A phenolic resin and its preparation method and application

By optimizing the hydroxyl/aromatic ring ratio and structure in the phenolic resin, combined with the condensation reaction and column separation and purification process, the problems of softening deformation and insufficient adhesion of the phenolic resin at high temperatures were solved, and a resin with high Tg and high adhesion was achieved. Preparation, suitable for high-resolution photoresists.

CN113801279BActive Publication Date: 2024-10-25SHANDONG SHENGQUAN NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202010555602.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-17
Publication Date
2024-10-25
Estimated Expiration
2040-06-17

AI Technical Summary

Technical Problem

Existing phenolic resin softens and deforms when baked at high temperatures, resulting in poor resolution and inability to achieve high-precision microelectronics processing. Its wide molecular weight distribution results in insufficient adhesion and toughness, which affects the application performance of photoresist.

Method used

A phenolic resin was designed with a hydroxyl/aromatic ring ratio of more than 1.05 in its structure, containing polyhydroxyl and polyphenyl rings. Through condensation reaction and column separation and purification process, a resin with high glass transition temperature and high adhesion was prepared. .

Benefits of technology

It achieves high Tg and high adhesion of phenolic resin, improves the heat resistance and narrow molecular weight distribution of photoresist, is suitable for etching preparation of high-resolution fine circuit structures, and the preparation process is environmentally friendly and reduces waste liquid disposal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113801279B_ABST
    Figure CN113801279B_ABST
Patent Text Reader

Abstract

The present invention provides a phenolic resin and a preparation method and application thereof. The phenolic resin provided by the present invention has a structural unit of multiple hydroxyl groups and multiple benzene rings, which gives the phenolic resin a high glass transition temperature, and the hydroxyl groups in the structure are not shielded by large steric groups; the preparation process of the phenolic resin includes a chromatographic column separation step, so that the product has the characteristics of a narrow molecular weight distribution, and a large amount of chemical waste liquid is not generated during the preparation process, which is an environmentally friendly preparation process. The phenolic resin provided by the present invention is suitable for the preparation of positive photoresist, and the photoresist based on the phenolic resin of the present invention has excellent resolution, heat resistance and adhesion to the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a phenolic resin and a preparation method and application thereof. Background Art

[0002] Photolithography and photoresist are the core technologies and key materials in microelectronics. In recent years, the innovation and improvement of microelectronics processing technology has driven the application depth of photoresist in the industry. In the semiconductor chip processing and liquid crystal display FPD manufacturing process, photoresist is used to produce fine circuit patterns, and the fine circuits are formed on the substrate by etching; among them, the positive photoresists used in TFT-LCD, TN / STN, and LED production are mostly based on phenolic resin system photoresists.

[0003] The phenolic resin-diazonaphthoquinone positive photoresist is composed of a linear phenolic resin, a diazonaphthoquinone type photosensitizer, an additive and a solvent. When exposed, the diazonaphthoquinone group is converted into enone, and further generates indene carboxylic acid after contact with water, so that the exposed area is washed away when developing with alkaline water, and an etching image consistent with the pattern on the mask is obtained after development. Based on the performance requirements of the photoresist itself on the linear phenolic resin and the influence of the chemical structure of the linear phenolic resin, this type of photoresist will soften and deform when baked at high temperature, resulting in poor resolution and degradation of the photoresist performance, making it impossible to achieve high-precision microelectronic processing. At present, with the development of refined circuit patterns, the sensitivity and resolution of the photoresist are required to be further improved, and the phenolic resin as a film-forming resin is required to have better high temperature resistance and alkali solubility processing performance.

[0004] The prior art discloses a modified hydroxynaphthol phenol-formaldehyde varnish resin, a method for manufacturing the modified hydroxynaphthol phenol-formaldehyde varnish resin, a photosensitive composition, an anti-corrosion material and a coating film. The modified hydroxynaphthol phenol-formaldehyde varnish resin uses 1-naphthol and 2,7-dihydroxynaphthalene as phenol monomers, reacts with formaldehyde to obtain a naphthol phenol-formaldehyde resin, and then uses a modifier to replace hydrogen in a part of the phenolic hydroxyl groups to obtain a modified naphthol phenol-formaldehyde resin composition in which a part of the hydroxyl groups are blocked.

[0005] The prior art also discloses a method for preparing a high glass transition temperature linear phenolic resin for use in high-resolution photoresist compositions. The high glass transition temperature linear phenolic resin uses formaldehyde as an aldehyde monomer, and polysubstituted phenols such as 3,5-dimethylphenol, resorcinol, etc. as phenolic monomers. A linear phenolic resin having a glass transition temperature higher than 120°C is obtained through a condensation reaction between the aldehyde monomer and the phenolic monomer.

[0006] However, although high Tg phenolic resin can be obtained by increasing the density of benzene rings in the polymer chain segments, the large steric hindrance effect of the benzene rings causes the phenolic hydroxyl groups in the phenolic resin to be shielded, thereby affecting the substrate adhesion and toughness of the phenolic resin in the later application in the field of photoresists; and when the molecular weight distribution of the phenolic resin is wide, the proportion of structural units with low polymerization degree in the phenolic resin is relatively high (for example, more than 7%), resulting in the volatilization of the low molecular weight resin under high temperature conditions when it is later applied to photoresists, the softening and deformation of the pattern, and the reduction of resolution.

[0007] Based on this, developing a phenolic resin with high Tg, high adhesion and narrow molecular weight distribution and a preparation method thereof is a research focus in this field. Summary of the invention

[0008] In view of the deficiencies in the prior art, the object of the present invention is to provide a phenolic resin and a preparation method and application thereof, wherein the structural unit of the phenolic resin contains multiple hydroxyl groups and aromatic groups, giving the phenolic resin the characteristics of high Tg and high adhesion.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a phenolic resin, wherein the ratio of hydroxyl groups to aromatic rings in the phenolic resin structure is greater than 1.05, and optionally less than 1.3 or 1.25. The aromatic rings refer to six-membered carbon rings connected in the form of conjugated chemical bonds, including six-membered rings contained in condensed ring compounds. When calculating the aromatic rings, the number of aromatic rings of each six-membered carbon ring is 1, for example, the number of aromatic rings of the naphthalene ring resin is 2, the number of aromatic rings of the anthracene ring is 3, and so on.

[0011] Furthermore, the ratio of hydroxyl group to aromatic ring in the phenolic resin structure is greater than 1.1.

[0012] Furthermore, the content of dimer components in the phenolic resin is less than 5% (calculated based on the area percentage of the corresponding peak by gel permeation chromatography).

[0013] According to an optional embodiment of the present invention, the phenolic resin has a structure as shown in Formula I:

[0014]

[0015] R 01 , R 03 is selected from substituted or unsubstituted monohydroxyphenol, polyhydroxyphenol or naphthol, R 02 is selected from H, substituted or unsubstituted monohydroxyphenol, polyhydroxyphenol or naphthol, R 04 Selected from H, halogen, C1~C 30 Acyclic or cycloalkyl, C1~C 30 Acyclic or cycloalkenyl, C1~C30 Acyclic or cycloalkynyl, substituted or unsubstituted C6~C 30 Aryl; R 04 Further, C1-C6 non-cyclic or cycloalkyl, C1-C6 non-cyclic or cycloalkenyl, C1-C6 non-cyclic or cycloalkynyl, substituted or unsubstituted C1-C 10 Aryl.

