Lubricating wear-resistant bearing bush and preparation method thereof
By adding modified carbon nanotube/molybdenum disulfide composite material and modified basalt fibers to the polyether ether ketone bearing shell, combined with a specific preparation process, the problem of insufficient wear resistance and mechanical properties of the polyether ether ketone bearing shell is solved, and the problem of insufficient wear resistance and mechanical properties of the polyether ether ketone bearing shell is achieved. Higher lubricating wear resistance and service life.
Patent Information
- Application Number
- CN202411218321.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
Polyether ether ketone bearings have insufficient wear resistance and mechanical properties in sliding bearings equipped with marine engineering equipment, and need to be improved to adapt to strict environment and service life requirements.
Using polyether ether ketone as the matrix, modified carbon nanotube/molybdenum disulfide composite material and modified basalt fibers are added to prepare composite materials through hydrothermal reaction and surface modification treatment, and lubricating resistance is prepared by cold pressing and hot pressing forming processes. Grinded bearing shell.
It significantly improves the lubricating wear resistance and mechanical properties of bearing shells, extends service life, and enhances bearing capacity and overall strength.
Smart Images

Figure BDA0005022215320000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bearing bushes, and in particular to a lubricating and wear-resistant bearing bush and a preparation method thereof. Background Art
[0002] At present, due to the advantages of polymer bearings such as high elasticity, long life, low noise, and excellent friction characteristics, the research on polymer bearing materials has attracted more and more attention from researchers. Common polymer bearing materials include engineering plastics, rubber, etc.
[0003] Among them, engineering plastic bearings have been widely used and promoted in various fields due to their advantages such as good wear resistance, strong corrosion resistance, light weight, high strength, and convenient processing. For example, this type of bearing is used in sliding bearings of marine engineering equipment. The sliding bearings in marine engineering equipment have the characteristics of large shaft diameter, large load bearing, and high working life requirements. Therefore, there are also high requirements for the wear resistance and bearing capacity of the bearings. Among them, polyetheretherketone (PEEK) has become one of the engineering plastics for preparing bearings due to its excellent mechanical properties and friction and wear characteristics. However, although polyetheretherketone has certain self-lubrication, if the bearings prepared by this material are to be used in sliding bearings of marine engineering equipment for a long time, their wear resistance and mechanical properties need to be further improved. Therefore, it is necessary to develop a bearing with better lubrication, wear resistance and mechanical properties on the basis of polyetheretherketone, so that the prepared bearing can better adapt to various environments and have better application effects in marine engineering equipment. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the shortcomings and defects mentioned in the above background technology, and provide a lubricating and wear-resistant bearing and a preparation method thereof. The prepared bearing has excellent lubricating and wear-resistant properties, and has higher strength and strong bearing capacity as a whole, so that the bearing has stronger performance and longer service life.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0006] A lubricating and wear-resistant bearing bush comprises the following raw materials in parts by weight: 100 parts of polyetheretherketone, 3.5-5 parts of modified carbon nanotube / molybdenum disulfide composite material, 3-6 parts of reinforcing fiber and 2-5 parts of carbon black.
[0007] Preferably, the preparation method of the modified carbon nanotube / molybdenum disulfide composite material comprises the following steps:
[0008] S1, preparing a carbon nanotube aqueous dispersion;
[0009] S2, mixing the carbon nanotube aqueous dispersion with ammonium molybdate tetrahydrate and thiourea, and preparing a carbon nanotube / molybdenum disulfide composite material through a hydrothermal reaction;
[0010] S3. Using γ-aminopropyltriethoxysilane to perform surface modification on the carbon nanotube / molybdenum disulfide composite material to obtain the modified carbon nanotube / molybdenum disulfide composite material.
