Membrane electrode assembly, electrochemical device, and electrochemical system
The membrane electrode assembly with BaZr1-xMxO3-γ solid electrolyte and LSCFPd electrodes addresses low power generation efficiency by reducing reaction resistance, enhancing proton conductivity, and improving efficiency and durability at low temperatures.
Patent Information
- Application Number
- CN202080007992.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-04-26
- Filing Date
- 2020-03-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-03-09
Smart Images

Figure CN113260737B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a membrane electrode assembly, an electrochemical device, and an electrochemical system. Background Art
[0002] As electrochemical devices having a membrane electrode assembly including an electrolyte membrane, solid oxide fuel cells, water electrolysis units, and steam electrolysis units are known. Among the solid electrolytes of the electrochemical devices, oxygen ions (O 2 ) represented by stabilized zirconium oxide are widely used. 2- ) conductor. The lower the temperature, the lower the ion conductivity of the oxygen ion conductor. Therefore, for example, in a solid oxide fuel cell using stabilized zirconium oxide as a solid electrolyte, an operating temperature of 700°C or higher is preferred.
[0003] However, in electrochemical devices using solid electrolytes composed of solid oxides, such as solid oxide fuel cells, as their operating temperatures increase, there are issues such as the need for high performance of thermal insulation materials, or the increase in cost due to the increase in thickness of thermal insulation materials, and the need for expensive special heat-resistant metals for metal materials used in structural components, which increase the overall cost of the system. In addition, due to high-temperature operation, there are also issues such as reduced system reliability due to the difference in thermal expansion of the components during start-up and stop, and increased start-up time and energy. Therefore, lowering the operating temperature of electrochemical devices using solid electrolytes composed of solid oxides has become one of the major goals in their practical application.
[0004] Non-patent document 1 discloses an electrochemical device that uses a lanthanum strontium cobalt iron compound containing palladium (Pd) as an air electrode capable of achieving a low operating temperature, and uses Ce as a reaction prevention layer for preventing a reaction between an electrolyte and an air electrode caused by contact between the two. 0.9 G 0.1 O 1.95 , zirconium oxide added with 8 mol% yttrium oxide (Y2O3) is used as the electrolyte membrane, and a mixture of nickel (Ni) and zirconium oxide added with yttrium oxide, namely metal ceramic (cermet), is used as the fuel electrode to form an electrochemical unit, which has an active solid electrolyte layer stack at 600°C to 800°C, namely a membrane electrode assembly composed of an air electrode and an electrolyte membrane.
[0005] Prior art literature
[0006] Non-patent document 1: Shaoli Guo et al., “B-Site Metal (Pd, Pt, Ag, Cu, Zn, Ni) Promoted La1-xSrxCo1-yFeyO3-δPerovskite Oxides as Cathodes for IT-SOFCs”, Catalysts, MDPI, 2015, Vol. 5, Issue 1, pp. 366-391 Summary of the invention
[0007] However, in electrochemical devices using conventional membrane electrode assemblies, power generation efficiency at low temperatures of 600° C. or lower is insufficient.
[0008] Therefore, the present disclosure provides a membrane electrode assembly and the like that can improve power generation efficiency.
[0009] A membrane electrode assembly in one embodiment of the present disclosure comprises: an electrolyte membrane including a solid electrolyte, and a first electrode bonded to the electrolyte membrane, wherein the solid electrolyte is composed of a composition formula (1): BaZr 1-x M x O 3-γ The compound represented by the composition formula (1) is characterized in that M is at least one element selected from Sc, Er, Ho, Dy, Gd, Y, In, Tm, Yb and Lu, and satisfies 0<x<1 and 0<γ<0.5, and the first electrode comprises lanthanum strontium cobalt iron palladium composite oxide.
[0010] An electrochemical device according to one aspect of the present disclosure includes the above-mentioned membrane electrode assembly and a second electrode, wherein the electrolyte membrane is disposed between the first electrode and the second electrode.
[0011] An electrochemical system according to one aspect of the present disclosure includes the electrochemical device described above.
[0012] The membrane electrode assembly and the like disclosed herein can improve power generation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a cross-sectional view schematically showing the structure of the membrane electrode assembly according to the first embodiment.
[0014] Figure 2 is a diagram showing a table of properties of BZM containing various dopants.
[0015] Figure 3 This is a cross-sectional view schematically showing the battery structure of the second embodiment.
[0016] Figure 4This is a diagram showing materials used in membrane electrode assemblies for evaluation in Examples and Comparative Examples 1 to 3, and a table showing measurement results of ohmic resistance and reaction resistance at 600°C.
[0017] Figure 5 The table shows materials used in the membrane electrode assemblies for evaluation in Examples and Comparative Examples 1 to 3, and measurement results of the terminal voltage, ohmic resistance, and reaction resistance at each temperature.
[0018] Figure 6 This is a diagram showing an example of the results of AC impedance measurement using a Cole-Cole curve.
[0019] Fig. 7A This is a graph showing the current-voltage performance of the membrane electrode assembly for evaluation in Example 1 and Comparative Example 1 at 600°C.
[0020] Figure 7B This is a graph showing the current-voltage performance of the membrane electrode assembly for evaluation in Example 1 and Comparative Example 1 at 500°C. DETAILED DESCRIPTION
[0021] (The process of obtaining the method of the present disclosure)
[0022] When a membrane electrode assembly having a lanthanum strontium cobalt iron palladium compound (hereinafter referred to as "LSCFPd") as an air electrode and a solid electrolyte having oxygen ion conductivity, i.e., yttria-doped zirconium oxide (hereinafter referred to as "YSZ"), is used at about 600°C, the ion conduction of the solid electrolyte is overwhelmingly greater than the electron conduction of the solid electrolyte. Therefore, the terminal voltage of a power device having a membrane electrode assembly when the external extraction current (hereinafter referred to as "external current") is 0A is substantially consistent with the voltage calculated by the Nernst equation.
[0023] Specifically, the present inventors studied the conventional membrane electrode assembly disclosed in Non-Patent Document 1 to obtain a membrane electrode assembly with high ion conductivity at low temperatures. As a result, the present inventors obtained the following findings. That is, as disclosed in Non-Patent Document 1, the present inventors have studied the conventional membrane electrode assembly disclosed in Non-Patent Document 1 to obtain a membrane electrode assembly with high ion conductivity at low temperatures. 0.9 G 0.1 O 1.95 When a membrane electrode assembly in which cerium oxide (CeO2) (hereinafter referred to as "GDC") was substituted with gadolinium oxide (Gd2O3) as a part of a membrane electrode assembly was used in an electrochemical device (such as a fuel cell), the case where a lanthanum strontium cobalt iron compound (hereinafter referred to as "LSCF") was used as the air electrode was compared with the case where LSCFPd, which has a higher activity than LSCF, was used as the air electrode, and the finding was that the terminal voltages were the same when the external current was 0 A.