[0016] The substitution includes mono-substitution or poly-substitution, and the poly-substitution number is 2 to 3; n is an integer of 0 to 350 (0, 1, 2, 3, ..., any positive integer of 350);

[0017] The substituted substituents include halogen, hydroxyl, C1-C 30 Straight or branched alkyl, C1~C 30 Straight or branched alkenyl, C1~C 30 Straight chain or branched chain alkynyl, C1~C 30 Alkoxy or C6~C 30 Aromatic hydrocarbon group; preferably halogen, C1~C 10 Straight or branched alkyl, C1~C 10 Straight or branched alkenyl, C1~C 10 Straight chain or branched chain alkynyl, C1~C 10 Alkoxy or C6~C 10 Aromatic hydrocarbon group; more preferably halogen, C1-C6 straight chain or branched alkyl, C1-C6 straight chain or branched alkenyl, C1-C6 straight chain or branched alkynyl, C1-C6 alkoxy or C6-C 10 Aromatic hydrocarbon group.

[0018] The term "C1-C 30 "Alkenyl" refers to an unsaturated straight or branched hydrocarbon group having 2 to 30 carbon atoms and one free valence. Unsaturation means that the alkenyl contains at least one CC double bond. For example, ethenyl, 1-propenyl, 2-propenyl, 1-n-butenyl, 2-n-butenyl, isobutenyl, 1-pentenyl, 1-hexenyl, 1-heptenyl, 1-octenyl, 1-nonenyl, 1-decenyl, etc.

[0019] The term "C1-C 30 "Alkynyl" refers to an unsaturated straight or branched hydrocarbon group having 2 to 30 carbon atoms and one free valence, wherein the hydrocarbon group contains at least one C-C triple bond. For example, ethynyl, 1-propynyl, 2-propynyl, 1-n-butyl, 2-n-butynyl, isobutyl, 1-pentynyl, 1-hexynyl, -heptynyl, 1-octynyl, 1-nonynyl, 1-decynyl, etc.

[0020] As used herein, the term "C6-C 30"Aryl" means an aromatic 6- to 30-membered hydrocarbon ring or condensed ring having one free valence. Examples of C6-C30 aryl are phenyl and naphthyl.

[0021] Furthermore, R 01 , R 02 , R 03 The phenolic resin structure may be the same or different, and may include substituted or unsubstituted polyhydroxyphenol groups and naphthol groups; and may also include substituted or unsubstituted monohydroxyphenol groups.

[0022] Further, the naphthol can be monohydroxy naphthol or polyhydroxy naphthol. The polyhydroxyl group can be 2-3 hydroxyl groups on the phenol ring.

[0023] Furthermore, in the phenolic resin, the proportion of the component where n=1 is 0-5%; the sum of the proportions where n=2, 3, 4, 5, 6 is 5-30%; and the proportion of the component where n≥7 is 65-95%.

[0024] Furthermore, the sum of the proportions of n=2, 3, 4, 5, and 6 is 10-20%, and the proportion of the components with n≥7 is 70-90%.

[0025] The present invention also provides a phenolic resin, characterized in that the phenolic resin has at least one of the following structures:

[0026]

[0027] Wherein, P1, P2, P3, and P4 are each independently selected from H, halogen, substituted or unsubstituted monohydroxyphenol, polyhydroxyphenol or naphthol, C1-C 30 Acyclic or cycloalkyl, C1~C 30 Acyclic or cycloalkenyl, C1~C 30 Acyclic or cycloalkynyl, substituted or unsubstituted C6~C 30 Aryl, and at least one is selected from substituted or unsubstituted polyhydroxyphenol; wherein K1 is selected from integers of 1 to 5, K2 is selected from integers of 1 to 5, the sum of K1 and K2 is not greater than 6, K3 is selected from integers of 1 to 3; m1 and m2 are integers of 1 to 350, and m1+m2 is not greater than 350, preferably not greater than 150; or,

[0028]

[0029] Wherein, P5, P6, P7, P8 are each independently selected from H, halogen, substituted or unsubstituted monohydroxyphenol, polyhydroxyphenol or naphthol, C1-C 30 Acyclic or cycloalkyl, C1~C 30 Acyclic or cycloalkenyl, C1~C 30Acyclic or cycloalkynyl, substituted or unsubstituted C6~C 30 aryl, and at least one selected from substituted or unsubstituted monohydroxyphenol group, K2 selected from integers of 1 to 5, K4 selected from integers of 2 to 4, K5 selected from integers of 1 to 2; m3 and m4 are integers of 1 to 350, and m3+m4 is not greater than 350, preferably not greater than 150; or,

[0030]

[0031] Among them, P9, P 10 , P 11 , P 12 Each independently selected from H, halogen, substituted or unsubstituted monohydroxyphenol, polyhydroxyphenol or naphthol, C1-C 30 Acyclic or cycloalkyl, C1~C 30 Acyclic or cycloalkenyl, C1~C 30 Acyclic or cycloalkynyl, substituted or unsubstituted C6~C 30 Aryl, and at least one selected from substituted or unsubstituted naphthol, K3 selected from an integer of 1 to 3, K4 selected from an integer of 2 to 4, K5 selected from an integer of 1 to 2; m5 and m6 are integers of 1 to 350, and m5+m6 is not greater than 350, preferably not greater than 150;

[0032] In the formulas (1), (2), and (3), R 001 Selected from hydrogen, halogen, hydroxyl, C1~C 30 Straight or branched alkyl, C1~C 30 Straight or branched alkenyl, C1~C 30 Straight chain or branched chain alkynyl, C1~C 30 Alkoxy or C6~C 30 Aromatic hydrocarbon group; preferably halogen, C1~C 10 Straight or branched alkyl, C1~C 10 Straight or branched alkenyl, C1~C 10 Straight chain or branched chain alkynyl, C1~C 10 Alkoxy or C6~C 10 Aromatic hydrocarbon group; more preferably halogen, C1-C6 straight chain or branched alkyl, C1-C6 straight chain or branched alkenyl, C1-C6 straight chain or branched alkynyl, C1-C6 alkoxy or C6-C 10 Aromatic hydrocarbon group.

[0033] The substitution includes single substitution or multiple substitution, and the number of multiple substitution is 2 to 3; the substituents of the substitution include halogen, hydroxyl, C1 to C 30 Straight or branched alkyl, C1~C 30 Straight or branched alkenyl, C1~C 30 Straight chain or branched chain alkynyl, C1~C 30Alkoxy or C6~C 30 Aromatic hydrocarbon group; preferably halogen, C1~C 10 Straight or branched alkyl, C1~C 10 Straight or branched alkenyl, C1~C 10 Straight chain or branched chain alkynyl, C1~C 10 Alkoxy or C6~C 10 Aromatic hydrocarbon group; more preferably halogen, C1-C6 straight chain or branched alkyl, C1-C6 straight chain or branched alkenyl, C1-C6 straight chain or branched alkynyl, C1-C6 alkoxy or C6-C 10 Aromatic hydrocarbon group.

[0034] Optionally, P1, P2, P3, P4, P5, P6, P7, P8, P9, P 10 , P 11 , P 12 Each is independently selected from H, halogen, substituted or unsubstituted monohydroxyphenol, polyhydroxyphenol or naphthol, C1-C6 acyclic or cycloalkyl, C1-C6 acyclic or cycloalkenyl, C1-C6 acyclic or cycloalkynyl, substituted or unsubstituted C6-C 10 Aryl.

[0035] Furthermore, in the phenolic resin, the proportion of the component where n=1 is 0-5%; the sum of the proportions where n=2, 3, 4, 5, 6 is 5-30%; and the proportion of the component where n≥7 is 65-95%.

[0036] Furthermore, the sum of the proportions of n=2, 3, 4, 5, and 6 is 10-20%, and the proportion of the components with n≥7 is 70-90%.

