Light emitting element and method for manufacturing the same
By setting specially designed protruding patterns and void structures on the substrate of the light-emitting element, the growth of the semiconductor layer is optimized, which solves the problems of low light extraction efficiency and reliability of existing light-emitting elements and achieves more efficient light output.
Patent Information
- Application Number
- CN202110829729.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-07-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2039-07-09
AI Technical Summary
Existing light-emitting elements have low light extraction efficiency and reliability, making it difficult to meet the requirements of high-efficiency applications.
By setting protruding patterns on a substrate, including a first layer and a second layer, adjusting the diameter, peak spacing, and height ratio of the protruding patterns, and combining them with the design of voids, the growth process of the semiconductor layer is optimized, thereby improving the efficiency of light scattering and refraction.
It significantly improves the light extraction efficiency and reliability of the light-emitting element, enhances the light scattering and refraction effects, and improves the overall light output performance.
Smart Images

Figure CN113555477B_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with the application date of July 9, 2019, application number 201980016369.2, and invention name “Light-emitting element and method for manufacturing the light-emitting element”. Technical Field
[0002] The present invention relates to a light-emitting element and a method for manufacturing the light-emitting element. Background Art
[0003] As one of the self-luminous light sources, light emitting diodes (LEDs) are widely used recently. Light emitting diodes use the characteristics of compound semiconductors to convert electrical signals into the form of light such as infrared rays, visible rays, and ultraviolet rays. As the light efficiency of light emitting elements increases, light emitting elements are being used in various fields such as display devices and lighting equipment. Summary of the invention
[0004] Technical issues
[0005] An object of the present invention is to provide a light-emitting element having high light extraction efficiency and reliability and a method for manufacturing the light-emitting element.
[0006] Technical Solution
[0007] According to one embodiment of the present invention, a light-emitting element includes: a substrate; a plurality of protruding patterns protruding from the substrate; a first semiconductor layer disposed on the substrate; an active layer disposed on the first semiconductor layer; and a second semiconductor layer disposed on the active layer, wherein each protruding pattern includes: a first layer formed as an inseparable whole with the substrate and protruding from the upper surface of the substrate; and a second layer disposed on the first layer and composed of a material different from that of the first layer, wherein when the distance between the centers of two adjacent protruding patterns is called a peak distance, the ratio of the diameter of the protruding pattern to the peak distance is 0.8 to 1.0.
[0008] According to an embodiment of the present invention, the diameter of each protruding pattern may be 2.5 μm to 3.5 μm, and the peak interval may be greater than 2.5 μm and less than 3.5 μm.
[0009] According to an embodiment of the present invention, the diameter of each protruding pattern may be 2.6 μm to 2.8 μm, and the peak distance may be 2.9 μm to 3.1 μm.
[0010] According to an embodiment of the present invention, the diameter of each protruding pattern may be 2.8 μm.
[0011] According to an embodiment of the present invention, the height ratio of the first layer to the second layer may be 0.2 to 1.5, and the height ratio of the first layer to the second layer may be 0.75 to 1.5. Alternatively, the height of the second layer may be greater than the height of the first layer.
[0012] According to an embodiment of the present invention, a diameter of the protruding pattern may be the same as or smaller than the peak distance.
[0013] According to an embodiment of the present invention, the side inclination of the first layer and the side inclination of the second layer may be different from each other.
[0014] According to an embodiment of the present invention, a cavity may be provided in a portion of the first semiconductor layer corresponding to the side of the protruding pattern.
[0015] According to an embodiment of the present invention, a light-emitting element may include: a substrate; a plurality of protruding patterns, including a first layer and a second layer, wherein the first layer is formed as an inseparable whole with the substrate and protrudes from the upper surface of the substrate, and the second layer is arranged on the first layer and is formed using a material different from that of the first layer; and a light-emitting stack, which is arranged on the substrate and emits light, wherein the light-emitting stack has a cavity arranged on at least one side of the first layer of the protruding pattern, and a ratio of the height of the second layer to the first layer is greater than 2.5 and less than 9.5.
[0016] According to one embodiment of the present invention, the light-emitting stack may include: a first semiconductor layer disposed on the substrate; an active layer disposed on the first semiconductor layer; and a second semiconductor layer disposed on the active layer, wherein the cavity is disposed in the first semiconductor layer.
[0017] According to an embodiment of the present invention, the uppermost portion of the cavity and the uppermost portion of the first layer may have the same height from the surface of the substrate.
[0018] According to an embodiment of the present invention, when the upper surface of the first layer has a circular shape when viewed from a plane, the holes may be provided corresponding to vertices of a regular hexagon inscribed in the circle.
[0019] According to an embodiment of the present invention, when cut along a plane perpendicular to the upper surface of the substrate and passing through the center of the circle, the shape of the cavity may be a right triangle, and the hypotenuse of the right triangle may be a side surface of the first layer.
[0020] According to an embodiment of the present invention, a ratio of the height of the second layer to the height of the first layer may be greater than 2.5 and less than 9.5.
[0021] According to an embodiment of the present invention, the height of the first layer may be greater than or equal to 0.25 μm and less than or equal to 0.55 μm, and the sum of the heights of the first layer and the second layer may be 2.1 μm.
[0022] A method for manufacturing a light-emitting element according to an embodiment of the present invention described above may include the following steps: forming a plurality of protruding patterns on a substrate, including a first layer protruding from the upper surface of the substrate and a second layer arranged on the first layer and made of a material different from that of the first layer; and sequentially forming a first semiconductor layer, an active layer and a second semiconductor layer on the substrate, wherein the step of forming the first semiconductor layer may include the following steps: growing a first semiconductor layer material 3D on the substrate; and growing a first semiconductor layer material 2D on the substrate.
[0023] According to one embodiment of the present invention, a light-emitting element includes: a substrate; a plurality of protruding patterns, including: a first layer and a second layer, wherein the first layer is formed as an inseparable whole with the substrate and protrudes from the surface of the substrate, and the second layer is arranged on the first layer and is composed of a material different from that of the first layer; and a light-emitting stack, which is arranged on the substrate and emits light, wherein the first layer includes an upper surface and a side surface connecting the substrate surface and the upper surface, and the upper surface of the first layer has a rough surface.
[0024] According to an embodiment of the present invention, the roughness root mean square deviation Rq of the rough surface of the upper surface of the first layer may be 0.300 nm to 0.550 nm, and the roughness arithmetic mean deviation Ra may be 0.250 nm to 0.400 nm.
[0025] According to one embodiment of the present invention, the light-emitting stack may include: a first semiconductor layer, disposed on the substrate and covering the protruding pattern; an active layer, disposed on the first semiconductor layer; and a second semiconductor layer, disposed on the active layer, wherein light emitted from the active layer passes through the first semiconductor layer and travels toward the substrate.
[0026] According to an embodiment of the present invention, the refractive index of the first layer may be greater than the refractive index of the second layer.
[0027] According to an embodiment of the present invention, the refractive index of the first layer may be 1.6 to 2.45, and the refractive index of the second layer may be 1.3 to 2.0.
[0028] According to an embodiment of the present invention, the refractive indexes of the first layer and the second layer may be smaller than the refractive index of the first semiconductor layer.
[0029] According to an embodiment of the present invention, the refractive index of the first semiconductor layer may be 2.0 to 2.5.
[0030] According to an embodiment of the present invention, the substrate may have a rough surface in a region where the protruding pattern is not provided.
[0031] According to an embodiment of the present invention, the side surface may be a reflective surface that reflects more than 90% of light traveling from the first semiconductor layer toward the side surface.
[0032] According to one embodiment of the present invention, a method for manufacturing a light-emitting element of the above-mentioned structure may include the following steps: preparing a substrate; forming a rough surface on the upper surface of the substrate; forming an insulating layer on the substrate with a material having a refractive index different from that of the substrate; forming a photoresist on the substrate and patterning the photoresist using photolithography; reflowing the photoresist; etching the insulating layer and the substrate by using the photoresist as a mask; and forming a light-emitting stack on the substrate.
[0033] According to an embodiment of the present invention, the rough surface can be formed by at least one of wet etching, dry etching and grinding.
[0034] According to an embodiment of the present invention, the step of etching the insulating layer and the substrate may be performed using anisotropy.
[0035] Technical Effects
[0036] An embodiment of the present invention provides a light-emitting element with high light extraction efficiency and reliability and a method for manufacturing the light-emitting element. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a schematic cross-sectional view illustrating a light emitting element according to an embodiment of the present invention.
[0038] Figure 2 Observed from a plane Figure 1 A plan view of a substrate having a protruding pattern among components of a light-emitting element.
[0039] Figure 3 is along Figure 2 Cross-sectional view taken along line I-I'.
[0040] Figure 4a is a diagram illustrating a substrate having a protruding pattern formed thereon and a growth direction of a first semiconductor layer in a light emitting device according to an embodiment of the present invention, Figure 4b It is a graphic Figure 4a FIG. 1 is a photograph of the shape of the first semiconductor layer actually grown on the substrate having the protruding pattern formed thereon.
[0041] Figure 5a It is an enlarged image Figure 4aThe figure inside the quadrilateral formed by the dotted line in Figure 5b yes Figure 5a Partial photos.
[0042] Figure 6 FIG. 1 is a cross-sectional view showing a semiconductor chip according to an embodiment of the present invention, and is a view showing a lateral semiconductor chip.
[0043] Figure 7 FIG. 1 is a cross-sectional view showing a semiconductor chip according to an embodiment of the present invention, and is a view showing a flip-chip type semiconductor chip.
[0044] Figure 8 TABLE 1 is a graph showing changes in light extraction efficiency according to the peak spacing of the protrusion pattern.
[0045] Fig. 9 TABLE 2 is a graph showing changes in light extraction efficiency according to the peak spacing of the protrusion pattern.
[0046] Fig.10 is a graph illustrating changes in light extraction efficiency according to diameters in Tables 3 to 6.
[0047] Fig.11 is a schematic cross-sectional view illustrating a light emitting element according to an embodiment of the present invention.
[0048] Fig.12 Observed from a plane Fig.11 A plan view of a substrate having a protruding pattern among components of a light-emitting element.
[0049] Fig.13 is along Fig.12 Cross-sectional view taken along line I-I'.
[0050] Fig.14 It is an enlarged image Fig.13 A cross-sectional view of P1.
[0051] Figures 15a to 15d It is a diagram illustrating the structure of a protruding pattern of a light emitting element in which no cavity is provided.
[0052] Figures 16a to 16d It is a diagram illustrating a structure in which a protruding pattern with a cavity is provided.
[0053] Fig.17 11 is a graph showing the simulation results of Table 11.
[0054] Figure 18a to Figure 18b It is a cross-sectional view illustrating a part of the steps of manufacturing a protruding pattern.
[0055] Fig.19FIG. 1 is a photograph of the protruding pattern and the first semiconductor layer according to an embodiment of the present invention manufactured by the aforementioned method.
[0056] Fig.20a and Fig.20b The photographs are taken of the light path and light intensity of the light emitting element having no cavity and the light emitting element having the cavity.
[0057] Fig.21 FIG. 1 is a cross-sectional view showing a semiconductor chip according to an embodiment of the present invention.
[0058] Fig. 22 is a schematic cross-sectional view illustrating a light emitting element according to an embodiment of the present invention.
[0059] Fig.23 Observed from a plane Fig. 22 A plan view of a substrate having a protruding pattern among components of a light-emitting element.
[0060] Fig.24 is along Fig.23 Cross-sectional view taken along line I-I'.
[0061] Fig.25a It is an enlarged image Fig.24 A cross-sectional view of P1, Fig.25b It is an enlarged image Fig.25a A cross-sectional view of P4.
[0062] Figure 26a to Figure 26b 1 and 10 are photographs respectively illustrating the upper surface of the first layer of a light emitting element according to a conventional invention and a light emitting element according to an embodiment of the present invention.
[0063] Figure 27a to Figure 27b is a method for manufacturing a light emitting element according to an embodiment of the present invention. Fig.24 Transmission electron microscope (TEM) photographs of parts P2 and P3.
[0064] Figure 28a to Figure 28b is a PhET simulation photograph showing the path of light caused by the shape of the side surface of the first layer.
[0065] Figure 29a to Figure 29g 1 and 2 are cross-sectional views sequentially illustrating a method of manufacturing a protruding pattern in a light emitting element according to an embodiment of the present invention.
[0066] Fig.30 FIG. 1 is a cross-sectional view showing a semiconductor chip according to an embodiment of the present invention, and is a view showing a lateral semiconductor chip.
[0067] Fig.31 FIG. 1 is a cross-sectional view showing a semiconductor chip according to an embodiment of the present invention, and shows a flip-chip type semiconductor chip.
[0068] Fig.32 Graphs showing the intensity of emitted light as the wavelength of the light emitting elements according to Comparative Example 1, Comparative Example 3, and the embodiment changes.
