Adhesive sheet, adherend with adhesive sheet, and method of using adhesive sheet
By using a urethane-based adhesive sheet containing a multifunctional isocyanate compound and a radically polymerizable monomer in the manufacturing process of liquid crystal displays and touch panel displays, ultraviolet irradiation is used to reduce the adhesive force and solve the problems of difficulty in peeling off and contamination after pasting. problem, achieving an efficient sticking and peeling process.
Patent Information
- Application Number
- CN202110610900.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-06-01
AI Technical Summary
Existing urethane-based adhesives are difficult to peel off during the manufacturing process of liquid crystal displays and touch panel displays, and silicone-based adhesives may cause contamination and volatilization, affecting equipment performance.
A urethane-based adhesive sheet containing a multifunctional isocyanate compound and a radically polymerizable monomer was developed to reduce the adhesive force through ultraviolet irradiation and achieve controllable sticking and peeling.
It achieves good wetting, expansion and re-peelability of the adherend before ultraviolet irradiation, and can be easily peeled off from the adherend after irradiation, avoiding excessive adhesion and contamination problems during the pasting process.
Smart Images

Figure CN113755112B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority based on Japanese patent application No. 2020-095352, filed on June 1, 2020, the disclosure of which is incorporated herein in its entirety. Technical Field
[0003] The present invention relates to an adhesive sheet, an adherend with the adhesive sheet, and a method for using the adhesive sheet. Background Art
[0004] At present, as the surface protection sheet of various components, the adhesive sheet with an adhesive layer formed on the substrate sheet is widely used. As the adhesive, there are acrylic adhesive, silicone adhesive and urethane adhesive etc. The acrylic adhesive has excellent adhesion, but due to its high adhesion, it has poor re-peelability after being pasted on the adherend. The silicone adhesive is easy to cause pollution on the adherend, and the silicone resin with lower molecular weight volatilizes and adsorbs on the surface of machines such as electronic equipment, thereby possibly causing undesirable conditions. In contrast, the urethane adhesive has good adhesion to the adherend, and its re-peelability is also relatively excellent and difficult to volatilize.
[0005] In this specification, unless otherwise specified, the “adhesive” refers to an adhesive having removable properties (removable adhesive), and the “adhesive sheet” refers to an adhesive sheet having removable properties (removable adhesive sheet).
[0006] As a method for producing a urethane-based adhesive, there are a method using a hydroxyl-terminated urethane prepolymer and a polyfunctional isocyanate compound which are reaction products of an active hydrogen group-containing compound such as a polyol and a polyisocyanate, and a method (a one shot method) in which a polyol and a polyfunctional isocyanate compound are reacted at once without using a hydroxyl-terminated urethane prepolymer.
[0007] A conventional method for producing an adhesive sheet includes a coating step of coating an adhesive on a substrate sheet, a heating step of heating and drying the formed coating layer to form an adhesive layer, a winding step of winding the obtained adhesive sheet on a winding core to form an adhesive sheet roll, and a curing step of curing the adhesive sheet roll.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2015-124301
[0011] Patent Document 2: Japanese Patent Application Publication No. 2016-28020 Summary of the invention
[0012] Problems to be solved by the invention
[0013] Panel displays such as liquid crystal displays (LCD) and organic electroluminescence displays (OELD), as well as touch panel displays formed by combining the panel displays with touch panels, are widely used in electronic devices such as televisions (TV), personal computers (PC), mobile phones, and portable information terminals.
[0014] Urethane adhesive sheets are preferably used as surface protection sheets for panel displays such as LCDs and touch panel displays, as well as substrates (glass substrates, and ITO / glass substrates with an indium tin oxide (ITO) film formed on a glass substrate, etc.) and optical components manufactured or used in their manufacturing processes.
[0015] In the manufacturing process of panel displays such as LCDs and touch panel displays, in order to improve productivity, it is preferred to be able to transport the adherend with an adhesive sheet to a processing unit that performs necessary processes at high speed. For example, automatic high-speed transportation using a vacuum suction member to suck the adherend with an adhesive sheet from the adhesive sheet side, lift it up, and transport it to a desired location is being studied.
[0016] In the above-mentioned automatic high-speed conveying, it is preferred that the adherend with the adhesive sheet has sufficient adhesive force so that the adhesive sheet will not peel off from the adherend during the period of being adsorbed by the vacuum adsorption member. On the other hand, on the adherend with the adhesive sheet after completing the necessary process, it is preferred that the adhesive sheet has a low adhesive force so that the adhesive sheet can be peeled off at a high speed. It is preferred that the adhesive sheet can be easily peeled off from the adherend with the adhesive sheet after completing the necessary process, and it is more preferred that the adhesive sheet can be peeled off naturally.
[0017] Patent Documents 1 and 2 are examples of related art of the present invention.
[0018] Patent Document 1 relates to an acrylic adhesive tape (claim 1).
[0019] In the adhesive tape described in Patent Document 1, the adhesive layer may contain a free radical polymerizable multifunctional oligomer or monomer (Paragraph 0044). The adhesive layer containing the free radical polymerizable multifunctional oligomer or monomer can be polymerized by irradiation with active energy rays such as ultraviolet rays, thereby reducing the adhesive force.
[0020] In the adhesive tape described in Patent Document 1, the adhesive layer may contain a gas generating agent such as an azo compound, an azide compound, a tetrazole compound and its salts, and a bi-tetrazole compound (Paragraph 0037). When the adhesive layer contains a gas generating agent, the gas generating agent may generate gas by irradiating active energy rays such as ultraviolet rays.
[0021] In the adhesive tape described in Patent Document 1, by irradiating active energy rays such as ultraviolet rays, oligomers or monomers are polymerized, thereby reducing the adhesive strength of the adhesive layer, and by irradiating active energy rays such as ultraviolet rays, gas is generated from a gas generator, thereby making it easy to peel the adhesive tape from the adherend.
[0022] Patent Document 2 discloses an adhesive composition containing an adhesive component and a tetrazole compound-basic azo compound complex obtained by reacting a tetrazole compound with a basic azo compound (claim 1).
[0023] Patent Document 2 discloses an adhesive tape having an adhesive layer formed of the above-mentioned adhesive composition on one surface or both surfaces of a substrate (claim 7).
[0024] In the section [Examples], only an acrylic adhesive composition and an adhesive tape were produced.
[0025] When the adhesive component contains a curable adhesive, the curable adhesive may contain a free radical polymerizable multifunctional oligomer or monomer (Paragraph 0031). The adhesive layer containing the free radical polymerizable multifunctional oligomer or monomer can be polymerized by irradiation with active energy rays such as ultraviolet rays, thereby reducing the adhesive force.
[0026] When the adhesive component contains a curable adhesive, the adhesive tape can be easily peeled off from the adherend by irradiating active energy rays such as ultraviolet rays to generate gas from the tetrazole compound-basic azo compound complex (Paragraph 0022).
[0027] Patent Document 1 relates to an acrylic adhesive tape, but does not relate to a urethane adhesive sheet.
[0028] In the section "Examples" of Patent Document 2, only an acrylic adhesive composition and an adhesive tape are produced, and Patent Document 2 does not disclose the specific production of a urethane adhesive sheet.
[0029] Generally, urethane-based adhesives have higher wettability and spreadability on adherends than acrylic-based adhesives, and are therefore more difficult to peel from adherends.
[0030] The present invention has been completed in view of the above situation, and its purpose is to provide a urethane-based adhesive sheet, which has good wetting and spreading properties on the adherend before irradiation with active energy rays, has removable properties that can be re-adhered to the adherend, can be adhered with an adhesive force that is not easy to be peeled off from the adherend, and can be easily peeled off from the adherend after irradiation with active energy rays.
[0031] Means of solving problems
[0032] The adhesive sheet of the present invention comprises a base sheet and an active energy ray-curable adhesive layer formed on the base sheet, wherein:
[0033] The adhesive layer comprises:
[0034] One or more non-radical polymerizable active hydrogen group-containing compounds (HC) having a plurality of active hydrogen groups and no (meth)acryloyl group,
[0035] one or more radical polymerizable monomers (M) containing one or more radical polymerizable active hydrogen group-containing monomers (MH) having one or more active hydrogen groups and two or more (meth)acryloyl groups,
[0036] A polyfunctional isocyanate compound (I), and
[0037] A gas generating agent (G) that generates gas by irradiation with active energy rays, a dried product of an adhesive coating,
[0038] The adhesive layer has an adhesive force of 0.1 gf / 25 mm to 26 gf / 25 mm when measured using a tensile tester at a peeling speed of 0.3 m / min and a peeling angle of 180° in accordance with JIS Z0237.
[0039] The adherend with an adhesive sheet of the present invention is an adherend obtained by attaching the above-mentioned adhesive sheet of the present invention to an adherend.
[0040] The first method of using the adhesive sheet of the present invention includes:
[0041] a step of attaching the adhesive sheet of the present invention to the surface of an adherend; and
[0042] The step of irradiating the adhesive sheet attached to the surface of the adherend with active energy rays to reduce the adhesive force of the adhesive sheet.
[0043] The second method of using the adhesive sheet of the present invention includes:
[0044] a step of attaching the adhesive sheet of the present invention to the surface of an adherend; and
[0045] The adhesive sheet affixed to the surface of the adherend is irradiated with active energy rays to reduce the adhesive strength of the adhesive sheet, and the self-weight adhesion time of the adhesive layer to the acrylic resin plate after the active energy ray irradiation measured by the following method is set to more than 30 seconds, and the adhesive sheet with reduced adhesive strength is peeled off from the adherend.
[0046] Hold the two ends of the adhesive sheet with a width of 100 mm and a length of 200 mm with both hands in the longitudinal direction, bend the adhesive sheet so that the adhesive layer faces outward, and align the two ends of the adhesive sheet with each other. In this state, the adhesive layer in the central part of the adhesive sheet is brought into contact with the acrylic resin plate. In this state, release the hands holding the two ends. Measure the time from releasing the hands to the entire adhesive layer being in close contact with the acrylic resin plate as the self-weight adhesion time.
[0047] Effects of the Invention
[0048] According to the present invention, a urethane-based adhesive sheet can be provided, which has good wettability and spreadability with respect to an adherend before irradiation with active energy rays, has removability for being able to re-attach the adherend, can be adhered with an adhesive force that is not easily peeled off from the adherend, and can be easily peeled off from the adherend after irradiation with active energy rays. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is a schematic cross-sectional view of the adhesive sheet according to the first embodiment of the present invention.
[0050] Figure 2 It is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to a second embodiment of the present invention. DETAILED DESCRIPTION
[0051] The present invention relates to a urethane adhesive sheet having a base sheet and an adhesive layer formed on at least one surface of the base sheet.
[0052] In the present invention, the adhesive layer comprises a coated and dried product of a urethane-based adhesive and contains a reaction product of one or more active hydrogen group-containing compounds and one or more polyfunctional isocyanate compounds.
[0053] In the present invention, the adhesive layer has active energy ray-curing properties.
[0054] The adhesive sheet of the present invention is preferably used as a surface protection sheet for panel displays such as liquid crystal displays (LCDs) and organic electroluminescent displays (OELDs), touch panel displays formed by combining the above panel displays with touch panels, and substrates (glass substrates, and ITO / glass substrates with an ITO (indium tin oxide) film formed on a glass substrate, etc.) and optical components manufactured or used in their manufacturing processes.
[0055] In this specification, the "adherend with an adhesive sheet" refers to a laminated body in which an adhesive sheet is attached to the surface of an adherend such as a glass substrate, an ITO (indium tin oxide) film formed on a glass substrate / glass substrate, and an optical member.
[0056] [Adhesive]
[0057] The adhesive as the material of the adhesive layer includes:
[0058] One or more non-radical polymerizable active hydrogen group-containing compounds (HC) having a plurality of active hydrogen groups and no (meth)acryloyl group,
[0059] one or more radical polymerizable monomers (M) containing one or more radical polymerizable active hydrogen group-containing monomers (MH) having one or more active hydrogen groups and two or more (meth)acryloyl groups,
[0060] A polyfunctional isocyanate compound (I), and
[0061] A gas generating agent (G) that generates gas when irradiated with active energy rays.
[0062] The active hydrogen group-containing compound (HC) is a non-radical polymerizable compound having a plurality of active hydrogen groups and having no (meth)acryloyl group.
[0063] Examples of active hydrogen groups include hydroxyl groups, mercapto groups, and amino groups (in this specification, unless otherwise specified, amino groups include imino groups). Examples of active hydrogen group-containing compounds (HC) include polyols having multiple hydroxyl groups, polyamines having multiple amino groups, amino alcohols having amino groups and hydroxyl groups, and polythiols having multiple mercapto groups. These active hydrogen group-containing compounds (HC) may be either non-polymers or polymers. One or more of them may be used.
[0064] Among them, polyols are preferred. Since polyamines and polythiols are highly reactive and have short pot life, they are preferably used in combination with polyols when used. In addition, when the active hydrogen group of the polyol is a secondary hydroxyl group, the initial curability of the urethane adhesive will not be improved. Therefore, from the viewpoint of pot life and initial curability, the polyol preferably contains a primary hydroxyl group with moderate reactivity.
[0065] (Hydroxy-terminated urethane prepolymer (UPH))
[0066] As the active hydrogen group-containing compound (HC), a hydroxyl-terminated urethane prepolymer (UPH) which is a reaction product obtained by copolymerizing one or more active hydrogen group-containing compounds (HX) with one or more polyisocyanates (N) is preferred. The copolymerization reaction can be carried out in the presence of one or more catalysts as needed. In the copolymerization reaction, one or more solvents can be used as needed. The hydroxyl-terminated urethane prepolymer (UPH) does not contain a (meth)acryloyl group.
[0067] <Active hydrogen group-containing compounds (HX)>
[0068] The active hydrogen group-containing compound (HX) as a raw material of the hydroxyl-terminated urethane prepolymer (UPH) is a compound having a plurality of active hydrogen groups and having no (meth)acryloyl group.
[0069] Examples of active hydrogen groups include hydroxyl groups, mercapto groups, and amino groups (in this specification, unless otherwise specified, amino groups include imino groups). Examples of active hydrogen group-containing compounds (HX) include polyols having multiple hydroxyl groups, polyamines having multiple amino groups, amino alcohols having amino groups and hydroxyl groups, and polythiols having multiple mercapto groups. These active hydrogen group-containing compounds (HX) may be either non-polymers or polymers. One or more of them may be used.
[0070] Among them, polyols are preferred. Polyamines and polythiols have high reactivity with polyisocyanates, so when using them, attention should be paid to reaction control. In addition, since the reaction product of polyamine and polyisocyanate has greater cohesive force than the reaction product of polyol and polyisocyanate, and is easy to become highly viscous, it is preferred to reduce the concentration used during UPH production, or use polyamine and polyol together.
