A low bulk ratio ultrafine iron powder reduction furnace tube and use method thereof
By adopting technologies such as bending design and guide plates in the furnace tube of the low bulk ratio ultrafine iron powder reduction furnace, the problems of high hydrogen loss and insufficient reduction atmosphere are solved, achieving more efficient hydrogen utilization and safer production. process.
Patent Information
- Application Number
- CN202111032962.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-09-03
AI Technical Summary
The existing high-temperature muffle type reduction furnace has high hydrogen loss during the reduction process of low bulk ratio ultrafine iron powder, and it is difficult to achieve efficient reduction atmosphere and full contact with the materials, which affects product quality.
A low bulk ratio ultra-fine iron powder reduction furnace tube is designed. It adopts a bent inlet and outlet, combined with a guide plate and a nitrogen sealing curtain, and utilizes the low density characteristics of hydrogen to achieve sealing and increase the presence of hydrogen. The curved flow and diffusion within the muffle tube increase the hydrogen pressure and the permeability of the reducing atmosphere.
It improves the hydrogen pressure and reduction quality in the furnace, reduces hydrogen loss and production costs, avoids the formation of dust and mixed explosive gases, and ensures a more efficient and safer reduction process.
Smart Images

Figure CN113579242B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder metallurgy equipment, and in particular relates to a furnace tube of a low-bulk ratio ultrafine iron powder reduction furnace and a use method thereof. Background Art
[0002] With the rapid development of powder metallurgy technology, high-temperature muffle reduction furnaces have been widely used. Its basic working principle is: the material is pre-loaded into the material boat (or stainless steel belt) and enters the muffle tube. The material gradually completes the reduction reaction under sufficient reducing atmosphere and process temperature, and then is cooled by the cooling device and discharged from the furnace. The core component of the high-temperature muffle reduction furnace is the muffle tube, which is generally pressed from SU S310S stainless steel plates imported from Japan or Sweden. The process temperature is divided into 3 to 5 temperature zones for independent regulation according to specifications and material requirements. The steel belt reduction furnace tubes currently used in the market mainly play the role of particle hardening, purification, and protective atmosphere. The proportion of hydrogen as a reducing atmosphere is relatively low (generally, all-iron TFe97 is reduced to TFe99). However, the reduction process of low-loose ratio ultrafine iron powder requires a greatly increased amount of hydrogen to reduce the total iron content TFe68 (primary reduction process TFe68, secondary reduction process TFe85) to pure iron powder with a total iron content of TFe99. In order to adapt to the reduction process of low bulk ratio ultrafine iron powder, improve product quality and reduce hydrogen loss, it is necessary to find a reduction equipment that is more suitable for this type of iron powder. Summary of the invention
[0003] In order to solve the above technical problems, the object of the present invention is to provide a low bulk ratio ultrafine iron powder reduction furnace tube and a use method thereof.
[0004] The technical solution adopted by the present invention to solve its technical problem is: a low-bulk ratio ultrafine iron powder reduction furnace tube, comprising a feed end, a muffle section, an air-cooling section, a water-cooling section, and a discharge end, the feed end is connected to one end of the muffle section through a flange, the other end of the muffle section is connected to one end of the water-cooling section through an air-cooling section, and the other end of the water-cooling section is connected to the discharge end through a flange.
[0005] The feed end includes a feed port, a steel belt pressure roller, a steel belt steering roller 1, a feed bin, a waste hydrogen release port, and a distributor. The bottom of the feed bin is connected to the distributor through a bearing seat. Steel belt pressure rollers are respectively arranged on both sides of the distributor. Both ends of the steel belt pressure rollers are connected to the feed port through bearing seats. A stainless steel belt is arranged below the steel belt pressure roller. The steel belt pressure roller is used to ensure the flatness of the stainless steel belt and ensure uniform distribution. A steel belt steering roller 1 is arranged below the stainless steel belt. The steel belt steering roller 1 is fixed to the feed port through a bearing seat. The stainless steel belt changes direction through the action of the steel belt steering roller 1. Waste hydrogen is not easy to overflow from here due to its low density. The waste hydrogen release port is welded to the end of the feed port close to the furnace body, and the end of the feed port away from the furnace body is tilted downward.
