

[0084] The transmission loss suppression layer BS1 to the transmission loss suppression layer BS3 preferably have a maximum storage elastic coefficient of 1.0 GHz or less in the temperature range of 100°C to 250°C. With such a storage elastic coefficient, the internal stress during thermocompression bonding can be relieved, and the dimensional stability after circuit processing can be maintained. In addition, even after the reflow process after circuit processing, warping is not likely to occur.

[0085] The resin constituting the first transmission loss suppression layer BS1, the second transmission loss suppression layer BS2, and the intermediate transmission loss suppression layer BS3 is preferably a polyimide, and more preferably a thermoplastic polyimide obtained by imidizing a polyamic acid obtained by reacting an anhydride component with a diamine component (hereinafter sometimes referred to as "DDA-based polyimide") or a crosslinked cured product thereof, wherein the diamine component contains 50 mol parts or more of a dimer diamine in which both terminal carboxylic acid groups of a dimer acid are substituted with a primary aminomethyl group or an amino group relative to 100 mol parts of the total amount of the diamine component. Furthermore, when referred to as a polyimide in the present invention, in addition to polyimide, it also refers to a resin containing a polymer having an imide group in the molecular structure, such as polyamide-imide, polyether-imide, polyester-imide, polysiloxane-imide, polybenzimidazole-imide, etc.

[0086] <DDA-based polyimide>

[0087] DDA-based polyimide is an aliphatic thermoplastic polyimide, is highly flexible, has sufficient toughness even when a large amount of liquid crystal polymer filler is added, and has a high ability to maintain its shape when formed into a resin film.

[0088] DDA-based polyimide contains a tetracarboxylic acid residue derived from a tetracarboxylic anhydride as a raw material and a diamine residue derived from a diamine compound as a raw material. In the present invention, the tetracarboxylic acid residue represents a tetravalent group derived from a tetracarboxylic dianhydride, and the diamine residue represents a divalent group derived from a diamine compound. By reacting the tetracarboxylic anhydride and the diamine compound as raw materials in approximately equimolar amounts, the type and amount of the tetracarboxylic acid residue and the diamine residue contained in the DDA-based polyimide can be made to roughly correspond to the type and amount of the raw materials.

[0089] (anhydride component)

[0090] DDA polyimide can use tetracarboxylic anhydride commonly used in thermoplastic polyimide as raw material without particular limitation, but preferably contains tetracarboxylic anhydride represented by the following general formula (1) and / or general formula (2) in a total of 90 mol% or more relative to all anhydride components. In other words, DDA polyimide preferably contains a total of 90 mol% or more of tetracarboxylic acid residues derived from tetracarboxylic anhydride represented by the following general formula (1) and / or general formula (2) relative to 100 mol parts of all tetracarboxylic acid residues. By containing a total of 90 mol% or more of tetracarboxylic acid residues derived from tetracarboxylic anhydride represented by the following general formula (1) and / or general formula (2) relative to 100 mol parts of tetracarboxylic acid residues, it is easy to achieve the coexistence of softness and heat resistance of DDA polyimide and it is preferred. If the total amount of tetracarboxylic acid residues derived from tetracarboxylic anhydride represented by the following general formula (1) and / or general formula (2) is less than 90 mol parts, there is a tendency for the solvent solubility of DDA polyimide to decrease.

[0091] [Chemistry 1]

[0092]

[0093] In the general formula (1), X represents a single bond or a divalent group selected from the following formula; in the general formula (2), the cyclic part represented by Y represents a cyclic saturated hydrocarbon group selected from a 4-membered ring, a 5-membered ring, a 6-membered ring, a 7-membered ring or an 8-membered ring.

[0094] [Chemistry 2]

[0095]

[0096] In the above formula, Z represents -C6H4-, -(CH2)n- or -CH2-CH(-OC(=O)-CH3)-CH2-, and n represents an integer of 1 to 20.

[0097] Examples of the tetracarboxylic anhydride represented by the general formula (1) include 3,3',4,4'-biphenyl tetracarboxylic dianhydride (BPDA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride (DSDA), 4,4'-oxydiphthalic dianhydride (ODPA), 4,4'-(hexafluoroisopropylidene) diphthalic anhydride (D ... anhydride, 6FDA), 2,2-bis[4-(3,4-dicarboxyphenoxy]propane dianhydride (BPADA), p-phenylene bis(trimellitic acid monoester) anhydride (TAHQ), ethylene glycol bistrimellitic anhydride ( anhydride, TMEG) and the like. Among these, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) is particularly preferred. When BTDA is used, the carbonyl group (ketone group) contributes to adhesion, so the adhesion of DDA-based polyimide can be improved. In addition, BTDA has a ketone group in the molecular skeleton that reacts with the amino group of the amino compound used for cross-linking to form a C=N bond, which easily shows the effect of improving heat resistance. From this point of view, it is preferable to contain 50 mol parts or more, more preferably 60 mol parts or more of tetracarboxylic acid residues derived from BTDA relative to 100 mol parts of tetracarboxylic acid residues.

[0098] Examples of the tetracarboxylic anhydride represented by the general formula (2) include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 1,2,4,5-cycloheptanetetracarboxylic dianhydride, and 1,2,5,6-cyclooctanetetracarboxylic dianhydride.

[0099] The DDA-based polyimide may contain a tetracarboxylic acid residue derived from an acid anhydride other than the tetracarboxylic acid anhydride represented by the general formula (1) and the general formula (2) within a range that does not impair the effects of the invention. Such a tetracarboxylic acid residue is not particularly limited, and examples thereof include pyromellitic acid dianhydride, 2,3',3,4'-biphenyltetracarboxylic acid dianhydride, 2,2',3,3'-benzophenonetetracarboxylic acid dianhydride or 2,3,3',4'-benzophenonetetracarboxylic acid dianhydride, 2,3',3,4'-diphenylethertetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, 3,3",4,4"-p-terphenyltetracarboxylic acid dianhydride, 2,3,3",4"-p-terphenyltetracarboxylic acid dianhydride or 2,2",3,3"-p-terphenyltetracarboxylic acid dianhydride, 2,2- (2,3-dicarboxyphenyl)-propane dianhydride or 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride or bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride or bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride or 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-phenanthrene-tetracarboxylic dianhydride, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride or 1,2,9,10-phenanthrene-tetracarboxylic dianhydride carboxylic acid dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)tetrafluoropropane dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride or 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-(or 1,4,5,8-)tetrachloro A tetracarboxylic acid residue derived from an aromatic tetracarboxylic acid dianhydride such as naphthalene-1,4,5,8-(or 2,3,6,7-)tetracarboxylic dianhydride, 2,3,8,9-perylene-tetracarboxylic dianhydride, 3,4,9,10-perylene-tetracarboxylic dianhydride, 4,5,10,11-perylene-tetracarboxylic dianhydride or 5,6,11,12-perylene-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride, or 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride.

[0100] (Diamine component)

[0101] DDA-based polyimide uses a diamine component as a raw material, wherein the diamine component contains 50 mol parts or more, more preferably 70 mol parts or more of a dimer diamine in which both terminal carboxylic acid groups of a dimer acid are substituted with a primary aminomethyl group or an amino group, relative to 100 mol parts of the total amount of the diamine component. By containing the dimer diamine in such an amount, the dielectric properties of the polyimide can be improved, and the thermocompression bonding properties can be improved by lowering the glass transition temperature (low Tg) of the polyimide, and the internal stress can be relieved by lowering the elastic modulus.

[0102] The so-called dimer diamine refers to a diamine in which the two terminal carboxylic acid groups (-COOH) of the dimer acid are substituted by primary aminomethyl (-CH2-NH2) or amino group (-NH2). Dimer acid is a known dibasic acid obtained by intermolecular polymerization of unsaturated fatty acids. Its industrial production process has been roughly standardized in the industry, and it can be obtained by dimerizing unsaturated fatty acids with carbon numbers of 11 to 22 using clay catalysts, etc. As for the industrially obtained dimer acid, the main component is a dibasic acid with a carbon number of 36 obtained by dimerizing unsaturated fatty acids with a carbon number of 18 such as oleic acid, linoleic acid, and linolenic acid, and it contains any amount of monomer acid (carbon number 18), trimer acid (carbon number 54), and other polymerized fatty acids with carbon numbers of 20 to 54, depending on the degree of purification. In addition, after the dimerization reaction, double bonds remain, but in the present invention, dimer acid also includes compounds that are further hydrogenated to reduce the degree of unsaturation. Dimer diamine can be defined as a diamine compound obtained by substituting the terminal carboxylic acid group of a dibasic acid compound having a carbon number in the range of 18 to 54, preferably in the range of 22 to 44, with a primary aminomethyl group or an amino group.

[0103] As the characteristic of dimer diamine, the characteristic of the skeleton derived from dimer acid can be given. That is, dimer diamine is a macromolecular aliphatic with a molecular weight of about 560 to 620, so the molar volume of the molecule can be increased, and the polar group of DDA-based polyimide can be relatively reduced. It is believed that the characteristics of such dimer acid-type diamines contribute to suppressing the reduction of the heat resistance of DDA-based polyimide, and reducing the dielectric constant and dielectric loss tangent to improve dielectric properties. In addition, due to the presence of two freely movable hydrophobic chains of 7 to 9 carbon numbers and two chain aliphatic amino groups with a length close to 18 carbon numbers, not only flexibility can be given to DDA-based polyimide, but also DDA-based polyimide can be set to an asymmetric chemical structure or a non-planar chemical structure, so it is believed that low dielectric constant can be achieved.

[0104] The dimer diamine used in the present invention is preferably refined for the purpose of reducing the components other than the dimer diamine. As a refining method, there is no particular limitation, but it is suitable to be a known method such as a distillation method or a precipitation refining method. The dimer diamine before refining can be obtained with a commercially available product, for example, PRIAMINE 1073 (trade name) manufactured by Croda Japan, PRIAMINE 1074 (trade name) manufactured by Croda Japan, PRIAMINE 1075 (trade name) manufactured by Croda Japan, etc.