[0071] As polyols that can be used as active hydrogen group-containing compounds (HX), polyester polyols, polyether polyols, polyacrylic acid polyols, polycaprolactone polyols, polycarbonate polyols, and castor oil polyols can be listed. Among them, polyester polyols, polyether polyols and combinations thereof are preferred. It is preferred that at least one active hydrogen group-containing compound (HX) contains a polyether polyol.
[0072] As the polyester polyol that can be used as the active hydrogen group-containing compound (HX), known polyester polyols can be used. Examples of the polyester polyol include compounds (esters) obtained by esterification reaction of one or more polyol components with one or more acid components.
[0073] Examples of the polyol component as a raw material include ethylene glycol (EG), propylene glycol (PG), diethylene glycol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 2-ethyl-1,3-hexanediol, 1,8-octanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, 1,8-decanediol, octadecanediol, glycerol, trimethylolpropane, and pentaerythritol.
[0074] Examples of the acid component of the raw material include succinic acid, methylsuccinic acid, adipic acid, pimelic acid, azelaic acid, sebacic acid, 1,12-dodecanedioic acid, 1,14-tetradecanedioic acid, dimer acid, 2-methyl-1,4-cyclohexanedicarboxylic acid, 2-ethyl-1,4-cyclohexanedicarboxylic acid, phthalic acid, isophthalic acid, terephthalic acid, 1,4-naphthalene dicarboxylic acid, 4,4'-biphenyl dicarboxylic acid, and anhydrides thereof.
[0075] As the polyether polyol that can be used as the active hydrogen group-containing compound (HX), known polyether polyols can be used. Examples of the polyether polyol include compounds (addition polymers) obtained by addition-polymerizing one or more oxirane compounds using an active hydrogen group-containing compound having a plurality of active hydrogen groups as an initiator.
[0076] Examples of the initiator include hydroxyl-containing compounds and amines, etc. Specifically, examples include bifunctional initiators such as ethylene glycol (EG), propylene glycol (PG), 1,4-butanediol, neopentyl glycol, butylethylpentanediol, N-aminoethylethanolamine, isophoronediamine, and xylyldiamine; trifunctional initiators such as glycerol, trimethylolpropane, and triethanolamine; and tetrafunctional initiators such as pentaerythritol, ethylenediamine, and aromatic diamine.
[0077] Examples of the oxirane compound include ethylene oxide (EO), propylene oxide (PO), alkylene oxide (AO) such as butylene oxide (BO), and tetrahydrofuran (THF).
[0078] As the polyether polyol, an alkylene oxide adduct of an active hydrogen-containing compound (also called polyoxyalkylene polyol) is preferred. Among them, bifunctional polyether polyols such as polyethylene glycol (PEG), polypropylene glycol (PPG), PPG to which ethylene oxide (EO) is added at the end (PPG-EO), and polybutylene glycol, and trifunctional polyether polyols such as alkylene oxide adducts of glycerol are preferred.
[0079] Examples of the polyamine that can be used as the active hydrogen group-containing compound (HX) include ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,12-dodecanediamine, 1,14-tetradecanediamine, 1,16-hexadecanediamine, hexamethylenediamine, trimethylhexamethylenediamine, iminobispropylamine, methyliminobispropylamine, 1,5-diamino-2-methylpentane, isophoronediamine, 1,3-diaminomethylcyclohexane, 1-cyclohexylamino-3-aminopropane, 3-aminomethyl-3,3,5-trimethylcyclohexylamine, norbornane skeleton dimethyleneamine, meta-xylylene diamine, aliphatic polyamines such as 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA), 4,4'-diaminodiphenylmethane, 2,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,2'-diaminobiphenyl, 3,3'-diaminobiphenyl, 2,4-diaminophenol, 2,5-diaminophenol, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 2,3-toluenediamine, 2,4-toluenediamine, 2,5-toluenediamine, 2,6-toluenediamine, 3,4-toluenediamine and diethyltoluenediamine; etc.
[0080] Amino alcohols that can be used as active hydrogen group-containing compounds (HX) include monoamines having a hydroxyl group, such as monoethanolamine, diethanolamine, 2-amino-2-methyl-1-propanol, tris(hydroxymethyl)aminomethane, and 2-amino-2-ethyl-1,3-propanediol; and diamines having a hydroxyl group, such as N-(2-hydroxypropyl)ethanolamine; and the like.
[0081] Examples of the polythiol that can be used as the active hydrogen group-containing compound (HX) include methanedithiol, 1,3-butanedithiol, 1,4-butanedithiol, 2,3-butanedithiol, 1,2-benzenedithiol, 1,3-benzenedithiol, 1,4-benzenedithiol, 1,10-decanedithiol, 1,2-ethanedithiol, 1,6-hexanedithiol, 1,9-nonanedithiol, 1,8-octanedithiol, 1,5-pentanedithiol, 1,2-propanedithiol, 1,3-propanedithiol, toluene-3,4-thiophene. dithiol, 3,6-dichloro-1,2-benzenedithiol, 1,5-naphthalenedithiol, 1,2-benzenedithiol, 1,3-benzenedithiol, 1,4-benzenedithiol, 4,4'-thiobisbenzenethiol, 2,5-dimercapto-1,3,4-thiadiazole, 1,8-dimercapto-3,6-dioxaoctane, 1,5-dimercapto-3-thiapentane, 2-di-n-butyl-amino-4,6-dimercapto-s-triazine, and thiol-terminated polymers (polysulfide polymers, etc.), etc.
[0082] One or more active hydrogen group-containing compounds (HX) may include bifunctional active hydrogen group-containing compounds and / or trifunctional or higher active hydrogen group-containing compounds. Typically, bifunctional active hydrogen group-containing compounds have two-dimensional crosslinking properties and can impart moderate flexibility to the adhesive layer. Trifunctional or higher active hydrogen group-containing compounds have three-dimensional crosslinking properties and can impart moderate hardness to the adhesive layer. By selecting the number of functional groups (the number of active hydrogen groups) of each active hydrogen group-containing compound (HX), the adhesion, cohesion, and re-peelability of the urethane adhesive can be adjusted. Depending on the purpose, etc., the number of functional groups of each material can be selected so that the characteristics such as adhesion, cohesion, and re-peelability are within a preferred range.
[0083] From the viewpoint of easily achieving both adhesive strength and removability, the one or more active hydrogen group-containing compounds (HX) preferably include a bifunctional active hydrogen group-containing compound and a trifunctional or higher active hydrogen group-containing compound.
[0084] The number average molecular weight (Mn) of the active hydrogen group-containing compound (HX) is not particularly limited. From the viewpoint of the adhesive force and wettability of the adhesive layer, the Mn of the active hydrogen group-containing compound (HX) is preferably 50 to 20,000, more preferably 100 to 7,000, and particularly preferably 400 to 5,000.
[0085] <Polyisocyanate (N)>
[0086] As the polyisocyanate (N) as a raw material of the hydroxyl-terminated urethane prepolymer (UPH), a known polyisocyanate can be used, and examples thereof include aromatic polyisocyanates, aliphatic polyisocyanates, and alicyclic polyisocyanates.
[0087] One or more polyisocyanates (N) may be used. The number of functional groups of the polyisocyanate (N) is not particularly limited, but preferably difunctional. That is, one or more polyisocyanates (N) are preferably mainly difunctional polyisocyanates, and one or more polyisocyanates (N) are more preferably difunctional polyisocyanates.
[0088] Examples of the aromatic polyisocyanate include 1,3-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,4-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-toluidine diisocyanate, 2,4,6-triisocyanate toluene, 1,3,5-triisocyanate benzene, dimethoxyaniline diisocyanate, 4,4'-diphenyl ether diisocyanate, 4,4',4"-triphenylmethane triisocyanate, ω,ω'-diisocyanate-1,3-dimethylbenzene, ω,ω'-diisocyanate-1,4-dimethylbenzene, ω,ω'-diisocyanate-1,4-diethylbenzene, 1,4-tetramethylphenylene diisocyanate, and 1,3-tetramethylphenylene diisocyanate.
[0089] Examples of the aliphatic polyisocyanate include trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butene diisocyanate, 1,3-butene diisocyanate, dodecamethylene diisocyanate, and 2,4,4-trimethylhexamethylene diisocyanate.
[0090] Examples of the alicyclic polyisocyanate include isophorone diisocyanate (IPDI), 1,3-cyclopentane diisocyanate, 1,3-cyclohexane diisocyanate, 1,4-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 4,4′-methylenebis(cyclohexyl isocyanate), and 1,4-bis(isocyanate methyl)cyclohexane.
[0091] In addition, examples of the polyisocyanate include trimethylolpropane adducts, biuret forms, allophanate forms, and trimers (the trimer contains an isocyanurate ring) of the above-mentioned polyisocyanates.
[0092] A preferred raw material blending ratio of the hydroxyl-terminated urethane prepolymer (UPH) is as follows.
[0093] Preferably, the raw material mixing ratio is determined in such a manner that the ratio of the number of moles of isocyanate groups (NCO) possessed by the polyisocyanate (N) to the total number of moles of active hydrogen groups (H) possessed by the plurality of active hydrogen group-containing compounds (HX) (NCO / H ratio) is 0.20 to 0.95, more preferably 0.40 to 0.80. There is a tendency that the closer the NCO / H ratio is to 1, the easier it is to gel when synthesizing the hydroxyl-terminated urethane prepolymer (UPH). If the NCO / H ratio is 0.95 or less, gelation during the synthesis of the hydroxyl-terminated urethane prepolymer (UPH) can be effectively suppressed.
[0094] <Catalyst>
[0095] In the polymerization of the hydroxyl-terminated urethane prepolymer (UPH), one or more catalysts may be used as necessary. As the catalyst, a known catalyst may be used, and examples thereof include tertiary amine compounds and organic metal compounds.
[0096] Examples of the tertiary amine compound include triethylamine, triethylenediamine, and 1,8-diazabicyclo(5,4,0)-undecene-7 (DBU).
[0097] Examples of the organometallic compound include tin compounds and non-tin compounds.
[0098] Examples of the tin compound include dibutyltin dichloride, dibutyltin oxide, dibutyltin dibromide, dibutyltin dimaleate, dibutyltin dilaurate (DBTDL), dibutyltin diacetate, dioctyltin dilaurate, dibutyltin sulfide, tributyltin sulfide, tributyltin oxide, tributyltin acetate, triethyltin ethoxide, tributyltin ethoxide, dioctyltin oxide, tributyltin chloride, tributyltin trichloroacetate, and 2-ethyltin hexanoate.
[0099] As non-tin compounds, there can be listed titanium compounds such as dibutyltitanium dichloride, tetrabutyl titanate, and butoxytitanium trichloride; lead compounds such as lead oleate, lead 2-ethylhexanoate, lead benzoate, and lead naphthenate; iron compounds such as iron 2-ethylhexanoate and iron acetylacetonate; cobalt compounds such as cobalt benzoate and cobalt 2-ethylhexanoate; zinc compounds such as zinc naphthenate and zinc 2-ethylhexanoate; and zirconium compounds such as zirconium naphthenate.
[0100] The type and amount of the catalyst added can be appropriately designed within the range in which the reaction proceeds satisfactorily.
[0101] In the case of using a plurality of active hydrogen-containing compounds (HX) with different reactivity, due to the difference in their reactivity, in a single catalyst system, there is a concern that the polymerization stability is poor or the reaction solution is turbid. In this case, by using two or more catalysts, it is easy to control the reaction (such as reaction rate, etc.), which can solve the above problems. In a system in which a plurality of active hydrogen-containing compounds (HX) with different reactivity are used, it is preferred to use two or more catalysts. The combination of two or more catalysts is not particularly limited, and tertiary amine / organic metal system, tin system / non-tin system, and tin system / tin system, etc. can be listed. Preferably, tin system / tin system, more preferably dioctyltin dilaurate and 2-ethylhexanoic acid tin.
[0102] The mass ratio of tin 2-ethylhexanoate to dioctyltin dilaurate (tin 2-ethylhexanoate / dioctyltin dilaurate) is not particularly limited, but is preferably greater than 0 and less than 1, more preferably 0.2 to 0.8. If the mass ratio is less than 1, the catalyst activity is well balanced, gelation and turbidity of the reaction solution are effectively suppressed, and polymerization stability is further improved.
[0103] The amount of one or more catalysts used is not particularly limited, but is preferably 0.01% to 1.0% by mass based on the total amount of one or more active hydrogen group-containing compounds (HX) and one or more polyisocyanates (N).
[0104] <Solvent>
[0105] In the polymerization of the hydroxyl-terminated urethane prepolymer (UPH), more than one solvent can be used as needed. As the solvent, a known solvent can be used, and methyl ethyl ketone, ethyl acetate, toluene, xylene and acetone can be listed. From the viewpoint of the solubility of the hydroxyl-terminated urethane prepolymer (UPH) and the boiling point of the solvent, ethyl acetate and toluene are particularly preferred.
[0106] <Polymerization method of hydroxyl-terminated urethane prepolymer (UPH)>
[0107] The polymerization method of the hydroxyl-terminated urethane prepolymer (UPH) is not particularly limited, and a known polymerization method such as a bulk polymerization method and a solution polymerization method can be applied.
[0108] Examples of the polymerization process of the hydroxyl-terminated urethane prepolymer (UPH) include:
[0109] Step 1) a step of placing one or more active hydrogen group-containing compounds (HX), one or more polyisocyanates (N), one or more catalysts as required, and one or more solvents as required into a flask;
[0110] Step 2) a step of placing one or more active hydrogen group-containing compounds (HX), one or more catalysts as needed, and one or more solvents as needed into a flask, and adding one or more polyisocyanates (N) dropwise therein.
[0111] When a plurality of active hydrogen group-containing compounds (HX) and / or polyisocyanates (N) are used, the reaction may be performed in a plurality of stages.
[0112] When a catalyst is used, the reaction temperature is preferably less than 100° C., more preferably 50° C. to 95° C., and particularly preferably 60° C. to 85° C. When the reaction temperature is 100° C. or higher, there is a concern that it becomes difficult to control the reaction rate and polymerization stability, and it is difficult to produce a hydroxyl-terminated urethane prepolymer (UPH) having a desired molecular weight. When no catalyst is used, the reaction temperature is preferably 100° C. or higher, more preferably 110° C. or higher.
[0113] (Polyfunctional isocyanate compound (I))
[0114] As the polyfunctional isocyanate compound (I), a known polyfunctional isocyanate compound can be used, and a compound exemplified as a polyisocyanate (N) as a raw material for a hydroxyl-terminated urethane prepolymer (UPH) can be used (specifically, aromatic polyisocyanates, aliphatic polyisocyanates, aromatic aliphatic polyisocyanates, alicyclic polyisocyanates, and trimethylolpropane adducts / biuret bodies / allophenate bodies / trimers thereof).
