Method for preparing embedded ceramic substrate
By creating through holes in the ceramic substrate and performing vacuum sintering, the problems of chip fixation and heat dissipation were solved, resulting in thinner packages and better heat dissipation performance.
Patent Information
- Application Number
- CN202110768483.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-07
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-07-07
Smart Images

Figure CN113571424B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, in particular to a ceramic substrate. Background Art
[0002] Ceramic substrates have the characteristics of high thermal conductivity, good heat resistance, low thermal expansion coefficient, high mechanical strength, good insulation, corrosion resistance, and radiation resistance. They are widely used in electronic device packaging. According to different preparation principles and processes, the current mainstream products can be divided into thick film printing ceramic substrates (Thick Printing Ceramic Substrate, TPC), direct bonded copper ceramic substrates (Direct Bonded Copper Ceramic Substrate, DBC), active metal brazing ceramic substrates (Active Metal Brazing Ceramic Substrate, AMB), etc. Miniaturized high-voltage and high-power modules are one of the important development directions of semiconductor devices. In the design of semiconductor devices, as the size decreases, the chip power density increases sharply, which puts forward new requirements for the reliability of module heat dissipation packaging.
[0003] The existing preparation method of ceramic substrate is often to simply compound the metal layer with the ceramic sheet, and fix the ceramic sheet on the metal layer. This structure greatly limits the thickness of the subsequent package and is not easy to ensure the relative fixation effect of the chip. Moreover, the heat dissipation area of the chip is only transmitted outward from the front metal layer, which has a poor heat dissipation effect on the chip. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a method for preparing an embedded ceramic substrate to solve at least one of the above technical problems.
[0005] In order to achieve the above object, the present invention provides a method for preparing an embedded ceramic substrate, which is characterized by comprising the following steps:
[0006] Step 1: pre-treating the front metal layer and the back metal layer;
[0007] The front metal layer includes at least two layers of metal sheets, the at least two layers of metal sheets include a first metal sheet close to the ceramic sheet, and the remaining metal sheets of the at least two layers of metal sheets except the first metal sheet are provided with at least one through hole penetrating from top to bottom;
[0008] Step 2: stack the front metal layer, the ceramic sheet and the back metal layer in sequence from top to bottom and perform vacuum sintering.
[0009] The through hole is used for embedding a chip.
[0010] This patent opens a through hole on the front metal layer to facilitate the limiting and fixing effect of the chip. Correspondingly, the thickness of the later package is thinned. In addition, the heat of the chip can be dissipated from the metal layer in the circumferential direction to the outside and the downward area, greatly improving the heat dissipation range.
[0011] Further preferably, a blind hole is opened on the first metal sheet by a precision engraving machine.
[0012] Further preferably, the depth of the blind hole is 2 / 3 of the depth of the first metal sheet.
[0013] Further preferably, the cross-section of the through hole is one or more of square, rectangular, circular, pentagonal and hexagonal.
[0014] Further preferably, the front metal layer includes a first metal sheet, a second metal sheet and a third metal sheet arranged in sequence from bottom to top;
[0015] The thickness of the first metal sheet is 0.2 mm-0.4 mm, the thickness of the second metal sheet is 0.2 mm-0.3 mm, the thickness of the third metal sheet is 0.2 mm-0.3 mm, and the thickness of the back metal layer is 0.5 mm-1.0 mm.
[0016] Further preferably, the front metal layer is a copper layer or an aluminum layer.
[0017] Further preferably, the back metal layer is a copper layer or an aluminum layer.
[0018] Further preferably, in step one, all metal sheets of the front metal layer are stacked from top to bottom and then connected by diffusion welding, and in step two, the front metal layer, the ceramic sheet and the back metal layer are connected by vacuum brazing.
[0019] Solder is coated between the ceramic sheet and the front metal layer and the back metal layer.
[0020] Alternatively, in step 2, all metal sheets, ceramic sheets and back metal layers of the front metal layer are stacked in sequence from top to bottom and then vacuum brazed;
[0021] Brazing material is coated between the ceramic sheet, the first metal sheet and the back metal layer.
