Negative electrode active material for lithium secondary battery, preparation method thereof, and lithium secondary battery comprising the same

By using high-pressure molded porous silicon-carbonaceous material composites in lithium-ion secondary batteries, the problem of battery performance degradation caused by volume changes in silicon-based anode materials is solved, achieving higher capacity and stability, and is suitable for electric vehicles High performance requirements of automobiles.

CN113169321BActive Publication Date: 2024-10-29POSCO HLDG INC +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201980079152.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-08-13
Publication Date
2024-10-29
Estimated Expiration
2039-08-13

AI Technical Summary

Technical Problem

In lithium-ion secondary batteries, the volume change of the silicon-based anode material leads to the formation of the solid electrolyte interface layer and electrode peeling, resulting in a sharp reduction in battery performance and unable to meet the high capacity and long life requirements of electric vehicles.

Method used

By embedding nano-silica particles in carbonaceous materials and using a high-pressure molding process to form a porous silicon-carbonaceous material composite, the specific surface area and carbonization yield are controlled, the formation of the solid electrolyte interface layer is suppressed, and the stability of the battery is improved. and capacity characteristics.

Benefits of technology

It effectively suppresses the formation of the solid electrolyte interface layer, reduces electrode expansion and contraction, improves the electrochemical performance and life of lithium-ion secondary batteries, increases capacity characteristics, and meets the high-performance needs of electric vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113169321B_ABST
    Figure CN113169321B_ABST
Patent Text Reader

Abstract

One embodiment of the present invention provides a negative electrode active material for lithium secondary batteries. The negative electrode active material for lithium secondary batteries is a porous silicon-carbon composite material containing multiple nano-silicon particles embedded in a carbonaceous material and including multiple pores. The carbonaceous material includes graphite particles, soft carbon, hard carbon, or combinations thereof. Relative to 100% by weight of the porous silicon-carbon composite material, the weight ratio of the graphite particles to the soft carbon, the hard carbon, or combinations thereof is 1:5 to 5:1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a negative electrode active material for a lithium secondary battery, a preparation method thereof, and a lithium secondary battery comprising the negative electrode active material. Background Art

[0002] As the demand for capacity increases due to the high performance of portable home appliances and mobile phones and environmental issues become the focus, lithium-ion secondary batteries (LIBs) are being researched and invested heavily as the most powerful and efficient energy system for driving electric vehicles, which are proposed as an alternative to internal combustion engines using fossil fuels.

[0003] Lithium-ion secondary batteries are composed of positive electrode materials, negative electrode materials, separation membranes, and electrolytes. The performance and activity of the battery are closely related to the components. Among them, since the development of LIB in 1991, hard / soft carbon or graphite materials, which are carbon allotropes, have been used as negative electrode active materials for nearly 30 years.

[0004] Graphite, which is now widely used as a negative electrode material for lithium-ion secondary batteries, has advantages in low operating voltage, stable life characteristics, efficiency, price and environmental protection. However, due to the theoretical capacity limit of 372mAh / g, there are problems to be overcome in ensuring the driving distance of electric vehicles and various application fields.

[0005] As a new generation of materials considered to overcome the capacity of graphite, there can be, for example, oxides of various elements (Fe3O4: 924mAh / g, FeO: 744mAh / g, Co3O4: 890mAh / g, NiO: 718mA / g, SnO2: 781mAh / g, etc.) and Group 4 elements represented by Si (Si: 4200mAh / g, Sn: 994mAh / g, Ge: 1600mAh / g). Among them, Si can be said to be the material that is most actively researched for the development of high-capacity electrodes.

[0006] Theoretically, silicon-based negative electrode materials are known to have a capacity more than 10 times higher than commercial graphite-based negative electrode materials. However, the problem that silicon negative electrode materials change in volume by about 4 times with repeated charging and discharging, and even the battery performance decreases sharply due to particle cracking or electrode peeling, has always been a stumbling block to commercialization.

[0007] At this time, if we consider that when lithium ions are inserted, the salt and solution of the electrolyte form a solid electrolyte interphase (SEI) on the Si surface, then cracks occur on the SEI surface due to the shrinkage / expansion of the electrode, and SEI is formed again on the newly exposed surface. Due to this repeated phenomenon, the diffusion path of Li ions increases, the consumption of the electrolyte increases, the conductivity deteriorates, and the coulombic efficiency deteriorates, which ultimately results in the battery being unusable. Summary of the invention

[0008] Technical issues to be solved

[0009] One embodiment of the present invention provides a Si-based negative electrode active material including primary particles with a minimized specific surface area and high-density secondary particles to suppress SEI formation. Specifically, a negative electrode active material for lithium secondary batteries is provided that controls the weight range of asphalt, the temperature increase conditions of the secondary particles, the co-carbonization effect with petroleum asphalt, etc. in order to reduce the carbonization yield variation of asphalt.

[0010] Therefore, it is possible to provide a negative electrode active material for a lithium secondary battery having an increased carbonization yield and a reduced specific surface area.

[0011] Solutions to technical problems

[0012] Embodiments of the present invention are described in detail below. However, these are merely examples and the present invention is not limited thereto. The present invention is defined only by the scope of the claims described below.

[0013] The negative electrode active material for a lithium secondary battery in one embodiment of the present invention is a composite material in which a plurality of nano-silicon particles are embedded in a carbonaceous material and compressed under high pressure to minimize the specific surface area. The carbonaceous material may include graphite particles, easily graphitized carbon (soft carbon), hardly graphitized carbon (hard carbon) or a combination thereof.

[0014] First, the porous silicon-carbonaceous material composite has a plurality of nano-silicon particles embedded in the carbonaceous material, and is in a form in which pores are minimized by means of a high-pressure molding process.

[0015] This state corresponds to a state in which the plurality of nano-silicon particles are embedded in the carbonaceous material even when the volume of the plurality of nano-silicon particles expands or contracts, thereby being able to maintain electrical contact with the internal constituent material.

[0016] In addition, the composite material that is highly densified by the pressurization process plays a role in controlling volume expansion during charging and minimizing short circuits during discharge. This composite material can exhibit stable electrochemical performance depending on the type and amount of silicon input and the type and bonding properties of the binder pitch that maintains a network with graphite.

[0017] The nano silicon particles may be particles controlled at the nanometer level by irradiating carbon dioxide laser on silane gas, or specifically, nano silicon particles having a carbon coating by thermally decomposing acetylene gas at high temperature and then depositing it on the surface of the nano silicon particles.

[0018] In addition, the nano silicon particles can be dry-synthesized by thermal deposition, chemical deposition (CVD), physical deposition (PVD), electromagnetic melting, and simultaneous volatilization, and do not require an additional pulverization process. Specifically, the average particle size (D50) of the nano silicon particles can be 30 to 100 nm, preferably, in the range of 40 to 50 nm.

[0019] At this time, the carbonaceous material may be graphite particles, soft carbon, hard carbon or a combination thereof.