[0115] The polyfunctional isocyanate compound (I) may be one or more than two. The number of functional groups of the polyfunctional isocyanate compound (I) is not particularly limited, but is preferably trifunctional or more. That is, the polyfunctional isocyanate compound (I) preferably mainly contains trifunctional or more polyisocyanates, and the polyfunctional isocyanate compound (I) preferably is trifunctional or more polyisocyanates.
[0116] (Radical polymerizable monomer (M))
[0117] The adhesive as a material of the adhesive layer contains one or more radical polymerizable monomers (M).
[0118] The radical polymerizable monomer (M) is a material that polymerizes and cures by irradiation with active energy rays such as ultraviolet rays and electron beams in the presence of a radical polymerization initiator (RI) as required. The radical polymerizable monomer (M) is preferably an ultraviolet curable monomer that cures by ultraviolet irradiation.
[0119] In this specification, unless otherwise specified, ultraviolet rays (hereinafter, may be simply abbreviated as "UV") are defined as "light irradiated from a high-pressure mercury lamp that generates ultraviolet rays having a peak wavelength in the range of 250 nm to 440 nm".
[0120] When an adherend with an adhesive sheet is irradiated with active energy rays, one or more radical polymerizable monomers (M) contained in the adhesive layer are polymerized and cured, and the adhesive force and wettability of the adhesive layer are reduced, making it easy to peel the adhesive sheet from the adherend.
[0121] When the active hydrogen group-containing compound as the main component has a (meth)acryloyl group like the free radical polymerizable monomer (M), there is a concern that the reactivity of the adhesive layer is too high, and the reaction is more likely to be initiated and carried out due to the small amount of ultraviolet rays contained in ambient light such as fluorescent light and sunlight, and the adhesive strength of the adhesive layer will be reduced. It is not preferred that the adhesive strength of the adhesive layer will be reduced due to the small amount of ultraviolet rays contained in the ambient light when the adherend is transported by vacuum adsorption.
[0122] In the present invention, since a non-radical polymerizable active hydrogen group-containing compound (HC) having no (meth)acryloyl group (preferably a hydroxy-terminated urethane prepolymer (UPH)) is used as the active hydrogen group-containing compound as the main component, the cross-linking reaction caused by a small amount of ultraviolet rays contained in the irradiated ambient light can be suppressed, and the adherend can be suppressed from peeling off from the adhesive sheet during vacuum suction transportation.
[0123] In the present invention, the one or more radical polymerizable monomers (M) include one or more radical polymerizable active hydrogen group-containing monomers (MH) having one or more active hydrogen groups and two or more (meth)acryloyl groups, and may contain one or more other radical polymerizable monomers (MO) as required.
[0124] Examples of the active hydrogen group contained in the active hydrogen group-containing compound (MH) include a hydroxyl group (hydroxyl group), a mercapto group, and an amino group (in this specification, unless otherwise specified, an amino group includes an imino group), etc., preferably a hydroxyl group and an amino group, and particularly preferably a hydroxyl group.
[0125] In the present invention, "(meth)acryloyl" means acryloyl and methacryloyl.
[0126] One or more non-radical polymerizable active hydrogen group-containing compounds (HC) and one or more radical polymerizable active hydrogen group-containing monomers (MH) may react with the polyfunctional isocyanate compound (I). The adhesive layer may contain a reaction product thereof.
[0127] One or more radically polymerizable active hydrogen group-containing monomers (MH) can be bonded to the urethane resin via the polyfunctional isocyanate compound (I) during polymerization, and can more effectively cause curing of the adhesive layer and thereby reduce adhesive strength and wet spreadability.
[0128] One or more active hydrogen group-containing monomers (MH) are preferably trifunctional or higher active hydrogen group-containing monomers (MHT) having three or more (meth)acryloyl groups. In this case, a crosslinking reaction is carried out during free radical polymerization, which can effectively cause the curing of the adhesive layer, and the resulting reduction in adhesion and wettability.
[0129] From the viewpoint of further increasing the above-mentioned effects, the number of (meth)acryloyl groups in the active hydrogen group-containing monomer (MH) is more preferably 4 or more, particularly preferably 5 or more.
[0130] That is, the one or more active hydrogen group-containing monomers (MH) are more preferably one or more tetrafunctional or higher active hydrogen group-containing monomers (MHQ) having four or more (meth)acryloyl groups. The one or more active hydrogen group-containing monomers (MH) are particularly preferably one or more pentafunctional or higher active hydrogen group-containing monomers (MHF) having five or more (meth)acryloyl groups.
[0131] Examples of the active hydrogen group-containing monomer (MH) having one or more active hydrogen groups and two (meth)acryloyl groups include glycerol diacrylate, glycerol dimethacrylate, and 2-hydroxy-3-acryloyl propoxy methacrylate, etc. These may be used alone or in combination of two or more.
[0132] Examples of the active hydrogen group-containing monomer (MH) having one or more active hydrogen groups and three or more (meth)acryloyl groups include tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and dipentaerythritol penta(meth)acrylate, etc. These can be used alone or in combination.
[0133] The one or more radical polymerizable monomers (M) may contain one or more other radical polymerizable monomers (MO) other than the active hydrogen group-containing monomer (MH) as required. Examples of the radical polymerizable monomer (MO) include compounds having two or more (meth)acryloyl groups and having no active hydrogen group.
[0134] One or more other free radical polymerizable monomers (MO) preferably include one or more trifunctional free radical polymerizable monomers (MOT) having three or more (meth)acryloyl groups. In this case, a crosslinking reaction is carried out during free radical polymerization, which can effectively cause the curing of the adhesive layer, and the resulting reduction in adhesion and wettability.
[0135] From the viewpoint that the above-mentioned effects are more effective, the number of (meth)acryloyl groups in the radical polymerizable monomer (MO) is more preferably 4 or more, particularly preferably 5 or more.
[0136] That is, the one or more radical polymerizable monomers (MO) are preferably one or more tetrafunctional or higher-functional radical polymerizable monomers (MOQ) having four or more (meth)acryloyl groups. The one or more radical polymerizable monomers (MO) are particularly preferably one or more pentafunctional or higher-functional radical polymerizable monomers (MOF) having five or more (meth)acryloyl groups.
[0137] Examples of the radical polymerizable monomer (MO) having two (meth)acryloyl groups and having no active hydrogen group include ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, ethoxylated bisphenol A dimethacrylate, tricyclodecane dimethanol dimethacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, and neopentyl glycol dimethacrylate. One or more of these may be used.
[0138] Examples of the radical polymerizable monomer (MO) having three or more (meth)acryloyl groups and having no active hydrogen group include trimethylolpropane tri(meth)acrylate, glycerol tri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, propylene oxide-modified trimethylolpropane tri(meth)acrylate, tri(acryloyloxyethyl)isocyanurate, caprolactone-modified tri(acryloyloxyethyl)isocyanurate, trimethylolethane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, caprolactone-modified dipentaerythritol tri(meth)acrylate, and the like. Ester compounds of polyols and (meth)acrylic acid such as alcohol hexa(meth)acrylate and 1,2,3-cyclohexane tetra(meth)acrylate; polyurethane poly(meth)acrylate, polyester poly(meth)acrylate, polyether poly(meth)acrylate, polyacrylic acid poly(meth)acrylate, polyalkyd resin poly(meth)acrylate, polyepoxy poly(meth)acrylate, polyspiroacetal poly(meth)acrylate, polybutadiene poly(meth)acrylate, polythiol poly(meth)acrylate, and polysilicon poly(meth)acrylate, etc., and polyfunctional poly(meth)acrylate compounds can be used alone or in combination.
[0139] Since it can more effectively cause the curing of the adhesive layer and the resulting reduction in adhesion and wettability, the total amount of one or more pentafunctional or higher free radical polymerizable monomers is preferably 20% by mass to 100% by mass, more preferably 40% by mass to 100% by mass, further preferably 60% by mass to 100% by mass, particularly preferably 70% by mass to 100% by mass, and most preferably 80% by mass to 100% by mass, relative to the total amount of one or more free radical polymerizable monomers (M).
[0140] The “one or more pentafunctional or higher radical polymerizable monomers” mentioned here include one or more pentafunctional or higher active hydrogen group monomers (MHF) and / or one or more pentafunctional or higher radical polymerizable monomers (MOF).
[0141] Since it can more effectively cause the curing of the adhesive layer and the resulting reduction in adhesion and wettability, the amount of one or more pentafunctional or higher active hydrogen group monomers (MHF) is preferably 20% by mass to 100% by mass, more preferably 40% by mass to 100% by mass, further preferably 60% by mass to 100% by mass, particularly preferably 70% by mass to 100% by mass, and most preferably 80% by mass to 100% by mass, relative to the total amount of one or more free radical polymerizable monomers (M).
[0142] (Gas generating agent (G))
[0143] The gas generating agent (G) is a compound that generates gas when irradiated with active energy rays such as ultraviolet rays and electron beams.
[0144] When an adherend with an adhesive sheet is irradiated with active energy rays, the gas generating agent (G) contained in the adhesive layer generates gas, and the generated gas can be retained between the adherend and the adhesive layer. A sufficient amount of gas retained between the adherend and the adhesive layer can play a role in causing the adhesive layer to be naturally peeled off from the adherend.
[0145] In the adhesive sheet of the present invention, by irradiating active energy rays, the radical polymerizable monomer (M) polymerizes, the adhesion and wettability of the adhesive layer are reduced, and gas is generated from the adhesive layer. These effects complement each other, and after irradiation with active energy rays, the adhesive sheet can be easily peeled off from the adherend. For example, the adhesive sheet can be easily peeled off from the adherend by blowing air, etc., or the adhesive sheet can be naturally peeled off from the adherend.
[0146] The gas generating agent (G) is preferably a nitrogen-containing compound that contains an N=N bond and generates nitrogen gas by irradiation with active energy rays. The gas generating agent (G) is preferably at least one of an azo compound, an azide compound, a tetrazole compound, a tetrazole compound salt, and a bi-tetrazole compound. Among them, an azo compound is particularly preferred from the viewpoint of chemical stability of the compound and ease of controlling gas generation.
[0147] The N2 generation volume per 1g of the gas generating agent (G) theoretically calculated from the chemical structural formula is preferably 30mL / g to 400mL / g, more preferably 40mL / g to 200mL / g, and particularly preferably 50mL / g to 120mL / g.
[0148] If the N2 generation volume per 1g of the gas generating agent is 30mL / g or more, a sufficient amount of gas can be stably generated when the adhesive layer is irradiated with active energy rays. If the N2 generation volume per 1g of the gas generating agent is 400mL / g or less, it is possible to stably suppress the easy initiation and reaction due to a small amount of ultraviolet rays contained in ambient light such as fluorescent light and sunlight.
[0149] The volume of N2 generated per 1g of gas generating agent is calculated by the following formula.
[0150] [N2 generation volume per 1g of gas generating agent] (mL / g) = 22.4 × 1000 × [number of N=N groups contained in one molecule] / [molecular weight]
[0151] Table 1 shows examples of gas generating agents (G), the molecular weight of each compound, the number of N=N groups contained in one molecule, and the theoretical value of the N 2 generation volume per 1 g of the gas generating agent.
[0152] In the table, gas generating agents (G11) to (G19) are examples of azo compounds.
[0153] In the table, gas generating agents (G21) to (G22) are examples of tetrazole compounds.
[0154] [Table 1]
[0155]
[0156] Among the nitrogen-containing compounds illustrated in Table 1, there are compounds known as free radical polymerization initiators that generate free radicals by heating and become the starting point of polymerization. The amount used when added as a free radical polymerization initiator is usually less than 1 mass part relative to a total of 100 mass parts of one or more monomers as the polymerization object. The content of the gas generating agent (G) in the adhesive layer is more than the amount of the free radical polymerization initiator added, preferably 2 mass% or more, more preferably 3 mass% to 30 mass%, and particularly preferably 5 mass% to 20 mass%.
[0157] When the content of the gas generating agent (G) in the adhesive layer is 2 mass % or more, the amount of gas generated by active energy ray irradiation is sufficient, and the adhesive sheet can be easily peeled from the adherend after active energy ray irradiation.
[0158] If the content of the gas generating agent (G) is 30% by mass or less, it is easy to obtain an adhesive sheet having sufficient transparency and good UV transmittance, which can be used as a surface protection sheet for panel displays such as LCDs and touch panel displays, as well as substrates and optical components manufactured or used in their manufacturing processes. The preferred UV transmittance will be described later.
[0159] When a compound known as a radical polymerization initiator is used as the gas generating agent (G), a part of the compound of the radical polymerization initiator serves as the radical polymerization initiator and also serves as the gas generating agent (G).
[0160] (Radical polymerization initiator (RI))
[0161] The adhesive may contain a radical polymerization initiator (RI) which initiates polymerization of the radical polymerizable monomer (M) when irradiated with active energy rays as required. When the radical polymerizable monomer (M) is ultraviolet curable, the adhesive preferably contains a radical polymerization initiator (RI) (the radical polymerization initiator (RI) in this case is also referred to as a photopolymerization initiator).
[0162] The radical polymerization initiator (RI) is not particularly limited, and a known radical polymerization initiator can be used. For example, acetophenone-based polymerization initiators such as 4-phenoxydichloroacetophenone, 4-tert-butyl-dichloroacetophenone, diethoxyacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one, 1-hydroxycyclohexylphenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butane-1-one and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one can be listed; benzoin, benzoin methyl ether can be listed. , benzoin ethyl ether, benzoin isopropyl ether and benzyl dimethyl ketal and other benzoin series polymerization initiators; benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-methylbenzophenone, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, and 4-benzoyl-4'-methyldiphenyl sulfide and other benzophenone series polymerization initiators; thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, and thioxanthone polymerization initiators such as 2,4-diisopropylthioxanthone; 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-biphenyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-phenylvinyl-s-triazine Triazine polymerization initiators such as 2-(naphthalene-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphthalene-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(biphenyl)-6-triazine, and 2,4-trichloromethyl(4'-methoxyphenyl)-6-triazine; acylphosphine oxide polymerization initiators; borate (salt) polymerization initiators; carbazole polymerization initiators; imidazole polymerization initiators, etc. These can be used alone or in combination.
[0163] Some of the radical polymerization initiators (RI) exemplified above may also be used as the gas generating agent (G).
[0164] The amount of the radical polymerization initiator (RI) contained in the adhesive layer is not particularly limited, and is, for example, about 0.5% by mass to 1.5% by mass.
