A magnetic metal nanoparticle-modified carbon hollow sphere wave absorbing material and preparation method thereof
By modifying the surface of carbon hollow spheres with magnetic metal nanoparticles, the problems of low magnetic permeability and poor impedance matching of carbon-based absorbing materials are solved, the absorbing performance and bandwidth are significantly improved, and better electromagnetic wave absorption effects are achieved.
Patent Information
- Application Number
- CN202110863091.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The low magnetic permeability and poor spatial impedance matching of carbon-based absorbing materials limit the improvement of its reflection loss, resulting in insufficient absorbing performance.
By modifying magnetic metal nanoparticles (such as Ni, Co, Mn) on the surface of carbon hollow spheres, an unstable polarization center is formed, which increases spatial polarization charge accumulation and improves eddy current loss and hysteresis loss under the electromagnetic wave alternating electric field. Improve the relative magnetic permeability and spatial impedance matching of materials.
The reflection loss and bandwidth of the absorbing material are significantly improved, and the RL value is extended from 2.3GHz to 3.4~5.3GHz, which improves the absorbing performance while maintaining the stability of the material.
Smart Images

Figure CN113597247B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wave absorbing materials, and in particular to a carbon hollow sphere wave absorbing material modified by magnetic metal nanoparticles and a preparation method thereof. Background Art
[0002] Absorbing materials are a type of material that can absorb electromagnetic waves of different bands and convert them into other energies (heat, electricity, kinetic energy, etc.) to dissipate or cause coherent destructive electromagnetic waves. They are widely used in modern military, information technology (security) and other fields. Absorbing materials can be tailored to their absorbing properties according to their physical and chemical properties, morphological design or material composites, so as to achieve good absorption of electromagnetic waves in a specific frequency band while taking into account the characteristics of "thin, light, wide and strong".
[0003] Mesoporous carbon hollow spheres are particularly suitable for electromagnetic waves to enter and reflect multiple times due to their unique geometric morphology, namely, nano-scale through holes on the surface and hollow spherical cavities, and are easy to achieve high-performance absorption of the bulk material. Carbon-based materials are dielectric absorption materials with high dielectric loss, but their magnetic permeability is low and the spatial impedance matching is poor, which limits the further increase of reflection loss (RL value). Therefore, the absorption performance of this type of material can still be further improved on the basis of the bulk material. Summary of the invention
[0004] The purpose of the present invention is to provide a carbon hollow sphere absorbing material modified by magnetic metal nanoparticles and a preparation method thereof. The present invention increases the reflection loss and further improves the absorbing performance of the material by improving the magnetic permeability and spatial impedance matching of the absorbing material.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The invention provides a carbon hollow ball absorbing material modified by magnetic metal nanoparticles, comprising a carbon hollow ball and magnetic metal nanoparticles; the magnetic metal nanoparticles are located on the inner and outer wall surfaces of the carbon hollow ball; the magnetic metal nanoparticles are Ni, Co or Mn nanoparticles.
[0007] Preferably, the diameter of the hollow carbon sphere is 200-300 nm, and the wall thickness is 20-50 nm.
[0008] Preferably, the particle size of the magnetic metal nanoparticles is 5 to 10 nm.
[0009] The present invention provides a method for preparing the hollow carbon sphere absorbing material described in the above scheme, comprising the following steps:
[0010] Ammonia water, an alcohol-water mixed solvent and tetrapropoxysilane are mixed to cause a hydrolysis reaction to form SiO2 cores to obtain a hydrolyzate;
[0011] Adding resorcinol and formaldehyde to the hydrolyzate to cause phenolic condensation and coating reaction, and obtaining phenolic resin-coated SiO2 after solid-liquid separation;
[0012] The phenolic resin is coated with SiO2 for carbonization to obtain carbonized powder;
[0013] The carbonized powder is mixed with an HF aqueous solution, and then etched to obtain a carbon hollow sphere absorbing body material after solid-liquid separation;
[0014] The carbon hollow sphere absorbing body material and the ethanol solution of metal acetate are mixed for modification, and the metal salt-modified carbon hollow spheres are obtained after solid-liquid separation; the metal acetate is nickel acetate, cobalt acetate or manganese acetate;
[0015] The metal salt-modified carbon hollow spheres are mixed with a methanol-ethanol mixed solution of NaBH4 and subjected to a reduction reaction to obtain a magnetic metal nanoparticle-modified carbon hollow sphere wave absorbing material.
