Liquid rocket cryogenic connector surface coating process and cryogenic connector

By spraying Teflon raw materials on the surface of the liquid rocket's low-temperature connector and heating at high temperatures, a non-stick coating is formed, which solves the problem of difficulty in the connector falling off after the low-temperature propellant is filled, and the reliability and production efficiency of rocket launch are improved.

CN113720215BActive Publication Date: 2024-11-05ZHEJIANG BLUE ARROW SPACE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110847110.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-27
Publication Date
2024-11-05
Estimated Expiration
2041-07-27

AI Technical Summary

Technical Problem

After the low-temperature propellant is filled, the ice layer between the rocket liquid circuit connector and the rocket liquid circuit interface is too thick, which affects the normal shedding of the connector and thus affects the rocket's launch process.

Method used

Teflon raw materials are used for surface coating treatment, and bond it to the low-temperature connector through cleaning, spraying and high-temperature heating to form a non-stick and low-temperature stable Teflon coating, reducing icing and ensuring that the connectors and A firm connection to the rocket pipeline.

Benefits of technology

It effectively reduces the surface icing of the low-temperature connector, ensures the connector to fall off reliably under low-temperature conditions, improves the reliability and production efficiency of rocket launch, avoids the fall off and deformation of Teflon coating, and has a reasonable design and stable structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113720215B_ABST
    Figure CN113720215B_ABST
Patent Text Reader

Abstract

The present invention discloses a surface coating process for a liquid rocket cryogenic connector and a cryogenic connector. The spraying process includes: first, providing a cryogenic connector and cleaning the surface of the cryogenic connector; second, spraying Teflon raw material evenly on the surface of the cryogenic connector; third, heating the cryogenic connector at high temperature so that the Teflon raw material in a molten state is bonded to the cryogenic connector. Compared with the prior art, the process has the advantages of reasonable design, stable structure, and convenient connector detachment after the cryogenic propellant is filled, which effectively avoids the icing phenomenon caused by the cryogenic propellant and improves the reliability of connector detachment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of liquid rockets, and in particular to a surface coating process for a liquid rocket cryogenic connector and a cryogenic connector. Background Art

[0002] With the rapid development of the aerospace industry, various technologies involved in the field of rockets have also achieved rapid progress. At present, rockets are the main means of transporting satellites into space. Therefore, continuously reducing the cost of rocket manufacturing and launching is the goal pursued by major commercial aerospace companies.

[0003] The cryogenic propellant filling and discharge connector is used to transport liquid propellant media such as liquid hydrogen, liquid oxygen, and liquid methane to the rocket, and can realize the functions of connection, sealing, and shedding between the connector and the rocket liquid circuit interface. Since liquid rockets use cryogenic propellants, the cryogenic propellant medium in the channel will cause frost and ice to form at the joint between the connector and the rocket liquid circuit interface during use. Especially when the cryogenic propellant filling is completed, the excessive thickness of ice at the joint between the connector and the rocket liquid circuit interface will affect the normal shedding of the connector, thereby affecting the rocket test and launch process.

[0004] Therefore, how to provide a connector with reasonable design and stable structure, which can facilitate the detachment of the connector after the filling of cryogenic propellant is the problem to be solved at present. Summary of the invention

[0005] The purpose of the present invention is to provide a liquid rocket cryogenic connector surface coating process and a cryogenic connector, which have the advantages of reasonable design, stable structure, and easy detachment of the connector after filling with cryogenic propellant.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A liquid rocket cryogenic connector surface coating process, the main steps are as follows:

[0008] Provide low-temperature connectors and clean the surfaces of low-temperature connectors;

[0009] Evenly spray the Teflon material on the surface of the low-temperature connector;

[0010] The low-temperature connector is heated at high temperature so that the Teflon raw material in a molten state is bonded to the low-temperature connector.

[0011] In the same embodiment, the cleaning process for the surface of the low-temperature connector includes cleaning the surface of the low-temperature connector by using an organic solvent.

[0012] In the same embodiment, the cleaning process of the surface of the low-temperature connector by using an organic solvent includes: heating the low-temperature connector to volatilize the organic solvent on its surface; the temperature at which the low-temperature connector is heated to volatilize the organic solvent on its surface is A, wherein 300°C≤A≤400°C.