[0022] Further preferably, the front metal layer includes a first metal sheet, a second metal sheet and a third metal sheet arranged in sequence from bottom to top;
[0023] The through holes are formed on the second metal sheet and the third metal sheet, and the through holes on the second metal sheet and the third metal sheet are connected to each other;
[0024] The area of the through hole of the second metal sheet is smaller than the area of the through hole of the third metal sheet.
[0025] It is convenient to realize chip limiting.
[0026] A method for preparing an embedded ceramic substrate, characterized in that it comprises the following steps:
[0027] Step 1: pre-treating the front metal layer and the back metal layer;
[0028] The front metal layer includes at least two layers of metal sheets, the at least two layers of metal sheets include a first metal sheet close to the ceramic sheet, and the remaining metal sheets of the at least two layers of metal sheets except the first metal sheet are provided with at least one through hole penetrating from top to bottom;
[0029] Step 2, the first metal sheet, the ceramic sheet and the back metal layer are stacked in sequence from top to bottom and then vacuum brazed and sintered;
[0030] Step 3, etching the first metal sheet to form a pattern, so that the first metal sheet is provided with an inwardly concave portion, and the first metal sheet is also provided with a zigzag groove running through from top to bottom, the zigzag groove is located at the periphery of the zigzag portion, and the zigzag groove is used to arrange the zigzag portion in an island shape on the first metal sheet;
[0031] Step 4, stacking the remaining metal sheets of the front metal layer on the metal substrate manufactured in step 3 in sequence, and then vacuum diffusion welding them;
[0032] The through hole is vertically connected to the inner concave portion.
[0033] By optimizing the preparation method, in order to prevent the structure of the inner recess from detaching or shifting from the first metal sheet, this patent adopts a two-step sintering method. The pattern preparation method of the first metal sheet is first sintering and then preparing. In the first sintering, the first metal sheet, the ceramic sheet and the back metal layer are vacuum brazed together, and then the metal layer on the first metal sheet is etched into a pattern, and the metal substrate is vacuum diffusion welded together with the second metal sheet and the third metal sheet.
[0034] In step 2, the temperature of vacuum brazing sintering is controlled at 700°C-940°C, the vacuum degree is less than 0.01 Pa, and the sintering time is 60min-540min.
[0035] In step 4, the process parameters of vacuum diffusion welding are as follows: diffusion welding sintering temperature is 500°C-900°C, vacuum degree is less than 0.1 Pa, and sintering time is 10min-540min.
[0036] Further preferably, the depth of the inner recess is 2 / 3 of the depth of the first metal sheet.
[0037] Further preferably, the cross-section of the through hole is one or more of square, rectangular, circular, pentagonal and hexagonal.
[0038] Further preferably, the thickness of the first metal sheet is 0.2 mm-0.4 mm, the thickness of the second metal sheet is 0.2 mm-0.3 mm, the thickness of the third metal sheet is 0.2 mm-0.3 mm, and the thickness of the back metal layer is 0.5 mm-1.0 mm.
[0039] Further preferably, the front metal layer is a copper layer or an aluminum layer.
[0040] Further preferably, the back metal layer is a copper layer or an aluminum layer.
[0041] The beneficial effects are: 1) the thickness of the packaging module can be reduced, thereby reducing the packaging density of the chip; 2) the embedded copper-clad substrate can provide better heat dissipation for the chip and provide a chip positioning groove to prevent the chip from shifting during welding. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a flow chart of a specific embodiment 1 of the present invention;
[0043] Figure 2 It is a schematic diagram of the three-dimensional structure of structure 1 of specific embodiment 1 of the present invention;
[0044] Figure 3 It is an exploded view of the front metal layer of structure 1 of specific embodiment 1 of the present invention;
[0045] Figure 4 It is a schematic diagram of the three-dimensional structure of Structure 2 of specific embodiment 1 of the present invention;
[0046] Figure 5 This is a schematic structural diagram of a first metal sheet of Structure 2 of Specific Embodiment 1 of the present invention;
[0047] Figure 6 Schematic diagram of the three-dimensional structure of the product of specific embodiment 2 of the present invention;
[0048] Figure 7 This is a schematic structural diagram of the first metal sheet of the product of specific embodiment 2 of the present invention.