[0016] Preferably, the alcohol-water mixed solvent is an ethanol-water mixed solvent, and the volume ratio of ethanol to water in the ethanol-water mixed solvent is (7-9):1.
[0017] Preferably, the mass fraction of the ammonia water is 25-28%; the volume ratio of the ammonia water, alcohol-water mixed solvent and tetrapropoxysilane is 15:400:(8-26); and the hydrolysis reaction time is 10-20 min.
[0018] Preferably, the amount of the hydrolyzate is calculated based on the amount of tetrapropoxysilane, and the amount ratio of resorcinol to tetrapropoxysilane is 1g: (4-13)mL; the amount ratio of resorcinol to formaldehyde is 2g: (2.8-4.3)mL; the mass fraction of formaldehyde is 36-38%.
[0019] Preferably, the carbonization temperature is 680-720° C., and the time is 5-8 hours; the carbonization is carried out under a protective atmosphere.
[0020] Preferably, the concentration of the metal acetate ethanol solution is 0.05-0.20 mol / L; the usage ratio of the carbon hollow sphere absorbing body material to the metal acetate ethanol solution is 0.1 g:10 mL.
[0021] Preferably, the concentration of the HF aqueous solution is 3-6 wt %.
[0022] The present invention provides a carbon hollow sphere absorbing material modified by magnetic metal nanoparticles, comprising a carbon hollow sphere and magnetic metal nanoparticles; the magnetic metal nanoparticles are located on the inner and outer wall surfaces of the carbon hollow sphere; the magnetic metal nanoparticles are Ni, Co or Mn nanoparticles. The present invention uses magnetic metal nanoparticles to modify the carbon hollow sphere, which can form an unstable polarization center on the contact interface between the two, resulting in a large amount of spatial polarization charge accumulation, which is beneficial to the absorption of electromagnetic waves and improves the RL value; at the same time, the eddy current loss and hysteresis loss under the alternating electric field of the electromagnetic wave further improve the RL value. In addition, the present invention can also solve the problem of poor spatial impedance matching of the carbon hollow sphere by introducing magnetic metal nanoparticles to increase the relative magnetic permeability of the material, reduce the reflection of electromagnetic waves at the interface of the absorbing material, and thus improve its absorbing performance. The results of the embodiment show that the hollow sphere modified by the metal particles introduced in the present invention not only improves the RL value, but also further broadens the bandwidth. The bandwidth of the unmodified carbon hollow sphere is 2.3GHz, and the bandwidth becomes 3.4-5.3GHz after modification. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a TEM photo of the absorbing material prepared in Example 1;
[0024] Figure 2 This is the EDS-mapping diagram of the absorbing material prepared in Example 1;
[0025] Figure 3 The XRD patterns of the absorbing materials prepared in Example 1 and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0026] The invention provides a carbon hollow ball absorbing material modified by magnetic metal nanoparticles, comprising a carbon hollow ball and magnetic metal nanoparticles; the magnetic metal nanoparticles are located on the inner and outer wall surfaces of the carbon hollow ball; the magnetic metal nanoparticles are Ni, Co or Mn nanoparticles.
[0027] In the present invention, the diameter of the hollow carbon sphere is preferably 200 to 300 nm, and the wall thickness is preferably 20 to 50 nm, more preferably 30 to 40 nm. In the present invention, the hollow carbon sphere is preferably a mesoporous hollow carbon sphere.
[0028] In the present invention, the particle size of the magnetic metal nanoparticles is preferably 5 to 10 nm, more preferably 6 to 9 nm. In the present invention, the magnetic metal nanoparticles are Ni, Co or Mn nanoparticles, preferably Co or Mn nanoparticles, more preferably Mn nanoparticles.
[0029] The present invention uses Ni, Co or Mn nanoparticles to modify the carbon hollow sphere, which can form an unstable polarization center at the contact interface between the two, resulting in a large amount of spatial polarization charge accumulation, which is beneficial to the absorption of electromagnetic waves and improves the RL value; at the same time, the eddy current loss and hysteresis loss under the electromagnetic wave alternating electric field further improve the RL value. In addition, the present invention can also solve the problem of poor spatial impedance matching of the carbon hollow sphere by introducing magnetic metal nanoparticles, reduce the reflection of electromagnetic waves at the interface of the absorbing material, and thus improve its absorbing performance.
