A method for preparing lithium fluoride

The preparation process of lithium fluoride is simplified through ultrasonic dispersion technology, and the problems of complex processes, waste resources and low purity in the existing processes are solved, and efficient and environmentally friendly preparation of lithium fluoride is achieved, which improves lithium yield and purity, and through Hydrochloric acid recycling reduces waste acid emissions.

CN113697829BActive Publication Date: 2024-12-03JIANGSU RONGHUI GENERAL LITHIUM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111040962.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-07
Publication Date
2024-12-03
Estimated Expiration
2041-09-07

AI Technical Summary

Technical Problem

The existing process methods for preparing lithium fluoride in liquid phase reactions have problems such as long process routes, many steps, waste of lithium resources, waste of energy and water, high production costs and low product purity.

Method used

Ultrasonic dispersion technology is used to react lithium sulfate solution with calcium chloride, sodium carbonate, etc. to form lithium chloride mother liquor, and then react with hydrofluoric acid to prepare lithium fluoride, eliminating the process of lithium carbonate or lithium hydroxide, and simplifying the process. The reaction conversion rate and lithium yield are improved, and waste acid emissions are reduced through hydrochloric acid recycling.

Benefits of technology

The process route is significantly shortened, energy consumption and water consumption are reduced, the purity and lithium yield of lithium are improved, and the green circulation process is realized, reducing lithium losses and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113697829B_ABST
    Figure CN113697829B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing lithium fluoride, comprising: (1) ultrasonically treating a lithium sulfate solution, adding calcium chloride to carry out ultrasonic stirring reaction, separating and washing to obtain a lithium chloride mother liquor 1 and a byproduct calcium sulfate; (2) ultrasonically treating a lithium sulfate solution, adding sodium carbonate to carry out ultrasonic stirring reaction, separating and washing to obtain lithium carbonate and a byproduct sodium sulfate; (3) reacting the lithium carbonate obtained in step (2) with the hydrochloric acid obtained in step (5), separating and washing to obtain a lithium chloride mother liquor 2; (4) removing impurities and purifying the lithium chloride mother liquor to obtain a lithium chloride purified liquid; (5) reacting the lithium chloride purified liquid with hydrofluoric acid, drying the lithium fluoride wet crystal obtained by separation and washing to obtain a finished product lithium fluoride, and removing the hydrochloric acid obtained by step (3) for recycling. The invention effectively improves the conversion rate of the reaction and the yield of lithium, shortens the process, simplifies the steps, reduces energy consumption, has no waste acid or wastewater discharge, and all byproducts are comprehensively utilized, and is a green recycling process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing lithium fluoride. Background Art

[0002] The existing process for preparing lithium fluoride by liquid phase reaction is to use finished lithium carbonate and lithium hydroxide as lithium sources and react with hydrofluoric acid, sodium fluoride, ammonium fluoride, potassium fluoride, etc. to prepare lithium fluoride.

[0003] However, this type of process has many disadvantages. First, the lithium ore leaching solution - lithium sulfate solution must undergo a series of processes such as reaction, washing and filtration, impurity removal, concentration, cooling and separation, and drying to produce finished lithium carbonate, lithium hydroxide or lithium sulfate. Therefore, the long process route and many steps increase the loss of lithium in the process, reduce the total yield of lithium, and cause a waste of precious lithium resources. Second, after repeated washing, concentration, cooling and crystallization, energy and water are wasted and a large amount of wastewater is generated; third, the production line is too long, the equipment investment is large, the operation process is complicated, the operating expenses are high, and the production cost is high.

[0004] The invention patent with application number 201410229271.4 discloses a process for producing lithium fluoride from spodumene concentrate, which comprises preparing lithium fluoride by reacting lithium sulfate leaching solution with sodium fluoride, ammonium fluoride or potassium fluoride after a series of steps including purification, evaporation concentration, filtration and impurity removal.