[0105] Examples of diamine compounds other than the dimer diamine used in the DDA-based polyimide include aromatic diamine compounds and aliphatic diamine compounds. Specific examples thereof include 1,4-diaminobenzene (p-PDA (p-phenylenediamine; p-phenylenediamine), 2,2'-dimethyl-4,4'-diaminobiphenyl (2,2'-dimethyl-4,4'-diaminobiphenyl, m-TB), 2,2'-n-propyl-4,4'-diaminobiphenyl (2,2'-n-propyl-4,4'-diaminobiphenyl, m-NPB), 4-aminophenyl-4'-aminobenzoate (4-aminophenyl-4'-aminobenzoate, m-TB), 4-aminophenyl-4'-aminobenzoate (4-aminophenyl-4'-aminobenzoate ...NPB), 4-aminophenyl-4'-aminobenzoate (4-aminophenyl-4'-aminobenzoate, m-TB), 2,2'-dimethyl-4,4'-diaminobiphenyl (2,2'-dimethyl-4,4'-diaminobiphenyl, m-TB), 2,2'-n-propyl-4,4'-diaminobiphenyl (2,2'-n-propyl-4,4'-diaminobiphenyl, m-NPB), 4-aminophenyl-4'-aminobenzoate (4-aminophenyl-4'-aminobenzoate, m-NPB), 4-aminophenyl-4'-aminobenzoate (4-aminophenyl-4'-aminobenzoate, m-NPB), 4-aminophenyl-4'-aminobenzoate (4-aminophenyl-4'-amino benzoate, APAB), 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]biphenyl, bis[1-(3-aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)]benzophenone, 9,9-bis[4-(3-aminophenoxy)phenyl]fluorene, 2,2-bis-[4 -(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis-[4-(3-aminophenoxy)phenyl]hexafluoropropane, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-methylenebis-o-toluidine, 4,4'-methylenebis-2,6-dimethylaniline, 4,4'-methylenebis-2,6-diethylaniline, 3,3'-diaminodiphenylethane, 3,3'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 3,3"-diamino-p-terphenyl, 4,4'-[1,4 -phenylenebis(1-methylethylidene)]dianiline, 4,4'-[1,3-phenylenebis(1-methylethylidene)]dianiline, bis(p-aminocyclohexyl)methane, bis(p-β-amino-tert-butylphenyl) ether, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis(β-amino-tert-butyl)toluene, 2,4-diaminotoluene, m- Diamine compounds such as xylene-2,5-diamine, p-xylene-2,5-diamine, m-phenylenediamine, p-phenylenediamine, 2,6-diaminopyridine, 2,5-diaminopyridine, 2,5-diamino-1,3,4-oxadiazole, piperazine, 2'-methoxy-4,4'-diaminobenzanilide, 4,4'-diaminobenzanilide, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, 6-amino-2-(4-aminophenoxy)benzoxazole, and 1,3-bis(3-aminophenoxy)benzene.

[0106] DDA-based polyimide can be manufactured by reacting the anhydride component with the diamine component in a solvent to generate polyamic acid and then heating for ring closure. For example, the anhydride component and the diamine component are dissolved in an organic solvent in approximately equimolar amounts, and the polymerization reaction is carried out by stirring for 30 minutes to 24 hours at a temperature in the range of 0°C to 100°C, thereby obtaining a polyamic acid as a precursor of the polyimide. During the reaction, the reaction components are dissolved in a manner such that the generated precursor is in the range of 5% by weight to 50% by weight, preferably in the range of 10% by weight to 40% by weight in the organic solvent. Examples of the organic solvent used in the polymerization reaction include N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide, N-methyl-2-pyrrolidone (NMP), 2-butanone, dimethylsulfoxide (DMSO), hexamethylphosphoramide, N-methylcaprolactam, dimethyl sulfate, cyclohexanone, methylcyclohexane, dioxane, tetrahydrofuran, diethylene glycol dimethyl ether (diglyme), triethylene glycol dimethyl ether (triglyme), methanol, ethanol, benzyl alcohol, cresol, etc. These solvents may be used in combination of two or more, and aromatic hydrocarbons such as xylene and toluene may also be used in combination. The amount of the organic solvent used is not particularly limited, but is preferably adjusted so that the concentration of the polyamic acid solution obtained by the polymerization reaction becomes about 5% by weight to 50% by weight.

[0107] The synthesized polyamic acid is advantageously usually used as a reaction solvent solution, and can be concentrated, diluted or replaced with other organic solvents as needed. In addition, polyamic acid is usually excellent in solvent solubility, so it is advantageously used. The viscosity of the solution of polyamic acid is preferably within the range of 500mPa·s~100000mPa·s. If it deviates from the scope, it is easy to produce uneven thickness, stripes and other defects in the film when applying the coating operation using a coating machine etc.

[0108] The method for imidizing the polyamic acid to form the polyimide is not particularly limited, and for example, a heat treatment such as heating in the solvent at a temperature condition in the range of 80° C. to 400° C. for 1 to 24 hours can be suitably adopted. In addition, the temperature can be heated under a fixed temperature condition or the temperature can be changed in the middle of the process.

[0109] By selecting the types of the anhydride component and the diamine component in the DDA polyimide, or the respective molar ratios when two or more anhydride components or diamine components are used, it is possible to control dielectric properties, thermal expansion coefficient, tensile elastic coefficient, glass transition temperature, etc. In addition, when the DDA polyimide has a plurality of polyimide structural units, they may exist in the form of blocks or randomly, but preferably exist randomly.

[0110] The weight average molecular weight of DDA-based polyimide is preferably in the range of 10,000 to 200,000, for example. If it is within this range, it is easy to control the weight average molecular weight of the polyimide. In addition, for example, when used as an adhesive for FPC, the weight average molecular weight of DDA-based polyimide is more preferably in the range of 20,000 to 150,000, and further preferably in the range of 40,000 to 150,000. When used as an adhesive for FPC, when the weight average molecular weight of DDA-based polyimide is less than 20,000, there is a tendency for the fluidity resistance to deteriorate. On the other hand, if the weight average molecular weight of DDA-based polyimide exceeds 150,000, there is an excessive increase in viscosity and insolubility in the solvent, and it is easy to produce uneven thickness of the adhesive layer, streaks and other defects during the coating operation.

[0111] The imide group concentration of the DDA-based polyimide is preferably 22% by weight or less, more preferably 20% by weight or less. Here, "imide group concentration" refers to the value obtained by dividing the molecular weight of the imide group (-(CO)2-N-) in the polyimide by the molecular weight of the entire structure of the polyimide. If the imide group concentration exceeds 22% by weight, the molecular weight of the resin itself becomes smaller, and the low hygroscopicity is also deteriorated due to the increase in polar groups, and Tg and elastic modulus increase.

[0112] The DDA-based polyimide is most preferably a completely imidized structure. However, a portion of the polyimide may also be amic acid. The imidization rate can be measured by using a Fourier transform infrared spectrophotometer (commercially available: FT / IR620 manufactured by JASCO Corporation) and using the attenuated total reflection (ATR) method to measure the infrared absorption spectrum of the polyimide film at 1015 cm -1 Based on the benzene ring absorber nearby, according to 1780cm -1 The absorbance derived from the C=O expansion and contraction of the imide group was calculated.

[0113] The DDA-based polyimide may be appropriately formulated with, for example, a plasticizer, other curing resin components such as epoxy resin, a curing agent, a curing accelerator, an inorganic filler, a coupling agent, a bulking agent, a solvent, a flame retardant, and the like as optional components.

[0114] [Cross-linking formation of DDA-based polyimide]

[0115] In the case where the DDA polyimide has a ketone group, the ketone group is reacted with an amino group of an amino compound (hereinafter, sometimes referred to as "crosslinking forming amino compound") having at least two primary amino groups as functional groups to form a C=N bond, thereby forming a crosslinked structure. By forming a crosslinked structure, the heat resistance of the DDA polyimide can be improved. As a preferred tetracarboxylic anhydride for forming a DDA polyimide having a ketone group, for example, 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA) can be cited, and as a diamine compound, for example, aromatic diamines such as 4,4'-bis(3-aminophenoxy)benzophenone (4,4'-bis(3-aminophenoxy)benzophenone, BABP), 1,3-bis[4-(3-aminophenoxy)benzoyl]benzene (1,3-bis[4-(3-aminophenoxy)benzoyl]benzene, BABB) can be cited.

[0116] In order to form a crosslinked structure, it is particularly preferred to include the DDA-based polyimide and the amino compound for crosslinking formation, wherein the DDA-based polyimide contains preferably 50 mol% or more, more preferably 60 mol% or more of BTDA residues derived from BTDA relative to all tetracarboxylic acid residues. In the present invention, the "BTDA residue" refers to a tetravalent group derived from BTDA.

[0117] As the amino compound for crosslinking formation, there can be exemplified: (I) dihydrazide compounds, (II) aromatic diamines, (III) aliphatic amines, etc. Among these, dihydrazide compounds are preferred. Aliphatic amines other than dihydrazide compounds are easy to form crosslinked structures even at room temperature, and there are concerns about the storage stability of the varnish. On the other hand, aromatic diamines need to be set to high temperature in order to form a crosslinked structure. As described above, when a dihydrazide compound is used, the storage stability of the varnish can be achieved while shortening the curing time. As the dihydrazide compound, for example, dihydrazide compounds such as oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, adipic acid dihydrazide, pimelic acid dihydrazide, suberic acid dihydrazide, azelaic acid dihydrazide, sebacic acid dihydrazide, dodecanedioic acid dihydrazide, maleic acid dihydrazide, fumaric acid dihydrazide, diglycolic acid dihydrazide, tartaric acid dihydrazide, malic acid dihydrazide, phthalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, 2,6-naphthoic acid dihydrazide, 4,4-diphenyl dihydrazide, 1,4-naphthoic acid dihydrazide, 2,6-pyridine dihydrazide, and itaconic acid dihydrazide are preferred. The above dihydrazide compounds may be used alone or in combination of two or more.

[0118] Furthermore, the amino compounds (I) dihydrazide compounds, (II) aromatic diamines, (III) aliphatic amines, etc. may be used in combination of two or more, such as a combination of (I) and (II), a combination of (I) and (III), or a combination of (I) and (II) and (III).

