Ion conductive membrane having ion transport paths arranged in thickness direction by utilizing magnetic field and method for producing the same
By using magnetic nanoparticles and an external magnetic field to orient the one-dimensional composite in the thickness direction of the film, the ion conductivity of the proton conductive membrane is improved, solving the problem in the existing technology that the conductivity cannot be effectively improved in the thickness direction, and improving Improves the performance of electrochemical components and reduces potential contamination risks.
Patent Information
- Application Number
- CN202110183954.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-02-10
AI Technical Summary
Existing proton conductive membranes have difficulties in improving the power performance of electrochemical components, especially due to the inability to effectively stretch and deform in the thickness direction of the membrane to increase ion conductivity.
An ion conductive membrane containing magnetic nanoparticles is used, and the one-dimensional complex is oriented along the thickness direction of the membrane through an external magnetic field, thereby improving the ion conductivity. The membrane consists of a core of non-conductive one-dimensional nanostructures, an intermediate layer encased with magnetic nanoparticles, and a surface layer that conducts the same kinds of ions as within the matrix.
It significantly improves the ion conductivity in the thickness direction of the membrane, improves the power performance of electrochemical components, and removes magnetic nanoparticles through the activation step to prevent free radical generation and catalyst poisoning.
Smart Images

Figure CN113258110B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an ion conductive membrane and a method for producing the same, and more particularly to an ion conductive membrane based on a polymer electrolyte having ion transport paths arranged in a thickness direction using a magnetic field and a method for producing the same. Background Art
[0002] As the demand for electrochemical elements such as fuel cells, electrolyzers, and flow batteries increases, the use of proton conductive membranes (proton exchange membranes) has also increased. In previous proton conductive membranes, protons moved through channels of water clusters formed around some ions of polymer electrolytes. In the field of proton conductive membranes, the connection of water channels or the increase in volume is the main research direction for improving proton conductivity, and technologies such as the addition of polymer electrolytes with new structures or hydrophobic additives have been proposed. However, since the power performance of an electrochemical element is mainly determined by the membrane resistance in the thickness direction, arranging the proton movement path along the thickness direction of the membrane is very advantageous in improving the power performance of the element compared to simple water channel connection or volume increase.
[0003] Park et al. analyzed the anisotropic properties of stretched high-fluorinated ion exchange resin (Nafion) and proved that proton conductivity was greatly improved in the direction of water channel arrangement. Similarly, Kusoglu et al. observed the shape of compressed high-fluorinated ion exchange resin membrane using small-angle X-ray scattering (SAXS) and proved the change of proton conduction. Regarding the increase of proton conductivity, the method of physically modifying the high-fluorinated ion exchange resin membrane as a polymer electrolyte membrane has no disadvantages and is a simple and excellent approach that does not reduce durability. However, as mentioned above, although it is necessary to increase the ionic conductivity of the thickness direction of the ion conductive membrane in the actual electrochemical element, it is actually impossible to stretch the cast ion conductive membrane in the thickness direction.
[0004] Prior art literature
[0005] Non-patent literature
[0006] JKPark,J.Li,GMDivoux,LAMadsen,RBMoore, Macromolecules 2011,44,5701. Summary of the invention
[0007] An object of the present invention is to provide an ion-conducting membrane having improved ion conductivity in the thickness direction of the membrane.
[0008] Another object of the present invention is to provide a method capable of producing an ion-conducting membrane having improved ion conductivity in the thickness direction of the membrane by a simple and rapid process.
[0009] According to one embodiment of the present invention, an ion conductive membrane includes an ion conductive matrix, and a one-dimensional composite dispersed in the ion conductive matrix and oriented along the thickness direction of the membrane, wherein the one-dimensional composite includes: a core of a non-conductive one-dimensional nanostructure, an intermediate layer wrapping the core and having magnetic nanoparticles bonded to its surface, and a surface layer conducting ions of the same type as the ions in the matrix.
[0010] According to another embodiment of the present invention, an ion conductive membrane in which a one-dimensional dispersed phase is oriented along the thickness direction of the membrane includes an ion conductive matrix, and a one-dimensional dispersed phase dispersed in the above-mentioned ion conductive matrix. The above-mentioned one-dimensional dispersed phase is formed by removing magnetic nanoparticles bound to the above-mentioned intermediate layer after the one-dimensional composite body is arranged along the thickness direction of the membrane by an external magnetic field. The above-mentioned one-dimensional composite body includes: a core of a non-conductive one-dimensional nanostructure, an intermediate layer that wraps the above-mentioned core and has magnetic nanoparticles bound to its surface, and a surface layer that conducts ions of the same type as the ions in the above-mentioned matrix.
[0011] According to another embodiment of the present invention, an ion conductive membrane includes an ion conductive matrix and a one-dimensional dispersed phase dispersed in the ion conductive matrix and oriented along the membrane thickness direction, wherein the one-dimensional dispersed phase includes a core of a non-conductive one-dimensional nanostructure and a surface layer that conducts ions of the same type as the ions in the matrix.
[0012] In the ion conductive membrane according to one specific example of the present invention, the ion conductive matrix may have cation conductive properties, and the intermediate layer may contain a cationic polymer.
[0013] In the ion conductive membrane according to one embodiment of the present invention, the magnetic nanoparticles have a negative zeta potential, and the magnetic nanoparticles may be fixed and bonded to the intermediate layer by electrostatic attraction.
[0014] In the ion conductive membrane according to one specific example of the present invention, the one-dimensional nanostructure has a negative zeta potential, and the one-dimensional nanostructure and the intermediate layer, and the intermediate layer and the surface layer may be bonded to each other through ionic interaction.
[0015] In the ion conductive membrane according to one specific example of the present invention, the one-dimensional nanostructure may be one or more selected from nanowires, nanotubes, and nanorods.
[0016] In the ion conductive membrane according to a specific example of the present invention, the density of the dispersed phase, which is the number of the one-dimensional dispersed phase per unit area of the ion conductive membrane, can be 500 to 1,000,000 / mm2, based on the cross section perpendicular to the orientation direction of the one-dimensional dispersed phase. 2 .
[0017] In the ion conductive membrane according to one embodiment of the present invention, the thickness of the surface layer may be 1 to 100 nm.
[0018] In the ion conductive membrane according to one embodiment of the present invention, the matrix or the surface layer may contain a sulfonated block copolymer, a perfluorinated polymer having a sulfonate group on a side chain, or a sulfonated aromatic polymer.
[0019] In the ion conductive membrane according to one specific example of the present invention, the ion conductivity of the surface layer may be greater than the ion conductivity of the matrix.
[0020] In the ion conductive membrane according to a specific example of the present invention, the cationic polymer can be selected from poly(allylamine hydrochloride), poly(diallyldimethylammonium chloride), poly(acrylamide-diallyldimethylammonium chloride), polyethyleneimine, polymethacryloyloxyethyltrialkylammonium halide, polyarylamine chloride, polyacrylamide, aminoethylated polyacrylamide, polyvinylamine and polyethyleneamine Select one or more.
[0021] In the ion conductive membrane according to one specific example of the present invention, the surface layer may be a porous membrane having through-type pores.
[0022] In the ion conductive membrane according to one embodiment of the present invention, the magnetic nanoparticles may be ferromagnetic nanoparticles.
[0023] The present invention includes a method for producing the above-mentioned ion conductive membrane.
[0024] The method for manufacturing an ion conductive membrane according to the present invention comprises the following steps: a coating step of manufacturing a coating film by coating a composition comprising an ion conductive resin, a one-dimensional composite, and a solvent; and a drying step of drying the coating film, wherein the one-dimensional composite comprises: a core of a non-conductive one-dimensional nanostructure, an intermediate layer wrapping the core and having magnetic nanoparticles bonded to its surface, and a surface layer conducting ions of the same type as the ions in the ion conductive resin, and before, while, or during the drying of the coating film, a magnetic field is applied along the thickness direction of the coating film to orient the one-dimensional composite along the thickness direction of the film.
[0025] According to a specific example of the manufacturing method of the present invention, the one-dimensional composite manufacturing step may further include a one-dimensional composite manufacturing step before the coating step. The one-dimensional composite manufacturing step may include the following steps: a first step of forming an intermediate layer containing a cationic polymer on the one-dimensional nanostructure; a second step of fixing magnetic nanoparticles with a negative zeta potential on the surface of the intermediate layer by electrostatic attraction in a liquid medium; and a third step of forming a surface layer on the one-dimensional nanostructure with the magnetic nanoparticles fixed thereon and the intermediate layer formed thereon.
[0026] In a manufacturing method according to a specific example of the present invention, the ion conductive resin may be a cation conductive resin, and the one-dimensional nanostructure may have a negative zeta potential.
[0027] In the production method according to a specific example of the present invention, the solvent can be water, a glycol solvent, a glycol ether solvent, an alcohol solvent, a ketone solvent, an ester solvent, an amide solvent, a sulfoxide or sulfone solvent, a phenolic solvent or a mixed solvent thereof.
[0028] In a production method according to a specific example of the present invention, the composition may contain 0.05 to 10 parts by weight of the one-dimensional composite and 500 to 10,000 parts by weight of a solvent, based on 100 parts by weight of the ion conductive resin.
[0029] The production method according to one specific example of the present invention may further include, after the drying step, an activation step of immersing the obtained dried film in an acidic aqueous solution for activation.
[0030] In the manufacturing method according to one specific example of the present invention, the magnetic nanoparticles may be removed during the activation.
[0031] In a manufacturing method according to a specific example of the present invention, the intensity of the magnetic field can be 0.1T to 100T.
[0032] In a manufacturing method according to a specific example of the present invention, the magnetic nanoparticles may be ferromagnetic nanoparticles, and the strength of the magnetic field may be 0.005T to 0.1T.
[0033] The present invention includes an ion conductive membrane produced by the above-mentioned production method.
[0034] The ion-conducting membrane according to the present invention comprises an ion-conducting matrix and a surface layer having ion-conducting properties for conducting ions of the same kind, and contains a one-dimensional dispersed phase oriented in the thickness direction of the membrane, thereby having the advantage of having significantly improved ion conductivity in the thickness direction of the membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a schematic diagram illustrating the ion conduction mechanism of a conventional cation conductive membrane ( Figure 1 (a)) and a schematic diagram illustrating the ion conduction mechanism of the ion conductive membrane according to a specific example of the present invention ( Figure 1 (b)).
[0036] Figure 2 The diagram is a schematic diagram illustrating each of a bare WS2 nanowire (WS2), a nanowire with an intermediate layer (p-WS2), a nanowire with magnetic nanoparticles attached to the intermediate layer (pm-WS2), and a nanowire with a surface layer (pms-WS2).
[0037] Figure 3 It is a diagram showing the zeta potential of each of WS2, p-WS2, pm-WS2 and pms-WS2 measured using deionized water as a dispersion medium.
[0038] Figure 4 is to observe the bare WS2 nanowires ( Figure 4 (a), WS2) and nanowires with magnetic nanoparticles attached to the middle layer ( Figure 4 (b), Transmission electron micrograph of pm-WS2).
[0039] Figure 5 It is illustrated in Figure 4 (b) STEM-EDS mapping of the area indicated by the square in pm-WS2, Figure 5 (a) is the mapping result of Fe, Figure 5 (b) is the mapping result of oxygen.
[0040] Figure 6 The graph is a graph showing measurement and graphing of X-ray photoelectron spectra (XPS) of each of WS2, p-WS2, pm-WS2, and pms-WS2, and is a graph showing Fe 2p spectra and S 2p spectra.