[0005] The invention first uses 50% NaOH solution to adjust the pH value of lithium sulfate leaching solution to 12 and then adds Na2CO3 to react and filter to remove Ca ++ After evaporation and concentration, it is filtered to remove impurities. Adding NaOH and Na2CO3 will cause a large amount of Na + The introduction of sodium fluoride into the lithium sulfate solution not only increases the difficulty of impurity removal, is not conducive to the improvement of the purity of lithium fluoride, but also increases the energy consumption of the process; the invention uses lithium sulfate and sodium fluoride, ammonium fluoride or potassium fluoride to react in solution to generate lithium fluoride, but the solubility of lithium sulfate is low and decreases with increasing temperature, so the reaction conversion rate and lithium yield are low. The addition of sodium fluoride, ammonium fluoride or potassium fluoride will inevitably bring a large amount of difficult-to-remove Na into the reaction system. + , K + and NH4 + , reducing the purity of the target product. In addition, NaF has great harm to the environment. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing lithium fluoride which is environmentally friendly, has simple procedures, high reaction conversion rate and lithium yield, and high product purity.

[0007] The technical solution of the present invention is:

[0008] A method for preparing lithium fluoride, characterized in that it comprises the following steps:

[0009] (1) ultrasonically dispersing a lithium sulfate solution, adding calcium chloride to the lithium sulfate solution for sufficient reaction, separating and washing the resulting product to obtain a lithium chloride mother solution 1, and placing the resulting lithium chloride mother solution 1 in a lithium chloride mother solution storage tank for standby use;

[0010] (2) ultrasonically dispersing a lithium sulfate solution, adding sodium carbonate to the lithium sulfate solution for sufficient reaction, and separating and washing the resulting product to obtain lithium carbonate;

[0011] (3) reacting the lithium carbonate obtained in step (2) with hydrochloric acid, separating and washing to obtain a lithium chloride mother liquor 2, and placing the obtained lithium chloride mother liquor 2 in the LiCl mother liquor storage tank described in step (1) for standby use;

[0012] (4) Purification of lithium chloride mother liquor: ultrasonically dispersing the lithium chloride mother liquor in the mother liquor storage tank, adding lithium carbonate to the lithium chloride mother liquor for sufficient reaction, and then separating and washing to remove the impurities remaining in the mother liquor to obtain a purified lithium chloride solution;

[0013] (5) placing the purified lithium chloride solution into a polytetrafluoroethylene reactor, adding a measured amount of hydrofluoric acid, allowing the lithium chloride and hydrofluoric acid to fully react at room temperature, and then separating and washing to obtain wet lithium fluoride crystals; drying and packaging the wet lithium fluoride crystals to obtain finished lithium fluoride; and the obtained hydrochloric acid is recycled to step (3).

[0014] The lithium sulfate solution in step (1) and step (2) is a lithium ore leaching solution - lithium sulfate solution.

[0015] The preparation method of lithium fluoride comprises the following specific steps:

[0016] (1) slowly adding calcium chloride to a lithium sulfate solution and stirring the solution while performing ultrasonication to react, wherein the molar ratio of the reactants CaCl2 / Li2SO4 is 1.05 to 1.08, the reaction temperature is 80 to 90° C., reacting for 25 to 35 minutes, then keeping the solution warm for 30 minutes or more, filtering and separating the obtained product, and washing the product with deionized hot water at 80° C. or above to obtain a lithium chloride mother solution 1 and a by-product calcium sulfate;

[0017] (2) slowly adding sodium carbonate to the lithium sulfate solution and stirring the solution while ultrasonicating to react, wherein the molar ratio of reactants Na2CO3 / Li2SO4 is 1.01-1.05, the reaction temperature is 40-50°C, and the reaction time is 25-35 minutes; after the reaction is completed, heating to 80-85°C and keeping the temperature for 40 minutes or more to precipitate lithium carbonate and filtering and separating the lithium carbonate while hot, washing with deionized hot water at 80°C or above to obtain lithium carbonate and a by-product sodium sulfate mother liquor;

[0018] (3) slowly adding the lithium carbonate obtained in step (2) to the hydrochloric acid obtained in step (5) in batches, with a reactant molar ratio of HCl / Li2CO3 of 2.02 to 2.08, reacting at room temperature for 30 to 40 minutes;

[0019] (4) After preparing a lithium carbonate solution and ultrasonically dispersing it for 10 to 20 minutes, the lithium carbonate solution is added to the lithium chloride mother liquor, reacted at room temperature for 25 minutes or more, and then separated and washed; the amount of lithium carbonate added is based on the amount of Ca in the lithium chloride mother liquor. 2+ , Ba 2+ Mg 2+ 、Al 3+ Depends on the total content of impurities;

[0020] (5) Place the purified lithium chloride solution into a polytetrafluoroethylene reactor, add a measured amount of hydrofluoric acid while stirring, react at room temperature for 20 minutes or more, separate and wash with deionized hot water at 35° C. or above, and the molar ratio of the reactants HF / LiCl is 1.01 to 1.03.

