Resin composition, adhesive member, and display device including the adhesive member
By using specific resin compositions, including low and high molecular weight acrylic resins, free radical polymerization initiators and polyrotane compounds, the problem of reliability and durability of flexible display devices at high temperatures in folding or bending operations, achieving high levels of high Display device for adhesion and durability.
Patent Information
- Application Number
- CN202110289991.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-20
- Filing Date
- 2021-03-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-03-18
AI Technical Summary
The existing flexible display devices have reliability problems in folding or bending operations, and it is difficult for the adhesive resin to maintain high durability and high adhesion at high temperatures.
Using a resin composition, comprising a first (meth)acrylic resin having a weight average molecular weight of about 500 or less, a second (meth)acrylic resin having a weight average molecular weight of about 6,000 or more, a free radical polymerization initiator and polyrotane compounds have a viscosity of about 1.0 mPa·s to about 100 mPa·s at 25°C and meet a storage modulus ratio of 0.9
High reliability of the display device in the folded or bending state is achieved, and high durability and high adhesion of the adhesive member are maintained under a high temperature environment to prevent the adhesive member from being lifted off or delaminated.
Smart Images

Figure CN113493593B_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] This application claims the priority and all rights arising therefrom of Korean Patent Application No. 10-2020-0034594, filed on Mar. 20, 2020, the content of which is incorporated herein by reference in its entirety. Technical field
[0003] The present disclosure relates herein to a resin composition, an adhesive member including the resin composition, and a display device including the adhesive member. Background art
[0004] Various display devices are being developed for multimedia devices such as televisions, mobile phones, tablet computers, navigation units, and game consoles. Recently, display devices that can be folded, bent, or rolled up by providing a flexible display member have been developed to promote portability and improve user convenience. Summary of the invention
[0005] In a flexible display device, it is desirable that its corresponding members, elements, or layers ensure reliability during folding or bending operations. In addition, it may be desirable that an adhesive resin for forming an adhesive layer applied to various types of display devices has high coating properties for its corresponding members, elements, or layers.
[0006] The present disclosure provides a resin composition that can provide high applicability even at high temperatures and maintain high durability, and an adhesive member including the resin composition or prepared from the resin composition.
[0007] The present disclosure also provides a display device, which has high reliability or improved reliability in various operating states such as folding and at high temperatures by including an adhesive member that can maintain high adhesive properties regardless of external conditions.
[0008] Embodiments of the present invention provide a resin composition including a first (meth)acrylic resin having a weight average molecular weight of about 500 or less than 500, a second (meth)acrylic resin having a weight average molecular weight of about 6,000 or more than 6,000, a radical polymerization initiator, and a polyrotaxane compound, wherein the resin composition has a viscosity of about 1.0 millipascal-seconds (mPa·s) to about 100 mPa·s at 25°C.
[0009] In an embodiment, the resin composition may satisfy the following formula: 0.9 < A / B < 4, where A represents the storage modulus of the resin composition at 25°C after UV curing, and B represents the storage modulus of the resin composition at 60°C after UV curing.
[0010] In an embodiment, the resin composition may further comprise an organic solvent in an amount of from about 0 weight percent (wt%) to about 1 wt%.
[0011] In an embodiment, the polyrotaxane compound may have a radically curable group on its side chain.
[0012] In an embodiment, the radically curable group may be an acrylate group or a methacrylate group.
[0013] In an embodiment, the radical polymerization initiator may include a self-cleavage type radical polymerization initiator and a hydrogen abstraction type radical polymerization initiator.
[0014] In an embodiment, relative to the total content of 100 wt% of the first (meth)acrylic resin and the second (meth)acrylic resin, the content of the second (meth)acrylic resin may be from about 5 wt% to about 20 wt%.
[0015] In an embodiment, the content of the radical polymerization initiator may be from about 0.5 wt% to about 5 wt%.
[0016] In an embodiment, the content of the polyrotaxane compound may be from about 1 wt% to about 10 wt%.
[0017] In an embodiment of the present invention, the adhesive member comprises a resin composition, wherein the resin composition comprises a first (meth)acrylic resin having a weight average molecular weight of about 500 or less than 500, a second (meth)acrylic resin having a weight average molecular weight of about 6,000 or greater than 6,000, a radical polymerization initiator, and a polyrotaxane compound. In such an embodiment, the resin composition has a viscosity of from about 1.0 mPa·s to about 100 mPa·s at 25°C.
[0018] In an embodiment, the adhesive member may satisfy the following formula: 0.9 < A' / B' < 4, where A' represents the storage modulus of the adhesive member at 25°C and B' represents the storage modulus of the adhesive member at 60°C.
[0019] The resin composition may be an inkjet printing composition.
[0020] In an embodiment of the present invention, a display device includes a display panel, a window disposed on the display panel, and an adhesive member disposed between the display panel and the window, wherein the adhesive member includes a resin composition, and the resin composition includes a first (meth)acrylic resin having a weight average molecular weight of about 500 or less than 500, a second (meth)acrylic resin having a weight average molecular weight of 6,000 or more than 6,000, a radical polymerization initiator, and a polyrotaxane compound. In such an embodiment, the resin composition has a viscosity of about 1.0 mPa·s to about 100 mPa·s at 25°C.
[0021] In an embodiment, the thickness of the adhesive member may be about 20 micrometers (μm) to about 200 μm.
[0022] In an embodiment, the adhesive member may be defined by a layer formed by directly providing the resin composition on one surface of the display panel and UV-curing the provided resin composition.
[0023] In an embodiment, a folding region may be defined in the display device, and the folding region may have a radius of curvature of about 5 millimeters (mm) or less than 5 mm.
[0024] In an embodiment, the adhesive member may satisfy the following formula: 0.9 < A' / B' < 4, where A' represents the storage modulus of the adhesive member at 25°C, and B' represents the storage modulus of the adhesive member at 60°C.
[0025] In an embodiment, the resin composition may further include an organic solvent in an amount of about 0 wt% to about 1 wt%.
[0026] In an embodiment, the display device may further include a light control layer disposed between the adhesive member and the window, and an optical adhesive layer disposed between the light control layer and the window, wherein the optical adhesive layer may include a polymer derived from the resin composition.
