A porous carbon-nickel composite electrode and its preparation method and application in the detection of organic pollutants in water
By preparing a porous carbon-nickel composite electrode and combining it with differential pulse voltammetry, the problem of high cost and complexity of existing phenolic pollutant detection methods has been solved, and rapid and sensitive detection of trace amounts of phenolic pollutants in water has been achieved, improving improve detection efficiency and sensitivity.
Patent Information
- Application Number
- CN202110742865.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-06-30
AI Technical Summary
Existing phenolic pollutant detection methods are costly, complex sample processing and cannot achieve real-time detection, making it difficult to quickly and accurately detect trace amounts of phenolic pollutants in water bodies.
A porous carbon-nickel composite electrode was used to prepare a nanoporous nickel layer through electrodeposition and chemical oxidation, and the porous carbon material was modified in situ on its surface to form an electrode with a three-dimensional porous structure, which was combined with differential pulse voltammetry for detection.
Rapid and sensitive detection of m-nitrophenol, p-nitrophenol and o-nitrophenol is achieved, which reduces detection costs, simplifies sample processing, enables instant detection in complex environments, and significantly improves detection efficiency and sensitivity.
Smart Images

Figure CN113552185B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemical sensors and relates to a porous carbon-nickel composite electrode and a preparation method thereof and application thereof in detecting organic pollutants in water bodies. Background Art
[0002] As the basic raw materials of the organic chemical industry, phenolic compounds are widely used in the manufacture of phenolic resins, polymer materials, ion exchange resins, synthetic fibers, dyes, drugs, explosives, etc. There are more than 2,000 phenolic compounds in nature. Phenolic compounds in surface water mainly come from industrial wastewater such as oil refining, gas washing, coking, papermaking, synthetic ammonia, wood preservation and chemical industry. In addition to industrial phenolic wastewater, feces and nitrogen-containing organic matter also produce a small amount of phenolic compounds during the decomposition process. Due to the presence of oxygen atoms in the structure of phenolic compounds, most phenolic compounds have a fairly high solubility in water, which enhances the ability of phenolic compounds to migrate and transform, making it one of the main pollutants in the environment. It is commonly found in domestic sewage, natural water and drinking water.
[0003] Phenolic compounds are protoplasmic poisons and highly toxic substances. They can invade the cell plasma of the human body, making the cells inactive until they cause spinal cord irritation and lead to systemic poisoning. As the degree of substitution of phenolic compounds increases, the toxicity also increases. Most nitrophenols are mutagenic, and the methyl derivatives of phenols are not only teratogenic, but also carcinogenic. When a certain amount is ingested by the human body, acute poisoning symptoms may occur. Long-term drinking of water contaminated by phenols can cause dizziness, rash, itching, anemia and various neurological symptoms. When the water contains low concentrations (0.1-0.2 mg / L) of phenols, fish meat may have an unpleasant smell, and high concentrations (>5 mg / L) may cause poisoning and death. Wastewater with high phenol content should not be used for farmland irrigation, otherwise it will cause crops to wither or reduce production.
[0004] Since phenolic pollutants are extremely harmful to soil and water environment, the demand for accurate detection is becoming increasingly urgent. At present, the detection methods of phenolic pollutants mainly include chromatography, spectrophotometry, fluorescence, and immunoassay. However, these analytical methods have the disadvantages of high detection cost, complex sample processing process, and the need for professional operation, which is not conducive to the detection of a large number of samples and cannot be detected in real time. Electrochemical analysis is a type of analytical method established by using the relationship between the composition and content of the analyzed solution and its electrochemical properties. It has the advantages of fast response, low cost, high sensitivity, good selectivity, and easy operation. Therefore, the development and application of highly sensitive electrochemical sensor electrodes are crucial for realizing the rapid detection of phenolic pollutants. Summary of the invention
[0005] The purpose of the present invention is to provide a porous carbon-nickel composite electrode and a preparation method thereof and application thereof in the detection of organic pollutants in water bodies.
[0006] The porous carbon-nickel composite electrode provided by the present invention takes a metal electrode as a substrate, and comprises an electrode substrate and an electrode modification layer, wherein the surface of the electrode substrate is modified with a metal nickel layer or a copper-nickel alloy layer, the electrode modification layer is located above the electrode substrate, and the electrode modification layer comprises a porous carbon-nickel modification layer.