[0119] In addition, from the viewpoint of making the network structure formed by crosslinking using the crosslink-forming amino compound denser, the molecular weight of the crosslink-forming amino compound used in the present invention (the weight average molecular weight when the crosslink-forming amino compound is an oligomer) is preferably 5,000 or less, more preferably 90 to 2,000, and further preferably 100 to 1,500. Among them, a crosslink-forming amino compound having a molecular weight of 100 to 1,000 is particularly preferred. If the molecular weight of the crosslink-forming amino compound is less than 90, one amino group of the crosslink-forming amino compound is limited to forming a C=N bond with the ketone group of the DDA-based polyimide, and the surrounding of the remaining amino group becomes sterically bulky, so there is a tendency that the remaining amino group is not easy to form a C=N bond.

[0120] When the ketone group in the DDA polyimide is cross-linked with the cross-linking amino compound, the cross-linking amino compound is added to the resin solution containing the DDA polyimide to cause the ketone group in the DDA polyimide to undergo a condensation reaction with the primary amino group of the cross-linking amino compound. The resin solution is cured by the condensation reaction to become a cured product. In the case, the amount of the cross-linking amino compound added may be 0.004 mol to 1.5 mol, preferably 0.005 mol to 1.2 mol, more preferably 0.03 mol to 0.9 mol, and most preferably 0.04 mol to 0.6 mol of the primary amino group relative to 1 mol of the ketone group. Regarding the addition amount of the cross-linking amino compound such as less than 0.004 mol of the total primary amino group relative to 1 mol of the keto group, since the cross-linking by the cross-linking amino compound is insufficient, there is a tendency that the heat resistance after curing is difficult to exhibit. If the addition amount of the cross-linking amino compound exceeds 1.5 mol, the unreacted cross-linking amino compound acts as a thermoplastic agent, and there is a tendency to reduce the heat resistance of the adhesive layer.

[0121] The conditions for the condensation reaction for crosslinking formation are not particularly limited as long as the ketone group in the DDA-based polyimide reacts with the primary amino group of the crosslinking amino compound to form an imine bond (C=N bond). Regarding the temperature of the heating condensation, for the reasons of releasing the water generated by the condensation to the outside of the system, or simplifying the condensation process when the heating condensation reaction is carried out after the synthesis of the DDA-based polyimide, it is preferably in the range of 120°C to 220°C, and more preferably in the range of 140°C to 200°C. The reaction time is preferably about 30 minutes to 24 hours. The end point of the reaction can be measured, for example, by using a Fourier transform infrared spectrophotometer (commercially available product: FT / IR620 manufactured by JASCO Corporation) to measure the infrared absorption spectrum and using 1670cm -1 The absorption peaks at 1635 cm-1 and 1635 cm-2 derived from the ketone groups in the polyimide resin decrease or disappear. -1 This was confirmed by the appearance of an absorption peak derived from an imine group nearby.

[0122] The heating condensation of the ketone group of the DDA-based polyimide and the primary amino group of the crosslinking-forming amino compound can be performed, for example, by the following method.

[0123] (1) A method in which an amino compound for crosslinking is added immediately after the synthesis (imidization) of a DDA-based polyimide and then heated;

[0124] (2) A method in which an excess amount of an amino compound is added as a diamine component in advance, and then the DDA-based polyimide is synthesized (imidized), and the remaining amino compound that does not participate in imidization or amidation is used as an amino compound for crosslinking and heated together with the DDA-based polyimide;

[0125] or

[0126] (3) A method of heating a composition of a DDA-based polyimide to which the crosslink-forming amino compound is added after processing it into a predetermined shape (for example, after coating it on an arbitrary substrate or forming it into a film).

[0127] In order to impart heat resistance to DDA-based polyimide, the formation of imide bonds is described in the formation of a cross-linked structure, but the present invention is not limited thereto. As a method for curing the polyimide, for example, epoxy resin, epoxy resin hardener, maleimide or activated ester resin or a resin having a styrene skeleton, or other compounds having unsaturated bonds may be formulated for curing.

[0128] [Dimensional accuracy maintenance layer]

[0129] Regarding the dimensional accuracy maintaining layer PL, in order to maintain the mechanical strength of the metal-clad laminate 10, the minimum value of the storage elastic coefficient in the temperature range of 100°C to 250°C is preferably in the range of 1.0GPa to 8.0GPa, and more preferably in the range of 2.0GPa to 6.0GPa. If the minimum value of the storage elastic coefficient of the dimensional accuracy maintaining layer PL is less than 1.0GPa, sufficient mechanical strength and dimensional accuracy after circuit processing cannot be obtained. In the case where the minimum value of the storage elastic coefficient exceeds 8.0GPa, warping is likely to occur during lamination pressing.

[0130] In addition, regarding the dimensional accuracy maintaining layer PL, in order to maintain the dimensional accuracy when the metal-clad laminate 10 is subjected to circuit processing, the coefficient of thermal expansion (CTE) is preferably within the range of 15ppm / K to 25ppm / K, and more preferably within the range of 16ppm / K to 23ppm / K. If the CTE of the dimensional accuracy maintaining layer PL is less than 15ppm / K, the metal-clad laminate 10 is prone to warping, and if it exceeds 25ppm / K, the dimensional accuracy after circuit processing cannot be obtained.

[0131] The dimensional accuracy maintaining layer PL is not particularly limited as long as it contains a resin having electrical insulation properties, and examples thereof include polyimide, epoxy resin, phenol resin, polyethylene, polypropylene, polytetrafluoroethylene, silicone, ethylene tetrafluoroethylene (ETFE), etc., and preferably contains polyimide. That is, the dimensional accuracy maintaining layer PL is preferably a single layer or a multilayer low thermal expansion polyimide layer.

[0132] When the dimensional accuracy maintaining layer PL is a single-layer polyimide layer, it can be set to the same structure as the non-thermoplastic polyimide layer 31 described later. As the single-layer polyimide layer, commercial products such as Kapton EN (trade name; manufactured by Toray Dupont Co., Ltd.) and Apical NPI (trade name; manufactured by Kaneka Co., Ltd.) can be used.

[0133] In the case where the dimensional accuracy maintaining layer PL includes a plurality of polyimide layers, as Figure 4As shown in FIG. 1 , the dimensional accuracy maintaining layer PL may be, for example, a structure in which a thermoplastic polyimide layer 33 containing a thermoplastic polyimide as a resin component is stacked on both sides of a non-thermoplastic polyimide layer 31 containing a non-thermoplastic polyimide as a resin component. The so-called "non-thermoplastic polyimide" is generally a polyimide that does not show softening or adhesiveness even when heated, but in the present invention, it refers to a non-thermoplastic polyimide having a storage elastic coefficient of 1.0×10 9 Pa and the storage elastic coefficient at 350°C is 1.0×10 8 The so-called "thermoplastic polyimide" is generally a polyimide whose glass transition temperature (Tg) can be clearly confirmed, but in the present invention, it means a polyimide whose storage elastic modulus at 30°C measured by DMA is 1.0×10 9 Pa or more and the storage elastic coefficient at 350°C is less than 1.0×10 8 Polyimide of Pa.

[0134] Next, a description will be given of a preferred structural example of the non-thermoplastic polyimide layer 31 and the thermoplastic polyimide layer 33 constituting the dimensional accuracy maintaining layer PL.

[0135] Non-thermoplastic polyimide layer:

[0136] The non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer 31 contains a tetracarboxylic acid residue and a diamine residue. The polyimide preferably contains an aromatic tetracarboxylic acid residue derived from an aromatic tetracarboxylic dianhydride and an aromatic diamine residue derived from an aromatic diamine.

[0137] (Tetracarboxylic acid residue)

[0138] The non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer 31 preferably contains a tetracarboxylic acid residue derived from at least one of 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA) and 1,4-phenylene bis(trimellitic acid monoester) dianhydride (TAHQ) and a tetracarboxylic acid residue derived from at least one of pyromellitic dianhydride (PMDA) and 2,3,6,7-naphthalene tetracarboxylic dianhydride (NTCDA) as the tetracarboxylic acid residue.

[0139] The tetracarboxylic acid residue derived from BPDA (hereinafter, also referred to as "BPDA residue") and the tetracarboxylic acid residue derived from TAHQ (hereinafter, also referred to as "TAHQ residue") easily form an ordered structure of the polymer, and can reduce the dielectric loss tangent or hygroscopicity by inhibiting the movement of molecules. The BPDA residue can impart self-supporting properties to the gel film of polyamic acid, which is a polyimide precursor, but on the other hand, there is a tendency to increase the CTE after imidization, reduce the glass transition temperature, and reduce the heat resistance.

[0140] According to this viewpoint, the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer 31 is controlled to contain BPDA residues and TAHQ residues in a total amount preferably in a range of 30 mol parts or more and 60 mol parts or less, and more preferably in a range of 40 mol parts or more and 50 mol parts or less, relative to 100 mol parts of all tetracarboxylic acid residues. If the total amount of BPDA residues and TAHQ residues is less than 30 mol parts, the formation of the ordered structure of the polymer becomes insufficient, the moisture absorption resistance decreases, or the reduction of the dielectric loss tangent becomes insufficient. If it exceeds 60 mol parts, in addition to the increase in CTE or the increase in the amount of change in the in-plane retardation (RO), there is also a risk of reduced heat resistance.

[0141] In addition, tetracarboxylic acid residues derived from pyromellitic acid dianhydride (hereinafter, also referred to as "PMDA residues") and tetracarboxylic acid residues derived from 2,3,6,7-naphthalenetetracarboxylic acid dianhydride (hereinafter, also referred to as "NTCDA residues") are owing to rigidity, and therefore improve in-plane orientation, suppress CTE to a low level and assume the effect of controlling in-plane delay (RO) or controlling glass transition temperature. On the other hand, PMDA residues are due to small molecular weight, so if their amount becomes too much, the imide concentration of polymer becomes high, polar groups increase and hygroscopicity becomes large, and dielectric loss tangent increases due to the influence of moisture inside the molecular chain. In addition, NTCDA residues exist because of the high naphthalene skeleton of rigidity and the film is easily brittle and the tendency of increasing the elastic coefficient is increased.

