Polarizer protective laminate and polarizing plate using the same

By using a laminate of thermoplastic acrylic resin with a high glass transition temperature and a curable resin in the polarizing plate, a thin and durable laminate for polarizing plate protection was constructed, which solved the reduction of optical characteristics of the polarizing plate in the heating and humidification environment. The problem is to achieve both high durability and thinness.

CN113711093BActive Publication Date: 2024-11-05NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080027555.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-09
Filing Date
2020-04-06
Publication Date
2024-11-05
Estimated Expiration
2040-04-06

AI Technical Summary

Technical Problem

The optical characteristics of the existing polarizer plates are reduced in a heating and humidification environment, and it is difficult to take into account both the durability and the thickness of the polarizer protective film.

Method used

The laminated body of the first layer composed of a thermoplastic acrylic resin having a glass transition temperature of 95°C or more and a second layer composed of a curable resin is used as the laminated body for protection of polarizers. The thickness of the first layer is 10 μm or less. The second layer is 2nd The layer thickness is 1.0 μm or more, the elastic modulus of the second layer is 50 MPa or more, and the pencil hardness is 2H or more, so as to realize a thin and durable polarizer.

Benefits of technology

A polarizing plate with excellent optical characteristics maintenance and durability in a heating and humidified environment is realized, which suppresses cracks and ruptures of the polarizing plate protection film, and significantly improves the overall performance of the polarizing plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113711093B_ABST
    Figure CN113711093B_ABST
Patent Text Reader

Abstract

The present invention provides a polarizer protective laminate that can realize a thin and durable polarizing plate, and further suppresses cracks and / or breakage. The polarizer protective laminate of the present invention comprises: a first layer and a second layer, wherein the first layer is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin having a glass transition temperature of 95° C. or higher, and the second layer is composed of a cured product of a curable resin, and the thickness of the second layer is 1.0 μm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizer protective laminate and a polarizing plate using the laminate. Background Art

[0002] In image display devices (such as liquid crystal display devices, organic EL display devices), due to their image formation methods, in most cases, a polarizing plate is arranged on at least one side of the display unit. In recent years, with the progress of thinning and flexibility of image display devices, there is also a strong demand for thinning of polarizing plates and their constituent films (such as polarizer protective films). However, the thinner the polarizer protective film is, the more obvious the durability problem of the polarizer in a heated and humidified environment, such as reduced optical properties. As a polarizer protective film that can realize a thin and durable polarizer, a polarizer protective film composed of a cured product of a coating film of a specified resin solution has been studied. Such technology is in the initial stage of development, and there is room for various studies.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-210474 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide a polarizing plate protective laminate that can realize a thin polarizing plate with excellent durability and in which cracks and / or breakage are suppressed.

[0008] Solutions for solving problems

[0009] The polarizer protective laminate of the present invention comprises: a first layer and a second layer, wherein the first layer is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin having a glass transition temperature of 95° C. or higher, and the second layer is composed of a cured product of a curable resin, and the thickness of the second layer is 1.0 μm or higher.

[0010] In one embodiment, the elastic modulus of the second layer is 50 MPa or more, and the elongation is 2% or more. In one embodiment, the pencil hardness of the second layer is 2H or more.

[0011] In one embodiment, the thickness of the first layer is 10 μm or less.

[0012] In one embodiment, the first layer has an in-plane retardation Re(550) of 0 nm to 10 nm, and a thickness direction retardation Rth(550) of -20 nm to +10 nm.

[0013] According to another embodiment of the present invention, a polarizing plate is provided. The polarizing plate comprises a polarizer and the polarizer-protecting laminate disposed on one side of the polarizer. The polarizer-protecting laminate is disposed such that the first layer is on the polarizer side.

[0014] In one embodiment, the polarizing plate is disposed on the visible side of the image display device, and the second layer of the polarizer protective laminate is disposed on the visible side.

[0015] Effects of the Invention

[0016] According to the present invention, a polarizer protective film is made into a laminate having a first layer and a second layer, wherein the first layer is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin having a glass transition temperature of 95° C. or higher, and the second layer is composed of a cured product of a curable resin (representatively an active energy ray-curable resin), thereby achieving a thin and highly durable polarizing plate, and further a polarizer protective film (polarizer protective laminate) in which cracks and / or breakage are suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a schematic cross-sectional view of a polarizer-protective laminate according to one embodiment of the present invention.

[0018] Figure 2 This is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention.

[0019] Figure 3 This is a schematic diagram showing an example of a drying shrinkage treatment using a heating roller in the method for producing a polarizing plate according to one embodiment of the present invention. DETAILED DESCRIPTION

[0020] A. Polarizer Protective Laminate

[0021] A-1. Overview of polarizer protective laminate

[0022] Figure 1 It is a schematic cross-sectional view of a polarizer protective laminate according to one embodiment of the present invention. The polarizer protective laminate 100 shown in the figure has a first layer 10 and a second layer 20. The first layer 10 is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin having a glass transition temperature of 95° C. or more. The second layer 20 is composed of a cured product of a curable resin. In an embodiment of the present invention, the thickness of the second layer is 1.0 μm or more. The first layer and the second layer are specifically described below.

[0023] A-2. First floor

[0024] The first layer can typically function as a protective layer of the polarizer. The first layer is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin (hereinafter referred to as an acrylic resin) as described above. The constituent components of the first layer are specifically described below, followed by a description of the properties of the first layer.

[0025] A-2-1. Acrylic resin

[0026] As mentioned above, the glass transition temperature (Tg) of the acrylic resin is 95°C or higher. As a result, the Tg of the first layer is 95°C or higher. As long as the Tg of the acrylic resin is 95°C or higher, the polarizing plate including the first layer obtained from such a resin tends to have excellent durability. The Tg of the acrylic resin is typically 100°C or higher, preferably 110°C or higher, more preferably 115°C or higher, further preferably 120°C or higher, and particularly preferably 125°C or higher. On the other hand, the Tg of the acrylic resin is preferably 300°C or lower, more preferably 250°C or lower, further preferably 200°C or lower, and particularly preferably 160°C or lower. As long as the Tg of the acrylic resin is within such a range, the moldability is excellent.

[0027] Any suitable acrylic resin can be used as long as it has a Tg as described above. The acrylic resin typically contains an alkyl (meth)acrylate as a main component as a monomer unit (repeating unit). In this specification, "(meth)acrylic acid" refers to acrylic acid and / or methacrylic acid. As the alkyl (meth)acrylate constituting the main skeleton of the acrylic resin, there can be exemplified those having a linear or branched alkyl group with 1 to 18 carbon atoms. These can be used alone or in combination. Furthermore, any suitable comonomer can be introduced into the acrylic resin by copolymerization. The repeating unit derived from the alkyl (meth)acrylate is typically represented by the following general formula (1):

[0028]

[0029] In the general formula (1), R 4 represents a hydrogen atom or a methyl group, R 5represents a hydrogen atom or a substituted aliphatic or alicyclic hydrocarbon group having 1 to 6 carbon atoms. Examples of the substituent include halogen and hydroxyl. Specific examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, dicyclopentaneoxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, chloromethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2,3,4,5,6-pentahydroxyhexyl (meth)acrylate, 2,3,4,5-tetrahydroxypentyl (meth)acrylate, methyl 2-(hydroxymethyl)acrylate, ethyl 2-(hydroxymethyl)acrylate, and methyl 2-(hydroxyethyl)acrylate. In the general formula (1), R 5 A hydrogen atom or a methyl group is preferred. Therefore, a particularly desirable alkyl (meth)acrylate is methyl acrylate or methyl methacrylate.