[0069] Preferred Embodiments
[0070] The present invention is capable of various modifications and may have various forms, and specific embodiments are illustrated in the drawings and described in detail in this specification. However, this is not intended to limit the present invention to a specific disclosed form, and should be understood as including all modifications, equivalents, and even substitutes included in the concept and technical scope of the present invention.
[0071] Hereinafter, preferred embodiments of the present invention will be described in more detail with reference to the accompanying drawings.
[0072] Figure 1 is a schematic cross-sectional view illustrating a light emitting element according to an embodiment of the present invention.
[0073] Reference Figure 1 According to an embodiment of the present invention, a light-emitting element includes a substrate 10 and a light-emitting stacked body disposed on the substrate 10 .
[0074] The light emitting stack includes a first semiconductor layer 20 , an active layer 30 , and a second semiconductor layer 40 which are sequentially disposed on a substrate 10 .
[0075] The substrate 10 may be a light-transmitting or non-light-transmitting substrate, and may be a conductive or insulating substrate. The substrate 10 may be a growth substrate used for growing a semiconductor single crystal, for example, a growth substrate used for growing a nitride single crystal.
[0076] A sapphire substrate may be used as the substrate 10. However, the material of the substrate 10 is not limited thereto, and may be composed of a variety of materials, for example, SiC, Si, GaAs, GaN, ZnO, GaP, InP, Ge, Ga2O3, etc. In particular, sapphire may have a crystal having hexa-rhombo R3c symmetry. In the case of sapphire, the lattice constants in the c-axis and a-axis directions are and It has C(0001) plane, A(1120) plane, R(1102) plane, etc. The C-plane of sapphire is easier to grow nitride thin films and is stable at high temperatures, so it can be used as a substrate for growing nitride semiconductors.
[0077] In one embodiment of the present invention, the substrate 10 is a patterned substrate, and a plurality of protruding patterns 11 are arranged on its upper surface. In other words, the protruding patterns 11 are arranged to protrude upward from the upper surface of the substrate 10. In one embodiment of the present invention, the protruding patterns 11 may be arranged in an inverted cone shape whose width gradually decreases upward, and when the protruding patterns 11 are cut along a vertical surface on the substrate 10, the cross-section of the protruding patterns 11 may be approximately triangular.
[0078] The protruding pattern 11 includes a first layer 13 and a second layer 15 which are sequentially stacked from the upper surface of the substrate 10. The first layer 13 is disposed on the substrate 10, and the second layer 15 is disposed on the first layer 13.
[0079] The first layer 13 is integrally formed with the substrate 10. Therefore, the first layer 13 is composed of the same material as the substrate 10. In the case where the shape of the protruding pattern 11 is a cone, the upper surface of the first layer 13 may have a circular shape.
[0080] The second layer 15 is made of a material different from that of the first layer 13. The material of the second layer 15 may be a material having a different refractive index from that of the material of the first layer 13. In one embodiment of the present invention, the refractive index of the first layer 13 may be greater than that of the second layer 15. In this case, the material of the second layer 15 may be a variety of insulating materials with a refractive index smaller than that of the first layer 13. For example, an insulating material having a refractive index of about 1.0 to about 1.7 may be used. As a material having such a refractive index, SiO x 、SiO x N y 、SiN x In one embodiment of the present invention, the first layer 13 may be made of sapphire and the second layer 15 may be made of SiO 2 . In this case, the refractive index of the first layer 13 is 1.76 and the refractive index of the second layer 15 is about 1.46, which may be smaller than the refractive index of the substrate 10 .
[0081] A plurality of compound semiconductor layers may be disposed on the substrate 10 having the protruding pattern 11. The plurality of compound semiconductor layers may be formed by various methods, for example, electron beam deposition, physical vapor deposition (PVD: physical vapor deposition), chemical vapor deposition (CVD: chemical vapor deposition), plasma laser deposition (PLD: plasma laser deposition), dual-type thermal evaporation, sputtering, metal organic chemical vapor deposition (MOCVD: metal organic chemical vapor deposition), etc. However, the method of forming the plurality of compound layers is not limited thereto.
[0082] The first semiconductor layer 20 may be disposed on the substrate 10. The first semiconductor layer 20 is a semiconductor layer doped with a first conductive type dopant. The first conductive type dopant may be an n-type dopant. The first conductive type dopant may be Si, Ge, Se, Te or C.
[0083] In one embodiment of the present invention, the first semiconductor layer 20 may include a nitride-based semiconductor material. For example, the first semiconductor layer 20 may include a nitride-based semiconductor material. x Al y Ga 1-x-y N(0≤x≤1, 0≤y≤1, 0≤x+y≤1). In one embodiment of the present invention, the semiconductor material having the composition formula may include GaN, AlN, AlGaN, InGaN, InN, InAlGaN, AlInN, AlGaAs, GaP, GaAs, GaAsP, AlGaInP, etc. The first semiconductor layer 20 may be formed by growing the semiconductor material into an n-type dopant including Si, Ge, Sn, Se, Te, etc.
[0084] In one embodiment of the present invention, the first semiconductor layer 20 may also have a structure formed by alternating two types of layers having different band gaps. The structure formed by alternating two types of layers having different band gaps may be a superlattice structure, whereby the current spreading of the first semiconductor layer 20 may be improved and stress may be relieved.
[0085] Two types of layers with different band gaps are formed alternately, thereby including different thin film crystal layers. In this case, when two layers with different band gaps are alternately stacked, the periodic structure is composed of a crystal lattice longer than the basic unit lattice. The two layers with different band gaps are a layer with a wide band gap and a layer with a narrow band gap. In one embodiment of the present invention, the layer with a wide band gap may be Al a Ga b In (1-a-b) N (0≤a<1, 0<b≤1), for example, can be a GaN layer. The layer with a narrow band gap can be an Al a Ga b In (1-a-b) N (0≤a<1, 0<b≤1), for example, can be Ga b In (1-b) N(0<b≤1).
[0086] In one embodiment of the present invention, at least one of the wide bandgap layer and the narrow bandgap layer may include n-type impurities.
[0087] The active layer 30 corresponds to a light emitting layer provided on the first semiconductor layer 20 .
[0088] The active layer 30 is a layer that releases light by the difference in band gap according to the energy band of the material forming the active layer 30 when electrons (or holes) injected through the first conductive semiconductor layer and holes (or electrons) injected through the second semiconductor layer 40 meet each other. The active layer 30 can emit at least one peak wavelength among ultraviolet, blue, green, and red.
[0089] The active layer 30 may be implemented by a compound semiconductor. The active layer 30 may be implemented by, for example, at least one of a group 3-5 or group 2-6 compound semiconductor. A quantum well structure may be used in the active layer 30, and a multi-quantum well structure (Multi-Quantum Well) may be provided in which quantum well layers and barrier layers are alternately stacked. However, the structure of the active layer 30 is not limited thereto, and may also be a quantum wire structure, a quantum dot structure, or the like.
[0090] In one embodiment of the present invention, the quantum well may be composed of In x Al y Ga 1-x-y The barrier layer can be made of a material having a composition formula of In x Al y Ga 1-x-yThe barrier layer may be formed of a semiconductor material having a composition formula of N(0≤x≤1, 0≤y≤1, 0≤x+y≤1) and may be provided at a composition ratio different from that of the well layer. Here, the barrier layer may have a wider band gap than that of the well layer.
[0091] For example, the well layer and the barrier layer may be formed using at least one of the paired materials of AlGaAs / GaAs, InGaAs / GaAs, InGaN / GaN, GaN / AlGaN, AlGaN / AlGaN, InGaN / AlGaN, InGaN / InGaN, InGaP / GaP, AlInGaP / InGaP, and InP / GaAs. In one embodiment of the present invention, the well layer of the active layer 30 may be implemented by InGaN, and the barrier layer may be implemented by an AlGaN-based semiconductor. In one embodiment of the present invention, the indium component of the well layer may have a higher composition ratio than the indium component of the barrier layer, and the barrier layer may not have an indium component. Alternatively, aluminum is not included in the well layer, while aluminum may be included in the barrier layer. However, the composition of the well layer and the barrier layer is not limited thereto.
[0092] According to one embodiment of the present invention, the barrier layer may have a thickness thicker than that of the well layer. However, if the well layer is too thin, the carrier confinement efficiency will be reduced, and if it is too thick, the carrier may be over-confined. If the barrier layer is too thin, the electron blocking efficiency will be reduced, and if it is too thick, the electrons may be over-blocked.
[0093] Accordingly, by appropriately adjusting the thickness of the barrier layer and the well layer, each carrier can be effectively confined to the well layer according to the wavelength of light and the quantum well structure.
[0094] In one embodiment of the present invention, the thickness of each well layer is not particularly limited, and each thickness may be the same or different. When the thickness of each well layer is the same, since the quantum energy level is the same, the wavelength of light emitted from each well layer may become the same. In this case, a light emission spectrum with a narrow half-width can be obtained. When the thickness of each well layer is different, the wavelength of light emission in each well layer may become different, thereby widening the width of the light emission spectrum.
[0095] In one embodiment of the present invention, at least one of the plurality of barrier layers may include a dopant, for example, at least one of an n-type dopant and a p-type dopant. When the barrier layer is added with an n-type dopant, it may be an n-type semiconductor layer. When the barrier layer is an n-type semiconductor layer, the injection efficiency of electrons injected into the active layer 30 may be increased.
[0096] In one embodiment of the present invention, although the barrier layers may have various thicknesses, the barrier layer located at the uppermost portion may have the same thickness as or a greater thickness than the other barrier layers.
[0097] In the case where the active layer 30 has a multi-quantum well structure, the composition of the quantum well layer and the barrier layer can be set according to the light emission wavelength required by the light emitting element. In one embodiment of the present invention, the composition of the multiple well layers can be the same or different. For example, the well layer on the lower side may include impurities, while the well layer on the upper side may not include impurities.
[0098] The second semiconductor layer 40 is disposed on the active layer 30 .
[0099] The second semiconductor layer 40 is a semiconductor layer having a second conductive type dopant, wherein the second conductive type dopant has a polarity opposite to that of the first conductive type dopant. The second conductive type dopant may be a p-type dopant, and may include Mg, Zn, Ca, Sr, Ba, etc., for example.
[0100] In one embodiment of the present invention, the second semiconductor layer 40 may include a nitride-based semiconductor material. x Al y Ga 1-x-y N(0≤x≤1, ≤y≤1, 0≤x+y≤1). In one embodiment of the present invention, the semiconductor material having the composition formula may include GaN, AlN, AlGaN, InGaN, InN, InAlGaN, AlInN, AlGaAs, GaP, GaAs, GaAsP, AlGaInP, etc. The second semiconductor layer 40 may be formed by growing the semiconductor material into a p-type dopant including Mg, Zn, Ca, Sr, Ba, etc.
[0101] Although not shown, in addition to the substrate 10 , the first semiconductor layer 20 , the active layer 30 , and the second semiconductor layer 40 , a functional layer such as a buffer layer and / or an electron blocking layer may be additionally provided.
[0102] For example, a buffer layer may be disposed on the substrate 10 and the first semiconductor layer 20. The buffer layer may be formed as a single layer or multiple layers. In one embodiment of the present invention, the buffer layer may be formed as In x Al y Ga 1-x-y N (0≤x≤1, 0≤y≤1, 0≤x+y≤1) may include at least one of materials such as AlN, AlGaN, InGaN, InN, InAlGaN, AlInN, AlGaAs, GaP, GaAs, GaAsP, AlGaInP and ZnO.
[0103] The buffer layer may be formed into a superlattice structure by alternately arranging different semiconductor layers. The buffer layer may be arranged to ease the lattice constant between the substrate 10 and the nitride series semiconductor layer, and may be defined as a defect control layer. The lattice constant of the buffer layer may have a value between the lattice constants of the substrate 10 and the nitride series semiconductor layer. The buffer layer may not be formed, and there is no restriction on this.
[0104] Furthermore, an electron blocking layer may be additionally arranged between the second semiconductor layer 40 and the active layer 30. The electron blocking layer may reduce the decrease in crystallinity caused by the dopant in the second semiconductor layer 40, and may prevent the dopant in the second semiconductor layer 40 from diffusing to the active layer 30. Furthermore, the electron blocking layer may block electrons from the active layer 30 from traveling to the second semiconductor layer 40, thereby preventing the diffusion of current between the electron blocking layer and the second semiconductor layer 40. In one embodiment of the present invention, the electron blocking layer may be formed by using a material having In x Al y Ga 1-x-y The electron blocking layer may be formed of a semiconductor material having a composition formula of N (0≤x≤1, 0≤y≤1, 0≤x+y≤1). As an example, the electron blocking layer may be formed of at least one of GaN, AlGaN, InGaN, InAlGaN, and AlInN.
[0105] The electron blocking layer may have a wider band gap than the band gap of the barrier layer in the active layer 30. The band gap of the electron blocking layer may vary according to the composition of the material constituting the electron blocking layer. For example, in the case where the electron blocking layer is composed of AlGaN, the band gap may be set to be different by changing the composition ratio of aluminum. The wider the band gap, the better the electron blocking effect.
