Anti-agglomeration agent for polyisobutylene production
By using LCST compounds to mix with an aqueous medium during the preparation of polyisobutylene, the suspension state of polyisobutylene particles in the aqueous medium is controlled, thus solving the problem of easy agglomeration of polyisobutylene particles and improving product quality and application performance.
Patent Information
- Application Number
- CN202110749813.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2015-06-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2035-06-29
AI Technical Summary
In the existing technology for preparing polyisobutylene, polyisobutylene particles are prone to agglomeration in aqueous media, leading to clogging and scaling problems during production. The use of traditional anti-agglomeration agents results in excessively high turbidity and ash content in the product, affecting its application performance.
The LCST compound is contacted with an organic medium and then mixed with an aqueous medium. By partially removing the organic diluent, an aqueous slurry containing polyisobutylene particles is formed. The reversible precipitation effect of the LCST compound at a specific temperature reduces the tendency of particle agglomeration. Combined with appropriate surfactants and metal salts, the suspension state of the particles is controlled.
It effectively reduces the agglomeration tendency of polyisobutylene particles in aqueous media, avoids clogging and scaling during the production process, improves the turbidity and optical appearance of the product, reduces ash content, and meets the requirements of applications such as sealants and adhesives.
Smart Images

Figure SMS_12
Abstract
Description
[0001] This application is a divisional application of the invention patent application No. 201580046084.5 entitled “New Anti-Agglomeration Agent for Polyisobutylene Production”. The original application corresponds to international application PCT / CA2015 / 050609, with the application date of June 29, 2015 and the priority date of June 30, 2014. Technical Field
[0002] The present invention relates to a method for reducing or preventing agglomeration of polyisobutylene particles in an aqueous medium by means of LCST compounds, and to a highly pure isobutylene such as polyisobutylene obtained thereby. The present invention also relates to a polyisobutylene product comprising or obtained from the highly pure isobutylene. Background Art
[0003] Rubbers, in particular rubbers comprising repeating units derived from isoolefins, are prepared industrially by carbocationic polymerization. Of particular importance is polyisobutylene.
[0004] The carbocationic polymerization of isoolefins is mechanistically complex. The initiator system usually consists of two components: an initiator and a Lewis acid co-initiator such as aluminum trichloride which is often used in large-scale industrial processes.
[0005] Examples of initiators include proton sources such as hydrogen halides, alcohols, phenols, carboxylic acids and sulfonic acids, and water.
[0006] During the initiation step, the isoolefin reacts with the Lewis acid and the initiator to generate a carbocation which further reacts with monomers to form new carbocations in the so-called propagation step.
[0007] The type of monomer, the type of diluent or solvent and its polarity, the polymerization temperature, and the specific combination of Lewis acid and initiator influence the chemistry of propagation and therefore the incorporation of monomer into the growing polymer chain.
[0008] It has been generally accepted in the industry that slurry polymerization is widely used in methyl chloride as a diluent to produce butyl rubber, polyisobutylene, etc. Typically, the polymerization process is carried out at low temperatures, generally below -90°C. Methyl chloride is used for a variety of reasons, including that it dissolves monomers and aluminum chloride catalysts but does not dissolve polymer products. Methyl chloride also has a suitable freezing point and boiling point to allow low temperature polymerization and effective separation of polymer and unreacted monomer, respectively. The slurry polymerization process in methyl chloride provides many additional advantages, namely, a polymer concentration of up to 40% by weight can be obtained in the reaction mixture compared to the polymer concentration of up to 20% by weight in solution polymerization. An acceptable relatively low viscosity polymer mass is obtained, which enables more effective removal of polymerization heat by surface heat exchange. The slurry polymerization process in methyl chloride is used to produce high molecular weight polyisobutylene and isobutylene-isoprene butyl rubber polymers.
[0009] In polyisobutylene slurry polymerization, the reaction mixture generally comprises polyisobutylene, diluent, residual monomers and initiator residues. This mixture is transferred in batches or in a continuous manner more commonly used in the industry to a vessel containing water containing
[0010] an anti-agglomeration agent, which may be, for example, a fatty acid salt of a polyvalent metal ion, particularly calcium stearate or zinc stearate, in order to form and preserve polyisobutylene rubber particles, more often referred to as "polyisobutylene rubber crumbs"
[0011] and optionally but preferably, a terminator, which is typically aqueous sodium hydroxide to neutralize initiator residues.
[0012] The water in the vessel is typically heated with steam to remove and recover the diluent and unreacted monomer.
[0013] Thus, a slurry of polyisobutylene particles is obtained, which is then dehydrated to separate the polyisobutylene particles. The polyisobutylene rubber particles are then dried, baled and packaged for transportation.
[0014] The antiagglomerating agent ensures that, during the above-mentioned process steps, the polyisobutylene rubber particles remain suspended and exhibit a reduced tendency to agglomerate.
[0015] In the absence of an anti-agglomerant, the naturally high adhesiveness of polyisobutylene will result in the rapid formation of a non-dispersed mass of rubber in the process water, plugging the process. In addition to forming particles, sufficient anti-agglomerant must be added to retard the natural tendency of the formed polyisobutylene rubber particles to agglomerate during the stripping process - which leads to fouling and plugging of the process.
[0016] Anti-agglomeration agents, particularly calcium stearate and zinc stearate, are used as physical-mechanical barriers to limit intimate contact and adhesion of the polyisobutylene particles.
[0017] The physical properties required of these anti-agglomerates are: very low solubility in water, typically less than 20 mg / liter under standard conditions; sufficient mechanical stability to maintain an effective barrier; and the ability to be subsequently processed and mixed with the polyisobutylene to allow finishing and drying.
[0018] A fundamental disadvantage of fatty acid salts of monovalent or multivalent metal ions (particularly sodium, potassium, calcium or zinc stearates or palmitates) is the high loadings required to achieve a sufficient anti-agglomeration effect. This is a result of the need to form a continuous surface coating that provides a physical mechanical barrier. At these high levels of anti-agglomerant loading, problems with turbidity, optical appearance and high ash content of the resulting polymers become problematic in subsequent applications such as sealants and adhesives.
[0019] Many other polyisobutenes obtained after polymerization or after postpolymerization modification in organic solutions or slurries are usually subjected to aqueous work-up, where the same problems also apply.
[0020] Therefore, there is still a need to provide a process for preparing polyisobutene in an aqueous medium which has a reduced or low tendency to agglomerate. Summary of the invention
[0021] According to one aspect of the present invention, there is provided a method for preparing an aqueous slurry comprising a plurality of polyisobutylene particles suspended therein, the method comprising at least the following steps:
[0022] A) bringing the organic medium into contact with the aqueous medium,
[0023] The organic medium comprises
[0024] i) polyisobutylene, and
[0025] ii) organic diluent,
[0026] The aqueous medium comprises at least one LCST compound having a cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 70°C, and
[0027] The organic diluent is at least partially removed to obtain an aqueous slurry containing polyisobutylene particles.
[0028] In another aspect of the present invention, there is provided a method for preparing an aqueous slurry comprising a plurality of polyisobutylene particles suspended therein, the method comprising at least the following steps:
[0029] A) bringing the organic medium into contact with the aqueous medium,
[0030] The organic medium comprises
[0031] i) polyisobutylene, and
[0032] ii) organic diluent,
[0033] The aqueous medium comprises at least one compound selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, hydroxyalkyl alkyl cellulose and carboxyalkyl cellulose, preferably alkyl cellulose, hydroxyalkyl cellulose and hydroxyalkyl alkyl cellulose, and
[0034] The organic diluent is at least partially removed to obtain an aqueous slurry containing polyisobutylene particles. DETAILED DESCRIPTION
[0035] The invention also includes all combinations of the preferred embodiments, range parameters as disclosed below, with each other or with the broadest range or parameter disclosed.
[0036] In one embodiment, the organic medium comprising polyisobutylene and the organic diluent is obtained from a polymerization reaction.
[0037] In the case where the organic medium comprising polyisobutylene and organic diluent is obtained from a polymerization reaction, said medium may also comprise residual isobutylene of the polymerization reaction.
[0038] The aqueous medium may further comprise a non-LCST compound, wherein the non-LCST compound:
[0039] selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, or in another embodiment
[0040] · a salt of a monovalent or polyvalent metal ion, or in another embodiment
[0041] stearate or palmitate of a monovalent or polyvalent metal ion, or in another embodiment
[0042] · Stearates or palmitates of sodium, potassium, calcium and zinc.
[0043] Thus, in one embodiment, the aqueous medium comprises 20,000 ppm or less, preferably 10,000 ppm or less, more preferably 8,000 ppm or less, even more preferably 5,000 ppm or less and still even more preferably 2,000 ppm or less of non-LCST compounds, and in another yet even more preferred embodiment, 1,000 ppm or less of non-LCST compounds, wherein the non-LCST compounds are selected from the above four groups and are preferably calculated relative to the amount of polyisobutylene present in the organic medium.
[0044] In another embodiment, the aqueous medium contains 500 ppm or less, preferably 100 ppm or less, more preferably 50 ppm or less, even more preferably 30 ppm or less and still even more preferably 10 ppm or less of non-LCST compounds, and in another still even more preferred embodiment, 1,000 ppm or less of non-LCST compounds, wherein the non-LCST compounds are selected from the above four groups and are preferably calculated relative to the amount of polyisobutylene present in the organic medium.
[0045] In another embodiment, the aqueous medium is substantially free of non-LCST compounds.
[0046] If not expressly stated otherwise, ppm means parts per million by weight.
[0047] In one embodiment, the aqueous medium comprises 0 to 5,000 ppm, preferably 0 to 2,000 ppm, more preferably 10 to 1,000 ppm, even more preferably 50 to 800 ppm and still even more preferably 100 to 600 ppm of a salt of a monovalent or polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0048] In another embodiment, the aqueous medium comprises 0 to 5,000 ppm, preferably 0 to 2,000 ppm, more preferably 10 to 1,000 ppm, even more preferably 50 to 800 ppm and still even more preferably 100 to 600 ppm of a salt of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0049] In another embodiment, the weight ratio of stearate, palmitate and oleate of monovalent and polyvalent metal ions (if present) to the LCST compound in aqueous medium is 1:2 to 1:100, preferably 1:2 to 1:10 and more preferably 1:5 to 1:10.
[0050] In one embodiment, the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of the salt of the metal ion, and in another yet even more preferred embodiment, 100 ppm or less of the salt of the metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0051] In yet another embodiment, the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of the salt of the polyvalent metal ion, and in another still even more preferred embodiment, 100 ppm or less of the salt of the polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0052] In one embodiment, the aqueous medium comprises 8,000 ppm or less, preferably 5,000 ppm or less, more preferably 2,000 ppm or less, yet even more preferably 1,000 ppm or less of nonionic surfactants, and in another embodiment preferably 500 ppm or less, more preferably 100 ppm or less and even more preferably 15 ppm or less and yet even more preferably no or 1 ppm to 10 ppm of nonionic surfactants, said nonionic surfactants being non-LCST compounds selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
[0053] As used herein, LCST compounds are compounds which are soluble in a liquid medium at relatively low temperatures but precipitate out of the liquid medium above a certain temperature, the so-called lower critical solution temperature or LCST temperature. This process is reversible, so that the system becomes homogeneous again on cooling. The temperature at which the solution becomes clear on cooling is called the cloud point (see German standard specification DIN EN 1890, September 2006). This temperature is specific to a specific substance and a specific process.
[0054] Depending on the nature of the LCST compound, which generally comprises a hydrophilic group and a hydrophobic group, the determination of the cloud point may require different conditions as described in DIN EN 1890 of September 2006. Although this DIN was originally developed for nonionic surfactants obtained by condensation of ethylene oxide, the method also allows the determination of the cloud point of various LCST compounds. However, it was found that suitable conditions facilitated easier determination of the cloud point of structurally different compounds.
[0055] Therefore, the term LCST compound as used herein includes all compounds, wherein its cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 80°C can be determined by at least one of the following methods:
[0056] 1) DIN EN 1890, Method A, September 2006
[0057] 2) DIN EN 1890, Method C, September 2006
[0058] 3) DIN EN 1890, Method E, September 2006
[0059] 4) DIN EN 1890, September 2006, method A, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water
[0060] 5) DIN EN 1890, September 2006, method A, wherein the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.2 g / 100 ml distilled water.
[0061] In another embodiment, the cloud point indicated above may be determined by at least one of methods 1), 2), or 4).
[0062] In a preferred embodiment, the LCST compound is a LCST compound whose turbidity point can be determined by at least one of methods 1), 3) or 4). Method 4) is most preferred.
[0063] Thus, non-LCST compounds are those compounds that have no cloud point or a cloud point outside the range as defined above. It is obvious to the person skilled in the art and known from various commercial products that the above different methods may lead to slightly different cloud points. However, the measurements of each method are consistent and reproducible within the inherent range of its error, and as long as the cloud point is found to be within the range described above using at least one of the above methods, the general principle of the present invention is not affected by different LCST temperatures determined for the same compound.
[0064] For the sake of clarity, it should be mentioned that metal ions, in particular polyvalent metal ions such as aluminium originating from the initiator system used in step b), are not included in the calculation of the metal ions present in the aqueous medium used in step A).
[0065] In another embodiment, the aqueous medium comprises 70 ppm or less, preferably 50 ppm or less, more preferably 30 ppm or less and even more preferably 20 ppm or less and still even more preferably 10 ppm or less of the salt of the polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0066] In yet another embodiment, the aqueous medium comprises 25 ppm or less, preferably 10 ppm or less, more preferably 8 ppm or less and even more preferably 7 ppm or less and still even more preferably 5 ppm or less of the salt of the polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0067] In another embodiment, the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of carboxylic acid salts of polyvalent metal ions, and in another still even more preferred embodiment, 100 ppm or less of carboxylic acid salts of polyvalent metal ions, calculated as metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is chosen from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms. In one embodiment, such carboxylic acids are chosen from monocarboxylic acids. In another embodiment, such carboxylic acids are chosen from saturated monocarboxylic acids such as stearic acid.
[0068] The following example shows how the calculation is performed.
[0069] Calcium stearate (C 36 H 70 The molecular weight of calcium metal is 607.04 g / mol. The atomic weight of calcium metal is 40.08 g / mol. In order to provide, for example, 1 kg of an aqueous medium containing 550 ppm of a salt of a polyvalent metal ion (calcium stearate) (calculated based on its metal content (calcium) and relative to the amount of polyisobutylene present in the organic medium), which is sufficient to form a slurry from an organic medium containing 10 g of polyisobutylene, the aqueous medium must contain (607.04 / 40.08)×(10 g of 550 ppm)=83 mg of calcium stearate or 0.83% by weight of calcium stearate relative to polyisobutylene or 83 ppm of calcium stearate relative to the aqueous medium. In this case, the weight ratio of the aqueous medium to the polyisobutylene present in the organic medium is 100:1.
[0070] In yet another embodiment, the aqueous medium comprises 70 ppm or less, preferably 50 ppm or less, more preferably 30 ppm or less and even more preferably 20 ppm or less and yet even more preferably 10 ppm or less of a carboxylate of a polyvalent metal ion, calculated in terms of its metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms. In one embodiment, such carboxylic acids are selected from monocarboxylic acids and dicarboxylic acids, preferably dicarboxylic acids. In another embodiment, such carboxylic acids are selected from saturated monocarboxylic acids such as palmitic acid or stearic acid. The carboxylic acids, preferably monocarboxylic acids, can be saturated or unsaturated, preferably saturated. Examples of unsaturated monocarboxylic acids are oleic acid, elaidic acid, erucic acid, linoleic acid, linolenic acid and eleostearic acid.
[0071] Examples of dicarboxylic acids are 2-alkenyl-substituted succinic acids, such as dodecenylsuccinic acid and polyisobutenylsuccinic acid, where the polyisobutenyl residue has 12 to 50 carbon atoms.
[0072] In yet another embodiment, the aqueous medium comprises 25 ppm or less, preferably 10 ppm or less, more preferably 8 ppm or less and even more preferably 7 ppm or less and still even more preferably 5 ppm or less of a carboxylate of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is chosen from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms. In one embodiment, such carboxylic acids are chosen from monocarboxylic acids. In another embodiment, such carboxylic acids are chosen from saturated monocarboxylic acids such as stearic acid.
[0073] In one embodiment, the aqueous medium does not contain carboxylates of polyvalent metal ions, wherein the carboxylic acid is selected from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms. In one embodiment, such carboxylic acids are selected from monocarboxylic acids. In another embodiment, such carboxylic acids are selected from saturated monocarboxylic acids such as stearic acid.
[0074] In another embodiment, the aqueous medium contains 100 ppm or less, preferably 50 ppm or less, more preferably 20 ppm or less and even more preferably 15 ppm or less and still even more preferably 10 ppm or less of a salt of a monovalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0075] In another embodiment, the aqueous medium additionally or alternatively comprises 100ppm or less, preferably 50ppm or less, more preferably 30ppm or less, even more preferably 20ppm or less and also even more preferably 10ppm or less of carboxylate of monovalent metal ions, and in another even more preferred embodiment, comprises 5ppm or less of carboxylate of monovalent metal ions, such as sodium stearate, sodium palmitate and sodium oleate and potassium stearate, potassium palmitate and potassium oleate, calculated with respect to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from those carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms. In one embodiment, such carboxylic acids are selected from monocarboxylic acids. In another embodiment, such carboxylic acids are selected from saturated monocarboxylic acids such as stearic acid. Examples of monovalent salts of carboxylic acids include sodium stearate, sodium palmitate and sodium oleate and potassium stearate, potassium palmitate and potassium oleate.
[0076] In one embodiment, the aqueous medium does not contain carboxylates of monovalent metal ions, wherein the carboxylic acid is selected from those having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms. In one embodiment, such carboxylic acids are selected from monocarboxylic acids. In another embodiment, such carboxylic acids are selected from saturated monocarboxylic acids such as palmitic acid or stearic acid.
[0077] In another embodiment, the aqueous medium comprises 0 to 5,000 ppm, preferably 0 to 2,000 ppm, more preferably 10 to 1,000 ppm, even more preferably 50 to 800 ppm and still even more preferably 100 to 600 ppm of carbonate of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0078] In another embodiment, the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of carbonates of polyvalent metal ions, and in another still even more preferred embodiment, 100 ppm or less of carbonates of polyvalent metal ions, calculated as metal content and relative to the amount of polyisobutylene present in the organic medium.
[0079] In yet another embodiment, the aqueous medium comprises 70 ppm or less, preferably 50 ppm or less, more preferably 30 ppm or less and even more preferably 20 ppm or less and still even more preferably 10 ppm or less of carbonates of polyvalent metal ions, calculated as their metal content and relative to the amount of polyisobutylene present in the organic medium.
[0080] In particular, the carbonates of polyvalent metal ions are magnesium carbonate and calcium carbonate.
[0081] In particular, the term polyvalent metal ion includes divalent alkaline earth metal ions such as magnesium, calcium, strontium and barium, preferably magnesium and calcium; trivalent metal ions of Group 13 such as aluminum; polyvalent metal ions of Groups 3 to 12, especially the divalent metal ion zinc.
[0082] In particular, the term monovalent metal ion includes alkali metal ions such as lithium, sodium and potassium.
[0083] In another embodiment, the aqueous medium comprises 500 ppm or less, preferably 200 ppm or less, more preferably 100 ppm or less, even more preferably 50 ppm or less and still even more preferably 20 ppm or less of layered minerals, and in another yet even more preferred embodiment, contains no layered minerals, such as talc, calculated relative to the amount of polyisobutylene present in the organic medium.
[0084] In another embodiment, the aqueous medium comprises 500 ppm or less, preferably 200 ppm or less, more preferably 100 ppm or less, even more preferably 20 ppm or less and still even more preferably 10 ppm or less of dispersants, emulsifiers or anti-agglomeration agents other than LCST compounds, and in another yet even more preferred embodiment comprises 5 ppm or less and yet even more preferably comprises no dispersants, emulsifiers or anti-agglomeration agents other than LCST compounds. The term "multiple" means an integer of at least 2, preferably at least 20, more preferably at least 100.
[0085] In one embodiment, the expression "aqueous slurry comprising a plurality of polyisobutylene particles suspended therein" refers to a slurry having at least 10 discrete particles per liter suspended therein, preferably at least 20 discrete particles per liter, more preferably at least 50 discrete particles per liter and even more preferably at least 100 discrete particles per liter.
[0086] The term polyisobutylene particles refers to discrete particles of any form and consistency, which in a preferred embodiment have a particle size between 0.05 mm and 25 mm, more preferably between 0.1 and 20 mm. These polyisobutylene particles with a particle size between 0.05 mm and 25 mm are formed by agglomeration of primary particles formed in the polymerization reaction. In the context of the present invention, these polyisobutylene particles may also be referred to as "pellets" or "secondary particles".
[0087] In one embodiment, the polyisobutylene particles have a weight average particle size of about 0.3 to about 10.0 mm, preferably about 0.6 to about 10.0 mm.
[0088] For practical industrial production of polyisobutylene, it is important that the polyisobutylene particles (pellets) fall within a predictable particle size distribution, since process equipment such as pump and pipe diameters are selected to some extent based on this particle size. Thus, extraction of residual solvent and monomer from polyisobutylene particles is more effective for polyisobutylene particles within a specific particle size distribution. Polyisobutylene particles that are too coarse may contain a large amount of residual hydrocarbons, while polyisobutylene particles that are too fine may have a higher tendency to cause fouling.
[0089] The particle size distribution of the polyisobutylene particles can be measured, for example, by using a conventional stack of standard size sieves, wherein the size of the sieve openings decreases from the top to the bottom of the stack. A sample of the polyisobutylene particles is taken from the aqueous slurry and placed on the top sieve, and the stack is then shaken manually or by an automatic shaker. Optionally, the polyisobutylene particles can be manually processed through one sieve at a time. Once the polyisobutylene particles are separated by size, the pellets in each sieve are collected and weighed to determine the polyisobutylene particle size distribution in weight percent.
[0090] A typical sieving experiment has 6 sieves with mesh openings of about 19.00 mm, about 12.50 mm, about 8.00 mm, about 6.30 mm, about 3.35 mm, and about 1.60 mm. In a typical embodiment, 90% by weight or more of the polyisobutylene particles will be collected on a sieve between about 12.50 mm and about 1.60 mm (inclusive). In another embodiment, 50% by weight or more, 60% by weight or more, 70% by weight or more, or 80% by weight or more of the polyisobutylene particles will be collected on a sieve between about 8.00 mm and about 3.35 mm (inclusive).
[0091] In one embodiment, the particle size distribution of the polyisobutylene particles indicates that less than 10 wt. %, preferably less than 5 wt. %, more preferably less than 3 wt. %, and even more preferably less than 1 wt. % of the particles are not retained on any of the sieves having mesh openings of about 19.00 mm, about 12.50 mm, about 8.00 mm, about 6.30 mm, about 3.35 mm, and about 1.60 mm.
[0092] In another embodiment, the polyisobutylene particles have a particle size distribution indicating that less than 5 wt%, preferably less than 3 wt%, preferably less than 1 wt% of the particles are retained on a sieve having a mesh size of about 19.00 mm.
[0093] Of course, by adjusting the variables in the process, the polyisobutylene particle size distribution can be biased toward higher or lower values.
[0094] It is obvious to those skilled in the art that the polyisobutylene particles formed according to the present invention may still contain organic diluents and / or residual monomers, and may also contain water encapsulated within the polyisobutylene particles. In one embodiment, the polyisobutylene particles contain 90% by weight or more polyisobutylene, based on the sum of organic diluents, isobutylene and polyisobutylene, preferably 93% by weight or more, more preferably 94% by weight or more and even more preferably 96% by weight or more.
[0095] As mentioned above, polyisobutylene particles are often referred to as agglomerates in the literature. Typically, the polyisobutylene particles or agglomerates have a non-uniform shape and / or geometry.
[0096] The term aqueous medium denotes a medium comprising 80 wt% or more water, preferably 90 wt% or more and even more preferably 95 wt% or more water and still even more preferably 99 wt% or more.
[0097] The remainder to 100% by weight comprises LCST compounds and may also comprise compounds selected from the group consisting of
[0098] Non-LCST compounds as defined above
[0099] Compounds and salts which are neither LCST compounds as defined above nor non-LCST compounds as defined above, including, for example, inorganic bases for neutralizing the reaction and controlling the pH of the process
[0100] · Organic diluents that are soluble in the aqueous medium to some extent
[0101] Where it is desired to extend the shelf life of the product: antioxidants and / or stabilizers.
[0102] Examples of such inorganic bases are hydroxides, oxides, carbonates and bicarbonates of alkali metals (preferably sodium and potassium). Preferred examples are sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate and potassium bicarbonate.
[0103] In embodiments in which the content of polyvalent metal ions is not particularly critical, other suitable inorganic bases are hydroxides, oxides, carbonates and bicarbonates of alkaline earth metals, preferably calcium and magnesium.
[0104] Preferred examples are calcium hydroxide, calcium carbonate, magnesium carbonate, calcium hydrogen carbonate and magnesium hydrogen carbonate.
[0105] The process pH measured at 20° C. and 1013 hPa is preferably from 5 to 10, preferably from 6 to 9 and more preferably from 7 to 9.
[0106] In one embodiment, the aqueous medium contains 1 to 2,000 ppm of antioxidant, preferably 50 to 1,000 ppm, more preferably 80 to 500 ppm, relative to the amount of polyisobutylene present in the organic medium.
[0107] When very high purity products are desired, the water used to prepare the aqueous medium is demineralized by standard methods such as ion exchange, membrane filtration techniques such as reverse osmosis, and the like.
[0108] Usually, it is sufficient to use water having a hardness of 8.0 German degrees (°dH) or less, preferably 6.0°dH or less, more preferably 3.75°dH or less and even more preferably 3.00°dH or less.
[0109] In one embodiment, water is mixed with at least one LCST compound to obtain a concentrate which, depending on the temperature, is a slurry or solution having a concentration of LCST compound of 0.1 to 2% by weight, preferably 0.5 to 1% by weight. This concentrate is then metered into the vessel in which step A) is carried out and diluted with more water to the desired concentration.
[0110] Preferably, the concentrate is a solution and is metered into a container at a temperature of 0 to 35°C, preferably 10 to 30°C.
[0111] If not mentioned otherwise, ppm refers to ppm by weight.
[0112] The aqueous medium may also contain antioxidants and stabilizers:
[0113] Antioxidants and stabilizers include 2,6-di-tert-butyl-4-methyl-phenol (BHT) and pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid (also known as 1010), 3,5-di(tert-butyl)-4-hydroxyhydrocinnamate (also known as 1076), tert-butyl-4-hydroxyanisole (BHA), 2-(1,1-dimethyl)-1,4-benzenediol (TBHQ), tris(2,4-di-tert-butylphenyl) phosphate ( 168), dioctyl diphenylamine ( S), butylated products of p-cresol and dicyclopentadiene (Wingstay), and other phenolic antioxidants and hindered amine light stabilizers.