[0027] In an embodiment, the light control layer may be a polarization layer or a color filter layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The above and other features of the present invention will become more apparent by describing embodiments of the present invention in further detail with reference to the accompanying drawings, in which:
[0029] Figure 1 is a perspective view of a display device according to an embodiment;
[0030] Figure 2 illustrates Figure 1A view showing a display device in a folded state;
[0031] Figure 3 is a perspective view of a display device according to an embodiment;
[0032] Figure 4 is an exploded perspective view of a display device according to an embodiment;
[0033] Figure 5 is a cross-sectional view of a display device according to the embodiment;
[0034] FIG. 6A to FIG. 6C is a view illustrating a method for preparing an adhesive member according to an embodiment;
[0035] Fig. 7A and Figure 7B is a view illustrating a method for preparing an adhesive member according to an alternative embodiment; and
[0036] Figure 8 is a cross-sectional view of a display device according to an alternative embodiment. DETAILED DESCRIPTION
[0037] The present invention will now be described more fully below with reference to the accompanying drawings, in which various embodiments are shown. However, the present invention may be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. Instead, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the invention to those skilled in the art.
[0038] In the present disclosure, when an element (or region, layer, portion, etc.) is referred to as being "on," "connected to," or "coupled to" another element, it means that the element can be directly disposed on / connected to / coupled to another element, or a third element can be disposed therebetween.
[0039] Meanwhile, in the specification, “directly disposed” means that there is no added layer, film, region, plate, etc. between a part of a layer, film, region, plate, etc. and another part. For example, “directly disposed” may mean disposed without an additional member (e.g., an adhesive member) between two layers or two members.
[0040] The same reference numerals refer to the same elements. In addition, in the drawings, the thickness, ratio and size of elements are exaggerated for effective description of the technical contents.
[0041] The terms used herein are only for the purpose of describing specific embodiments and are not intended to be limiting. As used herein, "one (kind) (a)", "one (kind) (an)", "the" and "at least one (kind)" do not represent quantitative limitations, but are intended to include both the singular and the plural, unless the context clearly indicates otherwise. For example, "an element" has the same meaning as "at least one element", unless the context clearly indicates otherwise. "At least one (kind)" should not be interpreted as limiting "one (kind) (a)" or "one (kind) (an)". "Or" means "and / or". As used herein, the term "and / or" includes any combination and all combinations of one or more than one of the related listed items. It should be further understood that the terms “comprises” and / or “comprising”, or “includes” and / or “including” when used in the present specification specify the presence of specified features, regions, integers, steps, operations, elements and / or components, but do not preclude the presence or addition of one or more other features, regions, integers, steps, operations, elements, components and / or groups thereof.
[0042] It should be understood that although the terms "first", "second", etc. can be used to describe various elements in this article, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. For example, without departing from the scope of the exemplary embodiment of the present invention, the first element can be referred to as the second element, and similarly, the second element can be referred to as the first element. The term in the singular form can include the plural form unless the context clearly indicates otherwise.
[0043] In addition, terms such as "below", "lower", "above", "on", etc. are used to describe the relationship of the configurations shown in the drawings. The terms are used as relative concepts and are described with reference to the directions indicated in the drawings. In the present disclosure, the term "on..." may include the case of being disposed on the lower part as well as on the upper part.
[0044] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the present invention belongs. It should also be understood that terms defined in commonly used dictionaries should be interpreted as having a meaning consistent with the meaning in the context of the relevant art and are clearly defined herein unless they are interpreted in an ideal or overly formal sense.
[0045] As used herein, "about" or "approximately" includes the specified value and means within an acceptable range of deviation of the specified value as determined by one of ordinary skill in the art taking into account the relevant measurements and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more than one standard deviation of the specified value, or within ±30%, ±20%, ±10%, or ±5% of the specified value.
[0046] Embodiments are described herein with reference to cross-sectional diagrams, which are schematic diagrams of idealized embodiments. As such, variations in the shapes of the diagrams due to, for example, manufacturing techniques and / or tolerances should be expected. Therefore, the embodiments described herein should not be interpreted as being limited to the specific shapes of the zones as illustrated herein, but should include deviations in shapes resulting from, for example, manufacturing. For example, a zone illustrated or described as flat may typically have rough and / or nonlinear features. In addition, illustrated acute angles may be rounded. Therefore, the zones illustrated in the accompanying drawings are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the zones, and are not intended to limit the scope of the claims of the present application.
[0047] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0048] Figure 1 is a perspective view of a display device according to the embodiment. Figure 2 It is an example Figure 1 FIG. 4 is a view showing a display device in a folded state.
[0049] refer to Figure 1 , an embodiment of the display device DD may have a rectangular shape having a long side extending in the direction of the first direction axis DR1 and a short side extending in the direction of the second direction axis DR2 intersecting the first direction axis DR1. However, embodiments of the present invention are not limited thereto. The display device DD may be modified to have one of other various shapes such as a circular shape and a polygonal shape. The display device DD may be a rigid display device or a flexible display device.
[0050] In the embodiment of the display device DD according to the present invention, the display surface DS on which the image IM is displayed can be parallel to the plane defined by the first direction axis DR1 and the second direction axis DR2. The normal direction of the display surface DS is represented by the third direction axis DR3, that is, the thickness direction of the display device DD. The front surface (or upper surface) and the rear surface (or lower surface) of each component can be defined by the third direction axis DR3. However, the direction represented by the first direction axis to the third direction axis (DR1, DR2 and DR3) is a relative concept, and therefore can be changed to other directions. Hereinafter, the first direction to the third direction correspond to the directions represented by the first direction axis to the third direction axis (DR1, DR2 and DR3), respectively, and are given the same reference numerals.
[0051] In an embodiment, the display device DD may include at least one folding area FA. Figure 1 and Figure 2 The display device DD may include a folding area FA and a plurality of non-folding areas NFA. The folding area FA is disposed between the non-folding areas NFA, and the folding area FA and the non-folding area NFA may be arranged adjacent to each other in the first direction axis DR1 direction.
[0052] The folding area FA may be a portion variable into a shape folded with respect to a folding axis FX extending in the second direction axis DR2 direction, which is one direction. The folding area FA may have a curvature radius RD of 5 mm or less.