[0106] In one embodiment of the present invention, the electron blocking layer may be arranged as a single layer or multiple layers, and may include a second conductive type dopant, for example, may include a p-type conductive type dopant. Accordingly, the electron blocking layer may be a p-type semiconductor layer having a p-type dopant such as Mg, Zn, Ca, Sr, Ba, etc., and the electron blocking layer may be at least one of GaN, AlGaN, and InGaN including a p-type dopant. In one embodiment of the present invention, the resistance blocking layer may be formed as a superlattice structure in which at least two layers different from each other are alternately arranged.
[0107] In this embodiment, the buffer layer and the electron blocking layer are disclosed as an example, and at least one of the buffer layer and the electron blocking layer can be omitted. In addition, of course, additional functional layers other than the buffer layer and the electron blocking layer can be added to the light emitting element.
[0108] As described above, in the light emitting element according to an embodiment of the present invention, a plurality of protruding patterns 11 are disposed on the substrate 10 . The protruding patterns 11 are described in detail.
[0109] Figure 2 Observed from a plane Figure 1 A plan view of a substrate 10 provided with a protruding pattern 11 among the components of a light emitting element, Figure 3 is along Figure 2 A cross-sectional view taken along line I-I'.
[0110] Reference Figure 2 and Figure 3 A protruding pattern 11 is disposed on the upper surface of the substrate 10 , and the protruding pattern 11 includes a first layer 13 and a second layer 15 .
[0111] Each protrusion pattern 11 may have a circular shape when viewed from a plane. In the case where the protrusion pattern 11 is provided in a cone shape, the apex portion of the cone becomes the center.
[0112] The protruding pattern 11 may be set to have a size of a predetermined diameter DM and a height HT. The diameter DM means the width of the lowest end of the protruding pattern 11 when viewed in cross section, and the height HT means the distance from the upper surface of the substrate 10 to the vertex of the protruding pattern 11. In the present embodiment, each protruding pattern 11 may have the same diameter DM and height HT as each other. However, each protruding pattern 11 may not have exactly the same diameter DM and height HT, as the diameter DM and height HT may differ within a predetermined range.
[0113] When viewed from a plane, the first layer 13 and the second layer 15 have different diameters, but can be set in a concentric shape with the same center. In the case where the protruding pattern 11 is set in a conical shape, the diameter of the first layer 13 is larger than the diameter of the second layer 15. Here, the diameters of the first layer 13 and the second layer 15 mean the width of the lowest end of the first layer 13 and the second layer 15 when viewed from a cross section.
[0114] In one embodiment of the present invention, the protruding pattern 11 can be arranged in various forms on the upper surface of the substrate 10. For example, the protruding pattern 11 can be arranged at each vertex of a quadrilateral in a quadrangular lattice pattern, or at each vertex of a hexagon in a hexagonal lattice pattern. In one embodiment of the present invention, the protruding pattern 11 is arranged at each vertex of a quadrilateral in a quadrangular lattice pattern as an example.
[0115] The protruding patterns 11 may be arranged with a predetermined peak pitch PT and a distance DT. The peak pitch PT is the distance between the centers of two adjacent protruding patterns 11 when viewed from a plane, and the distance DT is the distance between the edges of two adjacent protruding patterns 11 when viewed from a plane.
[0116] In one embodiment of the present invention, the diameter DM of the protruding pattern 11 may be the same as or smaller than the peak pitch PT. In the case where the diameter DM of the protruding pattern 11 is larger than the peak pitch PT, the protruding pattern 11 will be overlapped on the plane, and the area of the upper surface of the substrate 10 where the protruding pattern 11 is not provided will become too small. The upper surface of the substrate 10 not blocked by the protruding pattern 11 is the location where the growth of the first semiconductor layer 20 will occur later. Therefore, in the case where the diameter DM of the protruding pattern 11 is larger than the peak pitch PT, the first semiconductor layer 20 (see FIG. 2 ) will not be sufficiently grown later. Figure 1 ) growth, which is not conducive to the manufacture of light-emitting components.
[0117] According to an embodiment of the present invention, the peak spacing PT and the spacing may have different values according to the arrangement direction. Although the peak spacing PT and / or the spacing DT are shown to be the same in this embodiment, this is only for the convenience of explanation, and the peak spacing PT and the spacing do not need to be all the same, and the peak spacing PT and / or the spacing DT may have some differences within a predetermined range.
[0118] In one embodiment of the present invention, the peak distance PT of the protruding pattern 11 may have a value within a predetermined range according to the diameter DM, and the ratio of the diameter DM of the protruding pattern 11 to the peak distance PT may be within a range of about 0.8 to about 1.0. For example, when the diameter DM of the protruding pattern 11 is 2.5 μm to 3.5 μm, the peak distance PT may be greater than 2.5 μm and less than 3.5 μm. Alternatively, when the diameter DM of the protruding pattern 11 is 2.5 μm to 2.8 μm, the peak distance PT may be 2.9 μm to 3.1 μm.
[0119] In one embodiment of the present invention, in the protruding pattern 11, the first layer 13 and the second layer 15 may be formed at a plurality of height ratios. Here, the height H1 of the first layer 13 is formed to have a value greater than a predetermined value. If, in the case where the height H1 of the first layer 13 is 0, the growth of the first semiconductor layer 20 from the substrate 10 may be hindered due to impurities remaining on the upper surface of the substrate 10 during the process. In one embodiment of the present invention, the ratio of the height H1 of the first layer 13 to the height H2 of the second layer 15 may be 0.2 to 1.5. In one embodiment of the present invention, the ratio of the height H1 of the first layer 13 to the height H2 of the second layer 15 may be 0.75 to 1.5, or the ratio of the height H1 of the first layer 13 to the height H2 of the second layer 15 may exceed 1. In one embodiment of the present invention, the ratio of the height H1 of the first layer 13 to the height H2 of the second layer 15 is 0.75, so the first layer 13 may be 0.9 μm, the second layer 15 may be 1.2 μm, and the diameter DM of the protruding pattern 11 may be about 2.7 μm to 2.9 μm, for example, 2.8 μm.
[0120] In one embodiment of the present invention, when the height H2 of the second layer 15 is formed to be greater than the height H1 of the first layer 13 , the growth of crystals toward the side of the first layer 13 is reduced, thereby improving the quality of the crystals.
[0121] In one embodiment of the present invention, the side inclinations of the first layer 13 and the second layer 15 may be at least partially the same or different from each other. Although the figure illustrates a situation where the inclinations of the first layer 13 and the second layer 15 have the same value, it is not limited to this. The side inclinations of the first layer 13 and the second layer 15 may be at least partially the same or different from each other. In particular, the inclinations of the portions where the first layer 13 and the second layer 15 are connected may be different from each other. Since the materials of the first layer 13 and the second layer 15 are different from each other, when the etching process is performed, the side inclinations can be set to be different according to the process conditions. In one embodiment of the present invention, by forming the inclinations of the first layer 13 and the second layer 15 to be different, the scattering degree of light emitted from the light-emitting element can be increased, thereby improving the light emission efficiency.
[0122] In one embodiment of the present invention, the arrangement of the protruding patterns 11 may be arranged regularly as shown in the figure, but is not limited thereto. For example, the protruding patterns 11 may be arranged irregularly. In this case, from the perspective of the entire substrate 10, the peak pitch PT and the spacing of the protruding patterns 11 in each single area are within a predetermined range, and in this case, the density may be substantially set to the same level.
[0123] In one embodiment of the present invention, for the sake of convenience, only the protruding pattern 11 is shown as a cone. However, within the scope of the present invention, the protruding pattern 11 can be deformed into various forms. For example, the protruding pattern 11 can have a polygonal cone shape. Alternatively, even if it is set to a cone shape, the shape of the curved surface constituting the side surface can be partially deformed.
[0124] Below, refer to Figures 1 to 3 , describing the light-emitting element in the above structure.
[0125] First, a substrate 10 is prepared, and an insulating layer is stacked on the substrate 10 using a material for forming the second layer 15. As described above, the substrate 10 can be made of materials such as SiC, Si, GaAs, GaN, ZnO, GaP, InP, Ge, and Ga2O3, and the insulating layer can be made of SiO x 、SiO x N y 、SiN x And other materials.
[0126] Thereafter, a photoresist is coated on the insulating layer, and after a photoresist pattern is formed by exposure and development, the insulating layer and a portion of the substrate 10 are etched using the photoresist pattern as a mask. Accordingly, the insulating layer except for the portion where the protruding pattern 11 needs to be formed is etched, thereby forming the second layer 15. The upper surface of the substrate 10 is exposed in the portion where the second layer 15 is not formed. Here, the upper surface of the substrate 10 is further etched so that more is etched than the original upper surface of the substrate 10, thereby forming the first layer. If etching is performed in a manner that only the second layer 15 is formed and the original upper surface of the substrate 10 is exposed, theoretically, since the upper surface of the substrate 10 is exposed, it can be judged that the growth of the semiconductor layer is likely to occur later, but in fact, due to etching residues or impurities remaining on the upper surface of the substrate 10, the growth of the first semiconductor layer 20 will not occur normally later. Therefore, further etching is performed to completely remove the etching residues or impurities on the substrate 10. Accordingly, the first layer 13 is formed.
[0127] The etching for forming the first layer 13 and the second layer 15 may be performed using various methods under various conditions according to the material. For example, the insulating layer and a portion of the substrate 10 may be patterned using dry etching.
[0128] The second layer 15 and the first layer 13 can be sequentially formed in the above-described method, and patterning can be performed using the same or different etching gases.
[0129] A first semiconductor layer 20 is formed on the substrate 10 formed with the protruding pattern 11. The first semiconductor layer 20 grows from the exposed surface of the substrate 10 first in an upper direction, and then in an upper direction and a side direction.
[0130] Figure 4a is a diagram illustrating a substrate 10 having a protruding pattern 11 formed thereon and a growth direction of a first semiconductor layer 20 in a light emitting device according to an embodiment of the present invention, Figure 4b is for Figure 4a The photograph showing the state in which the first semiconductor layer 20 is actually grown on the substrate 10 on which the protruding pattern 11 is formed is shown. Figure 5a It is an enlarged image Figure 4a The figure inside the quadrilateral formed by the dotted line in Figure 5b yes Figure 5a Some photos. Figure 4a and Figure 5a In the figure, for the convenience of explanation, the main growth direction of the semiconductor layer is indicated by an arrow.
[0131] Reference Figure 4a , Figure 4b , Figure 5a and Figure 5b First, the first semiconductor layer 20 is formed upward.
[0132] The first semiconductor layer 20 can be formed of semiconductor layers of various materials, for example, an n-type nitride semiconductor layer, and can be formed by metalorganic vapor phase epitaxy (Metalorganic vapor phase epitaxy), molecular beam epitaxy (MBE), or hydride vapor phase epitaxy (HVPE).
[0133] The initial growth of the first semiconductor layer 20 mainly occurs from the exposed surface of the substrate 10 toward the upper direction, and no growth occurs on the upper surface of the second layer 15 .
[0134] After partially growing upward, the first semiconductor layer 20 grows upward and sideways. For ease of explanation, the figure shows a first growth pattern 21 that mainly grows upward and a second growth pattern 23 that grows upward and sideways and has a dominant growth direction.
[0135] In one embodiment of the present invention, in order to grow the first semiconductor layer 20 in the lateral direction (horizontal direction in the figure), a lateral epitaxial overgrowth (ELOG: Epitaxiallateral over-growth) can be used by a metal organic chemical vapor deposition (MOCVD) method. The first semiconductor layer 20 continues to grow in the lateral direction and the upper direction, so as to be merged to cover the entire surface of the substrate 10 including the surface of the second layer 15. Accordingly, the first semiconductor layer 20 becomes a plate shape that covers the entire surface of the substrate 10.
[0136] In one embodiment of the present invention, when forming the protruding pattern 11 , the ratio of the diameter DM to the peak interval is formed within a range of about 0.8 to about 1.0, in order to reduce defects when the first semiconductor layer 20 is grown.
[0137] In one embodiment of the present invention, the upper surface of the substrate 10 exposed between the protruding patterns 11 becomes a substantial part of the growth core, and growth occurs in the upper direction from the upper surface of the substrate 10 as in the first growth pattern 21. Thereafter, the first semiconductor layer 20 grows in the horizontal direction by the lateral epitaxial overgrowth method as in the second growth pattern 23. When the first semiconductor layer 20 grows, if the surface in the upper direction is called the upper surface, and the surface in the side direction is called the side surface, then in the case where the first semiconductor layer 20 is epitaxially grown by the lateral epitaxial overgrowth, due to the conditions of the lateral epitaxial overgrowth, the growth of the side surface is more dominant than the growth of the upper surface, and the growth ratio of the m-axis and the c-axis becomes about 2:1. Although the side surface of the first semiconductor layer 20 may be perpendicular to the upper surface of the first semiconductor layer 20 during growth, it is not limited thereto, and may be a surface inclined to the upper surface of the first semiconductor layer 20. In one embodiment of the present invention, the upper surface of the first semiconductor layer 20 is equivalent to the (0001) surface, and the side surface of the first semiconductor layer 20 is equivalent to the (10-11) surface.