[0006] The muffle section comprises a muffle tube, a guide plate, and a hydrogen inlet. The top of the muffle tube is arc-shaped, a plurality of guide plates are welded on the inner wall of the top, and a hydrogen inlet is arranged at the end of the muffle tube.
[0007] The discharging end comprises a discharging port, a nitrogen inlet, a nitrogen sealing curtain, and two steel belt steering rollers. The nitrogen inlet and the nitrogen sealing curtain are both welded to the upper part of the discharging port. The nitrogen inlet and the nitrogen sealing curtain are arranged at intervals. Two steel belt steering rollers are arranged at the corner where the discharging port is connected to the water cooling section. Both ends of the two steel belt steering rollers are connected and fixed to the discharging port through bearing seats.
[0008] Furthermore, the muffle tube is divided into temperature zones, and a guide plate is welded in each temperature zone. First, the risk of collapse of the arc-shaped top of the muffle tube due to long-term heating is reduced; second, the hydrogen is prevented from moving in a straight line along the arc-shaped top of the muffle tube, the hydrogen running speed is slowed down and the movement trajectory is changed, so that the hydrogen runs along the curve under the obstruction of the guide plate and further diffuses horizontally to the muffle tube (the edge of the muffle tube), so as to achieve the purpose of full contact between the reducing atmosphere and the material.
[0009] Furthermore, the nitrogen sealing curtains are provided with two groups, the nitrogen inlet is composed of six rows of steel pipes, every two rows of steel pipes are arranged at intervals with one group of nitrogen sealing curtains, and each row of steel pipes is covered with pinholes with a diameter of about 1 mm.
[0010] Furthermore, a hydrogen control valve is provided at the hydrogen inlet, and a nitrogen control valve is provided at the nitrogen inlet, and the hydrogen flows in a direction opposite to the rotation direction of the steel belt.
[0011] Furthermore, the feeder adopts variable frequency feeding control, which is more suitable for the feeding control of low bulk ratio iron oxide powder (low bulk ratio, poor fluidity, difficult automatic feeding, and easy clogging of the feeding port).
[0012] Furthermore, the feed port and the discharge port are both bent, and the end of the feed port away from the furnace body is tilted downward by 30°-40°. The stainless steel belt changes its horizontal movement direction to a downward tilt through the steel belt steering roller 1, so that the counterflowing hydrogen is not easy to flow out with the steel belt due to its low density; the thickness of the cloth is controlled by the frequency converter to control the speed of the distributor, and the discharge port is placed in the furnace body while keeping the material not empty to further prevent the outflow of hydrogen; thus, the hydrogen pressure in the furnace body is increased. The corner of the discharge port is tilted downward by about 45°, and the stainless steel belt at the discharge end is changed from the horizontal movement direction to a downward tilt through the steel belt steering roller 2, so that the counterflowing hydrogen is not easy to flow out with the steel belt due to its low density; at the same time, the nitrogen flow at the nitrogen inlet is timely controlled by the manual nitrogen control valve against the flowmeter to further prevent the outflow of hydrogen and ensure the safety of the furnace body.
[0013] Furthermore, the waste hydrogen discharge port adopts a steel pipe design, which greatly increases the reducing atmosphere pressure in the furnace, is beneficial to the penetration of the reducing atmosphere, and improves the reduction effect.
[0014] The method for using the low bulk ratio ultrafine iron powder reduction furnace tube comprises the following steps:
[0015] 1) First, open the stainless steel belt, introduce nitrogen into the nitrogen inlet, open the hydrogen control valve and slowly introduce hydrogen, and ignite the torch at the waste hydrogen release port until the waste hydrogen is ignited;
[0016] 2) Turn on the fabric feeder and measure the fabric thickness until it reaches the required thickness;
[0017] 3) Adjust the hydrogen control valve according to the flame changes of the waste hydrogen to ensure that the flame of the waste hydrogen discharge port is ignited normally;
[0018] 4) Adjust the nitrogen control valve at the nitrogen inlet to ensure good sealing and prevent the material from being blown away;
[0019] 5) When shutdown is required, first stop the distributor, then close the hydrogen control valve to stop the hydrogen supply; finally stop the nitrogen and stop the operation of the steel belt.