[0030] Compared with other magnetic metals such as Fe, the magnetic metal of the present invention improves the wave absorbing performance and the obtained wave absorbing material also has good stability.
[0031] The present invention provides a method for preparing the hollow carbon sphere absorbing material described in the above scheme, comprising the following steps:
[0032] Ammonia water, an alcohol-water mixed solvent and tetrapropoxysilane are mixed to cause a hydrolysis reaction to form SiO2 cores to obtain a hydrolyzate;
[0033] Adding resorcinol and formaldehyde to the hydrolyzate to cause phenolic condensation and coating reaction, and obtaining phenolic resin-coated SiO2 after solid-liquid separation;
[0034] The phenolic resin is coated with SiO2 for carbonization to obtain carbonized powder;
[0035] The carbonized powder is mixed with an HF aqueous solution, and then etched to obtain a carbon hollow sphere absorbing body material after solid-liquid separation;
[0036] The carbon hollow sphere absorbing body material and the ethanol solution of metal acetate are mixed for modification, and the metal salt-modified carbon hollow spheres are obtained after solid-liquid separation; the metal acetate is nickel acetate, cobalt acetate or manganese acetate;
[0037] The metal salt-modified carbon hollow spheres are mixed with a methanol-ethanol mixed solution of NaBH4 and subjected to a reduction reaction to obtain a magnetic metal nanoparticle-modified carbon hollow sphere wave absorbing material.
[0038] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0039] The invention mixes ammonia water, alcohol-water mixed solvent and tetrapropoxysilane to generate a hydrolysis reaction to form SiO2 cores and obtain a hydrolyzate.
[0040] In the present invention, the mass fraction of the ammonia water is preferably 25-28%; the alcohol-water mixed solvent is preferably an ethanol-water mixed solvent, and the volume ratio of ethanol to water in the ethanol-water mixed solvent is (7-9): 1. In the present invention, the ethanol-water mixed solvent is preferably obtained by mixing anhydrous ethanol and deionized water.
[0041] In the present invention, the ammonia water is used as a hydrolysis accelerator to promote the hydrolysis of tetrapropoxysilane, and provides a catalytic effect for the later synthesis of phenolic resin. The present invention adopts an alcohol-water mixed solvent, which can prevent the hydrolysis reaction from being too fast, and the phenolic resin is completely precipitated and cannot be coated, and can also adjust the interfacial tension to ensure that the subsequent reaction can be well carried out on the surface of the spherical SiO2 core, thereby forming a phenolic resin-coated SiO2 core structure.
[0042] In the present invention, the volume ratio of the aqueous ammonia, the alcohol-water mixed solvent and tetrapropoxysilane is preferably 15:400:(8-26), and more preferably 15:400:(10-20).
[0043] In the present invention, the mixing of aqueous ammonia, alcohol-water mixed solvent and tetrapropoxysilane preferably comprises: firstly mixing aqueous ammonia and alcohol-water mixed solvent, and then adding tetrapropoxysilane and vortex mixing for 10 to 20 minutes.
[0044] After tetrapropoxysilane is added in the present invention, the tetrapropoxysilane is hydrolyzed when it meets water to form SiO2 core.
[0045] After obtaining the hydrolyzate, the present invention directly adds resorcinol and formaldehyde to the hydrolyzate without any post-treatment, so that phenolic condensation and coating reactions occur, and after solid-liquid separation, phenolic resin-coated SiO2 is obtained.
[0046] In the present invention, the amount of the hydrolyzate is calculated based on the amount of tetrapropoxysilane, and the amount ratio of the resorcinol to tetrapropoxysilane is preferably 1g: (4-13) mL, more preferably 1g: (2-10) mL; the amount ratio of the resorcinol to formaldehyde is preferably 2g: (2.8-4.3) mL, more preferably 2g: (3.0-4.0) mL. In the present invention, the mass fraction of the formaldehyde is preferably 36-38%.
[0047] In the present invention, the phenolic condensation and coating reaction are preferably carried out under stirring conditions. The present invention has no special requirements for the stirring rate, and the stirring rate known in the art can be used. In the present invention, the time of the phenolic condensation and coating reaction is preferably 20 to 28 hours, more preferably 24 hours.