[0138] In one embodiment of the present invention, the peak spacing between the protruding patterns 11 is set within the above range, thereby facilitating the growth of the first semiconductor layer 20 and ultimately improving the light extraction efficiency of the light emitting element.
[0139] If, in the case where the peak spacing is smaller than the above-mentioned range, the spacing between adjacent protruding patterns 11 is not sufficient, so that the growth of crystals is relatively slow. Moreover, even if growth occurs, since the growth occurs in the side direction when the growth area is small, a void VD is formed on the side. Here, the void VD is ultimately formed corresponding to the growth direction of the crystal surface, and is formed on the side corresponding to each vertex of the hexagon with the center of the protruding pattern 11 as a reference. In the case where the void VD is formed larger, since the crystals also grow in a direction different from the overall growth direction on the side of the protruding pattern 11 of the first layer 13 corresponding to the portion where the void VD is formed (the portion indicated by the dotted ellipse in the figure), it appears as a defect. The defect will eventually cause a reduction in the light extraction efficiency of the light-emitting element. If, when the peak spacing is greater than the above range, the spacing between adjacent protruding patterns 11 is wide enough so that the crystal growth is faster, thereby, although the size of the void is smaller and the defects in the side of the protruding pattern are reduced, the protruding patterns 11 are farther apart, so that the light scattering effect caused by the protruding patterns 11 will be reduced, thereby reducing the light extraction efficiency.
[0140] After the first semiconductor layer 20 is formed as a whole by side growth, the first semiconductor layer 20 can be selectively grown further upward by using a hydride vapor phase growth method. When the first semiconductor layer 20 is formed by a metal organic chemical vapor deposition method, the film formation speed is slower than that of the hydride vapor phase growth method, so the hydride vapor phase growth method can be used when the first semiconductor layer 20 is grown to a sufficient thickness faster.
[0141] Again, refer to Figures 1 to 3 In one embodiment of the present invention, a buffer layer may be formed on the substrate 10 before forming the first semiconductor layer 20. In one embodiment of the present invention, in the first semiconductor layer 20, two layers with different band gaps are alternately stacked, thereby forming a superlattice structure. An active layer 30 is formed on the first semiconductor layer 20. In one embodiment of the present invention, as the active layer 30, a quantum well layer and a barrier layer may be alternately stacked to form a quantum well structure. An electron blocking layer is formed on the active layer 30, and then a second semiconductor layer 40 is formed on the active layer 30, thereby manufacturing a light-emitting stack.
[0142] The light emitting element having the above structure improves light extraction efficiency and reduces defects, thereby improving reliability.
[0143] The light emitting element of the above structure can be realized as semiconductor chips in various forms.
[0144] Figure 6 FIG. 1 is a cross-sectional view showing a semiconductor chip according to an embodiment of the present invention, and is a view showing a lateral semiconductor chip.
[0145] Reference Figure 6 The semiconductor chip includes a light emitting element, a first electrode 110 and a second electrode 120 connected to the light emitting element. The light emitting element includes a substrate 10 and a first semiconductor layer 20, an active layer 30, and a second semiconductor layer 40 disposed on the substrate 10.
[0146] In this embodiment, the first electrode 110 is disposed on the first semiconductor layer 20 where the active layer 30 and the second semiconductor layer 40 are not disposed, and the second electrode 120 is arranged on the second semiconductor layer 40 .
[0147] The first electrode 110 and / or the second electrode 120 may be formed of a single layer or multiple layers of metal. The material of the first electrode 110 and / or the second electrode 120 may include various metals such as Al, Ti, Cr, Ni, Au, Ag, Cr, Cu, Ti, Ru, Rh, Ir, Mg, Zn, Al, In, Ta, Pd, Co, and alloys thereof.
[0148] Here, a plurality of protrusion patterns 11 for improving light emission efficiency are provided on the upper surface of the substrate 10. As described above, the protrusion pattern 11 may be provided on the substrate 10 in a conical shape including the first layer 13 and the second layer 15.
[0149] An insulating film 130 is disposed on the first electrode 110 and the second electrode 120, and a contact hole is disposed on the insulating film 130 to expose the first electrode 110 and the second electrode 120. The insulating film 130 can be arranged on the upper surface of the second semiconductor layer 40 and the side of the semiconductor layer, and can selectively contact the first electrode 110 and the second electrode 120. The insulating film 130 may include an insulating material or an insulating resin formed by at least one of an oxide, nitride, fluoride and sulfide having at least one of Al, Cr, Si, Ti, Zn and Zr. For example, the insulating film 130 can be selectively formed in SiO2, Si3N4, Al2O3, TiO2. The insulating film 130 can be formed as a single layer or a multilayer, which is not limited.
[0150] In one embodiment of the present invention, the first electrode 110 and the second electrode 120 may be connected to other components by exposing the contact hole. For example, the first electrode 110 and the second electrode 120 may be provided with a first pad and a second pad connected by the contact hole. Figure 1 Although the above description is given, the light emitting element may include components with additional functions in addition to the above layers. For example, it may include a reflection layer for reflecting light, an additional insulation layer for insulating a specific component, a solder prevention layer for preventing solder diffusion, and other layers.
[0151] Furthermore, when forming a lateral light-emitting element, the mesa may be formed in various forms. Of course, the positions or shapes of the first electrode 110 and the second electrode 120 may also be changed in various ways.
[0152] The light emitting device according to an embodiment of the present invention emits light by applying a signal to the first electrode 110 and the second electrode 120 to turn them on. The emitted light may travel toward the lower part of the first semiconductor layer 20 or toward the upper part of the second semiconductor layer 40 .
[0153] Although the semiconductor chip using the light emitting element according to one embodiment of the present invention is illustrated as a lateral semiconductor chip, it is not limited thereto. For example, the light emitting element according to one embodiment of the present invention can be applied to a vertical or flip chip type semiconductor chip.
[0154] Figure 71 is a cross-sectional view of a semiconductor chip according to an embodiment of the present invention, and is a view of a flip-chip type semiconductor chip. After a flip-chip type semiconductor is formed on a substrate 10, it can be flipped and mounted on other components, and the figure shows a flipped state.
[0155] Reference Figure 7 The semiconductor chip includes a light emitting element, a first electrode 110 and a second electrode 120 connected to the light emitting element. The light emitting element includes a substrate 10 and a first semiconductor layer 20, an active layer 30, and a second semiconductor layer 40 stacked on the substrate 10.
[0156] In this embodiment, the light emitting element may include at least one mesa having an active layer 30 and a second semiconductor layer 40. The mesa may include a plurality of protruding patterns 11, and the plurality of protruding patterns 11 may be spaced apart from each other. An insulating film 130 is disposed on the mesa, and the insulating film 130 has a contact hole exposing a portion between the first semiconductor layer 20 and the mesa and the second semiconductor layer 40. The first electrode 110 is connected to the exposed first semiconductor layer 20 through the contact hole between the mesas, and the second electrode 120 is connected to the exposed second semiconductor layer 40 through the contact hole formed on the second semiconductor layer 40.
[0157] Hereinafter, the light extraction efficiency of the light emitting element according to the above-described embodiment of the present invention will be described.
[0158] Table 1 is data showing changes in light extraction efficiency according to changes in the peak spacing when the diameter and height of the protruding pattern on the substrate are the same in the light emitting element. Figure 8 TABLE 1 is a graph showing changes in light extraction efficiency according to the peak spacing of the protrusion pattern.
[0159] In the following embodiments, the light intensity increase / decrease rate represents the light intensity increase / decrease rate compared to a light emitting element according to the prior invention in which the protruding pattern is composed of only the first layer but not the second layer, and the peak spacing of the protruding pattern of the prior invention is 3 μm, the total height is 1.7 μm, and the diameter is 2.7 μm.
[0160]
Table 1
[0161]
[0162] Table 2 is data showing changes in light extraction efficiency according to changes in the peak spacing when the diameter and height of the protruding pattern on the substrate are the same in the light emitting element. Fig. 9 TABLE 2 is a graph showing changes in light extraction efficiency according to the peak spacing of the protrusion pattern.
[0163]
Table 2
[0164]
[0165] As described above, when the height and the diameter are the same, the amount of light varies depending on the peak spacing, and when the ratio of the protruding pattern diameter to the peak spacing is in the range of about 0.8 to about 1.0, the rate of increase in brightness is the highest. In particular, as can be seen in Tables 1 and 2, the rate of increase in light amount varies slightly depending on the height of the first layer and the height of the second layer, but both show a maximum value at 3 μm.
[0166] Tables 3 to 6 are data showing changes in light extraction efficiency according to changes in diameter when the peak pitch and height of the protrusion pattern on the substrate are the same in the light emitting element. Fig.10 Graphs illustrating changes in light extraction efficiency according to diameters in Tables 3 to 6. Fig.10 In the figure, the figures representing Examples 1 to 4 represent the data of Tables 3 to 6 respectively.
[0167]
Table 3
[0168]
[0169]
Table 4
[0170]
[0171]
[0172]
Table 5
[0173]
[0174]
Table 6
[0175]
[0176] As shown in Tables 3 to 5 above and Fig.10 It can be confirmed that when the diameter of the protruding pattern is 2.8, the luminous efficiency is relatively high regardless of the peak interval and height, and in particular, when the ratio of the second layer to the first layer is 0.75, the highest luminous efficiency is exhibited.
[0177] Tables 7 to 10 are data showing changes in light extraction efficiency according to changes in the heights of the first layer and the second layer when the peak interval and the diameter of the protrusion pattern on the substrate are the same in the light emitting element.
[0178]
Table 7
[0179]
[0180]
Table 8
[0181]
[0182]
Table 9
[0183]
[0184]
Table 10
[0185]
[0186] Referring to Tables 7 and 8, there are differences in the light intensity increase and decrease rates according to the heights of the first and second layers. Generally speaking, the light intensity increase rate is greater when the height of the second layer is higher than that of the first layer, but this is not the case for some layers.
[0187] As described above, the present invention provides a light emitting element in which the light extraction efficiency is significantly improved by setting the diameter of the protrusion pattern on the substrate, the height of the protrusion pattern, and the peak pitch of the protrusion pattern to be different. DETAILED DESCRIPTION
[0188] Fig.11 is a cross-sectional view schematically illustrating a light emitting element according to an embodiment of the present invention.
[0189] In the following embodiments, in order to avoid repeated description, the differences from the above-mentioned embodiments are mainly described, and the parts not described refer to the above-mentioned embodiments or matters obvious to those skilled in the art.
[0190] Reference Fig.11 According to one embodiment of the present invention, a light-emitting element includes a substrate 10 and a light-emitting stack disposed on the substrate 10. The light-emitting stack includes a first semiconductor layer 20, an active layer 30, and a second semiconductor layer 40 disposed sequentially on the substrate 10. In one embodiment of the present invention, the substrate 10 is a patterned substrate, and a plurality of protruding patterns 11 are disposed on its upper surface. The first semiconductor layer 20 may be disposed on the substrate 10. The first semiconductor layer 20 may cover the protruding pattern 11 on the substrate 10. To this end, the first semiconductor layer 20 may be epitaxially grown from the upper surface of the substrate 10, and in this case, may grow in an upward direction to completely cover the side and upper surface of the protruding pattern 11. The first semiconductor layer 20 has a plurality of cavities at positions corresponding to the side portions of the protruding pattern 11. This will be described later.
[0191] Fig.12 Observed from a plane Fig.11 A plan view of a substrate provided with a protruding pattern among the components of a light-emitting element, Fig.13 yes Fig.12 A cross-sectional view taken along line I-I', Fig.14 It is an enlarged image Fig.13 A cross-sectional view of P1.
[0192] Reference Figure 12 to Figure 14A protruding pattern 11 including a first layer 13 and a second layer 15 is disposed on the upper surface of the substrate 10 , and a plurality of voids VD are disposed adjacent to the protruding pattern 11 .
[0193] In one embodiment of the present invention, the peak distance PT of the protruding pattern 11 may have a value within a predetermined range according to DM. For example, the ratio of the diameter DM of the protruding pattern 11 to the peak distance PT is in the range of about 0.3 to about 2.0. However, the ratio of the diameter DM of the protruding pattern 11 to the peak distance PT is not limited thereto and may also be set to other values.
[0194] In one embodiment of the present invention, a plurality of voids VD are formed on the side of the protruding pattern 11, that is, between the protruding pattern 11 and the first semiconductor layer. In particular, voids VD are formed near the edge of the interface between the first layer 13 and the second layer 15 in the protruding pattern 11. The voids have a shape extending toward the lower side of the extension surface, that is, toward the downward direction of the substrate 10, based on the extension surface of the interface between the first layer 13 and the second layer 15. Accordingly, voids VD are formed on at least one side along the outer side of the uppermost portion of the first layer 13.