[0007] The porous carbon-nickel modified layer has a three-dimensional porous structure, the pore size is 20 to 80 μm, and the ligament width is 20 to 30 μm.
[0008] The porous carbon-nickel composite electrode provided by the present invention comprises a working electrode, a reference electrode and an auxiliary electrode, wherein the surface of the working electrode is modified with the porous carbon-nickel modification layer, the surface of the auxiliary electrode is modified with a platinum layer or a carbon paste modification layer, the surface of the reference electrode is modified with silver-silver chloride or porous silver-silver chloride, and the working electrode, the reference electrode and the auxiliary electrode are integrated on the same plane.
[0009] Another object of the present invention is to provide a method for preparing a porous carbon-nickel composite electrode.
[0010] The specific steps include:
[0011] S1. depositing a copper-nickel alloy layer on the surface of an electrode substrate by an electrodeposition method, and obtaining a nanoporous nickel layer by a dealloying method;
[0012] S2. Using nanoporous nickel as a substrate, porous carbon material is in situ modified on its surface, and then sintered at high temperature to obtain a porous carbon-nickel composite electrode.
[0013] Furthermore, in step S1, the electrodeposition method is specifically as follows: stainless steel is selected as the anode, the electrode substrate is used as the cathode, a copper-nickel alloy plating solution is prepared, its pH is adjusted to 8.0-9.0, the stirring speed is 300-500rmp, the current density is 2.0-4.0ASD, and the electrodeposition is performed at 45-55°C for 10-20min to obtain a copper-nickel alloy layer.
[0014] Generally, the principles for selecting complexing agents in electrodeposition solutions are: first, the selected complexing agents can form stable complexes with copper ions and nickel ions, and because the standard electrode potential of copper ions is relatively positive, the selected complexing agents must have a higher complexing ability for copper ions, while the complexing ability for nickel ions is relatively weak; second, the selected complexing agents can significantly change the precipitation potential of metal ions and increase the overpotential, but they themselves do not interfere with the anode reaction; third, the complexing system formed by the selected complexing agents and metal ions should minimize the impact on the environment. In summary, triethanolamine and trisodium citrate are selected as complexing agents for electrodeposition of copper-nickel alloys.
[0015] The copper-nickel alloy plating solution is composed of: 20-40 g / L nickel sulfate, 5-15 g / L copper sulfate, 150-200 g / L triethanolamine, 60-120 g / L trisodium citrate, 0.05-0.15 g / L 1,4-bis(2-hydroxyethoxy)-2-butyne, and 0.20-0.50 g / L 1-(2-hydroxy-3-sulfopropyl)pyridine amine salt.
[0016] Furthermore, in step S1, the dealloying method is specifically as follows: using a copper-nickel alloy electrode as a working electrode, Pt as a counter electrode, and an Ag / AgCl electrode as a reference electrode, a chronoamperometry method is used, and a 20-40 mV potential is applied in a 1.0-1.5 M HCl solution for dealloying, and the dealloying time is 300-600 s to obtain a porous nickel film layer.
[0017] Furthermore, in step S2, the preparation method of the porous carbon-nickel composite electrode is specifically as follows: using a chemical oxidation method, the porous nickel electrode is placed in a 0.05-0.10 mol / L pyrrolidone solution, and then 80-120 μL of hydrogen peroxide is added dropwise, the stirring speed is 200-300 rpm, and the reaction time is 10-12 hours; the obtained film layer is sintered at a temperature of 500-600°C for 30-40 minutes.
[0018] The surface morphology of the porous carbon-nickel composite electrode prepared by the present invention was observed by scanning electron microscope.
[0019] As attached Figure 1 The figure shows the surface morphology of the porous carbon-nickel composite electrode prepared by the present invention. It can be seen from the figure that the porous structure modified on the electrode surface greatly increases the active contact area of the material and achieves a rapid response to trace phenol pollutants, wherein the size of the pores is 20 to 80 μm and the width of the ligaments is 20 to 30 μm.
[0020] Another object of the present invention is to provide an application of a porous carbon-nickel composite electrode in the detection of organic pollutants.
[0021] The porous carbon-nickel composite electrode prepared by the present invention can realize the individual detection and simultaneous detection of m-nitrophenol, p-nitrophenol and o-nitrophenol. The porous carbon-nickel composite electrode can be connected to an electrochemical workstation via a USB interface for use, and can realize instant detection on site.