[0011] Preferably, in step S1, the concentration of the carbon nanotube aqueous dispersion is 20-60 mg / mL;
[0012] The method for preparing the carbon nanotube aqueous dispersion comprises the following steps:
[0013] The multi-walled carbon nanotubes are placed in a mixed acid solution, wherein the mixed acid solution is composed of concentrated nitric acid and concentrated sulfuric acid mixed in a volume ratio of 1:2-3; ultrasonic treatment is performed for 1-2 hours, and then the temperature is raised to 70-75°C while stirring, and stirred for 4-5 hours, and then diluted with water, filtered, and washed to obtain pretreated carbon nanotubes; the pretreated carbon nanotubes are placed in water and ultrasonically treated for 2-4 hours to prepare the carbon nanotube aqueous dispersion.
[0014] Preferably, the step S2 specifically includes the following steps:
[0015] Adding ammonium molybdate tetrahydrate and thiourea to the carbon nanotube aqueous dispersion, stirring and mixing, transferring the resulting solution to a reactor, sealing the reactor, and then performing a hydrothermal reaction at 200-210° C. for 15-20 hours; after the hydrothermal reaction is completed, cooling to room temperature, filtering, washing, and vacuum drying to obtain a carbon nanotube / molybdenum disulfide composite material;
[0016] The mass volume ratio of the carbon nanotube aqueous dispersion to ammonium molybdate tetrahydrate and thiourea is 100 mL: 4.5-5 g: 7.5-8 g.
[0017] Preferably, the step S3 specifically includes the following steps:
[0018] The carbon nanotube / molybdenum disulfide composite material and γ-aminopropyltriethoxysilane are placed in ethanol, heated to 70-75° C., refluxed and stirred for 10-15 hours, then cooled to room temperature, filtered, and dried to obtain the modified carbon nanotube / molybdenum disulfide composite material;
[0019] The mass volume ratio of the carbon nanotube / molybdenum disulfide composite material, γ-aminopropyltriethoxysilane and ethanol is 10g: 0.2-0.5g: 100-150mL.
[0020] Preferably, the reinforcing fiber is modified basalt fiber; the preparation method of the modified basalt fiber comprises the following steps:
[0021] 1) The basalt fiber is first immersed in hydrochloric acid with a concentration of 0.2-0.5 mol / L for 30-60 min, and then immersed in a sodium hydroxide solution with a concentration of 0.2-0.5 mol / L for 30-60 min, and then filtered, washed with water, dried, and then heated to 250-300° C. and calcined for 30-55 min to obtain pretreated basalt fiber;
[0022] 2) adding ethanol and γ-aminopropyltriethoxysilane to water, stirring and mixing, and then adding the pretreated basalt fiber, and then heating to 50-55° C. while stirring, and stirring at a constant temperature for 3.5-5 hours, and then filtering, washing with water, and drying to obtain the modified basalt fiber.
[0023] Preferably, in step 1), the basalt fiber has a length of 5-6 mm and a diameter of 14-15 μm;
[0024] In step 2), the mass volume ratio of the water, ethanol, γ-aminopropyltriethoxysilane and pretreated basalt fiber is 10-15 mL: 60-80 mL: 0.7-1 g: 10 g.
[0025] Preferably, the particle size of the polyetheretherketone is 20-50 μm.
[0026] As a general inventive concept, the present invention provides a method for preparing a lubricating and wear-resistant bearing bush, comprising the following steps:
[0027] Weigh each raw material according to the ratio, then place each raw material in a high-speed mixer and mix them evenly to obtain a mixture; first place the mixture in a mold for cold pressing; then place the mixture in a mold for hot pressing, and after demolding, the lubricating and wear-resistant bearing shell is obtained.
[0028] Preferably, the molding pressure of the cold press molding is 15-20MPa, and the holding time is 20-30min; during the hot press molding, the mold is first heated to 220-230°C, and kept warm and pressed at a pressure of 10-15MPa for 30-40min, then heated to 380-395°C, and kept warm and pressed at a pressure of 20-25MPa for 30-40min, then cooled to 340-345°C, and kept warm and pressed at a pressure of 30-35MPa for 50-60min, then cooled to 240-245°C, and kept warm and pressed at a pressure of 40-45MPa for 50-60min, and then cooled to room temperature.