[0114] Suitable antioxidants generally include 2,4,6-tri-tert-butylphenol, 2,4,6-triisobutylphenol, 2-tert-butyl-4,6-dimethylphenol, 2,4-dibutyl-6-ethylphenol, 2,4-dimethyl-6-tert-butylphenol, 2,6-di-tert-butylhydroxytoluene (BHT), 2,6-di-tert-butyl-4-ethylphenol, 2,6-di-tert-butyl-4-n-butylphenol, 2,6-di-tert-butyl-4-isobutylphenol, 2,6-dicyclopentyl-4-methylphenol, 4-tert-butyl-2,6-dimethylphenol, 4-tert-butyl-2,6-dicyclopentylphenol, 4-tert-butyl -2,6-diisopropylphenol, 4,6-di-tert-butyl-2-methylphenol, 6-tert-butyl-2,4-dimethylphenol, 2,6-di-tert-butyl-3-methylphenol, 4-hydroxymethyl-2,6-di-tert-butylphenol, 2,6-di-tert-butyl-4-phenylphenol and 2,6-dioctadecyl-4-methylphenol, 2,2'-ethylene-bis[4,6-di-tert-butylphenol], 2,2'-ethylene-bis[6-tert-butyl-4-isobutylphenol], 2,2'-isobutylene-bis[4,6-dimethylphenol], 2,2'-methylene-bis[4,6-di-tert-butylphenol], 2 ,2'-methylene-bis[4-methyl-6-(α-methylcyclohexyl)phenol], 2,2'-methylene-bis[4-methyl-6-cyclohexylphenol], 2,2'-methylene-bis[4-methyl-6-nonylphenol], 2,2'-methylene-bis[6-(α,α'-dimethylbenzyl)-4-nonylphenol], 2,2'-methylene-bis[6-(α-methylbenzyl)-4-nonylphenol], 2,2'-methylene-bis[6-cyclohexyl-4-methylphenol], 2,2'-methylene-bis[6-tert-butyl-4-ethylphenol], 2,2'-methylene-bis[6- tert-butyl-4-methylphenol], 4,4'-butylene-bis[2-tert-butyl-5-methylphenol], 4,4'-methylene-bis[2,6-di-tert-butylphenol], 4,4'-methylene-bis[6-tert-butyl-2-methylphenol], 4,4'-isopropylidene-biphenol, 4,4'-decylene-bisphenol, 4,4'-dodecylene-bisphenol, 4,4'-(1-methyloctylene)bisphenol, 4,4'-cyclohexylene-bis(2-methylphenol), 4,4'-cyclohexylene-bisphenol and pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid (also known as 1010).
[0115] In one embodiment, the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 100 to 3,000 kg / mol, preferably in the range of 250 to 3,000 kg / mol.
[0116] In another embodiment, the viscosity average molecular weight (M) of the polyisobutylene isv ) is in the range of 100 to 2,000 kg / mol, preferably in the range of 200 to 2,000 kg / mol, more preferably in the range of 350 to 1,800 kg / mol, even more preferably in the range of 400 to 1500 kg / mol and still even more preferably 700 to 1300 kg / mol.
[0117] In yet another embodiment, the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 2,001 to 3,000 kg / mol.
[0118] In yet another embodiment, the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 3,001 to 10,000 kg / mol.
[0119] In another embodiment, the number average molecular weight (M) of the polyisobutylene is n ) is in the range of about 5 to about 1100 kg / mol, preferably in the range of about 80 to about 500 kg / mol.
[0120] In one embodiment, the polyisobutylene of the present invention has a polydispersity in the range of 1.1 to 6.0, preferably in the range of 3.0 to 5.5, as measured by the ratio of the weight average molecular weight to the number average molecular weight determined by gel permeation chromatography (preferably using tetrahydrofuran as solvent and polystyrene as molecular weight standard).
[0121] For example and typically, the polyisobutylene has a Mooney viscosity of at least 10 (ML 125°C 1+8, ASTM D1646-07 (2012)), preferably 10 to 80, more preferably 20 to 80 and even more preferably 25 to 60 (ML 125°C 1+8, ASTM D 1646).
[0122] monomer
[0123] In one embodiment, the organic medium used in step A) is obtained by a process comprising at least the following steps:
[0124] a) providing a reaction medium comprising an organic diluent and isobutylene
[0125] b) polymerizing the isobutylene in the reaction medium in the presence of an initiator system or catalyst to form an organic medium comprising the polyisobutylene, an organic diluent and optionally residual monomers.
[0126] Isobutylene may be present in the reaction medium in an amount from 0.01 wt% to 80 wt%, preferably from 0.1 wt% to 65 wt%, more preferably from 10.0 wt% to 65.0 wt% and even more preferably from 25.0 wt% to 65.0 wt%, or in another embodiment from 10.0 wt% to 20.0 wt%.
[0127] In one embodiment, the isobutylene is purified before use in step a), especially when it is recovered from step d). The purification of the isobutylene can be carried out by passing it through an adsorption column containing a suitable molecular sieve or an alumina-based adsorption material. In order to minimize interference with the polymerization reaction, the total concentration of water and substances such as alcohols and other organic oxygenates that act as reaction poisons is preferably reduced to less than about 100 parts per million by weight.
[0128] Organic diluent
[0129] The term organic diluent includes diluted or dissolved organic chemicals that are liquid under the reaction conditions.Any suitable organic diluent that does not react with the monomers or components of the initiator system or does not react with the monomers or components of the initiator system to any appreciable extent may be used.
[0130] However, those skilled in the art are aware that interactions may occur between the diluent and the components of the monomer or initiator system or the catalyst.
[0131] Furthermore, the term organic diluent includes mixtures of at least two diluents.
[0132] Examples of organic diluents include hydrochlorocarbon(s) such as methyl chloride, methylene chloride or ethyl chloride.
[0133] Other examples of organic diluents include those of the formula: x H y F z The hydrofluorocarbon represented by wherein x is an integer from 1 to 40, or from 1 to 30, or from 1 to 20, or from 1 to 10, or from 1 to 6, or from 2 to 20, or from 3 to 10, or from 3 to 6, most preferably from 1 to 3, wherein y and z are integers and are at least 1.
[0134] In one embodiment, the hydrofluorocarbon is selected from the group consisting of saturated hydrofluorocarbons, for example, fluoromethane, difluoromethane, trifluoromethane, fluoroethane, 1,1-difluoroethane, 1,2-difluoroethane, 1,1,1-trifluoroethane, 1,1,2-trifluoroethane, 1,1,2,2-tetrafluoroethane, 1,1,1,2,2-pentafluoroethane, 1-fluoropropane, 2-fluoropropane, 1,1-difluoropropane, 1,2-difluoropropane, 1,3-difluoropropane, 2,2-difluoropropane, 1,1,1-trifluoropropane, 1,1,2-trifluoropropane, 1,1,3-trifluoropropane, 1,2,2-trifluoropropane, 1,2,3-trifluoropropane, 1,1,1,2-tetrafluoropropane, 1,1,1,3-tetrafluoropropane, 1,1,2,2-tetrafluoropropane, 1,1,1,2,2-pentafluoroethane, ... Fluoropropane, 1,1,2,3-tetrafluoropropane, 1,1,3,3-tetrafluoropropane, 1,2,2,3-tetrafluoropropane, 1,1,1,2,2-pentafluoropropane, 1,1,1,2,3-pentafluoropropane, 1,1,1,3,3-pentafluoropropane, 1,1,2,2,3-pentafluoropropane, 1,1,2,3,3-pentafluoropropane, 1,1,1, 2,2,3-Hexafluoropropane, 1,1,1,2,3,3-Hexafluoropropane, 1,1,1,3,3,3-Hexafluoropropane, 1,1,1,2,2,3,3-Heptafluoropropane, 1,1,1,2,3,3,3-Heptafluoropropane, 1-Fluorobutane, 2-Fluorobutane, 1,1-Difluorobutane, 1,2-Difluorobutane, 1,3-Difluorobutane, 1,4 -Difluorobutane, 2,2-difluorobutane, 2,3-difluorobutane, 1,1,1-trifluorobutane, 1,1,2-trifluorobutane, 1,1,3-trifluorobutane, 1,1,4-trifluorobutane, 1,2,2-trifluorobutane, 1,2,3-trifluorobutane, 1,3,3-trifluorobutane, 2,2,3-trifluorobutane, 1,1,1,2-tetrafluorobutane , 1,1,1,3-tetrafluorobutane, 1,1,1,4-tetrafluorobutane, 1,1,2,2-tetrafluorobutane, 1,1,2,3-tetrafluorobutane, 1,1,2,4-tetrafluorobutane, 1,1,3,3-tetrafluorobutane, 1,1,3,4-tetrafluorobutane, 1,1,4,4-tetrafluorobutane, 1,2,2,3-tetrafluorobutane, 1,2,2,4 -tetrafluorobutane, 1,2,3,3-tetrafluorobutane, 1,2,3,4-tetrafluorobutane, 2,2,3,3-tetrafluorobutane, 1,1,1,2,2-pentafluorobutane, 1,1,1,2,3-pentafluorobutane, 1,1,1,2,4-pentafluorobutane, 1,1,1,3,3-pentafluorobutane, 1,1,1,3,4-pentafluorobutane, 1,1,1 ,4,4-pentafluorobutane, 1,1,2,2,3-pentafluorobutane, 1,1,2,2,4-pentafluorobutane, 1,1,2,3,3-pentafluorobutane, 1,1,2,4,4-pentafluorobutane, 1,1,3,3,4-pentafluorobutane, 1,2,2,3,3-pentafluorobutane, 1,2,2,3,4-pentafluorobutane, 1,1,1,2,2,3-Hexafluorobutane, 1,1,1,2,2,4-Hexafluorobutane, 1,1,1,2,3,3-Hexafluorobutane, 1,1,1,2,3,4-Hexafluorobutane, 1,1,1,2,4,4-Hexafluorobutane, 1,1,1,3,3,4-Hexafluorobutane, 1,1,1,3,4,4-Hexafluorobutane, 1,1,1,4,4,4-Hexafluorobutane, 1,1,2,2,3,3-Hexafluorobutane, 1,1,2,2,3,4-Hexafluorobutane, 1,1,2,2,4,4-Hexafluorobutane, 1,1,2,3,3,4-Hexafluorobutane, 1,1,2,2,3,3,4-Hexafluorobutane, 1,1,2,2,4,4-Hexafluorobutane 1,1,2,2,3,3-heptafluorobutane, 1,1,1,2,2,4,4-heptafluorobutane, 1,1,1,2,2,3,4-heptafluorobutane, 1,1,1,2,3,3,4-heptafluorobutane, 1,1,1,2,3,4,4-heptafluorobutane, 1,1,1,2,4,4,4-heptafluorobutane, 1,1,1,3,3,4,4-heptafluorobutane, 1,1,1,2,2,3,3,4-octafluorobutane, 1,1,1,2,2,3,4,4-octafluorobutane, 1,1,1,2,3,4,4,4- Octafluorobutane, 1,1,1,2,2,3,3,4,4-nonafluorobutane, 1,1,1,2,2,3,4,4,4-nonafluorobutane, 1-fluoro-2-methylpropane, 1,1-difluoro-2-methylpropane, 1,3-difluoro-2-methylpropane, 1,1,1-trifluoro-2-methylpropane, 1,1,3-trifluoro-2-methylpropane, 1,3-difluoro-2-(fluoromethyl)propane, 1,1,1,3-tetrafluoro-2-methylpropane, 1,1,3,3-tetrafluoro-2-methylpropane, 1,1,3-trifluoro-2-(fluoromethyl)propane, 1,1,1,3,3-pentafluoro-2-methylpropane, 1,1,3,3-tetrafluoro-2-(fluoromethyl)propane )propane, 1,1,1,3-tetrafluoro-2-(fluoromethyl)propane, fluorocyclobutane, 1,1-difluorocyclobutane, 1,2-difluorocyclobutane, 1,3-difluorocyclobutane, 1,1,2-trifluorocyclobutane, 1,1,3-trifluorocyclobutane, 1,2,3-trifluorocyclobutane, 1,1,2,2-tetrafluorocyclobutane, 1,1,3,3-tetrafluorocyclobutane, 1,1,2,2,3-pentafluorocyclobutane, 1,1,2,3,3-pentafluorocyclobutane, 1,1,2,2,3,3-hexafluorocyclobutane, 1,1,2,2,3,4-hexafluorocyclobutane, 1,1,2,3,3,4-hexafluorocyclobutane, 1,1,2,2,3,3,4-heptafluorocyclobutane;
[0135] Particularly preferred HFC's include difluoromethane, trifluoromethane, 1,1-difluoroethane, 1,1,1-trifluoroethane, fluoromethane and 1,1,1,2-tetrafluoroethane.
[0136] In another embodiment, the hydrofluorocarbon is selected from unsaturated hydrofluorocarbons, for example, vinyl fluoride, 1,2-difluoroethylene, 1,1,2-trifluoroethylene, 1-fluoropropylene, 1,1-difluoropropylene, 1,2-difluoropropylene, 1,3-difluoropropylene, 2,3-difluoropropylene, 3,3-difluoropropylene, 1,1,2-trifluoropropylene, 1,1,3-trifluoropropylene, 1,2,3-trifluoropropylene, 1,3,3-trifluoropropylene, 2,3,3-trifluoropropylene, 3,3,3-trifluoropropylene, 2,3,3,3-tetrafluoro-1-propylene, 1-fluoro-1-butene, 2-fluoro-1-butene, 3-fluoro-1-butene, 4-fluoro-1-butene, 1,1-difluoro-1-butene, 1,2-difluoro-1-butene, 1,3-difluoropropylene , 1,4-difluoro-1-butene, 2,3-difluoro-1-butene, 2,4-difluoro-1-butene, 3,3-difluoro-1-butene, 3,4-difluoro-1-butene, 4,4-difluoro-1-butene, 1,1,2-trifluoro-1-butene, 1,1,3-trifluoro-1-butene, 1,1,4-trifluoro-1-butene, 1,2,3-trifluoro-1 -Butene, 1,2,4-trifluoro-1-butene, 1,3,3-trifluoro-1-butene, 1,3,4-trifluoro-1-butene, 1,4,4-trifluoro-1-butene, 2,3,3-trifluoro-1-butene, 2,3,4-trifluoro-1-butene, 2,4,4-trifluoro-1-butene, 3,3,4-trifluoro-1-butene, 3,4,4-trifluoro- 1-Butene, 4,4,4-trifluoro-1-butene, 1,1,2,3-tetrafluoro-1-butene, 1,1,2,4-tetrafluoro-1-butene, 1,1,3,3-tetrafluoro-1-butene, 1,1,3,4-tetrafluoro-1-butene, 1,1,4,4-tetrafluoro-1-butene, 1,2,3,3-tetrafluoro-1-butene, 1,2,3,4-tetrafluoro -1-butene, 1,2,4,4-tetrafluoro-1-butene, 1,3,3,4-tetrafluoro-1-butene, 1,3,4,4-tetrafluoro-1-butene, 1,4,4,4-tetrafluoro-1-butene, 2,3,3,4-tetrafluoro-1-butene, 2,3,4,4-tetrafluoro-1-butene, 2,4,4,4-tetrafluoro-1-butene, 3,3,4,4 -tetrafluoro-1-butene, 3,4,4,4-tetrafluoro-1-butene, 1,1,2,3,3-pentafluoro-1-butene, 1,1,2,3,4-pentafluoro-1-butene, 1,1,2,4,4-pentafluoro-1-butene, 1,1,3,3,4-pentafluoro-1-butene, 1,1,3,4,4-pentafluoro-1-butene, 1,1,4,4,4- Pentafluoro-1-butene, 1,2,3,3,4-pentafluoro-1-butene, 1,2,3,4,4-pentafluoro-1-butene, 1,2,4,4,4-pentafluoro-1-butene, 2,3,3,4,4-pentafluoro-1-butene, 2,3,4,4,4-pentafluoro-1-butene, 3,3,4,4,4-pentafluoro-1-butene, 1,1,2,3,3,4-Hexafluoro-1-butene, 1,1,2,3,4,4-Hexafluoro-1-butene, 1,1,2,4,4,4-Hexafluoro-1-butene, 12,3,3,4,4-Hexafluoro-1-butene, 1,2,3,4,4,4-Hexafluoro-1-butene, 2,3,3,4,4,4-Hexafluoro-1-butene, 1,1,2,3,3,4,4-Hexafluoro-1-butene, 1,1,2,3,4,4,4-Hexafluoro-1-butene, 1,1,3,3,4,4,4-Hexafluoro-1-butene, 1,2 ,3,3,4,4,4-heptafluoro-1-butene, 1-fluoro-2-butene, 2-fluoro-2-butene, 1,1-difluoro-2-butene, 1,2-difluoro-2-butene, 1,3-difluoro-2-butene, 1,4-difluoro-2-butene, 2,3-difluoro-2-butene, 1,1,1-trifluoro-2-butene, 1,1,2-trifluoro-2-butene, 1,1,3-trifluoro-2-butene, 1,1,4-trifluoro-2-butene, 1,2,3-trifluoro-2-butene, 1,2,4-trifluoro-2- Butene, 1,1,1,2-tetrafluoro-2-butene, 1,1,1,3-tetrafluoro-2-butene, 1,1,1,4-tetrafluoro-2-butene, 1,1,2,3-tetrafluoro-2-butene, 1,1,2,4-tetrafluoro-2-butene, 1,2,3,4-tetrafluoro-2-butene, 1,1,1,2,3-pentafluoro-2-butene, 1,1,1,2,4-pentafluoro-2-butene, 1,1,1,3,4-pentafluoro-2-butene, 1,1,1,4,4-pentafluoro-2-butene, 1,1,2,3 ,4-pentafluoro-2-butene, 1,1,2,4,4-pentafluoro-2-butene, 1,1,1,2,3,4-hexafluoro-2-butene, 1,1,1,2,4,4-hexafluoro-2-butene, 1,1,1,3,4,4-hexafluoro-2-butene, 1,1,1,4,4,4-hexafluoro-2-butene, 1,1,2,3,4,4-hexafluoro-2-butene, 1,1,1,2,3,4,4-hexafluoro-2-butene, 1,1,1,2,3,4,4-hexafluoro-2-butene, 1,1,1,2,4,4,4-heptafluoro-2-butene, and mixtures thereof.
[0137] Other examples of organic diluents include hydrochlorofluorocarbons.
[0138] Other examples of organic diluents include hydrocarbons, preferably alkanes, and in another preferred embodiment, the alkanes are those selected from the group consisting of propane, isobutane, pentane, methylcyclopentane, isohexane, 2-methylpentane, 3-methylpentane, 2-methylbutane, 2,2-dimethylbutane, 2,3-dimethylbutane, 2-methylhexane, 3-methylhexane, 3-ethylpentane, 2,2-dimethylpentane, 2,3-dimethylpentane, 2,4-dimethylpentane, 3,3-dimethylpentane, Pentane, 2-methylheptane, 3-ethylhexane, 2,5-dimethylhexane, 2,2,4-trimethylpentane, octane, heptane, butane, ethane, methane, nonane, decane, dodecane, undecane, hexane, methylcyclohexane, cyclopropane, cyclobutane, cyclopentane, methylcyclopentane, 1,1-dimethylcyclopentane, cis-1,2-dimethylcyclopentane, trans-1,2-dimethylcyclopentane, trans-1,3-dimethyl-cyclopentane, ethylcyclopentane, cyclohexane, methylcyclohexane.
[0139] Other examples of hydrocarbon diluents include benzene, toluene, xylene, ortho-xylene, para-xylene, and meta-xylene.
[0140] Suitable organic diluents also include mixtures of at least two compounds selected from hydrochlorocarbons, hydrofluorocarbons, hydrochlorofluorocarbons and hydrocarbons. Specific combinations include mixtures of hydrochlorocarbons and hydrofluorocarbons, such as mixtures of methyl chloride and 1,1,1,2-tetrafluoroethane, in particular mixtures of 40 to 60% by volume of methyl chloride and 40 to 60% by volume of 1,1,1,2-tetrafluoroethane, wherein the above two diluents together account for 90 to 100% by volume of the total diluent, preferably 95 to 100% by volume, wherein the remaining possible parts up to 100% by volume include: other halogenated hydrocarbons; or a mixture of methyl chloride and at least one alkane, or a mixture of multiple alkanes such as a mixture containing at least 90% by weight, preferably 95% by weight of alkanes, wherein the boiling point of the alkane at a pressure of 1013 hPa is from -5°C to 100°C, or in another embodiment, from 35°C to 85°C. In another embodiment, at least 99.9 wt. %, preferably 100 wt. % of the alkanes have a boiling point of 100° C. or lower, preferably in the range of 35 to 100° C., more preferably 90° C. or lower, even more preferably in the range of 35 to 90° C., at a pressure of 1013 hPa.
[0141] Depending on the nature of the polymerisation used in step b), the organic diluent is chosen to allow for a slurry polymerisation or a solution polymerisation.
[0142] Initiator system
[0143] In step b), isobutylene in the reaction medium is polymerized in the presence of an initiator system to form a medium comprising polyisobutylene, an organic diluent and optionally residual isobutylene.
[0144] In particular, initiator systems for polyisobutenes obtained by cationic polymerization generally comprise at least one Lewis acid and an initiator.
[0145] Lewis acid
[0146] Suitable Lewis acids include compounds represented by the formula MX3, wherein M is a Group 13 element and X is a halogen. Examples of such compounds include aluminum trichloride, aluminum tribromide, boron trifluoride, boron trichloride, boron tribromide, gallium trichloride, and indium trifluoride, with aluminum trichloride being preferred.
[0147] Other suitable Lewis acids include those of the formula MR (m) X (3-m) The compound represented by wherein M is a Group 13 element, X is a halogen, and R is selected from C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14 and m is 1 or 2. X can also be an azido group, an isocyanate group, a thiocyanate group, an isothiocyanate group, or a cyano group.
[0148] Examples of such compounds include methylaluminum dibromide, methylaluminum dichloride, ethylaluminum dibromide, ethylaluminum dichloride, butylaluminum dibromide, butylaluminum dichloride, dimethylaluminum bromide, dimethylaluminum chloride, diethylaluminum bromide, diethylaluminum chloride, dibutylaluminum bromide, dibutylaluminum chloride, methylaluminum sesquibromide, methylaluminum sesquichloride, ethylaluminum sesquibromide, ethylaluminum sesquichloride, and any mixtures thereof. Diethylaluminum chloride (Et2AlCl or DEAC), ethylaluminum sesquichloride (Et2AlCl or DEAC), and ethylaluminum sesquichloride (Et2AlCl or DEAC) are preferred. 1.5 AlCl 1.5 or EASC), ethylaluminum dichloride (EtAlCl2 or EADC), diethylaluminum bromide (Et2AlBr or DEAB), ethylaluminum sesquibromide (Et 1.5 ABr 1.5 or EASB) and ethylaluminum dibromide (EtAlBr2 or EADB) and any mixture thereof.
[0149] Other suitable Lewis acids include those of the formula M(RO) n R' m X (3-(m+n)) wherein M is a Group 13 metal; wherein RO is a monovalent hydrocarboxy group selected from the following: C1-C 30 Alkoxy, C7-C 30 Aryloxy, C7-C 30 Arylalkoxy, C7-C 30Alkyl aryloxy; R' is a monovalent hydrocarbon group selected from the following: C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14 an alkylaryl group; n is a number from 0 to 3 and m is a number from 0 to 3 such that the sum of n and m is not greater than 3;
[0150] X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X can also be an azido group, an isocyanate group, a thiocyanate group, an isothiocyanate group or a cyano group.
[0151] For purposes of the present invention, those skilled in the art will recognize that the terms alkoxy and aryloxy are structural equivalents of alkoxide and phenoxide, respectively. The term "arylalkoxy" refers to a group that contains both aliphatic and aromatic structures, said group being in the alkoxy position. The term "alkylaryl" refers to a group that contains both aliphatic and aromatic structures, said group being in the aryloxy position.
[0152] Non-limiting examples of these Lewis acids include methoxyaluminum dichloride, ethoxyaluminum dichloride, 2,6-di-tert-butylphenoxyaluminum dichloride, methoxymethylaluminum chloride, 2,6-di-tert-butylphenoxymethylaluminum chloride, isopropoxygallium dichloride, and phenoxymethylindium fluoride.
[0153] Other suitable Lewis acids include those of the formula M (RC=OO) n R' m X (3-(m+n)) The compound represented by wherein M is a Group 13 metal; wherein RC=OO is a monovalent hydrocarbacyl group selected from the following: C1-C 30 Alkyl acyloxy, C7-C 30 Aryl acyloxy, C7-C 30 Arylalkyl acyloxy, C7-C 30 Alkyl aryl acyloxy group; R' is a monovalent hydrocarbon group selected from the following: C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14 an alkylaryl group; n is a number from 0 to 3 and m is a number from 0 to 3 such that the sum of n and m is not greater than 3; X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X may also be an azido group, an isocyanate group, a thiocyanate group, an isothiocyanate group or a cyano group.
[0154] The term "arylalkyl acyloxy" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the alkyl acyloxy position. The term "alkylaryl acyloxy" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the aryl acyloxy position. Non-limiting examples of these Lewis acids include acetoxyaluminum dichloride, benzoyloxyaluminum dibromide, benzoyloxygallium difluoride, methylacetoxyaluminum chloride, and isopropionyloxyindium trichloride.
[0155] Other suitable Lewis acids include compounds based on metals from Groups 4, 5, 14 and 15 of the Periodic Table of the Elements, including titanium, zirconium, tin, vanadium, arsenic, antimony and bismuth.
[0156] However, those skilled in the art will recognize that some elements are more suitable for the practice of the present invention. The Lewis acids of Groups 4, 5 and 14 have the general formula MX4; wherein M is a Group 4, 5 or 14 metal; and X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X may also be an azido, an isocyanate, a thiocyanate, an isothiocyanate or a cyano group. Non-limiting examples include titanium tetrachloride, titanium tetrabromide, vanadium tetrachloride, tin tetrachloride and zirconium tetrachloride. The Lewis acids of Groups 4, 5 or 14 may also contain more than one type of halogen. Non-limiting examples include monobromotitanium trichloride, dibromotitanium dichloride, monobromovanadium trichloride and monochlorotin trifluoride.
[0157] The Group 4, 5 and 14 Lewis acids useful in the present invention may also have the general formula MR n X (4-n) ; wherein M is a Group 4, 5 or 14 metal; wherein R is a monovalent hydrocarbon group selected from the following: C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14 An alkylaryl group; n is an integer from 0 to 4; X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X can also be an azido group, an isocyanate group, a thiocyanate group, an isothiocyanate group or a cyano group.
[0158] The term "arylalkyl" refers to a group containing an aliphatic structure and an aromatic structure, the group being in the alkyl position.
[0159] The term "alkylaryl" refers to a group containing an aliphatic structure and an aromatic structure, the group being in the aryl position.
[0160] Non-limiting examples of these Lewis acids include benzyltitanium trichloride, dibenzyltitanium dichloride, benzylzirconium trichloride, dibenzylzirconium dibromide, methyltitanium trichloride, dimethyltitanium difluoride, dimethyltin dichloride, and phenylvanadium trichloride.
[0161] The Group 4, 5 and 14 Lewis acids useful in the present invention may also have the general formula M(RO) n R' m X 4-(m+n) wherein M is a Group 4, 5 or 14 metal, wherein RO is a monovalent hydrocarbon oxy group selected from the following: C1-C 30 Alkoxy, C7-C 30 Aryloxy, C7-C 30 Arylalkoxy, C7-C 30 Alkyl aryloxy group; R' is a monovalent hydrocarbon group selected from the following: C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14 an alkylaryl group; n is an integer from 0 to 4 and m is an integer from 0 to 4 such that the sum of n and m is not greater than 4; X is selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X may also be an azido group, an isocyanate group, a thiocyanate group, an isothiocyanate group or a cyano group.
[0162] For purposes of the present invention, one skilled in the art will recognize that the terms alkoxy and aryloxy are structural equivalents of alkoxide and phenoxide, respectively. The term "arylalkoxy" refers to a group containing both aliphatic and aromatic structures, said group being in the alkoxy position.