[0195] Here, the void VD is formed corresponding to the growth direction of the crystal plane, and is formed on the side corresponding to each vertex of the hexagon with the center of the protruding pattern 11 as a reference. Each void VD may have a triangular shape when viewed from a plane. To further illustrate this, when the protruding pattern 11 is set to a conical shape, the upper surface of the first layer 13 has a circular shape. In this case, the void VD is set at a position corresponding to the vertex of the regular hexagon of the circle inscribed in the upper surface of the first layer 13 when viewed from a plane. In addition, the void VD may have a right triangle shape when cut along a plane perpendicular to the upper surface of the substrate 10 and passing through the center of the circle. At this time, in the right triangle shape, the hypotenuse may be equivalent to the side of the first layer 13. Furthermore, in each void VD, the uppermost surface constituting the void VD may be a surface substantially the same as the surface extending the upper surface of the first layer 13. That is, each void VD is formed in the first semiconductor layer 20 corresponding to the outer side of the upper surface of the first layer 13 , and the upper surface of the first layer 13 serves as the upper side surface in the structure constituting each void VD.
[0196] According to an embodiment of the present invention, the first semiconductor layer 20 undergoes a process of merging into one crystal while growing from the upper surface of the substrate 10 in an upward direction and / or a side direction. In such a merging process, a portion that is not closely attached to the side surface of the first layer 13 of the protruding pattern 11 is intentionally controlled to form, thereby forming a void VD.
[0197] The void VD is an empty space where the first layer 13 and the first semiconductor layer 20 are not provided. Accordingly, the void VD has a refractive index different from that of the first layer 13 and the first semiconductor layer 20. Refraction, scattering, reflection, etc. of light will occur at the interface between the first layer 13 and each void and at the interface between the first semiconductor layer 20 and the void VD, thereby increasing the light extraction efficiency with the help of the chamber. However, generally speaking, the increase in refraction, scattering, reflection, etc. of light can improve the light extraction efficiency, but when the position where the void VD is generated is too close to or too far away from the upper surface of the substrate 10, the light extraction efficiency may be reduced instead.
[0198] In one embodiment of the present invention, the heights of the first layer 13 and the second layer 15 in the protruding pattern 11 are maintained within a predetermined range so that the light extraction efficiency can be improved by the void VD. As described above, since the position of the void VD is set at a position corresponding to the interface between the first layer 13 and the second layer 15, the position of the void can be adjusted by adjusting the position of the first layer 13 and the second layer 15 to a specific range. Here, the height H1 of the first layer 13 can be formed to have a value greater than a predetermined value. If, in the case where the height H1 of the first layer 13 is 0, the first semiconductor layer 20 may be hindered from growing from the substrate 10 due to impurities remaining on the upper surface of the first layer 13 during the process. In addition, in the case where the height H2 of the second layer 15 has a larger value than the height H1 of the first layer 13, since the growth of crystals in the side direction of the first layer 13 will be reduced, the quality of crystals can be improved, and therefore the height of the second layer 15 can have a larger value than the height of the first layer 13.
[0199] In other words, in order to make the void VD fully improve the light extraction efficiency, the height of the first layer 13 and the second layer 15 and the position of the void VD based thereon may be within a predetermined range. For example, the ratio of the height of the second layer 15 to the first layer 13 may be approximately greater than 2.5 and approximately less than 9.5. In one embodiment of the present invention, the ratio of the height of the second layer 15 to the first layer 13 may be approximately 4.25. Specifically, for example, when the sum of the heights of the first layer 13 and the second layer 15 is approximately 2.1 μm, the first layer 13 may have a height of approximately greater than 0.2 μm and approximately less than 0.6 μm. In another embodiment of the present invention, when the sum of the heights of the first layer 13 and the second layer 15 is approximately 2.1 μm, the first layer 13 may have a height of approximately 0.25 μm or more and approximately 0.55 μm or less. In yet another embodiment, the first layer 13 may have a height of approximately 0.3 μm or more and approximately 0.5 μm or less.
[0200] If the height of the first layer 13 is less than the above range from the surface of the substrate 10, the void VD cannot be sufficiently formed, and even if it is formed, the light scattering effect caused by the void VD may not be fully manifested. In addition, the size of the void VD is small or cannot be sufficiently formed, and it acts as a defect, thereby reducing the transmittance of light passing through the void VD. In this case, the incident ratio of light from the first semiconductor layer 20 to the inner direction of the substrate 10 may eventually be reduced.
[0201] When the height of the first layer 13 is within the above range from the surface of the substrate 10, the void VD is sufficiently formed, which not only improves the scattering effect caused by the void VD, but also increases the ratio of light incident from the first semiconductor layer 20 toward the substrate 10 through the void VD. In particular, in addition to the light directly incident from the first semiconductor layer 20 to the substrate 10, there is additional light that is refracted by the void VD and then transmitted to the surface of the substrate 10, thereby improving the overall light emission efficiency.
[0202] When the height of the first layer 13 is formed higher than the above range from the surface of the substrate 10, the path of the light traveling in the substrate 10 increases for the light traveling from the first semiconductor layer 20 toward the substrate 10, so that the absorption rate of the light in the substrate 10 becomes higher, and the amount of light transmitted through the substrate 10 may be reduced. In addition, in this case, since the height of the first layer 13 becomes relatively high, the growth of crystals toward the side of the first layer 13 may occur, and the quality of the crystals may be reduced, which may cause a reduction in light efficiency.
[0203] The light emitting element having the above structure improves light extraction efficiency by means of the protruding patterns and the cavities.
[0204] Table 11 shows the simulation results of the light extraction efficiency of the light-emitting element having a structure without a cavity and the light-emitting element having a cavity. In each light-emitting element, the remaining structure and size are identical except for the presence or absence of the cavity, and are set as a pair. Here, the light-emitting element is configured as a flip chip type. The light extraction efficiency is measured by measuring the brightness of light transmitted through the substrate, and the direction of light travel is set to pass from the active layer through the first semiconductor layer.
[0205] Here, the extraction efficiency of the light emitting element was measured by changing the structure of the protrusion pattern, that is, changing the height of the first layer and the second layer. Figures 15a to 15d In the figure, a structure with a protruding pattern of a hole is provided. Figures 16a to 16d Medium picture. Figures 15a to 15d and Figures 16a to 16d The specifications of the figures are not completely consistent with the actual simulation conditions, and some figures are enlarged or reduced for the convenience of explanation. Fig.17is a graph showing the simulation results of Table 11. For ease of explanation, Figure 15a to Figure 15b The structures are shown as Comparative Examples 1 to 4, Figure 16a to Figure 16b The structures are shown as Examples 1 to 4.
[0206]
Table 11
[0207]
[0208]
[0209] Referring to Table 11, in the case of Comparative Example 1 and Example 1, the height of the first layer is 0.2 μm, which is equivalent to the case where the upper surface of the first layer is arranged very close to the substrate surface. Referring to Comparative Example 1 and Example 1, compared with the existing light-emitting element without a cavity, the amount of light passing through the substrate in the light-emitting element with a cavity is reduced, and in particular, the overall light efficiency is reduced by 3.6%. This is believed to be because the cavity is not fully formed due to the lower height of the first layer, and even if it is formed, the light scattering effect caused by the cavity is not fully manifested. Similarly, in Comparative Example 3 and Example 3 and Comparative Example 4 and Example 4, compared with the existing light-emitting element without a cavity, the cavity in the light-emitting element reduces the amount of light passing through the cavity, and in particular, the overall light efficiency is reduced by 4.8% and 4.2%. This is believed to be because when the height of the first layer exceeds the above range from the substrate surface and is formed higher, the path of the light traveling in the substrate increases for the light traveling from the first semiconductor layer toward the substrate through the cavity, thereby increasing the absorption rate of the light in the substrate.
[0210] In contrast, in the case of Comparative Example 2 and Example 2, the amount of light transmitted through the substrate in the light-emitting element provided with the cavity increased by 4.4% compared to the existing light-emitting element without the cavity. This is believed to be because the cavity is sufficiently formed due to the sufficient height of the first layer, so that the side effects that may occur when the first layer is too high do not occur, such as the increase in light absorption efficiency caused by the decrease in crystallinity or the increase in the light path traveling in the substrate. Accordingly, when the cavity is formed as in Example 2, in addition to the light directly incident from the first semiconductor layer to the substrate, there is also additional light that is refracted through the cavity and transmitted to the substrate surface, thereby improving the overall light emission efficiency.
[0211] Through these, it can be confirmed that when a cavity is provided at the side of the protruding pattern and the height of the first layer and the second layer is within the above range, the light efficiency is significantly increased. In particular, when a cavity is provided at the side of the protruding pattern, the sum of the heights of the first layer and the second layer is 2.1 μm, and the height of the first layer is between 0.2 μm and 0.6 μm, the light efficiency is significantly increased.
[0212] The light emitting element having the structure according to the above-described embodiment can be manufactured by adjusting the process conditions in such a manner that a plurality of cavities are formed on the side of the protruding pattern when forming the first semiconductor layer.
[0213] Figure 18a to Figure 18b It is a cross-sectional view showing a part of the step of manufacturing the protruding pattern having the above structure, and is a view sequentially showing a substrate on which the protruding pattern is formed in order to form a cavity and the growth direction of the first semiconductor layer. Fig.18a and Fig.18b For ease of explanation, arrows are used to indicate the main growth direction of the semiconductor layer.
[0214] Reference Figures 11 to 14 , Fig.18a and Fig.18b First, the first semiconductor layer 20 is formed upward.
[0215] The first semiconductor layer 20 can be formed using semiconductor layers of various materials, for example, can be formed using an n-type nitride series semiconductor layer, and can be formed using metalorganic vapor phase epitaxy (Metalorganic vapor phase epitaxy) or molecular beam epitaxy (MBE) or hydride vapor phase epitaxy (HVPE).
[0216] The initial growth of the first semiconductor layer 20 is 3D growth (e.g., island growth) that occurs mainly from the exposed surface of the substrate 10 in an upward direction, and no growth occurs on the upper surface of the second layer 15. The 3D growth condition is relatively low in growth temperature and high in growth pressure compared to 2D growth (e.g., Frank van der Merwe growth) that mainly grows in a horizontal direction.
[0217] After a portion of the growth in the upward direction is carried out, the first semiconductor layer 20 grows in the upward and side directions. In the figure, for the convenience of explanation, it is divided into a first growth pattern 21 that mainly grows in the upward direction and a second growth pattern 23 that grows in the upward and side directions while growing more dominantly in the side directions. At this time, the second growth pattern 23 is a 2D growth that mainly grows in the horizontal direction, which can be achieved by maintaining a higher growth temperature and a lower growth pressure than the above-mentioned 3D growth.
[0218] In one embodiment of the present invention, epitaxial lateral growth (ELOG) may be used by metal organic chemical vapor deposition (MOCVD) to grow the first semiconductor layer 20 in a lateral direction (horizontal direction in the figure).
[0219] The first semiconductor layer 20 continues to grow in the side direction and the upper direction, and is merged to cover the entire surface of the substrate 10 including the surface of the second layer 15. The first semiconductor layer 20 undergoes a process of merging into one crystal in the process of growing from the substrate surface to the upper direction and / or the side direction. In such a merging process, a portion that is not closely attached to the side of the first layer 13 of the protruding pattern 11 is controlled to form, thereby forming a void VD. Here, in particular, during 3D growth and 2D growth, by adjusting the thickness ratio of the first semiconductor layer 20 formed according to each growth, the size and position of the void VD formed in the first semiconductor layer 20 can be intentionally controlled.
[0220] In one embodiment of the present invention, the upper surface of the substrate 10 exposed between the protruding patterns 11 is a portion that becomes a substantial growth nucleus, and growth occurs in an upward direction from the upper surface of the substrate 10 as in the first growth pattern 21. Thereafter, the first semiconductor layer 20 grows in a horizontal direction by a lateral epitaxial overgrowth method as in the second growth pattern 23. When the first semiconductor layer 20 grows, if the surface in the upper direction is referred to as the upper surface, and the surface in the side direction is referred to as the side surface, then in the case where the first semiconductor layer 20 is epitaxially grown by lateral epitaxial overgrowth, due to the conditions of lateral epitaxial overgrowth, the growth of the side surface is more dominant than the growth of the upper surface, and the growth ratio of the m-axis to the c-axis becomes about 2:1. Although the side surface of the first semiconductor layer 20 may be perpendicular to the upper surface of the first semiconductor layer 20 during growth, it is not limited thereto, and may be a surface inclined to the upper surface of the first semiconductor layer 20. In one embodiment of the present invention, the upper surface of the first semiconductor layer 20 corresponds to the (0001) surface, and the side surface of the first semiconductor layer 20 corresponds to the (10-11) surface.