[0142] Therefore, the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer contains PMDA residues and NTCDA residues in a total of preferably 40 mol parts or more and 70 mol parts or less, more preferably 50 mol parts or more and 60 mol parts or less, and more preferably 50 mol parts to 55 mol parts relative to 100 mol parts of all tetracarboxylic acid residues. If the total of PMDA residues and NTCDA residues is less than 40 mol parts, there is a risk of CTE increase or heat resistance reduction, and if it exceeds 70 mol parts, there is a risk of the imide group concentration of the polymer becoming high, the polar group increases and the low hygroscopicity is impaired, and the dielectric loss tangent increases; or the film becomes brittle and the self-supporting property of the film is reduced.

[0143] The total amount of at least one of BPDA residue and TAHQ residue and at least one of PMDA residue and NTCDA residue is preferably 80 mol parts or more, preferably 90 mol parts or more, based on 100 mol parts of all tetracarboxylic acid residues.

[0144] In addition, it is preferable to control the CTE and the formation of an ordered structure of the polymer by setting the molar ratio of at least one of BPDA residues and TAHQ residues to at least one of PMDA residues and NTCDA residues {(BPDA residue + TAHQ residue) / (PMDA residue + NTCDA residue)} to a range of greater than 0.4 and less than 1.5, preferably within a range of greater than 0.6 and less than 1.3, and more preferably within a range of greater than 0.8 and less than 1.2.

[0145] PMDA and NTCDA have a rigid skeleton, so compared with other common anhydride components, the in-plane orientation of the molecules in the polyimide can be controlled, and the thermal expansion coefficient (CTE) is suppressed and the glass transition temperature (Tg) is improved. In addition, compared with PMDA, the molecular weight of BPDA and TAHQ is larger, so the imide group concentration is reduced due to the increase in the input ratio, which has an effect on the reduction of the dielectric loss tangent or the reduction of the hygroscopicity. On the other hand, if the input ratio of BPDA and TAHQ increases, the in-plane orientation of the molecules in the polyimide is reduced, which leads to an increase in CTE. And then, the formation of the ordered structure in the molecule is promoted, and the haze value increases. From this point of view, the total input amount of PMDA and NTCDA is in the range of 40 to 70 molar parts relative to 100 molar parts of all anhydride components of the raw material, preferably in the range of 50 to 60 molar parts, and more preferably in the range of 50 to 55 molar parts. If the total amount of PMDA and NTCDA is less than 40 parts by mole relative to 100 parts by mole of all the anhydride components of the raw material, the in-plane orientation of the molecules is reduced, and it becomes difficult to lower the CTE. In addition, the heat resistance or dimensional stability of the film during heating due to the reduction in Tg is reduced. On the other hand, if the total amount of PMDA and NTCDA exceeds 70 parts by mole, there is a tendency to deteriorate the moisture absorption rate or increase the elastic modulus due to the increase in the imide group concentration.

[0146] In addition, BPDA and TAHQ are effective in reducing the dielectric loss tangent and moisture absorption rate caused by the suppression of molecular motion or the reduction of the imide group concentration, but the CTE of the polyimide film after imidization is increased. From this point of view, the total input amount of BPDA and TAHQ is preferably within the range of 30 to 60 mol parts, preferably within the range of 40 to 50 mol parts, relative to 100 mol parts of all the anhydride components of the raw materials.

[0147] Examples of tetracarboxylic acid residues other than the BPDA residue, TAHQ residue, PMDA residue, and NTCDA residue contained in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer 31 include 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride or 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,3',3,4'-diphenyl ether tetracarboxylic dianhydride, and bis(2,3-dicarboxyphenyl)ether dianhydride. , 3,3",4,4"-terphenyltetracarboxylic dianhydride, 2,3,3",4"-terphenyltetracarboxylic dianhydride or 2,2",3,3"-terphenyltetracarboxylic dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-propane dianhydride or 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride or bis(3,4-dicarboxyphenyl)methane dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride or bis(3,4-dicarboxyphenyl)sulfone dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride or 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-phenanthrene -tetracarboxylic dianhydride, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride or 1,2,9,10-phenanthrene-tetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)tetrafluoropropane dianhydride, 2,3,5,6-cyclohexane dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride or 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-(or 1,4,5,8- ) tetracarboxylic acid residues derived from aromatic tetracarboxylic acid dianhydrides such as tetrachloronaphthalene-1,4,5,8-(or 2,3,6,7-)tetracarboxylic dianhydride, 2,3,8,9-perylene-tetracarboxylic dianhydride, 3,4,9,10-perylene-tetracarboxylic dianhydride, 4,5,10,11-perylene-tetracarboxylic dianhydride or 5,6,11,12-perylene-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride, and ethylene glycol ditrimellitate dianhydride.

[0148] (Diamine residue)

[0149] As the diamine residue contained in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer 31 , a diamine residue derived from a diamine compound represented by the general formula (A1) is preferred.

[0150] [Chemistry 3]

[0151]

[0152] In formula (A1), the linking group Z represents a single bond or -COO-, Y independently represents a monovalent hydrocarbon group with 1 to 3 carbon atoms which may be substituted with a halogen atom or a phenyl group, or an alkoxy group with 1 to 3 carbon atoms or a perfluoroalkyl or alkenyl group with 1 to 3 carbon atoms, n represents an integer of 0 to 2, and p and q independently represent integers of 0 to 4. Here, the term "independently" means that in the formula (A1), a plurality of substituents Y, and integers p and q may be the same or different. Furthermore, in the formula (A1), the hydrogen atoms in the two amino groups at the terminals may be substituted, for example, -NR2R3 (here, R2 and R3 independently refer to any substituent such as an alkyl group).

[0153] The diamine compound represented by the general formula (A1) (hereinafter, sometimes referred to as "diamine (A1)") is an aromatic diamine having one or three benzene rings. Since diamine (A1) has a rigid structure, it has the effect of imparting an ordered structure to the polymer as a whole. Therefore, a polyimide with low air permeability and low hygroscopicity can be obtained, which can reduce the moisture inside the molecular chain, thereby reducing the dielectric loss tangent. Here, as a linking group Z, a single bond is preferred.

[0154] Examples of the diamine (A1) include 1,4-diaminobenzene (p-PDA; p-phenylenediamine), 2,2′-dimethyl-4,4′-diaminobiphenyl (m-TB), 2,2′-n-propyl-4,4′-diaminobiphenyl (m-NPB), and 4-aminophenyl-4′-aminobenzoate (APAB).

[0155] The non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer 31 preferably contains 80 mol parts or more, more preferably 85 mol parts or more of diamine residues derived from the diamine (A1) relative to 100 mol parts of all diamine residues. By using the diamine (A1) in an amount within the above range, it is easy to form an ordered structure in the entire polymer by utilizing the rigid structure derived from the monomer, and it is easy to obtain a non-thermoplastic polyimide with low air permeability, low hygroscopicity and low dielectric loss tangent.

[0156] When the amount of the diamine residue derived from the diamine (A1) is in the range of 80 parts by mole or more and 85 parts by mole or less based on 100 parts by mole of all the diamine residues in the non-thermoplastic polyimide, 1,4-diaminobenzene is preferably used as the diamine (A1) from the viewpoint of having a more rigid structure and excellent in-plane orientation.

[0157] Examples of other diamine residues contained in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer 31 include 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]biphenyl, bis[1-(3-aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)]benzophenone, 9,9-bis[4-(3-aminophenoxy)phenyl]fluorene, 2 ... ,2-bis-[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis-[4-(3-aminophenoxy)phenyl]hexafluoropropane, 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-methylenebis-o-toluidine, 4,4'-methylenebis-2,6-dimethylaniline, 4,4'-methylenebis-2,6-diethylaniline, 3,3'-diaminodiphenylethane, 3,3'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 3,3"-diamino-p-terphenyl, 4,4'-[1,4-phenylenebis(1-methylphenylene) bis(p-aminocyclohexyl)methane, bis(p-β-amino-tert-butylphenyl)ether, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis(β-amino-tert-butyl)toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-xylene diamine residues derived from aromatic diamine compounds such as diamine, p-xylylenediamine, 2,6-diaminopyridine, 2,5-diaminopyridine, 2,5-diamino-1,3,4-oxadiazole, piperazine, 2'-methoxy-4,4'-diaminobenzanilide, 4,4'-diaminobenzanilide, 1,3-bis[2-(4-aminophenyl)-2-propyl]benzene, and 6-amino-2-(4-aminophenoxy)benzoxazole; and diamine residues derived from aliphatic diamine compounds such as dimer acid-type diamines in which both terminal carboxylic acid groups of a dimer acid are substituted with primary aminomethyl or amino groups.

[0158] By selecting the types of the tetracarboxylic acid residue and the diamine residue in the non-thermoplastic polyimide, or the respective molar ratios when two or more tetracarboxylic acid residues or diamine residues are used, the thermal expansion coefficient, storage elastic coefficient, tensile elastic coefficient, etc. can be controlled. In addition, when there are a plurality of polyimide structural units in the non-thermoplastic polyimide, they may exist in the form of blocks or randomly, but from the viewpoint of suppressing the deviation of the in-plane retardation (RO), they are preferably randomly present.

[0159] Furthermore, by making both the tetracarboxylic acid residue and the diamine residue contained in the non-thermoplastic polyimide an aromatic group, the dimensional accuracy of the polyimide film in a high temperature environment can be improved and the variation amount of the in-plane retardation (RO) can be reduced, which is preferred.

[0160] The imide group concentration of the non-thermoplastic polyimide is preferably less than 33%, more preferably more than 32%. Here, "imide group concentration" refers to the value obtained by dividing the molecular weight of the imide group (-(CO)2-N-) in the polyimide by the molecular weight of the entire structure of the polyimide. If the imide group concentration exceeds 33%, the molecular weight of the resin itself becomes smaller, and the low hygroscopicity is also deteriorated due to the increase in polar groups. By selecting the combination of the acid anhydride and the diamine compound to control the orientation of the molecules in the non-thermoplastic polyimide, the increase in CTE associated with the decrease in the imide group concentration is suppressed, thereby ensuring low hygroscopicity.

[0161] The weight average molecular weight of the non-thermoplastic polyimide is preferably in the range of 10,000 to 400,000, and more preferably in the range of 50,000 to 350,000. If the weight average molecular weight is less than 10,000, the strength of the film is reduced and the film tends to be brittle. On the other hand, if the weight average molecular weight exceeds 400,000, the viscosity is excessively increased, and defects such as uneven film thickness and streaks are easily generated during coating.