[0053] Figure 1 and Figure 2 An embodiment in which a single folding area FA and two non-folding areas NFA are defined is illustrated, but the number of folding areas FA and non-folding areas NFA is not limited thereto. In an alternative embodiment, for example, the display device DD may include a plurality of non-folding areas NFA greater than two and a plurality of folding areas FA disposed between the non-folding areas NFA.
[0054] In an embodiment of the display device DD, the non-folding areas NFA may be arranged to be symmetrical with respect to the folding area FA. However, embodiments of the present invention are not limited thereto. In an alternative embodiment, in which the folding area FA is arranged between the non-folding areas NFA, the areas of the two non-folding areas NFA facing each other with respect to the folding area FA may be different from each other.
[0055] The display surface DS of the display device DD may include a display area DD-DA (or Figure 3 and Figure 5 DA in the display area) and a non-display area DD-NDA (or Figure 3 and Figure 5The display area DD-DA may display the image IM, and the non-display area DD-NDA may not display the image. The non-display area DD-NDA may surround the display area DD-DA and define an edge (or baffle) portion of the display device DD.
[0056] refer to Figure 2 , an embodiment of the display device DD may be a foldable display device DD that is folded or unfolded. In one embodiment, for example, the folding area FA may be folded along a folding axis FX parallel to the second direction axis DR2, so that the display device DD may be folded. The folding axis FX may be defined as a short axis parallel to the short side of the display device DD.
[0057] When the display device DD is folded, the non-folding areas NFA face each other, and the display device DD can be folded inward so that the display surface DS is not exposed to the outside. However, the embodiments of the present invention are not limited thereto. Unlike the case illustrated in the drawings, the display device DD can be folded outward so that the display surface DS is exposed to the outside.
[0058] Figure 3 is a perspective view of a display device according to an embodiment. An embodiment of the display device DD-b includes bending areas BA1 and BA2 and a non-bending area NBA, and the bending areas BA1 and BA2 may be bent from one side of the non-bending area NBA.
[0059] refer to Figure 3 , an embodiment of the display device DD-b may include a non-bending area NBA in which an image IM is displayed on a front surface, a first bending area BA1 in which an image IM is displayed on a side surface, and a second bending area BA2. The first bending area BA1 and the second bending area BA2 may be bent from opposite sides of the non-bending area NBA, respectively.
[0060] refer to Figure 3 , the non-bending area NBA of the front surface of the display device DD-b can provide an image IM in the direction of the third directional axis DR3, and the first bending area BA1 can provide an image IM in the direction of the fifth directional axis DR5, and the second bending area BA2 can provide an image IM in the direction of the fourth directional axis DR4. The fourth directional axis DR4 and the fifth directional axis DR5 may be directions intersecting with the first directional axis to the third directional axis (DR1, DR2, and DR3). However, the directions represented by the first directional axis DR1 to the fifth directional axis DR5 are relative concepts and are not limited to the directional relationships illustrated in the drawings.
[0061] In an embodiment, the display device DD-b may be a curved display device including a non-curved area NBA and a curved area BA1 and a curved area BA2 respectively disposed on opposite sides of the non-curved area NBA. In an alternative embodiment, although not shown, the display device may be a curved display device including a single non-curved area and a single curved area. In such an embodiment, the curved area may be provided by bending only one side of the non-curved area.
[0062] Figures 1 to 3 The embodiments of a foldable display device, a curved display device, etc. as described above are exemplified, but the embodiments of the present invention are not limited thereto. Alternatively, the display device may be a rollable display device, a flat rigid display device, or a curved rigid display device.
[0063] Hereinafter, an embodiment of a display device in which the display device DD is foldable relative to a short axis is described, but the embodiments of the present invention are not limited thereto, and the following description can be applied to various types of display devices as well as a display device DD-b including a bending area.
[0064] Figure 4 is an exploded perspective view of a display device DD according to the embodiment. Figure 5 is a cross-sectional view of a display device DD of the embodiment. Figure 5 It can be corresponding to Figure 1 A cross-sectional view of a portion of line II'.
[0065] The display device DD may include a display panel DP and a window WP disposed on the display panel DP. The display device DD may include an adhesive member (or layer) AP disposed between the display panel DP and the window WP. The adhesive member AP may be an optically clear adhesive film ("OCA") or an optically clear adhesive resin layer ("OCR").
[0066] The adhesive member AP may include a resin composition according to an embodiment of the present invention, or be formed by a resin composition according to an embodiment of the present invention. The resin composition includes a first (meth) acrylic resin having a weight average molecular weight of 500 or less, a second (meth) acrylic resin having a weight average molecular weight of 6,000 or more, a free radical polymerization initiator, and a polyrotaxane compound. In this article, (meth) acrylic acid refers to acrylic acid or methacrylic acid.
[0067] The resin composition has a viscosity of about 1.0 millipascal-second (mPa·s) to about 100 mPa·s at 25°C measured by the JIS K2283 method before polymerization with the photoinitiator. Alternatively, the viscosity may be about 50 mPa·s or less than 50 mPa·s. When the viscosity of the resin composition is less than 1.0 mPa·s, the viscosity is low, resulting in the flow of the resin composition liquid provided for forming the adhesive member, and therefore, it may be difficult to form a coating film having a uniform thickness using the resin composition. In addition, when the viscosity of the resin composition exceeds the above range, that is, greater than 100 mPa·s, it may be difficult to discharge the resin composition from the applicator for applying the resin composition in an appropriate amount.
[0068] The resin composition may satisfy Formula 1 below.
[0069] [Formula 1]
[0070] 0.9
[0071] In Formula 1, A represents the storage modulus of the resin composition at 25° C. after UV curing, and B represents the storage modulus of the resin composition at 60° C. after UV curing.
[0072] The resin composition of the embodiment may have a storage modulus of about 0.005 mPa to about 0.100 mPa, or about 0.010 mPa to about 0.070 mPa at 60° C. after UV curing. The resin composition of the embodiment does not cause a decrease in storage modulus at high temperatures, and thus can maintain high reliability even in a high temperature environment.