[0029] The beneficial effects of the present invention are:
[0030] The present invention uses polyetheretherketone as a matrix to prepare the bearing, and on this basis, adds an appropriate amount of modified carbon nanotube / molybdenum disulfide composite material, in which the carbon nanotube is the core and the molybdenum disulfide is the outer coating layer. The molybdenum disulfide with the outer layer structure of the carbon nanotube is very easy to slide relative to each other during the friction process, so that the bearing can form a stable transfer film during the friction process, thereby effectively improving the wear resistance of the bearing. The core carbon nanotube with high strength and high rigidity can effectively improve the mechanical properties of the bearing, and the improvement of the mechanical properties is conducive to improving the wear resistance of the bearing, and the carbon nanotubes in the polyetheretherketone matrix can also effectively disperse the stress concentration caused by the friction process and inhibit crack propagation. When the present invention prepares the modified carbon nanotube / molybdenum disulfide composite material, molybdenum disulfide is compounded with carbon nanotubes, and further modified with γ-aminopropyltriethoxysilane, so that the obtained modified carbon nanotube / molybdenum disulfide composite material has excellent dispersibility in polyetheretherketone, thereby effectively exerting its performance. In addition, the use of carbon nanotubes treated with strong acid in the preparation of composite materials can make the composite materials more effective in modifying polyetheretherketone. This may be because the surface roughness of the carbon nanotubes treated with strong acid is enhanced and the number of surface active groups increases, which improves the coating effect of molybdenum disulfide on the surface of the carbon nanotubes.
[0031] When preparing the bearing bushing according to the present invention, in addition to using the modified carbon nanotube / molybdenum disulfide composite material for modification, a certain amount of reinforcing fiber (modified basalt fiber) is also added. After the basalt fiber is treated with acid and alkali, combined with roasting and γ-aminopropyltriethoxysilane modification, it can have a high dispersibility in polyetheretherketone and is tightly combined with polyetheretherketone, thereby effectively enhancing the strength of the bearing bushing and further enhancing the wear resistance of the bearing bushing.
[0032] The present invention selects polyetheretherketone, modified carbon nanotube / molybdenum disulfide composite material, reinforcing fiber, and carbon black as preparation raw materials, reasonably sets the addition amount of each component, and combines a suitable method to prepare the bearing. The prepared bearing has excellent lubrication and wear resistance, and has higher strength and strong bearing capacity as a whole, so that the bearing has stronger performance and longer service life. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Embodiment 1:
[0035] A lubricating and wear-resistant bearing bush comprises the following raw materials in parts by weight: 100 parts of polyetheretherketone, 4.5 parts of modified carbon nanotube / molybdenum disulfide composite material, 4 parts of modified basalt fiber, and 5 parts of carbon black.
[0036] The particle size of polyetheretherketone is 20-50 μm; the particle size of carbon black is 10-30 μm.
[0037] The preparation method of the modified carbon nanotube / molybdenum disulfide composite material comprises the following steps:
[0038] S1. Place multi-walled carbon nanotubes in a mixed acid solution, which is composed of concentrated nitric acid and concentrated sulfuric acid mixed in a volume ratio of 1:3; ultrasonically treat for 2 hours, then heat to 75°C while stirring, stir for 5 hours, then dilute with water, filter, and wash to obtain pretreated carbon nanotubes; place the pretreated carbon nanotubes in water and ultrasonically treat for 3 hours to prepare a carbon nanotube aqueous dispersion with a concentration of 50 mg / mL.
[0039] S2. Add ammonium molybdate tetrahydrate and thiourea to a 50 mg / mL carbon nanotube aqueous dispersion, stir and mix, transfer the resulting solution to a reactor, seal the reactor, and then conduct a hydrothermal reaction at 210°C for 18 hours. After the hydrothermal reaction, cool to room temperature, filter, wash, and vacuum dry to obtain a carbon nanotube / molybdenum disulfide composite material. The mass volume ratio of the carbon nanotube aqueous dispersion to ammonium molybdate tetrahydrate and thiourea is 100 mL: 5 g: 8 g.