[0163] The term "alkylaryl" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the aryloxy position. Non-limiting examples of these Lewis acids include methoxytitanium trichloride, n-butoxytitanium trichloride, di(isopropoxy)titanium dichloride, phenoxytitanium tribromide, phenylmethoxyzirconium trifluoride, methylmethoxytitanium dichloride, methylmethoxytin dichloride, and benzylisopropoxyvanadium dichloride.
[0164] The Group 4, 5 and 14 Lewis acids useful in the present invention may also have the general formula M(RC=OO) n R' m X 4-(m+n) ; wherein M is a Group 4, 5 or 14 metal; wherein RC=OO is a monovalent hydrocarbon acyloxy group selected from the following: C1-C 30 Alkyl acyloxy, C7-C 30 Aryl acyloxy, C7-C 30 Arylalkyl acyloxy, C7-C 30 Alkyl aryl acyloxy group; R' is a monovalent hydrocarbon group selected from the following: C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14an alkylaryl group; n is an integer from 0 to 4 and m is an integer from 0 to 4 such that the sum of n and m is not greater than 4; X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X may also be an azido group, an isocyanate group, a thiocyanate group, an isothiocyanate group or a cyano group.
[0165] The term "arylalkylacyloxy" refers to a group containing an aliphatic structure and an aromatic structure, which is in the position of an alkylacyloxy group.
[0166] The term "alkylaryl acyloxy" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the aryl acyloxy position. Non-limiting examples of these Lewis acids include acetoxy titanium trichloride, benzoyl zirconium tribromide, benzoyloxy titanium trifluoride, isopropionyloxy tin trichloride, methylacetoxy titanium dichloride, and benzylbenzoyloxy vanadium chloride.
[0167] The Group 5 Lewis acids useful in the present invention may also have the general formula MOX3; wherein M is a Group 5 metal and wherein X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. A non-limiting example is vanadium oxytrichloride. The Group 15 Lewis acids have the general formula MX y , wherein M is a Group 15 metal and X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine, and y is 3, 4 or 5. X may also be an azido, an isocyanate, a thiocyanate, an isothiocyanate or a cyano group. Non-limiting examples include antimony hexachloride, antimony hexafluoride and arsenic pentafluoride. Group 15 Lewis acids may also contain more than one type of halogen. Non-limiting examples include monochloroantimony pentafluoride, arsenic trifluoride, bismuth trichloride and monofluoroarsenic tetrachloride.
[0168] The Group 15 Lewis acids useful in the present invention may also have the general formula MR n X y-n ; wherein M is a Group 15 metal; wherein R is a monovalent hydrocarbon group selected from the following: C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14 An alkylaryl group; and n is an integer from 0 to 4; y is 3, 4 or 5, so that n is less than y; X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X can also be an azido, isocyanate, thiocyanate, isothiocyanate or cyano. The term "arylalkyl" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the alkyl position. The term "alkylaryl" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the aryl position. Non-limiting examples of these Lewis acids include tetraphenylantimony chloride and triphenylantimony dichloride.
[0169] The Group 15 Lewis acids useful in the present invention may also have the general formula M(RO)n R' m X y-(m+n) wherein M is a Group 15 metal, wherein RO is a monovalent hydrocarbon oxy group selected from the following: C1-C 30 Alkoxy, C7-C 30 Aryloxy, C7-C 30 Arylalkoxy, C7-C 30 Alkyl aryloxy group; R' is a monovalent hydrocarbon group selected from the following: C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14 Alkylaryl group; n is an integer from 0 to 4 and m is an integer from 0 to 4 and y is 3, 4 or 5, such that the sum of n and m is less than y; X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X can also be an azido, isocyanate, thiocyanate, isothiocyanate or cyano. For the purposes of the present invention, those skilled in the art will recognize that the terms alkoxy and aryloxy are structural equivalents of alkoxide and phenolate, respectively. The term "arylalkoxy" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the alkoxy position. The term "alkylaryl" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the aryloxy position. Non-limiting examples of these Lewis acids include tetrachloromethoxyantimony, dimethoxyantimony trichloride, dichloromethoxyarsine, chlorodimethoxyarsine and difluoromethoxyarsine. The Group 15 Lewis acids useful in the present invention can also have the general formula M (RC = OO) n R' m X y-(m+n) ; wherein M is a Group 15 metal; wherein RC=OO is a monovalent hydrocarbon acyloxy group selected from the following: C1-C 30 Alkacyloxy, C7-C 30 Aryl acyloxy, C7-C 30 Arylalkyl acyloxy, C7-C 30 Alkyl aryl acyloxy group; R' is a monovalent hydrocarbon group selected from the following: C1-C 12 Alkyl, C6-C 10 Aryl, C7-C 14 Arylalkyl and C7-C 14Alkyl aryl groups; n is an integer from 0 to 4 and m is an integer from 0 to 4 and y is 3, 4 or 5, so that the sum of n and m is less than y; X is a halogen independently selected from fluorine, chlorine, bromine and iodine, preferably chlorine. X can also be an azido, isocyanate, thiocyanate, isothiocyanate or cyano. The term "arylalkyl acyloxy" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the alkyl acyloxy position. The term "alkyl aryl acyloxy" refers to a group comprising an aliphatic structure and an aromatic structure, the group being in the aryl acyloxy position. Non-limiting examples of these Lewis acids include acetate antimony tetrachloride, (benzoate) antimony tetrachloride and bismuth chloroacetate.
[0170] In the context of the present invention, Lewis acids such as methylaluminoxane (MAO) and specifically designed weakly coordinating Lewis acids such as B(C6F5)3 are also suitable Lewis acids.
[0171] Weakly coordinating Lewis acids are disclosed in detail in paragraphs
[117] to
[129] of WO 2004 / 067577 A, which is incorporated herein by reference.
[0172] Initiator
[0173] Initiators useful in the present invention are those that are capable of coordinating with the selected Lewis acid to produce a complex that reacts with the monomer to form a growing polymer chain.
[0174] In a preferred embodiment, the initiator includes at least one compound selected from the group consisting of water, hydrogen halides, carboxylic acids, carboxylic acid halides, sulfonic acids, sulfonyl halides, alcohols (e.g., primary, secondary, and tertiary alcohols), phenols, tertiary alkyl halides, tertiary aralkyl halides, tertiary alkyl esters, tertiary aralkyl esters, tertiary alkyl ethers, tertiary aralkyl ethers, alkyl halides, aryl halides, alkylaryl halides, and arylalkyl acyl halides.
[0175] Preferred hydrogen halide initiators include hydrogen chloride, hydrogen bromide and hydrogen iodide. A particularly preferred hydrogen halide is hydrogen chloride.
[0176] Preferred carboxylic acids include aliphatic carboxylic acids and aromatic carboxylic acids. Examples of carboxylic acids that can be used in the present invention include acetic acid, propionic acid, butyric acid; cinnamic acid, benzoic acid, 1-chloroacetic acid, dichloroacetic acid, trichloroacetic acid, trifluoroacetic acid, p-chlorobenzoic acid and p-fluorobenzoic acid. Particularly preferred carboxylic acids include trichloroacetic acid, trifluoroacetic acid and p-fluorobenzoic acid.
[0177] The carboxylic acid halides that can be used in the present invention are structurally similar to carboxylic acids, wherein the OH of the acid is replaced by a halide. The halide can be fluoride, chloride, bromide or iodide, with chloride being preferred.
[0178] The carboxylic acid halides that can be used in the present invention include acetyl chloride, acetyl bromide, cinnamoyl chloride, benzoyl chloride, benzoyl bromide, trichloroacetyl chloride, trifluoroacetyl chloride, trifluoroacetyl chloride and p-fluorobenzoyl chloride. Particularly preferred acyl halides include acetyl chloride, acetyl bromide, trichloroacetyl chloride, trifluoroacetyl chloride and p-fluorobenzoyl chloride.
[0179] Sulfonic acids which can be used as initiators in the present invention include aliphatic sulfonic acids and aromatic sulfonic acids. Examples of preferred sulfonic acids include methanesulfonic acid, trifluoromethanesulfonic acid, trichloromethanesulfonic acid and p-toluenesulfonic acid.
[0180] Sulfonyl halides that can be used for the present invention are similar in structure to sulfonic acid, wherein the OH of the parent acid is replaced by a halide. The halide can be a fluoride, chloride, bromide or iodide, wherein chloride is preferred. It is known in the prior art that sulfonyl halides are prepared by the parent sulfonic acid and those skilled in the art should be familiar with these methods. Preferred sulfonyl halides that can be used for the present invention include methanesulfonyl chloride, methanesulfonyl bromide, trichloromethanesulfonyl chloride, trifluoromethanesulfonyl chloride and p-toluenesulfonyl chloride.
[0181] Alcohols useful in the present invention include methanol, ethanol, propanol, 2-propanol, 2-methylpropan-2-ol, cyclohexanol, and benzyl alcohol.
[0182] Phenols that can be used in the present invention include phenol, 2-methylphenol, 2,6-dimethylphenol, p-chlorophenol, p-fluorophenol, 2,3,4,5,6-pentafluorophenol and 2-hydroxynaphthalene.
[0183] In addition to the above compounds, the initiator system may also contain oxygen- or nitrogen-containing compounds to further influence or enhance the activity.
[0184] Such compounds include ethers, amines, N-heteroaromatics, ketones, aldehydes, sulfones and sulfoxides and also carboxylic acid esters and carboxylic acid amides.
[0185] The ethers include methyl ethyl ether, diethyl ether, di-n-propyl ether, tert-butyl methyl ether, di-n-butyl ether, tetrahydrofuran, dioxane, anisole or phenetole.
[0186] Amines include n-pentylamine, N,N-diethylmethylamine, N,N-dimethylpropylamine, N-methylbutylamine, N,N-dimethylbutylamine, N-ethylbutylamine, hexylamine, N-methylhexylamine, N-butylpropylamine, heptylamine, 2-aminoheptane, 3-aminoheptane, N,N-dipropylethylamine, N,N-dimethylhexylamine, octylamine, aniline, benzylamine, N-methylaniline, phenethylamine, N-ethylaniline, 2,6-diethylaniline, amphetamine, N-propylaniline, phenbutylamine, N-butylaniline, N,N-diethylaniline, 2,6-diethylaniline, diphenylamine, piperidine, N-methylpiperidine and triphenylamine.
[0187] N-heteroaromatic compounds include pyridine, 2-, 3- or 4-methylpyridine, lutidine, vinylpyridine and 3-methyl-2-phenylpyridine.
[0188] Ketones include acetone, butanone, pentanone, hexanone, cyclohexanone, 2,4-hexanedione, acetylacetone, and acetonylacetone.
[0189] Aldehydes include formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde and 2-ethylhexanal.
[0190] Sulfones and sulfoxides include dimethyl sulfoxide, diethyl sulfoxide and sulfolane.
[0191] Carboxylic acid esters include methyl acetate, ethyl acetate, vinyl acetate, propyl acetate, allyl acetate, benzyl acetate, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, dimethyl maleate, diethyl maleate, dipropyl maleate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, allyl benzoate, butylene benzoate, benzyl benzoate, phenylethyl benzoate, dimethyl phthalate, diethyl phthalate, dipropyl phthalate, dibutyl phthalate, dipentyl phthalate, dihexyl phthalate, diheptyl phthalate, and dioctyl phthalate.
[0192] The carboxylic acid amides include N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide and N,N-diethylacetamide.
[0193] Preferred tertiary alkyl and aralkyl initiators include tertiary compounds represented by the formula: wherein X is a halogen, pseudohalogen, ether or ester, or a mixture thereof, preferably a halogen, preferably chlorine, and R1, R2 and R3 are independently any linear, cyclic or branched alkyl, aryl or arylalkyl, preferably containing 1 to 15 carbon atoms and more preferably containing 1 to 8 carbon atoms. n is the number of initiator sites and is a number greater than or equal to 1, preferably between 1 and 30, more preferably n is a number from 1 to 6. Arylalkyl may be substituted or unsubstituted. For purposes of the present invention and any claims thereto, arylalkyl is defined to mean a compound containing an aromatic structure and an aliphatic structure. Preferred examples of the initiator include 2-chloro-2,4,4-trimethylpentane, 2-bromo-2,4,4-trimethylpentane, 2-chloro-2-methylpropane, 2-bromo-2-methylpropane, 2-chloro-2,4,4,6,6-pentamethylheptane, 2-bromo-2,4,4,6,6-pentamethylheptane, 1-chloro-1-methylethylbenzene, 1-chloroadamantane, 1-chloroethylbenzene, 1,4-bis(1-chloro-1-methylethyl)benzene, 1-Acetoxy-2,4,4-trimethylpentane, 2-benzoyloxy-2,4,4-trimethylpentane, 2-acetoxy-2-methylpropane, 2-benzoyloxy-2-methylpropane, 2-acetoxy-2,4,4,6,6-pentamethylheptane, 2-benzoyloxy-2,4,4,6,6-pentamethylheptane, 1 ... Acyloxy-1-methylethylbenzene, 1-acetoxyadamantane, 1-benzoyloxyethylbenzene, 1,4-bis(1-acetoxy-1-methylethyl)benzene, 5-tert-butyl-1,3-bis(1-acetoxy-1-methylethyl)benzene, 2-methoxy-2,4,4-trimethylpentane, 2-isopropoxy-2,4,4-trimethylpentane, 2-methoxy-2-methylpropane, 2-benzyloxy-2-methylpropane, 2-methoxy-2,4,4,6,6-pentamethylheptane, 2-isopropoxy-2,4,4,6,6-pentamethylheptane, 1-methoxy-1-methylethylbenzene, 1-methoxyadamantane, 1-methoxyethylbenzene, 1,4-bis(1-methoxy-1-methylethyl)benzene, 5-tert-butyl-1,3-bis(1-methoxy-1-methylethyl)benzene, and 1,3,5-tris(1-chloro-1-methylethyl)benzene. Other suitable initiators can be found in U.S. Pat. No. 4,946,899. For purposes of the present invention and the claims thereto, a pseudohalogen is defined as any compound that is an azide, an isocyanate, a thiocyanate, an isothiocyanate, or a cyanide.
[0194] Another preferred initiator is a polymeric halide, one of R1, R2 or R3 is an olefin polymer, and the remaining R groups are as defined above. Preferred olefin polymers include polyisobutylene, polypropylene and polyvinyl chloride. The polymerization initiator can have a halogenated tertiary carbon at the chain end or along the polymer backbone or in the position in the polymer backbone. When the olefin polymer has multiple halogen atoms at the tertiary carbon (in the side chain of the polymer backbone or in the polymer backbone), the product can include a polymer with a comb-like structure and / or side chain branches, depending on the number and position of the halogen atoms in the olefin polymer. Similarly, a method for preparing a product that can contain block polyisobutylene is provided using a chain end tertiary polymer halide initiator.
[0195] Particularly preferred initiators may be any initiator useful for the cationic polymerization of isobutylene polyisobutylene, including: water, hydrogen chloride, 2-chloro-2,4,4-trimethylpentane, 2-chloro-2-methylpropane, 1-chloro-1-methylethylbenzene, and methanol.
[0196] Initiator systems useful in the present invention may also comprise a composition comprising a reactive cation and a weakly coordinating anion ("WCA") as defined above.
[0197] The preferred molar ratio of Lewis acid to initiator is generally from 1:5 to 100:1, preferably from 5:1 to 100:1, more preferably from 8:1 to 20:1.
[0198] The initiator system comprising the Lewis acid and the initiator is preferably present in the reaction mixture in an amount of 0.002 to 5.0% by weight, preferably 0.1 to 0.5% by weight, based on the weight of the monomers used.
[0199] In another embodiment, in particular when aluminum chloride is used, the weight ratio of monomer used to Lewis acid (in particular aluminum chloride) is in the range of 500 to 20,000, preferably 1,500 to 10,000.
[0200] In one embodiment, at least one control agent for the initiator system is used. Control agents help control the activity and thus help adjust the properties, especially the molecular weight of the desired copolymer, see for example US 2,580,490 and US 2,856,394.
[0201] Suitable control agents include ethylene, mono- or di-substituted C3-C 20 Monoalkene, wherein substitution is intended to denote an alkyl group bonded to the double bond of the olefin. Preferred control agents are monosubstituted C3-C 20 Monoolefins (also called primary olefins), more preferably the control agent is (C3-C 20)-1-ene, such as 1-butene. The above-mentioned control agent ethylene, monosubstituted or disubstituted C3-C 20 The monoolefins are generally used in an amount of 0.01 to 20% by weight, based on the monomers used in step a), preferably 0.2 to 15% by weight and more preferably 1 to 15% by weight.
[0202] The polymerization can optionally be carried out in the presence of at least one chain regulator, which is generally an ethylenically unsaturated system and contains one or more tertiary olefin carbon atoms, optionally in addition to one or more primary and / or secondary olefin carbon atoms. Typically, such chain regulators are monoethylenically or polyethylenically unsaturated hydrocarbons having 6 to 30, in particular 6 to 20 and in particular 6 to 16 carbon atoms; their structure can be open-chain or cyclic. Typical representatives of such chain regulators are diisobutene, triisobutene, tetraisobutene and 1-methylcyclohexene. In a preferred embodiment, diisobutene is used as chain regulator. Diisobutene (isooctenes) is generally understood to mean an isomer mixture of 2,4,4-trimethyl-1-pentene and 2,4,4-trimethyl-2-pentene; the 2,4,4-trimethyl-1-pentene and 2,4,4-trimethyl-2-pentene isomers used individually can of course also be used as chain regulators. By means of the amount of chain regulator used according to the invention, the molecular weight of the isobutene homopolymer obtained can be adjusted in a simple manner: the higher the amount of chain regulator, the lower the molecular weight will generally be. Chain regulators generally control the molecular weight by incorporating into the polymer chain at an early or late stage and thus leading to chain termination at this point.
[0203] In another embodiment, 2-methyl-2-butene is used as chain regulator.
[0204] The chain regulators are generally used in an amount of 0.001 to 3% by weight, based on the monomers used in step a), preferably in an amount of 0.01 to 2% by weight and more preferably in an amount of 0.01 to 1.5% by weight.
[0205] In another embodiment, isoprene (2-methyl-1,3-butadiene) is used as a chain regulator in an amount of 0.001 to 0.35 wt %, preferably 0.01 to 0.2 wt %. Another preferred suitable control agent includes diisobutylene. As used herein, the term diisobutylene means 2,4,4-trimethylpentene, i.e., 2,4,4-trimethyl-1-pentene or 2,4,4-trimethyl-2-pentene or any mixture thereof, in particular a commercially available mixture of 2,4,4-trimethyl-1-pentene and 2,4,4-trimethyl-2-pentene in a ratio of about 3:1. For ethylene, mono- or di-substituted C3-C 20Monoolefins, diisobutylene may alternatively or additionally be used. Diisobutylene is generally used in an amount of 0.001 to 3% by weight, based on the monomers used in step a), preferably in an amount of 0.01 to 2% by weight and more preferably in an amount of 0.01 to 1.5% by weight.
[0206] In cases where lower conversions are desired in the process, additives may also be used to "poison" the reaction. This results in a lower conversion of the monomers being polymerized. Examples of such inhibitors are straight chain olefins such as straight chain C3-C 20 By controlling the separate addition of chain transfer agents such as diisobutylene and inhibitors such as linear olefins, molecular weight and reaction conversion can be adjusted essentially independently.
[0207] It will of course be understood that greater or lesser amounts of initiator are still within the scope of the present invention.
[0208] In one particularly preferred initiator system, the Lewis acid is ethylaluminum sesquichloride, which is preferably formed by mixing equimolar amounts of diethylaluminum chloride and ethylaluminum dichloride, preferably in a diluent. The diluent is preferably the same as the diluent used to carry out the polymerization reaction.
[0209] In the case of using alkylaluminum halides, water and / or alcohols, preferably water, are used as proton sources. In one embodiment, the amount of water is in the range of 0.40 to 4.0 moles of water / mole of aluminum in the alkylaluminum halide, preferably in the range of 0.5 to 2.5 moles of water / mole of aluminum in the alkylaluminum halide, and most preferably 1 to 2 moles of water / mole of aluminum in the alkylaluminum halide.
[0210] When using aluminum halides, in particular aluminum trichloride, water and / or alcohols, preferably water, are used as proton sources.
[0211] In one embodiment, the amount of water is in the range of 0.05 to 2.0 moles of water per mole of aluminum in the aluminum halide, preferably in the range of 0.1 to 1.2 moles of water per mole of aluminum in the aluminum halide.
[0212] Aggregation conditions
[0213] In one embodiment, the organic diluent and isobutylene used are substantially free of water. As used herein, substantially free of water is defined as less than 50 ppm, preferably less than 30 ppm, more preferably less than 20 ppm, even more preferably less than 10 ppm, and even more preferably less than 5 ppm based on the total weight of the reaction medium.
[0214] The person skilled in the art knows that the water content of the organic diluent and the isobutylene must be low to ensure that the initiator system is not affected by additional amounts of water which are not added for the purpose of, for example, acting as an initiator.
[0215] Step a) and / or b) can be carried out in a continuous process or in a batch process, with the continuous process being preferred.
[0216] In one embodiment of the invention, the polymerization of step b) is carried out using a polymerization reactor. Suitable reactors are those known to those skilled in the art, including straight-through polymerization reactors, plug flow reactors, stirred tank reactors, conveyor belt reactors or conveyor drum reactors, jet reactors or nozzle reactors, tubular reactors and self-refrigerated boiling pool reactors. Specific suitable examples are disclosed in WO 2011 / 000922 A and WO2012 / 089823A.
[0217] In one embodiment, the polymerization of step b) is carried out in the presence of the initiator system, isobutylene and the organic diluent in a single phase. Preferably, the polymerization is carried out in a continuous polymerization process in which the initiator system, the monomers and the organic diluent are present in a single phase.
[0218] Depending on the choice of the organic diluent, the polymerization in step b) is carried out as a slurry polymerization or a solution polymerization.
[0219] In a slurry polymerization, the isobutylene and initiator system are typically soluble in the diluent or diluent mixture, i.e., constitute a single phase, and the polyisobutylene, once formed, precipitates out of the organic diluent. Ideally, reduced or no polymer "swelling" is exhibited, as indicated by little or no Tg depression of the polymer and / or little or no mass absorption of the organic diluent.
[0220] In solution polymerization, the monomers, initiator system and polymer are generally all soluble in the diluent or diluent mixture, ie, constitute a single phase, so that polyisobutylene is formed during the polymerization.
[0221] The solubility of the desired polymer in the abovementioned organic diluents and its swelling behavior under the reaction conditions are well known to those skilled in the art.
[0222] The advantages and disadvantages of solution polymerization versus slurry polymerization are extensively discussed in the literature and are therefore known to those skilled in the art.
[0223] In one embodiment, step b) is carried out at a temperature in the range of -110°C to 20°C, preferably in the range of -100°C to -50°C and even more preferably in the range of -100°C to -70°C.
[0224] In a preferred embodiment, the polymerization temperature is within 20°C above the solidification point of the organic diluent, preferably within 10°C above the solidification point of the organic diluent.
[0225] The reaction pressure in step b) is generally from 100 to 100,000 hPa, preferably from 200 to 20,000 hPa, more preferably from 500 to 5,000 hPa.
[0226] The polymerization of step b) is generally carried out in such a way that the solids content of the slurry in step b) is preferably in the range of 1 to 45 wt.-%, more preferably 3 to 40 wt.-%, even more preferably 15 to 40 wt.-%.
[0227] As used herein, the term "solids content" or "solids level" refers to the weight percentage of polyisobutylene obtained according to step b) (i.e. in the polymerization) and present in the medium obtained according to step b), said medium comprising polyisobutylene, organic diluent and optionally residual monomers.
[0228] In one embodiment, the reaction time in step b) is from 2 min to 2 h, preferably from 10 min to 1 h and more preferably from 20 to 45 min.
[0229] The process can be carried out batchwise or continuously. In the case of a continuous reaction, the reaction times given above represent average residence times.
[0230] In one embodiment, the reaction is stopped by a quencher, such as a 1 wt % sodium hydroxide solution in water, methanol or ethanol.
[0231] In another embodiment, the reaction is quenched by contacting with an aqueous medium in step A), which in one embodiment may have a pH of 5 to 10, preferably 6 to 9 and more preferably 7 to 9 measured at 20°C and 1013 hPa.
[0232] If necessary, pH adjustment can be carried out by adding acidic or basic compounds which preferably do not contain polyvalent metal ions. pH adjustment to higher pH values can be carried out, for example, by adding sodium hydroxide or potassium hydroxide.
[0233] In particular, for solution polymerization, the conversion is generally stopped after the monomer consumption is 5 to 25% by weight, preferably 10 to 20% by weight, of the monomer initially used.
[0234] During polymerization, monomer conversion can be followed by online viscometry or spectroscopic monitoring.
[0235] In step A), an organic medium, e.g. the organic medium obtained according to step b), is contacted with an aqueous medium and the organic diluent is at least partially removed to obtain an aqueous slurry comprising a plurality of polyisobutylene particles, the aqueous medium comprising at least one LCST compound having a cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 70°C.
[0236] The contacting can be carried out in any vessel suitable for this purpose. In industry, such contacting is usually carried out in a flash tank or any other vessel known for separating liquid phases or vapors.
[0237] During step A), the organic diluent is at least partially removed to obtain an aqueous slurry comprising polyisobutylene particles.
[0238] Removal of the organic diluent may also use other types of distillation to subsequently or together remove residual monomers and the organic diluent to the desired extent. Distillation methods for separating liquids of different boiling points are well known in the art and are described, for example, in Encyclopedia of Chemical Technology, Kirk Othmer, 4th edition, pages 8-311, which is incorporated herein by reference. Typically, the organic diluent may be recycled to step a) of the polymerization reaction alone or together.
[0239] The pressure in step A and in one embodiment in the steam-stripper or flash tank depends on the organic diluent and, where applicable, the isobutene used in step b), but is generally in the range from 100 to 5000 hPa.
[0240] The temperature in step A) is selected to be sufficient to remove the organic diluent at least partially and to such an extent that residual isobutene is still present.
[0241] In one embodiment, the temperature is from 10 to 100°C, preferably from 50 to 100°C, more preferably from 60 to 95°C and even more preferably from 75 to 95°C.
[0242] Once the organic medium is contacted with the aqueous medium comprising at least one LCST compound, the medium is destabilized due to the removal of the stabilizing organic diluent and, in some cases, particularly where the temperature of the organic medium is below the glass transition temperature of the polyisobutylene, is typically rapidly heated to above the glass transition temperature of the polyisobutylene, thereby forming polyisobutylene particles suspended in the aqueous slurry.
[0243] Where slurry polymerization is used, the polyisobutylene, once formed, is precipitated from the organic diluent to form a fine suspension of primary particles. In one embodiment, 80% or more of the primary particles are from about 0.1 to about 800 μm in size, preferably from about 0.25 to about 500 μm.
[0244] Upon contact with an aqueous medium comprising at least one LCST compound, an aqueous slurry of polyisobutylene particles is formed. During the slurry polymerization, the primary particles obtained agglomerate to form (larger, secondary) polyisobutylene particles as described elsewhere. In a preferred embodiment, this formation and removal of the diluent is carried out within a time frame of 0.1 s to 30 s, preferably within 0.5 to 10 s.