[0165] (Sensitizer (RS))
[0166] The adhesive may contain one or more sensitizers (RS) as needed. The sensitizer (RS) absorbs active energy rays such as ultraviolet rays and electron beams, and provides the energy obtained therefrom to other substances, thereby promoting polymerization reactions.
[0167] As the sensitizer (RS), known sensitizers can be used, for example, pigment compounds such as xanthene pigments, coumarin pigments, 3-coumarin keto compounds, and pyrromethene pigments; dialkylaminobenzene compounds such as ethyl 4-dimethylaminobenzoate and 2-ethylhexyl 4-dimethylaminobenzoate; thiol hydrogen donors such as 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, and 2-mercaptobenzimidazole, etc. These can be used alone or in combination.
[0168] When the adhesive layer contains a sensitizer (RS), the reactivity of free radical polymerization caused by irradiation with active energy rays can be increased, and the UV transmittance of the adhesive layer can be effectively reduced. However, when the amount added is too much, there is the following concern: the reactivity of the adhesive layer is too high, and it is easier to initiate and react due to the small amount of ultraviolet rays contained in ambient light such as fluorescent light and sunlight, and the adhesion of the adhesive layer will be reduced. When using a sensitizer (RS), it is preferably used in a small amount within the range that free radical polymerization will not occur before irradiation with active energy rays.
[0169] (Plasticizer (P))
[0170] From the viewpoint of reducing the adhesive force of the adhesive layer and improving the wet expansibility, the adhesive may also contain one or more plasticizers (P) as required. The "plasticizer" mentioned here is a known plasticizer usually added to the adhesive to improve the wet expansibility, and is a material that does not have active energy ray curability. There is no particular limitation on the plasticizer (P), and from the viewpoint of compatibility with other components, organic acid esters are preferred.
[0171] Examples of esters between monobasic or polybasic acids and alcohols include isostearyl laurate, isopropyl myristate, isocetyl myristate, octyldodecyl myristate, isostearyl palmitate, isocetyl stearate, octyldodecyl oleate, dibutyl phthalate, dioctyl phthalate, diheptyl phthalate, dibenzyl phthalate, butyl benzyl phthalate, diisodecyl adipate, diisostearyl adipate, dibutyl sebacate, diisocetyl sebacate, acetyl tributyl citrate, tributyl trimellitate, trioctyl trimellitate, trihexyl trimellitate), trioleyl trimellitate, and triisocetyl trimellitate.
[0172] Examples of esters between other acids and alcohols include esters between unsaturated fatty acids or branched acids such as myristic acid, oleic acid, linoleic acid, linolenic acid, isopalmitic acid, and isostearic acid, and alcohols such as ethylene glycol, propylene glycol, glycerol, trimethylolpropane, pentaerythritol, and sorbitan.
[0173] Examples of esters between a monobasic acid or a polybasic acid and a polyalkylene glycol include polyethylene glycol dicaproate, di-2-ethyl polyethylene glycol caproate, polyethylene glycol dilaurate, polyethylene glycol dioleate, and adipate dimethylene glycol methyl ether.
[0174] From the viewpoint of improving wettability and spreadability, the molecular weight (formula weight or Mn) of the organic acid ester is preferably 250 to 1,000, more preferably 400 to 900, and particularly preferably 500 to 850. When the molecular weight is 250 or more, the heat resistance of the adhesive layer becomes good, and when the molecular weight is 1,000 or less, the wettability and spreadability of the adhesive becomes good.
[0175] The adhesive may not contain the plasticizer (P). In the present invention, even if the plasticizer (P) is not added to the adhesive, one or more radical polymerizable monomers (M) may be used as the plasticizer.
[0176] (Solvent)
[0177] The adhesive may contain one or more solvents as required. As the solvent, known solvents may be used, and methyl ethyl ketone, ethyl acetate, toluene, xylene and acetone etc. may be cited. From the viewpoint of the solubility of the hydroxyl-terminated urethane prepolymer (UPH) and the boiling point of the solvent etc., ethyl acetate and toluene etc. are particularly preferred.
[0178] (Anti-deterioration agent)
[0179] The adhesive may contain one or more anti-deterioration agents as required. Thus, the reduction of various properties caused by long-term use of the adhesive layer can be suppressed. As the anti-deterioration agent, anti-hydrolysis agents, antioxidants, ultraviolet absorbers, and light stabilizers can be listed.
[0180] <Anti-hydrolysis agent>
[0181] In the case of (wet) hot environment, hydrolysis reaction occurs in the adhesive layer and carboxyl is generated, in order to block the carboxyl, an anti-hydrolysis agent can be used. As the anti-hydrolysis agent, carbodiimide system, oxazoline system and epoxy system etc. can be listed. Among them, from the viewpoint of hydrolysis inhibition effect, preferably carbodiimide system.
[0182] The carbodiimide hydrolysis inhibitor is a compound having one or more carbodiimide groups.
[0183] Examples of the monocarbodiimide compound include dicyclohexylcarbodiimide, diisopropylcarbodiimide, dimethylcarbodiimide, diisobutylcarbodiimide, dioctylcarbodiimide, diphenylcarbodiimide, and naphthylcarbodiimide.
[0184] The polycarbodiimide compound can be produced by subjecting a diisocyanate to a decarboxylation condensation reaction in the presence of a carbodiimidization catalyst. Examples of the diisocyanate include 4,4'-diphenylmethane diisocyanate, 3,3'-dimethoxy-4,4'-diphenylmethane diisocyanate, 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate, 4,4'-diphenylether diisocyanate, 3,3'-dimethyl-4,4'-diphenylether diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1-methoxyphenyl-2,4-diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and tetramethylxylylene diisocyanate. Examples of the carbodiimidization catalyst include phosphole oxides such as 1-phenyl-2-phosphole-1-oxide, 3-methyl-2-phosphole-1-oxide, 1-ethyl-3-methyl-2-phosphole-1-oxide, 1-ethyl-2-phosphole-1-oxide, and 3-phosphole isomers thereof.
[0185] Examples of the oxazoline hydrolysis inhibitor include 2,2'-o-phenylenebis(2-oxazoline), 2,2'-m-phenylenebis(2-oxazoline), 2,2'-p-phenylenebis(2-oxazoline), 2,2'-p-phenylenebis(4-methyl-2-oxazoline), 2,2'-m-phenylenebis(4-methyl-2-oxazoline), 2,2'-p-phenylenebis(4,4'-dimethyl-2-oxazoline, oxazoline), 2,2'-m-phenylenebis(4,4'-dimethyl-2-oxazoline), 2,2'-ethylenebis(2-oxazoline), 2,2'-tetramethylenebis(2-oxazoline), 2,2'-hexamethylenebis(2-oxazoline), 2,2'-octamethylenebis(2-oxazoline), 2,2'-ethylenebis(4-methyl-2-oxazoline) and 2,2'-diphenylenebis(2-oxazoline), etc.
[0186] Examples of epoxy hydrolyzing agents include diglycidyl ethers of aliphatic diols such as 1,6-hexanediol, neopentyl glycol, and polyalkylene glycol; polyglycidyl ethers of aliphatic polyols such as sorbitol, sorbitan, polyglycerol, pentaerythritol, diglycerol, glycerol, and trimethylolpropane; polyglycidyl ethers of alicyclic polyols such as cyclohexanedimethanol; diglycidyl esters or polyglycidyl esters of aliphatic or aromatic polycarboxylic acids such as terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, trimellitic acid, adipic acid, and sebacic acid; resorcinol, bis-(p-hydroxyphenyl)methane, 2,2-bis-(p-hydroxyphenyl)methane, and 1,2-bis-(p-hydroxyphenyl)-1,1-diol. ) propane, tris-(p-hydroxyphenyl)methane, and 1,1,2,2-tetra(p-hydroxyphenyl)ethane, etc., diglycidyl ethers or polyglycidyl ethers of polyphenols; N,N-diglycidyl aniline, N,N-diglycidyl toluidine, and N,N,N',N'-tetraglycidyl-bis-(p-aminophenyl)methane, etc., N-glycidyl derivatives of amines; triglycidyl derivatives of aminophenol; triglycidyl tris(2-hydroxyethyl)isocyanurate and triglycidyl isocyanurate; epoxy resins such as o-cresol type epoxy resins and phenolic novolac epoxy resins, etc.
[0187] The amount of the anti-hydrolysis agent added is not particularly limited, but is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 4.5 parts by mass, and particularly preferably 0.5 to 3 parts by mass, relative to 100 parts by mass of the active hydrogen group-containing compound (HC) (preferably a hydroxyl-terminated urethane prepolymer (UPH)).
[0188] <Antioxidants>
[0189] As antioxidants, free radical scavengers and peroxide decomposers can be listed. As free radical scavengers, phenolic compounds and amine compounds can be listed. As peroxide decomposers, sulfur compounds and phosphorus compounds can be listed.
[0190] Examples of the phenolic compound include 2,6-di-tert-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-tert-butyl-4-ethylphenol, stearin β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-butylenebis(3-methyl-6-tert-butylphenol), 3,9-bis[1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]2,4,8,10-tetraoxaspiro[5, 5] undecane, phenylpropionic acid, 3,5-bis(1,1-dimethylethyl)-4-hydroxy-, C7-C9 side chain alkyl ester, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris[3,5-di-tert-butyl-4-hydroxybenzyl]benzene, tetrakis[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane, bis[3,3'-bis-[(4'-hydroxy-3'-tert-butylphenyl)butyric acid]ethylene glycol ester, 1,3,5-tris[3',5'-di-tert-butyl-4'-hydroxybenzyl]-s-triazine-2,4,6-(1H,3H,5H)trione and tocopherol, etc.
[0191] Examples of the sulfur-based antioxidant include dilauryl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, and distearyl 3,3'-thiodipropionate.
[0192] Examples of the phosphorus compound include triphenylphosphine, diphenyl isodecyl phosphite, 4,4'-butylene-bis(3-methyl-6-tert-butylphenyl di-tridecyl)phosphite, cycloneopentanatetraylbis(octadecylphosphite), tris(nonylphenyl)phosphite, tris(monononylphenyl)phosphite, tris(dinonylphenyl)phosphite, diisodecyl pentaerythritol diphosphite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene (phospha 10-(3,5-di-tert-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 10-decyloxy-9,10-dihydro-9-oxa-10-phosphaphenanthrene, tris(2,4-di-tert-butylphenyl)phosphite, cycloneopentanatetraylbis(2,4-di-tert-butylphenyl)phosphite, cycloneopentanatetraacylbis(2,6-di-tert-butyl-4-methylphenyl)phosphite, and 2,2-methylenebis(4,6-di-tert-butylphenyl)octylphosphite.
[0193] By using an antioxidant, thermal degradation of the hydroxyl-terminated urethane prepolymer (UPH) can be prevented.
[0194] The amount of the antioxidant added is not particularly limited, but is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, and particularly preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the active hydrogen group-containing compound (HC) (preferably a hydroxyl-terminated urethane prepolymer (UPH)).
[0195] As the antioxidant, from the viewpoint of stability and antioxidant effect, it is preferred to use one or more phenolic compounds as free radical scavengers, and it is more preferred to use one or more phenolic compounds as free radical scavengers and one or more phosphorus compounds as peroxide decomposers. Furthermore, as the antioxidant, it is particularly preferred to use a phenolic compound as a free radical scavenger and a phosphorus compound as a peroxide decomposer, and to use these antioxidants and the above-mentioned anti-hydrolysis agent in combination.
[0196] <Ultraviolet light absorber>
[0197] Examples of the ultraviolet absorber include benzophenone compounds, benzotriazole compounds, salicylic acid compounds, oxalic acid anilide compounds, cyanoacrylate compounds, and triazine compounds.
[0198] The amount of ultraviolet light absorber added can be appropriately designed within the range that does not hinder the polymerization of the radical polymerizable monomer (M) initiated and carried out by the active energy ray irradiation, and does not easily initiate the reaction of the radical polymerizable monomer (M) due to the light of fluorescent lamps and ambient light such as sunlight. In the case where the radical polymerizable monomer (M) is ultraviolet curable, the amount of ultraviolet light absorber added is designed according to the type of ultraviolet light absorber, and the wavelength range and cumulative light amount of the ultraviolet light irradiated to the adhesive layer. The amount of ultraviolet light absorber added is preferably 0.01 to 3 parts by mass, more preferably 0.1 to 2.5 parts by mass, and particularly preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the active hydrogen group-containing compound (HC) (preferably a hydroxyl-terminated urethane prepolymer (UPH)).
[0199] <Light Stabilizer>
[0200] Examples of the light stabilizer include hindered amine compounds and hindered piperidine compounds. The amount of the light stabilizer added is not particularly limited, but is preferably 0.01 to 2 parts by mass, more preferably 0.1 to 1.5 parts by mass, and particularly preferably 0.2 to 1 part by mass, relative to 100 parts by mass of the active hydrogen group-containing compound (HC) (preferably a hydroxyl-terminated urethane prepolymer (UPH)).
[0201] (Antistatic Agent (AS))
[0202] The adhesive may contain one or more antistatic agents (AS) as needed. Examples of the antistatic agent (AS) include inorganic salts, ionic liquids, ionic solids, and surfactants, among which ionic liquids and ionic solids are preferred. In addition, "ionic liquids" are also called room temperature molten salts, which are salts that have fluidity at 25°C.
[0203] Examples of the inorganic salt include sodium chloride, potassium chloride, lithium chloride, lithium perchlorate, ammonium chloride, potassium chlorate, aluminum chloride, cupric chloride, ferrous chloride, ferric chloride, ammonium sulfate, potassium nitrate, sodium nitrate, sodium carbonate, and sodium thiocyanate.
[0204] Examples of the ionic liquid containing imidazolium ions include 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1,3-dimethylimidazolium bis(trifluoromethylsulfonyl)imide, and 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide.
[0205] Examples of the ionic liquid containing pyridinium ions include 1-methylpyridinium bis(trifluoromethylsulfonyl)imide, 1-butylpyridinium bis(trifluoromethylsulfonyl)imide, 1-hexylpyridinium bis(trifluoromethylsulfonyl)imide, 1-octylpyridinium bis(trifluoromethylsulfonyl)imide, 1-hexyl-4-methylpyridinium bis(trifluoromethylsulfonyl)imide, 1-hexyl-4-methylpyridinium hexafluorophosphate, 1-octyl-4-methylpyridinium bis(trifluoromethylsulfonyl)imide, 1-octyl-4-methylpyridinium bis(fluorosulfonyl)imide, 1-methylpyridinium bis(perfluoroethylsulfonyl)imide, and 1-methylpyridinium bis(perfluorobutylsulfonyl)imide.