[0030] The acrylic resin may contain only a single (meth)acrylic acid alkyl ester unit, or may contain a plurality of R 4 and R 5 Different alkyl (meth)acrylate units.

[0031] The content ratio of the (meth)acrylic acid alkyl ester unit in the acrylic resin is preferably 50 mol% to 98 mol%, more preferably 55 mol% to 98 mol%, further preferably 60 mol% to 98 mol%, particularly preferably 65 mol% to 98 mol%, and most preferably 70 mol% to 97 mol%. If the content ratio is less than 50 mol%, the effects (e.g., high heat resistance, high transparency) derived from the (meth)acrylic acid alkyl ester unit cannot be fully exerted. If the above-mentioned content ratio is greater than 98 mol%, the resin is brittle and easily broken, and the high mechanical strength cannot be fully exerted, and there is a concern of poor productivity.

[0032] The acrylic resin may also have a repeating unit containing a ring structure. Examples of the repeating unit containing a ring structure include a lactone ring unit, a glutaric anhydride unit, a glutarimide unit, a maleic anhydride unit, and a maleimide (N-substituted maleimide) unit. The repeating unit containing a ring structure may contain only one type, or may contain two or more types.

[0033] The lactone ring unit is preferably represented by the following general formula (2):

[0034]

[0035] In the general formula (2), R 1 , R 2 and R 3 Each independently represents a hydrogen atom or an organic residue having 1 to 20 carbon atoms. It should be noted that the organic residue may also contain an oxygen atom. The acrylic resin may contain only a single lactone ring unit or may contain a plurality of R in the general formula (2). 1 , R 2 and R 3 Different lactone ring units. Acrylic resins having a lactone ring unit are described in, for example, Japanese Patent Application Laid-Open No. 2008-181078, the contents of which are incorporated herein by reference.

[0036] The glutarimide unit is preferably represented by the following general formula (3):

[0037]

[0038] In the general formula (3), R 11 and R 12 Each independently represents hydrogen or an alkyl group having 1 to 8 carbon atoms, and R 13 represents an alkyl group having 1 to 18 carbon atoms, a cycloalkyl group having 3 to 12 carbon atoms, or an aryl group having 6 to 10 carbon atoms. 11 and R 12 are independently hydrogen or methyl, R 13 is hydrogen, methyl, butyl or cyclohexyl. More preferably, R 11 is methyl, R 12 is hydrogen, R 13 The acrylic resin may contain only a single glutarimide unit or may contain a plurality of R in the general formula (3). 11 , R 12 and R 13 Different glutarimide units. Acrylic resins having glutarimide units are described in, for example, Japanese Patent Publication No. 2006-309033, Japanese Patent Publication No. 2006-317560, Japanese Patent Publication No. 2006-328334, Japanese Patent Publication No. 2006-337491, Japanese Patent Publication No. 2006-337492, Japanese Patent Publication No. 2006-337493, and Japanese Patent Publication No. 2006-337569, and the descriptions of these publications are incorporated herein by reference. It should be noted that the glutaric anhydride units are excluding those replaced by R in the general formula (3). 13 Except that the substituted nitrogen atom is replaced by an oxygen atom, the explanation regarding the glutarimide unit is applicable.

[0039] The maleic anhydride unit and the maleimide (N-substituted maleimide) unit can be defined in structure by name, and thus a specific description is omitted.

[0040] The content ratio of the repeating unit containing a ring structure in the acrylic resin is preferably 1 mol% to 50 mol%, more preferably 10 mol% to 40 mol%, and further preferably 20 mol% to 30 mol%. When the content ratio is too low, Tg may be lower than 110° C., and the heat resistance, solvent resistance and surface hardness of the first layer obtained may become insufficient. When the content ratio is too high, moldability and transparency may become insufficient.

[0041] The acrylic resin may contain repeating units other than the (meth)acrylic acid alkyl ester unit and the repeating unit containing a ring structure. Examples of such repeating units include repeating units derived from vinyl monomers copolymerizable with the monomers constituting the above units (other vinyl monomer units). As other vinyl monomers, for example, acrylic acid, methacrylic acid, crotonic acid, 2-(hydroxymethyl) acrylic acid, 2-(hydroxyethyl) acrylic acid, acrylonitrile, methacrylonitrile, ethacrylonitrile, allyl glycidyl ether, maleic anhydride, itaconic anhydride, N-methylmaleimide, N-ethylmaleimide, N-cyclohexylmaleimide, aminoethyl acrylate, propylaminoethyl acrylate, dimethylaminoethyl methacrylate, ethylaminopropyl methacrylate, cyclohexylaminoethyl methacrylate, N-vinyldiethylamine, N-acetylvinylamine, allylamine, methylallylamine, N-methylallylamine, 2-isopropenyl-oxazoline, 2-vinyl-oxazoline, 2-acryloyl-oxazoline, N-phenylmaleimide, phenylaminoethyl methacrylate, styrene, α-methylstyrene, p-glycidylstyrene, p-aminostyrene, 2-styryl-oxazoline, etc. These can be used alone or in combination. The type, number, combination, content ratio and the like of other vinyl monomer units can be appropriately set depending on the purpose.

[0042] The weight average molecular weight of the acrylic resin is preferably 1,000 to 2,000,000, more preferably 5,000 to 1,000,000, further preferably 10,000 to 500,000, particularly preferably 50,000 to 500,000, and most preferably 60,000 to 150,000. The weight average molecular weight can be determined, for example, by polystyrene conversion using gel permeation chromatography (GPC system, manufactured by Tosoh Corporation). It should be noted that tetrahydrofuran can be used as a solvent.

[0043] The acrylic resin may be prepared by appropriately combining the above-mentioned monomer units and polymerizing them by any appropriate polymerization method.

[0044] In the embodiment of the present invention, acrylic resins and other resins can also be used in combination. That is, the monomer components constituting the acrylic resin can be copolymerized with the monomer components constituting the other resins, and the copolymer can be used for the molding of the first layer described later; or the mixture of the acrylic resin and other resins can be used for the molding of the first layer. As other resins, for example, thermoplastic resins such as styrene resins, polyethylene, polypropylene, polyamide, polyphenylene sulfide, polyetheretherketone, polyester, polysulfone, polyphenylene ether, polyacetal, polyimide, and polyetherimide can be listed. The type and blending amount of the resins used in combination can be appropriately set according to the purpose and the desired properties of the obtained film. For example, a styrene resin (preferably an acrylonitrile-styrene copolymer) can be used in combination as a phase difference controller.