[0021] The present invention eliminates the entire process of preparing or producing lithium carbonate or lithium hydroxide from a lithium sulfate solution, thereby greatly shortening the process route, greatly simplifying the operation steps, reducing energy consumption and water consumption, and reducing lithium loss in the process. The high solubility of lithium chloride and its favorable properties for liquid phase reaction are scientifically utilized, and the "three transmissions and one reaction" are strengthened by ultrasonic technology, so that the conversion rate and lithium yield of the reaction are significantly improved. The hydrochloric acid produced in the preparation process of lithium fluoride is recycled, and no waste acid or wastewater is discharged. The evaporation and concentration process is eliminated, and the energy-saving benefits are extremely significant. The present invention is a green circulation process technology, which realizes the innovation of the preparation method of lithium fluoride. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0023] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0024] Example 1

[0025] (1) 800 ml of lithium sulfate solution with a Li2O content of 55 g / L was transferred into a reactor and ultrasonically dispersed for 20 minutes. Then, 179 g of calcium chloride was slowly added while ultrasonically stirring. The mixture was kept at 80°C for 25 minutes and then kept at this temperature for 30 minutes. The obtained product was vacuum filtered and the calcium sulfate filter cake was washed twice with 85°C deionized water to obtain LiCl mother solution 1.

[0026] (2) The LiCl mother solution 1 obtained in step (1) was ultrasonically dispersed for 10 minutes, and the prepared 0.18 mol / L lithium carbonate solution was ultrasonically dispersed for 10 minutes. Then 30 ml was added to the LiCl mother solution 1 and stirred for 25 minutes. The solution was centrifuged and washed with deionized water at room temperature to obtain a purified LiCl solution.

[0027] (3) The purified LiCl solution obtained in step (2) is placed in a polytetrafluoroethylene reactor, and 130 ml of a measured HF solution is added while stirring. The mixture is stirred at room temperature for 20 minutes, and then centrifuged and washed twice with 35° C. deionized water to obtain wet crystals of lithium fluoride. The wet crystals of lithium fluoride are dried to obtain a lithium fluoride product. The purity of the product is 99.957% as determined by (XRD, ICP, GB / T22660-2008 "Chemical Analysis Methods for Lithium Fluoride"), and the total lithium yield is 95.686%.

[0028] The hydrochloric acid obtained by separation and washing is placed in a hydrochloric acid storage tank for recycling.

[0029] Example 2

[0030] (1) As in Example 1 (1), the obtained LiCl solution (mother solution 1) is placed in a LiCl mother solution storage tank.

[0031] (2) Take another 760 ml of the same lithium sulfate solution as step (1) and ultrasonically disperse it in a reactor for 20 minutes, then slowly add 156 g of sodium carbonate while stirring and ultrasonicating, and react at 40°C for 25 minutes. After the reaction is completed, heat to 80°C, keep it at room temperature for 40 minutes, filter it while hot, and wash it twice with 80°C deionized water to obtain Li2CO3. After washing, the Na2SO4 solution is used to prepare sodium sulfate decahydrate using our company's existing patented technology (200910024433.X).

[0032] (3) 1070 ml of hydrochloric acid was transferred from the hydrochloric acid storage tank into the reactor, and the Li2CO3 obtained in step (2) was slowly added in two portions while stirring. After fully reacting at room temperature for 30 minutes, the obtained LiCl mother solution 2 was added to the LiCl mother solution storage tank described in step (1).

[0033] (4) Take 60 ml of 0.18 mol / L lithium carbonate solution and ultrasonically disperse it for 20 minutes. At the same time, place the LiCl mother liquor in the LiCl mother liquor storage tank into the reactor and ultrasonically stir it for 15 minutes. Then, add the lithium carbonate solution to the LiCl mother liquor, stir and react for 30 minutes while ultrasonicating. Then, centrifuge and wash with ion-free water at room temperature to obtain a purified LiCl solution.

[0034] (5) The purified LiCl solution obtained in step (4) was placed in a polytetrafluoroethylene reactor, and 253 ml of the measured HF solution was added while stirring. After reacting at room temperature for 30 minutes, the mixture was centrifuged and washed twice with 40° C. deionized water. The wet crystals of lithium fluoride were dried to obtain a lithium fluoride product. The purity of the product was 99.955% and the total lithium yield was 95.752%.