[0020] The present invention has the following beneficial effects:
[0021] 1. The feed port and the discharge port of the present invention are both bent. The stainless steel belt in the furnace tube section from the hydrogen inlet to the waste hydrogen diffusion port is trapezoidal and higher than other sections. The hydrogen atmosphere moves horizontally and parallel to the stainless steel belt. The density of hydrogen is extremely small and always floats in the upper area of the furnace tube, which further plays a sealing role. The sealed feeding at the feed end is adopted, and the isolation from the outside air is achieved by turning the stainless steel belt and utilizing the low density characteristics of hydrogen; the uninterrupted feeding of the material further isolates the contact between hydrogen and the outside air, and the hydrogen pressure in the furnace is increased to improve the reduction quality.
[0022] 2. The present invention adopts a sealed discharge end, which is isolated from the outside air by turning the stainless steel belt and utilizing the low density of hydrogen; at the same time, the nitrogen seal plays a certain barrier role, further isolating the contact between hydrogen and the outside air, and the hydrogen pressure in the furnace is increased, thereby improving the reduction quality.
[0023] 3. The muffle tube of the present invention adopts a guide plate design. The guide plate is placed at the top of the arc of the muffle tube to guide and disperse the hydrogen, change the flow mode of the hydrogen in the muffle tube, make the hydrogen fully contact with the material and increase the contact area, thereby improving the reduction quality.
[0024] 4. The present invention realizes fully enclosed operation in both feeding and discharging, thus avoiding the formation of various types of dust and being more environmentally friendly.
[0025] 5. The present invention further prevents the contact between hydrogen and the outside air through the sealing design of the feeding and discharging ends, avoiding the formation of mixed explosive gas, which is safer and more reliable.
[0026] 6. As the reduction efficiency per unit time is further improved, the stainless steel strip, power consumption, hydrogen loss, etc. are further reduced, and the production cost is significantly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a structural schematic diagram of the feeding end of the reduction furnace tube of the present invention.
[0028] Figure 2 It is a structural schematic diagram of the muffle section of the reduction furnace tube of the present invention.
[0029] Figure 3 It is a structural schematic diagram of the discharge end of the reduction furnace tube of the present invention.
[0030] In the figure, 1, feed inlet, 2, steel belt pressure roller, 3, steel belt steering roller 1, 4, unloading bin, 5, waste hydrogen release port, 6, distributor, 7, muffle tube, 8, guide plate, 9, hydrogen, 10, nitrogen inlet, 11, discharge port, 12, nitrogen sealing curtain, 13, steel belt steering roller 2, 14, stainless steel belt, 15, hydrogen inlet. DETAILED DESCRIPTION
[0031] The following are specific embodiments of the present invention, which further describe the technical solution of the present invention, but the protection scope of the present invention is not limited to these embodiments. Any changes or equivalent substitutions that do not deviate from the concept of the present invention are included in the protection scope of the present invention.
[0032] A furnace tube for a low-bulk ratio ultrafine iron powder reduction furnace comprises a feed end, a muffle section, an air cooling section, a water cooling section and a discharge end, wherein the feed end is connected to one end of the muffle section via a flange, the other end of the muffle section is connected to one end of the water cooling section via an air cooling section, and the other end of the water cooling section is connected to the discharge end via a flange.
[0033] like Figure 1As shown, the feed end includes a feed port 1, a steel belt pressure roller 2, a steel belt steering roller 3, a feed bin 4, a waste hydrogen release port 5, and a distributor 6. The bottom of the feed bin 4 is connected to the distributor 6 through a bearing seat. The distributor 6 adopts a variable frequency feeding control, which is more suitable for the feeding control of low bulk ratio iron oxide powder (low bulk ratio, poor fluidity, difficult automatic feeding, and easy to block the feed port). Steel belt pressure rollers 2 are respectively arranged on both sides of the distributor 6. The two ends of the steel belt pressure roller 2 are connected to the feed port 1 through a bearing seat. A stainless steel belt 14 is arranged below the steel belt pressure roller 2. The steel belt pressure roller 2 is used to ensure the flatness of the stainless steel belt 14 and ensure uniform feeding. A steel belt steering roller 3 is provided below the stainless steel belt 14. The steel belt steering roller 3 is fixed on the feed port 1 through a bearing seat. The stainless steel belt 14 changes direction through the steel belt steering roller 3. Waste hydrogen is not easy to overflow from here due to its low density. The waste hydrogen release port 5 is welded to the end of the feed port 1 close to the furnace body. The waste hydrogen release port 5 adopts a steel pipe design, which greatly increases the pressure of the reducing atmosphere in the furnace, is conducive to the penetration of the reducing atmosphere, and improves the reduction effect. The end of the feed port 1 away from the furnace body is tilted downward by 30°-40°. The stainless steel belt 14 changes the horizontal movement direction through the steel belt steering roller 3 to a downward tilt, so that the hydrogen flowing back is not easy to flow out with the steel belt due to its low density. The thickness of the cloth is controlled by controlling the speed of the distributor 6 through the frequency converter. The discharge port is placed in the furnace body while keeping the material not empty to further prevent the outflow of hydrogen. In this way, the hydrogen pressure in the furnace body is increased.