[0045] When an acrylic resin and other resins are used in combination, the content of the acrylic resin in the mixture of the acrylic resin and other resins is preferably 50% by weight to 100% by weight, more preferably 60% by weight to 100% by weight, further preferably 70% by weight to 100% by weight, and particularly preferably 80% by weight to 100% by weight. If the content is less than 50% by weight, there is a concern that the high heat resistance and high transparency inherent in the acrylic resin may not be fully reflected.

[0046] A-2-2. Structure and characteristics of the first layer

[0047] As mentioned above, the first layer is composed of a cured product of a coating film of an organic solvent solution of an acrylic resin with a glass transition temperature of 95°C or more. As long as it is a cured product of such a coating film, the thickness can be significantly thinner than the extrusion film. The thickness of the first layer is, for example, 10 μm or less, preferably 7 μm or less, more preferably 5 μm or less, and further preferably 3 μm or less. The lower limit of the thickness of the first layer can be, for example, 1 μm. In addition, although it is not clear in theory, the cured product of this coating film shrinks less than the cured product of a thermosetting resin or an active energy ray-curable resin (such as an ultraviolet curable resin) during film molding, and does not contain residual monomers, etc., so it has the advantages of suppressing the deterioration of the film itself and suppressing the adverse effects of residual monomers on the polarizing plate (polarizer). Furthermore, since the hygroscopicity and moisture permeability are smaller than the cured product of a water-based coating film such as an aqueous solution or a water dispersion, it has the advantage of excellent humidification durability. As a result, a polarizing plate with excellent durability and optical properties can be achieved even in a heated and humidified environment.

[0048] The Tg of the first layer is as described in the above section A-2-1 regarding the acrylic resin.

[0049] The first layer is preferably substantially optically isotropic. In this specification, "substantially optically isotropic" means that the in-plane phase difference Re(550) is 0nm to 10nm, and the phase difference Rth(550) in the thickness direction is -20nm to +10nm. The in-plane phase difference Re(550) is more preferably 0nm to 5nm, further preferably 0nm to 3nm, and particularly preferably 0nm to 2nm. The phase difference Rth(550) in the thickness direction is more preferably -5nm to +5nm, further preferably -3nm to +3nm, and particularly preferably -2nm to +2nm. As long as the Re(550) and Rth(550) of the first layer are within such a range, when the polarizing plate containing the first layer is applied to an image display device, adverse effects on the display characteristics can be prevented. In addition, Re(550) is the in-plane phase difference of the film measured at 23°C with light of a wavelength of 550nm. Re(550) can be calculated by the formula: Re(550) = (nx-ny) × d. Rth(550) is the phase difference in the thickness direction of the film measured at 23°C with light of a wavelength of 550nm. Rth(550) can be calculated by the formula: Rth(550) = (nx-nz) × d. Here, nx is the refractive index in the direction where the in-plane refractive index is the largest (i.e., the slow axis direction), ny is the refractive index in the direction orthogonal to the slow axis in the plane (i.e., the fast axis direction), nz is the refractive index in the thickness direction, and d is the thickness of the film (nm).

[0050] The higher the transmittance of the first layer at 380 nm at a thickness of 3 μm, the more preferred. Specifically, the transmittance is preferably 85% or more, more preferably 88% or more, and further preferably 90% or more. As long as the transmittance is within this range, the desired transparency can be ensured. The transmittance can be measured, for example, according to the method of ASTM-D-1003.

[0051] The lower the haze of the first layer, the more preferred. Specifically, it is preferably 5% or less, more preferably 3% or less, further preferably 1.5% or less, and particularly preferably 1% or less. As long as the haze is 5% or less, the film can be given a good sense of transparency. Furthermore, even in the case of a polarizing plate on the visible side of an image display device, the displayed content can be well identified.

[0052] The YI of the first layer at a thickness of 3 μm is preferably 1.27 or less, more preferably 1.25 or less, further preferably 1.23 or less, and particularly preferably 1.20 or less. When the YI exceeds 1.3, the optical transparency sometimes becomes insufficient. It should be noted that the YI can be obtained by measuring the color tristimulus values ​​(X, Y, Z) obtained by using a high-speed integrating sphere spectroscopic transmittance measuring instrument (trade name DOT-3C: made by Murakami Color Technology Research Institute), for example, using the following formula.

[0053] YI=[(1.28X-1.06Z) / Y]×100

[0054] The b value (hue scale based on the Hunter colorimetric system) of the first layer at a thickness of 3 μm is preferably less than 1.5, and more preferably less than 1.0. When the b value is 1.5 or more, an undesirable color tone may sometimes appear. It should be noted that the b value can be obtained, for example, in the following manner: a sample of the thin film constituting the first layer is cut into 3 cm squares, the hue is measured using a high-speed integrating sphere spectroscopic transmittance meter (trade name DOT-3C: manufactured by Murakami Color Technology Research Institute), and the hue is evaluated according to the Hunter colorimetric system to obtain the b value.

[0055] The first layer (cured product of the coating film) may also contain any suitable additives depending on the purpose. Specific examples of additives include: ultraviolet absorbers; leveling agents; antioxidants such as hindered phenols, phosphorus, and sulfur; stabilizers such as light stabilizers, weather stabilizers, and heat stabilizers; reinforcing materials such as glass fiber and carbon fiber; near-infrared absorbers; flame retardants such as tris(dibromopropyl)phosphate, triallyl phosphate, and antimony oxide; antistatic agents such as anionic, cationic, and nonionic surfactants; colorants such as inorganic pigments, organic pigments, and dyes; organic fillers or inorganic fillers; resin modifiers; organic fillers and inorganic fillers; plasticizers; lubricants; antistatic agents; flame retardants, etc. The additives may be added during the polymerization of the acrylic resin, or added to the solution during the film formation. The type, quantity, combination, and addition amount of the additives may be appropriately set according to the purpose.

[0056] An easy bonding layer can be formed on the side of the first layer opposite to the second layer (representatively, the polarizer side when used for a polarizing plate). The easy bonding layer, for example, comprises a water-based polyurethane and an oxazoline crosslinking agent. By forming such an easy bonding layer, the adhesion between the first layer and the polarizer can be improved.

[0057] A-3. Second floor

[0058] The second layer can typically function as a hard coat. By providing the second layer, the excellent properties of the first layer can be maintained (a polarizing plate with excellent durability can be achieved even if it is very thin), and cracks and / or ruptures of the first layer can be suppressed. The second layer is composed of a cured product of a curable resin as described above. Although the theory is not yet clear, it can be inferred that the three-dimensional cross-linked structure of the cured product suppresses cracks and / or ruptures. The curable resin can be an active energy ray curable resin or a thermosetting resin. Preferably, it is an active energy ray curable resin. Active energy ray curable resins are easy to control reactions and have the advantage of excellent operability.