[0013] In the same embodiment, before uniformly spraying the Teflon raw material on the surface of the spraying portion of the low-temperature connector, the method further includes: sandblasting the spraying portion of the surface of the low-temperature connector to make its surface rough.

[0014] In the same embodiment, the sandblasting treatment of the sprayed part of the surface of the low-temperature connector to make its surface rough is specifically: 40-70 mesh quartz sand and 170-180 mesh brown corundum are prepared in a ratio of 2:1, and sprayed onto the sprayed part of the low-temperature connector with the assistance of high-pressure gas, so that the surface roughness (Ra) of the low-temperature connector reaches 2.0-3.5μm, and the surface of the low-temperature connector is cleaned.

[0015] In the same embodiment, the process of uniformly spraying the Teflon raw material on the surface of the spraying part of the low-temperature connector may be a wet method or a dry method, wherein:

[0016] The wet method is to use a spray gun to spray the Teflon dispersion liquid raw material on the surface of the low-temperature connector where spraying is required;

[0017] The dry method is to blow the powdered Teflon raw material out of the collector with high-pressure gas to form a uniform cloud spray, which adheres to the surface of the low-temperature connector where spraying is required.

[0018] In the same embodiment, the thickness of the coating sprayed on the spraying part of the low-temperature connector is B, 5 μm≤B≤200 μm.

[0019] In the same embodiment, the wet process further includes: heating the low-temperature connector sprayed with the wet Teflon coating in a furnace, wherein the heating temperature is C, and 60°C≤C≤100°C, the heating time is T, and 2h≤T≤4h.

[0020] In the same embodiment, the high temperature heating temperature for bonding the Teflon material in a molten state to the low temperature connector is D, wherein 360°C≤D≤400°C.

[0021] Another aspect of the present invention provides a cryogenic connector, comprising an on-arrow interface structure and a ground interface structure, wherein the ground interface structure comprises a first connector and a locking structure provided on the first connector, wherein two ends of the locking structure are respectively connected to the on-arrow interface structure and the first connector, wherein the on-arrow interface structure is used to connect to a pipeline on the arrow, and the first connector is used to connect to a ground pipeline to ensure that a cryogenic propellant medium on the ground is transported to the arrow, wherein:

[0022] The locking structure comprises a claw, a pin and a pressure ring, wherein the pressure ring is sleeved on one end of the first connector close to the arrow interface structure, the pin passes through the pressure ring and the claw, and the claw is configured to rotate freely along the surface of the pin to control the locking / separation of the arrow interface structure and the first connector.

[0023] The surface of the butt joint end of the arrow interface structure and the first connector, as well as the claw and the pressure ring are respectively provided with Teflon coatings, and the Teflon coatings are in close contact with the arrow interface structure, the ground interface structure, the claw and the pressure ring surface;

[0024] The Teflon coating is used to reduce ice formation at the connection between the on-arrow interface structure and the first connector, thereby ensuring that the on-arrow interface structure is safely separated from the ground interface structure after the internal coolant of the rocket is filled.

[0025] Compared with the prior art, the embodiments of the present invention have at least one of the following advantages:

[0026] First, by evenly spraying Teflon material on the surface of the cryogenic connector, the ice on the surface of the cryogenic connector can be reduced. When the cryogenic propellant is filled, it is easy to separate the connector from the rocket pipeline, which is beneficial to the launch of the rocket.

[0027] Second, by heating the low-temperature connector at high temperature, the Teflon material in the molten state is bonded to the low-temperature connector, thereby making the connection between the Teflon material and the low-temperature connector tighter and more firmly fixed. This can prevent the Teflon coating from falling off the surface of the low-temperature connector and improve the reliability of the connector.

[0028] Third, the connector provided by the embodiment of the present application optimizes the component structure and improves production efficiency. The present invention only needs to set Teflon coatings on the surface of the connecting end of the arrow interface structure and the ground interface structure, as well as the claws and the pressure ring. The Teflon coating is non-sticky (low viscosity) and has good low-temperature stability, so that it can reduce the icing phenomenon. Due to its low-temperature stability, the Teflon coating is prevented from deforming and affecting the use effect. The overall design improvement is small and there is no need to redesign the components.