[0245] In one embodiment, the removal of the organic diluent is carried out within a time range of 0.1 s to 30 s, preferably within 0.5 to 10 s, so that the aqueous slurry contains less than 10 wt.-% of organic diluent, preferably less than 7 wt.-% and even more preferably less than 5 wt.-% and still even more preferably less than 3 wt.-% and still even more preferably less than 1 wt.-% of organic diluent, calculated on the basis of the polyisobutylene contained in the polyisobutylene particles of the obtained aqueous slurry.
[0246] It will be apparent to one skilled in the art that the amount of energy to be introduced into the mixture of aqueous and organic media (e.g., per liter of organic medium) to compensate for heating from the polymerization temperature to the boiling point of the organic diluent, the heat of vaporization of the organic diluent, and heating to the desired final slurry temperature depends on the level of polyisobutylene present in the organic medium, the type of solvent, the starting temperature, and the rate of addition.
[0247] In one embodiment, steam, such as saturated steam or superheated steam, is preferably introduced in step A).
[0248] In another preferred embodiment, this increase in the reaction mixture is carried out within the above-mentioned time range of 0.1 s to 30 s, preferably within 0.5 to 10 s.
[0249] The contact of the organic medium with the aqueous medium is carried out in a countercurrent or cocurrent manner in a suitable device. Preferably, the contact is carried out in a mixing circuit, a mixing pump, a jet mixing device, a coaxial mixing nozzle, a Y-mixer, a T-mixer and a vortex impinging-jet mixing structure.
[0250] Another result, according to the observations of the applicant, without being bound by theory, is that it was previously observed that at least the LCST compound used for conventional anti-agglomeration agents such as calcium stearate, the aqueous medium comprising at least one LCST compound is depleted of the LCST compound, so that in the final aqueous slurry, at least part, according to the observations disclosed in the experimental part even a considerable part of the LCST compound forms part of the polyisobutylene particles and is presumably bound to the surface of the polyisobutylene particles, which results in an excellent anti-agglomeration effect.
[0251] Suitable LCST compounds are, for example, selected from:
[0252] Poly(N-isopropylacrylamide); poly(N-isopropylacrylamide-co-N,N-dimethylacrylamide); poly(N-isopropylacrylamide)-alt-2-hydroxyethyl methacrylate; poly(N-vinylcaprolactam); poly(N,N-diethylacrylamide); poly[2-(dimethylamino)ethyl methacrylate]; poly(2-oxazoline)glypolyisobutylenes; poly(3-ethyl-N-vinyl-2-pyrrole alkylone); hydroxybutyl chitosan; polyoxyethylene (20) sorbitan monostearate; polyoxyethylene (20) sorbitan monolaurate; polyoxyethylene (20) sorbitan monooleate; methylcellulose; hydroxypropyl cellulose; hydroxyethyl methylcellulose; hydroxypropyl methylcellulose; poly(ethylene glycol) methacrylate having 2 to 6 ethylene glycol units; polyethylene glycol-co-polypropylene glycol, preferably those having 2 to 6 ethylene glycol units and 2 to 6 polypropylene units; compounds of formula (I) (I) HO-[-CH2-CH2-O] x -[-CH(CH3)-CH2-O] y -[-CH2-CH2-O] z -H
[0253] wherein y=3 to 10 and x and z=1 to 8, wherein y+x+z is 5 to 18;
[0254] Polyethylene glycol-co-polypropylene glycol, preferably those having 2 to 8 ethylene glycol units and 2 to 8 polypropylene units; ethoxylated iso-C 13 H 27-alcohols, preferably with a degree of ethoxylation of 4 to 8; polyethylene glycols having 4 to 50, preferably 4 to 20 ethylene glycol units; polypropylene glycols having 4 to 30, preferably 4 to 15 propylene glycol units; polyethylene glycol monomethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol monoethyl ether and polyethylene glycol diethyl ether having 4 to 50, preferably 4 to 20 ethylene glycol units; polypropylene glycol monomethyl ether, polypropylene glycol dimethyl ether, polypropylene glycol monoethyl ether and polypropylene glycol diethyl ether having 4 to 50, preferably 4 to 20 propylene glycol units; wherein in another embodiment, the above LCST compound further comprises hydroxyethyl cellulose, and wherein methyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose and hydroxypropyl methyl cellulose are preferred. In one embodiment, at least one LCST compound is selected from alkyl celluloses, hydroxyalkyl celluloses and hydroxyalkyl alkyl celluloses.
[0255] In another embodiment, at least one LCST compound is cellulose, wherein at least one hydroxyl functional group -OH is functionalized to form one of the following groups:
[0256] OR c , where R c is methyl, 2-hydroxyethyl, 2-methoxyethyl, 2-methoxypropyl, 2-hydroxypropyl, -(CH2-CH2O) n H, -(CH2-CH2O) n CH3, -(CH2-CH(CH3)O) n H, -(CH2-CH(CH3)O) n CH3, wherein n is an integer from 1 to 20, preferably from 3 to 20.
[0257] According to another aspect of the present invention, there is provided a method for preparing an aqueous slurry comprising a plurality of polyisobutylene particles suspended therein, the method comprising at least the following steps:
[0258] A) bringing the organic medium into contact with the aqueous medium,
[0259] The organic medium comprises
[0260] i) polyisobutylene, and
[0261] ii) organic diluent,
[0262] The aqueous medium comprises at least one compound selected from the group consisting of: alkyl cellulose, hydroxyalkyl cellulose, hydroxyalkyl alkyl cellulose, carboxyalkyl cellulose, or a mixture thereof;
[0263] The organic diluent is at least partially removed to obtain an aqueous slurry containing polyisobutylene particles.
[0264] In one embodiment, in the cellulose compound, at least one hydroxyl functional group -OH of the cellulose is functionalized to form one of the following groups:
[0265] OR c , where R c is methyl, 2-hydroxyethyl, 2-methoxyethyl, 2-methoxypropyl, 2-hydroxypropyl, -(CH2-CH2O) n H, -(CH2-CH2O) n CH3, -(CH2-CH(CH3)O) n H, -(CH2-CH(CH3)O) n CH3, wherein n is an integer from 1 to 20, preferably from 3 to 20, more preferably from 4 to 20, and
[0266] The organic diluent is at least partially removed to obtain an aqueous slurry containing polyisobutylene particles.
[0267] Alkylcellulose is an alkyl ether of cellulose, such as a C1-C4 alkyl ether of cellulose, in particular a C1-C2 alkyl ether of cellulose. Examples of alkylcelluloses are methylcellulose and ethylcellulose. In one embodiment, the degree of substitution of these alkylcelluloses is between 1.2 and 2.0.
[0268] Hydroxyalkylcelluloses are alkylcelluloses with at least one additional hydroxyl functional group in the alkyl group, such as hydroxyethylcellulose or hydroxypropylcellulose. In hydroxyalkylcelluloses, the hydroxyl groups may also be substituted by ethylene glycol or propylene glycol groups. Typically, the number of moles of substitution (MS) of ethylene glycol or propylene glycol units per hydroxyl group is between 1 and 20. Examples of hydroxyalkylcelluloses are hydroxyethylcellulose or hydroxypropylcellulose, etc., just mentioned above.
[0269] Hydroxyalkyl alkylcellulose is an alkylcellulose in which the alkyl moiety carries at least one additional hydroxyl function in the alkyl group. Examples include hydroxypropyl methylcellulose and hydroxyethyl methylcellulose. In this context, the number of moles of substitution (MS) of ethylene glycol or propylene glycol units per hydroxyl group is between 1 and 20.
[0270] Carboxyalkylcelluloses are alkylcelluloses which carry at least one additional carboxyl (COOH) function in the alkyl group, for example carboxymethylcellulose.
[0271] In one embodiment, the degree of substitution of methylcellulose, hydroxypropylcellulose, hydroxyethylmethylcellulose and hydroxypropylmethylcellulose is from 0.5 to 2.8 (theoretical maximum is 3), preferably from 1.2 to 2.5 and more preferably from 1.5 to 2.0.
[0272] In one embodiment, hydroxypropyl cellulose, hydroxyethyl methyl cellulose and hydroxypropyl methyl cellulose have an MS (moles of substitution) of 3 or more, preferably 4 or more, more preferably 4 to 20, relative to ethylene glycol or propylene glycol groups per glucose unit.
[0273] The amount of LCST compound present in the aqueous medium used in step A) is, for example, 1 to 20,000 ppm, preferably 3 to 10,000 ppm, more preferably 5 to 5,000 ppm and even more preferably 10 to 5,000 ppm, relative to the amount of polyisobutene present in the organic medium.
[0274] In one embodiment, the molecular weight of the LCST compound is at least 1,500 g / mol, preferably at least 2,500 g / mol and more preferably at least 4,000 g / mol.
[0275] In case a mixture of different LCST compounds is used, the weight average molecular weight is, for example, 1,500 to 3,000,000, 1,500 to 2,600,000, 1,500 to 2,000,000.
[0276] In one embodiment of the present invention, the process according to the invention does not allow the presence of polycarboxylic acids.
[0277] The unique ability of LCST compounds to stabilize polyisobutylene particles in aqueous solution is the main discovery of the present invention. Therefore, the present invention also includes a method for preventing or reducing or slowing down agglomeration of a slurry comprising polyisobutylene particles suspended in an aqueous medium by adding or using a LCST compound having a cloud point of 0 to 100° C., preferably 5 to 100° C., more preferably 15 to 80° C. and even more preferably 20 to 70° C.
[0278] For the avoidance of doubt, it should be noted that the aqueous slurry obtained in step A) is distinct from and unrelated to the polymeric slurry which may be obtained in step b) in some of the embodiments described.
[0279] In the case where step b) is carried out as a solution polymerization, upon contact with water, the organic diluent evaporates and the polyisobutene forms polyisobutene particles suspended in an aqueous slurry.
[0280] The at least partial removal of the organic diluent generally requires a large amount of heat to balance the heat of evaporation, which heat can be provided, for example, by heating the vessel, in which step A) is carried out externally or in a preferred embodiment additionally or alternatively by introducing steam, which also assists in the removal of the organic diluent and to the extent that it is still present after the polymerization of the isobutene (stripping).
[0281] Step A) can be carried out batchwise or continuously, with continuous operation being preferred.
[0282] In one embodiment, the temperature of the resulting slurry obtained in step A) is from 50 to 100 °C, preferably from 60 to 100 °C, more preferably from 70 to 95 °C and even more preferably from 75 to 95 °C.
[0283] In one embodiment, it has even been found that the temperature of step A) does not have to be higher than the highest measured cloud point of the at least one LCST compound used.
[0284] The highest measured turbidity point means the highest turbidity point measured with 5 methods as disclosed above or with 3 methods as disclosed above in another embodiment. If the turbidity point cannot be determined with one or two methods for whatever reason, the highest turbidity point determined by the other methods is taken as the highest measured turbidity point.
[0285] In one embodiment, the removal of the organic diluent is carried out until the aqueous slurry contains less than 10 wt.-% of organic diluent, calculated on the polyisobutylene contained in the polyisobutylene particles of the resulting aqueous slurry, preferably less than 7 wt.-% and even more preferably less than 5 wt.-% and still even more preferably less than 3 wt.-%.
[0286] It was not previously known and is quite surprising that an aqueous slurry comprising a plurality of polyisobutylene particles is obtainable at all in the presence of very low levels or even in the absence of an anti-agglomerating agent selected from carboxylates of monovalent or multivalent metal ions and layered minerals.
[0287] The present invention therefore also encompasses the use of LCST compounds having a cloud point of 0 to 100° C., preferably 5 to 100° C., more preferably 15 to 80° C. and even more preferably 20 to 70° C. as antiagglomeration agents, in particular for the defined polyisobutylene particles.
[0288] Therefore, the present invention also comprises the aqueous slurry disclosed above and obtainable according to step A) itself.
[0289] The aqueous slurry obtained according to step A) serves as the ideal starting material for obtaining the polyisobutene particles in isolated form.
[0290] Thus, in a further step C), the polyisobutene particles contained in the aqueous slurry obtained according to step B) can be separated to obtain polyisobutene particles.
[0291] The separation may be performed by screening, flotation, centrifugation, filtration, dewatering in a dewatering extruder, or by any other means known to those skilled in the art for separating solids from fluids.
[0292] In one embodiment, the separated aqueous medium is recycled to step A) if necessary after replacement of the LCST compound, water and optionally further components removed together with the polyisobutene particles.
[0293] In a further step D), the polyisobutene granules obtained according to step C) are dried, preferably to a residual content of volatiles of 7,000 or less, preferably 5,000 or less, even more preferably 4,000 or less, and in another embodiment to 2,000 ppm or less, preferably 1,000 ppm or less.
[0294] As used herein, the term volatiles refers to compounds having a boiling point below 250°C, preferably 200°C or less at standard pressure, including water and residual organic diluent.
[0295] Drying can be carried out using conventional means known to those skilled in the art, including drying on a heated wire conveyor belt.
[0296] Depending on the drying method, the polyisobutylene granules can also be produced in different shapes—referred to below as reshaped polyisobutylene granules.
[0297] The reshaped polyisobutylene particles are, for example, pellets. Such reshaped polyisobutylene particles are also included in the present invention and are obtained, for example, by drying in an extruder and subsequent pelletizing at the extruder outlet. This pelletizing process can also be carried out underwater. The process of the present invention allows the preparation of polyisobutylene particles and polyisobutylene products with adjustable or, if desired, unprecedented low levels of monovalent and polyvalent metal ions.
[0298] Thus, the present invention includes polyisobutylene particles and reshaped polyisobutylene particles having a polyisobutylene content of 98.5 wt % or more, preferably 98.8 wt % or more, more preferably 99.0 wt % or more, even more preferably 99.2 wt % or more, still even more preferably 99.4 wt % or more, and in another embodiment 99.5 wt % or more, preferably 99.7 wt % or more.
[0299] In one embodiment, the (reshaped) polyisobutylene particles and polyisobutylene products contain 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of salts of monovalent or polyvalent metal ions, and in another yet even more preferred embodiment, 100 ppm or less of salts of monovalent or polyvalent metal ions, calculated as the metal content and relative to the amount of polyisobutylene present in the organic medium.
[0300] In one embodiment, the (reshaped) polyisobutylene particles contain 5000 ppm or less, preferably 2000 ppm or less, more preferably 1000 ppm or less, even more preferably 500 ppm or less and still even more preferably 100 ppm or less of non-LCST compounds, and in another yet even more preferred embodiment contain 50 ppm or less, preferably 50 ppm or less, more preferably 10 ppm or less and still even more preferably contain no non-LCST compounds selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents.
[0301] On the other hand, the present invention provides (reshaped) polyisobutylene particles which comprise a salt of a polyvalent metal ion in an amount of 500 ppm or less, preferably 400 ppm or less, more preferably 250 ppm or less, even more preferably 150 ppm or less and yet even more preferably 100 ppm or less, and in an even more preferred embodiment 50 ppm or less, calculated on the metal content.
[0302] The (reshaped) copolymer particles of the invention may also comprise an antioxidant, for example at least one of the antioxidants listed above.
[0303] Particularly preferred is pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid (also known as 1010) and 2,6-di-tert-butyl-4-methyl-phenol (BHT).
[0304] The amount of antioxidant in the (reshaped) copolymer particles is, for example, from 50 ppm to 1000 ppm, preferably from 80 ppm to 500 ppm, and in another embodiment from 300 ppm to 700 ppm.
[0305] Typically, the remainder up to 100 wt % comprises the LCST compound, volatiles, to the extent used in the presence of all the salts of the multivalent metal ions and low levels of residual monovalent metal ion salts such as sodium chloride.
[0306] In one embodiment, the amount of LCST compounds present in the polyisobutylene particles and reshaped polyisobutylene particles is from 1 ppm to 18,000 ppm, preferably from 1 ppm to 10,000 ppm, more preferably from 1 ppm to 5,000 ppm, even more preferably from 1 ppm to 2,000 ppm, and in a more preferred embodiment, from 5 to 1,000 ppm or from 5 to 500 ppm.
[0307] In one embodiment, the amount of the salt of the monovalent metal ion present in the polyisobutylene particles and reshaped polyisobutylene particles is from 1 ppm to 1,000 ppm, preferably from 10 ppm to 500 ppm, and in a more preferred embodiment, from 10 to 200 ppm.
[0308] In one embodiment, the amount of stearate or palmitate of monovalent or multivalent metal ions present in the polyisobutylene particles and polyisobutylene products is from 0 to 4,000 ppm, preferably from 0 to 2,000 ppm, more preferably from 0 to 1,000 ppm, and in a more preferred embodiment, from 0 to 500 ppm.
[0309] In one embodiment, the amount of LCST compounds present in the polyisobutylene particles and reshaped polyisobutylene particles is from 1 ppm to 5,000 ppm, preferably from 1 ppm to 2,000 ppm, and in a more preferred embodiment, from 5 to 1,000 ppm or from 5 to 500 ppm.
[0310] In another preferred embodiment, the amount of LCST compounds present in the polyisobutylene particles and reshaped polyisobutylene particles is from 5 to 100 ppm, preferably from 5 to 50 ppm and more preferably from 5 to 30 ppm.
[0311] In one embodiment, the amount of the salt of the monovalent metal ion present in the polyisobutylene particles and reshaped polyisobutylene particles is from 1 ppm to 1,000 ppm, preferably from 10 ppm to 500 ppm, and in a more preferred embodiment, from 10 to 200 ppm.
[0312] In one embodiment, the amount of stearate or palmitate of the multivalent metal ion present in the polyisobutylene particles and reshaped polyisobutylene particles is from 0 to 4,000 ppm, preferably from 0 to 2,000 ppm, more preferably from 0 to 1,000 ppm, and in a more preferred embodiment, from 0 to 500 ppm.
[0313] Thus, in one embodiment, the present invention includes polyisobutylene particles and polyisobutylene products comprising
[0314] I) 96.0 wt% or more, preferably 97.0 wt% or more, more preferably 98.0 wt% or more, even more preferably 99.0 wt% or more, still even more preferably 99.2 wt% or more of polyisobutylene, and in another embodiment 99.5 wt% or more of polyisobutylene
[0315] II) 0 to 3.0% by weight, preferably 0 to 2.5% by weight, more preferably 0 to 1.0% by weight and more preferably 0 to 0.40% by weight of salts of monovalent or polyvalent metal ions, preferably stearates and palmitates of polyvalent metal ions, and
[0316] III) 1 ppm to 5,000 ppm, preferably 1 ppm to 2,000 ppm, of at least one LCST compound, and in a more preferred embodiment, 5 to 1,000 ppm or 5 to 500 ppm of at least one LCST compound.
[0317] In case the LCST compound is defined as a mandatory component, the present invention comprises not only the polyisobutylene particles or reshaped polyisobutylene particles, collectively referred to herein as (reshaped) polyisobutylene particles, but also any type of polyisobutylene composition comprising a LCST compound.
[0318] Thus, in another embodiment, the present invention comprises a polyisobutylene composition, in particular a (reshaped) polyisobutylene granulate, comprising
[0319] I) 96.0 wt% or more, preferably 97.0 wt% or more, more preferably 98.0 wt% or more, even more preferably 99.0 wt% or more, still even more preferably 99.2 wt% or more of polyisobutylene, and in another embodiment 99.5 wt% or more of polyisobutylene
[0320] II) 0 to 3.0% by weight, preferably 0 to 2.5% by weight, more preferably 0 to 1.0% by weight and more preferably 0 to 0.40% by weight of salts of monovalent or polyvalent metal ions, preferably stearates and palmitates of polyvalent metal ions, and
[0321] III) 1 ppm to 5,000 ppm, preferably 1 ppm to 2,000 ppm, of at least one LCST compound, and in a more preferred embodiment, 5 to 1,000 ppm or 5 to 500 ppm of at least one LCST compound.
[0322] Since the salts of multivalent metal ions contribute to the ash content measurable according to ASTM D5667 (version reapproved in 2010), the present invention also includes a polyisobutylene composition, in particular a (reshaped) polyisobutylene granule, which comprises 98.5 wt. % or more, preferably 98.8 wt. % or more, more preferably 99.0 wt. % or more, even more preferably 99.2 wt. % or more, yet even more preferably 99.4 wt. % or more of polyisobutylene, and in another embodiment 99.5 wt. % or more of polyisobutylene, and has an ash content of 0.2 wt. % or less, preferably 0.1 wt. % or less, more preferably 0.08 wt. % or less and even more preferably 0.05 wt. % or less, yet even more preferably 0.03 wt. % or less and most preferably 0.015 wt. % or less, as measured according to ASTM D5667.
[0323] In a preferred embodiment, the above-described polyisobutylene composition, in particular the (reshaped) copolymer particles, further comprises 1 ppm to 5,000 ppm, preferably 1 ppm to 2,000 ppm, of at least one LCST compound, and in a more preferred embodiment, 5 to 1,000 ppm or 5 to 500 ppm of at least one LCST compound.
[0324] In yet another embodiment, the present invention comprises polyisobutylene compositions, in particular (reshaped) polyisobutylene granules and polyisobutylene products, comprising
[0325] 1) 100 parts by weight of polyisobutylene (100 phr)
[0326] II) 0.0001 to 0.5, preferably 0.0001 to 0.2, more preferably 0.0005 to 0.1, even more preferably 0.0005 to 0.05 phr of at least one LCST compound, and
[0327] III) no or 0.0001 to 3.0, preferably no or 0.0001 to 2.0, more preferably no or 0.0001 to 1.0, even more preferably no or 0.0001 to 0.5, still even more preferably no or 0.0001 to 0.3 and most preferably no or 0.0001 to 0.2 phr of salts of monovalent or polyvalent metal ions, preferably stearates and palmitates of monovalent or polyvalent metal ions, preferably comprising calcium stearate, calcium palmitate, zinc stearate or zinc palmitate, and
[0328] IV) no or 0.005 to 0.1, preferably 0.008 to 0.05, more preferably 0.03 to 0.07 phr of antioxidant,
[0329] V) 0.005 to 0.5, preferably 0.01 to 0.3, more preferably 0.05 to 0.2 phr of volatile matter having a boiling point of 200° C. or lower at standard pressure.
[0330] Preferably, the above-mentioned components I) to V) amount to 100.00501 to 104.100000 parts by weight, preferably 100.01 to 103.00 parts by weight, more preferably 100.10 to 101.50 parts by weight, even more preferably 100.10 to 100.80 parts by weight, and together represent 99.80 to 100.00% by weight, preferably 99.90 to 100.00% by weight, more preferably 99.95 to 100.00% by weight and even more preferably 99.97 to 100.00% by weight of the total weight of the polyisobutene composition, in particular the (reshaped) polyisobutene granules.
[0331] The remainder, if any, may represent salts or components other than the abovementioned components, for example originating from the water used for preparing the aqueous medium used in step a) or - if applicable - from products including decomposition products and remaining salts of the initiator system used in step b).
[0332] The determination of free carboxylic acids and their salts, in particular calcium stearate and zinc stearate or calcium palmitate and zinc palmitate, can be accomplished by measuring using gas chromatography with a flame ionization detector (GC-FID) according to the following procedure:
[0333] Weigh 2 g of the copolymer composition sample to an accuracy of 0.0001 g, place it in a 100 mL wide-mouth bottle and
[0334] a) In cases where the level of free carboxylic acid is to be determined, combine with 25 mL of hexane, 1,000 mL of internal standard solution, and
[0335] b) In cases where the level of carboxylate is to be determined, combine with 25 mL of hexane, 1,000 mL of internal standard solution, and 5 drops of concentrated sulfuric acid.
[0336] The jar was placed on a shaker for 12 hours. 23 ml of acetone were then added and the remaining mixture was evaporated to dryness at 50°C, typically taking 30 minutes.
[0337] After that, 10 ml of methanol and 2 drops of concentrated sulfuric acid were added, shaken to mix and heated at 50° C. for 1 hour to convert the carboxylic acid into its methyl ester. After that, 10 ml of hexane and 10 ml of demineralized water were added, shaken vigorously, and finally the hexane layer was separated. GC-FID analysis was performed using 2 ml of the hexane solution.
[0338] It is known to those skilled in the art that industrial stearates such as calcium stearate and zinc stearate also contain portions of other calcium and zinc carboxylates such as palmitate. However, GC-FID can also determine the content of other carboxylic acids.
[0339] Direct determination of carboxylates, especially stearates and palmitates, can be accomplished by FTIR as follows: The rubber sample is squeezed between two sheets of silicone release paper in a paper sample holder and analyzed on an infrared spectrometer. The carbonyl peaks of calcium stearate are located at 1541.8 and 1577.2 cm -1 The peaks of thermally converted calcium stearate (different modifications of calcium stearate, see, for example, Journal of Colloid Science, Vol. 4, No. 2, April 1949, pp. 93-101) are located at 1562.8 and 1600.6 cm -1 and are also included in the calcium stearate calculation. These peaks are -1 The ratio of the peaks at is used to account for thickness variations in the sample.
[0340] By comparing the peak height to that of a known standard having a predetermined level of calcium stearate, the concentration of calcium stearate can be determined. The same is true for other carboxylates, particularly stearates and palmitates. For example, the carbonyl peak of zinc stearate alone is located at 1539.5 cm -1 The carbonyl peak of sodium stearate is located at 1558.5 cm -1 Place.
[0341] The content of monovalent or polyvalent metal ions, in particular polyvalent metal ions such as calcium and zinc, can generally be determined and, if not mentioned otherwise, is determined by inductively coupled plasma atomic emission spectroscopy (ICP-AES) according to EPA 6010 Method C, using NIST traceable calibration standards, after microwave digestion according to EPA 3052 Method C.
[0342] Additionally or alternatively, the content of various elements can be determined by X-ray fluorescence (XRF). The sample is irradiated with X-ray radiation of sufficient energy to excite the element of interest. The element will emit energy specific to the element type, which is detected by an appropriate detector. Comparison with standards of known concentration and similar matrix will yield quantitative amounts of the desired element. The content of LCST compounds, particularly methylcellulose content, is measurable and measured relative to standards of known concentration using gel filtration chromatography on a Waters Alliance 2690 / 5 separation module equipped with the following equipment: PolySep-GFC-P4000, 300×7.8 mm aqueous GFC column and PolySep-GFC-P4000, 35×7.8 mm guard column and Waters 2414 differential refractometer. Since gel filtration chromatography separates based on molecular weight, it may be necessary to use a column different from the above column in order to analyze LCST compounds of different molecular weight ranges.
[0343] The samples were prepared, for example, according to the following procedure:
[0344] 2 g of the copolymer composition sample was weighed to the nearest 0.0001 g and dissolved in 30 ml of hexane in a sealed vial using a low speed oscillator overnight. 5 ml of HPLC grade water was accurately added at room temperature, the vial was recapped and oscillated for another 30 minutes. After phase separation, the aqueous phase was used for gel filtration chromatography and injected through a 0.45 micron syringe filter.
[0345] It is obvious to those skilled in the art that different analytical methods may lead to slightly different results. However, at least to the extent that the above-described methods are involved, the results are found to be consistent within their own and inherent error ranges.
[0346] For all of the above polyisobutylene compositions, in one embodiment, the ash content measured according to ASTM D5667 is, for example, 0.2 wt. % or less, preferably 0.1 wt. % or less, more preferably 0.08 wt. % or less and even more preferably 0.05 wt. % or less, still even more preferably 0.03 wt. % or less and most preferably 0.015 wt. % or less.
[0347] Preferred polyisobutylenes are those already described above in the process section.
[0348] In one embodiment, the polyisobutylene particles and polyisobutylene products have a bulk density of 0.05 kg / l to 0.900 kg / l, preferably 0.5 kg / l to 0.900 kg / l.
[0349] In a further step e), the polyisobutylene granules obtained in step f) are subjected to a shaping process such as baling.