[0059] In an embodiment of the present invention, the thickness of the second layer is 1.0 μm or more as described above, more preferably 2.0 μm or more, and further preferably 2.5 μm or more. By making the thickness of the second layer be above the specified value, the desired rigidity can be obtained and cracking can be suppressed. The upper limit of the thickness of the second layer can be, for example, 5.0 μm. If the thickness of the second layer is too small, the curing reaction sometimes becomes insufficient and sometimes it is difficult to form a layer, and sometimes the rigidity of the formed layer becomes insufficient. If the thickness of the second layer is too large, the bendability is insufficient and sometimes it becomes easy to crack.

[0060] Preferably, the elastic modulus of the second layer is 50MPa or more, and the elongation is 2% or more. By providing such a second layer, cracks and / or ruptures of the first layer (resulting in a polarizer protective laminate) can be significantly suppressed. The elastic modulus of the second layer is more preferably 500MPa or more, further preferably 1000MPa or more, particularly preferably 2800MPa or more, and particularly preferably 2900MPa or more. The upper limit of the elastic modulus of the second layer can be, for example, 7000MPa. If the elastic modulus of the second layer is too high, it becomes brittle and sometimes cannot function as a protective layer. The elongation of the second layer is preferably 5% or more, further preferably 10% or more, particularly preferably 20% or more, and particularly preferably 40% or more. The upper limit of the second layer can be, for example, 300%. When the elastic modulus of the second layer is large, the elongation can be reduced, and when the elastic modulus of the second layer is small, the elongation can be increased. The elastic modulus and elongation can be measured, for example, according to JIS K 7161.

[0061] The pencil hardness of the second layer is preferably 2H or more, more preferably 3H or more, and further preferably 4H or more. The upper limit of the pencil hardness of the second layer may be, for example, 6H. As long as the pencil hardness of the second layer is within such a range, cracks and / or breakages of the first layer can be more effectively suppressed. The pencil hardness can be measured, for example, in accordance with JIS K 5400.

[0062] The second layer can be representatively composed of any suitable active energy ray curable resin that satisfies the above-mentioned characteristics. As active energy ray curable resins, there can be listed: ultraviolet curable resins, electron beam curable resins. Ultraviolet curable resins are preferred. The reason is that the second layer can be effectively formed by simple processing operations. As ultraviolet curable resins, for example, various resins such as polyester, acrylic, urethane, amide, silicone, and epoxy can be listed. In one embodiment, the ultraviolet curable resin is an urethane acrylate resin. It should be noted that the details of the ultraviolet curable resin are recorded as organic components of the hard coat layer in, for example, Japanese Patent No. 6199605. The records in this gazette are cited as reference in this specification.

[0063] B.Polarizing plate

[0064] The polarizer-protective laminate described in the above section A can be applied to a polarizing plate as a polarizer-protective film. Therefore, the embodiment of the present invention also includes such a polarizing plate. Figure 2 1 is a schematic cross-sectional view of a polarizing plate according to an embodiment of the present invention. The polarizing plate 200 shown in the figure has a polarizer 120 and a polarizer protective laminate 100 disposed on one side of the polarizer 120. The polarizer protective laminate 100 is a polarizer protective laminate according to an embodiment of the present invention described in the aforementioned item A. The polarizer protective laminate 100 is configured so that the first layer 10 becomes the polarizer 120 side, and when the polarizing plate 200 is applied to an image display device, it is typically configured on the visible side of the display unit. At this time, the second layer 20 of the polarizer protective laminate 100 is typically configured on the visible side.

[0065] Another protective layer (not shown) may also be provided on the opposite side of the polarizer 120 to the polarizer protective laminate 100 as required. Typically, the polarizing plate may have an adhesive layer as the outermost layer on one side (typically, the opposite side of the polarizer 120 to the polarizer protective laminate 100) and be attached to the display unit. The surface protection film and / or the carrier film may be temporarily bonded to the polarizing plate in a removable manner as required to enhance and / or support the polarizing plate. When the polarizing plate includes an adhesive layer, a separator is temporarily bonded to the surface of the adhesive layer in a removable manner to protect the adhesive layer until the actual use, and the polarizing plate can be rolled up.

[0066] The polarizing plate may be in a long strip shape or a thin sheet shape. When the polarizing plate is in a long strip shape, the polarizing plate may be preferably wound into a roll shape.

[0067] In an embodiment of the present invention, by adopting the polarizer protective laminate described in the aforementioned A project, the thickness of the polarizer protective film can be made very thin. Furthermore, such a polarizer protective laminate can be formed directly (i.e., without an adhesive layer or adhesive layer) on the polarizer. As a result, the total thickness of the polarizer can be made extremely thin. The total thickness of the polarizer is, for example, less than 40 μm, preferably less than 30 μm, more preferably less than 25 μm, and more preferably less than 15 μm. The lower limit of the total thickness of the polarizer can be, for example, 10 μm.

[0068] Furthermore, by adopting the polarizer protective laminate described in the aforementioned item A, a polarizing plate with excellent durability can be realized even if it is very thin. Specifically, a polarizing plate in which the reduction of optical characteristics is suppressed even in a heated and humidified environment can be realized. For the polarizing plate of the present invention, the change ΔTs of the monomer transmittance Ts and the change ΔP of the polarization degree P after being placed in an environment of 85°C and 85% RH for 48 hours are each very small. The monomer transmittance Ts can be measured by using, for example, an ultraviolet visible spectrophotometer (manufactured by JASCO Corporation, product name "V7100"). The polarization degree P can be calculated using the following formula using the monomer transmittance (Ts), parallel transmittance (Tp) and orthogonal transmittance (Tc) measured using an ultraviolet visible spectrophotometer.

[0069] Polarization degree (P) (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0070] It should be noted that the above Ts, Tp and Tc are Y values ​​obtained by measuring with a 2 degree field of view (light source C) according to JIS Z 8701 and correcting for visibility. In addition, Ts and P are substantially characteristics of the polarizing plate. ΔTs and ΔP are respectively calculated by the following formulas.

[0071] ΔTs(%)=Ts 48 -Ts0

[0072] ΔP(%)=P 48 -P0

[0073] Here, Ts0 is the monomer transmittance before placement (initial), Ts 48 is the transmittance of the monomer after placement, P0 is the polarization degree before placement (initial), P 48 is the degree of polarization after standing. ΔTs is preferably 3.0% or less, more preferably 2.7% or less, and even more preferably 2.4% or less. ΔP is preferably -0.05% to 0%, more preferably -0.03% to 0%, and even more preferably -0.01% to 0%.

[0074] As described above, the polarizing plate of the present invention is extremely thin, and therefore can be suitably used in a flexible image display device. More preferably, the image display device has a curved shape (a substantially curved display screen), and / or can be bent or folded. Specific examples of image display devices include: liquid crystal display devices, electroluminescent (EL) display devices (e.g., organic EL display devices, inorganic EL display devices). Needless to say, the foregoing description does not prevent the polarizing plate of the present invention from being applied to a conventional image display device.

[0075] B-1. Polarizer

[0076] Any appropriate polarizer can be used as the polarizer. The polarizer can be typically produced using a laminate of two or more layers. The method for producing the polarizer is described in the section B-2 as the method for producing the polarizing plate.