[0020] Specifically, when graphite particles are included, the long life characteristics can be supplemented due to the excellent reversibility of graphite. In addition, the particle size (D50) of the graphite may be 10 to 40 μm.

[0021] The soft carbon may be derived from pitch. Therefore, when pitch is used, structural stability may be enhanced after carbonization by heat treatment.

[0022] The hard carbon may be derived from a binder used in a method for preparing a negative electrode active material for a lithium secondary battery described below.

[0023] Specifically, the weight ratio of the graphite particles to the easily graphitizable carbon, the hardly graphitizable carbon, or a combination thereof may be 1:5 to 5:1 relative to 100 weight % of the porous silicon-carbonaceous material composite.

[0024] More specifically, when the weight ratio of the carbonaceous material is within the above range, the specific surface area of ​​the nano-silicon-carbonaceous material composite can be 20 m 2 / g or less. Specifically, it can be 10m 2 / g or less. More specifically, it can be 5m 2 / g or less.

[0025] More specifically, when the weight of the graphitizable carbon derived from pitch is greater than that of graphite as described above, the specific surface area of ​​the negative electrode active material can be reduced.

[0026] The porous silicon-carbonaceous material composite may contain 30 to 40 wt % of nano-silicon and 60 to 70 wt % of carbonaceous material particles relative to 100 wt %.

[0027] When the content of nano-silicon satisfies the above range, while ensuring excellent capacity characteristics, for a battery using the negative electrode active material of this embodiment, it is very advantageous because it can suppress the volume expansion of the electrode caused by the progress of charge and discharge.

[0028] In addition, the average particle size (D50) of the nano-silicon particles may be 30 to 100 nm.

[0029] As described above, with silicon particles having an average particle size of nanometers, volume expansion caused by battery charging and discharging can be minimized.

[0030] The binder material used to form the porous silicon-carbonaceous material composite is carbonized to become non-graphitizable carbon. This non-graphitizable carbon will degrade the properties of the silicon-carbonaceous material composite. To prevent this, a polymer material having a residual carbon content of 5 to 10% after carbonization by heat treatment is more suitable.

[0031] In addition, the asphalt is carbonized to become the above-mentioned graphitized carbon (soft carbon). The asphalt can also play the role of a binder that stably supports the silicon / carbon composite structure. Therefore, the difficult-graphitized carbon and the easily graphitized carbon are dispersed between the pores of the porous silicon-carbonaceous material complex, so that when the negative electrode active material of an embodiment of the present invention is applied to a battery, even if the charge and discharge cycles are repeated, the porous structure of the silicon-carbonaceous material complex can be prevented from collapsing.

[0032] The volume of the pores may be 3 volume % or less, and specifically, 1 to 3 volume %, relative to the entire volume (100 volume %) of the negative electrode active material.

[0033] When the porosity of the negative electrode active material meets the above range, the volume expansion of silicon can be effectively alleviated.

[0034] The D50 particle size of the negative electrode active material may be 8 to 15 μm.

[0035] When the D50 particle size of the negative electrode active material exceeds the above range, the particles may be damaged by the rollers when the electrode is rolled after coating, which may lead to a decrease in overall performance such as battery efficiency, life, and electrode expansion rate.

[0036] In addition, the negative electrode active material may have a carbon coating on its surface.

[0037] Specifically, relative to 100 weight % of the negative electrode active material, the deposition amount of the carbon coating layer may be 3 to 15 weight %.

[0038] As described above, when the surface of the negative electrode active material further has a carbon coating, the specific surface area of ​​the negative electrode active material can be further reduced.

[0039] Another embodiment of the present invention may include a method for preparing a negative electrode active material for a lithium secondary battery, comprising: preparing a porous silicon-carbonaceous material mixed powder by mixing nano-silicon particles, graphite particles and asphalt particles by dry grinding; preparing a mixed solution by adding the porous silicon-carbonaceous material mixed powder and a binder into distilled water; preparing primary particles by spray-drying the mixed solution; preparing secondary particles by loading the primary particles into a mold and press-molding them; heat-treating the secondary particles; and crushing and classifying the heat-treated secondary particles.

[0040] First, a step of preparing a porous silicon-carbonaceous material mixed powder by mixing nano-silicon particles, graphite particles, and pitch particles by dry grinding may be performed.

[0041] In this case, the nano silicon particles are the same as those described above in the negative electrode active material for lithium secondary battery, and thus are omitted.

[0042] In the step of preparing the porous-carbonaceous material mixed powder, the pitch particles may be included in an amount of 30 wt % or more relative to 100 wt % of the porous-carbonaceous material mixed powder.

[0043] Specifically, relative to 100 wt % of the porous-carbonaceous material mixed powder, 30 to 40 wt % of nano silicon particles, 10 to 30 wt % of graphite particles, and 30 to 50 wt % of pitch may be included.

[0044] In this case, the weight of the pitch may be greater than the weight of the graphite.

[0045] Specifically, the weight ratio of the asphalt to the graphite may be 1:1 to 5:1.

[0046] When the mixed powder is prepared by mixing the pitch and the graphite in the aforementioned weight range, the carbonization yield can be increased and the specific surface area of ​​the prepared negative electrode active material can be reduced even after the heat treatment step is performed later. Therefore, a negative electrode active material with a high tap density can be provided.

[0047] More specifically, the asphalt may include coal-based asphalt, petroleum-based asphalt, or a combination thereof.

[0048] Specifically, when the petroleum-based pitch is combined with the coal-based pitch, the weight of the coal-based pitch may be greater than the weight of the petroleum-based pitch.

[0049] More specifically, the weight ratio of the coal-based asphalt to the petroleum-based asphalt may be 5:5 to 9:1 relative to 100 weight % of the asphalt.

[0050] When coal-based pitch is used as described above, the adhesion and yield are high. When petroleum-based pitch is compared with the structure of the same softening point, the permeability into the pores is excellent due to its high fluidity, but there is a high possibility of defects in adhesion and yield. Therefore, when coal-based pitch is mixed with petroleum-based pitch according to the above weight, a negative electrode active material with excellent carbonization yield can be obtained even after the later heat treatment step.

[0051] In addition, the pitch preferably has fixed carbon and coking value as high as possible. However, if the softening point of the pitch is excessively increased, the unit price of the pitch will increase and the processability will be disadvantageous. It is important to select the appropriate level of softening point and yield.

[0052] More specifically, the fixed carbon value of the asphalt may be 70 or more.

[0053] The more the fixed carbon value of the asphalt increases, the more conductive paths can be generated with Si, which has low conductivity, to induce increased capacity and efficiency. When the fixed carbon value meets the above range, the internal pores of the negative electrode active material of this embodiment can be reduced. Therefore, the side reaction with the electrolyte will also be reduced, which will help increase the initial efficiency of the battery.

[0054] The β-resin value of the asphalt may be 20 or more.

[0055] Specifically, the β-resin value means the value of excluding the quinoline soluble amount from the benzene insoluble amount. This β-resin value is proportional to the adhesiveness. In one embodiment of the present invention, the asphalt containing the β-resin value satisfies the range, so that the porous structure of the porous silicon-carbonaceous material composite can be maintained more stably. Therefore, a lithium secondary battery with excellent life characteristics and plate expansion characteristics can be embodied.