[0029] It should be understood that the above general description and the following detailed description are merely exemplary and illustrative and are not intended to limit the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Attached Figure 1 It is a simplified structural diagram of the ground interface structure of the present invention;

[0031] Attached Figure 2It is a structural diagram of the interface structure on the arrow of the present invention;

[0032] Attached Figure 3 A simplified structural diagram of a low-temperature connector assembly of the present invention;

[0033] Attached Figure 4 is a cross-sectional view of a low-temperature connector assembly of the present invention;

[0034] Attached Figure 5 It is a simplified structural diagram of the extension part of the present invention;

[0035] Attached Figure 6 It is a structural diagram of the pin of the present invention;

[0036] Attached Figure 7 is a process flow chart of the present invention;

[0037] Attached Figure 8 It is a schematic diagram of the adhesion between the Teflon material and the low-temperature connector of the present invention as the temperature changes.

[0038] Description of reference numerals:

[0039] 1Interface structure on arrow 2Claw

[0040] 3 pin shaft 4 pressure ring

[0041] 5Ground interface structure 6Coating

[0042] 7 Coating structure 8 Epitaxial

[0043] 9Extension DETAILED DESCRIPTION

[0044] In order to make the objectives, technical solutions and advantages of the embodiments of the present invention more clearly understood, the spirit of the contents disclosed by the present invention will be clearly explained with the accompanying drawings and detailed descriptions below. After understanding the embodiments of the contents of the present invention, any technician in the relevant technical field can change and modify the techniques taught by the contents of the present invention without departing from the spirit and scope of the contents of the present invention.

[0045] The exemplary embodiments and descriptions of the present invention are used to explain the present invention, but are not intended to limit the present invention. In addition, elements / components with the same or similar reference numerals used in the drawings and embodiments are used to represent the same or similar parts.

[0046] The terms “first”, “second”, etc. used in this document do not particularly refer to an order or sequence, nor are they used to limit the present invention. They are only used to distinguish elements or operations described with the same technical terms.

[0047] The directional terms used in this document, such as up, down, left, right, front or back, etc., are only used to refer to the directions of the drawings. Therefore, the directional terms used are used to illustrate and not to limit the present invention.

[0048] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0049] As used herein, "and / or" includes any or all combinations of the items described.

[0050] The terms "substantially" and "approximately" used herein are used to modify any quantity or error that may vary slightly, but these slight changes or errors do not change their essence. Generally speaking, the range of slight changes or errors modified by such terms may be 20% in some embodiments, 10% in some embodiments, 5% in some embodiments, or other values. Those skilled in the art should understand that the aforementioned values ​​can be adjusted according to actual needs and are not limited thereto.

[0051] Certain terms used to describe the present application are discussed below or elsewhere in this specification to provide additional guidance to those skilled in the art regarding the description of the present application.

[0052] See also Figure 7 As shown, the present invention provides a liquid rocket cryogenic connector surface coating process, the main steps are as follows:

[0053] S1: Provide low-temperature connectors and clean the surfaces of low-temperature connectors;

[0054] S2: spraying Teflon raw material evenly on the surface of the low-temperature connector;

[0055] S3: The low-temperature connector is heated at high temperature to make the Teflon raw material in a molten state bonded to the low-temperature connector.

[0056] In order to facilitate the spraying of Teflon raw materials and reduce the influence of impurities on the properties of Teflon raw materials, for example, when cleaning the surface of the low-temperature connector, the surface of the low-temperature connector can be cleaned by an organic solvent. The organic solvent can be ethanol, acetone, ether, styrene, etc., and no examples are given here.

[0057] In this embodiment, in order to facilitate the volatilization of the organic solvent, for example, the cleaning treatment of the surface of the low-temperature connector by the organic solvent includes: heating the low-temperature connector to volatilize the organic solvent on the surface. The temperature of heating the low-temperature connector can be 270°C, 300°C, 330°C, etc. According to a large amount of experimental data, it is concluded that the temperature at which the low-temperature connector is heated to volatilize the organic solvent on the surface is A. When 300°C≤A≤400°C is satisfied, the organic solvent is ensured to volatilize quickly from the surface of the low-temperature connector.