[0040] S3. Place the carbon nanotube / molybdenum disulfide composite material and γ-aminopropyltriethoxysilane in ethanol, heat to 75°C, reflux with stirring for 13 hours, then cool to room temperature, filter and dry to obtain a modified carbon nanotube / molybdenum disulfide composite material; wherein the mass volume ratio of the carbon nanotube / molybdenum disulfide composite material, γ-aminopropyltriethoxysilane and ethanol is 10g:0.5g:100mL.
[0041] The preparation method of modified basalt fiber comprises the following steps:
[0042] 1) basalt fiber (length 5-6 mm, diameter 14-15 μm) is first immersed in 0.5 mol / L hydrochloric acid for 50 min, then immersed in 0.5 mol / L sodium hydroxide solution for 30 min, then filtered, washed with water, dried, and then heated to 280° C. and calcined for 50 min to obtain pretreated basalt fiber;
[0043] 2) Add ethanol and γ-aminopropyltriethoxysilane to water, stir and mix, then add pretreated basalt fiber, then heat to 55°C while stirring, and stir at constant temperature for 3.5 hours, then filter, wash and dry to obtain modified basalt fiber. The mass volume ratio of water, ethanol, γ-aminopropyltriethoxysilane and pretreated basalt fiber is 15mL:70mL:1g:10g.
[0044] The method for preparing the lubricating and wear-resistant bearing bush in this embodiment comprises the following steps:
[0045] (1) Weighing various raw materials according to the proportion, and then placing the various raw materials in a high-speed mixer and mixing them uniformly to obtain a mixture;
[0046] (2) The mixed material is first placed in a mold for cold pressing, the molding pressure of the cold pressing molding is 20 MPa, and the holding time is 25 minutes; then the mixed material is placed in the mold for hot pressing molding, during hot pressing molding, the mold is first heated to 220°C and kept at a pressure of 15 MPa for 40 minutes, then heated to 395°C and kept at a pressure of 20 MPa for 35 minutes, then cooled to 340°C and kept at a pressure of 35 MPa for 50 minutes, then cooled to 240°C and kept at a pressure of 45 MPa for 50 minutes, and then cooled to room temperature; after demolding, the lubricating and wear-resistant bearing shell is obtained.
[0047] Embodiment 2:
[0048] A lubricating and wear-resistant bearing bush comprises the following raw materials in parts by weight: 100 parts of polyetheretherketone, 4.5 parts of modified carbon nanotube / molybdenum disulfide composite material, 5.5 parts of modified basalt fiber and 3 parts of carbon black.
[0049] The particle size of polyetheretherketone is 20-50 μm; the particle size of carbon black is 10-30 μm.
[0050] The preparation method of the modified carbon nanotube / molybdenum disulfide composite material comprises the following steps: S1, placing multi-walled carbon nanotubes in a mixed acid solution, the mixed acid solution being composed of concentrated nitric acid and concentrated sulfuric acid mixed in a volume ratio of 1:2; ultrasonically treating for 1 hour, then heating to 70°C while stirring, stirring for 5 hours, then diluting with water, filtering, and washing to obtain pretreated carbon nanotubes; placing the pretreated carbon nanotubes in water and ultrasonically treating for 2 hours to prepare a carbon nanotube aqueous dispersion with a concentration of 30 mg / mL.
[0051] S2. Add ammonium molybdate tetrahydrate and thiourea to a 30 mg / mL carbon nanotube aqueous dispersion, stir and mix, transfer the resulting solution to a reactor, seal the reactor, and then perform a hydrothermal reaction at 200°C for 20 hours. After the hydrothermal reaction, cool to room temperature, filter, wash, and vacuum dry to obtain a carbon nanotube / molybdenum disulfide composite material. The mass volume ratio of the carbon nanotube aqueous dispersion to ammonium molybdate tetrahydrate and thiourea is 100 mL: 4.5 g: 7.5 g.