[0056] In addition, asphalt can be finely crushed into a few μm level for application.

[0057] In addition, the graphite used may have battery grade purity and be controlled to have a particle size of several μm to several tens of μm for the preparation of primary particles.

[0058] When the graphite particles, asphalt particles and nano silicon particles are mixed by dry grinding (dry grinding) as described above and the negative electrode active material is applied to a battery, the nano silicon particles can maintain electrical contact with other materials even under the volume expansion and contraction phenomenon caused by cycling. Specifically, the graphite particles and asphalt particles can control the expansion of the nano silicon particles.

[0059] In addition, the grinding process may utilize mechanical fusion or ball milling, but the present invention is not limited thereto, and any process may be used as long as the medium contacts the powder.

[0060] Then, a step of adding the porous silicon-carbonaceous material mixed powder and a binder into distilled water to prepare a mixed solution may be performed.

[0061] At this time, the adhesive may include an organic adhesive, a water-based adhesive or a combination thereof. Specifically, the adhesive may be a water-based adhesive. When a water-based adhesive is used, equipment investment is small and the process can be simpler.

[0062] Specifically, the water-based adhesive may include polyacrylic acid (PAA), gum Arabic, polyvinyl alcohol (PVA), polyethylene glycol (PEG), Pluronic ( F-127) and at least one of the group consisting of cellulose compounds.

[0063] Specifically, one embodiment of the present invention uses a water-based binder, and thus a water-based slurry can be used.

[0064] At this time, the binder may be contained in an amount of 15 parts by weight or less based on 100 parts by weight of the porous silicon-carbonaceous material mixed powder.

[0065] Specifically, when the content of the binder is within the above range, the dispersion of the porous silicon-carbonaceous material mixed powder and the pitch in the mixed solution can be stimulated.

[0066] As described later, the binder becomes hard carbon after the heat treatment step.

[0067] Specifically, the mixed powder and the binder are added to distilled water and then dispersed sufficiently for more than 1 hour by ultrasonic wave to prepare a colloidal mixed solution.

[0068] On the other hand, if solvents such as ethanol, isopropyl alcohol (IPA), acetone, etc. are used as the solvent of the mixed solution instead of distilled water, the bonding force between the nano-silicon particles and the graphite particles and asphalt particles will be reduced, and the performance of the battery using it will be low.

[0069] A step of spray-drying the mixed solution to prepare primary particles may be performed.

[0070] Specifically, the mixed solution prepared above is spray-dried using a spray device, thereby preparing spherical primary particles.

[0071] Specifically, when the spray drying process is not performed, there is a limitation in uniformly dispersing the nano-silicon particles, graphite particles, and pitch particles.

[0072] That is, the dispersion effect cannot be expected by only using the dry milling process or the spray drying process. Therefore, when the dispersion effect is low, when the battery is used to measure the electrochemical performance, it will cause side effects such as poor life and severe swelling.

[0073] The step of placing the primary particles into a mold and press-molding to prepare secondary particles may be performed.

[0074] When the secondary particles are prepared by pressure molding as described above, the density can be increased.

[0075] Specifically, the step of preparing the secondary particles may be performed at a temperature ranging from 50 to 100° C. higher than the softening point of the asphalt.

[0076] The softening point of the asphalt used in one embodiment of the present invention may be 250° C. or higher.

[0077] Therefore, when pressure molding is performed within the temperature range, pores existing in the porous silicon-carbon material can be minimized.

[0078] Specifically, when the temperature range during press molding is controlled to be 50 to 100°C higher than the softening point of the asphalt, the asphalt has viscosity and can fill the pores existing in the porous silicon-carbonaceous material. When used in a battery, the pores in the composite provide a place for side reactions with the electrolyte, resulting in poor electrochemical performance. Therefore, controlling the temperature within the temperature range can improve the electrochemical characteristics.

[0079] In addition, a pressure of 100 to 200 tons can be applied for 5 minutes to 1 hour to prepare secondary particles. Applying the pressure within the above range can further increase the bonding force between the nano-silicon particles and the graphite particles and the pitch particles.

[0080] A step of heat treating the secondary particles may be performed.

[0081] At this time, the heat treatment may be performed at 700 to 1000° C. in an inert atmosphere. By means of the heat treatment step, the secondary particles may be carbonized.

[0082] Specifically, the reason for performing the heat treatment under the above conditions is to prevent Si oxidation, impart high temperature viscosity characteristics to pitch, and increase the bonding strength.

[0083] As described above, by means of the steps, the pitch and the binder can be carbonized into soft carbon and hard carbon, respectively.

[0084] More specifically, the step of heat treating the secondary particles may include: a primary isothermal step of heating the secondary particles to a temperature 50 to 350°C higher than the softening point of asphalt at a rate of less than 7°C / min and then maintaining the temperature; and a secondary isothermal step of heating the secondary particles to a temperature range of 700 to 1000°C at a rate of less than 7°C / min and then maintaining the temperature after the primary isothermal step.

[0085] More specifically, the heating rates in the primary isothermal step and the secondary isothermal step may be 5° C. / min or less.

[0086] Alternatively, the primary isothermal step may be maintained for a period of 1 to 4 hours.

[0087] In another aspect, the secondary isothermal step can be maintained for a period of 1 to 4 hours.

[0088] At this time, as described above, the softening point of the asphalt used in one embodiment of the present invention may be 250° C. or higher.

[0089] More specifically, in an isothermal step, the temperature is raised to 50 to 350°C above the softening point of the pitch and then maintained for a predetermined time, thereby slowly removing low molecular weight volatile components that can decompose at high temperatures. Alternatively, the process of inducing polycondensation can play an important role in improving the carbonization yield of the negative electrode active material.

[0090] More specifically, in the primary isothermal step, when the temperature is slowly increased to the temperature range, the carbonization yield of the negative electrode active material obtained is better.

[0091] In addition, after the primary isothermal step, a secondary isothermal step of slowly raising the temperature to a temperature range of 700 to 1000° C. at a rate of 7° C. / min or less and then maintaining the temperature is performed, thereby further improving the carbonization yield.

[0092] After the step of heat treating the secondary particles, the carbonization yield of the secondary particles may be 60 to 95%, specifically, 80 to 95%.

[0093] Hereinafter, in this specification, the so-called "carbonization yield" means the result obtained by dividing the weight of carbon obtained after heat treatment by the carbon content before heat treatment and converting the result into percentage.

[0094] More specifically, the nano-silicon particles and graphite particles contained in the primary particles hardly change in weight even after heat treatment. On the other hand, the pitch undergoes drastic structural and morphological changes due to heat treatment. Therefore, the change in yield is the greatest.

[0095] More specifically, when the weight change of the pitch increases due to the heat treatment, the carbonization yield decreases, and therefore, pores are formed inside the secondary particles, and the specific surface area (BET) increases.