[0048] During the phenolic condensation and coating reaction, resorcinol and formaldehyde undergo a phenolic condensation reaction under the catalytic action of ammonia water to generate a phenolic resin, which is coated on the surface of the SiO2 core. At the same time, the hydrolysis reaction in the previous step is still carried out in trace amounts.
[0049] The present invention has no special requirements for the solid-liquid separation method, and can use a solid-liquid separation method well known in the art, such as centrifugation. After completing the solid-liquid separation, the present invention preferably centrifuges the obtained solid with anhydrous ethanol / deionized water (volume ratio of 1:1) mixed solvent for 3 to 5 times, collects the powder and dries it under vacuum at 60°C for 24 hours to obtain phenolic resin-coated SiO2.
[0050] After obtaining the phenolic resin coated SiO2, the present invention carbonizes the phenolic resin coated SiO2 to obtain carbonized powder.
[0051] In the present invention, the carbonization temperature is preferably 680-720°C, more preferably 690-710°C; the carbonization time is preferably 5-8h, more preferably 5h. In the present invention, the carbonization is preferably carried out under a protective atmosphere, more preferably under a nitrogen atmosphere.
[0052] After obtaining the carbonized powder, the present invention mixes the carbonized powder with an HF aqueous solution, performs etching, and obtains a carbon hollow sphere absorbing body material after solid-liquid separation.
[0053] In the present invention, the concentration of the HF aqueous solution is preferably 3 to 6 wt%, more preferably 5 wt%. The present invention has no special requirements for the amount of the HF aqueous solution, as long as it can etch away all SiO2. The present invention preferably disperses the carbonized powder into the HF aqueous solution and magnetically stirs for 6 hours for etching. The present invention has no special requirements for the stirring rate during the etching process, and the stirring rate well known in the art can be used. The present invention uses the HF aqueous solution to etch SiO2 to form hollow spheres and surface mesopores.
[0054] The present invention has no special requirements for the solid-liquid separation method, and can use a solid-liquid separation method known in the art, such as centrifugation. The present invention preferably washes the solid obtained after solid-liquid separation by centrifugation for 3 times with deionized water, collects the powder again and dries it at 60°C under vacuum for 24 hours to obtain a carbon hollow sphere absorbing body material.
[0055] After obtaining the carbon hollow sphere absorbing body material, the present invention mixes the carbon hollow sphere absorbing body material with an ethanol solution of a metal acetate for modification, and obtains the metal salt-modified carbon hollow sphere after solid-liquid separation; the metal acetate is nickel acetate, cobalt acetate or manganese acetate.
[0056] In the present invention, the concentration of the ethanol solution of metal acetate is preferably 0.05-0.20 mol / L, more preferably 0.15 mol / L; the ethanol solution of metal acetate is preferably obtained by dissolving metal acetate in anhydrous ethanol.
[0057] In the present invention, the usage ratio of the carbon hollow sphere absorbing body material and the ethanol solution of metal acetate is preferably 0.1 g:10 mL.
[0058] In the present invention, mixing the carbon hollow sphere absorbing body material and the ethanol solution of metal acetate preferably includes: vortex dispersing the carbon hollow sphere absorbing body material in the ethanol solution of metal acetate for 5 to 10 minutes, and the metal acetate penetrates from the mesopores of the outer wall of the hollow sphere and enters the interior of the hollow sphere, thereby achieving the modification purpose.
[0059] After the modification is completed, the present invention preferably performs solid-liquid separation by centrifugation, and then the obtained solid is dried at 60° C. under vacuum conditions for 12 h to obtain metal salt-modified carbon hollow spheres.
[0060] After obtaining the metal salt-modified carbon hollow spheres, the present invention mixes the metal salt-modified carbon hollow spheres with a methanol-ethanol mixed solution of NaBH4 and performs a reduction reaction to obtain a magnetic metal nanoparticle-modified carbon hollow sphere absorbing material.