[0221] After the first semiconductor layer 20 is formed as a whole by side growth, the first semiconductor layer 20 can be selectively grown further upward by using a hydride vapor phase growth method. When the first semiconductor layer 20 is formed by a metal organic chemical vapor deposition method, the film formation speed is slower than that of the hydride vapor phase growth method, so the hydride vapor phase growth method can be used when the first semiconductor layer 20 is grown to a sufficient thickness faster.
[0222] The first semiconductor layer 20 formed in this way covers the surface of the substrate 10 and the protruding pattern 11 in a state where cavities are formed.
[0223] In one embodiment of the present invention, a buffer layer may be further formed on the substrate 10 before forming the first semiconductor layer 20. In one embodiment of the present invention, in the first semiconductor layer 20, two layers with different band gaps are alternately stacked, thereby forming a superlattice structure. An active layer 30 is formed on the first semiconductor layer 20. In one embodiment of the present invention, as the active layer 30, a quantum well layer and a barrier layer may be alternately stacked to form a quantum well structure. An electron blocking layer is formed on the active layer 30, and then a second semiconductor layer 40 is formed on the active layer 30, thereby manufacturing a light-emitting stack.
[0224] Fig.19 The protruding pattern and the first semiconductor layer according to one embodiment of the present invention are photographed by the above-mentioned method. Fig.19 As shown, in the case of a light emitting element of one embodiment of the present invention, a plurality of protruding patterns can be formed on the substrate, each of which has six cavities. Each cavity is arranged at a position corresponding to the vertex of a hexagon, which is related to the crystal growth direction of the semiconductor layer.
[0225] Fig.20a and Fig.20b The photographs are taken of the light path and light intensity of the light emitting element having no cavity and the light emitting element having the cavity. Fig.20a and Fig.20b In the figure, if the direction in which the vertex of the protruding pattern is facing is called the upper side, then the direction of light travel is from the upper side to the lower side.
[0226] Reference Fig.20a and Fig.20b , light from the upper side to the lower side is incident on the lower side of the substrate through the inclined surface of the protruding pattern and the substrate surface. Fig.20b In the case where a cavity is provided on the side of the protruding pattern, it can be clearly seen that the light refracted and scattered by the cavity is incident toward the lower part of the substrate, and the degree is greater than that of the case where no cavity is provided. Fig.20a Significantly larger.
[0227] In this way, a cavity is formed in the first semiconductor layer in the region corresponding to the side of the protruding pattern, so that the amount of light traveling downward can be significantly increased, resulting in a light-emitting element with high light efficiency.
[0228] The light emitting element according to an embodiment of the present invention can be used in various types of semiconductor chips, for example, Figure 6 and Figure 7 The present invention may be employed in a semiconductor chip of the type shown in FIG. 1 , or may be employed in a semiconductor chip of the type described later.
[0229] Fig.21The figure is a cross-sectional view of a semiconductor chip according to an embodiment of the present invention, and is a diagram showing a flip-chip type semiconductor chip. After being formed on a substrate, a flip-chip type semiconductor can be flipped and mounted on other components, and the figure shows a flipped state.
[0230] Reference Fig.21 The light emitting element includes a substrate 10 , a light emitting stack disposed on an upper surface 10R of the substrate 10 , and a first electrode 110 and a second electrode 120 connected to the light emitting stack.
[0231] In one embodiment of the present invention, the substrate 10 is a patterned substrate, and a plurality of protruding patterns and cavities are disposed on the upper surface of the substrate.
[0232] The light-emitting stack includes a first semiconductor layer 20, an active layer 30, and a second semiconductor layer 40 sequentially stacked on the upper surface 10R of the substrate 10. In the present embodiment, the light-emitting stack may also be configured to have at least one table form including the active layer 30 and the second semiconductor layer 40. When the light-emitting stack is configured to have a table form, the light-emitting stack may include a plurality of protruding patterns, and the plurality of protruding patterns may be spaced apart from each other.
[0233] An insulating film 130a is provided on the light emitting stack. The light emitting stack is provided with at least one contact hole CH that penetrates the active layer 30, the second semiconductor layer 40 and the insulating film 130a and exposes a portion of the first semiconductor layer 20. The first electrode 110 is connected to the exposed first semiconductor layer 20 through the contact hole CH. The second electrode 120 is connected to the exposed second semiconductor layer 40 through an opening formed in the insulating film 130a. An additional insulating film 130b may be further provided on the side of the light emitting stack. The additional insulating film 130b may be formed by a variety of mirrors (for example, a metal mirror or a dielectric mirror) so that the light emitted from the active layer 30 cannot be emitted toward the side of the light emitting stack.
[0234] The light emitting element according to an embodiment of the present invention has the first electrode 110 and the second electrode 120 arranged on the same side and has a small size, so it can be easily mounted on the wiring of the substrate 10 .
[0235] The light emitting device according to an embodiment of the present invention emits light by applying a signal to the first electrode 110 and the second electrode 120 to turn them on. The emitted light travels downward through the first semiconductor layer 20 and the substrate 10, and the light extraction efficiency in the downward direction is improved by the protruding pattern 11 and the cavity provided on the substrate 10.
[0236] In one embodiment of the present invention, for the sake of convenience, only the case where the protruding pattern is in a conical shape is illustrated, but within the limits of the concept of the present invention, the protruding pattern can be deformed into various forms. For example, the shape of the protruding pattern can have a polygonal cone shape. Alternatively, even if it is set to a conical shape, the shape of the curved surface constituting the side surface can be partially deformed. In addition, the cross-section of the protruding pattern can be close to a semi-ellipsoidal sphere.
[0237] Fig. 22 is a schematic cross-sectional view illustrating a light emitting element according to an embodiment of the present invention.
[0238] Reference Fig. 22 According to an embodiment of the present invention, a light-emitting element includes a substrate 10 and a light-emitting stacked body disposed on the substrate 10 .
[0239] In one embodiment of the present invention, the substrate 10 is a patterned substrate, and a plurality of protruding patterns 11 are disposed on its upper surface. In other words, the protruding patterns 11 are disposed in a shape protruding upward from the upper surface of the substrate 10. In one embodiment of the present invention, the protruding patterns 11 may be disposed in a shape whose width gradually decreases upward, and when the protruding patterns 11 are cut along a vertical surface on the substrate 10, the cross-section of the protruding patterns 11 may be approximately a semi-ellipsoid, and may also be close to a triangular shape depending on the situation.
[0240] The protruding pattern 11 includes a first layer 13 and a second layer 15 which are sequentially stacked from the upper surface of the substrate 10. The first layer 13 is disposed on the substrate 10, and the second layer 15 is disposed on the first layer 13.
[0241] The first semiconductor layer 20 may be disposed on the substrate 10. The first semiconductor layer 20 may cover the protruding pattern 11 on the substrate 10. To this end, the first semiconductor layer 20 may be epitaxially grown from the upper surface of the substrate 10, and in this case, may grow in an upward direction to completely cover the side and upper surface of the protruding pattern 11.
[0242] In one embodiment of the present invention, the refractive index of the first semiconductor layer may be greater than the refractive indexes of the first layer 13 and the second layer 15. For example, when the refractive index of the first layer 13 is 1.6 to 2.45 and the refractive index of the second layer 15 is 1.3 to 2.0, the refractive index of the first semiconductor layer 20 may be 2.0 to 2.5.
[0243] Fig.23 Observed from a plane Fig. 22 A plan view of a substrate having a protruding pattern among components of a light-emitting element. Fig.24 is along Fig.23 Cross-sectional view taken along line I-I'. Fig.25a It is an enlarged image Fig.24 A cross-sectional view of P1, Fig.25bIt is an enlarged image Fig.25a A cross-sectional view of P4.
[0244] Reference Fig.23 , Fig.24 , Fig.25a and Fig.25b A protruding pattern 11 including a first layer 13 and a second layer 15 is disposed on an upper surface of a substrate 10 .
[0245] The first layer 13 is integrally formed with the substrate 10. Therefore, the first layer 13 is composed of the same material as the substrate 10. The upper surface of the first layer 13 may have a circular shape.
[0246] The second layer 15 is made of a material different from that of the first layer 13. The material of the second layer 15 may be a material having a different refractive index from that of the first layer 13. In one embodiment of the present invention, the refractive index of the first layer 13 may be greater than the refractive index of the second layer 15. In this case, the material of the first layer 13 and the material of the second layer 15 may use a variety of insulating materials having different refractive indices.
[0247] For example, within the limit that the first layer 13 and the second layer 15 use materials with different refractive indices, a material having a refractive index of about 1.6 to about 2.45 can be used as the material of the first layer 13, and a material having a refractive index of about 1.3 to about 2.0 can be used as the material of the second layer 15. As materials having such refractive indices, sapphire can be cited for the first layer 13, and SiO2 can be cited for the second layer 15. x 、SiO x N y 、SiN x In one embodiment of the present invention, the first layer 13 may be made of sapphire, and the second layer 15 may be made of SiO2. In this case, the refractive index of the first layer 13 is equivalent to 1.76, and the refractive index of the second layer 15 is equivalent to about 1.46.
[0248] Each protrusion pattern 11 may have a circular shape when viewed from a plane. In the case where the protrusion pattern 11 is provided in an ellipsoidal sphere or a cone shape, the vertex portion of the ellipsoidal sphere or the cone becomes the center.
[0249] The protruding pattern 11 may be set to have a predetermined diameter DM and height HT. The diameter DM means the width of the lowest end of the protruding pattern 11 when viewed in cross section, and the height HT means the distance from the upper surface of the substrate 10 to the top of the protruding pattern 11. In this embodiment, each protruding pattern 11 may have the same diameter DM and height HT. However, each protruding pattern 11 may not have exactly the same diameter DM and height HT, and the diameter DM and height HT may also differ within a predetermined range.
[0250] In one embodiment of the present invention, the height H1 of the first layer 13 is formed to have a value greater than a predetermined value. If the height H1 of the first layer 13 is 0, the growth of the first semiconductor layer 20 from the substrate 10 may be hindered due to impurities remaining on the upper surface of the substrate 10 during the process. In addition, when the height H2 of the second layer 15 is formed to be greater than the height H1 of the first layer 13, the growth of crystals toward the side direction of the first layer 13 will be reduced, thereby improving the quality of the crystals. Therefore, the height of the second layer 15 can have a value greater than the height of the first layer 13.
[0251] In one embodiment of the present invention, when the height of the first layer 13 is formed to be higher than the above range from the surface of the substrate 10, for the light traveling from the first semiconductor layer 20 toward the substrate 10, the path of the light traveling in the substrate 10 increases, so that the absorption rate of the light in the substrate 10 becomes higher, thereby possibly reducing the amount of light transmitted through the substrate 10. In addition, in this case, since the height of the first layer 13 becomes relatively high, the growth of crystals toward the side direction of the first layer 13 occurs, which may reduce the quality of the crystals, which may cause a reduction in light efficiency.
[0252] In one embodiment of the present invention, the side inclinations of the first layer 13 and the second layer 15 may be at least partially the same or different from each other. Although the figure illustrates a situation where the inclinations of the first layer 13 and the second layer 15 have the same value, it is not limited to this. The side inclinations of the first layer 13 and the second layer 15 may be at least partially the same or different from each other. In particular, the inclinations of the portions where the first layer 13 and the second layer 15 are connected may be different from each other. Since the materials of the first layer 13 and the second layer 15 are different from each other, when the etching process is performed, the side inclinations can be set to be different according to the process conditions. In one embodiment of the present invention, by forming the inclinations of the first layer 13 and the second layer 15 to be different, the reflectivity of the light emitted from the light-emitting element can be increased, thereby improving the light emission efficiency.
[0253] In one embodiment of the present invention, the arrangement of the protruding patterns 11 may be a regular arrangement as shown in the figure, but is not limited thereto. For example, the protruding patterns 11 may be arranged irregularly. In this case, from the perspective of the entire substrate 10, the peak pitch PT and the spacing of the protruding patterns 11 in each single area are within a predetermined range, and in this case, the density may be substantially set to the same level.
[0254] In one embodiment of the present invention, for the sake of convenience, the protruding pattern 11 is only shown as a conical shape. However, within the scope of the concept of the present invention, the protruding pattern 11 can be deformed into various forms. For example, the shape of the protruding pattern 11 can have a polygonal cone shape. Alternatively, even if it is set to a conical shape, the shape of the curved surface constituting the side surface can also be partially deformed.
[0255] In one embodiment of the present invention, the peak distance PT of the protruding pattern 11 may have a value within a predetermined range according to DM. For example, the ratio of the diameter DM of the protruding pattern 11 to the peak distance PT is in the range of about 0.3 to about 2.0. However, the ratio of the diameter DM of the protruding pattern 11 to the peak distance PT is not limited thereto and may also be set to other values.
[0256] In one embodiment of the present invention, the interface between the first layer 13 and the second layer 15 is formed substantially horizontally with the substrate surface, that is, with the upper surface of the substrate 10 , and the surface thereof has a rough surface.