[0096] Therefore, the negative electrode active material of one embodiment of the present invention has an excellent carbonization yield even after heat treatment. This is the result of fully controlling the above conditions.

[0097] The heat-treated secondary particles may be pulverized and classified.

[0098] Specifically, the heat-treated secondary particles may be pulverized using a jet mill, a pin mill, or a combination thereof.

[0099] The pulverization is followed by sieving to obtain negative electrode active materials having an average particle size (D50) of 8 to 15 μm.

[0100] After the step of pulverizing and classifying the heat-treated secondary particles, a step of forming a carbon coating on the surface of the secondary particles may be performed.

[0101] Specifically, the carbon coating can be formed by CVD precipitation at 750 to 1000° C. for 30 minutes to 2 hours. More specifically, the carbon coating can be formed by CVD precipitation using an inert gas and a hydrocarbon gas. Specifically, when the temperature is too high, there is a risk of Si oxidation, and when the temperature is too low, it is not easy to form the coating.

[0102] Alternatively, a carbon coating may be formed on the surface of the secondary particles by a CVD deposition method in an atmosphere containing argon gas and hydrocarbon gas.

[0103] More specifically, the amount of the carbon coating formed on the surface of the secondary particles by the above step can be 3 to 15 wt % relative to 100 wt % of the entire secondary particles. The above amount of carbon coating can be formed only if the above conditions are met.

[0104] In addition, the specific surface area of ​​the secondary particles forming the coating layer can be further reduced.

[0105] The aforementioned negative electrode active material can be usefully used in a negative electrode of a lithium secondary battery.

[0106] That is, a lithium secondary battery according to one embodiment includes a positive electrode, a negative electrode including the negative electrode active material, and an electrolyte.

[0107] A lithium secondary battery in one embodiment may include an electrode assembly, wherein the electrode assembly includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. The electrode assembly is wound or folded and accommodated in a housing, thereby forming a lithium secondary battery.

[0108] In this case, the housing may have a cylindrical shape, a square shape, a film shape, or the like, and may be appropriately deformed according to the type of device to be used.

[0109] The negative electrode can be prepared by mixing a negative electrode active material, a binder, and an optionally selected conductive material to prepare a composition for forming a negative electrode active material layer, and then applying the composition to a negative electrode current collector.

[0110] The negative electrode current collector may be, for example, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or a combination thereof.

[0111] As described in one embodiment, the negative electrode active material may include a porous silicon-carbon material composite having a plurality of pores and a plurality of nano-silicon particles embedded in a carbon material. The specific contents of each composition are the same as those described above, and thus are omitted here.

[0112] As the binder, polyvinyl alcohol, carboxymethyl cellulose / styrene-butadiene rubber, hydroxypropylene cellulose, diacetylene cellulose, polyvinyl chloride, polyvinyl pyrrolidone, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene or polypropylene can be used, but it is not limited thereto. The binder can be mixed in an amount of 1 wt % to 30 wt % relative to the total amount of the negative electrode active material layer forming composition.

[0113] The conductive material is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity. Specifically, graphite such as natural graphite and artificial graphite, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, summer black, conductive fibers such as carbon fibers and metal fibers, metal powders such as carbon fluoride, aluminum, and nickel powders, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, conductive materials such as polyphenylene, etc. The conductive material can be mixed in an amount of 0.1% by weight to 30% by weight relative to the total amount of the negative electrode active material layer forming composition.

[0114] Then, the positive electrode can be prepared by mixing a positive electrode active material, a binder and an optionally selected conductive material to prepare a positive electrode active material layer-forming composition, and then applying the composition to a positive electrode current collector. In this case, the binder and the conductive material are used in the same manner as in the negative electrode.

[0115] The positive electrode current collector may be made of, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc.

[0116] The positive electrode active material may use a compound that can reversibly intercalate and deintercalate lithium (intercalation and deintercalation compound).

[0117] The positive electrode active material may be one or more of a composite oxide of cobalt, manganese, nickel or a combination of metals thereof and lithium. As a specific example, a compound represented by one of the following chemical formulas may be used: Li a A 1- b R b D2 (in the above formula, 0.90≤a≤1.8 and 0≤b≤0.5); Li a E 1-b R b O 2-c D c (In the above formula, 0.90≤a≤1.8, 0≤b≤0.5, and 0≤c≤0.05); LiE 2-b R b O 4-c D c (In the above formula, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b- c Co b R c D α (In the above formula, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Co b Rc O 2-α Z α (In the above formula, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Co b R c O 2-α Z2 (in the above formula, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Mn b R c D α (In the above formula, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Mn b R c O 2-α Z α (In the above formula, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Mn b R c O 2-α Z2 (in the above formula, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni b E c G d O2 (In the above formula, 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5 and 0.001≤d≤0.1 .);Li a Ni b Co c Mn d GeO2 (in the above formula, 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5 and 0.001≤e≤0.1); Li a NeG b O2 (in the above formula, 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a CoG b O2 (in the above formula, 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a MnG b O2 (in the above formula, 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a Mnb O4 (in the above formula, 0.90≤a≤1.8 and 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiTO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2);Li (3-f) Fe2(PO4)3(0≤f≤2); and LiFePO4.

[0118] In the above chemical formula, A is Ni, Co, Mn or a combination thereof, R is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof, D is O, F, S, P or a combination thereof, E is Co, Mn or a combination thereof, Z is F, S, P or a combination thereof, G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof, Q is Ti, Mo, Mn or a combination thereof, T is Cr, V, Fe, Sc, Y or a combination thereof, and J is V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0119] As the electrolyte filled in the lithium secondary battery, a non-aqueous electrolyte or a known solid electrolyte can be used, and an electrolyte in which a lithium salt is dissolved can be used.

[0120] The lithium salt may be, for example, one or more selected from the group consisting of LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiSbF6, LiAlO4, LiAlCl4, LiCl and LiI.

[0121] As the solvent of the non-aqueous electrolyte, for example, cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate, chain carbonates such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 1,2-dimethoxyethane ... The solvents include, but are not limited to, ethers such as alkanes and 2-methyltetrahydrofuran, nitriles such as acetonitrile, amides such as dimethylformamide, etc. They can be used alone or in combination. A mixed solvent of a cyclic carbonate and a linear carbonate can be particularly preferably used.

[0122] The electrolyte may be a gel polymer electrolyte in which an electrolyte solution is impregnated in a polymer electrolyte such as polyethylene oxide or polyacrylonitrile, or an inorganic solid electrolyte such as LiI or Li3N.

[0123] The separator may be made of chemically resistant and hydrophobic olefin polymers such as polypropylene, sheets or nonwoven fabrics made of glass fiber, polyethylene, etc. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte may also serve as a separation membrane.

[0124] Effects of the Invention

[0125] In the primary particles, the Si nanoparticles well dispersed with the hard carbon derived from the pitch and the pores can have a dense structure so that even if it expands / contracts during charging / discharging, short circuits with carbon materials do not occur. In addition, the pitch can maintain the connection with the graphite particles and maintain a conductive network with the graphite particles.