[0052] S3. Place the carbon nanotube / molybdenum disulfide composite material and γ-aminopropyltriethoxysilane in ethanol, heat to 72°C, reflux with stirring for 10 hours, then cool to room temperature, filter and dry to obtain a modified carbon nanotube / molybdenum disulfide composite material; wherein the mass volume ratio of the carbon nanotube / molybdenum disulfide composite material, γ-aminopropyltriethoxysilane and ethanol is 10g:0.2g:100mL.
[0053] The preparation method of modified basalt fiber comprises the following steps:
[0054] 1) basalt fiber (length 5-6 mm, diameter 14-15 μm) is first immersed in 0.3 mol / L hydrochloric acid for 60 min, then immersed in 0.2 mol / L sodium hydroxide solution for 30 min, then filtered, washed with water, dried, and then heated to 265° C. and calcined for 35 min to obtain pretreated basalt fiber;
[0055] 2) Add ethanol and γ-aminopropyltriethoxysilane to water, stir and mix, then add pretreated basalt fiber, then heat to 55°C while stirring, and stir at constant temperature for 5 hours, then filter, wash and dry to obtain modified basalt fiber. The mass volume ratio of water, ethanol, γ-aminopropyltriethoxysilane and pretreated basalt fiber is 10mL:80mL:0.8g:10g.
[0056] The method for preparing the lubricating and wear-resistant bearing bush in this embodiment comprises the following steps:
[0057] (1) Weighing various raw materials according to the proportion, and then placing the various raw materials in a high-speed mixer and mixing them uniformly to obtain a mixture;
[0058] (2) The mixed material is first placed in a mold for cold pressing, the molding pressure of the cold pressing molding is 20 MPa, and the holding time is 20 minutes; then the mixed material is placed in the mold for hot pressing molding, during hot pressing molding, the mold is first heated to 230°C and kept at this temperature for 35 minutes at a pressure of 10 MPa, then heated to 385°C and kept at this temperature for 30 minutes at a pressure of 25 MPa, then cooled to 340°C and kept at this temperature for 60 minutes at a pressure of 30 MPa, then cooled to 240°C and kept at this temperature for 60 minutes at a pressure of 45 MPa, and then cooled to room temperature; after demolding, the lubricating and wear-resistant bearing shell is obtained.
[0059] Embodiment 3:
[0060] A lubricating and wear-resistant bearing bush comprises the following raw materials in parts by weight: 100 parts of polyetheretherketone, 3.5 parts of modified carbon nanotube / molybdenum disulfide composite material, 3 parts of modified basalt fiber, and 5 parts of carbon black.
[0061] The particle size of polyetheretherketone is 20-50 μm; the particle size of carbon black is 10-30 μm.
[0062] The preparation method of the modified carbon nanotube / molybdenum disulfide composite material is the same as that of Example 1; the preparation method of the modified basalt fiber is the same as that of Example 1.
[0063] The method for preparing the lubricating and wear-resistant bearing bush in this embodiment comprises the following steps:
[0064] (1) Weighing various raw materials according to the proportion, and then placing the various raw materials in a high-speed mixer and mixing them uniformly to obtain a mixture;
[0065] (2) The mixed material is first placed in a mold for cold pressing, the molding pressure of the cold pressing molding is 15 MPa, and the holding time is 30 minutes; then the mixed material is placed in the mold for hot pressing molding, during hot pressing molding, the mold is first heated to 225°C and kept at a pressure of 15 MPa for 30 minutes, then heated to 380°C and kept at a pressure of 25 MPa for 40 minutes, then cooled to 345°C and kept at a pressure of 35 MPa for 55 minutes, then cooled to -245°C and kept at a pressure of 40 MPa for 55 minutes, and then cooled to room temperature; after demolding, the lubricating and wear-resistant bearing shell is obtained.