[0041] Figure 7 This is a diagram showing the FTIR spectrum of the manufactured ion conductive membrane measured and plotted. Figure 7 (a) is the FTIR spectra of the high fluoride ion exchange resin membrane (Recast Nafion) without adding nanowires, 0.5 wt% pms-WS2 / high fluoride ion exchange resin ion conductive membrane, 2 wt% pms-WS2 / high fluoride ion exchange resin ion conductive membrane and 5 wt% pms-WS2 / high fluoride ion exchange resin ion conductive membrane, Figure 7(b) is the FTIR spectra of a 2 wt % pms-WS2 / highly fluorinated ion exchange resin ion conductive membrane and a 2 wt % pm-WS2 / highly fluorinated ion exchange resin ion conductive membrane in which pm WS2 is mixed instead of pms-WS2 in the manufacturing example and the highly fluorinated ion exchange resin membrane contains 2 wt % pm WS2.
[0042] Figure 8 (a) and Figure 8 (b) is a schematic diagram illustrating the structure of IP-pms-WS2 / high fluorinated ion exchange resin membrane and TP-pms-WS2 / high fluorinated ion exchange resin membrane, Figure 8 (c) Figure 8 (d) and Figure 8 (e) are optical photographs of U-pms-WS2 / highly fluorinated ion exchange resin membrane, IP-pms-WS2 / highly fluorinated ion exchange resin membrane, and TP-pms-WS2 / highly fluorinated ion exchange resin membrane.
[0043] Fig. 9 It is observed that U-pms-WS2 / high fluoride ion exchange resin membrane ( Fig. 9 (a)), IP-pms-WS2 / high fluoride ion exchange resin membrane ( Fig. 9 (b)) and TP-pms-WS2 / highly fluorinated ion exchange resin membrane ( Fig. 9 (c) Scanning electron micrograph of the sample.
[0044] Fig.10 It is a graph illustrating the magnetization curves of 5 wt% U-pms-WS2 / high fluoride ion exchange resin membrane, 5 wt% IP-pms-WS2 / high fluoride ion exchange resin membrane and 5 wt% TP-pms-WS2 / high fluoride ion exchange resin membrane measured using a sample vibrating fluxmeter (VSM).
[0045] Fig.11 This is a graph showing measured proton conductivities in the plane and in the direction perpendicular to the plane of an ion conductive membrane as an activated composite membrane.
[0046] Fig.12 This is a graph showing the voltage-current density measured and plotted according to the relative humidity, which is the result of testing the performance of a membrane electrode assembly (MEA) having an ion conductive membrane in which nanowires are arranged in the thickness direction. DETAILED DESCRIPTION
[0047] Hereinafter, the ion conductive membrane of the present invention will be described in detail with reference to the accompanying drawings. The accompanying drawings introduced below are provided as examples in order to fully convey the concept of the present invention to those skilled in the art. Therefore, the present invention is not limited to the accompanying drawings presented below, and can also be embodied in other forms. In order to clarify the concept of the present invention, the accompanying drawings presented below can be enlarged and illustrated. At this time, in the technical terms and scientific terms used, as long as there is no other definition, in the technical field to which the present invention belongs, it has the meaning commonly understood by those skilled in the art. In the following description and drawings, the description of the well-known functions and structures that may unnecessarily confuse the main purpose of the present invention is omitted. In addition, unless otherwise specified in the context, the singular form used in the specification and the attached claims can be understood to also include the plural form. In addition, the expression "including / comprising" in this specification is an open-ended record with equivalent meanings to expressions such as "having", "containing", "having" or "characterized by...", and does not exclude elements, materials or processes that are not further listed. In addition, the expression "consisting essentially of..." means that the amount of other elements, materials or processes not listed together with the specific elements, materials or processes does not have an unacceptable and significant impact on at least one basic and novel technical idea of the present invention. In this specification and the attached claims, when a part such as a film (layer), region, constituent element, etc. is indicated to be on or above another part, it includes not only the case where it is in contact with other parts and is located directly above, but also the case where other films (layers), other regions, other constituent elements, etc. are present in between. In the specification and the attached claims, the units used without special mention are based on weight. As an example, the unit of % or ratio refers to weight % or weight ratio.
[0048] In the present invention, the ion conducting layer may be collectively referred to as an ion exchange membrane or an ion exchange electrolyte membrane, and may refer to a polymer-based membrane having a fixed charge and only allowing ions of opposite polarity to selectively pass (move). In the present invention, the ion conducting membrane may be a cation conducting membrane or an anion conducting membrane. As a non-limiting example, cations may include protons, and anions may include hydroxide ions. Unless otherwise specifically limited, when the ion conducting membrane is a cation conducting membrane, the ions (including ions in the matrix), ion conducting resins, ion conducting materials, etc. collectively referred to below may refer to cations, cation conducting resins, cation conducting materials, etc. that can be conducted through the membrane. As a specific example, the cation conducting membrane may be a proton (hydrogen ion) conducting membrane, and the cations may be protons (hydrogen ions). Similarly, unless otherwise specified or explained, when the ion conductive membrane is an anion conductive membrane, the ions (including ions inside the matrix), ion conductive resins, ion conductive substances, etc. collectively referred to below may refer to anions, anion conductive resins, anion conductive substances, etc. that can be conducted through the membrane.
[0049] According to one embodiment, an ion conductive membrane includes an ion conductive matrix and a one-dimensional dispersed phase dispersed in the ion conductive matrix and oriented along the membrane thickness direction, wherein the one-dimensional dispersed phase includes a core of a non-conductive one-dimensional nanostructure and a surface layer that conducts ions of the same type as ions in the matrix.
[0050] The ion-conducting matrix may be a solid (including gel) medium in which a one-dimensional dispersed phase is dispersed. The ion-conducting matrix may include an ion-conducting polymer.
[0051] The one-dimensional dispersed phase may refer to a dispersion of a one-dimensional structure dispersed in the ion conductive matrix. The one-dimensional dispersed phase may be in a state of being impregnated (embedded) in the ion conductive matrix.
[0052] The one-dimensional dispersed phase may include a one-dimensional nanostructured core and a surface layer that conducts the same type of ions as the matrix. That is, when the matrix is a matrix with cation conductivity, the surface layer may be a cation conductive material, and when the matrix is a matrix with anion conductivity, the surface layer may be an anion conductive material. At this time, the ion conductive material may be an ion conductive polymer material. Since the surface layer is an ion conductive material that conducts the same type of ions as the matrix, the one-dimensional dispersed phase may also conduct ions.
[0053] In a one-dimensional dispersed phase, the surface layer may refer to a layer located at the outermost shell of the one-dimensional dispersed phase. Since the one-dimensional dispersed phase is dispersed in the ion conductive matrix, the one-dimensional dispersed phase may directly contact the ion conductive matrix through the surface layer. Therefore, the interface between the one-dimensional dispersed phase and the ion conductive matrix may be substantially the interface between the surface layer and the ion conductive matrix.
[0054] The one-dimensional nanostructure of the overall shape of the one-dimensional dispersed phase can be the one-dimensional nanostructure of rigidity (rigid) that is not bent (that is, not soft).When the one-dimensional nanostructure has flexibility, it is substantially impossible that the dispersed phase is arranged along a certain direction.Because the core is a rigid one-dimensional nanostructure, the one-dimensional dispersed phase can also have a linear one-dimensional structure, and the surface layer can have a straight one-dimensional structure on a macroscopic level.The microscopic surface layer has a hollow cross section (cross-sectional shape) corresponding to the cross section (cross-sectional shape) of the one-dimensional nanostructure, and is a nanotube (hollow column) shape with a length corresponding to the length of the one-dimensional nanostructure, and can be a nanotube shape that is not bent and straight along the length direction.At this time, the thickness of the surface layer can correspond to the thickness of the tube wall of the nanotube shape.
[0055] That is, the surface layer contains an ion conductive material that conducts the same type of ions as the matrix, so the one-dimensional dispersed phase can provide (can have) an ion conduction path with a one-dimensional structure that is straight on a macroscopic level through the surface layer, and on a microscopic level, can provide a two-dimensional ion conduction path in the shape of a nanotube (hollow cylinder) that is not bent in the longitudinal direction and extends straight.
[0056] Experimentally, the rigid one-dimensional nanostructure (or the one-dimensional dispersed phase including the core of the rigid one-dimensional nanostructure) may mean that the one-dimensional dispersed phase in the ion conductive membrane is observed as a straight line on a microstructure observation image such as a scanning electron microscope observation image.
[0057] The one-dimensional dispersed phase can be oriented along the thickness direction of the ion conductive membrane and impregnated and dispersed in the ion conductive matrix. At this time, the one-dimensional dispersed phase has a one-dimensional structure, so the orientation direction can be the direction from one end of the long axis of the one-dimensional structure to the other end (long axis direction). The one-dimensional dispersed phase contained in the ion conductive membrane can be oriented in the thickness direction of all ion conductive membranes. At this time, the orientation of all one-dimensional dispersed phases in the same direction is to prevent strict mathematical interpretation, and the deviation between the orientation directions of the one-dimensional dispersed phases cannot be mathematically zero. That is, even if the distribution diagram of the orientation direction of the one-dimensional dispersed phase is narrow, it can only be a Gaussian distribution diagram with a dispersion greater than 0. Therefore, it is more appropriate to explain the same orientation direction in the substantially same direction rather than in the strictly same mathematical direction. Experimentally, when the maximum angular difference of the orientation direction of the one-dimensional dispersed phase observed in a scanning electron microscope observation image of an observation area of 10 to 200 μm × 10 to 200 μm of the ion conductive membrane is within 10°, substantially within 8°, and more substantially within 5°, it can be considered to be arranged in the same direction.
[0058] The ion-conducting matrix can conduct ions through a network of three-dimensional ion-conducting channels. Although such a network structure provides many migration paths within the membrane, the ions must pass through relatively long and complex channels until they move a certain distance in the thickness direction of the membrane.
[0059] According to a specific example, an ion conductive membrane includes an ion conductive matrix and a one-dimensional dispersed phase, wherein the one-dimensional dispersed phase includes a surface layer having ion conductivity for conducting ions of the same type, the ion conductive matrix and the surface layer are in contact with each other to form an interface, and the one-dimensional dispersed phase is oriented along the thickness direction of the ion conductive membrane, so that a large number of ions can move smoothly through the network of three-dimensional ion conductive channels, and at the same time can have a significantly improved ion conductivity in the thickness direction of the membrane.
[0060] In detail, if the movement of ions through the ion conductive membrane is observed, in the early stage of the movement, the ions moving through the matrix providing more ion conductive paths can contact the one-dimensional dispersed phase during the movement, and can move in the thickness direction of the membrane through the surface layer of the one-dimensional dispersed phase. That is, the ions collected by the one-dimensional dispersed phase through the ion conductive matrix move along the long axis direction of the one-dimensional dispersed phase through the surface layer of the one-dimensional dispersed phase, so the ion conductive membrane can have a significantly improved ion conductivity in the thickness direction of the membrane.
[0061] As a substantial example, the ion conductive membrane may satisfy the following formula 1.
[0062] (Formula 1)
[0063] 1.5C ref ≤C ICM
[0064] In formula 1, C ICM is the ion conductivity (mS / cm) along the membrane thickness direction of an ion conductive membrane according to a specific example at a relative humidity of 30% and a temperature of 80°C, C ref It is the ion conductivity (mS / cm) in the thickness direction of a membrane (standard membrane) made of an ion conductive resin contained in an ion conductive matrix of an ion conductive membrane under the same conditions. The specific ion conductivity measurement conditions are based on the ion conductivity measurement method in the examples described below.