[0073] The resin combination of the embodiment may further include an organic solvent in an amount of about 0 weight percent (wt%) to about 1wt%. In such embodiments, the resin combination does not include an organic solvent at all, or even when an organic solvent is included, the organic solvent may be a trace of 1wt% or less than 1wt%, and therefore, it may be particularly effective for an inkjet printing method that may not use a separate drying process after applying the resin combination. When an organic solvent is included, the organic solvent may be an aromatic hydrocarbon (such as toluene and xylene), an ester (such as ethyl acetate and butyl acetate), an aliphatic alcohol (such as n-propyl alcohol and isopropyl alcohol), a ketone (such as methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone), etc.
[0074] In an embodiment of the resin composition, the first (meth)acrylic resin may have a weight average molecular weight of 500 or less, or 400 or less. In an embodiment, the first (meth)acrylic resin may have a weight average molecular weight of 100 or more.
[0075] In an embodiment of the resin composition, the first (meth)acrylic resin may include at least one acryloyl group or at least one methacryloyl group per monomer unit. In an embodiment of the resin composition, the first (meth)acrylic resin may include a plurality of different monomers.
[0076] In an embodiment of the resin composition, the first (meth)acrylic resin may include at least one selected from alicyclic (meth)acrylates, hydroxyl group-containing (meth)acrylates, alkyl (meth)acrylates, and aromatic (meth)acrylates.
[0077] In an embodiment of the resin composition, the first (meth) acrylic resin may include at least one selected from 2-ethylhexyl acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl acrylate, 4-hydroxybutyl acrylate, 4-acryloylmorpholine, isobornyl acrylate, n-butyl acrylate, butyl methacrylate, methyl (meth)acrylate, 2-hydroxyethyl acrylate and octyl (meth)acrylate.
[0078] In one embodiment of the resin composition, for example, the first (meth) acrylic resin may include 2-ethylhexyl acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl) methyl acrylate, 4-hydroxybutyl acrylate, and 4-acryloyl morpholine. However, the embodiments of the present invention are not limited thereto, and alternatively, a (meth) acrylic monomer containing at least one acryloyl group or methacryloyl group may be used. In one embodiment, for example, the (meth) acrylic acid alkyl ester may be n-butyl (meth) acrylate, isobutyl (meth) acrylate, tert-butyl (meth) acrylate, isooctyl (meth) acrylate, isodecyl (meth) acrylate, lauryl (meth) acrylate, stearyl (meth) acrylate, isostearyl (meth) acrylate, etc. In one embodiment, for example, alicyclic (meth) acrylate may include dicyclopentenyloxyethyl (meth) acrylate, norbornene (meth) acrylate, dicyclopentyl (meth) acrylate, isobornyl (meth) acrylate, etc. In one embodiment, for example, the cyclic ether (meth)acrylate may include tetrahydrofurfuryl (meth)acrylate, (5-ethyl-1,3-dioxane-5-yl)methyl (meth)acrylate, etc. In one embodiment, for example, the hydroxyalkyl acrylate may include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, etc. In one embodiment, for example, the (meth)acrylate having a nitrogen-containing heterocycle may include N-(meth)acryloylmorpholine, N-(meth)acryloylpyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-(meth)acryloylaziridine, aziridinylethyl (meth)acrylate, etc.
[0079] In embodiments of the resin composition, the second (meth)acrylic resin may have a weight average molecular weight of 6,000 or more, or 10,000 or more. In embodiments, the second (meth)acrylic resin may have a weight average molecular weight of 50,000 or less.
[0080] In an embodiment of the resin composition, the second (meth)acrylic resin may include at least one acryloyl group or at least one methacryloyl group per monomer unit. In an embodiment of the resin composition, the second (meth)acrylic resin may include a plurality of different monomers.
[0081] In an embodiment, the second (meth) acrylic resin may include at least one selected from a (meth) acrylic acid ester oligomer having a polyurethane backbone, a (meth) acrylic acid ester oligomer having a polyisoprene backbone, and a (meth) acrylic acid ester oligomer having a polybutadiene backbone. The second (meth) acrylic resin may include one or two or more (meth) acrylic acid ester oligomers.
[0082] In an embodiment, the second (meth) acrylic resin may include a photocurable compound containing at least one (meth) acryloyl group having a carbamate bond. The carbamate acrylate oligomer may include at least one selected from acrylates having a carbamate bond, carbamate acrylates having a polycarbonate skeleton, and carbamate acrylates having a polyether skeleton. In one embodiment, for example, the resin composition may include at least one selected from UN-5500 (Negami Chemical Industrial), UF-C051 (KYOEISHA CHEMICAL), KRM8792 (DAICEL-ALLNEX), and UN-6305 (Negami Chemical Industrial) as a carbamate acrylate oligomer.
[0083] The resin composition including the second (meth)acrylic resin having a weight average molecular weight of 6,000 or more may exhibit low viscosity properties, which may be effectively applied by a method such as inkjet printing or dispensing.
[0084] In an embodiment, the resin composition may include the second (meth) acrylic resin in an amount of about 5 wt % to about 20 wt % relative to 100 wt % of the total content of the first (meth) acrylic resin and the second (meth) acrylic resin. The resin composition includes the second (meth) acrylic resin in an amount of about 10 wt % to about 20 wt %, and thus exhibits a low viscosity of about 1.0 mPa·s to about 100 mPa·s in a resin state, and has high coating properties in an inkjet printing method.
[0085] In an embodiment of the resin composition, the polyrotaxane compound is a compound formed by: a pseudopolyrotaxane is obtained when the cavities of a plurality of cyclic molecules are pierced by linear molecules in a threaded manner and the plurality of cyclic molecules accommodate the linear molecules, and a blocking group is placed at both ends of the pseudopolyrotaxane (both ends of the linear molecules) so as not to release the cyclic molecules.
[0086] In the embodiment of the resin composition, the polyrotaxane compound may have a radically curable group on its side chain. When the polyrotaxane compound has a radically curable group, polymerization with the first (meth) acrylic resin and the second (meth) acrylic resin may be applicable. The type of radically curable group may be an unsaturated double bond, and for example, the radically curable group may include a (meth) acrylate group, a (meth) acryloyl group, a vinyl ether group, a styryl group, etc., but is not limited thereto.
[0087] In an embodiment of the resin composition, the polyrotaxane compound may have an acrylate group or a methacrylate group on a side chain thereof.