[0077] The thickness of the polarizer is preferably 1 μm to 8 μm, more preferably 1 μm to 7 μm, and further preferably 2 μm to 5 μm.

[0078] The boric acid content of the polarizer is preferably 10% by weight or more, more preferably 13% by weight to 25% by weight. As long as the boric acid content of the polarizer is within such a range, the ease of adjusting the curling during lamination can be well maintained by the synergistic effect with the iodine content described later, and the curling during heating can be well suppressed, while improving the durability of the appearance during heating. The boric acid content can be calculated, for example, by the neutralization method using the following formula in the form of the amount of boric acid contained in the polarizer per unit weight.

[0079]

[0080] The iodine content of the polarizer is preferably 2% by weight or more, preferably 2% to 10% by weight. As long as the iodine content of the polarizer is within this range, the synergistic effect with the boric acid content can be used to well maintain the ease of adjusting the curling during lamination, and well suppress the curling during heating, while improving the durability of the appearance during heating. The "iodine content" in this specification refers to the amount of all iodine contained in the polarizer (PVA-based resin film). More specifically, iodine is present in the polarizer as iodide ions (I - ), iodine molecules (I2), polyiodide ions (I3-, I5-), etc., and the iodine content in this specification refers to the amount of iodine including all these forms. The iodine content can be calculated using, for example, a calibration curve method of fluorescent X-ray analysis. It should be noted that polyiodide ions exist in the polarizer in the form of a PVA-iodine complex. By forming such a complex, it is possible to exhibit absorption dichroism in the wavelength range of visible light. Specifically, the complex of PVA and triiodide ion (PVA·I3 - ) has an absorption peak near 470nm; the complex of PVA and pentaiodide ion (PVA·I5 - ) has an absorption peak near 600nm. As a result, polyiodide ions can absorb light in a wide range of visible light depending on their form. On the other hand, iodide ions (I - ) has an absorption peak near 230nm, which has no substantial correlation with the absorption of visible light. Therefore, the polyiodide ions existing in the complex state with PVA may be mainly related to the absorption performance of the polarizer.

[0081] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance Ts of the polarizer is preferably 40% to 48%, more preferably 41% to 46%. The polarization degree P of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and further preferably 99.9% or more.

[0082] B-2. Method for manufacturing polarizing plate

[0083] B-2-1. Method for manufacturing polarizing plate

[0084] The manufacturing method of the polarizer described in the aforementioned B-1 item includes the following steps: forming a polyvinyl alcohol resin layer (PVA resin layer) containing a halide and a polyvinyl alcohol resin (PVA resin) on one side of a long thermoplastic resin substrate to form a laminate; and sequentially applying an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment and a drying shrinkage treatment to the laminate, wherein the drying shrinkage treatment is performed by heating the laminate while conveying it in the length direction, thereby shrinking it by more than 2% in the width direction. The halide content in the PVA resin layer is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA resin. The drying shrinkage treatment is preferably performed using a heating roller, and the temperature of the heating roller is preferably 60°C to 120°C. According to such a manufacturing method, a polarizer as described above can be obtained. In particular, a laminate comprising a PVA-based resin layer containing a halide is prepared, the stretching of the laminate is subjected to multi-stage stretching including air auxiliary stretching and underwater stretching, and the stretched laminate is heated with a heating roller, thereby obtaining a polarizer having excellent optical properties (representatively, monomer transmittance and polarization degree) and suppressed deviation of the optical properties. Specifically, by using a heating roller in the drying and shrinking treatment process, the entire laminate can be uniformly shrunk while conveying the laminate. Thereby, not only the optical properties of the obtained polarizer can be improved, but also polarizers with excellent optical properties can be stably produced, and the deviation of the optical properties of the polarizer (especially monomer transmittance) can be suppressed. The halide and the drying and shrinking treatment are described below. The details of the manufacturing method other than these are recorded, for example, in Japanese Patent Publication No. 2012-73580. The entire record of the publication is cited as a reference in this specification.

[0085] B-2-1-1. Halides

[0086] The PVA resin layer containing a halide and a PVA resin can be formed by applying a coating liquid containing a halide and a PVA resin on a thermoplastic resin substrate and drying the coating film. The coating liquid is typically a solution formed by dissolving the aforementioned halide and the aforementioned PVA resin in a solvent. As solvents, for example, water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyols such as trimethylolpropane, amines such as ethylenediamine and diethylenetriamine can be listed. These can be used alone or in combination of two or more. Water is also preferred among these. The PVA resin concentration of the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. As long as the resin concentration is such, a uniform coating film that is closely attached to the thermoplastic resin substrate can be formed.

[0087] Any appropriate halide may be used as the halide. Examples thereof include iodide and sodium chloride. Examples of iodide include potassium iodide, sodium iodide, and lithium iodide. Of these, potassium iodide is also preferred.

[0088] The amount of the halide in the coating liquid is preferably 5 to 20 parts by weight, more preferably 10 to 15 parts by weight, based on 100 parts by weight of the PVA-based resin. If the amount of the halide is too large, the halide may bleed out and the polarizing plate finally obtained may become cloudy.

[0089] Generally speaking, the orientation of the polyvinyl alcohol molecules in the PVA resin layer becomes higher by stretching, but if the stretched PVA resin layer is immersed in a water-containing liquid, the orientation of the polyvinyl alcohol molecules is sometimes disordered and the orientation is reduced. In particular, when the laminate of the thermoplastic resin substrate and the PVA resin layer is stretched in boric acid water, in order to stabilize the stretching of the thermoplastic resin substrate, when the laminate is stretched in boric acid water at a relatively high temperature, the tendency of the orientation degree to decrease is obvious. For example, the stretching of the PVA film alone in boric acid water is usually carried out at 60°C. In contrast, the stretching of the laminate of A-PET (thermoplastic resin substrate) and the PVA resin layer is carried out at a temperature of about 70°C, that is, at a higher temperature. In this case, the orientation of the PVA at the initial stretching stage will decrease before it rises due to the stretching in water. In this regard, by making a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate, and stretching the laminate at a high temperature in the air (auxiliary stretching) before stretching in boric acid water, the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the orientation disorder and the reduction of the orientation of the polyvinyl alcohol molecules can be suppressed more than when the PVA-based resin layer does not contain a halide. As a result, the optical properties of the polarizer obtained by the treatment process of immersing the laminate in a liquid such as dyeing treatment and underwater stretching treatment can be improved.