[0049] Among them: 1 is the front metal layer, 11 is the first metal sheet, 111 is the chip positioning groove, 112 is the loop groove, 113 is the inner concave part, 12 is the second metal sheet, 121 is the second metal sheet through-area, 13 is the third metal sheet, 131 is the third metal sheet through-area, 2 is the ceramic sheet, and 3 is the back metal layer. DETAILED DESCRIPTION
[0050] The present invention will be further described below in conjunction with the accompanying drawings.
[0051] See also Figure 1 , Specific embodiment 1, a method for preparing an embedded ceramic substrate, comprising the following steps:
[0052] Step 1: pre-treating the front metal layer and the back metal layer;
[0053] The front metal layer includes at least two layers of metal sheets, the at least two layers of metal sheets include a first metal sheet close to the ceramic sheet, and the remaining metal sheets of the at least two layers of metal sheets except the first metal sheet are provided with at least one through hole penetrating from top to bottom;
[0054] Step 2: stack the front metal layer, the ceramic sheet and the back metal layer in sequence from top to bottom and perform vacuum sintering.
[0055] Through holes are used to embed chips.
[0056] This patent opens a through hole on the front metal layer to facilitate the limiting and fixing effect of the chip. Correspondingly, the thickness of the later package is thinned. In addition, the heat of the chip can be dissipated from the metal layer in the circumferential direction to the outside and the downward area, greatly improving the heat dissipation range.
[0057] Pretreatment includes cleaning and drying pretreatment.
[0058] The first metal sheet is provided with a blind hole through a precision engraving machine. The depth of the blind hole is 2 / 3 of the depth of the first metal sheet. The cross section of the through hole is one or more of square, rectangular, circular, pentagonal, and hexagonal.
[0059] The thickness of the first metal sheet is 0.2 mm-0.4 mm, the thickness of the second metal sheet is 0.2 mm-0.3 mm, the thickness of the third metal sheet is 0.2 mm-0.3 mm, and the thickness of the back metal layer is 0.5 mm-1.0 mm.
[0060] The front metal layer is a copper layer or an aluminum layer.
[0061] The back metal layer is a copper layer or an aluminum layer.
[0062] The front metal layer includes a first metal sheet, a second metal sheet and a third metal sheet arranged in sequence from bottom to top; the second metal sheet and the third metal sheet are both provided with through holes, and the through holes on the second metal sheet and the third metal sheet are mutually connected; the area of the through hole of the second metal sheet is smaller than the area of the through hole of the third metal sheet, so as to facilitate the positioning of the chip.
[0063] There are several vacuum sintering methods for the front metal layer, the back metal layer and the ceramic tile:
[0064] Method 1: Step 2, stacking the front metal layer, the ceramic sheet and the back metal layer from top to bottom in sequence and then vacuum brazing them;
[0065] Brazing material is coated between the ceramic sheet, the first metal sheet and the back metal layer.
[0066] The temperature of vacuum brazing is controlled at 700℃-940℃, the vacuum degree is less than 0.01Pa, and the sintering time is 60min-540min.
[0067] Method 2: In step 1, all metal sheets of the front metal layer are stacked from top to bottom and then connected by diffusion welding;
[0068] In step 1, the process parameters of diffusion welding are as follows: diffusion welding sintering temperature is 500°C-900°C, vacuum degree is less than 0.1 Pa, and sintering time is 10min-540min.
[0069] In step 2, the front metal layer, the ceramic sheet and the back metal layer are connected by vacuum brazing;
[0070] Brazing material is coated between the ceramic sheet, the first metal sheet and the back metal layer.
[0071] The temperature of vacuum sintering is controlled at 700°C-940°C, the vacuum degree is less than 0.01Pa, and the sintering time is 60min-540min.
[0072] The products can be the following two:
[0073] See also Figure 2 as well as Figure 3 , Structure 1: The first metal sheet does not have a blind hole:
[0074] The metal layer is provided with three metal sheets, namely, the first metal sheet 11, the second metal sheet 12 and the third metal sheet 13, which are arranged in sequence from bottom to top; the second metal sheet 12 and the third metal sheet 13 are each provided with at least one through hole, and the through hole on the second metal sheet 12 (that is, the second metal sheet through area 121) and the through hole on the third metal sheet 13 (that is, the third metal sheet through area 131) are mutually conductive; the area of the through hole of the second metal sheet 12 (that is, the second metal sheet through area 121) is smaller than the area of the through hole of the third metal sheet 13 (that is, the third metal sheet through area 131). Preferably, the area of the second metal sheet through area 121 is proportionally reduced relative to the third metal sheet through area 131. This is convenient for realizing the limit of the chip.