[0024] On the other hand, a membrane electrode assembly has been proposed, which comprises, as a solid electrolyte, barium zirconate to which yttrium is added (hereinafter referred to as "BZY"), or a solid electrolyte in which yttrium constituting BZY is replaced with ytterbium (hereinafter referred to as "BZYb"), and as an air electrode, a cathode electrode layer composed of a lanthanum strontium cobalt compound (hereinafter referred to as "LSC"), and uses a solid electrolyte having proton conductivity operating at 500°C to 800°C. + ) The conductor is used in the membrane electrode assembly of the solid electrolyte, and the hole conductivity increases to a level that cannot be ignored relative to the proton conductivity in the solid electrolyte. Therefore, the terminal voltage of the power device using the membrane electrode assembly when the external current is 0A is different from the theoretical voltage calculated according to the Nernst formula and becomes lower than the theoretical voltage. Here, if a highly active air electrode material is used in power generation, the exchange current density when the external current is 0A increases. As a result, the terminal voltage increases when the external current is 0A, and the power generation efficiency is also improved by the increase in the terminal voltage. Furthermore, even when the external current is above 0A, the terminal voltage increases and the power generation efficiency is also improved.
[0025] In order to improve the power generation efficiency of a membrane electrode assembly using a solid electrolyte having proton conductivity, it is desired to realize a membrane electrode assembly having a high inter-terminal voltage when an external current is 0 A.
[0026] Specifically, the following problem was discovered: when a membrane electrode assembly used in an electrochemical device is a combination of an air electrode composed of a lanthanum strontium cobalt iron compound (hereinafter referred to as "LSCF") and a BaZr 1-x MxD 3-γ In the case of the structure of the electrolyte membrane composed of the solid electrolyte represented by the embodiment, the voltage between the terminals is low when the external current is 0 A, and further, a sufficiently high voltage between the terminals and power generation efficiency cannot be obtained when the external current is above 0 A. Therefore, the inventors further studied the combination of electrodes and electrolyte membranes that can increase the voltage between the terminals when the external current is 0 A and obtain high power generation efficiency, thereby obtaining the present disclosure.
[0027] That is, the inventors found that when BaZr 1-x M x O 3-γ (wherein, a proton conductor represented by 0<x<1 and 0<γ<0.5) is used for the electrolyte membrane, and LSCFPd obtained by replacing some sites of cobalt and iron constituting LSCF with palladium is used in the membrane electrode assembly of the air electrode, and the air electrode composed of LSCF and the air electrode composed of BaZr 1-x MxD 3-γCompared with the membrane electrode assembly of the electrolyte composed of the present invention, the terminal voltage when the external current is 0 A is improved, and even when the external current is 0 A or more, the terminal voltage becomes larger, and the power generation efficiency can be improved even at a low temperature of 600° C. or less.
[0028] This is believed to be due to the fact that the air electrode composed of LSCFPd and the 1-x MxD 3-γ The membrane electrode assembly obtained by combining an electrolyte membrane composed of a solid electrolyte represented by (wherein 0<x<1 and 0<γ<0.5, hereinafter referred to as "BZM") can reduce the reaction resistance component of the air electrode generated between the air electrode, the electrolyte membrane and the gas at a temperature of 600℃ which is lower than 700℃, and further at a low temperature of 500℃, compared with the membrane electrode assembly obtained by combining an air electrode composed of LSCF and an electrolyte membrane composed of BZM.
[0029] In addition, since the BZM used as an electrolyte is both a proton conductor and a hole conductor, in the power generation state, the current caused by the hole (hereinafter referred to as the "hole current") becomes non-negligible relative to the current caused by the proton (hereinafter referred to as the "proton current"). Therefore, when the external current is 0A, the proton current and the hole current become the same value, and the proton current flows, so it essentially becomes a power generation state, which deviates from the theoretical electromotive force. In the power generation state, according to the combination of the electrolyte and the air electrode composed of BZM, the reaction resistance component and the reaction activity in the air electrode change. As an air electrode, the reaction activity of LSCFPd is higher than that of LSCF, so the terminal voltage becomes larger when the external current is 0A, and then even when the external current is more than 0A, the terminal voltage becomes larger. As a result, it is believed that the overall power generation performance of the membrane electrode assembly is improved.
[0030] In the case of using a proton conductive solid electrolyte, the reaction of the following formula (A) is carried out in the air electrode. In the case of using a proton conductive solid electrolyte BZM for an electrolyte membrane and using LSCF for an air electrode, protons hardly propagate in the air electrode, so it is believed that the reaction of the following formula (A) is carried out only at the three-phase interface (i.e., the interface of the electrolyte (BZM), the air electrode (LSCF) and the air). That is, at the three-phase interface of the BZM with protons and the air electrode and the air as a reaction catalyst, the reaction of the following formula (A) is carried out. In contrast, Pd has high hydrogen permeability and hydrogen adsorption capacity, so in the case of using a proton conductive solid electrolyte BZM for an electrolyte membrane and using LSCFPd for an air electrode, the reaction of the following formula (A) is also carried out at the two-phase interface (i.e., the interface of the air electrode (LSCFPd) and the air) with a high possibility. In other words, in the case of using LSCFPd for an air electrode, protons propagate in the air electrode, and protons can exist in the air electrode, so it is possible to carry out the reaction of the following formula (A) in a wide range at the two-phase interface. Therefore, it is considered that when LSCFPd is used for the air electrode, the reaction resistance component can be significantly reduced.
[0031] 2H + +1 / 2O2+2e-→H2O…(A)
[0032] Furthermore, when oxygen-ion-conductive YSZ or GDC is used for the electrolyte membrane, since the electron conductivity at a low temperature of 600°C is low, the current caused by oxygen ions is almost entirely in the power generation state, so the terminal voltage when the external current is 0 A does not change according to the activity of the air electrode.