[0065] Formula 1 means that, according to a favorable example, the ion conductive membrane in which the one-dimensional dispersed phase is oriented in the thickness direction has an ion conductivity (ion conductivity in the thickness direction) that is improved by 50% or more compared to the ion conductivity (ion conductivity in the thickness direction) of a membrane (standard membrane) composed of an ion conductive resin contained in a matrix. As a practical example, the ion conductive membrane in which the one-dimensional dispersed phase is oriented in the thickness direction can have an ion conductivity that is improved by 60% or more, and more practically, can have an ion conductivity that is improved by 70% or more, relative to the standard membrane. Therefore, the ion conductive membrane can satisfy the 1.6C ref ≤C ICM , more practically speaking, it can meet 1.7C ref ≤C ICM .
[0066] In a specific example, the one-dimensional structure of the one-dimensional dispersed phase can be provided by a one-dimensional nanostructure as a core. The one-dimensional nanostructure can be selected from one or more of nanowires, nanotubes and nanorods. However, nanowires with a larger aspect ratio and excellent mechanical properties and mechanical stability are more advantageous.
[0067] The one-dimensional nanostructure can be any non-conductive and rigid material. Considering the use of the ion conductive membrane, in an environment where the membrane is exposed according to the use, it can be any electrochemically stable material. As an example, the one-dimensional nanostructure can be a ceramic, and the one-dimensional ceramic nanostructure can include metal oxides, metal carbides, metal nitrides, metal oxynitrides, metal carbonitrides, metal sulfides or their complexes (solid solutions, intermetallic compounds, etc.). At this time, the metal in the metal oxide, metal carbide, metal nitride, metal oxynitride, metal carbonitride, metal sulfide, etc. can be selected from one or more of alkali metals, alkaline earth metals, transition metals and post-transition metals, but is not limited thereto.
[0068] But, as described later, the same as magnetic nanoparticle, by the electrostatic interaction between the intermediate layer and the one-dimensional nanostructure that contains cationic polymer, thereby the intermediate layer can stably wrap up the one-dimensional nanostructure, in order to increase the bonding force between the intermediate layer and the one-dimensional nanostructure, preferably the one-dimensional nanostructure is the material with negative surface charge (negative zeta potential).As the example of the one-dimensional nanostructure with negative zeta potential, metal oxide or metal chalcogenide etc. can be enumerated, but need not be limited to this.
[0069] In this case, the non-conductive material may refer to a material having a band gap energy greater than 0, specifically, a material having a band gap energy greater than 0.5 eV, greater than 1.0 eV, greater than 1.5 eV, greater than 2.0 eV, or greater than 2.5 eV, but it is not necessarily limited thereto. In this case, the band gap energy of the non-conductive material may actually be less than 6 eV or less than 5 eV.
[0070] In a specific example, the aspect ratio (long axis length / minor axis diameter) of the one-dimensional nanostructure can be 5 to 500, and as a specific example, can be 10 to 500 or 10 to 100, but is not limited thereto. However, a one-dimensional nanostructure with a large aspect ratio is advantageous because it can generate a stable ion conduction path across the membrane in the orientation direction even with a small amount of one-dimensional dispersed phase.
[0071] In a specific example, based on t, which is the thickness of the ion conductive membrane, the major axis length of the one-dimensional nanostructure is 0.005t to 0.500t, specifically 0.010t to 0.300t, 0.010t to 0.200t or 0.010t to 0.100t, but it is not limited to this. At this time, if the thickness of the ion conductive membrane is considered for the purpose, it is sufficient to have a thickness suitable for the purpose. When considering conventional electrochemical elements, the thickness of the ion conductive membrane can be 5 to 300 μm, and can actually be 20 to 200 μm, but it is not limited to this.
[0072] In one specific example, the minor axis diameter of the one-dimensional nanostructure may be 10 1 Nanoscale (10 1 nm order) to 10 2 Nanoscale (10 2In the embodiment of the present invention, the one-dimensional nanostructure has a small minor axis diameter, and ...
[0073] In a specific example, the thickness of the surface layer may be 1 nm to 100 nm, but is not necessarily limited thereto.
[0074] In a specific example, the surface layer can be a continuum that wraps the above-mentioned one-dimensional nanostructure. The surface layer as a continuum can refer to a state in which the ion conductive material contained in the surface layer is continuously connected at least in the length direction of the two-dimensional nanostructure. At this time, the surface layer as a continuum can include not only a simple film (dense film without holes) of the ion conductive material, but also a porous film of the ion conductive material with through-type pores, and a porous film (membrane of a mesh structure) in which the ion conductive material forms a two-dimensional mesh structure.
[0075] In a specific example, when the one-dimensional dispersed phase is regarded as a point existing at the center point in the length direction (the center of gravity of the one-dimensional dispersed phase), the one-dimensional dispersed phase may be randomly distributed in the ion conductive matrix.
[0076] In a specific example, in the ion conductive membrane, the dispersed phase density, which is the number of the one-dimensional dispersed phases present per unit area of the ion conductive membrane, is 500 to 1,000,000 / mm based on a cross section perpendicular to the thickness direction of the ion conductive membrane of the one-dimensional dispersed phase. 2 , but it is not necessarily limited thereto. However, when the density of the dispersed phase is too high, the content of the matrix in the ion conductive membrane is relatively reduced, so that the ion conductivity may be reduced, and when it is too low, the number of ion conductive paths along a certain direction (orientation direction) is reduced, so that the ion conductivity may be reduced. Considering the specific use of the ion conductive membrane, the dispersed phase density can be made to have the above-mentioned appropriate range line.
[0077] In a specific example, the ion conductive resin contained in the ion conductive matrix and the ion conductive material contained in the surface layer of the one-dimensional dispersed phase are different from each other, but any polymer material commonly used to selectively move ions in an ion exchange membrane may be used. In this case, the weight average molecular weight of the polymer material may be in the range of 10,000 to 5,000,000, but is not limited thereto.
[0078] As an example of a polymer substance commonly used for selectively moving ions in an ion exchange membrane, when the ion conductive membrane is a cation conductive membrane, there can be mentioned a polymer having a -SO3 - , -COO - , PO3 2- ,PO3H - 、C6H4O - Typically, polymers containing sulfonate groups (-SO3 - When the ion conductive membrane is an anion conductive membrane, examples thereof include polymers having positively charged ion exchange groups such as primary to quaternary ammonium groups, and typically, polymers containing quaternary ammonium groups that are strong bases are used.
[0079] Examples of commonly used polymers containing sulfonate groups include sulfonated block copolymers, perfluorinated polymers having sulfonate groups on side chains, sulfonated aromatic polymers, etc. As an example of a sulfonated block copolymer, a sulfonated poly(styryl-b-vinyl-r-butenyl-b-styryl) triblock copolymer, polystyryl poly(styryl-b-isobutylenyl-b-styryl) styrene), poly(norbornene ethylstyryl-s-styryl)-b-(n-propyl-p-styryl sulfonate), poly(tert-butylstyryl-b-hydrogenated isoprene-b-sulfonated styryl-b-hydrogenated isoprene-b-tert-butylstyrene) or a combination thereof, but the present invention is not limited thereto. As a perfluorinated polymer having a sulfonate group on the side chain, a fluorine-based resin having a sulfonate group at the end of the side chain with a perfluoroalkylene group as the main skeleton can be cited. As an example, a copolymer of tetrafluoroethylene and perfluoro(alkyl vinyl ether) and sulfonyl fluoride, a sulfonated polymer of α, β, β-trifluorostyrene, or a combination thereof can be cited, but it is not limited thereto. As an example of a sulfonated aromatic polymer, sulfonated polystyrene, sulfonated polysulfone, sulfonated polyethersulfone, sulfonated polyphenylsulfone, sulfonated 2,6-dimethyl polyphenylene ether, sulfonated polyetherketone, sulfonated polyetheretherketone, sulfonated polyimide, sulfonated polyphenylene sulfide, sulfonated polybenzimidazole, sulfonated poly(arylene ether ether nitrile), sulfonated poly(arylene ether sulfone), sulfonated poly(arylene ether benzonitrile), their derivatives or a combination thereof can be cited. The amount of the sulfonate group in the polymer containing the sulfonate group may be 0.1 to 7.0 milliequivalents (meq) / g, but is not limited thereto.
[0080] However, the ion conductivity of the surface layer is preferably greater than that of the matrix. Thus, ions that have passed through the ion-conductive matrix and reached the surface layer of the one-dimensional dispersed phase can continuously move through the surface layer without moving again from the surface layer to the ion-conductive matrix.
[0081] That is, the ion-conductive matrix (or the ion-conductive resin of the matrix) and the surface layer of the one-dimensional dispersed phase (or the ion-conductive substance contained in the surface layer) are different from each other, and the content of ion exchange groups per unit mass of the surface layer substance (the number of ion exchange groups) can be greater than the content of ion exchange groups per unit mass of the matrix substance (the number of ion exchange groups).
[0082] Specifically, the amount of ion exchange groups contained in the ion conductive material contained in the surface layer (equivalent / g, hereinafter referred to as IonEx1) can be greater than the amount of ion exchange groups contained in the ion conductive resin contained in the ion conductive matrix (equivalent / g, hereinafter referred to as IonEx2). In essence, IonEx1 / IonEX2 can be 1.0 to 10.0, and more substantially, it can be 2.5 to 7.0. As a simple example, when the ion conductive matrix and the surface layer are realized by using a polymer containing a sulfonate group as a representative cation conductive material, the amount of sulfonate groups (IonEX2) of the ion conductive resin contained in the ion conductive matrix can be 0.1 to 2.0 milliequivalents / g, and the amount of sulfonate groups (IonEx1) of the ion conductive material contained in the surface layer can be 5.0 to 7.0 milliequivalents / g.
[0083] In addition, advantageously, the ion-conducting resin contained in the ion-conducting matrix may be a resin having an ion-exchange group and a hydrophobic (non-polar, water-repellent) main skeleton. In this case, by the spontaneous phase separation of the ion-conducting resin, the ion-exchange groups aggregate and form cluster domains by their self-assembly characteristics, thereby enabling the ion-conducting matrix to have a three-dimensional network (net-like) ion-conducting channel. When the ion-conducting membrane is activated or utilized, the net-like ion-conducting channel maintains appropriate mechanical properties and swelling, and has a large number of contact points between the ion-conducting channel and the one-dimensional dispersed phase, thereby facilitating the supply of the conducted ions to the one-dimensional dispersed phase through the matrix.
[0084] As a representative example of a cation conductive resin that can form an ion conductive channel of a three-dimensional network (net-like) in an ion conductive matrix, a perfluorinated polymer with a sulfonate group on the side chain can be enumerated, particularly a polymer with a perfluoroalkylene group as the main skeleton and a sulfonate group on the side chain. These materials are also sold as commercial products, for example, known high-fluorinated ion exchange resins (Nafion, Dupont), Dow (Dow Chemical), Aciplex (Asahi Chemical Industries) and Flemion (Asahi Glass). In addition, as a representative example of a surface layer with a large ion exchange group content per unit mass compared to the ion exchange group content per unit mass of the matrix, a sulfonated aromatic polymer can be enumerated, and of course, the present invention is not limited to the type of detailed material that meets the above conditions.
[0085] In a specific example, the ion conductive matrix may further include, together with the ion conductive resin, known additives used in conventional ion exchange membranes to improve mechanical properties or dimensional stability. Examples of such additives include hydrophilic fiber phases such as cellulose nanofibers or polyvinyl alcohol; free radical scavengers such as cerium oxide and aluminum oxide; and metal nanoparticles such as platinum, palladium and cobalt. However, the present invention is not limited to the specific types of additives contained in the ion conductive matrix.
[0086] In a specific example, the one-dimensional dispersed phase is located between the core and the surface layer, and may further include an intermediate layer containing a cationic polymer. The cationic polymer imparts a positive surface potential to the one-dimensional nanostructure, so that the magnetic nanoparticles can be fixed to the one-dimensional nanostructure by electrostatic attraction. Furthermore, when the ion conductive membrane is a cation conductive membrane, the surface layer can be formed by the ionic interaction between the intermediate layer containing the cationic polymer and the ionic conductive material of the surface layer, and the surface layer in which the magnetic nanoparticles are not covered by the intermediate layer can be formed.