[0075] See also Figure 4 as well as Figure 5 , Structure 2: A blind hole (chip positioning groove 111) is opened in the first metal sheet:
[0076] The metal layer is provided with three metal sheets, namely, a first metal sheet 11, a second metal sheet 12 and a third metal sheet 13 arranged in sequence from bottom to top. A chip positioning groove 111 is provided on the first metal sheet 11, and the chip positioning groove 111 is a non-through blind groove. The depth of the chip positioning groove 111 is 2 / 3 of the depth of the first metal sheet 11.
[0077] The through holes on the second metal sheet and the third metal sheet are formed by laser engraving.
[0078] Specific embodiment 2, a method for preparing an embedded ceramic substrate, comprising the following steps:
[0079] Step 1: pre-treating the front metal layer and the back metal layer;
[0080] The front metal layer includes at least two metal sheets, and the at least two metal sheets include a first metal sheet close to the ceramic sheet.
[0081] Step 2, the first metal sheet, the ceramic sheet and the back metal layer are stacked in sequence from top to bottom and then vacuum brazed and sintered;
[0082] Step 3, etching the first metal sheet to form a pattern, so that the first metal sheet is provided with an inwardly concave portion, and the first metal sheet is also provided with a meandering groove, the meandering groove is located at the periphery of the inwardly concave portion, and the depth of the meandering groove is greater than the depth of the inwardly concave portion and less than the thickness of the first metal sheet;
[0083] Step 4: stack the remaining metal sheets of the front metal layer in sequence on the metal substrate manufactured in step 3, and then perform vacuum diffusion welding; the through hole and the inner concave portion are connected vertically.
[0084] By optimizing the preparation method, in order to prevent the structure of the inner recess from detaching or shifting from the first metal sheet, this patent adopts a two-step sintering method. The pattern preparation method of the first metal sheet is first sintering and then preparing. In the first sintering, the first metal sheet, the ceramic sheet and the back metal layer are vacuum brazed together, and then the metal layer on the first metal sheet is etched into a pattern, and the metal substrate is vacuum diffusion welded together with the second metal sheet and the third metal sheet.
[0085] In step 2, the temperature of vacuum brazing sintering is controlled at 700°C-940°C, the vacuum degree is less than 0.01 Pa, and the sintering time is 60min-540min.
[0086] In step 4, the process parameters of vacuum diffusion welding are as follows: diffusion welding sintering temperature is 500°C-900°C, vacuum degree is less than 0.1 Pa, and sintering time is 10min-540min.
[0087] The depth of the inner recess is 2 / 3 of the depth of the first metal sheet.
[0088] The cross section of the through hole is one or more of square, rectangular, circular, pentagonal, and hexagonal. The thickness of the first metal sheet is 0.2mm-0.4mm, the thickness of the second metal sheet is 0.2mm-0.3mm, the thickness of the third metal sheet is 0.2mm-0.3mm, and the thickness of the back metal layer is 0.5mm-1.0mm. The front metal layer is a copper layer or an aluminum layer. The back metal layer is a copper layer or an aluminum layer.
[0089] For the structure of the specific product, see Figure 6 to Figure 7 The front metal layer includes a first metal sheet 11, a second metal sheet 12 and a third metal sheet 13 arranged in sequence from bottom to top.
[0090] The first metal sheet 11 is provided with an inwardly concave portion 113 (i.e., an island-shaped graphic area), and the first metal sheet 11 is also provided with a zigzag groove 112 running through from top to bottom. The zigzag groove 112 is located at the periphery of the concave portion, and the zigzag groove is used to set the concave portion in an island shape on the first metal sheet.
[0091] The through holes on the second metal sheet and the third metal sheet are formed by laser engraving.
[0092] The beneficial effects are: 1) the thickness of the packaging module can be reduced, thereby reducing the packaging density of the chip; 2) the embedded copper-clad substrate can provide better heat dissipation for the chip and provide a chip positioning groove to prevent the chip from shifting during welding.