[0035] The hydrochloric acid obtained by separation and washing is placed in a hydrochloric acid storage tank for recycling.

[0036] Example 3

[0037] (1) 800 ml of lithium sulfate solution with a Li2O content of 70 g / L was transferred to a reactor for ultrasonic dispersion for 25 minutes, and 230 g of calcium chloride was slowly added while stirring and ultrasonic dispersion. The mixture was fully reacted at 85°C for 30 minutes and then kept at this temperature for 40 minutes. The obtained product was vacuum filtered and the calcium sulfate filter cake was washed twice with 85°C deionized water. The obtained LiCl mother solution 1 was placed in a LiCl mother solution storage tank.

[0038] (2) Take 1167 ml of the same lithium sulfate solution as step (1) and ultrasonically disperse it in a reactor for 30 minutes, then slowly add 293 g of sodium carbonate while stirring and ultrasonicating, and fully react at 45°C for 30 minutes. After the reaction is completed, heat to 85°C, keep it warm and stand for 45 minutes, filter it while hot, and wash it twice with 85°C deionized water to obtain Li2CO3. The washed Na2SO4 solution is used to prepare sodium sulfate decahydrate.

[0039] (3) 2347 ml of hydrochloric acid in the hydrochloric acid storage tank was transferred into the reactor, and the Li2CO3 obtained in step (2) was slowly added in four portions while stirring. After fully reacting at room temperature for 40 minutes, the obtained LiCl mother solution 2 was added to the LiCl mother solution storage tank described in step (1).

[0040] (4) 110 ml of 0.18 mol / L lithium carbonate solution was transferred and ultrasonically dispersed for 20 minutes. Meanwhile, the LiCl mother solution in the LiCl mother solution storage tank was placed in the reactor and ultrasonically dispersed for 15 minutes. The lithium carbonate solution was then added to the LiCl mother solution. The mixture was stirred and reacted for 35 minutes while ultrasonicating. Impurities were separated by centrifugation and washed with ion-free water at room temperature to obtain a purified LiCl solution.

[0041] (5) The purified LiCl solution obtained in step (4) was placed in a polytetrafluoroethylene reactor, and 398 ml of the measured HF solution was added while stirring. After reacting at room temperature for 30 minutes, the mixture was centrifuged and washed twice with 40° C. deionized water. The lithium fluoride wet crystals were dried to obtain a lithium fluoride product. The purity of the product was 99.952% and the total lithium yield was 95.646%.

[0042] The hydrochloric acid obtained by filtering and washing is placed in a hydrochloric acid storage tank for recycling.

[0043] Example 4

[0044] (1) 800 ml of lithium sulfate solution with a Li2O content of 55 g / L was transferred to a reactor for ultrasonic dispersion for 25 minutes, and 179 g of calcium chloride was slowly added while ultrasonically dispersing and stirring. The mixture was kept at 90°C for a full reaction for 35 minutes and then kept at this temperature for 35 minutes. The obtained product was vacuum filtered and the calcium sulfate filter cake was washed twice with 90°C deionized water. The obtained LiCl mother solution 1 was placed in a LiCl mother solution storage tank.

[0045] (2) Take 893 ml of the same lithium sulfate solution as in step (1) and ultrasonically disperse it in a reactor for 25 minutes, then slowly add 178 g of sodium carbonate while stirring and ultrasonically dispersing it, and fully react it at 50°C for 35 minutes. After the reaction is completed, heat it to 85°C, keep it warm and let it stand for 45 minutes, filter it while hot, and wash it twice with 85°C deionized water to obtain Li2CO3 。 The washed Na2SO4 solution is used to prepare sodium sulfate decahydrate.

[0046] (3) 1900 ml of hydrochloric acid in the hydrochloric acid storage tank is transferred into the reactor, and the Li2CO3 obtained in step (2) is slowly added in three portions while stirring. After fully reacting at room temperature for 30 minutes, the obtained LiCl mother solution 2 is added into the LiCl mother solution storage tank described in step (1).

[0047] (4) 70 ml of 0.18 mol / L lithium carbonate solution was transferred and ultrasonically dispersed for 15 minutes. Meanwhile, the LiCl mother solution in the LiCl mother solution storage tank was placed in the reactor and ultrasonically dispersed for 15 minutes. The lithium carbonate solution was then added to the LiCl mother solution. The reaction was stirred while ultrasonicating for 30 minutes. Impurities were separated by centrifugation and washed with ion-free water at room temperature to obtain a purified LiCl solution.