[0087] In detail, the magnetic nanoparticles may have a negative zeta potential, and the magnetic nanoparticles may be fixed and bonded to the middle layer by electrostatic attraction. In addition, since the magnetic nanoparticles have a negative zeta potential, the surface layer that selectively covers the middle layer that is exposed without bonding to the magnetic nanoparticles may be formed by the electrostatic repulsion between the material of the surface layer having cation conductivity and the magnetic nanoparticles.
[0088] Since the surface layer does not cover the magnetic nanoparticles and has a structure in which the nanoparticles penetrate, the magnetic nanoparticles can be removed by activating the ion conductive membrane after orientation is achieved in the thickness direction by applying an external magnetic field as described below. Therefore, according to a specific example, the ion conductive membrane includes not only an ion conductive membrane containing magnetic nanoparticles, but also an ion conductive membrane from which the magnetic nanoparticles are removed. In the ion conductive membrane from which the magnetic nanoparticles are removed, the one-dimensional dispersed phase may include: a core of a non-conductive one-dimensional nanostructure, a cation conductive surface layer, and an intermediate layer located between the core and the surface layer and containing a cationic polymer, and the surface layer may be a porous membrane with through-type pores.
[0089] In addition, when the one-dimensional nanostructure has a negative zeta potential, the one-dimensional nanostructure and the intermediate layer, and the intermediate layer and the surface layer may be bonded to each other through ionic interaction.
[0090] Therefore, in an advantageous example, the ion conductive membrane may be a cation conductive membrane, and the one-dimensional nanostructure and the magnetic nanoparticles may each have a negative zeta potential. As a specific example of the one-dimensional nanostructure with a negative zeta potential, metal oxides or metal sulfides may be cited, and as the magnetic nanoparticles with a negative zeta potential, oxide-based magnetic nanoparticles may be cited.
[0091] Examples of cationic polymers for the intermediate layer include, but are not limited to, poly(allylamine hydrochloride), poly(diallyldimethylammonium chloride), poly(acrylamide-diallyldimethylammonium chloride), polyethyleneimine, polymethacryloyloxyethyltrialkylammonium halide, polyarylamine chloride, polyacrylamide, aminoethylated polyacrylamide, polyethyleneamine and polyethyleneamine.
[0092] The intermediate layer containing the cationic polymer may have a thickness sufficient to stably wrap the one-dimensional nanostructure. As a specific example, the thickness of the intermediate layer may be 1 to 100 nm or 3 to 100 nm, but is not limited thereto.
[0093] As described above, the one-dimensional dispersed phase may further include an intermediate layer between the core and the surface layer and containing a cationic polymer, and at the same time, may also include magnetic nanoparticles bonded to the surface of the intermediate layer. The magnetic nanoparticles provide magnetism to the one-dimensional dispersed phase, so that the one-dimensional dispersed phase can be arranged in the direction of application of the magnetic field by an external magnetic field in the manufacturing method described later.
[0094] In a specific example, the magnetic nanoparticles may be paramagnetic nanoparticles, ferrimagnetic nanoparticles, or ferromagnetic nanoparticles. When the magnetic nanoparticles are ferromagnetic nanoparticles, it is advantageous because the one-dimensional dispersed phase can be oriented in the thickness direction of the film by applying an external magnetic field with a small intensity of 0.005T to 0.1T.
[0095] In the process of manufacturing the ion conductive membrane, the magnetic nanoparticles are preferably oxide-based particles having a negative zeta potential from the viewpoint of being stably bonded to the intermediate layer containing proton polymers by electrostatic attraction in a liquid medium and being uniformly dispersed and bonded.
[0096] As an example of oxide-based magnetic nanoparticles having a negative zeta potential according to a favorable example, iron oxide nanoparticles, manganese oxide nanoparticles, gadolinium oxide nanoparticles, erbium oxide nanoparticles, chromium oxide nanoparticles, nickel oxide nanoparticles or a combination thereof can be mentioned, but are not limited to these.
[0097] The magnetic nanoparticles are bound together through the intermediate layer, so that the one-dimensional nanostructure can be endowed with uniform magnetic properties. 1d ) is taken as the reference, the diameter of magnetic nanoparticles (D np ) can be 0.01D 1d Up to 0.30D 1d The level can be 0.01D 1d Up to 0.20D 1d The level, more specifically, can be 0.05D 1d Up to 0.15D 1d level, but is not limited to this.
[0098] The content of the magnetic nanoparticles in the one-dimensional dispersed phase is sufficient as long as the one-dimensional dispersed phase exhibits magnetism to such an extent that the one-dimensional dispersed phase can be arranged in the direction of the applied magnetic field when an external magnetic field is applied to a coating film coated with a liquid containing an ion conductive resin and the one-dimensional dispersed phase. As an example, the one-dimensional dispersed phase may contain 1 to 20 parts by weight of magnetic nanoparticles relative to 100 parts by weight of the one-dimensional nanostructure, but the present invention is not limited thereto.
[0099] In a specific example, the shape and size of the ion conductive membrane can be determined by the ion conductive matrix. That is, the shape of the ion conductive membrane can correspond to the shape of the ion conductive matrix, and the size of the ion conductive membrane can correspond to the size of the ion conductive matrix. The shape and size of the ion conductive membrane can be appropriately adjusted in consideration of the specific use and the scale of the device equipped with the membrane. However, the thickness of the ion conductive membrane can be in the range of 5 to 300 μm, and is actually in the range of 20 to 200 μm, but is not necessarily limited thereto.
[0100] If the ion conductive membrane according to a specific example of the present invention is described in detail from the aspect of ion conductive channels, the ion conductive membrane includes a three-dimensional ion conductive channel in a network; and a thickness direction ion conductive channel which is in contact with the three-dimensional ion conductive channel and is oriented along the thickness direction of the ion conductive membrane and connects the two ends of the one-dimensional nanostructure through a surface layer on the one-dimensional nanostructure.
[0101] As described above, a network of three-dimensional ion-conducting channels can be provided by an ion-conducting matrix. In addition, a thickness-direction ion-conducting channel can be provided by a surface layer of a one-dimensional nanostructure.
[0102] Figure 1 (a) is a schematic diagram illustrating a conduction mechanism of cations (e.g., protons) through a network-like three-dimensional ion-conducting channel formed of a cation-conducting resin, Figure 1 (b) is a schematic diagram illustrating a cation conduction mechanism of an ion-conducting membrane including ion-conducting channels in the thickness direction according to one embodiment of the present invention. Figure 1 The upper figure shows the macroscopic membrane shape and the macroscopic cation conduction path (red arrows). Figure 1 The figure below illustrates the conduction of ions through the ion conduction channel (red arrows). Figure 1 As an example shown in (a), a conventional ion-conducting membrane having a three-dimensional network of ion-conducting channels enables ions to pass through a complex and long path of the membrane and conduct ions along the thickness direction of the membrane. Figure 1 (b) As shown in the example shown in FIG. 1 , the ion conductive membrane according to one embodiment of the present invention is provided with a surface layer ( Figure 1 (b) The proton conductive magnetic 1D material conducts ions, so the shortest distance linear ion conduction can be achieved through such a thickness direction ion conduction channel.
[0103] The ion conductive membrane may be activated by hydration or the like.
[0104] The ion conductive membrane may be an inactive ion conductive membrane.
[0105] The present invention includes a composite for ion conduction.
[0106] According to the present invention, the ion-conducting composite comprises an ion-conducting matrix, and a one-dimensional composite dispersed in the ion-conducting matrix and oriented along the film thickness direction, wherein the one-dimensional composite comprises a core of a non-conductive one-dimensional nanostructure, an intermediate layer wrapping the core and having magnetic nanoparticles bonded to its surface, and a surface layer conducting ions of the same type as the ions in the matrix.
[0107] The ion-conducting composite may correspond to an ion-conducting membrane containing magnetic nanoparticles, and the one-dimensional composite may correspond to a one-dimensional dispersed phase (one-dimensional dispersion) containing magnetic nanoparticles. The ion-conducting composite may correspond to an ion-conducting membrane in an unactivated state in which the ion-conducting channel is not activated by hydration or the like.
[0108] According to the ion-conducting complex of the present invention, it can be converted into the above-mentioned activated ion-conducting membrane by activation. The activated ion-conducting membrane can correspond to the ion-conducting membrane with the magnetic nanoparticles removed. As a specific example, the ion-conducting membrane with the magnetic nanoparticles removed can include an ion-conducting matrix and a one-dimensional dispersed phase dispersed in the ion-conducting matrix, and the one-dimensional dispersed phase can be formed by removing the magnetic nanoparticles bound to the above-mentioned intermediate layer after the one-dimensional complex is arranged along the thickness direction of the membrane by an external magnetic field, and the above-mentioned one-dimensional complex includes a core of a non-conductive one-dimensional nanostructure, an intermediate layer that wraps the above-mentioned core and has magnetic nanoparticles bound to its surface, and a surface layer that conducts ions of the same type as the ions in the above-mentioned matrix.
[0109] In a specific example, a one-dimensional composite may include a one-dimensional nanostructure; an intermediate layer containing a cationic polymer coated on the one-dimensional nanostructure; magnetic nanoparticles bonded to the intermediate layer by electrostatic attraction; and a surface layer containing an ion conductive material that covers the intermediate layer that is not bonded to the magnetic nanoparticles and is exposed to the surface and contains an ion conductive material that conducts the same type of ions as the matrix. In this case, the magnetic nanoparticles may also have a structure that penetrates the surface layer. When the ion conductive composite is a cation conductive composite, the magnetic nanoparticles having a negative zeta potential may be bonded to the intermediate layer that exhibits a positive zeta potential by the cationic polymer by electrostatic attraction. Therefore, the ion conductive material having a negatively charged ion exchange group such as a sulfonate group selectively covers the exposed surface of the intermediate layer that exhibits a positive charge without the magnetic nanoparticles bonding due to the electrostatic repulsion with the magnetic nanoparticles having the same type of charge, thereby forming a structure in which the magnetic nanoparticles penetrate the surface layer.
[0110] The ion conductive matrix in the ion conductive composite, the orientation in the one-dimensional composite oriented in a certain direction, the one-dimensional nanostructure, the intermediate layer, the cationic polymer in the intermediate layer, the magnetic nanoparticles, the surface layer, and the ion conductive material in the surface layer are similar to or identical to the above-mentioned ion conductive matrix, orientation, one-dimensional nanostructure, the intermediate layer, the cationic polymer, the magnetic nanoparticles, the surface layer, and the ion conductive material in the surface layer in the ion conductive membrane.
[0111] The present invention includes a method for activating the above-mentioned ion conducting complex.
[0112] The activation method according to the present invention comprises the step of immersing the above-mentioned ion conducting complex in an aqueous solution (activation solution) containing ions having the same kind of charge as ions conducted through the ion conducting matrix.
[0113] As an example, when the complex is a cation-conducting complex, the aqueous solution may be an aqueous solution containing hydrogen ions, i.e., an acidic aqueous solution. As another example, when the complex is an anion-conducting complex, the aqueous solution may be an aqueous solution containing hydroxide ions, i.e., an alkaline aqueous solution.