[0162] From the viewpoint of ensuring the function as a base layer and the transportability during manufacturing and thermoplastic polyimide coating, the thickness of the non-thermoplastic polyimide layer 31 is preferably within the range of 6 μm to 100 μm, and more preferably within the range of 9 μm to 50 μm. When the thickness of the non-thermoplastic polyimide layer 31 is less than the lower limit, the electrical insulation and handling properties become insufficient, and when the thickness exceeds the upper limit, the productivity decreases.

[0163] From the viewpoint of heat resistance, the glass transition temperature (Tg) of the non-thermoplastic polyimide layer 31 is preferably 280° C. or higher.

[0164] In addition, from the perspective of suppressing warping, the thermal expansion coefficient of the non-thermoplastic polyimide layer 31 is preferably in the range of 1 ppm / K to 30 ppm / K, preferably in the range of 1 ppm / K to 25 ppm / K, and more preferably in the range of 15 ppm / K to 25 ppm / K.

[0165] In addition, other curing resin components such as plasticizers, epoxy resins, curing agents, curing accelerators, coupling agents, fillers, solvents, flame retardants, etc. may be appropriately formulated as arbitrary components in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer 31. However, some plasticizers contain a large number of polar groups, and there is a concern that the plasticizers promote the diffusion of copper from the copper wiring, so it is preferred not to use plasticizers as much as possible.

[0166] Thermoplastic polyimide layer:

[0167] The thermoplastic polyimide constituting the thermoplastic polyimide layer 33 contains a tetracarboxylic acid residue and a diamine residue, and preferably contains an aromatic tetracarboxylic acid residue derived from an aromatic tetracarboxylic dianhydride and an aromatic diamine residue derived from an aromatic diamine.

[0168] (Tetracarboxylic acid residue)

[0169] As the tetracarboxylic acid residue used in the thermoplastic polyimide constituting the thermoplastic polyimide layer 33 , the same groups as exemplified as the tetracarboxylic acid residue in the non-thermoplastic polyimide constituting the non-thermoplastic polyimide layer can be used.

[0170] (Diamine residue)

[0171] As the diamine residue contained in the thermoplastic polyimide constituting the thermoplastic polyimide layer 33 , a diamine residue derived from a diamine compound represented by General Formula (B1) to General Formula (B7) is preferred.

[0172] [Chemistry 4]

[0173]

[0174] In formula (B1) to formula (B7), R1 independently represents a monovalent hydrocarbon group or alkoxy group having 1 to 6 carbon atoms, the linking group A independently represents a divalent group selected from -O-, -S-, -CO-, -SO-, -SO2-, -COO-, -CH2-, -C(CH3)2-, -NH- or -CONH-, and n1 independently represents an integer of 0 to 4. However, the part repeating with formula (B2) is removed from formula (B3), and the part repeating with formula (B4) is removed from formula (B5). Here, the so-called "independently" means that multiple linking groups A, multiple R1s or multiple n1s in one formula or two or more formulas in the formula (B1) to formula (B7) may be the same or different. Furthermore, in the formula (B1) to formula (B7), the hydrogen atoms in the two terminal amino groups may be substituted, for example, they may be -NR2R3 (here, R2 and R3 independently refer to any substituent such as an alkyl group).

[0175] The diamine represented by formula (B1) (hereinafter, sometimes referred to as "diamine (B1)") is an aromatic diamine having two benzene rings. It is believed that the diamine (B1) is in the meta position with the divalent linking group A through the amino group directly bonded to at least one benzene ring, and the degree of freedom of the polyimide molecular chain is increased and has high flexibility, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B1), the thermoplasticity of the polyimide is improved. Here, as the linking group A, preferably -O-, -CH2-, -C(CH3)2-, -CO-, -SO2-, -S-.

[0176] Examples of the diamine (B1) include 3,3'-diaminodiphenylmethane, 3,3'-diaminodiphenylpropane, 3,3'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylpropane, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminobenzophenone, and (3,3'-bisamino)diphenylamine.

[0177] The diamine represented by formula (B2) (hereinafter, sometimes referred to as "diamine (B2)") is an aromatic diamine having three benzene rings. It is believed that the diamine (B2) is in the meta position with the divalent linking group A through the amino group directly bonded to at least one benzene ring, and the degree of freedom of the polyimide molecular chain is increased and has high flexibility, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B2), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O- is preferred.

[0178] As a diamine (B2), 1, 4- bis (3-aminophenoxy) benzene, 3- [4- (4-aminophenoxy) phenoxy] aniline, 3- [3- (4-aminophenoxy) phenoxy] aniline, etc. are mentioned, for example.

[0179] The diamine represented by formula (B3) (hereinafter, sometimes referred to as "diamine (B3)") is an aromatic diamine having three benzene rings. It is believed that the diamine (B3) is in the meta position with two divalent linking groups A directly bonded to one benzene ring, and the degree of freedom of the polyimide molecular chain is increased and has high flexibility, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B3), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O- is preferred.

[0180] Examples of the diamine (B3) include 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,3-bis(3-aminophenoxy)benzene (APB), 4,4'-[2-methyl-(1,3-phenylene)bisoxy]dianiline, 4,4'-[4-methyl-(1,3-phenylene)bisoxy]dianiline, and 4,4'-[5-methyl-(1,3-phenylene)bisoxy]dianiline.

[0181] The diamine represented by formula (B4) (hereinafter, sometimes referred to as "diamine (B4)") is an aromatic diamine having four benzene rings. It is believed that the diamine (B4) has high flexibility due to the amino group directly bonded to at least one benzene ring and the divalent linking group A being in the meta position, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B4), the thermoplasticity of the polyimide is improved. Here, as the linking group A, preferably -O-, -CH2-, -C(CH3)2-, -SO2-, -CO-, -CONH-.

[0182] Examples of the diamine (B4) include bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]propane, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)]benzophenone, and bis[4,4′-(3-aminophenoxy)]benzanilide.

[0183] The diamine represented by formula (B5) (hereinafter, sometimes referred to as "diamine (B5)") is an aromatic diamine having four benzene rings. It is believed that the diamine (B5) is in the meta position with two divalent linking groups A directly bonded to at least one benzene ring, and the degree of freedom of the polyimide molecular chain is increased and has high flexibility, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B5), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O- is preferred.

[0184] Examples of the diamine (B5) include 4-[3-[4-(4-aminophenoxy)phenoxy]phenoxy]aniline and 4,4′-[oxybis(3,1-phenyleneoxy)]dianiline.

[0185] The diamine represented by formula (B6) (hereinafter, sometimes referred to as "diamine (B6)") is an aromatic diamine having four benzene rings. It is believed that the diamine (B6) has high flexibility due to having at least two ether bonds, which helps to improve the flexibility of the polyimide molecular chain. Therefore, by using diamine (B6), the thermoplasticity of the polyimide is improved. Here, as the linking group A, preferably -C(CH3)2-, -O-, -SO2-, -CO-.

[0186] Examples of the diamine (B6) include 2,2-bis[4-(4-aminophenoxy)phenyl]propane (2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), bis[4-(4-aminophenoxy)phenyl]ether (BAPE), bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), and bis[4-(4-aminophenoxy)phenyl]ketone (BAPK).

[0187] The diamine represented by formula (B7) (hereinafter, sometimes referred to as "diamine (B7)") is an aromatic diamine having four benzene rings. The diamine (B7) has a divalent linking group A with high flexibility on both sides of the diphenyl skeleton, and is therefore believed to contribute to the improvement of the flexibility of the polyimide molecular chain. Therefore, by using diamine (B7), the thermoplasticity of the polyimide is improved. Here, as the linking group A, -O- is preferred.

[0188] As a diamine (B7), bis[4-(3-aminophenoxy)]biphenyl, bis[4-(4-aminophenoxy)]biphenyl, etc. are mentioned, for example.

[0189] The thermoplastic polyimide constituting the thermoplastic polyimide layer 33 preferably contains diamine residues derived from at least one diamine compound selected from diamine (B1) to diamine (B7) in an amount of 60 mol parts or more, preferably in a range of 60 mol parts or more and 99 mol parts or less, and more preferably in a range of 70 mol parts or more and 95 mol parts or less, relative to 100 mol parts of all diamine residues. Since diamine (B1) to diamine (B7) contain a molecular structure having flexibility, by using at least one diamine compound selected from these in an amount within the above range, the flexibility of the polyimide molecular chain can be improved and thermoplasticity can be imparted. If the total amount of diamine (B1) to diamine (B7) in the raw material is less than 60 mol parts relative to 100 mol parts of all diamine components, sufficient thermoplasticity cannot be obtained due to insufficient flexibility of the polyimide resin.

[0190] In addition, as the diamine residue contained in the thermoplastic polyimide constituting the thermoplastic polyimide layer 33, it is also preferably a diamine residue derived from a diamine compound represented by the general formula (A1). About the diamine compound [diamine (A1)] represented by the formula (A1), as described in the description of the non-thermoplastic polyimide. Diamine (A1) has a rigid structure and has the effect of imparting an ordered structure to the polymer as a whole, so that the dielectric loss tangent or hygroscopicity can be reduced by suppressing the movement of molecules. And then, by being used as a raw material for thermoplastic polyimide, a polyimide with low air permeability and excellent long-term heat-resistant adhesion can be obtained.

[0191] The thermoplastic polyimide constituting the thermoplastic polyimide layer 33 may contain a diamine residue derived from the diamine (A1) in a range of preferably 1 mol part or more and 40 mol parts or less, more preferably 5 mol parts or more and 30 mol parts or less. By using the diamine (A1) in an amount within the above range and forming an ordered structure in the entire polymer by utilizing the rigid structure derived from the monomer, a thermoplastic polyimide having low air permeability and hygroscopicity and excellent long-term heat-resistant adhesiveness can be obtained.

[0192] The thermoplastic polyimide constituting the thermoplastic polyimide layer 33 may contain a diamine residue derived from a diamine compound other than the diamine (A1) and the diamines (B1) to (B7) within a range that does not impair the effects of the invention.

[0193] By selecting the types of the tetracarboxylic acid residue and the diamine residue in the thermoplastic polyimide, or the respective molar ratios when two or more tetracarboxylic acid residues or diamine residues are used, the thermal expansion coefficient, tensile elastic coefficient, glass transition temperature, etc. can be controlled. In addition, when there are a plurality of polyimide structural units in the thermoplastic polyimide, they may exist in the form of blocks or randomly, but preferably randomly.