[0206] Examples of the ionic liquid containing ammonium ions include 1-butyl-3-methylpyridinium bis(trifluoromethanesulfonyl)imide, trimethylheptyl ammonium bis(trifluoromethanesulfonyl)imide, N,N-diethyl-N-methyl-N-propyl ammonium bis(trifluoromethanesulfonyl)imide, N,N-diethyl-N-methyl-N-pentylammonium bis(trifluoromethanesulfonyl)imide, N,N-diethyl-N-methyl-N-heptyl ammonium bis(trifluoromethanesulfonyl)imide, and tri-n-butylmethylammonium bis(trifluoromethanesulfonyl)imide.
[0207] In addition, commercially available ionic liquids such as pyrrolidinium salts, phosphonium salts, and sulfonium salts can be used as appropriate.
[0208] Ionic solids are salts of cations and anions, similarly to ionic liquids, but are substances that exhibit solid properties at normal pressure and 25° C. Examples of the cations that are preferred include alkali metal ions, phosphonium ions, pyridinium ions, and ammonium ions.
[0209] As the ionic solid containing an alkali metal ion, for example, there can be cited lithium bisfluorosulfonyl imide, lithium bistrifluoromethylsulfonyl imide, lithium bispentafluoroethylsulfonyl imide, lithium bisheptylfluoropropylsulfonyl imide, lithium bisnonafluorobutylsulfonyl imide, sodium bisfluorosulfonyl imide, sodium bistrifluoromethylsulfonyl imide, sodium bispentafluoroethylsulfonyl imide, sodium bisheptylfluoropropylsulfonyl imide, sodium bisnonafluorobutylsulfonyl imide, potassium bisfluorosulfonyl imide, potassium bistrifluoromethylsulfonyl imide, potassium bispentafluoroethylsulfonyl imide, potassium bisheptylfluoropropylsulfonyl imide and potassium bisnonafluorobutylsulfonyl imide.
[0210] Examples of the ionic solid containing phosphonium ions include tetrabutylphosphonium bis(fluorosulfonyl)imide, tetrabutylphosphonium bis(trifluoromethylsulfonyl)imide, tetrabutylphosphonium bis(pentylfluoroethylsulfonyl)imide, tetrabutylphosphonium bis(heptylfluoropropyl)sulfonyl)imide, tetrabutylphosphonium bis(nonafluorobutyl)sulfonylimide, tributylhexadecylphosphonium bis(fluorosulfonyl)imide, tributylhexadecylphosphonium bis(trifluoromethylsulfonyl)imide, and tributylphosphonium bis(trifluoromethyl)sulfonyl)imide. Butyl hexadecylphosphonium bispentafluoroethylsulfonyl imide, tributyl hexadecylphosphonium bisheptylfluoropropylsulfonyl imide, tributyl hexadecylphosphonium bisnonafluorobutylsulfonyl imide, tetraoctylphosphonium bisfluorosulfonyl imide, tetraoctylphosphonium bistrifluoromethylsulfonyl imide, tetraoctylphosphonium bispentafluoroethylsulfonyl imide, tetraoctylphosphonium bisheptylfluoropropylsulfonyl imide, and tetraoctylphosphonium bisnonafluorobutylsulfonyl imide.
[0211] Examples of the ionic solid containing pyridinium ions include 1-hexadecyl-4-methylpyridinium bisfluorosulfonyl imide, 1-hexadecyl-4-methylpyridinium bistrifluoromethylsulfonyl imide, 1-hexadecyl-4-methylpyridinium bispentylfluoroethylsulfonyl imide, 1-hexadecyl-4-methylpyridinium bisheptylfluoropropylsulfonyl imide, and 1-hexadecyl-4-methylpyridinium bisnonafluorobutylsulfonyl imide.
[0212] Examples of the ionic solid containing ammonium ions include dodecyltrimethylammonium chloride, tributylmethylbistrifluoromethylsulfonylimide, tributylmethylbispentafluoroethylsulfonylimide, tributylmethylbisheptafluoropropylsulfonylimide, tributylmethylmethylenebisnonafluorobutylsulfonylimide, octyltributylbistrifluoromethylsulfonylimide, octyltributylbispentafluoroethylsulfonylimide, octyltributylbisheptafluoropropylsulfonylimide, octyltributylbisnonafluorobutylsulfonylimide, tetrabutylbisfluorosulfonylimide, tetrabutylbistrifluoromethylsulfonylimide, tetrabutylbispentafluoroethylsulfonylimide, tetrabutylbisheptafluoropropylsulfonylimide, and tetrabutylbisnonafluorobutylsulfonylimide.
[0213] As the cation, known ionic solids such as pyrrolidinium ion, imidazolium ion, and sulfonium ion can be used as appropriate.
[0214] Examples of the surfactant include nonionic surfactants and anionic surfactants, and both types are classified into low-molecular surfactants and high-molecular surfactants.
[0215] Examples of the nonionic low-molecular surfactant include glycerol fatty acid esters, polyoxyalkylene ethers, polyoxyalkylene phenyl ethers, polyoxyalkylene amines, polyoxyalkylene amine fatty acid esters, and fatty acid diethanolamides.
[0216] Examples of the anionic low-molecular surfactant include alkyl sulfonates, alkylbenzene sulfonates, and alkyl phosphates.
[0217] Examples of the amphoteric low-molecular surfactant include alkyl betaine and alkyl imidazolium betaine.
[0218] Examples of the nonionic polymer surfactant include polyether ester amide type, ethylene oxide-epichlorohydrin type, and polyether ester type.
[0219] Examples of the anionic polymer surfactant include polystyrene sulfonic acid type surfactants.
[0220] Examples of the amphoteric polymer surfactant include amino acid-type amphoteric surfactants such as higher alkylaminopropionates, and betaine-type amphoteric surfactants such as higher alkyl dimethyl betaine and higher alkyl dihydroxyethyl betaine.
[0221] The amount of the antistatic agent (AS) added is preferably 0.01 to 10 parts by mass, more preferably 0.03 to 5 parts by mass, based on 100 parts by mass of the active hydrogen group-containing compound (HC).
[0222] (Leveling agent)
[0223] The adhesive may contain a leveling agent as required. By adding a leveling agent, the leveling property of the adhesive layer can be improved. As the leveling agent, acrylic leveling agents, fluorine leveling agents, and silicone leveling agents can be listed. From the viewpoint of suppressing contamination of the adherend after the adhesive sheet is peeled off again, acrylic leveling agents are preferably used.
[0224] There is no particular limitation on the amount of the leveling agent added, but from the viewpoint of suppressing contamination of the adherend after the adhesive sheet is peeled off again and improving the leveling property of the adhesive layer, the amount is preferably 0.001 to 2 parts by mass, more preferably 0.01 to 1.5 parts by mass, and particularly preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the active hydrogen group-containing compound (HC) (preferably a hydroxyl-terminated urethane prepolymer (UPH)).
[0225] (Other optional ingredients)
[0226] The adhesive may contain other arbitrary components as required within the scope of not damaging the effect of the present invention. As other arbitrary components, catalysts, other resins other than urethane resins, fillers (talc, calcium carbonate, and titanium oxide, etc.), metal powders, colorants (pigments, etc.), foils, softeners, conductive agents, silane coupling agents, lubricants, corrosion inhibitors, heat stabilizers, weather stabilizers, inhibitors, and defoamers, etc. can be listed.
[0227] When the adhesive contains a catalyst, it is preferable to add a known catalyst inhibitor such as acetylacetone in order to increase the pot life of the adhesive.
[0228] (Mix ratio)
[0229] The adhesive contains:
[0230] One or more non-radical polymerizable active hydrogen group-containing compounds (HC) having a plurality of active hydrogen groups and no (meth)acryloyl group;
[0231] One or more radical polymerizable monomers (M) comprising one or more radical polymerizable active hydrogen group-containing monomers (MH) having one or more active hydrogen groups and two or more (meth)acryloyl groups;
[0232] a polyfunctional isocyanate compound (I); and
[0233] Gas generating agent (G).
[0234] These mixing ratios are not particularly limited, but preferred mixing ratios are as follows.
[0235] The amount of the at least one polyfunctional isocyanate compound (I) is preferably 1 to 40 parts by mass, more preferably 3 to 40 parts by mass, and particularly preferably 5 to 35 parts by mass, relative to 100 parts by mass of at least one active hydrogen group-containing compound (HC) (preferably at least one hydroxyl-terminated urethane prepolymer (UPH)). If the amount of the at least one polyfunctional isocyanate compound (I) is 1 part by mass or more, the cohesive force of the adhesive layer is good, and if it is 40 parts by mass or less, the pot life is good.
[0236] The amount of the one or more radically polymerizable active hydrogen group-containing monomers (MH) relative to 100 parts by mass of the one or more active hydrogen group-containing compounds (HC) (preferably one or more hydroxyl-terminated urethane prepolymers (UPH)) is preferably 2 parts by mass to 150 parts by mass, more preferably 2 parts by mass to 95 parts by mass, particularly preferably 2 parts by mass to 50 parts by mass, and most preferably 2 parts by mass to 35 parts by mass from the viewpoint of adhesive strength before irradiation with active energy rays.
[0237] The amount of the one or more radically polymerizable active hydrogen group-containing monomers (MH) relative to 100 parts by mass of the one or more active hydrogen group-containing compounds (HC) (preferably one or more hydroxyl-terminated urethane prepolymers (UPH)) is preferably 2 to 150 parts by mass, more preferably 10 to 140 parts by mass, particularly preferably 30 to 130 parts by mass, and most preferably 50 to 120 parts by mass, from the viewpoint of the effect of reducing the wettability and spreadability due to irradiation with active energy rays.
[0238] From the viewpoint of balancing the above two required performances, the amount of the one or more radically polymerizable active hydrogen group-containing monomers (MH) is preferably 2 to 150 parts by mass, more preferably 10 to 95 parts by mass, and particularly preferably 30 to 50 parts by mass, relative to 100 parts by mass of the one or more active hydrogen group-containing compounds (HC) (preferably one or more hydroxyl-terminated urethane prepolymers (UPH)). However, when more emphasis is placed on one of the above two required performances, the amount of the one or more radically polymerizable active hydrogen group-containing monomers (MH) can be designed according to the performance that is emphasized.
[0239] As described above, the one or more radical polymerizable monomers (M) may contain one or more other radical polymerizable monomers (MO) other than the active hydrogen group-containing monomer (MH) as required. The amount of the one or more radical polymerizable monomers (M) is preferably 10 to 150 parts by mass, more preferably 30 to 100 parts by mass, relative to 100 parts by mass of the one or more active hydrogen group-containing compounds (HC) (preferably one or more hydroxyl-terminated urethane prepolymers (UPH)).
[0240] From the viewpoint of the effect of improving the releasability by irradiation with active energy rays, the content of the gas generating agent (G) in the adhesive layer is preferably 2 mass % or more, more preferably 3 mass % to 30 mass %, particularly preferably 5 mass % to 20 mass %.
[0241] (Method for producing adhesive)
[0242] The method for producing the adhesive is not particularly limited.
[0243] One or more active hydrogen group-containing compounds (HC), preferably one or more hydroxyl-terminated urethane prepolymers (UPH) synthesized by the above method are prepared. The hydroxyl-terminated urethane prepolymer (UPH) may also be in the form of a solution containing a solvent.
[0244] The adhesive can be produced by adding and mixing the above-mentioned one or more active hydrogen group-containing compounds (HC) (preferably one or more hydroxyl-terminated urethane prepolymers (UPH)), one or more free radical polymerizable monomers (M) including one or more free radical polymerizable active hydrogen group-containing monomers (MH) having one or more active hydrogen groups and two or more (meth)acryloyl groups, a polyfunctional isocyanate compound (I), a gas generating agent (G), and one or more other optional components as required.
[0245] [Adhesive sheet]
[0246] The adhesive sheet of the present invention comprises a substrate sheet and an adhesive layer formed on at least one surface of the substrate sheet. The adhesive layer comprises a coating dried product of the above-mentioned adhesive and has active energy ray curing property. As required, the exposed surface of the adhesive layer can be covered by a release sheet. In addition, the release sheet is peeled off before the adhesive sheet is pasted to the adherend.
[0247] Figure 1 A schematic cross-sectional view of a pressure-sensitive adhesive sheet according to a first embodiment of the present invention is shown. Figure 1 In the figure, reference numeral 10 is an adhesive sheet, reference numeral 11 is a base sheet, reference numeral 12 is an adhesive layer, and reference numeral 13 is a release sheet. The adhesive sheet 10 is a single-sided adhesive sheet in which an adhesive layer is formed on one side of a base sheet.
[0248] Figure 2 A schematic cross-sectional view of a pressure-sensitive adhesive sheet according to a second embodiment of the present invention is shown. Figure 2 In the figure, reference numeral 20 is an adhesive sheet, reference numeral 21 is a base sheet, reference numerals 22A and 22B are adhesive layers, and reference numerals 23A and 23B are release sheets. The adhesive sheet 20 is a double-sided adhesive sheet in which adhesive layers are formed on both sides of a base sheet.
[0249] As the substrate sheet, there is no particular limitation, and resin sheets, paper and metal foil etc. can be cited. The substrate sheet can also be a laminated sheet formed by laminating any one or more layers on at least one surface of these substrate sheets. On the surface of the substrate sheet on the side where the adhesive layer is formed, easy adhesion treatments such as corona discharge treatment and anchor coating agent coating can also be implemented as needed.
[0250] The constituent resin of the resin sheet is not particularly limited, and examples thereof include ester resins such as polyethylene terephthalate (PET); olefin resins such as polyethylene (PE) and polypropylene (PP); ethylene resins such as polyvinyl chloride; amide resins such as nylon 66; urethane resins (including foams); combinations thereof, etc.
[0251] The thickness of the resin sheet other than the polyurethane sheet is not particularly limited, but is preferably 15 μm to 300 μm. The thickness of the polyurethane sheet (including the foam) is not particularly limited, but is preferably 20 μm to 50,000 μm.
[0252] The paper is not particularly limited, and examples thereof include plain paper, coated paper, and art paper.
[0253] The constituent metal of the metal foil is not particularly limited, and examples thereof include aluminum, copper, and combinations thereof.
[0254] The release sheet is not particularly limited, and a known release sheet can be used in which a surface of a base sheet such as a resin sheet or paper is subjected to a known release treatment such as coating with a release agent.
[0255] The thickness of the adhesive layer is not particularly limited and can be appropriately designed according to the application, etc. For applications such as surface protection sheets, it is preferably 0.1 μm to 200 μm, more preferably 30 μm to 200 μm, particularly preferably 50 μm to 200 μm, and most preferably 75 μm to 150 μm.