[0350] The present invention therefore includes shaped articles, in particular bales obtainable by shaping, in particular baling, the polyisobutylene granules and polyisobutylene products obtained in step d). Shaping can be carried out using any standard equipment known to the person skilled in the art for such purposes. Baling can be carried out, for example, using conventional, commercially available balers. Shaped articles made of or comprising (reshaped) polyisobutylene granules are also encompassed by the term polyisobutylene composition.
[0351] In one embodiment, the shaped article, in particular the bag, has a density of 0.700 kg / l to 0.850 kg / l.
[0352] In another embodiment, the shaped article is cubic and has a weight of 10 to 50 kg, preferably 25 to 40 kg.
[0353] It is obvious to the person skilled in the art that the density of the shaped articles, in particular bags, is higher than the bulk density of the polyisobutylene granules used for their production.
[0354] Blend
[0355] The polyisobutylene compositions, in particular the (reshaped) polyisobutylene granules and the shaped articles made from or comprising the (reshaped) polyisobutylene granules, are referred to hereinafter as polyisobutylene according to the invention. One or more polyisobutylenes of the present invention may be blended with each other or additionally or alternatively with at least one second rubber, which is different from the polyisobutylene forming the polyisobutylene particles and which is preferably selected from natural rubber (NR), epoxidized natural rubber (ENR), polyisoprene rubber, poly(styrene-co-butadiene) rubber (SBR), chloroprene rubber (CR), polybutadiene rubber (BR), perfluoropolyisobutylene (FFKM / FFPM), ethylene vinyl acetate (EVA) rubber, vinyl acrylate rubber, polysulfide rubber (TR), poly(isoprene-co-butadiene) rubber (IBR), styrene-isoprene-butadiene rubber (SIBR), ethylene-propylene rubber (EPR), ethylene-propylene-diene M-grade rubber (EPDM), polyphenylenesulfide (PES), polyisoprene rubber (PPR), polyisoprene rubber (PDM ... e), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), propylene oxide polymers, star-branched butyl rubber and halogenated star-branched butyl rubber, butyl rubber not the subject of the present invention (i.e. having different levels of polyvalent metal ions or purity grades), brominated butyl rubber and chlorinated butyl rubber, star-branched polyisobutylene rubber, star-branched brominated butyl (polyisobutylene / isoprene polyisobutylene) rubber; poly(isobutylene-co-p-methylstyrene) and halogenated poly(isobutylene-co-p-methylstyrene), halogenated poly(isobutylene-co-isoprene-co-p-methylstyrene), poly(isobutylene-co-isoprene-co-styrene), halogenated poly(isobutylene-co-isoprene-co-styrene), poly(isobutylene-co-isoprene-co-α-methylstyrene), halogenated poly(isobutylene-co-isoprene-co-α-methylstyrene).
[0356] One or more polyisobutylenes of the present invention or blends with the above-mentioned second rubber may further be additionally or alternatively blended, for example simultaneously or separately, with at least one thermoplastic polymer, preferably selected from polyphenylene sulfide (PPS), polyurethane (PU), polyacrylate (ACM, PMM), thermoplastic polyester urethane (AU), thermoplastic polyether urethane (EU), perfluoroalkoxyalkane (PFA), polytetrafluoroethylene (PTFE) and polytetrafluoroethylene (PTFE).
[0357] One or more polyisobutylenes of the present invention or blends with the above-mentioned second rubber and / or thermoplastic polymer can be mixed with one or more fillers. The filler can be a non-mineral filler, a mineral filler or a mixture thereof. In some embodiments, non-mineral fillers are preferred, including, for example, carbon black, rubber gel and mixtures thereof. Suitable carbon black is preferably prepared by lamp black process, furnace black process or gas black process. The carbon black preferably has a BET specific surface area of 20 to 200 m 2 / g. Some specific examples of carbon black are SAF, ISAF, HAF, FEF and GPF carbon black. The rubber gel is preferably a rubber gel based on polybutadiene, butadiene / styrene polyisobutylene, butadiene / acrylonitrile polyisobutylene or polychloroprene.
[0358] Suitable mineral fillers include, for example, silica, silicates, clays, bentonite, vermiculite, nontronite, beidellite, volcanoite, hectorite, saponite, laponite, sauconite, magadiite, kenyaite, ledikite, gypsum, alumina, talc, glass, metal oxides (e.g., titanium dioxide, zinc oxide, magnesium oxide, aluminum oxide), metal carbonates (e.g., magnesium carbonate, calcium carbonate, zinc carbonate), metal hydroxides (e.g., aluminum hydroxide, magnesium hydroxide), or mixtures thereof.
[0359] The average agglomerated particle diameter that the amorphous silicon dioxide particles that are suitable for drying as mineral filler have can be in the scope of 1 to 100 microns, or 10 to 50 microns, or 10 to 25 microns. In one embodiment, the agglomerated particles less than 10 volume % can be below 5 microns. In one embodiment, the size of the agglomerated particles less than 10 volume % can be above 50 microns. The BET surface area (measured according to DIN (Deutsche Industrie Norm) 66131) of suitable amorphous drying silicon dioxide can be, for example, between 50 and 450 square meters / gram. The DBP absorption measured according to DIN 53601 can be between 150 and 400 grams / 100 grams of silicon dioxide. The drying loss measured according to DIN ISO 787 / 11 can be 0 to 10 weight %. Suitable silicon dioxide fillers are commercially available from PPG Industries Inc with the names HiSil™210, HiSil™233 and HiSil™243. Also suitable are Vulkasil™ MS and Vulkasil™ N, commercially available from Bayer AG.
[0360] The high aspect ratio fillers that can be used in the present invention may include clay, talc, mica, etc. having an aspect ratio of at least 1:3. The filler may include a round material or a nonisometric material having a plate-like or needle-like structure. The aspect ratio is defined as the ratio of the average diameter of a circle having the same area as the plate surface to the average thickness of the plate. The aspect ratio of needle-like and fibrous fillers is the ratio of length to diameter. The aspect ratio of the high aspect ratio filler may be at least 1:5, or at least 1:7, or in the range of 1:7 to 1:200. The average particle size of the high aspect ratio filler may be, for example, in the range of 0.001 to 100 microns, or 0.005 to 50 microns, or 0.01 to 10 microns. The BET surface area of a suitable high aspect ratio filler (measured in accordance with DIN (Deutsche Industrie Norm) 66131) may be between 5 and 200 square meters / gram. The high aspect ratio filler may include nanoclays, for example, organically modified nanoclays. Examples of nanoclays include natural powdered montmorillonite clays (e.g., sodium montmorillonite or calcium montmorillonite) or synthetic clays (e.g., hydrotalcite or synthetic hectorite). In one embodiment, high aspect ratio fillers may include organically modified montmorillonite nanoclays. As known in the art, clays may be modified by replacing transition metals with onium ions to provide surfactant functions to clays that contribute to the dispersion of clays in a generally hydrophobic polymer environment. In one embodiment, the onium ions are phosphorus-based (e.g., phosphonium ions) or nitrogen-based (e.g., ammonium ions) and contain functional groups having 2 to 20 carbon atoms. Clays may be provided, for example, with nanometer-scale particle sizes, for example, less than 25 μm by volume. The particle size may be in the range of 1 to 50 μm, or 1 to 30 μm, or 2 to 20 μm. In addition to silica, nanoclays may also include a portion of aluminum oxide. For example, the nanoclay may contain 0.1 to 10 wt% alumina, or 0.5 to 5 wt% alumina, or 1 to 3 wt% alumina. Examples of commercially available organically modified nanoclays that are high aspect ratio mineral fillers include, for example, those sold under the trade names Those sold as clays 10A, 20A, 6A, 15A, 30B or 25A.
[0361] One or more polyisobutylenes of the present invention or blends with the above-mentioned second rubber and / or thermoplastic polymer or compound are collectively referred to as polymer products hereinafter, and may also contain other ingredients, such as curing agents, reaction accelerators, vulcanization accelerators, vulcanization accelerating aids, antioxidants, foaming agents, anti-aging agents, heat stabilizers, light stabilizers, ozone stabilizers, processing aids, plasticizers, tackifiers, foaming agents, dyes, pigments, waxes, fillers (extenders), organic acids, inhibitors, metal oxides, and activators such as triethanolamine, polyethylene glycol, hexanetriol, etc., which are all known in the rubber industry. These ingredients are used in conventional amounts depending, inter alia, on the intended use.
[0362] application
[0363] The polymer products have been found to be particularly useful for preparing compounds for specific applications.
[0364] Such applications include sealants, adhesives, coatings and roofing materials (roofing) and white and black filled sheeting (white and black filled sheeting).
[0365] The present invention therefore also includes the use of the polyisobutylenes of the present invention in or as sealants, adhesives, coatings and roofing materials and white and black filler sheets.
[0366] The polymer products can also be used in tire sidewalls and tread compounds. In the sidewalls, the properties of polyisobutylene impart good ozone resistance, crack cut growth and appearance.
[0367] In a preferred embodiment 1, the present invention relates to a method for preparing an aqueous slurry comprising a plurality of elastomer particles suspended therein, the method comprising at least the following steps:
[0368] A*) bringing the organic medium into contact with the aqueous medium,
[0369] The organic medium comprises
[0370] i) at least one elastomer, and
[0371] ii) organic diluent,
[0372] the aqueous medium comprises at least one LCST compound having a cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 70°C,
[0373] and
[0374] The organic diluent is at least partially removed to obtain an aqueous slurry containing elastomeric particles, wherein the elastomer is polyisobutylene.
[0375] In embodiment 2 according to embodiment 1, the organic medium comprising at least one polyisobutylene and an organic diluent is obtained by polymerization or post-polymerization.
[0376] In embodiment 3 according to embodiment 1 or 2, the organic medium is obtained from a polymerization reaction and may further contain residual monomers of the polymerization reaction.
[0377] In a specific embodiment 4 according to one of specific embodiments 1 to 3, the aqueous medium comprises 0 to 5,000 ppm, preferably 0 to 2,000 ppm, more preferably 10 to 1,000 ppm, even more preferably 50 to 800 ppm and still even more preferably 100 to 600 ppm of a salt of a polyvalent metal ion, calculated as to its metal content and relative to the amount of polyisobutene present in the medium obtained according to step A).
[0378] In embodiment 5 according to one of embodiments 1 to 4, the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of carboxylates of polyvalent metal ions and in another yet even more preferred embodiment 100 ppm or less of carboxylates of polyvalent metal ions, calculated as metal content and relative to the amount of polyisobutene present in the medium obtained according to step b).
[0379] In embodiment 6 according to embodiment 4 or 5, the salt of the polyvalent metal ion is calcium stearate and / or zinc stearate and / or calcium palmitate and / or zinc palmitate.
[0380] In embodiment 7 according to embodiment 6, the carboxylate of the polyvalent metal ion is calcium stearate and / or zinc stearate and / or calcium palmitate and / or zinc palmitate.
[0381] In embodiment 8 according to one of embodiments 1 to 7, the organic medium comprising at least one elastomer and an organic diluent is obtained by a polymerization reaction comprising at least the following steps:
[0382] a) providing a reaction medium comprising an organic diluent and at least one polymerizable monomer
[0383] b) polymerizing the monomers in the reaction medium in the presence of an initiator system or catalyst to form an organic medium comprising the elastomer, the organic diluent and optionally residual monomers.
[0384] In embodiment 9 according to one of embodiments 1 to 8, step A*) is carried out batchwise or continuously, preferably continuously.
[0385] In embodiment 10 according to one of embodiments 1 to 9, the temperature in step A*) is from 10 to 100°C, preferably from 50 to 100°C, more preferably from 60 to 95°C and even more preferably from 75 to 95°C.
[0386] In a specific embodiment 11 according to one of specific embodiments 1 to 10, the at least one LCST compound is selected from:
[0387] Poly(N-isopropylacrylamide); poly(N-isopropylacrylamide-co-N,N-dimethylacrylamide); poly(N-isopropylacrylamide)-alt-2-hydroxyethyl methacrylate; poly(N-vinylcaprolactam); poly(N,N-diethylacrylamide); poly[2-(dimethylamino)ethyl methacrylate]; poly(2-oxazoline) glyelastomers; poly(3-ethyl-N-vinyl) 2-pyrrolidone); hydroxybutyl chitosan; polyoxyethylene (20) sorbitan monostearate; polyoxyethylene (20) sorbitan monolaurate; polyoxyethylene (20) sorbitan monooleate; methylcellulose; hydroxypropyl cellulose; hydroxyethyl methylcellulose; hydroxypropyl methylcellulose; poly(ethylene glycol) methacrylate having 2 to 6 ethylene glycol units; polyethylene glycol-co-polypropylene glycol, preferably those having 2 to 6 ethylene glycol units and 2 to 6 polypropylene units; compounds of formula (I)
[0388] (I)HO-[-CH2-CH2-O] x -[-CH(CH3)-CH2-O] y -[-CH2-CH2-O] z -H
[0389] wherein y=3 to 10 and x and z=1 to 8, wherein y+x+z is 5 to 18;
[0390] Polyethylene glycol-co-polypropylene glycol, preferably those having 2 to 8 ethylene glycol units and 2 to 8 polypropylene units; ethoxylated iso-C 13 H 27-alcohols, preferably having a degree of ethoxylation of 4 to 8; polyethylene glycols having 4 to 50, preferably 4 to 20 ethylene glycol units; polypropylene glycols having 4 to 30, preferably 4 to 15 propylene glycol units; polyethylene glycol monomethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol monoethyl ether and polyethylene glycol diethyl ether having 4 to 50, preferably 4 to 20 ethylene glycol units; polypropylene glycol monomethyl ether, polypropylene glycol dimethyl ether, polypropylene glycol monoethyl ether and polypropylene glycol diethyl ether having 4 to 50, preferably 4 to 20 propylene glycol units; among which methylcellulose, hydroxypropyl cellulose, hydroxyethyl methylcellulose and hydroxypropyl methylcellulose are preferred.
[0391] In embodiment 12 according to one of embodiments 1 to 11, the method comprises a further step, in which the elastomer particles contained in the aqueous slurry obtained according to step A*) are separated to obtain separated elastomer particles.
[0392] In embodiment 13 according to one of embodiments 1 to 11, the method comprises a further step in which the elastomer particles contained in the aqueous slurry obtained according to step A*) are separated to obtain separated elastomer particles; and comprises a further step in which the (separated) elastomer particles are dried, preferably to a residual content of volatiles of 7,000 or less, preferably 5,000 or less, even more preferably 4,000 or less, and in another embodiment, to 2,000 ppm or less, preferably 1,000 ppm or less.
[0393] In a specific embodiment 14 according to one of specific embodiments 1 to 12, the method comprises as a further step shaping the elastomer particles to obtain reshaped elastomer particles such as pellets or shaped articles such as bags.
[0394] In embodiment 15, the present invention comprises an aqueous slurry obtainable according to one of embodiments 1 to 14.
[0395] In a sixteenth embodiment, the present invention comprises the use of a LCST compound as defined in the first embodiment, having a cloud point of 0 to 100° C., preferably 5 to 100° C., more preferably 15 to 80° C. and even more preferably 20 to 70° C., as an anti-agglomeration agent, in particular for polyisobutylene particles.
[0396] In a 17th embodiment, the present invention comprises a method for preventing or reducing or slowing down agglomeration of a slurry comprising polyisobutylene particles suspended in an aqueous medium by adding or using a LCST compound, as defined in the 1st embodiment, wherein the LCST compound has a cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 70°C.
[0397] In specific embodiment 18, the present invention comprises polyisobutylene particles having a polyisobutylene content of 98.5 wt % or more, preferably 98.8 wt % or more, more preferably 99.0 wt % or more, even more preferably 99.2 wt % or more, still even more preferably 99.4 wt % or more, and in another embodiment, 99.5 wt % or more.
[0398] In specific embodiment 19 according to specific embodiment 18, the weight average molecular weight of the polyisobutylene is in the range of 10 to 2,000 kg / mol, preferably in the range of 20 to 1,000 kg / mol, more preferably in the range of 50 to 1,000 kg / mol, even more preferably in the range of 200 to 800 kg / mol, still more preferably in the range of 375 to 550 kg / mol, and most preferably in the range of 400 to 500 kg / mol.
[0399] In embodiment 20 according to embodiment 18 or 19, the polyisobutylene has a Mooney viscosity of at least 10 (ML 125°C 1+8, ASTM D 1646), preferably 20 to 80 and even more preferably 25 to 60 (ML 125°C 1+8, ASTM D 1646).
[0400] In a specific embodiment 21 according to one of specific embodiments 18 to 20, the polyisobutylene particles further comprise 0 to 0.4% by weight, preferably 0 to 0.2% by weight, more preferably 0 to 0.1% by weight and more preferably 0 to 0.05% by weight of salts of polyvalent metal ions, preferably stearates and palmitates of polyvalent metal ions.
[0401] In a specific embodiment 22 according to one of specific embodiments 18 to 21, the polyisobutylene particles further comprise 1 ppm to 18,000 ppm, preferably 1 ppm to 5,000 ppm, more preferably 1 ppm to 2,000 ppm of at least one LCST compound, and in a more preferred embodiment, 5 to 1,000 ppm or 5 to 500 ppm of at least one LCST compound.
[0402] In embodiment 23, the present invention comprises shaped articles, in particular pellets or bags, obtainable by shaping the polyisobutylene particles of embodiments 18 to 22.
[0403] In Embodiment 24, the present invention includes a blend or mixture obtainable by blending or mixing the polyisobutylene particles of Embodiments 18 to 22 or the shaped article of Embodiment 23.
[0404] In embodiment 25, the present invention comprises the use of the polyisobutylene particles of embodiments 18 to 22 or the shaped articles of embodiment 23 or the blends or mixtures of embodiment 24 for use in liners, bladders, tubes, air cushions, pneumatic springs, bellows, accumulator bags, hoses, conveyor belts and pharmaceutical seals, automotive suspension shock absorbers, automotive exhaust hangers, body mounts, shoe soles, chewing gum, tire sidewall and tread rubber, belts, hoses, shoe soles, gaskets, O-rings, wires / cables, films, rollers, bladders (e.g., cured bladders), tire liners, tire treads, shock absorbers, machine parts, balloons, balls, golf balls, protective clothing, medical tubing, tank linings, electrical insulation, bearings, pharmaceutical plugs, stoppers, adhesives; containers, such as bottles, totes, tanks, container closures or lids; seals or sealants, such as gaskets or caulking materials; material handling devices, such as augers or conveyor belts; cooling towers; metalworking equipment, or any device that comes in contact with metalworking fluids; engine parts, such as fuel lines, fuel filters, fuel tanks, gaskets, seals, etc.; membranes, such as membranes used for fluid filtration or tank sealing.
[0405] The present invention also includes specific embodiments that are combinations of the 25 specific embodiments and general embodiments listed above, including any levels of preferred embodiments, range parameters as disclosed above.
[0406] The present invention also includes the following embodiments.
[0407] Embodiment 1. A method for preparing an aqueous slurry, the aqueous slurry comprising a plurality of polyisobutylene particles suspended therein, the method comprising at least the following steps:
[0408] A) bringing the organic medium into contact with the aqueous medium,
[0409] The organic medium comprises
[0410] i) polyisobutylene, and
[0411] ii) organic diluent,
[0412] The aqueous medium comprises at least one LCST compound having a cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 70°C, and
[0413] The organic diluent is at least partially removed to obtain an aqueous slurry containing polyisobutylene particles.
[0414] Embodiment 2. A method for preparing an aqueous slurry comprising a plurality of polyisobutylene particles suspended therein, the method comprising at least the following steps:
[0415] A) bringing the organic medium into contact with the aqueous medium,
[0416] The organic medium comprises
[0417] i) polyisobutylene, and
[0418] ii) organic diluent,
[0419] The aqueous medium comprises at least one compound selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, hydroxyalkyl alkyl cellulose, and carboxyalkyl cellulose;
[0420] The organic diluent is at least partially removed to obtain an aqueous slurry containing polyisobutylene particles.
[0421] Embodiment 3. The method of embodiment 1 or 2, wherein the LCST compound is a LCST compound having a cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 80°C, the cloud point being determined by at least one of the following methods:
[0422] DIN EN 1890, Method A, September 2006
[0423] DIN EN 1890, Method C, September 2006
[0424] DIN EN 1890, Method E, September 2006
[0425] DIN EN 1890, September 2006, Method A, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water
[0426] DIN EN 1890, method A, September 2006, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.2 g / 100 ml distilled water.
[0427] Embodiment 4. The method of embodiment 1 or 2, wherein the LCST compound is a LCST compound having a cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 80°C, the cloud point being determined by at least one of the following methods:
[0428] DIN EN 1890, Method A, September 2006
[0429] DIN EN 1890, Method E, September 2006
[0430] DIN EN 1890, method A, September 2006, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water.
[0431] Embodiment 5. The method of embodiment 1 or 2, wherein the LCST compound is a LCST compound having a cloud point of 0 to 100°C, preferably 5 to 100°C, more preferably 15 to 80°C and even more preferably 20 to 80°C, the cloud point being determined by at least one of the following methods:
[0432] DIN EN 1890, Method A, September 2006
[0433] DIN EN 1890, Method C, September 2006
[0434] DIN EN 1890, method A, September 2006, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water.
[0435] Embodiment 6. The method of embodiment 1 or 2, wherein the LCST compound is a LCST compound having a turbidity point of 10 to 90° C., the turbidity point being determined by the following method:
[0436] DIN EN 1890, method A, September 2006, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water.
[0437] Embodiment 7. The method of any one of embodiments 1 to 6, wherein the LCST compound is selected from cellulose compounds, wherein at least one hydroxyl functional group -OH of the cellulose is functionalized to form one of the following groups:
[0438] OR c , where R c is methyl, 2-hydroxyethyl, 2-methoxyethyl, 2-methoxypropyl, 2-hydroxypropyl, -(CH2-CH2O) nH, -(CH2-CH2O) n CH3, -(CH2-CH(CH3)O) n H, -(CH2-CH(CH3)O) n CH3, wherein n is an integer from 1 to 20, preferably from 3 to 20.
[0439] Embodiment 8. The method of any one of Embodiments 1 to 7, wherein the degree of substitution (DS) of the alkyl cellulose, hydroxyalkyl cellulose and carboxyalkyl cellulose is from 0.5 to 2.8, preferably from 1.2 to 2.5.
[0440] Embodiment 9. The method of any one of Embodiments 1 to 8, wherein the organic medium comprising polyisobutylene and an organic diluent is obtained by a polymerization reaction.
[0441] Embodiment 10. The method of any one of Embodiments 1 to 9, wherein the organic medium is obtained from a polymerization reaction and further contains residual polyisobutylene from the polymerization reaction.
[0442] Embodiment 11. The method of any one of embodiments 1 to 10, wherein the aqueous medium further comprises a non-LCST compound, and preferably the non-LCST compound is calculated relative to the amount of polyisobutylene present in the organic medium.
[0443] selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, or in another embodiment
[0444] · a salt of a monovalent or polyvalent metal ion, or in another embodiment
[0445] stearate or palmitate of a monovalent or polyvalent metal ion, or in another embodiment
[0446] · Stearates or palmitates of sodium, potassium, calcium and zinc.
[0447] Embodiment 12. The method of any one of embodiments 1 to 11, wherein the aqueous medium comprises 20,000 ppm or less, preferably 10,000 ppm or less, more preferably 8,000 ppm or less, even more preferably 5,000 ppm or less and still even more preferably 2,000 ppm or less of non-LCST compounds, and in another yet even more preferred embodiment, 1,000 ppm or less of non-LCST compounds, and preferably calculated relative to the amount of polyisobutylene present in the organic medium, wherein the non-LCST compounds
[0448] selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, or in another embodiment
[0449] · a salt of a monovalent or polyvalent metal ion, or in another embodiment
[0450] stearate or palmitate of a monovalent or polyvalent metal ion, or in another embodiment
[0451] · Stearates or palmitates of sodium, potassium, calcium and zinc.
[0452] Embodiment 13. The method of any one of embodiments 1 to 12, wherein the aqueous medium contains 500 ppm or less, preferably 100 ppm or less, more preferably 50 ppm or less, even more preferably 30 ppm or less and still even more preferably 10 ppm or less of non-LCST compounds, and in another yet even more preferred embodiment, contains 1,000 ppm or less of non-LCST compounds, and preferably calculated relative to the amount of polyisobutylene present in the organic medium, wherein the non-LCST compounds
[0453] selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, or in another embodiment
[0454] · a salt of a monovalent or polyvalent metal ion, or in another embodiment
[0455] stearate or palmitate of a monovalent or polyvalent metal ion, or in another embodiment
[0456] · Stearates or palmitates of sodium, potassium, calcium and zinc.
[0457] Embodiment 14. The process of any one of Embodiments 1 to 13, wherein the aqueous medium comprises 0 to 5,000 ppm, preferably 0 to 2,000 ppm, more preferably 10 to 1,000 ppm, even more preferably 50 to 800 ppm and still even more preferably 100 to 600 ppm of a salt of a monovalent or polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0458] Embodiment 15. The process of any one of Embodiments 1 to 14, wherein the aqueous medium comprises 0 to 5,000 ppm, preferably 0 to 2,000 ppm, more preferably 10 to 1,000 ppm, even more preferably 50 to 800 ppm and still even more preferably 100 to 600 ppm of a salt of a polyvalent metal ion, calculated as to its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0459] Embodiment 16. The method of any one of embodiments 1 to 15, wherein the weight ratio of stearate, palmitate and oleate of monovalent or polyvalent metal ions to the LCST compound in the aqueous medium is 1:2 to 1:100, preferably 1:2 to 1:10 and more preferably 1:5 to 1:10.
[0460] Embodiment 17. The process of any one of Embodiments 1 to 16, wherein the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of the salt of the metal ion, and in another still even more preferred embodiment, 100 ppm or less of the salt of the metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0461] Embodiment 18. The process of any one of Embodiments 1 to 17, wherein the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of the salt of the polyvalent metal ion, and in another still even more preferred embodiment, 100 ppm or less of the salt of the polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0462] Embodiment 19. The method of any one of Embodiments 1 to 18, wherein the aqueous medium comprises 8,000 ppm or less, preferably 5,000 ppm or less, more preferably 2,000 ppm or less, yet even more preferably 1,000 ppm or less of a nonionic surfactant, and in another embodiment preferably 500 ppm or less, more preferably 100 ppm or less and even more preferably 15 ppm or less and yet even more preferably no or 1 ppm to 10 ppm of a nonionic surfactant, the nonionic surfactant being a non-LCST compound selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, and relative to the amount of polyisobutylene present in the organic medium.
[0463] Embodiment 20. The process of any one of Embodiments 1 to 19, wherein the aqueous medium comprises 70 ppm or less, preferably 50 ppm or less, more preferably 30 ppm or less and even more preferably 20 ppm or less and still even more preferably 10 ppm or less of the salt of the polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0464] Embodiment 21. The process of any one of Embodiments 1 to 20, wherein the aqueous medium comprises 25 ppm or less, preferably 10 ppm or less, more preferably 8 ppm or less and even more preferably 7 ppm or less and still even more preferably 5 ppm or less of the salt of the polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
[0465] Embodiment 22. The process of any one of embodiments 1 to 21, wherein the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of carboxylic acid salts of polyvalent metal ions, and in another still even more preferred embodiment, 100 ppm or less of carboxylic acid salts of polyvalent metal ions, calculated as their metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms.