[0194] Furthermore, by making both the tetracarboxylic acid residue and the diamine residue contained in the thermoplastic polyimide an aromatic group, the dimensional accuracy of the polyimide film in a high temperature environment can be improved, and the change amount of the in-plane retardation (RO) can be suppressed.

[0195] The imide group concentration of the thermoplastic polyimide is preferably 33% or less, more preferably 32% or more. Here, "imide group concentration" refers to the value obtained by dividing the molecular weight of the imide group (-(CO)2-N-) in the polyimide by the molecular weight of the entire structure of the polyimide. If the imide group concentration exceeds 33%, the molecular weight of the resin itself becomes smaller, and the low hygroscopicity is also deteriorated due to the increase in polar groups. By selecting a combination of the diamine compounds to control the orientation of the molecules in the thermoplastic polyimide, the increase in CTE associated with the decrease in the imide group concentration is suppressed, thereby ensuring low hygroscopicity.

[0196] The weight average molecular weight of the thermoplastic polyimide is preferably in the range of 10,000 to 400,000, and more preferably in the range of 50,000 to 350,000. If the weight average molecular weight is less than 10,000, the strength of the film is reduced and the film tends to be brittle. On the other hand, if the weight average molecular weight exceeds 400,000, the viscosity is excessively increased, and defects such as uneven film thickness and streaks are easily generated during coating.

[0197] The thermoplastic polyimide constituting the thermoplastic polyimide layer 33 is, for example, an adhesive layer in the insulating resin of the circuit substrate, so in order to suppress the diffusion of copper, a completely imidized structure is most preferably used. However, a portion of the polyimide may also be an amic acid. The imidization rate can be measured by using a Fourier transform infrared spectrophotometer (commercially available product: FT / IR620 manufactured by JASCO Corporation) and using a single reflection ATR method to measure the infrared absorption spectrum of the polyimide film at 1015 cm -1 Based on the benzene ring absorber nearby, according to 1780cm -1 The absorbance derived from the C=O expansion and contraction of the imide group was calculated.

[0198] From the viewpoint of ensuring the adhesive function, the thickness of the thermoplastic polyimide layer 33 is preferably within the range of 1 μm to 10 μm, and more preferably within the range of 1 μm to 5 μm. When the thickness of the thermoplastic polyimide layer 33 is less than the lower limit, the adhesiveness becomes insufficient, and when the thickness exceeds the upper limit, the dimensional stability tends to deteriorate.

[0199] From the viewpoint of suppressing warpage, the thermal expansion coefficient of the thermoplastic polyimide layer 33 is preferably 30 ppm / K or more, preferably 30 ppm / K or more and 100 ppm / K or less, and more preferably 30 ppm / K or more and 80 ppm / K or less.

[0200] In addition, the resin used in the thermoplastic polyimide layer 33 may include, in addition to polyimide, other curable resin components such as plasticizers, epoxy resins, curing agents, curing accelerators, inorganic fillers, coupling agents, fillers, solvents, flame retardants, etc. as arbitrary components.

[0201] The non-thermoplastic polyimide and thermoplastic polyimide used to form the non-thermoplastic polyimide layer 31 and the thermoplastic polyimide layer 33 can be manufactured in the same manner as the DDA-based polyimide by reacting anhydride components and diamine components in a solvent to generate polyamic acid and then heating the closed loop. In the synthesis of the non-thermoplastic polyimide and the thermoplastic polyimide, the anhydride and diamine can be used only one type, or two or more types can be used in combination. By selecting the types of anhydride and diamine, or the respective molar ratios when using two or more anhydrides or diamines, thermal expansion, adhesion, glass transition temperature, etc. can be controlled.

[0202] <Coefficient of thermal expansion>

[0203] In the metal-clad laminate 10, the thermal expansion coefficient (CTE) of the resin laminate 20 as a whole is preferably 10ppm / K or more, preferably in the range of 10ppm / K or more and 30ppm / K or less, and more preferably in the range of 15ppm / K or more and 25ppm / K or less. If the CTE is less than 10ppm / K or exceeds 30ppm / K, warping or reduced dimensional stability will occur. By appropriately changing the combination, thickness, and drying / hardening conditions of the raw materials used, a polyimide layer having a desired CTE can be produced.

[0204] <Dielectric loss tangent>

[0205] In the metal-clad laminate 10, the dielectric loss tangent (Tanδ) of the entire resin laminate 20 at 10GHz is preferably within a range of 0.02 or less, more preferably within a range of 0.0005 or more and 0.01 or less, and further preferably within a range of 0.001 or more and 0.008 or less. If the dielectric loss tangent of the entire resin laminate 20 at 10GHz exceeds 0.02, when applied to a circuit substrate, it is easy to cause an undesirable situation such as loss of electrical signals on the transmission path of high-frequency signals. On the other hand, the lower limit of the dielectric loss tangent of the entire resin laminate 20 at 10GHz is not particularly limited, but the physical property control of the insulating resin layer as a circuit substrate should be considered.

[0206] <Dielectric constant>

[0207] In the metal-clad laminate 10, when the resin laminate 20 is used as an insulating resin layer of a circuit board, for example, in order to ensure impedance matching, the dielectric constant of the resin laminate 20 as a whole at 10 GHz is preferably 4.0 or less. If the dielectric constant of the resin laminate 20 as a whole at 10 GHz exceeds 4.0, when used in a circuit board, the dielectric loss increases, and it is easy to cause disadvantages such as loss of electric signals in the transmission path of high-frequency signals.

[0208] [Manufacturing of Metal-Clad Laminated Plate]

[0209] The metal-clad laminate 10 can be manufactured, for example, in the following manner: prepare resin sheets corresponding to the first transmission loss suppression layer BS1, the second transmission loss suppression layer BS2, a plurality of dimensional accuracy maintaining layers PL and one or more intermediate transmission loss suppression layers BS3, arrange these resin sheets between the first metal layer M1 and the second metal layer M2, adhere them, and perform heat pressing.

[0210] The metal-clad laminate 10 of the present embodiment obtained in the above manner can be processed into a circuit board such as a single-sided FPC or a double-sided FPC by etching the first metal layer M1 and / or the second metal layer M2 to form a wiring circuit.

[0211] [Circuit board]

[0212] The metal-clad laminate 10 is mainly effectively used as a circuit substrate material such as an FPC and a rigid-flexible circuit substrate. By processing one or both of the first metal layer M1 and the second metal layer M2 of the metal-clad laminate 10 in a patterned manner using a conventional method to form a wiring layer, a circuit substrate such as an FPC as an embodiment of the present invention can be manufactured. Although the circuit substrate is omitted in the figure, it includes a resin laminate 20 and a wiring layer provided on one side or both sides of the resin laminate 20, which can reduce transmission loss even in high-frequency transmission and has excellent dimensional stability.

[0213] [Example]

[0214] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples. In the following examples, unless otherwise specified, various measurements and evaluations were performed based on the following contents.

[0215] [Viscosity measurement]

[0216] The viscosity was measured at 25° C. using an E-type viscometer (Brookfield, trade name: DV-II+Pro). The rotation speed was set so that the torque was 10% to 90%, and the value when the viscosity stabilized was read 2 minutes after the start of the measurement.

[0217] [Determination of storage elastic coefficient]

[0218] The resin sheet having a size of 5 mm×20 mm was measured using a dynamic viscoelasticity measuring apparatus (DMA: manufactured by UBM, trade name: E4000F) at a heating rate of 4° C. / min and a frequency of 11 Hz from 30° C. to 400° C.

[0219] [Determination of coefficient of thermal expansion (CTE)]

[0220] A thermomechanical analyzer (manufactured by Bruker, trade name: 4000SA) was used for a polyimide film of 3 mm × 20 mm size. The temperature was raised from 30°C to 265°C at a certain heating rate while applying a load of 5.0 g. The film was then kept at the temperature for 10 minutes and then cooled at a rate of 5°C / min to determine the average thermal expansion coefficient (thermal expansion coefficient) from 250°C to 100°C.

[0221] [Determination of dielectric constant and dielectric loss tangent]

[0222] The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin sheet at 10 GHz were measured using a vector network analyzer (manufactured by Agilent, trade name: E8363C) and a SPDR resonator. The material used in the measurement was left for 24 hours under the conditions of temperature: 24°C to 26°C and humidity: 45% to 55% RH.

[0223] [Measurement of dimensional change rate]

[0224] The measurement of the dimensional change rate is carried out by the following steps. First, using a 150 mm square sample, the dry film resist is exposed and developed at intervals of 100 mm to form a target for position measurement. The dimensions before etching (normal state) are measured in an environment with a temperature of 23±2°C and a relative humidity of 50±5%, and then the copper outside the target of the test piece is removed by etching (liquid temperature below 40°C, time within 10 minutes). Let it stand for 24±4 hours in an environment with a temperature of 23±2°C and a relative humidity of 50±5%, and then measure the dimensions after etching. Calculate the dimensional change rate relative to the normal state for each of the three locations in the longitudinal and transverse directions, and set the respective average values ​​as the dimensional change rate after etching. The dimensional change rate after etching is calculated by the following formula.

[0225] Dimension change rate after etching (%) = (BA) / A×100

[0226] A: Target distance before etching

[0227] B: Distance between targets after etching

[0228] Next, the test piece was heated in an oven at 250°C for 1 hour, and the distance between the position targets was measured. The dimensional change rate after etching was calculated for each of the three locations in the longitudinal and transverse directions, and the average value of each was set as the dimensional change rate after heating. The dimensional change rate after heating was calculated using the following formula.

[0229] Dimensional change rate after heating (%) = (CB) / B×100

[0230] B: Distance between targets after etching

[0231] C: Distance between targets after heating

[0232] [Measurement of Surface Roughness (Rz; Ten-Point Average Roughness) of Copper Foil]

[0233] The surface roughness was determined using a stylus surface roughness meter (manufactured by Kosaka Laboratory Co., Ltd., trade name: Surfcorder ET-3000) under the measurement conditions of force: 100 μN, speed: 20 μm, and range: 800 μm. The surface roughness was calculated according to the method of Japanese Industrial Standards (JIS)-B0601:1994.