[0090] B-2-1-2. Drying shrinkage treatment

[0091] The drying shrinkage treatment can be carried out by heating the region as a whole, or by heating the conveying roller (so-called using a heating roller) (heating roller drying method). Preferably, both are used. By using a heating roller to dry it, the heating curling of the laminate can be effectively suppressed, and a polarizer with excellent appearance is manufactured. Specifically, by drying the laminate along the state of the heating roller, the crystallization of the aforementioned thermoplastic resin substrate can be effectively promoted and the degree of crystallization can be increased, even at a relatively low drying temperature, the degree of crystallization of the thermoplastic resin substrate can be well increased. As a result, the rigidity of the thermoplastic resin substrate increases and becomes a state that can withstand the shrinkage of the PVA-based resin layer due to drying, and curling is suppressed. In addition, by using a heating roller, it is possible to dry while the laminate is maintained in a flat state, so that not only the generation of curling can be suppressed, but also the generation of wrinkles can be suppressed. At this time, the laminate can be shrunk in the width direction by the drying shrinkage treatment to improve optical properties. The reason is that the orientation of PVA and PVA / iodine complex can be effectively improved. The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment is preferably 2% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%. By using a heated roller, the laminate can be continuously shrunk in the width direction while being conveyed, and high productivity can be achieved.

[0092] Figure 3 1 is a schematic diagram showing an example of a drying shrinkage process. In the drying shrinkage process, the laminate 200 is dried while being transported by using the transport rollers R1 to R6 and the guide rollers G1 to G4 heated to a predetermined temperature. In the example shown in the figure, the transport rollers R1 to R6 are arranged so as to alternately and continuously heat the surface of the PVA resin layer and the surface of the thermoplastic resin substrate, but, for example, the transport rollers R1 to R6 may be arranged so as to continuously heat only one side of the laminate 200 (for example, the surface of the thermoplastic resin substrate).

[0093] The drying conditions can be controlled by adjusting the heating temperature of the conveying roller (the temperature of the heating roller), the number of heating rollers, and the contact time with the heating roller. The temperature of the heating roller is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. An optical laminate with excellent durability can be produced while well increasing the degree of crystallization of the thermoplastic resin and well suppressing curling. It should be noted that the temperature of the heating roller can be measured using a contact thermometer. In the example shown in the figure, 6 conveying rollers are provided, but there is no particular limitation as long as there are multiple conveying rollers. The number of conveying rollers is usually 2 to 40, and preferably 4 to 30. The contact time (total contact time) between the laminate and the heating roller is preferably 1 second to 300 seconds, more preferably 1 to 20 seconds, and more preferably 1 to 10 seconds.

[0094] The heating roller can be set in a heating furnace (such as an oven) or in a general production line (under room temperature environment). It is preferably set in a heating furnace equipped with an air supply mechanism. By combining the drying based on the heating roller and the hot air drying, the rapid temperature change between the heating rollers is suppressed, and the shrinkage in the width direction can be easily controlled. The temperature of the hot air drying is preferably 30°C to 100°C. In addition, the hot air drying time is preferably 1 second to 300 seconds. The wind speed of the hot air is preferably about 10m / s to 30m / s. It should be noted that the wind speed is the wind speed in the heating furnace and can be measured with a micro-vane digital anemometer.

[0095] It is preferred that a cleaning treatment be performed after the underwater stretching treatment and before the drying shrinkage treatment. The cleaning treatment is typically performed by immersing the PVA-based resin layer in a potassium iodide aqueous solution.

[0096] Thereby, a laminate of thermoplastic resin substrate / polarizer can be obtained.

[0097] B-2-2. Method for manufacturing polarizing plate

[0098] An organic solvent solution of an acrylic resin is applied to the surface of the laminate obtained in the above item B-2-1 to form a coating film, and the coating film is cured to form the first layer of the polarizer protective laminate.

[0099] The acrylic resin is as described in the above section A-2-1.

[0100] As the organic solvent, any appropriate organic solvent that can dissolve or uniformly disperse the acrylic resin can be used. Specific examples of the organic solvent include ethyl acetate, toluene, methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), cyclopentanone, and cyclohexanone.

[0101] The acrylic resin concentration of the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. With such a resin concentration, a uniform coating film that is closely attached to the polarizer can be formed.

[0102] The solution can be applied to any suitable substrate or to a polarizer. When the solution is applied to the substrate, the cured product of the coating film formed on the substrate is transferred to the polarizer. When the solution is applied to the polarizer, the first layer is directly formed on the polarizer by drying (curing) the coating film. Preferably, the solution is applied to the polarizer to form the first layer directly on the polarizer. As long as it is such a structure, the adhesive layer or adhesive layer required for transfer can be omitted, so the polarizing plate can be made thinner. As a coating method for the solution, any suitable method can be adopted. As specific examples, roller coating, spin coating, wire rod coating, dip coating, die coating, curtain coating, spray coating, and blade coating (comma coating, etc.) can be cited.

[0103] The first layer can be formed by drying (curing) the coating film of the solution. The drying temperature is preferably 100° C. or less, and more preferably 50° C. to 70° C. As long as the drying temperature is within this range, it is possible to prevent adverse effects on the polarizer. The drying time can be varied according to the drying temperature. The drying time can be, for example, 1 minute to 10 minutes.

[0104] Next, the second layer is formed by applying an active energy ray-curable resin on the surface of the first layer and curing it. The coating method of the active energy ray-curable resin is as described above with respect to the first layer. The active energy ray-curable resin (resin composition) may also contain a leveling agent. As a leveling agent, for example, a fluorine-based leveling agent and a silicone-based leveling agent can be cited. Furthermore, additives may also be included in the active energy ray-curable resin (resin composition). As additives, microparticles, fillers, dispersants, plasticizers, ultraviolet absorbers, surfactants, antioxidants, thixotropic agents, etc. can be cited. The curing conditions can be appropriately set according to the type of active energy ray-curable resin.

[0105] Thus, a polarizer protective laminate is formed. It should be noted that, in the above description, the polarizer protective laminate is directly formed on the polarizer, but the pre-formed polarizer protective laminate can also be transferred to the polarizer. For example, the second layer and the first layer can be formed in sequence on any suitable substrate to prepare a laminate having a structure of substrate / polarizer protective laminate (second layer / first layer), and the polarizer protective laminate is transferred to the polarizer from the laminate.

[0106] As a result, a laminate having a structure of a thermoplastic resin substrate / polarizer / polarizer protective laminate can be obtained. By peeling off the thermoplastic resin substrate from the laminate, a laminate such as Figure 2 The polarizing plate 200 shown in the figure has a polarizer 120 and a polarizer protective laminate 100. Alternatively, a resin film constituting another protective layer can be attached to the polarizer surface of the thermoplastic resin substrate / polarizer laminate, and then the thermoplastic resin substrate is peeled off to form a polarizer protective laminate on the peeled surface. In this case, a polarizing plate further having another protective layer can be obtained.

[0107] Example

[0108] The present invention is specifically described below by way of examples, but the present invention is not limited to these examples. The measuring methods of various properties are as follows. It should be noted that, unless otherwise stated, the "parts" and "%" in the examples are by weight.

[0109] (1) Glass transition temperature Tg

[0110] The thin film constituting the first layer of the polarizer protective laminate used in the examples and comparative examples was measured using a heated TMA analyzer (manufactured by Hitachi High-Tech Science Corporation, product name "TMA-7100C"). The measurement conditions are as follows: load 2g; nitrogen atmosphere (200ml / min); heating from 25°C to 150°C, holding at 150°C for 5 minutes, cooling to 25°C, heating again to 150°C, and holding at 150°C for 5 minutes; heating rate 2°C / min.