[0034] like Figure 2 As shown, the muffle section includes a muffle tube 7, a guide plate 8, and a hydrogen inlet 15. The top of the muffle tube 7 is arc-shaped, and a plurality of guide plates 8 are welded to the inner wall of the top. A hydrogen inlet 15 is provided at the end of the muffle tube 7, and a hydrogen control valve is provided at the hydrogen inlet 15. The muffle tube 7 is divided into temperature zones, and a guide plate 8 is welded in each temperature zone. First, the risk of collapse of the arc-shaped top of the muffle tube 7 due to long-term heating is reduced; second, the hydrogen is prevented from moving in a straight line along the arc-shaped top of the muffle tube, the hydrogen running speed is slowed down and the movement trajectory is changed, so that the hydrogen 9 runs along the curve under the obstruction of the guide plate 8 and further diffuses to the muffle tube 7 laterally (the edge of the muffle tube), so as to achieve the purpose of full contact between the reducing atmosphere and the material.
[0035] like Figure 3As shown, the discharge end includes a discharge port 11, a nitrogen inlet 10, a nitrogen sealing curtain 12, and a second steel belt steering roller 13. The nitrogen inlet 10 and the nitrogen sealing curtain 12 are welded to the upper part of the discharge port 11. A nitrogen control valve is provided at the nitrogen inlet 10. The nitrogen inlet 10 and the nitrogen sealing curtain 12 are arranged at intervals. A second steel belt steering roller 13 is provided at the corner where the discharge port 11 is connected to the water cooling section. Both ends of the second steel belt steering roller 13 are connected and fixed to the discharge port 11 through a bearing seat. The nitrogen sealing curtain 12 blocks the internal reducing atmosphere from the external air to avoid the formation of mixed explosive gas. There are two groups of nitrogen sealing curtains 12. The nitrogen inlet 10 is composed of six rows of steel pipes. Every two rows of steel pipes are arranged at intervals with a group of nitrogen sealing curtains 12. Each row of steel pipes is covered with pinholes with a diameter of about 1 mm. The corner of the discharge port 11 is tilted downward at about 45 degrees, and the stainless steel belt 14 at the discharge end is changed from a horizontal movement direction to a downward tilt through the steel belt steering roller 13, so that the hydrogen flowing back is not easy to flow out with the steel belt due to its low density; at the same time, the nitrogen flow at the nitrogen inlet 10 is timely controlled by a manual nitrogen control valve against a flow meter to further prevent the outflow of hydrogen and ensure the safety of the furnace.
[0036] The method for using the low bulk ratio ultrafine iron powder reduction furnace tube comprises the following steps:
[0037] 1) First, open the stainless steel belt 14, introduce nitrogen into the nitrogen inlet 10, open the hydrogen control valve, and let hydrogen enter from the hydrogen inlet 15 at the upper opening of the furnace tube at the discharge end and control the flow rate by the hydrogen control valve, and ignite the torch at the waste hydrogen release port 5 until the waste hydrogen is ignited;
[0038] 2) Turn on the cloth feeder 6 and measure the cloth thickness until the required thickness is reached;
[0039] 3) Adjust the hydrogen control valve according to the flame changes of the waste hydrogen to ensure that the flame of the waste hydrogen discharge port 5 is ignited normally;
[0040] 4) Adjust the nitrogen control valve at the nitrogen inlet 10 to ensure good sealing and prevent the material from being blown away;
[0041] 5) When shutdown is required, first stop the distributor 6, then close the hydrogen control valve to stop the supply of hydrogen; finally stop the nitrogen and stop the operation of the steel belt.