[0234] The abbreviations used in the synthesis examples represent the following compounds.

[0235] BTDA: 3,3',4,4'-Benzophenonetetracarboxylic dianhydride

[0236] PMDA: Pyromellitic Dianhydride

[0237] BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride

[0238] BPADA: 2,2-Bis[4-(3,4-dicarboxyphenoxy)phenyl]propane dianhydride

[0239] DAPE: 4,4'-diaminodiphenyl ether

[0240] p-PDA: p-phenylenediamine

[0241] BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane

[0242] m-TB: 2,2'-dimethyl-4,4'-diaminobiphenyl

[0243] TPE-R: 1,3-bis(4-aminophenoxy)benzene

[0244] DDA: C36 aliphatic diamine (manufactured by Croda Japan Co., Ltd., trade name: PRIAMINE 1074, amine value: 205 mgKOH / g, mixture of dimer diamines of cyclic structure and chain structure, content of dimer component: 95 wt % or more)

[0245] OP935: Aluminum organic phosphonate (manufactured by Clariant Japan, trade name: Exolit OP935)

[0246] N-12: Dodecanedioic acid dihydrazide

[0247] DMAc: N,N-dimethylacetamide

[0248] NMP: N-methyl-2-pyrrolidone

[0249] (Synthesis example 1)

[0250] 312 g of DMAc was placed in a reaction container including a thermocouple and a stirrer and capable of introducing nitrogen. 14.67 g of DAPE (0.073 mol) was dissolved in the reaction container while stirring in the container. Then, 23.13 g of BTDA (0.072 mol) was added. Thereafter, stirring was continued for 3 hours to prepare a polyamic acid resin solution a having a solution viscosity of 2,960 mPa·s.

[0251] (Synthesis example 2)

[0252] 200 g of DMAc was placed in a reaction vessel including a thermocouple and a stirrer and capable of introducing nitrogen. 1.335 g of m-TB (0.0063 mole) and 10.414 g of TPE-R (0.0356 mole) were dissolved in the reaction vessel while stirring in the vessel. Then, 0.932 g of PMDA (0.0043 mole) and 11.319 g of BPDA (0.0385 mole) were added. Thereafter, stirring was continued for 2 hours to prepare a resin solution b of polyamic acid having a solution viscosity of 1,420 mPa·s.

[0253] (Synthesis example 3)

[0254] 250 g of DMAc was placed in a reaction vessel including a thermocouple and a stirrer and capable of introducing nitrogen. 2.561 g of p-PDA (0.0237 mole) and 16.813 g of DAPE (0.0840 mole) were dissolved in the reaction vessel while stirring in the vessel. Then, 18.501 g of PMDA (0.0848 mole) and 6.239 g of BPDA (0.0212 mole) were added. Thereafter, stirring was continued for 3 hours to prepare a resin solution c of polyamic acid having a solution viscosity of 29,500 mPa·s.

[0255] (Synthesis Example 4)

[0256] 250 g of DMAc was placed in a reaction vessel including a thermocouple and a stirrer and capable of introducing nitrogen. 12.323 g of m-TB (0.0580 mole) and 1.886 g of TPE-R (0.0064 mole) were dissolved in the reaction vessel while stirring in the vessel. Then, 8.314 g of PMDA (0.0381 mole) and 7.477 g of BPDA (0.0254 mole) were added. Thereafter, stirring was continued for 3 hours to prepare a resin solution d of polyamic acid having a solution viscosity of 31,500 mPa·s.

[0257] (Synthesis Example 5)

[0258] <Preparation of resin solution e for adhesive layer>

[0259] 44.92g of BTDA (0.139 mol), 75.08g of DDA (0.141 mol), 168g of NMP and 112g of xylene were placed in a 500mL four-necked flask with a nitrogen inlet tube, a stirrer, a thermocouple, a Dean-Stark trap and a cooling tube, and mixed at 40°C for 30 minutes to prepare a polyamic acid solution. The polyamic acid solution was heated to 190°C and heated and stirred for 4 hours, and the distilled water and xylene were removed to the outside of the system. Thereafter, it was cooled to 100°C, 112g of xylene was added and stirred, and then cooled to 30°C, thereby completing imidization, thereby obtaining a resin solution e (solid content: 29.5% by weight) for an adhesive layer.

[0260] (Synthesis Example 6)

[0261] <Preparation of resin solution f for adhesive layer>

[0262] A polyamic acid solution was prepared in the same manner as in Synthesis Example 5 except that 42.51 g of BPADA (0.082 mol), 34.30 g of DDA (0.066 mol), 6.56 g of BAPP (0.016 mol), 208 g of NMP and 112 g of xylene were used as the raw material composition. The polyamic acid solution was treated in the same manner as in Synthesis Example 5 to obtain a resin solution f for an adhesive layer (solid content: 30.0 wt %).

[0263] (Production example 1)

[0264] <Preparation of polyimide film>

[0265] The resin solution c of polyamic acid is uniformly applied to one surface of an electrolytic copper foil 1 (thickness 12 μm, Rz: 2.1 μm) so that the thickness after curing is about 25 μm, and then heated and dried at 120°C to remove the solvent. Furthermore, a stepwise heat treatment is performed from 120°C to 360°C within 30 minutes to complete imidization. An aqueous solution of ferric chloride is used to etch and remove the copper foil to prepare a polyimide film 1 (thickness: 25 μm, Dk: 3.4, Df: 0.0085, CTE: 16 ppm / K, storage elastic coefficient minimum value (100°C to 250°C) 2.9 GPa).

[0266] (Production example 2)

[0267] <Preparation of polyimide film>

[0268] A polyimide film 2 (thickness: 25 μm, Dk: 3.3, Df: 0.0034, CTE: 17 ppm / K, storage elastic modulus minimum value (100° C. to 250° C.) 3.0 GPa) was prepared in the same manner as in Preparation Example 1 except that the resin solution d was used.

[0269] (Production example 3)

[0270] <Preparation of polyimide film>

[0271] Resin solution a is uniformly applied to a single surface of an electrolytic copper foil 1 (thickness 12 μm, Rz: 2.1 μm) in such a manner that the thickness after curing becomes about 2 μm to 3 μm, and then heated and dried at 120°C to remove the solvent. Subsequently, resin solution d is uniformly applied thereon in such a manner that the thickness after curing becomes about 21 μm, and then heated and dried at 120°C to remove the solvent. Furthermore, resin solution a is uniformly applied thereon in such a manner that the thickness after curing becomes about 2 μm to 3 μm, and then heated and dried at 120°C to remove the solvent. In the above manner, a three-layer polyamic acid layer is formed, and then a staged heat treatment is performed from 120°C to 360°C to complete imidization. The copper foil layer was etched away using an aqueous ferric chloride solution to prepare a polyimide film 3 (thickness: 25 μm, Dk: 3.4, Df: 0.0052, CTE: 21 ppm / K, storage elastic coefficient minimum value (100° C. to 250° C.) 2.8 GPa).

[0272] (Production example 4)

[0273] <Preparation of polyimide film>

[0274] Resin solution b is evenly applied to a single surface of an electrolytic copper foil 1 (thickness 12 μm, Rz: 2.1 μm) in such a manner that the thickness after curing becomes about 2 μm to 3 μm, and then heated and dried at 120°C to remove the solvent. Subsequently, resin solution d is evenly applied thereon in such a manner that the thickness after curing becomes about 21 μm, and then heated and dried at 120°C to remove the solvent. Furthermore, resin solution b is evenly applied thereon in such a manner that the thickness after curing becomes about 2 μm to 3 μm, and then heated and dried at 120°C to remove the solvent. In the above manner, a three-layer polyamic acid layer is formed, and then a staged heat treatment is performed from 120°C to 360°C to complete imidization. The copper foil layer was etched away using an aqueous ferric chloride solution to prepare a polyimide film 4 (thickness: 25 μm, Dk: 3.3, Df: 0.0032, CTE: 23 ppm / K, storage elastic coefficient minimum value (100° C. to 250° C.) 2.7 GPa).

[0275] (Production example 5)

[0276] <Preparation of resin sheet>

[0277] 1.8 g of N-12 (0.0036 mol) and 12.5 g of OP935 were mixed in 169.49 g of resin solution e (solid content: 50 g), and 6.485 g of NMP and 19.345 g of xylene were added for dilution to prepare a polyimide varnish 1.

[0278] The polyimide varnish 1 was applied to the silicone-treated surface of the release substrate so as to have a thickness of 25 μm after drying, and then dried by heating at 80° C. and peeled from the release substrate to prepare a resin sheet 1. The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin sheet 1 were 2.7 and 0.0023, respectively.

[0279] (Production example 6)

[0280] <Preparation of resin sheet>

[0281] A resin sheet 2 was prepared in the same manner as in Production Example 6 except that the thickness after drying was 50 μm. The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin sheet 2 were 2.7 and 0.0023, respectively.

[0282] (Production example 7)

[0283] <Preparation of resin sheet>

[0284] The resin sheet 3 was prepared in the same manner as in Production Example 6 except that the thickness after drying was 75 μm. The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin sheet 3 were 2.7 and 0.0023, respectively.

[0285] (Production example 8)

[0286] <Preparation of resin sheet>

[0287] A resin sheet 4 was prepared in the same manner as in Production Example 6 except that the thickness after drying was 5 μm. The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin sheet 4 were 2.7 and 0.0023, respectively.

[0288] (Production example 9)

[0289] <Preparation of resin sheet>

[0290] The resin solution f for the adhesive layer was applied to the silicone-treated surface of the release substrate so that the thickness after drying was 25 μm, and then heated and dried at 80° C. and peeled from the release substrate to prepare a resin sheet 5. The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin sheet 5 were 2.8 and 0.0028, respectively.

[0291] (Production example 10)

[0292] <Preparation of resin sheet>

[0293] A resin sheet 6 was prepared in the same manner as in Production Example 9 except that the thickness after drying was 50 μm. The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin sheet 6 were 2.8 and 0.0028, respectively.

[0294] [Example 1]

[0295] Two electrolytic copper foils 1, two resin sheets 1, one resin sheet 2, and two polyimide films 4 were prepared, and stacked in the order of electrolytic copper foil 1 / resin sheet 1 / polyimide film 4 / resin sheet 2 / polyimide film 4 / resin sheet 1 / electrolytic copper foil 1, and then thermally pressed at 160° C. and 4 MPa for 60 minutes to prepare a double-sided metal-clad laminate 1. The results of the evaluation of the double-sided metal-clad laminate 1 are as follows.