[0114] As a representative activation solution based on a cation-conducting complex, the activation solution can be a strong acid aqueous solution, and can be a strong acid aqueous solution including sulfuric acid, radical acid, nitric acid or a mixed acid thereof. The acid concentration in the strong acid aqueous solution can be at a level of 1M to 3M, but the present invention is not limited by the specific type or concentration of the activation solution used during activation, and the activation can be performed using any method or material known to be used to activate a cation exchange membrane or anion exchange membrane in the past. As an example, instead of being immersed in the activation solution, activation can be performed by bubbling or droplet spraying, and activation can also be performed by a normal temperature ionic liquid of a non-aqueous solution. However, when the ion-conducting complex is immersed in the activation solution for activation, an ion-conducting channel, such as a water channel, is formed in the complex, and the magnetic nanoparticles are removed at the same time, and the complex can be converted into an ion-conducting membrane (an ion-conducting membrane with magnetic nanoparticles removed). During activation, by removing the magnetic nanoparticles, in the application of ion-conducting membranes such as fuel cell drives, it is possible to prevent the generation of highly active free radicals by the magnetic nanoparticles, the catalyst poisoning caused by the generated free radicals, the decomposition of ion exchange polymers and other adverse effects.
[0115] The present invention includes the above-mentioned method for producing an ion conductive membrane. In this case, an ion conductive membrane containing magnetic nanoparticles is produced, and an ion conductive membrane not containing magnetic nanoparticles is produced by activation, so the method for producing an ion conductive membrane includes a method for producing an ion conductive composite.
[0116] The method for manufacturing an ion conductive membrane according to the present invention includes the following steps: a step of manufacturing a coating film by coating a composition comprising an ion conductive resin, a one-dimensional composite, and a solvent; and a step of drying the coated coating film, wherein the one-dimensional composite includes a core of a non-conductive one-dimensional nanostructure, an intermediate layer that wraps the core and has magnetic nanoparticles bound to its surface, and a surface layer that conducts ions of the same type as the ions in the ion conductive resin, and before, while, or during the drying of the coating film, a magnetic field is applied along the thickness direction of the coating film to orient the one-dimensional composite along the thickness direction of the film.
[0117] In this case, the one-dimensional composite may correspond to a one-dimensional dispersed phase including magnetic nanoparticles in the ion conductive membrane. In addition, the ion conductive resin may correspond to an ion conductive resin contained in the ion conductive matrix in the ion conductive membrane.
[0118] In the coating step, any coating method known for manufacturing a film by coating a liquid phase or a dispersed phase (suspension, etc.) can be used when applying the composition. As an example, inkjet printing, slot die coating, gravure printing, flexographic printing, blade coating, screen printing, electrostatic hydraulic printing, micro-contact printing, embossing, reverse offset printing, rod coating, gravure offset printing, roller coating, etc. can be used for coating, but it is not limited thereto.
[0119] Based on 100 parts by weight of the ion conductive resin, the composition may contain 0.05 to 10 parts by weight of the one-dimensional complex and 500 to 10,000 parts by weight of the solvent, but is not limited to this. Considering the density of the one-dimensional dispersed phase in the target ion conductive membrane, the content in the composition can of course be appropriately adjusted.
[0120] The solvent can be a polar protic solvent, a non-polar solvent or a mixed solvent thereof. As an example, it can be water, a glycol solvent, a glycol ether solvent, an alcohol solvent, a ketone solvent, an ester solvent, an amide solvent, a sulfoxide or sulfone solvent, a phenolic solvent or a mixed solvent thereof. At this time, the glycol solvent may include ethylene glycol, propylene glycol, butylene glycol, triethylene glycol, hexylene glycol, polyethylene glycol, ethoxydiglycol, dipropylene glycol or a combination thereof, etc., the glycol ether solvent may include methyl glycol ether, ethylene glycol ether, isopropyl glycol ether or a combination thereof, etc., the alcohol solvent may include methanol, ethanol, n-propanol, isopropanol, butanol or a combination thereof, etc., the ketone solvent may include acetone, methyl ethyl ketone, methyl isobutyl ketone or a combination thereof, etc., the ester solvent may include ethyl acetate, butyl acetate, diethylene glycol ether acetate, methoxypropyl acetate, ethylene carbonate, propylene carbonate or a combination thereof, etc., the amide solvent may include dimethylformamide, dimethylacetamide, dimethyl caprylic acid / capric acid fatty acid amide, N-alkylpyrrolidone or a combination thereof, etc., the sulfoxide or sulfone solvent may include dimethyl sulfoxide (DMSO) or cyclopentane sulfone, etc., the phenolic solvent may include toluene or xylene, etc., but is not limited thereto.
[0121] The composition may be a composition in which the ion conductive resin is dissolved in a solvent and a one-dimensional complex is dispersed, or may be a composition in which the ion conductive resin is suspended in a solvent and a one-dimensional complex is dispersed.
[0122] As mentioned above, after the coating composition is applied to manufacture the coating film, the step of applying a magnetic field in the thickness direction of the coating film can be implemented. By applying the magnetic field to the coating film, the one-dimensional complex in the coating film can be oriented in the thickness direction of the coating film. The intensity of the applied magnetic field can be 0.005T to 100T, specifically 0.1T to 100T, and when the magnetic nanoparticles are ferromagnetic nanoparticles, a magnetic field with an intensity of about 0.005T to 0.1T can be applied.
[0123] The magnetic field may be applied to the coating film before, during or after the coating film is dried. The magnetic field may be applied to the coating film at a time when the one-dimensional complex contained in the coating film rotates and can be arranged in the direction of magnetic field application, and the movement of the one-dimensional complex is suppressed.
[0124] Such a time point (time point of applying the magnetic field) is related to the strength of the magnetic field and the viscosity of the composition or the coating film. When a magnetic field of a certain strength is applied, the viscosity of the composition can realize the rotation of the one-dimensional complex, but when it is so high that it is difficult to rotate, the magnetic field can be applied before drying or simultaneously with drying. In addition, in order to have coating adaptability according to a specific coating method, when there is a danger of the one-dimensional complex moving due to the magnetic field when the coating film is formed due to the low viscosity of the composition, a magnetic field can be applied during the drying process. As the drying proceeds, the solvent in the coating film evaporates and is removed. As the viscosity of the coating film increases, by controlling the time point of applying the magnetic field during the drying process, the one-dimensional complex rotates, and is arranged along the direction of application of the magnetic field, and the two-dimensional complex can be prevented from moving from its original position to the direction of application of the magnetic field.
[0125] In consideration of satisfying the above-mentioned coating suitability and controlling the viscosity of the coating film at an appropriate level when a magnetic field is applied, the composition may include a first solvent having a first boiling point and a second solvent having a second boiling point lower than the first boiling point, based on 1 atm of the solvent. At this time, the first solvent and the second solvent may be selected from water, a glycol-based solvent, a glycol ether-based solvent, an alcohol-based solvent, a ketone-based solvent, an ester-based solvent, an amide-based solvent, a sulfoxide or sulfone-based solvent, and a phenolic-based solvent, respectively.
[0126] When the composition contains a first solvent and a second solvent, during the drying of the coating film, the second solvent contained in the coating film evaporates and is removed faster than the first solvent, thereby increasing the viscosity of the coating film. Since the first solvent evaporates and is removed relatively slowly, the viscosity increased by removing the second solvent can be stably maintained for a certain period of time. Therefore, the fluidity of the one-dimensional complex in the coating film when the magnetic field is applied can be controlled by the mixing ratio of the first solvent and the second solvent. In addition, the mixing ratio of the first solvent and the second solvent, the difference in boiling points between the first solvent and the second solvent, etc., take into account the drying temperature and the intensity of the applied magnetic field, and change the time point of applying the magnetic field. Of course, it can be appropriately adjusted by repeated experiments to observe the arrangement and movement of the one-dimensional complex. As a specific example, the mixing volume ratio of the first solvent and the second solvent can be 1:100 to 100:1, the boiling point difference between the first solvent and the second solvent can be 50 to 200°C, specifically 50 to 150°C, the boiling point of the first solvent with a relatively high boiling point can be 150 to 350°C, and the drying temperature can be 50 to the second boiling point * 0.9, but it is not limited thereto. However, the present invention does not exclude a single solvent. By controlling the intensity of the magnetic field applied with a single solvent or the time of applying the magnetic field, the one-dimensional composite structure is arranged (arranged along the direction of magnetic field application), and the movement of the one-dimensional composite can be prevented. At this time, the orientation direction of the one-dimensional composite can be controlled by adjusting the direction of application of the magnetic field. As an example, by applying a magnetic field perpendicular to the coating film, a composite in which the one-dimensional composite is oriented in the thickness direction of the film can be manufactured.
[0127] The magnetic field may be continuously applied until the one-dimensional composite material loses fluidity and is fixed in the coating film to be dried, as an example, until drying is completed.
[0128] According to a specific example of the manufacturing method, a synthesis step of manufacturing a one-dimensional composite may be further included before the coating step.
[0129] The synthesis process includes the following steps: a first step of forming an intermediate layer containing a cationic polymer on a one-dimensional nanostructure; a second step of fixing magnetic nanoparticles on the surface of the intermediate layer by electrostatic attraction under a liquid medium; and a third step of forming a surface layer containing an ion conductive substance on the one-dimensional nanostructure on which the magnetic nanoparticles are fixed and the intermediate layer is formed.
[0130] More specifically, the synthesis step may include the following steps: a first step of forming an intermediate layer containing a cationic polymer on the one-dimensional nanostructure using a one-dimensional nanostructure having a negative zeta potential and a first solution containing a cationic polymer; a second step of using the one-dimensional nanostructure formed with the intermediate layer and a second solution containing magnetic nanoparticles having a negative zeta potential and fixing the magnetic nanoparticles on the surface of the intermediate layer by electrostatic attraction; and a third step of forming a surface layer containing an ion conductive substance using the one-dimensional nanostructure with the magnetic particles fixed and the intermediate layer formed and a third liquid containing an ion conductive substance.
[0131] According to a specific example, when the ion conductive material used to form the surface layer is a cation conductive material, it can electrostatically interact with the intermediate layer to which magnetic nanoparticles are not attached through negatively charged ion exchange groups such as sulfonate groups, and can evenly and stably cover the exposed intermediate layer through strong adhesion.
[0132] In a specific example, the first step may include the following steps: a step of applying ultrasound to a first solution in which a one-dimensional nanostructure is dispersed and a cationic polymer is dissolved; a step of adding a metal salt to the first liquid and stirring. By adding a metal salt to the first liquid, the cationic component (a polymer with a positive charge) of the cationic polymer can wrap the one-dimensional nanostructure faster and more stably. At this time, the metal salt eliminates the electrostatic repulsion between the polymer chains to be coated, thereby forming a thicker and more uniform coating film. The metal salt is dissolved in the first liquid as long as metal particles as cations and counterions as anions are produced. As an example, the metal salt can be a halide of an alkali metal or an alkaline earth metal (for example, chloride, etc.), but is not limited to this.
[0133] The content of the one-dimensional nanostructure and the proton polymer can be any content that can form a stable coating. As an example, the first solution can contain 0.1 to 5.0 g / L of one-dimensional nanostructure, and the concentration of the proton polymer in the first solution can be 0.1 to 5.0 weight %, but is not limited to this. The solvent of the first solution can be any solvent in which the proton polymer is stably dissolved, such as a polar solvent such as water. The amount of metal salt added can also be any amount that can promote the coating of the cationic polymer. As an example, the salt can be added in a manner that the concentration of the metal salt in the first solution is 0.1 to 0.8 M, but is not limited to this. In order to promote the coating of the proton polymer, the first liquid can be heated to about 40 to 70° C. while stirring, but the present invention is certainly not limited to heating or a specific heating temperature.