[0126] In addition, the primary particles are pressurized to reduce the porosity within the particles. Due to the strong bonding force of the three components of nano-silicon particles, asphalt particles and graphite particles, short circuits can be minimized even after repeated charge and discharge. At this time, as the specific surface area is minimized, the capacity loss caused by SEI is also minimized, and the newly exposed surface area is minimized, which can prevent the continued increase of SEI. BRIEF DESCRIPTION OF THE DRAWINGS

[0127] Figure 1 The correlation between asphalt content and specific surface area (BET) is graphically shown.

[0128] Figure 2 The internal cross-sectional structures of the primary particles of Comparative Example A1 and Example A1 are shown.

[0129] Figure 3 The change in specific surface area according to the heat treatment conditions in the secondary particle heat treatment step in Examples B1 to B3 and Comparative Examples B1 to B2 is shown in a graph.

[0130] Figure 4 The graph shows the carbonization yield after heat treatment as the coal-based pitch content increases.

[0131] Figure 5 The measurement results of the coulombic efficiency (a) and the capacity retention rate (b) according to the number of charge and discharge times of the lithium secondary batteries of Example A1 and Comparative Example A1 are shown.

[0132] Figure 6 The charge and discharge curves of the lithium secondary batteries of Example A1(a) and Comparative Example A1(b) at the first cycle are shown.

[0133] Figure 7 The adsorption / desorption curves (a) of the lithium secondary batteries of Examples C1 to C2 and Comparative Example C1 and the pore distribution curve (b) investigated by the DFT method are shown. DETAILED DESCRIPTION

[0134] The specific embodiments of the present invention are described below. However, the following embodiments are only specific embodiments of the present invention, and the present invention is not limited to the following embodiments.

[0135] Example A: Comparison of properties according to bitumen content

[0136] Example A1

[0137] (1) Preparation of negative electrode active material

[0138] The nano-silicon particles, graphite particles and asphalt particles were milled under dry conditions for 1 hour to prepare a mixed powder. At this time, in the mixed powder, the weight ratio of the nano-silicon particles: the graphite particles: the asphalt particles was 4:1:5.

[0139] At this time, the asphalt used was coal-based asphalt, and the softening point of the asphalt was 250°C.

[0140] Then, the aqueous binder (gum arabic) and the mixed powder were added to distilled water, and after confirming that they were well dispersed in water using a magnetic stirrer, they were fully dispersed for 1 hour using a horn-type ultrasonic wave to prepare a mixed solution.

[0141] At this time, the concentration of the mixed powder contained in 100 wt % of the mixed solution is 3 to 20%.

[0142] Then, the mixed solution was added at a rate of 50 mL / min and spray-dried at 20,000 rpm by a sprayer to prepare primary particles.

[0143] Then, the primary particle powder was placed in a mold and a uniaxial press molding machine was used to prepare secondary particles. Specifically, the mold was pressed at a temperature 50°C higher than the softening point of the pitch and a pressure of 16 tons for 20 minutes. After molding, air cooling was performed.

[0144] Then, the secondary particles were heat treated in an inert atmosphere and then naturally cooled to room temperature. At this time, the heat treatment step was carried out by maintaining the temperature at 300° C. for 2 hours and then maintaining the temperature at 900° C. for 1 hour.

[0145] After cooling, the secondary particles were crushed into a particle size range of 8 to 15 μm based on the D50 standard using a jet mill. After crushing, the particles were classified by sieving with a #635 mesh (20 μm) to obtain the negative electrode active material.

[0146] (2) Preparation of lithium secondary battery (half-cell)

[0147] The negative electrode active material, binder (PAA) and conductive material (Super P: conductive carbon black) of (1) were prepared so that the weight ratio of negative electrode active material: binder: conductive material was 75:24:01, and then added to distilled water and uniformly mixed to prepare slurry.

[0148] The above slurry was uniformly applied to a copper (Cu) current collector, pressed on a roll press, and then dried to prepare a negative electrode. Specifically, the loading amount was 4 g / cm 2 , the electrode density has a range of 1.0 to 1.2 g / cc.

[0149] Lithium metal (Li-metal) was used as the relative electrode, and as the electrolyte, a solution of 1 mol of LiPF6 dissolved in a mixed solvent of ethylene carbonate (EC: Ethylene Carbonate): dimethyl carbonate (DMC: Dimethyl Carbonate) in a volume ratio of 1:1 was used.

[0150] A CR 2032 half coin cell was prepared using the negative electrode, lithium metal and electrolyte according to a common preparation method.

[0151] Example A2

[0152] (1) Preparation of negative electrode active material

[0153] Compared with Example A1 (1), a negative electrode active material was prepared in the same manner except that the weight ratio of nano silicon particles: graphite particles: pitch particles in the mixed powder was 4:2:4.

[0154] (2) Preparation of lithium secondary batteries

[0155] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0156] Example A3

[0157] (1) Preparation of negative electrode active material

[0158] Compared with Example A1 (1), a negative electrode active material was prepared in the same manner except that the weight ratio of nano silicon particles: graphite particles: pitch particles in the mixed powder was 4:3:3.

[0159] (2) Preparation of lithium secondary batteries

[0160] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0161] Comparative Example A1

[0162] (1) Preparation of negative electrode active material

[0163] Compared with Example A1 (1), a negative electrode active material was prepared in the same manner except that the weight ratio of nano silicon particles: graphite particles: pitch particles in the mixed powder was 4:5:1.

[0164] (2) Preparation of lithium secondary batteries

[0165] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0166] Comparative Example A2

[0167] (1) Preparation of negative electrode active material

[0168] Compared with Example A1 (1), a negative electrode active material was prepared in the same manner except that the weight ratio of nano silicon particles: graphite particles: pitch particles in the mixed powder was 4:4:2.

[0169] (2) Preparation of lithium secondary batteries

[0170] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0171] Then, in the Example A and the Comparative Example A, the specific surface area according to the asphalt content was measured and disclosed in Tables 1 and 2.

[0172] The porosity, specific surface area and tap density were measured as follows.

[0173] Total pore volume (TPV), Vt-plot, fmicro, APD measurement methods

[0174] The total pore volume (TPV) can be calculated as the relative pressure measured at a single point at a relative pressure of 0.95.

[0175] Vt-plot is the volume of the micropores obtained with the aid of t-plot.

[0176] Fmicro is calculated as the ratio of Vt-plot to TPV (=V(t-plot) / TPV).

[0177] APD (average pore diameter) is calculated as TPV (total pore volume), that is, as a function of the relationship between surface area and volume assuming that the pores are cylindrical in shape.

[0178] Surface area measurement

[0179] The specific surface area was measured using the BET method (specific surface area and porosity analyzer, Micromeritics Instruments Co., Ltd., ASAP2020).

[0180] Tap density measurement

[0181] Packing density was measured according to ASTM-B527 after adding 10 g of powder in a 50 mL container and tapping at 3000 cycles @ 284 cycles / min.