[0037] According to an optional embodiment of the present invention, the phenolic resin has a repeating unit having a structure as shown in Formula II:

[0038]

[0039] Wherein, R1, R3, R4, R5, R6, and R8 are each independently selected from hydroxyl, halogen, C1-C 30 Straight or branched alkyl, C1~C 30 Straight or branched alkenyl, C1~C 30 Straight chain or branched chain alkynyl, C1~C 30 Alkoxy or C6~C 30 One of the aromatic hydrocarbon groups; preferably hydroxyl, halogen, C1~C 10 Straight or branched alkyl, C1~C 10 Straight or branched alkenyl, C1~C 10 Straight chain or branched chain alkynyl, C1~C 10 Alkoxy or C6~C 10An aromatic hydrocarbon group; more preferably a hydroxyl group, a halogen group, a C1-C6 straight chain or branched chain alkyl group, a C1-C6 straight chain or branched chain alkenyl group, a C1-C6 straight chain or branched chain alkynyl group, a C1-C6 alkoxy group or a C6-C 10 A type of aromatic hydrocarbon group;

[0040] R2 and R7 are each independently selected from hydrogen, halogen, C1-C 30 Straight or branched alkyl, C1~C 30 Straight or branched alkenyl, C1~C 30 Straight chain or branched chain alkynyl, C1~C 30 Alkoxy or C6~C 30 One of the aromatic hydrocarbon groups; preferably hydrogen, halogen, C1~C 10 Straight or branched alkyl, C1~C 10 Straight or branched alkenyl, C1~C 10 Straight chain or branched chain alkynyl, C1~C 10 Alkoxy or C6~C 10 An aromatic hydrocarbon group; more preferably hydrogen, halogen, C1-C6 straight chain or branched alkyl, C1-C6 straight chain or branched alkenyl, C1-C6 straight chain or branched alkynyl, C1-C6 alkoxy or C6-C 10 A type of aromatic hydrocarbon group;

[0041] h, q, i, j are each independently selected from an integer of 0 to 4 (e.g., 0, 1, 2, 3 or 4), k, l, m are each independently selected from an integer of 0 to 3 (e.g., 0, 1, 2 or 3), p is an integer of 0 to 2 (e.g., 0, 1 or 2), p is selected from 2 or 3, and n is an integer of 0 to 350 (e.g., 0, 2, 4, 5, 7, 10, 15, 20, 40, 60, 80, 100, 120, 150, 180, 200, 230, 250, 280, 300 or 330, etc.).

[0042] The C1-C30 include C2, C4, C6, C8, C10, C13, C15, C17, C20, C22, C25, C28 or C29, etc.

[0043] The C6 to C30 include C7, C9, C11, C13, C15, C17, C20, C22, C25, C28 or C29, etc.

[0044] The structural unit of the phenolic resin of the present invention contains a benzene ring and a naphthalene ring, so that the density of the large steric hindered group in the molecular structure is large, which can increase the glass transition temperature T of the phenolic resin. gAt the same time, the number of hydroxyl groups in the repeating structural unit of the phenolic resin is greater than or equal to the number of benzene rings contained, which effectively avoids the shielding effect of the large steric benzene ring on the hydroxyl group, ensuring that the phenolic resin has good adhesion to the substrate when it is later applied to the photoresist. The present invention achieves high T of the phenolic resin through the special design of the structure. g and high adhesion balance.

[0045] Preferably, the weight average molecular weight of the phenolic resin is 2000-40000, for example, 2500, 3000, 4000, 5000, 7000, 9000, 11000, 13000, 15000, 17000, 20000, 25000, 28000, 30000, 35000, 37000 or 39000, more preferably 2500-30000.

[0046] Preferably, the mass percentage of the dimer component in the phenolic resin is less than 5%, for example 4.9%, 4.7%, 4.5%, 4.3%, 4%, 3.5%, 3%, 2.5%, 2%, 1.5% or 1%, etc.

[0047] Furthermore, the phenolic resin has a Tg>100°C, preferably>110°C.

[0048] Furthermore, the phenolic resin has a softening point temperature >140°C, preferably >150°C, and more preferably greater than 155°C.

[0049] Optionally, the phenolic resin has the following structure as a repeating unit:

[0050]

[0051] Herein, n is an integer of 0 to 300, for example, 0, 2, 4, 5, 7, 10, 15, 20, 40, 60, 80, 100, 120, 150, 180, 200, 230, 250, 270 or 290, and is preferably an integer of 1 to 150.

[0052] In another aspect, the present invention provides a method for preparing the phenolic resin as described above, the method comprising the following steps:

[0053] (1) adding a phenolic compound, an aldehyde compound and a catalyst into a reaction device for condensation reaction to obtain a crude product; (2) purifying the crude product obtained in step (1) by a chromatographic column separation method to obtain the phenolic resin.

[0054] In the preparation process, a purification step of chromatographic column separation is added to effectively separate the products with low polymerization degree in the crude product, and obtain a phenolic resin with a narrow molecular weight distribution, which can improve the high resolution of the photoresist prepared using the phenolic resin. In addition, compared with methods such as water washing and extraction, the chromatographic column separation method of the present invention has high separation efficiency, the solvent involved can be recycled, and the burden of waste liquid treatment is reduced, which is an environmentally friendly preparation process.

[0055] Furthermore, the phenolic compound in step (1) includes substituted or unsubstituted monohydroxyphenol, polyhydroxyphenol and naphthol compounds; wherein,

[0056] The substitution includes mono-substitution or poly-substitution, and the poly-substitution number is 2 to 3;

[0057] The substituted substituents include halogen, C1-C 30 Straight or branched alkyl, C1~C 30 Alkoxy or C6~C 30 Aromatic hydrocarbon group; preferably halogen, C1~C 10 Straight or branched alkyl, C1~C 10 Straight or branched alkenyl, C1~C 10 Straight chain or branched chain alkynyl, C1~C 10 Alkoxy or C6~C 10 Aromatic hydrocarbon group; more preferably halogen, C1-C6 straight chain or branched alkyl, C1-C6 straight chain or branched alkenyl, C1-C6 straight chain or branched alkynyl, C1-C6 alkoxy or C6-C 10 Aromatic hydrocarbon group. The naphthol group can be monohydroxy naphthol or polyhydroxy naphthol. The polyhydroxy group refers to a phenol ring having 1 to 3 phenolic hydroxyl groups.

[0058] Preferably, the molar ratio of the phenolic compound to the aldehyde compound in step (1) is 1:(0.2-1.0), for example 1:0:3, 1:0:4, 1:0:5, 1:0:6, 1:0:7, 1:0:8 or 1:0:9, etc., more preferably 1:(0.4-1.0), and even more preferably 1:(0.5-0.9).

[0059] Preferably, the phenolic compound in step (1) includes monohydroxyphenol, polyhydroxyphenol and naphthol compounds.

[0060] Preferably, the monohydroxyphenol is selected from any one or a combination of at least two of phenol, m-cresol, p-cresol, 2,3-xylenol, 2,4-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, 3,5-xylenol, 2,3,5-trimethylphenol, o-ethylphenol, m-ethylphenol, p-ethylphenol, isopropylphenol, butylphenol, p-tert-butylphenol, p-amylphenol, p-octylphenol, p-nonylphenol, p-cumylphenol, and phenylphenol.

[0061] Preferably, the polyhydroxyphenol is selected from any one or more combinations of resorcinol, alkylresorcinol, pyrogallol, catechol, alkylcatechol, hydroquinone, alkylhydroquinone, pyrogallol, bisphenol A, bisphenol F, bisphenol S, and dihydroxynaphthalene.