[0058] It should be noted that, in order to facilitate the uniform spraying of the Teflon raw material on the surface of the spraying part of the low-temperature connector, so that the Teflon raw material adheres to the low-temperature connector, for example, before the Teflon raw material is uniformly sprayed on the surface of the spraying part of the low-temperature connector, it also includes: sandblasting the spraying part of the surface of the low-temperature connector to make its surface rough. The sandblasting of the spraying part of the surface of the low-temperature connector to make its surface rough is specifically: quartz sand of 40-70 mesh and brown corundum of 170-180 mesh are prepared in a ratio of 2:1, and sprayed to the spraying part of the low-temperature connector with the assistance of high-pressure gas, so that the surface roughness (Ra) of the low-temperature connector reaches 2.0-3.5μm, and the surface of the low-temperature connector is cleaned.

[0059] It should be particularly noted that, in order to facilitate uniform spraying of the Teflon material, for example, uniform spraying of the Teflon material on the surface of the spraying portion of the low-temperature connector may be performed by either a wet method or a dry method.

[0060] The wet method is explained as follows. The wet method is to use a spray gun to spray the Teflon dispersion raw material on the surface of the low-temperature connector where the spraying is required. Specifically, the wet method used in this embodiment is to use a spray gun with a caliber of 1.0 to 1.5 mm to spray the Teflon dispersion raw material on the surface of the low-temperature connector at a pressure of 0.2 to 0.3 MPa. The distance between the spray gun and the surface of the low-temperature connector is 20 to 30 cm, the spray gun and the surface of the low-temperature connector part are parallel at 90°, and the movement speed of the spray gun is 30-60 cm / s. By adjusting the parameters of the wet spraying, a low-temperature connector coating product with a denser and more stable connection is obtained. In addition, in order to evaporate the liquid medium of the Teflon dispersion raw material, for example, after the wet process, it also includes: heating the low-temperature connector sprayed with the wet Teflon coating in a baking oven, wherein the heating temperature is C, and 60°C≤C≤100°C, the heating time is T, and 2h≤T≤4h.

[0061] The dry method is now explained. The dry method is to blow the powdered Teflon raw material out of the collector by high-pressure gas to form a uniform cloud spray, so that it adheres to the surface of the low-temperature connector where it needs to be sprayed. During the entire process of dry spraying, the spray gun is connected to the negative electrode and the part to be sprayed is connected to the positive electrode (ground). At this time, a static area is formed between the spray gun and the part. Through repeated experiments, it is known that by adjusting the voltage of the electrostatic spray gun to between 25 and 40kV, and using a spray gun with a diameter of 1.0 to 1.5mm to blow the powdered Teflon raw material out of the collector by compressed air at a pressure of 0.08 to 0.12MPa, a powdered Teflon raw material with a better dispersion state can be obtained. On the way to the spray gun nozzle, the powdered Teflon raw material passes through the static area and carries a negative charge. Since the particles carry the same charge, they repel each other on their flight path, forming a uniform and consistent cloud spray. The Teflon powder particles are attracted by the positive charge of the part and adhere to the part of the low-temperature connector that needs to be sprayed. Unlike wet spraying, the parameters of the spray gun need to be adjusted. After testing, the distance between the spray gun and the surface of the part is 12 to 18 cm, the spray gun and the surface of the low-temperature connector part are parallel at 90°, and the spray gun moves at a speed of 10 cm / s. The dispersion state of powdered Teflon is the best, the charge is carried more evenly, and the surface of the low-temperature connector is denser.

[0062] After a large number of experiments, it is concluded that when the coating thickness sprayed on the spraying part of the low-temperature connector is B and meets 5μm≤B≤200μm, it can not only reduce the ice on the surface of the low-temperature connector, but also ensure that the sealing of the low-temperature connector is more rigorous.

[0063] like Figure 8 As shown, the high-temperature heating temperature for bonding the Teflon material in the molten state to the low-temperature connector is D, wherein, when 360°C≤D≤400°C is satisfied, it can ensure that the Teflon material and the low-temperature connector are more tightly connected and more firmly fixed (the X-axis represents temperature, and the Y-axis represents adhesion, that is, the degree of firmness of bonding between the Teflon material and the low-temperature connector), and the probability of deformation of the low-temperature connector is low.

[0064] With the long-term use of the low-temperature connector, the Teflon material on its surface will become thinner or even fall off due to wear, and the Teflon material at the thinned area needs to be removed and re-applied. When the thinned area is less than 4 square centimeters, use a cutting knife to clean the thinned area to expose the surface of the low-temperature connector, and then use a wet method to spray the Teflon dispersion liquid material on the surface of the low-temperature connector where spraying is required (the thinned area is cleaned), and then heat it to make the Teflon material bonded to the low-temperature connector. When the thinned area is larger than 4 square centimeters, use a high-temperature spray gun to heat and melt the Teflon material at the thinned area, and then use a dry method to spray the powdered Teflon material on the surface of the low-temperature connector where spraying is required, and then heat it to make the Teflon material bonded to the low-temperature connector.