[0182] Carbonization yield measurement

[0183] The carbonization yield was measured using TG-DTA, and the yield according to the heating curve was measured at 900°C. The differences in heating rate, step temperature during heating, step holding time, and holding time at the final temperature were investigated.

[0184]

Table 1

[0185]

[0186]

Table 2

[0187]

[0188] From the contents disclosed in Table 1, the pore structures of the primary particles and secondary particles of the examples and comparative examples can be understood.

[0189] Specifically, in the comparative example in which the amount of graphite is greater than that of pitch, it is found that the specific surface area tends to increase after the secondary particles are prepared.

[0190] This can be understood as follows: depending on the composition ratio, when there is more pitch, plasticity increases, and when graphite is dominant, elasticity acts dominantly, and the specific surface area increases due to the phenomenon that the restoring force acts due to the pressure during compression.

[0191] Of course, depending on the particle size of graphite, the particle contact during compression may behave differently, but in order to have a high-density compressed structure, it can be confirmed that the relative content of pitch plays a dominant role.

[0192] Table 2 discloses the carbonization yield and tap density of the negative electrode active materials prepared according to the examples and comparative examples.

[0193] As shown in Table 2, it can be confirmed that the carbonization yield decreases and the tap density increases as the asphalt content increases.

[0194] It can be seen that this is related to the following Figure 1 The result is the opposite that the specific surface area decreases according to the bitumen content.

[0195] In addition, this is also shown in Figure 1 middle.

[0196] Figure 1 The correlation between asphalt content and specific surface area (BET) is shown in a graph.

[0197] Compared with the secondary particles (After press) prepared by molding composite spheres defined as primary particles, the specific surface area generally tends to decrease with the increase of asphalt.

[0198] However, if we examine the decreasing trend and the changes before and after extrusion, for primary particles, when the asphalt input is more than 30%, the decrease in specific surface area shows a saturation trend, but in secondary particles, the greater the asphalt amount, the greater the specific surface area shows a linear decreasing tendency.

[0199] Specifically, it can be seen that when the pitch is less and the graphite is more (Comparative Example 1), the specific surface area tends to increase after the first pellet extrusion. However, when the pitch weight is 30% or more, the specific surface area decreases significantly after extrusion.

[0200] As mentioned above, this is because when there is more asphalt, plasticity increases. Specifically, when graphite is dominant, elasticity acts dominantly, and the specific surface area increases by virtue of the phenomenon that the restoring force acts due to the pressure during compression. Therefore, it can be seen that in order to have a high-density compressed structure, when the relative content of asphalt is greater than or equal to that of graphite particles, the effect of reducing the specific surface area caused by it is dominant.

[0201] Figure 2 The internal cross-sectional structures of the primary particles of Comparative Example A1 and Example A1 are shown.

[0202] like Figure 2 As shown, in Comparative Example A1 in which graphite is dominant, the connection between the components is relatively imperfect, and a large number of spaces such as voids are observed.

[0203] However, it has been previously confirmed that the specific surface area, which is the space between particles, tends to decrease as the asphalt content increases.

[0204] Specifically, if Figure 2 As shown in Example A1, when 50 wt% of pitch is added, it can be seen that the aggregation area of ​​the pitch separated from the graphite phase increases.

[0205] That is, based on the cross-sectional structure of the porous silicon-carbonaceous material composite, it can be seen that in order to increase the uniform dispersion and contact between particles, it is important to derive the optimal ratio of the above composition.

[0206] Figure 5 The measurement results of the coulombic efficiency (a) and the capacity retention rate (b) according to the number of charge and discharge times of the lithium secondary batteries of Example A1 and Comparative Example A1 are shown.

[0207] The coulombic efficiency and capacity retention rate according to the number of charge and discharge times are measured as follows.

[0208] Coulombic efficiency and capacity retention measurement

[0209] In the above-mentioned examples and comparative examples, each finally obtained active material was applied to a half-cell and tested.

[0210] Specifically, the battery is driven under the conditions of 0.5C, 0.005V, 0.005_C cut-off charging and 0.5C, 1.5V cut-off discharging, and the coulombic efficiency and capacity retention rate are measured and displayed on Figure 6 .

[0211] Specifically, Figure 5 The electrochemical characteristics of the lithium secondary battery are shown in a graph according to the amount of asphalt added. Figure 5 As shown in (a), it can be confirmed that for Comparative Example A1 having a low asphalt content (10 wt%), the efficiency decreases sharply in the range of 20 to 30 charge and discharge cycles compared with Example A1.

[0212] This is because, when the asphalt content is too low as described above, the number of disconnected electrical contact paths due to expansion and contraction increases, and efficiency decreases sharply.

[0213] This disconnection of the electrical contact path can also be seen Figure 5 Specifically, if Figure 5 As shown in (b), in Comparative Example A1, the number of disconnected electrical contact paths increased in the range of 20 to 30 charge and discharge cycles, and the capacity retention rate also decreased sharply.

[0214] Figure 6 The charge and discharge curves of the lithium secondary batteries of Example A1(a) and Comparative Example A1(b) at the first cycle are shown.

[0215] like Figure 6 As shown, the initial efficiency of Example A1 is 86.5%, and the initial efficiency of Comparative Example A1 is 86.3%, which have similar tendencies, but the slopes of the initial discharge curves are different, and the impedance during discharge has a larger value in the composite material containing a large amount of graphite.

[0216] This is also due to the difference caused by the asphalt content in Example A1(a) and Comparative Example A1(b).

[0217] Example B: Comparison of properties according to the conditions of the secondary particle heat treatment step

[0218] Example B1

[0219] (1) Preparation of negative electrode active material

[0220] Compared with Example A1 (1), the weight ratio of nano silicon particles: graphite particles: asphalt particles in the mixed powder is 3:3:4. The asphalt used here is coal-based asphalt, and the softening point of the asphalt is 250°C.

[0221] Then, in the step of heat treating the secondary particles, a negative electrode active material was prepared in the same manner except that a primary isothermal step of heating the temperature to 600°C at a rate of 5°C / min and holding the temperature for 1 hour was performed, and then a secondary isothermal step of heating the temperature to 900°C at a rate of 5°C / min and holding the temperature for 1 hour was performed.

[0222] (2) Preparation of lithium secondary batteries

[0223] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0224] Example B2

[0225] (1) Preparation of negative electrode active material

[0226] Compared with Example B1 (1), the asphalt used is coal-based asphalt, and the softening point of the asphalt is 250°C.

[0227] Then, in the step of performing secondary particle heat treatment, the negative electrode active material was prepared in the same manner except that a primary isothermal step of heating the temperature to 400°C at a rate of 5°C / min and holding the temperature for 2 hours was performed, and a secondary isothermal step of heating the temperature to 900°C at a rate of 5°C / min and holding the temperature for 1 hour was performed.

[0228] (2) Preparation of lithium secondary batteries

[0229] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0230] Comparative Example B1

[0231] (1) Preparation of negative electrode active material

[0232] Compared with (1) of Example B1, in the step of heat treating the secondary particles, the negative electrode active material was prepared in the same manner except that a first isothermal step of heating the temperature to 600°C at a rate of 10°C / min and holding the temperature for 2 hours, and then a second isothermal step of heating the temperature to 900°C at a rate of 10°C / min and holding the temperature for 1 hour.