[0062] Preferably, the molar ratio of the polyhydric phenol to the monohydric phenol is (0.2-0.6):1, such as 0.35:1, 0.4:1, 0.45:1, 0.5:1, 0.55:1 or 0.6:1.

[0063] Preferably, the naphthol compound is selected from any one or a combination of at least two of 1-naphthol, 2-naphthol, dihydroxynaphthalene, trihydroxynaphthol, 3-hydroxynaphthalene-2-carboxaldehyde, 2-hydroxynaphthalene 1-carboxaldehyde, 1-hydroxynaphthalene 2-carboxaldehyde, 1,5-dihydroxynaphthalene-2-carboxaldehyde, 2,7-dihydroxynaphthalene 1-carboxaldehyde or tetrahydroxynaphthol.

[0064] Preferably, the molar ratio of the naphthol compound to the monohydroxyphenol is (0.1-0.5):1, for example, 0.15:1, 0.2:1, 0.25:1, 0.28:1, 0.3:1, 0.35:1 or 0.45:1, etc.

[0065] Preferably, the aldehyde compound in step (1) is selected from any one of formaldehyde, acetaldehyde, butyraldehyde, furfural, valeraldehyde, trioxymethylene, tetraoxymethylene, polyoxymethylene, acrolein, o-hydroxybenzaldehyde, benzaldehyde, hydroxybenzaldehyde, alkylhydroxybenzaldehyde, and hydroxynaphthaldehyde, or a combination of at least two thereof.

[0066] Preferably, the catalyst in step (1) is an acid catalyst, specifically, an acid catalyst capable of initiating a polycondensation reaction between phenols and aldehydes.

[0067] Preferably, the acidic catalyst is selected from one or a combination of hydrochloric acid, oxalic acid, acetic acid, benzenesulfonic acid, toluenesulfonic acid, phosphoric acid, nitric acid or sulfuric acid.

[0068] Preferably, the amount of the acid catalyst added is 0.1-5% by mass of the phenolic compound, for example, 0.7%, 0.9%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%, etc.

[0069] Preferably, the temperature of the condensation reaction in step (1) is 90-160°C, for example, 92°C, 95°C, 98°C, 100°C, 103°C, 105°C, 108°C, 110°C, 113°C, 115°C, 118°C, 120°C, 125°C or 129°C, etc.

[0070] Preferably, the condensation reaction time in step (1) is 2 to 10 h, for example, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h or 5.5 h.

[0071] Preferably, the condensation reaction in step (1) is carried out under stirring conditions.

[0072] Preferably, the condensation reaction in step (1) is carried out in the presence of a solvent, and the selected organic solvent may be aromatic solvents such as benzene, toluene, and xylene; may also be ketone solvents such as acetone, butanone, methyl isoamyl ketone, and cyclohexanone; may also be monohydric alcohols such as methanol, ethanol, propanol, and butanol; may also be polyhydric alcohols such as ethylene glycol, propylene glycol, diethylene glycol, polyethylene glycol, and glycerol; may also be alcohol ethers such as ethylene glycol methyl ether, ethylene glycol monobutyl ether, ethylene glycol dimethyl ether, and ethylene glycol methyl ethyl ether; may also be cyclic ethers such as 1,3-dioxane, 1,4-dioxane, and tetrahydrofuran; and may be ketones such as acetone, butanone, methyl isobutyl ketone, and cyclohexanone. These solvents may be used alone or in the form of a mixed solvent of two or more.

[0073] Preferably, the steps of the chromatographic column separation method are: dissolving the crude product in an organic solvent to obtain a solution, passing the solution through a silica gel chromatographic column, and removing low-polymerization units with a molecular weight of less than 300 in the crude product.

[0074] Preferably, the organic solvent is acetonitrile.

[0075] Preferably, the stationary phase of the silica gel chromatographic column is C8 or C18 silica gel particles.

[0076] Preferably, the mobile phase of the silica gel chromatography column is selected from any one of acetonitrile, methanol, tetrahydrofuran or water, or a combination of at least two of them.

[0077] Preferably, the preparation method specifically comprises the following steps:

[0078] (1) adding a phenolic compound, an aldehyde compound and an acid catalyst into a reaction device, and carrying out a condensation reaction at 90 to 160° C. under stirring for 2 to 10 hours to obtain a crude product; the molar ratio of the phenolic compound to the aldehyde compound is 1:(0.2 to 1.0), and the amount of the acid catalyst added is 0.1 to 5% of the mass of the phenolic compound;

[0079] (2) dissolving the crude product obtained in step (1) in an organic solvent to obtain a solution, passing the solution through a C8 or C18 silica gel column to remove low-polymerization units with a molecular weight of less than 300 in the crude product, and distilling off excess solvent and monomers to obtain the phenolic resin.

[0080] On the other hand, the present invention also provides a phenolic resin prepared by any of the above preparation methods.

[0081] Optionally, the weight average molecular weight of the phenolic resin as described above is 2000-40000, preferably 2500-30000.

[0082] Optionally, the ratio of hydroxyl groups to aromatic rings in the phenolic resin as described above is greater than 1.05, and optionally less than 1.3 or 1.25. Further, the ratio of hydroxyl groups to aromatic rings in the phenolic resin structure is greater than 1.1.

[0083] Optionally, the mass percentage of the dimer component in the phenolic resin as described above is less than 5%.

[0084] Optionally, the phenolic resin as described above has a Tg>100°C, preferably>110°C.

[0085] Optionally, the phenolic resin as described above has a softening point temperature > 140°C, preferably > 150°C, and more preferably greater than 155°C.

[0086] On the other hand, the present invention provides an application of the phenolic resin as described above in the fields of photoresist preparation, semiconductor chip processing and liquid crystal panel processing.

[0087] In another aspect, the present invention provides a photoresist composition comprising any of the above phenolic resins,

[0088] Furthermore, the photoresist composition also includes a diazonaphthoquinone photosensitizer and the phenolic resin described above.

[0089] Specifically, the photoresist composition further comprises 2-40% by mass of a naphthoquinone diazide photosensitizer, 0-2% by mass of a surfactant, and 40-90% by mass of a solvent.

[0090] The present invention has the following beneficial effects:

[0091] (1) The phenolic resin provided by the present invention has a structural unit of multiple hydroxyl groups and multiple benzene rings, which gives the phenolic resin a high glass transition temperature. The hydroxyl groups in the structure are not shielded by large steric groups, which effectively improves the heat resistance and adhesion of the phenolic resin in applications.

[0092] (2) The phenolic resin provided by the present invention is firstly prepared by condensing a mixed phenol monomer of monohydroxyphenol, polyhydroxyphenol and naphthol with an aldehyde monomer under the action of an acid catalyst to obtain a crude product, and then the crude product is treated by a classification method of chromatographic column separation, and the obtained product has a high Tg and a narrow molecular weight distribution; the phenolic resin of the present invention does not generate a large amount of chemical waste liquid during the preparation process, and is an environmentally friendly preparation process.

[0093] (3) The photoresist based on the phenolic resin of the present invention has excellent developability, heat resistance and substrate adhesion, and is suitable for etching and preparing high-resolution fine circuit structures. BRIEF DESCRIPTION OF THE DRAWINGS

[0094] Figure 1 is the GPC spectrum of Example 1;

[0095] Figure 2 The C13-NMR spectrum of Example 1;

[0096] Figure 3 It is the GPC spectrum of Example 2;

[0097] Figure 4 The C13-NMR spectrum of Example 2;

[0098] Figure 5 It is the GPC spectrum of Example 3;

[0099] Figure 6 The C13-NMR spectrum of Example 3;

[0100] Figure 7 It is the GPC spectrum of Example 4;

[0101] Figure 8 The C13-NMR spectrum of Example 4;

[0102] Fig. 9 It is the GPC spectrum of Comparative Example 1;

[0103] Fig.10 The C13-NMR spectrum of Comparative Example 1 is shown in FIG.