[0256] When the thickness of the adhesive layer is within the above range, it is easy to obtain an adhesive sheet having sufficient transparency and good UV transmittance as a surface protection sheet for panel displays such as LCDs and touch panel displays, as well as substrates and optical components manufactured or used in their manufacturing processes.
[0257] [Method for producing adhesive sheet]
[0258] The adhesive sheet can be produced by a known method.
[0259] First, an adhesive is applied to the surface of the substrate sheet to form a coating layer including the adhesive. The coating method may be a known method, such as roll coating, comma coating, die coating, reverse coating, screen printing, and gravure coating.
[0260] Next, the coating layer is heated and dried to form an adhesive layer. The heating and drying temperature is not particularly limited, but is preferably about 60° C. to 150° C. The thickness of the adhesive layer (thickness after drying) can be appropriately designed within a range that allows for obtaining a preferred transparency and UV transmittance according to the intended use.
[0261] Next, if necessary, a release sheet is attached to the exposed surface of the adhesive layer by a known method.
[0262] As described above, a single-sided adhesive sheet can be produced.
[0263] By performing the above operation on both sides, a double-sided adhesive sheet can be produced.
[0264] Conversely to the above method, an adhesive may be applied to the surface of the release sheet to form a coating layer including the adhesive, and then the coating layer may be dried by heating to form an adhesive layer, and the base sheet may be laminated on the exposed surface of the adhesive layer.
[0265] The manufacturing method of the adhesive sheet preferably includes a coating step of coating an adhesive on a base sheet, a heating step of heating and drying the formed coating layer to form an adhesive layer, a winding step of winding the obtained adhesive sheet on a winding core to form an adhesive sheet roll, and a curing step of curing the adhesive sheet roll.
[0266] Immediately after the adhesive is prepared, one or more non-radical polymerizable active hydrogen group-containing compounds (HC), one or more radical polymerizable active hydrogen group-containing monomers (MH) having one or more active hydrogen groups and two or more (meth)acryloyl groups, and a polyfunctional isocyanate compound (I) are reacted. The adhesive layer of the adhesive sheet contains their reaction product.
[0267] (UV transmittance)
[0268] When the radical polymerizable monomer (M) is ultraviolet curable, the adhesive sheet of the present invention preferably has appropriate ultraviolet transmittance.
[0269] In this specification, the transmittance at a wavelength of 365 nm is defined as “UV transmittance.” The “UV transmittance” can be measured by the method described in the section of [Examples] later.
[0270] The adhesive layer contained in the adhesive sheet of the present invention absorbs ultraviolet rays, converts the absorbed ultraviolet rays into energy, and performs free radical polymerization and foaming, so the UV transmittance is preferably low. From this point of view, the UV transmittance of the adhesive sheet of the present invention is preferably 82% or less, more preferably 81% or less, particularly preferably 79% or less, and most preferably 75% or less.
[0271] Preferably, when the adherend with the adhesive sheet is irradiated with ultraviolet rays from the substrate sheet side, the ultraviolet rays can reach the contact interface between the adhesive layer and the adherend. From this point of view, the UV transmittance of the adhesive sheet of the present invention is preferably 1% or more, more preferably 10% or more, and particularly preferably 20% or more.
[0272] The UV transmittance varies depending on the type (chemical structure) and amount of the gas generating agent (G), the type (chemical structure) and amount of the sensitizer (RS), the thickness of the adhesive layer, etc. These conditions are preferably adjusted so that the UV transmittance is 82% or less.
[0273] In the present invention, the adhesive layer includes a gas generating agent (G) that absorbs ultraviolet rays and, if necessary, a sensitizer (RS) that absorbs ultraviolet rays, thereby being able to effectively reduce UV transmittance.
[0274] (Haze)
[0275] The adhesive sheet of the present invention is preferably highly transparent when used for panel displays such as LCDs and touch panel displays, and surface protection sheets for substrates and optical components manufactured or used in their manufacturing processes. As an indicator of transparency, a "haze value" can be cited.
[0276] The haze value of the adhesive sheet of the present invention is not particularly limited, but is preferably 3 or less, more preferably 2 the following.
[0277] The haze value can be measured according to, for example, JIS-K7136.
[0278] [How to use the adhesive sheet]
[0279] The first method of using the adhesive sheet of the present invention includes:
[0280] a step of attaching the adhesive sheet of the present invention to the surface of an adherend; and
[0281] A process of irradiating an adhesive sheet attached to the surface of an adherend with active energy rays such as ultraviolet rays and electron beams to reduce the adhesive strength of the adhesive sheet.
[0282] The second method of using the adhesive sheet of the present invention includes:
[0283] A step of attaching an adhesive sheet to the surface of an adherend; and
[0284] The adhesive sheet of the present invention adhered to the surface of an adherend is irradiated with active energy rays to reduce the adhesive strength of the adhesive sheet, and the self-weight adhesion time of the adhesive layer to the acrylic resin plate after the active energy ray irradiation measured by the method described below is set to 30 seconds or more, and the adhesive sheet with reduced adhesive strength is peeled off from the adherend.
[0285] In the manufacturing process of panel displays such as liquid crystal displays (LCDs) and organic electroluminescent displays (OELDs), and touch panel displays, in order to improve productivity, it is preferred that an adherend with an adhesive sheet can be transported at high speed to a processing unit that performs necessary processes. For example, automatic high-speed transportation using a vacuum adsorption member to adsorb, lift, and transport an adherend with an adhesive sheet to a desired location from the adhesive sheet side is being studied. In this automatic high-speed transportation, it is preferred that the adherend with an adhesive sheet has sufficient adhesion so that the adhesive sheet will not peel off from the adherend during the period of adsorption by the vacuum adsorption member. On the other hand, on the adherend with an adhesive sheet after completing the necessary process, it is preferred that the adhesive sheet has a lower adhesion so that the adhesive sheet can be peeled off at high speed. It is preferred that the adhesive sheet can be easily peeled off from the adherend with an adhesive sheet after completing the necessary process.
[0286] The adhesive layer contained in the adhesive sheet of the present invention includes a free radical polymerizable monomer (M) and a gas generating agent (G) that generates gas by irradiating active energy rays. In the adhesive sheet of the present invention, by irradiating active energy rays, the free radical polymerizable monomer (M) is polymerized, the adhesion and wettability of the adhesive layer are reduced, and gas is generated from the adhesive layer. These effects complement each other, and after irradiation with active energy rays, the adhesive sheet can be easily peeled off from the adherend. For example, the adhesive sheet can be easily peeled off from the adherend by blowing, etc., or the adhesive sheet can be naturally peeled off from the adherend.
[0287] The adhesive strength and wettability of the adhesive layer before and after irradiation with active energy rays can be appropriately designed according to the application and use conditions. In terms of the use of the vacuum suction member to convey the adherend with the adhesive sheet at high speed, it is preferably designed as follows.
[0288] The adhesive layer has an adhesive strength of 0.1 gf / 25 mm or more, preferably 0.5 gf / 25 mm or more, particularly preferably 1.0 gf / 25 mm or more, measured using a tensile tester at a peeling speed of 0.3 m / min and a peeling angle of 180° in accordance with JIS Z0237 before irradiation with active energy rays.
[0289] The adhesive layer has an adhesive strength of 26 gf / 25 mm or less, preferably 20 gf / 25 mm or less, and particularly preferably 10 gf / 25 mm or less, as measured using a tensile tester at a peeling speed of 0.3 m / min and a peeling angle of 180° in accordance with JIS Z0237 before irradiation with active energy rays.
[0290] When the adhesive strength of the adhesive layer is equal to or greater than the lower limit, the adherend with the adhesive sheet can have sufficient adhesive strength so that the adhesive sheet does not peel off from the adherend while being sucked by the vacuum suction member.
[0291] When the adhesive strength of the adhesive layer is not less than the above lower limit, the adherend with the adhesive sheet can have sufficient adhesive strength that the adhesive sheet is not easily peeled from the adherend by air blowing.
[0292] When the adhesive strength of the adhesive layer is not more than the above upper limit, the adhesive layer has good removability before active energy ray irradiation, and can be re-adhered.
[0293] The reduction rate of the adhesive strength after irradiation with active energy rays relative to that before irradiation with active energy rays of the adhesive layer is not particularly limited, but is preferably 2 / 3 or less, more preferably 1 / 2 or less, and particularly preferably 1 / 3 or less.
[0294] The "wetting and spreading property" can be evaluated, for example, by the self-weight adhesion time to an acrylic resin plate. In the present specification, the "self-weight adhesion time to an acrylic resin plate" is measured by the following method.
[0295] Hold the two ends of the length direction of the adhesive sheet with a width of 100 mm and a length of 200 mm with both hands, bend the adhesive sheet in a way that the adhesive layer faces outward, and align the two ends of the adhesive sheet with each other. In this state, the adhesive layer in the central part of the adhesive sheet is in contact with the acrylic resin plate. In this state, release the hands holding the two ends. Measure the time from releasing both hands to the entire adhesive layer being in close contact with the acrylic resin plate as the self-weight attachment time. As the acrylic resin plate, for example, "Acrylite L" manufactured by Mitsubishi Rayon can be used.
[0296] The shorter the self-weight adhesion time of the adhesive layer to the acrylic resin plate before irradiation with active energy rays, the better the wettability and spreadability (affinity for the adherend), which is preferred.
[0297] The self-weight adhesion time of the adhesive layer to the acrylic resin plate before irradiation with active energy rays is preferably 15 seconds or less, more preferably 10 seconds or less, and particularly preferably 8 seconds or less.
[0298] When the self-weight adhesion time of the adhesive layer to the acrylic resin plate is 15 seconds, the adhesive layer has sufficient wettability and spreadability to the adherend before irradiation with active energy rays, and the adhesive sheet can be cleanly attached to the adherend without entrapment of air bubbles.
[0299] Generally speaking, acrylic adhesive layers have poor wetting and spreading properties, and the self-weight adhesion time to an acrylic resin plate exceeds 15 seconds.
[0300] Generally speaking, since the urethane adhesive layer has excellent wettability and spreadability, the self-weight adhesion time to the acrylic resin plate before the active energy ray irradiation is less than 15 seconds. In order to improve the wettability and spreadability of the urethane adhesive layer, a plasticizer (P), a radical polymerizable monomer (M) having an alkylene oxide group such as an ethylene oxide (EO) group and a propylene oxide (PO) group, or a radical polymerizable monomer (M) having an alkyl chain, etc. can be used as needed.
[0301] In the present invention, the wettability and spreadability of the adhesive layer can be effectively reduced by irradiating the active energy ray. Preferably, after the active energy ray irradiation, the self-weight adhesion time of the adhesive layer to the acrylic resin plate is more than 30 seconds. If the self-weight adhesion time of the adhesive layer to the acrylic resin plate is more than 30 seconds, the natural re-adhesion of the part that is naturally peeled off due to gas generation can be effectively suppressed.
[0302] As described above, according to the present invention, a urethane-based adhesive sheet can be provided, which has good wettability and spreadability with respect to an adherend before irradiation with active energy rays, has removability for being able to re-adhere to the adherend, can be adhered with an adhesive force that is not easily peeled off from the adherend, and can be easily peeled off from the adherend after irradiation with active energy rays.
[0303] After the active energy ray irradiation, the adhesive sheet may be easily peeled off from the adherend by, for example, air blowing or the like, or may be naturally peeled off from the adherend.
[0304] [use]
[0305] The adhesive sheet of the present invention can be used in the form of tapes, labels, stickers, double-sided tapes, etc. The adhesive sheet of the present invention is preferably used as a surface protection sheet, a cosmetic sheet, an anti-slip sheet, and the like.
[0306] In addition, in this specification, unless otherwise specified, "sheet" is assumed to include "film" and "tape".
[0307] Panel displays such as liquid crystal displays (LCDs) and organic electroluminescent displays (OELDs), and touch panel displays combining the panel displays with touch panels are widely used in electronic devices such as televisions (TVs), personal computers (PCs), mobile phones, and portable information terminals.
[0308] The adhesive sheet of the present invention is preferably used as a surface protection sheet for panel displays such as LCDs and touch panel displays, as well as substrates (glass substrates, and ITO / glass substrates with an ITO (indium tin oxide) film formed on a glass substrate, etc.) and optical components manufactured or used in their manufacturing processes.
[0309] [Example]
[0310] Hereinafter, the synthesis examples, the embodiments and comparative examples involved in the present invention will be described. In addition, in the following description, unless otherwise specified, "parts" refer to parts by mass, "%" refers to mass %, and "RH" refers to relative humidity. Unless otherwise specified, the unit of the amount of blending in the table is "parts by mass". Unless otherwise specified, the amount of the components other than the solvent is the non-volatile component conversion value.
[0311] [Measurement of molecular weight]
[0312] The weight average molecular weight (Mw) and the number average molecular weight (Mn) are measured by gel permeation chromatography (GPC). The measurement conditions are as follows. In addition, Mw and Mn are both polystyrene-equivalent values.
[0313] Device: SHIMADZU Prominence (manufactured by Shimadzu Corporation),
[0314] Column: Three SHODEX LF-804 (manufactured by Showa Denko KK) were connected in series.
[0315] Detector: Differential refractive index detector,
[0316] Solvent: tetrahydrofuran (THF),
[0317] Flow rate: 1mL / min,
[0318] Solvent temperature: 40℃,
[0319] Sample concentration: 0.2%,
[0320] Sample injection volume: 200 μL.
[0321] [Material]
[0322] The materials used are listed below.
[0323] <Active hydrogen group-containing compounds (HX)>
[0324] (HX-1): Kuraray Polyol P-2010, polyester polyol, number average molecular weight Mn is 2000, number of hydroxyl groups is 2, manufactured by Kuraray Co., Ltd.,
[0325] (HX-2): SANNIX GP-3000, polyether polyol, number average molecular weight Mn: 3000, number of hydroxyl groups: 3, manufactured by Sanyo Chemical Industries Ltd.
[0326] (HX-3): SANNIX GL-3000, a polyether polyol having a number average molecular weight Mn of 3000 and a hydroxyl group number of 3, manufactured by Sanyo Chemical Industries, Ltd.
[0327] <Polyisocyanate (N)>
[0328] (N-1): Desmodur H, hexamethylene diisocyanate (HDI), manufactured by Sumika Covestro Urethane Co., Ltd.,
[0329] (N-2): Desmodur T-80, toluene diisocyanate (TDI), manufactured by Sumika Covestro Urethanes Co., Ltd.
[0330] <Polyfunctional isocyanate compound (I)>
[0331] (I-1): Sumidur N3300, urate ester of hexamethylene diisocyanate, non-volatile content 100%, manufactured by Sumika Covestro Urethanes Co., Ltd.