[0111] (2) Elastic modulus and elongation

[0112] The film constituting the second layer of the polarizer protective laminate used in Examples and Comparative Examples was measured in accordance with JIS K 7161 and JIS K 7113.

[0113] (3) Crack

[0114] A test piece (50 mm × 50 mm) was cut out from the polarizing plate obtained in the embodiment and the comparative example, and the test piece formed two sides opposite to the direction perpendicular to the absorption axis direction of the polarizer and the absorption axis direction, respectively. The test piece was bonded to a glass plate with an adhesive in such a way that the polarizer protective laminate or protective layer became the outer side to prepare a test sample, and the test sample was placed in an oven at 85°C and 85% RH for 48 hours for heating and humidification, and the state of the polarizer protective laminate or protective layer of the polarizing plate after humidification was observed visually or under a microscope, and evaluated according to the following criteria.

[0115] ○: No cracks observed

[0116] △: Some cracks were observed

[0117] ×: Cracks are noticeable and breakage is also confirmed

[0118] (4) Single-body transmittance and polarization degree

[0119] The single transmittance (Ts), parallel transmittance (Tp) and orthogonal transmittance (Tc) of the polarizing plates obtained in Examples and Comparative Examples were measured using an ultraviolet visible spectrophotometer (manufactured by JASCO Corporation, product name "V7100"), and the polarization degree (P) was calculated using the following formula.

[0120] Polarization degree (P) (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0121] It should be noted that the above-mentioned Ts, Tp and Tc are Y values ​​obtained by measuring with a 2-degree field of view (light source C) according to JIS Z 8701 and performing visibility correction. In addition, Ts and P are substantially characteristics of the polarizing plate.

[0122] Then, the polarizing plate was placed in an oven at 85°C and 85% RH for 48 hours for heating and humidification (heating test). The single transmittance Ts0 before the heating test and the single transmittance Ts0 after the heating test were 48 The single body transmittance change ΔTs was calculated using the following formula.

[0123] ΔTs(%)=Ts 48 -Ts0

[0124] Similarly, from the polarization degree P0 before the heating test and the polarization degree P0 after the heating test 48 The polarization degree change ΔP is calculated using the following formula.

[0125] ΔP(%)=P 48 -P0

[0126] In addition, the heating test was carried out by preparing a test sample in the same manner as in the case of the above-mentioned crack.

[0127] <Example 1>

[0128] 1. Preparation of polarizer / resin substrate laminate

[0129] As the resin substrate, a long amorphous isophthalic acid copolymer polyethylene terephthalate film (thickness: 100 μm) having a water absorption rate of 0.75% and a Tg of about 75° C. was used. One surface of the resin substrate was subjected to a corona treatment.

[0130] To 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER Z410") in a ratio of 9:1, 13 parts by weight of potassium iodide was added to prepare a PVA aqueous solution (coating solution).

[0131] The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60° C. to form a PVA-based resin layer having a thickness of 13 μm, thereby producing a laminate.

[0132] The obtained laminate was subjected to free-end uniaxial stretching by 2.4 times in the longitudinal direction (length direction) between rolls of different peripheral speeds in an oven at 130° C. (in-air auxiliary stretching treatment).

[0133] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).

[0134] Next, the film is immersed in a dyeing bath (an iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 relative to 100 parts by weight of water) having a liquid temperature of 30°C for 60 seconds (dyeing treatment) while adjusting the concentration so that the final polarizing film has a monomer transmittance (Ts) of 41.5%±0.1%.

[0135] Next, the film was immersed in a crosslinking bath (boric acid aqueous solution prepared by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).

[0136] Then, while immersing the laminate in an aqueous boric acid solution (boric acid concentration: 4.0 wt %, potassium iodide: 5.0 wt %) at a liquid temperature of 62°C, the laminate is uniaxially stretched in the longitudinal direction (length direction) between rollers of different circumferential speeds so that the total stretching ratio is 5.5 times (underwater stretching treatment).

[0137] Then, the laminated body was immersed in a cleaning bath (an aqueous solution prepared by mixing 4 parts by weight of potassium iodide with respect to 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment).

[0138] Then, the laminate was dried in an oven maintained at 90° C. while being brought into contact with a SUS heating roll maintained at a surface temperature of 75° C. for about 2 seconds (drying shrinkage treatment). The shrinkage rate in the width direction of the laminate due to the drying shrinkage treatment was 5.2%.

[0139] In this way, a polarizing plate having a thickness of 5 μm was formed on the resin substrate, thereby producing a polarizing plate / resin substrate laminate.

[0140] 2. Production of polarizing plate

[0141] On the surface of the polarizer obtained above, a cycloolefin film (Zeon Corporation, ZT-12, thickness 23 μm) is bonded as a film constituting another protective layer by an ultraviolet curing adhesive. Specifically, the curing adhesive is applied in a manner such that the total thickness becomes 1.0 μm, and a roller mill is used for bonding. After that, UV light is irradiated from the film side to cure the adhesive. Next, the resin substrate is peeled off to obtain a polarizing plate having a structure of another protective layer (ZT-12) / polarizer.

[0142] 20 parts of an acrylic resin having a methyl methacrylate unit (manufactured by Kusumoto Chemicals, product name "B728") were dissolved in 80 parts of methyl ethyl ketone to obtain an acrylic resin solution (20%). The acrylic resin solution was applied to the surface of the polarizer of the polarizing plate obtained above using a wire rod, and the coated film was dried at 60°C for 5 minutes to form the first layer of a polarizer protective laminate in the form of a cured product of the coated film. The thickness of the first layer was 2 μm and the Tg was 116°C. A second layer forming composition was applied to the surface of the first layer. The second layer forming composition contained 100 parts of an ultraviolet curable urethane acrylate resin for a hard coat layer (manufactured by DIC, product name "UNIDIC 17-806"), 0.01 parts of a leveling agent (manufactured by DIC, product name "GRANDIC PC4100"), and 3 parts of a photopolymerization initiator (manufactured by IGM Resins BV, product name "Omnirad907"). The coating film was dried at 90°C for 1 minute and then irradiated with a high pressure mercury lamp at a cumulative light intensity of 200 mW / cm 2 The second layer of the polarizer protective laminate formed in the form of a cured product of the coating film is formed by ultraviolet rays. The thickness of the second layer is 3 μm, the elastic modulus is 5000 MPa, and the elongation is greater than 3%. Thus, a polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) is obtained. The obtained polarizing plate is provided for the evaluation of the above (3) and (4). The results are shown in Table 1.

[0143] <Example 2>

[0144] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Example 1, except that "UNIDIC ELS-888" (manufactured by DIC Corporation) was used instead of "UNIDIC 17-806" as a UV-curable urethane acrylate resin for hard coating to form the second layer. The second layer had a thickness of 3 μm, an elastic modulus of 3000 MPa, and an elongation of 40%.