[0061] In the present invention, the volume ratio of methanol and ethanol in the methanol-ethanol mixed solution is preferably 1:1; the concentration of NaBH4 in the methanol-ethanol mixed solution of NaBH4 is preferably 2 mol / L. In the present invention, the methanol-ethanol mixed solution of NaBH4 is preferably obtained by mixing NaBH4, anhydrous methanol and anhydrous ethanol. The present invention uses anhydrous mixed alcohol to ensure that the metal elements are not modified in the form of hydroxides. Methanol has a lower specific surface tension but its solubility in metal acetates is not as good as ethanol, so the present invention uses a mixed alcohol solvent. The low specific surface tension is conducive to the methanol-ethanol mixed solution of NaBH4 entering the interior along the mesopores of the C hollow sphere to modify the interior of the sphere.
[0062] In the present invention, the mass of the metal salt-modified carbon hollow spheres is based on the mass of the carbon hollow spheres, and the usage ratio of the carbon hollow spheres to the methanol-ethanol mixed solution of NaBH4 is preferably 0.1 g:10 mL.
[0063] In the present invention, the reduction reaction preferably comprises: dispersing the metal-modified carbon hollow spheres into a methanol-ethanol mixed solution of NaBH4 and vortex mixing for 30 minutes, followed by vacuum treatment for 5 minutes.
[0064] The present invention utilizes vacuum treatment to extract air from the hollow sphere and simultaneously introduces a methanol-ethanol mixed solution of NaBH4. Methanol-ethanol is extremely easy to boil under low vacuum conditions and can promote a better reduction reaction between sodium borohydride and metal salt.
[0065] After the reduction reaction is completed, the product is collected by centrifugation and washed 3 to 5 times with a mixed solvent of anhydrous ethanol / deionized water (volume ratio of 1:1), and then dried at 60° C. under vacuum conditions for 24 hours to obtain a magnetic metal nanoparticle-modified carbon hollow sphere absorbing material.
[0066] The magnetic metal nanoparticle-modified carbon hollow sphere absorbing material and the preparation method thereof provided by the present invention are described in detail below in conjunction with the examples, but they should not be construed as limiting the protection scope of the present invention.
[0067] Example 1
[0068] Ni nanoparticle modification
[0069] 15 mL of ammonia water (commercially available, 25-28 wt%) was added to a total volume of 400 mL of anhydrous ethanol-deionized water mixed solvent (volume ratio controlled to be 9:1), and then 10 mL of tetrapropoxysilane was added to the above mixed solvent and vortexed to mix evenly. The mixing process was maintained for 15 minutes. After 15 minutes, 2.0 g of resorcinol and 3 mL of formaldehyde (commercially available, 37 wt%) were added in sequence, and the mixed solution was magnetically stirred for 24 hours. The obtained powder was collected by centrifugation and mixed with anhydrous ethanol / deionized water (volume ratio was 1:1). The solvent is centrifuged and washed three times, and the powder is collected and dried at 60°C under vacuum conditions for 24 hours to obtain phenolic resin-coated SiO2; the phenolic resin-coated SiO2 is placed in a tubular furnace and heat treated at 680°C for 5 hours under N2 protective atmosphere to induce carbonization to obtain carbonized powder; the carbonized powder is dispersed in a 5wt% HF aqueous solution and magnetically stirred for 6 hours, the obtained powder is centrifuged and washed three times with deionized water, the powder is collected again and dried at 60°C under vacuum conditions for 24 hours to obtain the mesoporous carbon hollow sphere absorbing body material.
[0070] A 30 mL nickel acetate anhydrous ethanol solution with a solute concentration of 0.15 mol / L was prepared; 0.3 g of the bulk material was vortex dispersed in the solution, and the process lasted for 10 min to allow the acetate to fully modify the inner and outer walls of the bulk material. The resulting product was collected by centrifugation and dried at 60°C under vacuum conditions for 12 h to obtain metal salt-modified carbon hollow spheres.
[0071] The metal salt modified carbon hollow spheres were dispersed in 30 mL of 2 mol / L NaBH4 anhydrous methanol-ethanol mixed solution (volume ratio of 1:1) and vortex mixed for 30 min, and then vacuum treated for 5 min; the obtained product was collected by centrifugation and washed three times by centrifugation with a mixed solvent of anhydrous ethanol / deionized water (volume ratio of 1:1), and then dried at 60°C under vacuum conditions for 24 h to obtain nickel nanoparticle-modified carbon hollow sphere absorbing material, recorded as Ni@C mesoporous spheres.