[0033] In the case of using an oxygen ion conductive solid electrolyte, the reaction of the following formula (B) is carried out in the air electrode. In the case of using an oxygen ion conductive solid electrolyte YSZ or GDC for the electrolyte membrane, whether LSCF or LSCFPd is used as the air electrode, protons do not participate, so the reaction of the following formula (B) is carried out at the two-phase interface (i.e., the interface between the air electrode and the air). Similarly, in the case of using LSCFPd or LSCF as the air electrode, the oxygen ion conductive solid electrolyte carries out the reaction of the following formula (B), and the proton conductive solid electrolyte carries out the reaction of the above formula (A). In other words, it is believed that since protons do not contribute to the reaction, whether LSCF or LSCFPd is used as the air electrode, the reaction of the following formula (B) is carried out by the reaction of oxygen ions at the two-phase interface. Therefore, it is believed that in the case of using an oxygen ion conductive solid electrolyte, in the case of using the highly reactive LSCFPd as the air electrode, the reaction resistance component will not be significantly reduced in the comparison between the proton conductive solid electrolyte BZM and the air electrode LSCFPd.
[0034] 1 / 2O2+2e - →O 2- …(B)
[0035] The above findings have not been completely clarified so far, but new problems have been discovered and new technical features have been developed that exert significant effects. In the present disclosure, the following solutions are specifically provided.
[0036] (Overview of the present disclosure)
[0037] A membrane electrode assembly according to one embodiment of the present disclosure comprises: an electrolyte membrane including a solid electrolyte, and a first electrode bonded to the electrolyte membrane, wherein the solid electrolyte is composed of a composition formula (1): BaZr 1-x M x O 3-γ The compound represented by the composition formula (1) is characterized in that M is at least one element selected from Sc, Er, Ho, Dy, Gd, Y, In, Tm, Yb and Lu, and satisfies 0<x<1 and 0<γ<0.5, and the first electrode comprises lanthanum strontium cobalt iron palladium composite oxide.
[0038] As a result, the reaction resistance between the first electrode, the electrolyte membrane, and the gas phase of the air can be reduced, and as a result, the reaction resistance of the membrane electrode assembly as a whole is reduced, and the voltage between the terminals when the external current is 0 A when used as an electric power device is increased, and the voltage between the terminals when the external current is 0 A or more is also increased. Therefore, it can be used in a state where the external current and the voltage between the terminals are high, and the power generation efficiency can be improved.
[0039] In addition, for example, in the composition formula (1) representing the solid electrolyte, M may be at least one element selected from Y, Tm, Yb, and Lu.
[0040] This makes it easy for the proton conductivity of the solid electrolyte to increase, thereby reducing the resistance of the membrane electrode assembly and improving the power generation efficiency.
[0041] In addition, for example, in the composition formula (1) representing the solid electrolyte, 0.05<x<0.3 may be satisfied.
[0042] Thus, in the composition formula (1), when 0.05 < x is satisfied, the performance of the solid electrolyte is improved, and when x < 0.3 is satisfied, the crystal stability of the solid electrolyte is improved. Therefore, in the composition formula (1), by satisfying 0.05 < x < 0.3, the performance and durability stability of the solid electrolyte can be improved at the same time.
[0043] In addition, for example, in the composition formula (1) representing the solid electrolyte, M may be at least one element selected from Lu and Yb.
[0044] As a result, the proton conductivity of the solid electrolyte is easily increased, and when mixed with a Ni-containing compound and fired, impurities that cause a decrease in durability against carbon dioxide gas are less likely to be generated. Therefore, the performance and reliability of power generation efficiency can be improved at the same time.
[0045] In addition, for example, in the composition formula (1) representing the solid electrolyte, M may be Yb, and x=0.2 may be satisfied.
[0046] This makes it possible to achieve a balance between the performance of the solid electrolyte, durability against carbon dioxide, and crystal stability, thereby improving power generation efficiency, reliability, and durability stability.
[0047] In addition, for example, the lanthanum strontium cobalt iron palladium composite oxide may be: 1- m Sr m Co y Fe z Pd 1-y-z O 3-δ The compound represented by the above composition formula (2) satisfies 0≤m≤0.5, 0.1≤y≤0.9, 0.1≤z≤0.9, y+z<1 and 0≤δ≤0.5.
[0048] Thus, in the composition formula (2), when 0≤m, 0.1≤y and z≤0.9 are satisfied, the performance of the first electrode is improved, and when m≤0.5, y≤0.9 and 0.1≤z are satisfied, the durability of the first electrode is improved. Therefore, in the composition formula (2), by satisfying 0≤m≤0.5, 0.1≤y≤0.9 and 0.1≤z≤0.9, the performance and durability of the first electrode can be taken into account.
[0049] Therefore, the reaction resistance of the membrane electrode assembly as a whole is reduced, and the voltage between the terminals is increased when the external current is 0 A when used as an electric power device. Therefore, it is possible to use the membrane electrode assembly with high external current and high voltage between the terminals, and the power generation efficiency can be improved.
[0050] In addition, for example, in the composition formula (2) representing the lanthanum strontium cobalt iron palladium composite oxide, 0.01≤1-yz≤0.05 may be satisfied.
[0051] Thus, in the composition formula (2), when 0.01≤1-yz is satisfied, the activity of the electrode as the first electrode is improved, and when 1-yz≤0.05 is satisfied, the crystal stability of the first electrode is improved. Therefore, in the composition formula (2), by satisfying 0.01≤1-yz≤0.05, the performance and durability stability of the air electrode can be improved at the same time.
[0052] In addition, for example, in the composition formula (2) representing the lanthanum strontium cobalt iron palladium composite oxide, m=0.4, y=0.38, and z=0.57 are satisfied.
[0053] This further improves the performance and durability of the first electrode. As a result, the resistance of the entire membrane electrode assembly is reduced, and the durability stability is also improved.
[0054] Furthermore, an electrochemical device according to one aspect of the present disclosure includes the membrane electrode assembly described above and a second electrode, wherein the electrolyte membrane is disposed between the first electrode and the second electrode.
[0055] Thus, the electrochemical device having the membrane electrode assembly and the second electrode has a small resistance, and the voltage between the terminals is increased when the external current is 0 A, and further the voltage between the terminals is increased when the external current is greater than 0 A. Therefore, the device can be used in a state where the external current and the voltage between the terminals are high, and the power generation efficiency is improved.
[0056] Furthermore, an electrochemical system according to one aspect of the present disclosure includes the above-mentioned electrochemical device.
[0057] Thus, since the electrochemical system includes the above-described electric power device, an electrochemical system with improved power generation efficiency can be realized.
[0058] In addition, the electrochemical system may further include a temperature control unit. The temperature control unit controls so that the operating temperature of the electrochemical device becomes 600° C. or less.