[0093] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an embedded ceramic substrate, characterized in that: The steps include: Step 1: pre-treating the front metal layer and the back metal layer; The front metal layer includes at least two layers of metal sheets, the at least two layers of metal sheets include a first metal sheet close to the ceramic sheet, and the remaining metal sheets of the at least two layers of metal sheets except the first metal sheet are provided with at least one through hole penetrating from top to bottom; Step 2: vacuum sintering the front metal layer, the ceramic sheet and the back metal layer; In step 2, all metal sheets, ceramic sheets and back metal layers of the front metal layer are stacked in sequence from top to bottom and then vacuum brazed; Brazing material is coated between the ceramic sheet, the first metal sheet and the back metal layer.
2. The method for preparing an embedded ceramic substrate according to claim 1, characterized in that: The first metal sheet is provided with a blind hole by means of a precision engraving machine.
3. The method for preparing an embedded ceramic substrate according to claim 1, characterized in that: The cross section of the through hole is one or more of square, rectangular, circular, pentagonal and hexagonal.
4. The method for preparing an embedded ceramic substrate according to claim 1, characterized in that: The front metal layer includes a first metal sheet, a second metal sheet and a third metal sheet arranged in sequence from bottom to top; The thickness of the first metal sheet is 0.2 mm-0.4 mm, the thickness of the second metal sheet is 0.2 mm-0.3 mm, the thickness of the third metal sheet is 0.2 mm-0.3 mm, and the thickness of the back metal layer is 0.5 mm-1.0 mm; The front metal layer is a copper layer or an aluminum layer; The back metal layer is a copper layer or an aluminum layer.
5. The method for preparing an embedded ceramic substrate according to claim 1, characterized in that: The front metal layer includes a first metal sheet, a second metal sheet and a third metal sheet arranged in sequence from bottom to top; The second metal sheet and the third metal sheet are both provided with the through holes, and the through holes on the second metal sheet and the third metal sheet are connected to each other; The area of the through hole of the second metal sheet is smaller than the area of the through hole of the third metal sheet.
6. A method for preparing an embedded ceramic substrate, characterized in that: The steps include: Step 1: pre-treating the front metal layer and the back metal layer; The front metal layer includes at least two layers of metal sheets, the at least two layers of metal sheets include a first metal sheet close to the ceramic sheet, and the remaining metal sheets of the at least two layers of metal sheets except the first metal sheet are provided with at least one through hole penetrating from top to bottom; Step 2, the first metal sheet, the ceramic sheet and the back metal layer are stacked in sequence from top to bottom and then vacuum brazed and sintered; Step 3, etching the first metal sheet to form a pattern, so that the first metal sheet is provided with an inwardly concave portion, and the first metal sheet is also provided with a zigzag groove running through from top to bottom, the zigzag groove is located at the periphery of the zigzag portion, and the zigzag groove is used to arrange the zigzag portion in an island shape on the first metal sheet; Step 4, stacking the remaining metal sheets of the front metal layer on the metal substrate manufactured in step 3 in sequence, and then vacuum diffusion welding them; The through holes of the metal sheets except the first metal sheet in the at least two layers of metal sheets are vertically connected to the inner concave portion.
7. The method for preparing an embedded ceramic substrate according to claim 6, characterized in that: In step 2, the temperature of vacuum brazing sintering is controlled at 700°C-940°C, the vacuum degree is less than 0.01 Pa, and the sintering time is 60min-540min.
8. The method for preparing an embedded ceramic substrate according to claim 6, characterized in that: In step 4, the process parameters of vacuum diffusion welding are as follows: diffusion welding sintering temperature is 500°C-900°C, vacuum degree is less than 0.1 Pa, and sintering time is 10min-540min.
Citation Information
Patent Citations
Manufacturing method of metallized ceramic substrate and manufactured metallized ceramic substrate
CN106169426A
LED ceramic package
JP2005210056A
Package for electronic component housing, and electronic device
JP2006013420A
Heat dissipation structure
JP2010219215A
Ceramic package, metal frame used in ceramic package, and electronic component device using package, and method of manufacturing the same
JP2016171093A