[0134] In a specific example, the second step can be implemented by dispersing the one-dimensional nanostructure and magnetic nanoparticles formed with the intermediate layer containing the cationic polymer obtained by the first step in a liquid medium. At this time, the liquid medium can be a polar solvent such as water, and the pH of the liquid medium can be controlled to be alkaline in order to further reduce the negative zeta potential of the magnetic nanoparticles to increase the electrostatic attraction between the magnetic nanoparticles and the intermediate layer. At this time, the liquid medium can be controlled to be alkaline using a water-soluble base such as sodium hydroxide, and the pH of the alkaline liquid medium can be controlled to be 9.0 to 12.0, but the present invention is certainly not limited to a specific alkaline substance or a specific pH of the second solution.
[0135] As mentioned above, the cationic polymer with positive charge in intermediate layer and the magnetic nanoparticle with negative zeta potential can only be combined with each other by electrostatic force in the liquid medium through mixed dispersion.The one-dimensional nanostructure that is formed with intermediate layer in the second solution: the mass ratio of magnetic nanoparticle can be 1:0.01 to 0.2 level, but is not limited to this.In addition, in order to be formed with the one-dimensional nanostructure of intermediate layer and the dispersion of magnetic nanoparticle, conventional dispersion means such as ultrasonic wave can be used, but is not limited to this.
[0136] In a specific example, the third step may include the following steps: a step of dispersing the one-dimensional nanostructure to which the magnetic nanoparticles obtained in the second step are attached in the intermediate layer, and applying ultrasound to the third liquid in which the ion conductive material is dissolved; a step of adding a metal salt (a second metal salt) to the third liquid and stirring it. Similar to the case of the first solution, by adding a metal salt to the third solution, the polymer ion conductive material can cover the intermediate layer more uniformly and thicker to form a surface layer. At this time, the metal salt (the second metal salt) is dissolved in the third solution independently of the metal salt (the first metal salt) added to the first solution, as long as it produces metal ions as cations and counter ions as anions. For example, the metal salt may be a halide of an alkali metal or an alkaline earth metal (e.g., chloride, etc.), but is not limited thereto.
[0137] The content of the one-dimensional nanostructure (one-dimensional nanostructure with magnetic nanoparticles attached to the middle layer) and the protonic polymer in the third solution can form a stable coating. As an example, the third solution can contain 0.1 to 5.0 g / L of one-dimensional nanostructure (one-dimensional nanostructure with magnetic nanoparticles attached to the middle layer), and the concentration of the ion conductive material in the third solution can be 0.1 to 5.0 weight %, but it is not limited to this. The solvent of the third solution can be a solvent in which the ion conductive material is stably dissolved, such as a polar solvent such as water. The amount of metal salt added can be as long as it can promote the coating of the ion conductive material. As an example, the salt can also be added in a manner that the salt concentration in the third solution is 0.1 to 0.8 M, but it is not limited to this. In order to promote the coating of the ion conductive material, the third liquid can be heated to about 40 to 70°C while stirring, but the present invention is of course not limited to heating or a specific heating temperature.
[0138] The dry film obtained in the drying step in parallel with the application of the magnetic field may correspond to the above-mentioned ion-conducting composite. According to a specific example of the manufacturing method, an activation step of activating the obtained dry film may be further included after the drying step, and through such an activation step, the ion-conducting resin contained in the matrix and the ion-conducting material contained in the surface layer are hydrated, and a path for conducting ions can be formed. The activation step may correspond to the activation method of the composite mentioned above.
[0139] The present invention includes an ion conductive membrane produced by the above-mentioned production method.
[0140] The present invention includes an ion conducting composite produced by a method including a drying step in parallel with applying a magnetic field before the above-mentioned activation step.
[0141] The present invention includes a device including the above-mentioned ion-conducting membrane. The device can be any known electrochemical device having a cation-conducting membrane (cation exchange membrane or cation electrolyte membrane) or an anion-conducting membrane (anion exchange membrane or anion electrolyte membrane) as a part of the device. Representative examples of such devices include fuel cells, redox flow batteries, electrolysis devices, dialysis devices, water treatment devices, or electrochemical double-layer capacitors. Fuel cells may include proton direct methanol fuel cells (DMFC), polymer electrolyte fuel cells (PEMFC), direct borohydride fuel cells (DBFC), solid alkaline fuel cells (SAFC), etc. In terms of the use of fuel cells, the present invention includes a membrane electrode complex for fuel cells including the above-mentioned ion-conducting membrane. The electrolysis device may include an electrochemical or photoelectrochemical water splitting device, and the dialysis device may include an electrodialysis process (electrodialysis) or a diffusion dialysis process (diffusion dialysis) or an electrodeionization process (electrodeionization) for desalination and purification. The water treatment device may include a Fenton oxidation device, but is not limited to this.
[0142] Below, a WS2 nanowire (short axis diameter 100-200 nm, long axis length 1-2 μm) having a high aspect ratio, straightness due to rigid physical properties, insulating properties, chemical stability in acidic solutions or Fenton solutions, and having a negative zeta potential according to a favorable example is used as a one-dimensional nanostructure, iron oxide nanoparticles having a negative zeta potential are used as magnetic nanoparticles, and taking cation conductivity as an example, a highly fluorinated ion exchange resin, which is a representative ion conductive resin of cation conductivity, is used as a matrix material, and polystyrene sulfonate having better ion conductivity than the highly fluorinated ion exchange resin is used as a surface layer material, and an example of the manufacture of an ion conductive membrane is provided, but this is to help a more comprehensive understanding of the present invention, considering appropriate nanowires for use and examples of using the most commonly used ion conductive substances that meet the conditions according to a specific example. Of course, the present invention is not limited to the substances used in the manufacture examples.
[0143] Manufacturing example
[0144] One-dimensional composite material manufacturing
[0145] The tungsten disulfide (WS2) nanowires were ultrasonically dispersed in a 1 wt% polydiallyldimethylammonium chloride (PDDA, Mw = 200000-3500000, Sigma-Aldrich) aqueous solution for 1 hour to prepare a first solution with a concentration of 1 g / L. Then, NaCl (Sigma Aldrich) was added to the first solution at a concentration of 0.5 M and stirred at 50° C. for 12 hours to form an intermediate layer on the nanowires. The nanowires formed with the intermediate layer were washed three times with deionized water and dried at 50° C.
[0146] The nanowires with intermediate layers and Fe3O4 nanoparticles (10-20 nm) were dispersed in a NaOH aqueous solution at pH 11 for 3 hours and allowed to stand for 12 hours, thereby producing nanowires with fixed nanoparticles. The weight ratio of the nanowires with intermediate layers to the Fe3O4 nanoparticles put into the pH 11 aqueous solution was 10:1. Since the produced nanowires have magnetism due to the magnetic nanoparticles, the nanowires were collected using a magnet and washed three times with a magnet and deionized water.
[0147] The nanowires with magnetic nanoparticles fixed thereon were ultrasonically dispersed in an aqueous solution of 1 wt% polystyrene sulfonate (PSS, Mw=70000, sulfonate group=5.58 meq / g) for 1 hour, thereby producing a third solution with a concentration of 1 g / L. Then, NaCl (Sigma Aldrich) was added to the third solution at a concentration of 0.5 M and stirred at 50° C. for 12 hours, thereby forming a surface layer on the nanowires. The nanowires with the surface layer formed thereon were washed 3 times with deionized water and dried at 50° C.
[0148] In order to confirm the Fe3O4 attached to the surface of WS2 nanowires, transmission electron microscopy (TEM, TalosF200X, FEI) analysis was performed. The WS2 nanowires without any treatment and the WS2 nanowires attached with Fe3O4 were completely dispersed on the TEM grid (Lacey carbon, Cu-200) with a pipette for measurement. At the same time, X-ray energy dispersive spectroscopy (EDS) was performed, and elemental analysis was performed with a silicon drift detector (SDD). The surface charge was measured using a zeta potential meter (Zetasizer Nano ZS90, Malvern (Malvern Nanopotential Analysis), 25°C and atmosphere), and ultrasound was applied to all samples, and they were well dispersed in deionized water at a concentration of 1g / L. The content of polymer-encapsulated WS2 nanowires was analyzed using thermogravimetric analysis (TGA, G209 F1 Libra, NETZSCH), and X-ray photoelectron spectroscopy (XPS, Al K-alpha, ThermoVG Scientific) was used to characterize the surface properties of WS2 nanowires.
[0149] Figure 2 The diagram shows schematic diagrams of bare WS2 nanowires (hereinafter referred to as WS2), nanowires with intermediate layers (hereinafter referred to as p-WS2), nanowires with magnetic nanoparticles attached to the intermediate layers (hereinafter referred to as pm-WS2), and nanowires with surface layers (hereinafter referred to as pms-WS2).
[0150] Figure 3 2 is a diagram showing the measurement of the zeta potential of WS2, p-WS2, pm-WS2 and pms-WS2 using deionized water as the dispersion medium. Figure 3 It can be seen that the cationic polymer is coated on the nanowire with a negative zeta potential and the zeta potential becomes positive, and it can be confirmed that the oxide-based magnetic nanoparticles with a negative zeta potential are attached, the zeta potential decreases, and the PSS as a cationic conductive material covers the surface of the cationic polymer coating (intermediate layer) and finally shows a negative zeta potential.
[0151] Figure 4 The bare WS2 nanowires ( Figure 4 (a), WS2) and nanowires with magnetic nanoparticles attached in the middle layer ( Figure 4 (b), transmission electron micrograph of pm-WS2). Figure 4 It can be seen that the cationic polymer PDDA and the oxide-based magnetic nanoparticles are successfully combined through electrostatic attraction, so that the magnetic nanoparticles with a size of 10-20 nm are uniformly distributed on the surface of p-WS2.
[0152] Figure 5 Pictured Figure 4 The STEM-EDS mapping image of the rectangular area in pm-WS2 is shown in the figure. Figure 5 (a) is the mapping image of iron, Figure 5 (b) is the mapping image of oxygen. Figure 5 It can be seen that the iron oxide nanoparticles are very evenly combined and distributed on the surface of the nanowires through the electrostatic attraction between the intermediate layer and the nanoparticles.
[0153] Figure 6 1 is a diagram showing the X-ray photoelectron spectroscopy (XPS) measurements of WS2, p-WS2, pm-WS2, and pms-WS2, respectively, and is a diagram showing the Fe 2p spectrum and the S 2p spectrum. Figure 6 It can be seen that the Fe 2p peak of Fe3O4 appears at pm-WS2 and pms-WS2, which proves that Fe3O4 is well coated on the surface. In addition, the S 2p peak (169.5 eV) due to the sulfonate group of PSS was observed only in pms-WS2, which confirmed the formation of a PSS surface layer. In addition, by confirming that pms-WS2 moves through a magnet in an aqueous dispersion, it was confirmed that pms-WS2 was well endowed with magnetic properties.
[0154] Preparation of ion-conducting composites
[0155] 5 wt% of a high fluorinated ion exchange resin dispersion (D520, Dupont, high fluorinated ion exchange resin sulfonate group = 0.90 meq / g) and deionized water were mixed and a high fluorinated ion exchange resin powder was prepared using a spray dryer (Buchi, B-290). The obtained high fluorinated ion exchange resin powder was dispersed in dipropylene glycol (DPG) at 10 wt% by a roller mill for 24 hours to prepare a suspension, and then pms WS2 was added to the suspension and a cutting-edge ultrasonic disperser was used. Dispersed for 1 hour, thereby uniformly manufacturing a mixed solution. Then, the mixture solution was cast on a glass plate using a scraper to form a coating film, a 300G magnetic field was applied to the coating film and dried at 60°C. At this time, the nanowires (pms WS2) were mixed in such a way that the nanowire content in the dried coating film (composite film) became 2wt%, 5wt% or 0.5wt%. The thickness of the final dried coating film (composite film) was 40μm. In addition, the magnetic field was applied 2 hours after the start of drying, which is the time point when the viscosity of the coating film increases and the nanowires can rotate and prevent it from moving, and the magnetic field was applied continuously until the drying was completed. At this time, the total drying time was 24 hours.