[0257] This is described in further detail below.
[0258] When observed with the first layer 13 as a reference, the first layer 13 may generally have a conical shape with a flat upper surface and a cut upper portion. Accordingly, the first layer 13 is composed of an upper surface substantially parallel to the substrate surface and a side surface connecting the substrate surface and the upper surface. The upper surface of the first layer 13 has a rough surface (i.e., concavoconvex) so that as much light as possible incident from the first semiconductor layer 20 toward the substrate 10 direction (the lower direction in the figure) is incident into the substrate 10. In other words, the upper surface of the first layer has concavoconvex portions that protrude toward the upper direction of the substrate surface and concave portions that are recessed toward the lower direction of the substrate surface. In the case where the upper surface of the first layer 13, i.e., the interface between the second layer 15 and the first layer 13 is a flat surface without concavoconvex portions, the reflectivity of light is higher than when there are concavoconvex portions, thereby reducing the amount of light traveling toward the lower direction of the substrate 10. When the first layer 13 has unevenness on its upper surface, light is scattered or refracted rather than reflected at the unevenness portion, thereby making it easier for light to travel into the substrate 10. Light incident into the substrate 10 passes through the substrate 10 and then exits toward the back side of the substrate 10.
[0259] For the concave and convex between the first and second layers, Fig.25a and 25b Also, Figure 26a to Figure 26b 2 and 3 respectively show photographs of the upper surface of the first layer of a light emitting element according to the prior art and a light emitting element according to an embodiment of the present invention. Figure 26a to Figure 26b In the figures, each photograph is an atomic force microscope (AFM) photograph, and the test piece corresponding to the upper surface of the first layer was manufactured with a width of 2 μm and a height of 2 μm.
[0260] As shown in the figure, in the case of the existing invention, Fig.26aThe upper surface of the first layer is not provided with bumps, but is provided as a flat surface. In the roughness of the prior invention, the root mean square deviation of the roughness Rq can be 0.200nm to 0.300nm, and the arithmetic mean deviation of the roughness Ra can be 0.140nm to 0.190nm. For example, Rq can be 0.216nm, and Ra can be 0.169nm
[0261] In one embodiment of the present invention, Figure 26b The upper surface of the first layer is provided with a rough surface, i.e., concavoconvex. Here, the roughness can be set to various degrees. In the roughness according to an embodiment of the present invention, the root mean square deviation Rq of the roughness can be 0.300nm to 0.550nm, and the arithmetic mean deviation Ra of the roughness can be 0.250nm to 0.400nm. For example, the root mean square deviation Rq can be 0.477nm, and the arithmetic mean deviation Ra can be 0.327nm.
[0262] As described above, in a light-emitting element according to one embodiment of the present invention, a protruding pattern is provided on the substrate, and by means of the protruding pattern, when light is transmitted in a specific direction, the light extraction efficiency is significantly increased. In particular, the light generated in the active layer travels in the direction of penetrating the substrate through the first semiconductor layer, and when penetrating the substrate, light diffusion and light scattering occur by means of the protruding pattern, so that the light extraction effect in the back direction of the substrate will be significantly improved. The light diffusion and light scattering by means of the protruding pattern are mainly increased by the rough surface of the interface provided between the first layer and the second layer, so the amount of light traveling in the downward direction will increase. Moreover, in the case of the present invention, the interface between the first layer and the second layer is provided as an irregular concave-convex, so that the reflection of light passing through the first layer and the second layer is minimized. In particular, in one embodiment of the present invention, the refractive indexes of the first layer, the second layer and the first semiconductor layer are formed to be different from each other, and the refractive indexes are successively reduced in the order of the first semiconductor layer, the first layer and the second layer, so that the refraction or reflection of light passing through the first semiconductor layer, the first layer and the second layer can maximize the emission of light in the downward direction.
[0263] In this embodiment, in the first layer, the side surfaces other than the upper surface are not substantially provided with rough surfaces. The side surfaces may be provided as reflective surfaces with substantially very little light penetrating the side surfaces. In this embodiment, the side surfaces may be reflective surfaces that reflect more than 80% of the light traveling from the first semiconductor layer toward the side surfaces of the first layer described later, for example, more than 90% of the light, preferably more than 95% of the light. In one embodiment of the present invention, the rough surface may not be provided in the area on the substrate surface where the protruding pattern is not provided.
[0264] Figure 27a to Figure 27b is a method for manufacturing a light emitting element according to an embodiment of the present invention. Fig.24Transmission electron microscope (TEM) photographs of parts P2 and P3.
[0265] Reference Fig.27a , the portion indicated in white is the second layer 15, and the portion arranged at the lower portion of the second layer 15 corresponds to the first layer 13. As shown in the figure, the upper surface of the first layer 13 may be irregularly formed with concavities and convexities.
[0266] Reference Figure 27b The side surfaces of the first layer 13 other than the upper surface are substantially not provided with rough surfaces, but are provided with substantially flat surfaces without projections and depressions.
[0267] Furthermore, the substrate surface, that is, the upper surface of the substrate 10 can be set to be a flat surface having substantially no irregularities.
[0268] However, in one embodiment of the present invention, the upper surface of the substrate 10 may be set to a flat surface without any concavo-convex shapes, but it is not limited thereto. The upper surface of the first layer 13 may be formed with concavo-convex shapes to increase the incidence rate of light in the downward direction. That is, a rough surface may be set on the surface of the substrate without a protruding pattern to increase the diffusion rate or scattering rate of light traveling in the downward direction through the portion without the protruding pattern. As a result, the light extraction effect in the light-emitting element can be improved.
[0269] Figure 28a to Figure 28b is a PhET simulation photograph showing the path of light caused by the shape of the side surface of the first layer. Figure 28a to Figure 28b In the figure, for a structure in which a first semiconductor layer is grown after forming a first layer on a substrate, the direction of light travel is shown, and all conditions except the shape of the side surface of the first layer are set to be the same. The side surface of the first layer is set to be Fig.28a In the case of unevenness, Fig.28b The middle is a case where a flat reflecting surface without any concavities or convexities is formed.
[0270] Reference Fig.28a When light travels from the first semiconductor layer toward the side of the first layer, the light is scattered and reflected in multiple directions by the concave and convex formed on the side of the first layer. The light extraction efficiency of the light-emitting element is determined by the amount of light traveling toward the back side of the substrate, that is, from the active layer through the first semiconductor layer and the substrate toward the back side of the substrate. Fig.28a As shown, in the case of radial reflection or scattering, there is a problem that the light efficiency in the downward direction is significantly reduced.
[0271] On the contrary, refer to Fig.28bWhen light travels from the first semiconductor layer toward the side of the first layer, the side of the first layer acts as a reflective surface. Since the reflective surface is flat, most of the light is reflected in a specific direction at the side of the first layer, and the reflected light is incident into the substrate. Therefore, it can be found that the light traveling in the downward direction is significantly increased.
[0272] As described above, the light extraction efficiency of the light emitting element having the protrusion pattern, in particular, the protrusion pattern having a rough surface on the upper surface of the first layer and a side surface configured as a reflective surface, is significantly improved compared to the prior art.
[0273] The protrusion pattern having the above-mentioned structure can be manufactured by the following method.
[0274] Figure 29a to Figure 29g 1 and 2 are cross-sectional views sequentially illustrating a method of manufacturing a protruding pattern in a light emitting element according to an embodiment of the present invention.
[0275] First, refer to Fig.29a First, prepare the substrate 10. As described above, the substrate 10 can be made of materials such as SiC, Si, GaAs, GaN, ZnO, GaP, InP, Ge, Ga2O3, etc., and the insulating layer can be made of SiO x 、SiO x N y 、SiN x And other materials.
[0276] Reference Fig.29b The upper surface of the substrate 10 is formed with a rough surface, that is, a concavoconvex surface PR. The concavoconvex surface PR can be formed by various methods such as wet etching, dry etching, grinding, or a combination of these methods, but is not limited thereto.
[0277] Reference Fig.29c The insulating layer 15i is stacked on the substrate 10 using a material for forming the second layer. The insulating layer 15i is a layer that can form the second layer, and can be formed on the substrate 10 using a material having a different refractive index from that of the substrate 10.
[0278] Reference Fig.29d Thereafter, a photoresist 50 is coated on the insulating layer 15 i , and a photolithography process including exposure and development is performed, thereby forming a pattern of the photoresist 50 .
[0279] Reference Fig.29e , the pattern of the photoresist 50 will be reflowed. By reflowing the photoresist 50, the thickness of the photoresist 50 can be different according to the region, and accordingly, the etching shapes of the insulating layer 15i and the substrate 10 thereunder will become different.
[0280] Reference Fig.29e and29f , the insulating layer 15i and the substrate 10 are etched using the photoresist 50 as a mask, thereby forming a protruding pattern 11 having a first layer 13 and a second layer 15. In further detail, the insulating layer and a portion of the substrate 10 are etched using the pattern of the photoresist 50 as a mask, and the insulating layer 151i other than the portion where the protruding pattern 11 is to be formed is etched, thereby forming the second layer 15. In the portion where the second layer 15 is not formed, the upper surface of the substrate 10 is exposed. Here, the upper surface of the substrate 10 is further etched than the original upper surface of the substrate 10 by the additional etching, thereby forming the first layer 13 protruding from the upper surface of the substrate 10. If etching is performed to form only the second layer 15 and the original upper surface of the substrate 10 is exposed, it may be judged in theory that the growth of the semiconductor layer is likely to occur later because the upper surface of the substrate 10 is exposed, but in reality, due to etching residues or impurities remaining on the upper surface of the substrate 10, the growth of the first semiconductor layer 20 does not occur normally later. Therefore, additional etching is performed on the substrate 10 to completely remove etching residues, impurities, etc. Thus, the first layer 13 is formed.
[0281] The etching for forming the first layer 13 and the second layer 15 may be performed using various methods under various conditions according to the material. For example, the insulating layer 15i and a portion of the substrate 10 may be patterned using dry etching.
[0282] The second layer 15 and the first layer 13 may be sequentially formed using the above method, and patterning may be performed using the same or different etching gases.
[0283] The insulating layer 15i and the substrate 10 may be etched anisotropically, which allows etching in the up-down direction but relatively cannot allow etching in the left-right direction.
[0284] Reference Figure 29g , a light-emitting laminate including a first semiconductor layer 20 is sequentially formed on a substrate having a protruding pattern 11, thereby forming a light-emitting element. First, the first semiconductor layer 20 is formed on the substrate 10 having the protruding pattern 11. The first semiconductor layer 20 first grows upward from the exposed surface of the substrate 10, and then grows upward and sideways. After the first semiconductor layer 20 is grown, an active layer 30 (see Fig. 22 ) and the second semiconductor layer 40 (refer to Fig. 22 ).
[0285] To explain this in more detail, first, the first semiconductor layer 20 is formed upward. The first semiconductor layer 20 can be formed using semiconductor layers of various materials, for example, using an n-type nitride semiconductor layer, and can be formed using a metal organic vapor phase epitaxy method (Metalorganic vapour phase epitaxy) or a molecular beam epitaxy method (MBE: molecular beam epitaxy) or a hydride vapor phase epitaxy method (HVPE: Hydride vapour phase epitaxy) and the like.
[0286] The initial growth of the first semiconductor layer 20 is a 3D growth (e.g., island growth) that occurs mainly from the exposed surface of the substrate 10 toward the upper direction, and no growth occurs on the upper surface of the second layer 15. After a portion of the growth toward the upper direction is performed, the first semiconductor layer 20 grows toward the upper and side directions. In one embodiment of the present invention, in order to grow toward the side direction (horizontal direction in the figure) of the first semiconductor layer 20, lateral epitaxial growth (ELOG) can be used by metal organic chemical vapor deposition (MOCVD).
[0287] The first semiconductor layer 20 also continues to grow in the lateral and upward directions, thereby merging to cover the entire surface of the substrate 10 including the surface of the second layer 15. The first semiconductor layer 20 grows from the substrate surface to the upward and / or lateral directions and then merges into a crystallization process.
[0288] After the first semiconductor layer 20 is formed as a whole by side growth, the first semiconductor layer 20 can be selectively grown further upward by using a hydride vapor phase growth method. When the first semiconductor layer 20 is formed by using a metal organic chemical vapor deposition method, the film formation speed is slower than that of the hydride vapor phase growth method, so the hydride vapor phase growth method can be used when the first semiconductor layer 20 is grown to a sufficient thickness faster.
[0289] The first semiconductor layer 20 formed in this way covers the surface of the substrate 10 and the protruding pattern 11 in a state where cavities are formed.