[0296] Dimensional change rate after etching in the machine direction (MD): -0.05%

[0297] Transverse Direction (TD) dimensional change after etching: -0.04%

[0298] Dimensional change rate after heating in MD direction: -0.03%

[0299] Dimensional change rate after heating in TD direction: 0.03%

[0300] The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 1 (thickness: 150 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal-clad laminate 1 were 2.9 and 0.0026, respectively. The total thickness of the dimensional accuracy maintaining layer was 33% of the total thickness of the resin laminate 1.

[0301] [Example 2]

[0302] Two electrolytic copper foils 1, two resin sheets 1, one resin sheet 3, and two polyimide films 4 were prepared, and stacked in the order of electrolytic copper foil 1 / resin sheet 1 / polyimide film 4 / resin sheet 3 / polyimide film 4 / resin sheet 1 / electrolytic copper foil 1, and then thermally pressed at 160° C. and 4 MPa for 60 minutes to prepare a double-sided metal-clad laminate 2. The results of the evaluation of the double-sided metal-clad laminate 2 are as follows.

[0303] Dimensional change rate after etching in MD direction: -0.06%

[0304] Dimension change rate after etching in TD direction: -0.04%

[0305] Dimensional change rate after heating in MD direction: -0.04%

[0306] Dimensional change rate after heating in TD direction: 0.04%

[0307] The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 2 (thickness: 175 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal-clad laminate 2 were 2.92 and 0.0026, respectively. The total thickness of the dimensional accuracy maintaining layer was 29% of the total thickness of the resin laminate 2.

[0308] [Example 3]

[0309] Two electrolytic copper foils 1, one resin sheet 1, two resin sheets 2, and two polyimide films 4 were prepared, and stacked in the order of electrolytic copper foil 1 / resin sheet 2 / polyimide film 4 / resin sheet 1 / polyimide film 4 / resin sheet 2 / electrolytic copper foil 1, and then thermally pressed for 60 minutes at 160° C. and 4 MPa to prepare a double-sided metal-clad laminate 3. The results of the evaluation of the double-sided metal-clad laminate 3 are as follows.

[0310] Dimensional change rate after etching in MD direction: -0.02%

[0311] Dimension change rate after etching in TD direction: 0.03%

[0312] Dimensional change rate after heating in MD direction: -0.06%

[0313] Dimensional change rate after heating in TD direction: -0.02%

[0314] The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 3 (thickness: 175 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal-clad laminate 3 were 2.9 and 0.0026, respectively. The total thickness of the dimensional accuracy maintaining layer was 29% of the total thickness of the resin laminate 3.

[0315] [Example 4]

[0316] The double-sided metal-clad laminate 4 was prepared in the same manner as in Example 1 except that the polyimide film 1 was used instead of the polyimide film 4. The double-sided metal-clad laminate 4 was evaluated, and the result showed that there was no problem with the dimensional change. In addition, the dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 4 (thickness: 150 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal-clad laminate 4 were 2.9 and 0.0044, respectively. The total thickness of the dimensional accuracy maintenance layer was 33% of the total thickness of the resin laminate 4.

[0317] [Example 5]

[0318] The double-sided metal-clad laminate 5 was prepared in the same manner as in Example 1 except that the polyimide film 2 was used instead of the polyimide film 4. The double-sided metal-clad laminate 5 was evaluated, and the result showed that there was no problem with the dimensional change. In addition, the dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 5 (thickness: 150 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal-clad laminate 5 were 2.9 and 0.0027, respectively. The total thickness of the dimensional accuracy maintenance layer was 33% of the total thickness of the resin laminate 5.

[0319] [Example 6]

[0320] The double-sided metal-clad laminate 6 was prepared in the same manner as in Example 1 except that the polyimide film 3 was used instead of the polyimide film 4. The double-sided metal-clad laminate 6 was evaluated, and the result showed that there was no problem with the dimensional change. In addition, the dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 6 (thickness: 150 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal-clad laminate 6 were 2.9 and 0.0033, respectively. The total thickness of the dimensional accuracy maintenance layer was 33% of the total thickness of the resin laminate 6.

[0321] [Example 7]

[0322] The double-sided metal laminate 7 was prepared in the same manner as in Example 1, except that the resin sheet 5 was used instead of the resin sheet 1 and the resin sheet 6 was used instead of the resin sheet 2. The double-sided metal laminate 7 was evaluated, and the result showed that there was no problem with the dimensional change. In addition, the dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 7 (thickness: 150 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal laminate 7 were 3.0 and 0.0029, respectively. The total thickness of the dimensional accuracy maintenance layer was 33% of the overall thickness of the resin laminate 7.

[0323] [Example 8]

[0324] The double-sided metal-clad laminate 8 was prepared in the same manner as in Example 1 except that the resin sheet 4 was used instead of the resin sheet 1. The double-sided metal-clad laminate 8 was evaluated, and the result showed that there was no problem with the dimensional change. In addition, the dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 8 (thickness: 110 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal-clad laminate 8 were 3.0 and 0.0027, respectively. The total thickness of the dimensional accuracy maintenance layer was 45% of the overall thickness of the resin laminate 8.

[0325] [Comparative Example 1]

[0326] Two electrolytic copper foils 1, two resin sheets 2, and one polyimide film 1 were prepared, and stacked in the order of electrolytic copper foil 1 / resin sheet 2 / polyimide film 1 / resin sheet 2 / electrolytic copper foil 1, and then thermally pressed for 60 minutes at 160° C. and 4 MPa to prepare a double-sided metal-clad laminate 9. The results of the evaluation of the double-sided metal-clad laminate 9 are as follows.

[0327] Dimensional change rate after etching in MD direction: 0.02%

[0328] Dimension change rate after etching in TD direction: 0.08%

[0329] Dimensional change rate after heating in MD direction: -0.10%

[0330] Dimensional change rate after heating in TD direction: -0.05%

[0331] The dielectric constant (Dk) and dielectric loss tangent (Df) of the resin laminate 9 (thickness: 125 μm) prepared by etching away the electrolytic copper foil 1 in the double-sided metal-clad laminate 9 were 2.8 and 0.0035, respectively. The total thickness of the dimensional accuracy maintaining layer was 20% of the total thickness of the resin laminate 9.

[0332] As mentioned above, although embodiment of this invention was described in detail for the purpose of illustration, this invention is not limited to the said embodiment, Various deformation|transformation is possible.

Claims

1. A metal-clad laminate comprising: The first metal layer, a first transmission loss suppression layer disposed in contact with one side of the first metal layer, The second metal layer a second transmission loss suppression layer disposed in contact with one side of the second metal layer, and a plurality of resin layers interposed between the first transmission loss suppression layer and the second transmission loss suppression layer, and The first transmission loss suppression layer, the second transmission loss suppression layer, and the plurality of resin layers form a resin laminate. The resin laminate has At least two dimensional accuracy maintenance layers, and an intermediate transmission loss suppression layer stacked between the dimensional accuracy maintaining layers, and Satisfy the following conditions i and ii; Condition i: when the dielectric loss tangent of the first transmission loss suppression layer and the second transmission loss suppression layer is set to Df1 and the dielectric loss tangent of the dimensional accuracy maintaining layer is set to Df2, the relationship of Df1<Df2 exists, and the dielectric loss tangent is the dielectric loss tangent at 10 GHz measured by separating the dielectric resonator after humidity adjustment at constant temperature and humidity conditions of 23°C and 50%RH for 24 hours; Condition ii: The total thickness of the dimensional accuracy maintaining layers is within a range of 25% to 60% of the total thickness of the resin laminate, The dielectric loss tangent Tanδ of the resin laminate as a whole at 10 GHz is within the range of 0.0005 or more and 0.01 or less, The first transmission loss suppression layer, the second transmission loss suppression layer and the intermediate transmission loss suppression layer are made of the same material.

2. The metal-clad laminate according to claim 1, wherein: The dimensional accuracy maintaining layer is a low thermal expansion polyimide layer having a minimum storage elastic coefficient in a temperature range of 100° C. to 250° C. within a range of 1.0 GPa to 8.0 GPa and a thermal expansion coefficient within a range of 15 ppm / K to 25 ppm / K.

3. The metal-clad laminate according to claim 1 or 2, wherein: The resin constituting the first transmission loss suppression layer and the second transmission loss suppression layer is a polyimide formed by reacting an acid anhydride component and a diamine component, and contains 50 mol parts or more of a dimer diamine relative to 100 mol parts of the total amount of the diamine component, and the two terminal carboxylic acid groups of the dimer acid of the dimer diamine are substituted with a primary aminomethyl group or an amino group.

4. A circuit substrate, comprising: The first wiring layer, a first transmission loss suppression layer provided in contact with one side of the first wiring layer, The second wiring layer, a second transmission loss suppression layer provided in contact with one side of the second wiring layer, and a plurality of resin layers interposed between the first transmission loss suppression layer and the second transmission loss suppression layer, and The first transmission loss suppression layer, the second transmission loss suppression layer, and the plurality of resin layers form a resin laminate. The resin laminate has At least two dimensional accuracy maintenance layers, and an intermediate transmission loss suppression layer stacked between the dimensional accuracy maintaining layers, and Satisfy the following conditions i and ii; Condition i: when the dielectric loss tangent of the first transmission loss suppression layer and the second transmission loss suppression layer is set to Df1 and the dielectric loss tangent of the dimensional accuracy maintaining layer is set to Df2, the relationship of Df1<Df2 exists, and the dielectric loss tangent is the dielectric loss tangent at 10 GHz measured by separating the dielectric resonator after humidity adjustment at constant temperature and humidity conditions of 23°C and 50%RH for 24 hours; Condition ii: The total thickness of the dimensional accuracy maintaining layers is within a range of 25% to 60% of the total thickness of the resin laminate, The dielectric loss tangent Tanδ of the resin laminate as a whole at 10 GHz is within the range of 0.0005 or more and 0.01 or less, The first transmission loss suppression layer, the second transmission loss suppression layer and the intermediate transmission loss suppression layer are made of the same material.