[0022] The response performance of the porous carbon-nickel composite electrode prepared by the present invention to m-nitrophenol, p-nitrophenol and o-nitrophenol was tested by differential pulse voltammetry.
[0023] The specific method for detecting metal ions using porous carbon-nickel composite electrodes is to use differential pulse voltammetry to quantitatively analyze three phenolic pollutants. The sensitivity and resolution of this test method are significantly better than those of cyclic voltammetry. Specifically, specific concentrations of m-nitrophenol, p-nitrophenol and o-nitrophenol are added to a 0.1M PBS (pH=7.0) solution containing 0.01M KCl.
[0024] As attached Figure 2 As shown, the porous carbon-nickel composite electrode prepared by the present invention detects the differential pulse voltammetry curve of m-nitrophenol, p-nitrophenol and o-nitrophenol of different concentrations. As can be seen from the figure, along with the gradual increase of three kinds of phenol pollutant concentrations, its peak current density increases gradually, indicating that the porous carbon-nickel composite electrode prepared by the present invention has excellent response characteristics to three kinds of phenol pollutants. As can be seen from the figure simultaneously, the three current peaks at -0.9V, 0.56V and 0.15V correspond to the oxidation peaks of m-nitrophenol (M-nitrophenol, m-np for short), p-nitrophenol (P-nitrophenol, p-np for short) and o-nitrophenol (O-nitrophenol, o-np for short) respectively, even if it can be found that they are very close, they can also produce obvious separation, showing that the porous carbon-nickel composite electrode prepared by the present invention can realize the simultaneous detection of m-nitrophenol, p-nitrophenol and o-nitrophenol.
[0025] Attached Figures 3 to 5 The porous carbon-nickel composite electrode prepared by the present invention is respectively a fitting diagram of the concentration and oxidation peak current density of m-nitrophenol, p-nitrophenol and o-nitrophenol detected by the porous carbon-nickel composite electrode prepared by the present invention. It can be seen from the three figures that there is a good linear relationship between the response current density and the concentration of the detected object, and the fitting values are 0.999, 0.984 and 0.979, respectively, indicating that the porous carbon-nickel composite electrode prepared by the present invention can detect m-nitrophenol, p-nitrophenol and o-nitrophenol in a wide concentration range (20-180 μM).
[0026] The present invention adopts an electrochemical in-situ modification method to in-situ modify flaky carbon materials on the surface of porous nickel, thereby ensuring the stable performance of the electrode modified material and improving the reliability of the electrode. The porous nickel with catalytic activity is compounded with carbon with high conductivity, which greatly improves the sensitivity of the electrode to the detection of trace environmental pollutants, while reducing the preparation cost, and realizing the separate detection and simultaneous detection of water pollutants such as m-nitrophenol, p-nitrophenol and o-nitrophenol in complex environments.
[0027] The beneficial effects of the present invention are:
[0028] (1) The present invention in situ modifies porous carbon and porous nickel film layers on the surface of a substrate, thereby compounding a highly conductive carbon material with catalytically active metallic nickel. The synergistic effect of the porous structure greatly increases the active sites of the reaction and improves the sensitivity of electrode detection, thereby achieving simultaneous detection of trace amounts of m-nitrophenol, p-nitrophenol and o-nitrophenol in a complex environment.
[0029] (2) The present invention has a simple preparation process and high-performance electrode materials, which can realize instant detection at the sampling site under complex environments, greatly improving the detection efficiency.
[0030] (3) The present invention adopts an electrochemical-in-situ modification method to avoid the reduction of electrode performance and improve the stability of the detection electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.
[0032] Figure 1 is a surface morphology of a porous carbon-nickel composite electrode prepared by the present invention;
[0033] Figure 2 The DPV curves of the porous carbon-nickel composite electrode prepared by the present invention for detecting m-nitrophenol, p-nitrophenol and o-nitrophenol of different concentrations;
[0034] Figure 3 It is a fitting diagram of the concentration and current density of m-nitrophenol detected by the porous carbon-nickel composite electrode prepared by the present invention;
[0035] Figure 4 It is a fitting diagram of the concentration and current density of p-nitrophenol tested by the porous carbon-nickel composite electrode prepared by the present invention;
[0036] Figure 5 It is a fitting diagram of the concentration and current density of o-nitrophenol detected by the porous carbon-nickel composite electrode prepared by the present invention. DETAILED DESCRIPTION
[0037] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail in conjunction with the following specific embodiments and with reference to the accompanying drawings.