[0066] Embodiment 4:
[0067] A lubricating and wear-resistant bearing bush comprises the following raw materials in parts by weight: 100 parts of polyetheretherketone, 5 parts of modified carbon nanotube / molybdenum disulfide composite material, 5.5 parts of modified basalt fiber and 2 parts of carbon black.
[0068] The particle size of polyetheretherketone is 20-50 μm; the particle size of carbon black is 10-30 μm.
[0069] The preparation method of the modified carbon nanotube / molybdenum disulfide composite material is the same as that of Example 1; the preparation method of the modified basalt fiber is the same as that of Example 2.
[0070] The preparation method of the lubricating and wear-resistant bearing bushing in this embodiment is the same as that in Embodiment 3.
[0071] Embodiment 5:
[0072] A lubricating and wear-resistant bearing bush comprises the following raw materials in parts by weight: 100 parts of polyetheretherketone, 3.5 parts of modified carbon nanotube / molybdenum disulfide composite material, 6 parts of modified basalt fiber, and 4.5 parts of carbon black.
[0073] The particle size of polyetheretherketone is 20-50 μm; the particle size of carbon black is 10-30 μm.
[0074] The preparation method of the modified carbon nanotube / molybdenum disulfide composite material is the same as that of Example 2; the preparation method of the modified basalt fiber is the same as that of Example 2.
[0075] The preparation method of the lubricating and wear-resistant bearing bushing in this embodiment is the same as that in Embodiment 2.
[0076] Comparative Example 1:
[0077] The difference from Example 5 is that the modified carbon nanotube / molybdenum disulfide composite material is replaced by modified carbon nanotubes and modified molybdenum disulfide in a mass ratio of 1:2.
[0078] The method for preparing modified carbon nanotubes comprises the following steps:
[0079] Pretreated carbon nanotubes were prepared according to the method in step S2 of Example 2; the pretreated carbon nanotubes and γ-aminopropyltriethoxysilane were placed in ethanol, heated to 72°C, refluxed with stirring for 10 hours, then cooled to room temperature, filtered, and dried to obtain modified carbon nanotubes; wherein the mass volume ratio of the pretreated carbon nanotubes, γ-aminopropyltriethoxysilane, and ethanol was 10g:0.2g:100mL.
[0080] The preparation method of modified molybdenum disulfide comprises the following steps:
[0081] Add ammonium molybdate tetrahydrate and thiourea to water, stir and mix, transfer the resulting solution to a reactor, seal the reactor, and then carry out a hydrothermal reaction at 200°C for 20 hours. After the hydrothermal reaction, cool to room temperature, filter, wash, and vacuum dry to obtain molybdenum disulfide. The mass volume ratio of water to ammonium molybdate tetrahydrate and thiourea is 100 mL: 4.5 g: 7.5 g.
[0082] The molybdenum disulfide and γ-aminopropyltriethoxysilane are placed in ethanol, heated to 72° C., refluxed with stirring for 10 hours, then cooled to room temperature, filtered, and dried to obtain modified molybdenum disulfide; wherein the mass volume ratio of molybdenum disulfide, γ-aminopropyltriethoxysilane, and ethanol is 10 g:0.2 g:100 mL.
[0083] Comparative Example 2:
[0084] Different from Comparative Example 1, the method for preparing modified carbon nanotubes comprises the following steps:
[0085] The unpretreated carbon nanotubes and γ-aminopropyltriethoxysilane were placed in ethanol, heated to 72°C, refluxed with stirring for 10 hours, then cooled to room temperature, filtered, and dried to obtain modified carbon nanotubes; wherein the mass volume ratio of the carbon nanotubes, γ-aminopropyltriethoxysilane, and ethanol was 10g:0.2g:100mL.
[0086] Comparative Example 3:
[0087] The difference from Example 5 is that the modified basalt fiber is replaced by unmodified basalt fiber (with a length of 5-6 mm and a diameter of 14-15 μm).