[0059] Thus, since the electrochemical system includes the membrane electrode assembly, it is possible to realize an electrochemical system with improved power generation efficiency even at an operating temperature of 600° C. or lower.
[0060] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0061] Furthermore, the embodiments described below represent general examples or specific examples. The numerical values, shapes, materials, components, configuration positions and connection methods of components, steps, and the order of steps shown in the following embodiments are only examples and do not limit the present disclosure. In addition, the components in the following embodiments that are not recorded in the independent claims are described as optional components.
[0062] In addition, each figure is a schematic diagram and is not necessarily a strict illustration. Therefore, for example, the scales in each figure are not necessarily the same. In addition, in each figure, the same reference numerals are given to substantially the same structure, and repeated descriptions are omitted or simplified.
[0063] In addition, in this specification, terms such as parallel that indicate the relationship between elements, terms such as rectangular that indicate the shape of elements, and numerical ranges are not strictly defined, but are used to indicate that they include substantially equivalent ranges, such as differences of several %. Furthermore, the "thickness direction" in this specification refers to the direction in which the electrodes and the electrolyte membrane are stacked.
[0064] (Implementation Method 1)
[0065] Figure 1 This is a cross-sectional view schematically showing the structure of the membrane electrode assembly 10 according to the first embodiment. Figure 1 FIG. 2 shows a cross section of the membrane electrode assembly 10 cut along the thickness direction. Figure 1 As shown, the membrane electrode assembly 10 includes an electrolyte membrane 11 including a solid electrolyte and an air electrode 12 joined to the electrolyte membrane 11. That is, the membrane electrode assembly 10 has a structure in which the electrolyte membrane 11 and the air electrode 12 are stacked. In this specification, the air electrode 12 is an example of a first electrode.
[0066] As described above, the electrolyte membrane 11 includes a solid electrolyte having proton conductivity. The solid electrolyte is composed of the composition formula (1): BaZr 1-x M x O 3-γ A compound represented by (BZM). In the composition formula (1), M is at least one element selected from Sc, Er, Ho, Dy, Gd, Y, In, Tm, Yb and Lu, and satisfies 0<x<1. Hereinafter, M is sometimes referred to as a dopant. In addition, in the composition formula (1), the value of γ satisfies 0<γ<0.5. In the composition formula (1), when the value of x becomes larger, the performance of the solid electrolyte is easily improved. In addition, in the composition formula (1), when the value of x becomes smaller, the crystal structure of the solid electrolyte is easily stabilized. From the viewpoint of simultaneously improving the performance and durable stability of the solid electrolyte, the solid electrolyte can satisfy 0.05<x<0.3 in the composition formula (1), and more preferably satisfies x=0.2.
[0067] Figure 2 is a table showing the properties of BZM containing various dopants at x = 0.20. Specifically, Figure 2It records whether the impurity BaM2NiO5 is generated after the BZM containing each dopant and NiO are mixed and fired in order of the ion radius of the dopant from small to large, and the proton conductivity of the BZM containing each dopant at 600°C. Due to the generation of the impurity BaM2NiO5, the durability of BZM to carbon dioxide gas is easily reduced. Furthermore, the "-" in the conductivity result means that there is no measurement data. In composition formula (1), from the point of view of proton conductivity, M (dopant) can be at least one element selected from Y, Tm, Yb and Lu. From the point of view of proton conductivity and the difficulty in generating impurities when mixed and fired with Ni-containing compounds, in composition formula (1), M is preferably at least one element selected from Lu and Yb.
[0068] As the solid electrolyte having the composition formula (1) as described above, for example, BaZr wherein M is Yb and x=0.2 is preferable. 0.8 Yb 0.2 O 3-γ This makes it easy to obtain a membrane electrode assembly 10 having improved power generation efficiency and durability. The value of γ satisfies 0<γ<0.5.
[0069] As described above, BZM has proton conductivity. For example, when the element M is Yb and the molar ratio of Zr to Yb is 8:2, the proton conductivity of BZM at 600°C is about 0.011 S / cm. Furthermore, in order to reduce the ohmic resistance (i.e., IR resistance) of the electrolyte membrane 11, the electrolyte membrane 11 constituting the battery 100 can be made as thin as possible.
[0070] The air electrode 12 is composed of an oxygen ion-electron mixed conductor material containing lanthanum strontium cobalt iron palladium composite oxide (LSCFPd). LSCFPd contains Pd, so in addition to the conductivity of oxygen ions and electrons, it may also provide proton conductivity. The air electrode 12 may be composed of LSCFPd alone, or it may be a structure in which LSCFPd is combined with other oxygen ion-electron mixed conductor materials. In addition, for example, the air electrode 12 may contain an electrolyte material (such as BZM).
[0071] When the air electrode 12 is used as an air electrode of a solid oxide fuel cell, for example, a reaction of electrochemically reducing oxygen in the gas phase occurs. Therefore, in order to ensure a diffusion path for oxygen and promote the reaction, the air electrode 12 may be a porous body. When the air electrode 12 is a porous body, for example, a porous body having a porosity of 20% by volume or more and 50% by volume or less may be used.
[0072] LSCFPd can be composed of formula (2): La 1-m Sr m Co y Fe zPd 1-y-z O 3-δ Indicates a compound that satisfies 0≤m≤0.5, 0.1≤y≤0.9, 0.1≤z≤0.9, y+z<1, and 0≤δ≤0.5 in the composition formula (2). In the composition formula (2), as a basic composition, δ is 0, and when the membrane electrode assembly 10 is used, it may vary in the range of about 0 to 0.5. In the composition formula (2), when the value of 1-yz becomes larger, the activity as an electrode is easily improved, and when the value of 1-yz becomes smaller, the crystal structure of LSCFPd is easily stabilized. From the viewpoint of taking into account both the crystal stability of LSCFPd and the high activity as an electrode, LSCFPd in the composition formula (2) can satisfy 0.01≤1-yz≤0.05, and more preferably satisfies m=0.4, y=0.38 and z=0.57. In addition, LSCFPd in the composition formula (2) may satisfy 1-yz=0.05, 0.19≤y≤0.38, and 0.57≤z≤0.76, or may satisfy 1-yz=0.01, 0.19≤y≤0.40, and 0.57≤z≤0.79.
[0073] The membrane electrode assembly 10 of Embodiment 1 has a structure in which the air electrode 12 is stacked on one side of the electrolyte membrane 11, so that the reaction resistance generated in the membrane electrode assembly 10 can be reduced. Therefore, the power generation efficiency of the electrochemical device using the membrane electrode assembly 10 can be improved.