[0332] (I-2): Takenate D-110N, trimethylolpropane adduct of xylene diisocyanate, non-volatile content: 75%, manufactured by Mitsui Chemicals, Inc.
[0333] <Active hydrogen group-containing radically polymerizable monomer (M) (radical polymerizable active hydrogen group-containing monomer (MH))>
[0334] (MH-1): MIRAMER M500, dipentaerythritol pentaacrylate, 5 acryloyl groups, 1 hydroxyl group, manufactured by Miwon Commercial Co., Ltd.
[0335] (MH-2): MIRAMER M340, pentaerythritol triacrylate, the number of acryloyl groups is 3, the number of hydroxyl groups is 1, manufactured by Miwon Trading Co., Ltd.
[0336] <Free Radical Polymerizable Monomer (M) Not Containing Active Hydrogen Group>
[0337] (MO-3): MIRAMER M600, dipentaerythritol hexaacrylate, 6 acryloyl groups, 0 hydroxyl groups, manufactured by Miwon Trading Co., Ltd.
[0338] (MO-4): MIRAMER M220, tripropylene glycol diacrylate, 2 acryloyl groups, 0 hydroxyl groups, manufactured by Miwon Trading Co., Ltd.
[0339] (MO-5): Miramer M202, 1,6-hexanediol ethoxy diacrylate, having 2 acryloyl groups and 0 hydroxyl groups, manufactured by Migen Trading Co., Ltd.
[0340] <Photopolymerization Initiator (RI)>
[0341] (RI-1): Irgacure TPO, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, manufactured by BASF SE,
[0342] (RI-2): SB-PI 712, 4-methylbenzophenone, manufactured by Sanyo Trading Co., Ltd.
[0343] <Gas Generant (G)>
[0344] As the gas generating agent (G), (G-18) and (G-14) shown in Table 1 were prepared.
[0345] <Sensitizer (RS)>
[0346] (RS-1): UVS-1331, a compound represented by the following structural formula, manufactured by Kawasaki Kasei Chemicals Ltd.
[0347] [Chemical formula 1]
[0348]
[0349] <Plasticizer (P)>
[0350] (P-1): Acetyl tributylcitrate (ATBC), manufactured by Mitsubishi Chemical Co., Ltd.
[0351] <Antioxidant (O)>
[0352] (O-1): Irganox 1010, a hindered phenol antioxidant, manufactured by BASF AG.
[0353] <Antistatic Agent (AS)>
[0354] (AS-1): IL-P14, an ionic liquid, manufactured by Koei Chemical Co., Ltd.
[0355] [Synthesis Example of a Solution of a Hydroxyl-Terminated Urethane Prepolymer (UPH)]
[0356] (Synthesis example 1)
[0357] In a four-necked flask equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, a thermometer, and a dropping funnel, 400 parts of an active hydrogen group-containing compound (HX-1), 600 parts of an active hydrogen group-containing compound (HX-2), and 57 parts of a polyisocyanate (N-1) were placed. 705 parts of toluene, 0.1 parts of dibutyltin dilaurate as a catalyst, and 0.04 parts of 2-ethylhexanoic acid tin were added and mixed. The reaction solution was slowly heated to 90° C. and reacted at 90° C. for 2 hours.
[0358] Sampling was performed at any time, and after confirming the disappearance of the residual isocyanate group by infrared absorption (IR) spectroscopy, the reaction solution was cooled to 30° C. to terminate the reaction.
[0359] As described above, a solution of a hydroxyl-terminated urethane prepolymer (UPH1) having a hydroxyl value of 17.1 mgKOH / g (non-volatile content: 60%) was obtained. The weight average molecular weight Mw of the obtained hydroxyl-terminated urethane prepolymer (UPH1) was 83,000. The formulation composition and the Mw and hydroxyl value of the obtained hydroxyl-terminated urethane prepolymer are shown in Table 2.
[0360] (Synthesis Examples 2 to 5)
[0361] In Synthesis Examples 2 to 5, except that the type of active hydrogen group-containing compound (HX), the type of polyisocyanate (N) and their mixing ratio were changed, colorless and transparent solutions of hydroxyl-terminated urethane prepolymers (UPH-2) to hydroxyl-terminated urethane prepolymers (UPH-5) were obtained in the same manner as in Synthesis Example 1. In each synthesis example, the mixing composition and the Mw and hydroxyl value of the obtained hydroxyl-terminated urethane prepolymers are shown in Table 2.
[0362] [Table 2]
[0363]
[0364] [Acrylic resin (AR) synthesis example]
[0365] (Synthesis Example 21)
[0366] In a four-necked flask including a stirrer, a reflux cooling tube, a nitrogen inlet tube, a thermometer, and a dropping funnel, 990 parts of n-butyl acrylate, 10 parts of 4-hydroxybutyl acrylate, and 1000 parts of ethyl acetate were placed and mixed. The content liquid was slowly heated to 90°C, and after confirming that the solvent was refluxed, 2 parts of azobisisobutyronitrile were added and mixed. After 8 hours, the reaction solution was cooled and the reaction was terminated. As described above, a solution of acrylic resin (AR-1) (non-volatile component: 50%) was obtained. The weight average molecular weight Mw of the obtained acrylic resin was 890,000.
[0367] [Manufacture of adhesives and adhesive sheets]
[0368] (Example 1)
[0369] A solution containing 100 parts of the hydroxyl-terminated urethane prepolymer (UPH1) obtained in Synthesis Example 1 was mixed with 5 parts of a polyfunctional isocyanate compound (I-1), 25 parts of a radical polymerizable monomer containing an active hydrogen group (MH-1), 10 parts of a radical polymerizable monomer containing no active hydrogen group (MO-4), 1 part of a photopolymerization initiator (RL-1), 1 part of a photopolymerization initiator (RL-2), 20 parts of a gas generator (G-1), 0.1 parts of an antioxidant (O-1), and 0.1 parts of an antistatic agent (AS-1), and 80 parts of ethyl acetate as a solvent, and stirred with a disperser to obtain a urethane adhesive. In addition, the amount of each material other than the solvent is expressed as the amount of the non-volatile component (the same applies to other examples and comparative examples).
[0370] As a substrate sheet, a 75 μm thick polyethylene terephthalate sheet (double-sided easy-to-attach PET sheet, Cosmoshine A-4300, manufactured by TOYOBO Co., Ltd.) was prepared. The adhesive obtained was applied to one side of the substrate sheet, and heated and dried at 100°C for 5 minutes to form a 75 μm thick adhesive layer. A 38 μm thick peeling sheet (Super stick SP-PET38, manufactured by LINTEC Co., Ltd.) was pasted on the adhesive layer to obtain an adhesive sheet. After curing for 1 week in an environment of 23°C-50% RH, various evaluations were performed.
[0371] The compounding composition of the adhesive, the thickness of the adhesive layer, and the evaluation results are shown in Tables 3 and 7. In addition, in each example of Tables 3 to 6, the conditions not described in the table are common conditions.
[0372] (Example 2 to Example 27, Comparative Example 1 to Comparative Example 6)
[0373] In each of Examples 2 to 27 and Comparative Examples 1 to 6, urethane or acrylic adhesive sheets were produced in the same manner as in Example 1 except that the adhesive composition and the thickness of the adhesive layer were changed as shown in Tables 3 to 6. The evaluation results are shown in Tables 7 to 10.
[0374] (Example 28)
[0375] A urethane adhesive sheet was produced in the same manner as in Example 1 except that the following materials were blended and stirred with a disperser to obtain a urethane adhesive sheet by a single-shot method.
[0376] Active hydrogen group-containing compound (HX-1): 40 parts,
[0377] Active hydrogen group-containing compound (HX-2): 60 parts,
[0378] Polyfunctional isocyanate compound (I-1): 15 parts,
[0379] Dibutyltin dilaurate (catalyst): 0.1 parts,
[0380] 2-Ethylhexanoate Tin (Catalyst): 0.04 parts,
[0381] Radical polymerizable monomer (MH-1): 25 parts,
[0382] Free radical polymerizable monomer (MO-4): 10 parts,
[0383] Photopolymerization initiator (RI-1): 1 part,
[0384] Photopolymerization initiator (RI-2): 1 part,
[0385] Gas generating agent (G-18): 20 parts,
[0386] Antioxidant (O-1): 0.1 parts,
[0387] Antistatic agent (AS-1): 0.1 parts,
[0388] Ethyl acetate (solvent): 80 parts.
[0389] Tables 5 and 9 show the compounding compositions of the adhesives, the thickness of the adhesive layers, and the evaluation results.
[0390] [Evaluation items and evaluation methods]
[0391] Evaluation items and evaluation methods of the adhesive sheet are as follows.
[0392] (Adhesion and removability before ultraviolet (UV) irradiation)
[0393] A test piece with a width of 25 mm and a length of 100 mm was cut from the obtained adhesive sheet and placed in an environment of 23°C-50% RH for 30 minutes. Next, under the same environment, the peeling sheet was peeled off from the test piece, and the exposed adhesive layer side of the test piece was pasted on a stainless steel (SUS) plate, crimped using a 2kg roller, and placed for 24 hours. For the adherend with the obtained adhesive sheet, according to JIS Z0237, a tensile testing machine (TENSILON: manufactured by ORIENTEC CORPORATION) was used to measure the adhesion (adhesion before UV irradiation) at a peeling speed of 0.3 m / min and a peeling angle of 180°. When the adhesion is low, the re-peelability is high and it is easy to re-bond. The evaluation criteria are as follows.
[0394] ◎: 10gf / 25mm or less, excellent.
[0395] ○: More than 10 gf / 25 mm and 20 gf / 25 mm or less, good.
[0396] △: More than 20gf / 25mm and less than 26gf / 25mm, practical.
[0397] x: Over 26gf / 25mm, not practical.
[0398] (Difficulty of peeling by blowing air before UV irradiation)
[0399] A test piece with a width of 100 mm and a length of 100 mm was cut from the obtained adhesive sheet and placed in an environment of 23°C-50% RH for 30 minutes. Next, in the same environment, the peeling sheet was peeled off from the test piece, and the exposed adhesive layer side of the test piece was pasted on an acrylic resin plate ("Acrylite L" manufactured by Mitsubishi Rayon Co., Ltd., with a width of 110 mm and a length of 110 mm) that was one circle larger than the test piece, and placed for 24 hours. The center of the test piece was roughly aligned with the center of the acrylic resin plate.
[0400] The obtained adherend with the adhesive sheet was sprayed with a nozzle having a diameter of 1.0 mm from a position 10 mm away from one end of the adhesive sheet in the horizontal direction. Use an air gun to spray air for 10 seconds at a compressor pump pressure of 0.3 MPa to check whether the adhesive sheet is peeled off.
[0401] The above test was performed on 20 test pieces, and the number of test pieces peeled off (peeling number) was investigated. When the adhesive sheet was not peeled off for all test pieces (i.e., the peeling number was 0), in the manufacturing process of LCD and touch panel display, the adhesive sheet was difficult to peel off from the adherend with the adhesive sheet, so it was good.
[0402] ◎: The number of peeling pieces was 0, which was excellent.
[0403] ×: The number of peelings is 1 to 20, which is not practical.
[0404] (Self-adhesion before ultraviolet (UV) irradiation (wetting and spreading ease))
[0405] A test piece of 100 mm in width and 200 mm in length was cut from the obtained adhesive sheet and left to stand in an environment of 23°C and 50% RH for 30 minutes. Next, the release sheet was peeled off from the test piece in the same environment, and the self-weight adhesion was evaluated as follows.
[0406] Hold the two ends of the adhesive sheet in the length direction with both hands, bend the adhesive sheet in a way that the adhesive layer faces outward, and align the two ends of the adhesive sheet with each other. In this state, make the adhesive layer in the central part of the adhesive sheet contact with the acrylic resin plate ("Acrylite L" manufactured by Mitsubishi Rayon Co., Ltd.). In this state, release the hands holding the two ends. Measure the time from releasing the hands to the entire adhesive layer and the acrylic resin plate clinging to each other due to their own weight as the self-weight adhesion time, and evaluate the wetting and expansion of the adhesive.
[0407] The shorter the self-weight adhesion time is, the better the wetting and spreading property (affinity for the adherend) is. The evaluation criteria are as follows.
[0408] ◎: The self-weight adhesion time is 8 seconds or less, which is excellent.
[0409] ○: The self-weight adhesion time is more than 8 seconds and less than 10 seconds, which is good.
[0410] △: The self-weight adhesion time is more than 10 seconds and less than 15 seconds, which is practical.
[0411] ×: The self-weight attachment time exceeds 15 seconds and is not practical.
[0412] (Ultraviolet (UV) transmittance)
[0413] A test piece of 20 mm in width and 40 mm in length was cut from the obtained adhesive sheet and placed in an environment of 23°C-50% RH for 30 minutes. Next, under the same environment, the peeling sheet was peeled off from the test piece, and the transmission spectrum was measured using a spectrophotometer ("V-750" manufactured by JASCO Corporation). The transmittance (UV transmittance) of the adhesive sheet at a wavelength of 365 nm was measured. The evaluation criteria are as follows.
[0414] ◎: UV transmittance is 81% or less, which is excellent.
[0415] ○: The UV transmittance is more than 81% and less than 82%, which is good.
[0416] ×: UV transmittance exceeds 82%, which is not practical.
[0417] (Foaming due to ultraviolet (UV) irradiation)
[0418] A test piece with a width of 25 mm and a length of 100 mm was cut from the obtained adhesive sheet and placed in an environment of 23°C-50% RH for 30 minutes. Next, in the same environment, the peeling sheet was peeled off from the test piece, and the exposed adhesive layer side of the test piece was attached to an acrylic resin plate ("Acrylite L" manufactured by Mitsubishi Rayon Co., Ltd.), pressed using a 2 kg roller, and placed for 24 hours.
[0419] Next, the test piece was irradiated with ultraviolet light (UV) from the PET sheet side as the substrate sheet using a high-pressure mercury lamp (peak wavelength: 254nm, 365nm, 405nm and 435nm, output power: 120W) under the condition of cumulative light quantity of 1000mJ. After air cooling for 1 hour under the environment of 23℃-50%RH, the area of the part where the adhesive sheet and the acrylic resin plate were in close contact was measured, and the close contact area ratio was calculated based on the following formula. The evaluation criteria are as follows.
[0420] [Close contact area ratio (%)] = [Area of close contact part (cm 2 )] / 25(cm 2 )
[0421] ◎: The close contact area ratio is 5% or less, which is excellent.
[0422] ○: The close contact area ratio is more than 5% and less than 20%, which is good.
[0423] △: The close contact area ratio is more than 20% and less than 70%, which is practically applicable.