[0088] Performance Testing:
[0089] The wear-resistant test specimens of bearing materials were prepared by the methods in Examples 1-5 of the present invention and Comparative Examples 1-3, and the friction coefficients of the specimens under dry friction conditions, seawater lubrication conditions, and oil lubrication conditions were measured. Test parameters: load F = 100N, rotation speed n = 200r / min, test duration t = 60min. In addition, the tensile strength test specimens of bearing materials were prepared by the methods in Examples 1-5 of the present invention and Comparative Examples 1-3, and the tensile strength was tested according to the method in ASTM D638. The specific test results are shown in Table 1.
[0090] Table 1 Performance test results
[0091]
[0092] It can be seen from the test data of Examples 1-5 in Table 1 that the modified carbon nanotube / molybdenum disulfide composite material, modified basalt fiber, etc. are used to modify polyetheretherketone, so that the obtained bearing bush has excellent lubrication and wear resistance, and at the same time, the tensile strength is relatively high. And from the comparison between Comparative Example 1 and Example 5, it can be seen that if the modified carbon nanotube / molybdenum disulfide composite material is replaced by modified carbon nanotubes and modified molybdenum disulfide, its tensile strength and wear resistance will be reduced. It can be seen that after carbon nanotubes and molybdenum disulfide are compounded to prepare the modified carbon nanotube / molybdenum disulfide composite material, the two can show a good synergistic effect, and have a better modification effect on polyetheretherketone. From the comparison between Comparative Example 2 and Comparative Example 1, it can be seen that the pretreatment of carbon nanotubes in the present invention can also improve the strength and wear resistance of the bearing. It may be that the surface properties of the carbon nanotubes are improved after the pretreatment, which further improves the subsequent coating of molybdenum disulfide on the surface of the carbon nanotubes, so that the modified carbon nanotube / molybdenum disulfide composite material exhibits a better synergistic effect. From the comparison between Comparative Example 3 and Example 5, it can be seen that the modification of basalt fiber can also improve the wear resistance and strength of the bearing.
[0093] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A lubricating and wear-resistant bearing bushing, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of polyetheretherketone, 3.5-5 parts of modified carbon nanotube / molybdenum disulfide composite material, 3-6 parts of reinforcing fiber and 2-5 parts of carbon black.
2. The lubricating and wear-resistant bearing bushing according to claim 1, characterized in that: The preparation method of the modified carbon nanotube / molybdenum disulfide composite material comprises the following steps: S1, preparing a carbon nanotube aqueous dispersion; S2, mixing the carbon nanotube aqueous dispersion with ammonium molybdate tetrahydrate and thiourea, and preparing a carbon nanotube / molybdenum disulfide composite material through a hydrothermal reaction; S3. Using γ-aminopropyltriethoxysilane to perform surface modification on the carbon nanotube / molybdenum disulfide composite material to obtain the modified carbon nanotube / molybdenum disulfide composite material.
3. The lubricating and wear-resistant bearing bushing according to claim 2, characterized in that: In the step S1, the concentration of the carbon nanotube aqueous dispersion is 20-60 mg / mL; The method for preparing the carbon nanotube aqueous dispersion comprises the following steps: The multi-walled carbon nanotubes are placed in a mixed acid solution, wherein the mixed acid solution is composed of concentrated nitric acid and concentrated sulfuric acid mixed in a volume ratio of 1:2-3; ultrasonic treatment is performed for 1-2 hours, and then the temperature is raised to 70-75°C while stirring, and stirred for 4-5 hours, and then diluted with water, filtered, and washed to obtain pretreated carbon nanotubes; the pretreated carbon nanotubes are placed in water and ultrasonically treated for 2-4 hours to prepare the carbon nanotube aqueous dispersion.