[0074] (Implementation Method 2)
[0075] Embodiment 2 is described below with reference to the drawings. In the following description of Embodiment 2, differences from Embodiment 1 are mainly described, and the same reference numerals are given to the same or corresponding components in all the drawings, and their description may be omitted.
[0076] The electrochemical device according to the second embodiment includes the membrane electrode assembly according to the first embodiment.
[0077] The electrochemical device according to the second embodiment includes a second electrode. The electrolyte membrane is disposed between the first electrode and the second electrode.
[0078] According to the above structure, an electrochemical device with improved power generation efficiency can be realized.
[0079] Hereinafter, a specific example of a battery will be described as an example of an electrochemical device.
[0080] Figure 3 It is a cross-sectional view schematically showing the structure of a battery 100 according to the second embodiment. Figure 3The cross section taken along the thickness direction of the film-like battery 100 is shown. The battery 100 of the second embodiment includes the membrane electrode assembly 10 of the first embodiment and a fuel electrode 13 .
[0081] like Figure 3 As shown, the electrolyte membrane 11 is disposed between the air electrode 12 and the fuel electrode 13. In this specification, the fuel electrode 13 is an example of a second electrode.
[0082] The membrane electrode assembly 10 is the same as the membrane electrode assembly 10 of Embodiment 1, and therefore its description is omitted.
[0083] The fuel electrode 13 may include a composition of BaZr 1-x M x O 3-γ A proton-conductive compound represented by (M is one or more elements selected from Lu, Tm, Y, Yb and In, and satisfies 0<x<1, 0<γ<0.5) and Ni.
[0084] The fuel electrode 13 may be a cermet of a mixture of Ni and the solid electrolyte BZM of the electrolyte membrane 11 .
[0085] Furthermore, in Figure 3 In the embodiment, although the electrolyte membrane 11 is stacked on the fuel electrode 13 , another layer made of an ion conductive material different from the electrolyte membrane 11 may be formed between the fuel electrode 13 and the electrolyte membrane 11 .
[0086] For example, when the fuel electrode 13 is used as a fuel electrode of a solid oxide fuel cell, a reaction of oxidizing hydrogen in the gas phase into protons occurs at the fuel electrode 13. Therefore, in order to promote the oxidation reaction from hydrogen to protons, the fuel electrode 13 can be formed as a joint of Ni having electron conductivity and hydrogen oxidation activity and a compound having the above-mentioned proton conductivity. In addition, in order to ensure the diffusion path of gaseous hydrogen, the fuel electrode 13 can be a porous body. In the case where the fuel electrode 13 is a porous body, for example, it can be a porous body with a porosity of 20 volume % or more and 50 volume % or less.
[0087] In addition, when the cell 100 including the membrane electrode assembly 10 is used in a solid oxide fuel cell, for example, air is supplied to the surface of the electrolyte membrane 11 on the side where the air electrode 12 is provided, and hydrogen-containing gas is supplied to the other side where the air electrode 12 is not provided, thereby generating electricity. Therefore, when the electrochemical device is a solid oxide fuel cell, the electrolyte membrane 11 must be airtight.
[0088] As described above, the battery 100 of embodiment 2 has a structure in which the air electrode 12, the electrolyte membrane 11 and the fuel electrode 13 are stacked in this order, so as in embodiment 1, the reaction resistance of the membrane electrode assembly 10 composed of the air electrode 12 and the electrolyte membrane 11 can be reduced, thereby improving the power generation efficiency.
[0089] In addition, the electrochemical device of embodiment 2 can be used for electrochemical devices such as gas sensors, hydrogen pumps, or water electrolysis devices in addition to batteries. Therefore, since the membrane electrode assembly of embodiment 1 is provided, an electric power device can be realized in which the reaction resistance of the membrane electrode assembly is reduced, and the sensor sensitivity, pump capacity, or electrolysis capacity is improved.
[0090] When the battery 100 of embodiment 2 is used in a fuel cell, it is used, for example, as the following electrochemical system. First, a raw material such as hydrocarbon gas supplied from the outside through a raw material supply path is supplied to a reformer. The reformer reforms the supplied raw material to generate a hydrogen-containing gas. The hydrogen-containing gas generated by the reformer is supplied to the fuel electrode 13 of the battery 100 through a gas supply path. In addition, an oxidant gas supplied from the outside is supplied to the air electrode 12 through another gas supply path. Thus, the battery 100 generates electricity through an electrochemical reaction between hydrogen in the supplied hydrogen-containing gas and oxygen in the oxidant gas. Such an electrochemical system of a fuel cell can achieve high power generation efficiency because it is equipped with the battery 100 of embodiment 2.
[0091] In addition, the electrochemical system using the electrochemical device of embodiment 2 may further include a temperature control unit. The temperature control unit controls so that the operating temperature of the electrochemical device is controlled to be below 600°C. Such an electrochemical system includes the membrane electrode assembly of embodiment 1, so that high power generation efficiency can be achieved even below 600°C. In addition, by operating the electrochemical device at a lower temperature, the insulation material can be reduced. As a result, the miniaturization and cost reduction of the electrochemical device can be achieved.
[0092] (Example)
[0093] Hereinafter, the membrane electrode assembly and the electric power device of the present disclosure will be specifically described in Examples, but the present disclosure is not limited to the following Examples.
[0094] [Manufacture of Evaluation Membrane Electrode Assembly]
[0095] Hereinafter, the method for producing the membrane electrode assembly for evaluation in Example 1 and Comparative Examples 1 to 3 will be described. The membrane electrode assembly for evaluation comprises Figure 3 The battery 100 shown has the same structure.
[0096] For the stack of electrolyte membrane and fuel electrode, the slurry of air electrode material used in Example 1 and Comparative Examples 1 to 3 was prepared respectively. Then, the slurry of air electrode material was applied to the surface of the electrolyte membrane of the stack opposite to the fuel electrode by screen printing. The coating area of air electrode material was 0.79 cm 2 (φ10mm). The laminate coated with the air electrode material is fired in an atmosphere at 950°C for 2 hours, thereby sintering and attaching the air electrode to the electrolyte membrane. In this way, a membrane electrode assembly for evaluation is obtained. The thicknesses of the electrolyte membrane, air electrode and fuel electrode of the obtained membrane electrode assembly for evaluation are 13μm, 10μm and 0.6mm, respectively. In the fuel electrode, NiO is reduced to Ni at 700°C for more than 4 hours before power generation. By such treatment, during power generation after reduction, the mixture of NiO and BZM in the fuel electrode during production becomes a metal ceramic of Ni and BZM with a predetermined porosity (i.e., more than 20 volume % and less than 50 volume %).