[0104] Fig.11 It is the GPC spectrum of Comparative Example 2;

[0105] Fig.12 The C13-NMR spectrum of Comparative Example 2 is shown in FIG.

[0106] Fig.13 It is the GPC spectrum of Comparative Example 3;

[0107] Fig.14It is the C13-NMR spectrum of Comparative Example 3. DETAILED DESCRIPTION

[0108] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0109] The present invention is specifically described by way of examples and comparative examples. 13 -NMR spectra were measured under the following conditions:

[0110] GPC measurement conditions:

[0111] Measurement device: "HLC-8320GPC" manufactured by TOSOH CORPORATION

[0112] Chromatographic columns: "PLgel 5um MIXED-C 300x7.5mm" manufactured by Agilent (Varian), USA + "PLgel 5um MIXED-D 300x7.5mm" manufactured by Agilent (Varian), USA + "PLgel 5um MIXED-D 300x7.5mm" manufactured by Agilent (Varian), USA + "PLgel5um MIXED-E 300x7.5mm" manufactured by Agilent (Varian), USA.

[0113] Detector: RI (differential refractometer)

[0114] Data processing: "GPC-8320 Model II Data Analysis System Version 2.01" manufactured by TOSOH CORPORATION

[0115] Measurement conditions: column temperature 40°C

[0116] Developing solvent: tetrahydrofuran (THF)

[0117] Flow rate 1.0ml / min

[0118] Sample: A solution containing 1.0% by mass of tetrahydrofuran in terms of resin solid content was filtered through a microfilter (5 μl).

[0119] Standard sample: According to the operation manual of the aforementioned "GPC-8320 Model II Data Analysis System Version 2.01", the following monodisperse polystyrene with a known molecular weight was used.

[0120] "S-0.5" manufactured by Showa Denko K.K.

[0121] "S-0.9" manufactured by Showa Denko K.K.

[0122] "S-1.3" manufactured by Showa Denko K.K.

[0123] "S-1.9" manufactured by Showa Denko K.K.

[0124] "S-3.0" manufactured by Showa Denko K.K.

[0125] "S-3.8" manufactured by Showa Denko K.K.

[0126] "S-4.9" manufactured by Showa Denko K.K.

[0127] "S-7.2" manufactured by Showa Denko K.K.

[0128] "S-10" manufactured by Showa Denko K.K.

[0129] "S-20" manufactured by Showa Denko K.K.

[0130] C13-NMR measurement conditions:

[0131] Device: BrukerAvance III HD 400M NMR spectrometer

[0132] Solvent: dimethyl sulfoxide (DMSO)

[0133] Pulse angle: 45° pulse

[0134] Sample concentration: 15wt%

[0135] Cumulative times: 10,000 times

[0136] Example 1

[0137] This embodiment provides a phenolic resin, which includes the following structure:

[0138]

[0139] The preparation method comprises the following steps:

[0140] (1) 0.4 mol of p-cresol, 0.2 mol of m-cresol, 0.3 mol of resorcinol and 0.15 mol of 3-hydroxynaphthalene 2-carboxaldehyde are added to a reaction kettle, and the temperature is raised to 90° C. with stirring; then 2.2 g of oxalic acid and 0.55 mol of formaldehyde (the raw material is a 37% formaldehyde aqueous solution) are added, and the mixture is heated to reflux with stirring; the mixture is condensed and reacted for 4 hours under stirring and reflux conditions, and dehydrated under reduced pressure to obtain a crude product;

[0141] (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column (eluted with acetonitrile as the mobile phase), and low-polymerization units with a molecular weight of less than 300 in the crude product are removed, and the solvent is distilled off to obtain a phenolic resin having a weight average molecular weight Mw of 4782.

[0142] Among the polymers included in the phenolic resin product obtained by the above preparation method, the proportion of n=0 component (low polymerization degree unit, representing dimer in this embodiment, the same below) is 4.2%, the sum of the proportions of n=1, 2, 3, 4, 5 is 16.92%, and the proportion of components with n≥6 is 78.88%.

[0143] The obtained phenolic resin was dissolved in deuterated dimethyl sulfoxide and tested on a Bruker Avance III HD 400M nuclear magnetic resonance spectrometer to obtain a nuclear magnetic resonance carbon spectrum (NMR-C 13 See the attachment for details Figure 2 .

[0144] Figure 2 The sample has absorption peaks at chemical shifts of 15.6, 19.39, 19.86, 20.13, 21.25, 113.05, 117.24, 131.17, 131.28, 137.54, and 155.32 ppm, corresponding to the m-cresol structure; there are absorption peaks at chemical shifts of 20.77, 20.90, 115.29, 127.68, 128.16, 128.82, 130.85, and 150.43 ppm, corresponding to the p-cresol structure; the substance has absorption peaks at chemical shifts of 107.71, 124.56, 125.64, 127.28, 128.05, 129.55, There are absorption peaks at 131.28, 136.35, 137.54, and 155.32 ppm, corresponding to the 3-hydroxynaphthalene structure; there are absorption peaks at chemical shifts 115.21, 115.29, 116.00, 142.66, 153.13, and 153.19 ppm, corresponding to meta-diphenol; the absorption peaks at 23.9, 29.71, 30.32, 32.12, and 34.94 ppm correspond to the methylene structure provided by formaldehyde, and the absorption peak at 49.34 ppm corresponds to the methine structure provided by 3-hydroxynaphthalene-2-carboxaldehyde. The NMR-C13 spectrum shows that the obtained phenolic resin has a polymer with the chemical structure shown above. According to the peak areas of hydroxyl hydrogen and aromatic ring hydrogen given by the NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 1.13.

[0145] Example 2

[0146] This embodiment provides a phenolic resin, which includes the following structure:

[0147]

[0148] The preparation method comprises the following steps:

[0149] (1) 0.4 mol of m-cresol, 0.4 mol of p-cresol, 0.3 mol of resorcinol and 0.2 mol of 3-hydroxynaphthalene 2-carboxaldehyde are added to a reaction kettle, and the mixture is heated to 95° C. with stirring; then 2.1 g of oxalic acid, 0.55 mol of formaldehyde (the raw material is a 48% formaldehyde aqueous solution) and 0.2 mol of o-hydroxybenzaldehyde are added, and the mixture is heated to reflux with stirring; the mixture is condensed and reacted for 3.5 hours under stirring and reflux conditions, and dehydrated under reduced pressure to obtain a crude product;

[0150] (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column (eluted with acetonitrile as the mobile phase), and low-polymerization units with a molecular weight of less than 300 in the crude product are removed, and the solvent is distilled off to obtain a phenolic resin having a weight average molecular weight Mw of 20748.

[0151] Among the polymers included in the phenolic resin product obtained by the above preparation method, the proportion of n=0 component (low polymerization degree unit) is 4.17%, the sum of the proportions of n=1, 2, 3, 4, 5 is 11.16%, and the proportion of n≥6 components is 84.67%.