4. The lubricating and wear-resistant bearing bushing according to claim 2, characterized in that: The step S2 specifically includes the following steps: Adding ammonium molybdate tetrahydrate and thiourea to the carbon nanotube aqueous dispersion, stirring and mixing, transferring the resulting solution to a reactor, sealing the reactor, and then performing a hydrothermal reaction at 200-210° C. for 15-20 hours; after the hydrothermal reaction is completed, cooling to room temperature, filtering, washing, and vacuum drying to obtain a carbon nanotube / molybdenum disulfide composite material; The mass volume ratio of the carbon nanotube aqueous dispersion to ammonium molybdate tetrahydrate and thiourea is 100 mL: 4.5-5 g: 7.5-8 g.
5. The lubricating and wear-resistant bearing bushing according to claim 2, characterized in that: The step S3 specifically comprises the following steps: The carbon nanotube / molybdenum disulfide composite material and γ-aminopropyltriethoxysilane are placed in ethanol, heated to 70-75° C., refluxed and stirred for 10-15 hours, then cooled to room temperature, filtered, and dried to obtain the modified carbon nanotube / molybdenum disulfide composite material; The mass volume ratio of the carbon nanotube / molybdenum disulfide composite material, γ-aminopropyltriethoxysilane and ethanol is 10g: 0.2-0.5g: 100-150mL.
6. The lubricating and wear-resistant bearing bushing according to claim 1, characterized in that: The reinforcing fiber is modified basalt fiber; the preparation method of the modified basalt fiber comprises the following steps: 1) The basalt fiber is first immersed in hydrochloric acid with a concentration of 0.2-0.5 mol / L for 30-60 min, and then immersed in a sodium hydroxide solution with a concentration of 0.2-0.5 mol / L for 30-60 min, and then filtered, washed with water, dried, and then heated to 250-300° C. and calcined for 30-55 min to obtain pretreated basalt fiber; 2) adding ethanol and γ-aminopropyltriethoxysilane to water, stirring and mixing, and then adding the pretreated basalt fiber, and then heating to 50-55° C. while stirring, and stirring at a constant temperature for 3.5-5 hours, and then filtering, washing with water, and drying to obtain the modified basalt fiber.
7. The lubricating and wear-resistant bearing bushing according to claim 6, characterized in that: In step 1), the basalt fiber has a length of 5-6 mm and a diameter of 14-15 μm; In step 2), the mass volume ratio of the water, ethanol, γ-aminopropyltriethoxysilane and pretreated basalt fiber is 10-15 mL: 60-80 mL: 0.7-1 g: 10 g.
8. The lubricating and wear-resistant bearing bushing according to claim 1, characterized in that: The particle size of the polyetheretherketone is 20-50 μm.
9. A method for preparing a lubricating and wear-resistant bearing bush according to any one of claims 1 to 8, characterized in that: The following steps are involved: Weigh each raw material according to the ratio, then place each raw material in a high-speed mixer and mix them evenly to obtain a mixture; first place the mixture in a mold for cold pressing; then place the mixture in a mold for hot pressing, and after demolding, the lubricating and wear-resistant bearing shell is obtained.
10. The preparation method according to claim 9, characterized in that: The molding pressure of the cold press molding is 15-20MPa, and the holding time is 20-30min. During the hot press molding, the mold is first heated to 220-230°C, and kept warm and pressed for 30-40min at a pressure of 10-15MPa, then heated to 380-395°C, and kept warm and pressed for 30-40min at a pressure of 20-25MPa, then cooled to 340-345°C, and kept warm and pressed for 50-60min at a pressure of 30-35MPa, then cooled to 240-245°C, and kept warm and pressed for 50-60min at a pressure of 40-45MPa, and then cooled to room temperature.
Citation Information
Cited By
Molybdenum disulfide nanoflower-carbon nanotube-polyether-ether-ketone composite material and preparation method thereof
CN119735936A
A molybdenum disulfide nanoflower-carbon nanotube-polyether ether ketone composite material and a preparation method thereof
CN119735936B
Molybdenum disulfide nanotube-carbon nanotube-polyether-ether-ketone composite material and preparation method thereof
CN119735937A
A molybdenum disulfide nanotube-carbon nanotube-polyether ether ketone composite material and a preparation method thereof
CN119735937B