[0088] In an embodiment of the resin composition, the polyrotaxane compound may be included in an amount of about 1 wt % to about 10 wt %. The resin composition may include the polyrotaxane compound within the above range to effectively prevent storage modulus degradation at high temperatures after curing and ensure durability at high temperatures.
[0089] The resin composition may include at least one free radical polymerization initiator. In one embodiment, for example, the resin composition may include a self-cleavage type free radical polymerization initiator and a hydrogen abstraction type free radical polymerization initiator.
[0090] The self-cleavage initiator can be 4-phenoxydichloroacetophenone, 4-tert-butyl-dichloroacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylidenephenyl)-2-hydroxy-2-methylpropan-1-one, 1-(4-dodecylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy-phenyl(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexane The invention also includes, but is not limited to, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 4-benzoyl-4'-methyldiphenyl sulfide, 4'-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 4'-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 4'-(2-benzoyl ...-2-propyl)ketone, 4'-(2-hydroxy-2-propyl)ketone, 4'-(2-hydroxy-2-propyl)ketone, 4'-(2-hydroxy-2-propyl)ketone, 4'-
[0091] The hydrogen abstraction initiator may be benzophenone, benzoyl benzoate, methyl benzoyl benzoate, 4-phenylbenzophenone, hydroxybenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 2,4,6-trimethylbenzophenone, 4-methylbenzophenone, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, camphorquinone, dibenzosuberone, 2-ethylanthraquinone, 3,3',4,4'-tetrakis(tert-butylperoxycarbonyl)benzophenone, or 9,10-phenanthrenequinone, but is not limited thereto.
[0092] In the embodiment, the resin composition contains both a self-cleavage type photopolymerization initiator and a hydrogen abstraction type photopolymerization initiator, and the adhesive member formed of the resin composition has an improved balance of photocrosslinking on the surface portion and internal photocrosslinking, thereby having high adhesiveness.
[0093] In an embodiment, the resin composition may include a free radical polymerization initiator in an amount of about 0.5 wt % to about 5 wt %. When the free radical polymerization initiator exceeds 5 wt %, it tends to easily cause a change in curing by irradiation with active energy rays, and when the free radical polymerization initiator is less than 0.5 wt %, the bridging density decreases and the adhesion decreases.
[0094] In an embodiment, the resin composition may further selectively include conventional known additives, such as fillers, pigments, diluents, anti-aging agents, UV absorbers, UV stabilizers, antistatic agents, etc., which are usually mixed within the range of not deteriorating the desired physical properties. One or two or more than two additives may be used. The content of such additives may be appropriately set to obtain the desired physical properties.
[0095] Return to reference Figure 4 and Figure 5 , an embodiment of the display panel DP may include a base substrate BS, a circuit layer DP-CL disposed on the base substrate BS, a display element layer DP-EL disposed on the circuit layer DP-CL, and an encapsulation layer TFE covering the display element layer DP-EL. In one embodiment, for example, the display panel DP may include a plurality of organic light emitting elements or a plurality of quantum dot light emitting elements in the display element layer DP-EL.
[0096] Figure 5 The configuration of the display panel DP shown in FIG. 1 is merely exemplary, and the configuration of the display panel DP is not limited to Figure 5 In an alternative embodiment, for example, the display panel DP may include a liquid crystal display element, and the encapsulation layer TFE may be omitted.
[0097] The window WP may protect the display panel DP. The image IM generated by the display panel DP may be transmitted through the window WP and provided to the user. In an embodiment of the display device DD including the folding area FA, the window WP may be a flexible window.
[0098] The window WP may include a base layer BL and a printed layer BM. The window WP may include a transmissive area TA and a baffle area BZA ( Figure 4 ). A front surface of the window WP including the transmissive area TA and the baffle area BZA corresponds to a front surface of the display device DD.
[0099] The transmission area TA may be an optically transparent area. The baffle area BZA may be an area having a relatively lower light transmittance than the transmission area TA. The baffle area BZA may have a predetermined color. The baffle area BZA may be adjacent to the transmission area TA and surround the transmission area TA. The baffle area BZA may define the shape of the transmission area TA. However, embodiments of the present invention are not limited thereto, and alternatively, the baffle area BZA may be disposed adjacent to only one side of the transmission area TA, and a portion thereof may be omitted.
[0100] The base layer BL may be a glass substrate or a plastic substrate. In one embodiment, for example, the base layer BL may be a tempered glass substrate. Alternatively, the base layer BL may include or be formed of a flexible polymer resin. In one embodiment, for example, the base layer BL may include or be formed of at least one material selected from the following: polyimide, polyacrylate, polymethyl methacrylate, polycarbonate, polyethylene naphthalate, polyvinylidene chloride, polyvinylidene fluoride, polystyrene, ethylene-vinyl alcohol copolymer, and combinations thereof. However, the embodiments of the present invention are not limited thereto, and the general form of the base layer BL known in the art as the window WP may be used without restriction.
[0101] The printing layer BM may be disposed on one surface of the base layer BL. In an embodiment, the printing layer BM may be provided on the lower surface of the base layer BL adjacent to the display panel DP. The printing layer BM may be disposed on an edge region of the base layer BL. The printing layer BM may be an ink printing layer. In an embodiment, the printing layer BM may be a layer formed by including a pigment or a dye. In the window WP, the baffle area BZA ( Figure 4 ) may be a portion in which a printing layer BM is provided.
[0102] In an embodiment, the window WP may further include at least one functional layer (not shown) provided on the base layer BL. In an embodiment, for example, the functional layer (not shown) may be a hard coating, an anti-fingerprint coating, etc., but the embodiments of the present invention are not limited thereto.
[0103] In an embodiment, a stepped structure may be formed or defined between a portion provided with a printed layer BM and a base layer BL without the printed layer BM. In an embodiment, an adhesive member AP including or formed of a resin composition has high applicability as described above, and thus may be attached to the window WP without lifting off at the stepped portion.
[0104] In an embodiment, the adhesive member AP may include or be formed from the resin composition described above. In such an embodiment, the adhesive member AP includes or is formed from a resin composition, the resin composition including a first (meth) acrylic resin having a weight average molecular weight of 500 or less, a second (meth) acrylic resin having a weight average molecular weight of 6,000 or more, a free radical polymerization initiator, and a polyrotaxane compound, and having a viscosity of about 1.0 mPa·s to about 100 mPa·s at 25°C. In such an embodiment, the first (meth) acrylic resin, the second (meth) acrylic resin, the free radical polymerization initiator, and the polyrotaxane compound are substantially the same as those described above, and any repeated detailed description thereof will be omitted or simplified.