[0233] (2) Preparation of lithium secondary batteries

[0234] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0235] Comparative Example B2

[0236] (1) Preparation of negative electrode active material

[0237] Compared with (1) of Example B1, in the step of heat treating the secondary particles, the negative electrode active material was prepared in the same manner except that a first isothermal step of heating the temperature to 400°C at a rate of 10°C / min and holding the temperature for 1 hour was performed, and then a second isothermal step of heating the temperature to 900°C at a rate of 10°C / min and holding the temperature for 1 hour was performed.

[0238] (2) Preparation of lithium secondary batteries

[0239] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0240] Comparative Example B3

[0241] (1) Preparation of negative electrode active material

[0242] A negative electrode active material was prepared in the same manner as in Example B1 (1), except that the heat treatment at 900° C. at a rate of 10° C. / min was performed without an isothermal step in the heat treatment of the secondary particles.

[0243] (2) Preparation of lithium secondary batteries

[0244] A lithium secondary battery was prepared by the same method as in Example 1 (2) using the negative electrode active material of (1) above.

[0245] Then, the carbonization yields of Examples B1 to B3 and Comparative Examples B1 to B2 were measured and are disclosed in Table 3 below.

[0246] The specific surface area was measured in the same manner as described above, and the carbonization yield was measured in the following manner.

[0247]

Table 3

[0248]

[0249] Specifically, the specific surface areas of the negative electrode active materials prepared according to Examples B1 to B2 and Comparative Examples B1 to B3 were measured, as shown in Tables 3 and Figure 3 middle.

[0250] Figure 3 The change in specific surface area according to the heat treatment conditions in the secondary particle heat treatment step in Examples B1 to B3 and Comparative Examples B1 to B2 is shown in a graph.

[0251] As shown in Table 3 and Figure 3 As shown, for Comparative Example B3 in which the heat treatment was performed without the 700°C isothermal step, the specific surface area was high and the carbonization yield was very low. On the other hand, as shown in the Examples, when the isothermal step was performed, the specific surface area was low and the carbonization yield was excellent.

[0252] It can be seen from this that there is a clear trend difference between the example in which an isothermal step is performed near the softening point to slow down the thermal decomposition of the asphalt as much as possible and the sample in which the temperature is linearly increased to the target temperature at a predetermined rate (Comparative Example B3).

[0253] On the other hand, it can be seen that even when an isothermal step is performed, the results vary depending on the temperature and the speed.

[0254] More specifically, it can be seen that the slower the heating rate is until the temperature near the softening point of the pitch, the better the carbonization yield is. Specifically, the carbonization yields of Examples B1 and B2, which are heated to the primary isothermal step temperature at a rate of 5°C / min, are higher than those of Comparative Examples B1 and B2.

[0255] It can be seen that among the comparative examples B1 and B2 with fast heating rates, the carbonization yield of comparative example B2 in which the temperature of the primary isothermal step is maintained near the softening point is better. Specifically, when the low molecular weight volatile components (volatile) that decompose during heat treatment under the same heating rate are removed for a long time, a higher yield is achieved.

[0256] That is, it is found that the final carbonization yield of the negative electrode active material is closely related to the conditions for heat treatment of the secondary particles.

[0257] Example C: Comparison of properties based on carbon deposition on the surface of Si-C composites

[0258] Example C1

[0259] (1) Preparation of negative electrode active material

[0260] The negative electrode active material prepared according to (1) of Example A1 was placed in a horizontal furnace, and argon (Ar) 200 sccm and CH4 400 sccm were placed at 760°C for 1 hour to perform a CVD deposition experiment. The deposition amounts obtained in the two experiments had a value of about 2%. Therefore, in addition to depositing a carbon component on the surface of the negative electrode active material prepared according to (1) of Example A1, a negative electrode active material was prepared in the same manner.

[0261] (2) Preparation of lithium secondary batteries

[0262] A lithium secondary battery was prepared by using the negative electrode active material of (1) in the same manner as (2) of Example A1.

[0263] Example C2

[0264] (1) Preparation of negative electrode active material

[0265] The negative electrode active material prepared according to (1) of Example A1 was placed in a horizontal furnace, and argon (Ar) 200 sccm and CH4 400 sccm were added at 1000°C for 1 hour to perform a CVD deposition experiment. The deposition amount obtained in the two experiments had a value of about 7%. Therefore, in addition to depositing a carbon component on the surface of the negative electrode active material prepared according to (1) of Example A1, a negative electrode active material was prepared in the same manner.

[0266] Comparative Example C1

[0267] (1) Preparation of negative electrode active material

[0268] The negative electrode active material prepared according to (1) of Comparative Example A1 was placed in a horizontal furnace, and argon (Ar) 200 sccm and CH4 400 sccm were placed at 760°C for 1 hour to perform a CVD deposition experiment. The deposition amounts obtained in the two experiments had a value of about 7%. Therefore, in addition to depositing a carbon component on the surface of the negative electrode active material prepared according to (1) of Example A1, a negative electrode active material was prepared in the same manner.

[0269] (2) Preparation of lithium secondary batteries

[0270] A lithium secondary battery was prepared by using the negative electrode active material of (1) in the same manner as (2) of Example C1.

[0271] The specific surface area and pore size of the lithium secondary batteries of the embodiments and comparative examples are shown in Tables 4 and Figure 7 .

[0272]

Table 4

[0273]

[0274] As shown in Table 4, it can be seen that the specific surface area and pore size of Examples C1 and C2 and Comparative Example C1 obtained by introducing CH4 gas and further forming an amorphous carbon layer changed.

[0275] The characteristics are also shown in Figure 7 middle.

[0276] Figure 7The adsorption / desorption curves (a) of the lithium secondary batteries of Examples C1 to C2 and Comparative Example C1 and the pore distribution curve (b) investigated by the DFT method are shown.

[0277] That is, from Table 4 and Figure 7 As shown in the figure, the amount of carbon layer deposited varies depending on the temperature in the CVD deposition step. Specifically, it can be confirmed that the deposition experiment at 760°C resulted in a 2% deposition amount, while at 1000°C, a 7% deposition amount was formed. Therefore, it can be seen that setting the appropriate temperature range for CVD deposition is important.

[0278] Specifically, the specific surface area investigated by the BET method shows a decrease as the deposition amount increases. This is because the external pores and defect structures are coated and filled during CVD deposition.

[0279] In addition, if Figure 7 As shown, if the change in pore structure is investigated according to the DFT method, the greater the deposition amount, the more significantly the micropores below 2 nm decrease, and when the deposition amount is 2%, the porosity in the moderate area decreases slightly, and shows a tendency to increase again at a deposition amount of 7%.

[0280] Therefore, it can be confirmed that the more microscopic the pores are, the easier it is for the BET value to increase, and that CVD deposition is more effective in reducing BET.