[0072] Example 2
[0073] Co nanoparticle modification
[0074] 15 mL of ammonia water (commercially available, 25-28 wt%) was added to a total volume of 400 mL of anhydrous ethanol-deionized water mixed solvent (volume ratio controlled at 9:1), and then 10 mL of tetrapropoxysilane was added to the mixed solvent and vortexed to mix evenly. The mixing process was maintained for 15 min. After 15 min, 2.0 g of resorcinol and 3.6 mL of formaldehyde (commercially available, 37 wt%) were added in sequence. The mixed solution was magnetically stirred for 24 h. The obtained powder was collected by centrifugation and mixed with anhydrous ethanol / deionized water (volume ratio of 1:1). The mixed solvent is centrifuged and washed three times, and the powder is collected and dried at 60°C under vacuum conditions for 24 hours to obtain phenolic resin-coated SiO2; the phenolic resin-coated SiO2 is placed in a tubular furnace and heat treated at 700°C for 5 hours under N2 protective atmosphere to induce carbonization to obtain carbonized powder; the carbonized powder is dispersed in a 5wt% HF aqueous solution and magnetically stirred for 6 hours, the obtained powder is centrifuged and washed three times with deionized water, the powder is collected again and dried at 60°C under vacuum conditions for 24 hours to obtain the mesoporous carbon hollow sphere absorbing body material.
[0075] A 30 mL anhydrous ethanol solution of cobalt acetate was prepared with a solute concentration of 0.15 mol / L; 0.3 g of the bulk material was vortex dispersed in the solution for 10 min to allow the acetate to fully modify the inner and outer walls of the bulk material. The resulting product was collected by centrifugation and dried at 60°C under vacuum conditions for 12 h to obtain metal salt-modified carbon hollow spheres.
[0076] The metal salt modified carbon hollow spheres were dispersed in 30 mL of 2 mol / L NaBH4 anhydrous methanol-ethanol mixed solution (volume ratio of 1:1) and vortex mixed for 30 min, and then vacuum treated for 5 min; the obtained product was collected by centrifugation and washed three times with anhydrous ethanol / deionized water (volume ratio of 1:1) mixed solvent, and then dried at 60°C under vacuum conditions for 24 h to obtain cobalt nanoparticle-modified carbon hollow sphere absorbing material, recorded as Co@C mesoporous spheres.
[0077] Example 3
[0078] Mn nanoparticle modification
[0079] 15 mL of ammonia water (commercially available, 25-28 wt%) was added to a total volume of 400 mL of anhydrous ethanol-deionized water mixed solvent (volume ratio controlled at 9:1), and then 10 mL of tetrapropoxysilane was added to the mixed solvent and vortexed to mix evenly. The mixing process was maintained for 15 min. After 15 min, 2.0 g of resorcinol and 4.0 mL of formaldehyde (commercially available, 37 wt%) were added in sequence. The mixed solution was magnetically stirred for 24 h. The obtained powder was collected by centrifugation and mixed with anhydrous ethanol / deionized water (volume ratio of 1:1). The mixed solvent is centrifuged and washed three times, and the powder is collected and dried at 60°C under vacuum conditions for 24 hours to obtain phenolic resin-coated SiO2; the phenolic resin-coated SiO2 is placed in a tubular furnace and heat treated at 720°C for 5 hours under N2 protective atmosphere to induce carbonization to obtain carbonized powder; the carbonized powder is dispersed in a 5wt% HF aqueous solution and magnetically stirred for 6 hours, the obtained powder is centrifuged and washed three times with deionized water, the powder is collected again and dried at 60°C under vacuum conditions for 24 hours to obtain the mesoporous carbon hollow sphere absorbing body material.
[0080] A 30 mL anhydrous ethanol solution of manganese acetate was prepared with a solute concentration of 0.15 mol / L; 0.3 g of the bulk material was vortex dispersed in the solution for 10 min to allow the acetate to fully modify the inner and outer walls of the bulk material. The resulting product was collected by centrifugation and dried at 60°C under vacuum conditions for 12 h to obtain metal salt-modified carbon hollow spheres.