[0065] After the molten Teflon material is bonded to the low-temperature connector, the low-temperature connector is placed in a cold environment (temperature between -220℃ and -196℃), and the product quality is judged by observing the elongation of the Teflon material on the surface of the low-temperature connector. When the elongation of the Teflon material (the diameter of the raw material molecule) is less than 5%, the low-temperature connector coating (the Teflon material is bonded to the part of the low-temperature connector that needs to be sprayed) is considered qualified.

[0066] Another aspect of the present invention provides a low temperature connector, such as Figure 1 , Figure 2 , Figure 3 , Figure 4 , Figure 5 and Figure 6 As shown, the cryogenic connector assembly comprises an arrow interface structure 1 and a ground interface structure 5, the ground interface structure 5 comprises a first connector and a locking structure arranged on the first connector, the two ends of the locking structure are respectively connected to the arrow interface structure 1 and the first connector, the arrow interface structure 1 is used to connect to the pipeline on the arrow, and the first connector is used to connect to the ground pipeline to ensure that the cryogenic propellant medium on the ground is transported to the arrow. The locking structure comprises a claw 2, a pin 3 and a pressure ring 4, the pressure ring 4 is sleeved on one end of the first connector close to the arrow interface structure 1, the pin 3 passes through the pressure ring 4 and the claw 2, and the claw 2 is configured to rotate freely along the surface of the pin 3 to control the locking / separation of the arrow interface structure 1 and the first connector. The surface of the butt end of the arrow interface structure 1 and the first connector, as well as the claw 2 and the pressure ring 4 are respectively provided with a Teflon coating, and the Teflon coating is in close contact with the surface of the arrow interface structure 1, the first connector, the claw 2 and the pressure ring 4.

[0067] The Teflon coating is used to reduce the icing phenomenon at the connection between the on-arrow interface structure 1 and the first connector, so as to ensure the safe separation of the on-arrow interface structure from the ground interface structure after the internal coolant of the rocket is filled.

[0068] It should be noted that, except for the sprayed parts, surface protection measures should be taken for the low-temperature connector parts, especially the sealing parts. Special shields or masking tape can be used to protect the non-sprayed parts.

[0069] See also Figure 1 and Figure 3 As shown, an embodiment of the present invention provides a ground interface structure of a cryogenic connector, comprising a first connector and a locking structure arranged on the first connector, the first connector having two ends connected and an internal passage for circulating cryogenic propellant, the locking structure being arranged on the circumferential outer surface of the first connector, and being used to connect the first connector with an on-arrow connector connected to an on-arrow interface, so as to transport the cryogenic propellant on the ground to the arrow.

[0070] One end of the first connector used for connecting to the connector on the arrow is provided with a coating 7 for reducing ice formation on the surface of the first connector.

[0071] In order to reduce ice formation on the surface of the first connector, for example, the coating 7 is a Teflon coating. At the same time, in order to ensure that the Teflon coating is tightly connected to the first connector and firmly fixed, for example, the Teflon coating is thermoformed to the surface of the first connector.

[0072] In addition, the locking structure includes a claw 2, a pin shaft 3 and a pressure ring 4. The pressure ring 4 is sleeved on the outside of the first connector and connected to the first connector. The claw 2 is fixed on the pressure ring 4 through the pin shaft 3, and the claw 2 rotates freely along the circumferential surface of the pin shaft 3, which is used to control the locking and separation of the first connector and the upper connector.

[0073] It should be pointed out that in order to prevent water vapor from freezing on the clamping claw 2 and affecting the use of the clamping claw 2 (the clamping claw 2 is fixed and cannot rotate after freezing), for example, a Teflon coating is provided on the surface of the clamping claw 2.