[0466] Embodiment 23. The process of any one of Embodiments 1 to 22, wherein the aqueous medium comprises 70 ppm or less, preferably 50 ppm or less, more preferably 30 ppm or less and even more preferably 20 ppm or less and still even more preferably 10 ppm or less of a carboxylate of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms.
[0467] Embodiment 24. The process of any one of Embodiments 1 to 23, wherein the aqueous medium contains 25 ppm or less, preferably 10 ppm or less, more preferably 8 ppm or less and even more preferably 7 ppm or less and still even more preferably 5 ppm or less of a carboxylate of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms.
[0468] Embodiment 25. The method of any one of Embodiments 1 to 24, wherein the aqueous medium of one embodiment does not contain a carboxylate salt of a polyvalent metal ion, wherein the carboxylic acid is selected from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, and more preferably 12 to 18 carbon atoms.
[0469] Embodiment 26. The process of any one of Embodiments 1 to 25, wherein the aqueous medium comprises 100 ppm or less, preferably 50 ppm or less, more preferably 20 ppm or less and even more preferably 15 ppm or less and still even more preferably 10 ppm or less of salts of monovalent metal ions, calculated as their metal content and relative to the amount of polyisobutylene present in the organic medium.
[0470] Embodiment 27. The method of any one of embodiments 1 to 26, wherein the aqueous medium additionally or alternatively comprises 100 ppm or less, preferably 50 ppm or less, more preferably 30 ppm or less, even more preferably 20 ppm or less and still even more preferably 10 ppm or less of carboxylates of monovalent metal ions, and in another yet even more preferred embodiment, 5 ppm or less of carboxylates of monovalent metal ions, such as sodium stearate, sodium palmitate and sodium oleate and potassium stearate, potassium palmitate and potassium oleate, calculated based on their metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms, and in one embodiment such carboxylic acids are selected from monocarboxylic acids.
[0471] Embodiment 28. The method of any one of Embodiments 1 to 27, wherein the aqueous medium does not contain a carboxylate salt of a monovalent metal ion, wherein the carboxylic acid is selected from carboxylic acids having 6 to 30 carbon atoms, preferably 8 to 24 carbon atoms, more preferably 12 to 18 carbon atoms.
[0472] Embodiment 29. The method of any one of Embodiments 22 to 28, wherein the carboxylic acid is selected from monocarboxylic acids, preferably saturated monocarboxylic acids, more preferably palmitic acid or stearic acid.
[0473] Embodiment 30. The method of any one of Embodiments 1 to 29, wherein the aqueous medium comprises 0 to 5,000 ppm, preferably 0 to 2,000 ppm, more preferably 10 to 1,000 ppm, even more preferably 50 to 800 ppm and still even more preferably 100 to 600 ppm of
[0474] carbonates of polyvalent metal ions, calculated based on their metal content relative to the amount of polyisobutylene present in the organic medium, or in another embodiment
[0475] - Magnesium carbonate and calcium carbonate, calculated on the basis of their metal content and relative to the amount of polyisobutylene present in the organic medium.
[0476] Embodiment 31. The method of any one of Embodiments 1 to 30, wherein the aqueous medium comprises 550 ppm or less, preferably 400 ppm or less, more preferably 300 ppm or less, even more preferably 250 ppm or less and still even more preferably 150 ppm or less of the following substances, and in another still even more preferred embodiment, 100 ppm or less of the following substances:
[0477] carbonates of polyvalent metal ions, calculated based on their metal content relative to the amount of polyisobutylene present in the organic medium, or in another embodiment
[0478] - Magnesium carbonate and calcium carbonate, calculated on the basis of their metal content and relative to the amount of polyisobutylene present in the organic medium.
[0479] Embodiment 32. The process of any one of embodiments 1 to 31, wherein the aqueous medium comprises 70 ppm or less, preferably 50 ppm or less, more preferably 30 ppm or less and even more preferably 20 ppm or less and still even more preferably 10 ppm or less of carbonate of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium, or in another embodiment
[0480] - Magnesium carbonate and calcium carbonate, calculated on the basis of their metal content and relative to the amount of polyisobutylene present in the organic medium.
[0481] Embodiment 33. The method of any one of Embodiments 1 to 32, wherein the aqueous medium contains 500 ppm or less, preferably 200 ppm or less, more preferably 100 ppm or less, even more preferably 50 ppm or less and still even more preferably 20 ppm or less of layered minerals, and in another yet even more preferred embodiment, contains no layered minerals, such as talc, calculated relative to the amount of polyisobutylene present in the organic medium.
[0482] Embodiment 34. The method of any one of embodiments 1 to 33, wherein the aqueous medium comprises 500 ppm or less, preferably 200 ppm or less, more preferably 100 ppm or less, even more preferably 20 ppm or less and still even more preferably 10 ppm or less of dispersants, emulsifiers or anti-agglomerating agents other than LCST compounds, and in another yet even more preferred embodiment comprises 5 ppm or less and still even more preferably comprises no dispersants, emulsifiers or anti-agglomerating agents other than LCST compounds.
[0483] Embodiment 35. The method of any one of Embodiments 1 to 34, wherein the polyisobutylene particles are discrete particles of any form and consistency, and in a preferred embodiment, the discrete particles have a particle size between 0.05 mm and 25 mm, more preferably between 0.1 and 20 mm.
[0484] Embodiment 36. The method of any one of Embodiments 1 to 35, wherein the polyisobutylene particles have a weight average particle size of 0.3 to 10.0 mm.
[0485] Embodiment 37. The method of any one of Embodiments 1 to 36, wherein 90% by weight or more of the polyisobutylene particles are between 12.50 mm and 1.6 mm in size, and 80% by weight or more of the polyisobutylene particles are between 8.00 mm and 3.35 mm in size, as determined by sieving.
[0486] Embodiment 38. The method of any one of embodiments 1 to 37, wherein the aqueous medium contains 1 to 2,000 ppm of an antioxidant and / or stabilizer, preferably 50 to 1,000 ppm, more preferably 80 to 500 ppm, calculated relative to the amount of polyisobutylene present in the organic medium, wherein preferred antioxidants and stabilizers are 2,6-di-tert-butyl-4-methyl-phenol, pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid, 3,5-di(tert)butyl-4-hydroxyhydrocinnamic acid octadecyl ester, tert-butyl-4-hydroxyanisole, 2-(1,1-dimethyl)-1,4-benzenediol, tris(2,4-di-tert-butylphenyl)phosphate, dioctyldiphenyl 2,4,6-tri-tert-butylphenol, 2,4,6-triisobutylphenol, 2-tert-butyl-4,6-dimethylphenol, 2,4-dibutyl-6-ethylphenol, 2,4-dimethyl-6-tert-butylphenol, 2,6-di-tert-butylhydroxytoluene (BHT), 2,6-di-tert-butyl-4-ethylphenol, 2,6-di-tert-butyl-4-n-butylphenol, 2,6-di-tert-butyl-4-isobutylphenol, 2,6-dicyclopentyl-4-methylphenol, 4-tert-butyl-2,6-dimethylphenol, 4-tert-butyl-2,6-dicyclopentylphenol, 4-tert-butyl-2,6-diisopropylphenol, 4,6-di-tert-butyl-2-methylphenol, 6-tert-butyl- 2,4-Dimethylphenol, 2,6-di-tert-butyl-3-methylphenol, 4-hydroxymethyl-2,6-di-tert-butylphenol, 2,6-di-tert-butyl-4-phenylphenol and 2,6-di-octadecyl-4-methylphenol, 2,2'-ethylene-bis[4,6-di-tert-butylphenol], 2,2'-ethylene-bis[6-tert-butyl-4-isobutylphenol], 2,2'-isobutylene-bis[4,6-dimethyl-phenol], 2,2'-methylene-bis[4,6-di-tert-butylphenol], 2,2'-methylene-bis[4-methyl-6-(α-methylcyclohexyl)phenol], 2,2'-methylene-bis[4-methyl-6-cyclohexylphenol], 2,2'-methylene-bis[4-methyl-6 -nonylphenol], 2,2'-methylene-bis[6-(α,α'-dimethylbenzyl)-4-nonylphenol], 2,2'-methylene-bis[6-(α-methylbenzyl)-4-nonylphenol], 2,2'-methylene-bis[6-cyclohexyl-4-methylphenol], 2,2'-methylene-bis[6-tert-butyl-4-ethylphenol], 2,2'-methylene-bis[6-tert-butyl-4-methylphenol], 4,4'-butylene-bis[2-tert-butyl-5-methylphenol], 4,4'-methylene-bis[2,6-di-tert-butylphenol], 4,4'-methylene-bis[6-tert-butyl-2-methylphenol], 4,4'-isopropylidene-biphenol, 4,4'-decylene-bisphenol, 4,4'-Dodecylene-bisphenol, 4,4'-(1-methyloctylene)bisphenol, 4,4'-cyclohexylene-bis(2-methylphenol), 4,4'-cyclohexylene-bisphenol and pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid.
[0487] Embodiment 39. The method of any one of Embodiments 1 to 38, wherein the viscosity average molecular weight (M v ) is in the range of 100 to 3,000 kg / mol, preferably in the range of 250 to 3,000 kg / mol, or in another embodiment, in the range of 100 to 2,000 kg / mol, preferably in the range of 200 to 2,000 kg / mol, more preferably in the range of 350 to 1,800 kg / mol, even more preferably in the range of 400 to 1500 kg / mol and still even more preferably 700 to 1300 kg / mol, or in another embodiment, the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 2,001 to 3,000 kg / mol, or in yet another embodiment, the viscosity average molecular weight (M v ) is in the range of 3,001 to 10,000 kg / mol.
[0488] Embodiment 40. The method of any one of Embodiments 1 to 39, wherein the number average molecular weight (M n ) is in the range of 5-1100 kg / mol, preferably in the range of 80 to 500 kg / mol.
[0489] Embodiment 41. The method of any one of Embodiments 1 to 40, wherein the polyisobutylene of the present invention has a polyisobutylene polydispersity in the range of 1.1 to 6.0, preferably in the range of 3.0 to 5.5, wherein the polydispersity is measured by the ratio of the weight average molecular weight to the number average molecular weight determined by gel permeation chromatography.
[0490] Embodiment 42. The method of any one of Embodiments 1 to 41, wherein the polyisobutylene has a Mooney viscosity of at least 10 (ML 125°C 1+8, ASTM D 1646-7 (2012)), preferably 10 to 80, more preferably 20 to 80 and even more preferably 25 to 60 (ML 125°C 1+8, ASTM D 1646).
[0491] Embodiment 43. The method of any one of Embodiments 1 to 42, wherein the organic medium is obtained by a method comprising at least the following steps:
[0492] a) providing a reaction medium comprising an organic diluent and isobutylene
[0493] b) polymerizing the isobutylene in the reaction medium in the presence of an initiator system or catalyst to form an organic medium comprising the polyisobutylene, an organic diluent and optionally residual isobutylene.
[0494] Embodiment 44. The method of Embodiment 43, wherein the isobutylene is present in the reaction medium in an amount of 0.01 wt% to 80 wt%, preferably 0.1 wt% to 65 wt%, more preferably 10.0 wt% to 65.0 wt% and even more preferably 25.0 wt% to 65.0 wt%.
[0495] Embodiment 45. The method of any one of Embodiments 43 to 44, wherein the organic diluent is a hydrochlorocarbon; or a x H y F z The hydrofluorocarbon represented by wherein x is an integer from 1 to 40, or from 1 to 30, or from 1 to 20, or from 1 to 10, or from 1 to 6, or from 2 to 20, or from 3 to 10, or from 3 to 6, most preferably from 1 to 3, wherein y and z are integers and are at least 1; or a hydrocarbon, preferably an alkane, in another preferred embodiment, the alkane is selected from the group consisting of propane, isobutane, pentane, methylcyclopentane, isohexane, 2-methylpentane, 3-methylpentane, 2-methylbutane, 2,2-dimethylbutane, 2,3-dimethylbutane, 2-methylhexane, 3-methylhexane, 3-ethylpentane, 2,2-dimethylpentane, 2 ,3-dimethylpentane, 2,4-dimethylpentane, 3,3-dimethylpentane, 2-methylheptane, 3-ethylhexane, 2,5-dimethylhexane, 2,2,4-trimethylpentane, octane, heptane, butane, ethane, methane, nonane, decane, dodecane, undecane, hexane, methylcyclohexane, cyclopropane, cyclobutane, cyclopentane, methylcyclopentane, 1,1-dimethylcyclopentane, cis-1,2-dimethylcyclopentane, trans-1,2-dimethylcyclopentane, trans-1,3-dimethyl-cyclopentane, ethylcyclopentane, cyclohexane, methylcyclohexane and mixtures of the above diluents.
[0496] Embodiment 46. The method of any one of Embodiments 43 to 45, wherein the polymerization of step b) is carried out as a slurry polymerization or a solution polymerization.
[0497] Embodiment 47. The method of Embodiment 46, wherein the polymerization of step b) is carried out as a slurry polymerization, and 80% of the particles obtained during the slurry polymerization have a size of about 0.1 to about 800 μm, preferably about 0.25 to about 500 μm.
[0498] Embodiment 48. The method of any of Embodiments 1 to 47, wherein 50% by weight or more, 60% by weight or more, 70% by weight or more, or 80% by weight or more of the polyisobutylene particles have a particle size between about 3.35 mm and 8.00 mm.
[0499] Embodiment 49. The method of any one of Embodiments 1 to 48, wherein in a sieving experiment with sieves having 6 mesh openings of about 19.00 mm, about 12.50 mm, about 8.00 mm, about 6.30 mm, about 3.35 mm, and about 1.60 mm, about 50% by weight or more, 60% by weight or more, 70% by weight or more, or 80% by weight or 90% by weight or more of the polyisobutylene particles are found in the sieve between about 8.00 mm and about 3.35 mm (inclusive).
[0500] Embodiment 50. The method of any one of Embodiments 1 to 49, wherein the removal of the diluent is performed within a time range of 0.1 s to 30 s, preferably within 0.5 to 10 s.
[0501] Embodiment 51. The method of any one of Embodiments 1 to 50, wherein the removal of the organic diluent is carried out within a time range of 0.1 s to 30 s, preferably within 0.5 to 10 s, so that the aqueous slurry contains less than 10 wt.-% of organic diluent, calculated as polyisobutylene contained in the polyisobutylene particles of the obtained aqueous slurry, preferably less than 7 wt.-% and even more preferably less than 5 wt.-% and still even more preferably less than 3 wt.-% and still even more preferably less than 1 wt.-% of organic diluent.
[0502] Embodiment 52. The method of any one of Embodiments 43 to 51, wherein step b) is carried out batchwise or continuously, preferably continuously.
[0503] Embodiment 53. The process of any one of Embodiments 43 to 52, wherein at least one control agent for the initiator system is used in step b).
[0504] Embodiment 54. The method of Embodiment 53, wherein the at least one control agent comprises ethylene, a mono-substituted or di-substituted C3-C 20 Monoolefins, preferably monosubstituted C3-C 20 Monoolefins, more preferably (C3-C 20 )-1-ene, such as 1-butene, is preferably used in an amount of 0.01 to 20% by weight, based on the monomers used in step a), preferably in an amount of 0.2 to 15% by weight and more preferably in an amount of 1 to 15% by weight.
[0505] Embodiment 55. The method of embodiment 53 or 54, wherein the at least one control agent comprises diisobutylene, preferably in an amount of 0.001 to 3 weight percent, based on the monomers used in step a), preferably in an amount of 0.01 to 2 weight percent, and more preferably 0.01 to 1.5 weight percent.
[0506] Embodiment 56. The method of any one of Embodiments 43 to 55, wherein the initiator comprises aluminum chloride, preferably in a weight ratio of isobutylene to aluminum chloride of 500 to 20,000, preferably 1,500 to 10,000.
[0507] Embodiment 57. The method of Embodiment 56, wherein water and / or an alcohol, preferably water, is used as the proton source, preferably in an amount of 0.05 to 2.0 mol water / mol aluminum in aluminum chloride, preferably in the range of 0.1 to 1.2 mol water / mol aluminum in aluminum chloride.
[0508] Embodiment 58. The process of any one of Embodiments 43 to 57, wherein the temperature of step A) is from 10 to 100°C, preferably from 50 to 100°C, more preferably from 60 to 95°C and even more preferably from 75 to 95°C.
[0509] Embodiment 59. The method of any one of Embodiments 1 and 3 to 58, wherein the at least one LCST compound is selected from:
[0510] Poly(N-isopropylacrylamide); Poly(N-isopropylacrylamide-co-N,N-dimethylacrylamide); Poly(N-isopropylacrylamide)-alt-2-hydroxyethyl methacrylate; Poly(N-vinylcaprolactam); Poly(N,N-diethylacrylamide); Poly[2-(dimethylamino)ethyl methacrylate]; Poly(2-oxazoline)glycine copolymer; Poly(3-ethyl-N-vinyl-2-pyrrolidone); Hydroxybutyl chitosan ; polyoxyethylene (20) sorbitan monostearate; polyoxyethylene (20) sorbitan monolaurate; polyoxyethylene (20) sorbitan monooleate; methylcellulose; hydroxypropyl cellulose; hydroxyethyl methylcellulose; hydroxypropyl methylcellulose; poly(ethylene glycol) methacrylate having 2 to 6 ethylene glycol units; polyethylene glycol-co-polypropylene glycol, preferably those having 2 to 6 ethylene glycol units and 2 to 6 polypropylene units; compounds of formula (I)
[0511] (I)HO-[-CH2-CH2-O] x -[-CH(CH3)-CH2-O] y -[-CH2-CH2-O] z -H
[0512] wherein y=3 to 10 and x and z=1 to 8, wherein y+x+z is 5 to 18;
[0513] Polyethylene glycol-co-polypropylene glycol, preferably those having 2 to 8 ethylene glycol units and 2 to 8 polypropylene units; ethoxylated iso-C 13 H 27 -alcohols, preferably having a degree of ethoxylation of 4 to 8; polyethylene glycols having 4 to 50, preferably 4 to 20 ethylene glycol units; polypropylene glycols having 4 to 30, preferably 4 to 15 propylene glycol units; polyethylene glycol monomethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol monoethyl ether and polyethylene glycol diethyl ether having 4 to 50, preferably 4 to 20 ethylene glycol units; polypropylene glycol monomethyl ether, polypropylene glycol dimethyl ether, polypropylene glycol monoethyl ether and polypropylene glycol diethyl ether having 4 to 50, preferably 4 to 20 propylene glycol units; in another embodiment, additionally hydroxyethylcellulose; among which methylcellulose, hydroxypropylcellulose, hydroxyethylmethylcellulose and hydroxypropylmethylcellulose are preferred.
[0514] Embodiment 60. The method of any one of embodiments 1 and 3 to 56, wherein the LCST compound is selected from methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, or a combination thereof.
[0515] Embodiment 61. The method of any one of Embodiments 2 to 56, wherein the cellulose is selected from methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, or a combination thereof.
[0516] Embodiment 62. The method of any one of Embodiments 58 and 59, wherein the cellulose has a degree of substitution (DS) of 0.5 to 2.8, preferably 1.2 to 2.5.
[0517] Embodiment 63. The method of any one of Embodiments 58 to 60, wherein the weight average molecular weight is about 1500 to 3000000, preferably 1500 to 2600000.
[0518] Embodiment 64. The process according to any of Embodiments 1 to 63, wherein the amount of LCST compound present in the aqueous medium used in step A) is from 1 to 20,000 ppm, preferably from 3 to 10,000 ppm, more preferably from 5 to 5,000 ppm and even more preferably from 10 to 5,000 ppm, relative to the amount of polyisobutylene present in the organic medium.
[0519] Embodiment 65. The process according to any one of Embodiments 1 to 64, wherein the amount of LCST compound present in the aqueous medium used in step A) is from 1 to 5,000 ppm, preferably from 3 to 1,000 ppm, more preferably from 5 to 500 ppm and even more preferably from 5 to 100 ppm, relative to the amount of polyisobutylene present in the organic medium.
[0520] Embodiment 66. The method of any one of Embodiments 1 to 65, wherein the LCST compound has a molecular weight of at least 1,500 g / mol, preferably at least 2,500 g / mol and more preferably at least 4,000 g / mol.
[0521] Embodiment 67. The method of any one of Embodiments 43 to 66, comprising a further step wherein the polyisobutylene particles contained in the aqueous slurry are separated to obtain separated polyisobutylene particles.
[0522] Embodiment 68. The method of any one of Embodiments 43 to 67, comprising a further step in which the polyisobutylene particles contained in the aqueous slurry are separated to obtain separated polyisobutylene particles; and comprising a further step in which the (separated) polyisobutylene particles are dried, preferably to a residual content of volatiles of 7,000 or less, preferably 5,000 or less, even more preferably 4,000 or less, and in another embodiment, to 2,000 ppm or less, preferably 1,000 ppm or less.
[0523] Embodiment 69. The method according to any one of embodiments 1 to 68, comprising as a further step shaping the polyisobutylene particles to obtain reshaped polyisobutylene particles such as pellets or shaped articles such as bags.
[0524] Embodiment 70. Aqueous slurry obtainable by the process according to embodiments 1 to 69.
[0525] Embodiment 71. Polyisobutylene particles obtainable by the process according to embodiment 67 or 68.
[0526] Embodiment 72. Reshaped polyisobutylene particles obtainable according to the method of Embodiment 69.
[0527] Embodiment 73. Polyisobutylene compositions, in particular polyisobutylene granules and reshaped polyisobutylene granules, comprising
[0528] I) 96.0 wt% or more, preferably 97.0 wt% or more, more preferably 98.0 wt% or more, even more preferably 99.0 wt% or more, still even more preferably 99.2 wt% or more of polyisobutylene, and in another embodiment 99.5 wt% or more of polyisobutylene
[0529] II) 0 to 3.0 wt. %, preferably 0 to 2.5 wt. %, more preferably 0 to 1.0 wt. % and more preferably 0 to 0.40 wt. %
[0530] · a salt of a monovalent or polyvalent metal ion, or in another embodiment
[0531] stearates and palmitates of polyvalent metal ions, or in another embodiment
[0532] Calcium and zinc stearate and palmitate
[0533] III) 1 ppm to 5,000 ppm, preferably 1 ppm to 2,000 ppm, of at least one LCST compound, and in a more preferred embodiment, 5 to 1,000 ppm or 5 to 500 ppm of at least one LCST compound.
[0534] Embodiment 74. A polyisobutylene composition, in particular (reshaped) polyisobutylene granules, comprising 98.5 wt.-% or more, preferably 98.8 wt.-% or more, more preferably 99.0 wt.-% or more, even more preferably 99.2 wt.-% or more, still even more preferably 99.4 wt.-% or more of polyisobutylene, and in another embodiment 99.5 wt.-% or more of polyisobutylene, and having an ash content of 0.2 wt.-% or less, preferably 0.1 wt.-% or less, more preferably 0.08 wt.-% or less and even more preferably 0.05 wt.-% or less, as measured according to ASTM D5667.
[0535] Embodiment 75. The polyisobutylene composition of Embodiment 74, further comprising 1 ppm to 5,000 ppm, preferably 1 ppm to 2,000 ppm, and in a more preferred embodiment, 5 to 1,000 ppm or 5 to 500 ppm of at least one LCST compound.
[0536] Embodiment 76. Polyisobutylene compositions, in particular (reshaped) polyisobutylene granules and polyisobutylene products, comprising
[0537] 1) 100 parts by weight of polyisobutylene (100 phr)
[0538] II) 0.0001 to 0.5, preferably 0.0001 to 0.2, more preferably 0.0005 to 0.1, even more preferably 0.0005 to 0.05 phr of at least one LCST compound, and
[0539] III) no or 0.0001 to 3.0, preferably no or 0.0001 to 2.0, more preferably no or 0.0001 to 1.0, even more preferably no or 0.0001 to 0.5, still even more preferably no or 0.0001 to 0.3, and most preferably no or 0.0001 to 0.2 phr
[0540] · a salt of a monovalent or polyvalent metal ion, or in another embodiment
[0541] stearates and palmitates of monovalent or polyvalent metal ions, or in another embodiment
[0542] Calcium stearate, calcium palmitate, zinc stearate or zinc palmitate
[0543] and
[0544] IV) no or 0.005 to 0.1, preferably 0.008 to 0.05, more preferably 0.03 to 0.07 phr of antioxidant, and
[0545] V) 0.005 to 0.5, preferably 0.01 to 0.3, more preferably 0.05 to 0.2 phr of volatile matter having a boiling point of 200° C. or lower at standard pressure.
[0546] Embodiment 77. The polyisobutylene composition of embodiment 76, wherein components I) to V) total 100.00501 to 104.100000 parts by weight, preferably 100.01 to 103.00 parts by weight, more preferably 100.10 to 101.50 parts by weight, even more preferably 100.10 to 100.80 parts by weight, and together represent 99.80 to 100.00 wt. %, preferably 99.90 to 100.00 wt. %, more preferably 99.95 to 100.00 wt. % and even more preferably 99.97 to 100.00 wt. % of the total weight of the polyisobutylene composition.
[0547] Embodiment 78. The polyisobutylene particles of embodiment 71, the reshaped polyisobutylene particles of embodiment 72, and the polyisobutylene compositions of embodiments 73 to 77, wherein the viscosity average molecular weight (M v) is in the range of 100 to 3,000 kg / mol, preferably in the range of 250 to 3,000 kg / mol, or in another embodiment, in the range of 100 to 2,000 kg / mol, preferably in the range of 200 to 2,000 kg / mol, more preferably in the range of 350 to 1,800 kg / mol, even more preferably in the range of 400 to 1500 kg / mol and still even more preferably 700 to 1300 kg / mol, or in another embodiment, the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 2,001 to 3,000 kg / mol, or in yet another embodiment, the viscosity average molecular weight (M v ) is in the range of 3,001 to 10,000 kg / mol.
[0548] Embodiment 79. The polyisobutylene particles of Embodiment 71, the reshaped polyisobutylene particles of Embodiment 72, and the polyisobutylene compositions of Embodiments 73 to 78, wherein the polyisobutylene has a polydispersity in the range of 1.1 to 6.0, preferably 3.0 to 5.5, as measured by the ratio of the weight average molecular weight to the number average molecular weight as determined by gel permeation chromatography.
[0549] Embodiment 80. The polyisobutylene particles of embodiment 71, the reshaped polyisobutylene particles of embodiment 72, and the polyisobutylene compositions of embodiments 73 to 79, wherein the Mooney viscosity of the polyisobutylene is at least 10 (ML 125°C 1+8, ASTM D 1646-07 (2012)), preferably 10 to 80, more preferably 20 to 80 and even more preferably 25 to 60 (ML 125°C 1+8, ASTM D 1646-07 (2012)).
[0550] Embodiment 81. The reshaped polyisobutylene particles of embodiments 72 and 78 to 80, wherein they are pellets or shaped articles, or are formed into pellets or shaped articles, the shaped articles are preferably bags.
[0551] Embodiment 82. Shaped articles, in particular pellets or bags, obtainable by shaping the polyisobutylene granules of embodiments 71, 78 to 80 or the reshaped polyisobutylene granules of embodiments 72, 78 to 81.
[0552] Embodiment 83. A blend or mixture obtainable by blending or mixing the polyisobutylene particles, reshaped polyisobutylene particles or polyisobutylene compositions or shaped articles of embodiments 71 to 82.
[0553] Embodiment 84. Use of the polyisobutylene particles, reshaped polyisobutylene particles or polyisobutylene compositions or shaped articles of embodiments 71 to 82 or the blends and mixtures of embodiment 83 for sealants, coatings, adhesives and roofing materials.