[0156] Fabrication of ion-conducting membranes
[0157] The fabricated composite membrane was immersed in a 2M sulfuric acid aqueous solution for 12 hours to perform an activation (hydration and protonation) treatment. The activated membrane was then washed with deionized water to remove residual protons and other impurities. After activation, the results of the analysis using TEM / EDS, UV-vis and ICP-MS showed that all magnetic nanoparticles were removed after activation.
[0158] When manufacturing a composite membrane, the direction of application of the magnetic field was applied in a manner parallel to the membrane (indicated by IP- in the manufactured samples and the drawings) or perpendicular to the membrane (indicated by TP- in the manufactured samples and the drawings). For comparison, a composite membrane was manufactured without applying a magnetic field (indicated by U- in the manufactured samples and the drawings) and pms WS2 was added in the same manner. In addition, a control group of composite membranes and ion conductive membranes were manufactured in the same manner without applying a magnetic field and without adding any nanowires (highly fluorinated ion exchange resin membrane) or by adding p-WS2 or pm-WS2 instead of pms-WS2. In the following, in the manufactured samples, the state before activation is referred to as a membrane or a composite membrane, and the activated state is referred to as an ion conductive membrane (or ion conductive membrane).
[0159] Manufacturing of catalyst layers and membrane electrode assemblies for fuel cells
[0160] A Pt-C catalyst (46.2 wt % Pt, TEC10E50E, Tanaka Kikinzoku Kogyo) and dipropylene glycol (DPG) were mixed with an Aquivion 16 ionomer dispersion (25 wt % Aquivionin aqueous solution, D72-25BS, Sigma-Aldrich) by planetary ball milling for 3 hours. The mass ratio of ionomer to Pt-C catalyst was 1:2. The mixed slurry was cast on a polyimide film flatly attached to a glass plate with a spatula and dried in an oven at 60°C for 24 hours to produce a catalyst layer. In order to manufacture a membrane electrode assembly (MEA), the catalyst layer was attached to both sides of the ion conductive membrane. The activation area of the MEA was 25 cm 2 The ion conductive membrane and catalyst layer were pressurized at 20 atm and 135°C for 3 minutes, and then the polyimide membrane was peeled off from the MEA and removed. The Pt loading of the anode catalyst layer and the cathode catalyst layer was 0.2±0.01 mg / cm 2 .
[0161] In order to observe the nanowires arranged on the high-fluorinated ion exchange resin membrane, scanning electron microscopy analysis and optical (BX51, Olympus) analysis were performed. The samples observed with a scanning electron microscope were made by freezing with liquid nitrogen and vacuum sputtering Pt on its surface. In order to confirm the arrangement of the nanowires in the membrane, the magnetic properties of the membrane were measured using a sample vibration fluxmeter (VSM, MPMS3-Evercool, Quantum Design). All samples were placed perpendicular to the magnetic field and the magnetic susceptibility was calculated. Attenuated total reflection-Fourier transform infrared spectroscopy (ATR-FTIR, Thermo Fisher Scientific Instrument, Nicolet iS50) was used at 400-4000cm -1 The properties of the film were measured in the range of 100° to 200°. Prior to the measurement, small angle X-ray scattering (SAXS, NANOPIX, RIGAKU) analysis was performed in the range of 0-0.32° in order to determine the area size of the film. All samples were hydrated with deionized water and sealed with Kapton tape to avoid interference with the measurement. X-rays were transmitted along the thickness direction of the film.
[0162] To measure the proton conductivity, the activated composite membrane (ion exchange membrane) was cut into 1 cm × 4 cm, placed in a horizontal conductivity cell (MCC, Won-A Tech), and assembled into a fuel cell frame. Then, the fuel cell frame was connected to a test bench, and the conductivity was measured under nitrogen atmosphere, 80°C, and various humidity conditions. The horizontal conductivity was measured by current impedance analysis using a 2-probe method (HCP-803, BioLogic Science Instrument). The amplitude of the alternating current was 10 mV, and the frequency was 1 MHz to 0.1 Hz. The conductivity value (σ) of the membrane was calculated by the following formula: σ = l / (R·A). In the formula, l, R, and A correspond to the distance between the electrodes, the ohmic resistance, and the area of the ion conductive membrane, respectively.
[0163] For fuel cell testing and electrochemical analysis of MEA equipped with the fabricated ion-conducting membrane, the MEA was assembled from a pair of gas diffusion media (JNT 20A3, JNTG), a pair of gaskets, and a pair of graphite blocks with a single serpentine flow field. A load of 8 volts was applied to the assembled single cell, and a torque of 80 kgf·cm was applied. The polarization curve of the single cell was measured using a fuel cell test station (CNL), and the measurement was carried out without back-pressure under relative humidity conditions of 30%, 50%, 80%, and 100% and a temperature of 80°C. Hydrogen and air were flowed into the anode and cathode, and the flow rates of hydrogen and air were 500 sccm and 1400 sccm, respectively. In order to evaluate the ohmic resistance of the single cell, electrochemical impedance spectroscopy (ESI) analysis was carried out using an AC impedance analyzer (HCP-803, BioLogic Science Instrument). In the ESI analysis, the amplitude was 10 mV and the frequency was 0.45 V to 100 kHz-100 mHz. In addition, in order to check the crossover and short-circuit of hydrogen, linear sweep voltammetry was performed in the range of 0.07 to 0.7 V under a hydrogen / nitrogen atmosphere with a scan rate of 1 mVs -1 .
[0164] The results of the composite film fabrication were observed by optical microscopy. 2 / Highly fluorinated ion exchange resin membrane or pmWS 2 In the case of pms-WS2 / high fluoride ion exchange resin membrane, the miscibility was poor, and thus it was confirmed that the nanowires could not be evenly distributed and aggregated in the high fluoride ion exchange resin matrix. In contrast, it was confirmed that in the case of pms-WS2 / high fluoride ion exchange resin membrane, separation of the nanowires did not occur, and a transparent film in which the nanowires were evenly dispersed was manufactured. This can be explained by the fact that the matrix and the surface layer of the nanowires are substances that conduct the same kind of ions, so they have very high miscibility (affinity) with each other.
[0165] To confirm the addition of protons, the activated pms-WS was observed using attenuated total reflectance-Fourier transform infrared spectroscopy (ATR-FTIR). 2 / Highly fluorinated ion exchange resin membrane. Figure 7 is a diagram illustrating the measurement of the FTIR spectrum of the manufactured film, Figure 7(a) is a high fluoride ion exchange resin membrane without nanowires (Recast Nafion), 0.5 wt% pms-WS2 / high fluoride ion exchange resin membrane, 2 wt% pms-WS2 / high fluoride ion exchange resin membrane and 5 wt% pms-WS 2 / FTIR spectrum of high fluorinated ion exchange resin membrane, Figure 7 (b) is the FTIR spectra of 2 wt % pm-WS2 / highly fluorinated ion exchange resin membrane and 2 wt % pm-WS2 / highly fluorinated ion exchange resin membrane containing 2 wt % pm-WS2 by replacing pms-WS2 with mixed pm-WS2 in the manufacturing example.
[0166] from Figure 7 (a) It can be seen that for each film produced, the spectrum is found to be between 1400 and 2100 cm -1 The range of 1740cm -1 and 1630cm -1 The two peaks centered at + ·(H2O) n ]) bending mode, bulk water δ[(H2O) n ] bending mode. It can be seen that with the increase of the amount of pms-WS2, relative to 1630cm -1 Peak 1740cm -1 The intensity of the peak increases. This means that SO3 is locally concentrated on the surface of WS2. -1 The more ion exchange groups (ion exchange groups derived from PSS) contained in pms-WS2, the higher the concentration of protons in the water cluster. In the same range, there is no big difference in the FTIR spectra between pm-WS2 / high fluorinated ion exchange resin membrane and high fluorinated ion exchange resin membrane. It can also be seen that 1740 cm -1 The increase in peak intensity is attributed to PSS.
[0167] Figure 8 (a) and Figure 8 (b) is a schematic diagram illustrating the structure of IP-pms-WS2 / high fluorinated ion exchange resin membrane and TP-pms-WS2 / high fluorinated ion exchange resin membrane, Figure 8 (c) Figure 8 (d) and Figure 8 (e) Optical photographs of U-pms-WS2 / high fluoride ion exchange resin membrane, IP-pms-WS2 / high fluoride ion exchange resin membrane and TP-pms-WS2 / high fluoride ion exchange resin membrane. Figure 8The direction of applied magnetic field is shown in purple B. Fig. 9 It is observed that U-pms-WS2 / high fluoride ion exchange resin membrane ( Fig. 9 (a)), IP-pms-WS2 / high fluoride ion exchange resin membrane ( Fig. 9 (b)) and TP-pms-WS2 / highly fluorinated ion exchange resin membrane ( Fig. 9 (c) Scanning electron micrograph of the sample.
[0168] from Figure 8 and Fig. 9 The observation results show that when no magnetic field is applied, the pms-WS2 nanowires are randomly embedded in the form of micro-sized bundles. However, when a magnetic field is applied during the drying process, the pms-WS2 nanowires form a structure arranged along the direction of the magnetic field. Each arranged pms-WS2 bundle is significantly smaller than 10μm, indicating that they are uniformly distributed in the high-fluorinated ion exchange resin membrane.
[0169] Fig.10 It is a graph illustrating the magnetization curves of 5 wt% U-pms-WS2 / high fluoride ion exchange resin membrane, 5 wt% IP-pms-WS2 / high fluoride ion exchange resin membrane and 5 wt% TP-pms-WS2 / high fluoride ion exchange resin membrane measured using a sample vibrating fluxmeter (VSM).
[0170] from Fig.10 It can be seen that the degree of magnetization is different according to the orientation of the pms-NW in the high-fluorination ion exchange resin membrane. When the direction of the magnetic field (VSM magnetic field applied in the thickness direction of the membrane) is the same as the arrangement direction of the nanowires, it can be seen that the magnetization becomes stronger. Compared with the unarranged U-pms-WS2 / high-fluorination ion exchange resin membrane, the TP-pms-WS2 / high-fluorination ion exchange resin membrane arranged in the thickness direction shows a strong magnetization, and the IP-pms-WS2 / high-fluorination ion exchange resin membrane in the horizontal direction shows a weaker magnetization under the change of the external magnetic field. That is, the TP-pms-WS2 / high-fluorination ion exchange resin membrane in the thickness direction is parallel to the magnetic field direction, and the IP-pms-WS2 / high-fluorination ion exchange resin membrane in the horizontal direction is perpendicular to the magnetic field direction. Therefore, it can be seen that the magnetic susceptibility is TP-pms-WS2 / high-fluorination ion exchange resin membrane, U-pms-WS2 / high-fluorination ion exchange resin membrane, and IP-pms-WS2 / high-fluorination ion exchange resin membrane, respectively. The magnetic susceptibility was calculated by VSM measurement. The magnetic susceptibilities of TP-pms-WS2 / highly fluorinated ion exchange resin membrane, U-pms-WS2 / highly fluorinated ion exchange resin membrane, and IP-pms-WS2 / highly fluorinated ion exchange resin membrane were 201.14, 62.18, and 29.94, respectively.
[0171] Although not necessarily limited to this explanation, in an ion-conducting membrane, the effect of nanowires on ion conductivity can be divided into two parts. One is an "additive effect" that occurs according to the content of functionalized nanowires on the surface, and the other is an "alignment effect" that promotes ion movement in the alignment direction when the proton transfer channels of the nanowires are aligned. That is, the abundant proton transport channels on the nanowire surface provide a less complicated proton transport path and also allow directional transport of proton ions.