[0105] The adhesive member AP may satisfy Formula 2 below.
[0106] [Formula 2]
[0107] 0.9 <A' / B'<4
[0108] In the above Formula 2, A' represents the storage modulus of the adhesive member at 25°C, and B' represents the storage modulus of the adhesive member at 60°C.
[0109] In an embodiment, the adhesive member AP included in the display device DD is provided on one surface of the window WP or on one surface of the display panel DP in a liquid resin composition state, and can be formed by UV-curing the liquid resin composition provided between the window WP and the display panel DP. In an alternative embodiment, the adhesive member AP can be provided by UV-curing the liquid resin composition in a separate process, laminating one surface of the adhesive member AP in a cured state on one surface of the window WP (or on one surface of the display panel DP) in the form of an adhesive film, and attaching one surface of the display panel DP (or one surface of the window WP) that is not attached to the other surface of the adhesive member AP.
[0110] The thickness of the adhesive member AP may be about 20 micrometers (μm) to about 200 μm. In one embodiment, for example, the adhesive member AP may have a thickness of about 30 μm or more, or about 40 μm or more, and may have a thickness of about 150 μm or less, or about 100 μm or less.
[0111] An embodiment of the display device DD includes an adhesive component AP comprising the resin composition described above or formed from the resin composition described above, and the adhesive component AP exhibits high durability, thereby effectively preventing lifting at the interface of the adhesive component AP even when the display device DD is folded or bent, and maintains effective adhesion even in a high temperature environment to exhibit high reliability characteristics.
[0112] FIG. 6A to FIG. 6C is a view schematically illustrating a method of preparing an adhesive member AP according to the embodiment. Fig. 6A A process of providing a resin composition RC for forming an adhesive member AP is exemplified, Figure 6B illustrates the process of UV irradiation, and Figure 6C The process of removing the carrier film CF is illustrated.
[0113] refer to FIG. 6A to FIG. 6C In an embodiment of the method for preparing an adhesive member AP, a resin composition RC may be provided on a carrier film CF. In one embodiment, for example, a polyethylene terephthalate ("PET") film may be used as a carrier film CF, but embodiments of the present invention are not limited thereto. The carrier film CF is used as a substrate for coating a liquid resin composition RC, and may be used without restriction as long as it is easily separated from the adhesive member AP after UV curing. In one embodiment, for example, a release treatment may be performed on one surface of the carrier film CF provided with the resin composition RC.
[0114] The resin composition RC may be provided by a predetermined method such as an inkjet printing method or a dispensing method. In one embodiment, for example, the resin composition RC may be an inkjet printing composition having properties suitable for use with the inkjet printing method. In an embodiment, the resin composition RC may be easily discharged from a nozzle NZ or the like by having a viscosity value of about 1.0 mPa·s to about 100 mPa·s at 25° C., and may be provided to maintain a constant coating thickness.
[0115] The pre-adhesive member P-AP provided by coating the resin composition RC at a constant thickness may be irradiated with ultraviolet ("UV") light. Figure 6B An embodiment in which the coated pre-adhesive member P-AP is directly irradiated with UV light is illustrated, but the embodiment is not limited thereto. In an alternative embodiment, an auxiliary carrier film (not shown) may be further disposed on the pre-adhesive member P-AP, and the auxiliary carrier film (not shown) transmits UV light during the UV curing process and may cover the pre-adhesive member P-AP.
[0116] After ultraviolet curing, the adhesive member AP may be formed. The adhesive member AP finally provided by removing the carrier film CF used in the process may satisfy Formula 2 described above.
[0117] exist FIG. 6A to FIG. 6C The adhesive member AP prepared in the process can be applied to the display device DD described above. In one embodiment, for example, one surface of the adhesive member AP is attached to the display panel DP, and then the window WP can be sequentially attached on the opposite surface of the adhesive member AP facing the one surface of the adhesive member AP attached to the display panel DP. In an embodiment, unlike the above embodiment, the adhesive member AP can be provided to the display device DD by attaching one surface of the adhesive member AP to one surface of the window WP to face the display panel DP, and then attaching the other surface of the adhesive member AP facing the one surface of the adhesive member AP attached to the window WP to the display panel DP.
[0118] In an alternative embodiment, the resin composition in a liquid state provided between the display panel DP and the window WP may be cured to form the adhesive member AP. Fig. 7A and Figure 7B A method of preparing an adhesive member AP included in a display device DD according to an alternative embodiment of the method is illustrated, which is different from the method described with reference to FIG. FIG. 6A to FIG. 6C A method for preparing an adhesive member AP is described.
[0119] Fig. 7A The process of providing the resin composition RC on the display panel DP is illustrated, and Figure 7B A process of irradiating the pre-adhesive member P-AP formed of the resin composition RC with ultraviolet light is exemplified.
[0120] The resin composition RC may be provided by a predetermined method such as an inkjet printing method or a dispensing method. The resin composition RC may be easily discharged from a nozzle NZ or the like by having a viscosity value of about 1.0 mPa·s to about 100 mPa·s at 25°C, and may be provided to maintain a thin, constant coating thickness. In such embodiments, the resin composition may be provided by having a viscosity value of about 1.0 mPa·s to about 100 mPa·s while covering the uneven structure of the stepped portion SP-a of the display panel DP. In such embodiments, by having a low viscosity value of 100 mPa·s or less than 100 mPa·s, the resin composition RC may be effectively filled without an empty space in an uneven portion such as a stepped portion SP-a. In such embodiments, the resin composition RC provided by the nozzle NZ may have a viscosity value of 1.0 mPa·s or greater than 1.0 mPa·s to be substantially uniformly coated to have a predetermined thickness without flowing out of the display panel DP.