[0152] The obtained phenolic resin was dissolved in deuterated acetone and tested on a Bruker Avance III HD 400M nuclear magnetic resonance spectrometer to obtain a nuclear magnetic resonance carbon spectrum (NMR-C 13 See the attachment for details Figure 4 :

[0153] Figure 4The sample has absorption peaks at chemical shifts of 19.80, 19.84, 21.25, 113.00, 118.68, 129.5, 134.2, 137.54, and 155.86 ppm, corresponding to the m-cresol structure; there are absorption peaks at chemical shifts of 20.76, 20.89, 115.23, 127.61, 128.13, 128.85, 130.88, and 150.43 ppm, corresponding to the p-cresol structure; the substance has absorption peaks at chemical shifts of 107.72, 124.52, 127.24, 127.96, 128.07, 129.5, 13 There are absorption peaks at 1.12, 136.32, 137.51, and 155.29 ppm, corresponding to the 3-hydroxynaphthalene structure; there are absorption peaks at chemical shifts 113.0, 113.23, 115.23, 116.01, 142.66, 152.7, and 153.12 ppm, corresponding to meta-diphenol; among them, the absorption peaks at 29.63, 30.25, and 32.07 ppm correspond to the methylene structure provided by formaldehyde, the absorption peak at 59.13 ppm corresponds to the methylene carbon provided by 3-hydroxynaphthalene-2-carboxaldehyde, and the absorption peak at 43.64 ppm corresponds to the methylene carbon of o-hydroxybenzaldehyde. 13 The spectrum shows that the obtained phenolic resin has a polymer with the chemical structure shown above. According to the peak areas of hydroxyl hydrogen and aromatic ring hydrogen given by the NMR hydrogen spectrum, the hydroxyl / aromatic ring ratio is calculated to be 1.10.

[0154] Example 3

[0155] This embodiment provides a phenolic resin, which includes the following structure:

[0156]

[0157] The preparation method comprises the following steps:

[0158] (1) 0.5 mol of p-cresol, 0.3 mol of m-cresol, 0.35 mol of resorcinol and 0.2 mol of 2-hydroxynaphthalene are added to a reaction kettle, stirred and heated to 95° C.; then 0.25 mol of o-hydroxybenzaldehyde and 0.7 mol of formaldehyde (the raw material is a 44% formaldehyde aqueous solution) and 1.7 g of hydrochloric acid (the raw material is a 30% hydrochloric acid solution, the mass is calculated as the effective component HCl) are added, and heated to reflux; condensation reaction is carried out under stirring and reflux conditions for 2.5 hours, and dehydration is carried out under reduced pressure to obtain a crude product;

[0159] (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column (eluted with acetonitrile as the mobile phase), and low-polymerization units with a molecular weight of less than 300 in the crude product are removed, and the solvent is distilled off to obtain a phenolic resin having a weight average molecular weight Mw of 11366.

[0160] Among the polymers included in the phenolic resin product obtained by the above preparation method, the proportion of n=0 component (low polymerization degree unit) is 3.51%, the sum of the proportions of n=1, 2, 3, 4, 5 is 17.55%, and the proportion of n≥6 components is 78.94%.

[0161] The obtained phenolic resin was dissolved in deuterated dimethyl sulfoxide and tested on a Bruker Avance III HD 400M nuclear magnetic resonance spectrometer to obtain a nuclear magnetic resonance carbon spectrum (NMR-C 13 See the attachment for details Figure 6 :

[0162] Figure 6 The sample has absorption peaks at chemical shifts of 19.74, 21.25, 113.23, 117.38, 129.62, 134.2, 137.51, and 155.29 ppm, corresponding to the m-cresol structure; there are absorption peaks at chemical shifts of 21.25, 115.26, 127.56, 128.31, 128.92, 130.5, and 152.63 ppm, corresponding to the p-cresol structure; the substance has absorption peaks at chemical shifts of 115.23, 123.66, 124.32, 127.0, 129.7, and 137.51 ppm, corresponding to the m-cresol structure. There are absorption peaks at 30.49, 131.12, 134.2, 139.1, and 150.29 ppm, corresponding to 2-hydroxynaphthalene structure; there are absorption peaks at chemical shifts 113.0, 113.23, 115.23, 116.01, 142.66, 152.7, and 153.12 ppm, corresponding to meta-diphenol; the absorption peaks at 27.65, 31.68, and 33.11 ppm correspond to the methylene structure provided by formaldehyde, and the absorption peak at 42.54 ppm corresponds to the methylene carbon provided by o-hydroxybenzaldehyde. NMR-C 13 The spectrum shows that the obtained phenolic resin has a polymer with the chemical structure shown above. According to the peak areas of hydroxyl hydrogen and aromatic ring hydrogen given by the NMR hydrogen spectrum, the hydroxyl / aromatic ring ratio is calculated to be 1.25.

[0163] Example 4

[0164] This embodiment provides a phenolic resin, which includes the following structure:

[0165]

[0166] The preparation method comprises the following steps:

[0167] (1) 0.5 mol of p-cresol, 0.4 mol of m-cresol, 0.3 mol of resorcinol and 0.2 mol of 1,5-dihydroxynaphthalene 2-carboxaldehyde were added to a reaction kettle, and the temperature was raised to 95° C. with stirring; then 2.3 g of oxalic acid and 0.65 mol of formaldehyde (the raw material is a 50% formaldehyde aqueous solution) were added, and the mixture was heated to reflux with stirring; the mixture was condensed and reacted for 3.5 hours under stirring and reflux conditions, and dehydrated under reduced pressure to obtain a crude product;

[0168] (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column (eluted with acetonitrile as the mobile phase), and low-polymerization units with a molecular weight of less than 300 in the crude product are removed, and the solvent is distilled off to obtain a phenolic resin having a weight average molecular weight Mw of 8917.

[0169] Among the polymers included in the phenolic resin product obtained by the above preparation method, the proportion of n=0 component (low polymerization degree unit) is 4.74%, the sum of the proportions of n=1, 2, 3, 4, 5 is 14.24%, and the proportion of n≥6 components is 81.02%.

[0170] The obtained phenolic resin was dissolved in deuterated acetone and tested on a Bruker Avance III HD 400M nuclear magnetic resonance spectrometer to obtain a nuclear magnetic resonance carbon spectrum (NMR-C 13 See the attachment for details Figure 8 :

[0171] Figure 8 The sample has absorption peaks at chemical shifts of 15.6, 19.81, 20.13, 21.25, 112.82, 113.05, 117.34, 130.90, 131.17, 137.54, and 155.89 ppm, corresponding to the m-cresol structure; there are absorption peaks at chemical shifts of 20.77, 20.90, 115.21, 127.83, 128.05, 128.91, 130.18, and 153.13 ppm, corresponding to the p-cresol structure; the substance has absorption peaks at chemical shifts of 110.23, 124.56, 125.64, 127.28, and 128. Absorption peaks exist at 05, 129.55, 131.28, 136.35, 137.54, and 155.32 ppm, corresponding to 1,5-dihydroxynaphthalene structure; absorption peaks exist at chemical shifts 115.21, 115.29, 116.00, 142.66, 153.13, and 153.19 ppm, corresponding to meta-diphenol; the absorption peaks at 26.69, 30.32, 32.12, 34.94, and 40.31 ppm correspond to the methylene structure provided by formaldehyde, and the absorption peak at 48.74 ppm corresponds to the methyne structure provided by 1,5-di-hydroxynaphthalene-2-formaldehyde. NMR-C13 The spectrum shows that the obtained phenolic resin has a polymer with the chemical structure shown above. According to the peak areas of hydroxyl hydrogen and aromatic ring hydrogen given by the NMR hydrogen spectrum, the hydroxyl / aromatic ring ratio is calculated to be 1.13.