[0290] In one embodiment of the present invention, a buffer layer may be further formed on the substrate 10 before forming the first semiconductor layer 20. In one embodiment of the present invention, in the first semiconductor layer 20, two layers with different band gaps are alternately stacked, thereby forming a superlattice structure. An active layer 30 is formed on the first semiconductor layer 20. In one embodiment of the present invention, as the active layer 30, a quantum well layer and a barrier layer may be alternately stacked to form a quantum well structure. An electron blocking layer is formed on the active layer 30, and then a second semiconductor layer 40 is formed on the active layer 30, thereby manufacturing a light-emitting stack.
[0291] By forming the projections and depressions on the upper surface of the first layer in this manner, the amount of light traveling downward can be significantly increased, and as a result, a light-emitting element with high light efficiency can be manufactured.
[0292] The light emitting element of the above structure can be realized as semiconductor chips in various forms.
[0293] Fig.30 FIG. 1 is a cross-sectional view showing a semiconductor chip according to an embodiment of the present invention, and shows a lateral semiconductor chip.
[0294] Reference Fig.30 The semiconductor chip includes a light emitting element, a first electrode 110 and a second electrode 120 connected to the light emitting element. The light emitting element includes a substrate 10 and a first semiconductor layer 20, an active layer 30, and a second semiconductor layer 40 disposed on the substrate 10.
[0295] In this embodiment, the first electrode 110 is disposed on the first semiconductor layer 20 where the active layer 30 and the second semiconductor layer 40 are not disposed, and the second electrode 120 is arranged on the second semiconductor layer 40 .
[0296] The first electrode 110 and / or the second electrode 120 may be formed of a single layer or multiple layers of metal. The material of the first electrode 110 and / or the second electrode 120 may include various metals such as Al, Ti, Cr, Ni, Au, Ag, Cr, Cu, Ti, Ru, Rh, Ir, Mg, Zn, Al, In, Ta, Pd, Co, and alloys thereof.
[0297] Here, a plurality of protrusion patterns 11 and cavities are provided on the upper surface of the substrate 10 for improving light emission efficiency. As described above, the protrusion pattern on the substrate 10 may be provided in a conical shape including the first layer 13 and the second layer 15, and a cavity is provided near the interface between the first layer and the second layer.
[0298] An insulating film 130 is disposed on the first electrode 110 and the second electrode 120, and a contact hole is disposed on the insulating film 130 to expose the first electrode 110 and the second electrode 120. The insulating film 130 can be arranged on the upper surface of the second semiconductor layer 40 and the side of the semiconductor layer, and can selectively contact the first electrode 110 and the second electrode 120. The insulating film 130 may include an insulating material or an insulating resin formed by at least one of an oxide, nitride, fluoride and sulfide having at least one of Al, Cr, Si, Ti, Zn and Zr. For example, the insulating film 130 can be selectively formed in SiO2Si3N4Al2O3TiO2. The insulating film 130 can be formed as a single layer or a multilayer, which is not limited.
[0299] In one embodiment of the present invention, the first electrode 110 and the second electrode 120 may be connected to other components by exposing the contact hole. For example, the first electrode 110 and the second electrode 120 may be provided with a first pad and a second pad connected by the contact hole. Figure 1 Although the above-mentioned layers are described above, the light emitting element may include components having additional functions, such as a reflection layer for reflecting light, an additional insulating layer for insulating a specific component, a solder prevention layer for preventing solder from diffusing, and other layers.
[0300] Furthermore, when forming a lateral light-emitting element, the mesa may be formed in various forms. Of course, the positions or shapes of the first electrode 110 and the second electrode 120 may also be changed in various ways.
[0301] The light emitting device according to an embodiment of the present invention emits light by applying a signal to the first electrode 110 and the second electrode 120 to turn them on. The emitted light can travel downward through the first semiconductor layer 20 and the substrate 10, and the light extraction efficiency in the downward direction is improved by the protruding pattern 11 and the cavity provided on the substrate 10.
[0302] Although the semiconductor chip using the light emitting element according to one embodiment of the present invention is illustrated as a lateral semiconductor chip, it is not limited thereto. For example, the light emitting element according to one embodiment of the present invention can be applied to a vertical or flip chip type semiconductor chip.
[0303] Fig.31 1 is a cross-sectional view of a semiconductor chip according to an embodiment of the present invention, and is a view of a flip-chip type semiconductor chip. After a flip-chip type semiconductor is formed on a substrate 10, it can be flipped and mounted on other components, and the figure shows a flipped state.
[0304] Reference Fig.31 The light emitting element includes a substrate 10, a light emitting stack disposed on an upper surface 10R of the substrate 10, and a first electrode 110 and a second electrode 120 connected to the light emitting stack.
[0305] In one embodiment of the present invention, the substrate 10 is a patterned substrate, and a plurality of protruding patterns and cavities are disposed on the upper surface of the substrate.
[0306] The light-emitting stack includes a first semiconductor layer 20, an active layer 30, and a second semiconductor layer 40 sequentially stacked on the upper surface 10R of the substrate 10. In the present embodiment, the light-emitting stack may also be configured to have at least one table form including the active layer 30 and the second semiconductor layer 40. When the light-emitting stack is configured to have a table form, the light-emitting stack may include a plurality of protruding patterns, and the plurality of protruding patterns may be spaced apart from each other.
[0307] An insulating film 130a is provided on the light emitting stack. The light emitting stack is provided with at least one contact hole CH that penetrates the active layer 30, the second semiconductor layer 40 and the insulating film 130a and exposes a portion of the first semiconductor layer 20. The first electrode 110 is connected to the exposed first semiconductor layer 20 through the contact hole CH. The second electrode 120 is connected to the exposed second semiconductor layer 40 through an opening formed in the insulating film 130a. An additional insulating film 130b may be further provided on the side of the light emitting stack. The additional insulating film 130b may be formed by a variety of mirrors (for example, a metal mirror or a dielectric mirror) so that the light emitted from the active layer 30 cannot be emitted toward the side of the light emitting stack.
[0308] The light emitting element according to an embodiment of the present invention has the first electrode 110 and the second electrode 120 arranged on the same side and has a small size, so it can be easily mounted on the wiring of the substrate 10 .
[0309] The light emitting device according to an embodiment of the present invention emits light by applying a signal to the first electrode 110 and the second electrode 120 to turn them on. The emitted light travels downward through the first semiconductor layer 20 and the substrate 10, and the light extraction efficiency in the downward direction is improved by the protruding pattern 11 and the cavity provided on the substrate 10.
[0310] The light-emitting element having the above structure has high light extraction efficiency. An experiment was conducted below to compare the light-emitting efficiency of the light-emitting element according to the prior art and one embodiment of the present invention.
[0311] In the following experiment, first, light extraction efficiency was examined by using a light-emitting element having a total height of 1.7 μm and 2.1 μm, respectively, using a substrate having a protruding pattern consisting of only the first layer as the first and second comparative examples, and using a light-emitting element having a substrate having a protruding pattern consisting of the first layer and the second layer as the third comparative example. In this experiment, the substrate and the first layer were formed of sapphire, and the second layer was formed of SiO2. All the structures except the protruding pattern were the same in Comparative Examples 1 to 3. In Comparative Example 3, the height of the first layer was 0.4 μm and the height of the second layer was 1.7 μm.
[0312] Table 12 is a table showing the luminous efficiency of the first to third comparative examples.
[0313]
Table 12
[0314]
[0315]
[0316] Referring to Table 12, Comparative Examples 1 and 2 in which the protruding pattern is formed only by the first layer are examined. Comparative Example 2 with a higher protruding pattern height has a luminous efficiency improved by 2.2% compared to Comparative Example 1. When the height of the protruding pattern is fixed at 2.1 μm, the luminous efficiency of Comparative Example 3 formed by the first layer and the second layer is significantly higher than that of Comparative Example 2 formed only by the first layer. Compared with Comparative Example 1, the luminous efficiency of Comparative Example 2 is improved by 2.2%, while the luminous efficiency of Comparative Example 3 is improved by as much as 5.7%.
[0317] From this, it was confirmed that when the protruding pattern was formed by the first layer and the second layer, the light emission efficiency was significantly improved compared to the case where this was not the case.
[0318] Hereinafter, a light emitting element having a protrusion pattern with a rough surface formed at the interface between the first layer and the second layer was used as an example, and the light emitting efficiency was measured together with Comparative Examples 1 and 3. Fig.32 It is a graph showing the intensity of emitted light according to the change in wavelength of the light emitting elements of Comparative Example 1, Comparative Example 3 and the working example. Fig.32 In the embodiment, the light emitting element was manufactured under the same conditions as those of Comparative Example 3 except for the protrusion pattern. The protrusion pattern of the embodiment differs from that of the Comparative Example in that projections and depressions are formed at the interface between the first layer and the second layer.
[0319] Reference Fig.32 It can be confirmed that the luminous efficiency of Comparative Example 3 is higher than that of Comparative Example 1, which is substantially the same as the result in Table 12 above. Fig.32 Compared with Comparative Example 3, in most wavelength ranges, especially in the range of about 450nm to about 460nm, the luminous efficiency of the embodiment is significantly higher. Comparative Example 3 and the embodiment are formed in the same manner except for the presence or absence of the concavo-convex on the upper surface of the first layer, so it is explained that the difference in luminous efficiency is caused by the concavo-convex on the upper surface of the first layer.
[0320] Although the above description is made with reference to the preferred embodiments of the present invention, it should be understood that any person skilled in the art or a person with basic knowledge in the technical field can make various modifications and changes to the present invention without departing from the scope of the idea and technical field of the present invention as recorded in the claims.
[0321] Therefore, the technical scope of the present invention is not limited to the contents described in the detailed description, but should be determined only by the scope described in the claims.
Claims
1. A light emitting element, comprising: substrate; a plurality of protruding patterns, including a first layer and a second layer, wherein the first layer is integrally formed with the substrate and protrudes from the upper surface of the substrate, and the second layer is disposed on the first layer and is formed of a material different from that of the first layer; and a light-emitting laminated body, which is disposed on the substrate and emits light, The light-emitting laminate has a cavity disposed on at least one side of the protruding pattern. The ratio of the diameter of the protruding pattern to the peak spacing is 0.8 to 1.0, The diameter means the width of the lowest end of the protruding pattern when viewed in cross section, and the peak distance means the distance between the centers of two protruding patterns adjacent to each other when viewed in plane. The ratio of the height of the second layer to the height of the first layer is greater than 2.5 and less than 9.5, The refractive index of the first layer is greater than the refractive index of the second layer, The cavity is formed to extend in a direction toward the substrate while being spaced apart from an upper surface of the substrate.
2. The light emitting element according to claim 1, wherein The light-emitting laminate comprises: A first semiconductor layer is disposed on the substrate; an active layer disposed on the first semiconductor layer; and A second semiconductor layer is disposed on the active layer, Wherein, the cavity is arranged in the first semiconductor layer.
3. The light emitting element according to claim 2, wherein: The uppermost portion of the cavity and the uppermost portion of the first layer have the same height from the surface of the substrate.
4. The light emitting element according to claim 3, wherein When the upper surface of the first layer has a circular shape when viewed from a plane, the holes are provided corresponding to vertices of a regular hexagon inscribed in the circle.
5. The light emitting element according to claim 4, wherein When cut along a plane perpendicular to the upper surface of the substrate and passing through the center of the circle, the shape of the cavity has a right triangle shape, and the hypotenuse of the right triangle is a side surface of the first layer.
6. The light emitting element according to claim 1, wherein The height of the first layer is 0.25 μm or more and 0.55 μm or less, and the sum of the heights of the first layer and the second layer is 2.1 μm.
7. The light emitting element according to claim 1, wherein The light emitting element is of a lateral type or a flip chip type.
8. The light emitting element according to claim 7, wherein The light emitted from the light emitting stack travels in a direction penetrating the substrate.
9. The light emitting element according to claim 1, wherein The side inclination of the first layer and the side inclination of the second layer are different from each other.
10. The light emitting element according to claim 1, wherein The first layer includes any one of SiC, Si, GaAs, GaN, ZnO, GaP, InP, Ge, and Ga2O3, and the second layer includes SiO x 、SiO x N y 、SiN x Any one of .
11. The light emitting element according to claim 1, wherein The protrusion patterns are regularly arranged.
12. The light emitting element according to claim 1, wherein The protrusion patterns are irregularly arranged.
13. A method for manufacturing a light emitting element, as a method for manufacturing the light emitting element according to any one of claims 1 to 12, comprising the following steps: forming, on a substrate, a plurality of protruding patterns including a first layer protruding from an upper surface of the substrate and a second layer disposed on the first layer and made of a material different from that of the first layer; and forming a first semiconductor layer, an active layer and a second semiconductor layer in sequence on the substrate, in, The step of forming the first semiconductor layer comprises the following steps: growing a first semiconductor layer material 3D on the substrate; and A first semiconductor layer material 2D is grown on the substrate.
Citation Information
Patent Citations
Light emitting device, light emitting device package, and lighting system
CN102148302A
Light-emitting element
CN210489638U
Light emitting device and lighting system having the same
KR1020150132974A
Semiconductor light emitting device
US20160372643A1
Light emitting element
WO2011058890A1