[0145] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0146] <Example 3>

[0147] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Example 1, except that "UNIDIC V-4221" (manufactured by DIC Corporation) was used instead of "UNIDIC 17-806" as a UV-curable urethane acrylate resin for hard coating to form the second layer. The second layer had a thickness of 3 μm, an elastic modulus of 60 MPa, and an elongation of 200%.

[0148] <Example 4>

[0149] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Example 1, except that a copolymer of methyl acrylate / butyl acrylate (molar ratio 80 / 20) was used instead of "B728" as the acrylic resin to form the first layer. The first layer had a thickness of 2 μm and a Tg of 95°C.

[0150] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0151] <Example 5>

[0152] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Example 4 except that "UNIDIC ELS-888" (manufactured by DIC Corporation) was used instead of "UNIDIC 17-806" as the ultraviolet curable urethane acrylate resin for the hard coat layer to form the second layer. The second layer had a thickness of 3 μm, an elastic modulus of 3000 MPa, and an elongation of 40%.

[0153] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0154] <Example 6>

[0155] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Example 4 except that "UNIDIC V-4221" (manufactured by DIC Corporation) was used instead of "UNIDIC 17-806" as the ultraviolet curable urethane acrylate resin for the hard coat layer to form the second layer. The second layer had a thickness of 3 μm, an elastic modulus of 60 MPa, and an elongation of 200%.

[0156] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0157] <Comparative Example 1>

[0158] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Example 1 except that "B734" (manufactured by Kusumoto Chemicals Co., Ltd.) was used as the acrylic resin instead of "B728" to form the first layer. The first layer had a thickness of 2 μm and a Tg of 71°C.

[0159] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0160] <Comparative Example 2>

[0161] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Comparative Example 1, except that "UNIDIC ELS-888" (manufactured by DIC Corporation) was used instead of "UNIDIC 17-806" as a UV-curable urethane acrylate resin for hard coating to form the second layer. The second layer had a thickness of 3 μm, an elastic modulus of 3000 MPa, and an elongation of 40%.

[0162] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0163] <Comparative Example 3>

[0164] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Comparative Example 1, except that "UNIDIC V-4221" (manufactured by DIC Corporation) was used instead of "UNIDIC 17-806" as a UV-curable urethane acrylate resin for hard coating to form the second layer. The second layer had a thickness of 3 μm, an elastic modulus of 60 MPa, and an elongation of 200%.

[0165] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0166] <Comparative Example 4>

[0167] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Example 1 except that "B722" (manufactured by Kusumoto Chemicals Co., Ltd.) was used as the acrylic resin instead of "B728" to form the first layer. The first layer had a thickness of 2 μm and a Tg of 39°C.

[0168] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0169] <Comparative Example 5>

[0170] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Comparative Example 4, except that "UNIDIC ELS-888" (manufactured by DIC Corporation) was used instead of "UNIDIC 17-806" as the ultraviolet curable urethane acrylate resin for hard coating to form the second layer. The second layer had a thickness of 3 μm, an elastic modulus of 3000 MPa, and an elongation of 40%.

[0171] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0172] <Comparative Example 6>

[0173] A polarizing plate having a structure of a polarizer protective laminate (second layer / first layer) / polarizer / another protective layer (ZT-12) was obtained in the same manner as in Comparative Example 4, except that "UNIDIC V-4221" (manufactured by DIC Corporation) was used instead of "UNIDIC 17-806" as the ultraviolet curable urethane acrylate resin for the hard coat layer to form the second layer. The second layer had a thickness of 3 μm, an elastic modulus of 60 MPa, and an elongation of 200%.

[0174] The obtained polarizing plate was subjected to the evaluations of (3) and (4) above. The results are shown in Table 1.

[0175] <Comparative Example 7>

[0176] A polarizing plate was produced in the same manner as in Example 1 except that the second layer was not formed (that is, only the first layer constituted the protective layer). The obtained polarizing plate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0177] <Comparative Example 8>

[0178] A polarizing plate was produced in the same manner as in Example 4 except that the second layer was not formed (that is, only the first layer constituted the protective layer). The obtained polarizing plate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0179] <Comparative Example 9>

[0180] A polarizing plate was produced in the same manner as in Comparative Example 1 except that the second layer was not formed (that is, only the first layer constituted the protective layer). The obtained polarizing plate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0181] <Comparative Example 10>

[0182] A polarizing plate was produced in the same manner as in Comparative Example 4 except that the second layer was not formed (that is, only the first layer constituted the protective layer). The obtained polarizing plate was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0183] [Table 1]

[0184]

[0185] * "Full light transmission" means that light is virtually completely transmitted and the polarization performance disappears

[0186] * "Partially transparent" means that part of the light is transmitted, and the polarization performance is significantly reduced

[0187] <Evaluation>

[0188] It is clear from Table 1 that the polarizer protective laminate of the present invention is still cracked in a heated and humidified environment. By using such a polarizer protective laminate, a polarizing plate with excellent durability and optical properties that is still reduced in a heated and humidified environment can be realized even if it is very thin.

[0189] Industrial Applicability

[0190] The polarizing plate of the present invention can be suitably used in an image display device. Examples of the image display device include: portable devices such as mobile information terminals (PDAs), smart phones, mobile phones, clocks, digital cameras, and portable game consoles; OA equipment such as computer monitors, notebook computers, and copiers; home electrical appliances such as cameras, televisions, and microwave ovens; in-vehicle equipment such as rear monitors, monitors for car navigation systems, and car audio systems; display equipment such as digital signage and information monitors for commercial stores; security inspection equipment such as surveillance monitors; nursing / medical equipment such as nursing monitors and medical monitors, etc.

[0191] Description of Reference Numerals

[0192] 10. Layer 1

[0193] 20: Layer 2

[0194] 100: Polarizer protective laminate

[0195] 120: Polarizer

[0196] 200: Polarizing plate

Claims

1. A polarizing plate comprising: a polarizer, and a polarizer protective laminate disposed on one side of the polarizer, The polarizer protective laminate comprises: a first layer and a second layer, The first layer is composed of a cured product of a coating film of an organic solvent solution of a thermoplastic acrylic resin having a glass transition temperature of 95° C. or higher, and the second layer is composed of a cured product of a curable resin. The thickness of the second layer is 1.0 μm or more. The thickness of the first layer is 7 μm or less. The polarizer protective laminate is formed directly on the polarizer so that the first layer is on the polarizer side. The weight average molecular weight of the thermoplastic acrylic resin is 10,000 or more and 2,000,000 or less. The second layer has an elastic modulus of 50 MPa or more and an elongation of 2% or more.

2. The polarizing plate according to claim 1, wherein The second layer has a pencil hardness of 2H or more.

3. The polarizing plate according to claim 1, wherein The in-plane phase difference Re(550) of the first layer is 0 nm to 10 nm, and the phase difference Rth(550) in the thickness direction is -20 nm to +10 nm. 4 . The polarizing plate according to claim 1 , which is disposed on the visible side of an image display device, and the second layer of the polarizer protective laminate is disposed on the visible side.