[0172] Example 5

[0173] This embodiment provides a phenolic resin, and the preparation method thereof comprises the following steps:

[0174] (1) 0.5 mol of p-cresol, 0.2 mol of 3,5-dimethylphenol and 0.3 mol of 2,5-dihydroxynaphthalene are added to a reaction kettle, and the temperature is raised to 95° C. with stirring; then 2.3 g of oxalic acid, 0.15 mol of o-hydroxybenzaldehyde and 0.4 mol of formaldehyde (the raw material is a 50% formaldehyde aqueous solution) are added, and the mixture is heated to reflux with stirring; the mixture is condensed and reacted for 4 hours under stirring and reflux conditions, and dehydrated under reduced pressure to obtain a crude product;

[0175] (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column (eluted with acetonitrile as the mobile phase), and low-polymerization units with a molecular weight of less than 300 in the crude product are removed, and the solvent is distilled off to obtain a phenolic resin having a weight average molecular weight Mw of 6733.

[0176] In the polymer of the phenolic resin product obtained by the above preparation method, the proportion of n=0 component (low polymerization degree unit) is 3.35%, the sum of the proportions of n=1, 2, 3, 4, 5 is 16.27%, and the proportion of n≥6 components is 82.02%. According to the peak area of ​​hydroxyl hydrogen and aromatic ring hydrogen given by NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 1.25.

[0177] Example 6

[0178] This embodiment provides a phenolic resin, and the preparation method thereof comprises the following steps:

[0179] (1) 0.5 mol of p-cresol, 0.5 mol of m-cresol and 0.2 mol of phloroglucinol were added to a reaction kettle, and the mixture was heated to 95° C. with stirring; then 4.0 g of oxalic acid, 0.2 mol of 3-hydroxynaphthalene-2-carboxaldehyde and 0.7 mol of formaldehyde (the raw material is a 50% formaldehyde aqueous solution) were added, and the mixture was heated to reflux with stirring; the mixture was condensed and reacted for 10 hours under stirring and reflux conditions, and dehydrated under reduced pressure to obtain a crude product;

[0180] (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column (eluted with acetonitrile as the mobile phase), and low-polymerization units with a molecular weight of less than 300 in the crude product are removed, and the solvent is distilled off to obtain a phenolic resin having a weight average molecular weight Mw of 23640.

[0181] In the polymer of the phenolic resin product obtained by the above preparation method, the proportion of n=0 component (low polymerization degree unit) is 3.03%, the sum of the proportions of n=1, 2, 3, 4, 5 is 10.52%, and the proportion of n≥6 components is 86.45%. According to the peak area of ​​hydroxyl hydrogen and aromatic ring hydrogen given by NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 1.16.

[0182] Example 7

[0183] This embodiment provides a phenolic resin, and the preparation method thereof comprises the following steps:

[0184] (1) 0.4 mol of p-cresol, 0.2 mol of m-cresol, 0.2 mol of resorcinol and 0.2 mol of 2,7-dihydroxynaphthalene are added to a reaction kettle, and the temperature is raised to 95° C. with stirring; then 6.0 g of oxalic acid, 0.2 mol of o-hydroxybenzaldehyde and 0.45 mol of formaldehyde (the raw material is a 50% formaldehyde aqueous solution) are added, and the mixture is heated to reflux with stirring; the mixture is condensed and reacted for 6 hours under stirring and reflux conditions, and dehydrated under reduced pressure to obtain a crude product;

[0185] (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column (eluted with acetonitrile as the mobile phase), and low-polymerization units with a molecular weight of less than 300 in the crude product are removed, and the solvent is distilled off to obtain a phenolic resin having a weight average molecular weight Mw of 17617.

[0186] In the polymer of the phenolic resin product obtained by the above preparation method, the proportion of n= / 0 component (low polymerization degree unit) is 3.33%, the sum of the proportions of n=1, 2, 3, 4, 5 is 14.63%, and the proportion of n≥6 components is 82.04%. According to the peak areas of hydroxyl hydrogen and aromatic ring hydrogen given by NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 1.18.

[0187] Example 8

[0188] This embodiment provides a phenolic resin, and the preparation method thereof comprises the following steps:

[0189] (1) 0.5 mol of p-cresol, 0.4 mol of resorcinol and 0.2 mol of 2-hydroxynaphthalene are added to a reaction kettle, and the temperature is raised to 95° C. with stirring; then 3.0 g of sulfuric acid diluted to a mass ratio concentration of 10%, 0.4 mol of o-hydroxybenzaldehyde and 0.3 mol of formaldehyde (the raw material is a 50% formaldehyde aqueous solution) are added, and the mixture is stirred and heated to reflux; the condensation reaction is carried out under stirring and reflux conditions for 7 hours, and dehydration is carried out under reduced pressure to obtain a crude product;

[0190] (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column (eluted with acetonitrile as the mobile phase), and low-polymerization units with a molecular weight of less than 300 in the crude product are removed, and the solvent is distilled off to obtain a phenolic resin having a weight average molecular weight Mw of 6613.

[0191] In the polymer of the phenolic resin product obtained by the above preparation method, the proportion of n=0 component (low polymerization degree unit) is 3.29%, the sum of the proportions of n=1, 2, 3, 4, 5, 6 is 16.98%, and the proportion of n≥ / 6 components is 79.73%. According to the peak area of ​​hydroxyl hydrogen and aromatic ring hydrogen given by NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 1.15.

[0192] Comparative Example 1

[0193] The difference between this comparative example and Example 1 is that the chromatographic column separation and purification process in step (2) is not performed. Fig. 9 It can be seen that the molecular weight distribution is significantly different from that in Example 1. Fig.10 It can be seen that the chemical structure of the NMR spectrum is basically unchanged. The weight average molecular weight of the obtained phenolic resin is 4870, of which the proportion of n=0 component is 8.93%, the sum of the proportions of n=1, 2, 3, 4, 5 is 23.17%, and the proportion of n≥6 components is 67.91%. According to the peak area of ​​hydroxyl hydrogen and aromatic ring hydrogen given by NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 1.74.

[0194] Comparative Example 2

[0195] The difference between this comparative example and Example 1 is that resorcinol is replaced by an equimolar amount of m-cresol. Fig.11 It can be seen that the molecular weight distribution is close to that of Example 1. Fig.12 The significant difference between the two can be seen in the comparative example, where the characteristic peak of resorcinol corresponding to 142.66ppm is missing. The weight average molecular weight of the obtained phenolic resin is 5113, of which the proportion of n=0 component is 4.17%, the sum of the proportions of n=1, 2, 3, 4, 5 is 30.92%, and the proportion of n≥6 components is 64.91%. According to the peak areas of hydroxyl hydrogen and aromatic ring hydrogen given by NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 0.84.

[0196] Comparative Example 3

[0197] The difference between this comparative example and Example 1 is that 3-hydroxynaphthalene-2-carboxaldehyde is replaced by an equimolar amount of m-cresol. Fig.13 It can be seen that the molecular weight decreases significantly due to the change in the aldehyde-phenol ratio. Fig.14The significant difference between the two can be seen in the comparative example. The characteristic peaks of naphthalene ring carbon and methine carbon provided by 3-hydroxynaphthalene-2-carboxaldehyde corresponding to 107.7ppm and 49.34ppm are missing in the comparative example. The weight average molecular weight of the obtained phenolic resin is 3763, of which the proportion of n=0 component is 4.39%, the sum of the proportions of n=1, 2, 3, 4, 5 is 22.25%, and the proportion of n≥6 components is 73.36%. According to the peak areas of hydroxyl hydrogen and aromatic ring hydrogen given by NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 1.39.

[0198] Comparative Example 4

[0199] This comparative example provides a phenolic resin, and its preparation method comprises the following steps:

[0200] (1) 0.4 mol of p-cresol, 0.4 mol of resorcinol and 0.2 mol of 2,5-dimethylphenol were added to a reaction kettle, and the temperature was raised to 95° C. with stirring; then 3.0 g of sulfuric acid diluted to a mass ratio concentration of 10% and 0.7 mol of formaldehyde (the raw material is a 50% formaldehyde aqueous solution) were added, and the mixture was heated to reflux with stirring; the condensation reaction was carried out under stirring and reflux conditions for 8 hours, and dehydration was carried out under reduced pressure to obtain a phenolic resin with a weight average molecular weight Mw of 8659.