[0042] The present invention is not limited to the above-mentioned implementation modes, and anyone should be aware of the structural changes made under the enlightenment of the present invention, and all those having the same or similar technical solutions as the present invention fall within the protection scope of the present invention.
[0043] The techniques, shapes, and structural parts not described in detail in the present invention are all well-known techniques.
Claims
1. A low bulk ratio ultrafine iron powder reduction furnace tube, characterized in that: It includes a feed end, a muffle section, an air cooling section, a water cooling section, and a discharge end. The feed end is connected to one end of the muffle section through a flange, the other end of the muffle section is connected to one end of the water cooling section through an air cooling section, and the other end of the water cooling section is connected to the discharge end through a flange; The feed end includes a feed port, a steel belt pressure roller, a steel belt steering roller, a lower feed bin, a waste hydrogen release port, and a distributor. The bottom of the lower feed bin is connected to the distributor through a bearing seat. Steel belt pressure rollers are respectively provided on both sides of the distributor. A stainless steel belt is provided below the steel belt pressure roller. A steel belt steering roller is provided below the stainless steel belt. The steel belt steering roller is fixed to the feed port through a bearing seat. The waste hydrogen release port is welded to one end of the feed port close to the furnace body, and the end of the feed port away from the furnace body is inclined downward. The muffle section includes a muffle tube, a guide plate, and a hydrogen inlet. The top of the muffle tube is arc-shaped, a plurality of guide plates are welded to the inner wall of the top, and a hydrogen inlet is arranged at the end of the muffle tube. The discharging end comprises a discharging port, a nitrogen inlet, a nitrogen sealing curtain, and two steel belt steering rollers. The nitrogen inlet and the nitrogen sealing curtain are welded to the upper part of the discharging port. The nitrogen inlet and the nitrogen sealing curtain are arranged at intervals. A second steel belt steering roller is arranged at the corner where the discharging port is connected to the water cooling section. Both ends of the second steel belt steering roller are connected and fixed to the discharging port through a bearing seat. The muffle tube is divided into temperature zones, and a guide plate is welded in each temperature zone; The feed port and the discharge port are both bent in design, with the end of the feed port away from the furnace body tilted downward by 30°-40°, and the corner of the discharge port tilted downward by 45°.
2. The low bulk ratio ultrafine iron powder reduction furnace tube according to claim 1, characterized in that: The nitrogen sealing curtains are provided with two groups, and the nitrogen inlet is composed of six rows of steel pipes. Every two rows of steel pipes are arranged at intervals with one group of nitrogen sealing curtains, and each row of steel pipes is covered with pinholes with a diameter of 1 mm.
3. The low bulk ratio ultrafine iron powder reduction furnace tube according to claim 1, characterized in that: A hydrogen control valve is provided at the hydrogen inlet, and a nitrogen control valve is provided at the nitrogen inlet.
4. The low bulk ratio ultrafine iron powder reduction furnace tube according to claim 1, characterized in that: The waste hydrogen discharge port adopts a steel pipe design.
5. The low bulk ratio ultrafine iron powder reduction furnace tube according to claim 1, characterized in that: The material distributor adopts frequency conversion material feeding control.
6. The method for using the low bulk ratio ultrafine iron powder reduction furnace tube according to any one of claims 1 to 5, characterized in that: The following steps are involved: 1) First, open the stainless steel belt, introduce nitrogen into the nitrogen inlet, open the hydrogen control valve and slowly introduce hydrogen, and ignite the torch at the waste hydrogen release port until the waste hydrogen is ignited; 2) Turn on the fabric feeder and measure the fabric thickness until it reaches the required thickness; 3) Adjust the hydrogen control valve according to the flame changes of the waste hydrogen to ensure that the flame of the waste hydrogen discharge port is ignited normally; 4) Adjust the nitrogen control valve at the nitrogen inlet to ensure good sealing and prevent the material from being blown away; 5) When shutdown is required, first stop the distributor, then close the hydrogen control valve to stop the hydrogen supply; finally stop the nitrogen and stop the operation of the steel belt.