[0048] (5) Place the purified LiCl solution obtained in step (4) into a polytetrafluoroethylene reactor, add 269 ml of HF solution while stirring, react at room temperature for 30 minutes, centrifuge and filter, wash twice with 40° C. deionized water, and dry the wet crystals of lithium fluoride to obtain a lithium fluoride product.

[0049] (5) The purified LiCl solution obtained in step (4) was placed in a polytetrafluoroethylene reactor, and 398 ml of the measured HF solution was added while stirring. After reacting at room temperature for 30 minutes, the mixture was centrifuged and washed twice with 40° C. deionized water. The wet crystals of lithium fluoride were dried to obtain a lithium fluoride product. The purity of the product was 99.956% and the total lithium yield was 95.665%.

[0050] The hydrochloric acid obtained by filtering and washing is placed in a hydrochloric acid storage tank for recycling.

[0051] Example 5

[0052] In step (1) of Example 1, 184 g of calcium chloride was added, and the reaction was maintained at 85° C. for 30 minutes. The rest was the same as in Example 1. A lithium fluoride product was obtained with a purity of 99.945% and a total lithium yield of 95.691%.

[0053] Example 6

[0054] Step (1) is the same as step (1) in Example 5; the reaction time in step (2) in Example 2 is 30 minutes. The rest is the same as in Example 2.

[0055] The lithium fluoride product was obtained with a purity of 99.951% and a total lithium yield of 95.758%.

[0056] Example 7

[0057] The reaction time in step (1) of Example 3 is 35 minutes, the reaction temperature is 90° C., the washing water temperature is 90° C., and the rest is the same as in Example 3. A lithium fluoride product is obtained with a purity of 99.961% and a total lithium yield of 95.711%.

Claims

1. A method for preparing lithium fluoride, characterized in that: Follow these steps: (1) 800 ml of a lithium sulfate solution having a Li2O content of 55 g / L was transferred into a reactor and ultrasonically dispersed for 20 minutes, and then 179 g of calcium chloride was slowly added while ultrasonically dispersing and stirring, and the mixture was kept at 80° C. for a full reaction for 25 minutes and then kept at this temperature for 30 minutes; the obtained product was vacuum filtered and the calcium sulfate filter cake was washed twice with 85° C. deionized water to obtain LiCl mother solution 1; the obtained LiCl solution, i.e., mother solution 1, was placed in a LiCl mother solution storage tank; (2) Another 760 ml of the same lithium sulfate solution as in step (1) was ultrasonically dispersed in a reactor for 20 minutes, and then 156 g of sodium carbonate was slowly added while stirring and ultrasonicating, and the mixture was reacted at 40° C. for 25 minutes. After the reaction was completed, the mixture was heated to 80° C., kept at this temperature for 40 minutes, filtered while hot, and washed twice with 80° C. deionized water to obtain Li2CO3; the washed Na2SO4 solution was used to prepare sodium sulfate decahydrate; (3) 1070 ml of hydrochloric acid in a hydrochloric acid storage tank is transferred into a reactor, and the Li2CO3 obtained in step (2) is slowly added in two portions while stirring. After fully reacting at room temperature for 30 minutes, the obtained LiCl mother solution 2 is added to the LiCl mother solution storage tank described in step (1); (4) taking 60 ml of 0.18 mol / L lithium carbonate solution and dispersing it ultrasonically for 20 minutes, and at the same time placing the LiCl mother liquor in the LiCl mother liquor storage tank into the reactor and stirring it ultrasonically for 15 minutes, then adding the lithium carbonate solution to the LiCl mother liquor, stirring and reacting for 30 minutes while ultrasonicating, centrifuging and washing with room temperature deionized water to obtain a purified LiCl solution; (5) placing the purified LiCl solution obtained in step (4) into a polytetrafluoroethylene reactor, adding 253 ml of a measured HF solution while stirring, reacting at room temperature for 30 minutes, centrifuging and washing twice with 40° C. deionized water, and drying the wet crystals of lithium fluoride to obtain a lithium fluoride product. The purity of the product was found to be 99.955%, and the total lithium yield was 95.752%; The hydrochloric acid obtained by separation and washing is placed in a hydrochloric acid storage tank for recycling.