[0038] Example 1
[0039] Preparation of porous carbon-nickel composite electrode:
[0040] S1. A copper-nickel alloy layer was deposited on the surface of the substrate electrode by electrodeposition. The composition of the copper-nickel alloy solution was: 20 g / L nickel sulfate, 5 g / L copper sulfate, 150 g / L triethanolamine, 60 g / L trisodium citrate, 0.05 g / L 1,4-bis(2-hydroxyethoxy)-2-butyne, and 0.20 g / L 1-(2-hydroxy-3-sulfopropyl)pyridine lactone salt. The anode was stainless steel, the cathode was the electrode substrate material, the solution pH was adjusted to 8.0, the stirring speed was 300 rpm, the current density was 2.0 ASD, and the copper-nickel alloy layer was obtained by electrodeposition at 55°C for 20 min. Subsequently, the chronoamperometry was used, with the copper-nickel alloy electrode as the working electrode, Pt as the counter electrode, and the Ag / AgCl electrode as the reference electrode. A 20 mV potential was applied in a 1.0 M HCl solution for electro-de-alloying. The de-alloying time was 300 s to obtain a porous nickel film layer.
[0041] S2. Using nanoporous nickel as the substrate, the porous nickel electrode was placed in a 0.05 mol / L pyrrol solution by chemical oxidation, and then 80 μL of hydrogen peroxide was added dropwise, with a stirring speed of 200 rpm and a reaction time of 10 h. The obtained film layer was sintered at 500 ° C for 30 min to obtain a porous carbon-nickel composite electrode.
[0042] Example 2
[0043] Preparation of porous carbon-nickel composite electrode:
[0044] S1. A copper-nickel alloy layer was deposited on the surface of the substrate electrode by electrodeposition. The composition of the copper-nickel alloy solution was: 40 g / L nickel sulfate, 15 g / L copper sulfate, 200 g / L triethanolamine, 120 g / L trisodium citrate, 0.15 g / L 1,4-bis(2-hydroxyethoxy)-2-butyne, and 0.50 g / L 1-(2-hydroxy-3-sulfopropyl)pyridine lactone salt. The anode was stainless steel, the cathode was the electrode substrate material, the solution pH was adjusted to 9.0, the stirring speed was 500 rpm, the current density was 4.0 ASD, and the copper-nickel alloy layer was obtained by electrodeposition at 45°C for 20 min. Subsequently, the chronoamperometry was used, with the copper-nickel alloy electrode as the working electrode, Pt as the counter electrode, and the Ag / AgCl electrode as the reference electrode. A 40 mV potential was applied in a 1.5 M HCl solution for electro-de-alloying. The de-alloying time was 600 s to obtain a porous nickel film layer.
[0045] S2. Using nanoporous nickel as the substrate, the porous nickel electrode was placed in a 0.10 mol / L pyrrol solution by chemical oxidation, and then 120 μL of hydrogen peroxide was added dropwise, with a stirring speed of 300 rpm and a reaction time of 12 h. The obtained film layer was sintered at 600 ° C for 40 min to obtain a porous carbon-nickel composite electrode.
[0046] Example 3
[0047] Preparation of porous carbon-nickel composite electrode:
[0048] S1. A copper-nickel alloy layer was deposited on the surface of the substrate electrode by electrodeposition. The composition of the copper-nickel alloy solution was: 30 g / L nickel sulfate, 10 g / L copper sulfate, 170 g / L triethanolamine, 100 g / L trisodium citrate, 0.10 g / L 1,4-bis(2-hydroxyethoxy)-2-butyne, and 0.30 g / L 1-(2-hydroxy-3-sulfopropyl)pyridine lactone salt. The anode was stainless steel, the cathode was the electrode substrate material, the solution pH was adjusted to 8.5, the stirring speed was 400 rpm, the current density was 3.0 ASD, and the copper-nickel alloy layer was obtained by electrodeposition at 50°C for 15 min. Subsequently, the chronoamperometry was used, with the copper-nickel alloy electrode as the working electrode, Pt as the counter electrode, and the Ag / AgCl electrode as the reference electrode. A 30 mV potential was applied in a 1.2 M HCl solution for electro-de-alloying. The de-alloying time was 400 s to obtain a porous nickel film layer.