[0554] Embodiment 85. Sealants, adhesives, coatings and roofing materials made from or comprising the polyisobutylene particles, reshaped polyisobutylene particles or polyisobutylene compositions or shaped articles of embodiments 71 to 82 or the blends and mixtures of embodiment 83.
[0555] The present invention is further illustrated below by examples, but the present invention is not limited thereto.
[0556] Experimental Section
[0557] Examples 1 and 2
[0558] A polyisobutylene cement was prepared by dissolving polyisobutylene having a weight average molecular weight of 750,000, a viscosity average molecular weight of 800,000, and a polydispersity of 0.5 in hexane (-80% n-hexane, the remainder being branched hexane isomers). The total concentration of polyisobutylene in the cement was 5 wt%. This cement (71 g, 3.55 g total polyisobutylene by mass) was pumped into a stirred vessel containing 1% ethanol using a peristaltic pump at a flow rate of 50 mL / min.
[0559] Experiment 1): 2L deionized water at 65°C under atmospheric pressure
[0560] Experiment 2): 2 L of deionized water containing 0.01 g (or 0.12 wt %, relative to polyisobutylene) of methylcellulose.
[0561] As the binder enters the container containing the water, low pressure steam (approximately 5-10 psi) is injected into the binder stream.
[0562] For experiment 1, coarse agglomerates were formed, and in experiment 2, isolated polyisobutylene pellets were obtained.
[0563] The methylcellulose used was methylcellulose model M 0512 purchased from Sigma Aldrich, having a viscosity of 4000 cp at 2 wt% in water and 20°C, a molecular weight of 88,000, a degree of substitution of 1.5 to 1.9, and a methoxy substitution of 27.5 to 31.5 wt%.
[0564] The turbidity point thereof measured by method 5) was 39.0°C, and the turbidity point thereof measured by method 4) was 37.8°C.
[0565] Examples 3a to 3c
[0566] Continuous polyisobutylene granule formation:
[0567] Isobutylene is combined with methyl chloride and optionally diisobutylene to prepare a polymerization feed such that the total monomer concentration is about 15 to 18 weight percent with diisobutylene added in an amount of 0 to 0.1 weight percent of the isobutylene content. This feed stream is cooled to about -100°C and continuously fed to a stirred reaction vessel, which is also maintained at -100°C. In the reaction vessel, the feed is mixed with a continuously added initiator system stream, a 0.05 to 0.5 weight percent aluminum chloride solution in methyl chloride, which is activated with water in a molar ratio of water to aluminum chloride of 0.1:1 to 1:1. The feed and initiator system addition rates are adjusted in a conventional manner to provide a viscosity average molecular weight M v Polyisobutylene between 250,000 g / mol and 3,000,000 g / mol. Typically, the weight ratio of monomer to aluminum chloride in the feed stream is maintained in the range of 500 to 20,000, preferably 1,500 to 10,000.
[0568] To control the molecular weight of the polymer, diisobutylene (DIB) is added as a chain transfer agent. Thus, the amount of DIB varies depending on the desired molecular weight of the final product. For the highest molecular weight, no DIB is needed, and more DIB is added sequentially within the above range to reduce the molecular weight.
[0569] In the stirred reaction vessel, the polyisobutylene is obtained in the form of a finely divided slurry suspended in methyl chloride.
[0570] The reaction vessel is set up and operated so that the continuously added feedstock exceeds the volume of the reactor. When this volume is exceeded, the well-mixed reaction slurry containing methyl chloride, unreacted monomers and polyisobutylene is overflowed into another stirred container containing water, which is heated from 65° C. to 100° C. and used in an amount of 15:1 to 6:1 by weight (calculated based on polyisobutylene). Thus, most of the diluent methyl chloride is removed from the slurry.
[0571] After the solvent and monomer stripping is complete, before the polymer is dehydrated and finished, 100 to 500 ppm of 1010 is added to the aqueous medium. It is also possible to add this antioxidant earlier in the stripping process, or even add it directly to the finishing process after dehydration.
[0572] The addition of 50 to 500 ppm of methylcellulose (calculated on the basis of polyisobutylene) enables the formation of an aqueous slurry of polyisobutylene particles, wherein the concentration of copolymer particles in the aqueous slurry increases as the polymerization proceeds. The aqueous slurry is then dehydrated and dried using conventional means to provide a copolymer suitable for testing and analysis.
[0573] Higher or lower values were not tested in this experiment, however, the behavior indicates that levels above or below this range may be used successfully, depending on the desired adhesion of the polyisobutylene in the aqueous medium.
[0574] The methylcellulose used had a solution viscosity of 3000-5600 cps at 2 wt% solution, a molecular weight Mw of -90,000, a methoxy substitution of 27.5-31.5 wt%, and thus a degree of substitution of about 1.9.
[0575] Its turbidity point measured by method 5) is 39.0°C, and its turbidity point measured by method 4) is 37.8°C:
[0576] 5: DIN EN 1890, method A, September 2006, wherein the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.2 g / 100 ml distilled water.
[0577] 4: DIN EN 1890, method A, September 2006, wherein the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.04 g / 100 ml distilled water.
[0578] Using the experimental setup described above, after separation of the particles from the aqueous slurry and drying, three products were obtained which were distinguishable by their Mv ranges.
[0579] The viscosity average molecular weight is determined by measuring the viscosity of a solution of polyisobutylene in isooctane using an Ubbelohde viscometer and then comparing the viscosity to a known value. The test is performed as follows:
[0580] A polyisobutylene sample (0.0400 + / - 0.0050 g) was dissolved in 20 mL of isooctane. 11 mL of this solution was transferred to an Ubbelohde viscometer, which was then equilibrated in a temperature-controlled bath at 20° C. for 10 min. The solution was aspirated into the reservoir above the start timer of the viscometer using a pipette bulb. The pipette bulb was then removed to allow the solution to flow.
[0581] The time, t, is measured as the time (in seconds) for the meniscus to move from the start line to the stop line of the viscometer. This measurement is performed three times and the average is compared to a table of known viscosities to determine Mv.
[0582] The analytical data of the three products obtained are as follows:
[0583] Generally, if not mentioned otherwise, all analytical data were obtained according to the methods described in the above specification.
[0584] Molecular weight and polydispersity were determined by gel permeation chromatography in tetrahydrofuran and expressed as kg mol -1 The content of hindered phenolic antioxidant (IrganoxTM1010) was determined by HPLC and the result is expressed in weight %. The total unsaturation and microstructure are expressed by 1 The corresponding signals of the H NMR spectrum were determined and expressed in mol %.
[0585] Example 3a
[0586] Total unsaturation: <0.04 mol%
[0587] Mv: 620,000-950,000 g / mol, with a specific run (SR) Mv of 819,400
[0588] Polydispersity SR (Mw / Mn): 1.71
[0589] Calcium: <50ppm, SR: 24ppm
[0590] Calcium stearate content: below detection limit (completely)
[0591] Methylcellulose content: <0.05% by weight
[0592] 1010: 0.030-0.100 wt%
[0593] Volatile matter SP: 0.048 wt%
[0594] Other anti-agglomeration agents, surfactants, emulsifiers: None
[0595] Ions: (ICP-AES)
[0596] Aluminum SR (from catalyst): 17ppm
[0597] Magnesium SR: 32ppm
[0598] Other polyvalent metal ions SR (Mn, Pb, Cu, Cr, Ba, Fe, Zn): 24ppm Monovalent metal ions SR (Na, K): 29ppm
[0599] Total ash SR: (ASTM D5667) 0.008 wt%
[0600] Example 3b:
[0601] Total unsaturation: <0.04 mol%
[0602] Mv: 1,000,000-1,350,000 g / mol
[0603] Calcium: <50ppm
[0604] Calcium stearate content: below the detection limit
[0605] Methylcellulose content: <0.05% by weight
[0606] 1010: 0.030-0.100 wt%
[0607] Volatile matter: 0.3 wt%
[0608] Example 3c:
[0609] Total unsaturation: <0.04 mol%
[0610] Mv: 2,300,000-2,850,000 g / mol
[0611] Calcium: <50ppm
[0612] Calcium stearate content: below the detection limit
[0613] Methylcellulose content: <0.05% by weight
[0614] 1010: 0.030-0.100 wt%
[0615] Volatile matter: 0.3 wt%
[0616] For products 3b and 3c, the ash content was also found to be less than 0.2 wt%.
[0617] Thus, the polyisobutylene granules of Examples 3a to 3c comprise:
[0618] 1) 100 parts by weight of polyisobutylene (100 phr)
[0619] II) <0.005 phr of at least one LCST compound, and
[0620] III) less than 0.001 phr of a non-LCST compound selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, and
[0621] IV) 0.03 to 0.1 phr of an antioxidant
[0622] V) about 0.3 phr of volatiles having a boiling point of 200° C. or less at standard pressure
[0623] These components constitute more than 99.9% by weight of the total weight of the polyisobutylene particles.
[0624] Examples 4 to 7
[0625] The polyisobutylene adhesive was prepared by dissolving 2.8 g of polyisobutylene in 765 ml of hexane (-80% n-hexane, the remainder being branched hexane isomers). The total concentration of polyisobutylene in the adhesive was about 2.5 wt%. This adhesive was pumped at 15 rpm into a beaker containing 1 L of water that had been preheated with low pressure steam for 1 min using a peristaltic pump. Steam was then added to the adhesive for a further 2 min.
[0626] Before preheating the water, 6.25 mg of the LCST compound methylcellulose, hydroxyethylmethylcellulose or hydroxypropylmethylcellulose (or 2230 ppm, calculated on the polyisobutylene content in the organic medium) was added to the aqueous phase in the form of 0.25 ml of a 2.5 wt% aqueous solution.
[0627] For comparison, 100.00 mg of calcium stearate (or 35700 ppm, calculated based on the polyisobutylene content in the organic medium) was added to the aqueous phase in the form of 0.2 ml of a 50 wt% aqueous solution before preheating. Alternatively, the non-LCST compounds mentioned below were added or not before preheating.
[0628] Then check the formation of pellets:
[0629] FAIL means that the formation of discrete polyisobutylene particles was not observed, but sedimentation of a single material was observed.
[0630] PASS means that the formation of discrete polyisobutylene particles was observed.
[0631] The results are given in Table 1 below:
[0632] Table 1:
[0633]
[0634] 1*: weight average molecular weight of 340,000, viscosity average molecular weight of 400,000 and polydispersity of 5.0
[0635] 2*: Weight average molecular weight of 750,000, viscosity average molecular weight of 800,000 and polydispersity of 5.0
[0636] 3*: Weight average molecular weight of 1,100,000, viscosity average molecular weight of 1,110,000 and polydispersity of 5.0
[0637] 4*: Weight average molecular weight is 2,500,000, viscosity average molecular weight is 2,600,000 and polydispersity is 5.0
[0638] 5*: The methylcellulose used has a solution viscosity of 3000-5600 cps at 2 wt% solution, a molecular weight Mw of -90,000, a methoxy substitution of 27.5-31.5 wt% and thus a degree of substitution of about 1.9.
[0639] 6*: Viscosity 600-1500 mPas, 2 wt% in water (20°C), Sigma
[0640] 7*: Viscosity 2,600-5,600 cp (2 wt% in water at 20°C), H7509, Sigma
[0641] **: For comparison
[0642] LCST compounds Cloud point[℃] method Methylcellulose(*5) 39.0 5) Methylcellulose(*5) 37.8 4) Hydroxyethyl methyl cellulose (*6) 80.8 5) Hydroxyethyl methyl cellulose (*6) 80.6 4) Hydroxypropyl methylcellulose (*7) 49.9 4)
Claims
1. A method for preparing an aqueous slurry comprising a plurality of polyisobutylene particles suspended therein, the method comprising at least the following steps: A) bringing the organic medium into contact with the aqueous medium, The organic medium comprises i) polyisobutylene, and ii) organic diluent, The aqueous medium comprises at least one LCST compound having a cloud point of 0 to 100° C., and at least partially removing the organic diluent to obtain an aqueous slurry containing polyisobutylene particles, wherein the amount of the LCST compound present in the aqueous medium used in step A) is from 1 to 20,000 ppm, relative to the amount of polyisobutylene present in the organic medium; The LCST compound is selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, hydroxyalkyl alkyl cellulose and carboxyalkyl cellulose; and The aqueous medium contains 20,000 ppm or less of non-LCST compounds, calculated relative to the amount of polyisobutylene present in the organic medium, wherein the non-LCST compounds are selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents.
2. The method of claim 1, wherein the LCST compound has a cloud point of 5 to 100°C.
3. The method of claim 1, wherein the LCST compound has a cloud point of 15 to 80°C.
4. The method of claim 1, wherein the LCST compound has a cloud point of 20 to 70°C.
5. The method of claim 1, wherein the LCST compound is a LCST compound having a turbidity point of 0 to 100°C, the turbidity point being determined by at least one of the following methods: DIN EN 1890, Method A, September 2006 DIN EN 1890, Method C, September 2006 DIN EN 1890, Method E, September 2006 DIN EN 1890, September 2006, Method A, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water DIN EN 1890, method A, September 2006, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.2 g / 100 ml distilled water.
6. The method of claim 1, wherein the LCST compound is a LCST compound having a turbidity point of 0 to 100°C, the turbidity point being determined by at least one of the following methods: DIN EN 1890, Method A, September 2006 DIN EN 1890, Method E, September 2006 DIN EN 1890, method A, September 2006, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water.
7. The method of claim 1, wherein the LCST compound is a LCST compound having a turbidity point of 0 to 100°C, the turbidity point being determined by at least one of the following methods: DIN EN 1890, Method A, September 2006 DIN EN 1890, Method C, September 2006 DIN EN 1890, method A, September 2006, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water.
8. The method of claim 1, wherein the LCST compound is a LCST compound having a turbidity point of 10 to 90°C, the turbidity point being determined by the following method: DIN EN 1890, method A, September 2006, where the amount of the tested compound is reduced from 1 g / 100 ml distilled water to 0.05 g / 100 ml distilled water.
9. The method of claim 1, wherein the LCST compound is selected from cellulose compounds, wherein at least one hydroxyl functional group -OH of the cellulose is functionalized to form one of the following groups: OR c , where R c is methyl, 2-hydroxyethyl, 2-methoxyethyl, 2-methoxypropyl, 2-hydroxypropyl, -(CH2-CH2O) n H, -(CH2-CH2O) n CH3, -(CH2-CH(CH3)O) n H, -(CH2-CH(CH3)O) n CH3, wherein n is an integer from 1 to 20.
10. The method of claim 9, wherein n is an integer from 3 to 20.
11. The method of claim 1, wherein the alkyl cellulose, hydroxyalkyl cellulose and carboxyalkyl cellulose have a degree of substitution (DS) of 0.5 to 2.
8.
12. The method of claim 11, wherein the alkyl cellulose, hydroxyalkyl cellulose and carboxyalkyl cellulose have a degree of substitution (DS) of 1.2 to 2.
5.
13. The process of claim 1, wherein the organic medium comprising polyisobutylene and an organic diluent is obtained by polymerization.
14. The process of claim 13, wherein the organic medium is obtained from a polymerization reaction and further contains residual polyisobutylene from the polymerization reaction.
15. The method of any one of claims 1 to 14, wherein the aqueous medium comprises 10,000 ppm or less of non-LCST compounds.
16. The method according to claim 15, wherein the aqueous medium contains 8,000 ppm or less of non-LCST compounds.
17. The method according to claim 15, wherein the aqueous medium contains 5,000 ppm or less of non-LCST compounds.
18. The method according to claim 15, wherein the aqueous medium contains 2,000 ppm or less of non-LCST compounds.
19. The method according to claim 15, wherein the aqueous medium contains 1,000 ppm or less of non-LCST compounds.
20. The method of any one of claims 1 to 14, wherein the aqueous medium comprises 500 ppm or less of non-LCST compounds.
21. The method according to claim 20, wherein the aqueous medium contains 100 ppm or less of non-LCST compounds.
22. The method according to claim 20, wherein the aqueous medium contains 50 ppm or less of non-LCST compounds.
23. The method according to claim 20, wherein the aqueous medium contains 30 ppm or less of non-LCST compounds.
24. The method according to claim 20, wherein the aqueous medium contains 10 ppm or less of non-LCST compounds.
25. The process according to any one of claims 1 to 14, wherein the aqueous medium comprises from 0 to 5,000 ppm of a salt of a monovalent or polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
26. The process of claim 25, wherein the aqueous medium comprises from 0 to 2,000 ppm of a salt of a monovalent or polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
27. The process of claim 25, wherein the aqueous medium comprises from 10 to 1,000 ppm of a salt of a monovalent or polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
28. The process of claim 25, wherein the aqueous medium comprises from 50 to 800 ppm of a salt of a monovalent or polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
29. The process of claim 25, wherein the aqueous medium comprises from 100 to 600 ppm of a salt of a monovalent or polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
30. The process of any one of claims 1 to 14, wherein the aqueous medium comprises from 0 to 5,000 ppm of a salt of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
31. The process of claim 30, wherein the aqueous medium comprises from 0 to 2,000 ppm of a salt of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
32. The method of claim 30, wherein the aqueous medium comprises from 10 to 1,000 ppm of the salt of the polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
33. The process of claim 30, wherein the aqueous medium comprises from 50 to 800 ppm of the salt of the polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
34. The process of claim 30, wherein the aqueous medium comprises from 100 to 600 ppm of a salt of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
35. The process of any one of claims 1 to 14, wherein the aqueous medium contains 550 ppm or less of the salt of the metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
36. The process of claim 35, wherein the aqueous medium contains 400 ppm or less of the salt of the metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
37. The process of claim 35, wherein the aqueous medium contains 300 ppm or less of the salt of the metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
38. The process of claim 35, wherein the aqueous medium contains 250 ppm or less of the salt of the metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
39. The process of claim 35, wherein the aqueous medium contains 150 ppm or less of the salt of the metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
40. The method of claim 35, wherein the aqueous medium contains 100 ppm or less of the salt of the metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
41. The process of any one of claims 1 to 14, wherein the aqueous medium contains 550 ppm or less of the salt of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
42. The process of claim 41, wherein the aqueous medium contains 400 ppm or less of the salt of the polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
43. The process of claim 41, wherein the aqueous medium contains 300 ppm or less of the salt of the polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
44. The process of claim 41, wherein the aqueous medium contains 250 ppm or less of the salt of the polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
45. The process of claim 41, wherein the aqueous medium contains 150 ppm or less of the salt of the polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
46. The method of claim 41, wherein the aqueous medium contains 100 ppm or less of a salt of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
47. The process of any one of claims 1 to 14, wherein the aqueous medium comprises 8,000 ppm or less of non-LCST compounds selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
48. The method of claim 47, wherein the aqueous medium comprises 5,000 ppm or less of non-LCST compounds selected from the group consisting of ionic or nonionic surfactants, emulsifiers, and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
49. The method of claim 47, wherein the aqueous medium comprises 2,000 ppm or less of non-LCST compounds selected from ionic or nonionic surfactants, emulsifiers, and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
50. The method of claim 47, wherein the aqueous medium comprises 1,000 ppm or less of a non-LCST compound selected from the group consisting of ionic or nonionic surfactants, emulsifiers, and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
51. The method of claim 47, wherein the aqueous medium comprises 500 ppm or less of non-LCST compounds selected from the group consisting of ionic or nonionic surfactants, emulsifiers, and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
52. The method of claim 47, wherein the aqueous medium comprises 100 ppm or less of non-LCST compounds selected from the group consisting of ionic or nonionic surfactants, emulsifiers, and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
53. The method of claim 47, wherein the aqueous medium comprises 15 ppm or less of non-LCST compounds selected from the group consisting of ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
54. The process of claim 47, wherein the aqueous medium comprises from 1 ppm to 10 ppm of non-LCST compounds selected from ionic or nonionic surfactants, emulsifiers and anti-agglomeration agents, relative to the amount of polyisobutylene present in the organic medium.
55. The process of any one of claims 1 to 14, wherein the aqueous medium contains 70 ppm or less of the salt of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
56. The process of claim 55, wherein the aqueous medium contains 50 ppm or less of the salt of the polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
57. The process of claim 55, wherein the aqueous medium contains 30 ppm or less of the salt of the multivalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
58. The method of claim 55, wherein the aqueous medium contains 20 ppm or less of the salt of the multivalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
59. The method of claim 55, wherein the aqueous medium contains 10 ppm or less of the salt of the multivalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
60. The process of any one of claims 1 to 14, wherein the aqueous medium contains 25 ppm or less of a salt of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
61. The method of claim 60, wherein the aqueous medium contains 10 ppm or less of the salt of the multivalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
62. The method of claim 60, wherein the aqueous medium contains 8 ppm or less of the salt of the multivalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
63. The method of claim 60, wherein the aqueous medium contains 7 ppm or less of the salt of the multivalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
64. The method of claim 60, wherein the aqueous medium contains 5 ppm or less of the salt of the multivalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
65. The process of any one of claims 1 to 14, wherein the aqueous medium contains 550 ppm or less of a carboxylate of a polyvalent metal ion, calculated as a metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having from 6 to 30 carbon atoms.
66. The method of claim 65, wherein the aqueous medium contains 400 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
67. The method of claim 65, wherein the aqueous medium contains 300 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
68. The method of claim 65, wherein the aqueous medium contains 250 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
69. The method of claim 65, wherein the aqueous medium contains 150 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
70. The method of claim 65, wherein the aqueous medium contains 100 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
71. The method of claim 65, wherein the carboxylic acid is selected from carboxylic acids having from 8 to 24 carbon atoms.
72. The method of claim 65, wherein the carboxylic acid is selected from carboxylic acids having 12 to 18 carbon atoms.
73. The process of any one of claims 1 to 14, wherein the aqueous medium contains 70 ppm or less of a carboxylate of a polyvalent metal ion, calculated as a metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having from 6 to 30 carbon atoms.
74. The process of claim 73, wherein the aqueous medium contains 50 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
75. The method of claim 73, wherein the aqueous medium contains 30 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
76. The method of claim 73, wherein the aqueous medium contains 20 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
77. The method of claim 73, wherein the aqueous medium contains 10 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
78. The method of claim 73, wherein the carboxylic acid is selected from carboxylic acids having from 8 to 24 carbon atoms.
79. The method of claim 73, wherein the carboxylic acid is selected from carboxylic acids having 12 to 18 carbon atoms.
80. The process of any one of claims 1 to 14, wherein the aqueous medium contains 25 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as a metal content relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having from 6 to 30 carbon atoms.
81. The method of claim 80, wherein the aqueous medium contains 10 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
82. The method of claim 80, wherein the aqueous medium contains 8 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
83. The method of claim 80, wherein the aqueous medium contains 7 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
84. The method of claim 80, wherein the aqueous medium contains 5 ppm or less of a carboxylate salt of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
85. The method of claim 80, wherein the carboxylic acid is selected from carboxylic acids having from 8 to 24 carbon atoms.
86. The method of claim 80, wherein the carboxylic acid is selected from carboxylic acids having 12 to 18 carbon atoms.
87. The method of any one of claims 1 to 14, wherein the aqueous medium does not contain a carboxylate salt of a polyvalent metal ion, wherein the carboxylic acid is selected from carboxylic acids having from 6 to 30 carbon atoms.
88. The method of claim 87, wherein the carboxylic acid is selected from carboxylic acids having from 8 to 24 carbon atoms.
89. The method of claim 87, wherein the carboxylic acid is selected from carboxylic acids having 12 to 18 carbon atoms.
90. The process of any one of claims 1 to 14, wherein the aqueous medium contains 100 ppm or less of a salt of a monovalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
91. The method of claim 90, wherein the aqueous medium contains 50 ppm or less of a salt of a monovalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
92. The method of claim 90, wherein the aqueous medium contains 20 ppm or less of a salt of a monovalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
93. The method of claim 90, wherein the aqueous medium contains 15 ppm or less of a salt of a monovalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
94. The method of claim 90, wherein the aqueous medium contains 10 ppm or less of a salt of a monovalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
95. The process of any one of claims 1 to 14, wherein the aqueous medium additionally or alternatively comprises 100 ppm or less of carboxylates of monovalent metal ions selected from sodium stearate, sodium palmitate and sodium oleate and potassium stearate, potassium palmitate and potassium oleate, calculated on the basis of their metal content and relative to the amount of polyisobutylene present in the organic medium, wherein the carboxylic acid is selected from carboxylic acids having from 6 to 30 carbon atoms.
96. The method of claim 95, wherein the aqueous medium additionally or alternatively comprises 50 ppm or less of a carboxylate salt of a monovalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
97. The method of claim 95, wherein the aqueous medium additionally or alternatively comprises 30 ppm or less of a carboxylate salt of a monovalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
98. The method of claim 95, wherein the aqueous medium additionally or alternatively comprises 20 ppm or less of a carboxylate salt of a monovalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
99. The method of claim 95, wherein the aqueous medium additionally or alternatively comprises 10 ppm or less of a carboxylate salt of a monovalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
100. The method of claim 95, wherein the aqueous medium additionally or alternatively comprises 5 ppm or less of a carboxylate salt of a monovalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
101. The method of claim 95, wherein the carboxylic acid is selected from carboxylic acids having from 8 to 24 carbon atoms.
102. The method of claim 95, wherein the carboxylic acid is selected from carboxylic acids having 12 to 18 carbon atoms.
103. The method of claim 95, wherein the carboxylic acid is selected from monocarboxylic acids.
104. The method of any one of claims 1 to 14, wherein the aqueous medium does not contain carboxylate salts of monovalent metal ions, wherein the carboxylic acid is selected from carboxylic acids having from 6 to 30 carbon atoms.
105. The method of claim 104, wherein the carboxylic acid is selected from carboxylic acids having from 8 to 24 carbon atoms.
106. The method of claim 104, wherein the carboxylic acid is selected from carboxylic acids having 12 to 18 carbon atoms.
107. The method of claim 65, wherein the carboxylic acid is selected from monocarboxylic acids.
108. The method of claim 73, wherein the carboxylic acid is selected from monocarboxylic acids.
109. The method of claim 80, wherein the carboxylic acid is selected from monocarboxylic acids.
110. The method of claim 87, wherein the carboxylic acid is selected from monocarboxylic acids.
111. The method of claim 104, wherein the carboxylic acid is selected from monocarboxylic acids.
112. The method of any one of claims 107 to 111, wherein the carboxylic acid is selected from saturated monocarboxylic acids.
113. The method of any one of claims 107 to 111, wherein the carboxylic acid is selected from palmitic acid or stearic acid.
114. The process of any one of claims 1 to 14, wherein the aqueous medium comprises from 0 to 5,000 ppm of carbonate of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
115. The process of claim 114, wherein the aqueous medium comprises from 0 to 2,000 ppm of carbonate of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
116. The process of claim 114, wherein the aqueous medium comprises from 10 to 1,000 ppm of carbonate of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
117. The process of claim 114, wherein the aqueous medium comprises from 50 to 800 ppm of carbonate of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
118. The process of claim 114, wherein the aqueous medium comprises from 100 to 600 ppm of carbonate of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
119. The method of claim 114, wherein the carbonates of the polyvalent metal ions are magnesium carbonate and calcium carbonate.
120. The method of any one of claims 1 to 14, wherein the aqueous medium comprises 550 ppm or less of: Carbonates of polyvalent metal ions, calculated on the basis of their metal content relative to the amount of polyisobutylene present in the organic medium.
121. The method of claim 120, wherein the aqueous medium comprises 400 ppm or less of: Carbonates of polyvalent metal ions, calculated on the basis of their metal content relative to the amount of polyisobutylene present in the organic medium.