[0074] Another aspect of the present invention provides an arrow-on interface structure of a cryogenic connector, such as Figure 2 , Figure 3 , Figure 4 and Figure 5 As shown, it includes a second connector and an epitaxial body 8, the epitaxial body 8 is protrudingly arranged on the circumferential outer surface of the second connector and close to the side of the ground interface structure of the low-temperature connector, the second connector is connected at both ends and has a channel for the circulation of low-temperature propellant inside, and the second connector and the epitaxial body 8 are provided with a coating structure 6 at one end close to the ground interface structure for reducing icing on the surface of the second connector.

[0075] It should be noted that in order to facilitate the fixation of the second connector and the pipeline on the arrow, for example, the end of the second connector away from the extension body 8 (i.e., the end opposite to the extension body 8) is also provided with an extension portion 9, and the extension portion 9 is protruded along the circumferential surface of the second connector and is fixedly connected to the second connector. The extension portion 9 is used to connect to the pipeline on the arrow. The design of the extension portion 9 can increase the contact area with the pipeline on the arrow, thereby facilitating the connection between the two.

[0076] It is particularly important to point out that, in order to facilitate the delivery of cryogenic propellants, for example, the second connector is a cylindrical structure with two ends connected. In addition, in order to facilitate the cooperation with the claws and facilitate the opening of the claws, for example, the upper and lower side lines formed by cutting the epitaxial body 8 along the axial direction of the epitaxial body 8 are extended and connected to form an isosceles trapezoid. Among them, the long side of the isosceles trapezoid is close to one side of the ground interface structure 5, and the short side is away from one side of the ground interface structure 5. When the claws are opened, only a small rotation (for example, a small arc) along the pin shaft is required, thereby facilitating the separation of the ground interface structure from the arrow interface structure 1.

[0077] In addition, in actual application, in order to make the epitaxial body 8 and the second connector tightly connected and firmly fixed, for example, the epitaxial body 8 and the second connector are integrally formed. In addition, the coating structure 6 is a Teflon coating set by thermoplastic means. It should be further explained that in order to make the coating structure 6 and the surface of the second connector more tightly connected and more firmly fixed, for example, the surface of the epitaxial body 8 and the second connector is provided with a corrugated structure that cooperates with the fixed coating structure 6. The design of the corrugated structure can increase the contact area between the epitaxial body 8 and the surface of the second connector and the coating structure 6. When thermoplastic connection is adopted, the coating structure 6 can be effectively prevented from falling off, thereby reducing ice (a small amount of ice does not affect the separation of the connector), making it easier for the connector to fall off, and thus facilitating the launch of the rocket.

[0078] In the present invention, the application of Teflon coating in low-temperature connectors has the following properties: 1. Non-stickiness: The coating surface has extremely low surface tension, thus showing extremely strong non-stickiness. 2. Sliding property: Teflon coating has a low friction coefficient. The friction coefficient changes when the load slides, but the value is only between 0.05-0.15. 3. Low-temperature stability: Teflon coating can withstand the harsh absolute zero without losing mechanical properties, and can be used at temperatures as low as -240°C. 4. Corrosion resistance: Teflon coating can withstand all strong acids (including aqua regia), strong oxidants, reducing agents and various organic solvents except molten alkali metals, fluorinated media and sodium hydroxide above 300°C, and can protect parts from any kind of chemical corrosion. And Teflon includes PTFE, FEP, PFA, ETFE and other types.

[0079] Compared with the prior art, the present invention has at least one of the following advantages:

[0080] First, by evenly spraying Teflon material on the surface of the cryogenic connector, the ice on the surface of the cryogenic connector can be reduced. When the cryogenic propellant is filled, it is easy to separate the connector from the rocket pipeline, which is beneficial to the launch of the rocket.

[0081] Second, by heating the low-temperature connector at high temperature, the Teflon material in the molten state is bonded to the low-temperature connector, thereby making the connection between the Teflon material and the low-temperature connector tighter and more firmly fixed. This can prevent the Teflon coating from falling off the surface of the low-temperature connector and improve the reliability of the connector.

[0082] Third, the connector provided by the embodiment of the present application optimizes the component structure and improves production efficiency. The present invention only needs to set Teflon coatings on the surface of the connecting end of the arrow interface structure and the ground interface structure, as well as the claws and the pressure ring. The Teflon coating is non-sticky (low viscosity) and has good low-temperature stability, so that it can reduce the icing phenomenon. Due to its low-temperature stability, the Teflon coating is prevented from deforming and affecting the use effect. The overall design improvement is small and there is no need to redesign the components.