[0121] A window WP may be provided on the pre-adhesive member P-AP provided by coating the resin composition RC to a constant thickness. UV light for curing the resin composition RC may be provided through the window WP. When the window WP is provided on the pre-adhesive member P-AP, the resin composition RC may be filled in the stepped portion SP-b without an empty space. In such an embodiment, the resin composition RC has a low viscosity value of 100 mPa·s or less, thereby covering a curved shape at an uneven portion of the stepped portion SP-b such as between the base layer BL and the printed layer BM to provide the pre-adhesive member P-AP. The pre-adhesive member P-AP may be cured after being polymerized by the provided UV light to form the adhesive member AP.
[0122] In an alternative embodiment, with Figure 7B Unlike the example shown in FIG. 1 , UV light is provided to the pre-adhesive member P-AP before providing the window WP on the pre-adhesive member P-AP to perform a polymerization reaction in the resin composition RC. The amount of UV light irradiation may be an amount of light for completely curing the resin composition RC. Alternatively, the final adhesive member AP may be formed by partially performing a polymerization reaction of the resin composition RC in the state of the pre-adhesive member P-AP, and then further reacting the unreacted resin composition RC after covering the window WP.
[0123] In an embodiment according to the present invention, as described above with respect to Figures 1 to 3As described, the display device DD or the display device DD-b includes an adhesive member AP, which includes a polymer derived from the resin composition described above to maintain the bonding state of the window WP and the display panel DP without lifting of the adhesive member AP even in a folded state or in a bent area.
[0124] Figure 8 is a cross-sectional view illustrating a display device according to an alternative embodiment.
[0125] Figure 8 The embodiment of the display device DD-1 shown in FIG. Figures 1 to 7B The embodiments of the display device DD or display device DD-b described are substantially the same, but Figure 8 The display device DD-1 shown in FIG. 1 may further include a light control layer PP and an optical adhesive layer AP-a. Therefore, the display device DD-1 shown in FIG. 1 may further include a light control layer PP and an optical adhesive layer AP-a. Figure 8 Any repeated detailed description of the same or similar elements shown in FIG.
[0126] In the implementation scheme, Figure 8 As shown in the figure, the display device DD-1 may further include a light control layer PP and an optical adhesive layer AP-a. In such an embodiment, the display device DD-1 may further include a light control layer PP disposed between the adhesive member AP and the window WP, and an optical adhesive layer AP-a disposed between the light control layer PP and the window WP.
[0127] The light control layer PP is disposed on the display panel DP to control reflected light from the display panel DP due to external light. The light control layer PP may include, for example, a polarization layer or a color filter layer.
[0128] The optical adhesive layer AP-a may be an optically transparent adhesive film OCA or an optically transparent adhesive resin layer OCR. The optical adhesive layer AP-a may be formed in the same manner as the adhesive member AP ( Figure 5 ) In the same manner as in the embodiment of the present invention, the optical adhesive layer AP-a may include or be formed of a resin composition, the resin composition including a first (meth) acrylic resin having a weight average molecular weight of 500 or less, a second (meth) acrylic resin having a weight average molecular weight of 6,000 or more, a free radical polymerization initiator, and a polyrotaxane compound, and having a viscosity of about 1.0 mPa·s to about 100 mPa·s at 25° C.
[0129] Such an embodiment of the display device DD-1 includes an optical adhesive layer AP-a and an adhesive member AP comprising or formed from a resin composition, and the optical adhesive layer AP-a and the adhesive member AP exhibit high durability, thereby effectively preventing lift-off at the interface between the optical adhesive layer AP-a and the adhesive member AP even when the display device DD-1 is folded or bent, thereby exhibiting excellent reliability characteristics.
[0130] Hereinafter, embodiments of the resin composition, adhesive member, and display device of the present invention will be described in more detail with reference to Examples and Comparative Examples.The examples shown below are merely illustrative for understanding the present invention, and the scope of the present invention is not limited thereto.
[0131] [Example]
[0132] 1. Preparation of resin composition
[0133] The resin composition of the embodiment and comparative example is prepared by the mixing ratio shown in Table 1. It is provided in a heat-resistant light-shielding container with the weight (g) disclosed in Table 1. As an initiator, ominirad TPO-H, Esacure 3644, Photomer4250 and ominirad819 are mixed with a weight ratio of 60:10:1:30 relative to the total amount of acrylic resin and weighed 2 weight % to be added to the heat-resistant light-shielding container. The resin composition of the embodiment and comparative example is prepared by stirring at a rate of 100 revolutions per minute (rmp) for about 1 hour at room temperature and atmospheric pressure. The viscosity of the prepared resin composition is measured at 25 ° C using the JIS K2283 method and measured using a viscometer (TVE-25 manufactured by TOKI SANGYO CO., LTD) at a rate of 10 rpm.
[0134] [Table 1]
[0135]
[0136]
[0137] <Materials for Component A (First (Meth) Acrylic Resin)>
[0138] 4HBA: 4-Hydroxybutyl acrylate, molecular weight 144.2
[0139] IDAA: Isodecyl acrylate, molecular weight 212
[0140] <Material for Component B (Second (Meth) Acrylic Resin)>
[0141] UF-C051, average molecular weight 35,000
[0142] Polyrotaxane: represented by the following formula 3.
[0143] [Formula 3]
[0144]
[0145] In formula 3,
[0146]
[0147] -cyclodextrin or α-cyclodextrin to which a radical polymerizable group is added. For the method of synthesizing polyrotaxane, refer to Macromolecules 2017, 50, 5695-5700.
[0148] 1. Evaluation of physical properties of resin composition and adhesive member formed from the resin composition
[0149] [Method of measuring storage modulus]
[0150] The resin compositions of the examples and comparative examples were applied to a glass substrate at a thickness of 0.15 mm and heated to 4000 mJ / cm 2 ) of light intensity for photocuring to measure the storage modulus. The storage modulus was measured by dynamic viscoelasticity measurement at -20°C to 60°C (heating rate 5°C / min) using MCR302 manufactured by Anton-Paar at a frequency of 1 Hz. The value of Formula 2 was calculated from the values measured at 25°C and 60°C.