[0049] S2. Using nanoporous nickel as the substrate, the porous nickel electrode was placed in a 0.07 mol / L pyrrol solution by chemical oxidation, and then 100 μL of hydrogen peroxide was added dropwise, with a stirring speed of 260 rpm and a reaction time of 11 h. The obtained film layer was sintered at 550 ° C for 35 min to obtain a porous carbon-nickel composite electrode.
[0050] Example 4
[0051] Preparation of porous carbon-nickel composite electrode:
[0052] S1. A copper-nickel alloy layer was deposited on the surface of the substrate electrode by electrodeposition. The composition of the copper-nickel alloy solution was: 35 g / L nickel sulfate, 12 g / L copper sulfate, 180 g / L triethanolamine, 110 g / L trisodium citrate, 0.07 g / L 1,4-bis(2-hydroxyethoxy)-2-butyne, and 0.40 g / L 1-(2-hydroxy-3-sulfopropyl)pyridine lactone salt. The anode was stainless steel, the cathode was the electrode substrate material, the solution pH was adjusted to 8.0, the stirring speed was 500 rpm, the current density was 4.0 ASD, and the copper-nickel alloy layer was obtained by electrodeposition at 50°C for 10 min. Subsequently, the chronoamperometry was used, with the copper-nickel alloy electrode as the working electrode, Pt as the counter electrode, and the Ag / AgCl electrode as the reference electrode. A 35 mV potential was applied in a 1.5 M HCl solution for electro-de-alloying. The de-alloying time was 500 s to obtain a porous nickel film layer.
[0053] S2. Using nanoporous nickel as the substrate, the porous nickel electrode was placed in a 0.08 mol / L pyrrol solution by chemical oxidation, and then 110 μL of hydrogen peroxide was added dropwise, with a stirring speed of 300 rpm and a reaction time of 12 h. The obtained film layer was sintered at 600 ° C for 40 min to obtain a porous carbon-nickel composite electrode.
[0054] Example 5
[0055] Porous carbon-nickel composite electrode for simultaneous detection of three phenolic pollutants:
[0056] The porous carbon-nickel composite electrode prepared in Example 1 was taken as the working electrode, platinum as the counter electrode, and silver-silver chloride as the reference electrode. It was placed in a 0.01M KCl 0.1M PBS (pH=7.0) solution, and 20μM, 40μM, 60μM, 80μM, 100μM, 120μM, 160μM, and 180μM of m-nitrophenol, p-nitrophenol, and o-nitrophenol were gradually added. The differential pulse voltammetry curve was measured to obtain the attached Figure 2 .
[0057] Attached Figure 2 It shows that when the concentration range of the three phenols is 20-180 μM, the peak current density increases with the increase of the concentration of the detection object. Therefore, the porous carbon-nickel composite electrode prepared in Example 1 has excellent response characteristics to m-nitrophenol, p-nitrophenol and o-nitrophenol, and can be used for the simultaneous detection of the above three phenol pollutants.
[0058] Example 6
[0059] The porous carbon-nickel composite electrode detects three phenolic pollutants individually:
[0060] The porous carbon-nickel composite electrode prepared in Example 2 was taken as the working electrode, platinum as the counter electrode, and silver-silver chloride as the reference electrode. It was placed in a 0.01M KCl 0.1M PBS (pH = 7.0) solution, and 20μM, 40μM, 60μM, 80μM, 100μM, 120μM, 160μM, and 180μM of m-nitrophenol were gradually added. The differential pulse voltammetry curve was measured and the fitting curve was calculated to obtain the attached Figure 3 .
[0061] The differential pulse voltammetry curves of p-nitrophenol and o-nitrophenol detected by the porous carbon-nickel composite electrode prepared in Example 2 were measured in the same way, and then the fitting curves were calculated to obtain the attached Figure 4 and attached Figure 5 It is shown that the porous carbon-nickel composite electrode prepared in Example 2 has excellent response characteristics to m-nitrophenol, p-nitrophenol and o-nitrophenol, and can be used to detect the above three phenolic pollutants separately.
[0062] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0063] In addition, it should be understood that although this specification is described in accordance with the implementation methods, not every implementation method contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should take the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation methods that can be understood by those skilled in the art. The technical details not described in detail in the present invention can be implemented by any prior art in the art. In particular, all technical features not described in detail in the present invention can be implemented by any prior art.