[0083] The whole process has the advantages of reasonable design, stable structure, reduced icing, and easy detachment of the connector after filling with cryogenic propellant.

[0084] The above description is only an illustrative specific implementation manner of the present invention. Without departing from the concept and principle of the present invention, any equivalent changes and modifications made by those skilled in the art should fall within the scope of protection of the present invention.

Claims

1. A liquid rocket cryogenic connector surface coating process, characterized in that: Provide low-temperature connectors and clean the surfaces of low-temperature connectors; Evenly spray the Teflon material on the surface of the low-temperature connector; The low-temperature connector is heated to a high temperature so that the Teflon material in a molten state is bonded to the low-temperature connector; The process of uniformly spraying the Teflon raw material on the surface of the spraying part of the low-temperature connector can be either a wet method or a dry method, wherein: The wet method is to use a spray gun to spray the Teflon dispersion liquid raw material on the surface of the low-temperature connector where spraying is required; The dry method is to blow the powdered Teflon raw material out of the collector with high-pressure gas to form a uniform cloud spray, which adheres to the surface of the low-temperature connector where spraying is required; The coating thickness sprayed on the spraying part of the low-temperature connector is B, 5μm≤B≤200μm; The high temperature heating temperature for bonding the Teflon raw material in a molten state to the low temperature connector is D, wherein 360≤D≤400°C.

2. The surface coating process of the liquid rocket cryogenic connector according to claim 1 is characterized in that: The cleaning treatment of the surface of the low-temperature connector includes cleaning the surface of the low-temperature connector by using an organic solvent.

3. The surface coating process of the liquid rocket cryogenic connector according to claim 2 is characterized in that: After the surface of the low-temperature connector is cleaned by an organic solvent, the method includes: heating the low-temperature connector to volatilize the organic solvent on the surface, and the temperature at which the low-temperature connector is heated to volatilize the organic solvent on the surface is A, wherein 300°≤A≤400°.

4. The surface coating process of the liquid rocket cryogenic connector according to claim 1 is characterized in that: Before uniformly spraying the Teflon raw material on the surface of the spraying part of the low-temperature connector, the method further includes: performing sandblasting on the spraying part of the surface of the low-temperature connector to make the surface rough.

5. The surface coating process for a liquid rocket cryogenic connector according to claim 4, characterized in that: The sandblasting treatment of the sprayed part of the surface of the low-temperature connector to make its surface rough is specifically as follows: 40-70 mesh quartz sand and 170-180 mesh brown corundum are prepared in a ratio of 2:1, and are sprayed onto the sprayed part of the low-temperature connector with the assistance of high-pressure gas, so that the surface roughness (Ra) of the low-temperature connector reaches 2.0~3.5μm, and the surface of the low-temperature connector is cleaned.

6. The surface coating process of a liquid rocket cryogenic connector according to claim 1, characterized in that: The wet process also includes: heating the low-temperature connector sprayed with the wet Teflon coating in a furnace, wherein the heating temperature is C, and 60°C≤C≤100°C, the heating time is T, and 2h≤T≤4h.

7. A cryogenic connector using the liquid rocket cryogenic connector surface coating process according to any one of claims 1 to 6, characterized in that: It comprises an on-arrow interface structure and a ground interface structure, wherein the ground interface structure comprises a first connector and a locking structure arranged on the first connector, wherein two ends of the locking structure are respectively connected to the on-arrow interface structure and the first connector, wherein the on-arrow interface structure is used to connect to a pipeline on the arrow, and the first connector is used to connect to a ground pipeline to ensure that a cryogenic propellant medium on the ground is transported to the arrow, wherein: The locking structure comprises a claw, a pin and a pressure ring, wherein the pressure ring is sleeved on one end of the first connector close to the arrow interface structure, the pin passes through the pressure ring and the claw, and the claw is configured to rotate freely along the surface of the pin to control the locking / separation of the arrow interface structure and the first connector. The surface of the butt joint end of the arrow interface structure and the first connector, as well as the claw and the pressure ring are respectively provided with Teflon coatings, and the Teflon coatings are in close contact with the arrow interface structure, the ground interface structure, the claw and the pressure ring surface; The Teflon coating is used to reduce ice formation at the connection between the on-arrow interface structure and the first connector, thereby ensuring that the on-arrow interface structure is safely separated from the ground interface structure after the internal coolant of the rocket is filled.