[0081] The metal salt modified carbon hollow spheres were dispersed in 30 mL of 2 mol / L NaBH4 anhydrous methanol-ethanol mixed solution (volume ratio of 1:1) and vortex mixed for 30 min, and then vacuum treated for 5 min; the obtained product was collected by centrifugation and washed three times with anhydrous ethanol / deionized water (volume ratio of 1:1) mixed solvent, and then dried at 60°C under vacuum conditions for 24 h to obtain manganese nanoparticle-modified carbon hollow sphere absorbing material, recorded as Mn@C mesoporous spheres.
[0082] Comparative Example 1
[0083] The difference from Example 1 is that the nickel nanoparticles are not modified.
[0084] Structure and performance characterization:
[0085] 1. The nickel nanoparticle-modified carbon hollow sphere absorbing material prepared in Example 1 was observed by transmission electron microscopy. The results are as follows: Figure 1 As shown. Figure 1It can be seen that the diameter of the mesoporous carbon hollow sphere absorber modified by nickel nanoparticles is in the range of 200-300nm, the hollow morphology is obvious, and the average wall thickness is about 30nm. There are 4 carbon hollow spheres modified by Ni metal nanoparticles in the figure, one of which is not modified and is indicated by a dotted ball. It can be seen that the interiors of the other 4 spheres have obvious internal contrast differences, and the arrows here indicate that they are Ni nanoparticles.
[0086] In order to confirm that the modified object is Ni nanoparticles, a single Ni-modified carbon nanohollow sphere was selected for elemental surface scanning analysis. The results are as follows: Figure 2 shown. Figure 2 In the middle, the right picture shows obvious C element signals (blue dots). The blue dots in the central area clearly form a hollow sphere, which proves again that C elements are accumulated in the shape of hollow spheres. The surrounding C element signals are relatively strong because the Cu mesh used in TEM sample preparation is coated with an ultra-thin C film; the left picture shows the Ni element signal, which shows that Ni elements are evenly distributed on the inner wall of the carbon hollow sphere, and even a small amount is distributed on the inner wall of the pore wall, and a small part is distributed on the outer wall of the carbon hollow sphere.
[0087] 2. XRD test was performed on the absorbing materials prepared in Example 1 and Comparative Example 1. The results are as follows: Figure 3 shown. Figure 3 In the embodiment, C+Ni corresponds to the absorbing material of Example 1, and C corresponds to the absorbing material of Example 1. Figure 3 It can be seen that the modified C hollow spheres have obvious Ni derivative peaks, indicating that the modified products are indeed Ni nanoparticles. Analysis of the Ni derivative peaks (combined with the Scherrer formula) estimates that the Ni particle size is approximately 8 nm.
[0088] 3. The absorbing materials prepared in Examples 1 to 3 and Comparative Example 1 were tested for their absorbing performance. The specific testing method is as follows: The absorbing material and paraffin were uniformly mixed at a mass ratio of 20:80 and pressed into a metal mold with an inner diameter of 3.04 mm and an outer diameter of 7.00 mm to form a concentric ring sample to be tested. The electromagnetic performance parameters were tested using an Agilent N5230A vector network analyzer in the frequency range of 2 to 18 GHz. The results are shown in Table 1.
[0089] Table 1 Wave absorbing properties of the wave absorbing materials prepared in Examples 1 to 3 and Comparative Example 1
[0090] Sample name Optimized thickness(mm) RL(dB) Bandwidth (GHz) Mesoporous Carbon Spheres 2.0 -20.32 2.3 Ni@C mesoporous spheres 2.6 -38.92 3.4 Co@C mesoporous spheres 2.8 -54.58 4.8 Mn@C mesoporous spheres 3.2 -32.08 5.3
[0091] From the results in Table 1, it can be seen that when magnetic metal nanoparticles are used to modify the inner and outer surfaces of the carbon hollow spheres, compared with the carbon hollow sphere bulk material, they all show good wave absorbing performance, the RL value is improved, and the bandwidth is expanded.