Claims
1. A method for preparing a porous carbon-nickel composite electrode, wherein the electrode is based on a metal electrode and includes an electrode substrate and an electrode modification layer, characterized in that: The surface of the electrode substrate is modified with a metal nickel layer or a copper-nickel alloy layer, the electrode modification layer is located above the electrode substrate, and the electrode modification layer includes a porous carbon-nickel modification layer; and the preparation method thereof includes the following steps: S1. depositing a copper-nickel alloy layer on the surface of an electrode substrate by an electrodeposition method, and obtaining a nanoporous nickel layer by a dealloying method; S2. Using nanoporous nickel as a substrate, in situ modifying porous carbon materials on its surface, and sintering at high temperature to obtain a porous carbon-nickel composite electrode. Specifically, the porous nickel electrode is placed in a 0.05-0.10 mol / L pyrrole solution by chemical oxidation, and then 80-120 μL hydrogen peroxide is added dropwise, with a stirring speed of 200-300 rpm and a reaction time of 10-12 hours. The obtained film layer is sintered at 500-600°C for 30-40 minutes.
2. The method for preparing a porous carbon-nickel composite electrode according to claim 1, characterized in that: In step S1, the electrodeposition method is specifically as follows: stainless steel is selected as the anode, the electrode substrate is used as the cathode, a copper-nickel alloy plating solution is prepared, the pH value is adjusted to 8.0-9.0, the stirring speed is 300-500 rpm, the current density is 2.0-4.0 ASD, and the electrodeposition is performed at 45-55° C. for 10-20 minutes to obtain a copper-nickel alloy layer.
3. The method for preparing a porous carbon-nickel composite electrode according to claim 2, characterized in that: The copper-nickel alloy plating solution comprises: 20-40 g / L nickel sulfate, 5-15 g / L copper sulfate, 150-200 g / L triethanolamine, 60-120 g / L trisodium citrate, 0.05-0.15 g / L 1,4-bis(2-hydroxyethoxy)-2-butyne, and 0.20-0.50 g / L 1-(2-hydroxy-3-sulfopropyl)pyridine amine salt.
4. The method for preparing a porous carbon-nickel composite electrode according to claim 1, characterized in that: In step S1, the dealloying method is specifically as follows: using a copper-nickel alloy electrode as a working electrode, Pt as a counter electrode, and an Ag / AgCl electrode as a reference electrode, using a chronoamperometry method, applying a 20-40 mV potential in a 1.0-1.5 M HCl solution for dealloying, and the dealloying time is 300-600 s to obtain a porous nickel film layer.
5. The method for preparing the porous carbon-nickel composite electrode according to claim 1, characterized in that: In step S2, the preparation method of the porous carbon-nickel composite electrode is specifically as follows: using a chemical oxidation method, placing the porous nickel electrode in a 0.05 mol / L pyrrole solution, then adding 80 μL of hydrogen peroxide dropwise, stirring at a speed of 200 rpm, and reacting for a period of 10 hours; and sintering the obtained film layer at 500° C. for 30 minutes.
6. A porous carbon-nickel composite electrode prepared by the preparation method as claimed in claim 1, characterized in that: The porous carbon-nickel modified layer has a three-dimensional porous structure, a pore size of 20 to 80 μm, and a ligament width of 20 to 30 μm.
7. A porous carbon-nickel composite electrode prepared by the preparation method as described in claim 1, wherein the porous carbon-nickel composite electrode comprises a working electrode, a reference electrode and an auxiliary electrode, wherein the surface of the working electrode is modified with the porous carbon-nickel modification layer, the surface of the auxiliary electrode is modified with a platinum layer or a carbon paste modification layer, the surface of the reference electrode is modified with silver-silver chloride or porous silver-silver chloride, and the working electrode, the reference electrode and the auxiliary electrode are integrated on the same plane.
8. Use of a porous carbon-nickel composite electrode prepared by the preparation method according to any one of claims 1 to 5 in the detection of organic pollutants.
9. The use of the porous carbon-nickel composite electrode in the detection of organic pollutants according to claim 8, characterized in that: The porous carbon-nickel composite electrode can realize the individual detection and simultaneous detection of m-nitrophenol, p-nitrophenol and o-nitrophenol.
Citation Information
Patent Citations
Preparation method for carbon nano-material modified foam nickel electrode and application
CN107014878A
Preparation method and application of nano-porous gold / carbon fiber paper composite sensing electrode allowing uric acid and dopamine to be detected simultaneously
CN110320255A
Meniscus-confined three-dimensional electrodeposition