[0097] Figure 4 This is a table showing the materials used in the membrane electrode assemblies for evaluation in Examples and Comparative Examples 1 to 3, and the measurement results of the ohmic resistance and reaction resistance at 600°C. Figure 5 Table showing the materials used for the membrane electrode assembly for evaluation in Examples and Comparative Examples 1 to 3, and the results of the measurement of the terminal voltage, ohmic resistance, and reaction resistance when the external current is 0A at each temperature. The terminal voltage, ohmic resistance, and reaction resistance when the external current is 0A are values that serve as indicators of power generation performance. The higher the voltage is maintained during use, the higher the power generation efficiency of the battery. Therefore, the terminal voltage when the external current is 0A is an indicator of improving power generation efficiency by increasing. In addition, when the current during use becomes larger, the larger the resistance value, the easier it is to reduce the terminal voltage. Therefore, the ohmic resistance and reaction resistance are indicators of improving power generation efficiency by reducing.
[0098] Regarding the oxygen ion-electron mixed conductor material constituting the air electrode, for the LSCFPd used in Example 1 and Comparative Example 2, Figure 4 As shown, using La 0.6 Sr 0.4 Co 0.38 Fe 0.57 Pd 0.05 O 3-δ (0≤δ≤0.5) as a representative composition. For the LSCF used in Comparative Examples 1 and 3, Figure 4 As shown, using La 0.6 Sr 0.4 Co 0.4 Fe 0.6 O 3-δ As a representative composition.
[0099] In addition, regarding the solid electrolyte constituting the electrolyte membrane, for BZYb used in Example 1 and Comparative Example 1, Figure 4 As shown, using BaZr 0.8 Yb 0.2 O 2.90 As a representative composition. For Comparative Example 2 and YSZ used in Comparative Example 2, as Figure 4 As shown, using [ZrO2] 0.92 [Y2O3] 0.08 As a representative composition.
[0100] In addition, for the fuel electrodes used in Example 1 and Comparative Examples 1 to 3, cermets of nickel and a solid electrolyte constituting a solid electrolyte membrane were used.
[0101] [Materials for Electrolyte Membrane and Air Electrode, and Production of Laminated Body]
[0102] The materials constituting the electrolyte membrane and the air electrode, namely LSCFPd (LSCF6446 containing Pd), LSCF (LSCF6446), BZYb and YSZ, and the method for producing a laminate of the fuel electrode and the electrolyte membrane are described.
[0103] First, a method for producing green sheets of BZYb as an electrolyte membrane and a fuel electrode will be described.
[0104] BZYb, a proton conductor material, is prepared by the citric acid complex method by adding powders of Yb(NO3)3·xH2O (manufactured by Kojun Chemical) as starting materials to powders of Ba(NO3)2 (manufactured by Kanto Chemical) and ZrO(NO3)2·2H2O (manufactured by Kanto Chemical). Specifically, first, each powder weighed in a predetermined ratio is dissolved in distilled water, and the resulting aqueous solution is stirred. Then, 1.5 equivalents of citric acid monohydrate (manufactured by Kanto Chemical) and 1.5 equivalents of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical) are added to the aqueous solution relative to the metal cations contained in the aqueous solution. Then, the aqueous solution is stirred at 90°C. Next, the pH value of the aqueous solution is adjusted to 7 using ammonia water (28%) (manufactured by Kanto Chemical). After the pH is adjusted, the solution is heated to 95°C to 240°C using a hot stirrer to remove the solvent. In this way, a solid component is obtained. The obtained solid component is crushed in a mortar and defatted at about 400°C. After degreasing, the obtained powder was pressed into a cylindrical shape and pre-fired in an atmosphere at 900°C for 10 hours. After pre-fired, the coarsely crushed powder was placed in a plastic container together with zirconium oxide balls, and ethanol was added and crushed in a ball mill for more than 4 days. After crushing in a ball mill, the solvent was removed by lamp drying. Thus, BaZr 0.8 Yb0.2 O3(BZYb) electrolyte material powder. 0.8 Yb 0.2 O3(BZYb) electrolyte material powder, polyvinyl butyral as a resin, butyl benzyl ester as a plasticizer, butyl acetate and 1-butanol as solvents were mixed and then green sheets were obtained by tape casting. Figure 3 The method for manufacturing the fuel electrode 13 is described below. 0.8 Yb 0.2 O3 (BZYb) electrolyte material powder and NiO powder (manufactured by Sumitomo Metal Mining) were weighed in a weight ratio of NiO:BZYb=80:20 (i.e., the volume ratio of Ni and BZYb was 69:31). In order to make a green sheet, the electrolyte material powder, NiO powder, polyvinyl butyral as a resin, butyl benzyl phthalate as a plasticizer, butyl acetate and 1-butanol as a solvent were mixed, and the green sheet of the fuel electrode was obtained by a tape casting method.
[0105] Next, the method for manufacturing the stack of fuel electrodes and electrolyte membranes in Example 1 and Comparative Example 1 using BZYb is described. After the obtained fuel electrode green sheet is fired, the green sheet is cut into a predetermined size assuming a linear shrinkage of 22% so that it becomes a square with one side of 20 mm (4-C3: 3 mm chamfered corners). Next, a plurality of cut green sheets are stacked. The obtained electrolyte membrane is overlapped on the green sheet for stacking. Then, the green sheet overlapped with the electrolyte membrane is hot pressed under the condition of 50 MPa. In this way, a stack is obtained. The obtained stack is fired in an atmosphere of 1475°C for 2 hours. As a stack of fuel electrodes and electrolyte membranes, a half unit of a square with one side of 20 mm (4-C3: 3 mm chamfered corners) is produced. BZYb was confirmed as a single phase by X-ray diffraction (hereinafter sometimes referred to as XRD). Furthermore, by using inductively coupled plasma (hereinafter sometimes referred to as ICP) emission spectroscopy and fluorescent X-ray analysis (hereinafter sometimes referred to as XRF), it was confirmed that the difference between the composition ratio of BZYb (i.e., the composition ratio based on the charging ratio) and the target composition ratio (i.e., the composition ratio based on the actual measurement) was less than 1%.