[0151] [Durability measurement]
[0152] The resin composition according to the embodiment and the comparative example was applied to a thickness of 100 μm between a polyethylene terephthalate film (COSMOSHINE 4100, 100 μm thick, manufactured by Toyo Boseki Co., Ltd.) and a slide glass (S1112 manufactured by Matsunami Glass Ind., Ltd.) and attached. After attachment, on the slide glass side, a metal halide lamp (conveyor type ultraviolet irradiation device manufactured by Eye Graphics Co., Ltd.) was used at 4000 mJ / cm 2The laminate was irradiated with an integrated light intensity of 1000 nm to obtain a laminate. The laminate obtained above was kept under a high temperature or high temperature and high humidity (e.g., 85° C., 85% RH) environment for 72 hours to observe the occurrence of lift-off, delamination, etc. at the interface with the adherend. When there was no change in the appearance of the laminate, the laminate was evaluated as "◎", when there was no lift-off or delamination but deformation of the adhesive member was observed, the laminate was evaluated as "○", and when there was lift-off or delamination, the laminate was evaluated as "X".
[0153] [Properties of Cured Product]
[0154] After forming the laminate in the same manner as the durability measurement method, the transparency of the appearance was observed. When it was recognized as transparent, it was evaluated as "OK", and when defects were observed in white turbidity or curing, it was evaluated as "NG".
[0155] [Table 2]
[0156]
[0157] Referring to the results in Table 2, it can be confirmed that all adhesive members formed from the resin compositions of Examples 1 to 6 satisfy Formula 2 and effectively prevent the degradation of the storage modulus at high temperatures. As shown in Table 2, it can be confirmed that Example 6 containing less than 1% of an organic solvent has a similar effect compared to Example 1 containing no organic solvent. As shown in Table 2, the adhesive members formed from the resin compositions of Comparative Examples 1 to 3 do not satisfy Formula 2, and it can be confirmed that the storage modulus at high temperatures is particularly deteriorated.
[0158] The adhesive member formed from the resin composition of Comparative Example 4 had white turbidity, thereby confirming curing failure.
[0159] The resin composition having a viscosity of about 1.0 mPa s to about 100 mPa s before curing has desirable properties in forming a uniform coating of thin thickness, and can utilize inkjet printing due to the low viscosity characteristics, and exhibits high coating properties even on curved surfaces. In an embodiment, the adhesive member comprising or formed from the resin composition can maintain high durability even at high temperatures. In an embodiment, the display device includes an adhesive member having high durability to exhibit high reliability without delamination or lifting of the adhesive member in the curved portion, and even in a bent or folded operating state, there is no delamination between the adhesive member and the adjacent member to exhibit high operational reliability.
[0160] According to an embodiment of the present invention, the resin composition has a low viscosity property, and thus can exhibit high applicability to substrates of various shapes and prevent degradation of storage modulus at high temperatures.
[0161] According to an embodiment of the present invention, the adhesive member includes or is formed of a resin composition having a controlled predetermined viscosity, and thus can maintain high durability without being significantly affected by external conditions.
[0162] According to an embodiment of the present invention, a display device includes an adhesive member having high adhesiveness, and thus can exhibit high reliability in various operating states and a high-temperature environment.
[0163] The present invention should not be construed as being limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the concept of the present invention to those skilled in the art.
[0164] While the invention has been particularly shown and described with reference to embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit or scope of the invention as defined by the appended claims.
Claims
1. A resin composition comprising: a first (meth)acrylic resin having a weight average molecular weight of 500 or less; a second (meth)acrylic resin having a weight average molecular weight of 6,000 or more; a free radical polymerization initiator; and Polyrotaxane compounds, 0wt% to 1wt% of an organic solvent, wherein the first (meth) acrylic resin is composed of at least one selected from a (meth) acrylic acid ester containing a hydroxyl group and an alkyl (meth) acrylic acid ester, wherein the second (meth) acrylic resin comprises a photocurable compound having a urethane bond and containing at least one (meth) acryloyl group, wherein the resin composition has a viscosity of 1.0 mPa·s to 100 mPa·s at 25° C., wherein the content of the second (meth) acrylic resin is 5 wt % to 20 wt % relative to 100 wt % of the total content of the first (meth) acrylic resin and the second (meth) acrylic resin, The resin composition satisfies the following formula: A represents the storage modulus of the resin composition at 25° C. after UV curing, and B represents the storage modulus of the resin composition at 60° C. after UV curing. 2 . The resin composition according to claim 1 , wherein the polyrotaxane compound has a radical-curable group on a side chain thereof.
3. The resin composition of claim 2, wherein the radical-curable group is an acrylate group or a methacrylate group. 4 . The resin composition according to claim 1 , wherein the free radical polymerization initiator comprises a self-cleavage type free radical polymerization initiator and a hydrogen abstraction type free radical polymerization initiator. 5 . The resin composition according to claim 1 , wherein the content of the polyrotaxane compound is 1 wt % to 10 wt %.
6. Display device, include: Display panel; a window disposed on the display panel; as well as an adhesive member disposed between the display panel and the window, wherein the adhesive member comprises a resin composition, The resin composition comprises: a first (meth)acrylic resin having a weight average molecular weight of 500 or less; a second (meth)acrylic resin having a weight average molecular weight of 6,000 or more; Free radical polymerization initiators; as well as Polyrotaxane compounds, 0wt% to 1wt% of an organic solvent, wherein the first (meth) acrylic resin is composed of at least one selected from a (meth) acrylic acid ester containing a hydroxyl group and an alkyl (meth) acrylic acid ester, wherein the second (meth) acrylic resin comprises a photocurable compound having a urethane bond and containing at least one (meth) acryloyl group, wherein the resin composition has a viscosity of 1.0 mPa·s to 100 mPa·s at 25° C., wherein the content of the second (meth) acrylic resin is 5 wt % to 20 wt % relative to 100 wt % of the total content of the first (meth) acrylic resin and the second (meth) acrylic resin, The adhesive member satisfies the following formula: 0.9 <A' / B'<4 in A' represents the storage modulus of the adhesive member at 25°C, and B' represents the storage modulus of the adhesive member at 60°C. 7 . The display device of claim 6 , wherein a folding area is defined in the display device, and the folding area has a curvature radius of 5 mm or less.
Citation Information
Patent Citations
Transport apparatus and transport method
KR1020200034594A
Active energy ray-curable adhesive composition and adhesive composition for acrylic resin member using the same
JP2017210607A
Adhesive composition for optical film, adhesive layer, optical member, and image display device
JP2019099714A
Adhesive, polarizing film, liquid crystal panel, optical film, and image display device
WO2015108063A1