122. The method of claim 120, wherein the aqueous medium comprises 300 ppm or less of: Carbonates of polyvalent metal ions, calculated on the basis of their metal content relative to the amount of polyisobutylene present in the organic medium.
123. The method of claim 120, wherein the aqueous medium comprises 250 ppm or less of: Carbonates of polyvalent metal ions, calculated on the basis of their metal content relative to the amount of polyisobutylene present in the organic medium.
124. The method of claim 120, wherein the aqueous medium comprises 150 ppm or less of: Carbonates of polyvalent metal ions, calculated on the basis of their metal content relative to the amount of polyisobutylene present in the organic medium.
125. The method of claim 120, wherein the carbonates of the polyvalent metal ions are magnesium carbonate and calcium carbonate.
126. The process of any one of claims 1 to 14, wherein the aqueous medium contains 70 ppm or less of carbonate of a polyvalent metal ion, calculated as its metal content and relative to the amount of polyisobutylene present in the organic medium.
127. The method of claim 126, wherein the aqueous medium contains 50 ppm or less of carbonate of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
128. The method of claim 126, wherein the aqueous medium contains 30 ppm or less of carbonate of a polyvalent metal ion, calculated as the metal content relative to the amount of polyisobutylene present in the organic medium.
129. The method of claim 126, wherein the aqueous medium contains 20 ppm or less of carbonate of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
130. The method of claim 126, wherein the aqueous medium contains 10 ppm or less of carbonate of a polyvalent metal ion, calculated as the metal content thereof and relative to the amount of polyisobutylene present in the organic medium.
131. The method of claim 126, wherein the carbonates of the polyvalent metal ions are magnesium carbonate and calcium carbonate.
132. The method of any one of claims 1 to 14, wherein the aqueous medium comprises 500 ppm or less of layered minerals, calculated relative to the amount of polyisobutylene present in the organic medium.
133. The method of claim 132, wherein the aqueous medium contains 200 ppm or less of layered minerals, calculated relative to the amount of polyisobutylene present in the organic medium.
134. The method of claim 132, wherein the aqueous medium contains 100 ppm or less of layered minerals, calculated relative to the amount of polyisobutylene present in the organic medium.
135. The method of claim 132, wherein the aqueous medium contains 50 ppm or less of the layered mineral, calculated relative to the amount of polyisobutylene present in the organic medium.
136. The method of claim 132, wherein the aqueous medium contains 20 ppm or less of layered minerals, calculated relative to the amount of polyisobutylene present in the organic medium.
137. The method of claim 132, wherein the aqueous medium does not contain layered minerals.
138. The method of claim 132, wherein the layered mineral is talc.
139. The method of any one of claims 1 to 14, wherein the aqueous medium comprises 500 ppm or less of a dispersant, emulsifier, or anti-agglomeration agent other than a LCST compound.
140. The method of claim 139, wherein the aqueous medium comprises 200 ppm or less of a dispersant, emulsifier, or anti-agglomeration agent other than a LCST compound.
141. The method of claim 139, wherein the aqueous medium comprises 100 ppm or less of a dispersant, emulsifier, or anti-agglomeration agent other than a LCST compound.
142. The method of claim 139, wherein the aqueous medium comprises 20 ppm or less of a dispersant, emulsifier, or anti-agglomeration agent other than a LCST compound.
143. The method of claim 139, wherein the aqueous medium comprises 10 ppm or less of a dispersant, emulsifier, or anti-agglomeration agent other than a LCST compound.
144. The method of claim 139, wherein the aqueous medium comprises 5 ppm or less of a dispersant, emulsifier, or anti-agglomeration agent other than a LCST compound.
145. The method of claim 139, wherein the aqueous medium does not comprise a dispersant, emulsifier, or anti-agglomeration agent other than the LCST compound.
146. The process of any one of claims 1 to 14, wherein the polyisobutylene particles are discrete particles of any form and consistency, the discrete particles having a particle size between 0.05 mm and 25 mm.
147. The method of claim 146, wherein the discrete particles have a particle size between 0.1 and 20 mm.
148. The process of any one of claims 1 to 14, wherein the polyisobutylene particles have a weight average particle size of 0.3 to 10.0 mm.
149. The process of any one of claims 1 to 14, wherein 90% by weight or more of the polyisobutylene particles are between 12.50 mm and 1.6 mm in size, and 80% by weight or more of the polyisobutylene particles are between 8.00 mm and 3.35 mm in size, as determined by sieving.
150. The process of any one of claims 1 to 14, wherein the aqueous medium contains 1 to 2,000 ppm of an antioxidant and / or stabilizer, calculated relative to the amount of polyisobutylene present in the organic medium, wherein the antioxidant and stabilizer is 2,6-di-tert-butyl-4-methyl-phenol, pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid, 3,5-di(tert-butyl)-4-hydroxyhydrocinnamic acid octadecyl ester, tert-butyl-4-hydroxyanisole, 2-(1,1-dimethyl)-1,4-benzenediol, tris(2,4-di-tert-butylphenyl) phosphate, dioctyldiphenylamine, p-cresol and butylated products of dicyclopentadiene or 2,4,6-tri-tert-butylphenol, 2,4 ,6-triisobutylphenol, 2-tert-butyl-4,6-dimethylphenol, 2,4-dibutyl-6-ethylphenol, 2,4-dimethyl-6-tert-butylphenol, 2,6-di-tert-butylhydroxytoluene (BHT), 2,6-di-tert-butyl-4-ethylphenol, 2,6-di-tert-butyl-4-n-butylphenol, 2,6-di-tert-butyl-4-isobutylphenol, 2,6-dicyclopentyl-4-methylphenol, 4-tert-butyl-2,6-dimethylphenol, 4-tert-butyl-2,6-dicyclopentylphenol, 4-tert-butyl-2,6-diisopropylphenol, 4,6-di-tert-butyl-2-methylphenol, 6-tert-butyl-2,4-dimethylphenol, 2,6-di-tert-butyl-3-methylphenol, 4-hydroxymethyl- 2,6-di-tert-butylphenol, 2,6-di-tert-butyl-4-phenylphenol and 2,6-di-octadecyl-4-methylphenol, 2,2'-ethylene-bis[4,6-di-tert-butylphenol], 2,2'-ethylene-bis[6-tert-butyl-4-isobutylphenol], 2,2'-isobutylene-bis[4,6-dimethyl-phenol], 2,2'-methylene-bis[4,6-di-tert-butylphenol], 2,2'-methylene-bis[4-methyl-6-(α-methylcyclohexyl)phenol], 2,2'-methylene-bis[4-methyl-6-cyclohexylphenol], 2,2'-methylene-bis[4-methyl-6-nonylphenol], 2,2'-methylene-bis[6-(α,α'-dimethylbenzyl)phenol] -4-nonylphenol], 2,2'-methylene-bis[6-(α-methylbenzyl)-4-nonylphenol], 2,2'-methylene-bis[6-cyclohexyl-4-methylphenol], 2,2'-methylene-bis[6-tert-butyl-4-ethylphenol], 2,2'-methylene-bis[6-tert-butyl-4-methylphenol], 4,4'-butylene-bis[2-tert-butyl-5-methylphenol], 4,4'-methylene-bis[2,6-di-tert-butylphenol], 4,4'-methylene-bis[6-tert-butyl-2-methylphenol], 4,4'-isopropylidene-biphenol, 4,4'-decylene-bisphenol, 4,4'-dodecylene-bisphenol, 4,4'-(1-methyloctylene)bisphenol, 4,4'-cyclohexylidene-bis(2-methylphenol), 4,4'-cyclohexylidenebisphenol and pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionic acid.
151. The method of claim 150, wherein the aqueous medium comprises from 50 to 1,000 ppm of an antioxidant and / or stabilizer, calculated relative to the amount of polyisobutylene present in the organic medium.
152. The method of claim 150, wherein the aqueous medium comprises from 80 to 500 ppm of an antioxidant and / or stabilizer, calculated relative to the amount of polyisobutylene present in the organic medium.
153. The method of any one of claims 1 to 14, wherein the viscosity average molecular weight (M v ) is in the range of 100 to 3,000 kg / mol.
154. The method of claim 153, wherein the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 250 to 3,000 kg / mol.
155. The method of claim 153, wherein the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 100 to 2,000 kg / mol.
156. The method of claim 153, wherein the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 200 to 2,000 kg / mol.
157. The method of claim 153, wherein the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 350 to 1,800 kg / mol.
158. The method of claim 153, wherein the viscosity average molecular weight (M v ) is in the range of 400 to 1500 kg / mol.
159. The method of claim 153, wherein the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 700 to 1300 kg / mol.
160. The method of claim 153, wherein the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 2,001 to 3,000 kg / mol.
161. The method of claim 153, wherein the viscosity average molecular weight (M) of the polyisobutylene is v ) is in the range of 3,001 to 10,000 kg / mol.
162. The method of any one of claims 1 to 14, wherein the number average molecular weight (M) of the polyisobutylene is n ) is in the range of 5-1100 kg / mol.
163. The method of claim 162, wherein the polyisobutylene has a number average molecular weight (M n ) is in the range of 80 to 500 kg / mol.
164. The method of any one of claims 1 to 14, wherein the polyisobutylene has a polydispersity of polyisobutylene in the range of 1.1 to 6.0, as measured by the ratio of weight average molecular weight to number average molecular weight as determined by gel permeation chromatography.
165. The method of claim 164, wherein the polyisobutylene has a polydispersity of polyisobutylene in the range of 3.0 to 5.
5.
166. The method of any one of claims 1 to 14, wherein the polyisobutylene has a Mooney viscosity of at least 10, as determined according to ML 125°C 1+8, ASTM D 1646-7 (2012).
167. The method of claim 166, wherein the polyisobutylene has a Mooney viscosity of 10 to 80 as determined according to ML 125°C 1+8, ASTM D 1646-7 (2012).
168. The method of claim 166, wherein the polyisobutylene has a Mooney viscosity of 20 to 80 as determined according to ML 125°C 1+8, ASTM D 1646-7 (2012).
169. The method of claim 166, wherein the polyisobutylene has a Mooney viscosity of 25 to 60 as determined according to ML 125°C 1+8, ASTM D 1646-7 (2012).
170. The method of any one of claims 1 to 14, wherein the organic medium is obtained by a process comprising at least the steps of: a) providing a reaction medium comprising an organic diluent and isobutylene b) polymerizing the isobutylene in the reaction medium in the presence of an initiator system or catalyst to form an organic medium comprising the polyisobutylene, an organic diluent and optionally residual isobutylene.
171. The process of claim 170, wherein the isobutylene is present in the reaction medium in an amount ranging from 0.01 wt% to 80 wt%.
172. The process of claim 171, wherein the isobutylene is present in the reaction medium in an amount ranging from 0.1 wt% to 65 wt%.
173. The process of claim 171, wherein the isobutylene is present in the reaction medium in an amount ranging from 10.0 weight percent to 65.0 weight percent.
174. The process of claim 171, wherein the isobutylene is present in the reaction medium in an amount ranging from 25.0 weight percent to 65.0 weight percent.
175. The method of claim 170, wherein the organic diluent is a hydrochlorocarbon; or a x H y F z The hydrofluorocarbon represented by wherein x is an integer from 1 to 40, wherein y and z are integers and are at least 1.
176. The method of claim 170, wherein the organic diluent is an alkane selected from the group consisting of propane, isobutane, pentane, methylcyclopentane, isohexane, 3-methylpentane, 2-methylbutane, 2,2-dimethylbutane, 2,3-dimethylbutane, 2-methylhexane, 3-methylhexane, 3-ethylpentane, 2,2-dimethylpentane, 2,3-dimethylpentane, 2,4-dimethylpentane, 3,3-dimethylpentane, 2-methylheptane, 3-ethyl Hexane, 2,5-dimethylhexane, 2,2,4-trimethylpentane, octane, heptane, butane, ethane, methane, nonane, decane, dodecane, undecane, hexane, methylcyclohexane, cyclopropane, cyclobutane, cyclopentane, methylcyclopentane, 1,1-dimethylcyclopentane, cis-1,2-dimethylcyclopentane, trans-1,2-dimethylcyclopentane, trans-1,3-dimethyl-cyclopentane, ethylcyclopentane, cyclohexane, methylcyclohexane and mixtures of the above diluents.
177. The method of claim 175, wherein x is an integer from 1 to 30.
178. The method of claim 175, wherein x is an integer from 1 to 20.
179. The method of claim 175, wherein x is an integer from 1 to 10.
180. The method of claim 175, wherein x is an integer from 1 to 6.
181. The method of claim 175, wherein x is an integer from 2 to 20.
182. The method of claim 175, wherein x is an integer from 3 to 10.
183. The method of claim 175, wherein x is an integer from 3 to 6.
184. The method of claim 175, wherein x is an integer from 1 to 3.
185. The process of any one of claims 170 to 184, wherein the polymerization of step b) is carried out as a slurry polymerization or a solution polymerization.
186. The process of claim 185, wherein the polymerization of step b) is carried out as a slurry polymerization and 80% of the particles obtained during the slurry polymerization have a size of 0.1 to 800 μm.
187. The process of claim 185, wherein the polymerization of step b) is carried out as a slurry polymerization and 80% of the particles obtained during the slurry polymerization have a size of 0.25 to 500 μm.
188. The method of any one of claims 1 to 14, wherein 50% by weight or more of the polyisobutylene particles have a particle size between 3.35 mm and 8.00 mm.
189. The method of claim 188, wherein 60 weight percent or more of the polyisobutylene particles have a particle size between 3.35 mm and 8.00 mm.
190. The method of claim 188, wherein 70 weight percent or more of the polyisobutylene particles have a particle size between 3.35 mm and 8.00 mm.
191. The method of claim 188, wherein 80 weight percent or more of the polyisobutylene particles have a particle size between 3.35 mm and 8.00 mm.
192. The process of any one of claims 1 to 14, wherein in a sieving test with 6 sieves having mesh openings of 19.00 mm, 12.50 mm, 8.00 mm, 6.30 mm, 3.35 mm and 1.60 mm, 50 wt. % or more of the polyisobutylene particles are found in a sieve between 8.00 mm and 3.35 mm.
193. The method of claim 192, wherein in a sieving test with 6 sieves having mesh openings of 19.00 mm, 12.50 mm, 8.00 mm, 6.30 mm, 3.35 mm and 1.60 mm, 60 wt% or more of the polyisobutylene particles are found in the sieve between 8.00 mm and 3.35 mm.
194. The method of claim 192, wherein in a sieving test with 6 sieves having mesh openings of 19.00 mm, 12.50 mm, 8.00 mm, 6.30 mm, 3.35 mm and 1.60 mm, 70 wt% or more of the polyisobutylene particles are found in the sieve between 8.00 mm and 3.35 mm.
195. The method of claim 192, wherein in a sieving test having 6 sieves with mesh openings of 19.00 mm, 12.50 mm, 8.00 mm, 6.30 mm, 3.35 mm and 1.60 mm, 80 wt% or more of the polyisobutylene particles are found in the sieve between 8.00 mm and 3.35 mm.
196. The method of claim 192, wherein in a sieving test with 6 sieves having mesh openings of 19.00 mm, 12.50 mm, 8.00 mm, 6.30 mm, 3.35 mm and 1.60 mm, 90 weight percent or more of the polyisobutylene particles are found in the sieve between 8.00 mm and 3.35 mm.
197. The method of any one of claims 1 to 14, wherein the removal of the diluent is carried out in a time range of 0.1 s to 30 s.
198. The method of claim 197, wherein the removal of the diluent is carried out within 0.5 to 10 seconds.
199. The process of any one of claims 1 to 14, wherein the removal of the organic diluent is carried out in a time range of 0.1 s to 30 s, such that the aqueous slurry contains less than 10 wt. % of the organic diluent, calculated as the polyisobutylene contained in the polyisobutylene particles of the resulting aqueous slurry.
200. The method of claim 199, wherein the removal of the organic diluent is performed within 0.5 to 10 seconds.
201. The method of claim 199, wherein the aqueous slurry comprises less than 7 weight percent organic diluent, calculated as polyisobutylene contained in the polyisobutylene particles of the resulting aqueous slurry.
202. The method of claim 199, wherein the aqueous slurry comprises less than 5 weight percent organic diluent, calculated as polyisobutylene contained in the polyisobutylene particles of the resulting aqueous slurry.
203. The method of claim 199, wherein the aqueous slurry comprises less than 3 weight percent organic diluent, calculated as polyisobutylene contained in the polyisobutylene particles of the resulting aqueous slurry.
204. The method of claim 199, wherein the aqueous slurry comprises less than 1 weight percent organic diluent, calculated as polyisobutylene contained in the polyisobutylene particles of the resulting aqueous slurry.
205. The method of claim 170, wherein step b) is performed batchwise or continuously.
206. The method of claim 170, wherein at least one control agent for the initiator system is used in step b).
207. The method of claim 206, wherein the at least one control agent comprises ethylene, a mono-substituted or di-substituted C3-C 20 The monoolefins are used in amounts of 0.01 to 20% by weight, based on the monomers used in step a).
208. The method of claim 207, wherein the at least one control agent comprises (C3-C 20 )-1-ene.
209. The method of claim 207, wherein the at least one control agent comprises 1-butene.
210. The method of claim 207, wherein the control agent is used in an amount of 0.2 to 15 weight percent, based on the monomers used in step a).
211. The method of claim 207, wherein the control agent is used in an amount of 1 to 15 weight percent, based on the monomers used in step a).
212. The process of claim 206 or 207, wherein the at least one control agent comprises diisobutylene in an amount of 0.001 to 3% by weight, based on the monomers used in step a).
213. The method of claim 212, wherein the control agent is used in an amount of 0.01 to 2 weight percent, based on the monomers used in step a).
214. The method of claim 212, wherein the control agent is used in an amount of 0.01 to 1.5 weight percent, based on the monomers used in step a).
215. The method of any one of claims 206 to 214, wherein the initiator comprises aluminum chloride and the weight ratio of isobutylene to aluminum chloride is from 500 to 20,000.
216. The process of claim 215, wherein the weight ratio of isobutylene to aluminum chloride is from 1,500 to 10,000.
217. The process of claim 215, wherein water and / or alcohol is used as a proton source in an amount of 0.05 to 2.0 moles of water per mole of aluminum in the aluminum chloride.
218. The method of claim 217, wherein water is used as the proton source.
219. The method of claim 217, wherein the proton source is used in an amount of 0.1 to 1.2 moles of water per mole of aluminum in the aluminum chloride.
220. The process of claim 170, wherein the temperature of step A) is 10 to 100°C.
221. The process of claim 220, wherein the temperature of step A) is between 50 and 100°C.
222. The process of claim 220, wherein the temperature of step A) is between 60 and 95°C.
223. The process of claim 220, wherein the temperature of step A) is between 75 and 95°C.
224. The method of any one of claims 1 to 14, wherein the LCST compound is selected from methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, or a combination thereof.
225. The method of claim 224, wherein the cellulose has a degree of substitution (DS) of 0.5 to 2.
8.
226. The method of claim 224, wherein the cellulose has a degree of substitution (DS) of 1.2 to 2.
5.
227. The method of claim 224, wherein the LCST compound has a weight average molecular weight of 1,500 to 3,000,000.
228. The method of claim 224, wherein the LCST compound has a weight average molecular weight of 1,500 to 2,600,000.
229. The process according to any one of claims 1 to 14, wherein the amount of LCST compound present in the aqueous medium used in step A) is from 1 to 20,000 ppm, relative to the amount of polyisobutylene present in the organic medium.
230. The process of claim 229, wherein the amount of LCST compound in the aqueous medium used in step A) is from 3 to 10,000 ppm relative to the amount of polyisobutylene present in the organic medium.
231. The process of claim 229, wherein the amount of the LCST compound in the aqueous medium used in step A) is from 5 to 5,000 ppm relative to the amount of polyisobutylene present in the organic medium.
232. The process of claim 229, wherein the amount of the LCST compound in the aqueous medium used in step A) is from 10 to 5,000 ppm relative to the amount of polyisobutylene present in the organic medium.
233. The process according to any one of claims 1 to 14, wherein the amount of LCST compound present in the aqueous medium used in step A) is from 1 to 5,000 ppm, relative to the amount of polyisobutylene present in the organic medium.
234. The process of claim 233, wherein the amount of the LCST compound present in the aqueous medium used in step A) is from 3 to 1,000 ppm relative to the amount of polyisobutylene present in the organic medium.
235. The process of claim 233, wherein the amount of LCST compound present in the aqueous medium used in step A) is from 5 to 500 ppm, relative to the amount of polyisobutylene present in the organic medium.
236. The process of claim 233, wherein the amount of LCST compound present in the aqueous medium used in step A) is from 5 to 100 ppm, relative to the amount of polyisobutylene present in the organic medium.
237. The method of any one of claims 1 to 14, wherein the LCST compound has a molecular weight of at least 1,500 g / mol.
238. The method of claim 237, wherein the LCST compound has a molecular weight of at least 2,500 g / mol.
239. The method of claim 237, wherein the LCST compound has a molecular weight of at least 4,000 g / mol.
240. The method of claim 170, comprising a further step wherein the polyisobutylene particles contained in the aqueous slurry are separated to obtain separated polyisobutylene particles.
241. The method of claim 170, comprising a further step of separating polyisobutylene particles contained in the aqueous slurry to obtain separated polyisobutylene particles; and comprising a further step of drying the separated polyisobutylene particles to a residual content of volatiles of 7,000 or less.
242. The method of claim 241, wherein the separated polyisobutylene particles are dried to a residual volatile content of 5,000 or less.
243. The method of claim 241, wherein the separated polyisobutylene particles are dried to a residual volatile content of 4,000 or less.
244. The method of claim 241, wherein the separated polyisobutylene particles are dried to a residual volatile content of 2,000 ppm or less.
245. The method of claim 241, wherein the separated polyisobutylene particles are dried to a residual volatile content of 1,000 ppm or less.
246. The method according to any one of claims 1 to 14, comprising as a further step the following process: shaping the polyisobutylene particles to obtain reshaped polyisobutylene particles.
247. The method of claim 246, wherein the reshaped polyisobutylene particles are pellets.
248. The method according to any one of claims 1 to 14, comprising as a further step the following process: shaping the polyisobutylene particles to obtain shaped articles.
249. The method of claim 248, wherein the shaped article is a bag.
250. An aqueous slurry obtainable according to the process according to any one of claims 1 to 14.
251. Polyisobutylene particles obtainable according to the process of claim 240 or 241, comprising from 1 ppm to 5,000 ppm of at least one LCST compound.
252. Reshaped polyisobutylene particles obtained according to the process of claim 246, said reshaped polyisobutylene particles comprising from 1 ppm to 5,000 ppm of at least one LCST compound.
253. A polyisobutylene composition comprising 98.5 wt% or more of polyisobutylene and having an ash content of 0.2 wt% or less as measured according to ASTM D5667, further comprising at least one LCST compound selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, hydroxyalkyl alkyl cellulose and carboxyalkyl cellulose.
254. The polyisobutylene composition of claim 253, wherein the polyisobutylene composition is a reshaped polyisobutylene pellet.
255. The polyisobutylene composition of claim 253 comprising 98.8 weight percent or more polyisobutylene.
256. The polyisobutylene composition of claim 253 comprising 99.0 weight percent or more polyisobutylene.
257. The polyisobutylene composition of claim 253 comprising 99.2 weight percent or more polyisobutylene.
258. The polyisobutylene composition of claim 253 comprising 99.4 weight percent or more polyisobutylene.
259. The polyisobutylene composition of claim 253 comprising 99.5 weight percent or more polyisobutylene.
260. The polyisobutylene composition of claim 253 having an ash content of 0.1 wt% or less as measured according to ASTM D5667.
261. The polyisobutylene composition of claim 253 having an ash content of 0.08 wt% or less as measured according to ASTM D5667.
262. The polyisobutylene composition of claim 253 having an ash content of 0.05 wt% or less as measured according to ASTM D5667.
263. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the viscosity average molecular weight (M v ) is in the range of 100 to 3,000 kg / mol, or the viscosity average molecular weight (M v ) is in the range of 3,001 to 10,000 kg / mol.
264. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the viscosity average molecular weight (M v ) is in the range of 250 to 3,000 kg / mol.
265. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the viscosity average molecular weight (M v ) is in the range of 100 to 2,000 kg / mol.
266. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the viscosity average molecular weight (M v ) is in the range of 200 to 2,000 kg / mol.
267. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the viscosity average molecular weight (M v ) is in the range of 350 to 1,800 kg / mol.
268. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the viscosity average molecular weight (M v ) is in the range of 400 to 1500 kg / mol.
269. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the viscosity average molecular weight (M v ) is in the range of 700 to 1300 kg / mol.
270. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the viscosity average molecular weight (M v ) is in the range of 2,001 to 3,000 kg / mol.
271. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the polydispersity of the polyisobutylene is in the range of 1.1 to 6.0, and the polydispersity is measured by the ratio of the weight average molecular weight to the number average molecular weight determined by gel permeation chromatography.
272. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the polyisobutylene has a polydispersity in the range of 3.0 to 5.5 as measured by the ratio of the weight average molecular weight to the number average molecular weight as determined by gel permeation chromatography.
273. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the polyisobutylene has a Mooney viscosity of at least 10, wherein the Mooney viscosity is measured according to the following conditions: ML 125°C 1+8, ASTM D 1646-07, 2012.
274. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the polyisobutylene has a Mooney viscosity of 10 to 80, wherein the Mooney viscosity is measured according to the following conditions: ML 125°C 1+8, ASTM D 1646-07, 2012.
275. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the polyisobutylene has a Mooney viscosity of 20 to 80, wherein the Mooney viscosity is measured according to the following conditions: ML 125°C 1+8, ASTM D 1646-07, 2012.
276. The polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, and the polyisobutylene compositions of claims 253 to 262, wherein the polyisobutylene has a Mooney viscosity of 25 to 60, wherein the Mooney viscosity is measured according to the following conditions: ML 125°C 1+8, ASTM D 1646-07, 2012.
277. The reshaped polyisobutylene particles of claim 252 which are shaped articles, or which form shaped articles.
278. The reshaped polyisobutylene particles of claim 277, wherein the shaped article is a bag.
279. The reshaped polyisobutylene particles of claim 277 which are pellets, or are formed into pellets.
280. A shaped article obtained by shaping the polyisobutylene particles of claim 251 or the reshaped polyisobutylene particles of claim 252.
281. The shaped article of claim 280, which is a pellet or a bag.
282. A blend or mixture obtained by blending or mixing the polyisobutylene granules of claim 251, the reshaped polyisobutylene granules of claim 252, or the polyisobutylene composition of any one of claims 253 to 262 or the shaped article of any one of claims 280 to 281.
283. Use of the polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, or the polyisobutylene composition of any one of claims 253 to 262, or the shaped articles of any one of claims 280 to 281, or the blends and mixtures of claim 282 for sealants, coatings, adhesives and roofing materials.
284. Sealants, adhesives, coatings and roofing materials made from or containing the polyisobutylene particles of claim 251, the reshaped polyisobutylene particles of claim 252, or the polyisobutylene composition of any one of claims 253 to 262, or the shaped article of any one of claims 280 to 281, or the blends and mixtures of claim 282.
Citation Information
Patent Citations
Method for starting up low-tem-perature isoolefin polymerization
US2580490A
Polyisobutylene polymerization process having coarse and fine molecular weight control
US2856394A
Thermoplastic elastomers of isobutylene and process of preparation
US4946899A
Polymerization processes
WO2004067577A2
Reactor and method for continuous polymerization
WO2011000922A1