[0172] Fig.11 is a graph showing the measurement of the proton conductivity of the ion-conductive membrane as the activated composite membrane. Fig.11 (a) and Fig.11 (b) is a graph showing the measurement and diagram of the ion conductivity of protons according to relative humidity for 2 wt % U-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown by circles), 2 wt % IP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown by squares), 2 wt % TP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown by triangles), and a high fluoride ion exchange resin membrane (recast high fluoride ion exchange resin, shown by black solid circles) manufactured in the form of a high fluoride ion exchange resin suspension without adding nanowires and manufactured in the same manner as in the manufacturing example. Fig.11 (a) is a graph showing the measured proton ion conductivity in the thickness direction (plane) of the membrane. Fig.11 (b) is a graph showing the measured proton ion conductivity in the in-plane direction of the membrane. Fig.11 (c) is a graph showing the measurement and diagram of the ion conductivity of protons in the through-plane direction according to relative humidity for 0.5 wt % TP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown as diamonds), 2 wt % TP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown as triangles), and 5 wt % TP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown as inverted triangles). Fig.11(d) is a graph showing the moisture content (weight %) of 2 wt % U-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown as a circle), 2 wt % TP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown as a triangle), 5 wt % TP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane (shown as an inverted triangle), and a high fluoride ion exchange resin membrane (Recast high fluoride ion exchange resin, represented by a black solid circle) manufactured in the form of a high fluoride ion exchange resin suspension without adding nanowires and in the same manner as in the manufacturing example, respectively.
[0173] from Fig.11 It can be seen that the proton conductivity increases to 2 wt% pms-WS2, but it can be seen that the proton conductivity decreases as the content of pms-WS2 increases to 5 wt%. This can be explained by the fact that although the proton conductivity increases to pms-WS2 due to the addition effect, when the content of pms-WS2 is too large, the ionomer material in the ion conductive membrane decreases and the proton conductivity decreases.
[0174] The proton conductivity in the thickness direction is actually very important because it is directly connected to the ohmic resistance of the electrochemical cell. Fig.11 (a) The results of comparing the proton conductivity in the vertical direction of the high fluoride ion exchange resin membrane of 2 wt% U-pms-WS2 / high fluoride ion exchange resin ion conductive membrane, 2 wt% IP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane, and 2 wt% TP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane, the membrane arranged along the thickness direction (-TP) showed the highest conductivity in the thickness direction, regardless of the relative humidity, which is the result that proves that the proton movement path is consistent with the thickness direction. The proton conductivity of the horizontally oriented membrane (-IP) in the thickness direction is lower than that of the high fluoride ion exchange resin membrane. Similarly, it can be seen that the nanowires arranged horizontally in the proton transfer direction (vertical direction) have the effect of preventing movement. Based on the conductivity in the thickness direction, the proton conductivity of the membrane arranged along the thickness direction at a relative humidity of 40% is 70% higher than that of the recast high fluoride ion exchange resin membrane. Therefore, it can be seen that by arranging the proton-conducting channels in the thickness direction, it can be effectively used as a proton exchange membrane even under low humidity.
[0175] In addition, comparison Fig.11(b) The results of the horizontal proton conductivity of 2 wt% U-pms-WS2 / high fluoride ion exchange resin ion conductive membrane, 2 wt% IP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane, 2 wt% TP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane and high fluoride ion exchange resin membrane, the horizontally arranged (IP-) membrane has a higher conductivity than the unarranged membrane under all humidity conditions, which is due to the arrangement effect. In addition, the proton conductivity of the (TP-) ion conductive membrane arranged in the thickness direction is lower than that of the unarranged membrane, which means that the nanowires perpendicular to the proton transfer direction interfere with the movement of protons through the high fluoride ion exchange resin membrane. At a relative humidity of 30%, the in-plane conductivity of the IP-pms-WS2 / high fluoride ion exchange resin ion conductive membrane is 46.6% higher than that of the high fluoride ion exchange resin membrane.
[0176] Fig.12 The results are the results of testing the performance of a membrane electrode assembly (MEA) equipped with an ion conductive membrane in which nanowires are arranged in the thickness direction, and the relative humidity is divided into 30% ( Fig.12 (a) ), 50%( Fig.12 (b)), 80%( Fig.12 (c))、100%( Fig.12 (a)) and the voltage-current curve measured at 80°C (shown as boxes in the figure). For comparison, the results of MEAs made using ion-conducting membranes (U-pms-WS2 / high-fluorinated ion exchange resin ion-conducting membranes, shown as triangles) and high-fluorinated ion exchange resin membranes (recast high-fluorinated ion exchange resins, shown as circles) without applying a magnetic field when drying are also shown together, and the power performance gain is numerically compared through the arrangement effect and the addition effect. The overall power performance is undoubtedly determined by the proton conductivity. Regardless of the relative humidity, the membrane arranged along the thickness direction (TP-) shows much higher performance than the unarranged membrane (U-) and the high-fluorinated ion exchange resin membrane. The power performance gain increases with decreasing relative humidity, indicating that a well-connected and arranged high-speed movement path of protons is particularly important at low relative humidity. The power density of the membrane arranged along the thickness direction (-TP) is 336mW / cm at 0.4V 2 , and 160.4mW / cm 2 Compared with the high fluorinated ion exchange resin membrane, it is 110% higher and 201.5mW / cm 2 Compared with the unaligned film (U-), it is further increased by 67.1%.
[0177] The difference between the unaligned membrane (U-) and the high fluorinated ion exchange resin membrane can be explained as being due to the addition effect. Although the addition of nanowires forming ion conduction paths slightly improves the power performance at low humidity of 30-50%, the power performance is almost the same at high relative humidity of 80-100%. That is, the presence of more conductive proton conduction channels (channels provided by nanowires) is effective at lower relative humidity, but at higher relative humidity, conduction is well performed even through the high fluorinated ion exchange resin matrix, so it can be explained that the effect is not so good.
[0178] On the contrary, the alignment effect is significant in all relative humidity ranges, and designs such as proton high-speed movement paths arranged in the thickness direction are general strategies that can improve power performance in all relative humidity ranges. Observing the experimental results of proton conductivity, it is shown that the optimal content of pms-WS2 for maximum ionic conductivity is 2wt%, which is consistent with the power performance results.
[0179] As described above, in the present invention, specific matters and limited embodiments and drawings are used to illustrate, but this is only provided to help a more comprehensive understanding of the present invention, and the present invention is not limited to the above embodiments. Any person skilled in the art to which the present invention belongs can make various modifications and variations based on the above descriptions.
[0180] Therefore, the concept of the present invention is not limited to the described embodiments, and not only the claims described below, but also all modifications that are equivalent to or have equivalents to the claims belong to the scope of the concept of the present invention.
Claims
1. An ion-conducting membrane, wherein the one-dimensional dispersed phase is oriented along the membrane thickness direction, characterized in that: comprising an ion-conducting matrix, and a one-dimensional dispersed phase dispersed in the ion-conducting matrix, The one-dimensional dispersed phase is formed by removing the magnetic nanoparticles bound to the intermediate layer after the one-dimensional complex is arranged along the thickness direction of the membrane by an external magnetic field. The one-dimensional complex includes: a core of a non-conductive one-dimensional nanostructure, an intermediate layer that wraps the core and has magnetic nanoparticles bound to its surface, and a surface layer that conducts ions of the same type as the ions in the matrix.
2. The ion conductive membrane according to claim 1, wherein The ion conductivity is cation conductivity, and the intermediate layer contains a cationic polymer.
3. The ion conductive membrane according to claim 2, wherein The magnetic nanoparticles have a negative zeta potential and are fixed and bound to the intermediate layer by electrostatic attraction.
4. The ion conductive membrane according to claim 2, wherein The one-dimensional nanostructure has a negative zeta potential, and the one-dimensional nanostructure and the intermediate layer, and the intermediate layer and the surface layer are each bonded to each other through an ionic interaction.
5. The ion conductive membrane according to claim 1, wherein The one-dimensional nanostructure is selected from one or more of nanowires, nanotubes and nanorods.
6. The ion conductive membrane according to claim 1, wherein The dispersed phase density, which is the number of the one-dimensional dispersed phase per unit area of the ion conductive membrane, is 500 to 1,000,000 / mm based on a cross section perpendicular to the orientation direction of the one-dimensional dispersed phase. 2 .
7. The ion conductive membrane according to claim 1, wherein The thickness of the surface layer is 1 to 100 nm.
8. The ion conductive membrane according to claim 2, wherein The substrate or surface layer contains a sulfonated block copolymer, a perfluorinated polymer having sulfonate groups on the side chains, or a sulfonated aromatic polymer.
9. The ion conductive membrane according to claim 2, wherein The ionic conductivity of the surface layer is greater than the ionic conductivity of the matrix.
10. The ion conductive membrane according to claim 2, wherein The cationic polymer is selected from one or more of poly(allylamine hydrochloride), poly(diallyldimethylammonium chloride), poly(acrylamide-diallyldimethylammonium chloride), polyethyleneimine, polymethacryloyloxyethyltrialkylammonium halide, polyarylamine chloride, polyacrylamide, aminoethylated polyacrylamide, polyethyleneamine and polyethyleneamine.
11. The ion conductive membrane according to claim 2, wherein The surface layer is a porous film having through-type pores.
12. The ion conductive membrane according to claim 1, wherein The magnetic nanoparticles are ferromagnetic nanoparticles.
13. A method for producing an ion-conducting membrane, comprising the following steps: a coating step of coating a composition comprising an ion conductive resin, a one-dimensional composite, and a solvent to produce a coating film; as well as a drying step of drying the coating film, The one-dimensional composite body includes: a non-conductive one-dimensional nanostructure core, an intermediate layer that wraps the core and has magnetic nanoparticles bonded to its surface, and a surface layer that conducts the same type of ions as the ions in the ion conductive resin. Before, during or at the same time as the drying of the coating film, a magnetic field is applied along the thickness direction of the coating film to orient the one-dimensional composite along the thickness direction of the film. The manufacturing method further comprises a one-dimensional composite manufacturing step before the coating step. The one-dimensional composite manufacturing process includes the following steps: A first step of forming an intermediate layer containing a cationic polymer on a one-dimensional nanostructure; A second step of fixing magnetic nanoparticles having a negative zeta potential on the surface of the intermediate layer by electrostatic attraction in a liquid medium; and The third step is to form a surface layer on the one-dimensional nanostructure having the magnetic nanoparticles fixed thereto and the intermediate layer formed thereon.
14. The method for producing an ion conductive membrane according to claim 13, wherein: The ion conductive resin is a cation conductive resin, and the one-dimensional nanostructure has a negative zeta potential.
15. The method for producing an ion conductive membrane according to claim 13, wherein: The solvent is water, a glycol solvent, a glycol ether solvent, an alcohol solvent, a ketone solvent, an ester solvent, an amide solvent, a sulfoxide or sulfone solvent, a phenolic solvent or a mixed solvent thereof.
16. The method for producing an ion conductive membrane according to claim 13, wherein: The composition contains 0.05 to 10 parts by weight of the one-dimensional complex and 500 to 10,000 parts by weight of a solvent based on 100 parts by weight of the ion conductive resin.
17. The method for producing an ion conductive membrane according to claim 14, wherein: After the drying step, the method further includes an activation step of immersing the obtained dried film in an acidic aqueous solution for activation.
18. The method for producing an ion conductive membrane according to claim 17, wherein: During the activation, the magnetic nanoparticles are removed.
19. The method for producing an ion conductive membrane according to claim 13, wherein: The intensity of the magnetic field is 0.1T to 100T.
20. The method for producing an ion conductive membrane according to claim 13, wherein The magnetic nanoparticles are ferromagnetic nanoparticles, The intensity of the magnetic field is 0.005T to 0.1T.