[0092] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A carbon hollow sphere absorbing material modified by magnetic metal nanoparticles, comprising a carbon hollow sphere and magnetic metal nanoparticles; the magnetic metal nanoparticles are located on the inner and outer wall surfaces of the carbon hollow sphere; the magnetic metal nanoparticles are Co nanoparticles; The preparation method of the hollow carbon sphere absorbing material comprises the following steps: Ammonia water, an alcohol-water mixed solvent and tetrapropoxysilane are mixed to cause a hydrolysis reaction to form SiO2 cores to obtain a hydrolyzate; Adding resorcinol and formaldehyde to the hydrolyzate to cause phenolic condensation and coating reaction, and obtaining phenolic resin-coated SiO2 after solid-liquid separation; The phenolic resin is coated with SiO2 for carbonization to obtain carbonized powder; The carbonized powder is mixed with an HF aqueous solution, and then etched to obtain a carbon hollow sphere wave absorbing body material after solid-liquid separation; The carbon hollow sphere absorbing body material and the ethanol solution of metal acetate are mixed for modification, and the metal salt-modified carbon hollow spheres are obtained after solid-liquid separation; the metal acetate is cobalt acetate; The metal salt-modified carbon hollow spheres are mixed with a methanol-ethanol mixed solution of NaBH4 and subjected to a reduction reaction to obtain a magnetic metal nanoparticle-modified carbon hollow sphere wave absorbing material.
2. The carbon hollow sphere absorbing material according to claim 1, characterized in that: The diameter of the carbon hollow sphere is 200-300nm, and the wall thickness is 20-50nm.
3. The carbon hollow sphere absorbing material according to claim 1, characterized in that: The particle size of the magnetic metal nanoparticles is 5 to 10 nm.
4. The method for preparing the hollow carbon sphere absorbing material according to any one of claims 1 to 3, comprising the following steps: Ammonia water, an alcohol-water mixed solvent and tetrapropoxysilane are mixed to cause a hydrolysis reaction to form SiO2 cores to obtain a hydrolyzate; Adding resorcinol and formaldehyde to the hydrolyzate to cause phenolic condensation and coating reaction, and obtaining phenolic resin-coated SiO2 after solid-liquid separation; The phenolic resin is coated with SiO2 for carbonization to obtain carbonized powder; The carbonized powder is mixed with an HF aqueous solution, and then etched to obtain a carbon hollow sphere wave absorbing body material after solid-liquid separation; The carbon hollow sphere absorbing body material and the ethanol solution of metal acetate are mixed for modification, and the metal salt-modified carbon hollow spheres are obtained after solid-liquid separation; the metal acetate is cobalt acetate; The metal salt-modified carbon hollow spheres are mixed with a methanol-ethanol mixed solution of NaBH4 and subjected to a reduction reaction to obtain a magnetic metal nanoparticle-modified carbon hollow sphere wave absorbing material.
5. The preparation method according to claim 4, characterized in that: The alcohol-water mixed solvent is an ethanol-water mixed solvent, and the volume ratio of ethanol to water in the ethanol-water mixed solvent is (7-9):
1.
6. The preparation method according to claim 4 or 5, characterized in that: The mass fraction of the ammonia water is 25-28%; the volume ratio of the ammonia water, alcohol-water mixed solvent and tetrapropoxysilane is 15:400:(8-26); and the hydrolysis reaction time is 10-20 minutes.
7. The preparation method according to claim 4, characterized in that: The amount of the hydrolyzate is calculated based on the amount of tetrapropoxysilane, the amount ratio of resorcinol to tetrapropoxysilane is 1g: (4-13)mL; the amount ratio of resorcinol to formaldehyde is 2g: (2.8-4.3)mL; the mass fraction of formaldehyde is 36-38%.
8. The preparation method according to claim 4, characterized in that: The carbonization temperature is 680-720° C., and the time is 5-8 hours; the carbonization is carried out under a protective atmosphere.
9. The preparation method according to claim 4, characterized in that: The concentration of the metal acetate ethanol solution is 0.05-0.20 mol / L; the usage ratio of the carbon hollow sphere wave absorbing body material and the metal acetate ethanol solution is 0.1 g:10 mL.
10. The preparation method according to claim 4, characterized in that: The concentration of the HF aqueous solution is 3-6 wt %.
Citation Information
Patent Citations
Method for preparing porous carbon ball composite absorbing material loaded with magnetic metal element
CN105896099A
Hollow mesoporous carbon sphere electromagnetic wave absorber and preparation method thereof
CN106986325A
Mesoporous hollow carbon spheres and production and application in electromagnetic absorption thereof
CN110436441A
Preparation method of C@Ni composite material and electromagnetic shielding film
CN110498990A
Cited By
Egg yolk shell structure (magnetic metal-carbon)-air-porous carbon composite wave-absorbing material and preparation method thereof
CN121152196A