[0201] In the polymer of the phenolic resin product obtained by the above preparation method, the proportion of n=1 component (low polymerization degree unit) is 8.91%, the sum of the proportions of n=2, 3, 4, 5, 6 is 22.09%, and the proportion of n≥7 components is 69.00%. According to the peak area of ​​hydroxyl hydrogen and aromatic ring hydrogen given by NMR hydrogen spectrum, the ratio of hydroxyl / aromatic ring is calculated to be 1.

[0202] Phenolic resin performance test:

[0203] (1) Weight average molecular weight M w , polydispersity coefficient D and n = 0 (dimer) component content test: GPC test to obtain the weight average molecular weight M w and number average molecular weight M n , polydispersity coefficient D = M w / M n , n=0 component content is calculated based on the peak area in the GPC spectrum;

[0204] (2) Glass transition temperature T g :DSC test its glass transition temperature T g , under nitrogen atmosphere, the temperature range is 0-300°C, and the heating rate is 10°C / min;

[0205] (3) Softening point: According to the provisions of GB / T 4507-1999, the test was carried out using an LRY-35A asphalt softening point tester with silicone oil as the heating medium.

[0206] The weight average molecular weight, polydispersity coefficient, n=0 component content, glass transition temperature and softening point of the phenolic resins provided in Examples 1 to 4 and Comparative Examples 1 to 3 were tested according to the above method. The test data are shown in Table 1.

[0207] Table 1

[0208]

[0209]

[0210] From the data in Table 1, it can be seen that the phenolic resin obtained according to the raw materials and preparation method of the present invention has a small polydispersity coefficient, a narrow molecular weight distribution, a content of n=0 component below 5%, and a high glass transition temperature and softening point. When the preparation process of the phenolic resin does not include the chromatographic column separation and purification step of the present invention (Comparative Example 1), the molecular weight distribution of the obtained phenolic resin is wide, the content of n=0 component is as high as more than 8%, and the glass transition temperature and softening point are reduced; when the density of benzene rings in the molecular structure of the phenolic resin is reduced (Comparative Examples 2 and 3), the glass transition temperature and softening point of the phenolic resin are significantly reduced.

[0211] Application Examples

[0212] A photoresist composition, the raw materials for its preparation include the following components:

[0213]

[0214] The phenolic resins are the phenolic resins provided in Examples 1 to 8 and Comparative Examples 1 to 4, the diazonaphthoquinone photosensitizer is electronic grade 215 diazonaphthoquinone sulfonyl chloride, the organic solvent is propylene glycol monomethyl ether acetate, and the surfactant is dimethyl silicone oil.

[0215] The preparation method is as follows:

[0216] The phenolic resin, the diazonaphthoquinone photosensitizer, the organic solvent and the surfactant are mixed to obtain the photoresist composition.

[0217] Photoresist performance test:

[0218] (1) The photoresist was filtered through a 0.2 μm membrane filter to remove impurities, and then spin-coated on a single-side polished silicon wafer substrate to form a 15 μm wet film, and the coating uniformity was observed;

[0219] (2) Drying on a 100°C hot plate for 2 min to evaporate the solvent and solidify into a film;

[0220] (3) exposing the substrate surface with a stepper exposure machine, with a total irradiation energy in the range of 250 to 350 mJ / cm2; developing with 2.38 wt% tetramethylammonium hydroxide after exposure, with a developing time of 20 s;

[0221] (4) The developed substrate was dried on a 105° C. hot plate for 1.5 min to obtain a test sample.

[0222] Resolution test: Use a laser microscope to test the sample to confirm the resolution of the pattern. The situation where the line width is 5μm and the L / S is 1 / 1 and can be clearly distinguished is evaluated as A, and the situation where the line width is 5μm and cannot be clearly distinguished is evaluated as B;

[0223] Heat resistance test: After heating the test sample for 5 minutes, the resolution is tested according to the above method. The temperature at which the resolution evaluation changes from A to B is the heat resistance temperature. The higher the temperature, the better the heat resistance of the photoresist.

[0224] Adhesion test: The coating obtained in step (2) is rinsed with water for 4 minutes and then peeled off. The case where it cannot be peeled off is evaluated as level 1, the case where the degree of peeling is less than 15% of the total coating area is evaluated as level 2, the case where the degree of peeling is less than 30% of the total coating area is evaluated as level 3, and the case where the degree of peeling is greater than 30% of the total coating area is evaluated as level 4.

[0225] The resolution, heat resistance and adhesion of the photoresist were tested according to the above method. The specific test results are shown in Table 2:

[0226] Table 2

[0227]

[0228]

[0229] From the test results of Table 2, it can be seen that the photoresist prepared by the phenolic resin provided in Examples 1 to 8 of the present invention has high resolution, high heat resistance and strong adhesion. When the preparation process of the phenolic resin does not include the chromatographic column separation and purification step of the present invention (Comparative Example 1), the molecular weight distribution of the obtained phenolic resin is wide, and the proportion of low-polymer molecules is large, thereby affecting the resolution, heat resistance and adhesion of the photoresist; when the preparation raw materials of the phenolic resin do not include polyhydroxyphenol (Comparative Example 2), the hydroxyl groups in the molecular structure of the obtained phenolic resin are shielded by large sterically hindered benzene rings, resulting in poor adhesion between the photoresist and the substrate, and easily causing side corrosion between the coating film and the substrate in the process of development, water washing, etc., resulting in peeling and falling off; when the phenolic resin does not contain naphthalene rings (Comparative Examples 3 and 4), the glass transition temperature of the phenolic resin is low, and the resolution and heat resistance are poor.

[0230] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the phenolic resin and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A phenolic resin, characterized in that The preparation method comprises the following steps: (1) 0.5 mol of p-cresol, 0.5 mol of m-cresol and 0.2 mol of phloroglucinol are added to a reaction kettle, and the temperature is raised to 95° C. with stirring; then 4.0 g of oxalic acid, 0.2 mol of 3-hydroxynaphthalene-2-carboxaldehyde and 0.7 mol of formaldehyde are added, wherein the raw material is a 50% formaldehyde aqueous solution, and the mixture is heated to reflux with stirring; the mixture is condensed and reacted for 10 hours under stirring and reflux conditions, and dehydrated under reduced pressure to obtain a crude product; (2) The crude product obtained in step (1) is dissolved in acetonitrile to obtain a solution, and the solution is separated and purified by a C18 silica gel column, eluting with acetonitrile as the mobile phase to remove low-polymerization units with a molecular weight of less than 300 in the crude product, and the solvent is distilled off to obtain a phenolic resin.

2. The phenolic resin according to claim 1, characterized in that: The ratio of hydroxyl groups to aromatic rings in the phenolic resin structure is greater than 1.

16.

3. A photoresist composition, characterized in that: It is prepared from the following raw materials in parts by weight: 100 parts by weight of phenolic resin; 22 parts by weight of naphthoquinone diazine photosensitizer; 270 parts by weight of organic solvent; 0.15 parts by weight of surfactant; Wherein, the phenolic resin is the phenolic resin according to claim 1 or 2.

Citation Information

Patent Citations

  • Dihydroxy naphthalene modified phenolic resin for sand prevention and preparation method thereof

    CN102206317A

  • Resist underlayer film composition, method for producing polymer for resist underlayer film, and patterning process using the resist underlayer film composition

    US20130171569A1