[0281] Experimental example: Comparison of co-carbonization characteristics of mixed powders of petroleum-based asphalt and coal-based asphalt

[0282] Specifically, in order to confirm the co-carbonization behavior caused by heat treatment when preparing powder only with pitch, the following experimental example is disclosed. That is, as shown in Table 5 below, after preparing powder using one type of pitch or mixing pitches, the weight change was confirmed using TG / DTA.

[0283] Yield change measurement

[0284] In Table 5 below, the yield change means the yield change according to the holding time at the final target temperature of 900° C. Specifically, the yield change varies depending on the 900° C. isothermal treatment and the pitch composition.

[0285]

Table 5

[0286]

[0287] As shown in Table 5, it can be confirmed that the final carbonization yield of the mixed use example is higher than that of the case where the petroleum-based or coal-based pitch is used alone.

[0288] It is also found that even in the case of using asphalt alone, when only coal-based asphalt was used, the final yield was similar to that of other examples, but in the case of Comparative Example C1 using only petroleum-based asphalt, the final yield was poor.

[0289] These are achieved through Figure 4 It can also be confirmed.

[0290] Figure 4 The graph shows the carbonization yield after heat treatment as the coal-based pitch content increases.

[0291] Specifically, if Figure 4 As shown in Table 5, it can be seen that the carbonization yield is better and the specific surface area is smaller when the asphalt is used in combination than when the asphalt is used alone. Therefore, it can be confirmed that the co-carbonization of coal-based asphalt and petroleum-based asphalt leads to an improvement in yield.

[0292] Moreover, if Figure 4 As shown, in the case of coal with a fraction of 50% or more, the trend line of the quadratic equation is fully consistent, and the fit at the level of R2 = 0.9937 is confirmed. This means that the closer the consistency with the trend line of the theoretical quadratic equation is to 1, the more consistent it is with the theoretical tendency.

[0293] The present invention is not limited to the embodiments described above, and can be prepared in various forms that are different from each other. A person skilled in the art of the present invention can understand that the present invention can be implemented in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should only be understood that the embodiments described above are exemplary in all aspects, and not restrictive.

Claims

1. A negative electrode active material for a lithium secondary battery, wherein the negative electrode active material for a lithium secondary battery is a porous silicon-carbon material composite having pores and a plurality of nano-silicon particles embedded in a carbon material, wherein: The carbonaceous material includes a combination of graphite particles, easily graphitizable carbon, and non-graphitizable carbon. With respect to 100% by weight of the porous silicon-carbonaceous material composite, The weight ratio of the graphite particles to the graphitizable carbon is 1:1 to 1:5, and The graphitizable carbon is derived from pitch.

2. The negative electrode active material for lithium secondary battery according to claim 1, wherein The specific surface area of ​​the porous silicon-carbonaceous material composite is 20 m 2 / g or less.

3. The negative electrode active material for lithium secondary battery according to claim 2, wherein The porosity of the negative electrode active material is 3 volume % or less based on the total volume of the negative electrode active material.

4. The negative electrode active material for lithium secondary battery according to claim 3, wherein The negative electrode active material also has a carbon coating on its surface. The deposition amount of the carbon coating layer is 3 to 15 weight % relative to 100 weight % of the negative electrode active material.

5. The negative electrode active material for lithium secondary battery according to claim 4, wherein The porous silicon-carbon material composite comprises 30 to 40 weight % of nano silicon and 60 to 70 weight % of carbonaceous particles relative to 100 weight % of the porous silicon-carbonaceous material composite.

6. The negative electrode active material for lithium secondary battery according to claim 5, wherein The D50 particle size of the negative electrode active material is 8 to 15 μm.

7. A method for preparing a negative electrode active material for a lithium secondary battery, wherein: include: The step of preparing a porous silicon-carbonaceous material mixed powder by mixing nano silicon particles, graphite particles and asphalt particles by dry grinding; The step of adding the porous silicon-carbonaceous material mixed powder and a binder into distilled water to prepare a mixed solution; The step of spray drying the mixed solution to prepare primary particles; The step of placing the primary particles into a mold and press-molding to prepare secondary particles; The step of heat treating the secondary particles; and The step of crushing and classifying the heat-treated secondary particles; In the step of preparing the porous-carbonaceous material mixed powder, The asphalt particles contain 30% by weight or more relative to 100% by weight of the porous-carbonaceous material mixed powder. In the step of preparing a porous silicon-carbonaceous material mixed powder by mixing nano silicon particles, graphite particles and asphalt particles by dry grinding, The weight ratio of the asphalt to the graphite is 1:1 to 5:1, and The step of heat treating the secondary particles comprises: The secondary particles are heated to a temperature 50 to 350° C. higher than the softening point of the asphalt at a rate of 7° C. / min or less, and then maintained at an isothermal temperature; and After the primary isothermal step, the temperature is raised to a temperature range of 700 to 1000° C. at a rate of 7° C. / min or less, and then a secondary isothermal step is performed, wherein: The first isothermal step and the second isothermal step are maintained for 1 to 4 hours.

8. The method for preparing a negative electrode active material for a lithium secondary battery according to claim 7, wherein: In the step of preparing a porous silicon-carbonaceous material mixed powder by mixing nano silicon particles, graphite particles and asphalt particles by dry grinding, The weight of the pitch is greater than the weight of the graphite.

9. The method for preparing a negative electrode active material for a lithium secondary battery according to claim 7, wherein: The asphalt includes a combination of coal-based asphalt and petroleum-based asphalt. The weight of the coal-based asphalt is greater than the weight of the petroleum-based asphalt, wherein: Relative to 100 weight % of the asphalt, the weight ratio of coal-based asphalt to petroleum-based asphalt is 5:5 to 9:

1.

10. The method for preparing a negative electrode active material for a lithium secondary battery according to claim 7, wherein: The softening point of the asphalt is above 250°C.

11. The method for preparing a negative electrode active material for a lithium secondary battery according to claim 7, wherein: After the steps of crushing and classifying the heat-treated secondary particles, The step further comprises forming a carbon coating on the surface of the secondary particles, The step of forming the carbon coating layer is performed at 750 to 1000°C.

12. The method for preparing a negative electrode active material for a lithium secondary battery according to claim 7, wherein: After the step of heat treating the secondary particles, The carbonization yield of the secondary particles is 60 to 95%.

13. The method for preparing a negative electrode active material for a lithium secondary battery according to claim 7, wherein: By means of a step of heat treating the secondary particles, The pitch is carbonized to graphitizable carbon. The binder is carbonized to form non-graphitizable carbon.

14. A lithium secondary battery, wherein: include: positive electrode; negative electrode; and Electrolytes; The negative electrode comprises the negative electrode active material for a lithium secondary battery according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Negative electrode material for lithium-ion battery, and use therefor

    CN106233511A

  • High-performance silicon-carbon cathode material and preparation method thereof

    CN107785560A

  • Negative electrode active material for rechargeable lithium battery, method for manufacturing the same, and rechargeable lithium battery including the same