[0106] Next, the stack of fuel electrodes and electrolyte membranes in Comparative Examples 2 and 3 using YSZ is described. In the stack of fuel electrodes and electrolyte membranes using YSZ, a φ20mm AEB-2.0 fuel electrode supporting electrolyte half unit manufactured by Nexceris is used. In the fuel electrode supporting electrolyte half unit used, the fuel electrode is composed of a mixture of NiO and YSZ, and the thickness of the electrolyte membrane YSZ is 7 to 10 μm. In addition, in the fuel electrode supporting electrolyte half unit used, a 3 to 5 μm GDC layer is present on the side where the air electrode of the electrolyte membrane is set as a reaction prevention layer.
[0107] Next, a method for producing the air electrode material will be described.
[0108] The material of the air electrode used in Example 1 and Comparative Example 2, namely, LSCF6446 containing Pd (LSCFPd: La 0.6 Sr 0.4 Co 0.38 Fe 0.57 Pd 0.05 O 3-δ ) is described. First, La2O3, SrO, Co3O4 and Fe2O3 (all manufactured by Kanto Chemical) and citric acid are added to pure water to react, and then mixed with a dinitrosodiamminepalladium nitrate solution. In this way, a reaction solution is obtained. The obtained reaction solution is dried at 130°C.
[0109] The citric acid contained in the dried reaction solution was heated in an electric furnace to decompose it. Then, it was formally calcined at 1200°C in an air atmosphere. In this way, LSCFPd powder was obtained. The obtained LSCFPd was confirmed to be a single phase by XRD. By using ICP and XRF, it was confirmed that the difference between the composition ratio of LSCFPd and the target composition ratio was less than 1%.
[0110] Furthermore, the LSCFPd powder and the vehicle formed by mixing alcohol and ether were mixed at a predetermined weight ratio. Thus, a mixture was obtained. The obtained mixture was mixed with a rotation / revolution stirrer. Thus, the paste of the air electrode material used in Example 1 and Comparative Example 2 was prepared.
[0111] Next, the material of the air electrode used in Comparative Examples 1 and 3, LSCF6446 (LSCF: La 0.6 Sr 0.4 Co 0.4 Fe 0.6 O 3-δ ) is described below.
[0112] First, La2O3, SrO, Co3O4 and Fe2O3 (all manufactured by Kanto Chemical) and citric acid were added to pure water to react, and the reaction solution was dried at 130°C. The citric acid contained in the dried reaction solution was decomposed by heating it in an electric furnace, and then formal sintering was carried out in an air atmosphere at 1200°C. The obtained LSCF was confirmed to be a single phase by XRD. Using ICP and XRF, it was confirmed that the deviation of the composition ratio of LSCF from the target composition ratio was less than 1%. In addition, LSCF powder and a color carrier prepared by mixing alcohol and ether in a predetermined weight ratio were mixed. A mixture was thus obtained. The obtained mixture was mixed using a rotation / revolution mixer. In this way, a paste of air electrode materials used in Comparative Examples 1 and 3 was prepared.
[0113] [Measurement of resistance and inter-terminal voltage of membrane electrode assembly for evaluation]
[0114] The resistance of the membrane electrode assembly for evaluation was measured by the AC impedance method. The AC impedance measurement was performed using a 1287 type manufactured by Solartron. When the external current was 0A, an AC voltage was applied at an amplitude of 10 mV and the frequency was changed from 100 kHz to 0.01 Hz. Figure 4 and Figure 5 Carried out under the indicated temperature conditions. Figure 6 An example of the results of AC impedance measurement expressed as a Cole-Cole curve. Figure 6 The details of the resistance component in the AC impedance measurement are schematically shown in FIG. Figure 6 As shown in FIG. 1 , the results of AC impedance measurement can be illustrated by a Colcord curve that is shown with the real component Z' of impedance Z (=Z'+jZ') as the horizontal axis and the imaginary component Z" as the vertical axis. In the Colcord curve, for an arc drawn in the frequency range of about 10kHz to 0.01Hz, the intersection of the arc and the high-frequency side of the real axis (Z') becomes the ohmic resistance, and the length of the chord formed by the arc and the real axis, that is, the length of the two intersections of the arc cutting the real axis becomes the reaction resistance. The results of the ohmic resistance and reaction resistance obtained by the measurement are shown in FIG. Figure 4 and Figure 5 shown.
[0115] The humidified air is brought into contact with the air electrode, and the humidified hydrogen is brought into contact with the fuel electrode. Figure 5 The voltage between the terminals of the air electrode and the fuel electrode in the evaluation membrane electrode assembly was measured while changing the external current value under the temperature conditions shown. The results of the voltage between the terminals when the external current was 0A are shown in Figure 5 In addition, the measurement results of the current-voltage performance of the membrane electrode assembly for evaluation in Example 1 and Comparative Example 1 are as follows: Fig. 7A and Figure 7B shown. Fig. 7AThe current-voltage performance of the membrane electrode assemblies for evaluation in Example 1 and Comparative Example 1 at 600° C. is shown. Figure 7B The current-voltage performance of the membrane electrode assembly for evaluation in Example 1 and Comparative Example 1 at 500° C. is shown.
[0116] like Figure 5 As shown, in the evaluation membrane electrode assembly of Example 1 having an air electrode using LSCFPd, the terminal voltage at 600°C when the external current was 0A was 0.96V. In the evaluation membrane electrode assembly of Comparative Example 1 having the same electrolyte membrane as Example 1 and having an LSCF air electrode, the terminal voltage at 600°C when the external current was 0A was 0.92V. The evaluation membrane electrode assembly of Example 1 had a higher terminal voltage when the external current was 0A than that of Comparative Example 1, and the result was good. In addition, in the evaluation membrane electrode assemblies of Example 1 and Comparative Example 1, the ohmic resistance at 600°C was 0.36Ωcm, respectively. 2 and 0.37Ωcm 2 , which is a value of the same degree. On the other hand, at 600°C, the reaction resistance of Example 1 is 0.79Ωcm 2 , while the reaction resistance of Comparative Example 1 is 1.2Ωcm 2 . The evaluation membrane electrode assembly of Example 1 has significantly lower reaction resistance than that of Comparative Example 1, and the result is good. In addition, even at a low temperature of 500°C, the same tendency is observed, and the evaluation membrane electrode assembly of Example 1 has higher terminal voltage and lower reaction resistance than that of Comparative Example 1. Therefore, the evaluation membrane electrode assembly of Example 1 is more suitable as a membrane electrode assembly using a proton conductor than the evaluation membrane electrode assembly of Comparative Example 1. The reason for the difference in terminal voltage and reaction resistance in the membrane electrode assemblies using the proton conductors of Example 1 and Comparative Example 1 is believed to be due to the occurrence of the reaction of the above-mentioned formula (A). The details are as described above.