[0424] ×: The close contact area ratio exceeds 70%, which is not practical.
[0425] (Ease of peeling by air blowing after ultraviolet (UV) irradiation)
[0426] Using the same method as the evaluation of "difficulty of peeling due to air blowing before ultraviolet (UV) irradiation", a test piece with a width of 100 mm and a length of 100 mm was cut from the obtained adhesive sheet, the peeling sheet was peeled off, and the exposed adhesive layer side was adhered to a larger acrylic resin plate and left for 24 hours.
[0427] Next, the test piece was irradiated with ultraviolet light (UV) from the PET sheet side as the substrate sheet by the same method as the evaluation of "foaming property due to ultraviolet (UV) irradiation", and air-cooled for 1 hour in an environment of 23°C and 50%RH.
[0428] By the same method as the evaluation of "difficulty of peeling by air blowing before ultraviolet (UV) irradiation", air was blown to the adherend with the adhesive sheet after UV irradiation to confirm whether the adhesive sheet was peeled.
[0429] The above test was performed on 20 test pieces to investigate the number of test pieces that were peeled off (peeling number). Unlike before UV irradiation, after UV irradiation, the more peeling numbers there were, the easier it was to peel off from the adherend, so it was good, and peeling of the adhesive sheet of all test pieces (i.e., peeling number was 20) was the most preferred.
[0430] The above-mentioned peeling by air blowing does not require a step of holding the end of the adhesive sheet by hand or with a jig, and a step of peeling the adhesive sheet, and can be regarded as natural peeling or a level close to natural peeling.
[0431] ◎: The number of peelings was 20, which was excellent.
[0432] ○: The number of peeling pieces was 10 to 19, which was good.
[0433] △: The number of peelings is 1 to 10, which is practical.
[0434] ×: The number of peeling pieces is 0, which is not practical.
[0435] (Self-adhesion after ultraviolet (UV) irradiation (wetting and spreading difficulty))
[0436] A test piece having a size of 100 mm in width and 200 mm in length was cut out from the obtained adhesive sheet and left to stand in an environment of 23° C. and 50% RH for 30 minutes.
[0437] Next, the test piece was irradiated with ultraviolet light (UV) from the PET sheet side as the substrate sheet by the same method as the evaluation of "foaming property due to ultraviolet light (UV)", and air-cooled for 1 hour in an environment of 23°C and 50%RH.
[0438] Next, under the same environment, the release sheet was peeled off from the test piece, and the self-weight adhesion was evaluated as follows.
[0439] Hold the two ends of the adhesive sheet in the length direction with both hands, bend the adhesive sheet so that the adhesive layer faces outward, and align the two ends of the adhesive sheet with each other. In this state, make the adhesive layer in the center of the adhesive sheet contact with an acrylic resin plate ("Acrylite L" manufactured by Mitsubishi Rayon Co., Ltd.). In this state, release the hands holding the two ends.
[0440] 30 seconds after releasing both hands, measure the area of the part where the adhesive sheet and the acrylic resin plate are in close contact, and calculate the close contact area ratio based on the following formula. The smaller the close contact area ratio, the more difficult it is to re-adhere to the acrylic resin plate naturally, and the better. The evaluation criteria are as follows.
[0441] [Close contact area ratio (%)] = [Area of close contact part (cm 2 )] / 200(cm 2 )
[0442] ◎: The close contact area ratio after 30 seconds was 0%, which was excellent.
[0443] ○: The close contact area ratio after 30 seconds was more than 0% and 10% or less, which was good.
[0444] △: The close contact area ratio after 30 seconds is more than 10% and less than 100%, which is practically applicable.
[0445] ×: The time for the close contact area ratio to reach 100% is less than 30 seconds, or the close contact area ratio after 30 seconds is 100%, which is not practical.
[0446] [Table 3]
[0447]
[0448] [Table 4]
[0449]
[0450] [Table 5]
[0451]
[0452] [Table 6]
[0453]
[0454] [Table 7]
[0455]
[0456] [Table 8]
[0457]
[0458] [Table 9]
[0459]
[0460] [Table 10]
[0461]
[0462] [Summary of evaluation results]
[0463] The adhesive layers of the adhesive sheets obtained in Examples 1 to 28 had a self-weight adhesion time to the acrylic resin plate of 15 seconds or less, and had good wetting and spreading properties to the adherend.
[0464] The adhesive sheets obtained in these Examples all had appropriate adhesive strength before UV irradiation, had removability to allow re-adherence to an adherend, and could be attached with such an adhesive strength that they were not easily peeled off from an adherend even by air blowing.
[0465] The UV transmittance of the adhesive sheets obtained in these Examples was 20% or more and 82% or less, and the UV transmittance and UV absorbency were good.
[0466] In each of the adhesive sheets obtained in these Examples, generation of gas from the adhesive layer due to UV irradiation was clearly observed with the naked eye, and the contact area ratio of the adhesive sheet to the adherend was effectively reduced.
[0467] The adhesive sheets obtained in these examples were all polymerized by UV irradiation to polymerize the radical polymerizable monomer (M) to reduce the adhesive force and wettability of the adhesive layer, and gas was generated from the adhesive layer, so that after UV irradiation, they could be easily peeled off from the adherend only by blowing air. The peelability after UV irradiation was natural peeling or a level close to natural peeling.
[0468] The adhesive sheet of Comparative Example 1 using an acrylic adhesive containing a radical polymerizable monomer (M) and a gas generating agent (G) had very high adhesive strength before UV irradiation and poor removability. Furthermore, the self-weight adhesion time to the acrylic resin plate before UV irradiation exceeded 15 seconds, and the wetting and spreading properties to the adherend were poor.
[0469] The adhesive sheet obtained in Comparative Example 2 using a urethane adhesive that does not contain a free radical polymerizable monomer (M) and a gas generating agent (G) has moderate adhesive strength before UV irradiation, has removability that allows it to be re-adhered to the adherend, and can be adhered with an adhesive strength that is not easily peeled off from the adherend even when air is blown.
[0470] The adhesive sheet obtained in this comparative example had a UV transmittance exceeding 82% and had poor UV absorption.
[0471] Furthermore, since the adhesion and wettability of the adhesive layer are not reduced due to polymerization of the radical polymerizable monomer (M) during UV irradiation and gas is not generated from the adhesive layer, air blow peeling and wettability reduction effects are not obtained after UV irradiation.
[0472] The adhesive sheet obtained in Comparative Example 3 using the urethane adhesive containing no radical polymerizable monomer (M) and a small amount of the gas generating agent (G) had a UV transmittance exceeding 82%, and had poor UV absorption.
[0473] In this comparative example, when UV irradiation is performed, since the adhesion and wettability of the adhesive layer are not reduced due to polymerization of the free radical polymerizable monomer (M), and less gas is generated from the adhesive layer, the effect of air blowing peeling and reduced wettability is not obtained after UV irradiation. Even if UV irradiation is performed, the wettability remains high, so even if there is a part that is peeled off due to gas generation, it is easy to re-adhere naturally, and the peelability will not be improved.
[0474] The adhesive sheet obtained in Comparative Example 4 using a urethane adhesive containing no radical polymerizable monomer (M) but a large amount of a gas generating agent (G) generates a lot of gas from the adhesive layer when UV irradiated, but the adhesion and wettability of the adhesive layer are not reduced due to the polymerization of the radical polymerizable monomer (M), so after UV irradiation, the effects of air-blowing peeling and reduced wettability are not obtained. Even after UV irradiation, the wettability remains high, so even if there is a part that is peeled off due to gas generation, it is easy to re-adhere naturally, and the peelability will not be improved.
[0475] The adhesive sheet obtained in Comparative Example 5 using the urethane adhesive containing the radical polymerizable monomer (M) but not containing the gas generating agent (G) had a UV transmittance exceeding 82%, indicating poor UV absorption.
[0476] In this comparative example, although the adhesion and wettability of the adhesive layer were reduced due to polymerization of the radical polymerizable monomer (M) during UV irradiation, no air blow peeling effect was obtained after UV irradiation because no gas was generated.
[0477] The adhesive sheet obtained in Comparative Example 6, which did not contain a gas generating agent (G) and used a urethane adhesive in which the amount of free radical polymerizable monomer (M) used was reduced compared to Comparative Example 5, had a UV transmittance of more than 82%, and had poor UV absorption. In addition, when UV irradiation was performed, since the adhesion and wettability of the adhesive layer were hardly reduced due to the polymerization of the free radical polymerizable monomer (M), and almost no gas was generated from the adhesive layer, after UV irradiation, the effects of air blowing peeling and reduced wettability were not obtained.
[0478] The present invention is not limited to the above-described embodiments and examples, and design changes can be appropriately made without departing from the scope of the gist of the present invention.
[0479] Description of Reference Numerals
[0480] 10, 20 adhesive sheet
[0481] 11, 21 substrate sheet
[0482] 12, 22A, 22B Adhesive layer
[0483] 13, 23A, 23B peeling sheet
Claims
1. An adhesive sheet comprising a base sheet and an adhesive layer formed on the base sheet and having active energy ray curability, wherein: The adhesive layer comprises: One or more non-radical polymerizable active hydrogen group-containing compounds (HC) having two or more active hydrogen groups and no (meth)acryloyl group, one or more radical polymerizable monomers (M) containing one or more radical polymerizable active hydrogen group-containing monomers (MH) having one or more active hydrogen groups and two or more (meth)acryloyl groups, trifunctional or higher functional isocyanate compound (I), and A gas generating agent (G) that generates gas by irradiation with active energy rays, a dried product of an adhesive coating, The adhesive layer has an adhesive force of 0.1 gf / 25 mm to 26 gf / 25 mm when measured using a tensile tester at a peeling speed of 0.3 m / min and a peeling angle of 180° in accordance with JIS Z0237.
2. The adhesive sheet according to claim 1, wherein The transmittance at a wavelength of 365 nm is 1% to 82%.
3. The adhesive sheet according to claim 1 or 2, wherein The content of the gas generating agent (G) in the adhesive layer is 2% by mass or more.
4. The adhesive sheet according to claim 1 or 2, wherein The gas generating agent is a nitrogen-containing compound that contains an N═N bond and generates nitrogen gas upon irradiation with active energy rays.
5. The adhesive sheet according to claim 4, wherein The gas generating agent includes at least one of an azo compound, an azide compound, a tetrazole compound, a tetrazole compound salt and a bistetrazole compound.
6. The adhesive sheet according to claim 4, wherein The N2 generation volume of the gas generating agent theoretically calculated from the chemical formula per 1 g of the gas generating agent is 30 mL / g to 400 mL / g.
7. The adhesive sheet according to claim 1 or 2, wherein The one or more active hydrogen group-containing monomers (MH) include one or more pentafunctional or higher active hydrogen group-containing monomers (MHF) having one or more active hydrogen groups and five or more (meth)acryloyl groups.
8. The adhesive sheet according to claim 1 or 2, wherein The one or more radical polymerizable monomers (M) include one or more pentafunctional or higher active hydrogen group-containing monomers (MHF) having one or more active hydrogen groups and five or more (meth)acryloyl groups, The total amount of one or more pentafunctional or higher radical polymerizable monomers is 70% by mass to 100% by mass based on the total amount of one or more radical polymerizable monomers (M).
9. The adhesive sheet according to claim 1 or 2, wherein The active hydrogen group-containing compound (HC) is a reaction product of one or more active hydrogen group-containing compounds (HX) having two or more active hydrogen groups and one or more polyisocyanates (N), and is a hydroxyl-terminated urethane prepolymer (UPH) having no (meth)acryloyl group.
10. The adhesive sheet according to claim 9, wherein The one or more active hydrogen group-containing compounds (HX) include a trifunctional or higher-functional polyol having three or more hydroxyl groups.
11. The adhesive sheet according to claim 9, wherein The amount of the radical polymerizable monomer (M) is 10 to 150 parts by mass based on 100 parts by mass of the hydroxyl-terminated urethane prepolymer (UPH).
12. The adhesive sheet according to claim 9, wherein The amount of the trifunctional or higher functional isocyanate compound (I) is 5 to 35 parts by mass based on 100 parts by mass of the hydroxyl-terminated urethane prepolymer (UPH).
13. The adhesive sheet according to claim 1 or 2, wherein The self-weight attachment time of the adhesive layer to the acrylic resin plate measured by the following method is less than 15 seconds; Measuring method of self-weight attachment time: Hold the two ends of the adhesive sheet with a width of 100 mm and a length of 200 mm with both hands in the longitudinal direction, bend the adhesive sheet in such a way that the adhesive layer faces outward, and align the two ends of the adhesive sheet with each other; in this state, make the adhesive layer in the center of the adhesive sheet contact with the acrylic resin plate; in this state, release the hands holding the two ends; The time from releasing the hands to the time when the entire adhesive layer and the acrylic resin plate are in close contact is measured as the self-weight attachment time. 14 . The adhesive sheet according to claim 1 or 2, which is used for a surface protection sheet.
15. An adherend with an adhesive sheet, wherein: The adhesive sheet according to any one of claims 1 to 14 is attached to an adherend.
16. A method for using the adhesive sheet according to any one of claims 1 to 14, the method comprising: a step of attaching the adhesive sheet to a surface of an adherend; and The step of irradiating the adhesive sheet attached to the surface of the adherend with active energy rays to reduce the adhesive force of the adhesive sheet.
17. A method for using the adhesive sheet according to any one of claims 1 to 14, the method comprising: a step of attaching the adhesive sheet to a surface of an adherend; and The adhesive sheet attached to the surface of the adherend is irradiated with active energy rays to reduce the adhesive strength of the adhesive sheet, and the self-weight adhesion time of the adhesive layer to the acrylic resin plate after the active energy ray irradiation measured by the following method is set to 30 seconds or more, and the adhesive sheet with reduced adhesive strength is peeled off from the adherend; Measuring method of self-weight attachment time: Holding both ends of the adhesive sheet with a width of 100 mm and a length of 200 mm with both hands in the longitudinal direction, the adhesive sheet is bent in such a way that the adhesive layer faces outward, and the two ends of the adhesive sheet are aligned with each other; in this state, the adhesive layer in the center of the adhesive sheet is brought into contact with the acrylic resin plate; In this state, release the hands holding the two ends; The time from releasing the hands to the time when the entire adhesive layer and the acrylic resin plate are in close contact is measured as the self-weight attachment time.
Citation Information
Patent Citations
Pressure-sensitive adhesive tape
JP2015124301A
Tetrazole compound-basic azo compound complex, adhesive composition, and adhesion tape
JP2016028020A
Control device, control method and program
JP2020095352A
Resin composition for UV-curable adhesive, adhesive and laminate
CN103031104A
Adhesive sheet
CN108300366A