[0117] like Fig. 7A and Figure 7B As shown in the current-voltage performance graph in which the horizontal axis is the current density and the vertical axis is the terminal voltage, the line of the evaluation membrane electrode assembly of Example 1 is shifted to the upper side of the graph compared with the line of Comparative Example 1 in both the cases of 500°C and 600°C. That is, the evaluation membrane electrode assembly of Example 1 has a higher voltage than Comparative Example 1 under any current density conditions, and has good performance.
[0118] In addition, if Figure 5As shown, the terminal voltages of the evaluation membrane electrode assembly of Example 1 and the evaluation membrane electrode assembly of Comparative Examples 2 and 3, which use oxygen ion conductor YSZ as the electrolyte membrane, at 600°C when the external current is 0A are 0.96V, 1.13V, and 1.13V, respectively. The terminal voltage of the evaluation membrane electrode assembly of Example 1 is lower than that of Comparative Examples 2 and 3 when the external current is 0A. However, the ohmic resistance of the evaluation membrane electrode assembly of Example 1, Comparative Examples 2, and Comparative Examples 3 is 0.36Ωcm, respectively. 2 , 2.0Ωcm 2 and 2.0Ωcm 2 The reaction resistances of the evaluation membrane electrode assemblies of Example 1, Comparative Example 2, and Comparative Example 3 were 0.79 Ωcm and 0.79 Ωcm, respectively. 2 , 4.0Ωcm 2 and 5.0Ωcm 2 . The evaluation membrane electrode assembly of Example 1 has significantly lower ohmic resistance and reaction resistance than those of Comparative Examples 2 and 3. Therefore, although the terminal voltage of the evaluation membrane electrode assembly of Example 1 is low when the external current is 0A, the ohmic resistance and reaction resistance are significantly lower than those of Comparative Examples 2 and 3. As a result, the terminal voltage of the evaluation membrane electrode assembly of Example 1 is difficult to decrease even if the current increases compared with Comparative Examples 2 and 3. Therefore, when the terminal voltage is about 0.8V suitable for actual use, the evaluation membrane electrode assembly of Example 1 can take out a larger current than that of Comparative Examples 2 and 3, and has good performance. That is, by using the air electrode and electrolyte membrane of Example 1, a membrane electrode assembly with improved power generation performance at low temperatures below 600°C can be obtained compared with a membrane electrode assembly using an oxygen ion conductive electrolyte membrane.
[0119] In addition, as shown in the comparison between Example 1 and Comparative Example 1, when BZYb was used for the electrolyte membrane and the air electrode was changed from LSCF to the highly active LSCFPd, the reaction resistance was reduced by 34%. On the other hand, as shown in the comparison between Comparative Examples 2 and 3, when YSZ was used for the electrolyte membrane and the air electrode was changed from LSCF to LSCFPd, the reaction resistance was reduced by only 20%. This is considered to be because when the proton conductor BZYb is used, the reaction of the above formula (A) occurs, and when the oxygen ion conductor YSZ is used, the reaction of the above formula (B) occurs, and the details are as described above.
[0120] The membrane electrode assembly 10 disclosed in the present invention can be used in applications such as fuel cells, gas sensors, hydrogen pumps, and electrochemical devices such as water electrolysis devices.
[0121] It is clear from the above description that the present disclosure includes many improvements and other embodiments for those skilled in the art. Therefore, the above description should be interpreted as an example only and is provided for the purpose of teaching those skilled in the art the best way to implement the present disclosure. The details of its structure and / or function can be substantially changed without departing from the spirit of the present disclosure.
[0122] Industrial Applicability
[0123] The membrane electrode assembly disclosed herein can be used in electrochemical devices such as fuel cells, gas sensors, hydrogen pumps, and water electrolysis devices.
[0124] Description of Reference Numerals
[0125] 10Membrane electrode assembly
[0126] 11Electrolyte membrane
[0127] 12 Air electrode
[0128] 13 Fuel electrode
[0129] 100 battery
Claims
1. A membrane electrode assembly comprising: An electrolyte membrane including a solid electrolyte, and a first electrode joined to the electrolyte membrane, The solid electrolyte is a compound represented by composition formula (1), Composition formula (1): BaZr 1-x M x O 3-γ In the composition formula (1), M is at least one element selected from Sc, Er, Ho, Dy, Gd, Y, In, Tm, Yb and Lu, and satisfies 0<x<1 and 0<γ<0.5, The first electrode comprises a lanthanum strontium cobalt iron palladium composite oxide. The lanthanum strontium cobalt iron palladium composite oxide is a compound represented by composition formula (2), Composition formula (2): La 1-m Sr m Co y Fe z Pd 1-y-z O 3-δ In the composition formula (2), 0≤m≤0.5, 0.1≤y≤0.9, 0.1≤z≤0.9, y+z<1 and 0≤δ≤0.5 are satisfied, and 0.01≤1-yz≤0.05 is satisfied.
2. The membrane electrode assembly according to claim 1, In the composition formula (1) representing the solid electrolyte, M is at least one element selected from the group consisting of Y, Tm, Yb and Lu.
3. The membrane electrode assembly according to claim 1 or 2, In the composition formula (1) representing the solid electrolyte, 0.05<x<0.3 is satisfied.
4. The membrane electrode assembly according to claim 2, In the composition formula (1) representing the solid electrolyte, M is at least one element selected from Lu and Yb.
5. The membrane electrode assembly according to claim 3, In the composition formula (1) representing the solid electrolyte, M is at least one element selected from Lu and Yb.
6. The membrane electrode assembly according to claim 4 or 5, In the composition formula (1) representing the solid electrolyte, M is Yb, and x=0.2 is satisfied.
7. The membrane electrode assembly according to claim 1, In the composition formula (2) representing the lanthanum strontium cobalt iron palladium composite oxide, m=0.4, y=0.38 and z=0.57 are satisfied.
8. An electrochemical device comprising: The membrane electrode assembly according to any one of claims 1 to 7, and The second electrode, The electrolyte membrane is disposed between the first electrode and the second electrode. 9 . An electrochemical system comprising the electrochemical device according to claim 8 .
10. The electrochemical system according to claim 9, It also has a temperature control unit. The temperature control unit performs control so that the operating temperature of the electrochemical device becomes 600° C. or less.